Lithium manganese composite oxide for cathode active material in lithium secondary battery
A lithium manganese composite oxide with specific crystal structures addresses supply and cost issues of nickel and cobalt, offering high energy density and sustainable battery solutions for electric vehicles and portable devices.
Patent Information
- Application Number
- JP2024023166
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-02-19
- Publication Date
- 2024-10-07
AI Technical Summary
The existing lithium-ion battery cathode materials, such as LiCoO2 and Li(NiMnCo)O2, face supply issues and cost challenges due to limited resources of nickel and cobalt, while LiMn2O4 and LiFePO4 offer low specific capacity, and LiMnO2 undergoes phase transformation limiting practical capacitance.
A lithium manganese composite oxide with multiple crystal structures (R3-m, C2/m, and Pmnm space groups) is developed, providing a gradient discharge voltage profile between 3V and 4V, eliminating the need for nickel and cobalt, and maintaining high capacity.
The new cathode material achieves high energy density, cost-effectiveness, and sustainable manufacturing by avoiding cobalt supply instability, suitable for electric vehicles and portable devices.
Smart Images

Figure 2024137743000002 
Figure 2024137743000003 
Figure 2024137743000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a lithium manganese composite oxide for use as a cathode active material in lithium secondary batteries. [Background technology]
[0002] The recent development and spread of electric vehicles (EVs), portable electronic devices, and stationary power sources has increased the demand for secondary batteries as energy sources. Lithium-ion secondary batteries (LIBs) are widely used in commercial applications due to their high energy density, high operating voltage, long cycle life, and low self-discharge rate.
[0003] Lithium-containing cobalt oxide (LiCoO2) and Li(NiMnCo)O2 with layered rock salt structure are commonly used as cathode active materials for LIBs. Lithium-containing manganese oxide (LiMn2O4) with spinel structure and LiFePO4 with olivine structure are also commercially available. Among these cathode active materials, LiCoO2 and Li(NiMnCo)O2 are used in a wide range of applications due to their excellent cycle characteristics and charge / discharge efficiency. However, the cost of these materials is rising due to limited resources and supplies of the main materials (Ni and Co), making them less price-competitive for medium to large batteries used in EVs. On the other hand, LiMn2O4 and LiFePO4 are low-cost and environmentally friendly due to abundant supplies of Mn and Fe, but have only low specific capacity (about 150 mAh / g). Therefore, there is an increasing demand for the development of high-capacity cathode active materials that do not contain Ni and Co and, at the same time, alleviate supply issues and provide price competitiveness.
[0004] Layered LiMnO2 with monoclinic and triclinic structures is particularly attractive due to its high theoretical capacity compared to spinel LiMn2O4. However, LiMnO2 undergoes a phase transformation to a spinel structure under lithium extraction and shows two voltage plateaus near 4 V and below 3 V. Generally, battery capacity is estimated by the change in open circuit voltage (OCV), and it is difficult to predict the capacity of a battery using an active material with a flat voltage profile during discharge. In addition, the capacity below 3 V is too low, limiting the practical capacity.
[0005] Therefore, what is needed in the art is a Li-ion battery that does not contain nickel and / or cobalt, while at the same time achieving high energy density to avoid supply issues and remain cost competitive.
[0006] However, it was not apparent to one skilled in the art of the present invention how the shortcomings of the prior art could be overcome in light of the art as a whole at the time the invention was made.
[0007] Although certain aspects of the prior art are discussed to facilitate disclosure of the present invention, applicants are not in any way disclaiming these technical aspects, and it is contemplated that the claimed invention may include one or more of the prior art aspects discussed herein.
[0008] The present invention may address one or more of the problems and deficiencies of the prior art discussed above. However, it is contemplated that the present invention may be useful in addressing other problems and deficiencies in several technical fields. Thus, the claimed invention should not necessarily be construed as being limited to addressing any of the specific problems or deficiencies discussed herein.
