All-solid-state secondary battery

By using a carbon-based material matrix with nanostructures in the negative electrode active material layer and a protective layer, the issues of side reactions and short circuits in sulfide-based solid electrolyte lithium batteries are addressed, resulting in improved uniformity and cycle characteristics.

JP2024138229APending Publication Date: 2024-10-08SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024049759
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-05
Filing Date
2024-03-26
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Sulfide-based solid electrolytes in lithium batteries react with negative electrode current collectors, leading to side reactions, non-uniform thickness of the negative electrode active material layer, and aggregation of the active material, which can cause short circuits and lithium dendrite growth.

Method used

Incorporating a carbon-based material matrix with a carbon-based nanostructure in the negative electrode active material layer and a protective layer to suppress aggregation and ensure uniform thickness, thereby preventing short circuits and improving cycle characteristics.

Benefits of technology

The solution enhances the uniformity of the negative electrode active material layer thickness, suppresses aggregation, and improves the cycle characteristics and safety of the all-solid-state secondary battery by reducing short circuits and side reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138229000001_ABST
    Figure 2024138229000001_ABST
Patent Text Reader

Abstract

To provide an all-solid-state secondary battery.SOLUTION: An all-solid-state secondary battery includes: a positive electrode layer; a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, the positive electrode layer includes a positive electrode current collector, and a positive electrode active material layer, the solid electrolyte layer includes a sulfide-based solid electrolyte, the negative electrode layer includes a negative electrode current collector, a first negative electrode active material layer, and a first protective layer disposed between the negative electrode current collector and the first negative electrode active material layer, the first negative electrode active material layer includes a carbon-based material matrix and a metal-based negative electrode active material disposed within the carbon-based material matrix, the carbon-based material matrix includes a first carbon-based nanostructure, and the first protective layer includes a second carbon-based nanostructure.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to an all-solid-state secondary battery. [Background technology]

[0002] Recently, there has been active development of batteries that offer increased energy density and safety. Lithium batteries are used in information devices, communication devices, automobiles, etc. Since automobiles are connected to human life, safety is important.

[0003] Lithium batteries containing liquid electrolytes contain flammable organic solvents, which increases the risk of overheating and fire in the event of a short circuit.

[0004] Solid electrolytes have a reduced possibility of overheating and fire in the event of a short circuit compared to liquid electrolytes, and lithium batteries containing solid electrolytes may offer improved safety compared to lithium batteries containing liquid electrolytes. Summary of the Invention [Problem to be solved by the invention]

[0005] Sulfide-based solid electrolytes are prone to side reactions with negative electrode current collectors. For example, if a sulfide-based solid electrolyte comes into contact with a copper current collector during charging and discharging, the side reaction between the sulfide-based solid electrolyte and the copper current collector can shorten the life of the lithium battery. Therefore, a method is needed to prevent contact between the sulfide-based solid electrolyte and the negative electrode current collector.

[0006] A negative electrode active material layer, which is disposed between a solid electrolyte layer and a negative electrode current collector in a wet manner, is difficult to achieve a uniform thickness. Thickness deviations in the negative electrode active material layer can lead to uneven lithium deposition and lithium dendrite growth between the negative electrode active material layer and the negative electrode current collector. Such uneven lithium deposition and / or lithium dendrite growth can cause a short circuit in a lithium battery. A method for reducing thickness deviations in the negative electrode active material layer is needed.

[0007] A negative electrode active material layer that is wet-disposed between a solid electrolyte layer and a negative electrode current collector is prone to agglomeration of the negative electrode active material within the negative electrode active material layer during drying. The agglomerated negative electrode active material can result in non-uniform current density within the negative electrode active material layer. The non-uniform current density can cause non-uniform lithium deposition and / or lithium dendrite growth between the negative electrode active material layer and the negative electrode current collector. Such non-uniform lithium deposition and / or lithium dendrite growth can cause a short circuit in a lithium battery. A method for suppressing agglomeration of the negative electrode active material within the negative electrode active material layer is needed.

[0008] One aspect is to provide an all-solid-state secondary battery with a new structure. [Means for solving the problem]

[0009] According to one aspect, there is provided an all-solid-state secondary battery including: a positive electrode layer; a negative electrode layer; and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, wherein the positive electrode layer includes a positive electrode current collector; and a positive electrode active material layer, the solid electrolyte layer including a sulfide-based solid electrolyte; the negative electrode layer includes an negative electrode current collector; a first negative electrode active material layer; and a first protective layer disposed between the negative electrode current collector and the first negative electrode active material layer, wherein the first negative electrode active material layer includes a carbon-based material matrix and a metal-based negative electrode active material disposed within the carbon-based material matrix, the carbon-based material matrix including a first carbon-based nanostructure, and the first protective layer including a second carbon-based nanostructure. [Effects of the Invention]

[0010] According to an all-solid-state secondary battery having a new structure according to one aspect, it is possible to provide an all-solid-state secondary battery having improved cycle characteristics by improving the uniformity of the thickness of the negative electrode active material layer and suppressing aggregation of the negative electrode active material, thereby suppressing short circuits. [Brief explanation of the drawings]

[0011] [Figure 1] 1 is a cross-sectional view of an all-solid-state secondary battery according to an illustrative embodiment; [Figure 2]1 is a cross-sectional view of a bi-cell all-solid-state secondary battery according to an illustrative embodiment; [Figure 3] 1 is a cross-sectional view of an all-solid-state secondary battery according to an illustrative embodiment; [Figure 4] 1 is a cross-sectional view of an all-solid-state secondary battery according to an illustrative embodiment; [Figure 5] 1 is a cross-sectional view of a bi-cell all-solid-state secondary battery according to an illustrative embodiment; DETAILED DESCRIPTION OF THE INVENTION

[0012] Various embodiments are illustrated in the accompanying drawings. However, the present invention may be embodied in various other forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. Like reference numerals refer to like elements throughout.

[0013] When an element is referred to as being "on" another element, it will be understood that it may be located directly on top of the other element, or that there may be other intervening elements. In contrast, when an element is referred to as being "directly on" another element, there are no intervening elements.

[0014] Terms such as "first," "second," and "third" may be used herein to describe various components, components, regions, layers, and / or sections, but these components, components, regions, layers, and / or sections should not be limited by these terms. These terms are used to distinguish one component, component, region, layer, or section from another component, component, region, layer, or section. Thus, a first component, component, region, layer, or section described below could be referred to as a second component, component, region, layer, or section without departing from the teachings of this specification.

[0015] The terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the present invention. As used herein, the singular forms "a," "an," "the ...

[0016] Spatially relative terms such as "below," "lower," "bottom," "top," "upper," and "top" may be used herein to easily describe the relationship of one component or feature to another. It will be understood that spatially relative terms are intended to further encompass different orientations of the device in use or operation relative to the orientation depicted in the figures. For example, if the device in the figures were inverted, a component described as "below" or "below" another component or feature would be oriented "above" that other component or feature. Thus, the exemplary term "bottom" encompasses both an up-down orientation. The device could be otherwise oriented (rotated 90 degrees or rotated in another direction), and the spatially relative terms used herein would be interpreted accordingly.

[0017] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which this disclosure belongs. It will also be understood that terms as defined in commonly used dictionaries should be interpreted to have a meaning consistent with their meaning within the context of the relevant art and the content of this disclosure, and should not be interpreted as idealized or overly formal.

[0018] Example embodiments are described herein with reference to cross-section illustrations that are schematic illustrations of idealized embodiments. As such, variations from the shapes of the illustrations as a result, for example, of manufacturing techniques and / or tolerances, are to be expected. Therefore, the embodiments described herein should not be construed as limited to the specific shapes of regions as illustrated herein but are to include deviations in shapes that, for example, result from manufacturing. For example, regions illustrated or described as flat may typically have rough and / or non-linear characteristics. Additionally, corners illustrated as sharp may also be rounded. Accordingly, regions illustrated in the figures are schematic in nature, and their shapes are not intended to illustrate the precise shapes of the regions and are not intended to limit the scope of the claims.

[0019] "Group" means a group in the Periodic Table of the Elements according to the International Union of Pure and Applied Chemistry ("IUPAC") Group 1-18 group classification system.

[0020] In the present disclosure, "particle size" refers to the average diameter when the particles are spherical, and refers to the average major axis length when the particles are non-spherical. Particle size is measured using a particle size analyzer (PSA). "Particle size" is, for example, the average particle size. "Average particle size" is, for example, D50, which is the median particle size.

[0021] D50 is the particle size corresponding to 50% cumulative volume calculated from the particle side having a small particle size in the particle size distribution measured by laser diffraction method.

[0022] D90 is the particle size corresponding to 90% cumulative volume calculated from the particle side having a small particle size in the particle size distribution measured by laser diffraction method.

[0023] D10 is the particle size corresponding to 10% cumulative volume calculated from the particle side having a small particle size in the particle size distribution measured by laser diffraction method.

[0024] Meanwhile, in the present disclosure, the "particle size" is measured manually or by software from a scanning electron microscope and / or transmission electron microscope image of a cross section of an all-solid-state secondary battery, and is the arithmetic mean value of particle sizes of a plurality of particles shown in the image.

[0025] In this disclosure, "metal" includes both metals and metalloids such as silicon and germanium, in either the elemental or ionic state.

[0026] In this disclosure, "alloy" means a mixture of two or more metals.

[0027] In this disclosure, "electrode active material" refers to an electrode material that undergoes lithiation and delithiation.

[0028] In this disclosure, "positive electrode active material" refers to a positive electrode material that undergoes lithiation and delithiation.

[0029] In this disclosure, "negative electrode active material" refers to a negative electrode material that undergoes lithiation and delithiation.

[0030] As used herein, "lithiation" and "lithiating" refer to the process of adding lithium to an electrode active material.

[0031] As used herein, "delithiation" and "delithiating" refer to the process of removing lithium from an electrode active material.

[0032] In this disclosure, "charge" and "charging" refer to the process of providing electrochemical energy to a battery.

[0033] In this disclosure, "discharge" and "discharging" refer to the process of removing electrochemical energy from a battery.

[0034] In this disclosure, "positive electrode" and "cathode" refer to the electrode where electrochemical reduction and lithiation occurs during the discharge process.

[0035] In this disclosure, "negative electrode" and "anode" refer to the electrodes where electrochemical oxidation and delithiation occurs during the discharge process.

[0036] While particular embodiments have been described, presently unforeseen or unforeseeable alternatives, modifications, variations, improvements, and substantial equivalents may occur to applicant or those skilled in the art. Accordingly, the claims as filed, and as they may be amended, are intended to cover all such alternatives, modifications, variations, improvements, and substantial equivalents.

[0037] Hereinafter, the all-solid-state secondary battery according to an example embodiment will be described in more detail.

[0038] [All-solid-state secondary battery] An all-solid-state secondary battery according to an embodiment includes a positive electrode layer; a negative electrode layer; and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, wherein the positive electrode layer includes a positive electrode current collector and a positive electrode active material layer, the solid electrolyte layer including a sulfide-based solid electrolyte, and the negative electrode layer includes a negative electrode current collector; a first negative electrode active material layer; and a first protective layer disposed between the negative electrode current collector and the first negative electrode active material layer, wherein the first negative electrode active material layer includes a carbon-based material matrix and a metal-based negative electrode active material disposed in the carbon-based material matrix, the carbon-based material matrix including a first carbon-based nanostructure, and the first protective layer including a second carbon-based nanostructure.

[0039] The inclusion of a dry-applied carbon-based nanostructure in the first negative electrode active material layer prevents defects such as uneven thickness of the negative electrode active material layer and aggregation of the negative electrode active material that occur in wet-applied negative electrode active material layers. The inclusion of such a first negative electrode active material layer in an all-solid-state secondary battery suppresses uneven lithium deposition and / or lithium dendrite growth during charge and discharge. As a result, short circuits in the all-solid-state secondary battery are suppressed, improving its lifespan characteristics. The inclusion of a first protective layer in an all-solid-state secondary battery suppresses side reactions due to contact between the sulfide-based solid electrolyte and the negative electrode current collector. As a result, the reversibility of the electrode reaction is improved, improving the lifespan characteristics of the all-solid-state secondary battery.

[0040] 1 to 5, the all-solid-state secondary battery 1 includes a positive electrode layer 10; a negative electrode layer 20; and a solid electrolyte layer 30 disposed between the positive electrode layer 10 and the negative electrode layer 20. The positive electrode layer 10 includes a positive electrode current collector 11 and a positive electrode active material layer 12. The solid electrolyte layer 30 includes a sulfide-based solid electrolyte. The negative electrode layer 20 includes a negative electrode current collector 21; a first negative electrode active material layer 22; and a first protective layer 23 disposed between the negative electrode current collector 21 and the first negative electrode active material layer 22. The first negative electrode active material layer 22 includes a carbon-based material matrix and a metal-based negative electrode active material disposed in the carbon-based material matrix. The carbon-based material matrix includes a first carbon-based nanostructure. The first protective layer 23 includes a second carbon-based nanostructure.

[0041] [Negative electrode layer] [Anode layer: carbon-based material matrix] 1 to 5, the negative electrode layers 20, 20a, 20b include a negative electrode current collector 21; first negative electrode active material layers 22, 22a, 22b; and first protective layers 23, 23a, 23b disposed between the negative electrode current collectors 21, 21a, 21b and the first negative electrode active material layer 22. The first negative electrode active material layer 22 includes a carbon-based material matrix and a metal-based negative electrode active material disposed within the carbon-based material matrix.

[0042] The first negative electrode active material layer 22 includes a carbon-based material matrix. The carbon-based material matrix includes a first carbon-based nanostructure. A carbon-based nanostructure is a structure having nano-sized dimensions and made of a carbon-based material. The carbon-based nanostructure may include, for example, a one-dimensional carbon-based nanostructure, a two-dimensional carbon-based nanostructure, a three-dimensional carbon-based nanostructure, or a combination thereof. The one-dimensional carbon-based nanostructure may include, for example, a carbon nanorod, a nanofiber, a carbon nanotube, or a combination thereof. The two-dimensional carbon-based nanostructure may include, for example, a carbon nanosheet, a carbon nanobelt, a carbon nanoflake, graphene, graphene oxide (GO), reduced graphene oxide (rGO), or a combination thereof. The three-dimensional carbon-based nanostructure may also be a structure in which multiple one-dimensional and / or two-dimensional carbon-based nanostructures are connected or stacked. The first carbon-based nanostructure may include, for example, a two-dimensional carbon-based nanostructure. The first carbon-based nanostructure can include, for example, graphene, graphene oxide (GO), reduced graphene oxide (rGO), or a combination thereof.

[0043] The carbon-based material matrix may include, for example, first carbon-based nanostructures aligned in a certain direction. The first carbon-based nanostructures may include, for example, graphene. The carbon-based material matrix may include graphene aligned in a certain direction. The carbon-based material matrix may include, for example, first carbon-based nanostructures aligned in a direction parallel to the surface of the negative electrode current collector 21. The carbon-based material matrix may include, for example, graphene. The carbon-based material matrix may include graphene aligned in a direction parallel to the surface of the negative electrode current collector 21. The graphene may be aligned at an angle of, for example, -30° to 30°, -20° to 20°, -10° to 10°, or -5° to 5° with respect to the surface of the negative electrode current collector 21. The alignment of the first carbon-based nanostructures in the carbon-based material matrix in a direction parallel to the surface of the negative electrode current collector 21 may more effectively suppress the growth of lithium dendrites through the first negative electrode active material layer 22. In addition, the first negative electrode active material layer 22 has a structure in which first carbon-based nanostructures are stacked in the carbon-based material matrix along the thickness direction of the first negative electrode active material layer 22. A plurality of first carbon-based nanostructures may be stacked in the carbon-based material matrix along the thickness direction of the first negative electrode active material layer 22. The carbon-based material matrix may include, for example, a plurality of first carbon-based nanostructure layers stacked in the thickness direction of the first negative electrode active material layer 22. As the first carbon-based nanostructures are stacked in the carbon-based material matrix along the thickness direction of the first negative electrode active material layer 22, the structural compactness and structural stability of the first negative electrode active material layer 22 may be further improved.

[0044] The carbon-based material matrix may include, for example, first carbon-based nanostructures that are irregularly arranged and not aligned. The first carbon-based nanostructures may include, for example, graphene, and the carbon-based material matrix may include irregularly arranged and not aligned graphene. The carbon-based material matrix may include, for example, first carbon-based nanostructures that are irregularly and / or randomly aligned on the surface of the negative electrode current collector 21. The carbon-based material matrix may include, for example, graphene, and the carbon-based material matrix may include graphene that is irregularly and / or randomly aligned on the surface of the negative electrode current collector 21. The irregular and / or random alignment of the first carbon-based nanostructures on the surface of the negative electrode current collector 21 within the carbon-based material matrix diversifies the lithium ion transport pathways and / or electron transport pathways through the first negative electrode active material layer 22. Therefore, the internal resistance of an all-solid-state secondary battery including the carbon-based material matrix may be further reduced.

