Positive electrode active material for lithium secondary battery, manufacturing method thereof, and lithium secondary battery including positive electrode containing the same

By coating lithium cobalt-based oxide with zirconium-based oxide and optimizing aluminum and magnesium content, the active material addresses structural instability and efficiency issues, leading to high energy density batteries with enhanced resistance and lifespan.

JP2024138220APending Publication Date: 2024-10-08SAMSUNG SDI CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
JP2024048308
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-07
Filing Date
2024-03-25
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Lithium cobalt oxide-based positive electrode active materials in lithium secondary batteries suffer from capacity reduction and structural instability due to hydrogen fluoride corrosion and magnesium migration, leading to reduced efficiency and lifespan at high voltages and temperatures.

Method used

A positive electrode active material is developed by coating lithium cobalt-based oxide with a zirconium-based oxide, containing specific amounts of aluminum and magnesium, which stabilizes the structure and enhances resistance characteristics, allowing for improved high voltage and high temperature performance.

Benefits of technology

The proposed active material maintains structural stability and enhances charge/discharge efficiency, resulting in high energy density lithium secondary batteries with improved resistance and lifespan characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138220000001_ABST
    Figure 2024138220000001_ABST
Patent Text Reader

Abstract

To provide a positive electrode active material for a lithium secondary battery, a manufacturing method thereof, and a lithium secondary battery including a positive electrode containing the same.SOLUTION: A positive electrode active material for a lithium secondary battery includes a lithium cobalt oxide and a zirconium oxide disposed on the surface of the lithium cobalt oxide, the lithium cobalt oxide includes 4,000 ppm or more of aluminum, and the zirconium content in the positive electrode active material is 15,000 to 20,000 ppm, and there are also provided a method for manufacturing the positive electrode active material, a positive electrode for a lithium secondary battery including the positive electrode active material, and a lithium secondary battery including the positive electrode active material.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material for a lithium secondary battery, a method for producing the same, and a lithium secondary battery including a positive electrode containing the same. [Background technology]

[0002] Recently, the development of the cutting-edge electronics industry has made it possible to reduce the size and weight of electronic devices, leading to an increase in the use of portable electronic devices. Lithium secondary batteries, which have high energy density and can be used for a long time, are widely used as power sources for such portable electronic devices.

[0003] Lithium cobalt oxide (LiCoO2) is widely used as a positive electrode active material for high energy density lithium secondary batteries. However, when lithium cobalt oxide is used as a positive electrode active material, the positive electrode active material comes into contact with an electrolyte in a battery environment, and the interface structure is destroyed by corrosion of hydrogen fluoride (HF), cobalt (Co) is dissolved, and capacity is reduced, especially at high voltage and high temperature. In order to prevent the structure of the layered positive electrode active material from collapsing in a high voltage environment, magnesium (Mg) is doped into lithium cobalt oxide. However, when magnesium is doped in this way, capacity and efficiency are reduced, and when Ti coating is applied, Mg migrates to the surface due to the Kirkendall effect, reducing the internal doping effect. Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a novel positive electrode active material for lithium secondary batteries having improved high voltage stability, and a method for producing the same.

[0005] Another object of the present invention is to provide a high-energy density lithium secondary battery having improved stability at high voltages and improved high-temperature characteristics by using a positive electrode including the above-mentioned positive electrode active material for lithium secondary batteries. [Means for solving the problem]

[0006] According to one aspect, A positive electrode active material for a lithium secondary battery, comprising a lithium cobalt-based oxide and a zirconium-based oxide disposed on a surface of the lithium cobalt-based oxide, The lithium cobalt-based oxide contains 4,000 ppm or more of aluminum, The positive electrode active material for a lithium secondary battery may have a zirconium content of 15,000 to 20,000 ppm.

[0007] The zirconium-based oxide is a compound represented by the following Chemical Formula 1. [Chemical formula 1] Mg x Zr y M1 z O2 In chemical formula 1, 0≦x≦0.1, 0.8≦y≦1, 0≦z≦0.1, 0.9 <x+y+z<1.1であり、 M1 is one or more elements selected from the group consisting of Co, Al, B, Ca, Sr, Ba, V, Cr, Fe, Cu, W, Mo, Ta and Nb.

[0008] The zirconium oxide is, for example, ZrO2.

[0009] The zirconium-based oxide belongs to the space group Fd-3m and has a cubic structure.

[0010] In the above formula 1, x is 0.

[0011] The zirconium-based oxide may have a particle shape, the particle size being 0.2 μm to 2 μm, and the zirconium-based oxide may be coated on the surface of the lithium cobalt-based oxide in an island shape.

[0012] The aluminum content is between 4,000 ppm and 8,000 ppm.

[0013] In the positive electrode active material, the zirconium content is 18,000 to 20,000 ppm, and the zirconium content is higher than the magnesium content.

[0014] The molar ratio of Zr / (Co+Zr) has a range of about 0.25 to about 0.35.

[0015] The positive electrode active material further contains magnesium, and the zirconium content is greater than the magnesium content.

[0016] The positive electrode active material is a compound represented by the following chemical formula 2. [Chemical formula 2] Li a-b Mg b Co x Al y M1 z O2 In chemical formula 2, 0.9 <a<1.1、0≦b<0.1、0.02≦x≦1、0.015≦y≦0.03、0<z<0.03、0.9≦x+y+z≦1.1であり、 M1 is one or more elements selected from the group consisting of Zr, Ni, Mn, B, Ca, Sr, Ba, V, Cr, Fe, Cu, W, Mo, Ta and Nb.

[0017] The positive electrode active material is small particles, large particles, or a mixture of small and large particles, the large particles having a size of 10 μm to 20 μm, and the small particles having a size of 2 μm to 8 μm. In this disclosure, particle size means the average size of the particles.

[0018] The lithium cobalt-based oxide may also include a mixture of large and small particles.

[0019] In the mixture of the large particles and the small particles, the mixing weight ratio of the large particles to the small particles is 7:3 to 9:1.

[0020] According to another embodiment, a method for producing a lithium cobalt-based oxide having at least 4,000 ppm of aluminum and a zirconium precursor is provided, comprising the steps of: and heat-treating the mixture to produce the cathode active material.

[0021] The zirconium precursor is at least one selected from the group consisting of zirconium oxide, zirconium chloride, zirconium sulfate, and zirconium oxide, and the heat treatment is performed at a temperature of 900°C to 1,100°C.

[0022] The lithium cobalt-based oxide containing 4,000 ppm or more of aluminum may further contain magnesium.

[0023] According to yet another aspect, There is provided a lithium secondary battery including a positive electrode containing the above-mentioned positive electrode active material, a negative electrode, and an electrolyte interposed between the positive electrode and the negative electrode. Effect of the Invention

[0024] The positive electrode active material according to an embodiment has excellent characteristics of high voltage, high power, and high temperature. By using a positive electrode including such a positive electrode active material, it is possible to manufacture a high energy density lithium secondary battery having improved resistance characteristics at high voltage, power characteristics, and high temperature life characteristics. [Brief description of the drawings]

[0025] [Figure 1A] 1 is a scanning electron microscope (SEM) photograph showing a cross section of a positive electrode active material prepared in Example 4. [Figure 1B] 1 is an image showing a scanning electron microscope (SEM) analysis result for a positive electrode active material prepared according to Comparative Example 6. [Figure 2A] 1 is an image showing a scanning electron microscope-energy dispersive spectroscopy (SEM-EDS) analysis result for the positive electrode active material of Example 4. [Figure 2B] 1 is an image showing a scanning electron microscope-energy dispersive spectroscopy (SEM-EDS) analysis result for the positive electrode active material of Example 4. [Figure 2C] 1 is an image showing a scanning electron microscope-energy dispersive spectroscopy (SEM-EDS) analysis result for the positive electrode active material of Example 4. [Diagram 3] FIG. 1 is a diagram showing the Zr / (Co+Zr) molar ratio in the positive electrode active materials of Examples 3 and 4. [Figure 4A] 1 shows the results of a scanning electron microscope (SEM)-EDS analysis of zirconium in a zirconium coating layer of a positive electrode active material of Example 4. [Figure 4B] 1 shows the results of a scanning electron microscope (SEM)-EDS analysis of zirconium in a zirconium coating layer of a positive electrode active material of Example 4. [Figure 4C] 1 shows the results of a scanning electron microscope (SEM)-EDS analysis of zirconium in a zirconium coating layer of a positive electrode active material of Example 4. [Figure 4D] FIG. 13 is a diagram showing the results of SEM-EDS analysis of cobalt in the zirconium coating layer of the positive electrode active material of Example 4. [Figure 4E] FIG. 13 is a diagram showing the results of SEM-EDS analysis of cobalt in the zirconium coating layer of the positive electrode active material of Example 4. [Figure 4F] FIG. 13 is a diagram showing the results of SEM-EDS analysis of cobalt in the zirconium coating layer of the positive electrode active material of Example 4. [Diagram 5] FIG. 13 is a diagram showing the results of a TEM (transmission electron microscope)-SAED (selected area (electron) diffraction) analysis of the positive electrode active material of Example 4. [Figure 6] 1 is a schematic diagram illustrating a structure of a lithium secondary battery according to an embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] Hereinafter, a positive electrode active material, a manufacturing method thereof, and a lithium secondary battery including a positive electrode including the same according to example embodiments will be described in more detail.

