Bale molding, block copolymer, resin composition, and method for manufacturing block copolymer

A block copolymer with tailored molecular properties addresses the high hardness issue of aromatic vinyl-conjugated diene copolymers, enabling easy handling and crushing while preserving impact resistance and gloss in styrenic resin applications.

JP2024137757APending Publication Date: 2024-10-07JAPAN ELASTOMER CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024029695
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-02-29
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Aromatic vinyl-conjugated diene block copolymers used as modifiers for styrenic resins provide good impact resistance but often result in high hardness of molded products, leading to issues with handling and crushing, as they may not be easily penetrated by transportation robots and require spacing during stacking, which affects efficiency.

Method used

A block copolymer with specific molecular weight ratios, monomer unit contents, and viscosity is developed, featuring a content of aromatic vinyl monomer units between 10 to 30% by mass, a ratio of block aromatic vinyl moiety to total aromatic vinyl monomer units of 90 to 100% by mass, a peak top molecular weight of 10,000 to 30,000, and a molecular weight distribution of 1.15 to 1.40, ensuring appropriate hardness and crushability.

Benefits of technology

The solution results in a block copolymer that balances hardness and crushability, allowing easy handling and stacking, while maintaining excellent gloss and impact resistance when used as a toughening agent for styrenic resins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137757000001
    Figure 2024137757000001
  • Figure 2024137757000002
    Figure 2024137757000002
  • Figure 2024137757000003
    Figure 2024137757000003
Patent Text Reader

Abstract

To provide a bale molding composed of a block copolymer which has adequate hardness, is easily crushed and is excellent in handling property.SOLUTION: A bale molding of a block copolymer has an aromatic vinyl monomer unit and a conjugated diene monomer unit, wherein the block copolymer has a block aromatic vinyl part, and satisfies [conditions (a) to (d)]. [Condition (a)] A content of the aromatic vinyl monomer unit in the block copolymer is 10 to 30 mass%. [Condition (b)] A ratio of the block aromatic vinyl part to the total content of the aromatic vinyl monomer unit is 90 to 100 mass%. [Condition (c)] A peak top molecular amount of the block aromatic vinyl part is 10,000 to 30,000. [Condition (d)] A ratio (Mw / Mn) of a weight average molecular weight Mw to a number average molecular weight Mn of the block aromatic vinyl part is 1.15 to 1.40.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a bale molded article, a block copolymer, a resin composition, and a method for producing a block copolymer. [Background technology]

[0002] Styrene-based resins have been widely used for various applications because they have excellent rigidity, transparency, gloss, and moldability. However, because they have poor impact resistance, rubber-like polymers are added to styrene-based resins as modifiers. Methods for adding a rubbery polymer to a styrene-based resin include, for example, a method in which the rubbery polymer is mechanically blended with a polystyrene-based resin, a method in which a styrene solution of the rubbery polymer is subjected to bulk polymerization, and a method in which the rubbery polymer is subjected to bulk suspension polymerization. In particular, the method of adding a rubber-like polymer to a styrene-based resin by the various polymerization methods described above is widely practiced industrially to produce an impact-resistant styrene-based resin composition, since the physical properties of the resulting resin composition are excellent, and the composition is used as a material for household electrical appliances.

[0003] Regarding the resin modification of acrylonitrile-styrene resin (ABS), a technique is known in which a 5% by mass styrene solution of a low-viscosity aromatic vinyl-conjugated diene block copolymer is used to reduce the particle size of the rubber-like polymer particles used as a modifier. For example, Patent Documents 1 and 2 below disclose a technique for producing a styrene-based resin having good impact resistance by specifying the peak top molecular weight of the block styrene portion in an aromatic vinyl-conjugated diene block copolymer, which is a modifier, to a predetermined value. Furthermore, Patent Document 3 listed below discloses a method for producing a conjugated diene polymer having a reduced Li content, and further discloses a technology for adjusting the viscosity of a 5 mass % styrene solution of the conjugated diene polymer to 11 to 35 mPa s and using the solution to modify resins such as HIPS resins and ABS resins. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 4029470 [Patent Document 2] Patent No. 4029471 [Patent Document 3] Patent No. 6646437 Summary of the Invention [Problem to be solved by the invention]

[0005] The aromatic vinyl-conjugated diene block copolymer as described above as a modifier can provide good bale moldability by adjusting the viscosity of the styrene solution to a low value. However, even if such an aromatic vinyl-conjugated diene block copolymer has a low styrene solution viscosity, the molded bale may have a high hardness. In such a case, when the bale is moved by being pinched by the claws of a transport robot, the claws may not be able to bite into the bale, causing it to fall off. In addition, if the bale is hard, a load is applied when the bale is crushed, so that an interval between feeding the bale is required. The hardness of the bale molded body is affected by the structure of the aromatic vinyl-conjugated diene block copolymer. The bale moldability is described in the above Patent Document 2, but the hardness and crushability of the bale molded body are not described in the Patent Documents 1 to 3. The term "bale molded body" refers to a rectangular block unit weighing 25 to 35 kg, which is press-molded from synthetic rubber.

[0006] Therefore, an object of the present invention is to provide a bale molded product made of a block copolymer that has appropriate hardness, is easy to crush, and has excellent handleability, as well as a block copolymer constituting the bale molded product, and a resin composition that is a polymer of the block copolymer and a styrene-based resin. [Means for solving the problem]

[0007] As a result of intensive investigations to solve the above-mentioned problems of the conventional techniques, the present inventors have found that the above-mentioned problems of the conventional techniques can be solved by specifying the content of aromatic vinyl monomer units, the ratio of the block aromatic vinyl moiety to the total content of aromatic vinyl monomer units, the peak top molecular weight of the block aromatic vinyl moiety, and the molecular weight distribution of the block aromatic vinyl moiety, and have thus completed the present invention. That is, the present invention is as follows.