[0045] The carbon-based material matrix may include, for example, crystalline carbon, amorphous carbon, or a combination thereof. The carbon-based material matrix may include first carbon-based nanostructures, which may include, for example, crystalline carbon nanostructures, amorphous carbon nanostructures, or a combination thereof. A carbon-based material matrix made of crystalline carbon nanostructures has high crystallinity. A carbon-based material matrix made of amorphous carbon nanostructures has low crystallinity. For example, the carbon-based material matrix may include first carbon-based nanostructures aligned in a certain direction, thereby increasing the crystallinity of the carbon-based material matrix. The crystallinity of the first negative electrode active material layer 22 may increase as the content of the aligned first carbon-based nanostructures in the carbon-based material matrix increases. For example, the carbon-based material matrix may include, for example, irregularly arranged first carbon-based nanostructures, thereby decreasing the crystallinity of the carbon-based material matrix. An increase in the content of the first carbon-based nanostructures that are irregularly arranged in the carbon-based material matrix reduces the crystallinity of the first negative electrode active material layer 22. The crystallinity of the carbon-based material matrix can be determined by, for example, Raman spectroscopy, XRD spectroscopy, high-resolution transmission electron microscopy, etc.

[0046] The carbon-based material matrix may include a first carbon-based nanostructure, and the first carbon-based nanostructure may be doped with, for example, a dopant. The dopant may include an n-type dopant, a p-type dopant, or a combination thereof. An n-type dopant is, for example, a dopant that has more electrons than carbon and thereby introduces electrons into the carbon-based material. A p-type dopant is, for example, a dopant that has fewer electrons than carbon and thereby introduces holes into the carbon-based material. The first carbon-based nanostructure may include, for example, graphene doped with a dopant. The doped graphene may include, for example, an n-type dopant, a p-type dopant, or a combination thereof. The dopant may include, for example, nitrogen (N), phosphorus (P), boron (B), sulfur (S), fluorine (F), chlorine (Cl), bromine (Br), germanium (Ge), gallium (Ga), or a combination thereof. Nitrogen (N) and phosphorus (P) are examples of n-type dopants. Gallium (Ga) is an example of a p-type dopant. The content of the dopant in the doped first carbon-based nanostructure may be, for example, 3 at % or less, 2 at % or less, 1 at % or less, or 0.5 at % or less. The doping of the first carbon-based nanostructure with the dopant may further increase the conductivity of the first carbon-based nanostructure. The inclusion of the doped first carbon-based nanostructure in the carbon-based material matrix may reduce the internal resistance of the first negative electrode active material layer 22 and further reduce the interfacial resistance between the first negative electrode active material layer 22 and the solid electrolyte layer 30. As a result, the internal resistance of the all-solid-state secondary battery may be reduced, and the high-rate characteristics may be further improved.

[0047] The carbon-based material matrix does not contain a binder. Because the carbon-based material matrix does not contain a binder, the internal resistance of the first negative electrode active material layer 22 can be reduced, and the ionic conductivity and / or electronic conductivity can be improved. As a result, the cycle characteristics, such as the high-rate characteristics, of the all-solid-state secondary battery can be improved.

[0048] The carbon-based material matrix may further include, for example, pores arranged within the carbon-based material matrix. The carbon-based material matrix may include a plurality of first carbon-based nanostructures, and the plurality of first carbon-based nanostructures may be irregularly arranged, thereby forming pores defined by the plurality of first carbon-based nanostructures within the carbon-based material matrix. The carbon-based material matrix may have low porosity due to, for example, the first carbon-based nanostructures aligned in a certain direction. As the content of the aligned first carbon-based nanostructures within the carbon-based material matrix increases, the content of pores within the carbon-based material matrix may decrease. Therefore, the first negative electrode active material layer 22 may have a reduced porosity. For example, the carbon-based material matrix may include, for example, irregularly arranged first carbon-based nanostructures, thereby increasing the porosity of the carbon-based material matrix. As the content of the irregularly arranged first carbon-based nanostructures within the carbon-based material matrix increases, the content of pores within the carbon-based material matrix may increase. Therefore, the first negative electrode active material layer 22 has an increased porosity. The porosity of the carbon-based material matrix can be measured by, for example, a gas adsorption method.

[0049] The carbon-based material matrix may also be a lithium host, for example. The carbon-based material matrix may also be an electrochemically inert lithium host, for example. The electrochemically inert lithium host is a lithium host that does not react with lithium to form a compound but acts as a conductor for electron transfer and / or a receptor for accommodating deposited lithium. The carbon-based material matrix acts as an electrochemically inert lithium host, which may more effectively prevent deterioration of the all-solid-state secondary battery 1 due to volume changes and / or changes in physical properties of the first negative electrode active material layer 22 during charge and discharge. Therefore, the carbon-based material matrix acts as an electrochemically inert lithium host, which may more effectively perform electron transfer and / or lithium deposition in the first negative electrode active material layer 22. Meanwhile, the carbon-based material matrix may also be an electrochemically active lithium host, for example. The electrochemically active lithium host is a lithium host that reacts with lithium to form a compound. The carbon-based material matrix acts as an electrochemically active lithium host, which more effectively prevents non-uniform lithium deposition in the first negative electrode active material layer 22, thereby further improving the cycle characteristics of the all-solid-state secondary battery 1. Therefore, the carbon-based material matrix acts as an electrochemically active lithium host, which allows uniform lithium deposition in the first negative electrode active material layer 22. The carbon-based material matrix further includes pores, which allow lithium metal to be deposited in the pores.

[0050] [Negative electrode layer: negative electrode active material] 1 to 5, the negative electrode layer 20 includes a negative electrode current collector 21 and a first negative electrode active material layer 22 disposed on the negative electrode current collector. The first negative electrode active material layer 22 includes a metal-based negative electrode active material disposed in a carbon-based material matrix.

[0051] A metal-based negative electrode active material is a negative electrode active material that forms an alloy or compound with lithium. Examples of metal-based negative electrode active materials include, but are not limited to, one or more alloying elements selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). Any metal-based negative electrode active material that can form an alloy or compound with lithium in the art can be used. For example, nickel (Ni) does not form an alloy with lithium and is therefore not a metal-based negative electrode active material. Metal-based negative electrode active materials do not include, for example, metal oxides. Metal-based negative electrode active materials include, for example, metals that can form alloys or compounds with lithium, but do not include oxides of such metals. Metal-based negative electrode active materials include, for example, silver (Ag), but do not include silver (Ag) oxides (e.g., AgO).

[0052] The metal-based negative electrode active material may also be, for example, a composite negative electrode active material having a core / shell structure. The metal-based negative electrode active material may include, for example, a core and a shell disposed along the surface of the core. The shell may cover part or all of the surface of the core. The core may include, for example, a metal that forms an alloy or compound with lithium. The metal that forms an alloy or compound with lithium may include, for example, one or more alloying elements selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The shell may include, for example, a carbon-based material. The shell may include, for example, a third carbon-based nanostructure. The third carbon-based nanostructure may be, for example, a carbon-based nanostructure such as the first carbon-based nanostructure. The third carbon-based nanostructure may include, for example, graphene, graphene oxide, reduced graphene oxide, or a combination thereof. The third carbon-based nanostructures may be distinguished from the first carbon-based nanostructures contained in the carbon-based material matrix in one or more of their physical properties, such as composition, thickness, position, and crystallinity. The third carbon-based nanostructures may, for example, constitute a shell of a metal-based negative electrode active material and be distinguished from the carbon-based material matrix. The metal-based negative electrode active material may have a structure including, for example, a metal core containing a metal that forms an alloy or compound with lithium, and a shell containing the third carbon-based nanostructure disposed on the core. The metal-based negative electrode active material may have a structure including, for example, a metal core containing a metal that forms an alloy or compound with lithium, and a shell containing graphene disposed on the core. The shell may include, for example, amorphous carbon. The amorphous carbon content of the shell may facilitate ion and / or electron transfer between the core and the carbon-based material matrix. The shell may also be, for example, an amorphous carbon coating layer disposed on the core. The metal-based negative electrode active material may have a structure including, for example, a metal core containing a metal that forms an alloy or compound with lithium, and an amorphous carbon-containing shell disposed on the core.The metal-based negative electrode active material has a structure of, for example, a metal core containing a metal that forms an alloy or compound with lithium; and an amorphous carbon coating layer disposed on the core.

[0053] The metal-based negative electrode active material may be, for example, particulate. The particle size of the particulate metal-based negative electrode active material may be, for example, 2 μm or less, 1.5 μm or less, 1 μm or less, 0.5 μm or less, or 100 nm or less. The particle size of the particulate metal-based negative electrode active material may be, for example, 1 nm to 2 μm, 1 nm to 1.5 μm, 5 nm to 1 μm, 10 nm to 500 nm, 10 nm to 400 nm, 10 nm to 200 nm, or 10 nm to 100 nm. When the metal-based negative electrode active material has a particle size within such a range, reversible absorbing and / or desorbing of lithium during charging and discharging may be facilitated. The metal-based negative electrode active material may also be a reduction product of a metal-based negative electrode active material precursor. The metal-based negative electrode active material may also be a reduction product of metal ions. Because the metal-based negative electrode active material is a reduction product of metal ions, it does not aggregate and can be uniformly dispersed within the carbon-based material matrix. The particle size of the metal-based negative electrode active material is, for example, an arithmetic mean particle size of the metal-based negative electrode active material obtained by analyzing, using software or manually, an electron microscope image of a cross section of the first negative electrode active material layer 22. The metal-based negative electrode active material particles may include a core and a shell disposed along the surface of the core. The particle size of the core is, for example, 1 nm to 1 μm, 10 nm to 500 nm, 10 nm to 400 nm, 10 nm to 300 nm, 10 nm to 200 nm, or 10 nm to 100 nm. The thickness of the shell is, for example, 100 nm or less, 50 nm or less, 40 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less. The thickness of the shell is, for example, 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 40 nm, 1 nm to 30 nm, 1 nm to 20 nm, or 1 nm to 10 nm. When the core and shell have particle sizes and thicknesses within these ranges, the cycle characteristics of the all-solid-state secondary battery 1 containing the metal-based negative electrode active material particles can be further improved.

[0054] The content of the metal-based negative electrode active material may be 10 parts by weight or less, 5 parts by weight or less, 3 parts by weight or less, or 2 parts by weight or less, per 100 parts by weight of the carbon-based material matrix. The content of the metal-based negative electrode active material may be 0.1 to 10 parts by weight, 0.5 to 5 parts by weight, 0.5 to 3 parts by weight, or 0.5 to 2 parts by weight, per 100 parts by weight of the carbon-based material matrix. Having the metal-based negative electrode active material in this range may further improve the cycle characteristics of the all-solid-state secondary battery 1. Compared to a conventional first negative electrode active material layer 22 containing a simple blend of a metal-based negative electrode active material and a carbon-based material, the first negative electrode active material layer 22 employed in the all-solid-state secondary battery 1 of FIGS. 1 to 5 has a reduced content of the metal-based negative electrode active material. Since the first negative electrode active material layer 22 includes a metal-based negative electrode active material dispersed and disposed in a carbon-based material matrix by a dry method, it is possible to provide an all-solid-state secondary battery 1 having excellent cycle characteristics with a relatively low content of the metal-based negative electrode active material.

[0055] The carbon-based material matrix may further include a carbon-based negative electrode active material disposed within the carbon-based material matrix. The carbon-based negative electrode active material may be, for example, amorphous carbon. Examples of amorphous carbon include, but are not limited to, carbon black (CB), acetylene black (AB), furnace black (FB), and ketjen black (KB). Any amorphous carbon classified as amorphous carbon in the art may be used. Amorphous carbon is carbon with no or very low crystallinity and is distinguished from crystalline carbon or graphite-based carbon. The carbon-based negative electrode active material may be omitted.

[0056] [Negative electrode layer: first negative electrode active material layer] The thickness of the first negative electrode active material layer 22 is, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less of the thickness of the positive electrode active material layer 12. The thickness of the first negative electrode active material layer 22 is, for example, 20 μm or less, 10 μm or less, 7 μm or less, or 5 μm or less. The thickness of the first negative electrode active material layer 22 is, for example, 1 μm to 20 μm, 2 μm to 10 μm, 2 μm to 7 μm, or 2 μm to 5 μm. If the thickness of the first negative electrode active material layer 22 is excessively thin, lithium dendrites formed between the first negative electrode active material layer 22 and the negative electrode current collector 21 will collapse the first negative electrode active material layer 22, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery 1. If the thickness of the first negative electrode active material layer 22 increases excessively, the energy density of the all solid state secondary battery 1 decreases, and the first negative electrode active material layer 22 increases the internal resistance of the all solid state secondary battery 1, making it difficult to improve the cycle characteristics of the all solid state secondary battery 1.

[0057] If the thickness of the first negative electrode active material layer 22 is reduced, for example, the charge capacity of the first negative electrode active material layer 22 also decreases. The charge capacity of the first negative electrode active material layer 22 is, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, 5% or less, or 2% or less of the charge capacity of the positive electrode active material layer 12. The charge capacity of the first negative electrode active material layer 22 is, for example, 0.1% to 50%, 0.1% to 40%, 0.1% to 30%, 0.1% to 20%, 0.1% to 10%, 0.1% to 5%, or 0.1% to 2% of the charge capacity of the positive electrode active material layer 12. If the charge capacity of the first anode active material layer 22 is excessively small, the thickness of the first anode active material layer 22 becomes very thin, and thus lithium dendrites formed between the first anode active material layer 22 and the anode current collector 21 during repeated charge and discharge processes collapse the first anode active material layer 22, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery 1. If the charge capacity of the first anode active material layer 22 is excessively increased, the energy density of the all-solid-state secondary battery 1 decreases and the internal resistance of the all-solid-state secondary battery 1 increases due to the first anode active material layer 22, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery 1. The ratio C1 / C2 of the charge capacity C1 of the first negative electrode active material layer 22 to the charge capacity C2 of the positive electrode active material layer 12 is, for example, 0.001 to 0.45, 0.001 to 0.4, 0.001 to 0.3, 0.001 to 0.25, 0.001 to 0.2, 0.001 to 0.1, 0.001 to 0.05, or 0.001 to 0.02. The charge capacity of the positive electrode active material layer 12 is obtained by multiplying the charge capacity density (mAh / g) of the positive electrode active material by the mass of the positive electrode active material in the positive electrode active material layer 12. When many types of positive electrode active materials are used, the charge capacity density x mass value is calculated for each positive electrode active material, and the sum of these values ​​is the charge capacity of the positive electrode active material layer 12. The charge capacity of the first negative electrode active material layer 22 is calculated in a similar manner. That is, the charge capacity of the first negative electrode active material layer 22 is obtained by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the first negative electrode active material layer 22. When various negative electrode active materials are used, the charge capacity density x mass value is calculated for each negative electrode active material, and the sum of these values ​​is the capacity of the first negative electrode active material layer 22. Here, the charge capacity densities of the positive electrode active material and the negative electrode active material are capacities estimated using an all-solid-state half-cell using lithium metal as the counter electrode.The charge capacities of the positive electrode active material layer 12 and the first negative electrode active material layer 22 are directly measured by measuring the charge capacity using an all-solid-state half-cell. The charge capacity density is obtained by dividing the measured charge capacity by the mass of each active material. Meanwhile, the charge capacities of the positive electrode active material layer 12 and the first negative electrode active material layer 22 are also the initial charge capacities measured during the first charge cycle.

[0058] The first negative electrode active material layer 22 is also binder-free. Because the first negative electrode active material layer 22 is formed by a dry method, the first negative electrode active material layer 22 does not contain a binder. Because the first negative electrode active material layer 22 does not contain a binder, the electronic conductivity and / or ionic conductivity of the first negative electrode active material layer 22 may be improved, and the internal resistance may be reduced. Therefore, the cycle characteristics, such as the high rate characteristics, of the all-solid-state secondary battery 1 including such a first negative electrode active material layer 22 may be improved. The first negative electrode active material layer may be manufactured by a dry method such as CVD or PVD. The dry method used to manufacture the first negative electrode active material layer is not particularly limited, and any dry method commonly used in the art without a binder may be used.

[0059] The thickness of the first negative electrode active material layer 22 may be greater than the thickness of the first protective layers 23, 23a, and 23b. The thickness of the first negative electrode active material layer 22 may be 150% or more, 200% or more, 300% or more, or 500% or more of the thickness of the first protective layers 23, 23a, and 23b. When the first negative electrode active material layer 22 has a thickness in this range, the thickness of the first protective layers 23, 23a, and 23b is relatively reduced, and the energy density of the all-solid-state secondary battery may be further improved.

[0060] In the Raman spectrum of the negative electrode layer 20, the 1350 cm -1 The D band peak intensity (I D ) and 1580 cm originating from crystalline carbon -1 Nearby G-band peak intensity (I G ) peak intensity ratio (I D / I G) may be, for example, 20 or less, 15 or less, 10 or less, 5 or less, 3 or less, 2 or less, 1 or less, 0.8 or less, or 0.5 or less.

