Film, member, transfer device, fixing device, and image forming device
A film with a high-density, high-glass transition temperature resin and specific siloxane compound content ensures enhanced oil repellency, addressing sea-island structure issues and improving transfer and cleaning performance in electrophotographic devices.
Patent Information
- Application Number
- JP2024047165
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-07
AI Technical Summary
Existing films containing siloxane compounds and resins face issues with maintaining high oil repellency due to low glass transition temperatures or the formation of sea-island structures on the film surface, leading to decreased performance.
A film comprising a siloxane compound with alkyl groups and a resin having a density of 1.1 g/cm³ or higher and a glass transition temperature of 150°C or more, with a siloxane compound content between 3% to 7% by mass, and a polysiloxane compound with methyl groups in side chains, enhances oil repellency by restricting the movement of the siloxane compound's main chain.
The film maintains high oil repellency under various temperatures and conditions, improving transfer and cleaning properties in electrophotographic devices by reducing peeling forces and maintaining transferability.
Smart Images

Figure 2024137923000004 
Figure 2024137923000005 
Figure 2024137923000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a film, a member, a transfer device, a fixing device, and an image forming apparatus. [Background technology]
[0002] In an image forming apparatus (such as a copier, a facsimile, or a printer) using an electrophotographic method, a toner image formed on the surface of an image carrier is transferred to the surface of a recording medium and fixed on the recording medium to form an image.
[0003] For example, Patent Document 1 discloses a water- and oil-repellent film comprising: a resin layer containing a silicone (excluding organosilsesquioxanes of a T2m+6(m≧1) structure) that does not have a fluorine atom in the side chain group R1 that is bonded to a silicon atom; and a water- and oil-repellent layer laminated on the resin layer and containing an organosilsesquioxane of a T2m+6(m≧1) structure that has a hydrocarbon group R2 that is bonded to a silicon atom, with at least a part of the organosilsesquioxane being exposed on the surface, wherein the silicone has Hansen solubility parameters of a dispersion term δD of 10 MPa1 / 2 or more and 15 MPa1 / 2 or less, a polarization term δP of 0 MPa1 / 2 or more and 5 MPa1 / 2 or less, and a hydrogen bond term δH of 0 MPa1 / 2 or more and 5 MPa1 / 2 or less, and the organosilsesquioxane is octamethylsilsesquioxane.
[0004] Patent Document 2 discloses "an electrophotographic member having a base and a surface layer, the surface layer containing a binder resin having an acrylic skeleton and a modified silicone compound having a polyether group and a hydroxyl group in one molecule, and the surface layer has an n-hexadecane contact angle of 30° or more." [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6801474 [Patent Document 2] Patent Publication No. 6305220 Summary of the Invention [Problem to be solved by the invention]
[0006] The object of the present invention is to provide a film containing a siloxane compound having an alkyl group and a resin, the film having a density of the resin being 1.1 g / cm 3 The object of the present invention is to provide a film which maintains high oil repellency compared to a film having a thickness of less than 100° C., a resin having a glass transition temperature of less than 150° C., or a film surface having a sea-island structure in which a siloxane compound is an island portion and a resin is a sea portion. [Means for solving the problem]
[0007] Means for solving the above problems include the following aspects. <1> A siloxane compound having an alkyl group and a density of 1.1 g / cm 3 and a resin having a glass transition temperature of 150°C or higher. <2> The siloxane compound is a polysiloxane compound having the alkyl group on at least a part of the side chain. <1> The film according to claim 1. <3> The polysiloxane compound is a siloxane compound having a methyl group on at least a part of the side chain. <2> The film according to claim 1. <4> The content of the siloxane compound in the resin is 3% by mass or more and 7% by mass or less. <1> ~ <3> 13. The film according to any one of claims 1 to 12. <5> The content of the siloxane compound in the resin is 3% by mass or more and 5% by mass or less. <4> The film according to claim 1. <6> the siloxane compound is a polysiloxane compound having the alkyl group in at least a part of its side chain, The content of the siloxane compound in the resin is 3% by mass or more and 5% by mass or less. <1> ~ <5> 13. The film according to any one of claims 1 to 12. <7> The density of the resin is 1.3 g / cm 3 That's all. <1> ~ <5> 13. The film according to any one of claims 1 to 12. <8> The density of the resin is 1.3 g / cm 3 That's all. <6> The film according to claim 1. <9> The glass transition temperature of the resin is 200° C. or higher. <1> ~ <8> 13. The film according to any one of claims 1 to 12. <10> The density of the resin is 1.3 g / cm 3 That's all. The glass transition temperature of the resin is 200° C. or higher. <1> ~ <9> 13. The film according to any one of claims 1 to 12. <11> The peel strength of the surface of the film at 25°C is 20 kPa or less. <1> ~ <10> 13. The film according to any one of claims 1 to 12. <12> The peel strength of the surface of the film at 140°C is 25 kPa or less. <1> ~ <11> 13. The film according to any one of claims 1 to 12. <13> The layers constituting the outer surface are: <1> ~ <12> 13. A member having the film according to any one of claims 1 to 12. <14> <13> an intermediate transfer body having an outer peripheral surface on which a toner image is transferred; a primary transfer device for primarily transferring a toner image formed on a surface of an image carrier onto a surface of the intermediate transfer body; a secondary transfer device that secondarily transfers the toner image transferred onto the surface of the intermediate transfer body onto a surface of a recording medium; A transfer device comprising: <15> An image carrier; a charging device for charging the surface of the image carrier; an electrostatic latent image forming device for forming an electrostatic latent image on a charged surface of the image carrier; a developing device that contains a developer containing a toner and develops an electrostatic latent image formed on the surface of the image carrier with the developer to form a toner image; transferring the toner image onto a surface of a recording medium; <14> A transfer device according to the present invention; a fixing device for fixing the toner image onto a surface of a recording medium; An image forming apparatus comprising: <16> A first rotating body and a second rotating body arranged in contact with an outer surface of the first rotating body, At least one of the first rotating body and the second rotating body, <13> A fixing device comprising the member described in claim 1. <17> An image carrier; a charging device for charging the surface of the image carrier; an electrostatic latent image forming device for forming an electrostatic latent image on a charged surface of the image carrier; a developing device that contains a developer containing a toner and develops an electrostatic latent image formed on the surface of the image carrier with the developer to form a toner image; a transfer device for transferring the toner image onto a surface of a recording medium; Fixing the toner image on the surface of a recording medium; <16> a fixing device according to the above; An image forming apparatus comprising: Effect of the Invention
[0008] <1> According to the invention, in a film containing a siloxane compound having an alkyl group and a resin, the density of the resin is 1.1 g / cm 3 The film provided maintains high oil repellency compared to the case where the glass transition temperature of the resin is less than 150° C., or a sea-island structure is observed on the film surface.
[0009] <2> or <3> According to the invention relating to the above, a film is provided which maintains high oil repellency as compared with a case in which the siloxane compound is a polysiloxane compound having alkyl groups or methyl groups only at the terminals.
[0010] <4> According to the present invention, a film is provided which maintains high oil repellency, compared to when the content of the siloxane compound relative to the resin is less than 3 mass % or more than 7 mass %. <5> According to the present invention, a film is provided which maintains high oil repellency, compared to when the content of the siloxane compound relative to the resin is less than 3 mass % or more than 5 mass %. <6> According to the invention, when the siloxane compound is a polysiloxane compound having an alkyl group at a terminal, a film that maintains high oil repellency is provided, compared to when the content of the siloxane compound relative to the resin is less than 3 mass % or more than 5 mass %.
[0011] <7> According to the invention, the density of the resin is 1.3 g / cm 3 In this case, a film that maintains high oil repellency is provided as compared to a case where the thickness is less than 100 nm. <8> According to the invention, the density of the resin is 1.3 g / cm 3 In this case, a film that maintains high oil repellency is provided as compared to a case where the thickness is less than 100 nm. <9> According to the present invention, a film is provided which maintains high oil repellency compared to a case in which the glass transition temperature of the resin is lower than 200°C. <10> According to the invention, the density of the resin is 1.3 g / cm 3 In comparison with the case where the glass transition temperature of the resin is less than 200° C., or the case where the glass transition temperature of the resin is less than 200° C., a film that maintains high oil repellency is provided.
[0012] <11> According to the present invention, a film is provided which maintains high oil repellency as compared with a film surface having a peel strength at 25° C. of more than 20 kPa. <12> According to the present invention, a film is provided which maintains high oil repellency as compared with a film surface having a peel strength of more than 25 kPa at 140°C.
[0013] <13> , <14> , <15> , <16> , and <17> According to the invention, there are provided a member that maintains high oil repellency in a film containing a siloxane compound having an alkyl group and a resin, compared to a resin having a density of less than 1.1 and a resin having a glass transition temperature of less than 150°C, a transfer device and an image forming device that include an intermediate transfer body made of the member, and a fixing device and an image forming device that include a rotating body made of the member. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a schematic configuration diagram illustrating an example of a fixing device according to a first embodiment of the present invention. [Diagram 2] FIG. 11 is a schematic configuration diagram illustrating an example of a fixing device according to a second embodiment of the present invention. [Diagram 3] FIG. 11 is a schematic configuration diagram illustrating an example of a fixing device according to a third embodiment of the present invention. [Figure 4] 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, the present embodiment, which is an example of the present invention, will be described. These descriptions and examples are merely illustrative of the embodiment, and do not limit the scope of the embodiment.