[0027] According to one embodiment, the positive electrode active material is a lithium-cobalt-based oxide containing 4,000 ppm or more of aluminum, The zirconium-based oxide is disposed on the surface of the lithium cobalt-based oxide, and the zirconium content is 15,000 ppm to 20,000 ppm.

[0028] In this specification, the aluminum ppm content means the mass of aluminum per 1,000,000 of the total positive electrode active material mass, and the zirconium ppm content means the mass of zirconium per 1,000,000 of the total positive electrode active material mass.

[0029] The zirconium compound may be arranged in an island shape on the surface of the lithium cobalt-based oxide.

[0030] Lithium cobalt-based oxide (LiCoO2) has a structure (O3-type layered structure) in which lithium, cobalt, and oxygen are regularly arranged along the

[0111] crystal plane of a rock salt structure. When a lithium secondary battery using such a lithium cobalt-based oxide is charged, lithium ions are released from the crystal lattice of the lithium cobalt-based oxide to the outside of the lattice. However, when the charging voltage is high, the amount of lithium ions released from the crystal lattice of the lithium cobalt-based oxide increases, and at least a part of the O3-type layered structure may undergo a phase transition to an O1-type layered structure (O1-type layered structure) in which Li does not exist in the crystal lattice. As a result, in a high-voltage range of charging voltages of 4.52 V or more (full cell basis), the lithium cobalt-based oxide may undergo a phase transition to an H1-3-type layered structure in which both the O3-type layered structure and the O1-type layered structure exist in the crystal lattice. Such a phase transition from the O3-type layered structure to the H1-3-type layered structure and the O1-type layered structure is at least partially irreversible, and the amount of lithium ions that can be absorbed / released is reduced in the H1-3-type layered structure and the O1-type layered structure, and therefore, when such a phase transition occurs, the storage characteristics and life characteristics of the lithium secondary battery are rapidly deteriorated.

[0031] In order to solve the above problems, magnesium-doped lithium cobalt oxide has been proposed as a positive electrode active material that can prevent structural collapse in a high voltage environment. When magnesium is doped, magnesium occupies the lithium site and maintains a structurally stable state even if an excessive amount of lithium is released during discharge. However, in this case, the capacity and charge / discharge efficiency of the lithium secondary battery are reduced, and improvements are needed to address this issue.

[0032] In order to improve the charge / discharge efficiency and surface resistance, a method of coating a titanium (Ti) compound has been proposed. In this case, Mg doped inside the lithium cobalt oxide moves to the surface of the lithium cobalt oxide due to the Kirkendall effect to form an Mg-Ti composite material. However, in such a positive electrode active material, the amount of magnesium (Mg) doped inside the lithium cobalt oxide is reduced, which may deteriorate the life characteristics of the positive electrode active material.

[0033] In the present disclosure, in order to solve the above problems, lithium cobalt oxide is doped with aluminum (Al) at 4,000 ppm or more, and some of the doped aluminum replaces the lithium sites, so that a stable structure can be maintained without doping with magnesium (Mg). In addition, the surface of the lithium cobalt oxide is coated with zirconium, so that the resistance characteristics at high voltage can be improved, and even if magnesium is doped into the positive electrode active material, the side effects due to Ti and the Kirkendall effect can be minimized or reduced.

[0034] According to an embodiment, the positive electrode active material for a lithium secondary battery is a lithium cobalt-based oxide containing 4,000 ppm or more of aluminum, A zirconium-based oxide is disposed on the surface of the lithium cobalt-based oxide.

[0035] The positive electrode active material does not require cobalt coating, which is performed on the lithium-cobalt-based oxide for high voltage and high output characteristics, because the lithium-cobalt-based oxide has a zirconium coating on its surface, and therefore it is possible to prepare a positive electrode active material that is stable in a high voltage environment, has improved capacity and charge / discharge efficiency, and has improved surface resistance and high temperature characteristics without a decrease in life characteristics.

[0036] The lithium cobalt-based oxide is small particles, large particles, or a mixture of small and large particles. The size of the large particles is 10 μm to 20 μm, and the size of the small particles is 2 μm to 8 μm. In the mixture of the large particles and the small particles, the mixing ratio of the large particles to the small particles is 7:3 to 9:1 by weight. In the present disclosure, size refers to an average size.

[0037] The mixing weight ratio of the large particles to the small particles is, for example, 8: 2 to 9: 1. When the mixing weight ratio of the large particles to the small particles is in this range, the high temperature storage characteristics are improved.

[0038] The size of the large particles is, as mentioned above, 10 μm to 20 μm, for example, 14 μm to 20 μm, or 15 μm to 20 μm, and the size of the small particles is, as mentioned above, 2 μm to 8 μm, for example, 3 μm to 7 μm, or 3 μm to 5 μm.

[0039] In this specification, "size" refers to the average particle diameter when the particle being measured is spherical, and refers to the average major axis length when the particle is non-spherical.

[0040] The average particle size and the average major axis length indicate the average values ​​of the measured particle size and the measured major axis length, respectively.

[0041] The size of the particles may be evaluated using a particle size analyzer, a scanning electron microscope (SEM) or a transmission electron microscope (TEM), such as a HORIBA LA-950 laser particle size analyzer.

[0042] According to an embodiment, the average particle size is, for example, the average particle size observed by a scanning electron microscope (SEM), and may be calculated as the average particle size of about 10 to 30 particles using a scanning electron microscope (SEM) image.

[0043] When the particle size is measured with the aid of a particle size analyzer, the average particle size refers to the D50.

[0044] D50 means the average diameter of particles whose cumulative volume is 50% by volume in a particle size distribution, and means the particle size value corresponding to 50% from the smallest particle when the total number of particles is 100% in a distribution curve in which particle sizes are accumulated in order from the smallest particle to the largest particle. D50 can be measured using a particle size analyzer. Alternatively, D50 can be easily obtained by measuring using a measuring device using dynamic light-scattering, performing data analysis, counting the number of particles for each particle size range, and then performing calculations therefrom.

[0045] The zirconium-based oxide is a compound represented by the following Chemical Formula 1. [Chemical formula 1] Mg x Zr y M1 z O2 In chemical formula 1, 0≦x≦0.1, 0.8≦y≦1, 0≦z≦0.1, 0.9 <x+y+z<1.1であり、 M1 is one or more elements selected from the group consisting of Co, Al, B, Ca, Sr, Ba, V, Cr, Fe, Cu, W, Mo, Ta and Nb.

[0046] The zirconium-based oxide belongs to the space group Fd-3m and has a cubic structure. When the lithium cobalt-based oxide is not doped with magnesium to prevent the Kirkendall effect, x=0.

[0047] The zirconium-based oxide has a particle shape, i.e., a structure in which particles having a size of 0.2 μm to 2 μm are coated in an island shape. When the zirconium-based oxide is in the above range, a positive electrode active material having improved surface resistance characteristics can be obtained.

[0048] In the positive electrode active material according to an embodiment, the aluminum content is 4,000 ppm to 8,000 ppm (0.4 to 0.8 wt%) (1.5 to 2.9 mol%), or 5,000 to 6,500 ppm% (1.8 to 2.35 mol%). The aluminum content is 2.0 to 3.3 mol% based on the total metal content of the positive electrode active material. When the aluminum content is within the above range, a positive electrode active material with improved high voltage characteristics can be obtained. Here, the high voltage is in the range of 4.3 V to 4.8 V.

[0049] In the positive electrode active material, the zirconium content is 15,000 to 20,000 ppm (1.5 to 2 wt%) (1.59 to 2.1 mol%), or 18,000 to 20,000 ppm (1.9 to 2.2 mol%). When the zirconium content is within this range, a lithium secondary battery having excellent resistance characteristics and improved high-temperature life characteristics can be manufactured.

[0050] When the lithium sites of the positive electrode active material according to an embodiment are doped with aluminum, the structural stability of the crystal structure of the lithium cobalt-based oxide is improved even under high temperature and high voltage conditions, thereby improving the life and resistance characteristics. In particular, a portion of the cobalt sites of the positive electrode active material is replaced with zirconium, thereby further improving the surface resistance.

[0051] The positive electrode active material according to an embodiment has an internal R-3m rhombohedral layer structure, and a coating film has an Fm-3m cubic structure. The specific surface area of ​​the positive electrode active material is 0.1 to 3 m. 2 / g. The specific surface area is also the BET specific surface area.

[0052] The positive electrode active material containing 4,000 ppm or more of aluminum may further contain magnesium. Here, the magnesium content is, for example, 500 to 2,000 ppm or 1,000 to 1,200 ppm (0.4 to 0.5 mol %). When the positive electrode active material according to an embodiment further contains magnesium, high voltage characteristics and high temperature characteristics may be further improved.