[0061] In the Raman spectrum of the negative electrode layer 20, the 1350 cm -1 The D band peak intensity (I D ) and 1580 cm originating from crystalline carbon -1 Nearby G-band peak intensity (I G ) peak intensity ratio (I D / I G ) may be, for example, greater than 0, greater than or equal to 0.01, greater than or equal to 0.05, greater than or equal to 0.1, greater than or equal to 0.3, greater than or equal to 0.5, or greater than or equal to 1.

[0062] In the Raman spectrum of the negative electrode layer 20, the 1350 cm -1 The D band peak intensity (I D ) and 1580 cm originating from crystalline carbon -1 The ratio of the G-band peak intensity (IG) to the peak intensity of the neighboring G-band peak (I D / I G ) is, for example, more than 0 and not more than 20, more than 0 and not more than 15, more than 0 and not more than 10, 0.01 to 10, 0.01 to 5, 0.1 to 5, 0.1 to 3, or 0.1 to 1. In the Raman spectrum of the negative electrode layer 20, the 1350 cm -1 The D band peak intensity (I D ) and 1580 cm originating from crystalline carbon -1 Nearby G-band peak intensity (I G ) peak intensity ratio (I D / I G ) is, for example, 0.1 to 10, 0.5 to 5, 1 to 3, or 1 to 2. In the Raman spectrum of the negative electrode layer 20, the 1350 cm -1 The D band peak intensity (I D ) and 1580 cm originating from crystalline carbon -1 Nearby G-band peak intensity (I G ) peak intensity ratio (I D / I G) is, for example, 0.5 to 10, 1 to 5, 2 to 5, or 3 to 5. The Raman spectrum relates to the first anode active material layer 22 and the first protective layer 23 of the anode layer 20. When the anode layer 20 has a peak intensity ratio in such a range, deterioration of the anode current collector 21 due to the solid electrolyte can be more effectively prevented. If the intensity ratio of the anode layer 20 is excessively increased, it becomes difficult to effectively prevent deterioration of the anode current collector 21 due to the solid electrolyte. The anode layer 20 including the nickel anode current collector 21 has a relatively lower intensity ratio than the anode layer 20 including the copper anode current collector 21.

[0063] The porosity obtained using a nitrogen gas adsorption method (multi-point BET) for the negative electrode layer 20 is, for example, 30% or less, 20% or less, 15% or less, 10% or less, 5% or less, 3% or less, 2% or less, 1% or less, 0.8% or less, or 0.5% or less.

[0064] The porosity obtained by using a nitrogen gas adsorption method (multi-point BET) for the negative electrode layer 20 is, for example, greater than 0%, 0.1% or more, or 0.5% or more.

[0065] The porosity obtained by using a nitrogen gas adsorption method (multi-point BET) on the anode layer 20 may be, for example, more than 0% and less than 30%, more than 0% and less than 20%, 0.01 to 10%, 0.1 to 5%, 0.5 to 5%, or 1 to 5%. The porosity obtained by using a nitrogen gas adsorption method (multi-point BET) on the anode layer 20 may be, for example, 0.1 to 20%, 1 to 10%, or 5 to 10%. The porosity obtained by using a nitrogen gas adsorption method (multi-point BET) on the anode layer 20 may be, for example, 1 to 20%, 5 to 20%, or 10 to 20%. When the anode layer 20 has a porosity within this range, deterioration of the anode current collector 21 due to the solid electrolyte can be more effectively prevented. If the porosity of the anode layer 20 is excessively high, it is difficult to effectively prevent deterioration of the anode current collector 21 due to the solid electrolyte.

[0066] [Negative electrode layer: 1st protective layer] 1 to 5, the negative electrode layer 20 includes a negative electrode current collector 21; a first negative electrode active material layer 22; and first protective layers 23, 23a, and 23b disposed between the negative electrode current collector 21 and the first negative electrode active material layer 22.

[0067] The first protective layers 23, 23a, and 23b are, for example, conductive coating layers containing a carbon-based material. Using the first protective layers 23, 23a, and 23b as conductive coating layers can suppress an increase in the internal resistance of the all-solid-state secondary battery, despite the addition of the first protective layers 23, 23a, and 23b. The first protective layers 23a, 23a, and 23b include, for example, second carbon-based nanostructures. Carbon-based nanostructures are structures having nano-sized dimensions and made of carbon-based materials. The carbon-based nanostructures can include, for example, one-dimensional carbon-based nanostructures, two-dimensional carbon-based nanostructures, three-dimensional carbon-based nanostructures, or combinations thereof. The second carbon-based nanostructures can include, for example, two-dimensional carbon-based nanostructures. The second carbon-based nanostructures can include, for example, graphene, graphene oxide (GO), reduced graphene oxide (rGO), or combinations thereof. The second carbon-based nanostructure may be selected from the first carbon-based nanostructures described above. The second carbon-based nanostructure may be doped with a dopant. The second carbon-based nanostructure doped with a dopant may be selected from the first carbon-based nanostructure doped with a dopant.

[0068] The first protective layers 23, 23a, and 23b may include, for example, second carbon-based nanostructures aligned in a certain direction on the surface of the negative electrode current collector 21. The second carbon-based nanostructures may include, for example, graphene. The first protective layers 23, 23a, and 23b may include graphene aligned in a certain direction on the surface of the negative electrode current collector 21.

[0069] The first protective layers 23, 23a, and 23b may include, for example, second carbon-based nanostructures aligned in a direction parallel to the surface of the negative electrode current collector 21. The second carbon-based nanostructures may be aligned in a direction parallel to the surface of the negative electrode current collector 21. The first protective layers 23, 23a, and 23b may include, for example, graphene. The first protective layers 23, 23a, and 23b may include graphene aligned in a direction parallel to the surface of the negative electrode current collector 21. The graphene may be aligned at an angle of, for example, −30° to 30°, −20° to 20°, −10° to 10°, or −5° to 5° with respect to the surface of the negative electrode current collector 21. By aligning the second carbon-based nanostructures in the first protective layers 23, 23a, and 23b in a direction parallel to the surface of the negative electrode current collector 21, contact between the solid electrolyte and the negative electrode current collector 21 may be more effectively suppressed.

[0070] The first protective layers 23, 23a, and 23b may include, for example, second carbon-based nanostructures aligned in a direction protruding from the surface of the negative electrode current collector 21. The second carbon-based nanostructures may be aligned in a direction protruding from the surface of the negative electrode current collector 21. The first protective layers 23, 23a, and 23b may include, for example, graphene. The first protective layers 23, 23a, and 23b may include graphene aligned in a direction protruding from the surface of the negative electrode current collector 21. The second carbon-based nanostructures may be aligned at an angle of 45° to 135°, 50° to 130°, 60° to 120°, 70° to 110°, or 80° to 100° relative to the surface of the negative electrode current collector 21. The second carbon-based nanostructures may be aligned, for example, perpendicular to the surface of the negative electrode current collector 21. Since the second carbon-based nanostructures in the first protective layers 23, 23a, and 23b are aligned in a direction protruding from the surface of the negative electrode current collector 21, electron transfer may be more easily performed between the first negative electrode active material layer 22 and the negative electrode current collector 21. As a result, an increase in the internal resistance of the all-solid-state secondary battery 1 may be more effectively suppressed.

[0071] The first protective layers 23, 23a, and 23b have a structure in which second carbon-based nanostructures are stacked along the thickness direction of the first protective layers 23, 23a, and 23b. A plurality of second carbon-based nanostructures may be stacked along the thickness direction of the first protective layers 23, 23a, and 23b within the first protective layers 23, 23a, and 23b. The first protective layers 23, 23a, and 23b may include, for example, a plurality of second carbon-based nanostructure layers stacked along the thickness direction of the first protective layers 23, 23a, and 23b. As the second carbon-based nanostructures are stacked along the thickness direction of the negative electrode current collector 21 within the first protective layers 23, 23a, and 23b, the structural density and structural stability of the first protective layers 23, 23a, and 23b may be further improved. The second carbon-based nanostructures may be stacked in the first protective layer 23, 23a, 23b to a thickness of, for example, 2000 layers or less, 1500 layers or less, 1000 layers or less, 500 layers or less, 100 layers or less, 70 layers or less, 50 layers or less, or 30 layers or less. The second carbon-based nanostructures may be stacked in the first protective layer 23, 23a, 23b to a thickness of, for example, 1 to 100 layers, 5 to 70 layers, 10 to 50 layers, or 20 to 30 layers. The second carbon-based nanostructures may be stacked in the first protective layer 23, 23a, 23b to a thickness of, for example, 1 to 2000 layers, 10 to 1000 layers, 100 to 1000 layers, 100 to 500 layers, or 100 to 300 layers. The second carbon-based nanostructures may be stacked in the first protective layers 23, 23a, 23b in a number of layers, for example, 1 to 2000, 10 to 2000, 100 to 2000, 500 to 2000, or 1000 to 2000. When the second carbon-based nanostructures have a number of layers in such a range, the structural stability of the first protective layers 23, 23a, 23b may be further improved.

[0072] The first protective layers 23, 23a, and 23b may be disposed directly on one surface of the negative electrode current collector 21. The first protective layers 23, 23a, and 23b are also inert to solid electrolytes, particularly sulfide-based solid electrolytes. By disposing the first protective layers 23, 23a, and 23b directly on one surface of the negative electrode current collector 21, contact between the negative electrode current collector 21 and the sulfide-based solid electrolyte is blocked, thereby more effectively preventing deterioration of the negative electrode current collector 21, such as corrosion of the negative electrode current collector 21.

[0073] The first protective layers 23, 23a, and 23b may be disposed, for example, on one surface of the negative electrode current collector 21 facing the solid electrolyte layer. The first protective layers 23, 23a, and 23b may also be disposed on the other surface of the negative electrode current collector 21 facing the one surface of the negative electrode current collector 21, or on a side surface of the negative electrode current collector 21 between the one surface and the other surface. By covering part or all of the negative electrode current collector 21 with the first protective layers 23, 23a, and 23b, deterioration due to the sulfide-based solid electrolyte can be more effectively prevented. Therefore, the life characteristics of the all-solid-state secondary battery 1 including the first protective layers 23, 23a, and 23b can be improved.

[0074] The thickness of the first protective layers 23, 23a, 23b is, for example, 5 μm or less, 3 μm or less, 2 μm or less, 1.5 μm or less, 1 μm or less, 500 nm or less, 300 nm or less, or 100 nm or less. The thickness of the first protective layers 23, 23a, 23b is, for example, the thickness of a single graphene layer or more, 1 nm or more, 10 nm or more, 20 nm or more, 50 nm, or 100 nm or more. The thickness of the first protective layers 23, 23a, 23b is, for example, the thickness of a single graphene layer to 2 μm, 10 nm to 1.5 μm, 50 nm to 1 μm, 100 nm to 900 nm, 200 nm to 800 nm, or 300 nm to 700 nm. The thickness of the first protective layers 23, 23a, and 23b may be, for example, the thickness of a graphene single layer up to 2 μm, 1 nm to 1.5 μm, 5 nm to 1 μm, 10 nm to 500 nm, 20 nm to 300 nm, or 20 nm to 100 nm. If the first protective layers 23, 23a, and 23b are excessively thick, the internal resistance of the all-solid-state secondary battery may increase, resulting in a decrease in energy density. If the first protective layers 23, 23a, and 23b are excessively thin, it may be difficult to effectively prevent side reactions between the negative electrode current collector 21 and the solid electrolyte.

[0075] The first protective layers 23, 23a, and 23b are binder-free. The first protective layers 23, 23a, and 23b are formed by a dry method, and therefore do not contain a binder. Because the first protective layers 23, 23a, and 23b do not contain a binder, the electronic conductivity of the first protective layers 23, 23a, and 23b may be improved, and the internal resistance may be reduced. Therefore, the cycle characteristics, such as the high rate characteristics, of the all-solid-state secondary battery 1 including such first protective layers 23, 23a, and 23b may be improved. The first protective layers 23, 23a, and 23b may be manufactured by a dry method such as CVD or PVD. The dry method used to manufacture the first protective layers 23, 23a, and 23b is not particularly limited, and any dry method commonly used in the art without a binder may be used. The first protective layers 23, 23a, 23b are made of, for example, the second carbon-based nanostructure and do not contain a binder.The first protective layers 23, 23a, 23b are made of, for example, graphene and do not contain a binder.

[0076] [Negative electrode layer: negative electrode current collector] The negative electrode current collector 21 is made of a material that does not react with lithium, i.e., does not form any alloy or compound. Materials constituting the negative electrode current collector 21 include, but are not limited to, copper (Cu), indium (In), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), and chromium (Cr). Any material usable as an electrode current collector in the art can be used. The negative electrode current collector 21 can be made of one of the above-mentioned metals, an alloy of two or more metals, or a coating material. The negative electrode current collector 21 is, for example, in the form of a plate or foil.

[0077] Although not shown in the drawings, the negative electrode current collector 21 may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may also include, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. When the base film includes a thermoplastic polymer, the base film melts in the event of a short circuit, thereby suppressing a sudden increase in current. The base film may also be, for example, an insulator. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. In particular, the metal layer may include, for example, copper (Cu), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal layer may act as an electrochemical fuse, breaking in the event of an overcurrent and preventing a short circuit. The limiting current and maximum current may be adjusted by adjusting the thickness of the metal layer. The metal layer may be electrodeposited or vapor-deposited on the base film. A thinner metal layer reduces the limiting current and / or maximum current of the negative electrode current collector 21, thereby improving the stability of the lithium battery during a short circuit. A lead tab may be added to the metal layer for external connection. The lead tab may be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, or the like. During welding, the base film and / or metal layer melt, electrically connecting the metal layer to the lead tab. To further strengthen the welding between the metal layer and the lead tab, a metal chip may be added between the metal layer and the lead tab. The metal chip may be a thin piece of the same material as the metal of the metal layer. The metal chip may be, for example, a metal foil, a metal mesh, or a copper foil or a nickel foil.After placing a metal piece on the metal layer, the lead tab can be welded to the metal piece / metal layer laminate or the metal piece / metal layer / base film laminate. During welding, the base film, metal layer, and / or metal piece melt, electrically connecting the metal layer or the metal layer / metal piece laminate to the lead tab. A metal piece and / or lead tab can be added to a portion of the metal layer. The thickness of the base film can be, for example, 1 to 50 μm, 1.5 to 50 μm, 1.5 to 40 μm, or 1 to 30 μm. The weight of the electrode assembly can be further effectively reduced by using a base film having a thickness within this range. The melting point of the base film can be, for example, 100 to 300°C, 100 to 250°C, or 100 to 200°C. By using a base film having a melting point within this range, the base film can be melted during the lead tab welding process and easily bonded to the lead tab. To improve the adhesion between the base film and the metal layer, a surface treatment such as a corona treatment may be performed on the base film. The thickness of the metal layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to 1 μm. When the metal layer has a thickness within this range, the stability of the electrode assembly may be ensured while maintaining conductivity. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. When the metal piece has a thickness within this range, the connection between the metal layer and the lead tab may be more easily achieved. When the negative electrode current collector 21 has such a structure, the weight of the negative electrode may be reduced, thereby improving the energy density of the all-solid-state secondary battery.

[0078] The negative electrode current collector 21 may further include, for example, a thin film containing an element that forms an alloy with lithium on the negative electrode current collector 21. The thin film is disposed between the negative electrode current collector 21 and the first negative electrode active material layer 22. The thin film contains, for example, an element that forms an alloy with lithium. The element that forms an alloy with lithium may be, but is not limited to, gold, silver, zinc, tin, indium, silicon, aluminum, bismuth, etc. Any element known in the art that forms an alloy with lithium may be used. The thin film may be composed of one of these metals or an alloy of various metals. By disposing the thin film on the negative electrode current collector 21, for example, the deposition morphology of the second negative electrode active material layer deposited between the thin film and the first negative electrode active material layer 22 may be further flattened, thereby further improving the cycle characteristics of the all-solid-state secondary battery 1. The thin film can be disposed, for example, between the first protective layer 23 and the first negative electrode active material layer 22 or between the first protective layer 23 and the negative electrode current collector 21.

[0079] The thickness of the thin film is, for example, 1 nm to 800 nm, 10 nm to 500 nm, or 50 nm to 100 nm. If the thickness of the thin film is less than 1 nm, it is difficult for the thin film to exhibit its function. If the thin film is excessively thick, the thin film itself may irreversibly absorb lithium, thereby reducing the amount of lithium deposited in the negative electrode layer 20. As a result, the effective energy density of the all-solid-state secondary battery 1 may decrease, and the cycle characteristics of the all-solid-state secondary battery 1 may deteriorate. The thin film is disposed on the negative electrode current collector 21 by, for example, a vacuum deposition method, a sputtering method, a plating method, or the like, but is not necessarily limited to such methods, and any method for forming a thin film in the art may be used.

[0080] [Negative electrode layer: second negative electrode active material layer] Although not shown in the drawings, the all-solid-state secondary battery 1 further includes a second anode active material layer disposed between the solid electrolyte layer 30 and the anode current collector 21 during charging. The second anode active material layer may be disposed, for example, between the first anode active material layer 22 and the first protective layers 23, 23a, and 23b, and between the first anode active material layer 22 and the solid electrolyte layer 30. The all-solid-state secondary battery 1 further includes a second anode active material layer disposed between the first anode active material layer 22 and the first protective layers 23, 23a, and 23b. The all-solid-state secondary battery 1 further includes a second anode active material layer disposed between the first anode active material layer 22 and the solid electrolyte layer 30. The second anode active material layer is deposited, for example, between the first anode active material layer 22 and the first protective layers 23, 23a, and 23b during charging of the all-solid-state secondary battery 1.