[0016] In the numerical ranges described in the present embodiment, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range described in the present embodiment. In addition, in the numerical ranges described in the present embodiment, the upper or lower limit of the numerical range may be replaced with a value shown in the examples. In this embodiment, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved. When the embodiment is described with reference to the drawings, the configuration of the embodiment is not limited to the configuration shown in the drawings. Furthermore, the size of the members in each drawing is conceptual, and the relative relationship between the sizes of the members is not limited to this. In this embodiment, each component may contain multiple types of corresponding substances. When referring to the amount of each component in the composition in this embodiment, if multiple types of substances corresponding to each component are present in the composition, the amount refers to the total amount of the multiple types of substances present in the composition, unless otherwise specified.
[0017] <Film> The film according to the present embodiment is a film comprising a siloxane compound having an alkyl group (hereinafter, also simply referred to as a "siloxane compound") and a siloxane having a density of 1.1 g / cm 3 and a resin having a glass transition temperature of 150° C. or higher.
[0018] The film according to the present embodiment maintains high oil repellency due to the above-mentioned configuration, and the reason for this is presumed to be as follows.
[0019] Siloxane compounds having alkyl groups are highly oil-repellent compounds, and have a higher dielectric constant than fluorine compounds. Therefore, compared to the use of fluorine compounds, the use of siloxane compounds is advantageous in terms of strength stability as well as imparting high oil repellency to the film. When the siloxane compound is added to the film, the alkyl groups are oriented on the film surface, imparting high oil repellency. However, when a film containing a siloxane compound is subjected to an external load such as heat, the main chain of the siloxane compound may rotate, causing the alkyl groups to move and sink into the resin, resulting in a decrease in oil repellency.
[0020] On the other hand, if a resin with high density and glass transition point is used as the resin to be applied to the film, the rotation of the main chain of the siloxane compound (i.e., the movement of the methyl group) is restricted, and the penetration of the alkyl group into the resin is suppressed. This maintains the oil repellency derived from the siloxane compound. This is because, even in an environment where the molecular motion of the resin and siloxane compound becomes intense at high temperatures, the rotation of the main chain of the siloxane compound (i.e., the movement of the methyl group) is similarly restricted, so that high oil repellency is maintained.
[0021] From the above, it is presumed that the film according to this embodiment maintains high oil repellency. In addition, it is believed that the restriction of the rotation of the main chain of the siloxane compound (i.e., the movement of the methyl group) is also manifested in an environment where the molecular motion of the resin and the siloxane compound becomes intense at high temperatures, and the film maintains high oil repellency even at high temperatures. In particular, since the film according to this embodiment has high oil repellency, when a member having the film according to this embodiment as a layer constituting the outer peripheral surface is applied to a transfer member (particularly an intermediate transfer member) for an electrophotographic device, the amount of residual toner after transfer is small, and the transfer member (particularly an intermediate transfer member) has excellent transferability (particularly transfer maintainability) as well as cleanability (particularly cleaning maintainability).
[0022] The film according to this embodiment will be described in detail below.
[0023] The film according to the present embodiment contains a siloxane compound and a resin, and may contain other additives as necessary.
[0024] (Siloxane compounds) As the siloxane compound, a siloxane compound having an alkyl group is applied. The siloxane compound having an alkyl group is a compound having two or more siloxane bonds [Si-O] and an alkyl group. From the viewpoint of maintaining and improving high oil repellency, the alkyl group contained in the siloxane compound is preferably an alkyl group having 1 to 2 carbon atoms, and more preferably a methyl group.
[0025] As the siloxane compound, a polysiloxane compound having an alkyl group on the side chain is suitable. The polysiloxane compound having an alkyl group on the side chain includes both those in which at least a part of the side chain is alkylated and those in which the entire side chain is alkylated. By applying a polysiloxane compound having an alkyl group on at least a part of the side chain (particularly a siloxane compound having a methyl group on at least a part of the side chain), it is possible to impart even higher oil repellency. In addition, high oil repellency is easily maintained. Examples of polysiloxane compounds having an alkyl group on the side chain include straight silicone oils such as dimethylpolysiloxane, methylphenylpolysiloxane, and methylhydrogenpolysiloxane; and modified silicone oils such as polyether-modified dimethylpolysiloxane, amino-modified dimethylpolysiloxane, epoxy-modified dimethylpolysiloxane, carboxyl-modified dimethylpolysiloxane, carbinol-modified dimethylpolysiloxane, fluorine-modified dimethylpolysiloxane, methacryl-modified dimethylpolysiloxane, mercapto-modified dimethylpolysiloxane, phenol-modified dimethylpolysiloxane, and polyester resin-modified dimethylpolysiloxane. Among these, from the viewpoint of improving oil repellency, the siloxane compound is preferably straight silicone oil, and more preferably dimethyl silicone.
[0026] Other examples of the siloxane compound include silsesquioxane.
[0027] The content of the siloxane compound is preferably from 3 to 7% by mass, more preferably from 3 to 5% by mass, and even more preferably from 4 to 5% by mass, based on the resin. When the content of the siloxane compound is within the above range, it is possible to impart even higher oil repellency. In addition, high oil repellency can be easily maintained.
[0028] (resin) The resin used has a density of 1.1 or more and a glass transition temperature (Tg) of 150° C. or more. High oil repellency is maintained by increasing the density and glass transition temperature of the resin. The density of the resin is 1.1 g / cm 3 More than 1.3 g / cm is preferable. 3 The above is more preferable. The glass transition temperature (Tg) of the resin is preferably 150° C. or higher, and more preferably 200° C. or higher.
[0029] The density of the resin is measured as follows. It is measured by the immersion method. After measuring the weight of the test piece, measure the weight of the test piece immersed in the immersion liquid. When the weight of the test piece is m1, the weight of the immersed test piece is m2, and the water density is ρL, the density of the test piece is calculated as ρ=m1 / (m1-m2)×ρL.
[0030] The glass transition temperature of a resin is measured as follows. The test piece is heated using a differential scanning calorimeter (DSC, manufactured by Shimadzu Corporation) to measure the reaction heat. The point at which the baseline of the heat quantity shifts is taken as the glass transition temperature.
[0031] Examples of the resin include polyimide resin (PI resin), polyamideimide resin (PAI resin), polyetherketone resin (e.g., aromatic polyetheretherketone resin, etc.), polyphenylene sulfide resin (PPS resin), polyetherimide resin (PEI resin), polyester resin, polystyrene resin, polyamide resin, polycarbonate resin, silicone resin, etc. It is preferable to select a resin that satisfies the above-mentioned density and glass transition temperature from among these resin types.
[0032] The resin should be selected according to the intended use of the film. For example, when the film is applied to a single-layer intermediate transfer belt, the resin is preferably an imide resin (that is, a resin containing a structural unit having an imide bond, preferably a polyimide resin), a polyether ether ketone (PEEK) resin, or the like. For example, when the film is applied to the outermost layer of a fixing belt, the resin is preferably an imide resin (that is, a resin containing a structural unit having an imide bond, preferably a polyimide resin), a polyether ether ketone (PEEK) resin, or the like.
[0033] Here, polyimide will be described as a representative resin. Examples of polyimide resins include imidized products of polyamic acids (precursors of polyimide resins), which are polymers of tetracarboxylic dianhydrides and diamine compounds. An example of the polyimide resin is a resin having a structural unit represented by the following general formula (I).
[0034] [ka]
[0035] In general formula (I), R 1 represents a tetravalent organic group, R 2 represents a divalent organic group. R 1 Examples of the tetravalent organic group represented by the formula (1) include an aromatic group, an aliphatic group, a cyclic aliphatic group, a group in which an aromatic group and an aliphatic group are combined, and groups in which these groups are substituted. Specific examples of the tetravalent organic group include residues of tetracarboxylic dianhydrides, which will be described later. R 2 Examples of the divalent organic group represented by the formula (1) include an aromatic group, an aliphatic group, a cyclic aliphatic group, a group in which an aromatic group and an aliphatic group are combined, and groups in which these groups are substituted. Specific examples of the divalent organic group include residues of diamine compounds described below.
[0036] Specific examples of tetracarboxylic dianhydrides used as raw materials for polyimide resins include pyromellitic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4-biphenyltetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxyphenyl)sulfonic dianhydride, perylene-3,4,9,10-tetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, and ethylenetetracarboxylic dianhydride.
[0037] Specific examples of diamine compounds used as raw materials for polyimide resins include 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 3,3'-dichlorobenzidine, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 1,5-diaminonaphthalene, m-phenylenediamine, p-phenylenediamine, 3,3'-dimethyl 4,4'-biphenyldiamine, benzidine, and 3,3'-dimethyl Benzidine, 3,3'-dimethoxybenzidine, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenylpropane, 2,4-bis(β-amino tert-butyl)toluene, bis(p-β-amino-tert-butylphenyl)ether, bis(p-β-methyl-δ-aminophenyl)benzene, bis-p-(1,1-dimethyl-5-amino-pentyl)benzene, 1-isopropyl-2,4-m-phenylenediamine, m-xylylenediamine, p-xylylenediamine, di(p -aminocyclohexyl)methane, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, diaminopropyltetramethylene, 3-methylheptamethylenediamine, 4,4-dimethylheptamethylenediamine, 2,11-diaminododecane, 1,2-bis-3-aminopropoxyethane, 2,2-dimethylpropylenediamine, 3-methoxyhexamethylenediamine, 2,5-dimethylheptamethylenediamine, Examples include 3-methylheptamethylenediamine, 5-methylnonamethylenediamine, 2,17-diaminoeicosadecane, 1,4-diaminocyclohexane, 1,10-diamino-1,10-dimethyldecane, 12-diaminooctadecane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, piperazine, H2N(CH2)3O(CH2)2O(CH2)NH2, H2N(CH2)3S(CH2)3NH2, and H2N(CH2)3N(CH3)2(CH2)3NH2.
