Positive electrode active material for lithium secondary battery, manufacturing method therefor, positive electrode for lithium secondary battery including the same, and lithium secondary battery
A nickel-based lithium metal oxide with a cobalt compound coating and molybdenum doping addresses the challenges of particle aggregation and efficiency in single-crystal positive electrode active materials, enhancing discharge capacity and charge/discharge efficiency in lithium secondary batteries.
Patent Information
- Application Number
- JP2024046567
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-07
AI Technical Summary
Lithium secondary batteries face challenges with high energy density, safety, and reduced productivity due to particle aggregation and lower discharge capacity and charge/discharge efficiency of single-crystal positive electrode active materials.
A nickel-based lithium metal oxide with a cobalt compound coating and molybdenum doping is used, where the nickel-based lithium metal oxide single particles are 1 to 4 μm in size, and the cobalt compound-containing coating layer is 1 to 50 nm thick, with specific molybdenum and cobalt content, to improve discharge capacity and charge/discharge efficiency.
The solution suppresses interparticle aggregation, enhances productivity, reduces cation mixing, and improves capacity characteristics, resulting in lithium secondary batteries with improved discharge capacity and charge/discharge efficiency.
Smart Images

Figure 2024137912000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode active material for a lithium secondary battery, a method for producing the same, a positive electrode for a lithium secondary battery including the same, and a lithium secondary battery. [Background technology]
[0002] With the development of portable electronic devices and communication devices, there is a high demand for the development of high energy density lithium secondary batteries. However, the safety of high energy density lithium secondary batteries is reduced, and improvements to this issue are required.
[0003] In order to manufacture a lithium secondary battery with a long life and reduced gas generation, the use of a single-crystal positive electrode active material as the positive electrode active material of the lithium secondary battery has been considered. The single-crystal positive electrode active material has problems such as particle aggregation and reduced productivity due to high-temperature heat treatment for single crystallization.
[0004] Compared with polycrystalline positive electrode active materials, single-crystal positive electrode active materials exhibit relatively low discharge capacity and charge / discharge efficiency, and improvements in these respects are required. Summary of the Invention [Problem to be solved by the invention]
[0005] The problem to be solved by the present invention is to provide a novel positive electrode active material for a lithium secondary battery.
[0006] Another problem to be solved by the present invention is to provide a method for producing the above-mentioned positive electrode active material.
[0007] Another object of the present invention is to provide a positive electrode that includes the above-mentioned positive electrode active material and has improved discharge capacity and charge / discharge efficiency.
[0008] Another problem to be solved by the present invention is to provide a lithium secondary battery including the above-mentioned positive electrode. [Means for solving the problem]
[0009] According to one aspect, Nickel-based lithium metal oxide single particles, The size of the nickel-based lithium metal oxide single particle is 1 to 4 μm, The positive electrode active material for a lithium secondary battery includes a coating layer containing a cobalt compound disposed on the surface of the nickel-based lithium metal oxide single particle, and the nickel-based lithium metal oxide single particle is doped with molybdenum.
[0010] The molybdenum content is 0.1 mol% or more and less than 1.0 mol% based on 100 mol% of the total metal content excluding lithium in the positive electrode active material, and the cobalt compound-containing coating layer has a cobalt compound content of 0.1 to 5.0 mol% based on the total content of the positive electrode active material, and a thickness of the cobalt compound-containing coating layer is 1 nm to 50 nm.
[0011] In the coating layer containing a cobalt compound, the cobalt compound is cobalt oxide, lithium cobalt oxide, or a combination thereof, and the coating layer containing a cobalt compound further includes at least one selected from the group consisting of boron, manganese, phosphorus, aluminum, zinc, zirconium, and titanium.
[0012] The nickel-based lithium metal oxide is a compound represented by the following Chemical Formula 1.
[0013] [Chemical formula 1] Li a (Ni 1-x-y M1 x M2 y )O 2±α1 In Chemical Formula 1, M1 is one or more elements selected from Co, Mn, and Al; M2 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.95≦a≦1.1, 0.6≦(1-xy)<1, 0≦x<0.4, 0≦y<0.4, 0≦α1≦0.1, and the case where x and y are simultaneously 0 is excluded.
[0014] The nickel-based lithium metal oxide is a compound represented by the following Chemical Formula 2.
[0015] [Chemical formula 2] Li a (Ni 1-x-y-z Co x M3 y M4 z )O 2±α1 In Chemical Formula 2, M3 is one or more elements selected from Mn and Al; M4 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.95≦a≦1.1, 0.6≦(1-xyz)<1, 0≦x<0.4, 0≦y<0.4, 0≦z<0.4, 0≦α1≦0.1, and the case where x, y, and z are simultaneously 0 is excluded.
[0016] FWHM measured by X-ray diffraction analysis for the positive electrode active material (003) / FWHM (104) In this disclosure, FWHM (003) means the FWHM (Full with Half Maximum) of the peak corresponding to the (003) plane, and FWHM (104) means the FWHM of the peak corresponding to the (104) plane.
[0017] According to another embodiment, a nickel precursor, one or more selected from an M1 precursor and an M2 precursor, and a basic solution are mixed to obtain a mixture, and the mixture is co-precipitated, and then dried to obtain a nickel-based metal precursor having pores therein; obtaining a mixture of the nickel-based metal precursor having pores therein and a lithium precursor; adding a molybdenum precursor to the mixture and performing a first heat treatment of the resulting mixture; carrying out a grinding step of the primary heat treated product; adding a cobalt precursor to the product to obtain a mixture, and performing a second heat treatment on the mixture to produce the cathode active material; The first heat treatment is carried out at a higher temperature than the second heat treatment, The M1 precursor is at least one selected from a cobalt precursor, a manganese precursor, and an aluminum precursor; The M2 precursor is a precursor containing one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), and zirconium (Zr).
[0018] In the nickel-based metal precursor, the size of the internal pore region is 2 to 7 μm, and the cobalt precursor is Co(OH)2, CoOOH, CoO, Co2O3, Co3O4, Co(OCOCH3)2·4H2O, CoCl2, Co(NO3)2·6H2O, CoSO4, Co(SO4)2·7H2O, or a combination thereof.
[0019] The nickel-based metal precursor is a compound represented by the following Chemical Formula 3, a compound represented by the following Chemical Formula 4, or a combination thereof.
[0020] [Chemical formula 3] (Ni 1-x-y M1x M2 y )(OH)2 In Chemical Formula 3, M1 is one or more elements selected from Co, Mn, and Al; M2 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.6≦(1-xy)<1, 0≦x<0.4, 0≦y<0.4, and the case where x and y are simultaneously 0 is excluded. [Chemical formula 4] (Ni 1-x-y M1 x M2 y )O In Chemical Formula 4, M1 is one or more elements selected from Co, Mn, and Al; M2 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.6≦(1-xy)<1, 0≦x<0.4, 0≦y<0.4, and the case where x and y are simultaneously 0 is excluded.
[0021] The nickel-based metal precursor is represented by a compound of the following Formula 5, a compound of the following Formula 6, or a combination thereof.
[0022] [Chemical formula 5] Ni 1-x-y-z Co x M3 y M4 z (OH)2 In Chemical Formula 5, M3 is one or more elements selected from Mn and Al; M4 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.6≦(1-xyz)<1, 0≦x<0.4, 0≦y<0.4, 0≦z<0.4, except when x, y, and z are simultaneously 0; [Chemical formula 6] (Ni 1-x-y-z Co x M3 y M4 z )O In Chemical Formula 6, M3 is one or more elements selected from Mn and Al; M4 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.6≦(1-xyz)<1, 0≦x<0.4, 0≦y<0.4, 0≦z<0.4, and the case where x, y, and z are simultaneously 0 is excluded.
[0023] The nickel-based metal precursor and the lithium precursor are mixed so that the Li / Me (metals excluding Li) molar ratio is 0.9 or more and less than 1.1, and the lithium precursor is lithium hydroxide, lithium carbonate, lithium sulfate, lithium nitrate, or a combination thereof.
[0024] The primary heat treatment is carried out at 800° C. to 1,200° C. in an oxidizing gas atmosphere, and the secondary heat treatment is carried out at 600° C. to 850° C. in an oxidizing gas atmosphere.
[0025] According to yet another embodiment, there is provided a positive electrode for a lithium secondary battery, the positive electrode comprising a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, The positive electrode active material layer contains the above-mentioned positive electrode active material, and a positive electrode for a lithium secondary battery is provided.
