Method for producing nonwoven fabric

By employing a fiber dispersion with a controlled concentration and sticky agent in papermaking, the method addresses pinhole issues in nonwoven fabrics, improving their performance in electrochemical devices.

JP2024138714AInactive Publication Date: 2024-10-09MITSUBISHI PAPER MILLS LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023049345
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Nonwoven fabrics made from beaten solvent-spun cellulose fibers often have pinholes, which reduce filtration accuracy and cause issues like increased leakage current and decreased withstand voltage in electrochemical devices.

Method used

A method for producing nonwoven fabrics using a fiber dispersion with a specific concentration range (0.02% to 0.06% by mass) of beaten solvent-spun cellulose, combined with a sticky agent, is used in papermaking with a paper machine to minimize pinholes.

Benefits of technology

The method results in nonwoven fabrics with fewer pinholes, enhancing filtration accuracy and reducing leakage current and improving withstand voltage in electrochemical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138714000001_ABST
    Figure 2024138714000001_ABST
Patent Text Reader

Abstract

To provide a method for producing a nonwoven fabric by which the nonwoven fabric having few pinholes can be obtained in the method for producing the nonwoven fabric obtained by papermaking a beaten solvent-spun cellulose fiber.SOLUTION: A method for producing a nonwoven fabric obtained by papermaking from beaten solvent-spun cellulose according to the present invention is characterized in that a fiber dispersion for papermaking containing beaten solvent-spun cellulose and having a fiber concentration of 0.02% by mass or more and 0.06% by mass or less is papermade by using a papermaking machine, and it is more preferable to produce a fiber dispersion for papermaking containing a viscosifier and having a fiber concentration of 0.03% by mass or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a nonwoven fabric. [Background technology]

[0002] Nonwoven fabrics made from beaten solvent-spun cellulose fibers have the characteristics of small pore size and high resistance to organic solvents, and are therefore used as filters, separators for electrochemical devices, etc. Examples of electrochemical devices include lithium ion batteries and electric double layer capacitors. Hereinafter, in the present invention, unless otherwise specified, "nonwoven fabric" refers to "nonwoven fabric made from beaten solvent-spun cellulose fibers."

[0003] When pinholes are present in a nonwoven fabric, the filtering accuracy of the filter may decrease, and substances that should be filtered out may be missed. In addition, in a separator for an electrochemical device, problems such as an increase in leakage current and a decrease in withstand voltage may occur. Therefore, it is preferable that the nonwoven fabric has as few pinholes as possible.

[0004] It has been disclosed that a separator for electrochemical elements that contains fibrillated solvent-spun cellulose fibers and non-fibrillated fibers and is characterized by containing non-fibrillated fibers having a fiber length of 0.2 mm or less can provide a separator for electrochemical elements that is less likely to develop pinholes even when made thin (see, for example, Patent Document 1). However, the separator for electrochemical elements in Patent Document 1 is subject to design constraints that require non-fibrillated fibers having a fiber length of 0.2 mm or less to be an essential component. In addition, depending on the application of the nonwoven fabric, there may be a problem in which non-fibrillated fibers having a fiber length of 0.2 mm or less fall off during use. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2021-158273 A Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a method for producing a nonwoven fabric by papermaking beaten solvent-spun cellulose fibers, which can produce a nonwoven fabric with few pinholes. [Means for solving the problem]

[0007] The above problems can be solved by the following means.

[0008] (1) A method for producing a nonwoven fabric by papermaking from beaten solvent-spun cellulose, comprising the steps of: papermaking a fiber dispersion containing beaten solvent-spun cellulose and having a fiber concentration of 0.02% by mass or more and 0.06% by mass or less, using a papermaking machine.

[0009] (2) A method for producing a nonwoven fabric according to the above (1), comprising the steps of: forming a paper from a fiber dispersion for papermaking, which contains a viscosifier and has a fiber concentration of 0.03% by mass or more, using a papermaking machine. Effect of the Invention

[0010] According to the method for producing a nonwoven fabric of the present invention, a nonwoven fabric having few pinholes can be obtained by forming a sheet from beaten solvent-spun cellulose fibers. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic diagram showing an example of a white water circulation system of an inclined wire papermaking machine. [Diagram 2] 1 is a graph showing the correlation between the fiber concentration of a fiber dispersion for papermaking and the number of pinholes in an example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention relates to a method for producing a nonwoven fabric by papermaking from beaten solvent-spun cellulose, the method being characterized in that a papermaking fiber dispersion containing beaten solvent-spun cellulose and having a fiber concentration of 0.02% by mass or more and 0.06% by mass or less is papermade in a papermaking machine.