[0009] Any reference or discussion in this specification to a document, act, or article of knowledge is not an admission that that document, act, or article of knowledge, or any combination thereof, was publicly available, publicly known, part of the general knowledge, or otherwise constitutes prior art under applicable legal provisions or was known to be relevant to any attempt to solve any problem or problems to which this specification pertains. Summary of the Invention [Means for solving the problem]
[0010] In various embodiments, the present invention provides a cathode active material for Li-ion secondary batteries that considers limited use of nickel (Ni) and cobalt (Co) due to supply issues. The Ni- and Co-free cathode active material of the present invention has a ramped discharge voltage profile between 3 V and 4 V. The material includes multiple crystal structures with R3-m, C2 / m, and Pmnm space groups, and is further characterized by the ability to maintain high capacity when these phases are in specific ratios.
[0011] In one embodiment, the lithium manganese composite oxide (LiMnO2) for use as a cathode active material for a lithium secondary battery includes a LiMnO2-based crystal of the Pmnm space group, a LiMnO2-based crystal of the C2 / m space group, a LiAlO2 crystal of the R-3m space group, and a Li2MnO3 crystal of the C2 / m space group.
[0012] In one example, the X-ray diffraction peaks of the lithium manganese composite oxide of the present invention are observed at 15.5° with peak intensity A due to LiMnO2-based crystals of the Pmnm space group, at 18.3° with peak intensity B due to LiMnO2-based crystals of the C2 / m space group, and at 18.65° with peak intensity C due to LiAlO2 crystals of the R-3m space group and Li2MnO3 crystals of the C2 / m space group. In a specific example, the range of the peak intensity ratio (A+B) / C of this lithium manganese composite oxide is 0.74<(A+B) / C<2.26.
[0013] The lithium manganese composite oxide of the present invention exhibits a sloping discharge voltage profile between about 3V and about 4V.
[0014] In a further embodiment, a lithium manganese composite oxide cathode electrode for a lithium secondary battery is provided. The lithium manganese composite oxide cathode electrode includes a cathode current collector layer and a cathode layer located on the cathode current collector layer. The cathode layer of the lithium manganese composite oxide cathode electrode includes a lithium manganese composite oxide material, which includes a LiMnO2-based crystal of a Pnm space group, a LiMnO2-based crystal of a C2 / m space group, a LiAlO2 crystal of a R-3m space group, and a Li2MnO3 crystal of a C2 / m space group.
[0015] In another embodiment, the present invention provides a lithium secondary battery including a cathode electrode including a cathode current collector and a cathode layer located on the cathode current collector layer, an anode electrode, and an electrolyte located between the anode electrode and the cathode electrode. In this embodiment, the cathode layer includes a lithium manganese composite oxide material including a LiMnO2-based crystal of a Pmnm space group, a LiMnO2-based crystal of a C2 / m space group, a LiAlO2 crystal of a R-3m space group, and a Li2MnO3 crystal of a C2 / m space group.
[0016] The novel cathode chemistry according to embodiments of the present invention eliminates the cobalt supply problem and reduces the cost of the battery.
[0017] Thus, the present invention provides a new chemistry for cobalt-free layered transition metal oxide cathodes for lithium-ion batteries. The proposed cobalt-free cathode offers lower cost and eliminates the future risk of cobalt supply instability, providing sustainable manufacturing of batteries.
[0018] The above embodiments are applicable to many applications requiring rechargeable batteries, including, but not limited to, electric vehicles, portable electronic devices, and a variety of other applications requiring high capacity, long cycle life, and low cost.
[0019] The invention accordingly comprises the features of construction, combination of elements, and arrangement of parts exemplified in the disclosure which follows, the scope of the invention being indicated in the appended claims. [Brief description of the drawings]
[0020] For a more complete understanding of the present invention, reference should be made to the following detailed description taken in conjunction with the accompanying drawings.
[0021] [Figure 1] 1 shows powder X-ray diffraction data of lithium manganese composite oxide cathode samples 1 to 6. [Diagram 2] 1 shows powder X-ray diffraction data for lithium manganese composite oxide cathodes Comparative Examples 1 to 3. [Diagram 3] 1 shows the discharge curves and dQ / dV plots of lithium manganese composite oxide cathode samples 1 to 3. [Figure 4] 1 shows the discharge curves and dQ / dV plots of lithium manganese composite oxide cathode samples 4 to 6. [Diagram 5] 1 shows the discharge curves and dQ / dV plots of lithium manganese composite oxide cathode comparisons 1 to 3. [Figure 6] 3 shows the relationship between the crystal composition ratio and the discharge capacity of the lithium manganese composite oxide cathode material of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] In the following detailed description of the preferred embodiment, reference is made to the accompanying drawings which form a part hereof, and which show, by way of illustration, specific embodiments in which the invention may be practiced, It is to be understood that other embodiments may be utilized and structural changes may be made without departing from the scope of the present invention.
