Electrode structure, secondary battery, battery pack, vehicle, and stationary power source
The electrode structure with a composite layer having specific particle size distributions in distinct regions addresses the challenge of water electrolysis and resistance in secondary batteries, enhancing their performance and safety by optimizing ion and solvent movement.
Patent Information
- Application Number
- JP2023049781
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Existing secondary batteries face challenges in simultaneously suppressing electrolysis of water due to side reactions and lowering resistance, particularly in aqueous electrolyte systems.
The electrode structure incorporates a composite layer with distinct first and second regions, where the first region has a specific distribution of inorganic particles with smaller average particle sizes, and the second region has larger particles, optimizing the path for solvent and lithium ion movement to prevent water electrolysis while enhancing conductivity.
This configuration effectively suppresses water electrolysis and reduces resistance, ensuring efficient operation of the secondary battery by balancing the movement of solvent and lithium ions, thereby improving the battery's performance and safety.
Smart Images

Figure 2024139015000001_ABST
Abstract
Description
[Technical field]
[0001] An embodiment of the present invention relates to an electrode structure, a secondary battery, a battery pack, a vehicle, and a stationary power source. [Background technology]
[0002] Non-aqueous electrolyte batteries such as secondary batteries are used as power sources in a wide range of fields. Non-aqueous electrolyte batteries come in a wide variety of forms, from small ones for various electronic devices to large ones for electric vehicles. Non-aqueous electrolyte batteries use non-aqueous electrolytes containing flammable substances such as ethylene carbonate, and therefore require safety measures.
[0003] As a secondary battery, development is also underway of an aqueous electrolyte battery that uses an aqueous electrolyte containing a non-flammable aqueous solvent instead of a non-aqueous electrolyte.
[0004] In the above-mentioned secondary battery, a challenge is to simultaneously suppress the electrolysis of water caused by a side reaction and reduce the resistance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2003-77463 A [Patent Document 2] JP 2003-77542 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide an electrode structure that has low resistance while suppressing the electrolysis of water that occurs as a side reaction. [Means for solving the problem]
[0007] According to an embodiment, there is provided an electrode structure for a secondary battery, which includes an electrode and a composite layer containing inorganic particles. The composite layer has a first region and a second region. The first region is present between the electrode and the second region. In the cumulative frequency distribution of inorganic particles having an average particle size of 3 μm or more in the composite layer with respect to the thickness direction of the composite layer, when the total number of inorganic particles having an average particle size of 3 μm or more is normalized to 100, the first region has a cumulative frequency of inorganic particles having an average particle size of 3 μm or more in the range of 0 or more and less than 25. The first region is 5% or more and 40% or less of the thickness of the composite layer from the interface between the electrode and the composite layer. In the cross-sectional SEM image of the composite layer, the average particle size R1 of the inorganic particles in the first region and the average particle size R2 of the inorganic particles in the second region satisfy the relationship of R1 < R2.
Brief Description of Drawings
[0008] [Figure 1] Cross-sectional view schematically showing the electrode structure according to the embodiment. [Diagram 2] Another cross-sectional view schematically showing the electrode structure according to the embodiment. [Diagram 3] Cross-sectional view schematically showing an example of the secondary battery according to the embodiment. [Figure 4] Cross-sectional view along the IV-IV line of the secondary battery shown in FIG. 3. [Diagram 5] Partially cutaway perspective view schematically showing another example of the secondary battery according to the embodiment. [Figure 6] Enlarged cross-sectional view of part B of the secondary battery shown in FIG. 5. [Figure 7] Perspective view schematically showing an example of the assembled battery according to the embodiment. [Figure 8] Perspective view schematically showing an example of the battery pack according to the embodiment. [Figure 9] Exploded perspective view schematically showing another example of the battery pack according to the embodiment. [Figure 10] Block diagram showing an example of the electrical circuit of the battery pack shown in FIG. 9. [Figure 11] Partially transparent view schematically showing an example of the vehicle according to the embodiment. [Figure 12]A block diagram showing an example of a system including a stationary power supply according to an embodiment.
Mode for Carrying Out the Invention
[0009] Hereinafter, embodiments will be described with reference to the drawings. In the following description, components that exhibit the same or similar functions are given the same reference numerals throughout all the drawings, and redundant descriptions are omitted. Note that each drawing is a schematic diagram for facilitating the description and understanding of the embodiment, and its shape, dimensions, ratio, etc. may differ from those of an actual device, but these can be appropriately designed and changed in consideration of the following description and known techniques.
[0010] [First Embodiment] The electrode structure for a secondary battery according to the first embodiment has an electrode and a composite layer containing inorganic particles. The composite layer has a first region and a second region. The first region exists between the electrode and the second region. In the cumulative frequency distribution of inorganic particles having an average particle size of 3 μm or more in the composite layer with respect to the thickness direction of the composite layer, when the total number of inorganic particles having an average particle size of 3 μm or more is normalized to 100, and the first region is in the range where the cumulative frequency of inorganic particles having an average particle size of 3 μm or more is 0 or more and less than 25, the first region is 5% or more and 40% or less of the thickness of the composite layer from the interface between the electrode and the composite layer. In the cross-sectional SEM image of the composite layer, the average particle size R1 of the inorganic particles in the first region and the average particle size R2 of the inorganic particles in the second region satisfy the relationship R1 < R2.
[0011] In the electrode structure having the above configuration, a composite layer that functions as a separator when incorporated into a secondary battery is formed on the electrode. By satisfying the relationship R1 < R2 between the average particle diameter R1 of the inorganic particles in the first region and the average particle diameter R2 of the inorganic particles in the second region in the composite layer, it is possible to reduce the resistance while suppressing the electrolysis of water accompanying side reactions. This is because, regarding the suppression of the electrolysis of water accompanying side reactions, since the average particle diameter of the inorganic particles in the second region is large, it is possible to suppress the inflow of water in the electrolyte into the active material-containing layer. Further, regarding the reduction of resistance, since the average particle diameter of the inorganic particles in the first region is small, it is possible to sufficiently accelerate the movement of Li ions at the interface between the composite layer and the active material-containing layer, and it is possible to lower the resistance acting on the aforementioned interface.
[0012] FIG. 1 is a cross-sectional view schematically showing an electrode structure according to an embodiment. The electrode structure 70 has an electrode 50 and a composite layer 60 containing inorganic particles. The electrode 50 has a current collector and an active material-containing layer, respectively, which will be described later and are not shown.
[0013] The composite layer 60 contains inorganic particles 60a. Further, the composite layer 60 further contains a resin 60b. Materials that can be used for the inorganic particles 60a and the resin 60b will be described later in the section (Composite layer).
[0014] The composite layer 60 has a first region and a second region. The first region exists between the electrode and the second region. Here, the first region and the second region will be described with reference to FIG. 2.
[0015] FIG. 2 is another cross-sectional view schematically showing an electrode structure according to an embodiment. In FIG. 2, the thickness of the composite layer 60 along the thickness direction of the electrode structure 70 is denoted as 60t.
[0016] Here, the first region and the second region are defined as follows. A cumulative frequency distribution of inorganic particles having an average particle size of 3 μm or more in the composite layer is plotted in the direction 60t, which is the thickness direction of the composite layer, and the total number of inorganic particles having an average particle size of 3 μm or more is normalized to 100. In this case, the range in which the cumulative frequency of inorganic particles is 0 to less than 25 in the thickness direction of the composite layer is defined as the first region, and the range in which the inorganic particles are present in the composite layer except for the first region, that is, the range of 25 to 100, is defined as the second region. Hereinafter, when there are zero inorganic particles having an average particle size of 3 μm or more in the composite layer, the entire composite layer is defined as the first region. The ratio of the thickness 61t of the first region or the thickness 62t of the second region to the thickness 60t of the composite layer is referred to as the thickness ratio [%] of the first region 61 and the thickness ratio [%] of the second region 62, respectively.
[0017] The thickness ratio of the first region 61, that is, the thickness 61t of the first region with respect to the composite layer thickness 60t, is preferably 5% or more and 40% or less. When the thickness ratio of the first region 61 is 40% or less, the thickness ratio of the second region 62 becomes high, and side reactions can be suppressed. This is because the thickness ratio of the second region, which contains a large amount of inorganic particles with an average particle size of 3 μm or more, is sufficiently larger than the thickness ratio of the first region 61. As described above, when the solvent molecules such as water in the electrolyte move toward the electrode 50, the movement path of the solvent molecules through the pores of the composite layer 60 becomes longer than the linear distance that the solvent molecules move in the thickness direction of the composite layer 60. At this time, the solvent molecules such as water, which are close in size to the pore diameter, move from the composite layer to the active material-containing layer at a slower rate than lithium, which has a smaller ionic radius, so that side reactions such as electrolysis of water in the electrode 50 can be suppressed.
[0018] In addition, the thickness ratio of the first region is 5% or more, so that the resistance can be reduced. That is, the path along which Li ions move is shorter in the first region 61 than in the second region. Therefore, the movement of Li ions can be sufficiently fast at the interface between the composite layer 60 and the active material-containing layer, and the resistance acting on the interface can be reduced. As for solvent molecules such as water, the path along which water in the electrolyte moves in the second region 62 is long, so that the inflow of the solvent molecules into the active material-containing layer in the first region can be suppressed. In addition, in the first region near the interface between the composite layer 60 and the active material-containing layer, the path along which Li ions move is shortened, and the resistance acting on the interface is reduced, so that the electrode structure and the battery can both suppress side reactions and reduce resistance. The thickness ratio of the first region 61 is more preferably 8% or more and 30% or less, and even more preferably 10% or more and 20% or less.
[0019] The thickness ratio of the first region to the second region is measured, for example, as follows.
[0020] <Measurement of thickness ratio between first and second regions> (Pretreatment of secondary batteries) First, the secondary battery is put into a discharged state, and then disassembled to extract an electrode group including a composite layer. In the case of an aqueous lithium ion battery, this disassembly may be performed in the air, but in the case of a lithium ion battery using a non-aqueous solvent, it is performed in a glove box under an inert gas atmosphere such as argon. The discharged state refers to a state in which the battery is discharged until the charge rate becomes 0%. In the case of an aqueous lithium ion battery, the removed electrode group is immersed in pure water for 3 minutes, and then dried at 100°C for 5 minutes. In the case of a lithium ion battery using a non-aqueous solvent, the removed electrode group is immersed in a solvent for 3 minutes, and then dried in a glove box under an inert gas atmosphere. The solvent used is, for example, diethyl carbonate.
[0021] (Cutting off the electrodes) Next, the electrode group is subjected to focused ion beam (FIB) processing, and the cut cross section is observed by a scanning electron microscope (SEM). Here, as the FIB device, for example, Hitachi's SMI3300SE or FEI's Strata 400s can be used. The electrode group is cut at a position that divides the main surface of the electrode group into six equal parts in the short side direction when viewed from above, and five cross sections are obtained.