[0081] The second negative electrode active material layer is a metal layer containing lithium or a lithium alloy. The metal layer contains lithium or a lithium alloy. Therefore, since the second negative electrode active material layer is a metal layer containing lithium, it acts, for example, as a lithium reservoir. Examples of lithium alloys include, but are not limited to, Li-Al alloys, Li-Sn alloys, Li-In alloys, Li-Ag alloys, Li-Au alloys, Li-Zn alloys, Li-Ge alloys, and Li-Si alloys. Any lithium alloy known in the art can be used. The second negative electrode active material layer may be composed of one of these alloys or lithium, or may be composed of various alloys. The second negative electrode active material layer may be, for example, a plated layer.

[0082] The thickness of the second negative electrode active material layer is not particularly limited, and may be, for example, 1 μm to 200 μm, 1 μm to 150 μm, 1 μm to 100 μm, or 1 μm to 50 μm. If the thickness of the second negative electrode active material layer is too thin, it may be difficult for the second negative electrode active material layer to function as a lithium reservoir. If the thickness of the second negative electrode active material layer is too thick, the mass and volume of the all-solid-state secondary battery 1 may increase, and the cycle characteristics may actually deteriorate. The second negative electrode active material layer may be, for example, a metal foil having a thickness within this range.

[0083] In the all-solid-state secondary battery 1, the second negative electrode active material layer is disposed between the negative electrode current collector 21 and the solid electrolyte layer 30 before assembling the all-solid-state secondary battery 1, for example, or is deposited between the negative electrode current collector 21 and the solid electrolyte layer 30 by charging after assembling the all-solid-state secondary battery 1. In an all-solid-state secondary battery 1 in which the second negative electrode active material layer is disposed between the negative electrode current collector 21 and the solid electrolyte layer 30 before assembling the all-solid-state secondary battery 1, the second negative electrode active material layer is a metal layer containing lithium and therefore acts as a lithium reservoir. For example, a lithium foil is disposed between the negative electrode current collector 21 and the solid electrolyte layer 30 before assembling the all-solid-state secondary battery 1. This further improves the cycle characteristics of the all-solid-state secondary battery 1 including the second negative electrode active material layer. In an all-solid-state secondary battery 1 in which the second negative electrode active material layer is deposited by charging, the second negative electrode active material layer is not included during assembly of the all-solid-state secondary battery 1, and therefore the energy density of the all-solid-state secondary battery 1 is increased. For example, when charging the all-solid-state secondary battery 1, the first anode active material layer 22 is charged beyond its charge capacity. That is, the first anode active material layer 22 is overcharged. At the beginning of charging, lithium is absorbed into the first anode active material layer 22. The anode active material contained in the first anode active material layer 22 forms an alloy or compound with lithium ions transferred from the cathode layer 10. When the first anode active material layer 22 is charged beyond its capacity, lithium is deposited on the front and / or back surfaces of the first anode active material layer 22, i.e., between the first anode active material layer 22 and the first protective layers 23, 23a, and 23b, and / or between the first anode active material layer 22 and the solid electrolyte layer 30, and the deposited lithium forms a metal layer corresponding to the second anode active material layer. The second anode active material layer is a metal layer mainly composed of lithium (i.e., metallic lithium). Such a result can be obtained, for example, by including a substance that forms an alloy or compound with lithium in the anode active material contained in the first anode active material layer 22. During discharge, lithium in the first anode active material layer 22 and the second anode active material layer, i.e., the metal layer, is ionized and moves toward the cathode layer 10. Therefore, lithium can be used as the anode active material in the all-solid-state secondary battery 1.Furthermore, when the first anode active material layer 22 is disposed between the solid electrolyte layer 30 and the second anode active material layer, the first anode active material layer 22 covers the second anode active material layer, thereby serving as a protective layer for the second anode active material layer, i.e., the metal layer, and also serving to suppress the deposition and growth of lithium dendrites. This suppresses short circuits and capacity reduction in the all-solid-state secondary battery 1, thereby improving the cycle characteristics of the all-solid-state secondary battery 1. Furthermore, when the second anode active material layer is disposed by charging after assembly of the all-solid-state secondary battery 1, the region between the anode current collector 21 and the solid electrolyte layer 30 is a Li-free region that does not contain lithium (Li), for example, in the initial state or after discharge of the all-solid-state secondary battery.

[0084] [Solid electrolyte layer] [Solid electrolyte layer: sulfide solid electrolyte] 1 to 5, the solid electrolyte layer 30 is disposed between the positive electrode layer 10 and the negative electrode layer 20. The solid electrolyte layer 30 includes a sulfide-based solid electrolyte.

[0085] Examples of sulfide-based solid electrolytes contained in the solid electrolyte layer 30 include Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, and Li2S-P2S5-Z m S n (m and n are positive numbers, Z is one of Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (p and q are positive numbers, M is one of P, Si, Ge, B, Al, and GaIn), Li3PS4, Li7P3S 11 ,Li 7-x PS 6-x Cl x (0≦x≦2), Li 7-x PS 6-x Br x (0≦x≦2), and Li 7-x PS6-x I x (0≦x≦2). The sulfide-based solid electrolyte is prepared by processing starting materials such as Li2S and P2S5 by melt quenching or mechanical milling. After such processing, heat treatment can be performed. The solid electrolyte can be amorphous, crystalline, or a mixture thereof. The solid electrolyte may contain, for example, sulfur (S), phosphorus (P), and lithium (Li) as constituent elements from among the sulfide-based solid electrolyte materials described above. For example, the solid electrolyte can be a material containing Li2S-P2S5. When a sulfide-based solid electrolyte material containing Li2S-P2S5 is used to form the solid electrolyte, the molar ratio of Li2S to P2S5 is, for example, in the range of about Li2S:P2S5=50:50 to 90:10. The sulfide-based solid electrolyte includes, for example, an argyrodite-type solid electrolyte represented by the following chemical formula A: <Case A> Li + 12-n-x A n+ X 2- 6-x Y - x In the formula, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb, or Ta, X is S, Se, or Te, and Y is Cl, Br, I, F, CN, OCN, SCN, or N3, where 1≦n≦5, 0≦x≦2. The sulfide-based solid electrolyte is, for example, Li 7-x PS 6-x Cl x (0≦x≦2), Li 7-x PS 6-x Br x (0≦x≦2), and Li 7-x PS 6-x I x(0≦x≦2). The sulfide-based solid electrolyte may also be an argyrodite-type compound containing one or more selected from Li6PS5Cl, Li6PS5Br, and Li6PS5I. The density of the argyrodite-type solid electrolyte may be 1.5 to 2.0 g / cc. When the argyrodite-type solid electrolyte has a density of 1.5 g / cc or more, the internal resistance of the all-solid-state secondary battery is reduced, and penetration of the solid electrolyte layer by Li can be effectively suppressed.

[0086] The elastic modulus of the sulfide-based solid electrolyte is, for example, 40 GPa or less, 5 GPa to 40 GPa, 10 GPa to 40 GPa, or 15 GPa to 30 GPa, for example.

[0087] The sulfide-based solid electrolyte particles contained in the solid electrolyte layer 30 have an average particle size of, for example, 1 μm to 50 μm, 3 μm to 30 μm, or 3 μm to 20 μm. When the sulfide-based solid electrolyte particles have an average particle size in such a range, the cycle characteristics of the all-solid-state secondary battery can be further improved.

[0088] [Solid electrolyte layer: binder] The solid electrolyte layer 30 may further include, for example, a binder. Examples of the binder included in the solid electrolyte layer 30 include, but are not limited to, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, and polyethylene. Any binder available in the art may be used. The binder of the solid electrolyte layer 30 may be selected from the binders included in the positive electrode active material layer 12. The binder may be omitted.

[0089] The binder contained in the solid electrolyte layer may include, for example, a conductive binder and / or a non-conductive binder. The conductive binder may be, for example, an ionically conductive binder and / or an electronically conductive binder. A binder having both ion conductivity and electronic conductivity also belongs to both ionically conductive binders and electronically conductive binders. Any conductive binder used in the art may be used as the conductive binder.

[0090] The binder contained in the solid electrolyte layer 30 may include, for example, a first binder. The first binder may be, for example, a dry binder. The dry binder may be, for example, a binder that is not impregnated, dissolved, or dispersed in a solvent. The dry binder may be, for example, a binder that contains a solvent or is not in contact with a solvent.

[0091] The first binder may be, for example, a fibrillated binder. The fibrillated binder serves as a fibrous matrix that supports and binds together the sulfide-based solid electrolyte particles and inorganic particles contained in the solid electrolyte layer. The fibrillated binder may be confirmed to have a fibrous shape, for example, in a scanning electron microscope image of the electrode cross section. The fibrillated binder may have an aspect ratio of, for example, 10 or more, 20 or more, 50 or more, or 100 or more. The first binder may be, for example, polytetrafluoroethylene (PTFE), polyvinylidene fluoride-hexapropylene (PVDF-HFP) copolymer, etc., but is not limited thereto, and any fibrillated binder used in the preparation of a dry composition may be used. The first binder may particularly include a fluorine-based binder. The fluorine-based binder may be, for example, polytetrafluoroethylene (PTFE). The aspect ratio of the fiberized binder, i.e., the ratio of the diameter to the length of the fiberized binder, can be determined, for example, from SEM images.

[0092] The binder included in the solid electrolyte layer 30 may further include, for example, a second binder. The second binder is, for example, a dry binder. The description of the dry binder is the same as that of the first binder.

[0093] The second binder may be, for example, a non-fibrillated binder. The non-fibrillated binder supports the sulfide-based solid electrolyte particles and inorganic particles contained in the solid electrolyte layer and serves as a binding site for binding them together. The non-fibrillated binder may be seen to be arranged in a particulate form, rather than a fibrous form, in a scanning electron microscope image of the electrode cross section. The non-fibrillated binder may have an aspect ratio of, for example, 5 or less, 3 or less, or 2 or less. The second binder may be, for example, polyvinylidene fluoride (PVDF), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, cellulose, polyvinylpyrrolidone, polyethylene, polypropylene, ethylene propylene diene polymer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, or a copolymer thereof, but is not limited thereto. Any binder used in the manufacture of dry electrodes may be used. The second binder may particularly include a fluorine-based binder, such as polyvinylidene fluoride (PVDF).

[0094] The content of the binder in the solid electrolyte layer 30 is, for example, 1 wt% to 10 wt%, 1 wt% to 5 wt%, or 1 wt% to 3 wt% based on the total weight of the solid electrolyte layer. When the solid electrolyte layer contains a binder in such a content range, the binding strength of the solid electrolyte layer is improved, and the all-solid-state secondary battery can maintain a high energy density.

[0095] The solid electrolyte layer 30 is, for example, a self-standing film. The solid electrolyte layer maintains its film form without a support. Therefore, the solid electrolyte layer may be formed as a separate, self-standing film and then disposed between the positive electrode layer and the negative electrode layer. The solid electrolyte layer may also be free of, for example, residual processing solvents. For example, since the solid electrolyte layer is manufactured using a dry process, it does not contain intentionally added processing solvents. For example, it does not contain residual processing solvents. Although trace amounts of unintentional solvents may remain in the solid electrolyte layer, such solvents are not intentionally added processing solvents. Therefore, the solid electrolyte layer is distinguished from a wet solid electrolyte layer manufactured by mixing sulfide-based solid electrolyte particles with a processing solvent and then drying to remove some or all of the processing solvent.

[0096] [Positive electrode layer] [Cathode layer: Cathode active material] 1 to 5, the positive electrode active material layer 12 includes, for example, a positive electrode active material and a solid electrolyte. The solid electrolyte included in the positive electrode active material layer 12 may be selected from the solid electrolytes included in the solid electrolyte layer 30. For details regarding the solid electrolyte, refer to the section on the solid electrolyte layer 30. The solid electrolyte may be omitted.

[0097] The positive electrode active material contained in the positive electrode active material layer 12 is a positive electrode active material that reversibly absorbs and desorbs lithium ions. Examples of the positive electrode active material include oxide-based positive electrode active materials, sulfide-based positive electrode active materials, or combinations thereof. Examples of the oxide-based positive electrode active material include lithium transition metal oxides, metal oxides, or combinations thereof. Examples of the lithium transition metal oxides include lithium cobalt oxide, lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese oxide, lithium manganate, lithium iron phosphate, or combinations thereof. Metal oxides include, for example, iron oxide, vanadium oxide, or a combination thereof.

[0098] Sulfide-based positive electrode active materials include, for example, nickel sulfide, copper sulfide, Li2S, Li2S-containing composites, or combinations thereof.

[0099] The oxide-based positive electrode active material can be, for example, one or more composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof. a A 1-b B' b D2 (wherein 0.90≦a≦1, and 0≦b≦0.5); Li a E 1-b B' b O 2-c D c(wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05); LiE 2-b B' b O 4-c D c (wherein 0≦b≦0.5 and 0≦c≦0.05); Li a Ni 1-b-c Co b B' c D α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, 0<α≦2); Li a Ni 1-b-c Co b B' c O 2-α F' α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, 0<α<2); Li a Ni 1-b-c Co b B' c O2 (wherein 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05); Li a Ni 1-b-c Mn b B' c D α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, 0<α≦2); Li a Ni 1-b-c Mn b B' c O 2-α F' α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, 0<α<2); Li a Ni 1-b-c Mn b B' c O2 (wherein 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05); Li a Ni b E c G d O2 (wherein 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, 0.001≦d≦0.1); Li a Ni b Co c Mnd G e O2 (wherein 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, 0.001≦e≦0.1); Li a NiG b O2 (wherein 0.90≦a≦1, 0.001≦b≦0.1); Li a CoG b O2 (wherein 0.90≦a≦1, 0.001≦b≦0.1); Li a MnG b O2 (wherein 0.90≦a≦1, 0.001≦b≦0.1); Li a Mn2G b O4 (wherein 0.90≦a≦1, 0.001≦b≦0.1); LiV2O5; LiI'O2; LiNiVO4; Li (3-f) J2(PO4)3(0≦f≦2);Li (3-f) It may include a compound represented by any one of the chemical formulas Fe2(PO4)3(0≦f≦2); LiFePO4.

[0100] In the chemical formula representing the above-mentioned compound, A is Ni, Co, Mn, or a combination thereof; B' is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F' is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I' is Cr, V, Fe, Sc, Y, or a combination thereof; and J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. Compounds having a coating layer added to the surface of the above-mentioned compound can also be used, or a mixture of the above-mentioned compound and a compound having a coating layer added can also be used. The coating layer applied to the surface of the above-mentioned compound includes a coating element compound such as an oxide, hydroxide, oxyhydroxide, oxycarbonate, or hydroxycarbonate of the coating element. The compound forming the coating layer may be amorphous or crystalline. The coating element contained in the coating layer may be Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The coating layer formation method is selected within a range that does not adversely affect the physical properties of the positive electrode active material. Examples of the coating method include spray coating and dipping. The specific coating method is well known to those skilled in the art, so a detailed description will be omitted.

[0101] The oxide-based positive electrode active material includes, for example, lithium transition metal oxides represented by the following chemical formulas 1 to 8: <C1> Li a Ni x Co y M z O 2-b A b In the above Chemical Formula 1, 1.0 ≤ a ≤ 1.2, 0 ≤ b ≤ 0.2, 0.8 ≤ x < 1, 0 ≤ y ≤ 0.3, 0 < z ≤ 0.3, and x + y + z = 1, M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, A is F, S, Cl, Br or a combination thereof, <Chemical formula 2> LiNi x Co y Mn z [[ID=!4]]O2 <Chemical formula 3> LiNi x Co y Al z O2 In the chemical formulas 2 to 3, 0.8 ≤ x ≤ 0.95, 0 ≤ y < 0.2, 0 < z ≤ 0.2 and x + y + z = 1, <Chemical formula 4> LiNi x Co y Mn z Al w O2 In the chemical formula 4, 0.8 ≤ x ≤ 0.95, 0 ≤ y ≤ 0.2, 0 < z ≤ 0.2, 0 < w ≤ 0.2, and x + y + z + w = 1, <Chemical formula 5> Li a Co x M y O 2-b A b In the chemical formula 5, 1.0 ≤ a ≤ 1.2, 0 ≤ b ≤ 0.2, 0.9 ≤ x ≤ 1, 0 ≤ y ≤ 0.1, and x + y = 1, M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, A is F, S, Cl, Br, or a combination thereof, <Chemical formula 6> Li a Ni x Mn y M’ z O 2-b A b In the chemical formula 6, 1.0 ≤ a ≤ 1.2, 0 ≤ b ≤ 0.2, 0 < x ≤ 0.3, 0.5 ≤ y < 1, 0 < z ≤ 0.3, and x + y + z = 1, M’ is cobalt (Co), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof, A is F, S, Cl, Br, or a combination thereof, <Chemical formula 7> Li a M1 x [[ID=3​​​​​​​​​​​​​​​​​​​​In the above Chemical Formula 8, 0.90≦a≦1.1 and 0.9≦z≦1.1; M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof.