[0023] As used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. As used in this specification and the appended claims, the term "or" is generally used in its sense including "and / or" unless the context clearly dictates otherwise.
[0024] According to various embodiments, the present invention provides a novel Mn-based Li-ion battery (LIB) cathode that has high discharge capacity, low cost, and easy capacity estimation. The present invention further provides a high energy density LIB using the novel cathode.
[0025] The Mn-based cathode active material of the present invention has a slope voltage profile during discharge of about 3 V to about 4 V. This material exhibits high capacity when the ratio of the powder x-ray diffraction peak intensities originating from the orthorhombic or monoclinic LiMnO2-based layered structure, R-3m LiAlO2, and C2 / m Li2MnO3 is within a specific range.
[0026] The active material of the present invention has a capacitance of 10 mA g -1 3.4V vs Li / Li measured by discharge experiments at a temperature of 25°C in a small environmental test chamber starting from constant current charging (Li extraction) with a charge / discharge current density of 1.0V, an upper voltage cutoff limit of 4.3V and a lower limit of 2.5V. + -0.12mAh g -1 ·v -1 It is a Li-containing composite oxide having a dQ / dv of less than 100 nm.
[0027] The material of the present invention is a Li-containing composite oxide that exhibits X-ray diffraction peaks observed at 15.5° with peak intensity A attributable to LiMnO2-based crystals of the Pmnm space group, 18.3° with peak intensity B attributable to LiMnO2-based crystals of the C2 / m space group, and 18.65° with peak intensity C attributable to LiAlO2 crystals of the R-3m space group and Li2MnO3 crystals of the C2 / m space group. The range of the peak intensity ratio (A+B) / C is 0.74<(A+B) / C<2.26. The experimental conditions for identifying these peak intensities include an X-ray diffraction apparatus (Rigaku, SmartLab), an X-ray source (CuKa (0.15418 nm)), a divergence angle of the parallel slit analyzer: 5°, a lateral length of the entrance slit: 5.0 mm, an aperture angle of the parallel slit receiving: 5.0°, and a K β Filter step size: 0.01°, entrance slit: 1 / 6°, receiving slit 1: 4.0 mm, receiving slit 2: 13 mm were included.
[0028] The material of the present invention is a lithium (Li) manganese (Mn) oxide having the above-mentioned characteristics, in which one or more of the Mn sites are substituted with at least one of the following metal elements: Al, Ti, V, Cr, Fe, Li, Zn, Mg, Ga, Zr, Nb, Mo, and Sn.
[0029] The material of the present invention is a lithium (Li) manganese (Mn) oxide having the above characteristics, in which one or more of the Li sites are substituted with at least one of the following metal elements: Na, Mg, Ca, Zn, Cu, Ga, and Mn.
[0030] In various embodiments, the layered lithium manganese composite oxide of the present invention is prepared by sintering a mixture of manganese hydroxide and a lithium complex.
[0031] In a particular embodiment, to prepare manganese hydroxide, a precursor is obtained by dissolving at least one organometallic salt containing Mn and at least one organometallic salt containing an element other than Mn, and then dissolving OH for coprecipitation. - The mixture is concentrated and dried.
[0032] Examples of lithium complexes include inorganic acid salts such as Li2CO3 and LiNO3, and hydroxides such as LiOH and LiOH·H2O.
[0033] Sintering of the manganese hydroxide and lithium complex mixture can be carried out in low oxygen partial pressure, including vacuum and N2, Ar or He atmospheres. The sintering temperature range can be from 350° C. to 1200° C., preferably from 500° C. to 1000° C. The oxygen concentration after reaching the maximum temperature is maintained below 10000 ppm, preferably below 1000 ppm.
