Fuel electrode for solid oxide water electrolytic cell and solid oxide water electrolytic cell

A fuel electrode for solid oxide water electrolysis cells using Ni-based particles and YSZ-GDC mixture stabilizes the structure against Ni oxidation, ensuring high durability and efficient electrolysis performance.

JP2024137341APending Publication Date: 2024-10-07KK TOYOTA CHUO KENKYUSHO

Patent Information

Application Number
JP2023048832
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Conventional fuel electrodes for solid oxide water electrolysis cells suffer from structural deterioration due to Ni oxidation when exposed to high-temperature water vapor, leading to decreased electrolytic properties.

Method used

The fuel electrode incorporates Ni-based particles and electrolyte particles composed of a solid solution or mixture of YSZ and GDC, which suppresses Ni oxidation through the oxygen storage ability of GDC, maintaining electrode structure integrity and enhancing electron conductivity.

Benefits of technology

The electrode structure remains stable with reduced reaction resistance increase, exhibiting high durability and efficient electrolytic performance even under high-temperature water vapor conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137341000001_ABST
    Figure 2024137341000001_ABST
Patent Text Reader

Abstract

To provide a fuel electrode for a solid oxide water electrolytic cell where an electrode structure changes a little even when the fuel electrode is exposed to high-temperature steam, and the solid oxide water electrolytic cell including the same.SOLUTION: A fuel electrode for a solid oxide water electrolytic cell includes a Ni-based particle and an electrolyte particle composed of solid oxide electrolyte A. The electrolytic particle is composed of a solid solution with ZrO2(YSZ) doped with Y and CeO2(GDC) doped with Gd, or a mixture. The solid oxide water electrolytic cell is composed of those which use such a fuel electrode for a solid oxide water electrolytic cell.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fuel electrode for a solid oxide water electrolysis cell and a solid oxide water electrolysis cell, and more specifically to a fuel electrode for a solid oxide water electrolysis cell containing a solid solution or mixture of Y-doped ZrO2 (YSZ) and Gd-doped CeO2 (GDC) as a solid oxide electrolyte, and a solid oxide water electrolysis cell including the same. [Background technology]

[0002] A solid oxide fuel cell (SOFC) is a fuel cell that uses an oxide ion conductor as an electrolyte. When fuel gases such as H2, CO, and CH4 are supplied to the anode (fuel electrode) of the SOFC and O2 is supplied to the cathode (oxygen electrode), an electrode reaction proceeds and electricity can be extracted. The CO2 and H2O produced by the electrode reaction are discharged outside the SOFC. On the other hand, solid oxide water electrolysis cells (hereinafter referred to as "SOEC") have the same structure as SOFCs, but they induce the opposite reaction to that of SOFCs. That is, when H2O is supplied to the cathode (fuel electrode) of an SOEC and an electric current is passed between the electrodes, H2 can be produced.

[0003] The SOEC is equipped with a single cell in which an anode (air electrode) is bonded to one side of an electrolyte, and a cathode (fuel electrode) is bonded to the other side. The following materials are generally used as materials for components constituting such an SOEC (see Non-Patent Documents 1 to 6). (a) Electrolytes: yttria-stabilized zirconia (YSZ), scandia-stabilized zirconia (SSZ), samaria-doped ceria (SDC), lanthanum strontium gallium magnesium oxide (LSGM), etc. (b) Air electrode: lanthanum strontium manganite (LSM), lanthanum strontium cobalt ferrite (LSCF), lanthanum strontium cobaltite (LSC), etc. (c) Anode: Ni / YSZ, Ni / SDC, Ni-Fe / SDC, etc.

[0004] In addition, Patent Document 1 states: Electronically conductive oxide particles (e.g., La 0.1 Sr 0.9 TiO3(LST)) and ion-conducting oxide particles (e.g., Gd 0.1 Ce 0.9 O2(GDC)) and an electrode skeleton obtained by sintering the same; A composite electrocatalyst (e.g., Ni-GDC cermet) supported on the surface of an electrode framework; An anode comprising:

[0005] The same document states: (A) In a conventional fuel electrode made of a sintered body of a metal such as Ni and an ion-conductive oxide, when the volume expansion due to the oxidation of the metal and the volume contraction due to the reduction of the metal oxide are repeated, the skeleton of the fuel electrode is easily destroyed; and (B) If the electrode skeleton of the fuel electrode is made only of oxide, there is almost no volume change, so destruction of the skeleton of the fuel electrode can be avoided. is stated.

[0006] Patent Document 2 discloses a substrate for an electrochemical cell in which an active layer made of a cermet of Ni and YSZ is provided between a fuel electrode body and a solid electrolyte membrane. The same document states: (a) The thickness of the active layer is 3 μm or more and 15 μm or less, (b) the average particle size (dm) of the Ni particles and the average particle size (ds) of the YSZ particles contained in the active layer are set to 0.5 μm or more and 1.0 μm or less, respectively; (c) dm / ds is set to 0.8 to 1.2 It is also described that the adhesion between the fuel electrode and the solid electrolyte membrane is improved, and peeling and cracking of the solid electrolyte membrane are suppressed.