[0026] According to yet another aspect, there is provided a lithium secondary battery comprising the above-described positive electrode, negative electrode, and an electrolyte interposed therebetween. Effect of the Invention
[0027] By using the positive electrode active material for lithium secondary batteries according to one embodiment, it is possible to manufacture a nickel-based active material for lithium secondary batteries having improved capacity characteristics by suppressing interparticle aggregation, improving productivity, and reducing the cation mixing ratio. A lithium secondary battery manufactured using such a nickel-based active material for lithium secondary batteries has improved discharge capacity and charge / discharge efficiency. [Brief description of the drawings]
[0028] [Figure 1A] FIG. 2 is a schematic diagram illustrating a cross-sectional structure of a product having a one-layer structure obtained after a first heat treatment in preparing a positive electrode active material according to an embodiment. [Figure 1B] FIG. 4 is a schematic diagram illustrating a cross-sectional structure of a product having a two-layer structure obtained after a first heat treatment in preparing a positive electrode active material according to another embodiment. [Figure 1C] 2 is a scanning electron microscope photograph showing a cross-sectional structure of a product obtained after a primary heat treatment during the production of a positive electrode active material according to Example 1. [Figure 2A] 3 is an electron scanning microscope photograph of the surface of a primary heat treatment product during the production of the positive electrode active material of Example 1. [Figure 2B] 3 is an electron scanning microscope photograph of the surface of a primary heat treatment product during the production of the positive electrode active material of Example 1. [Figure 2C] 3 is an electron scanning microscope photograph of the surface of a primary heat treatment product during the production of the positive electrode active material of Example 1. [Figure 2D] 2 is a scanning electron microscope photograph of the surface of the positive electrode active material of Example 1. [Figure 2E] 2 is a scanning electron microscope photograph of the surface of the positive electrode active material of Example 1. [Figure 3A]4 is an electron scanning microscope photograph of the surface of a primary heat treatment product during the production of the positive electrode active material of Example 2. [Figure 3B] 4 is an electron scanning microscope photograph of the surface of a primary heat treatment product during the production of the positive electrode active material of Example 2. [Figure 3C] 4 is an electron scanning microscope photograph of the surface of a primary heat treatment product during the production of the positive electrode active material of Example 2. [Figure 3D] 4 is an electron scanning microscope photograph of the surface of the positive electrode active material of Example 2. [Figure 3E] 4 is an electron scanning microscope photograph of the surface of the positive electrode active material of Example 2. [Figure 4A] 1 is an electron scanning microscope photograph of a surface of a primary heat treatment product during the production of a positive electrode active material of Example 3. [Figure 4B] 1 is an electron scanning microscope photograph of a surface of a primary heat treatment product during the production of a positive electrode active material of Example 3. [Figure 4C] 1 is an electron scanning microscope photograph of a surface of a primary heat treatment product during the production of a positive electrode active material of Example 3. [Figure 4D] 1 is an electron scanning microscope photograph of the surface of the positive electrode active material of Example 3. [Figure 4E] 1 is an electron scanning microscope photograph of the surface of the positive electrode active material of Example 3. [Figure 5A] 1 is an electron scanning microscope photograph of the surface of a primary heat treatment product during the production of a positive electrode active material of Reference Example 1. [Figure 5B] 1 is an electron scanning microscope photograph of the surface of a primary heat treatment product during the production of a positive electrode active material of Reference Example 1. [Figure 5C] 1 is an electron scanning microscope photograph of the surface of a primary heat treatment product during the production of a positive electrode active material of Reference Example 1. [Figure 5D] 2 is an electron scanning microscope photograph of the surface of the positive electrode active material of Reference Example 1. [Figure 5E] 2 is an electron scanning microscope photograph of the surface of the positive electrode active material of Reference Example 1. [Figure 6]2 is an electron microscope photograph showing a cross-sectional structure of the positive electrode active material obtained in Preparation Example 1, obtained by performing an electron scanning microscope analysis on the nickel-based metal precursor in Preparation Example 1. [Figure 7] 1 is a graph showing particle size distribution characteristics in the positive electrode active materials of Examples 1 to 3 and Reference Example 1. [Figure 8A] 1 is a graph showing the change in capacity in the coin cells of Production Examples 1 to 3 and Reference Production Examples 1 and 2. [Figure 8B] 1 is a graph showing the change in capacity depending on the voltage that occurs during charging in the coin cells of Production Examples 1 to 3 and Reference Production Examples 1 and 2. [Figure 9] 1 is a graph showing capacity retention characteristics of the coin cells of Production Examples 1 to 3 and Reference Production Examples 1 and 2. [Figure 10] 1 is a schematic diagram of a lithium secondary battery according to an illustrative embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] Hereinafter, a positive electrode active material for a lithium secondary battery, a manufacturing method thereof, a positive electrode including the same, and a lithium secondary battery including the positive electrode according to an embodiment will be described in detail.
[0030] In order to manufacture a lithium secondary battery having improved life characteristics, a positive electrode containing a single crystal positive electrode active material is used. During manufacture of the single crystal positive electrode active material, an excess amount of lithium is added and a high-temperature heat treatment is performed, but the high-temperature heat treatment causes particles to agglomerate together, or reduces productivity and increases residual lithium. In addition, when a lithium secondary battery is manufactured using such a single crystal positive electrode active material, the capacity and charge / discharge efficiency are reduced.
[0031] Single crystal positive electrode active materials exhibit a particle aggregation phenomenon, and therefore must undergo a pulverization process during the manufacture of the positive electrode. In the case of typical single crystal positive electrode active materials, such a pulverization process reduces the single crystal characteristics of the positive electrode active material, generates residual pulverized material, and increases surface resistance.
[0032] As a result, the inventors have solved the above-mentioned problems and completed the present invention, which relates to a positive electrode active material having improved surface resistance characteristics without reducing the crystallinity of the positive electrode active material or causing almost no surface defects after a secondary heat treatment even if a pulverization process is performed.
[0033] According to an embodiment, the positive electrode active material for a lithium secondary battery is a nickel-based lithium metal oxide single particle. The size (e.g., average size) of the nickel-based lithium metal oxide single particle is 1 to 4 μm; The nickel-based lithium metal oxide single particle includes a coating layer containing a cobalt compound disposed on the surface of the nickel-based lithium metal oxide single particle (e.g., on the surface of each of the nickel-based lithium metal oxide single particles); The nickel-based lithium metal oxide single particles are doped with molybdenum.
[0034] In the present specification, the term "one body, monolith, or monolithic particle" refers to a structure in which particles are not mutually aggregated in terms of morphology and exist as an independent phase, and has a particle size of 1 to 4 μm, for example, 2 to 4 μm. In the present specification, the single particle has improved structural and morphological stability and can be mass-produced. Furthermore, by using a positive electrode including such a positive electrode active material, a lithium secondary battery having improved safety, capacity, and charge / discharge efficiency can be manufactured.
[0035] In this specification, when the particle is spherical, the "size" refers to the particle size or average particle size, and when the particle is non-spherical, the "size" refers to the major axis length or average major axis length. The particle size can be measured using an electron scanning microscope or a particle size analyzer. An example of the particle size analyzer is the HORIBA LA-950 laser particle size analyzer. When the particle size is measured using the particle size analyzer, the average particle size refers to D50. The D50 means the average diameter of particles whose cumulative volume corresponds to 50% by volume in the particle size distribution, and means the value of the particle size corresponding to 50% from the smallest particle when the total number of particles is 100% in a distribution curve in which particle sizes are accumulated in the order from the smallest particle to the largest particle.
[0036] When particle size is measured using an electron scanning microscope, it is defined as the average value of 30 or more randomly selected particles of 1 μm or more, excluding fine powder.
[0037] The average particle size of the positive electrode active material is measured, for example, by using a laser diffraction method. More specifically, the positive electrode active material is dispersed in a solution, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000). After irradiating the solution with ultrasonic waves of about 28 kHz at an output of 60 W, the average particle size (D50) at 50% of the particle size distribution measured by the measuring device can be calculated.
[0038] As used herein, the term "D10" refers to the average diameter of particles whose cumulative volume corresponds to 10% by volume in a particle size distribution, and "D90" refers to the average diameter of particles whose cumulative volume corresponds to 90% by volume in a particle size distribution.
[0039] The particle size distribution (span) is expressed as (D90-D10) / D50, and may be, for example, 0.9 to 1.5, 0.95 to 1.4, 0.98 to 1.2, or 0.98 to 1.1.
[0040] D90 is 4 to 7 μm, D10 is 1.2 to 2.0 μm, and D50 is 2 to 4 μm. When the D90, D10, and D50 of the positive electrode active material are within the above ranges, the positive electrode active material has excellent dispersion, the specific surface area is appropriately maintained, and the activity is excellent.
[0041] If the positive electrode active material includes a coating layer containing a cobalt compound, the surface resistance characteristics are improved, and a lithium secondary battery having a positive electrode using the same has improved life characteristics.
[0042] A monolithic particle as used herein is also a particle that comprises one or more single crystals. The monolithic particle is also a particle that comprises a single crystal or several crystals.
[0043] As used herein, single particle means a single particle (one body particle) having a primary particle size of 1 to 4 μm, for example, including 1 to 3 particles.
[0044] In the positive electrode active material according to an embodiment, the single particle size (e.g., average size) may be, for example, 1 to 4 μm, 2 to 4 μm, or 2 to 3.5 μm. When the single particle size of the positive electrode active material is within this range, a positive electrode active material having excellent capacity characteristics may be obtained.
[0045] In this specification, the term "interior" of a positive electrode active material refers to a region of 50 to 70% by volume, for example 60% by volume, from the center of the total volume from the center to the surface of the positive electrode active material, or the remaining region of the positive electrode active material excluding a region within 3 µm from the outermost periphery (exterior) of the total distance from the center to the surface of the positive electrode active material.
[0046] In the positive electrode active material according to an embodiment, the content of the doped molybdenum is 0.1 mol% or more and less than 1 mol%, 0.1 to 0.5 mol%, or 0.1 to 0.4 mol% based on 100 mol% of the total metal content excluding lithium in the positive electrode active material. When the molybdenum content is within the above range, a positive electrode active material having improved capacity and efficiency characteristics and improved life characteristics can be obtained.
[0047] The coating layer containing a cobalt compound may coat all or a portion of the surface of the positive electrode active material, for example, the coating layer may coat 90% or less, 80% or less, 70% or less, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 1 to 10% of the surface of the positive electrode active material.
[0048] In the coating layer, the content of the cobalt compound is 0.1 to 5.0 mol%, 0.5 to 5.0 mol%, 1 to 4 mol%, or 1.5 to 3 mol% based on the total content of the positive electrode active material (100 mol%). When the content of the cobalt compound is within the above range, Ni, which is present in large amounts in the metal layer during the synthesis of the positive electrode active material, is easily dissolved in the metal layer. 3+ Ni 2+ Reduce to Co 4+ Co 3+ / Co 2+ Alternatively, two types of ions can be reduced simultaneously, thereby reducing the reactivity between the interface of the positive electrode active material and the electrolyte.