[0008] [1] A veil molded article of a block copolymer having an aromatic vinyl monomer unit and a conjugated diene monomer unit, The block copolymer has a block aromatic vinyl moiety, A bale molded body that satisfies the following <Condition (a)> to <Condition (d)>. <Condition (a)> The content of aromatic vinyl monomer units in the block copolymer is 10 to 30 mass %. <Condition (b)> The ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units is 90 to 100 mass %. <Condition (c)> The peak top molecular weight of the block aromatic vinyl portion is 10,000 to 30,000. <Condition (d)> The ratio (Mw / Mn) of the weight average molecular weight Mw to the number average molecular weight Mn of the block aromatic vinyl portion is 1.15 to 1.40. [2] The bale molded article according to [1] above, wherein the viscosity of a 5% by mass styrene solution of the block copolymer is 7 to 15 mPa·s at a temperature of 25°C. [3] The veil molded article according to the above [1] or [2], wherein the 1,2-vinyl bond content of the conjugated diene monomer units of the block copolymer is 15 to 30 mol %. [4] The bale molded product according to any one of [1] to [3] above, which has a hardness of 50 to 72 as measured by a hardness tester type E in accordance with JIS K6253. [5] A block copolymer having an aromatic vinyl monomer unit and a conjugated diene monomer unit, The block copolymer has a block aromatic vinyl moiety, A block copolymer that satisfies the following conditions (a) to (d). <Condition (a)> The content of aromatic vinyl monomer units in the block copolymer is 10 to 30 mass %. <Condition (b)> The ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units is 90 to 100 mass %. <Condition (c)> The peak top molecular weight of the block aromatic vinyl portion is 10,000 to 30,000. <Condition (d)> The ratio (Mw / Mn) of the weight average molecular weight Mw to the number average molecular weight Mn of the block aromatic vinyl portion is 1.15 to 1.40. [6] The block copolymer according to [5] above, wherein a 5 mass % styrene solution of the block copolymer has a viscosity of 7 to 15 mPa·s under a temperature condition of 25°C. [7] The block copolymer according to [5] or [6] above, wherein the 1,2-vinyl bond content of the conjugated diene monomer units of the block copolymer is 15 to 30 mol %. [8] 3 to 20 parts by mass of a block copolymer constituting the bale molded body according to any one of [1] to [4] above; 97 to 80 parts by mass of a styrene-based resin; A resin composition which is a polymer of the above. [9] The resin composition according to [8] above, wherein the styrene-based resin is a copolymer of a styrene-based compound and acrylonitrile.

[10] A method for producing a block copolymer constituting the bale molded article according to any one of [1] to [4], comprising the steps of: supplying a conjugated diene compound to a reactor and polymerizing the conjugated diene compound so that the peak temperature is 91 to 100° C.; The method includes a step of supplying an aromatic vinyl compound and polymerizing the compound at a temperature of 90 to 100° C. in the reactor. A method for producing a block copolymer.

[11] 3 to 20 parts by mass of the block copolymer according to any one of [5] to [7] above; 97 to 80 parts by mass of a styrene-based resin; A resin composition which is a polymer of the above.

[12] The resin composition according to

[11] above, wherein the styrene-based resin is a copolymer of a styrene-based compound and acrylonitrile.

[13] A method for producing the block copolymer according to any one of [5] to [7], supplying a conjugated diene compound to a reactor and polymerizing the conjugated diene compound so that the peak temperature is 91 to 100° C.; The method includes a step of supplying an aromatic vinyl compound and polymerizing the compound at a temperature of 90 to 100° C. in the reactor. A method for producing a block copolymer. Effect of the Invention

[0009] According to the present invention, there can be provided a bale molded product made of an aromatic vinyl-conjugated diene block copolymer having appropriate hardness, being easily pulverized and having excellent handleability, a block copolymer constituting the bale molded product, and a resin composition which is a polymer of the block copolymer and a styrene-based resin and has excellent gloss and impact resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. It should be noted that the following embodiment is merely an example for explaining the present invention, and the present invention is not limited to the embodiment described below. The present invention can be carried out in various modified forms within the scope of the gist thereof.

[0011] [Bale Molded Body and Block Copolymer] The veil molded article of this embodiment is a veil molded article of the block copolymer of this embodiment having conjugated diene monomer units and aromatic vinyl monomer units. In this specification, a monomer that has become a constituent element of a block copolymer is referred to as a "monomer unit," and a monomer before being incorporated into a polymer is referred to as a "compound." The block copolymer of this embodiment constituting the bale molded article of this embodiment has a block aromatic vinyl portion and satisfies the following <Condition (a)> to <Condition (d)>. <Condition (a)> The content of aromatic vinyl monomer units in the block copolymer is 10 to 30 mass %. <Condition (b)> The ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units is 90 to 100 mass %. <Condition (c)> The peak top molecular weight of the block aromatic vinyl portion is 10,000 to 30,000. <Condition (d)> The ratio (Mw / Mn) of the weight average molecular weight Mw to the number average molecular weight Mn of the block aromatic vinyl portion is 1.15 to 1.40.

[0012] Since the bale molded article and block copolymer of this embodiment have the above-mentioned configuration, a bale molded article having appropriate hardness, being easy to crush, and having excellent handleability can be obtained.

[0013] In this specification, monomers used to prepare polymers are referred to as "compounds" and polymer components are referred to as "monomer units." Conjugated diene compounds forming the conjugated diene monomer units in the block copolymer include, but are not limited to, 1,3-butadiene, 2-methyl-1,3-butadiene (i.e., isoprene), 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, etc. Among these, 1,3-butadiene and 2-methyl-1,3-butadiene are preferred, and 1,3-butadiene is particularly preferred. These conjugated diene compounds may be used alone or in combination of two or more.

[0014] The aromatic vinyl compound forming the aromatic vinyl monomer unit in the block copolymer is not limited to the following, but examples thereof include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-diisopropylstyrene, 2,4-dimethylstyrene, 4-t-butylstyrene, 5-t-butyl-2-methylstyrene, monochlorostyrene, dichlorostyrene, monofluorostyrene, etc. Among these, styrene is preferred. Each of these aromatic vinyl compounds may be used alone or in combination of two or more.