[0007] Ni / YSZ cermet is generally used for the fuel electrode of SOEC. However, water vapor, which is the raw material for hydrogen production, is supplied to the fuel electrode at high temperatures (700°C or higher). As a result, the Ni contained in the fuel electrode is easily oxidized, causing a change in the electrode structure. As a result, the electrolytic characteristics are degraded. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2022-137626 A [Patent Document 2] JP 2004-362849 A [Non-patent literature]

[0009] [Non-Patent Document 1] Ebbesen, SD; Hansen, JB; Morgensen, MB ECS Trans. 2013, 57, 3217. [Non-Patent Document 2] Jensen, SH; Larsen, PH; Mogensen, M. Int. J. Hydrogen Energy 2007, 32, 3253. [Non-Patent Document 3] Katahira, K.; Kohchi, Y.; Shimura, T.; Iwahara, H. Solid State Ionics 2000, 138, 91. [Non-Patent Document 4] Languna-Bercero, MA; Skinner, SJ; Kilner, JAJ Power Sources 2009, 192, 126. [Non-Patent Document 5] O'Brien, JE; Stoots, CM; Herring, JS; Lessing, PA; Hartvigsen, JJ; Elangovan, SJ Fuel Cell Sci. Technol. 2005, 2, 156. [Non-Patent Document 6] Sune Dalgaard Ebbesen, Soren Hojgaard Jensen, Anne Hauch, and Morgens Bjerg Morgensen, Chem. Rev. 2014, 114, 1069 Summary of the Invention [Problem to be solved by the invention]

[0010] An object of the present invention is to provide a fuel electrode for a solid oxide water electrolysis cell which exhibits little change in electrode structure even when exposed to high-temperature water vapor. Another object of the present invention is to provide a solid oxide water electrolysis cell including such a solid oxide water electrolysis cell fuel electrode. [Means for solving the problem]

[0011] In order to solve the above problems, the present invention provides a fuel electrode for a solid oxide water electrolysis cell, comprising: Ni-based particles, Electrolyte particles made of solid oxide electrolyte A; Equipped with The electrolyte particles consist of a solid solution or mixture of Y-doped ZrO2 (YSZ) and Gd-doped CeO2 (GDC).

[0012] The solid oxide water electrolysis cell according to the present invention comprises: an electrolyte layer made of a solid oxide electrolyte C; a fuel electrode formed on one surface of the electrolyte layer; an air electrode formed on the other surface of the electrolyte layer; a reaction prevention layer inserted at the interface between the electrolyte layer and the air electrode; Equipped with The fuel electrode comprises the solid oxide water electrolysis cell fuel electrode according to the present invention. Effect of the Invention

[0013] When a cermet containing Ni-based particles and electrolyte particles is used for the fuel electrode of a solid oxide water electrolysis cell, the change in the electrode structure caused by the oxidation of Ni is suppressed if a solid solution or mixture of YSZ and GDC is used as the electrolyte particles. This is thought to be because the GDC component, which has oxygen storage capacity, suppresses the oxidation of the Ni-based particles.

[0014] Furthermore, the GDC component contained in the electrolyte particles has electronic conductivity in addition to oxide ion conductivity. Therefore, the fuel electrode containing the GDC component can expand the number and / or area of ​​electrode reaction points compared to a conventional fuel electrode not containing the GDC component. As a result, the reaction resistance (Rct2) increase rate of the fuel electrode according to the present invention is lower than that of a conventional fuel electrode, and the fuel electrode exhibits high durability. [Brief description of the drawings]

[0015] [Figure 1] This is a schematic diagram of a solid oxide water electrolysis cell using Ni / GDC-YSZ as the fuel electrode (active layer). [Diagram 2] FIG. 1 is a schematic diagram of a conventional solid oxide water electrolysis cell that uses Ni / YSZ as the fuel electrode (active layer). [Diagram 3] FIG. 1 is a schematic diagram of the water electrolysis cells of samples No. 1 and 2. [Figure 4] 4 shows the rate of increase in the reaction resistance (Rct2) of the fuel electrodes of samples Nos. 1 to 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] [Configuration 1] Ni-based particles, Electrolyte particles made of solid oxide electrolyte A; Equipped with The electrolyte particles consist of a solid solution or mixture of Y-doped ZrO2 (YSZ) and Gd-doped CeO2 (GDC). Fuel electrodes for solid oxide water electrolysis cells.

[0017] [Configuration 2] 2. A fuel electrode for a solid oxide water electrolysis cell according to claim 1, wherein the electrolyte particles have an average composition represented by the following formula (1): {Y y Zr 1-y O 2-δ'} 1-z {Gd x Ce 1-x O 2-δ} z (1) however, 0 <x≦0.30、0<y≦0.30、0<z<1.0、 δ and δ' are the values ​​at which electrical neutrality is maintained.

[0018] [Configuration 3] 3. The fuel electrode for a solid oxide water electrolysis cell according to claim 1 or 2, having a thickness of 15 μm or more and 200 μm or less.