[0049] The cobalt compound-containing coating layer includes cobalt oxide, lithium cobalt oxide, or a combination thereof, and the cobalt compound-containing coating layer further includes one or more selected from the group consisting of boron, manganese, phosphorus, aluminum, zinc, zirconium, and titanium.
[0050] The coating layer has a thickness of 1 to 50 nm, 5 to 45 nm, or 10 to 35 nm. When the coating layer has a thickness in this range, a positive electrode active material having improved surface resistance characteristics can be obtained.
[0051] The nickel-based lithium metal oxide single particle is a compound represented by the following chemical formula 1.
[0052] [Chemical formula 1] Li a (Ni 1-x-y M1 x M2 y )O 2±α1 In Chemical Formula 1, M1 is one or more elements selected from Co, Mn, and Al; M2 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.95≦a≦1.1, 0.6≦(1-xy)<1, 0≦x<0.4, 0≦y<0.4, 0≦α1≦0.1, and the case where x and y are simultaneously 0 is excluded.
[0053] The nickel-based lithium metal oxide monoparticle is, for example, a compound represented by the following chemical formula 2.
[0054] [Chemical formula 2] Li a (Ni 1-x-y-z Co x M3 y M4 z )O 2±α1 In Chemical Formula 2, M3 is one or more elements selected from Mn and Al; M4 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.95≦a≦1.1, 0.6≦(1-xyz)<1, 0≦x<0.4, 0≦y<0.4, 0≦z<0.4, 0≦α1≦0.1, and the case where x, y, and z are simultaneously 0 is excluded.
[0055] FWHM of a positive electrode active material according to an embodiment measured by X-ray diffraction analysis using CuKα radiation (1.54056 Å) (003) / FWHM (104) is 0.72 to 0.79, or 0.73 to 0.77. When the half-width ratio is within the above range, the stability of the crystal structure of the positive electrode active material may be improved.
[0056] The positive electrode active material of the present invention has a FWHM (003) is 0.089° to 0.094°, 0.0895° to 0.093°, for example, 0.0897° to 0.0910°, and FWHM (104) is between 0.11° and 0.13°, between 0.115° and 0.125°, for example, between 0.1198° and 0.1226°. (003) indicates the full width at half maximum (FWHM) of the peak corresponding to the (003) plane, and FWHM (104) FWHM indicates the half-width of the peak corresponding to the (104) plane. (003) / FWHM (104) is a parameter created to evaluate the degree of uniform orientation (orientation) of crystal grains.
[0057] In addition, when observing a cross-sectional microstructure of the positive active material according to an embodiment through a scanning electron microscope, it can be seen that the positive active material has a single particle shape through confirmation of grains and grain boundaries on a sub-micro scale or larger.
[0058] FWHM of the positive electrode active material and the electrode plate containing the positive electrode active material (003) / FWHM (104) has the same numerical range as that of the positive electrode active material. (003) / FWHM (104)When each of the above ranges is within the above range, the stability of the crystal structure of the positive electrode active material can be improved, and the expansion and contraction rates due to the absorption / release of lithium can be improved, thereby improving the capacity characteristics and charge / discharge efficiency of the battery.
[0059] Hereinafter, a method for manufacturing a positive electrode active material according to an embodiment will be described.
[0060] First, a nickel precursor, one or more metal precursors selected from the group consisting of M1 precursor and M2 precursor, and a basic solution are mixed to obtain a mixture, which is then co-precipitated and dried to obtain a nickel-based metal precursor having internal pores, which has amorphous properties.
[0061] The M1 precursor is the same as M1 in Chemical Formula 1, and is at least one selected from a cobalt precursor, a manganese precursor, and an aluminum precursor. The M2 precursor is the same as M2 in Chemical Formula 1, and is a precursor containing at least one element selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), and zirconium (Zr).
[0062] The metal precursor may include, for example, one or more selected from a nickel precursor, a cobalt precursor, a manganese precursor, and a metal (M2) precursor.
[0063] During the coprecipitation reaction, the pH of the mixture is adjusted in two stages. The first stage is a pore formation section, in which the pH of the mixture is controlled to 11.5 to 12. The second stage is a particle growth section, in which the pH of the mixture is controlled to, for example, 10.5 to 11.9. The second stage is carried out at a lower pH than the first stage. In this way, the coprecipitation rate is changed, and a difference in synthesis rate is generated between the inside and outside of the nickel-based metal precursor. As a result, a nickel-based metal precursor having pores therein can be obtained. Here, the nickel-based metal precursor refers to a precursor for obtaining nickel-based lithium metal oxide.
[0064] In the first stage, for example, the pH of the mixture is adjusted to 11.6 to 11.9, or 11.7 to 11.8. In the second stage, the pH of the mixture is adjusted to, for example, 10.8 to 11.7, 11 to 11.7, 11.2 to 11.6, or 11.3 to 11.6. The difference between the pH of the second stage and the pH of the first stage is about 0.1 to 1.5, 0.1 to 1.0, 0.1 to 0.8, 0.1 to 0.6, 0.1 to 0.5, 0.1 to 0.3, or 0.1 to 0.2. In this way, the pH of the second stage is lowered by the aforementioned difference compared to the pH of the first stage, changing the coprecipitation rate and generating a difference in synthesis rate between the inside and outside of the nickel-based metal precursor. As a result, a nickel-based metal precursor having pores inside can be obtained. Here, the nickel-based metal precursor refers to a precursor for obtaining nickel-based lithium metal oxide.
[0065] The stirring time in the first stage may vary depending on the pH conditions in the first stage, but is, for example, in the range of 8 to 12 hours, or 9 to 10 hours.
[0066] In the present invention, the co-precipitation reaction proceeds at a high speed compared to a typical method for producing a cathode active material precursor, and the pore dispersion is controlled to be high, so that the cathode active material can be easily produced without a separate grinding process for the cathode active material, and the productivity can be improved. If the pore dispersion is controlled to be high, the cathode active material has many pores after heat treatment, and the active material crumbles well when pressed, and the cathode can exhibit excellent electrochemical properties. Here, the co-precipitation reaction can be carried out at a high speed by increasing the stirring speed and shortening the stirring time.
[0067] The metal precursor having pores therein contains secondary particles including a plurality of primary particles, and has a hollow structure having pores therein, similar to the positive electrode active material. The secondary particle size is 10 to 18 μm. And the primary particle size is 0.2 to 0.3 μm.
[0068] The nickel-based metal precursor having pores in the interior exhibits amorphous characteristics, and includes an interior having pores and an exterior having a denser structure than the interior. The amorphous characteristics of the nickel-based metal precursor can be confirmed by X-ray diffraction analysis. In this specification, the "interior" of the nickel-based metal precursor refers to a pore region in which a large number of pores are present, and refers to a region of 50 to 70% by volume, for example 60% by volume, from the center of the total volume from the center of the precursor to the surface, or the remaining region of the positive electrode active material excluding a region within 3 μm from the outermost periphery (exterior) in the total distance from the center of the precursor to the surface.
[0069] According to another embodiment, the interior of the nickel-based metal precursor is a pore region having a major axis length of 2 μm to 7 μm, for example, 3.5 to 5 μm.
[0070] In the nickel-based metal precursor having pores therein, the size (e.g., major axis length) of the pore region having the pores is 2 to 7 μm, and the secondary particle size is 10 to 15 μm, or 11 to 14 μm. Here, each of the secondary particles has an average size. When the size of the pore region of the nickel-based metal precursor and the secondary particle size are within the above ranges, a positive electrode active material having excellent phase stability and improved capacity characteristics can be obtained.
[0071] In this specification, the "size of the pore area (e.g., average size)" is mainly measured using the mercury intrusion method, the gas adsorption method, or the SEM (scanning electron microscope). The gas adsorption method includes the BET (Brunauer-Emmett-Teller) method or the BJH (Barrett-Joyner-Halenda) method. In this specification, the pore size means the average pore size. In the embodiment of the present invention, the pore size is measured using the BET method. And, the SEM method evaluates the pore size using image analysis.
[0072] The mixture may also include a complexing agent, a pH adjuster, and the like.
[0073] The pH regulator serves to reduce the solubility of metal ions in the reactor and precipitate the metal ions as hydroxides. Examples of the pH regulator include ammonium hydroxide (NH4OH) (ammonia water), sodium hydroxide (NaOH), sodium carbonate (Na2CO3), etc. An example of the pH regulator is sodium hydroxide (NaOH).
[0074] The complexing agent plays a role in controlling the reaction rate of the formation of precipitate in the coprecipitation reaction. The complexing agent is ammonium hydroxide, citric acid, acrylic acid, tartaric acid, glycolic acid, etc. The content of the complexing agent is used at a general level. The complexing agent is, for example, aqueous ammonia.
[0075] The product obtained by the coprecipitation reaction is washed and then dried to obtain the target nickel-based metal precursor, which is dried under general conditions.
[0076] The one or more metal precursors selected from the nickel precursor, M1 precursor, and M2 precursor include, for example, a nickel precursor, a manganese precursor, and a cobalt precursor. Alternatively, the metal precursor includes, for example, a nickel precursor, a cobalt precursor, and an aluminum precursor.
[0077] Examples of nickel precursors can include Ni(OH)2, NiO, NiOOH, NiCO3·2Ni(OH)2·4H2O, NiC2O4·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, fatty acid nickel salts, nickel halides, or combinations thereof. Manganese precursors can include, for example, manganese oxides such as Mn2O3, MnO2, and Mn3O4; MnCO3; Mn(NO3)2; MnSO4; MnSO4·H2O; manganese acetate; manganese dicarboxylates, manganese citrates, and fatty acid manganese salts; manganese oxyhydroxide; manganese halides such as manganese chloride; or combinations thereof.