[0015] (<Condition (a)> Content of aromatic vinyl monomer units in block copolymer) The block copolymer constituting the bale molded product of this embodiment and the content of aromatic vinyl monomer units in the block copolymer of this embodiment are 10 to 30 mass%, preferably 14 to 26 mass%, and more preferably 17 to 23 mass%. The content of the conjugated diene monomer unit in the block copolymer is from 70 to 90% by mass, preferably from 74 to 86% by mass, and more preferably from 77 to 83% by mass. When the content of aromatic vinyl monomer units in the block copolymer is 10% by mass or more, the necessary hardness of the bale molded body is ensured and it tends to be difficult to deform under load. In addition, when used as a toughening agent for aromatic vinyl resins, it tends to have an improved rigidity. When the content of aromatic vinyl monomer units is 30% by mass or less, the hardness of the bale molded body is not too high, and good crushability and solubility of the bale molded body tend to be obtained, and impact resistance can be ensured when used as a toughening agent for aromatic vinyl resins. In this specification, the term "hardness of the veil molded body" refers to the hardness of the veil molded body molded without adding oil to the block copolymer. In this embodiment, the hardness of the veil molded body in a so-called non-oil-extended state is controlled by the structure of the block copolymer, thereby improving the handleability of the veil molded body, preventing unintended oil from being included in the application in which the veil molded body is used, and improving the design freedom of the resin composition. The content of the aromatic vinyl monomer unit in the block copolymer can be controlled within the above-mentioned numerical range by adjusting the amount of the aromatic vinyl compound added and the polymerization time in the polymerization step.

[0016] (<Condition (b)> Ratio of block aromatic vinyl moieties to the total content of aromatic vinyl monomer units in the block copolymer) The block copolymer constituting the bale molded product of this embodiment and the ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units in the block copolymer of this embodiment are in the range of 90 to 100 mass%, preferably 93 to 100 mass%, and more preferably 95 to 99.9 mass%. Here, the term "block aromatic vinyl portion" refers to a block portion in which 10 or more aromatic vinyl monomer units are bonded together. When the ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units in the block copolymer is 90 mass% or more, the solubility of the bale molded body in styrene, styrene / acrylonitrile, styrene / methacrylic acid ester, etc. after crushing tends to be good, and the impact resistance also tends to be improved when used as a toughening agent for aromatic vinyl resins. The ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units in the block copolymer can be controlled within the above numerical range by adjusting the timing of addition of the aromatic vinyl compound in the polymerization step.

[0017] (<Condition (c)> Peak top molecular weight of block aromatic vinyl part) In the bale molded article of this embodiment and the block copolymer constituting the block copolymer of this embodiment, the block aromatic vinyl portion constituting the block copolymer has a peak top molecular weight of 10,000 to 30,000. Specifically, the block copolymer is decomposed with ozonolysis, and the peak top molecular weight in the molecular weight distribution curve of the block aromatic vinyl portion is in the range of 10,000 to 30,000, preferably 11,000 to 27,000, and more preferably 12,000 to 25,000, in terms of standard monodisperse polystyrene, as measured by gel permeation chromatography (hereinafter also referred to as "GPC"). When the peak top molecular weight of the block aromatic vinyl moiety is 10,000 or more, the bale molded body of the present embodiment has the necessary hardness, and when the bale molded bodies are stacked, deformation of the bale molded body due to load tends not to occur. When the peak top molecular weight of the molecular weight distribution curve of the block aromatic vinyl moiety is 30,000 or less, the hardness of the bale molded body of the present embodiment does not become too high, the handleability is good, and the load increase during crushing tends to be prevented. In addition, when the peak top molecular weight of the block aromatic vinyl moiety is in the range of 10,000 to 30,000, the balance of impact resistance and gloss tends to be good when used as a toughening agent for aromatic vinyl resins. The peak top molecular weight of the aromatic vinyl portion can be controlled within the above numerical range by adjusting the amount of the polymerization initiator added and the amount of the aromatic vinyl compound added in the polymerization step.

[0018] (<Condition (d)> Ratio of weight average molecular weight Mw to number average molecular weight Mn of block aromatic vinyl portion) The block copolymer constituting the bale molded article of this embodiment and the ratio of the weight average molecular weight to the number average molecular weight (Mw / Mn) (hereinafter referred to as molecular weight distribution) of the block copolymer of this embodiment are 1.15 to 1.40. Specifically, when the block copolymer is decomposed by ozonolysis and the molecular weight of the block aromatic vinyl portion is measured, the molecular weight distribution (Mw / Mn) is in the range of 1.15 to 1.40. From the viewpoint of adjusting the hardness of the bale molded product of this embodiment, the range is preferably 1.15 to 1.35, more preferably 1.15 to 1.30, even more preferably 1.15 to 1.25, still more preferably 1.18 to 1.35, still more preferably 1.18 to 1.30, and particularly preferably 1.20 to 1.30. By setting the molecular weight distribution of the block aromatic vinyl moiety within the above range, the hardness of the bale molded product tends to be controlled to a practically favorable value. Here, the hardness of the bale molded product is the hardness measured by a hardness tester type E in accordance with JIS K 6253, and specifically, it can be measured by the method described in the examples below. When the molecular weight distribution (Mw / Mn) of the block aromatic vinyl portion is 1.15 or more, the hardness of the bale molded body can be easily adjusted to 72 or less, which tends to prevent the bale molded body from falling due to the claws of a robot or the like digging into the bale molded body when it is pinched and moved.When the molecular weight distribution (Mw / Mn) of the block aromatic vinyl portion is 1.40 or less, the hardness of the bale molded body can easily be 50 or more, which tends to prevent deformation of the bale molded body due to load when stacked. The molecular weight distribution of the block aromatic vinyl portion can be controlled within the above-mentioned range by adjusting the temperature in the reactor when the aromatic vinyl compound is added in the polymerization step.

[0019] The hardness of the bale molded body of the block copolymer of the present embodiment described above, that is, the hardness measured by a hardness tester type E according to JIS K 6253, is preferably in the range of 50 to 72, more preferably 53 to 70, and even more preferably 55 to 68. When the hardness of the bale molded body is 50 or more, when a plurality of bale molded bodies are stacked, the deformation of the lower bale molded body due to the load tends to be prevented. When the hardness of the bale molded body is 72 or less, the handleability of the bale molded body by the robot arm can be ensured, and the load is not high when the bale molded body is crushed, and the bale molded body can be continuously fed into the crusher without leaving an interval, and good crushing efficiency tends to be ensured. The hardness of the bale molded product of the block copolymer can be controlled within the above-mentioned numerical range by adjusting the molecular weight distribution (Mw / Mn) of the block aromatic vinyl portion constituting the block copolymer. Specifically, the hardness of the bale molded product can be controlled to 72 or less by adjusting the molecular weight distribution (Mw / Mn) to 1.15 or more, and the hardness of the bale molded product can be controlled to 50 or more by adjusting the molecular weight distribution (Mw / Mn) to 1.40 or less. The molecular weight distribution of the block aromatic vinyl portion can be controlled within the above-mentioned range by adjusting the temperature in the reactor when the aromatic vinyl compound is added in the polymerization step.