[0022] (Observation of the cross section of the electrode structure) After obtaining a cross section of the electrode group by the above-mentioned FIB processing, a cross section of the electrode structure 70 consisting of the electrodes 50 and the composite layer 60 is observed by SEM. As an SEM device, for example, U8020 manufactured by Hitachi High-Technologies Corporation can be used. As an observation site by SEM, a region where the electrodes 50 and the composite layer 60 exist is selected, and an image of the cross section of the selected region is taken at a magnification such that the entire electrodes 50 and the composite layer 60 are included in the observation region.
[0023] (Binarization of SEM images) The obtained SEM image is subjected to a binarization process using ImageJ, with the median value of the brightness of the inorganic particles 60a and the brightness of the resin 60b in the composite layer 60 being set as a threshold value.
[0024] (Calculation of thickness ratio of first region and second region) For the binarized SEM image, after detecting spherical or substantially spherical particles with high brightness in the composite layer, the average particle diameter Rp [μm] of one particle, which is the arithmetic mean of the maximum value and the minimum value of the diameter in each particle, is obtained. By calculating the arithmetic mean of Rp for each of all the particles included in the first region 61, the average particle diameter of each particle can be calculated. In the composite layer, particles with an average particle diameter Rp of 3 μm or more are detected, and a cumulative frequency distribution of inorganic particles with an average particle diameter Rp of 3 μm or more in the composite layer 60 is drawn in the thickness direction from the interface between the electrode 50 and the composite layer 60 to the surface of the composite layer 60 facing the aforementioned interface. At this time, the total number of inorganic particles with an average particle diameter Rp of 3 μm or more is normalized to 100. At this time, with respect to the axial direction of the thickness 60t of the composite layer 60, a range where the cumulative frequency of inorganic particles is 0 or more and less than 25 is defined as the first region, and a range of 25 or more and 100 or less is defined as the second region. However, it is assumed that the first region includes the interface between the electrode and the composite layer. When the number of inorganic particles with an average particle diameter of 3 μm in the composite layer is 0, the entire composite layer is defined as the first region. The ratio of the thickness 61t of the first region 61 or the thickness 62t of the second region 62 to the thickness 60t of the composite layer is hereinafter referred to as the thickness ratio of the first region 61 and the thickness ratio of the second region 62 [%], respectively.
[0025] The operations from the above-mentioned (observation of the cross-section of the electrode structure) to (calculation of the ratio of the first region and the second region) are performed for each cross-section, and the arithmetic mean of the ratio of the thickness 61t of the first region 61 to the thickness 61t of the composite layer 60 obtained for each cross-section is calculated. In the following measurement, the range of the first region uses this arithmetic mean value.
[0026] Next, in the cross-sectional SEM image of the composite layer 60 provided in the electrode structure according to the present embodiment, the average particle diameter R1 of the inorganic particles 60b in the first region 61 and the average particle diameter R2 of the inorganic particles 60a in the second region 62 satisfy the relationship R1 < R2. Since R2 is larger than R1, the average particle diameter of the inorganic particles in the second region becomes larger, and as a result, the path through which water in the electrolyte moves in the second region becomes longer, so that side reaction suppression becomes possible.
[0027] The ratio R1 / R2 of the average particle diameter R1 to the average particle diameter R2 is preferably 0.01 or more and 0.8 or less. When R1 is 0.2 μm or more and 3 μm or less and R2 is 3 μm or more, as calculated in the measurement of the average particle diameter of the inorganic particles 60a described later, the reason why the ratio R1 / R2 is preferably 0.01 or more and 0.8 or less will be described below. When R1 and R2 are 0.2 μm or more and 3 μm or more, respectively, by the measurement method described later, and the ratio R1 / R2 is 0.8 or less, the average particle diameter of the second region becomes high when the first region is used as a reference. Therefore, the path through which water in the electrolyte moves in the second region becomes longer, and side reactions can be suppressed. On the other hand, when R1 and R2 are 0.2 μm or more and 3 μm or more, respectively, by the measurement method described later, and the ratio R1 / R2 is 0.01 or more, the average particle diameter of the second region is 20 times or less when the first region is used as a reference. This prevents the difference in the length of the migration paths of Li ions and water in the electrolyte between the first and second regions and the difference in the concentration distribution of Li ions and water molecules in the thickness direction of the composite layer from becoming too large, and reduces the concentration overvoltage generated in the composite layer, resulting in low resistance. R1 / R2 is more preferably 0.1 or more and 0.7 or less, and even more preferably 0.25 or more and 0.5 or less.
[0028] The average particle size of the inorganic particles 60a in the composite layer is measured, for example, as follows.
[0029] <Measurement of the average particle size of the inorganic particles 60a in the composite layer> The average particle size R1 [μm] of the inorganic particles 60a in the first region can be calculated by the following method.
[0030] First, the thickness ratio of the first region 61, which is a constant ratio calculated in the above-mentioned <Measurement of the thickness ratio of the first region and the second region>, is applied to each cross section imaged by SEM.
[0031] Next, in the first region 61 of the SEM image binarized by the method described above in (Binarization of SEM image), spherical or nearly spherical particles with high brightness are detected, and the average particle size Rp [μm] of each particle, which is the arithmetic mean of the maximum and minimum diameters of each particle, is calculated. This calculation of Rp is performed for all particles contained in the first region 61. The Rp of each of the obtained particles is arithmetically averaged to obtain the average particle size R of the inorganic particles 60a in the first region 61 in one SEM image. 1-1 The above-mentioned R 1-1 By taking the arithmetic mean, it is possible to obtain the average particle size R1 of the inorganic particles 60a in the first region 61. The calculation for the second region 62 is carried out in the same manner as for the first region 61 to obtain the average particle size R2.
[0032] Furthermore, the relationship between the numbers of inorganic particles in the first region 61 and the second region 62 of the composite layer 60 will be described.
[0033] In the composite layer 60, it is preferable that the number N1 of the inorganic particles 60a having an average particle size of 0.2 μm or more and 3 μm or less in the first region 61 and the number N2 of the inorganic particles 60a having an average particle size of 0.2 μm or more and 3 μm or less in the second region satisfy the relationship N1>N2. N2 being smaller than N1 suggests that the second region contains many particles having an average particle size of 3 μm or less, and in this case, the path along which water in the electrolyte moves in the second region becomes longer, making it possible to suppress side reactions.
[0034] In addition to the relationship between N1 and N2, the ratio N1 / N2 of the number N1 of inorganic particles 60a having an average particle size of 0.2 μm or more and 3 μm or less to the number N2 of inorganic particles 60a having an average particle size of 0.2 μm or more and 3 μm or less is preferably 1.1 or more and 5.0 or less. When the aforementioned ratio N1 / N2 is 1.1 or more, the number of particles having an average particle size of 3 μm or more in the second region is greater than that in the first region, so that the path through which water in the electrolyte moves in the second region becomes longer, thereby making it possible to suppress side reactions. When the aforementioned ratio N1 / N2 is 5.0 or less, the number of inorganic particles having an average particle size of 0.2 μm or more and 3 μm or less in the second region is 5 times or less based on the first region. As a result, the difference in the length of the movement path of Li ions and water in the electrolyte generated in the thickness direction of the composite layer and the concentration distribution of Li are not too strong, and the concentration overvoltage generated in the composite layer is reduced, resulting in low resistance. The ratio N1 / N2 is more preferably in the range of 1.1 to 4.0, and even more preferably in the range of 1.5 to 3.0.
[0035] The numbers N1 and N2 of the inorganic particles 60a having an average particle size of 0.2 μm or more and 3 μm or less in the first region 61 and the second region 62 can be measured, for example, from a cross-sectional SEM image of the electrode structure 70 described above.
[0036] <Measurement of the number of inorganic particles N1 and N2> First, the thickness ratio of the first region 61, which is a constant ratio calculated in the above-mentioned <Measurement of the thickness ratio of the first region and the second region>, is applied to each cross section imaged by SEM.
[0037] Based on the <Measurement of the average particle size of the inorganic particles 60a in the composite layer>, the number of particles having an Rp of 0.2 μm or more and 3 μm or less is calculated from the Rp of each of all particles detected in the composite layer in the first region 61 and the second region 62 separately. The number of the above-mentioned particles in the first region 61 is N 1-1 Let the number of the above-mentioned particles in the second region 62 be N 2-1 This N calculated for each SEM image 1-1 and N 2-1 By taking the arithmetic mean of each of these, the desired numbers N1 and N2 can be calculated.
[0038] Furthermore, the average pore diameters in the first region 61 and the second region 62 of the composite layer 60 will be described.
[0039] It is preferable that the average pore diameter P1 in the first region 61 and the average pore diameter P2 in the second region 62 satisfy the relationship P1>P2. When P2 is smaller than P1, the size of the pores in the second region is narrowed when the solvent molecules such as water in the electrolyte move toward the electrode 50, and the movement of water molecules having a size similar to that of the pores is suppressed, thereby making it possible to suppress side reactions.
[0040] In addition to the above relationship between P1 and P2, the ratio P1 / P2 of the average particle diameter P1 to the average pore diameter P2 is preferably 1.01 or more and 2.0 or less. When the above ratio P1 / P2 is 1.01 or more, it is possible to narrow the size of the pores in the second region when the first region is used as a reference, and it is considered that the movement of water molecules having a size similar to that of the pores is suppressed, thereby making it possible to suppress side reactions. On the other hand, when the above ratio P1 / P2 is 2.0 or less, the difference in the length of the movement path of Li ions and water in the electrolyte generated in the thickness direction of the composite layer and the concentration distribution of Li are not too strong, and the concentration overvoltage generated in the composite layer is reduced, resulting in low resistance. The preferable range of the ratio P1 / P2 is 1.05 or more and 1.5 or less, and more preferably 1.1 or more and 1.2 or less.
[0041] The average pore diameters P1 and P2 in the first region 61 and the second region 62 can be measured, for example, from a cross-sectional SEM image of the electrode structure 70 described above.
[0042] <Measurement of pore diameters P1 and P2 contained in the first and second regions> First, the thickness ratio of the first region 61, which is a constant ratio calculated in the above-mentioned <Measurement of the thickness ratio of the first region and the second region>, is applied to each cross section imaged by SEM.
[0043] The SEM image described in (Observation of Cross Section of Electrode Structure) of <Measurement of Thickness Ratio of First Region and Second Region> is used. This SEM image is binarized using the median brightness between the brightness of the resin and the brightness of the interface between the composite layer 60 and the active material-containing layer as a threshold value, so that the solid particles and binder appear white and the voids appear black. After extracting the black voids from the first region 61 of the obtained image, the pore diameter in the voids is calculated by the sphere arrangement method. That is, multiple virtual spheres are fitted to the voids under the constraint that the diameter of each sphere is maximized, and the arithmetic average of the diameters of each sphere is taken as the pore diameter P. 1-1 The pore diameter P 1-1 is calculated for each SEM image, and the arithmetic average is taken as the desired pore diameter P1. The above calculation is also applied to the second region to calculate the pore volume P2 in the second region.