[0034] The primary particles of the material of the present invention are about 0.01 μm to about 50 μm, preferably about 0.02 μm to about 30 μm. When this material is used in a LIB cathode, if the primary particle size (particle diameter) is too small, the ion transport resistance at the solid electrolyte interface increases due to a side reaction with the electrolyte. On the other hand, if the primary particle size is too large, the interface area between the active material and the electrolyte becomes small, so that the resistance of electronic charge transport and Li diffusion in the active material increases, which causes a large overvoltage under high charge / discharge current density.
[0035] The secondary particles of the material of the present invention are 0.1 μm to 100 μm, preferably 0.2 μm to 60 μm. If the secondary particle size is too small, the material is difficult to handle, and if the secondary particle size is too large, the electrode slurry is difficult to prepare.
[0036] The specific surface area of the layered lithium manganese composite oxide of the present invention is 0.05 m 2 / g or more 100m 2 / g or less, preferably 0.1m 2 / g or more 50m 2 / g or less. If the specific surface area of this material is too large, the ion transport resistance at the solid electrolyte interface increases due to side reactions with the electrolyte. If the specific surface area is too small, the interface area between the active material and the electrolyte becomes small, so the resistance of electronic charge transport and Li diffusion in the active material increases, which causes a large overvoltage under high charge / discharge current density.
[0037] The layered lithium manganese composite oxide synthesized by the above method is a main material for battery reactions and can be used as a cathode active material for lithium ion secondary batteries capable of absorbing and releasing Li ions.
[0038] The cathode electrode for a lithium ion secondary battery of the present invention comprises the above-mentioned cathode active material, a binder polymer, a conductive assistant, and a cathode current collector. The cathode layer can be obtained by preparing a slurry mixture using the cathode active material, the binder polymer (described in detail below), the conductive assistant, and a solvent. The slurry mixture is then applied onto the cathode current collector and dried.
[0039] The proportion of the cathode active material in the cathode layer is about 50% by weight or more and about 99% by weight or less, preferably about 90% by weight or less. Examples of binder polymers include polyvinylidene difluoride, polytetrafluoroethylene, vinylidene fluoride, styrene butadiene rubber, and polymethyl methacrylate. The proportion of the binder polymer in the cathode layer is about 1% by weight or more and about 20% by weight or less. If the amount of the binder polymer is insufficient, the mechanical strength of the cathode decreases, causing a poor cycle life. On the other hand, if the amount of the polymer binder is excessive, the battery capacity and power decrease.
[0040] The cathode layer contains a conductive additive to enhance conductivity. Examples of the conductive additive include amorphous carbon materials such as natural graphite, artificial graphite, and acetylene black. The proportion of the conductive additive in the cathode layer is about 1% by weight to about 20% by weight. An insufficient amount of the conductive additive causes poor conductivity, and an excessive amount of the conductive additive reduces the battery capacity.
[0041] An organic solvent that dissolves or disperses the binder is used as a solvent to prepare the slurry mixture. Examples of the solvent include N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide. The active material can be made into a slurry with a latex such as styrene butadiene rubber by adding a dispersant or thickener.
[0042] The thickness of the cathode layer is generally about 10 μm to 200 μm. Examples of materials used for the current collector include aluminum, stainless steel, and nickel-coated steel. Aluminum is preferably used. The cathode layer prepared by slurry formation, spreading, and drying is preferably compressed, for example, by roll pressing, to increase the packing density of the cathode active material.
[0043] A lithium ion secondary battery consists of a cathode electrode, an anode electrode, and an electrolyte. The cathode active material of the present invention can be combined with any anode electrode commonly used in lithium ion secondary batteries. For example, carbonaceous materials used in lithium ion batteries can be used as the anode electrode. Lithium metal and alloys of lithium with other metals such as Al, Si, Sn, Pb, In, Bi, Sb, Ag, etc. can also be used as the anode electrode.
[0044] Examples of the carbonaceous material used in the anode electrode include natural graphite, artificial graphite, coal / petroleum pitch coke, resin compositions such as phenolic resin, and various celluloses sintered at high temperatures. Two or more of these carbonaceous materials can also be combined to form an anode electrode composite. Examples of the anode current collector include Cu, Ni, stainless steel, and Ni-coated steel, with Cu being preferred.