[0019] [Configuration 4] 4. A fuel electrode for a solid oxide water electrolysis cell according to any one of configurations 1 to 3, wherein the porosity is 15% or more and 40% or less.

[0020] [Configuration 5] 5. The fuel electrode for a solid oxide water electrolysis cell according to any one of configurations 1 to 4, wherein the content of the Ni-based particles is 30.0 mass % or more and 70.0 mass % or less.

[0021] [Configuration 6] an electrolyte layer made of a solid oxide electrolyte C; a fuel electrode formed on one surface of the electrolyte layer; an air electrode formed on the other surface of the electrolyte layer; a reaction prevention layer inserted at the interface between the electrolyte layer and the air electrode; Equipped with The fuel electrode is a solid oxide water electrolysis cell comprising the fuel electrode for a solid oxide water electrolysis cell according to any one of configurations 1 to 5.

[0022] [Configuration 7] An air electrode-side current collecting layer formed on the surface of the air electrode, and / or A fuel electrode-side current collecting layer formed on the surface of the fuel electrode 7. The solid oxide water electrolysis cell of claim 6, further comprising:

[0023] An embodiment of the present invention will be described in detail below. [1. Fuel electrodes for solid oxide water electrolysis cells] The fuel electrode for a solid oxide water electrolysis cell according to the present invention (hereinafter, simply referred to as "fuel electrode") comprises: Ni-based particles, Electrolyte particles made of solid oxide electrolyte A; It is equipped with:

[0024] [1.1. Ni-based particles] The "Ni-based particles" refer to metal particles in which the mass ratio of Ni to the total mass of metal elements contained in the particles is 90 mass% or more. The mass ratio of Ni contained in the Ni-based particles is preferably 95 mass% or more. The Ni-based particles function as an electrode catalyst and an electron conductor in the fuel electrode, and the composition of the Ni-based particles is not particularly limited as long as it exhibits such functions. Examples of Ni-based particles include Ni, Ni-Fe alloys, Ni-Co alloys, etc. Among these, the Ni-based particles are preferably Ni or Ni-Fe alloys.

[0025] [1.2. Electrolyte particles] [1.2.1. Definition] In the present invention, the term "electrolyte particles" refers to particles made of a solid solution or mixture of Y-doped ZrO2 (YSZ) and Gd-doped CeO2 (GDC).

[0026] When making an anode, the raw material for the electrolyte particles is: (a) a powder having the same composition as electrolyte particles having a desired average composition; (b) A mixture of YSZ and GDC powders capable of producing electrolyte particles with the desired average composition. etc. are used. In the latter case, (b1) Electrolyte particles with a uniform composition can be obtained, (b2) Electrolyte particles consisting of a mixture of YSZ and GDC are obtained. There is.

[0027] When the electrolyte particles are made of a mixture of YSZ and GDC, the YSZ and GDC constituting the electrolyte particles may have compositions different from those of the YSZ powder and GDC powder used as raw materials due to solid-state diffusion. The history of the electrolyte particles contained in the fuel electrode is not particularly limited, and they may be produced by any method.

[0028] [1.2.2. Oxygen storage and release capacity] The GDC component contained in the electrolyte particles has a function as an oxide ion conductor, a function as an electron conductor, and a function of suppressing the oxidation of Ni contained in the Ni-based particles in the fuel electrode.

[0029] The main function of Gd doped in CeO2 is to give high ionic conductivity to CeO2 and to further improve the inherent oxygen storage and release capacity of CeO2. Furthermore, CeO2 itself also functions as an electronic conductor. Therefore, when electrolyte particles containing GDC components are added to a fuel electrode containing Ni-based particles, the oxidation of Ni contained in the Ni-based particles is significantly suppressed while maintaining high electrode activity. Even if the Ni-based particles contain metal elements other than Ni, if the oxidation of Ni can be suppressed at least, a three-phase boundary (TPB) can be secured in the electrode. Furthermore, even if a part of the Ni-based particles is oxidized, electrons are conducted via the electrolyte particles.

[0030] The reaction of CeO2 for storing and releasing oxygen is shown in the following formula (a). In formula (a), the reaction proceeding to the right side is an oxidation reaction, and the reaction proceeding to the left side is a reduction reaction. CEO 2-x +(x / 2)O2 ⇔ CeO2 …(a)

[0031] Ce ions can reversibly take a trivalent state (reduced state) or a tetravalent state (oxidized state) depending on the oxygen partial pressure in the surrounding atmosphere. Therefore, when CeO2 is exposed to an oxidizing atmosphere, CeO2 incorporates oxygen ions in the atmosphere into its crystal lattice. On the other hand, when CeO2 is exposed to a reducing atmosphere, CeO2 releases oxygen ions in the crystal lattice into the atmosphere. This is also true for GDC and electrolyte particles containing GDC components.

[0032] [1.2.3. Composition] The electrolyte particles preferably have an average composition represented by the following formula (1). {Y y Zr 1-y O 2-δ'} 1-z {Gd x Ce 1-x O 2-δ} z (1) however, 0 <x≦0.30、0<y≦0.30、0<z<1.0、 δ and δ' are the values ​​at which electrical neutrality is maintained.