[0102] The oxide-based positive electrode active material is also covered with a coating layer. Any known coating layer for a positive electrode active material of an all-solid-state secondary battery can be used as the coating layer. For example, the coating layer is Li2O-ZrO2 (LZO).

[0103] The sulfide-based positive electrode active material may include, for example, a LiS-containing composite, such as a composite of LiS and carbon, a composite of LiS and carbon and a solid electrolyte, a composite of LiS and a solid electrolyte, a composite of LiS and a metal carbide, a composite of LiS and carbon and a metal carbide, a composite of LiS and a metal nitride, a composite of LiS and carbon and a metal nitride, a composite of LiS and a metal, a composite of LiS and a metal and carbon, or a combination thereof.

[0104] The Li2S and carbon composite contains carbon. Carbon can be, for example, any carbon-containing material known in the art as a conductive material. The carbon can be, for example, crystalline carbon, amorphous carbon, or a combination thereof. The carbon can be, for example, a calcined product of a carbon precursor. The carbon can be, for example, a carbon nanostructure. The carbon nanostructure can be, for example, a one-dimensional carbon nanostructure, a two-dimensional carbon nanostructure, a three-dimensional carbon nanostructure, or a combination thereof. The carbon nanostructure can be, for example, a carbon nanotube, a carbon nanofiber, a carbon nanobelt, a carbon nanorod, graphene, graphene oxide (GO), reduced graphene oxide (rGO), graphene balls (GB), or a combination thereof. The carbon can be, for example, porous carbon or non-porous carbon. The porous carbon can include, for example, periodic, regular two-dimensional or three-dimensional pores. Porous carbon can be, for example, carbon black such as Ketjen Black, acetylene black, denka black, thermal black, or channel black; graphite; activated carbon; or a combination thereof. The carbon can be in the form of, for example, particles, sheets, or flakes, but is not limited thereto. Any carbon usable in the art can be used. The LiS / carbon composite can be produced by, for example, a dry process, a wet process, or a combination thereof, but is not limited thereto. Furthermore, the LiS / carbon composite can be produced by, for example, milling, heat treatment, vapor deposition, or the like, but is not necessarily limited thereto. Any method usable in the art can be used.

[0105] The composite of Li2S, carbon, and a solid electrolyte includes carbon and a solid electrolyte. For carbon, see the composite of Li2S and carbon described above. The solid electrolyte can be, for example, any ion-conductive material available in the art. The solid electrolyte can be, for example, an inorganic solid electrolyte. The solid electrolyte can be, for example, a crystalline solid electrolyte, an amorphous solid electrolyte, or a combination thereof. The solid electrolyte can be, for example, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, a lithium salt compound, or a combination thereof. The sulfide-based solid electrolyte can contain, for example, Li, S, and P, and can optionally further contain a halogen element. The sulfide-based solid electrolyte can be selected from sulfide-based solid electrolytes used in the solid electrolyte layer. The sulfide-based solid electrolyte can have a specific surface area of, for example, 1×10 at room temperature. -5 Examples of sulfide-based solid electrolytes include Li3PO4-Li2SO4, Li2S-P2S5, Li2S-P2S5-LiX (X is a halogen element), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, and Li2S-P2S5-Z. m S n (m and n are positive numbers, Z is one of Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (p and q are positive numbers, M is one of P, Si, Ge, B, Al, and GaIn), Li 7-x PS 6-x Cl x (0≦x≦2), Li 7-x PS 6-x Br x (0≦x≦2), and Li 7-x PS 6-x I x (0≦x≦2). The oxide-based solid electrolyte may include, for example, Li, O, and a transition metal element, and may further include other elements selectively. The oxide-based solid electrolyte may have a specific surface area of ​​1×10-5 The solid electrolyte may also be a solid electrolyte having an ionic conductivity of 1000 S / cm or more. The oxide-based solid electrolyte may be selected from oxide-based solid electrolytes used in the solid electrolyte layer. The lithium salt compound may be, for example, an inorganic compound. The solid electrolyte may include, for example, a lithium salt compound, which does not include, for example, a sulfur (S) atom. The lithium salt compound may also be, for example, a binary compound consisting of lithium and one element selected from Groups 13 to 17 of the periodic table. The binary compound may include, for example, one or more selected from LiF, LiCl, LiBr, LiI, LiH, Li2S, Li2O, Li2Se, Li2Te, Li3N, Li3P, Li3As, Li3Sb, LiI3, and LiB3. The lithium salt compound may also be, for example, a ternary compound consisting of lithium and two elements selected from Groups 13 to 17 of the periodic table. Ternary compounds include, for example, one or more selected from Li3OCl, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiNO3, Li2CO3, LiBH4, Li2SO4, Li3BO3, Li3PO4, Li4NCl, Li5NCl2, and Li3BN2. The lithium salt compound is, in particular, one or more lithium halide compounds selected from LiF, LiCl, LiBr, and LiI. The solid electrolyte can also be, for example, a mixture of a sulfide-based solid electrolyte and a lithium salt compound. For example, it can be a mixture of Li3PO4-Li2SO4 and a binary lithium salt compound, or a mixture of Li3PO4-Li2SO4 and a ternary lithium salt compound.

[0106] The composite of Li2S and a solid electrolyte includes a solid electrolyte. The solid electrolyte refers to the solid electrolyte used in the composite of Li2S, carbon, and a solid electrolyte described above. The composite of Li2S and a solid electrolyte includes, for example, a composite of Li2S and one or more lithium salts selected from LiF, LiCl, LiBr, LiI, LiH, Li2S, Li2O, Li2Se, Li2Te, Li3N, Li3P, Li3As, Li3Sb, LiI3, and LiB3.

[0107] The composite of Li2S and metal carbide includes a metal carbide. The metal carbide is, for example, a two-dimensional metal carbide. The two-dimensional metal carbide is, for example, MXene. The two-dimensional metal carbide is, for example, M n+1 C n T x (M is a transition metal, T is an end group, T is O, OH and / or F, n=1, 2 or 3, x is the number of end groups). Two-dimensional metal carbides are, for example, Ti2CT x , (Ti 0.5 ,Nb 0.5 )2CT x , Nb2CT x , V2CT x , Ti3C2T x , (V 0.5 ,Cr 0.5 )3C2T x , Ti3CNT x , Ta4C3T x , Nb4C3T x or a combination thereof. The surface of the two-dimensional metal carbide is terminated with O, OH and / or F.

[0108] The composite of Li2S, carbon, and metal carbide includes carbon and metal carbide. For carbon, see the above-mentioned composite of Li2S and carbon. For metal carbide, see the above-mentioned composite of Li2S and metal carbide.

[0109] The composite of Li2S and metal nitride includes a metal nitride. The metal nitride is, for example, a two-dimensional metal nitride. The two-dimensional metal nitride is, for example, M n+1 N n T x (M is a transition metal, T is a terminal group, T is O, OH, and / or F, n=1, 2, or 3, and x is the number of terminal groups). The surface of the two-dimensional metal nitride is terminated with O, OH, and / or F.

[0110] The composite of Li2S, carbon, and metal nitride includes carbon and metal nitride. For carbon, refer to the composite of LiS and carbon described above. For metal nitride, refer to the composite of Li2S and metal nitride described above.

[0111] The shape of the positive electrode active material is, for example, a particle shape such as a perfect sphere or an oval sphere. The particle size of the positive electrode active material is not particularly limited and is within a range applicable to positive electrode active materials in conventional all-solid-state secondary batteries. The content of the positive electrode active material in the positive electrode layer 10 is also not particularly limited and is within a range applicable to positive electrode layers in conventional all-solid-state secondary batteries. The content of the positive electrode active material in the positive electrode active material layer 12 is, for example, 10 wt% to 99 wt%, 10 wt% to 90 wt%, 10 wt% to 80 wt%, 10 wt% to 70 wt%, or 10 wt% to 50 wt% of the total weight of the positive electrode active material layer 12.

[0112] [Positive electrode layer: solid electrolyte] The positive electrode active material layer 12 may further include, for example, a solid electrolyte. The positive electrode active material layer 12 may include an oxide-based solid electrolyte or a sulfide-based solid electrolyte.

[0113] The solid electrolyte contained in the positive electrode active material layer 12 is also a sulfide-based solid electrolyte. For details regarding the sulfide-based solid electrolyte, see the section on the solid electrolyte layer 30.

[0114] The solid electrolyte contained in the positive electrode active material layer 12 is also an oxide-based solid electrolyte. The oxide-based solid electrolyte is, for example, Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2,0≦y<3),BaTiO3,Pb(Zr,Ti)O3(PZT),Pb 1-x La x Zr 1-y Ti y O3(PLZT)(0≦x<1,0≦y<1),PB(Mg3Nb 2 / 3)O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2,0<y<3)、Li x Al y Ti z (PO4)3(0 <x<2,0<y<1,0<z<3)、Li 1+x+y (Al,Ga) x (Ti,Ge) 2-x Si y P 3-y O 12 (0≦x≦1,0≦y≦1), Li x La y TiO3(0 <x<2,0<y<3)、Li2O、LiOH、Li2CO3、LiAlO2、Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2、Li 3+x La3M2O 12 (M=Te, Nb, or Zr; x is an integer between 1 and 10). The solid electrolyte is produced by a sintering method or the like. For example, an oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10, 0≦a<2) is a garnet-type solid electrolyte selected from the group consisting of:

[0115] The solid electrolyte contained in the positive electrode active material layer 12 has a smaller diameter than the solid electrolyte contained in the solid electrolyte layer 30. For example, the particle diameter of the solid electrolyte contained in the positive electrode active material layer 12 is 90% or less, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, or even 20% or less of the particle diameter of the solid electrolyte contained in the solid electrolyte layer 30. The particle diameter of the solid electrolyte is, for example, the median particle diameter (D50). The median particle diameter (D50) is the size of particles corresponding to a 50% cumulative volume calculated from the particle side having a small particle size in a particle size distribution measured by, for example, laser diffraction.

[0116] [Positive electrode layer: binder] The positive electrode active material layer 12 may contain a binder. Examples of the binder include, but are not limited to, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, and polyethylene, and any binder that can be used in the art may be used.

[0117] [Positive electrode layer: conductive material] The positive electrode active material layer 12 may include a conductive material, such as, but not limited to, graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or metal powder, and any material known in the art may be used as a conductive material.

[0118] [Positive electrode layer: Other additives] The positive electrode active material layer 12 may further contain additives such as a filler, a coating agent, a dispersant, and an ion-conductive auxiliary agent in addition to the above-mentioned positive electrode active material, solid electrolyte, binder, and conductive material.

[0119] The filler, coating agent, dispersant, ion-conducting auxiliary agent, and the like contained in the positive electrode active material layer 12 may be any known material generally used in electrodes of all-solid-state secondary batteries.

[0120] [Positive electrode layer: Positive electrode current collector] The positive electrode current collector 11 is, for example, a plate or foil made of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector 11 can be omitted. The thickness of the positive electrode current collector 11 is, for example, 1 μm to 100 μm, 1 μm to 50 μm, 5 μm to 25 μm, or 10 μm to 20 μm.

[0121] The positive electrode current collector 11 may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. Such a structure of the positive electrode current collector 11 can reduce the weight of the electrode, thereby improving the energy density of the all-solid-state secondary battery.

[0122] [Positive electrode layer: inactive material] 3 to 5, the positive electrode layer 10 includes a positive electrode current collector 11, a positive electrode active material layer 12 disposed on one side of the positive electrode current collector, and further includes inactive members 40, 40a, and 40b disposed on one side of the positive electrode layer 10.

[0123] The inclusion of the inactive member 40 prevents cracks in the solid electrolyte layer 30 during the manufacture of the all solid state secondary battery 1 and / or during charge and discharge, resulting in improved cycle characteristics of the all solid state secondary battery 1. In an all solid state secondary battery 1 that does not include the inactive member 40, uneven pressure is applied to the solid electrolyte layer 30 that contacts the positive electrode 10 during the manufacture of the all solid state secondary battery 1 and / or during charge and discharge, causing cracks in the solid electrolyte layer 30, which increases the likelihood of short circuits occurring due to the growth of lithium metal.

[0124] The inactive member 40 is disposed along the side surface of the positive electrode layer 10, surrounding the positive electrode layer. For example, the inactive member 40 surrounds part or all of the side surface of the positive electrode layer 10 and contacts the solid electrolyte layer 30. By surrounding the side surface of the positive electrode layer 10 and contacting the solid electrolyte layer 30, the inactive member 40 can effectively prevent cracks in the solid electrolyte layer 30, which are not in contact with the positive electrode 10, from occurring due to a pressure difference during a pressing process. The inactive member 40 surrounds the side surface of the positive electrode 10 and separates it from the anode 20, specifically, the first anode active material layer 22. The inactive member 40 surrounds the side surface of the positive electrode layer 10, contacts the solid electrolyte layer 30, and separates it from the anode 20. This reduces the possibility of a short circuit occurring due to physical contact between the positive electrode layer 10 and the first anode active material layer 22, or due to lithium overcharging, etc. 3, an inactive member 40 is disposed on one side of the positive electrode active material layer 12 and also on one side of the positive electrode current collector 11, thereby more effectively preventing the occurrence of a short circuit due to contact between the positive electrode current collector 11 and the negative electrode 20. Meanwhile, referring to FIG. 4, the inactive member 40 is disposed on one side of the positive electrode active material layer 12 and is disposed between the solid electrolyte layer 30 and the positive electrode current collector 11 facing the solid electrolyte layer 30. The inactive member 40 is not disposed on one side of the positive electrode current collector 11. The inactive member 40 is disposed between the positive electrode current collector 11 and the solid electrolyte layer 30, thereby effectively preventing a short circuit due to contact between the positive electrode current collector 11 and the negative electrode 20.

[0125] Although not shown in the drawings, some or all of the inactive members 40, 40a, 40b may be disposed spaced apart from the side surfaces of the positive electrode layer 10. By disposing some or all of the inactive members 40, 40a, 40b spaced apart from the side surfaces of the positive electrode layer 10, the manufacturing process of the all-solid-state secondary battery 1 may be further facilitated and the manufacturing speed of the all-solid-state secondary battery 1 may be increased. By disposing some or all of the inactive members 40, 40a, 40b spaced apart from the side surfaces of the positive electrode layer 10, volume changes in the lateral direction of the positive electrode layer 10 during charge and discharge may be more effectively accommodated, thereby further improving the life characteristics of the all-solid-state secondary battery 1. The distances between the inactive members 40, 40a, 40b and the side surfaces of the positive electrode layer 10 may be, independently of one another, for example, 0.1 μm to 10 mm, 1 μm to 1 mm, 1 μm to 500 μm, 1 μm to 100 μm, 1 μm to 50 μm, or 1 μm to 10 μm.

[0126] The inactive member 40 may further include a positioning portion (not shown) configured to determine the position of the inactive member 40 on the solid electrolyte layer 30. When the inactive member 40 includes the positioning portion, it becomes easy to determine the position at which to place the inactive member 40 on the solid electrolyte layer 30. As a result, the manufacturing speed of the all-solid-state secondary battery 1 can be increased, and ease of manufacturing can be improved.

[0127] 3 and 4 , the inactive member 40 extends from one side surface of the positive electrode 10 to an end portion of the solid electrolyte layer 30. The inactive member 40 extends to the end portion of the solid electrolyte layer 30, thereby suppressing cracks from occurring at the end portion of the solid electrolyte layer 30. The end portion of the solid electrolyte layer 30 is the outermost portion that contacts the side surface of the solid electrolyte layer 30. The inactive member 40 extends to the outermost portion that contacts the side surface of the solid electrolyte layer 30. The inactive member 40 is separated from the anode layer 20, specifically, the first anode active material layer 22. The inactive member 40 extends to the end portion of the solid electrolyte layer 30 but does not contact the anode layer 20. The inactive member 40 fills a space extending from one side surface of the positive electrode layer 10 to the end portion of the solid electrolyte layer 30, for example.

[0128] The inert member 40 may be, for example, a gasket. By using a gasket as the inert member 40, cracks in the solid electrolyte layer 30 caused by a pressure difference during the pressing process can be effectively suppressed.

[0129] The inactive member 40 may have, for example, a single-layer structure. Meanwhile, although not shown in the drawings, the inactive member 40 may have a multi-layer structure. In the inactive member 40 having a multi-layer structure, each layer has a different composition. The inactive member having a multi-layer structure may have, for example, a two-layer structure, a three-layer structure, a four-layer structure, or a five-layer structure. The inactive member 40 having a multi-layer structure may include, for example, one or more adhesive layers and one or more support layers. The adhesive layer effectively prevents separation between the positive electrode layer 10 and the solid electrolyte layer 30 due to volumetric changes in the positive electrode layer 10 that occur during the charge / discharge process of the all-solid-state secondary battery 1, and improves the film strength of the inactive member 40 by providing bonding strength between the support layer and other layers. The support layer provides support to the inactive member 40 and prevents uneven pressure from being applied to the solid electrolyte layer 30 during the pressurization process or the charge / discharge process, thereby preventing deformation of the manufactured all-solid-state secondary battery 1.