[0044] The porosity of the composite layer 60 is 0.10% or more and 4.0% or less. When the porosity of the composite layer 60 is 4.0% or less, the composite layer 60 becomes dense, the movement of solvent molecules such as water moving through the composite layer becomes slow, and the side reaction of electrolysis of water can be suppressed. Furthermore, when the porosity of the composite layer 60 is 0.10% or more, the movement of solvent molecules such as water moving through the composite layer becomes sufficiently fast, resulting in low resistance. The porosity of the composite layer 60 is preferably 0.20% or more and 2.0% or less. Also, more preferably, it is 0.60% or more and 1.0% or less.
[0045] The porosity of the composite layer 60 can be measured, for example, as follows.
[0046] <Porosity measurement> First, the thickness ratio of the first region 61, which is a constant ratio calculated in the above-mentioned <Measurement of the thickness ratio of the first region and the second region>, is applied to each cross section imaged by SEM.
[0047] The SEM image described in (Observation of Cross Section of Electrode Structure) of <Measurement of Thickness Ratio of First Region and Second Region> is used. This SEM image is binarized using a threshold value between the brightness of the resin and the brightness of the interface between the composite layer 60 and the active material-containing layer, so that the solid particles and binder are displayed in white and the voids are displayed in black. The ratio of the number of black pixels corresponding to the voids to the total number of pixels in the SEM image is calculated, and the result is calculated as the void ratio.
[0048] The electrode structure according to the embodiment will be described in detail below.
[0049] (electrode) The electrode has a current collector and an active material-containing layer supported on one or both sides of the current collector and containing an active material and, if necessary, a conductive agent and a binder. The electrode included in the electrode structure of this embodiment can function as either a positive electrode or a negative electrode. The electrode included in the electrode structure of this embodiment preferably functions as a negative electrode. In this section, the case where the electrode functions as a negative electrode will be described.
[0050] The current collector is preferably made of, for example, copper, nickel, stainless steel, aluminum, or an aluminum alloy containing one or more elements selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The thickness of the current collector is preferably 5 μm or more and 20 μm or less. A current collector having such a thickness can balance the strength and weight of the electrode.
[0051] The current collector may include a portion on its surface where the active material-containing layer is not provided. This portion may function as a current collecting tab. Alternatively, a current collecting tab separate from the current collector may be electrically connected to the negative electrode or the positive electrode. When active material-containing layers are disposed on both main surfaces of the current collector, at least a portion of one main surface of the current collector may include a portion that is not in contact with the active material-containing layer. For example, a current collecting tab separate from the current collector may be connected to this portion.
[0052] The active material-containing layer contains an active material and, if necessary, a conductive agent and a binder. The active material-containing layer contains, as the active material, a lithium ion insertion-extraction potential of 1 V to 3 V relative to the oxidation-reduction potential of lithium (vs. Li / Li + It is preferable that the negative electrode active material contains a compound having the formula:
[0053] In an aqueous electrolyte battery having a negative electrode containing a compound in the negative electrode active material whose lithium ion insertion-extraction potential is within the above range, water contained in the solvent of the aqueous electrolyte may be electrolyzed inside and near the negative electrode during the initial charge. This is because the potential of the negative electrode decreases due to lithium ions being inserted into the negative electrode active material during the initial charge. When the negative electrode potential decreases below the hydrogen generation potential, some of the water inside and near the negative electrode is converted into hydrogen (H2) and hydroxide ions (OH - This causes the pH of the aqueous electrolyte inside and near the negative electrode to increase.
[0054] The hydrogen generation potential at the negative electrode depends on the pH of the aqueous electrolyte. In other words, as the pH of the aqueous electrolyte in contact with the negative electrode increases, the hydrogen generation potential at the negative electrode decreases. + In a battery using a negative electrode active material such as ), the potential of the negative electrode is lower than the hydrogen generation potential during the initial charge, but after the initial charge, the potential of the negative electrode tends to become higher than the hydrogen generation potential, making it difficult for water decomposition to occur at the negative electrode.
[0055] The lithium ion insertion-extraction potential is a potential based on the oxidation-reduction potential of lithium, and is between 1V and 3V (vs. Li / Li + ) include, for example, titanium oxide and titanium-containing oxide. Examples of titanium-containing oxide include lithium titanium composite oxide, niobium titanium composite oxide, and sodium niobium titanium composite oxide. The negative electrode active material may contain one or more of titanium oxide and titanium-containing oxide.
[0056] Titanium oxides include, for example, titanium oxides with a monoclinic structure, rutile structure titanium oxides, and anatase structure titanium oxides. The titanium oxides of each crystal structure have a composition before charging of TiO2 and a composition after charging of Li y TiO2 (where the subscript y satisfies 0 ≦ y ≦ 1). Also, the structure of the titanium oxide with a monoclinic structure before charging can be represented as TiO2(B).
[0057] Lithium titanium oxides include, for example, lithium titanium oxides with a spinel structure (e.g., a compound represented by the general formula Li 4+x Ti5O 12 where -1 ≦ x ≦ 3), lithium titanium oxides with a lamellarite structure (e.g., a compound represented by Li 2+x Ti3O7 where -1 ≦ x ≦ 3), a compound represented by Li 1+y Ti2O4 where 0 ≦ y ≦ 1, a compound represented by Li 1.1+y Ti 1.8 O4 where 0 ≦ y ≦ 1, a compound represented by Li 1.07+y Ti 1.86 O4 where 0 ≦ y ≦ 1, a compound represented by Li z TiO2 where 0 < z ≦ 1, etc. Also, the lithium titanium oxide may be a lithium titanium composite oxide into which a different element has been introduced.
[0058] Niobium titanium composite oxides include, for example, Li a TiMe b Nb 2±c O 7±σ where 0 ≦ a ≦ 5, 0 ≦ b 0.3, 0 ≦ c ≦ 0.3, 0 ≦ σ ≦ 0.3, and Me is one or more selected from the group consisting of Fe, V, Mo, and Ta.
[0059] Sodium niobium titanium composite oxides include, for example, the general formula Li 2+d Na 2-e Me1 f Ti 6-g-h Nb g Me2 h O 14+δIt is represented by 0≦d≦4, 0≦e<2, 0≦f<2, 0<g<6, 0≦h<3, g + h<6, -0.5≦δ≦0.5, Me1 contains one or more selected from Cs, K, Sr, Ba, Ca, and Me2 contains one or more selected from Zr, Sn, V, Ta, Mo, W, Fe, Co, Mn, Al, and includes an orthorhombic type Na-containing niobium titanium composite oxide.
[0060] As the negative electrode active material, it is preferable to use titanium oxide with anatase structure, titanium oxide with monoclinic structure, lithium titanium oxide with spinel structure, niobium titanium composite oxide, or a mixture thereof. On the one hand, when using titanium oxide with anatase structure, titanium oxide with monoclinic structure, or lithium titanium oxide with spinel structure as the negative electrode active material, for example, by combining with a positive electrode using lithium manganese composite oxide as the positive electrode active material, a high electromotive force can be obtained. On the other hand, by using niobium titanium composite oxide, high capacity can be exhibited.
[0061] The negative electrode active material can be contained in the active material-containing layer in the form of particles, for example. The negative electrode active material particles can be primary particles, secondary particles that are aggregates of primary particles, or a mixture of single primary particles and secondary particles. The shape of the particles is not particularly limited and can be, for example, spherical, elliptical, flat, and fibrous.
[0062] The secondary particles of the negative electrode active material can be obtained, for example, by the following method. First, the active material raw material is reactively synthesized to produce an active material precursor with an average particle diameter of 1 μm or less. Then, the active material precursor is subjected to a firing treatment and a grinding treatment using a grinder such as a ball mill or a jet mill. Next, in the firing treatment, the active material precursor is aggregated to grow into secondary particles with a large particle diameter.
[0063] The average particle diameter (diameter) of the secondary particles of the negative electrode active material is preferably 3 μm or more, and more preferably 5 μm or more and 20 μm or less. In this range, since the surface area of the active material is small, the decomposition of water can be more suppressed.
[0064] The average particle size of the primary particles of the negative electrode active material is preferably 1 μm or less. This shortens the diffusion distance of Li ions inside the active material and increases the specific surface area. Therefore, excellent high input performance (fast charging) can be obtained. On the other hand, if the average particle size of the primary particles of the negative electrode active material is small, the particles are more likely to aggregate. If the particles of the negative electrode active material aggregate, the aqueous electrolyte in the secondary battery is more likely to be unevenly distributed at the negative electrode, which may lead to a depletion of ion species at the counter electrode. Therefore, the average particle size of the primary particles of the negative electrode active material is preferably 0.001 μm or more. It is more preferable that the average particle size of the primary particles of the negative electrode active material is 0.1 μm or more and 0.8 μm or less.
[0065] The primary particle size and secondary particle size refer to the particle size at which the volume cumulative value is 50% in the particle size distribution obtained by a laser diffraction particle size distribution measuring device. For example, Shimadzu SALD-300 is used as the laser diffraction particle size distribution measuring device. The light intensity distribution is measured 64 times at 2-second intervals. The sample used for this particle size distribution measurement is a dispersion diluted with N-methyl-2-pyrrolidone so that the concentration of active material particles is 0.1% to 1% by mass. Alternatively, the measurement sample is one in which 0.1 g of active material is dispersed in 1 ml to 2 ml of distilled water containing a surfactant.
[0066] The negative electrode active material has a specific surface area of, for example, 3 m2 as measured by the BET method using nitrogen (N2) adsorption. 2 / g or more 200m 2 When the specific surface area of the negative electrode active material is within this range, the affinity between the negative electrode and the aqueous electrolyte can be further increased.
[0067] The specific surface area of the negative electrode active material-containing layer measured by the BET method using nitrogen (N2) adsorption is 3m 2 / g or more 50m 2 / g or less. 2When the specific surface area of the negative electrode active material-containing layer is 50 m / g or more, the affinity between the negative electrode active material and the aqueous electrolyte is good. As a result, the interface resistance of the negative electrode is suppressed, and the output performance and charge / discharge cycle performance of the secondary battery can be maintained at a high level. 2 / g or less, the distribution of ion species ionized from the electrolyte salt contained in the aqueous electrolyte is not biased toward the negative electrode, and a shortage of the ion species in the positive electrode can be prevented, thereby maintaining high output performance and charge / discharge cycle performance.
[0068] The specific surface area can be determined, for example, by the following method. When an electrode including the active material-containing layer to be measured is incorporated in a secondary battery, the secondary battery is disassembled and a part of the active material-containing layer is sampled. In nitrogen gas at 77K (the boiling point of nitrogen), the nitrogen gas pressure P (mmHg) is gradually increased while measuring the nitrogen gas adsorption amount (mL / g) of the sample for each pressure P. The pressure P (mmHg) is divided by the saturated vapor pressure P0 (mmHg) of nitrogen gas to obtain a relative pressure P / P0, and the nitrogen gas adsorption amount for each relative pressure P / P0 is plotted to obtain an adsorption isotherm. A BET plot is calculated from this nitrogen adsorption isotherm and the BET formula, and the specific surface area is obtained using this BET plot. The BET multipoint method is used to calculate the BET plot.