[0033] [A.x] In formula (1), x represents the ratio of the number of moles of Gd to the total number of moles of Gd and Ce contained in the electrolyte particles. If x is too small, the oxygen storage capacity of the electrolyte particles may decrease. Therefore, x must be greater than 0. x is preferably 0.05 or more. On the other hand, if x is excessive, the oxygen storage capacity of the electrolyte particles may be decreased. Therefore, x is preferably 0.30 or less. x is more preferably 0.25 or less.

[0034] [B.y] In formula (1), y represents the ratio of the number of moles of Y to the total number of moles of Y and Zr contained in the electrolyte particles. Y has the effect of improving the ionic conductivity of ZrO2 and the effect of stabilizing the high-temperature phase (tetragonal, cubic) of ZrO2 at room temperature. In order to obtain such effects, y must be greater than 0. y is preferably 0.05 or more.

[0035] On the other hand, in the present invention, the ionic conductivity of the electrolyte particles is mainly controlled by the doping amount of Y (y). In this case, the ionic conductivity is highest when the composition of the YSZ component contained in the electrolyte particles is close to the 8 mol% Y2O3-ZrO2 (8YSZ) composition. Therefore, if y becomes excessive, the ionic conductivity decreases. Therefore, y is preferably 0.3 or less. More preferably, y is 0.25 or less.

[0036] [C.z] z represents the ratio of the number of moles of the GDC component to the total number of moles of the YSZ component and the GDC component contained in the electrolyte particle. In general, the larger z is, the more durable the fuel electrode is. To obtain such an effect, z must be greater than 0. z is preferably 0.5 or more, 0.6 or more, or 0.7 or more. On the other hand, if z is excessive, there is a risk that the mechanical strength cannot be ensured due to reduction expansion. Therefore, z must be less than 1.0. z is preferably 0.95 or less.

[0037] [1.3. Composition of the fuel electrode] The "content of Ni-based particles" refers to the ratio of the mass of Ni-based particles to the total mass of the electrolyte particles and Ni-based particles contained in the fuel electrode.

[0038] If the content of the Ni-based particles is too low, the total cell resistance increases and the efficiency of the electrode reaction decreases. Therefore, the content of the Ni-based particles is preferably 30 mass% or more. The content is more preferably 40 mass% or more. On the other hand, if the content of the Ni-based particles is excessive, the content of the electrolyte particles becomes small, and the oxidation of Ni contained in the Ni-based particles cannot be sufficiently suppressed. Therefore, the content of the Ni-based particles is preferably 70 mass% or less.

[0039] 1.4. Porosity The porosity of the fuel electrode affects the electrolysis characteristics. If the porosity of the fuel electrode is too small, the gas diffusion decreases, and the efficiency of the electrode reaction decreases. Therefore, the porosity of the fuel electrode is preferably 15% or more. The porosity is more preferably 20% or more, or 25% or more. On the other hand, if the porosity of the fuel electrode is too large, the number of three-phase interfaces becomes relatively small, and the efficiency of the electrode reaction decreases. Therefore, the porosity of the fuel electrode is preferably 40% or less. The porosity is more preferably 35% or less, or 30% or less.

[0040] 1.5 Thickness The thickness of the fuel electrode is not particularly limited, and an optimal thickness can be selected depending on the purpose. If the thickness of the fuel electrode is too thin, the total amount of Ni-based particles that function as an electrode catalyst decreases, and the efficiency of the electrode reaction may decrease. Therefore, the thickness of the fuel electrode is preferably 15 μm or more. The thickness is more preferably 25 μm or more, 30 μm or more, 40 μm or more, or 50 μm or more. On the other hand, even if the thickness of the fuel electrode is made thicker than necessary, there is no difference in the effect and no practical benefit. Therefore, the thickness of the fuel electrode is preferably 200 μm or less. The thickness is more preferably 180 μm or less, 160 μm or less, or 140 μm or less.

[0041] [1.6. Attribute: Reaction Resistance (Rct2) Increase Speed] "Reaction resistance (Rct2) increase rate (% / h)" refers to the value expressed by the following formula (2). Reaction resistance (Rct2) increase rate = {R2 × 100 / R1-100} ÷ 100 (2) however, R1 is the electrochemical reaction resistance of the fuel electrode for the solid oxide water electrolysis cell immediately after production. R2 is the electrochemical reaction resistance of the fuel electrode for the solid oxide water electrolysis cell after the durability test. "Electrochemical reaction resistance (Rct2)" is the reaction resistance at the three-phase interface in the fuel electrode, obtained by measuring the impedance of the fuel electrode using a reference electrode for a solid oxide water electrolysis cell, and is the diameter of the arc (second arc) that contributes to the electrode reaction, The "durability test" refers to a test in which steam electrolysis is performed for 100 hours under the conditions shown in Table 1.