[0038] The resin content is the amount that constitutes the main component of the film. Here, the amount that constitutes the main component of the film means the amount of the component that is present in the largest amount among the components contained in the film.
[0039] (Other additives) Other additives include well-known additives such as conductive agents, reinforcing agents, antioxidants, surfactants, and heat aging inhibitors, depending on the application of the film.
[0040] Here, a conductive agent will be described as a representative additive. Examples of conductive agents include carbon black, metals (e.g., aluminum, nickel, etc.), metal oxides (e.g., yttrium oxide, tin oxide, etc.), and ion-conductive substances (e.g., potassium titanate, LiCl, etc.). Of these, carbon black is preferred. These conductive agents may be used alone or in combination of two or more.
[0041] Examples of carbon black include ketjen black, oil furnace black, channel black (i.e., gas black), acetylene black, etc. Carbon black having a treated surface (hereinafter also referred to as "surface-treated carbon black") may be used. Surface-treated carbon black can be obtained by imparting, for example, a carboxy group, a quinone group, a lactone group, a hydroxy group, etc. to its surface. Examples of the surface treatment method include an air oxidation method in which the carbon black is reacted by contacting with air in a high-temperature atmosphere, a method in which the carbon black is reacted with nitrogen oxides or ozone at room temperature (e.g., 22°C), and a method in which the carbon black is oxidized with air in a high-temperature atmosphere and then oxidized with ozone at a low temperature.
[0042] Among these, channel black is preferable as the conductive agent, and acidic carbon black having a pH of 5.0 or less is particularly preferable. Examples of acidic carbon black include carbon black whose surface has been subjected to an oxidation treatment, such as carbon black obtained by providing a carboxyl group, a quinone group, a lactone group, a hydroxyl group, or the like to the surface. As the acidic carbon black, from the viewpoint of improving transferability to textured paper, a carbon black having a pH of 4.5 or less is preferred, a more preferred acidic carbon black having a pH of 4.0 or less, an even more preferred acidic carbon black having a pH of 3.0 or less, an especially preferred acidic carbon black having a pH of 2.0 to 3.0, and an extremely preferred acidic carbon black having a pH of 2.0 to 2.8. The pH of the acidic carbon black is a value measured by the pH measurement method specified in JIS Z8802 (2011).
[0043] The content of the conductive agent in the film is preferably 10% by mass or more and 50% by mass or less, more preferably 12% by mass or more and 40% by mass or less, even more preferably 14% by mass or more and 30% by mass or less, and particularly preferably 15% by mass or more and 20% by mass or less. I wish.
[0044] The peel strength of the surface of the film according to this embodiment at 25° C. is preferably 20 kPa or less, more preferably 19 kPa or less, and even more preferably 18.5 kPa or less. The peel strength of the surface of the film according to this embodiment at 140° C. is preferably 25 kPa or less, more preferably 24 kPa or less, and even more preferably 23.5 kPa or less. When the peel strength at 25° C. and 140° C. of the surface of the film according to this embodiment is within the above range, the film has high oil repellency from room temperature to high temperatures.
[0045] Here, the peel strength of the film surface at 25° C. and 150° C. is measured as follows. First, a sample piece measuring 3 cm x 4 cm is taken from the target test piece. Next, in an environment of 22°C and 15% RH, polyester resin particles were scattered on the surface of the film of the sample piece from above at a height of 15 cm in a state where a voltage of 10 kV was applied horizontally to the surface of the film, and 3 g / cm 2The polyester resin particles are scattered from 10 cm above the surface of the film so that they fall naturally under their own weight, and the surface of the film is attached with a load of 0 g / cm. 2 Attach with. The polyester resin particles used here are a polycondensation product of dimethyl fumarate, which is a dicarboxylic acid, and propylene glycol, which is a dialcohol, and have a weight average molecular weight of 25,000 and a volume average particle size of 4.7 μm. The polyester resin particles used are those that are substantially free of frictional contact with each other or with other members (such as a carrier) and are substantially free of frictional electrification. Specifically, the polyester resin particles used are those that have been stored for half a year after production in an environment of 10°C to 22°C and 10% RH to 55% RH. Next, the probe of a tack tester (TA-500, manufactured by UBM) heated to 25°C and 140°C is pressed against the center of the polyester resin particle-adhered surface of the test piece at a speed of 0.1 mm / s, and then the probe is held at a pressure of 3900 gf for 10 s and pulled up at a speed of 10 mm / s to measure the peel force.
[0046] <Materials> The member according to this embodiment has the film according to this embodiment as a layer that constitutes the outer peripheral surface. The member according to this embodiment may be either a single-layer member of the film according to the above-mentioned embodiment, or a member in which the film according to the above-mentioned embodiment is provided on a substrate.
[0047] When the member according to the present embodiment is applied to an intermediate transfer body for an electrophotographic image forming apparatus, the member can be a single layer of the film according to the present embodiment, or a laminate having the film as the outermost layer. In the laminate, layers other than the film (for example, a base layer on which the film is provided, an elastic layer provided between the film and the base layer, etc.) can be well-known layers provided in intermediate transfer bodies.
[0048] When the member according to the present embodiment is applied to a fixing member (heating member, pressure member, sliding member, etc.) for an electrophotographic image forming apparatus, the member may have a substrate, an elastic layer provided on the substrate, and a release layer provided on the elastic layer and composed of the film according to the present embodiment. The substrate and elastic layer may be a well-known substrate and elastic layer provided as a fixing member. The fixing member may also have a well-known metal heating layer for electromagnetic induction heating between the substrate and the elastic layer.
[0049] Examples of members according to the present embodiment include intermediate transfer members, fixing members, and also paper transport members for electrophotographic image forming apparatuses.
[0050] Here, as an example of a method for manufacturing a member according to the present embodiment, a method for manufacturing a single-layer type endless belt applied to an intermediate transfer member will be described below.
[0051] The endless belt can be obtained, for example, through a coating film forming step of applying a coating solution containing a composition for forming an endless belt to the surface of a cylindrical core (hereinafter referred to as a cylindrical core) that has been blasted and previously coated with a release agent to form a coating film, a tubular body forming step of heat-drying the coating film and subjecting it to a heat reaction to form a tubular body, and a peeling step of peeling the tubular body from the cylindrical core. In addition, other steps may be included as necessary.
[0052] Hereinafter, the method for manufacturing an endless belt will be described step by step. (1) Paint film formation process In the coating film forming process, the surface of the cylindrical core body to which the coating solution is applied is preferably roughened to an arithmetic mean roughness Ra in the range of 0.2 μm to 2 μm by using a roughening method such as blasting, cutting, or sandpapering.
[0053] In addition, it is preferable that the surface of the cylindrical core body is provided with releasability. To provide releasability, a method of coating the cylindrical core body with a fluorine-based resin or a silicone resin, a method of applying a release agent to the surface of the cylindrical core body, or the like can be used.
[0054] As a method for applying the coating solution to the cylindrical core body, known methods can be used, such as a dip coating method in which the cylindrical core body is immersed in the coating solution and raised (pulled up), a ring coating method in which the film thickness is controlled by a ring body, a flow coating method in which the coating solution is discharged onto the surface while rotating the cylindrical core body, and a blade coating method in which the coating film is metered with a blade. Note that the above-mentioned "applying to the cylindrical core body surface" refers to applying to the surface of a layer, if the cylindrical core body has a layer on its surface. Also, "raising the cylindrical core body" refers to the relative relationship with the liquid level at the time of application, and includes the case where "the cylindrical core body is stopped and the coating liquid level is lowered." Among the above coating methods, flow coating and blade coating are more preferable.
[0055] (2) Tubular body formation process In this step, the coating film is dried by heating and reacted by heating to form a tubular body on the surface of the cylindrical core body. The tubular body means a film obtained by removing the solvent from the coating film and reacting by heating.
[0056] First, in the tubular body forming step, in order to remove the solvent present in the coating film, the coating film is dried by heating to a degree that does not cause deformation even when left to stand. For example, when a polyamide-imide resin is used, the heating conditions are preferably a temperature range of 100°C to 180°C for 15 minutes to 60 minutes. Also, when a polyimide resin is used, the heating conditions are preferably a temperature range of 120°C to 200°C for 60 minutes to 60 minutes. Within the above temperature range, the higher the temperature, the shorter the heating time may be. In addition to heating, blowing air on the material is also effective. Heating may be performed by increasing the temperature stepwise or at a constant rate.
[0057] In addition, the above heat drying is preferably carried out so that 20% by mass to 50% by mass of the solvent remains in the coating film.
[0058] The process from the heat drying of the coating film to the heat reaction may be carried out continuously, but the temperature may be lowered once during the process. Here, "lowering the temperature" refers to cooling the coating film, which has been heated by heat drying, together with the cylindrical core body, to lower the temperature. Lowering the temperature is effective when the heat drying device that removes the solvent and the heat reaction device that heats the coating film are different. When the heat drying device and the heat reaction device are integrated, it is not necessary to lower the temperature once.