[0053] In this specification, the ppm content of magnesium means the mass of magnesium relative to 1,000,000 of the total mass of the positive electrode active material.

[0054] In the positive electrode active material, the Zr / (Co+Zr) molar ratio is 0.25 to 0.35, 0.26 to 0.33, or 0.27 to 0.32. Here, the ratio indicates a molar ratio. When the Zr / (Co+Zr) molar ratio is in the above range, a positive electrode active material having improved resistance characteristics and high voltage characteristics can be obtained.

[0055] The positive electrode active material according to an embodiment is a compound represented by the following Formula 2:

[0056] [Chemical formula 2] Li a-b Mg b Co x Al y M1 z O2 In chemical formula 2, 0.9 <a<1.1、0≦b<0.1、0.02≦x≦1、0.015≦y≦0.03、0<z<0.03、0.9≦x+y+z≦1.1であり、 M1 is one or more elements selected from the group consisting of Zr, Ni, Mn, B, Ca, Sr, Ba, V, Cr, Fe, Cu, W, Mo, Ta and Nb.

[0057] For example, the compound of formula 2 also contains magnesium.

[0058] In the case where M1 in the formula 2 is Zr, the content of M1 is greater than the content of magnesium. In the formula 2, y is, for example, 0.016≦y≦0.028, 0.017≦y≦0.027, 0.017≦y≦0.025, 0.017≦y≦0.024, or 0.018≦y≦0.0235.

[0059] In chemical formula 2, 0.01≦z≦0.025, 0.012≦z≦0.025, 0.013≦z≦0.024, 0.015≦z≦0.024, 0.016≦z≦0.023, 0.017≦z≦0.022, or 0.019≦z≦0.021.

[0060] A positive electrode including the positive electrode active material and a lithium secondary battery are provided. The lithium secondary battery according to an embodiment exhibits excellent trickle charge stability. Here, the trickle charge stability refers to the time required for a current to increase rapidly during continuous charging.

[0061] According to an embodiment, the positive electrode active material may be prepared by mixing a lithium cobalt-based oxide containing 4,000 ppm or more of aluminum with a zirconium precursor to obtain a mixture, and heat-treating the mixture.

[0062] The zirconium precursor may, for example, comprise one or more selected from zirconium hydroxide, zirconium chloride, zirconium sulfate, and zirconium oxide.

[0063] The heat treatment is carried out at 900° C. to 1,100° C., or 900° C. to 1,000° C. When the heat treatment is carried out within the above range, a positive electrode active material having excellent particle strength, high voltage characteristics, and high temperature characteristics can be produced.

[0064] The lithium cobalt oxide may be, for example, a mixture of large particles and small particles. A method for producing a positive electrode active material using such a mixture will be described.

[0065] First, a cobalt precursor, an aluminum precursor, and a lithium precursor, each having a size of 1 μm to 10 μm, are mixed to obtain a first mixture.

[0066] If necessary, a magnesium precursor can be further added to the first mixture.

[0067] Specifically, the lithium precursor, the cobalt precursor, the aluminum precursor, and the magnesium precursor can be mixed while controlling the mixing ratio stoichiometrically so as to obtain the desired lithium-cobalt-based oxide, thereby obtaining a precursor mixture.

[0068] The lithium precursor may be one or more selected from the group consisting of lithium hydroxide (LiOH), lithium carbonate (Li2CO3), lithium chloride, lithium sulfate (Li2SO4) and lithium nitrate (LiNO3).

[0069] The cobalt precursor may be one or more selected from cobalt carbonate, cobalt oxide, cobalt chloride, cobalt sulfate, and cobalt nitrate, the aluminum precursor may be one or more selected from aluminum sulfate, aluminum chloride, and aluminum hydroxide, and the magnesium precursor may be one or more selected from magnesium sulfate, magnesium chloride, and magnesium hydroxide.

[0070] The mixing may be performed by mechanical dry mixing using, for example, a ball mill, a Banbury mixer, a homogenizer, a Henschel mixer, etc. The dry mixing may reduce production costs compared to wet mixing.

[0071] As described above, the size of the cobalt precursor is 1 μm to 10 μm, for example, 4 μm to 7 μm. If the size of the cobalt precursor is less than 1 μm, the particle growth is slow, and if the size of the cobalt precursor is more than 10 μm, it is difficult to obtain large-grained lithium-cobalt composite oxide having the desired size.

[0072] Subsequently, the first mixture is subjected to a primary heat treatment in an air atmosphere or an oxygen atmosphere, and a large-particle lithium-cobalt composite oxide can be obtained as a product of the primary heat treatment.

[0073] The particle size of the large-particle lithium-cobalt-based composite oxide which is the large-particle primary heat treatment product is 10 μm to 20 μm, for example, 14 μm to 20 μm, for example, 17 μm.

[0074] Separately, a cobalt precursor, an aluminum precursor, and a lithium precursor, each having a size of 2 μm to 3 μm, are mixed to obtain a second mixture, which is then subjected to a primary heat treatment to produce a small-particle lithium-cobalt composite oxide.

[0075] The primary heat treatment is carried out at 900 to 1,100°C.

[0076] During preparation of the second mixture, additional magnesium precursor may be added.

[0077] The size of the small-particle lithium-cobalt composite oxide is 2 μm to 8 μm, for example, 3 μm to 4 μm.

[0078] If the size of the cobalt precursor used in producing the small-particle lithium-cobalt composite oxide is less than 2 μm or exceeds 8 μm, it is difficult to obtain small-particle lithium-cobalt composite oxide having the desired size.

[0079] When producing the large-particle lithium-cobalt composite oxide and the small-particle lithium-cobalt composite oxide, the mixture molar ratio of lithium to metal (metal other than lithium in the composite) is 1.01 to 1.05, for example, 1.02 to 1.04.

[0080] In the step of preparing the large-particle lithium-cobalt composite oxide and the small-particle lithium-cobalt composite oxide, the heating rate is 4 to 8° C. / min. When the heating rate is within this range, it is possible to prevent cation mixing. If the heating rate is less than 4° C. / min, the improvement of phase stability at high voltage is insignificant.

[0081] The large-grain lithium-cobalt composite oxide and the small-grain lithium-cobalt composite oxide are mixed in a weight ratio of 7:3 to 9:1, and a zirconium precursor is added thereto to obtain a third mixture, which is then subjected to a second heat treatment. The second heat treatment can be performed at 900 to 1,000° C., for example, 950 to 1,000° C. The heating rate during the second heat treatment is 4 to 6° C. / min.

[0082] The zirconium precursor may, for example, comprise one or more selected from zirconium oxide, zirconium hydroxide, zirconium chloride, and zirconium sulfate.

[0083] The secondary heat treatment may be carried out in an air atmosphere or an oxygen atmosphere. Here, the oxygen atmosphere may be formed by using oxygen alone or by using oxygen, nitrogen and an inert gas together. The heat treatment time varies depending on the heat treatment temperature. For example, the heat treatment may be carried out for 5 to 20 hours.

[0084] The positive electrode active material according to an embodiment may be prepared by a preparation method such as a spray pyrolysis method in addition to the solid phase method.

[0085] According to another aspect, there is provided a lithium secondary battery including a positive electrode containing the above-mentioned lithium cobalt-based composite oxide. The method for producing the lithium secondary battery is as follows.

[0086] The positive electrode is prepared by the following method.

[0087] According to an embodiment of the present invention, a positive electrode active material, a binder, and a solvent are mixed to prepare a positive electrode active material composition. A conductive material may be further added to the positive electrode active material composition. The positive electrode active material composition is directly coated on a positive electrode current collector and dried to prepare a positive electrode plate. Alternatively, the positive electrode active material composition may be cast on a separate support, and the film peeled off from the support may be laminated on a metal current collector to prepare a positive electrode plate. The positive electrode may further include a first positive electrode active material, which is a positive electrode active material commonly used in lithium secondary batteries. The first positive electrode active material may further include at least one selected from the group consisting of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, and lithium manganese oxide, but is not necessarily limited thereto, and all positive electrode active materials available in the art may be used. For example, Li a A 1-b B b D2 (wherein, in the formula, 0.90≦a≦1.8 and 0≦b≦0.5); Li a E 1-b B b O 2-c D c (wherein, in the formula, 0.90≦a≦1.8, 0≦b≦0.5, and 0≦c≦0.05); LiE 2-b B b O 4-c D c (wherein, 0≦b≦0.5 and 0≦c≦0.05); Li a Ni 1-b-c Co b B c D α (wherein, in the formula, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Co b B c O 2-α F' α (wherein, in the formula, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-cMn b B c D α (wherein, in the formula, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Mn b B c O 2-α F' α (wherein, in the formula, 0.9≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni b E c G d O2 (wherein the formula is 0.9≦a≦1.8, 0≦b≦0.9, 0≦c≦0.5, and 0.001≦d≦0.1); Li a Ni b Co c Mn d G e O2 (wherein the formula is 0.9≦a≦1.8, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, and 0.001≦e≦0.1); Li a NiG b O2 (wherein, in the above formula, 0.9≦a≦1.8, 0.001≦b≦0.1); Li a CoG b O2 (wherein, in the above formula, 0.9≦a≦1.8, 0.001≦b≦0.1); Li a MnG b O2 (wherein, in the above formula, 0.9≦a≦1.8, 0.001≦b≦0.1); Li a Mn2G b O4 (wherein the above formula is 0.9≦a≦1.8, 0.001≦b≦0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0≦f≦2);LiNiVO4;Li (3-f) J2(f≦2);Li (3-f) Fe2(PO4)3(0≦f≦2);LiNiVO4;Li (3-f)A compound represented by any one of the chemical formulas J2(f≦2);LiFePO4 may be used. In the chemical formula, A is Ni, Co, Mn, or a combination thereof, B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof, D is O, F, S, P, or a combination thereof, E is Co, Mn, or a combination thereof, F' is F, S, P, or a combination thereof, G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof, Q is Ti, Mo, Mn, or a combination thereof, I is Cr, V, Fe, Sc, Y, or a combination thereof, and J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof.