[0042] [Table 1]

[0043] Conventional fuel electrodes have low oxidation resistance, so the reaction resistance (Rct2) increase rate exceeds 20% / h. In contrast, the fuel electrode of the present invention has high oxidation resistance, so the reaction resistance (Rct) increase rate is lower than that of conventional fuel electrodes. By further optimizing the manufacturing conditions, the reaction resistance (Rct2) increase rate becomes 15% / h or less, 10% / h or less, or 5% / h or less.

[0044] [1.7. Usage] The solid oxide water electrolysis cell fuel electrode according to the present invention is suitable as a fuel electrode for a water electrolysis cell, but can also be used as a fuel electrode for a solid oxide fuel cell.

[0045] [2. Manufacturing method of fuel electrodes for solid oxide water electrolysis cells] The fuel electrode for a solid oxide water electrolysis cell according to the present invention comprises: (a) preparing a compact using a raw material mixture containing raw materials for Ni-based particles and raw materials for electrolyte particles; (b) sintering the resulting green body; (c) The obtained sintered body is subjected to a reduction treatment. It can be produced by the above method.

[0046] [2.1. Molded object forming process] First, a compact is produced using a raw material mixture containing the raw material of the Ni-based particles and the raw material of the electrolyte particles.

[0047] "Raw material for Ni-based particles" refers to a raw material that becomes Ni-based particles after sintering and reduction. In the present invention, the type of raw material for Ni-based particles is not particularly limited, and an optimal raw material can be selected depending on the purpose. Examples of raw materials for Ni-based particles include NiO powder, Fe2O3 powder, Fe3O4 powder, a mixture of metal Fe and NiO or metal Ni, CoO powder, and Co2O3 powder.

[0048] The term "raw material for electrolyte particles" refers to a raw material that will become electrolyte particles after sintering. The type of raw material for electrolyte particles is not particularly limited, and an optimal raw material can be selected depending on the purpose. Examples of raw materials for electrolyte particles include: (a) an electrolyte powder having a desired composition; (b) a mixture of YSZ and GDC powders blended to obtain a desired composition; (c) a mixture of a Y-containing salt, a Zr-containing salt, a Gd-containing salt, and a Ce-containing salt (e.g., nitrates) blended to obtain a desired composition; etc.

[0049] The raw material mixture may contain a pore-forming material (e.g., carbon powder). The metal oxide (e.g., NiO powder) contained in the raw material of the Ni-based particles added to the raw material mixture is reduced after the sintered body is produced. During this process, volumetric shrinkage occurs, and pores are introduced into the sintered body. Therefore, the pore-forming material is not necessarily required. However, adding a pore-forming material to the raw material mixture increases the degree of freedom in controlling the porosity. Furthermore, the raw materials are preferably mixed so as to obtain a fuel electrode having a desired composition after sintering and reduction.

[0050] The method for producing the molded body is not particularly limited, and an optimal method can be selected depending on the purpose. Examples of the method for producing the molded body include (a) A method of tape-casting a slurry containing a raw material mixture, laminating the obtained green sheet on a substrate (e.g., a green sheet to be a current collector layer on the anode side after sintering, or a green sheet to be an electrolyte layer after sintering), and isostatically pressing the laminate; (b) preparing a slurry containing the raw material mixture and screen printing the slurry on a surface of a substrate; etc.

[0051] [2.2. Sintering process] Next, the obtained molded body is sintered (sintering step). It is preferable to select the optimum sintering conditions according to the raw material composition. Sintering is usually preferably performed in an air atmosphere at 1000°C to 1500°C for 1 hour to 5 hours. When the raw material mixture contains two or more oxides, a solid-phase reaction may occur during sintering, resulting in the formation of a solid solution with a desired composition. When the raw material mixture contains a pore-forming material, the pore-forming material disappears during sintering, forming pores in the sintered body.

[0052] [2.3. Reduction process] Next, the obtained sintered body is subjected to a reduction treatment (reduction step). As a result, the fuel electrode according to the present invention is obtained. The reduction treatment is carried out to reduce metal oxides such as NiO contained in the sintered body and generate Ni-based particles. The reduction conditions are not particularly limited, and it is preferable to select the optimum conditions depending on the composition of the electrode.

[0053] As described below, a solid oxide water electrolysis cell is composed of an assembly of a fuel electrode (cathode), an electrolyte layer, a reaction prevention layer, and an air electrode (anode). An anode-side current collecting layer may be further joined to the outside of the fuel electrode, and / or an air electrode-side current collecting layer may be further joined to the outside of the air electrode. Sintering and joining of each layer is performed by stacking the compacts and then heating the stack to a predetermined temperature. When the optimal sintering temperatures of each layer are different, sintering is usually performed in multiple stages. Furthermore, reduction of the fuel electrode is usually performed after all layers have been joined.