[0069] The conductive agent is mixed as necessary to improve the current collecting performance and suppress the contact resistance between the negative electrode active material and the current collector. Examples of the conductive agent include carbonaceous materials such as acetylene black, ketjen black, graphite, and coke. The conductive agent may be one type or a mixture of two or more types.
[0070] The binder has a function of binding the negative electrode active material and the conductive agent. As the binder, for example, at least one selected from the group consisting of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), cellulose-based polymers such as carboxymethyl cellulose (CMC), fluorine-based rubber, styrene butadiene rubber, acrylic resin or its copolymer, polyacrylic acid, and polyacrylonitrile can be used, but is not limited thereto.
[0071] The mixing ratios of the negative electrode active material, conductive agent, and binder in the negative electrode active material-containing layer are preferably in the ranges of 70% by mass or more and 95% by mass or less, 3% by mass or more and 20% by mass or less, and 2% by mass or more and 10% by mass or less, respectively. When the mixing ratio of the conductive agent is 3% by mass or more, the conductivity of the active material-containing layer can be improved, and when it is 20% by mass or less, the decomposition of the aqueous electrolyte on the conductive agent surface can be reduced. When the mixing ratio of the binder is 2% by mass or more, sufficient electrode strength can be obtained. Since the binder is a material that exhibits electrical insulation, when the mixing ratio is 10% by mass or less, the insulating part in the electrode can be reduced.
[0072] (electrolyte) The electrode structure may further include an electrolyte. The electrolyte may be an aqueous electrolyte or a non-aqueous electrolyte. Examples of the aqueous electrolyte and the non-aqueous electrolyte that can be used are described below.
[0073] First, the aqueous electrolyte includes an aqueous solvent and an electrolyte salt. The aqueous electrolyte is, for example, liquid. The liquid aqueous electrolyte is an aqueous solution prepared by dissolving an electrolyte salt as a solute in an aqueous solvent. When the aqueous electrolyte is held in both the negative electrode active material-containing layer and the positive electrode active material-containing layer, the types of the aqueous electrolytes may be the same or different.
[0074] The aqueous solution preferably contains 1 mol or more of the aqueous solvent per mol of the salt as the solute, and more preferably 3.5 mol or more.
[0075] As the aqueous solvent, a solution containing water can be used. The aqueous solution may be pure water or a mixed solvent of water and an organic solvent. The aqueous solvent contains water at a ratio of, for example, 50% by volume or more.
[0076] Whether an electrolyte contains water can be confirmed by GC-MS (Gas Chromatography - Mass Spectrometry) measurement. In addition, the salt concentration and water content in an electrolyte can be calculated, for example, by ICP (Inductively Coupled Plasma) emission spectrometry. The molar concentration (mol / L) can be calculated by weighing a specified amount of electrolyte and calculating the salt concentration contained therein. In addition, the number of moles of solute and solvent can be calculated by measuring the specific gravity of the electrolyte.
[0077] The aqueous electrolyte may be a gel electrolyte. The gel electrolyte is prepared by mixing the above-mentioned liquid aqueous electrolyte with a polymer compound to form a composite. Examples of the polymer compound include PVdF, polyacrylonitrile (PAN), and polyethylene oxide (PEO).
[0078] The electrolyte salt may be, for example, a lithium salt, a sodium salt, or a mixture thereof. One or more kinds of electrolyte salts may be used.
[0079] Examples of lithium salts that can be used include lithium chloride (LiCl), lithium bromide (LiBr), lithium hydroxide (LiOH), lithium sulfate (Li2SO4), lithium nitrate (LiNO3), lithium acetate (CH3COOLi), lithium oxalate (Li2C2O4), lithium carbonate (Li2CO3), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI; LiN(SO2CF3)2), lithium bis(fluorosulfonyl)imide (LiFSI; LiN(SO2F)2), and lithium bisoxalate borate (LiBOB: LiB[(OCO)2]2).
[0080] The lithium salt preferably contains LiCl. The use of LiCl can increase the lithium ion concentration of the aqueous electrolyte. The lithium salt preferably contains at least one of LiSO4 and LiOH in addition to LiCl.
[0081] As the sodium salt, sodium chloride (NaCl), sodium sulfate (Na2SO4), sodium hydroxide (NaOH), sodium nitrate (NaNO3), sodium trifluoromethanesulfonylamide (NaTFSA), and the like can be used.
[0082] The molar concentration of alkali metal ions (e.g., lithium ions) in the aqueous electrolyte may be 3 mol / L or more, 6 mol / L or more, or 12 mol / L or more. In one example, the molar concentration of alkali metal ions in the aqueous electrolyte is 14 mol / L or less. If the concentration of alkali metal ions in the aqueous electrolyte is high, the electrolysis of water, which is a side reaction at the negative electrode, is likely to be suppressed, and hydrogen generation from the negative electrode tends to be small.
[0083] Aqueous electrolytes contain chloride ions (Cl - ), hydroxide ion (OH - ), sulfate ion (SO4 2- ), nitrate ion (NO 3- ) is preferably contained.
[0084] The pH of the aqueous electrolyte is preferably 3 or more and 14 or less, and more preferably 4 or more and 13 or less. When separate electrolytes are used for the negative electrode side electrolyte and the positive electrode side electrolyte, the pH of the negative electrode side electrolyte is preferably in the range of 3 or more and 14 or less, and the pH of the positive electrode side electrolyte is preferably in the range of 1 or more and 8 or less.
[0085] When the pH of the negative electrode electrolyte is within the above range, the hydrogen generation potential at the negative electrode is reduced, and hydrogen generation at the negative electrode is suppressed. This improves the storage performance and cycle life performance of the battery. When the pH of the positive electrode electrolyte is within the above range, the oxygen generation potential at the positive electrode is increased, and oxygen generation at the positive electrode is reduced. This improves the storage performance and cycle life performance of the battery. It is more preferable that the pH of the positive electrode electrolyte is within the range of 3 to 7.5.
[0086] The aqueous electrolyte may contain a surfactant. Examples of the surfactant include nonionic surfactants such as polyoxyalkylene alkyl ether, polyethylene glycol, polyvinyl alcohol, thiourea, disodium 3,3'-dithiobis(1-propanephosphoric acid), dimercaptothiadiazole, boric acid, oxalic acid, malonic acid, saccharin, sodium naphthalenesulfonate, gelatin, potassium nitrate, aromatic aldehyde, and heterocyclic aldehyde. The surfactant may be used alone or in combination of two or more.
[0087] The pH of the aqueous electrolyte is preferably different between the negative electrode side and the positive electrode side after the initial charge. In the secondary battery after the initial charge, the pH of the first aqueous electrolyte on the negative electrode side is preferably 3 or more, more preferably 5 or more, and even more preferably 7 or more. In addition, in the secondary battery after the initial charge, the pH of the third aqueous electrolyte on the positive electrode side is preferably in the range of 0 to 7, and more preferably 0 to 6.
[0088] The pH of the aqueous electrolyte on the negative electrode side and the aqueous electrolyte on the positive electrode side can be obtained, for example, by disassembling the secondary battery and measuring the pH of the aqueous electrolyte present between the composite layer and the negative electrode and the positive electrode.
[0089] As the electrolyte, in addition to the aqueous electrolyte, a liquid non-aqueous electrolyte or a gel non-aqueous electrolyte can be used. The liquid non-aqueous electrolyte is prepared by dissolving an electrolyte salt as a solute in an organic solvent.
[0090] Examples of electrolyte salts include lithium perchlorate (LiClO), lithium hexafluorophosphate (LiPF), lithium tetrafluoroborate (LiBF), lithium hexafluoride (LiAsF), lithium trifluoromethanesulfonate (LiCFSO), and lithium salts such as lithium bistrifluoromethylsulfonylimide (LiN(CFSO)), lithium bis(fluorosulfonyl)imide (LiN(SOF); LiFSI), and mixtures thereof.
[0091] Examples of organic solvents include cyclic carbonates such as propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC); chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (MEC); cyclic ethers such as tetrahydrofuran (THF), 2-methyl tetrahydrofuran (2MeTHF), and dioxolane (DOX); chain ethers such as dimethoxyethane (DME) and diethoxyethane (DEE); γ-butyrolactone (GBL), acetonitrile (AN), and sulfolane (SL). These organic solvents can be used alone or as a mixed solvent.
[0092] The gelled non-aqueous electrolyte is prepared by combining a liquid non-aqueous electrolyte with a polymeric material, examples of which include PVdF, PAN, PEO, or mixtures thereof.
[0093] Alternatively, as the nonaqueous electrolyte, in addition to liquid nonaqueous electrolytes and gel nonaqueous electrolytes, room temperature molten salts containing lithium ions (ionic melts), polymer solid electrolytes, inorganic solid electrolytes, and the like may be used.
[0094] Room temperature molten salts (ionic melts) refer to organic salts consisting of a combination of organic cations and anions that can exist as a liquid at room temperature (15°C or higher and 25°C or lower). Room temperature molten salts include room temperature molten salts that exist as a liquid by themselves, room temperature molten salts that become liquid when mixed with an electrolyte salt, room temperature molten salts that become liquid when dissolved in an organic solvent, and mixtures of these. In general, the melting point of room temperature molten salts used in secondary batteries is 25°C or lower. In addition, organic cations generally have a quaternary ammonium skeleton.
[0095] (composite layer) The composite layer is provided on the active material-containing layer, and in a secondary battery including the electrode structure according to the present embodiment described later, it is present between the positive electrode and the negative electrode and functions as a separator. For example, in an electrode in which active material-containing layers are supported on both sides of a current collector, the composite layer may be provided on the main surface of one of the active material-containing layers, or may be provided on the main surfaces of both active material-containing layers.
[0096] The composite layer contains inorganic particles. Examples of inorganic particles contained in the composite layer include oxide ceramics such as alumina, silica, zirconia, yttria, magnesium oxide, calcium oxide, barium oxide, strontium oxide, and vanadium oxide, carbonates and sulfates such as sodium carbonate, potassium carbonate, magnesium carbonate, calcium carbonate, barium carbonate, lanthanum carbonate, cerium carbonate, calcium sulfate, magnesium sulfate, aluminum sulfate, gypsum, and barium sulfate, phosphates such as hydroxyapatite, lithium phosphate, zirconium phosphate, and titanium phosphate, and nitride ceramics such as silicon nitride, titanium nitride, and boron nitride. The inorganic particles listed above may be in the form of a hydrate.
[0097] The inorganic particles preferably include solid electrolyte particles having ionic conductivity for alkali metal ions, and more preferably inorganic solid particles having ionic conductivity for lithium ions and sodium ions.
[0098] Examples of inorganic solid particles having lithium ion conductivity include oxide-based solid electrolytes and sulfide-based solid electrolytes. Oxide-based solid electrolytes have a NASICON (Sodium (Na) Super Ionic Conductor) type structure and are represented by the general formula Li 1+u It is preferable to use a lithium phosphate solid electrolyte represented by M2(PO4)3. In the above general formula, M is, for example, one or more selected from the group consisting of titanium (Ti), germanium (Ge), strontium (Sr), zirconium (Zr), tin (Sn), aluminum (Al), and calcium (Ca). The subscript x is in the range of 0≦u≦2. The ionic conductivity of the lithium phosphate solid electrolyte represented by the general formula LiM2(PO4)3 is, for example, 1×10 -5 S / cm or more 1×10 -3 S / cm or less.