[0088] Examples of the binder in the positive electrode active material composition include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, polyamide-imide, polyacrylic acid (PAA), lithium polyacrylate, lithium polymethacrylate, and various copolymers.

[0089] The conductive material is not particularly limited as long as it has conductivity without inducing a chemical change in the battery, and examples of the conductive material that can be used include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon nanotubes, carbon fibers, and metal fibers; carbon fluoride; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0090] The content of the conductive material is 1 to 10 parts by weight, or 1 to 5 parts by weight, based on 100 parts by weight of the positive electrode active material. When the content of the conductive material is within the above range, the final electrode has excellent conductivity characteristics.

[0091] A non-limiting example of the solvent is N-methylpyrrolidone, and the content of the solvent is 20 to 200 parts by weight based on 100 parts by weight of the positive electrode active material. When the content of the solvent is within the above range, the operation for forming the positive electrode active material layer is easy.

[0092] The positive electrode current collector is not particularly limited as long as it has a thickness of 3 μm to 500 μm and has high conductivity without inducing chemical changes in the battery, and may be, for example, stainless steel, aluminum, nickel, titanium, heat-treated carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The current collector may have fine irregularities on its surface to increase the adhesive strength of the positive electrode active material, and may be in various forms such as a film, sheet, foil, net, porous body, foam, or nonwoven fabric.

[0093] The positive electrode current collector may be, for example, a plate or foil made of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector may be omitted. The thickness of the positive electrode current collector may be, for example, 1 μm to 100 μm, 1 μm to 50 μm, 5 μm to 25 μm, or 10 μm to 20 μm.

[0094] The positive electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may include, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. When the base film includes a thermoplastic polymer, the base film is liquefied when a short circuit occurs, and a sudden increase in current can be suppressed. The base film may be, for example, an insulator. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), or an alloy thereof. The positive electrode current collector may further include a metal chip and / or a lead tab. For more details regarding the base film, metal layer, metal chip, and lead tab of the positive electrode current collector, please refer to the negative electrode current collector described below. By having such a structure of the positive electrode current collector, the weight of the electrode can be reduced, and as a result, the energy density can be improved.

[0095] It is also possible to further add a plasticizer to the positive electrode active material composition and / or the negative electrode active material composition to form pores inside the electrode.

[0096] The contents of the aforementioned positive electrode active material, conductive material, binder, and solvent are at levels commonly used in lithium secondary batteries. Depending on the use and configuration of the lithium secondary battery, one or more of the aforementioned conductive material, binder, and solvent may be omitted.

[0097] The negative electrode can be obtained by implementing in almost the same manner as that in the aforementioned positive electrode manufacturing process, except that a negative electrode active material is used instead of the positive electrode active material.

[0098] As the negative electrode active material, a carbon-based material, silicon, silicon oxide, silicon-based alloy, silicon-carbon-based material composite, tin, tin-based alloy, tin-carbon composite, metal oxide, or a combination thereof is used.

[0099] The carbon-based material is also crystalline carbon, amorphous carbon, or a mixture thereof. The crystalline carbon is also graphite such as amorphous, plate-like, flaky, spherical, or fibrous natural graphite or artificial graphite, and the amorphous carbon is also soft carbon (low-temperature calcined carbon) or hard carbon, mesophase pitch carbide, calcined coke, graphene, carbon black, carbon nanotube, and carbon fiber, etc., but is not necessarily limited thereto, and any of them is possible as long as it can be used in the technical field.

[0100] The negative electrode active material can be selected from the group consisting of Si, SiO x (where 0 < x < 2, for example, 0.5 to 1.5), Sn, SnO2, or a silicon-containing metal alloy, and mixtures thereof. As the metal that can form the silicon alloy, one or more can be selected from Al, Sn, Ag, Fe, Bi, Mg, Zn, in, Ge, Pb, and Ti and used.

[0101] The negative electrode active material may also include a metal / semimetal capable of alloying with lithium, their alloys, or their oxides. For example, the metal / semimetal capable of alloying with lithium may be Si, Sn, Al, Ge, Pb, Bi, Sb, Si-Y alloy (where Y is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element, transition metal, rare earth element, or a combination element thereof, and not Si), Sn-Y alloy (where Y is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element, transition metal, rare earth element, or a combination element thereof, and not Sn), MnO x (0 < x ≤ 2), etc. Examples of the element Y include Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, or a combination thereof. For example, the oxides of the metal / semimetal capable of alloying with lithium may be lithium titanate, vanadium oxide, lithium vanadate, SnO2, SiO x (0 < x < 2), etc.

[0102] The negative electrode active material may also include, for example, one or more elements selected from the group consisting of Group 13 elements, Group 14 elements, and Group 15 elements of the periodic table of elements, specifically, one or more elements selected from the group consisting of Si, Ge, and Sn.

[0103] In the negative electrode active material composition, a binder can be a water-insoluble binder, a water-soluble binder, or a combination thereof.

[0104] Examples of the water-insoluble binder may include ethylene-propylene copolymer, polyacrylonitrile, polystyrene, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or a combination thereof.

[0105] The water-soluble binder may be styrene-butadiene rubber (SBR), acrylated styrene-butadiene rubber (ABR), acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, a polymer containing ethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, or a combination thereof.

[0106] When the negative electrode binder is a water-soluble binder, the negative electrode binder may further include a cellulose-based compound capable of imparting viscosity as a thickener. The cellulose-based compound may be a mixture of one or more of carboxymethylcellulose, hydroxypropylmethylcellulose, methylcellulose, or alkali metal salts thereof. The alkali metal may be Na, K, or Li. The content of the thickener is 0.1 to 3 parts by weight based on 100 parts by weight of the negative electrode active material.

[0107] The conductive material may be a carbon-based material such as natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, or carbon fiber; a metal-based material such as a metal powder or a metal fiber of copper, nickel, aluminum, or silver; a conductive polymer such as a polyphenylene derivative; or a mixture thereof.

[0108] The negative electrode active material composition may use the same solvent as that used in the positive electrode active material composition, and the content of the solvent is at a level generally used in lithium secondary batteries.

[0109] The negative electrode current collector is, for example, made of a material that does not react with lithium, i.e., does not form any alloy or compound with it. The material constituting the negative electrode current collector is, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co) and nickel (Ni), but is not necessarily limited thereto, and any material that is used as an electrode current collector in the technical field is possible. The negative electrode current collector can be made of one of the above-mentioned metals, or an alloy of two or more metals, or a coating material. The negative electrode current collector is, for example, in the form of a plate or foil.

[0110] The negative electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may include, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. When the base film includes a thermoplastic polymer, the base film may be liquefied in the event of a short circuit, which may suppress a sudden increase in current. The base film may be, for example, an insulator. The metal layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal layer may act as an electrochemical fuse and may be cut off in the event of an overcurrent, thereby performing a short circuit prevention function. The thickness of the metal layer may be adjusted to adjust the limit current and maximum current. The metal layer is plated or deposited on the base film. If the thickness of the metal layer is reduced, the limiting current and / or maximum current of the negative electrode current collector is reduced, and the stability of the lithium battery during a short circuit can be improved. A lead tab can be added to the metal layer for connection to the outside. The lead tab can be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, etc. During welding, the metal layer can be electrically connected to the lead tab while the base film and / or metal layer melts. In order to further strengthen the welding between the metal layer and the lead tab, a metal piece can be added between the metal layer and the lead tab. The metal piece can be a thin piece of the same material as the metal of the metal layer. The metal piece can be, for example, a metal foil, a metal mesh, etc. The metal piece can be, for example, an aluminum foil, a copper foil, a SUS (steel use stainless) foil, etc.After disposing a metal piece on the metal layer, the lead tab may be welded to the metal piece / metal layer laminate or the metal piece / metal layer / base film laminate. During welding, the base film, the metal layer, and / or the metal piece may be melted, and the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. The metal piece and / or the lead tab may be added to a portion on the metal layer. The thickness of the base film may be, for example, 1 μm to 50 μm, 1.5 μm to 50 μm, 1.5 μm to 40 μm, or 1 μm to 30 μm. The weight of the electrode assembly may be further effectively reduced by the base film having a thickness in such a range. The melting point of the base film may be, for example, 100° C. to 300° C., 100° C. to 250° C., or 100° C. to 200° C. Since the base film has a melting point in such a range, the base film can be melted and easily bonded to the lead tab during the process of welding the lead tab. In order to improve the adhesive strength between the base film and the metal layer, a surface treatment such as a corona treatment can be performed on the base film. The thickness of the metal layer can be, for example, 0.01 μm to 3 μm, 0.1 μm to 3 μm, 0.1 to 2 μm, or 0.1 to 1 μm. Since the metal layer has a thickness in such a range, the stability of the electrode assembly can be ensured while maintaining conductivity. The thickness of the metal piece can be, for example, 2 μm to 10 μm, 2 μm to 7 μm, or 4 μm to 6 μm. Since the metal piece has a thickness in such a range, the connection between the metal layer and the lead tab can be more easily performed. Since the negative electrode current collector has such a structure, the weight of the electrode can be reduced, and as a result, the energy density can be improved.