[0130] 5, the all-solid-state secondary battery 1 includes a positive electrode 10, a negative electrode 20, and solid electrolyte layers 30, 30a, and 30b disposed therebetween. The positive electrode layer 10 includes a positive electrode current collector 11 and a first positive electrode active material layer 12a and a second positive electrode active material layer 12b disposed on both surfaces of the positive electrode current collector 11, respectively. The solid electrolyte layer 30 includes a first solid electrolyte layer 30a in contact with the first positive electrode active material layer 12a and a second solid electrolyte layer 30b in contact with the second positive electrode active material layer 12b, respectively. The negative electrode layer 20 includes a first negative electrode layer 20a in contact with the first solid electrolyte layer 30a and a second negative electrode layer 20b in contact with the second solid electrolyte layer 30b, respectively. An inactive member 40 is disposed between the opposing first and second solid electrolyte layers 30a and 30b to surround the side surfaces of the positive electrode layer 10. The inactive member 40 includes, for example, a first inactive member 40a in contact with the first solid electrolyte layer 30a and a second inactive member 40b in contact with the second solid electrolyte layer 30b. Therefore, the all-solid-state secondary battery 1 has a bi-cell structure. The all-solid-state secondary battery 1 has such a bi-cell structure, where the solid electrolyte layer 30 and the anode layer 20 are symmetrically arranged facing each other with the cathode layer 10 at the center. This effectively suppresses structural deformation due to pressure applied during the manufacturing of the all-solid-state secondary battery 1. Therefore, cracks in the solid electrolyte layer 30 during the manufacturing process and / or the charge / discharge process of the all-solid-state secondary battery 1 are suppressed, thereby preventing short circuits in the all-solid-state secondary battery 1. As a result, the cycle characteristics of the all-solid-state secondary battery 1 are further improved. Furthermore, since only one cathode current collector 11 is used for multiple cathode active material layers 12a, 12b, the energy density of the all-solid-state secondary battery 1 is increased.

[0131] 3 to 5, the inert member 40 is, for example, a flame-retardant inert member. The flame-retardant inert member provides flame retardancy, thereby preventing thermal runaway and the possibility of fire in the all-solid-state secondary battery 1. As a result, the safety of the all-solid-state secondary battery 1 is further improved. The flame-retardant inert member absorbs residual moisture in the all-solid-state secondary battery 1, thereby preventing deterioration of the all-solid-state secondary battery 1 and improving the life characteristics of the all-solid-state secondary battery 1.

[0132] The flame-retardant inert member includes, for example, a matrix and a filler. The matrix includes, for example, a substrate and a reinforcing material. The matrix includes, for example, a fibrous substrate and a fibrous reinforcing material. When the matrix includes the substrate, the matrix has elasticity. Therefore, the matrix can be arranged in various positions while effectively accommodating volume changes during charging and discharging of the all-solid-state secondary battery 1. The substrate included in the matrix includes, for example, a first fibrous material. When the substrate includes the first fibrous material, the matrix effectively accommodates volume changes in the positive electrode layer 10 that occur during charging and discharging of the all-solid-state secondary battery 1, and effectively suppresses deformation of the inert member 40 due to volume changes in the positive electrode layer 10. The first fibrous material is, for example, a material with an aspect ratio of 5 or more, 20 or more, or 50 or more. The first fibrous material is, for example, a material with an aspect ratio of 5 to 1000, 20 to 1000, or 50 to 1000. The first fibrous material is, for example, an insulating material. The first fibrous material is an insulating material, which can effectively prevent short-circuiting between the positive electrode layer 10 and the negative electrode layer 20 due to lithium dendrites or the like that occur during the charge and discharge process of the all-solid-state secondary battery 1. The first fibrous material includes, for example, one or more selected from pulp fiber, insulating polymer fiber, and ion-conductive polymer fiber. The matrix includes a reinforcing material, which improves the strength of the matrix. Therefore, the matrix can prevent excessive volume change during charge and discharge of the all-solid-state secondary battery 1, thereby preventing deformation of the all-solid-state secondary battery. The reinforcing material included in the matrix includes, for example, a second fibrous material. The reinforcing material includes the second fibrous material, which can more uniformly increase the strength of the matrix. The second fibrous material is, for example, a material with an aspect ratio of 3 or more, 5 or more, or 10 or more. The second fibrous material is, for example, a material with an aspect ratio of 3 to 100, 5 to 100, or 10 to 100. The second fibrous material is, for example, a flame-retardant material. The flame-retardant second fibrous material can effectively prevent ignition due to thermal runaway that occurs during the charge / discharge process or due to external impact of the all-solid-state secondary battery 1. The second fibrous material is, for example, glass fiber, metal oxide fiber, ceramic fiber, etc.

[0133] The flame-retardant inert member includes a filler in addition to the matrix. The filler may be disposed inside the matrix, on the surface of the matrix, or both inside and on the surface. The filler may be, for example, an inorganic material. The filler included in the flame-retardant inert member may be, for example, a moisture getter, a flame retardant, or a lithium immobilizer. The moisture adsorbent adsorbs moisture at temperatures below 100°C, for example, to remove moisture remaining in the all-solid-state secondary battery 1 and prevent deterioration of the all-solid-state secondary battery 1. Furthermore, when the temperature of the all-solid-state secondary battery 1 increases to 150°C or higher due to thermal runaway caused by the charge / discharge process or external impact, the moisture adsorbent releases the adsorbed moisture, effectively suppressing ignition of the all-solid-state secondary battery 1. The moisture adsorbent may be, for example, a metal hydroxide having moisture adsorption properties. The metal hydroxide contained in the filler is, for example, Mg(OH)2, Fe(OH)3, Sb(OH)3, Sn(OH)4, Ti(OH)3, Zr(OH)4, Al(OH)3, or a combination thereof. The flame retardant is, for example, zinc borate, calcium molybdate zinc complex, MoO 3、 The filler includes one or more selected from (NH4)2Mo2O7, Sb2O3, and Sb3O5. The lithium immobilizing agent is a compound that reacts with liquid lithium at, for example, 180°C or higher, which is the melting temperature of lithium, to immobilize lithium. The lithium immobilizing agent can react with liquid lithium to convert it into another insoluble compound. The lithium immobilizing agent is, for example, a metal oxide that is reactive with liquid lithium. The metal oxide contained in the filler is, for example, TiO2, ZrO2, HfO2, ThO2, or a combination thereof. The metal oxide reacts with liquid lithium to produce Li2O and a metal. The reaction formula is, for example, 4Li + MO2 → M + 2Li2O. Liquid lithium reacts with the metal oxide to produce lithium oxide, thereby immobilizing the liquid lithium. Leakage of liquid lithium melted at high temperatures to the positive electrode can be suppressed. This can improve the safety of all-solid-state secondary batteries.

[0134] The content of the filler contained in the flame-retardant inert material is, for example, 1 to 80 parts by weight, 5 to 80 parts by weight, 10 to 80 parts by weight, 20 to 80 parts by weight, 30 to 80 parts by weight, 40 to 80 parts by weight, 50 to 80 parts by weight, 60 to 80 parts by weight, or 65 to 80 parts by weight per 100 parts by weight of the flame-retardant inert material 40.

[0135] The flame-retardant inert member may further include, for example, a binder. The binder may include, for example, a curable polymer or a non-curable polymer. The curable polymer is a polymer that is cured by heat and / or pressure. The curable polymer is, for example, solid at room temperature. The flame-retardant inert member may include, for example, a heat-pressure-curable film and / or its cured product. An example of a heat-pressure-curable polymer is TSA-66 from Toray Industries.

[0136] The flame-retardant inert member may further include other materials in addition to the above-described substrate, reinforcing material, filler, and binder. The flame-retardant inert member may further include at least one selected from the group consisting of paper, insulating polymers, ion-conducting polymers, insulating inorganic materials, oxide-based solid electrolytes, and sulfide-based solid electrolytes. The insulating polymer may be, for example, an olefin-based polymer such as polypropylene (PP) or polyethylene (PE).

[0137] The density of the substrate or the density of the reinforcing material contained in the flame-retardant inert member is, for example, 10% to 300%, 10% to 150%, 10% to 140%, 10% to 130%, or 10% to 120% of the density of the positive electrode active material contained in the positive electrode active material layer 22.

[0138] The inactive member 40 is a member that does not contain a material having electrochemical activity, such as an electrode active material. The electrode active material is a material that absorbs / desorbs lithium. The inactive member 40 is a member that is made of a material other than the electrode active material and is used in the art.

[0139] [Manufacturing all-solid-state secondary batteries] (Negative electrode layer manufacturing) A method for manufacturing a negative electrode layer includes, for example, providing a negative electrode current collector; and sequentially providing a first protective layer and a first negative electrode active material layer, wherein the first negative electrode active material layer includes a carbon-based material matrix and a metal-based negative electrode active material disposed within the carbon-based material matrix, the carbon-based material matrix includes a first carbon-based nanostructure, and the first protective layer includes a second carbon-based nanostructure.

[0140] A negative electrode current collector is provided. For details regarding the negative electrode current collector, please refer to the negative electrode current collector section described above.

[0141] The step of sequentially providing the first protective layer and the first negative electrode active material layer may include, for example, providing a negative electrode active material precursor on a negative electrode current collector, and supplying a reaction gas containing a carbon source gas to the negative electrode current collector on which the negative electrode active material precursor is provided, and performing a heat treatment. During the heat treatment, a negative electrode active material is formed from the negative electrode active material precursor, second carbon-based nanostructures are grown between the negative electrode current collector and the negative electrode active material by a gas-phase reaction to form the first protective layer, and first carbon-based nanostructures are grown on the negative electrode active material by a gas-phase reaction to form the first negative electrode active material layer.

[0142] The step of providing a negative electrode active material precursor on a negative electrode current collector may, for example, provide a precursor compound containing a metal that forms an alloy or compound with lithium on the negative electrode current collector. The negative electrode active material precursor may be provided by a dry or wet method. For example, a solution containing the negative electrode active material precursor may be coated on the negative electrode current collector and then dried to provide the negative electrode active material precursor on the negative electrode current collector. Examples of metals that form alloys or compounds with lithium include gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), zinc (Zn), or combinations thereof. Examples of precursor compounds containing metals that form alloys or compounds with lithium include, but are not limited to, nitrates of metals that form alloys or compounds with lithium, halogen salts of metals that form alloys or compounds with lithium, phosphates of metals that form alloys or compounds with lithium, and sulfates of metals that form alloys or compounds with lithium. Any precursor compound known in the art may be used. Examples of precursor compounds containing silver (Ag) include silver nitrate (AgNO), silver acetate (CHCOOAg), and silver diamine chloride (Ag(NH)Cl). Examples of solvents that dissolve the precursor compounds include, but are not limited to, water and alcohol. Examples of alcohol include methanol and ethanol.

[0143] The negative electrode current collector on which the negative electrode active material precursor is provided is then heat-treated by supplying a reaction gas containing a carbon source gas to the negative electrode current collector. The carbon source gas may further include one or more inert gases selected from the group consisting of nitrogen, helium, and argon.

[0144] The carbon source gas is a compound represented by the following Chemical Formula 9, a compound represented by the following Chemical Formula 10, a compound represented by the following Chemical Formula 11, or a mixed gas of two or more selected from the compound represented by the following Chemical Formula 9, the compound represented by the following Chemical Formula 10, and the compound represented by the following Chemical Formula 11:

[0145] <9> Cn H 2n+2 In the above Chemical Formula 9, n is 1 to 20, <C10> C n H2n In the above Chemical Formula 10, n is 2 to 6, <C11> C n H n In the above chemical formula 11, n is 2 to 6.

[0146] The compound represented by Chemical Formula 9, the compound represented by Chemical Formula 10, and the compound represented by Chemical Formula 11 are, for example, one or more selected from the group consisting of methane, acetylene, ethylene, and propylene.

[0147] After the heat treatment step of supplying a reaction gas containing a carbon source gas to the negative electrode current collector provided with the negative electrode active material precursor, a cooling step is further performed using one or more inert gases selected from the group consisting of nitrogen, helium, and argon. The cooling step refers to a step of adjusting the temperature to room temperature (20-25°C).

[0148] In the method for manufacturing the negative electrode layer, the process of growing carbon-based nanostructures through a gas phase reaction to form the first protective layer and the first negative electrode active material layer may be performed under various conditions.

[0149] According to the first condition, for example, methane is first supplied to a reactor in which a negative electrode current collector provided with a negative electrode active material precursor is placed, and the temperature is raised to a heat treatment temperature T. The temperature raising time to the heat treatment temperature T is 10 minutes to 4 hours, and the heat treatment temperature T is in the range of 500 to 1100°C. The heat treatment is carried out at the heat treatment temperature T for a reaction time. The reaction time is, for example, 10 minutes to 8 hours. The heat-treated resultant is cooled to room temperature to manufacture a negative electrode layer. The time required for the process of cooling from the heat treatment temperature T to room temperature is, for example, 10 minutes to 5 hours.

[0150] According to the second condition, for example, hydrogen is first supplied to a reactor containing a negative electrode current collector provided with a negative electrode active material precursor, and the temperature is raised to a heat treatment temperature T. The temperature raising time to the heat treatment temperature T is 10 minutes to 4 hours, and the heat treatment temperature T is in the range of 500 to 1100°C. After the heat treatment is performed for a certain reaction time at the heat treatment temperature T, methane gas is supplied and the heat treatment is performed for the remaining reaction time. The reaction time is, for example, 10 minutes to 8 hours. The heat-treated result is cooled to room temperature to produce a negative electrode layer. Nitrogen is supplied during the cooling process. The time required for the process of cooling from the heat treatment temperature T to room temperature is, for example, 10 minutes to 5 hours.

[0151] According to the third condition, for example, hydrogen is first supplied to a reactor containing a negative electrode current collector provided with a negative electrode active material precursor, and the temperature is raised to a heat treatment temperature T. The temperature rise time to the heat treatment temperature T is 10 minutes to 4 hours, and the heat treatment temperature T is in the range of 500 to 1100°C. After heat treatment at the heat treatment temperature T for a certain reaction time, a mixed gas of methane and hydrogen is supplied, and heat treatment is carried out for the remaining reaction time. The reaction time is, for example, 10 minutes to 8 hours. The heat-treated result is cooled to room temperature to produce a composite. Nitrogen is supplied during the cooling process. The time required for the process of cooling from the heat treatment temperature T to room temperature is, for example, 10 minutes to 5 hours.

[0152] The carbon source gas is, for example, methane; acetylene; a mixed gas containing methane and an inert gas; or a mixed gas containing acetylene and an inert gas.

[0153] The carbon source gas is, for example, a mixture of methane and nitrogen. In the mixture of methane and nitrogen, the molar ratio of methane to nitrogen is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. The carbon source gas does not contain an inert gas such as nitrogen. The carbon source gas is, for example, a mixture of acetylene and nitrogen. In the mixture of acetylene and nitrogen, the molar ratio of acetylene to nitrogen is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. The carbon source gas does not contain an inert gas such as nitrogen.

[0154] The heat treatment pressure can be selected taking into consideration the heat treatment temperature, the composition of the gas mixture, the desired thickness of the negative electrode layer, etc. The heat treatment pressure can be controlled by adjusting the amount of the inflowing gas mixture and the outflowing gas mixture. The heat treatment pressure can be, for example, 0.5 atm or more, 1 atm or more, 2 atm or more, 3 atm or more, 4 atm or more, or 5 atm or more.

[0155] The heat treatment time is not particularly limited and can be appropriately adjusted depending on the heat treatment temperature, the pressure during the heat treatment, the composition of the gas mixture, and the desired thickness of the negative electrode layer. For example, the reaction time at the heat treatment temperature may be, for example, 10 minutes to 100 hours, 30 minutes to 90 hours, or 50 minutes to 40 hours. As the heat treatment time increases, the content of grown carbon-based nanostructures increases, thereby improving the electrochemical properties of the resulting negative electrode layer. However, this trend is not necessarily directly proportional to the time. For example, after a certain time has elapsed, the growth of carbon-based nanostructures may cease or the growth rate may decrease.

[0156] (Manufacturing of solid electrolyte layer) The solid electrolyte layer can be produced by a dry process or a wet process.

[0157] The method for manufacturing a solid electrolyte layer by a dry method includes the steps of dry-mixing a sulfide-based solid electrolyte and a binder to prepare a dry mixture; forming the dry mixture to prepare a solid electrolyte layer; and disposing the solid electrolyte layer between a positive electrode layer and a negative electrode layer.