[0013] By using a papermaking fiber dispersion containing beaten solvent-spun cellulose and having a fiber concentration of 0.02% by mass or more and 0.06% by mass or less to produce a nonwoven fabric, it is possible to obtain the excellent effect of producing a nonwoven fabric with fewer pinholes, compared to when the fiber concentration of the papermaking fiber dispersion is less than 0.02% by mass or more than 0.06% by mass.

[0014] In a method for producing a nonwoven fabric by using a papermaking fiber dispersion containing beaten solvent-spun cellulose in a papermaking machine, if the fiber concentration of the fiber dispersion is too low, the amount of water dehydrated from the fiber dispersion in the papermaking machine relative to the amount of fiber is large. In this case, the fibers are easily detached from the nonwoven fabric along with the dehydrated water, and pinholes are easily generated. On the other hand, if the fiber concentration of the fiber dispersion is too high, the dispersion of the fibers in the fiber dispersion becomes uneven, and the texture (fiber density) of the nonwoven fabric is easily uneven, and pinholes are easily generated in areas with low fiber density. In the present invention, the fiber concentration of the fiber dispersion is 0.02% by mass or more, more preferably 0.03% by mass or more, and even more preferably 0.04% by mass or more. The fiber concentration of the fiber dispersion is 0.06% by mass or less. By using a papermaking fiber dispersion having a fiber concentration of 0.02% by mass or more and 0.06% by mass or less to produce a nonwoven fabric with fewer pinholes than when the fiber concentration is less than 0.02% by mass or more than 0.06% by mass.

[0015] In the present invention, solvent-spun cellulose refers to regenerated cellulose fibers spun by discharging a solution of cellulose such as wood pulp or cotton pulp dissolved in a solvent mainly composed of an amine oxide such as N-methylmorpholine oxide, or an ionic liquid such as N,N-diethyl-N-(2-methoxyethyl)-N-methylammonium=2-methoxyacetic acid or 1-ethyl-3-methylimidazolium acetate from a fine nozzle into a poor solvent such as water. Compared with regenerated cellulose fibers produced by the viscose method or the cuprammonium method, solvent-spun cellulose is characterized by being easier to fibrillate by beating and by the fact that fine fibers can be obtained.

[0016] The beaten solvent-spun cellulose used in the present invention can be obtained in the form of a dispersion by treating an aqueous dispersion containing solvent-spun cellulose with a beating device. Examples of beating devices include beaters; refiners such as disc refiners and conical refiners. The treatment with a beating device is usually carried out by passing an aqueous dispersion containing 0.1% by mass to 6.0% by mass of solvent-spun cellulose fibers through the beating device. A raw material dispersion is obtained by adding fibers other than the beaten solvent-spun cellulose, chemicals, etc. to the beaten solvent-spun cellulose as necessary. The raw material dispersion is diluted to a fiber concentration of 0.02% by mass to 0.06% by mass to obtain the fiber dispersion for papermaking used in the present invention.

[0017] Specific examples of fibers other than beaten solvent-spun cellulose include unbeaten solvent-spun cellulose, plant-derived pulps such as wood pulp and cotton pulp, and synthetic fibers such as polyester fibers, acrylic fibers, nylon fibers, and aramid fibers. Examples of chemicals include chemicals for improving the handleability of the fiber dispersion for papermaking, such as thickeners, defoamers, and fiber dispersants. In the present invention, the fiber concentration of the fiber dispersion for papermaking means the mass fraction of the bone dry mass of all fibers, including beaten solvent-spun cellulose and fibers other than beaten solvent-spun cellulose, in the mass of the fiber dispersion for papermaking.