[0099] A specific example of a lithium phosphate solid electrolyte having a NASICON structure is Li 1+v Al v Ti 2-v LATP compound represented by (PO4)3 and having a v of 0.1≦v≦0.5; Li 1+y AlwM1 2-w A compound represented by the formula (PO4)3, in which M1 is one or more selected from the group consisting of Ti, Ge, Sr, Zr, Sn, and Ca, and 0≦y≦1 and 0≦w≦1; Li 1+u Al u Ge 2-u (PO4)3, where 0≦u≦2; and Li 1+u Al u Zr 2-u Compounds represented by the formula (PO4)3, where 0≦u≦2; Li 1+p+q Al p Mα 2-p S q P 3-q O12 A compound represented by Mα is one or more selected from the group consisting of Ti and Ge, 0 < p ≤ 2, 0 ≤ q < 3; Li 1+2m Zr1Ca m Compounds represented by (PO4)3 where 0 ≤ m < 1 can be mentioned. Li 1+2m Zr 1-m Ca m (PO4)3 has high water resistance, low reducibility and low cost, and is preferably used as inorganic solid electrolyte particles.
[0100] In addition to the above lithium phosphate solid electrolyte, as the oxide-based solid electrolyte, Li r PO s N t An amorphous LIPON compound represented by 2.6 ≤ r ≤ 3.5, 1.9 ≤ s ≤ 3.8, and 0.1 ≤ t ≤ 1.3 (for example, Li 2.9 PO 3.3 N 0.46 ); Garnet-type structure La 5+l A l La 3-l Mβ2O 12 A compound represented by A is one or more selected from the group consisting of Ca, Sr, and Ba, Mβ is one or more selected from the group consisting of Nb and Ta, and 0 ≤ l ≤ 0.5; Li3Mγ 2-l L2O 12 A compound represented by Mγ is one or more selected from the group consisting of Ta and Nb, L may contain Zr, and 0 ≤ l ≤ 0.5; Li 7-3l Al l La3Zr3O 12 A compound represented by 0 ≤ l ≤ 0.5; Li 5+u La3M2 2-u Zr u O 12 A compound represented by M2 is one or more selected from the group consisting of Nb and Ta, and 0 ≤ u ≤ 2, LLZ compound (for example, Li7La3Zr2O 12 ); And having a perovskite-type structure La 2 / 3-χ Li χThe solid electrolyte may be one type or a mixture of two or more types. The ionic conductivity of LIPON is, for example, 1×10 -6 S / cm or more 5×10 -6 The ionic conductivity of LLZ is, for example, 1×10 -4 S / cm or more 5×10 -4 S / cm or less.
[0101] In addition, a sodium-containing solid electrolyte may be used as the inorganic solid particles having ion conductivity of sodium ions. The sodium-containing solid electrolyte has excellent ion conductivity of sodium ions. Examples of the sodium-containing solid electrolyte include sodium phosphorus sulfide and sodium phosphorus oxide. The sodium-ion-containing solid electrolyte is preferably in the form of glass ceramics.
[0102] Inorganic solid particles have a density of 1×10 at 25°C. -5 It is preferable that the solid electrolyte has a lithium ion conductivity of S / cm or more.
[0103] The shape of the inorganic solid particles is not particularly limited, but may be, for example, spherical, elliptical, flat, or fibrous.
[0104] The inorganic solid particles preferably have an average particle size of 15 μm or less, more preferably 12 μm or less. If the inorganic solid particles have a small average particle size, the denseness of the composite layer can be increased.
[0105] The inorganic solid particles preferably have an average particle size of 0.01 μm or more, more preferably 0.1 μm or more. If the inorganic solid particles have a large average particle size, aggregation of the particles tends to be suppressed.
[0106] In the composite layer, inorganic solid particles are preferably the main component. From the viewpoint of increasing the ion conductivity of the composite layer, the proportion of inorganic solid particles in the composite layer is preferably 70 mass % or more, more preferably 80 mass % or more, and even more preferably 85 mass % or more. From the viewpoint of increasing the film strength of the composite layer, the proportion of inorganic solid particles in the composite layer is preferably 95 mass % or less, and more preferably 90 mass % or less. The proportion of inorganic solid particles in the composite layer can be calculated by thermogravimetry (TG) analysis.
[0107] The composite layer may contain a polymeric material in addition to the inorganic particles. The polymeric material contained in the composite layer enhances the binding between the inorganic solid particles. The weight-average molecular weight of the polymeric material is, for example, 3000 or more. When the weight-average molecular weight of the polymeric material is 3000 or more, the binding between the inorganic solid particles can be further enhanced. The weight-average molecular weight of the polymeric material is preferably 3000 or more and 5,000,000 or less, more preferably 5000 or more and 2,000,000 or less, and even more preferably 10,000 or more and 1,000,000 or less. The weight-average molecular weight of the polymeric material can be determined by gel permeation chromatography (GPC).
[0108] The polymeric material may be a polymer made of a single monomer unit, a copolymer made of a plurality of monomer units, or a mixture thereof. The polymeric material preferably contains a monomer unit made of a hydrocarbon having a functional group containing at least one selected from the group consisting of oxygen (O), sulfur (S), nitrogen (N), and fluorine (F). In the polymeric material, the proportion of the portion made of the monomer unit is preferably 70 mol % or more. Hereinafter, this monomer unit is referred to as a first monomer unit. In addition, in the copolymer, the unit other than the first monomer unit is referred to as a second monomer unit. The copolymer of the first monomer unit and the second monomer unit may be an alternating copolymer, a random copolymer, or a block copolymer.
[0109] If the proportion of the portion constituted by the first monomer unit in the polymer material is less than 70 mol %, the water-proofing property of the composite layer may be reduced. It is preferable that the proportion of the portion constituted by the first monomer unit in the polymer material is 90 mol % or more. It is most preferable that the proportion of the portion constituted by the first monomer unit is 100 mol %, that is, the polymer is composed only of the first monomer unit.
[0110] The first monomer unit may be a compound having a functional group in a side chain containing one or more elements selected from the group consisting of oxygen (O), sulfur (S), nitrogen (N), and fluorine (F), and a main chain formed of a carbon-carbon bond. The hydrocarbon may have one or more functional groups containing one or more elements selected from the group consisting of oxygen (O), sulfur (S), nitrogen (N), and fluorine (F). The functional group in the first monomer unit increases the conductivity of alkali metal ions passing through the composite layer.
[0111] The hydrocarbon constituting the first monomer unit preferably has a functional group containing one or more selected from the group consisting of oxygen (O), sulfur (S), and nitrogen (N). When the first monomer unit has such a functional group, the conductivity of alkali metal ions in the composite layer tends to be higher, and the internal resistance tends to be lower.
[0112] The functional group contained in the first monomer unit preferably contains one or more selected from the group consisting of a formal group, a butyral group, a carboxymethyl ester group, an acetyl group, a carbonyl group, a hydroxyl group, and a fluoro group. The first monomer unit more preferably contains at least one of a carbonyl group and a hydroxyl group in the functional group, and even more preferably contains both.
[0113] The first monomer unit can be represented by the following formula: [ka]
[0114] In the above formula, R1 is preferably selected from the group consisting of hydrogen (H), an alkyl group, and an amino group, and R2 is preferably selected from the group consisting of a hydroxyl group (-OH), -OR1, -COOR1, -OCOR1, -OCH(R1)O-, -CN, -N(R1)3, and -SO2R1.
[0115] Examples of the first monomer unit include one or more selected from the group consisting of vinyl formal, vinyl alcohol, vinyl acetate, vinyl acetal, vinyl butyral, acrylic acid and derivatives thereof, methacrylic acid and derivatives thereof, acrylonitrile, acrylamide and derivatives thereof, styrene sulfonic acid, polyvinylidene fluoride, and tetrafluoroethylene.
[0116] The polymer material preferably includes one or more selected from the group consisting of polyvinyl formal, polyvinyl alcohol (PVA), polyvinyl acetal, polyvinyl butyral (PVB), polymethyl methacrylate, PVdF, PTFE, fluorine-based rubber, styrene butadiene rubber, polyacrylic acid compounds, imide compounds, and CMC.
[0117] An example of the structural formula of a compound that can be used as the polymer material is given below.
[0118] The structural formula of polyvinyl formal is as follows: In the following formula, it is preferable that a is 50 or more and 80 or less, b is 0 or more and 5 or less, and c is 15 or more and 50 or less. [ka]
[0119] The structural formula of polyvinyl butyral is as follows: In the following formula, it is preferable that l is 50 or more and 80 or less, m is 0 or more and 10 or less, and n is 10 or more and 50 or less. [ka]
[0120] The structural formula of polyvinyl alcohol is as follows: In the following formula, n is preferably 70 or more and 20,000 or less. [ka]
[0121] The structural formula of polymethyl methacrylate is as follows: In the following formula, n is preferably 30 or more and 10,000 or less. [ka]
[0122] The second monomer unit is a compound other than the first monomer unit, i.e., a compound that does not have a functional group containing one or more selected from the group consisting of oxygen (O), sulfur (S), nitrogen (N), and fluorine (F), or a compound that has such a functional group but is not a hydrocarbon. Examples of the second monomer unit include ethylene oxide and styrene. Examples of the polymer composed of the second monomer unit include polyethylene oxide (PEO) and polystyrene (PS).
[0123] The second monomer unit is a compound other than the first monomer unit, i.e., a compound that does not have a functional group containing one or more selected from the group consisting of oxygen (O), sulfur (S), nitrogen (N), and fluorine (F), or a compound that has such a functional group but is not a hydrocarbon. Examples of the second monomer unit include ethylene oxide and styrene. Examples of the polymer composed of the second monomer unit include polyethylene oxide (PEO) and polystyrene (PS).
[0124] The types of functional groups contained in the first monomer unit and the second monomer unit can be identified by Fourier Transform Infrared Spectroscopy (FT-IR). Furthermore, it can be determined that the first monomer unit is composed of a hydrocarbon by Nuclear Magnetic Resonance (NMR). Furthermore, the proportion of the portion composed of the first monomer unit in a copolymer of the first monomer unit and the second monomer unit can be calculated by NMR.
[0125] The polymer material may contain an aqueous electrolyte. The ratio of the aqueous electrolyte that may be contained in the polymer material may be understood by its water absorption rate. Here, the water absorption rate of the polymer material is defined as the mass M p’ From the mass M of the polymer material before immersion p The value obtained by subtracting p Divided by ([M p’ -M p ] / M p × 100). The water absorption rate of polymer materials is thought to be related to the polarity of the polymer materials.