[0078] Examples of cobalt precursors may include Co(OH)2, CoOOH, CoO, Co2O3, Co3O4, Co(OCOCH3)2·4H2O, CoCl2, Co(NO3)2·6H2O, CoSO4, Co(SO4)2·7H2O, or combinations thereof.
[0079] The aluminum precursor can include, for example, aluminum hydroxide, aluminum chloride, aluminum oxide, or a combination thereof.
[0080] In the M2 precursor, the precursor containing each element may be a salt, hydroxide, oxyhydroxide, halide, or a combination thereof containing each element. Here, the salt containing the above elements may be, for example, one or more selected from sulfate, alkoxide, oxalate, phosphate, halide, oxyhalide, sulfide, oxide, peroxide, acetate, nitrate, carbonate, citrate, phthalate, and perchlorate containing the above elements.
[0081] The contents of the nickel precursor and one or more metal precursors selected from the M1 precursor and the M2 precursor are stoichiometrically controlled so as to obtain the desired nickel-based metal precursor.
[0082] The nickel-based metal precursor is a compound represented by the following Chemical Formula 3, a compound represented by the following Chemical Formula 4, or a combination thereof.
[0083] [Chemical formula 3] (Ni 1-x-y M1 x M2 y )(OH)2 In Chemical Formula 3, M1 is one or more elements selected from Co, Mn, and Al; M2 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.6≦(1-xy)<1, 0≦x<0.4, 0≦y<0.4, and the case where x and y are simultaneously 0 is excluded. [Chemical formula 4] (Ni 1-x-y M1 x M2 y )O In Chemical Formula 4, M1 is one or more elements selected from Co, Mn, and Al; M2 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.6≦(1-xy)<1, 0≦x<0.4, 0≦y<0.4, and the case where x and y are simultaneously 0 is excluded.
[0084] The nickel-based metal precursor is, for example, a compound represented by the following Chemical Formula 5, a compound represented by the following Chemical Formula 6, or a combination thereof.
[0085] [Chemical formula 5] Ni 1-x-y-z Co x M3 y M4 z (OH)2 In Chemical Formula 5, M3 is one or more elements selected from Mn and Al; M4 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.6≦(1-xyz)<1, 0≦x<0.4, 0≦y<0.4, 0≦z<0.4, except when x, y, and z are simultaneously 0; [Chemical formula 6] (Ni 1-x-y-z Co x M3 y M4 z )O In Chemical Formula 6, M3 is one or more elements selected from Mn and Al; M4 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), and zirconium (Zr); 0.6≦(1-xyz)<1, 0≦x<0.4, 0≦y<0.4, 0≦z<0.4, and the case where x, y, and z are simultaneously 0 is excluded.
[0086] The nickel-based metal precursor is, for example, a compound represented by Chemical Formula 7, a compound represented by Chemical Formula 8, or a combination thereof.
[0087] [Chemical formula 7] Ni 1-x-y-z Co x Mn y M4 z (OH)2 In formula 7, M4 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zirconium (Zr) and aluminum; 0.6≦(1-xyz)<1, 0≦x<0.4, 0≦y<0.4, 0≦z<0.4, except when x, y, and z are simultaneously 0; [Chemical formula 8] Ni 1-x-y-z Co x Mn y M4 z (OH)2 In formula 8, M4 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), and zirconium (Zr); 0.6≦(1-xyz)<1, 0≦x<0.4, 0≦y<0.4, 0≦z<0.4, and the case where x, y, and z are simultaneously 0 is excluded.
[0088] Subsequently, a mixture of the nickel-based metal precursor having pores therein and a lithium precursor is obtained.
[0089] The mixture ratio of the lithium precursor and the nickel-based metal precursor is adjusted stoichiometrically to produce the desired cathode active material. After adding the molybdenum precursor to the mixture, the mixture is subjected to a first heat treatment. Through the first heat treatment, phase transition and grain growth are promoted.
[0090] 1A and 1B show cross-sectional structures of a product after a first heat treatment in preparing a positive electrode active material according to an embodiment.
[0091] The primary heat treatment product may also include up to two layers of primary particles.
[0092] The primary heat treatment product 10 includes a hollow primary particle layer having a one-layer structure, as can be seen from Fig. 1A. The hollow primary particle layer includes primary particles 11.
[0093] The primary heat treatment product also includes a hollow primary particle layer having a two-layer structure, as shown in Figure 1B. Such a structure facilitates the process of crumbling during grinding. In Figure 1B, reference numerals 11a and 11b indicate first and second primary particles, which respectively form the first and second primary particle layers.
[0094] The primary heat treated product is subjected to a crushing step to obtain a small, monoparticulate product.
[0095] According to an embodiment, the grinding is performed using a jet mill, a pin mill, an ACM mill, a disk mill, etc. The grinding is performed, for example, at 10,000 to 20,000 rpm, for example, 12,000 to 16,000 rpm. The stirring time for the grinding varies depending on the grinding conditions, and is, for example, 30 to 90 seconds, 40 to 80 seconds, or 50 to 60 seconds.
[0096] A crushing process may be additionally performed before the pulverization process of the primary heat treatment product. By performing such a crushing process, the hard cake-like product obtained after the primary heat treatment can be crushed into powder. By performing such a crushing process, single particles having a uniform particle shape can be obtained.
[0097] The crushing is carried out in a roll crusher at 100 to 300 rpm, 100 to 250 rpm, or 120 to 275 rpm. The gap of the roll crusher is 1 to 3 mm, 1.2 to 2.8 mm, or 1.5 mm. The stirring time for the crushing varies depending on the crushing conditions, but is generally carried out for 10 to 60 seconds.
[0098] The molybdenum precursor can include, for example, molybdenum hydroxide, molybdenum chloride, molybdenum oxide, ammonium molybdate, or combinations thereof.
[0099] Ammonium molybdate includes, for example, ammonium heptamolybdate hydrate ((NH4)6Mo7O 24 4H2O).
[0100] A cobalt precursor is then added to the small single particle product to obtain a mixture, which is utilized in forming a coating layer containing a cobalt compound disposed on the surface of the nickel-based lithium metal oxide.
[0101] In this specification, "pulverization" refers to a process in which secondary particles are formed by strong agglomerations between primary particles, and the process is carried out using equipment such as a jet mill that applies strong force (air pressure, mechanical pressure) to remove such strong agglomerations.
[0102] The mixture obtained by the above process is subjected to a second heat treatment to prepare a small single particle positive active material according to an embodiment.
[0103] The secondary heat treatment is performed at a lower temperature than the primary heat treatment, and if the secondary heat treatment is performed, the crystallinity is restored. If the secondary heat treatment is performed at a higher temperature than the primary heat treatment, it is difficult to obtain single particles with excellent phase stability. In addition, if the product of the primary heat treatment is subjected to a pulverization process in the manufacturing method, it is difficult to obtain a cathode active material having a hollow structure.
[0104] The nickel-based metal precursor and the lithium precursor may be mixed so that the Li / Me (metals excluding Li) molar ratio is 0.9 or more and less than 1.1, more than 1.0 and less than 1.1, 1.01 to 1.05, or 1.02 to 1.04. The mixing step of the nickel-based metal precursor and the lithium precursor may be performed in two steps instead of one step. Here, the mixing ratio of the nickel-based metal precursor and the lithium precursor is appropriately controlled so that the Li / Me (metals excluding Li) molar ratio in the finally obtained positive electrode active material through one or two steps can be in the above-mentioned range.
[0105] The lithium precursor can include, for example, lithium hydroxide, lithium carbonate, lithium sulfate, lithium nitrate, or combinations thereof.
[0106] The first heat treatment is carried out in an oxidizing gas atmosphere at 800° C. to 1,200° C., 830° C. to 1,150° C., 850° C. to 1,100° C., 850° C. to 950° C., or 870° C. to 920° C., and the second heat treatment is carried out in an oxidizing gas atmosphere at 600° C. to 850° C., 600° C. to 800° C., 650° C. to 800° C., 700° C. to 800° C., or 720° C. to 790° C. When the first heat treatment and the second heat treatment are carried out under the above conditions, a lithium secondary battery with high density and long life can be manufactured.
[0107] The time for the first heat treatment varies depending on the temperature of the first heat treatment, and is, for example, 8 to 20 hours.
[0108] The oxidizing gas atmosphere utilizes an oxidizing gas such as oxygen or air, and for example, the oxidizing gas is composed of 10 to 20 volume % of oxygen or air and 80 to 90 volume % of an inert gas.
[0109] The cobalt precursor used in forming the cobalt compound-containing coating layer may include a hydroxide, sulfate, alkoxide, oxalate, phosphate, halide, oxyhalide, sulfide, oxide, peroxide, acetate, nitrate, carbonate, citrate, phthalate, perchlorate, or a combination thereof containing a cobalt compound. For example, the cobalt precursor may include one or more compounds selected from Co3O4, Co(OH)2, CoO, CoOOH, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, and Co(SO4)2·7H2O.
[0110] The content of the cobalt precursor is stoichiometrically adjusted to be 0.1 to 5.0 mol %, or 0.5 to 5.0 mol %, based on the total content of the positive electrode active material, as the content of the cobalt compound contained in the cobalt compound-containing coating layer.
[0111] The mixing of the nickel-based metal precursor and the lithium precursor may be dry mixing, and may be carried out using a mixer or the like. The dry mixing may be carried out using milling. The milling conditions are not particularly limited, but may be carried out so that there is little deformation, such as pulverization, of the precursor used as the starting material. The size of the lithium precursor to be mixed with the nickel-based metal precursor may be controlled in advance. The size (average particle size) of the lithium precursor is in the range of 5 to 15 μm, for example, about 10 μm. The lithium precursor having such a size may be milled with the nickel-based metal precursor at 300 to 3,000 rpm to obtain the desired mixture. If the temperature inside the mixer rises to 30° C. or higher during the milling process, a cooling process may be carried out to maintain the temperature inside the mixer at room temperature (25° C.).