[0111] The separator is interposed between the positive electrode and the negative electrode, and is made of an insulating thin film having high ion permeability and mechanical strength.

[0112] The pore size of the separator is generally 0.01 μm to 10 μm, and the thickness is generally 5 μm to 20 μm. For example, a sheet or nonwoven fabric made of an olefin polymer such as polypropylene, glass fiber, or polyethylene is used as such a separator. When a solid polymer electrolyte is used as the electrolyte, the solid polymer electrolyte can also serve as the separator.

[0113] Specific examples of the olefin-based polymer in the separator include polyethylene, polypropylene, polyvinylidene fluoride, and multi-layer films of two or more layers thereof, and mixed multi-layer films such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, and a polypropylene / polyethylene / polypropylene three-layer separator may be used.

[0114] The lithium salt-containing non-aqueous electrolyte comprises a non-aqueous electrolyte and a lithium salt.

[0115] As the non-aqueous electrolyte, a non-aqueous electrolytic solution, an organic solid electrolyte, or an inorganic solid electrolyte is used.

[0116] The non-aqueous electrolyte contains an organic solvent. Any organic solvent that can be used as an organic solvent in the art can be used. For example, propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methylethyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, methylisopropyl carbonate, dipropyl carbonate, dibutyl carbonate, fluoroethylene carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or a mixture thereof.

[0117] As the organic solid electrolyte, for example, a polyethylene derivative, a polyethylene oxide derivative, a polypropylene oxide derivative, a phosphate polymer, polyvinyl alcohol, or the like can be used.

[0118] Examples of the inorganic solid electrolyte that can be used include Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, and Li3PO4-Li2S-SiS2.

[0119] The lithium salt is a substance that is easily dissolved in the non-aqueous electrolyte, and examples of the lithium salt include LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, Li(FSO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1SO2) (where x and y are natural numbers), LiCl, LiI, or a mixture thereof. In addition, for example, pyridine, triethylphosphide, triethyl alcohol amine, cyclic ether, ethylenediamine, n-glyme, hexamethyl phosphoramide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. may be added to the non-aqueous electrolyte for the purpose of improving charge / discharge characteristics, flame retardancy, etc. In some cases, a halogen-containing solvent such as carbon tetrachloride or trifluoroethylene may be further added to impart non-flammability. The concentration of the lithium salt is preferably within the range of 0.1M to 2.0M. If the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0120] The lithium secondary battery includes a positive electrode, a negative electrode, and a separator. As the separator, polyethylene, polypropylene, polyvinylidene fluoride, or a multi-layer film of two or more layers thereof is used, and it goes without saying that a mixed multi-layer film such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator can be used.

[0121] The positive electrode, negative electrode, and separator are wound or folded and housed in a battery case. An organic electrolyte is then injected into the battery case, which is then sealed with a cap assembly to complete a lithium secondary battery. The battery case may be cylindrical, rectangular, or thin-film type.

[0122] A separator may be disposed between the positive electrode and the negative electrode to form a battery structure. The battery structure may be stacked in a bi-cell structure, and then immersed in an organic electrolyte. The resulting structure may be placed in a pouch and sealed to complete a lithium ion polymer battery.

[0123] In addition, a plurality of the battery structures may be stacked to form a battery pack, which may be used in any device requiring high capacity and high output, such as a notebook computer, a smartphone, or an electric vehicle.

[0124] Although the lithium secondary battery according to the embodiment will be described as having a rectangular shape, the present invention is not limited thereto and may be applied to batteries of various shapes such as cylindrical, pouch, and coin shapes.

[0125] FIG. 6 is a cross-sectional view illustrating a typical structure of a lithium secondary battery according to an embodiment.

[0126] Referring to FIG. 6, the lithium secondary battery 31 includes a positive electrode 33, a negative electrode 32, and a separator 34. The positive electrode 33, the negative electrode 32, and the separator 34 are wound or folded, and the electrode assembly is housed in a battery case 35. Depending on the shape of the battery, the separator 34 may be disposed between the positive electrode 33 and the negative electrode 32, and a battery structure in which the positive electrode 33 and the negative electrode 32 are stacked on each other may be formed. Then, an organic electrolyte solution is injected into the battery case 35, and the battery case 35 is sealed with a cap assembly 36, thereby completing the lithium secondary battery 31. The battery case 35 may be cylindrical, rectangular, thin-film, etc. For example, the lithium secondary battery 31 may be a large-sized thin-film battery. The lithium secondary battery may be a lithium-ion battery. If the battery structure is housed in a pouch, impregnated with an organic electrolyte solution, and sealed, a lithium-ion polymer battery is completed. In addition, a plurality of the battery structures are stacked to form a battery pack, and such a battery pack may be used in all devices requiring high capacity and high output. For example, it can be used in notebook computers, smartphones, electric vehicles, etc.

[0127] The present invention will be described in more detail with reference to the following examples and comparative examples. However, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.

[0128] (Production of positive electrode active material) Example 1: LCO+Zr 18,000 ppm surface coating doped with Al 5,000 ppm and Mg 1,000 ppm Lithium carbonate (Li2CO3), cobalt precursor (Co3O4 (D50: 4.5 μm)), magnesium carbonate (MgCO3) and aluminum oxide (Al2O3) were mixed to obtain a first mixture. In the first mixture, the contents of lithium carbonate (Li2CO3), Co3O4 (D50: 4.5 μm), magnesium carbonate and aluminum oxide (Al2O3) were Li 1.04 Mg 0.004 Co 0.982 Al 0.018 The stoichiometry was controlled to obtain O2.

[0129] The first mixture was heated to 1,088° C. at a heating rate of 6° C. / min, and then subjected to a primary heat treatment at that temperature for 15 hours in an air atmosphere to obtain large particles (Li 1.04 Mg 0.004 Co 0.982 Al 0.018 O2) was manufactured.

[0130] Separately, a cobalt precursor, Co3O4 (D50: 2.5 μm), magnesium carbonate (MgCO3), aluminum oxide (Al2O3), and lithium carbonate were mixed to obtain a second mixture. In the second mixture, the contents of Co3O4 (D50: 2.5 μm), magnesium carbonate, and lithium carbonate (Li2CO3) were Li 1.04 Mg 0.004 Co 0.982 Al 0.018 The stoichiometry was controlled to obtain O2.

[0131] The second mixture was heated to 940° C. at a heating rate of 4.5° C. / min, and then a primary heat treatment was carried out at that temperature for 5 hours to obtain small particles (Li 1.04 Mg 0.004 Co 0.982 Al 0.018 O2) was obtained.

[0132] The large particles and small particles obtained in the above process were mixed in a weight ratio of 8:2, and zirconium oxide (ZrO2) was added thereto to obtain a third mixture. The third mixture was subjected to a second heat treatment at about 900°C to obtain a bimodal positive electrode active material. The content of zirconium oxide was stoichiometrically controlled so that the zirconium content in the bimodal positive electrode active material was 18,000 ppm.

[0133] The bimodal positive electrode active material is a large-grain Li with a ZrO2 coating film formed on its surface. 1.04 Mg 0.004 Co 0.982 Al 0.018 O2 (D50: 17μm) and small Li with a ZrO2 coating film on the surface. 1.04 Mg 0.004 Co 0.982 Al 0.018 The chemical formula of the final positive electrode active material containing large and small Zr-coated particles is Li 1.04 Mg 0.004 Co 0.982 Al 0.018 Zr 0.019 It's O2.

[0134] Example 2: LCO+Zr 20,000 ppm surface coating doped with Al 5,000 ppm and Mg 1,000 ppm Lithium carbonate, cobalt precursor (Co3O4 (D50: 4.5 μm)), magnesium carbonate (MgCO3), and aluminum oxide (Al2O3) were mixed to obtain a first mixture. In the first mixture, the contents of lithium carbonate, Co3O4 (D50: 4.5 μm), magnesium carbonate (MgCO3), and aluminum oxide (Al2O3) were Li 1.04 Mg 0.004 Co0.982 Al 0.018 The stoichiometry was controlled to obtain O2.