[0018] In the present invention, the fiber dispersion for papermaking refers to the fiber dispersion spread on the wire of the papermaking machine. In the present invention, the fiber concentration of the fiber dispersion for papermaking is low, at 0.02% by mass or more and 0.06% by mass or less, and there is a problem that a large storage tank is required to store the fiber dispersion for papermaking. In order to avoid this problem, it is common to prepare a raw material dispersion in which the raw materials such as fibers and chemicals constituting the nonwoven fabric are mixed and dispersed at a higher concentration than the fiber dispersion for papermaking, and then dilute it immediately before papermaking to use it as the fiber dispersion for papermaking. In addition, the surplus water removed from the fiber dispersion for papermaking in the papermaking machine is called white water. White water is usually recycled and reused, and the raw material dispersion is diluted with white water to obtain the fiber dispersion for papermaking. White water contains chemicals such as viscosifiers and defoamers among the components contained in the fiber dispersion for papermaking.

[0019] FIG. 1 is a schematic diagram showing an example of a white water circulation system of an inclined wire papermaking machine. The raw material dispersion is supplied from a raw material dispersion storage tank 3 by a raw material dispersion supply pump 5. The white water and raw material dispersion supplied from a white water circulation tank 2 by a white water circulation pump 4 are mixed and diluted to become a fiber dispersion for papermaking. A nonwoven fabric is formed from the fiber dispersion for papermaking supplied to an inclined wire papermaking machine 1. The white water removed from the fiber dispersion for papermaking through the wire of the inclined wire papermaking machine 1 returns to the white water circulation tank 2. The amount of white water in the white water circulation tank 2 is determined by the height of the overflow pipe 6. The part of the white water that exceeds the height of the overflow pipe 6 in the white water circulation tank 2 is discharged from the overflow pipe 6 to the outside of the white water circulation system. If necessary, the aqueous viscosity agent stored in the viscosity agent storage tank 7 is added to one of the white water, the raw material dispersion, and the fiber dispersion for papermaking by a viscosity agent supply pump 8. In FIG. 1, the viscosity agent is added at the point where the raw material dispersion and the white water are mixed. The fiber concentration of the fiber dispersion for papermaking is expressed as "fiber concentration of raw material dispersion × flow rate of raw material dispersion supply pump 5 / (flow rate of white water circulating pump 4 + flow rate of raw material dispersion supply pump 5 + flow rate of viscosity agent supply pump 8)".

[0020] The amount of fiber dispersion required to manufacture a unit area of ​​nonwoven fabric is inversely proportional to the fiber concentration of the fiber dispersion. Therefore, when a fiber dispersion with a low fiber concentration is used as in the present invention, a large amount of fiber dispersion must be used per unit area of ​​nonwoven fabric. Therefore, in the present invention, the papermaking machine is preferably an inclined wire papermaking machine or a cylinder papermaking machine, which is suitable for using a large amount of fiber dispersion per unit area of ​​nonwoven fabric. On the other hand, when a large amount of fiber dispersion is used per unit area of ​​nonwoven fabric in a Fourdrinier papermaking machine, the fiber dispersion overflows to the side of the wire, which is not suitable for the present invention.

[0021] The present invention uses a basis weight of 8 g / m 2 More than 20g / m 2 It is particularly useful for producing nonwoven fabrics with a basis weight of 8 g / m 2 When the technology of the present invention is used to produce a nonwoven fabric having a basis weight of less than 20 g / m, the number of pinholes can be reduced, but many pinholes may still remain. 2 When manufacturing nonwoven fabrics exceeding this limit, the occurrence of pinholes is low even without using the present invention, and there is little motivation to use the present invention.

[0022] In the present invention, the fiber dispersion for papermaking preferably contains a thickener. This is because the fiber dispersion for papermaking contains a thickener, which makes the texture of the nonwoven fabric more uniform and makes it less likely that pinholes will occur. The effect of containing a thickener is more pronounced when the fiber concentration of the fiber dispersion for papermaking is 0.03% by mass or more, and more pronounced when the fiber concentration is 0.04% by mass or more. A thickener is a water-soluble polymer with a high molecular weight that is added to the fiber dispersion for papermaking in order to suppress the dehydration rate and stabilize the dispersion state of the fibers in the wet papermaking method. In the present invention, polyethylene oxide or its copolymer, polyacrylamide or its copolymer, etc. are used as the thickener. It is preferable that the viscosity of a 0.5% by mass aqueous solution of the water-soluble polymer used as the thickener is 100 mPa seconds or more and 1000 mPa seconds or less, as measured by a Brookfield viscometer.