[0059] In the tubular body forming step, after the above-mentioned heat drying, the coating film is subjected to a heat reaction (baking) to form the tubular body. For example, when a polyamide-imide resin is used, the heating conditions for the heat reaction (baking) are preferably a temperature range of 200°C to 280°C for 60 minutes to 180 minutes. Also, when a polyimide resin is used, the heating conditions are preferably a temperature range of 300°C to 400°C for 100 minutes to 240 minutes. During the heating reaction, it is preferable to remove as much residual solvent as possible before the final heating temperature is reached. Specifically, it is preferable to remove residual solvent by heating and drying for 30 minutes to 100 minutes at a temperature range of 150°C to 250°C before heating, and then to heat the material by gradually increasing the temperature in stages or at a constant rate to form a tubular body.
[0060] (3) Peeling process After the heating reaction (firing), the cylindrical core body is cooled, and the formed tubular body is peeled off in the main step, whereby the endless belt according to the second embodiment can be obtained. Since a release agent is applied to the cylindrical core body in advance, the inner surface of the tubular body does not come into direct contact with the outer surface of the cylindrical core body, and the tubular body can be easily peeled off from the cylindrical core body to obtain an endless belt for an image forming device.
[0061] The endless belt thus removed may be subjected to a process of cutting off unnecessary portions at both ends thereof, and further to a process of punching holes, forming ribs, or the like.
[0062] <Transfer device> The transfer device according to this embodiment is an intermediate transfer member having an outer peripheral surface on which a toner image is transferred; a primary transfer device that primarily transfers a toner image formed on a surface of an image carrier onto a surface of an intermediate transfer body; a secondary transfer device that secondarily transfers the toner image transferred onto the surface of the intermediate transfer body onto the surface of a recording medium; Equipped with.
[0063] (Primary transfer device) In the primary transfer device, the primary transfer member is disposed opposite to the image carrier with the intermediate transfer body sandwiched therebetween. In the primary transfer device, the primary transfer member applies a voltage of a polarity opposite to the charge polarity of the toner to the intermediate transfer body, thereby performing primary transfer of the toner image onto the outer peripheral surface of the intermediate transfer body.
[0064] (Secondary transfer device) In the secondary transfer device, the secondary transfer member is disposed on the toner image carrying side of the intermediate transfer body. The secondary transfer device includes, for example, a backing member disposed on the opposite side of the intermediate transfer body to the toner image carrying side together with the secondary transfer member. In the secondary transfer device, the intermediate transfer body and the recording medium are sandwiched between the secondary transfer member and the backing member to form a transfer electric field, whereby the toner image on the intermediate transfer body is secondarily transferred to the recording medium. The secondary transfer member may be a secondary transfer roll or a secondary transfer belt. The backing member may be, for example, a backing roll.
[0065] The transfer device according to the present embodiment may be a transfer device that transfers a toner image onto a surface of a recording medium via multiple intermediate transfer bodies. In other words, the transfer device may be, for example, a transfer device that performs primary transfer of a toner image from an image carrier to a first intermediate transfer body, and then performs secondary transfer of the toner image from the first intermediate transfer body to a second intermediate transfer body, and then performs tertiary transfer of the toner image from the second intermediate transfer body to a recording medium. The transfer device applies an intermediate transfer body made of the member according to the present embodiment to at least one of a plurality of intermediate transfer bodies.
[0066] <Fixing material> The fixing member according to the present embodiment is A first rotating body and a second rotating body arranged in contact with an outer surface of the first rotating body, At least one of the first rotating body and the second rotating body is configured from the member according to the present embodiment.
[0067] Below, the fixing device according to this embodiment will be described in the following manner: as a first embodiment, a fixing device equipped with a heating roll and a pressure belt; as a second embodiment, a fixing device equipped with a heating belt and a heating roll; and as a third embodiment, a fixing device using an electromagnetic induction heating method equipped with a heating belt and a heating roll. The fixing device according to the present embodiment is not limited to the first to third embodiments, and may be a fixing device including a heating roll or a heating belt and a pressure belt. In the fixing device according to this embodiment, the member according to this embodiment may be applied to any of the pressure roll, the heating belt, the pressure roll, and the pressure belt.
[0068] (First embodiment of fixing device) A first embodiment of the fixing device will be described with reference to Fig. 1. Fig. 1 is a schematic diagram showing an example of the first embodiment of the fixing device (that is, fixing device 60).
[0069] As shown in FIG. 1, the fixing device 60 is configured to include, for example, a rotating heating roll 61 (an example of a first rotating body), a pressure belt 62 (an example of a second rotating body), and a pressure pad 64 (an example of a pressing member) that presses the heating roll 61 via the pressure belt 62. The pressing pad 64 may be configured to press the pressure belt 62 and the heating roll 61 relatively. Therefore, the pressure belt 62 side may be pressed against the heating roll 61, or the heating roll 61 side may be pressed against the pressure belt 62.
[0070] A halogen lamp 66 (an example of a heating device) is disposed inside the heating roll 61. The heating device is not limited to a halogen lamp, and other heat-generating members may be used.
[0071] On the other hand, for example, a temperature sensor 69 is arranged in contact with the surface of the heating roll 61. Based on the temperature measurement value by this temperature sensor 69, the lighting of the halogen lamp 66 is controlled, and the surface temperature of the heating roll 61 is maintained at a target set temperature (for example, 150°C).
[0072] The pressure belt 62 is rotatably supported by, for example, a pressure pad 64 and a belt running guide 63 disposed inside the pressure belt 62. The pressure belt 62 is disposed so as to be pressed against the heating roll 61 by the pressure pad 64 in a sandwiching region N (nip portion).
[0073] The pressure pad 64 is disposed, for example, inside the pressure belt 62 in a state where it is pressed by the heating roll 61 via the pressure belt 62, and forms a sandwiching region N between the pressure pad 64 and the heating roll 61. The pressure pad 64, for example, has a front clamping member 64a arranged on the entrance side of the clamping area N to ensure a wide clamping area N, and a peeling clamping member 64b arranged on the exit side of the clamping area N to impart distortion to the heating roll 61.
[0074] In order to reduce the sliding resistance between the inner circumferential surface of the pressure belt 62 and the pressure pad 64, for example, a sheet-like sliding member 68 is provided on the surfaces of the front clamping member 64a and the peeling clamping member 64b that come into contact with the pressure belt 62. The pressure pad 64 and the sliding member 68 are held by a holding member 65 made of metal. The sliding member 68 is provided, for example, so that its sliding surface comes into contact with the inner circumferential surface of the pressure belt 62 , and is involved in the retention and supply of oil present between the sliding member 68 and the pressure belt 62 .
[0075] For example, a belt running guide 63 is attached to the holding member 65, and the pressure belt 62 rotates.
[0076] The heating roll 61 is rotated in the direction of arrow S by, for example, a drive motor (not shown), and the pressure belt 62 is driven by this rotation to rotate in the direction of arrow R, which is opposite to the rotation direction of the heating roll 61. That is, for example, while the heating roll 61 rotates in the clockwise direction in FIG. 1, the pressure belt 62 rotates in the counterclockwise direction.
[0077] Then, the paper K (an example of a recording medium) having the unfixed toner image thereon is guided, for example, by the fixing entrance guide 56 and conveyed to the pinch region N. Then, when the paper K passes through the pinch region N, the unfixed toner image on the paper K is fixed by the pressure and heat acting on the pinch region N.
[0078] In the fixing device 60, for example, the front pinch member 64a having a concave shape conforming to the outer circumferential surface of the heating roll 61 ensures a wider pinch region N than in a configuration without the front pinch member 64a.
[0079] In addition, in the fixing device 60, for example, by arranging the peeling and pinching member 64b so as to protrude from the outer circumferential surface of the heating roll 61, the distortion of the heating roll 61 is locally increased in the exit area of the pinching region N.
[0080] By arranging the peeling and pinching member 64b in this manner, for example, when the paper K after fixing passes through the peeling and pinching area, it passes through a locally large distortion, making it easier for the paper K to peel off from the heating roll 61.
[0081] As an auxiliary device for peeling, for example, a peeling member 70 is disposed downstream of the pinching region N of the heating roll 61. The peeling member 70 is held by a holding member 72 in a state in which a peeling claw 71 is adjacent to the heating roll 61 in a direction opposite to the rotation direction of the heating roll 61 (counter direction), for example.
[0082] (Second embodiment of fixing device) A second embodiment of the fixing device will be described with reference to Fig. 2. Fig. 2 is a schematic diagram showing an example of the second embodiment of the fixing device (that is, fixing device 80).
[0083] 2, the fixing device 80 includes, for example, a fixing belt module 86 equipped with a heating belt 84 (an example of a first rotating body), and a pressure roll 88 (an example of a second rotating body) arranged to press against the heating belt 84 (fixing belt module 86). For example, a pinch region N (nip portion) is formed at the contact portion between the heating belt 84 (fixing belt module 86) and the pressure roll 88. In the pinch region N, a sheet K (an example of a recording medium) is pressurized and heated, and a toner image is fixed.