[0045] The electrolyte layer generally consists of an ion-conducting electrolyte and a separator. Usually, a porous polymer film is used as the separator. Examples of separators include polyolefin-based polymers such as nylon, cellulose acetate, nitrocellulose, polysulfone, polyacrylonitrile, polyvinylidene fluoride, polypropylene, polyethylene, and polybutene. In the lithium ion secondary battery of the present invention, organic solvents, polymer solid electrolytes, gel electrolytes, and inorganic solid electrolytes can be used as ion conductors. As organic solvents, carbonates, ethers, ketones, sulfolane complexes, lactones, nitriles, and chlorinated hydrocarbons can be used. Examples include propylene carbonate, ethylene carbonate, vinylene carbonate, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, 4-methyl-2-pentanone, 1,2-dimethoxyethane, 1,2-diethoxyethane, γ-butyrolactone, 1,3-dioxolane, 4-methyl-1,3-dioxolane, diethyl ether, sulfolane, methylsulfolane, acetonitrile, propionitrile, benzonitrile, butyronitrile, valeronitrile, 1,2-dichloroethane, and mixtures of two or more of these solvents. Examples of salts that dissolve in these solvents include lithium salts such as LiClO4, LiAsF6, LiPF6, LiBF4, and mixtures of two or more of these salts. EXAMPLES
[0046] In an exemplary embodiment for the preparation of the novel material of the present invention, solution B (5 g lithium hydroxide in 100 ml water) was added dropwise to solution A (17 g lithium nitrate dissolved in 200 ml water) to control the pH of solution A to about 10-11. Solution C (manganese nitrate and aluminum nitrate dissolved in 100 ml water) was added dropwise to solution A at pH 10-11 to obtain a precipitate. During the addition of solution C, solution B was added dropwise as necessary to maintain the pH of solution A at about 10-11. The obtained precipitate was then dried to obtain a manganese precursor.
[0047] The X-ray diffraction measurement conditions were: X-ray diffraction apparatus (Rigaku, SmartLab), X-ray source (CuKa (0.15418 nm)), parallel slit analyzer divergence angle: 5°, incident slit horizontal length: 5.0 mm, receiving parallel slit aperture angle: 5.0°, K β The filter step size was 0.01°, entrance slit was 1 / 6°, receiving slit 1 was 4.0 mm, and receiving slit 2 was 13 mm. The peak intensity ratio (A+B) / C was calculated as the intensity of the peaks observed at 15.5°±0.5°, 18.3°±0.5°, and 18.65°±0.5°, respectively.
[0048] The cathode electrode was prepared by making a slurry of N-methylpyrrolidone, 80 wt% active material, 10 wt% acetylene black, and 10 wt% polyvinylidene fluoride. The slurry was spread on an aluminum foil, dried, pressed at 15 tons, and punched into a disk with a diameter of 10 mm to prepare the cathode electrode. The total loading of the cathode active material was controlled to 3.5 mg.
[0049] The battery capacity was tested using a coin cell. The above 10 mm diameter cathode electrode was placed on the cathode cap, and a porous polyethylene film was placed on top of it as a separator. After placing the polypropylene film, a gasket was used to hold the separator. A lithium metal anode with a thickness of 0.5 mm was placed on top, and a spacer was added to control the thickness. Then, a non-aqueous electrolyte (1M LiPF6 in a mixture of ethylene carbonate and diethyl carbonate with a volume fraction of 1:1) was added to the cell and closed with the anode cap.
[0050] Using this coin cell, a current charge / discharge test was performed at a current density of 10 mA / g relative to the mass of the active material. The upper limit voltage was 4.3 V and the lower limit voltage was 2.5 V. In this specification, the capacity (unit: mAh / g) is defined as the discharge capacity per unit weight of the active material. From the discharge curve in the above voltage range, the vertical axis shows the voltage and the horizontal axis shows the derivative of the capacity with respect to the voltage (dQ / dV, mAh g -1 ·v -1) was obtained, and dQ / dV at 3.4 V was calculated.
[0051] The following Examples, Samples 1-6, and Comparative Examples, Comparisons 1-3 were analyzed and are summarized in Table 1 below. Table 1 includes the peak intensities, peak intensity ratios, differential capacities, and discharge capacities of the cathode samples synthesized and described below.