[0054] [3. Solid oxide water electrolysis cell] [3.1. Configuration] FIG. 1 shows a schematic diagram of a solid oxide water electrolysis cell using Ni / GDC-YSZ as the fuel electrode (active layer). In FIG. 1, a solid oxide water electrolysis cell (hereinafter, simply referred to as "SOEC") 10 is an electrolyte layer 12 made of a solid oxide electrolyte C; a fuel electrode 14 bonded to one surface of the electrolyte layer 12; a cathode 16 bonded to the other surface of the electrolyte layer 12; An intermediate layer (reaction prevention layer) 18 inserted between the electrolyte layer 12 and the air electrode 16; It is equipped with:

[0055] The solid oxide water electrolysis cell fuel electrode (Ni / GDC-YSZ) according to the present invention is used for the fuel electrode 14. Details of the fuel electrode 14 are as described above, and therefore will not be described here. 1, an anode-side current collecting layer 20 is further disposed on the outer side of the anode 14. The anode-side current collecting layer 20 is for supporting the anode 14 when the thickness of the anode 14 is thin. The anode-side current collecting layer 20 can be omitted. Similarly, although not shown, an air electrode side current collecting layer may be further disposed on the outside of the air electrode 16. The air electrode side current collecting layer (not shown) is for supporting the air electrode 16 when the thickness of the air electrode 16 is thin. The air electrode side current collecting layer may be omitted.

[0056] [3.2. Materials] The materials for the electrolyte layer 12, the air electrode 16, the intermediate layer 18, the fuel electrode side current collecting layer 20, and the air electrode side current collecting layer (not shown) are not particularly limited, and an optimum material can be selected depending on the purpose.

[0057] [3.2.1. Electrolyte layer, air electrode, intermediate layer] For example, the electrolyte layer 12 may be made of YSZ. The cathode 16 can be made of (La,Sr)CoO3 (LSC), (La,Sr)(Co,Fe)O3 (LSCF), (La,Sr)MnO3 (LSM), a composite of LSC and Gd-doped CeO2 (GDC), or the like. The intermediate layer 18 is inserted as necessary to prevent a reaction caused by direct contact between the electrolyte layer 12 and the air electrode 16. For example, when the electrolyte layer 12 is YSZ and the air electrode 16 is LSC, it is preferable to use Gd-doped CeO2 (GDC) for the intermediate layer 18.

[0058] [3.2.2. Fuel electrode side current collecting layer] The fuel electrode side current collecting layer 20 includes at least (a) a function of supporting the fuel electrode 14 formed on the surface of the electrolyte layer 12; (b) Diffusion of the raw material for electrolysis to the fuel electrode 14; (c) a function of transporting electrons required for the reduction reaction from the current collector to the fuel electrode 14; and (d) A function of discharging hydrogen generated at the fuel electrode 14 by the electrode reaction to the outside of the fuel electrode 14 It is necessary to have the following. There are no particular limitations on the composition of the fuel electrode side current collecting layer 20 as long as it exhibits the above-mentioned functions. The current collecting layer is preferably a cermet containing Ni-based particles and electrolyte particles made of a solid oxide electrolyte.

[0059] [A. Ni-based particles contained in the current collecting layer] The "Ni-based particles (hereinafter also referred to as "Ni-based particles B")" contained in the fuel electrode side current collecting layer 20 (hereinafter also simply referred to as the "current collecting layer") refer to metal particles in which the mass ratio of Ni to the total mass of metal elements contained in the particles is 10 mass% or more. The mass ratio of Ni contained in the Ni-based particles B is preferably 50 mass% or more, and more preferably 90 mass% or more.

[0060] The Ni-based particles B function as an electron conductor in the current collecting layer. The composition of the Ni-based particles B is not particularly limited as long as it exhibits such a function. Examples of the Ni-based particles B include Ni, Ni-Fe alloy, and Ni-Co alloy.

[0061] [B. Electrolyte particles] The composition of the electrolyte particles contained in the fuel electrode side current collecting layer 20 (hereinafter also referred to as "electrolyte particles B") is not particularly limited as long as it functions as a current collecting layer. Examples of the electrolyte particles B include: (a) Yttria-stabilized zirconia (YSZ) containing 3–15 mol% Y2O3; (b) a material having the same or similar composition as the electrolyte particles contained in the anode; etc. Among these, YSZ is preferable for the electrolyte particles B because it has stable mechanical strength.

[0062] [C. Composition of the current collecting layer] The "content of Ni-based particles B" refers to the ratio of the mass of Ni-based particles B to the total mass of electrolyte particles B and Ni-based particles B contained in the current collecting layer. The content of the Ni-based particles B is not particularly limited as long as the current collecting layer functions as such. The content of the Ni-based particles B contained in the current collecting layer may be the same as or different from the content of the Ni-based particles contained in the fuel electrode. The content of the Ni-based particles B contained in the current collecting layer is usually 30 to 70 mass%.

[0063] [D. Porosity] The porosity of the current collecting layer affects the gas diffusibility, strength, electronic conductivity, etc. of the current collecting layer. In general, if the porosity of the current collecting layer is too small, the gas diffusibility decreases. Therefore, the porosity of the current collecting layer is preferably 40% or more. The porosity is more preferably 45% or more, and even more preferably 50% or more. On the other hand, if the porosity of the current collecting layer is too high, the strength and electronic conductivity may decrease. Therefore, the porosity of the current collecting layer is preferably 60% or less. The porosity is preferably 58% or less, and more preferably 55% or less.