[0112] Nickel-based metal precursors include, for example, Ni 0.92 Co 0.06 Mn 0.02 (OH)2, Ni 0.92 Co 0.05 Al 0.03 (OH)2, Ni 0.94 Co 0.03 Al 0.03 (OH)2, Ni 0.88 Co 0.06 Al 0.06 (OH)2, Ni 0.96 Co 0.02 Al 0.02 (OH)2, Ni 0.93 Co 0.04 Al 0.03 (OH)2, Ni 0.8 Co 0.15 Al 0.05 O2(OH) 2、 Ni 0.75 Co 0.20 Al 0.05 (OH) 2、 Ni 0.92 Co 0.05 Mn 0.03 (OH)2, Ni 0.94 Co 0.03 Mn 0.03 (OH)2, Ni 0.88 Co 0.06 Mn 0.06 (OH)2, Ni 0.96 Co 0.02 Mn 0.02 (OH)2, Ni 0.93 Co 0.04 Mn 0.03 (OH)2, Ni 0.8 Co 0.15 Mn 0.05 (OH) 2、 Ni 0.75 Co 0.20 Mn 0.05 (OH) 2、 Ni 0.6 Co 0.2 Mn 0.2 (OH)2, Ni 0.7 Co 0.15 Mn 0.15 (OH)2, Ni 0.7 Co 0.1 Mn0.2 (OH)2, Ni 0.8 Co 0.1 Mn 0.1 (OH)2 or Ni 0.85 Co 0.1 Al 0.05 (OH)2.
[0113] According to an embodiment, the nickel-based lithium metal oxide may be, for example, LiNi 0.92 Co 0.06 Mn 0.02 O2, Li 1.05 Ni 0.92 Co 0.05 Al 0.03 O2, Li 1.05 Ni 0.94 Co 0.03 Al 0.03 O2, Li 1.05 Ni 0.88 Co 0.06 Al 0.06 O2, Li 1.05 Ni 0.96 Co 0.02 Al 0.02 O2, Li 1.05 Ni 0.93 Co 0.04 Al 0.03 O2, Li 1.05 Ni 0.8 Co 0.15 Al 0.05 O 2、 Li 1.05 Ni 0.75 Co 0.20 Al 0.05 O 2、 Li 1.05 Ni 0.92 Co 0.05 Mn 0.03 O2, Li 1.05 Ni 0.94 Co 0.03 Mn 0.03 O2, Li 1.05 Ni 0.88 Co 0.06 Mn 0.06 O2, Li 1.05 Ni 0.96 Co 0.02 Mn 0.02 O2, Li 1.05 Ni 0.93 Co 0.04Mn 0.03 O2, Li 1.05 Ni 0.8 Co 0.15 Mn 0.05 O 2、 Li 1.05 Ni 0.75 Co 0.20 Mn 0.05 O 2、 Li 1.05 Ni 0.6 Co 0.2 Mn 0.2 O2, Li 1.05 Ni 0.7 Co 0.15 Mn 0.15 O2, Li 1.05 Ni 0.7 Co 0.1 Mn 0.2 O2, Li 1.05 Ni 0.8 Co 0.1 Mn 0.1 O2 or Li 1.05 Ni 0.85 Co 0.1 Al 0.05 It's O2.
[0114] According to another aspect, there is provided a positive electrode for a lithium secondary battery, comprising a positive electrode current collector and a positive electrode active material layer comprising the above-described positive electrode active material.
[0115] According to yet another embodiment, a lithium secondary battery includes the above-described positive electrode, negative electrode, and an electrolyte interposed therebetween.
[0116] By using the method for manufacturing a positive electrode active material according to an embodiment, a lithium secondary battery having improved discharge capacity and charge / discharge efficiency may be manufactured.
[0117] Hereinafter, a method for manufacturing a lithium secondary battery having a positive electrode including a positive electrode active material, a negative electrode, a non-aqueous electrolyte containing a lithium salt, and a separator will be described according to an embodiment.
[0118] The positive electrode and the negative electrode are produced by applying a positive electrode active material layer forming composition and a negative electrode active material layer forming composition, respectively, onto a current collector and drying them to form a positive electrode active material layer and a negative electrode active material layer.
[0119] The composition for forming the positive electrode active material is prepared by mixing a positive electrode active material, a conductive material, a binder, and a solvent. The positive electrode active material is a nickel-based active material according to an embodiment.
[0120] The positive electrode binder serves to improve the adhesive strength between particles of the positive electrode active material and between the positive electrode active material and the positive electrode current collector. Specific examples of the positive electrode binder include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of them may be used alone or in combination.
[0121] The conductive material is not particularly limited as long as it has conductivity without inducing a chemical change in the battery, and examples of the conductive material that can be used include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon nanotubes, carbon fibers, and metal fibers; carbon fluoride; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0122] The content of the conductive material is 1 to 10 parts by weight, or 1 to 5 parts by weight, based on 100 parts by weight of the positive electrode active material. When the content of the conductive material is within the above range, the finally obtained electrode has excellent conductivity characteristics.
[0123] A non-limiting example of the solvent is N-methylpyrrolidone, and the content of the solvent is 20 to 200 parts by weight based on 100 parts by weight of the positive electrode active material. When the content of the solvent is within the above range, the operation for forming the positive electrode active material layer is easy.
[0124] The positive electrode current collector is not particularly limited as long as it has a thickness of 3 to 500 μm, does not induce chemical changes in the battery, and has high conductivity, and may be, for example, stainless steel, aluminum, nickel, titanium, heat-treated carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The current collector may have fine irregularities on its surface to increase the adhesive strength of the positive electrode active material, and may be in various forms such as a film, sheet, foil, net, porous body, foam, or nonwoven fabric.
[0125] The positive electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may include, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. When the base film includes a thermoplastic polymer, the base film is liquefied when a short circuit occurs, and a sudden increase in current can be suppressed or reduced. The base film may be, for example, an insulator. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector may further include a metal chip and / or a lead tab. For more details regarding the base film, metal layer, metal chip, and lead tab of the positive electrode current collector, please refer to the negative electrode current collector described below. By having such a structure of the positive electrode current collector, the weight of the electrode can be reduced, and as a result, the energy density can be improved.
[0126] Separately, a negative electrode active material, a binder, and a solvent are mixed to prepare a composition for forming a negative electrode active material layer.
[0127] The negative electrode active material may be a material capable of reversibly absorbing / desorbing lithium ions, lithium metal, a lithium metal alloy, a material capable of doping / de-doping lithium, a transition metal oxide, or a combination thereof. Lithium titanium oxide may be used as the transition metal oxide.
[0128] Examples of the substance capable of reversibly occluding / releasing the lithium ions include carbon substances, that is, in a lithium secondary battery, it may have a carbon-based negative electrode active material generally used. Representative examples of the carbon-based negative electrode active material include crystalline carbon, amorphous carbon, or both of them may be used. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flaky, spherical or fibrous natural graphite or artificial graphite, and examples of the amorphous carbon include soft carbon, hard carbon, mesophase pitch carbide, calcined coke, and the like.
[0129] As the alloy of the lithium metal, an alloy of lithium and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn can be used.
[0130] Examples of the substance capable of doping and dedoping lithium include silicon-based substances, for example, Si, SiO x (0 < x < 2), Si·Q alloy (wherein Q is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a Group 15 element, a Group 16 element, a rare earth element, and combinations thereof, and is not Si), Si·carbon composite, Sn, SnO2, Sn·R (wherein R is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a Group 15 element, a Group 16 element, a rare earth element, and combinations thereof, and is not Sn), Sn·carbon composite, or a combination thereof, and at least one of them and SiO2 can also be mixed and used. As the element Q and the element R, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, or a combination thereof can be used.
[0131] The transition metal oxide may be lithium titanium oxide.
[0132] The negative electrode binder may be, but is not limited to, various types of binder polymers such as polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, polyacrylic acid, and polymers in which hydrogen is substituted with Li, Na, Ca, or the like, or various copolymers.
[0133] The negative electrode active material layer further contains a thickener.
[0134] The thickener may be at least one of carboxymethyl cellulose (CMC), carboxyethyl cellulose, starch, regenerated cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, and polyvinyl alcohol, and may be, for example, carboxymethyl cellulose (CMC).
[0135] The content of the solvent is 100 to 300 parts by weight based on 100 parts by weight of the total weight of the negative active material. When the content of the solvent is within the above range, the operation for forming the negative active material layer is easy.
[0136] When the negative electrode active material layer has sufficient conductivity, a conductive material is not necessary. The negative electrode active material layer may further include a conductive material as necessary. The conductive material is not particularly limited as long as it is conductive without inducing a chemical change in the battery, and may be, for example, graphite such as natural graphite or artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black; conductive fiber such as carbon fiber or metal fiber; conductive tube such as carbon nanotube; carbon fluoride; metal powder such as aluminum or nickel powder; conductive whisker such as zinc oxide or potassium titanate; conductive metal oxide such as titanium oxide; or conductive material such as polyphenylene derivative. The conductive material is preferably carbon black, and more specifically, carbon black having an average particle size of several tens of nm.
[0137] When the negative electrode active material layer includes a conductive material, the content of the conductive material is 0.01 to 10 parts by weight, 0.01 to 5 parts by weight, or 0.1 to 2 parts by weight, based on 100 parts by weight of the total weight of the negative electrode active material layer.
[0138] The negative electrode current collector is generally made to a thickness of 3 to 500 μm. Such a negative electrode current collector is not particularly limited as long as it is conductive without inducing a chemical change in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, heat-treated carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, like the positive electrode current collector, the surface can be formed with fine irregularities to strengthen the binding force of the negative electrode active material, and it can be used in various forms such as a film, sheet, foil, net, porous body, foam, and nonwoven fabric.