[0023] When the viscosity of a 0.5% by mass aqueous solution of the water-soluble polymer used as a viscous agent measured by a Brookfield viscometer is less than 100 mPa seconds, the amount of viscous agent required to prevent pinholes from occurring is large, which is uneconomical. When the viscosity of a 0.5% by mass aqueous solution of the water-soluble polymer used as a viscous agent measured by a Brookfield viscometer exceeds 1000 mPa seconds, the viscosity is likely to decrease when shear force is applied to the fiber dispersion for papermaking, and the effect of including the viscous agent may not be obtained stably. Although it depends on the viscosity of a 0.5% by mass aqueous solution of the water-soluble polymer used as a viscous agent measured by a Brookfield viscometer, in the present invention, the amount of the viscous agent added is preferably 0.01 ppm by mass or more and 0.1 ppm by mass or less with respect to the mass of the fiber dispersion for papermaking. When the amount of the viscous agent added is too small, it is difficult to obtain the effect of making the texture uniform. On the other hand, when the amount of the viscous agent added is too large, dehydration in the papermaking machine may be slowed down, and the production speed may be reduced. EXAMPLES

[0024] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0025] Beating of solvent-spun cellulose. 20 kg of solvent-spun cellulose was dispersed in 980 kg of water using a pulper, and then the dispersion was circulated and beaten in a circulation system having a conical refiner to obtain an aqueous dispersion of beaten solvent-spun cellulose with a concentration of 2.0% by mass.

[0026] Preparation of raw material dispersion To the aqueous dispersion of the beaten solvent-spun cellulose, 5.0 kg of polyester short-cut fiber having a fineness of 0.2 dtex and a fiber length of 3 mm was added, and the mixture was dispersed using a pulper. Water was then added to bring the total amount to 25,000 kg, thereby preparing a raw material dispersion having a fiber concentration of 0.10% by mass.

[0027] The fiber dispersion for papermaking obtained by diluting the raw material dispersion was papered using an inclined wire papermaking machine having a white water circulation system as shown in Figure 1, to produce nonwoven fabrics 1-1 to 1-8. The flow rate of the raw material dispersion supply pump 5 was 30 kg per minute, the papermaking width in the inclined wire papermaking machine 1 was 0.45 m, and the wire speed was 6 m per minute. The concentration of the fiber dispersion for papermaking was adjusted by changing the flow rate of the white water circulation pump 4.

[0028] Nonwoven fabrics 2-1 to 2-8 were produced in the same manner as nonwoven fabrics 1-1 to 1-8, except that 0.015 kg of a 0.1 mass% aqueous solution of polyacrylamide, which has a viscosity of 200 mPa seconds when dissolved in water at a concentration of 0.5 mass%, was added per minute through a viscous agent supply pump 8.

[0029] Pinhole count evaluation The number of places where a certain amount of light or more was transmitted within a certain area of ​​the nonwoven fabric was counted by the following method, and was taken as the number of pinholes. A flatbed scanner (Seiko Epson, device name: GT-X970) was used in transmission mode to scan at a resolution of 800 dpi, and the number of areas with a luminance gradation of 90 / 255 or more in the scanned image was analyzed using image analysis software (ImageJ, a public domain software developed by the National Institutes of Health, USA). The number of such areas was taken as the "number of pinholes."

[0030] The "pinhole reduction rate" is an index showing the extent to which the effect of including a thickener has been manifested. It is the ratio calculated by "(AB) / A x 100" by comparing the number of pinholes A when the papermaking fiber dispersion does not contain a thickener with the number of pinholes B when the papermaking fiber dispersion contains a thickener, at the same fiber concentration. A large "pinhole reduction rate" indicates that the effect of including a thickener has been significantly manifested.

[0031] Table 1 shows the flow rate of the white water circulation pump 4, the flow rate of the thickener supply pump 8, the fiber concentration of the papermaking fiber dispersion, the number of pinholes, and the "pinhole reduction rate" due to the inclusion of a thickener for each nonwoven fabric. The correlation between the fiber concentration in the papermaking fiber dispersion and the number of pinholes is shown in Figure 2. In Figure 2, "◯" indicates nonwoven fabrics 1-1 to 1-8, and "△" indicates nonwoven fabrics 2-1 to 2-8.