[0020] In the block copolymer constituting the bale molded article of the present embodiment and in the block copolymer of the present embodiment, it is preferable that the block aromatic vinyl portion is located at the end of the block copolymer, which tends to improve the solubility in styrene, styrene / acrylonitrile, styrene / methacrylic acid ester, etc., when the bale molded article is dissolved in these after being crushed.

[0021] In addition, in the block copolymer constituting the bale molded product of the present embodiment and in the block copolymer of the present embodiment, the viscosity of a 5 mass % styrene solution of the block copolymer at a temperature condition of 25°C is preferably 7 to 15 mPa s, more preferably 8 to 13 mPa s, and even more preferably 9 to 12 mPa s. When the block copolymer has a 5 mass % styrene solution viscosity of 7 mPa s or more, it tends to improve impact resistance when used as a toughening agent for aromatic vinyl resins. In addition, because the viscosity of a 5 mass % styrene solution of the block copolymer is 15 mPa s or less, when used as a toughening agent for aromatic vinyl resin, it tends to facilitate the sufficient reduction in the particle size of the rubber particles in the aromatic vinyl resin, making it easier to achieve a good balance between impact resistance, gloss, and rigidity. The viscosity of a 5% by mass styrene solution of the block copolymer can be controlled within the above numerical range by adjusting the peak top molecular weight of the block copolymer.

[0022] The block copolymer constituting the veil molded body of this embodiment and the block copolymer of this embodiment preferably have a 1,2-vinyl bond content of the conjugated diene monomer unit of 15 to 30 mol%, more preferably 16 to 28%, and even more preferably 17 to 25%. When the 1,2-vinyl bond content is 30 mol% or less, when the veil molded body of this embodiment and the block copolymer of this embodiment are used as a toughening agent for an impact-resistant aromatic vinyl resin, the graft amount is easily controlled within an appropriate range so that the shape of the rubber particles in the impact-resistant aromatic vinyl resin becomes salami particles, and the particle size tends to be easily controlled. In addition, when the 1,2-vinyl bond content is 15 mol% or more, when the veil molded body of this embodiment and the block copolymer of this embodiment are used as a toughening agent for an impact-resistant aromatic vinyl resin, the rubber particles in the acrylonitrile-styrene resin (ABS) tend to be easily reduced in size, and the impact resistance of the resin composition, which is a polymer of such an impact-resistant aromatic vinyl resin and the block copolymer of this embodiment, tends to be easily improved. The amount of 1,2-vinyl bonds in the block copolymer can be controlled within the above numerical range by adjusting the amount of polar substance added and the polymerization reaction temperature in the polymerization step.

[0023] The block copolymer constituting the bale molded product of this embodiment and the block copolymer of this embodiment have an aromatic vinyl monomer unit content of 10 to 30 mass%, a ratio of the block aromatic vinyl moiety to the total content of the aromatic vinyl monomer units of 90 to 100 mass%, a peak top molecular weight of the block aromatic vinyl moiety of 10,000 to 30,000, and a molecular weight distribution (Mw / Mn) of 1.15 to 1.40. A block copolymer having this structure can be obtained by adjusting the amount of catalyst added, supplying a conjugated diene compound to a reactor, polymerizing the conjugated diene compound so that the peak temperature is 91 to 100°C, and then supplying an aromatic vinyl compound at a reactor temperature of 90 to 100°C and polymerizing the same. Preferably, the aromatic vinyl compound is supplied when the temperature inside the reactor is 91 to 99° C., and more preferably, the aromatic vinyl compound is supplied when the temperature inside the reactor is 92 to 98° C., and polymerization is carried out. When the temperature inside the reactor is less than 90° C., the molecular weight distribution (Mw / Mn) of the block aromatic vinyl portion tends to be lower than 1.15. When the temperature inside the reactor exceeds 100° C., the molecular weight distribution of the block aromatic vinyl portion becomes broad and may have two peaks, and the molecular weight distribution (Mw / Mn) tends to be more variable.

[0024] (Method of Producing Block Copolymer) The block copolymer constituting the bale molded article of this embodiment has an aromatic vinyl monomer unit and a conjugated diene monomer unit, and further has a block aromatic vinyl portion. The block copolymer can be produced, for example, by using an organolithium compound as a polymerization initiator and carrying out polymerization in a hydrocarbon solvent.

[0025] The organic lithium compound is not particularly limited, but may be a compound having one or more lithium atoms bonded in the molecule. It is not limited to the following, but may be, for example, ethyl lithium, n-propyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, hexamethylene lithium, butadienyl dilithium, isoprenyl dilithium, etc. These may be used alone or in combination of two or more.

[0026] Examples of the hydrocarbon solvent used in the production of the block copolymer include, but are not limited to, aliphatic hydrocarbons such as butane, pentane, hexane, isopentane, heptane, octane, and isooctane; alicyclic hydrocarbons such as cyclopentane, methylcyclopentane, cyclohexane, methylcyclohexane, and ethylcyclohexane; and aromatic hydrocarbons such as benzene, toluene, ethylbenzene, and xylene. These may be used alone or in combination of two or more.

[0027] Examples of a method for adjusting the amount of 1,2-vinyl bonds in the conjugated diene monomer units of the block copolymer include a method of adding a polar substance such as dimethyl ether, diethyl ether, diphenyl ether, tetrahydrofuran, diethylene glycol dimethyl ether, diethylene glycol dibutyl ether, trimethylamine, triethylamine, tetramethylethylenediamine, triphenylphosphine, or hexamethylphosphoramide to a polymerization system containing an organolithium compound as a polymerization initiator. These may be used alone or in combination of two or more.

[0028] Specifically, in a polymerization system containing an organolithium compound and a polar substance, it is preferable to supply a conjugated diene compound to a reactor, polymerize the conjugated diene compound so that the peak temperature is 91 to 100°C, and then supply an aromatic vinyl compound at a temperature in the reactor of 90 to 100°C and polymerize the compound. Although the polymerization time becomes longer, the molecular weight distribution (Mw / Mn) of the block aromatic vinyl moiety can be controlled within the range of 1.15 to 1.40 by extending the addition time of the aromatic vinyl compound or by adding the aromatic vinyl compound in portions. More preferably, a method is used in which a conjugated diene compound is supplied to a reactor, the conjugated diene compound is polymerized so that the peak temperature is 91 to 100°C, and then an aromatic vinyl compound is supplied at a temperature in the reactor of 90 to 100°C, and polymerized to obtain a block copolymer, and this method has the best polymerization rate and is efficient. Furthermore, the polymerization system is preferably made to have an inert gas atmosphere such as nitrogen gas. The polymerization pressure is not particularly limited as long as it is within a pressure range sufficient to maintain the monomer and the solvent in a liquid phase within the above-mentioned polymerization temperature range.