[0052] Sample 1 0.232g of LiOH·H2O and 0.531g of the above precursor were mixed in a mortar and sintered at 950℃ for 2h to obtain a powder sample. The X-ray peak intensity ratio (A+B) / C, the capacity obtained from the discharge test, and dQ / dV obtained from the discharge curve are shown in Table 1. Through X-ray diffraction analysis and comparison of the obtained results with X-ray powder diffraction database numbers 01-075-8605, 01-087-1255, 01-078-5048, and 01-074-2232, it was confirmed that the sample was lithium manganese oxides including monoclinic LiMnO2, triclinic LiAlO2, and monoclinic Li2MnO3.
[0053] Sample 2 0.216g of LiOH·H2O and 0.547g of the above precursor were mixed in a mortar and sintered at 950℃ for 2h to obtain a powder sample. The X-ray peak intensity ratio (A+B) / C, the capacity obtained from the discharge test, and the dQ / dV obtained from the discharge curve are shown in Table 1. Through X-ray diffraction analysis and comparison of the obtained results with X-ray powder diffraction database numbers 01-075-8605, 01-087-1255, 01-078-5048, and 01-074-2232, it was confirmed that the sample was lithium manganese oxides including monoclinic LiMnO2, triclinic LiAlO2, and monoclinic Li2MnO3.
[0054] Sample 3 0.198g of LiOH·H2O and 0.565g of the above precursor were mixed in a mortar and sintered at 950℃ for 2h to obtain a powder sample. The X-ray peak intensity ratio (A+B) / C, the capacity obtained from the discharge test, and dQ / dV obtained from the discharge curve are shown in Table 1. Through X-ray diffraction analysis and comparison of the obtained results with X-ray powder diffraction database numbers 01-075-8605, 01-087-1255, 01-078-5048, and 01-074-2232, it was confirmed that the sample was lithium manganese oxides including monoclinic LiMnO2, triclinic LiAlO2, and monoclinic Li2MnO3.
[0055] Sample 4 0.216g of LiOH·H2O and 0.547g of the above precursor were mixed in a mortar and sintered at 950℃ for 0.5h to obtain a powder sample. The X-ray peak intensity ratio (A+B) / C, the capacity obtained from the discharge test, and the dQ / dV obtained from the discharge curve are shown in Table 1. Through X-ray diffraction analysis and comparison of the obtained results with X-ray powder diffraction database numbers 01-075-8605, 01-087-1255, 01-078-5048, and 01-074-2232, it was confirmed that the sample was lithium manganese oxides including monoclinic LiMnO2, triclinic LiAlO2, and monoclinic Li2MnO3.
[0056] Sample 5 0.198g of LiOH·H2O and 0.565g of the above precursor were mixed in a mortar and sintered at 950℃ for 6 hours to obtain a powder sample. The X-ray peak intensity ratio (A+B) / C, the capacity obtained from the discharge test, and the dQ / dV obtained from the discharge curve are shown in Table 1. Through X-ray diffraction analysis and comparison of the obtained results with X-ray powder diffraction database numbers 01-075-8605, 01-087-1255, 01-078-5048, and 01-074-2232, it was confirmed that the sample was lithium manganese oxides including monoclinic LiMnO2, triclinic LiAlO2, and monoclinic Li2MnO3.
[0057] Sample 6 0.316g of LiNO3·H2O and 0.434g of the above precursor were mixed in a mortar and sintered at 950℃ for 2h to obtain a powder sample. The X-ray peak intensity ratio (A+B) / C, the capacity obtained from the discharge test, and dQ / dV obtained from the discharge curve are shown in Table 1. Through X-ray diffraction analysis and comparison of the obtained results with X-ray powder diffraction database numbers 01-075-8605, 01-087-1255, 01-078-5048, and 01-074-2232, it was confirmed that the sample was lithium manganese oxides including monoclinic LiMnO2, triclinic LiAlO2, and monoclinic Li2MnO3.