[0126] When a polymeric material with high water absorption is used, the alkali metal ion conductivity of the composite layer tends to increase. In addition, when a polymeric material with high water absorption is used, the binding force between the inorganic solid particles and the polymeric material is increased, so that the flexibility of the composite layer can be increased. The water absorption of the polymeric material is preferably 0.01% or more, more preferably 0.5% or more, and further preferably 2% or more.
[0127] The strength of the composite layer can be increased by using a polymer material with a low water absorption rate. That is, if the water absorption rate of the polymer material is too high, the composite layer may swell due to the aqueous electrolyte. Also, if the water absorption rate of the polymer material is too high, the polymer material in the composite layer may flow out into the aqueous electrolyte. The water absorption rate of the polymer material is preferably 15% or less, more preferably 10% or less, even more preferably 7% or less, and particularly preferably 3% or less.
[0128] From the viewpoint of increasing the flexibility of the composite layer, the proportion of the polymer material in the composite layer is preferably 5% by mass or more, and more preferably 10% by mass or more. In addition, the higher the proportion of the polymer material, the higher the density of the composite layer tends to be.
[0129] From the viewpoint of increasing the ionic conductivity of the composite layer, the proportion of the polymer material in the composite layer is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less. The proportion of the polymer material in the composite layer can be calculated by thermogravimetry (TG) analysis.
[0130] The polymeric materials contained in the composite layer may be the same or different, and may be a single type or a mixture of multiple types.
[0131] The composite layer may contain a plasticizer and an electrolyte salt in addition to the inorganic solid particles and the polymer material. For example, when the composite layer contains an electrolyte salt, the alkali metal ion conductivity of the composite layer can be further increased.
[0132] The electrode structure according to the embodiment can be produced, for example, as follows. First, a current collector is prepared. Next, an active material, a conductive agent, and a binder are suspended in an appropriate solvent to prepare a slurry, and the slurry is applied to one or both sides of the current collector. The coating on the current collector is dried to form an active material-containing layer. In order to control the density of the active material-containing layer and the composite layer to be formed in a later step, pressing may be performed before forming the composite layer. In this manner, an electrode is produced.
[0133] The composite layer is formed on the electrode, for example, as follows. Preparing a slurry for forming a separator layer The separator layer forming slurry can be obtained by mixing inorganic solid particles, a polymeric material, and a solvent, and stirring the mixture. The obtained slurry may be subjected to slurry dispersion using a wet bead mill or the like.
[0134] The solvent is preferably one capable of dissolving the polymeric material. Examples of the solvent include alcohols such as ethanol, methanol, isopropyl alcohol, normal propyl alcohol, and benzyl alcohol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and diacetone alcohol; esters such as ethyl acetate, methyl acetate, butyl acetate, ethyl lactate, methyl lactate, and butyl lactate; ethers such as methyl cellosolve, ethyl cellosolve, butyl cellosolve, 1,4-dioxane, and tetrahydrofuran; glycols such as ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, butyl carbitol acetate, and ethyl carbitol acetate; methyl Glycol ethers such as carbitol, ethyl carbitol, and butyl carbitol; aprotic polar solvents such as dimethylformamide, dimethylacetamide, acetonitrile, valeronitrile, N-methyl-2-pyrrolidone (NMP), N-ethyl-2-pyrrolidone, and γ-butyrolactam; cyclic carboxylic acid esters such as gamma butyrolactone, gamma valerolactone, gamma caprolactone, and epsilon caprolactone; and chain carbonate compounds such as dimethyl carbonate, diethyl carbonate, di-n-propyl carbonate, diisopropyl carbonate, n-propyl isopropyl carbonate, ethyl methyl carbonate, and methyl-n-propyl carbonate are used. Regarding the above separator layer forming slurry, slurry 1 and slurry 2 having different mode diameters are prepared.
[0135] The composite layer forming slurry 1 is applied, for example, by a doctor blade method on one main surface of the electrode, onto the active material-containing layer to obtain a coating. This coating is dried at a temperature of 50°C to 150°C. Next, the composite layer forming slurry 2 is applied to the surface of the area where the composite layer forming slurry 1 is applied to obtain a coating. This coating is again dried at a temperature of 50°C to 150°C. In this manner, a laminate that will become an electrode structure is obtained. Here, the laminate that will become an electrode structure may be pressed immediately before applying the composite layer forming slurry 2.
[0136] Here, by adjusting the mode diameters of the inorganic particles contained in Slurry 1 and Slurry 2 respectively, it is possible to control such that R1 and R2, which are the average particle diameters of the inorganic particles in the first region and the second region respectively, satisfy R1 < R2. For example, by making the mode diameter of the inorganic particles contained in Slurry 2 higher than the mode diameter of the inorganic particles contained in Slurry 1, the average particle diameter of the inorganic particles contained in the second region becomes larger than the average particle diameter of the inorganic particles contained in the first region, and R2 / R1 can be increased. Also, by making the coating thickness of Slurry 2 thinner than the coating thickness of Slurry 1, the number of inorganic particles contained in the second region can be reduced, and it can be controlled such that N1 > N2. Furthermore, by pressing the obtained electrode structure, the composite layer is crushed and the porosity can be lowered.
[0137] Next, this laminate is subjected to a roll pressing process. In the roll pressing process, for example, a pressing device equipped with two rollers, one on top and one on the bottom, is used. By using such a pressing device, when coating films are provided on both sides of the electrode, both coating films can be simultaneously subjected to pressing. At this time, the heating temperature of the rollers can be appropriately changed according to the desired structure. For example, the heating temperature of the rollers is set to a temperature within ±20°C of the softening point of the polymer material in the coating film. The heating temperature of the rollers is preferably lower than the melting point of the polymer material. If the heating temperature is increased above the melting point of the polymer material, the polymer material melts on the surface side of the coating film and pores can be completely lost. When the pores are completely lost, the ionic conductivity of the composite layer decreases, which is not desirable.
[0138] The softening point and melting point of the polymer material can vary depending on the molecular weight and the unit ratio of the monomers.
[0139] According to one example, the softening point of PVdF is 135°C or higher and 145°C or lower, and the melting point is 170°C or higher and 180°C or lower. The softening point of polyvinyl formal is 120°C or higher and 130°C or lower, and the melting point is 190°C or higher and 200°C or lower. The softening point of polyvinyl butyral is 120°C or higher and 130°C or lower, and the melting point is 190°C or higher and 200°C or lower.
[0140] Also, for each electrode, in order to control the density of each of the active material-containing layer and the composite layer, pressing may be performed prior to the application of the slurry for forming the composite layer, and after drying the slurry coating film, pressing may be performed again.
[0141] As described above, an electrode structure can be obtained in which the average particle diameter R1 of the inorganic particles in the first region and the average particle diameter R2 of the inorganic particles in the second region satisfy the relationship R1 < R2.
[0142] The electrode structure according to the first embodiment has an electrode and a composite layer containing inorganic particles. The composite layer has a first region and a second region. The first region exists between the electrode and the second region. In the cumulative frequency distribution of inorganic particles having an average particle diameter of 3 μm or more in the composite layer with respect to the thickness direction of the composite layer, when the total number of inorganic particles having an average particle diameter of 3 μm or more is normalized to 100, the first region is in the range where the cumulative frequency of inorganic particles having an average particle diameter of 3 μm or more is 0 or more and less than 25, and the first region is 5% or more and 40% or less of the thickness of the composite layer from the interface between the electrode and the composite layer. In the cross-sectional SEM image of the composite layer, the average particle diameter R1 of the inorganic particles in the first region and the average particle diameter R2 of the inorganic particles in the second region satisfy the relationship R1 < R2. Thereby, in the secondary battery including the electrode structure according to the present embodiment, it is possible to suppress an increase in resistance while suppressing electrolysis of water accompanying side reactions.
[0143] [Second Embodiment] According to the second embodiment, a secondary battery including the electrode structure according to the first embodiment and a counter electrode is provided.
[0144] Hereinafter, the configuration of the secondary battery according to the present embodiment will be described, but the description of the electrode structure will be omitted because it has been described in the first embodiment.
[0145] (Counter Electrode) In the first embodiment, the case where the electrode of the electrode structure is a negative electrode has been described, so here, the case where the counter electrode is a positive electrode will be described. As described above, the active material-containing layer of the electrode structure according to the first embodiment can also be used as a positive electrode active material-containing layer, so in that case, the counter electrode in this embodiment is a negative electrode.
[0146] The positive electrode may include a current collector (positive electrode current collector) and a positive electrode active material-containing layer provided on at least one main surface of the current collector. The positive electrode active material-containing layer includes a positive electrode active material, and optionally a conductive agent and a binder.
[0147] The positive electrode current collector includes metals such as stainless steel, aluminum (Al) and titanium (Ti). The positive electrode current collector has a shape of, for example, a foil, a porous body or a mesh. In order to prevent corrosion caused by a reaction between the positive electrode current collector and the aqueous electrolyte, the surface of the positive electrode current collector may be coated with a different element. The positive electrode current collector is preferably one having excellent corrosion resistance and oxidation resistance, such as Ti foil. In addition, when Li2SO4 is used as the aqueous electrolyte, Al may be used as the positive electrode current collector because corrosion does not progress.
[0148] The positive electrode active material-containing layer contains a positive electrode active material. The positive electrode active material-containing layer may be supported on both the front and back principal surfaces of the positive electrode current collector.
[0149] The positive electrode active material has a lithium ion insertion-extraction potential of 2.5 V (vs. Li / Li) relative to the oxidation-reduction potential of lithium. + ) or more 5.5V (vs.Li / Li + The positive electrode may contain one type of compound alone as the positive electrode active material, or may contain two or more compounds as the positive electrode active material.
[0150] Examples of compounds that can be used as the positive electrode active material include lithium manganese composite oxides, lithium nickel composite oxides, lithium cobalt aluminum composite oxides, lithium nickel cobalt manganese composite oxides, spinel-type lithium manganese nickel composite oxides, lithium manganese cobalt composite oxides, lithium iron oxides, lithium fluorinated iron sulfate, phosphate compounds having an olivine crystal structure (for example, a compound represented by Li z FePO4 where 0 < z ≦ 1, a compound represented by Li z MnPO4 where 0 < z ≦ 1), and the like. The phosphate compounds having an olivine crystal structure are excellent in thermal stability.
[0151] Examples of compounds capable of obtaining a high positive electrode potential include, for example, lithium manganese composite oxides such as a compound represented by Li z Mn2O4 where 0 < z ≦ 1, a compound represented by Li z MnO2 where 0 < z ≦ 1; for example, lithium nickel aluminum composite oxides such as a compound represented by Li z Ni 1-j Al j O2 where 0 < z ≦ 1, 0 < j < 1; for example, lithium cobalt composite oxides such as a compound represented by Li z CoO2 where 0 < z ≦ 1; for example, lithium nickel cobalt composite oxides such as a compound represented by Li z Ni 1-j-k Co j Mn k O2 where 0 < z ≦ 1, 0 < j < 1, 0 ≦ k < 1; for example, lithium manganese cobalt composite oxides such as a compound represented by Li z Mn j Co 1-j O2 where 0 < z ≦ 1, 0 < j < 1; for example, spinel-type lithium manganese nickel composite oxides such as a compound represented by Li z Mn 2-i Ni i O4 where 0 < z ≦ 1, 0 < i < 2; for example, a compound represented by Li z FePO4 where 0 < z ≦ 1, a compound represented by Li z Fe 1-y Mn yA compound represented by PO4 where 0 < z ≤ 1 and 0 ≤ y ≤ 1, Li z Lithium phosphates having an olivine structure such as a compound represented by CoPO4 where 0 < z ≤ 1; fluorinated iron sulfate (for example, Li z A compound represented by FeSO4F where 0 < z ≤ 1) may be mentioned.