[0135] The first mixture was heated to 1,088° C. at a heating rate of 6° C. / min, and then subjected to a primary heat treatment at that temperature for 15 hours in an air atmosphere to obtain large particles (Li 1.04 Mg 0.004 Co 0.982 Al 0.018 O2) was manufactured.

[0136] Separately, a cobalt precursor, Co3O4 (D50: 2.5 μm), aluminum oxide (Al2O3), magnesium carbonate, and lithium carbonate were mixed to obtain a second mixture. In the second mixture, the contents of Co3O4, magnesium carbonate, aluminum oxide (Al2O3), and lithium carbonate were Li 1.04 Mg 0.004 Co 0.982 Al 0.018 The stoichiometry was controlled to obtain O2.

[0137] The second mixture was heated to 940° C. at a heating rate of 4.5° C. / min, and then a primary heat treatment was carried out at that temperature for 5 hours to obtain small-grained Li particles having a layered structure and an average particle size (D50) of about 3.5 μm. 1.04 Mg 0.004 Co 0.982 Al 0.018 O2 was obtained.

[0138] The large particles and small particles obtained in the above process were mixed in a weight ratio of 8:2, and zirconium oxide (ZrO2) was added thereto to obtain a third mixture. The third mixture was subjected to a second heat treatment at about 900°C, and the content of zirconium oxide was adjusted to a stoichiometric content so that the zirconium content in the bimodal positive electrode active material was 20,000 ppm. The bimodal positive electrode active material was made of large Li particles with a ZrO2 coating film formed on the surface. 1.04 Mg 0.004 Co 0.982 Al0.018 O2 (D50: 17μm) and small Li with a ZrO2 coating film on the surface. 1.04 Mg 0.004 Co 0.982 Al 0.018 A bimodal positive electrode active material containing Zr-coated large particles and small particles was obtained. The chemical formula of the final positive electrode active material containing Zr-coated large particles and small particles was Li 1.04 Mg 0.004 Co 0.982 Al 0.018 Zr 0.021 It's O2.

[0139] Example 3: LCO+Zr 16,000 ppm surface coating doped with Al 6,500 ppm and Mg 1,000 ppm Lithium carbonate, cobalt precursor (Co3O4 (D50: 4.5 μm)), magnesium carbonate (MaCO3) and aluminum oxide (Al2O3) were mixed to obtain a first mixture. In the first mixture, the contents of lithium carbonate, Co3O4 (D50: 4.5 μm) and aluminum oxide (Al2O3) were Li 1.04 Mg 0.004 Co 0.959 Al 0.024 The stoichiometry was controlled to obtain O2.

[0140] The first mixture was heated to 1,088° C. at a heating rate of 6° C. / min, and then subjected to a primary heat treatment at that temperature for 15 hours in an air atmosphere to obtain large particles (Li 1.04 Mg 0.004 Co 0.959 Al 0.024 O2) was manufactured.

[0141] Separately, a cobalt precursor, Co3O4 (D50: 2.5 μm), magnesium carbonate (MaCO3), aluminum oxide (Al2O3), and lithium carbonate were mixed to obtain a second mixture. In the second mixture, the contents of Co3O4, magnesium carbonate, aluminum oxide (Al2O3), and lithium carbonate were Li 1.04 Mg 0.004 Co 0.959 Al 0.024The stoichiometry was controlled to obtain O2.

[0142] The second mixture was heated to 940° C. at a heating rate of 4.5° C. / min, and then a primary heat treatment was carried out at that temperature for 5 hours to obtain small-grained Li particles having a layered structure and an average particle size (D50) of about 3.5 μm. 1.04 Mg 0.004 Co 0.959 Al 0.024 O2 was obtained.

[0143] The large particles and small particles obtained in the above process were mixed in a weight ratio of 8:2, and zirconium oxide was added thereto to obtain a third mixture. The third mixture was subjected to a second heat treatment at about 900°C, and the content of zirconium oxide was adjusted to a stoichiometric content so that the zirconium content in the bimodal positive electrode active material was 16,000 ppm. The bimodal positive electrode active material was made of large Li particles with a ZrO2 coating film formed on the surface. 1.04 Mg 0.004 Co 0.959 Al 0.024 O2 (D50: 17 μm) and small Li with a Zr2O2 coating film formed on the surface. 1.04 Mg 0.004 Co 0.959 Al 0.024 A bimodal positive electrode active material containing Zr-coated large particles and small particles was obtained. The chemical formula of the final positive electrode active material containing Zr-coated large particles and small particles was Li 1.04 Mg 0.004 Co 0.959 Al 0.024 Zr 0.017 It's O2.

[0144] Example 4: LCO+Zr 18,000 ppm surface coating doped with Al 6,500 ppm and Mg 1,000 ppm Lithium carbonate, Co3O4 (D50: 4.5 μm), magnesium carbonate, and aluminum oxide (Al2O3) were mixed to obtain a first mixture. In the first mixture, the contents of lithium carbonate, Co3O4 (D50: 4.5 μm), magnesium carbonate, and aluminum oxide (Al2O3) were Li 1.04 Mg 0.004Co 0.957 Al 0.024 The stoichiometry was controlled to obtain O2.

[0145] The first mixture was heated to 1,088° C. at a heating rate of 6° C. / min, and then subjected to a primary heat treatment at that temperature for 15 hours in an air atmosphere to obtain large particles (Li 1.04 Mg 0.004 Co 0.957 Al 0.024 O2) was manufactured.

[0146] Separately, a cobalt precursor, Co3O4 (D50: 2.5 μm), aluminum oxide (Al2O3), and lithium carbonate were mixed to obtain a second mixture. In the second mixture, the contents of Co3O4, magnesium carbonate, aluminum oxide (Al2O3), and lithium carbonate were Li 1.04 Mg 0.004 Co 0.957 Al 0.024 The stoichiometry was controlled to obtain O2.

[0147] The second mixture was heated to 940° C. at a heating rate of 4.5° C. / min, and then heat-treated at that temperature for 5 hours to obtain small-grained Li particles having a layered structure and an average particle size (D50) of about 3.5 μm. 1.04 Mg 0.004 Co 0.957 Al 0.024 O2 was obtained.

[0148] The large particles and small particles obtained in the above process were mixed in a weight ratio of 8:2, and zirconium oxide was added thereto to obtain a third mixture. The third mixture was subjected to a second heat treatment at about 900°C, and the content of zirconium oxide was adjusted to a stoichiometric content so that the zirconium content in the bimodal positive electrode active material was 18,000 ppm. The bimodal positive electrode active material was composed of large Li particles with a ZrO2 coating film formed on the surface. 1.04 Mg 0.004 Co 0.957 Al 0.024O2 (D50: 17μm) and small Li with a ZrO2 coating film on the surface. 1.04 Mg 0.004 Co 0.957 Al 0.024 A bimodal positive electrode active material containing Zr-coated large particles and small particles was obtained. The chemical formula of the final positive electrode active material containing Zr-coated large particles and small particles was Li 1.04 Mg 0.004 Co 0.957 Al 0.024 Zr 0.019 It's O2.

[0149] Example 5: LCO+Zr 20,000 ppm surface coating doped with Al 6,500 ppm and Mg 1,000 ppm Lithium carbonate, Co3O4 (D50: 4.5 μm), magnesium carbonate, and aluminum oxide (Al2O3) were mixed to obtain a first mixture. In the first mixture, the contents of lithium carbonate, Co3O4 (D50: 4.5 μm), magnesium carbonate, and aluminum oxide (Al2O3) were Li 1.04 Mg 0.004 Co 0.955 Al 0.024 The stoichiometry was controlled to obtain O2.

[0150] The first mixture was heated to 1,088° C. at a heating rate of 6° C. / min, and then subjected to a primary heat treatment at that temperature for 15 hours in an air atmosphere to obtain large particles (Li 1.04 Mg 0.004 Co 0.955 Al 0.024 O2) was manufactured.

[0151] Separately, a cobalt precursor, Co3O4 (D50: 2.5 μm), aluminum oxide (Al2O3), magnesium carbonate, and lithium carbonate were mixed to obtain a second mixture. In the second mixture, the contents of Co3O4, magnesium carbonate, aluminum oxide (Al2O3), and lithium carbonate were Li 1.04 Mg 0.004 Co 0.955 Al 0.024 The stoichiometry was controlled to obtain O2.

[0152] The second mixture was heated to 940° C. at a heating rate of 4.5° C. / min, and then heat-treated at that temperature for 5 hours to obtain small-grained Li particles having a layered structure and an average particle size (D50) of about 3.5 μm. 1.04 Mg 0.004 Co 0.955 Al 0.024 O2 was obtained.