[0058] Comparison 1 0.248g LiOH·H2O and 0.515g of the above precursor were mixed in a mortar and sintered at 950℃ for 2h to obtain a powder sample. The X-ray peak intensity ratio (A+B) / C, the capacity obtained from the discharge test, and dQ / dV obtained from the discharge curve are shown in Table 1. Through X-ray diffraction analysis and comparison of the obtained results with X-ray powder diffraction database numbers 01-075-8605, 01-087-1255, 01-078-5048, and 01-074-2232, the sample was confirmed to be lithium manganese oxides including monoclinic LiMnO2, triclinic LiAlO2, and monoclinic Li2MnO3.
[0059] comparison 2 0.232g of LiOH·H2O and 0.531g of the above precursor were mixed in a mortar and sintered at 750℃ for 2h to obtain a powder sample. The X-ray peak intensity ratio (A+B) / C, the capacity obtained from the discharge test, and dQ / dV obtained from the discharge curve are shown in Table 1. Through X-ray diffraction analysis and comparison of the obtained results with X-ray powder diffraction database numbers 01-075-8605, 01-087-1255, 01-078-5048, and 01-074-2232, it was confirmed that the sample was lithium manganese oxides including monoclinic LiMnO2, triclinic LiAlO2, and monoclinic Li2MnO3.
[0060] Comparison 3 0.248g LiOH·H2O and 0.515g of the above precursor were mixed in a mortar and sintered at 1050℃ for 2h to obtain a powder sample. The X-ray peak intensity ratio (A+B) / C, the capacity obtained from the discharge test, and the dQ / dV obtained from the discharge curve are shown in Table 1. Through X-ray diffraction analysis and comparison of the obtained results with X-ray powder diffraction database numbers 01-075-8605, 01-087-1255, 01-078-5048, and 01-074-2232, it was confirmed that the sample was lithium manganese oxides including monoclinic LiMnO2, triclinic LiAlO2, and monoclinic Li2MnO3.
[0061] [Table 1]
[0062] FIG. 1 shows powder X-ray diffraction data for Samples 1 to 6. FIG. 2 shows powder X-ray diffraction data for Comparative Examples 1 to 3. FIG. 3 shows discharge curves and dQ / dV plots for Samples 1 to 3. FIG. 4 shows discharge curves and dQ / dV plots for Samples 4 to 6. FIG. 5 shows discharge curves and dQ / dV plots for Comparative Examples 1 to 3. FIG. 6 shows the relationship between the crystal composition ratio and discharge capacity of the cathode material of the present invention.
[0063] As shown and described, the present invention provides a layered lithium manganese composite oxide with improved initial discharge capacity that can be used as a cathode material in lithium ion secondary batteries.
[0064] All referenced publications are incorporated herein by reference in their entirety. Furthermore, if a definition or use of a term in a reference incorporated herein by reference is inconsistent with or contrary to the definition of that term provided herein, the definition of that term provided herein shall apply and the definition of that term in the reference shall not apply.
[0065] The above advantages and those made apparent from the foregoing description are efficiently attained. Since certain modifications may be made to the above construction without departing from the scope of the invention, it is intended that all matter contained in the above description or shown in the accompanying drawings shall be interpreted as illustrative and not in a limiting sense.
[0066] It is also to be understood that the appended claims are intended to cover all of the generic and specific features of the invention described herein, as well as all statements of the scope of the invention that may be said to fall therebetween as a matter of language.
Claims
1. Lithium manganese composite oxide (LiMnO) for use as cathode active material in lithium secondary batteries 2 ) LiMnO in Pmnm space group 2 and LiMnO in the C2 / m space group 2 and LiAlO in R-3m space group 2 Crystals and Li in the C2 / m space group 2 MnO 3 Crystals and A lithium manganese composite oxide comprising:
2. The X-ray diffraction peak of the lithium manganese composite oxide is LiMnO of the Pmnm space group with a peak intensity of A. 2 The peak intensity is B and is observed at 15.5° due to the LiMnO 2 The peak intensity C is observed at 18.3° due to the R-3m space group LiAlO 2 Crystals and the C2 / m space group Li 2 MnO 3 The lithium manganese composite oxide according to claim 1, which is observed at 18.65° due to the crystal.
3. 3. The lithium manganese composite oxide according to claim 2, wherein the peak intensity ratio (A+B) / C is in the range of 0.74<(A+B) / C<2.