[0152] As the positive electrode active material, it is preferable to include one or more selected from the group consisting of lithium cobalt composite oxides, lithium manganese composite oxides, and lithium phosphates having an olivine structure. The operating potential of these compounds is 3.5 V (vs. Li / Li + ) or more and 4.2 V (vs. Li / Li + ) or less. That is, the operating potential of these compounds as active materials is relatively high. By using these compounds in combination with negative electrode active materials such as the above-described spinel-type lithium titanate and anatase-type titanium oxide, a high battery voltage can be obtained.
[0153] The positive electrode active material is contained in the positive electrode in the form of particles, for example. The positive electrode active material particles can be single primary particles, secondary particles that are aggregates of primary particles, or a mixture of primary particles and secondary particles. The shape of the particles is not particularly limited, and can be, for example, spherical, elliptical, flat, or fibrous.
[0154] The average particle diameter (diameter) of the primary particles of the positive electrode active material is preferably 10 μm or less, more preferably 0.1 μm or more and 5 μm or less. The average particle diameter (diameter) of the secondary particles of the positive electrode active material is preferably 100 μm or less, more preferably 10 μm or more and 50 μm or less. The primary particle diameter and secondary particle diameter of the positive electrode active material can be measured by the same method as the negative electrode active material particles.
[0155] The conductive agent is blended as necessary to enhance the current collection performance and suppress the contact resistance between the positive electrode active material and the current collector. Examples of the conductive agent include carbonaceous materials such as acetylene black, ketjen black, graphite, and coke. The conductive agent may be of one type, or two or more types may be mixed and used.
[0156] The binder has the function of binding the positive electrode active material and the conductive agent. As the binder, for example, at least one selected from the group consisting of PTFE, PVdF, fluorine-based rubber, ethylene-butadiene rubber, polypropylene (PP), polyethylene (PE), CMC, polyimide (PI), and polyacrylimide (PAI) can be used, but is not limited thereto. For example, the polymer material contained in the separator layer can be used as the binder. By using the same material as the polymer material used in the separator layer as the binder used in the positive electrode active material-containing layer, the degree of binding between the two, that is, the peel strength, can be improved. The binder may be one type, or two or more types may be mixed and used.
[0157] The compounding ratios of the positive electrode active material, conductive agent, and binder in the positive electrode active material-containing layer are preferably 70% by mass or more and 95% by mass or less, 3% by mass or more and 20% by mass or less, and 2% by mass or more and 10% by mass or less, respectively. When the compounding ratio of the conductive agent is 3% by mass or more, the conductivity of the positive electrode can be improved, and when it is 20% by mass or less, the decomposition of the aqueous electrolyte on the conductive agent surface can be reduced. When the compounding ratio of the binder is 2% by mass or more, sufficient electrode strength can be obtained, and when it is 10% by mass or less, the insulating part of the electrode can be reduced.
[0158] (Exterior materials) For the exterior member in which the electrode group and the aqueous electrolyte are housed, a metal container, a laminate film container, or a resin container can be used.
[0159] As the metal container, a metal can made of nickel, iron, stainless steel, etc., and having a rectangular or cylindrical shape can be used. As the resin container, a container made of polyethylene, polypropylene, etc. can be used.
[0160] The thickness of each of the resin container and the metal container is preferably within a range of 0.05 mm to 1 mm, more preferably 0.5 mm or less, and further preferably 0.3 mm or less.
[0161] Examples of the laminate film include a multi-layer film in which a metal layer is coated with a resin layer. Examples of the metal layer include stainless steel foil, aluminum foil, and aluminum alloy foil. Polymers such as PP, PE, nylon, and polyethylene terephthalate (PET) can be used for the resin layer. The thickness of the laminate film is preferably within a range of 0.01 mm to 0.5 mm. The thickness of the laminate film is more preferably 0.2 mm or less.
[0162] Fig. 3 is a cross-sectional view showing an example of a secondary battery according to an embodiment of the present invention, Fig. 4 is a cross-sectional view taken along line IV-IV of the secondary battery shown in Fig. 3.
[0163] The electrode group 1 is housed in an exterior member 2 made of a rectangular cylindrical metal container. The electrode group 1 includes an electrode structure (negative electrode structure) including a negative electrode 3 and a composite membrane 4, and a positive electrode 5 which is the counter electrode of the negative electrode 3. The electrode group 1 has a structure in which the electrode structure and the positive electrode 5 are arranged so that the positive electrode 5 and the negative electrode 3 are interposed with the composite layer 4 as a separator, and are spirally wound to form a flat shape. An aqueous electrolyte (not shown) is held in the electrode group 1. As shown in FIG. 3, a strip-shaped negative electrode lead 16 is electrically connected to each of a plurality of points on the end of the negative electrode 3 located on the end face of the electrode group 1. In addition, a strip-shaped positive electrode lead 17 is electrically connected to each of a plurality of points on the end of the positive electrode 5 located on this end face. The plurality of negative electrode leads 16 are connected to the negative electrode terminal 6 in a bundled state as shown in FIG. 4. In addition, although not shown, the positive electrode lead 17 is also electrically connected to the positive electrode terminal 7 in a bundled state.
[0164] The metal sealing plate 10 is fixed to the opening of the metal exterior member 2 by welding or the like. The negative electrode terminal 6 and the positive electrode terminal 7 are each drawn out to the outside through an extraction hole provided in the sealing plate 10. A negative electrode gasket 8 and a positive electrode gasket 9 are disposed on the inner circumferential surface of each extraction hole of the sealing plate 10 to prevent a short circuit due to contact with the negative electrode terminal 6 and the positive electrode terminal 7, respectively. By disposing the negative electrode gasket 8 and the positive electrode gasket 9, the airtightness of the secondary battery 100 can be maintained.
[0165] A control valve 11 (safety valve) is disposed on the sealing plate 10. When the internal pressure in the battery cell increases due to gas generated by electrolysis of water, the generated gas can be released to the outside from the control valve 11. As the control valve 11, for example, a reset type that operates when the internal pressure becomes higher than a set value and functions as a sealing plug when the internal pressure decreases can be used. Alternatively, a non-reset type control valve that does not recover its function as a sealing plug once it is activated may be used. In FIG. 3, the control valve 11 is disposed in the center of the sealing plate 10, but the control valve 11 may be located at the end of the sealing plate 10. The control valve 11 may be omitted.
[0166] Further, the sealing plate 10 is provided with a liquid inlet 12. The aqueous electrolyte can be injected through this liquid inlet 12. After the aqueous electrolyte is injected, the liquid inlet 12 can be closed with a sealing plug 13. The liquid inlet 12 and the sealing plug 13 may be omitted.
[0167] Fig. 5 is a partially cutaway perspective view that illustrates another example of a secondary battery according to an embodiment. Fig. 6 is an enlarged cross-sectional view of part B of the secondary battery illustrated in Fig. 5. Figs. 5 and 6 illustrate an example of a secondary battery 100 that uses an exterior member made of a laminate film as the exterior member.
[0168] The secondary battery 100 shown in Figures 5 and 6 includes an electrode group 1 shown in Figures 5 and 6, an exterior member 2 shown in Figure 5, and an aqueous electrolyte (not shown). The electrode group 1 and the aqueous electrolyte are housed in the exterior member 2. The aqueous electrolyte is held in the electrode group 1.
[0169] The exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.
[0170] The electrode group 1 is a laminated type electrode group, as shown in Fig. 6. The laminated type electrode group 1 has a structure in which electrode structures 500 and positive electrodes 5 are laminated alternately.
[0171] The electrode group 1 includes a plurality of electrode structures 500. Each electrode structure 500 includes a negative electrode 3 and a composite film 4 supported on both sides of the negative electrode 3. Each negative electrode 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b supported on both sides of the negative electrode current collector 3a. Each composite film 4 is supported on the negative electrode active material-containing layer 3b of the negative electrode 3. The electrode group 1 also includes a plurality of positive electrodes 5. Each of the plurality of positive electrodes 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b supported on both sides of the positive electrode current collector 5a.
[0172] The negative electrode current collector 3a of each negative electrode 3 includes a portion on one side where the negative electrode active material-containing layer 3b is not provided on any surface. This portion serves as a negative electrode current collector tab 3c. As shown in FIG. 6, the negative electrode current collector tab 3c does not overlap with the positive electrode 5. The negative electrode current collector tabs 3c are electrically connected to a strip-shaped negative electrode terminal 6. The tip of the strip-shaped negative electrode terminal 6 is drawn out to the outside of the exterior member 2.
[0173] Although not shown, the positive electrode current collector 5a of each positive electrode 5 includes a portion on one side where the positive electrode active material-containing layer 5b is not supported on any surface. This portion serves as a positive electrode current collector tab. The positive electrode current collector tab does not overlap with the negative electrode 3, similar to the negative electrode current collector tab 3c. The positive electrode current collector tab is located on the opposite side of the electrode group 1 to the negative electrode current collector tab 3c. The positive electrode current collector tab is electrically connected to a strip-shaped positive electrode terminal 7. The tip of the strip-shaped positive electrode terminal 7 is located on the opposite side of the negative electrode terminal 6 and is drawn out to the outside of the exterior member 2.
[0174] The secondary battery according to the second embodiment includes the electrode structure according to the first embodiment and a counter electrode, which can suppress an increase in resistance while suppressing electrolysis of water caused by a side reaction.
[0175] [Third embodiment] According to a third embodiment, there is provided a battery pack including a plurality of secondary batteries according to the second embodiment.
[0176] In the battery pack according to this embodiment, the individual cells may be electrically connected in series or in parallel, or may be connected in a combination of series and parallel.
[0177] Next, an example of a battery pack will be described with reference to the drawings.
[0178] Fig. 7 is a perspective view showing an example of a battery pack according to an embodiment. The battery pack 200 shown in Fig. 7 includes five cells 100a to 100e, four bus bars 21, a positive electrode lead 22, and a negative electrode lead 23. Each of the five cells 100a to 100e is a secondary battery according to the third embodiment.
[0179] The bus bar 21 connects, for example, the negative electrode terminal 6 of one cell 100a and the positive electrode terminal 7 of the adjacent cell 100b. In this way, the five cells 100 are connected in series by the four bus bars 21. That is, the battery pack 200 in FIG. 7 is a five-series battery pack. Although no example is shown, in a battery pack including a plurality of cells electrically connected in parallel, for example, the plurality of negative electrode terminals are connected to each other by a bus bar and the plurality of positive electrode terminals are connected to each other by a bus bar, thereby electrically connecting the plurality of cells.