[0064] [3.2.3. Cathode side current collecting layer] The function of the air electrode side current collecting layer is almost the same as that of the anode side current collecting layer 20 , except that the reaction form at the air electrode 16 differs from that at the anode 14 . The material of the electrolyte particles in the air electrode side current collecting layer is LSC, LSCF, etc. Other points regarding the air electrode side current collecting layer are similar to those of the fuel electrode side current collecting layer 20, so a description thereof will be omitted.

[0065] [4. Effect] [4.1. Oxidation of Ni] Fig. 2 shows a schematic diagram of a conventional solid oxide water electrolysis cell (SOEC) using Ni / YSZ as the fuel electrode (active layer). In Fig. 2, the conventional SOEC 10' includes an electrolyte layer 12, a fuel electrode 14' bonded to one surface of the electrolyte layer 12, a cathode 16 bonded to the other surface of the electrolyte layer 12, and an intermediate layer 18 inserted between the electrolyte layer 12 and the cathode 16. The conventional SOEC 10' uses Ni / YSZ cermet as the fuel electrode 14'.

[0066] In an SOEC 10' having an anode 14' made of Ni / YSZ cermet, when H2O is supplied to the anode 14' and a current is passed between the anode 14' and the air electrode 16, a reduction reaction shown in the following formula (3) proceeds in the anode 14'. H2O+2e - → H2+O 2- …(3)

[0067] However, in water electrolysis using the SOEC 10', high-temperature (700°C or higher) water vapor, which serves as the raw material, is supplied to the fuel electrode 14'. As a result, the Ni contained in the fuel electrode 14' is easily oxidized to form Ni(OH)2. Since Ni(OH)2 is easily evaporated, the evaporation of Ni(OH)2 changes the morphology of the three-phase interface, which is the electrode reaction site. As a result, the electrolysis characteristics are degraded. The same is true for SOFCs. That is, water is generated by an electrode reaction at the anode (fuel electrode) of SOFCs. Therefore, especially under high-load operating conditions, the generated water may oxidize Ni in the fuel electrode, resulting in a decrease in power generation characteristics.

[0068] [4.2. Suppression of Ni oxidation by GDC components] In contrast, GDC exhibits high oxygen storage capacity. Therefore, when steam electrolysis is performed using an SOEC equipped with an anode containing Ni-based particles and electrolyte particles containing GDC components, the oxidation of Ni is significantly suppressed. The reason why the addition of GDC components to the anode in an SOEC significantly suppresses the oxidation of Ni is considered to be as follows.

[0069] [4.2.1. Oxygen fixation by GDC components] When a hydrogen electrode containing Ni and GDC components is exposed to high-temperature water vapor, the Ni is oxidized and the surface of the Ni particles becomes Ni(OH)2 (step 1). At this time, if there are GDC components in the vicinity of the Ni particles, oxygen is extracted from the Ni(OH)2 and the extracted oxygen is fixed to the GDC components (step 2). The trigger for this is thought to be the oxygen storage ability of the GDC components.

[0070] [4.2.2. Generation of reducing atmosphere by GDC components] The oxygen extracted from Ni(OH)2 is temporarily trapped by the GDC component (step 3). The fuel electrode is in a reducing atmosphere due to H2 generated from the Ni catalyst. The GDC component itself has water decomposition ability and generates hydrogen from it, so the GDC component also functions as a H2 source. Furthermore, in a reducing atmosphere, the GDC component easily releases the trapped oxygen atoms or oxygen ions as oxygen molecules. The oxygen molecules released from the GDC component are discharged outside the system before reoxidizing Ni (step 4). Alternatively, the oxygen ions in the electrolyte particles containing the GDC component diffuse within the electrolyte particles due to an electrolytic reaction, and oxygen vacancies are formed (step 5). It is believed that Ni oxidation is suppressed by repeating steps 1 to 5. EXAMPLES

[0071] (Samples No. 1 to 3) [1. Sample preparation] [1.1. Preparation of GDC powder (samples No. 1 and 2)] A certain amount of cerium nitrate Ce(NO3)3·6H2O and gadolinium nitrate Gd(NO3)3·5H2O were weighed out and dissolved in ion-exchanged water. A certain amount of cerium nitrate solution and a certain amount of gadolinium nitrate solution were added to a mixture of ion-exchanged water and 25% ammonia water, and the mixture was stirred for 15 minutes to obtain a precipitate. Next, the precipitate was heat-treated in air at 150°C for 7 h and 400°C for 5 h, and then dried to obtain GDC powders. The Gd doping amount was 10 at% (sample No. 1) or 20 at% (sample No. 2).