[0139] The negative electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may include, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. When the base film includes a thermoplastic polymer, the base film may be liquefied in the event of a short circuit, thereby suppressing a sudden increase in current. The base film may be, for example, an insulator. The metal layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal layer may act as an electrochemical fuse and may be cut off in the event of an overcurrent, thereby performing a short circuit prevention function. The thickness of the metal layer may be adjusted to adjust the limit current and maximum current. The metal layer may be electrolytically plated or vapor-deposited on the base film. If the thickness of the metal layer is reduced, the limiting current and / or maximum current of the negative electrode current collector is reduced, and the stability of the lithium battery during a short circuit may be improved. A lead tab may be added on the metal layer for connection to the outside. The lead tab may be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, or the like. During welding, the metal layer may be electrically connected to the lead tab while the base film and / or the metal layer melts. In order to further strengthen the welding between the metal layer and the lead tab, a metal piece may be added between the metal layer and the lead tab. The metal piece may be a thin piece of the same material as the metal of the metal layer. The metal piece may be, for example, a metal foil, a metal mesh, or the like. The metal piece may be, for example, aluminum foil, copper foil, or SUS (steel use stainless) foil.After disposing a metal piece on the metal layer, the lead tab can be welded to the metal piece / metal layer laminate or metal piece / metal layer / base film laminate. During welding, the base film, the metal layer, and / or the metal piece can be melted and the metal layer or the metal layer / metal piece laminate can be electrically connected to the lead tab. The metal piece and / or the lead tab can be added to a portion on the metal layer. The thickness of the base film can be, for example, 1 to 50 μm, 1.5 to 50 μm, 1.5 to 40 μm, or 1 to 30 μm. The weight of the electrode assembly can be further effectively reduced by the base film having a thickness in such a range. The melting point of the base film can be, for example, 100 to 300° C., 100 to 250° C., or 100 to 200° C. Since the base film has a melting point in such a range, the base film can be melted and easily bonded to the lead tab during the process of welding the lead tab. In order to improve the adhesion between the base film and the metal layer, a surface treatment such as a corona treatment can be performed on the base film. The thickness of the metal layer is, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to 1 μm. Since the metal layer has a thickness in such a range, the stability of the electrode assembly can be ensured while maintaining conductivity. The thickness of the metal piece is, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness in such a range, the connection between the metal layer and the lead tab can be more easily performed. Since the negative electrode current collector has such a structure, the weight of the electrode can be reduced, and as a result, the energy density can be improved.
[0140] A separator is interposed between the positive electrode and the negative electrode prepared by the above process.
[0141] The separation membrane has a pore size of 0.01 to 10 μm and a thickness of generally 5 to 30 μm. Specific examples include sheets and nonwoven fabrics made of olefin polymers such as polypropylene and polyethylene, or glass fibers. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte can also serve as the separation membrane.
[0142] The lithium salt-containing non-aqueous electrolyte is composed of a non-aqueous electrolyte solution and a lithium salt. The non-aqueous electrolyte may be a non-aqueous electrolyte solution, an organic solid electrolyte, an inorganic solid electrolyte, or the like.
[0143] The non-aqueous electrolyte may be, but is not limited to, an aprotic organic solvent such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate (DMC), diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, 2-methyltetrahydrofuran, dimethylsulfoxide, 1,3-dioxolane, N,N-formamide, N,N-dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ether, methyl propionate, or ethyl propionate.
[0144] Examples of the organic solid electrolyte include, but are not limited to, polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyester sulfide, polyvinyl alcohol, and polyvinylidene fluoride.
[0145] Examples of the inorganic solid electrolyte that may be used include, but are not limited to, nitrides, halides, and sulfates of Li, such as LiN, LiI, LiNI, LiN-LiI-LiOH, LiSiO, LiSiS, LiSiO, LiSiO-LiI-LiOH, and LiPO-LiS-SiS.
[0146] The lithium salt is a material that is easily dissolved in the non-aqueous electrolyte, and non-limiting examples thereof include LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, (CF3SO2)2NLi, (FSO2)2NLi, lithium chloroborate, or combinations thereof may be used.
[0147] FIG. 10 is an exploded perspective view illustrating a typical structure of a lithium secondary battery according to an embodiment.
[0148] Referring to FIG. 10, a lithium secondary battery 41 includes a positive electrode 43, a negative electrode 42, and a separator 44 according to an embodiment. The electrode assembly in which the positive electrode 43, the negative electrode 42, and the separator 44 are wound or folded is housed in a battery case 45. Depending on the shape of the battery, a separator 44 may be disposed between the positive electrode 43 and the negative electrode 42 to form a battery structure in which they are stacked one on the other. An organic electrolyte is then injected into the battery case 45 and sealed with a cap assembly 46 to complete the lithium secondary battery 41. The battery case 45 may be cylindrical, rectangular, thin-film, or the like. For example, the lithium secondary battery 41 may be a large-sized thin-film battery. The lithium secondary battery may be a lithium-ion battery. The battery structure is housed in a pouch, impregnated with an electrolyte (e.g., an organic electrolyte), and sealed to complete a lithium-ion polymer battery. In addition, a plurality of the battery structures may be stacked to form a battery pack, which may be used in any device requiring high capacity and high output, such as a notebook computer, a smartphone, or an electric vehicle (EV).
[0149] In addition, the lithium secondary battery has excellent storage stability, life characteristics, and high rate characteristics at high temperatures, and can be used in electric vehicles, for example, hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs).
[0150] The present invention will be described in more detail with reference to the following examples and comparative examples, which are given for illustrative purposes only and are not intended to be limiting.
[0151] (Production of nickel-based metal precursors) Manufacturing Example 1 Nickel-based metal precursor (Ni 0.92 Co 0.06 Mn 0.02 (OH)2) was synthesized.
[0152] Nickel sulfate (NiSO4·6H2O), cobalt sulfate (CoSO4·7H2O), and manganese sulfate (MnSO4·H2O) were dissolved in distilled water as a solvent so that the molar ratio of Ni:Co:Mn was 92:6:2, to prepare a metal raw material mixed solution. To form a complex compound, ammonia water (NH4OH) dilution solution and sodium hydroxide (NaOH) as a precipitant were prepared. Then, the metal raw material mixed solution, ammonia water, and sodium hydroxide were each put into the reactor. Sodium hydroxide was put in to maintain the pH inside the reactor.
[0153] The pH of the mixture is adjusted to 11.7 and stirred for 10 hours. Then, the pH of the mixture is adjusted to 11.5, and the pH is reduced by about 0.2 based on the initial pH, so that the coprecipitation rate is changed and a difference in the synthesis rate between the inside and outside of the nickel-based metal precursor is generated, and a nickel-based metal precursor having pores therein can be obtained.
[0154] The reaction mixture was allowed to react for about 20 hours while being stirred, and then the introduction of the metal raw material mixed solution was stopped.
[0155] The slurry solution in the reactor was filtered and washed with high-purity distilled water, and then dried in a hot air oven at 200°C for 24 hours to obtain a nickel-based metal precursor (Ni 0.92 Co 0.06 Mn 0.02 (OH)2) was obtained. The nickel-based metal precursor contained secondary particles that were aggregates of primary particles, and the average particle size of the secondary particles was about 14 μm.
[0156] (Manufacturing positive electrode active materials for lithium secondary batteries) Example 1: Co coating (2 mol%) and Mo doping (0.1 mol%) The nickel-based metal precursor having a hollow structure (Ni 0.92 Co 0.06 Mn 0.02To the first mixture, ammonium heptamolybdate hydrate ((NH4)6Mo7O 24 4H2O) was added, and the mixture was subjected to a primary heat treatment in an air atmosphere at 900°C for 15 hours. The content of ammonium heptamolybdate hydrate was controlled so that the content of doped molybdenum in the positive electrode active material was 0.1 mol%.
[0157] The primary heat treatment product was mixed in a Hosokawa Jet Mill (Blower 35Hz, AFG 8000rpm, Air 4kgf / cm 2 ) was used to carry out the grinding, producing a product of small monolithic particles having a particle size of 3-4 μm after grinding.
[0158] The product obtained by the above process is subjected to a secondary heat treatment in an oxygen atmosphere at about 770°C, and a cobalt precursor, Co(OH)2, is added thereto, and a secondary heat treatment is performed in an oxygen atmosphere at about 770°C for 12 hours to obtain a positive electrode active material (LiNi 0.899 Co 0.08 Mn 0.02 Mo 0.001 O2) was prepared in the form of single particles. The content of the cobalt precursor was controlled so that the content of the cobalt compound in the cobalt compound-containing coating layer was 2 mol% based on the total content of the positive electrode active material.
[0159] The positive electrode active material obtained in Example 1 was LiNi 0.899 Co 0.08 Mn 0.02 Mo 0.001 The content of the cobalt compound was 2 mol % based on the total content of the finally obtained positive electrode active material, and the thickness of the coating layer was about 20 nm.
[0160] Example 2: Co coating (2 mol%) and Mo doping (0.2 mol%) The same procedure as in Example 1 was carried out to prepare a positive electrode active material for a lithium secondary battery, LiNi, except that the molybdenum content was controlled to be about 0.2 mol % based on 100 mol % of the total metal content excluding lithium in the positive electrode active material. 0.898 Co 0.08 Mn 0.02 Mo0.002O2 was produced.
[0161] Example 3: Co coating (2 mol%) and Mo doping (0.4 mol%) The same procedure as in Example 1 was carried out to prepare a positive electrode active material for a lithium secondary battery, LiNi, except that the molybdenum content was controlled to be about 0.4 mol % based on 100 mol % of the total metal content excluding lithium in the positive electrode active material. 0.896 Co 0.08 Mn 0.02 Mo 0.004 was manufactured.