[0029] (Additives) The block copolymer of the present embodiment described above may be terminated with water, an alcohol, an organic acid, or the like in a solution of the block copolymer, and then various stabilizers such as phenol-based stabilizers, phosphorus-based stabilizers, sulfur-based stabilizers, and amine-based stabilizers, or other known additives may be added.

[0030] In addition, the block copolymer of this embodiment can be separated from the solution by removing the catalyst residue as necessary, for example, as described in Japanese Patent No. 6646437. Separation from the solvent can be performed by pouring the solution of the block copolymer into hot water under stirring and removing the solvent by steam stripping. After a solvent removal step such as steam stripping, the block copolymer is extruded using an extruder, and then dried with hot air or vacuum to obtain a crumb-like block copolymer, which can be molded into a bale molded body using a bale molding machine. The bale molded article of the present embodiment produced as described above can be adjusted to a hardness that is excellent in handleability, has excellent robotic handleability and crushability, and can reduce the particle size of rubber particles in aromatic vinyl resins such as ABS, thereby obtaining a resin composition with excellent gloss and impact resistance. That is, the block copolymer of the present embodiment can be used as a resin modifier (toughener) that can improve gloss and impact resistance.

[0031] [Resin composition] The resin composition of this embodiment is a polymer of 3 to 20 parts by mass of the block copolymer constituting the bale molded article of this embodiment or the block copolymer of this embodiment and 97 to 80 parts by mass of a styrene-based resin. As the styrene-based resin, a styrene-based compound used in the production of a resin composition can be used. The styrene-based compound includes any of the states of a polymer, a monomer, and an oligomer. Examples of the styrene-based compound include, but are not limited to, at least one of styrene and its derivatives, such as styrene, α-methylstyrene, vinyltoluene, and chlorostyrene. Among these, styrene is preferred. These styrene-based compounds can be used alone or in combination of two or more kinds. The styrene-based compound may be a homopolymer of the compound, or a copolymer of styrene and another compound copolymerizable therewith. Examples of compounds copolymerizable with styrene-based compounds include unsaturated nitrile compounds such as acrylonitrile and methacrylonitrile, acrylic acid esters such as methyl acrylate, and methacrylic acid esters such as methyl methacrylate, and other vinyl monomers, with acrylonitrile being particularly preferred. The content of the block copolymer of the present embodiment in the resin composition of the present embodiment is preferably from 5 to 18 parts by mass, and more preferably from 8 to 15 parts by mass. The content of the styrene-based resin is preferably from 95 to 82 parts by mass, and more preferably from 92 to 85 parts by mass. The resin composition of the present embodiment can be produced by polymerizing a styrene-based resin and a block copolymer, or by mixing a monomer of the styrene-based resin and a block copolymer and polymerizing the mixture. Specifically, the resin composition can be produced by the method described in the examples below. EXAMPLES

[0032] Hereinafter, the present embodiment will be described in more detail with reference to specific examples and comparative examples, but the present invention is not limited to the following examples and comparative examples. Measurement of physical properties and evaluation of characteristics in the examples and comparative examples were carried out as follows.

[0033] ((1) Content of aromatic vinyl monomer units in block copolymer) The content of the aromatic vinyl monomer unit in the block copolymer was obtained by using the block copolymer as a specimen, preparing a chloroform solution as a sample, and measuring the content of the aromatic vinyl monomer unit (mass%) by the UV254 nm absorption by the phenyl group of the aromatic vinyl using a measuring device (JASCO: V-550).

[0034] ((2) Ratio of the content of block aromatic vinyl moieties to the total content of aromatic vinyl monomer units in the block copolymer) The content of the block aromatic vinyl moiety relative to the total content of aromatic vinyl monomer units in the block copolymer was measured according to the osmic acid decomposition method described in LM Kolthoff, et al., J. Polym. Sci., 1, 429 (1948). Specifically, 0.05 g of the block copolymer was dissolved in 10 mL of chloroform, 16 mL of a 69% aqueous solution of tert-butyl hydroperoxide and 4 mL of a 0.05% chloroform solution of osmium tetroxide were added, and the mixture was refluxed in a 90°C bath for 12 minutes to carry out an oxidative decomposition reaction. After the reaction was completed, the reaction solution was cooled, and 200 mL of methanol was added to the reaction solution under stirring to precipitate the block aromatic vinyl moiety component, which was then filtered through a 5 μm glass filter to measure the content of the block aromatic vinyl moiety in the block copolymer. Next, the ratio of the block aromatic vinyl moiety to the total content of aromatic vinyl monomer units in the block copolymer, which is the value measured by (1) above, was calculated.

[0035] ((3) Peak top molecular weight of block copolymer) The peak top molecular weight of the block copolymer was measured by gel permeation chromatography (hereinafter, also referred to as "GPC"). Chromatography was performed using GPC (the apparatus was a Tosoh HLC-8320GPC EcoSEC, the columns were three PL Gel Chromn MiniMIX-C 4.6 mmΦ×300 mm columns, and the solvent was tetrahydrofuran. The measurement conditions were a column temperature of 40° C., a flow rate of 0.4 mL / min, a sample concentration of 0.1 mass%, and an injection volume of 50 μL). The peak top molecular weight was determined from the obtained GPC chromatogram using a calibration curve prepared using commercially available standard monodisperse polystyrene with known molecular weight. GPC: HLC-8320GPC EcoSEC (Tosoh Corporation) Detector: RI Column: PL Gel Column 5μm MiniMIX-C 4.6mmΦ×300mm 3 pieces Solvent: Tetrahydrofuran Flow rate: 0.4mL / min Concentration: 0.1% by mass Column temperature: 40℃ Injection volume: 50μL