[0084] The fixing belt module 86 includes, for example, an endless heating belt 84, a heating pressure roll 89 around which the heating belt 84 is wound on the pressure roll 88 side and which is rotated by the rotational force of a motor (not shown) and presses the heating belt 84 from its inner surface against the pressure roll 88 side, and a support roll 90 which supports the heating belt 84 from the inside at a position different from the heating pressure roll 89. The fixing belt module 86 includes, for example, a support roll 92 arranged on the outside of the heating belt 84 to define its rotational path, a posture correction roll 94 to correct the posture of the heating belt 84 from the heating pressure roll 89 to the support roll 90, and a support roll 98 to apply tension to the heating belt 84 from its inner surface downstream of the clamping area N formed by the heating belt 84 and the pressure roll 88.
[0085] The fixing belt module 86 is provided, for example, between the heating belt 84 and the heating pressure roll 89 so that a sheet-like sliding member 82 is interposed. The sliding member 82 is provided, for example, so that its sliding surface comes into contact with the inner circumferential surface of the heating belt 84 , and is involved in the retention and supply of oil present between the sliding member 82 and the heating belt 84 . Here, the sliding member 82 is provided in a state in which both ends thereof are supported by supporting members 96, for example.
[0086] Inside the heating and pressing roll 89, for example, a halogen heater 89A (one example of a heating device) is provided.
[0087] The support roll 90 is, for example, a cylindrical roll made of aluminum, and has a halogen heater 90A (an example of a heating device) disposed therein so as to heat the heating belt 84 from the inner circumferential surface side. At both ends of the support roll 90, for example, spring members (not shown) are provided to press the heating belt 84 outward.
[0088] The support roll 92 is a cylindrical roll made of, for example, aluminum, and a release layer made of fluororesin having a thickness of 20 μm is formed on the surface of the support roll 92 . The release layer of the support roll 92 is formed, for example, to prevent toner and paper powder from the outer circumferential surface of the heating belt 84 from accumulating on the support roll 92 . Inside the support roll 92, for example, a halogen heater 92A (one example of a heating device) is disposed, and the heating belt 84 is heated from the outer circumferential surface side.
[0089] That is, for example, the heating belt 84 is heated by a heating pressure roll 89 and a supporting roll 90 and a supporting roll 92 .
[0090] The posture correction roll 94 is, for example, a cylindrical roll made of aluminum, and an end position measuring mechanism (not shown) that measures the end position of the heating belt 84 is disposed near the posture correction roll 94. The posture correction roll 94 is provided with, for example, an axial displacement mechanism (not shown) that displaces the contact position in the axial direction of the heating belt 84 in accordance with the measurement results of the end position measuring mechanism, and is configured to control the meandering of the heating belt 84.
[0091] On the other hand, the pressure roll 88 is, for example, supported rotatably and is provided so as to be pressed against the portion where the heating belt 84 is wound around the heating pressure roll 89 by a biasing device such as a spring (not shown). As a result, as the heating belt 84 (heating pressure roll 89) of the fixing belt module 86 rotates in the direction of arrow S, the pressure roll 88 rotates in the direction of arrow R, following the heating belt 84 (heating pressure roll 89).
[0092] Then, the paper K having an unfixed toner image (not shown) is transported in the direction of arrow P and guided to a pinch area N of the fixing device 80. Then, when the paper K passes through the pinch area N, the unfixed toner image on the paper K is fixed by pressure and heat acting on the pinch area N.
[0093] In the fixing device 80, a form in which a halogen heater (halogen lamp) is applied as an example of a plurality of heating devices has been described, but the present invention is not limited to this, and a radiant lamp heating element (a heating element that emits radiation (infrared rays, etc.)) other than a halogen heater, or a resistive heating element (a heating element that generates Joule heat by passing a current through a resistor: for example, a film having resistance formed on a ceramic substrate and then fired) may also be applied.
[0094] (Third embodiment of fixing device) A fixing device according to a third embodiment will be described with reference to Fig. 3. Fig. 3 is a schematic diagram showing an example of the fixing device according to the third embodiment (that is, fixing device 200).
[0095] As shown in FIG. 3, fixing device 200 is an electromagnetic induction type fixing device including belt 220 having a metal layer. In the fixing device 200, a pressure roll (pressure member) 211 is disposed so as to pressurize a part of the belt 220, and from the viewpoint of efficient fixing, a contact area (nip) is formed between the belt 220 and the pressure roll 211, and the belt 220 is curved in a shape that follows the circumferential surface of the pressure roll 211. Also, from the viewpoint of ensuring the peelability of the recording medium, a bent portion where the belt is bent is formed at the end of the contact area (nip).
[0096] The pressure roll 211 is configured such that an elastic layer 211B made of silicone rubber or the like is formed on a base material 211A, and a release layer 211C made of a fluorine-based compound is further formed on the elastic layer 211B.
[0097] An opposing member 213 is disposed on the inner side of the belt 220 at a position opposing the pressure roll 211. The opposing member 213 is made of metal, heat-resistant resin, heat-resistant rubber, or the like, and has a pad 213B that comes into contact with the inner circumferential surface of the belt 220 to locally increase pressure, and a support 213A that supports the pad 213B.
[0098] An electromagnetic induction heating device 212 incorporating an electromagnetic induction coil (excitation coil) 212a is provided at a position facing the pressure roll 211 (an example of a pressure member) with the belt 220 at the center. The electromagnetic induction heating device 212 applies an alternating current to the electromagnetic induction coil, thereby changing the generated magnetic field with an excitation circuit and generating an eddy current in a metal layer (not shown) of the belt 220 (for example, an electromagnetic induction metal layer). This eddy current is converted into heat (Joule heat) by the electrical resistance of the metal layer (not shown), and as a result, the surface of the belt 220 generates heat. The position of the electromagnetic induction heating device 212 is not limited to the position shown in FIG. 3, and may be installed, for example, on the upstream side of the contact area of the belt 220 in the rotation direction B, or may be installed on the inside of the belt 220.
[0099] In the fixing device 200, a driving force is transmitted from a driving device to a gear fixed to the end of the belt 220, causing the belt 220 to rotate by itself in the direction of arrow B, and as the belt 220 rotates, the pressure roll 211 rotates in the opposite direction, i.e., in the direction of arrow C. The recording medium 215 on which the unfixed toner image 214 is formed is passed through a contact area (nip) between the belt 220 and the pressure roll 211 in the fixing device 200 in the direction of arrow A, and the unfixed toner image 214 is fixed to the recording medium 215 by applying pressure to the molten toner image 214.
[0100] <Image forming device> Next, the image forming apparatus according to the present embodiment will be described. The image forming apparatus according to the present embodiment includes: The image carrier includes an image holder, a charging device that charges the surface of the image carrier, an electrostatic latent image forming device that forms an electrostatic latent image on the surface of the charged image carrier, a developing device that contains a developer containing toner and uses the developer to develop the electrostatic latent image formed on the surface of the image carrier to form a toner image, a transfer device that transfers the toner image to the surface of a recording medium, and a fixing device that fixes the toner image to the surface of the recording medium. As the transfer device, the transfer device according to this embodiment is applied. As the fixing device, the fixing device according to the present embodiment is applied.
[0101] Here, in the image forming apparatus according to the present embodiment, the transfer device and the fixing device may each be made into a cartridge so as to be detachably attached to the image forming apparatus, i.e., the image forming apparatus according to the present embodiment may each include the transfer device according to the present embodiment and the fixing device according to the present embodiment as components of a process cartridge.
[0102] Hereinafter, an image forming apparatus according to the present embodiment will be described with reference to the drawings. FIG. 4 is a schematic diagram showing the configuration of the image forming apparatus according to the present embodiment.
[0103] 4, the image forming apparatus 100 according to the present embodiment is, for example, an intermediate transfer type image forming apparatus generally called a tandem type, and includes a plurality of image forming units 1Y, 1M, 1C, and 1K in which toner images of each color component are formed by an electrophotographic method, a primary transfer section 10 that sequentially transfers (primary transfer) the toner images of each color component formed by each image forming unit 1Y, 1M, 1C, and 1K onto an intermediate transfer belt 15, a secondary transfer section 20 that collectively transfers (secondary transfer) the superimposed toner images transferred onto the intermediate transfer belt 15 onto a recording medium, paper K, and a fixing device 60 that fixes the secondarily transferred image onto the paper K. The image forming apparatus 100 also has a control section 40 that controls the operation of each device (each section).
[0104] Each of the image forming units 1Y, 1M, 1C, and 1K of the image forming apparatus 100 includes a photoconductor 11 that rotates in the direction of arrow A as an example of an image carrier that carries a toner image formed on its surface.
[0105] Around the photoconductor 11, there is provided a charger 12 as an example of a charging device that charges the photoconductor 11, and there is provided a laser exposure device 13 (the exposure beam is indicated by the symbol Bm in the figure) as an example of an electrostatic latent image forming device that writes an electrostatic latent image on the photoconductor 11.
[0106] In addition, around the photoconductor 11, there is provided a developing device 14 as an example of a developing device, which contains toner of each color component and makes the electrostatic latent image on the photoconductor 11 visible using the toner, and there is provided a primary transfer roll 16 which transfers the toner image of each color component formed on the photoconductor 11 to an intermediate transfer belt 15 at the primary transfer section 10.
[0107] Furthermore, a photoreceptor cleaner 17 that removes residual toner on the photoreceptor 11 is provided around the photoreceptor 11, and electrophotographic devices including a charger 12, a laser exposure device 13, a developer 14, a primary transfer roll 16, and the photoreceptor cleaner 17 are sequentially arranged along the rotation direction of the photoreceptor 11. These image forming units 1Y, 1M, 1C, and 1K are arranged in a substantially linear fashion in the order of yellow (Y), magenta (M), cyan (C), and black (K) from the upstream side of the intermediate transfer belt 15.