[0162] Reference Example 1: Co coating (2 mol%) and Mo undoped A positive electrode active material for a lithium secondary battery was prepared in the same manner as in Example 1, except that the process of adding ammonium heptamolybdate hydrate to the first mixture was not performed.
[0163] Reference Example 2: Co coating (2 mol%) and Mo doping (1.0 mol%) A positive electrode active material for a lithium secondary battery was prepared in the same manner as in Example 1, except that the content of ammonium heptamolybdate hydrate added to the first mixture was controlled so that the content of doped molybdenum in the positive electrode active material was 1.0 mol% based on the total content of metals other than lithium in the positive electrode active material.
[0164] (Coin cell manufacturing) Example 1 The positive active material obtained in Example 1 was used as the positive active material, and a coin cell was manufactured as follows, without a separate pulverization process.
[0165] The nickel-based active material ((LiNi 0.899Co 0.08 Mn 0.02 Mo 0.001 A mixture of 96 g of O2, 2 g of polyvinylidene fluoride (PVdF (Solef 6020 (Solvey company)), 47 g of N-methylpyrrolidone as a solvent, and 2 g of carbon black as a conductive material was mixed in a mixer to remove air bubbles and uniformly disperse the mixture, thereby preparing a slurry for forming a positive electrode active material layer.
[0166] The slurry prepared by the above process was coated on an aluminum foil using a doctor blade to form a thin electrode plate, which was then dried at 135° C. for 3 hours or more, and then subjected to a pressing process and a vacuum drying process to prepare a positive electrode.
[0167] A 2032 type coin cell was manufactured using the positive electrode and a lithium metal counter electrode as a counter electrode. A separator (thickness: about 16 μm) made of a porous polyethylene (PE) film was interposed between the positive electrode and the lithium metal counter electrode, and an electrolyte was injected to manufacture a 2032 type coin cell. As the electrolyte, a solution containing 1.15M LiPF6 dissolved in a solvent in which ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) were mixed in a volume ratio of 20:40:40 was used. Vinylene carbonate was added to the electrolyte. The content of the vinylene carbonate was 1.5 wt% based on 100 wt% of the electrolyte.
[0168] Production examples 2 and 3: Coin cell manufacturing Coin cells were manufactured in the same manner as in Preparation Example 1, except that the positive electrode active materials of Examples 2 and 3 were used instead of the positive electrode active material of Example 1.
[0169] Reference production examples 1 and 2: Coin cell manufacturing Coin cells were manufactured in the same manner as in Preparation Example 1, except that the positive electrode active materials obtained in Reference Examples 1 and 2 were used as the positive electrode active materials.
[0170] Evaluation example 1: Scanning electron microscope analysis I The surfaces of the secondary particles of the positive electrode active materials of Examples 1 to 3 and Reference Example 1 were subjected to electron scanning microscope analysis. The electron scanning microscope used was a Magellan 400L (FEI company), and the analysis results of the products after the primary heat treatment during the manufacture of the positive electrode active materials of Examples 1 to 3 and Reference Example 1 are shown in Figures 2A, 2B, 2C, 3A, 3B, 3C, 4A, 4B, 4C, 5A, 5B, and 5C. The analysis results of the products after the secondary heat treatment during the manufacture of the positive electrode active materials of Examples 1 to 3 and Reference Example 1 are shown in Figures 2D, 2E, 3D, 3E, 4D, 4E, 5D, and 5E. Here, FIGS. 2A to 2E relate to the positive electrode active material of Example 1, FIGS. 3A to 3E relate to the positive electrode active material of Example 2, FIGS. 4A to 4E relate to the positive electrode active material of Example 3, and FIGS. 5A to 5E relate to the positive electrode active material of Reference Example 1.
[0171] In each of Examples 1 to 3 and Reference Example 1, large particles having a hollow structure were obtained after the first heat treatment, as shown in Figures 2A to 2C, 3A to 3C, 4A to 4C, and 5A to 5C. The large particles were then crushed to form small particles, and the second heat treatment was then carried out to produce the final small particles, as shown in Figures 2D and 2E, 3D and 3E, 4D and 4E, and 5D and 5E (images corresponding to Figures 2D to 5E).
[0172] Evaluation example 2: Scanning electron microscope analysis II The nickel-based metal precursor of Production Example 1 was analyzed using a scanning electron microscope, and the analysis results are shown in FIG.
[0173] Referring to this, the nickel-based metal precursor of Preparation Example 1 had pores inside and showed a secondary particle shape with a size of 14 μm. The inside where the pores existed had a major axis length of about 5.76 μm and showed an amorphous structure.
[0174] Furthermore, a scanning electron microscope analysis was performed on the cross section of the secondary particles of the positive electrode active material of Example 1. The scanning electron microscope used was a Magellan 400L (FEI company), and the analysis results are shown in FIG. 1C.
[0175] FIG. 1C is a scanning electron microscope (SEM) image of a cross section of a product obtained after a first heat treatment in preparing the positive electrode active material of Example 1.
[0176] Referring to FIG. 1C, it can be seen that the positive electrode active material of Example 1 is composed of single particles having a size of 3.0 μm.
[0177] Evaluation example 3: Particle size distribution characteristics A particulate size analyzer (PSA) was used to analyze the particle size distribution characteristics of the positive electrode active materials of Examples 1 to 3 and Reference Example 1. The analysis results are shown in Table 1 below and FIG.
[0178] In Table 1 below, span is shown as (D90-D10) / D50.
[0179] The particle size distribution graph can be obtained under the following PSD measurement conditions.
[0180] The laser particle size analyzer used was LS13320 (Beckmann Coulter), and the analysis conditions were as follows:
[0181] Pump speed (55%), sample ultrasonic dispersion 40KHz ultrasonic (60s), run length 60s, refractive index ratio Sample RI 1.6, e-factor 1.00, sample amount 0.20g, sample dispersant: 10% sodium hexamethaphosphate 1ml
[0182] [Table 1]
[0183] 7, it was found that the positive electrode active materials of Examples 1 to 3 had uniform particle sizes with spans of less than 1.1. It was also found that the positive electrode active materials of Examples 1 to 3 and Reference Example 1 were all products with uniform particles, and the size of the positive electrode active material gradually decreased as the molybdenum (Mo) content increased.
[0184] In addition, the average particle size of the positive electrode active materials of Examples 1 to 3 and the positive electrode active material of Reference Example 1 was analyzed using an electron scanning microscope. The average particle size during analysis was determined to be the average value of 30 or more randomly sampled particles having a size of 1 μm or more, excluding fine powder, using an electron scanning microscope.
[0185] As a result, the average particle size of the positive electrode active materials of Examples 1 to 3 and the positive electrode active material of Reference Example 1 showed results similar to D50 in Table 1 above.
[0186] Evaluation example 4: X-ray diffraction analysis The positive electrode active materials produced in Examples 1 to 3 and Reference Example 1 were subjected to X-ray diffraction analysis using X'pert pro (PANalytical) utilizing CuKα radiation (1.54056 Å). The results are shown in Table 2 below.
[0187] In Table 2 below, FWHM (003) indicates the full width at half maximum (FWHM) of the peak corresponding to the (003) plane (peak with 2θ of approximately 18° to 19°), and FWHM (104) indicates the half-width of the peak corresponding to the (104) plane (peak with 2θ of approximately 44.5°).
[0188] [Table 2]
[0189] The positive electrode active materials of Examples 1 to 3 have the FWHM shown in Table 2. (003) and FWHM (003) / FWHM (104)From the characteristics, it was found that the particles were single particles. It was also found that the positive electrode active materials of Examples 1 to 3 had little crystal damage and excellent crystal characteristics after the secondary heat treatment even after the pulverization process.
[0190] The fact that there is little crystal damage to the positive electrode active material means that the FWHM (003) and FWHM (003) / FWHM (104) This can be confirmed from the FWHM value. (003) The lower the FWHM, the larger the crystal grains in the active material are in the (003) direction, and the more uniform the crystal structure they have grown. (003) / FWHM (104) A higher ratio means that the crystals have grown into large, uniform crystal structures in the (104) direction.
[0191] As can be seen from Table 2, the positive electrode active materials of Examples 1 to 3 were similar to the positive electrode active material of Reference Example 1 and exhibited excellent crystallinity.
[0192] Evaluation example 5: Residual lithium The residual lithium characteristics of the positive electrode active materials of Examples 1 to 3 and Reference Example 1 were evaluated, and the evaluation results are shown in Table 3 below.
[0193] The residual lithium content was measured by acid-base titration, in which 50 g of the active material was added to a beaker together with 100 ml of ultrapure water and stirred, and the stirred solution was separated into solution and powder using filter paper, and the resulting solution was then subjected to pH titration using 0.1 N hydrochloric acid to determine the content of lithium hydroxide and lithium carbonate. The results are shown in Table 3 below.
[0194] [Table 3]
[0195] From Table 3, it can be seen that the positive electrode active materials of Examples 1 to 3, like Reference Example 1, have a low content of residual lithium.
[0196] Evaluation example 6: Room temperature charge / discharge characteristics The charge / discharge characteristics of the coin cells produced in Production Examples 1 to 3 and Reference Production Examples 1 and 2 were evaluated using a charger / discharger (manufacturer: TOYO, model: TOYO-3100).
[0197] The initial charge and discharge was performed at 25°C with a constant current of 0.1 C until the voltage reached 4.25 V, and then with a constant voltage of 0.05 C. After the fully charged cell was rested for about 10 minutes, it was discharged at a constant current of 0.1 C until the voltage reached 3 V.
[0198] In the second charge / discharge cycle, the cells were charged at a constant current of 0.2 C until the voltage reached 4.25 V, and then charged at a constant voltage of 0.05 C. After a rest period of about 10 minutes, the cells that had been fully charged were discharged at a constant current of 0.2 C until the voltage reached 3 V.