[0032] [Table 1]

[0033] As can be seen from Table 1 and Figure 2, in all of nonwoven fabrics 1-1 to 1-8 that do not contain a thickener in the papermaking fiber dispersion and nonwoven fabrics 2-1 to 2-8 that do contain a thickener in the papermaking fiber dispersion, the fiber concentration is 0.02 mass% or more and 0.06 mass% or less, and therefore the number of pinholes is smaller than when the fiber concentration in the papermaking fiber dispersion is less than 0.02 mass% and when the fiber concentration in the papermaking fiber dispersion is more than 0.06 mass%.

[0034] Among the nonwoven fabrics 1-1 to 1-8 that do not contain a thickener in the fiber dispersion for papermaking, the nonwoven fabrics 1-2 to 1-7, which have a fiber concentration of 0.02 mass% or more and 0.06 mass% or less, have fewer pinholes than the nonwoven fabric 1-1, which has a fiber concentration in the fiber dispersion for papermaking of less than 0.02 mass%, and the nonwoven fabric 1-8, which has a fiber concentration in the fiber dispersion for papermaking of more than 0.06 mass%.

[0035] Among the nonwoven fabrics 2-1 to 2-8 in which the fiber dispersion for papermaking contains a viscosity agent, the nonwoven fabrics 2-2 to 2-7 in which the fiber concentration of the fiber dispersion for papermaking is 0.02 mass% or more and 0.06 mass% or less have a smaller number of pinholes than the nonwoven fabric 2-1 in which the fiber concentration of the fiber dispersion for papermaking is less than 0.02 mass% and the nonwoven fabric 2-8 in which the fiber concentration of the fiber dispersion for papermaking exceeds 0.06 mass%.

[0036] The nonwoven fabrics 2-1 to 2-8 in which the papermaking fiber dispersion contains a thickener have fewer pinholes than the nonwoven fabrics 1-1 to 1-8 in which the papermaking fiber dispersion does not contain a thickener.

[0037] In the nonwoven fabrics 2-1 to 2-3 and 2-8 in which the fiber dispersion for papermaking contains a viscous agent and the fiber concentration of the fiber dispersion for papermaking is less than 0.03% by mass and more than 0.06% by mass, the reduction rate of pinholes was 13 to 18% when compared with the nonwoven fabrics 1-1 to 1-3 and 1-8 in which the fiber concentration was the same and the fiber dispersion for papermaking was made from a fiber dispersion for papermaking that did not contain a viscous agent. In the nonwoven fabrics 2-4 to 2-7 in which the fiber dispersion for papermaking contains a viscous agent and the fiber concentration of the fiber dispersion for papermaking is 0.03% by mass or more and 0.06% by mass or less, the reduction rate of pinholes was 28 to 90% when compared with the nonwoven fabrics 1-4 to 1-7 in which the fiber concentration was the same and the fiber dispersion for papermaking was made from a fiber dispersion for papermaking that did not contain a viscous agent. In the region in which the fiber concentration of the fiber dispersion for papermaking is 0.03% by mass or more and 0.06% by mass or less, the effect of the fiber dispersion for papermaking containing a viscous agent was significantly manifested. [Industrial Applicability]

[0038] The nonwoven fabric produced by the method for producing a nonwoven fabric of the present invention has few pinholes and can be used as a filter with high filtration accuracy, a separator for an electrochemical element with low leakage current, or a separator for an electrochemical element with high voltage resistance. [Explanation of symbols]

[0039] 1 Inclined Wire Paper Machine 2 White water circulation tank 3. Raw material dispersion storage tank 4 White water circulation pump 5. Raw material dispersion supply pump 6 Overflow pipe 7 Viscosity Storage Tank 8 Viscosity supply pump

Claims

1. A method for producing a nonwoven fabric by papermaking from beaten solvent-spun cellulose, comprising the steps of: forming a fiber dispersion for papermaking, which contains beaten solvent-spun cellulose and has a fiber concentration of 0.02% by mass or more and 0.06% by mass or less, into a paper using a papermaking machine.

2. 2. The method for producing a nonwoven fabric according to claim 1, wherein a fiber dispersion for papermaking containing a viscosifier and having a fiber concentration of 0.03% by mass or more is used to produce a paper using a papermaking machine.

Citation Information

Patent Citations

  • Separator for electrochemical element

    JP2021158273A