[0158] First, a sulfide-based solid electrolyte and a binder are dry-mixed to prepare a dry mixture. Dry mixing refers to mixing without a process solvent. A dry mixture refers to a mixture to which a process solvent is not intentionally added. The process solvent is, for example, a solvent used in preparing an electrode slurry. The binder is, for example, a dry binder. A dry binder refers to a binder that does not contain a process solvent. The process solvent is, for example, water, NMP, etc., but is not limited thereto, as long as it is a process solvent used in preparing an electrode slurry. Dry mixing may be performed using a stirrer at a temperature of, for example, 25 to 85°C or 65 to 85°C. Dry mixing may be performed using a stirrer at a rotation speed of, for example, 10 to 10,000 rpm or 100 to 10,000 rpm. Dry mixing may be performed using a stirrer for, for example, 1 to 200 minutes. Dry mixing may be performed, for example, one or more times. The dry mixing produces a dry mixture containing a fibrillated dry binder. The mixer is, for example, a mixer or kneader. The mixer includes, for example, a chamber; one or more rotating shafts disposed within the chamber; and blades rotatably coupled to the rotating shafts and arranged in the longitudinal direction of the rotating shafts. The blades may be, for example, one or more selected from a ribbon blade, a sigma blade, a jet (Z) blade, a dispersion blade, and a screw blade. The inclusion of the blades allows the electrode active material, the dry conductive material, and the dry binder to be effectively mixed without a solvent to produce a dough-like mixture.

[0159] The dry mixture can then be molded to prepare a solid electrolyte layer. The produced dry mixture can be, for example, fed into an extrusion device and extruded into a sheet. The extrusion pressure is, for example, 4 MPa to 100 MPa, or 10 MPa to 90 MPa. The resulting mixture can also be in the form of a sheet. That is, the resulting sheet-like mixture can also be the solid electrolyte layer. The extrusion device can be, for example, a roller or an extruder. The type and content of the sulfide-based solid electrolyte and binder can be found in the solid electrolyte layer section described above. The binder can be omitted. For example, the sulfide-based solid electrolyte particles can be partially sintered by pressure, so the binder can be omitted.

[0160] The wet method for manufacturing a solid electrolyte layer includes the steps of: mixing a sulfide-based solid electrolyte, a binder, and a solvent to prepare a slurry; forming and drying the slurry to prepare a solid electrolyte layer; and disposing the solid electrolyte layer between a positive electrode layer and a negative electrode layer.

[0161] First, a sulfide-based solid electrolyte, a binder, and a solvent are mixed to prepare a slurry. The sulfide-based solid electrolyte and the binder are described in the solid electrolyte layer section above. The binder may be the same as or different from the binder used in the dry method. Examples of binders used in the solid electrolyte layer include, but are not limited to, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, and polyethylene, and any binder known in the art may be used. The solvent is not particularly limited, and any binder that does not react with the sulfide-based solid electrolyte and can dissolve the binder may be used. For example, octyl acetate may be used as the solvent.

[0162] The slurry is then cast and dried to prepare a solid electrolyte layer. For example, the slurry may be coated on a substrate, dried, and then separated from the substrate to prepare a solid electrolyte layer. The coating method and drying conditions may be performed according to a method and / or a range of conditions commonly used in the art.

[0163] Next, a solid electrolyte layer is disposed between the positive electrode layer and the negative electrode layer. As described above, the solid electrolyte layer may be disposed on the positive electrode layer and / or the negative electrode layer after a separate solid electrolyte layer is prepared, or may be disposed on the positive electrode layer and / or the negative electrode layer by applying a slurry thereto and drying it.

[0164] (Positive electrode layer manufacturing) The positive electrode layer can be produced by a wet process or a dry process.

[0165] The positive electrode layer may be manufactured, for example, by a wet process. A positive electrode active material, a sulfide-based solid electrolyte, a conductive material, a binder, and a solvent are mixed to prepare a positive electrode slurry. The positive electrode slurry may be coated on a positive electrode current collector and then dried to prepare a positive electrode layer. The solvent used to manufacture the positive electrode slurry is not particularly limited, and any solvent used in the art for positive electrode slurries may be used. An example of the solvent used for the positive electrode slurry is paraxylene. For the types and contents of the positive electrode current collector, positive electrode active material, conductive material, and binder, please refer to the section on the positive electrode layer described above.

[0166] The positive electrode layer may be manufactured, for example, by a dry process. First, a positive electrode active material, a sulfide-based solid electrolyte, a conductive material, and a binder are dry-mixed to prepare a dry mixture. Then, the dry mixture is molded to prepare a positive electrode active material layer. Then, the formed positive electrode active material layer is placed on one or both sides of a positive electrode current collector and pressed to prepare a positive electrode layer. The binder is, for example, a dry binder. Specific manufacturing conditions and methods for the steps of preparing the dry mixture and molding the dry mixture are substantially the same as those for the above-described method of manufacturing a solid electrolyte layer. For the types and contents of the positive electrode current collector, positive electrode active material, conductive material, and binder, please refer to the above-described section on the positive electrode layer.

[0167] (Manufacturing all-solid-state secondary batteries) The all-solid-state secondary battery can be manufactured, for example, as follows.

[0168] First, an electrode assembly is provided, which includes a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer.

[0169] A solid electrolyte layer is placed on the anode layer so that the anode active material layer contacts the solid electrolyte layer, thereby preparing an anode layer / solid electrolyte layer stack. Then, the solid electrolyte layer is placed on one or both sides of the cathode layer so that it faces the cathode active material layer, thereby preparing an anode layer / solid electrolyte layer / cathode layer stack. A gasket, an inert member that surrounds the side of the cathode layer, is placed around the cathode layer. The prepared anode layer / solid electrolyte layer / cathode layer stack is subjected to a plate press treatment at 50-100°C and a pressure of 300-600 MPa for 10-60 minutes. This press treatment partially sinters the solid electrolyte layer, improving battery characteristics. The pressed stack is used as an electrode assembly. The electrode assembly is sealed with a sealant to complete an all-solid-state secondary battery.

[0170] The present invention will be explained in more detail with reference to the following examples and comparative examples, but the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.

[0171] Example 1: Methane 1000°C, horizontally aligned graphene layer (first protective layer) / Ag-embedded horizontally aligned graphene layer (first negative electrode active material layer), mono-cell all-solid-state secondary battery (Solid electrolyte layer manufacturing, dry method) Argyrodite-type crystal Li6PS5Cl sulfide-based solid electrolyte (D 50= 10 μm, crystalline), 98 parts by weight of solid electrolyte, 1 part by weight of polytetrafluoroethylene (PTFE) first binder, and 1 part by weight of polyvinylidene fluoride (PVDF) second binder were added to a grind mixer and mixed to prepare a mixture. The prepared mixture was added to a mortar heated to 80°C and stirred to prepare dough. The prepared dough was passed through a roller to form it into a sheet, preparing a solid electrolyte layer with a certain thickness. The solid electrolyte layer was manufactured through the above process. The elastic modulus of the sulfide-based solid electrolyte layer was approximately 15 GPa to 30 GPa.

[0172] (Negative electrode layer manufacturing) A carbon layer as a first protective layer and a carbon layer containing a negative electrode active material as a first negative electrode active material layer were sequentially deposited on one surface of a 20 μm thick Cu foil to prepare a negative electrode.

[0173] The first protective layer and the first negative electrode active material layer were formed by the following method.

[0174] AgNO3 as an Ag precursor compound was dissolved in methanol as an organic solvent to prepare a composition containing an Ag precursor compound.

[0175] The Ag precursor compound-containing composition was coated on a Cu foil, and the organic solvent was then removed to prepare a Cu foil coated with the Ag precursor compound.

[0176] The Cu foil coated with the Ag precursor compound was placed in a chamber, and then the temperature was raised to 1000°C while a mixture of methane gas as a hydrocarbon gas and argon gas as an inert gas was supplied, allowing horizontally aligned graphene to grow directly on the Cu foil.

[0177] At temperatures above 400°C in the chamber, Ag ions were reduced to Ag particles, and graphene was grown and stacked horizontally on the Cu current collector, forming a carbon layer between the Cu current collector and the Ag particles.

[0178] At a chamber temperature of 1000°C, graphene grew from the Ag particles, forming a carbon-based matrix containing graphene arranged horizontally on the carbon layer. The Ag particles were dispersed and embedded within the carbon-based matrix. A shell containing amorphous carbon formed along the surface of the Ag particles. The diameter of the Ag core particles was approximately 50 nm. The thickness of the shell was approximately 10 nm.

[0179] The carbon layer serving as the first protective layer had a thickness of about 500 nm, and the Ag-containing carbon layer serving as the first negative electrode active material layer had a thickness of about 3 μm.

[0180] Transmission electron microscope (TEM) and high-resolution scanning electron microscope (HR-SEM) measurements of the cross section of the fabricated negative electrode confirmed that the first protective layer contained graphene aligned in a direction parallel to the Cu current collector surface, that the first negative electrode active material layer contained graphene aligned in a direction parallel to the Cu current collector surface and Ag cores, and that a shell containing amorphous carbon was present on the Ag cores.

[0181] (Positive electrode layer manufacturing) Li2O-ZrO2 (LZO) coated LiNi as the positive electrode active material 0.8 Co 0.15 Mn 0.05O2 (NCM) was prepared. The LZO-coated cathode active material was prepared according to the method disclosed in Korean Patent Publication No. 10-2016-0064942. Argyrodite-type crystal Li6PS5Cl (D50 = 0.5 μm, crystalline) was prepared as the solid electrolyte. Polytetrafluoroethylene (PTFE) was prepared as the binder. Carbon nanofibers (CNF) were prepared as the conductive material. These materials were mixed with xylene solvent in a weight ratio of 84:11.5:3:1.5 cathode active material:solid electrolyte:conductive material:binder. The slurry was formed into a sheet and vacuum-dried at 40°C for 8 hours to prepare a cathode sheet. The prepared cathode sheet was placed on the carbon layer of a cathode current collector made of aluminum foil coated on one side, and the cathode layer was prepared using a heated roll press at 85°C. The total thickness of the positive electrode layer was about 120 μm, the thickness of each positive electrode active material layer was about 95 μm, and the thickness of the carbon-coated aluminum foil was about 25 μm.

[0182] (inert material) A slurry made by mixing pulp fiber, glass fiber, aluminum hydroxide (Al(OH)3), acrylic binder, and solvent was formed into a gasket shape, and then the solvent was removed to produce a flame-retardant inert member.

[0183] The weight ratio of cellulose fiber, glass fiber, aluminum hydroxide (Al(OH)3), and acrylic binder was 20:8:70:2. The thickness of the inert member was approximately 120 μm. The manufactured flame-retardant member was left at room temperature for one week before use.

[0184] Before application to the all-solid-state secondary battery, the inactive material was subjected to vacuum heat treatment at 80°C for 5 hours to remove moisture and other impurities from the inactive material.

[0185] (Manufacturing all-solid-state secondary batteries) 3, a solid electrolyte layer was disposed on the negative electrode layer such that the first negative electrode active material layer was in contact with the solid electrolyte layer. A flame-retardant inert member was disposed on the solid electrolyte layer under heat and pressure to prepare a laminate of the negative electrode layer / solid electrolyte layer / inert member.

[0186] The inert member was placed on one side of the positive electrode layer so as to face the positive electrode active material layer, preparing an anode layer / solid electrolyte layer / positive electrode layer electrode assembly. The inert member was placed around the positive electrode layer, surrounding the side of the positive electrode layer and contacting the solid electrolyte layer. The inert member was used as a gasket. The positive electrode layer was placed at the center of the solid electrolyte layer, and the gasket was placed around the positive electrode layer and extending to the end of the solid electrolyte layer. The area of ​​the positive electrode layer was approximately 90% of the area of ​​the solid electrolyte layer, and the gasket was placed over the entire remaining 10% area of ​​the solid electrolyte layer where the positive electrode layer was not placed.

[0187] The prepared anode / solid electrolyte / cathode electrode assembly was plate-pressed at 85°C and 500 MPa for 30 minutes. This pressurization sinters the solid electrolyte layer, improving battery performance. The thickness of the sintered solid electrolyte layer was approximately 45 μm. The sintered electrode assembly was placed in a pouch and sealed to prepare a sealed electrode assembly. Portions of the cathode current collector and anode current collector protruded from the sealed electrode assembly to serve as cathode and anode terminals.

[0188] The electrode assembly was placed between two pressure plates (not shown), which were screwed together to apply a constant pressure to both sides of the electrode assembly, thereby manufacturing an all-solid-state secondary battery.

[0189] Example 2: Methane 850°C, horizontally aligned graphene layer (first protective layer) / Ag-embedded disordered graphene layer (first negative electrode active material layer), mono-cell all-solid-state secondary battery A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that the deposition temperature was changed to 850°C.

[0190] A carbon layer as a first protective layer and a carbon layer containing a negative electrode active material as a first negative electrode active material layer were sequentially vapor-deposited on one surface of a 20 μm thick Cu foil to prepare a negative electrode.

[0191] The first protective layer had a structure in which multiple layers of graphene were stacked, with the graphene aligned horizontally to the surface of the Cu foil.

[0192] The first negative electrode active material layer had a structure in which a carbon-based material matrix consisting of irregularly arranged flake-like graphene was arranged, and Ag particles, which were the negative electrode active material, were dispersed and embedded within the carbon-based material matrix.

[0193] The surface of the Ag particles was coated with a shell containing amorphous carbon.

[0194] The carbon layer serving as the first protective layer had a thickness of about 500 nm, and the Ag-containing carbon layer serving as the first negative electrode active material layer had a thickness of about 3 μm.

[0195] Transmission electron microscopy (TEM) and high-resolution scanning electron microscopy (HR-SEM) of the cross section of the fabricated negative electrode confirmed that the first protective layer contained graphene aligned parallel to the surface of the Cu current collector. The first negative electrode active material layer also contained irregularly arranged graphene and Ag cores. The presence of a shell containing amorphous carbon arranged on the Ag cores was also confirmed.

[0196] Example 3: Acetylene 800°C, protruding aligned graphene layer (first protective layer) / Ag-embedded disordered graphene layer (first negative electrode active material layer), mono-cell all-solid-state secondary battery A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that the deposition temperature was changed to 800° C. and the hydrocarbon gas was changed to acetylene.

[0197] A carbon layer as a first protective layer and a carbon layer containing a negative electrode active material as a first negative electrode active material layer were sequentially vapor-deposited on one surface of a 20 μm thick Cu foil to prepare a negative electrode.

[0198] The first protective layer had a structure in which multiple layers of graphene were stacked, with the graphene aligned in a direction protruding from the surface of the Cu foil.

[0199] The first negative electrode active material layer had a structure in which a carbon-based material matrix consisting of irregularly arranged flake-like graphene was arranged, and Ag particles, which were the negative electrode active material, were dispersed and embedded within the carbon-based material matrix.

[0200] The surface of the Ag particle core is coated with a shell containing amorphous carbon. The first negative electrode active material layer contains pores inside the carbon-based material matrix due to the irregularly arranged graphene.

[0201] The carbon layer serving as the first protective layer had a thickness of about 500 nm, and the Ag-containing carbon layer serving as the first negative electrode active material layer had a thickness of about 3 μm.

[0202] Through transmission electron microscopy (TEM) and high-resolution scanning electron microscopy (HR-SEM) of the cross section of the fabricated anode, it was confirmed that the first protective layer contained stacked graphene aligned in a direction protruding from the Cu current collector surface. It was also confirmed that the first anode active material layer contained irregularly arranged graphene and Ag cores. It was also confirmed that a shell containing amorphous carbon was present on the Ag cores.

[0203] Example 4: Acetylene 600°C, protruding aligned graphene layer (first protective layer) / Ag-embedded disordered graphene layer (first negative electrode active material layer), mono-cell all-solid-state secondary battery A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that the heat treatment temperature was changed to 600° C. and the hydrocarbon gas was changed to acetylene.

[0204] A negative electrode current collector was prepared by sequentially depositing a carbon layer as a first protective layer and a carbon layer containing a negative electrode active material as a first negative electrode active material layer on one side of a 20 μm thick Cu foil.

[0205] The first protective layer had a structure in which multiple layers of graphene were stacked, with the graphene aligned in a direction protruding from the surface of the Cu foil.

[0206] The first negative electrode active material layer had a structure in which a carbon-based material matrix consisting of irregularly arranged flake-shaped graphene was arranged, and Ag particles, which were the negative electrode active material, were dispersed and embedded within the carbon-based material matrix.

[0207] The surface of the Ag particle core is coated with a shell containing amorphous carbon. The first negative electrode active material layer contains pores inside the carbon-based material matrix due to the irregularly arranged graphene.

[0208] The porosity of the first negative electrode active material layer in Example 4 was even higher than the porosity of the first negative electrode active material layer in Example 3.

[0209] The carbon layer serving as the first protective layer had a thickness of about 500 nm, and the Ag-containing carbon layer serving as the first negative electrode active material layer had a thickness of about 3 μm.

[0210] Through transmission electron microscopy (TEM) and high-resolution scanning electron microscopy (HR-SEM) of the cross section of the fabricated anode, it was confirmed that the first protective layer contained stacked graphene aligned in a direction protruding from the Cu current collector surface. It was also confirmed that the first anode active material layer contained irregularly arranged graphene and Ag cores. It was also confirmed that a shell containing amorphous carbon was present on the Ag cores.

[0211] Example 5: Bi-cell all-solid-state secondary battery (Production of solid electrolyte layer, negative electrode layer, and inactive member) It was produced in the same manner as in Example 1.