[0153] The large particles and small particles obtained in the above process were mixed in a weight ratio of 8:2, and zirconium oxide was added thereto to obtain a third mixture. The third mixture was subjected to a second heat treatment at about 900°C, and the content of zirconium oxide was adjusted to a stoichiometric content so that the zirconium content in the bimodal positive electrode active material was 20,000 ppm. The bimodal positive electrode active material was composed of large Li particles with a ZrO2 coating film formed on the surface. 1.04 Mg 0.004 Co 0.955 Al 0.024 O2 (D50: 17μm) and small Li with a ZrO2 coating film on the surface. 1.04 Mg 0.004 Co 0.955 Al 0.024 A bimodal positive electrode active material containing Zr-coated large particles and small particles was obtained. The chemical formula of the final positive electrode active material containing Zr-coated large particles and small particles was Li 1.04 Mg 0.004 Co 0.955 Al 0.024 Zr 0.021 It's O2.

[0154] Comparative Example 1: LCO+Zr 7,500 ppm surface coating doped with Al 5,000 ppm and Mg 1,000 ppm A bimodal positive electrode active material was obtained in the same manner as in Example 1, except that LCO doped with 5,000 ppm of aluminum and 1,000 ppm of magnesium and surface-coated with 7,500 ppm of zirconium was used as the positive electrode active material.

[0155] Comparative Example 2: LCO+Zr 2,250 ppm surface coating doped with Al 6,500 ppm and Mg 1,000 ppm A bimodal positive electrode active material was obtained in the same manner as in Example 1, except that LCO doped with 6,500 ppm of aluminum and 1,000 ppm of magnesium and surface-coated with 2,250 ppm of zirconium was used as the positive electrode active material.

[0156] Comparative Example 3: LCO+Zr 7,500 ppm surface coating doped with Al 6,500 ppm and Mg 1,000 ppm A bimodal positive electrode active material was obtained in the same manner as in Example 1, except that LCO doped with 6,500 ppm of aluminum and 1,000 ppm of magnesium and surface-coated with 7,500 ppm of zirconium was used as the positive electrode active material.

[0157] Comparative Example 4: LCO+Zr 12,750 ppm surface coating doped with Al 6,500 ppm and Mg 1,000 ppm A bimodal positive electrode active material was obtained in the same manner as in Example 1, except that LCO doped with 6,500 ppm of aluminum and 1,000 ppm of magnesium and surface-coated with 12,750 ppm of zirconium was used as the positive electrode active material.

[0158] Comparative Example 5: LCO+Zr 21,000 ppm surface coating doped with Al 6,500 ppm and Mg 1,000 ppm A bimodal positive electrode active material was obtained in the same manner as in Example 1, except that LCO doped with 6,500 ppm of aluminum and 1,000 ppm of magnesium and surface-coated with 21,000 ppm of zirconium was used as the positive electrode active material.

[0159] Comparative Example 6: LCO + Zr 16,000 ppm and Ti 700 ppm surface coating doped with Al 6,500 ppm and Mg 1,000 ppm The same procedure as in Example 1 was carried out, except that LCO doped with 6,500 ppm of aluminum and 1,000 ppm of magnesium was used as the positive electrode active material, to obtain large particles and small particles.

[0160] The large particles and small particles obtained in the above process were mixed in a weight ratio of 8:2, and then titanium oxide and zirconium oxide were added thereto to obtain a third mixture. The content of zirconium oxide was controlled so that the content of zirconium in the positive electrode active material was 16,000 ppm, and the content of titanium oxide was controlled so that the content of titanium in the positive electrode active material was 700 ppm.

[0161] The third mixture was subjected to a second heat treatment at about 900° C. to obtain a bimodal positive electrode active material.

[0162] Comparative Example 7: LCO + Zr 18,000 ppm and Ti 700 ppm surface coating doped with Al 6,500 ppm and Mg 1,000 ppm A bimodal positive active material was obtained in the same manner as in Comparative Example 6, except that the content of zirconium oxide in the positive active material was changed so that the content of zirconium was changed to 18,000 ppm.

[0163] In the above-mentioned Examples 1 to 5 and Comparative Examples 1 to 7, the contents of aluminum doped in the positive electrode active material core, and zirconium, titanium, and cobalt present on the surface are summarized in Table 1 below.

[0164] [Table 1]

[0165] (Manufacture of lithium secondary batteries) Example 1 A mixture of the positive electrode active material obtained in Example 1, polyvinylidene fluoride, and carbon black as a conductive material was mixed in a mixer to remove air bubbles, thereby preparing a uniformly dispersed positive electrode active material layer forming slurry. N-methyl-2-pyrrolidone as a solvent was added to the mixture, and the mixture ratio of the positive electrode active material, polyvinylidene fluoride, and carbon black was 98:1:1 by weight. The slurry prepared by the above process was coated on aluminum foil using a doctor blade to form a thin electrode plate, which was then dried at 135°C for 3 hours or more, and then rolled and vacuum dried to prepare a positive electrode.

[0166] The negative electrode was manufactured by mixing natural graphite, carboxymethyl cellulose (CMC), and styrene butadiene rubber (SBR) to obtain a composition for forming a negative electrode active material, which was then coated on a copper current collector and dried to manufacture the negative electrode. The weight ratio of natural graphite, carboxymethyl cellulose (CMC), and styrene butadiene rubber (SBR) was 97.5:1:1.5, and the content of distilled water was about 50 parts by weight per 100 parts by weight of the total weight of natural graphite, carboxymethyl cellulose (CMC), and styrene butadiene rubber (SBR).

[0167] A separator (thickness: about 10 μm) made of a porous polyethylene (PE) film was placed between the positive electrode and the negative electrode, and an electrolyte was injected to prepare a lithium secondary battery. The electrolyte used was a solution containing 1.1 M LiPF6 dissolved in a solvent in which ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:4:3.

[0168] Examples 2 to 5 The same procedure as in Preparation Example 1 was carried out, except that the positive electrode active materials of Examples 2 to 8 were used instead of the positive electrode active material of Example 1, to manufacture the lithium secondary batteries.

[0169] Comparative production examples 1-7 The same procedure as in Preparation Example 1 was carried out, except that the positive electrode active materials of Comparative Examples 1 to 7 were used instead of the positive electrode active material of Example 1, to manufacture the lithium secondary batteries.

[0170] Evaluation example 1: Scanning electron microscope (SEM) Scanning electron microscope (SEM) analysis was performed on the positive electrode active materials prepared in Example 4 and Comparative Example 6. The results of the SEM analysis on the positive electrode active materials prepared in Example 4 and Comparative Example 6 are shown in FIGS. 1A and 1B.

[0171] As shown in FIG. 1B, in the positive electrode active material of Comparative Example 6, titanium was contained in the coating film, and soaking areas were observed.

[0172] In contrast, referring to FIG. 1A, the positive electrode active material of Example 4 does not show the soaking region on the surface thereof, unlike the positive electrode active material of Comparative Example 6, and it was found that the zirconium-containing coating film was present in the form of an island coating film.

[0173] Evaluation example 2: SEM-EDS (energy dispersive spectroscopy) analysis SEM-EDS analysis was performed on the positive electrode active material of Example 4. The SEM-EDS analysis results for the positive electrode active material of Example 4 are shown in Figures 2A to 2C. Figures 2A and 2B respectively show the analysis results for magnesium and zirconium on the surface of the positive electrode active material, and Figure 2C shows the overall composition analysis results on the surface of the positive electrode active material.

[0174] 2A to 2C, magnesium was not detected on the surface of the lithium cobalt oxide coated with zirconium without titanium in the positive electrode active material of Example 4. The absence of magnesium means that titanium was not coated.

[0175] In addition, the ratio of the zirconium content to the cobalt and zirconium content on the surface, Zr / (Co+Zr) molar ratio, was investigated and is shown in Figure 3. The surface Zr / (Co+Zr) molar ratio was investigated using EDAX (energy dispersive X-ray microanalysis).

[0176] 3, the positive electrode active material of Example 4 had an increased amount of zirconium coating compared to the positive electrode active material of Example 3, and thus the Zr / (Co+Zr) molar ratio was increased.

[0177] Evaluation example 3: TEM-EDS analysis SEM-EDS analysis was performed on the positive electrode active material of Example 4, and the results are shown in Figures 4A to 4F. Figures 4A to 4C show the results of analysis of zirconium in the zirconium coating layer of the positive electrode active material, and Figures 4D to 4F show the results of analysis of cobalt in the zirconium coating layer of the positive electrode active material. Figures 4A and 4D show the results of SEM-EDS analysis of the same region of the positive electrode active material, Figures 4B and 4E show the results of SEM-EDS analysis of the same region of the positive electrode active material, and Figures 4C and 4F show the results of SEM-EDS analysis of the same region of the positive electrode active material.

[0178] By referring to these, it was confirmed that a dense zirconium coating film was formed on the positive electrode active material, and it was found that cobalt was detected only in the core of the positive electrode active material.

[0179] Evaluation example 4: Charge / discharge characteristics The lithium secondary batteries of Preparation Examples 1 to 5 and Comparative Preparation Examples 1 to 5 were charged at a constant current of 0.5C at 25°C to a state of charge (SOC) of 90%, and aged for 48 hours. After that, the batteries were cut off at a current of 0.05C rate while maintaining 4.58V in a constant current / constant voltage mode. Then, the batteries were discharged at a constant current of 0.5C rate until the voltage reached 3.0V (formation stage).