[0199] The life evaluation was performed by charging the cells at a constant current of 1 C until the voltage reached 4.25 V, and then charging at a constant voltage of 0.05 C. After the fully charged cells were rested for about 10 minutes, they were discharged at a constant current of 1 C until the voltage reached 3 V, and this cycle was repeated 50 times to evaluate the life evaluation.
[0200] The charge / discharge efficiency was calculated using Equation 1.
[0201] [Formula 1] Charge / discharge efficiency = [0.2C discharge capacity / 0.2C charge capacity] x 100
[0202] The charge / discharge efficiency was evaluated as shown in Table 4 below, the capacity change with voltage was investigated as shown in FIG. 8A, and the difference in resistance during initial charging was investigated as shown in FIG. 8B.
[0203] [Table 4]
[0204] Referring to Table 4 and FIGS. 8A and 8B, it can be seen that the coin cells manufactured according to Preparation Examples 1 to 3 have improved charge / discharge efficiency compared to the coin cells manufactured according to Reference Preparation Examples 1 and 2.
[0205] Evaluation example 7: High temperature charge / discharge characteristics The charge / discharge characteristics of the coin cells produced in Production Examples 1 to 3 and Reference Production Examples 1 and 2 were evaluated using a charger / discharger (manufacturer: TOYO, model: TOYO-3100).
[0206] The initial charge and discharge was performed at 45°C with a constant current of 0.1 C until the voltage reached 4.3 V, and then constant voltage charging was performed until the current reached 0.05 C. After the fully charged cell was rested for about 10 minutes, it was discharged at a constant current of 0.1 C until the voltage reached 3 V.
[0207] In the second charge / discharge cycle, the cells were charged at a constant current of 0.2 C until the voltage reached 4.3 V, and then charged at a constant voltage of 0.05 C. After a rest period of about 10 minutes, the cells that had been fully charged were discharged at a constant current of 0.2 C until the voltage reached 3 V.
[0208] The life evaluation was performed by charging the cells at a constant current of 1 C until the voltage reached 4.3 V, and then charging at a constant voltage of 0.05 C. After the fully charged cells were rested for about 10 minutes, they were discharged at a constant current of 1 C until the voltage reached 3 V, and this cycle was repeated 50 times to evaluate the life evaluation.
[0209] The capacity retention ratio (CRR) was calculated using the following formula 2.
[0210] [Formula 2] Capacity retention rate [%] = [50th cycle discharge capacity / first cycle discharge capacity] x 100
[0211] 9, the coin cells manufactured according to Production Examples 1 to 3 exhibited excellent capacity retention rates at the same level as the coin cells of Reference Production Examples 1 and 2.
[0212] Although an embodiment has been described above with reference to the drawings and examples, they are merely illustrative, and a person skilled in the art will understand that various modifications and equivalent embodiments are possible therefrom. Therefore, the scope of protection of the present invention is defined by the claims. [Explanation of symbols]
[0213] 10 Primary heat treatment products 11 Primary particles 41 Lithium battery 42 Negative electrode 43 Positive electrode 44 Separation membrane 45 Battery case 46 Cap Assembly
Claims
1. Nickel-based lithium metal oxide single particles, The nickel-based lithium metal oxide has a single particle size of 1 to 4 μm; The nickel-based lithium metal oxide single particle includes a coating layer containing a cobalt compound disposed on the surface thereof, The nickel-based lithium metal oxide single particle is doped with molybdenum to provide a positive electrode active material for a lithium secondary battery.
2. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the molybdenum content is 0.1 mol % or more and less than 1.0 mol % based on 100 mol % of the total metal content excluding lithium in the positive electrode active material.
3. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the content of the cobalt compound in the cobalt compound-containing coating layer is 0.1 to 5.0 mol % based on the total content of the positive electrode active material.
4. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the coating layer containing a cobalt compound has a thickness of 1 nm to 50 nm.
5. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein in the cobalt compound-containing coating layer, the cobalt compound is cobalt oxide, lithium cobalt oxide, or a combination thereof.
6. The positive electrode active material for a lithium secondary battery according to claim 5 , wherein the cobalt compound-containing coating layer further comprises at least one selected from the group consisting of boron, manganese, phosphorus, aluminum, zinc, zirconium, and titanium.
7. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the nickel-based lithium metal oxide is a compound represented by the following Chemical Formula 1: [Chemical formula 1] Li a (N 1-x-y M1 x M2 y )O 2±α1 In Formula 1, M1 is one or more elements selected from Co, Mn, and Al; M2 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.95≦a≦1.1, 0.6≦(1−x−y)<1, 0≦x<0.4, 0≦y<0.4, 0≦α1≦0.1, and the case where x and y are simultaneously 0 is excluded.
8. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the nickel-based lithium metal oxide is a compound represented by the following chemical formula 2: [Chemical formula 2] Li a (N 1-x-y-z Co x M3 y M4 z )O 2±α1 In Chemical Formula 2, M3 is one or more elements selected from Mn and Al; M4 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.95≦a≦1.1, 0.6≦(1−x−y−z)<1, 0≦x<0.4, 0≦y<0.4, 0≦z<0.4, 0≦α1≦0.1, and the case where x, y, and z are simultaneously 0 is excluded.
9. FWHM measured by X-ray diffraction analysis for the positive electrode active material (003) / FWHM (104) The positive electrode active material for a lithium secondary battery according to claim 1 , wherein the σ is 0.72 to 0.
79.
10. mixing a nickel precursor, at least one selected from an M1 precursor and an M2 precursor, with a basic solution to obtain a mixture, and then performing a co-precipitation reaction of the mixture and drying the mixture to obtain a nickel-based metal precursor having pores therein; obtaining a mixture of the nickel-based metal precursor having pores therein and a lithium precursor; adding a molybdenum precursor to the mixture and performing a first heat treatment of the mixture; carrying out a crushing step of the primary heat treated product to obtain a small, single-particle product; adding a cobalt precursor to the small, single-particle product to obtain a mixture, and performing a second heat treatment on the mixture to produce the cathode active material of claim 1; The first heat treatment is carried out at a higher temperature than the second heat treatment, The M1 precursor is at least one selected from the group consisting of a cobalt precursor, a manganese precursor, and an aluminum precursor; The M2 precursor is a precursor containing one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), and zirconium (Zr).
11. The method of claim 10, wherein the nickel-based metal precursor has an internal pore area having a size of 2 to 7 μm.
12. The cobalt precursor is Co(OH). 2 , CoOOH, CoO, Co 2 O 3 , Co 3 O 4 , Co(OCOCH 3 ) 2 ・4H 2 O, CoCl 2 , Co(NO 3 ) 2 ・6H 2 O, CoSO 4 , Co(SO 4 ) 2 ・7H 2 11. The method for producing a positive electrode active material for a lithium secondary battery according to claim 10, wherein the active material is selected from the group consisting of fluorine, fluorine, arsenic, fluorine, iodine, fluor ...
13. The method for producing a positive electrode active material for a lithium secondary battery according to claim 10, wherein the nickel-based metal precursor is a compound represented by the following Chemical Formula 3, a compound represented by the following Chemical Formula 4, or a combination thereof: [Chemical formula 3] (N) 1-x-y 11 x 2. The y (10) 2 In Chemical Formula 3, M1 is one or more elements selected from Co, Mn, and Al; M2 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.6≦(1−x−y)<1, 0≦x<0.4, 0≦y<0.4, and the case where x and y are simultaneously 0 is excluded; [Chemical formula 4] (N 1-x-y M1 x M2 y )O In Chemical Formula 4, M1 is one or more elements selected from Co, Mn, and Al; M2 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.6≦(1−x−y)<1, 0≦x<0.4, 0≦y<0.4, and the case where x and y are simultaneously 0 is excluded.
14. The method for producing a positive electrode active material for a lithium secondary battery according to claim 10, wherein the nickel-based metal precursor is represented by a compound of the following formula 5, a compound of the following formula 6, or a combination thereof: [Chemical formula 5] Ni 1-x-y-z Co x M3 y M4 z (OH) 2 In Chemical Formula 5, M3 is one or more elements selected from Mn and Al; M4 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.6≦(1−x−y−z)<1, 0≦x<0.4, 0≦y<0.4, 0≦z<0.4, and the case where x, y, and z are simultaneously 0 is excluded; [Chemical formula 6] (N 1-x-y-z Co x M3 y M4 z )O In Chemical Formula 6, M3 is one or more elements selected from Mn and Al; M4 is one or more elements selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu) and zirconium (Zr); 0.6≦(1−x−y−z)<1, 0≦x<0.4, 0≦y<0.4, 0≦z<0.4, and the case where x, y, and z are simultaneously 0 is excluded.
15. The method for producing a positive electrode active material for a lithium secondary battery according to claim 10, wherein the nickel-based metal precursor and the lithium precursor are mixed so that a Li / Me (metals excluding Li) molar ratio is 0.9 or more and less than 1.
1.
16. The method for producing a positive electrode active material for a lithium secondary battery according to claim 10, wherein the lithium precursor is lithium hydroxide, lithium carbonate, lithium sulfate, lithium nitrate, or a combination thereof.
17. The method of claim 10, wherein the primary heat treatment is performed in an oxidizing gas atmosphere at 800° C. to 1,200° C.
18. The method of claim 10, wherein the second heat treatment is performed in an oxidizing gas atmosphere at 600 to 850°C.
19. A positive electrode for a lithium secondary battery comprising a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, The positive electrode for a lithium secondary battery, wherein the positive electrode active material layer comprises the positive electrode active material according to claim 1 .
20. The positive electrode according to claim 19 , A negative electrode; and an electrolyte interposed therebetween.