[0036] ((4) Peak top molecular weight and molecular weight distribution (Mw / Mn) of the block aromatic vinyl portion in the block copolymer) A solution of 0.1 g of the block copolymer in 100 mL of dichloromethane was oxidatively decomposed by passing oxygen containing 1.5% ozone at 150 mL / min. The resulting ozonide was reduced by dropping it into diethyl ether mixed with lithium aluminum hydride. Next, pure water was added dropwise to hydrolyze the mixture, and potassium carbonate was added to salt out and then filtered to obtain a component of the blocked aromatic vinyl moiety. The blocked aromatic vinyl moiety was measured by GPC. The chromatograph was measured by GPC (the apparatus was a Tosoh HLC-8320GPC EcoSEC, the columns were Shodex KF-803L and KF-801, the solvent was tetrahydrofuran, and the measurement conditions were a column temperature of 40°C, a flow rate of 0.8 mL / min, a sample concentration of 0.1 mass%, and an injection amount of 50 μL) to obtain the peak top molecular weight. Using a calibration curve prepared using commercially available standard monodisperse polystyrene with known molecular weights, the weight average molecular weight Mw and number average molecular weight Mn were obtained from the obtained GPC chromatogram, and the molecular weight distribution (Mw / Mn) was calculated. GPC: HLC-8320GPC EcoSEC (Tosoh Corporation) Detector: UV Columns: Shodex K-803L, K801, K801 x 3 Solvent: Tetrahydrofuran Flow rate: 0.8mL / min Concentration: 0.1% by mass Column temperature: 40℃ Injection volume: 50μL

[0037] ((5) Amount of 1,2-vinyl bonds in conjugated diene monomer units in block copolymers) The amount of 1,2-vinyl bonds in the conjugated diene monomer units was determined by infrared spectroscopy (Hampton, Anal. Chem., 21, 923 (1941)).

[0038] ((6) Viscosity of 5% by mass styrene solution of block copolymer at 25°C) The viscosity of a styrene solution containing 5% by mass of the block copolymer at a temperature of 25°C was measured by dissolving 5 g of the block copolymer in 95 g of styrene at a measurement temperature of 25°C using a Cannon-Fenske type viscometer (manufactured by Kusano Scientific Instruments Manufacturing Co., Ltd., product name: Cannon-Fenske No. 200).

[0039] (7) Hardness of veiled block copolymers 35 kg of block copolymer crumbs were placed in a bale-forming mold (length 70 cm, width 35 cm) and compressed under a compression pressure of 200 kg / cm 2 The bale was molded under the conditions of compression time: 50 seconds and compression temperature: 60°C. The hardness of the obtained bale was measured using a JIS K 6253 hardness tester type E manufactured by Asker Corporation, and the maximum value was recorded when the hardness tester was pressed against the smooth part. The bale was turned over and five smooth areas were measured, and the average value was taken as the hardness of the bale.

[0040] ((8) Peak current during crushing of block copolymer bales) 35 kg of block copolymer bales were fed vertically into a leat cutter (Hosokawa Micron Corporation, leat rubber chopper, model PB15H), and then the power to the leat cutter was turned on to rotate the screw. The peak current value when the entire bale was vertically bitten into the rotating screw in the leat cutter was measured and used as an index of the load during crushing of the bale. In addition, when the bale cutting tool is turned on, there are cases where the current value momentarily exceeds the upper limit when the bale starts to be cut, but this is only for an instant and is not considered to be the peak current value.

[0041] ((9) Crushing time of baled block copolymer bodies) 35 kg of bale molded bodies were fed vertically into the leat cutter, and the bale molded bodies were sheared between the screw-type hammer and the fixed blade, and the crushed products pushed out of the orifice plate by the movement of the screw were further cut by the cut-off knife. The time from the start of feeding the bale molded bodies to the return of the current value before the next bale molded body was fed, when the crushed products no longer came out of the orifice plate, was defined as the crushing time per bale. The current value of the leat cutter when no bale molded bodies were fed was 19 amperes.

[0042] [Polymerization of block copolymer and preparation of veil molded body] [Example 1] (Polymerization of block copolymer (SBR1) and veil molding) A polymerization tank with a capacity of 100 liters and equipped with a rotating stirring blade and a jacket was used, and 79 parts by mass of 1,3-butadiene containing 100 ppm of 1,2-butadiene and 600 parts by mass of a cyclohexane solution containing 150 ppm of tetrahydrofuran (THF) were charged into the polymerization tank, 0.016 parts by mass of tetramethylethylenediamine (TMEDA) was added as a regulator of the amount of 1,2-vinyl bonds, and polymerization was carried out under stirring at a polymerization initiation temperature of 43.2 ° C. by adding 0.095 parts by mass of polymerization initiator n-butyllithium. The reaction peak temperature of 1,3-butadiene was 96.1 ° C. One minute after the reaction peak temperature was reached, 21 parts by mass of styrene was added. The temperature inside the reactor at the time of the addition of styrene was 95.2 ° C. Next, 5 minutes after the styrene reaction peak temperature was reached, methanol was added at 0.8 times the molar amount of the polymerization initiator n-butyllithium to deactivate the initiator, thereby completing the polymerization reaction of the block copolymer (SBR1). Thereafter, 2,4-bis(octylthiomethyl)-o-cresol was added as a stabilizer in an amount of 0.15% by mass relative to the mass of the block copolymer. Similarly, polymerization was carried out four times, and after inactivation with methanol, a stabilizer was added, and the block copolymer rubber solutions obtained in the four polymerizations were blended. The resulting block copolymer rubber solution was then dropped into boiling water with stirring, and the solvent was removed by steam stripping using pure water, followed by vacuum drying to obtain a crumb-like block copolymer. 35 kg of the obtained crumbs were put into a bale-forming machine (bale-forming mold: length 70 cm, width 35 cm) to produce a bale of block copolymer (SBR1). Table 1 shows the polymerization details of the block copolymer (SBR1), the physical properties of the block copolymer, the results of hardness adjustment of the bale molded body, and the crushability of the bale molded body.

[0043] [Examples 2 and 3 and Comparative Examples 1, 2, and 3] In the same manner as in Example 1, except that the polymerization initiation temperature, the reaction peak temperature of 1,3-butadiene, and the temperature inside the reactor when styrene was added were changed, bale molded bodies of block copolymers (SBR2, SBR3, SBR13, SBR14, SBR15) were obtained under the polymerization conditions shown in Tables 1 and 3. The polymerization details of the block copolymers (SBR2, SBR3, and SBR13, SBR14, and SBR15) of Examples 2 and 3 and Comparative Examples 1, 2, and 3, the physical properties of the block copolymers, the results of hardness adjustment of the bale molded bodies, and the crushability of the bale molded bodies are shown in Tables 1 and 3. It was found that SBR15 in Comparative Example 3 had a slightly larger amount of ground product adhering to the inside of the leat cutter after bale crushing, compared to SBR2 and SBR3 in the Examples and SBR13 and SBR14 in the Comparative Examples.