[0072] [1.2. Preparation of water electrolysis cell] [1.2.1. Samples No. 1 and 2] Figure 3 shows a schematic diagram of the water electrolysis cells of Samples No. 1 and 2. A GDC sheet (intermediate layer) was placed on one side of an 8YSZ electrolyte pellet (thickness: 500 μm) with a reference electrode (not shown) attached to the side, and then sintered at 1380°C. Next, a fuel electrode was formed on the other surface of the 8YSZ electrolyte pellet (the surface opposite to the surface on which the intermediate layer was baked) by applying Ni / GDC paste (NiO:GDC=1:1, mass ratio) by screen printing and firing at 1340°C.

[0073] Next, the LSC / GDC paste was applied onto the intermediate layer by screen printing and fired at 1125°C to form the air electrode. Furthermore, the LSC paste was applied onto the LSC / GDC electrode (air electrode) by screen printing and fired at 950°C to form an air electrode-side current collecting layer.

[0074] [1.2.2. Sample No. 3] A water electrolysis cell was fabricated in the same manner as in Sample No. 1, except that Ni / 8YSZ paste was used as the paste for forming the fuel electrode.

[0075] 2. Test Method Using the obtained water electrolysis cell, a steam electrolysis test (durability test) was carried out for 100 hours under the conditions shown in Table 1. In addition, impedance measurements were performed during the durability test to measure the reaction resistance (Rct2). Furthermore, the reaction resistance (Rct2) increase rate was calculated using the reaction resistance (Rct2) before and after the durability test.

[0076] [3. Results] The fuel electrode according to the present invention is characterized in that the change in particle size of Ni particles in the current collecting region (region away from the electrolyte layer / fuel electrode interface) is suppressed. This result means that the morphology of the Ni particles, which are the electron paths, does not change and the electrolytic reaction can be stably ensured. The reason that the change in particle size of Ni particles is suppressed is that the GDC component has oxygen storage capacity and suppresses the oxidation of Ni in the current collecting region. If the oxygen storage capacity is high, the effect extends not only to the current collecting region but also to the electrode active region (region near the electrolyte layer / fuel electrode interface).

[0077] FIG. 4 shows the reaction resistance (Rct2) increase rate of the fuel electrodes of samples No. 1 to 3. The reaction resistance increase rate of sample No. 3 was 23.5%. On the other hand, the reaction resistance increase rates of samples No. 1 and 2 were 3.2% and 2.6%, respectively. From FIG. 4, it can be seen that when Ni / GDC is used as the fuel electrode, the reaction resistance increase rate can be reduced to about 1 / 8 compared to Ni / YSZ. This result shows that when a solid solution or mixture of YSZ and GDC components is used as the fuel electrode, the reaction resistance increase rate decreases depending on the amount of GDC component. Furthermore, it can be seen from Figure 4 that the reaction resistance increase rate further decreases when the Gd doping amount is increased. This is believed to be because the oxygen storage capacity of GDC increases with the increase in the Gd doping amount.

[0078] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the gist of the present invention. [Industrial Applicability]

[0079] The fuel electrode for a solid oxide water electrolysis cell according to the present invention can be used as a fuel electrode for a solid oxide water electrolysis cell or a fuel electrode for a solid oxide fuel cell.

Claims

1. Ni-based particles; Electrolyte particles made of solid oxide electrolyte A; Equipped with The electrolyte particles are Y-doped ZrO 2 (YSZ) and Gd-doped CeO 2 (GDC) and a solid solution or mixture Fuel electrodes for solid oxide water electrolysis cells.

2. 2. The fuel electrode for a solid oxide water electrolysis cell according to claim 1, wherein the electrolyte particles have an average composition represented by the following formula (1): {Y y Zr 1-y O 2-δ'} 1-z {Gd x C.E. 1-x O 2-δ} z (1) however, 0<x≦0.30, 0<y≦0.30, 0<z<1.0, δ and δ' are the values ​​at which electrical neutrality is maintained.

3. 2. The fuel electrode for a solid oxide water electrolysis cell according to claim 1, having a thickness of 15 μm or more and 200 μm or less.

4. 2. The fuel electrode for a solid oxide water electrolysis cell according to claim 1, wherein the porosity is from 15% to 40%.

5. 2. The fuel electrode for a solid oxide water electrolysis cell according to claim 1, wherein the content of the Ni-based particles is 30.0 mass % or more and 70.0 mass % or less.

6. an electrolyte layer made of a solid oxide electrolyte C; a fuel electrode formed on one surface of the electrolyte layer; an air electrode formed on the other surface of the electrolyte layer; a reaction prevention layer inserted at the interface between the electrolyte layer and the air electrode; Equipped with A solid oxide water electrolysis cell, wherein the fuel electrode is the solid oxide water electrolysis cell fuel electrode according to claim 1 .

7. An air electrode-side current collecting layer formed on the surface of the air electrode, and / or A fuel electrode-side current collecting layer formed on the surface of the fuel electrode The solid oxide water electrolysis cell according to claim 6, further comprising:

Citation Information

Patent Citations

  • Base plate for electrochemical cell and electrochemical cell

    JP2004362849A

  • Reversible type fuel cell system and operational method therefor

    JP2022137626A

Cited By

  • Electrochemical cell, electrochemical cell stack, hot module, and electrolytic reactor

    JP2026077236A