[0212] (Positive electrode layer manufacturing) Li2O-ZrO2 (LZO) coated LiNi as the positive electrode active material 0.8 Co 0.15 Mn 0.05O2 (NCM) was prepared. The LZO-coated positive electrode active material was prepared according to the method disclosed in Korean Patent Publication No. 10-2016-0064942. Argyrodite-type crystal Li6PS5Cl (D50 = 0.5 μm, crystalline) was prepared as the solid electrolyte. Polytetrafluoroethylene (PTFE) was prepared as the binder. Carbon nanofibers (CNF) were prepared as the conductive material. These materials were mixed with xylene solvent in a weight ratio of 84:11.5:3:1.5 (positive electrode active material: solid electrolyte: conductive material: binder). The slurry was formed into a sheet and vacuum-dried at 40°C for 8 hours to prepare a positive electrode sheet. The prepared positive electrode sheets were placed on both sides of a positive electrode current collector made of aluminum foil coated on both sides with a carbon layer, and the positive electrode layer was prepared by heated roll pressing at 85°C. The total thickness of the positive electrode layer was about 220 μm, the thickness of each positive electrode active material layer was about 96 μm, and the thickness of the carbon-coated aluminum foil was about 28 μm.

[0213] (Manufacturing all-solid-state secondary batteries) 4, a solid electrolyte layer was disposed on the negative electrode layer such that the first negative electrode active material layer was in contact with the solid electrolyte layer. A flame-retardant inert member was disposed on the solid electrolyte layer by heat and pressure to prepare two negative electrode layer / solid electrolyte layer / inert member laminates.

[0214] The inactive members were placed on both sides of the positive electrode layer, facing the positive electrode active material layer, to prepare an anode layer / solid electrolyte layer / cathode layer / solid electrolyte layer / anode layer electrode assembly. The inactive members were placed around the positive electrode layer, surrounding the sides of the positive electrode layer and in contact with the solid electrolyte layer. The inactive members were used as gaskets. The positive electrode layer was placed at the center of the solid electrolyte layer, and the gasket was placed around the positive electrode layer and extending to the end of the solid electrolyte layer. The area of ​​the positive electrode layer was approximately 90% of the area of ​​the solid electrolyte layer, and the gasket was placed over the entire remaining 10% area of ​​the solid electrolyte layer where the positive electrode layer was not placed.

[0215] Using the prepared electrode assembly, an all-solid-state secondary battery was manufactured in the same manner as in Example 1.

[0216] Comparative Example 1: Coating-free negative electrode layer A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that a 20 μm thick Cu foil was used as the negative electrode layer.

[0217] Comparative Example 2: Carbon layer (first protective layer) alone (first negative electrode active material layer omitted) An anode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that only a carbon layer as a first protective layer was introduced onto one side of a 20 μm thick Cu foil without introducing an Ag precursor compound.

[0218] Comparative Example 3: Graphene wet coating (first protective layer) + Ag-carbon wet coating (first negative electrode active material layer) negative electrode layer A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that the first protective layer and the first negative electrode active material layer were respectively formed on one side of a 20 μm thick Cu foil by a wet method.

[0219] The negative electrode layer was produced by the following method.

[0220] (Negative electrode layer manufacturing) A carbon layer and a first negative electrode active material layer were wet-coated on one surface of a 20 μm thick Cu foil to prepare a negative electrode layer.

[0221] The carbon layer was fabricated by coating a graphene dispersion onto a Cu foil and then drying it. The graphene dispersion was prepared by dispersing graphene oxide and polyvinylidene fluoride (PVDF) binder in N-methylpyrrolidone.

[0222] Carbon black (CB) with a primary particle size of about 30 nm and silver (Ag) particles with an average particle size (D50) of about 60 nm were prepared as negative electrode active materials.

[0223] A mixed powder of 4 g of carbon black (CB) and silver (Ag) particles mixed at a weight ratio of 3:1 was placed in a container, and 4 g of an NMP solution containing 7 wt% PVDF binder (Kureha #9300) was added to prepare a mixed solution. Next, the mixed solution was stirred while gradually adding NMP to prepare a slurry. The prepared slurry was applied to the carbon layer of the prepared negative electrode layer using a bar coater and dried in air at 80°C for 10 minutes. The resulting laminate was then vacuum-dried at 40°C for 10 hours. The dried laminate was cold roll pressed to flatten the surface of the first negative electrode active material layer of the laminate. The negative electrode layer was fabricated through the above process.

[0224] The thickness of the first negative electrode active material layer included in the negative electrode layer was approximately 10 μm, and the thickness of the carbon layer serving as the first protective layer was approximately 1 μm.

[0225] Reference example 1: No inactive member (free) An all-solid-state secondary battery was produced in the same manner as in Example 1, except that no inert member was placed around the positive electrode active material layer.

[0226] Evaluation example 1: Crystallinity and porosity evaluation The crystallinity of the negative electrode layers prepared in Examples 1 to 4 was evaluated using XRD, Raman and transmission electron microscope.

[0227] In the Raman spectrum of the negative electrode layer, the 1350 cm spectrum originating from amorphous carbon was observed. -1 The D band peak intensity (I D ) and 1580 cm originating from crystalline carbon -1 Nearby G-band peak intensity (I G ) relative peak intensity ratio (I D / I G The relative crystallinity of the negative electrode layer was determined from the peak intensity ratio (I D / I G ) is higher, the crystallinity is lower, and the peak intensity ratio (I D / I G The lower the value, the higher the crystallinity. The measurement results are shown in Table 1 below.

[0228] Furthermore, the relative crystallinity was determined from the peak intensity and / or half-width in the XRD spectrum of the negative electrode layer, and from a high-resolution TEM image of the negative electrode layer and its diffraction pattern.

[0229] The porosity of the negative electrode layers prepared in Examples 1 to 4 was measured using a nitrogen gas adsorption method (multi-point BET), and the measurement results are shown in Table 1 below.

[0230] The crystallinity and porosity relate to the first negative electrode active material layer and the first protective layer of the negative electrode layer.

[0231] The crystallinity of the negative electrode layer manufactured in Example 1 was relatively highest, and the crystallinity of the negative electrode layer manufactured in Example 4 was relatively lowest.

[0232] The relative order of crystallinity of the negative electrode layer in the all-solid-state secondary batteries of Examples 1 to 4 was Example 1>Example 2>Example 3>Example 4.

[0233] The porosity of the negative electrode layer prepared in Example 1 was relatively the lowest, and the porosity of the negative electrode layer prepared in Example 4 was relatively the highest.

[0234] In the all-solid-state secondary batteries of Examples 1 to 4, the relative order of the porosity of the negative electrode layer was Example 4>Example 3>Example 2>Example 1.

[0235] [Table 1]

[0236] Evaluation example 2: Charge / discharge test The charge-discharge characteristics of the all-solid-state secondary batteries prepared in Examples 1 to 5, Comparative Examples 1 to 3, and Reference Example 1 were evaluated by the following charge-discharge test. The charge-discharge test was carried out by placing the all-solid-state secondary batteries in a thermostatic chamber at 45°C.

[0237] In the first cycle, the battery was charged at a constant current of 0.1 C until the battery voltage reached 4.2 V. Once 4.2 V was reached, a constant voltage charge was performed at 4.2 V with a 0.05 C cutoff. The battery was then discharged at a constant current of 0.1 C until the battery voltage reached 2.6 V.

[0238] After the second cycle, the battery was charged and discharged under the same conditions as the first cycle until it reached 1,250 cycles. The more cycles it took to short circuit, the better its lifespan. The results are shown in Table 2.

[0239] [Table 2]

[0240] As shown in Table 2, the all-solid-state secondary batteries of Examples 1 to 4 provided improved life characteristics compared to the all-solid-state secondary batteries of Comparative Examples 1 to 3.

[0241] It was determined that the all-solid-state secondary battery of Example 4 had relatively lower crystallinity in the first protective layer and the first negative electrode active material layer than the all-solid-state secondary batteries of Examples 1 to 3, and therefore the deterioration of the negative electrode current collector due to the solid electrolyte relatively increased.

[0242] The all-solid-state secondary battery of Comparative Example 1 did not include either the first protective layer or the first negative electrode active material layer, and therefore had significantly inferior life characteristics compared to the all-solid-state secondary batteries of Examples 1 to 4. It was determined that this was because the all-solid-state secondary battery of Comparative Example 1 did not include the first protective layer or the first negative electrode active material layer, and therefore the negative electrode current collector was easily degraded by the solid electrolyte, promoting the growth of lithium dendrites.

[0243] The all-solid-state secondary battery of Comparative Example 2 did not include a first negative electrode active material layer, and therefore had relatively poorer life characteristics than the all-solid-state secondary batteries of Examples 1 to 4. It was determined that the absence of a first negative electrode active material layer in the all-solid-state secondary battery of Comparative Example 2 made it impossible to effectively suppress the generation and growth of lithium dendrites, resulting in the deterioration of the all-solid-state secondary battery.

[0244] The all-solid-state secondary battery of Comparative Example 3, which included a wet graphene layer and a wet first anode active material layer, exhibited relatively poor life characteristics compared to the all-solid-state secondary batteries of Examples 1 to 4. This was determined to be because the wet graphene layer and wet first anode active material layer in the all-solid-state secondary battery of Comparative Example 3 were unable to effectively prevent degradation of the anode current collector due to the solid electrolyte compared to the first protective layer and first anode active material layer in Examples 1 to 4.

[0245] Although not shown in Table 2, the all-solid-state secondary battery of Example 5 had improved structural stability compared to the all-solid-state secondary battery of Example 1, and thus had relatively improved life characteristics.

[0246] Although not shown in Table 2, the all-solid-state secondary battery of Reference Example 1 had inferior life characteristics compared to the all-solid-state secondary batteries of Examples 1 to 4 because it did not include an inactive material gasket.

[0247] After the first cycle charging was completed for the all-solid-state secondary batteries of Examples 1 to 4, SEM images of the cross sections of the batteries were measured, and it was confirmed that a lithium metal deposition layer corresponding to the second negative electrode active material layer was formed between the solid electrolyte layer and the negative electrode current collector.

[0248] In the all-solid-state secondary batteries of Examples 1 to 4, the relative magnitude of the volume density of the first protective layer (carbon layer) was Example 1 ≒ Example 2 > Example 3 ≒ Example 4. The volume density of the dry-type first protective layer in Examples 1 to 4 was higher than the volume density of the wet-type first protective layer in Comparative Example 3.

[0249] As described above, the all-solid-state secondary battery according to this embodiment can be applied to various portable devices, vehicles, and the like.

[0250] Although exemplary embodiments have been described in detail above with reference to the accompanying drawings, the present invention is not limited to such examples. It is obvious that a person skilled in the art to which the present invention pertains can derive various modifications or alterations within the scope of the technical idea described in the claims, and it goes without saying that these also fall within the technical scope of the present invention. [Explanation of symbols]

[0251] 1 All-solid-state secondary battery 10 Positive electrode layer 11 Positive electrode current collector 12 Cathode active material layer 20 negative electrode layer 21 Negative electrode current collector 22 First negative electrode active material layer 23 1st protective layer 30 Solid electrolyte layer 40 Inert Materials

Claims

1. a positive electrode layer, a negative electrode layer, and a solid electrolyte layer between the positive electrode layer and the negative electrode layer; the positive electrode layer includes a positive electrode current collector and a positive electrode active material layer, the solid electrolyte layer includes a sulfide-based solid electrolyte, the negative electrode layer includes a negative electrode current collector, a first negative electrode active material layer, and a first protective layer disposed between the negative electrode current collector and the first negative electrode active material layer, the first negative electrode active material layer comprises a carbon-based material matrix and a metal-based negative electrode active material within the carbon-based material matrix; The carbon-based material matrix comprises a first carbon-based nanostructure, and the first protective layer comprises a second carbon-based nanostructure.

2. the first carbon-based nanostructure comprises a two-dimensional carbon-based nanostructure; 2. The all-solid-state secondary battery of claim 1, wherein the two-dimensional carbon-based nanostructure comprises graphene, graphene oxide, reduced graphene oxide, or a combination thereof.

3. 2. The all-solid-state secondary battery of claim 1, wherein the carbon-based material matrix includes a first carbon-based nanostructure arranged in a certain direction relative to a surface of the negative electrode current collector.

4. 2. The all-solid-state secondary battery of claim 1, wherein the carbon-based material matrix comprises a first carbon-based nanostructure that is randomly aligned.

5. 2. The all-solid-state secondary battery according to claim 1, wherein the carbon-based material matrix comprises crystalline carbon, amorphous carbon, or a combination thereof.

6. 2. The all-solid-state secondary battery according to claim 1, wherein the carbon-based material matrix further comprises pores, and the carbon-based material matrix is ​​a lithium host.

7. The metal-based negative electrode active material is a core and a shell disposed along a surface of the core; 2. The all-solid-state secondary battery of claim 1, wherein the core comprises a metal that forms an alloy or compound with lithium, and the shell comprises a carbon-based material.

8. 8. The all-solid-state secondary battery according to claim 7, wherein the metal comprises an alloying element selected from gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), zinc (Zn), or a combination thereof.

9. 8. The all-solid-state secondary battery of claim 7, wherein the shell comprises a third carbon-based nanostructure or the shell comprises amorphous carbon.

10. The all-solid-state secondary battery according to claim 7, wherein the metal-based negative electrode active material is particulate, the core has a particle size of 10 nm to 500 nm, and the shell has a thickness of 50 nm or less.

11. The all-solid-state secondary battery of claim 1 , wherein the content of the metal-based negative electrode active material is 10 parts by weight or less based on 100 parts by weight of the carbon-based material matrix.

12. the first negative electrode active material layer has a thickness of 20 μm or less and is free of a binder; a ratio C1 / C2 of a charge capacity C1 of the first negative electrode active material layer to a charge capacity C2 of the positive electrode active material layer is 0.001 to 0.45; the thickness of the first negative electrode active material layer is greater than the thickness of the first protective layer; In the Raman spectrum of the negative electrode layer, the 1350 cm -1 Nearby D band peak intensity (I D ) and 1580 cm originating from crystalline carbon -1 Nearby G band peak intensity (I G ) peak intensity ratio (I D / I G 2. The all-solid-state secondary battery according to claim 1, wherein the molecular weight of the all-solid-state secondary battery is 0.01 to 5.

13. the second carbon-based nanostructure comprises a two-dimensional carbon-based nanostructure; 2. The all-solid-state secondary battery of claim 1, wherein the two-dimensional carbon-based nanostructure comprises graphene, graphene oxide, reduced graphene oxide, or a combination thereof.

14. the first protective layer includes a second carbon-based nanostructure aligned in a predetermined direction relative to a surface of the negative electrode current collector; The second carbon-based nanostructures are aligned in a direction parallel to the surface of the negative electrode current collector or in a direction protruding from the surface of the negative electrode current collector; The all-solid-state secondary battery according to claim 13 , wherein the second carbon-based nanostructure is stacked along a thickness direction of the first protective layer, and the second carbon-based nanostructure is stacked in 100 layers or less.

15. the first protective layer is disposed directly on the negative electrode current collector, the first protective layer being inert to the sulfide-based solid electrolyte; The all-solid-state secondary battery according to claim 1 , wherein the first protective layer has a thickness of 2 μm or less, and the first protective layer is free of a binder.

16. a second negative electrode active material layer between the solid electrolyte layer and the negative electrode current collector, the second negative electrode active material layer is disposed at least between the first negative electrode active material layer and the first protective layer and between the first negative electrode active material layer and the solid electrolyte layer; The all-solid-state secondary battery according to claim 1 , wherein the second negative electrode active material layer is a metal layer containing lithium or a lithium alloy.

17. 2. The all-solid-state secondary battery according to claim 1, wherein the negative electrode current collector contains indium (In), copper (Cu), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), chromium (Cr), or an alloy thereof.

18. At least one of the positive electrode current collector and the negative electrode current collector includes a base film and a metal layer on one or both sides of the base film; the base film comprises a polymer, the polymer comprising polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof; 2. The all-solid-state secondary battery according to claim 1, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.

19. The positive electrode layer further includes an inactive member disposed on one side of the positive electrode layer, the inactive member surrounds the positive electrode layer along a side surface of the positive electrode layer, The all-solid-state secondary battery according to claim 1 , wherein the inactive member includes a positioning portion configured to determine a position of the inactive member on the solid electrolyte layer.

20. the positive electrode active material layer contains a positive electrode active material, The positive electrode active material includes an oxide-based positive electrode active material, a sulfide-based positive electrode active material, or a combination thereof; the oxide-based positive electrode active material includes a lithium transition metal oxide, a metal oxide, or a combination thereof, the lithium transition metal oxide includes lithium cobalt oxide, lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminium oxide, lithium nickel cobalt mangense oxide, lithium manganate, lithium iron phosphate, or a combination thereof, and the metal oxide includes iron oxide, vanadium oxide, or a combination thereof; The sulfide-based positive electrode active material is nickel sulfide, copper sulfide, Li 2 S., Li. 2 10. The all-solid-state secondary battery of claim 1 comprising an S-containing complex or a combination thereof.