[0044] [Example 4 and Comparative Example 4] Using the same method as in Example 1, the amount of tetramethylethylenediamine (TMEDA), an adjuster for the amount of 1,2-vinyl bonds, added was increased to obtain bale molded bodies of block copolymers SBR4 and SBR16. Tables 1 and 3 show the polymerization details of the block copolymers SBR4 and SBR16 in Example 4 and Comparative Example 4, the physical properties of the block copolymers, the results of hardness adjustment of the bale molded bodies, and the crushability of the bale molded bodies.

[0045] [Examples 5 and 6 and Comparative Example 5] Bale molded products of block copolymer (SBR5) with aromatic vinyl monomer unit content of 16.2 mass%, block copolymer (SBR6) with aromatic vinyl monomer unit content of 24.8 mass%, and block copolymer (SBR17) with aromatic vinyl monomer unit content of 34.8 mass% were obtained under the polymerization conditions shown in Tables 1 and 3. As Example 5, Example 6, and Comparative Example 5, the physical properties of the block copolymers, the hardness adjustment results of the bale molded products, and the crushability of the bale molded products are shown in Tables 1 and 3. In Comparative Example 5 (SBR17), the hardness of the bale molded body was high at 78, and therefore the peak current during crushing was 47 A, which was a large load on the crusher.

[0046] [Examples 7 and 8 and Comparative Example 6] Polymerization was carried out under the polymerization conditions shown in Tables 2 and 3, and styrene was added when the 1,3-butadiene reaction exceeded 90° C. and before the reaction peak. Styrene was added at 90.3° C. in Example 7 (SBR7), 95.2° C. in Example 8 (SBR8), and 92.0° C. in Comparative Example 6 (SBR18). As a result, the ratios of the content of the block aromatic vinyl moiety to the content of the aromatic vinyl monomer unit were 90.8 mass%, 90.5 mass%, and 91.4 mass%, respectively. In addition, in Comparative Example 6 (SBR18), the amount of catalyst added was reduced to increase the molecular weight, and as a result, the peak top molecular weight of the block aromatic vinyl portion exceeded 30,000, and the hardness of the bale molding exceeded 80, which increased the load during crushing and deteriorated the crushability.

[0047] [Comparative Example 7] Polymerization was carried out under the polymerization conditions shown in Table 3. Before the start of polymerization, 6.3 parts by mass of styrene was charged into a polymerization tank together with 79 parts by mass of 1,3-butadiene, and the remaining 14.7 parts by mass of styrene was added after the 1,3-butadiene reaction peak temperature was reached. As a result, a block copolymer (SBR19) was obtained in which the ratio of the content of block aromatic vinyl moieties to the content of aromatic vinyl monomer units was 73.1% by mass. The bale hardness was low at 42, and the load during bale crushing was small, but adhesion to the inside of the crusher due to heat generation during crushing was confirmed, as in Comparative Example 3 (SBR15). In addition, it was found that the bale molded bodies were easily deformed when stacked because the hardness of the bale molded bodies was low.

[0048] [Example 9] Using the same method as in Example 1, a bale molded product of a block copolymer (SBR9) was obtained in which the amount of n-BuLi added as a polymerization initiator was increased. By increasing the amount of the polymerization initiator, the peak top molecular weight of the block copolymer was lower than that of Example 1, and the veil hardness was 49. Table 2 shows the polymerization details of the block copolymer (SBR9), the physical properties of the block copolymer, the results of hardness adjustment of the bale molded body, and the crushability of the bale molded body.

[0049] [Example 10] Using the same method as in Example 1, a bale molded product of a block copolymer (SBR10) was obtained in which the amount of n-BuLi added as a polymerization initiator was reduced. By reducing the amount of the polymerization initiator, the peak top molecular weight of the block copolymer was higher than that of Example 1, and the veil hardness was 69. Table 2 shows the polymerization details of the block copolymer (SBR10), the physical properties of the block copolymer, the results of hardness adjustment of the bale molded body, and the crushability of the bale molded body.

[0050] [Example 11] A bale molded product of a block copolymer (SBR11) with a 1,2-vinyl bond content of 13.3 mass% was obtained by increasing the amount of tetrahydrofuran (THF) added without adding tetramethylethylenediamine (TMEDA), which is an adjuster of the 1,2-vinyl bond content, in the same manner as in Example 1. The polymerization contents of the block copolymer (SBR11), the physical properties of the block copolymer, the hardness adjustment results of the bale molded product, and the crushability of the bale molded product are shown in Table 2.

[0051] [Example 12] Using the same method as in Example 1, the amount of tetramethylethylenediamine (TMEDA), an agent for adjusting the amount of 1,2-vinyl bonds, was increased to obtain a bale molded product of a block copolymer (SBR12) having a 1,2-vinyl bond content of 31.2%. Table 2 shows the polymerization details of the block copolymer (SBR12), the properties of the block copolymer, the results of hardness adjustment of the bale compact, and the crushability of the bale compact.

[0052] [Table 1]

[0053] [Table 2]

[0054] [Table 3]

[0055] From Tables 1 to 3, it was found that the block copolymers SBR1 to 12 (Examples 1 to 12) were capable of adjusting the hardness of the bale molded body to an optimum level for crushing the bale molded body, had a low load (current value) during crushing, could be fed continuously, and had a short crushing time per bale molded body, which was favorable.

[0056] [Characteristics of impact-resistant aromatic vinyl resin composition] As shown in [Examples 13 to 19] and [Comparative Examples 8 and 9] described later, impact-resistant aromatic vinyl resin compositions were prepared, and the following properties were measured and evaluated.

[0057] <Average rubber particle size> An impact-resistant aromatic vinyl resin composition was dissolved in dimethylformamide to dissolve only the polystyrene resin portion forming the matrix in the resin composition. A part of the solution was dispersed in a dimethylformamide solvent in a measurement cell using a particle size distribution (laser diffraction / scattering type) measurement device, LA-920 model, manufactured by Horiba, Ltd., and measured. The volume average particle size obtained was taken as the rubber particle size.