[0108] The intermediate transfer belt 15, which is an intermediate transfer body, is a film-like pressure belt that has a base layer of resin such as polyimide or polyamide and contains an appropriate amount of antistatic agent such as carbon black. 6 Ωcm or more 10 14 It is formed to have a resistivity of Ωcm or less, and its thickness is, for example, about 0.1 mm.
[0109] The intermediate transfer belt 15 is driven (rotated) in a circular manner by various rolls at a speed suited to the purpose in the direction of the arrow B shown in Fig. 4. The various rolls include a drive roll 31 driven by a motor (not shown) excellent in constant speed performance to rotate the intermediate transfer belt 15, a support roll 32 supporting the intermediate transfer belt 15 extending in a substantially straight line along the arrangement direction of the photoconductors 11, a tensioning roll 33 that applies tension to the intermediate transfer belt 15 and functions as a correction roll to prevent the intermediate transfer belt 15 from meandering, a back roll 25 provided in the secondary transfer unit 20, and a cleaning back roll 34 provided in a cleaning unit that scrapes off residual toner on the intermediate transfer belt 15.
[0110] The primary transfer section 10 is composed of a primary transfer roll 16 arranged opposite the photoconductor 11 with an intermediate transfer belt 15 sandwiched therebetween. The primary transfer roll 16 is composed of a core body and a sponge layer as an elastic layer fixed to the periphery of the core body. The core body is a cylindrical rod made of a metal such as iron or SUS. The sponge layer is formed of a blend rubber of NBR, SBR and EPDM mixed with a conductive agent such as carbon black, and has a volume resistivity of 10 7.5 Ωcm or more 10 8.5 It is a sponge-like cylindrical roll with a surface resistance of less than Ωcm.
[0111] The primary transfer roll 16 is arranged in pressure contact with the photoconductor 11 with the intermediate transfer belt 15 sandwiched therebetween, and furthermore, a voltage (primary transfer bias) of the opposite polarity to the charge polarity of the toner (negative polarity; the same applies below) is applied to the primary transfer roll 16. As a result, the toner images on the photoconductors 11 are electrostatically attracted to the intermediate transfer belt 15 in sequence, and superimposed toner images are formed on the intermediate transfer belt 15.
[0112] The secondary transfer unit 20 includes a back roll 25 and a secondary transfer roll 22 that is disposed on the toner image bearing surface side of the intermediate transfer belt 15 .
[0113] The back roll 25 is made of a tube of EPDM and NBR blend rubber with carbon dispersed on the surface, and the inside is made of EPDM rubber. 7 Ω / □ or more 10 10 The hardness is set to, for example, 70° (Asker C: manufactured by Kobunshi Keiki Co., Ltd., the same applies below.) The back roll 25 is disposed on the back side of the intermediate transfer belt 15 to constitute an opposing electrode of the secondary transfer roll 22, and is in contact with a metallic power supply roll 26 to which a secondary transfer bias is stably applied.
[0114] On the other hand, the secondary transfer roll 22 is composed of a core body and a sponge layer as an elastic layer fixed around the core body. The core body is a cylindrical rod made of a metal such as iron or SUS. The sponge layer is made of a blend rubber of NBR, SBR and EPDM mixed with a conductive agent such as carbon black, and has a volume resistivity of 10 7.5 Ωcm or more 10 8.5 It is a sponge-like cylindrical roll with a surface resistance of less than Ωcm.
[0115] The secondary transfer roll 22 is placed in pressure contact with the back roll 25 with the intermediate transfer belt 15 sandwiched therebetween, and further, the secondary transfer roll 22 is grounded to form a secondary transfer bias between the secondary transfer roll 22 and the back roll 25, thereby secondarily transferring the toner image onto the paper K transported to the secondary transfer section 20.
[0116] In addition, downstream of the secondary transfer section 20 of the intermediate transfer belt 15, an intermediate transfer belt cleaner 35 that removes residual toner and paper dust on the intermediate transfer belt 15 after the secondary transfer and cleans the surface of the intermediate transfer belt 15 is provided so as to be freely movable toward and away from the intermediate transfer belt 15.
[0117] The intermediate transfer belt 15, the primary transfer section 10 (the primary transfer roll 16), and the secondary transfer section 20 (the secondary transfer roll 22) correspond to an example of a transfer device.
[0118] Meanwhile, upstream of the yellow image forming unit 1Y, there is provided a reference sensor (home position sensor) 42 that generates a reference signal that serves as a reference for timing image formation in each of the image forming units 1Y, 1M, 1C, and 1K. This reference sensor 42 generates a reference signal by recognizing a mark provided on the back side of the intermediate transfer belt 15, and each of the image forming units 1Y, 1M, 1C, and 1K is configured to start image formation in response to an instruction from the control unit 40 based on the recognition of this reference signal. Further, an image density sensor 43 for adjusting image quality is disposed downstream of the black image forming unit 1K.
[0119] Furthermore, in the image forming apparatus according to this embodiment, as a transport device for transporting paper K, there are provided a paper storage section 50 for storing paper K, a paper feed roll 51 for taking out and transporting paper K accumulated in the paper storage section 50 at a predetermined timing, a transport roll 52 for transporting paper K fed by the paper feed roll 51, a transport guide 53 for sending paper K transported by the transport roll 52 to the secondary transfer section 20, a transport belt 55 for transporting paper K transported after secondary transfer by the secondary transfer roll 22 to the fixing device 60, and a fixing entrance guide 56 for guiding paper K to the fixing device 60.
[0120] Next, a basic image forming process of the image forming apparatus according to this embodiment will be described. In the image forming apparatus of this embodiment, image data output from an image reading device (not shown) or a personal computer (PC) (not shown), etc., is subjected to image processing by an image processing device (not shown), and then image formation is performed by image forming units 1Y, 1M, 1C, and 1K.
[0121] The image processing device performs image processing on the input image data, such as shading correction, positional deviation correction, brightness / color space conversion, gamma correction, and various image editing such as frame erasure, color editing, and movement editing. The image data that has undergone image processing is converted into color material gradation data of four colors, Y, M, C, and K, and is output to the laser exposure device 13.
[0122] In the laser exposure device 13, an exposure beam Bm emitted from, for example, a semiconductor laser is irradiated onto the photoconductor 11 of each of the image forming units 1Y, 1M, 1C, and 1K in accordance with the input color material gradation data. In each of the photoconductors 11 of the image forming units 1Y, 1M, 1C, and 1K, the surface is charged by the charger 12, and then the surface is scanned and exposed by the laser exposure device 13 to form an electrostatic latent image. The formed electrostatic latent image is developed into a toner image of each color of Y, M, C, and K by each of the image forming units 1Y, 1M, 1C, and 1K.
[0123] The toner images formed on the photoconductors 11 of the image forming units 1Y, 1M, 1C, and 1K are transferred onto the intermediate transfer belt 15 in the primary transfer section 10 where each photoconductor 11 comes into contact with the intermediate transfer belt 15. More specifically, in the primary transfer section 10, a voltage (primary transfer bias) of the opposite polarity to the charging polarity (negative polarity) of the toner is applied to the base material of the intermediate transfer belt 15 by the primary transfer roll 16, and the toner images are sequentially superimposed on the surface of the intermediate transfer belt 15 to perform the primary transfer.
[0124] After the toner images are sequentially primarily transferred onto the surface of the intermediate transfer belt 15, the intermediate transfer belt 15 moves to transport the toner images to the secondary transfer unit 20. When the toner images are transported to the secondary transfer unit 20, in the transport device, the paper feed roll 51 rotates in accordance with the timing at which the toner images are transported to the secondary transfer unit 20, and paper K of the desired size is supplied from the paper storage unit 50. The paper K supplied by the paper feed roll 51 is transported by the transport roll 52 and reaches the secondary transfer unit 20 via the transport guide 53. Before reaching the secondary transfer unit 20, the paper K is temporarily stopped, and a positioning roll (not shown) rotates in accordance with the movement timing of the intermediate transfer belt 15 on which the toner images are held, thereby aligning the position of the paper K with the position of the toner image.
[0125] In the secondary transfer section 20, the secondary transfer roll 22 is pressed against the back roll 25 via the intermediate transfer belt 15. At this time, the paper K, which has been transported in time, is sandwiched between the intermediate transfer belt 15 and the secondary transfer roll 22. At this time, when a voltage (secondary transfer bias) of the same polarity as the charging polarity (negative polarity) of the toner is applied from the power supply roll 26, a transfer electric field is formed between the secondary transfer roll 22 and the back roll 25. Then, the unfixed toner images held on the intermediate transfer belt 15 are electrostatically transferred collectively onto the paper K in the secondary transfer section 20, which is pressed by the secondary transfer roll 22 and the back roll 25.
[0126] Thereafter, the paper K onto which the toner image has been electrostatically transferred is transported as it is after being peeled off from the intermediate transfer belt 15 by the secondary transfer roll 22, and is transported to a transport belt 55 provided downstream of the secondary transfer roll 22 in the paper transport direction. The transport belt 55 transports the paper K to the fixing device 60 at an optimal transport speed for the fixing device 60. The unfixed toner image on the paper K transported to the fixing device 60 is fixed onto the paper K by being subjected to a fixing process using heat and pressure by the fixing device 60. The paper K on which the fixed image has been formed is then transported to an ejected paper storage section (not shown) provided in the ejection section of the image forming apparatus.