26.
4. 2. The lithium manganese composite oxide according to claim 1, wherein one or more of the manganese (Mn) sites are substituted with one or more of Al, Ti, V, Cr, Fe, Li, Zn, Mg, Ga, Zr, Nb, Mo and Sn.
5. The lithium manganese composite oxide according to claim 1, wherein one or more of the lithium (Li) sites are substituted with one or more of Na, Mg, Ca, Zn, Cu, Ga, and Mn.
6. 2. The lithium manganese composite oxide for use as a cathode active material for a lithium secondary battery according to claim 1, wherein the lithium manganese composite oxide has a sloped discharge voltage profile between about 3 V and about 4 V.
7. The lithium manganese composite oxide of claim 1 , wherein the lithium manganate material is formed by sintering a mixture of manganese hydroxide and a lithium complex.
8. The lithium manganese composite oxide according to claim 7 , wherein the lithium complex comprises at least one of an inorganic acid salt and a hydroxide.
9. The lithium manganese composite oxide according to claim 1, wherein the primary particles of the lithium manganese composite oxide are about 0.01 μm to 50 μm.
10. The lithium manganese composite oxide according to claim 1, wherein the primary particles of the lithium manganese composite oxide are about 0.02 μm to 30 μm.
11. The lithium manganese composite oxide according to claim 1, wherein the secondary particles of the lithium manganese composite oxide are about 0.1 μm to about 100 μm.
12. The lithium manganese composite oxide according to claim 1, wherein the secondary particles of the lithium manganese composite oxide are about 0.2 μm to about 60 μm.
13. The specific surface area of the lithium manganese composite oxide is about 0.05 m 2 / g ~ approx. 100m 2 The lithium manganese composite oxide according to claim 1, wherein the lithium manganese complex oxide has a molecular weight of 1.0 to 1.0 g.
14. The specific surface area of the lithium manganese composite oxide is about 0.1 m 2 / g ~ approx. 50m 2 The lithium manganese composite oxide according to claim 1, wherein the lithium manganese complex oxide has a molecular weight of 1.0 to 1.0 g.
15. A lithium manganese composite oxide cathode electrode for a lithium secondary battery, comprising: A cathode current collector layer; a cathode layer located on the cathode current collector layer; and The cathode layer comprises a lithium manganese composite oxide material, the lithium manganese composite oxide material comprising: LiMnO in Pmnm space group 2 Crystals of this type, LiMnO in the C2 / m space group 2 Crystals of this type, LiAlO in R-3m space group 2 Crystals, and Li in the C2 / m space group 2 MnO 3 crystal A lithium manganese composite oxide cathode electrode comprising:
16. The lithium manganese composite oxide cathode according to claim 15 , wherein the cathode layer further comprises at least one of a binder polymer and a conductive assistant.
17. The proportion of the lithium manganese composite oxide in the cathode layer is about 50% by weight to about 90% by weight, the proportion of the binder polymer in the cathode layer is about 1% by weight to about 20% by weight, and the proportion of the conductive assistant in the cathode layer is about 1% by weight to about 20% by weight. The lithium manganese composite oxide cathode according to claim 16.
18. A lithium secondary battery, A cathode electrode comprising a cathode current collector and a cathode layer located on the cathode current collector layer, the cathode layer comprising a lithium manganese composite oxide material, the lithium manganese composite oxide material comprising: LiMnO in Pmnm space group 2 Crystals of this type, LiMnO in the C2 / m space group 2 Crystals of this type, LiAlO in R-3m space group 2 crystal, Li in the C2 / m space group 2 MnO 3 crystal A cathode electrode comprising: An anode electrode; an electrolyte located between the anode electrode and the cathode electrode; A lithium secondary battery comprising:
19. The X-ray diffraction peak of the lithium manganese composite oxide is LiMnO of the Pmnm space group with a peak intensity of A. 2 The peak intensity is B and is observed at 15.5° due to the LiMnO 2 The peak intensity C is observed at 18.3° due to the R-3m space group LiAlO 2 Crystals and the C2 / m space group Li 2 MnO 3 The lithium secondary battery according to claim 18, wherein the polarization angle is observed at 18.65° due to crystallization.