[0058] <Glossiness> The gloss was measured in accordance with JIS Z8742 (incident angle 60°).

[0059] <Impact resistance> The Izod impact strength was measured according to JIS K7110 (notched).

[0060] [Examples 13 to 19] In a nitrogen-purged stirred polymerization vessel, 20 parts by mass of ethylbenzene and 12 parts by mass of a block copolymer (listed in Table 4) were dissolved in 100 parts by mass of a monomer mixture containing 75% by mass of styrene and 25% by mass of acrylonitrile. 0.15 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate and 200 ppm by mass of 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexyl per 100 parts by mass of the monomer mixture were added. The polymerization was continued by successively increasing the temperature to 120°C for 1 hour, 135°C for 2 hours, 150°C for 2 hours, and 170°C for 2 hours, with stirring at 15 rpm. Finally, a heat treatment was carried out at 230°C for 30 minutes. After that, the pressure inside the polymerization tank was returned to atmospheric pressure, and the impact-resistant aromatic vinyl resin composition, which was the polymerized product during heating, was taken out and cooled in pure water. In order to remove unreacted styrene, acrylonitrile and ethylbenzene, 1000 ml of dichloromethane was added per 100 g of the cooled polymer, and the mixture was stirred and dissolved. The solution was dropped into 10 times the amount of isopropyl alcohol to cause reprecipitation. The reprecipitated impact-resistant aromatic vinyl resin composition was dried in a vacuum to obtain an impact-resistant aromatic vinyl resin composition (ABS resin composition). This was hot pressed at 200° C., cooled and then crushed to a size of 5 mmφ, and the crushed product was injection molded to measure the physical properties of the ABS resin composition. The measurement results are shown in Table 4.

[0061] [Comparative Example 8 and Comparative Example 9] ABS test pieces were prepared in the same manner as in Example 13, except that SBR14 and SBR15 were used as block copolymers. The physical property measurement results are shown in Table 4.

[0062] [Table 4]

[0063] As shown in Table 4, a comparison of the physical properties of ABS resin compositions using block copolymers SBR having different molecular weight distributions (Mw / Mn) of the block aromatic vinyl portion of the block copolymer was made. As a result, it was found that the physical properties of the ABS resin compositions of SBR1 having Mw / Mn = 1.20 in Example 13 and SBR14 having Mw / Mn = 1.07 in Comparative Example 8 were equivalent and good, but the impact resistance of ABS was inferior in SBR15 having Mw / Mn = 1.41 in Comparative Example 9. [Industrial Applicability]

[0064] The bale molded product of the block copolymer of the present embodiment has industrial applicability as a modifier for styrene-based resins.

Claims

1. A veil molded article of a block copolymer having an aromatic vinyl monomer unit and a conjugated diene monomer unit, The block copolymer has a block aromatic vinyl moiety, A veil molded body that satisfies the following conditions (a) to (d). <Condition (a)> The content of aromatic vinyl monomer units in the block copolymer is 10 to 30% by mass. <Condition (b)> The ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units is 90 to 100% by mass. <Condition (c)> The peak top molecular weight of the block aromatic vinyl portion is 10,000 to 30,000. <Condition (d)> The ratio of the weight average molecular weight Mw to the number average molecular weight Mn (Mw / Mn) of the block aromatic vinyl portion is 1.15 to 1.

40.

2. The viscosity of a 5% by mass styrene solution of the block copolymer is 7 to 15 mPa s under a temperature condition of 25°C. The bale molded body according to claim 1.

3. The 1,2-vinyl bond content of the conjugated diene monomer unit of the block copolymer is 15 to 30 mol %. The bale molded body according to claim 1.

4. The hardness measured by a hardness tester type E according to JIS K6253 is 50 to 72. The bale molded body according to claim 1.

5. A block copolymer having an aromatic vinyl monomer unit and a conjugated diene monomer unit, The block copolymer has a block aromatic vinyl moiety, A block copolymer satisfying the following conditions (a) to (d): <Condition (a)> The content of aromatic vinyl monomer units in the block copolymer is 10 to 30% by mass. <Condition (b)> The ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units is 90 to 100% by mass. <Condition (c)> The peak top molecular weight of the block aromatic vinyl portion is 10,000 to 30,000. <Condition (d)> The ratio of the weight average molecular weight Mw to the number average molecular weight Mn (Mw / Mn) of the block aromatic vinyl portion is 1.15 to 1.

40.

6. The viscosity of a 5% by mass styrene solution of the block copolymer is 7 to 15 mPa s under a temperature condition of 25°C. The block copolymer according to claim 5 .

7. The 1,2-vinyl bond content of the conjugated diene monomer unit of the block copolymer is 15 to 30 mol %. The block copolymer according to claim 5 .

8. 3 to 20 parts by mass of a block copolymer constituting the bale molded body according to any one of claims 1 to 4; 97 to 80 parts by mass of a styrene-based resin; A resin composition which is a polymer of the above.

9. The styrene-based resin is a copolymer of a styrene-based compound and acrylonitrile. The resin composition according to claim 8.

10. A method for producing a block copolymer constituting the bale molded article according to any one of claims 1 to 4, comprising the steps of: supplying a conjugated diene compound to a reactor and polymerizing the conjugated diene compound to a peak temperature of 91 to 100° C.; The method includes a step of supplying an aromatic vinyl compound and polymerizing the compound at a temperature of 90 to 100° C. in the reactor. A method for producing a block copolymer.

11. 3 to 20 parts by mass of the block copolymer according to any one of claims 5 to 7; 97 to 80 parts by mass of a styrene-based resin; A resin composition which is a polymer of the above.

12. The styrene-based resin is a copolymer of a styrene-based compound and acrylonitrile. The resin composition according to claim 11.

13. A method for producing the block copolymer according to any one of claims 5 to 7, comprising the steps of: supplying a conjugated diene compound to a reactor and polymerizing the conjugated diene compound to a peak temperature of 91 to 100° C.; The method includes a step of supplying an aromatic vinyl compound and polymerizing the compound at a temperature of 90 to 100° C. in the reactor. A method for producing a block copolymer.

Citation Information

Patent Citations

  • Aromatic vinyl-conjugated diene block copolymer and method for producing the same

    JP4029470B2

  • Aromatic vinyl-conjugated diene block copolymer and method for producing the same

    JP4029471B2

  • Method for producing conjugated diene polymer

    JP6646437B2