[0127] On the other hand, after the transfer to the paper K is completed, the residual toner remaining on the intermediate transfer belt 15 is transported to the cleaning section as the intermediate transfer belt 15 rotates, and is removed from the intermediate transfer belt 15 by the cleaning back roll 34 and the intermediate transfer belt cleaner 35.
[0128] Although the present embodiment has been described above, the present invention is not limited to the above embodiment, and various modifications, changes, and improvements are possible. EXAMPLES
[0129] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.
[0130] <Example A1> (1st step) A solution was prepared by adding polyether-modified dimethylpolysiloxane (KP-126, manufactured by Shin-Etsu Chemical Co., Ltd.) as a siloxane compound to polyamic acid of polyimide varnish (manufactured by JFE Chemical Co., Ltd., JIV300R, solid content rate of 18 mass%) as a resin or resin precursor in the blending amount shown in Table 1. The prepared solution was dispersed by a high-pressure collision type disperser to obtain a coating liquid. (2nd process) The coating solution was applied to the substrate with a bar coater to a thickness of 100 μm. (3rd step) The coating was dried by heating at 140° C. for 30 minutes. (4th step) The dried coating was heated for 120 minutes at a maximum temperature of 320° C. to form a resin coating, thereby obtaining a film.
[0131] <Examples A2 to A8 and Example B1> A film was obtained in the same manner as in Example A1, except that the types of resin or resin precursor, and siloxane compound, and the amount of siloxane compound were changed according to Table 1.
[0132] <Example C1> (1st step) Polycarbonate (TS-2040, manufactured by Teijin) as the resin was dissolved in THF (tetrahydrofuran, manufactured by Mitsubishi Chemical) to prepare a coating solution with a solid content of 20%, and then polyether-modified dimethylpolysiloxane (KP-126, manufactured by Shin-Etsu Chemical Co., Ltd.) as a siloxane compound was added to the coating solution and kneaded. (2nd process) The obtained coating solution was applied to a substrate with a bar coater to a thickness of 100 μm. (3rd step) The coating was dried by heating at 140° C. for 30 minutes to obtain a film.
[0133] <Comparative Example A1> (1st step) A polyether-modified dimethylpolysiloxane (KP-126 manufactured by Shin-Etsu Chemical Co., Ltd.) was added as a siloxane compound to 100 parts by mass of polyether ether ketone (VICTREXPEEK manufactured by Victrex) as a resin, and after pre-blending in advance, the mixture was hot-melt kneaded using a twin-screw extruder (TEX30α manufactured by Japan Steel Works, Ltd.) to prepare a thermoplastic resin composition. The kneading temperature was adjusted to be within the range of 250°C or more and 300°C or less, and the hot-melt kneading time was approximately 5 minutes. (2nd process) The obtained thermoplastic resin composition was pelletized and dried for 6 hours at a temperature of 140° C. The dried thermoplastic resin composition in pellet form was then placed in an injection molding machine (SE180D manufactured by Sumitomo Heavy Industries, Ltd.). The cylinder temperature was set to 300° C., and the thermoplastic resin composition was injection molded into a mold whose temperature was controlled at 30° C. to form a film.
[0134] <Comparative examples A2, B1> A film was obtained in the same manner as in Comparative Example A1, except that the amounts of the resin and the siloxane compound were changed according to Table 1.
[0135] <Characteristics> The film properties shown in Table 1 were measured according to the methods described above.
[0136] <Evaluation> (Surface free energy of film surface at room temperature and high temperature) The surface free energy of the film surface of each example was measured when the film was at room temperature (25° C.) and when it was heated to a high temperature of 140° C. The evaluation criteria were as follows. A: Surface free energy is less than 26 mN / m B: Surface free energy is 26 mN / m or more and less than 30 N / m C: Surface free energy is 30 mN / m or more and less than 35 N / m D: Surface free energy is 35N / m or more
[0137] The abbreviations shown in Table 1 are as follows. -resin- PI1: Polyimide varnish (JFE Chemical Corporation, JIV300R) PI2: Polyimide varnish (Unitika Ltd., KX-H) PAI: Polyamide-imide (Hitachi Chemical Co., Ltd., HPC-9000) PC: Polycarbonate (Teijin Ltd., ST-2040) PEEK: Polyetheretherketone (VICTRIX PE EK) PS: Polystyrene (MW1C, manufactured by Toyo Styrol Co., Ltd.)
[0138] -Siloxane compounds- S1: Polyether modified dimethylpolysiloxane, Shin-Etsu Chemical Co., Ltd., KP-126 S2: Polyether modified dimethylpolysiloxane, Shin-Etsu Chemical Co., Ltd., KP-101
[0139] [Table 1]
[0140] From the above results, the film of this example has a higher thermal conductivity than the film of the comparative example at room temperature and at high temperature. It is clear that the free energy is low and the maintenance of the free energy is high. Therefore, it is clear that the film of this example can maintain high oil repellency compared to the film of the comparative example. Furthermore, it is clear that, compared to the films of the comparative examples, the films of the present examples can impart high oil repellency to the outer peripheral surface of a member by being applied as a layer constituting the outer peripheral surface of the member.
[0141] <Examples A101 to A108 and B101> In the first step of Examples A1 to A8 and B1, the prepared solutions and carbon black (FW200 manufactured by Cabot) were dispersed by a high-pressure collision type disperser to obtain coating solutions. The amount of carbon black relative to the resin or resin precursor was as shown in Table 2. Next, an aluminum cylinder was prepared as a cylindrical mold. Next, the coating solution was discharged onto the outer circumferential surface of the cylinder using a dispenser in a width of 500 mm, and the coating was then heated and dried at 140° C. for 30 minutes. Next, the cylinder on which the coating was formed was kept horizontal and the dried coating was heated to a maximum temperature of 320°C for 120 minutes to form a resin coating. Next, the mold was removed by hand, and the resin film was peeled off from the mold. Both widthwise ends of the resin film were cut off to obtain endless belts having the thicknesses shown in Table 2.
[0142] <Example C101> In the first step in Example C1, carbon black (FW200 manufactured by Cabot) was further added to the coating liquid and kneaded. The amount of carbon black relative to the resin was as shown in Table 2. Next, an aluminum cylinder was prepared as a cylindrical mold. Next, the coating solution was discharged onto the outer circumferential surface of the cylinder using a dispenser in a width of 500 mm, and the coating was then dried by heating at 140° C. for 30 minutes to obtain a resin coating. Next, the mold was removed by hand, and the resin film was peeled off from the mold. Both widthwise ends of the resin film were cut off to obtain endless belts having the thicknesses shown in Table 2.
[0143] <Comparative Examples A101 to A102 and B101> In Comparative Examples A1 to A2 and B1, carbon black (FW200 manufactured by Cabot) was further added to obtain a thermoplastic resin composition, and an endless belt having a thickness shown in Table 1 was obtained by injection molding. The amount of carbon black relative to the resin was as shown in Table 2.
[0144] <Evaluation> The endless belts of Examples A101 to A108, B101, and C101 and Comparative Examples A101 to A102 and B101 were mounted as intermediate transfer belts in an image forming apparatus "Versant 180 press (manufactured by Fujifilm Business Innovation Co., Ltd.)" and the following evaluations were carried out.
[0145] -Transcriptional stability- In an environment of 25°C temperature / 50% humidity, 2000 A4 size halftone images with an image density of 30% were printed, and the image density of the first sheet and the 2000th sheet were measured with an X-Rite938 (manufactured by X-Rite), measuring five points each and calculating the average value. The ratio (%) of the average image density of the 2000th sheet to the average image density of the first sheet was calculated as an index of transfer retention. Evaluation was then performed according to the following evaluation criteria. A: When the ratio (%) of the average image density of the 2000th sheet to the average image density of the first sheet is 95% or more, it is evaluated as no decrease in image density. B: When the ratio (%) of the average image density of the 2000th sheet to the average image density of the first sheet is 90% or more and less than 95%, it is evaluated that a decrease in image density has occurred. C: When the ratio (%) of the average image density of the 2000th sheet to the average image density of the first sheet is less than 90%, it is evaluated as a significant decrease in image density.
[0146] -Cleaning maintenance- After printing 2000 A4 size halftone images with an image density of 30% in an environment of 25°C temperature and 50% humidity, the intermediate transfer belt was removed from the device. The surface of the intermediate transfer belt was then visually observed and the occurrence of toner filming (the phenomenon in which toner sticks) was evaluated according to the following criteria. A: No toner filming occurs B: Toner filming occurs C: Significant toner filming occurs
[0147] [Table 2]
[0148] From the above results, it can be seen that the endless belt of this embodiment is superior in transferability (particularly transfer retention) and cleanability (particularly cleaning retention) when applied to an intermediate transfer belt, compared with the endless belt of the comparative example.