[0180] The lithium secondary battery that had undergone the formation step was charged at a constant current of 0.2 C until the voltage reached 4.55 V. After the charged cell was rested for about 10 minutes, it was discharged at a constant current of 0.2 C until the voltage reached 3 V.

[0181] The initial charge / discharge efficiency was evaluated according to the following formula 1, and the evaluation results are shown in Table 2 below.

[0182] [Formula 1] Initial charge / discharge efficiency (%)=(1 time discharge capacity (0.2C) / 1 time charge capacity (0.2C))X100

[0183] Evaluation example 5: Evaluation of direct current internal resistance (DC-IR) before and after high-temperature charging and discharging The direct current internal resistance (DC-IR) was measured by the following method before and after the high-temperature charge-discharge evaluation for the lithium secondary batteries of Preparation Examples 1 to 5 using the positive electrode active materials of Examples 1 to 5 and the lithium secondary batteries of Comparative Preparation Examples 1 to 5 using the positive electrode active materials of Comparative Examples 1 to 5. The measurement results are shown in Table 2 below.

[0184] In the first cycle, the battery was charged at a constant current of 0.2 C rate until the voltage reached 4.45 V (vs. Li), and then cut off at a current of 0.05 C rate while maintaining 4.45 V in constant voltage mode. The battery was then discharged at a constant current of 0.2 C rate until the voltage reached 3.0 V (vs. Li) (formation stage).

[0185] In the second cycle, the battery was charged at a constant current of 0.2C rate to 4.45V (vs. Li), then maintained at 4.45V in constant voltage mode, and charged with a current cutoff of 0.05C rate. It was then discharged at a 0.2C rate for 2 hours and 30 minutes, and after reaching a SOC of 10% or 20%, it was discharged at a constant current of 3C for 10 seconds, then at a constant current of 0.2C for 10 seconds, and finally at a constant current of 3C for another 10 seconds.

[0186] The direct current internal resistance (DC-IR) (R=ΔV / ΔI) was calculated from the ratio of the average voltage change (ΔV) and the average current change (ΔI) during constant current discharge at each C-rate, and the average value was taken as the measured value.

[0187] Evaluation example 6: High temperature life The lithium secondary batteries of Preparation Examples 1 to 5 using the positive electrode active materials of Examples 1 to 5 and the lithium secondary batteries of Comparative Preparation Examples 1 to 5 using the positive electrode active materials of Comparative Examples 1 to 5 were charged at a constant current of 0.5C at 45°C to SOC 90%, and aged for 48 hours. After that, the current was cut off at a current of 0.05C rate while maintaining 4.58V in a constant current / constant voltage mode. Subsequently, the batteries were discharged at a constant current of 0.5C rate until the voltage reached 3.0V (formation stage (first cycle)).

[0188] The lithium secondary battery that had undergone the first cycle of the formation step was charged at a constant current of 0.2 C at 45° C. until the voltage reached 4.55 V. The charged cell was rested for about 10 minutes, and then discharged at a constant current of 0.2 C until the voltage reached 3 V. This cycle was repeated 30 times in total, and then evaluated.

[0189] The high temperature life was evaluated according to the following formula 2, and the evaluation results are shown in Table 2 below.

[0190] [Formula 2] High temperature life (%) = (discharge capacity after 30th cycle / discharge capacity after first cycle x 100

[0191] [Table 2]

[0192] As shown in Table 2, the lithium secondary batteries of Preparation Examples 1 to 5 have improved resistance characteristics compared to Comparative Preparation Examples 1 to 5. The charge / discharge efficiency of the lithium secondary batteries of Preparation Examples 1 to 5 is equal to or even better than that of Comparative Preparation Examples 1 to 5.

[0193] In comparison, the lithium secondary batteries of Comparative Preparation Examples 1 to 4 exhibit good charge / discharge efficiency, but the resistance characteristics are deteriorated as compared with those of Preparation Examples 1 to 5.

[0194] In addition, as can be seen from Table 2, the lithium secondary batteries of Preparation Examples 1 to 5 were confirmed to have improved high-temperature life compared to the lithium secondary batteries of Comparative Preparation Examples 1 to 5.

[0195] Evaluation example 7: TEM-SAED (selected area (electron) diffraction) analysis The positive electrode active material of Example 4 was subjected to TEM-SAED analysis, and the results are shown in FIG.

[0196] It was confirmed that a zirconium-containing coating film was formed on the surface of the positive electrode active material of Example 4, and cobalt was detected only in the core of the positive electrode active material. It was also found that the crystal structure of the inside of the positive electrode active material was an R-3m layered structure, and the coating particles of the zirconium coating film showed an Fm-3m (cubic structure) structure.

[0197] Although the above description has been given with reference to examples, it will be understood by those skilled in the art that various modifications and variations can be made without departing from the spirit and scope of the appended claims. [Explanation of symbols]

[0198] 31 Lithium secondary battery 32 negative electrode 33 Positive electrode 34 Separator 35 Battery case 36 Cap Assembly

Claims

1. A positive electrode active material for a lithium secondary battery, comprising a lithium cobalt-based oxide and a zirconium-based oxide disposed on a surface of the lithium cobalt-based oxide, The lithium cobalt-based oxide contains 4,000 ppm or more of aluminum, The positive electrode active material for a lithium secondary battery has a zirconium content of 15,000 to 20,000 ppm.

2. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the zirconium-based oxide is a compound represented by the following Chemical Formula 1: [Chemical formula 1] Mg x Zr y M1 z O 2 In Chemical Formula 1, 0≦x≦0.1, 0.8≦y≦1, 0≦z≦0.1, and 0.9<x+y+z<1.1; M1 is one or more elements selected from the group consisting of Co, Al, B, Ca, Sr, Ba, V, Cr, Fe, Cu, W, Mo, Ta and Nb.

3. The zirconium oxide is ZrO 2 The positive electrode active material for a lithium secondary battery according to claim 1 ,

4. 3. The positive electrode active material for a lithium secondary battery according to claim 2, wherein the zirconium-based oxide belongs to a space group of Fm-3m and has a cubic structure.

5. The positive electrode active material for a lithium secondary battery according to claim 2 , wherein x is 0 in Formula 1.

6. The zirconium-based oxide has a particulate form, and the particle size of the zirconium-based oxide is 0.2 μm to 2 μm; The positive electrode active material for a lithium secondary battery according to claim 1 , wherein the zirconium-based oxide is present in an island shape.

7. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the aluminum content is 4,000 ppm to 8,000 ppm.

8. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the positive electrode active material has a zirconium content of 18,000 to 20,000 ppm.

9. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the positive electrode active material has a Zr / (Co+Zr) molar ratio of 0.25 to 0.

35.

10. The positive electrode active material further contains magnesium, The positive electrode active material for a lithium secondary battery according to claim 1 , wherein the zirconium content is greater than the magnesium content.

11. 11. The positive electrode active material for a lithium secondary battery according to claim 10, wherein the magnesium content is 500 to 2,000 ppm.

12. The positive electrode active material for a lithium secondary battery according to claim 1, which is a compound represented by the following chemical formula 2: [Chemical formula 2] Li a-b MM b Co x Al y M1 z O 2 In chemical formula 2, 0.9<a<1.1, 0≦b<0.1, 0.02≦x≦1, 0.015≦y≦0.03, 0<z<0.03, and 0.9≦x+y+z≦1.1, M1 is one or more elements selected from the group consisting of Zr, Ni, Mn, B, Ca, Sr, Ba, V, Cr, Fe, Cu, W, Mo, Ta and Nb.

13. the positive electrode active material is small particles, large particles, or a mixture of small particles and large particles; The size of the large particles is 10 μm to 20 μm, 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the small particles have a size of 2 to 8 μm.

14. 14. The positive electrode active material for a lithium secondary battery according to claim 13, wherein the zirconium-based oxide comprises a mixture of large particles and small particles, and a weight ratio of the large particles to the small particles in the mixture of the large particles and the small particles is 7:3 to 9:

1.

15. Mixing a lithium cobalt-based oxide containing 4,000 ppm or more of aluminum with a zirconium precursor to obtain a mixture; and heat-treating the mixture to produce the cathode active material of claim 1.

16. The method for producing a positive electrode active material for a lithium secondary battery according to claim 15, wherein the zirconium precursor is at least one selected from the group consisting of zirconium oxide, zirconium chloride, zirconium sulfate, and zirconium oxide.

17. The method of claim 15, wherein the heat treatment is performed at a temperature of 900°C to 1,100°C.

18. The method for producing a positive electrode active material for a lithium secondary battery according to claim 15, wherein the lithium cobalt-based oxide containing 4,000 ppm or more of aluminum further contains magnesium.

19. The method of claim 18, wherein the magnesium content is 500 to 2,000 ppm.

20. A positive electrode comprising the positive electrode active material according to claim 1; A negative electrode; and an electrolyte interposed between the positive electrode and the negative electrode.

Citation Information

Cited By

  • Positive electrode active material for secondary battery