[0149] The present embodiment includes the following aspects. (((1))) A siloxane compound having an alkyl group and a density of 1.1 g / cm 3 and a resin having a glass transition temperature of 150°C or higher. (((2))) The film according to (((1))), wherein the siloxane compound is a polysiloxane compound having the alkyl group in at least a portion of its side chains. (((3))) The film according to (((2))), wherein the polysiloxane compound is a siloxane compound having methyl groups on at least a portion of the side chains. (((4))) The film according to any one of ((1))) to (((3))), wherein the content of the siloxane compound relative to the resin is 3% by mass or more and 7% by mass or less. (((5))) The content of the siloxane compound relative to the resin is 3% by mass or more and 5% by mass or less (((4))). (((6))) the siloxane compound is a polysiloxane compound having the alkyl group in at least a part of its side chain, The film according to any one of ((1))) to (((5))), wherein the content of the siloxane compound relative to the resin is 3% by mass or more and 5% by mass or less. (((7))) The density of the resin is 1.3 g / cm 3 The film according to any one of (((1))) to (((5))) above. (((8))) The density of the resin is 1.3 g / cm 3 The film according to (((6))) above. (((9))) The film according to any one of ((1))) to (((8))), wherein the resin has a glass transition temperature of 200° C. or higher. (((10))) The density of the resin is 1.3 g / cm 3 That's all. The film according to any one of ((1))) to (((9))), wherein the resin has a glass transition temperature of 200° C. or higher. (((11))) The film according to any one of (((1))) to (((10))), wherein the peel strength of the surface of the film at 25° C. is 20 kPa or less. (((12))) The film according to any one of ((1))) to (((11))), wherein the peel strength of the surface of the film at 140° C. is 25 kPa or less. (((13))) A member having the film according to any one of (((1))) to (((12))) as a layer constituting the outer peripheral surface. (((14))) an intermediate transfer body having an outer peripheral surface on which a toner image is transferred, the intermediate transfer body being constituted by the member described in (((13))); a primary transfer device for primarily transferring a toner image formed on a surface of an image carrier onto a surface of the intermediate transfer body; a secondary transfer device that secondarily transfers the toner image transferred onto the surface of the intermediate transfer body onto a surface of a recording medium; A transfer device comprising: (((15))) An image carrier; a charging device for charging the surface of the image carrier; an electrostatic latent image forming device for forming an electrostatic latent image on a charged surface of the image carrier; a developing device that contains a developer containing a toner and develops an electrostatic latent image formed on the surface of the image carrier with the developer to form a toner image; a transfer device according to (((14))) for transferring the toner image onto a surface of a recording medium; a fixing device for fixing the toner image onto a surface of a recording medium; An image forming apparatus comprising: (((16))) A first rotating body and a second rotating body arranged in contact with an outer surface of the first rotating body, A fixing device, wherein at least one of the first rotating body and the second rotating body is configured using the member described in (((13))). (((17))) An image carrier; a charging device for charging the surface of the image carrier; an electrostatic latent image forming device for forming an electrostatic latent image on a charged surface of the image carrier; a developing device that contains a developer containing a toner and develops an electrostatic latent image formed on the surface of the image carrier with the developer to form a toner image; a transfer device for transferring the toner image onto a surface of a recording medium; a fixing device according to (((16))) for fixing the toner image onto a surface of a recording medium; An image forming apparatus comprising:
[0150] The advantages of the above aspect are as follows. According to the invention of (((1))), in a film containing a siloxane compound having an alkyl group and a resin, the density of the resin is 1.1 g / cm 3 The film provided maintains high oil repellency compared to the case where the glass transition temperature of the resin is less than 150° C., or a sea-island structure is observed on the film surface.
[0151] According to the invention related to (((2))) or (((3))), a film is provided which maintains high oil repellency as compared with the case where the siloxane compound is a polysiloxane compound having alkyl groups or methyl groups only at the terminals.
[0152] According to the invention related to (((4))), a film is provided which maintains high oil repellency, compared to when the content of the siloxane compound relative to the resin is less than 3 mass % or more than 7 mass %. According to the invention related to (((5))), a film is provided which maintains high oil repellency, compared to when the content of the siloxane compound relative to the resin is less than 3 mass % or more than 5 mass %. According to the invention related to (((6))), when the siloxane compound is a polysiloxane compound having an alkyl group at a terminal, a film that maintains high oil repellency is provided, compared to when the content of the siloxane compound relative to the resin is less than 3 mass % or more than 5 mass %.
[0153] According to the invention related to (((7))), the density of the resin is 1.3 g / cm 3 In this case, a film that maintains high oil repellency is provided as compared to a case where the thickness is less than 100 nm. According to the invention related to (((8))), the density of the resin is 1.3 g / cm 3 In this case, a film that maintains high oil repellency is provided as compared to a case where the thickness is less than 100 nm. According to the invention related to (((9))), a film is provided which maintains high oil repellency compared to a case in which the glass transition temperature of the resin is lower than 200°C. According to the invention related to (((10))), the density of the resin is 1.3 g / cm 3 The film maintains high oil repellency compared to when the glass transition temperature of the resin is less than 200°C or when the glass transition temperature of the resin is less than 200°C. Provided.
[0154] According to the invention (((11))), a film is provided which maintains high oil repellency compared to a film surface having a peel strength at 25° C. of more than 20 kPa. According to the invention (((12))), a film is provided which maintains high oil repellency compared to a film surface having a peel strength of more than 25 kPa at 140°C.
[0155] According to the inventions relating to (((13))), (((14))), (((15))), (((16))), and (((17))), there are provided a member which maintains high oil repellency in a film containing a siloxane compound having an alkyl group and a resin, compared to a resin having a density of less than 1.1 and a resin having a glass transition temperature of less than 150°C, a transfer device and an image forming device which include an intermediate transfer body made of said member, and a fixing device and an image forming device which include a rotating body made of said member. [Explanation of symbols]
[0156] 60 Fixing device 62 Pressure Belt 63 Belt guide 64 Pressure Pad 64a Front clamping member 64b Peeling and clamping member 65 Retaining member 66 Halogen lamp 68 Sliding members 69 Thermosensor 70 Peeling member 71 Peeling Claw 72 Retaining member 80 Fixing device 82 Sliding member 84 Heating Belt 86 Fuser Belt Module 88 Pressure Roll 89A halogen heater 89 Heated pressure roll 90A halogen heater 90 Support Roll 92A halogen heater 92 Support Roll 94 Posture Correction Roll 96 Support member 98 Support Roll 100 Image forming device 200 Fixing device 211 Pressure Roll 212 Electromagnetic induction heating device
Claims
1. A siloxane compound having an alkyl group and a density of 1.1 g / cm 3 and a resin having a glass transition temperature of 150° C. or higher.
2. 2. The film according to claim 1, wherein the siloxane compound is a polysiloxane compound having the alkyl group in at least a portion of the side chain.
3. The film according to claim 2 , wherein the polysiloxane compound has a methyl group on at least a portion of the side chains.
4. The film according to claim 1 , wherein the content of the siloxane compound relative to the resin is 3% by mass or more and 7% by mass or less.
5. The film according to claim 4 , wherein the content of the siloxane compound relative to the resin is 3% by mass or more and 5% by mass or less.
6. the siloxane compound is a polysiloxane compound having the alkyl group in at least a part of its side chain, The film according to claim 1 , wherein the content of the siloxane compound relative to the resin is 3% by mass or more and 5% by mass or less.
7. The density of the resin is 1.3 g / cm 3 The film according to claim 1,
8. The density of the resin is 1.3 g / cm 3 The film according to claim 6, wherein
9. The film according to claim 1 , wherein the resin has a glass transition temperature of 200° C. or higher.
10. The density of the resin is 1.3 g / cm 3 That's all. The film according to claim 1 , wherein the resin has a glass transition temperature of 200° C. or higher.
11. 2. The film according to claim 1, wherein the peel strength of the surface of the film at 25° C. is 20 kPa or less.
12. 2. The film according to claim 1, wherein the peel strength of the surface of the film at 140° C. is 25 kPa or less.
13. A member having the film according to any one of claims 1 to 12 as a layer constituting an outer peripheral surface thereof.
14. an intermediate transfer member having an outer peripheral surface onto which a toner image is transferred, the intermediate transfer member being configured as described in claim 13; a primary transfer device for primarily transferring a toner image formed on a surface of an image carrier onto a surface of the intermediate transfer body; a secondary transfer device that secondarily transfers the toner image transferred onto the surface of the intermediate transfer body onto a surface of a recording medium; A transfer device comprising:
15. An image carrier; a charging device for charging the surface of the image carrier; an electrostatic latent image forming device for forming an electrostatic latent image on a charged surface of the image carrier; a developing device that contains a developer containing a toner and develops an electrostatic latent image formed on the surface of the image carrier with the developer to form a toner image; A transfer device according to claim 14 for transferring the toner image onto a surface of a recording medium; a fixing device for fixing the toner image onto a surface of a recording medium; An image forming apparatus comprising:
16. A first rotating body and a second rotating body arranged in contact with an outer surface of the first rotating body, A fixing device, wherein at least one of the first rotating body and the second rotating body is configured with the member according to claim 13 .
17. An image carrier; a charging device for charging the surface of the image carrier; an electrostatic latent image forming device for forming an electrostatic latent image on a charged surface of the image carrier; a developing device that contains a developer containing a toner and develops an electrostatic latent image formed on the surface of the image carrier with the developer to form a toner image; a transfer device for transferring the toner image onto a surface of a recording medium; The fixing device according to claim 16, which fixes the toner image onto a surface of a recording medium; An image forming apparatus comprising:
Citation Information
Patent Citations
Liquid level detector
JP1988005220A
Water- and oil-repellent film
JP6801474B2