[0180] The positive terminal 7 of at least one of the five cells 100a to 100e is electrically connected to a positive electrode lead 22 for external connection. Also, the negative terminal 6 of at least one of the five cells 100a to 100e is electrically connected to a negative electrode lead 23 for external connection.
[0181] As described above, the battery pack according to this embodiment includes the secondary battery according to the second embodiment. Therefore, the battery pack can suppress an increase in resistance while suppressing electrolysis of water caused by a side reaction.
[0182] [Fourth embodiment] According to a fourth embodiment, there is provided a battery pack including the secondary battery according to the second embodiment. This battery pack may include the battery assembly according to the third embodiment. This battery pack may include a single secondary battery according to the second embodiment instead of the battery assembly according to the third embodiment.
[0183] Such a battery pack may further include a protection circuit. The protection circuit has a function of controlling charging and discharging of the secondary battery. Alternatively, a circuit included in a device (e.g., electronic device, automobile, etc.) that uses the battery pack as a power source may be used as the protection circuit for the battery pack.
[0184] The battery pack may further include an external terminal for current flow. The external terminal for current flow is for outputting current from the secondary battery to the outside and / or inputting current from the outside to the secondary battery. In other words, when the battery pack is used as a power source, current is supplied to the outside through the external terminal for current flow. When the battery pack is charged, a charging current (including regenerative energy from the power of an automobile or the like) is supplied to the battery pack through the external terminal for current flow.
[0185] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.
[0186] FIG. 8 is a perspective view that illustrates an example of a battery pack according to an embodiment.
[0187] The battery pack 300 includes, for example, an assembled battery including the secondary batteries shown in FIG. 5 and FIG. 6. The battery pack 300 includes a housing 310 and an assembled battery 200 housed in the housing 310. The assembled battery 200 is a battery in which a plurality of (for example, five) secondary batteries 100 are electrically connected in series. The secondary batteries 100 are stacked in the thickness direction. The housing 310 has openings 320 on the top and on each of the four side surfaces. The side surface from which the negative electrode terminal 6 and the positive electrode terminal 7 of the secondary battery 100 protrude is exposed in the opening 320 of the housing 310. The output positive electrode terminal 332 of the assembled battery 200 is strip-shaped, one end of which is electrically connected to one of the positive electrode terminals 7 of the secondary batteries 100, and the other end of which protrudes from the opening 320 of the housing 310 and protrudes from the top of the housing 310. On the other hand, the output negative electrode terminal 333 of the battery pack 200 is strip-shaped, with one end electrically connected to one of the negative electrode terminals 6 of the secondary batteries 100, and the other end protruding from the opening 320 of the housing 310 and protruding from the top of the housing 310.
[0188] Another example of such a battery pack will be described in detail with reference to Fig. 9 and Fig. 10. Fig. 9 is an exploded perspective view showing a schematic diagram of another example of a battery pack according to an embodiment. Fig. 10 is a block diagram showing an example of an electric circuit of the battery pack shown in Fig. 9.
[0189] The battery pack 300 shown in Figs. 9 and 10 includes a container 31, a lid 32, a protective sheet 33, a battery pack 200, a printed wiring board 34, wiring 35, and an insulating plate (not shown).
[0190] 9 is a bottomed, square container having a rectangular bottom. The container 31 is configured to be able to accommodate a protective sheet 33, a battery pack 200, a printed wiring board 34, and wiring 35. The lid 32 has a rectangular shape. The lid 32 covers the container 31 to accommodate the battery pack 200 and the like. Although not shown, the container 31 and the lid 32 are provided with openings or connection terminals for connection to an external device or the like.
[0191] The battery pack 200 includes a plurality of cells 100, a positive electrode lead 22, a negative electrode lead 23, and an adhesive tape 24.
[0192] At least one of the plurality of unit cells 100 is a secondary battery according to the embodiment. Each of the plurality of unit cells 100 is electrically connected in series as shown in FIG. 10. The plurality of unit cells 100 may be electrically connected in parallel, or may be connected in a combination of series and parallel connections. When the plurality of unit cells 100 are connected in parallel, the battery capacity is increased compared to when they are connected in series.
[0193] The adhesive tape 24 fastens the plurality of unit cells 100. The plurality of unit cells 100 may be fixed using heat shrink tape instead of the adhesive tape 24. In this case, the protective sheets 33 are disposed on both side surfaces of the battery pack 200, the heat shrink tape is wrapped around the battery pack 200, and the heat shrink tape is then thermally shrunk to bind the plurality of unit cells 100 together.
[0194] One end of the positive electrode lead 22 is connected to the battery pack 200. One end of the positive electrode lead 22 is electrically connected to the positive electrode of one or more cells 100. One end of the negative electrode lead 23 is connected to the battery pack 200. One end of the negative electrode lead 23 is electrically connected to the negative electrode of one or more cells 100.
[0195] The printed wiring board 34 is disposed along one of the short side surfaces of the inner surface of the container 31. The printed wiring board 34 includes a positive connector 342, a negative connector 343, a thermistor 345, a protection circuit 346, wiring 342a and 343a, an external terminal 350 for supplying electricity, a positive wiring (positive wiring) 348a, and a negative wiring (negative wiring) 348b. One main surface of the printed wiring board 34 faces one side of the battery pack 200. An insulating plate (not shown) is interposed between the printed wiring board 34 and the battery pack 200.
[0196] The other end 22a of the positive electrode lead 22 is electrically connected to the positive electrode connector 342. The other end 23a of the negative electrode lead 23 is electrically connected to the negative electrode connector 343.
[0197] The thermistor 345 is fixed to one main surface of the printed wiring board 34. The thermistor 345 detects the temperature of each of the cells 100, and transmits a detection signal to the protection circuit 346.
[0198] The external terminal 350 for current supply is fixed to the other main surface of the printed wiring board 34. The external terminal 350 for current supply is electrically connected to a device present outside the battery pack 300. The external terminal 350 for current supply includes a positive terminal 352 and a negative terminal 353.
[0199] The protection circuit 346 is fixed to the other main surface of the printed wiring board 34. The protection circuit 346 is connected to the positive terminal 352 via a positive wiring 348a. The protection circuit 346 is connected to the negative terminal 353 via a negative wiring 348b. The protection circuit 346 is also electrically connected to the positive electrode connector 342 via a wiring 342a. The protection circuit 346 is electrically connected to the negative electrode connector 343 via a wiring 343a. Furthermore, the protection circuit 346 is electrically connected to each of the plurality of single cells 100 via the wiring 35.
[0200] The protective sheet 33 is disposed on both inner surfaces in the long side direction of the container 31 and on the inner surface in the short side direction that faces the printed wiring board 34 via the battery pack 200. The protective sheet 33 is made of, for example, resin or rubber.
[0201] The protection circuit 346 controls charging and discharging of the multiple cells 100. In addition, the protection circuit 346 cuts off electrical connection between the protection circuit 346 and external terminals 350 (positive terminal 352, negative terminal 353) for supplying electricity to an external device, based on a detection signal transmitted from the thermistor 345, or a detection signal transmitted from each of the cells 100 or the battery pack 200.
[0202] An example of the detection signal transmitted from the thermistor 345 is a signal that detects that the temperature of the cell 100 is equal to or higher than a predetermined temperature. An example of the detection signal transmitted from each cell 100 or the battery pack 200 is a signal that detects overcharging, overdischarging, and overcurrent of the cell 100. When detecting overcharging or the like for each cell 100, the battery voltage may be detected, or the positive electrode potential or the negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 100.
[0203] The protection circuit 346 may be a circuit included in a device (such as an electronic device or an automobile) that uses the battery pack 300 as a power source.
[0204] As described above, the battery pack 300 includes the external terminal 350 for current supply. Therefore, the battery pack 300 can output a current from the assembled battery 200 to an external device and input a current from the external device to the assembled battery 200 via the external terminal 350 for current supply. In other words, when the battery pack 300 is used as a power source, the current from the assembled battery 200 is supplied to the external device through the external terminal 350 for current supply. When the battery pack 300 is charged, a charging current from the external device is supplied to the battery pack 300 through the external terminal 350 for current supply. When the battery pack 300 is used as an in-vehicle battery, regenerative energy of the vehicle's power can be used as the charging current from the external device.
[0205] The battery pack 300 may include a plurality of assembled batteries 200. In this case, the plurality of assembled batteries 200 may be connected in series, in parallel, or in a combination of series and parallel connections. The printed wiring board 34 and the wiring 35 may be omitted. In this case, the positive electrode lead 22 and the negative electrode lead 23 may be used as a positive terminal and a negative terminal, respectively, of the external terminals for current supply.
[0206] Such a battery pack is used in applications that require excellent cycle performance, for example, when a large current is drawn. Specifically, the battery pack is used, for example, as a power source for electronic devices, a stationary battery, or an on-board battery for various vehicles. An example of the electronic device is a digital camera. The battery pack is particularly suitable for use as an on-board battery.
[0207] The battery pack according to the fourth embodiment includes the secondary battery according to the second embodiment or the battery pack according to the third embodiment, and therefore the battery pack can suppress an increase in resistance while suppressing electrolysis of water caused by a side reaction.
[0208] [Fifth embodiment] According to a fifth embodiment, a vehicle including the battery pack according to the fourth embodiment is provided.
[0209] In such a vehicle, the battery pack, for example, recovers regenerative energy of the vehicle's motive power. The vehicle may include a mechanism (regenerator) that converts the kinetic energy of the vehicle into regenerative energy.
[0210] Examples of vehicles according to the embodiment include two-wheeled to four-wheeled hybrid electric vehicles, two-wheeled to four-wheeled electric vehicles, power-assisted bicycles, and rail vehicles.
[0211] The mounting position of the battery pack in the vehicle according to the embodiment is not particularly limited. For example, when the battery pack is mounted in an automobile, the battery pack can be mounted in the engine compartment, the rear of the vehicle body, or under the seat of the vehicle.
[0212] The vehicle according to the embodiment may be equipped with a plurality of battery packs. In this case, the batteries included in each battery pack may be electrically connected in series, electrically connected in parallel, or electrically connected by a combination of series and parallel connections. For example, when each battery pack includes a battery pack, the battery packs may be electrically connected in series, electrically connected in parallel, or electrically connected by a combination of series and parallel connections. Alternatively, when each battery pack includes a single battery, the batteries may be electrically connected in series, electrically connected in parallel, or electrically connected by a combination of series and parallel connections.
[0213] Next, an example of a vehicle according to an embodiment will be described with reference to the drawings.
[0214] FIG. 11 is a partial see-through view that illustrates an example of a vehicle according to an embodiment.
[0215] A vehicle 400 shown in Fig. 11 includes a vehicle body 40 and a battery pack 300 according to the fifth embodiment. In the example shown in Fig. 11, the vehicle 400 is a four-wheeled automobile.
[0216] The vehicle 400 may be equipped with a plurality of battery packs 300. In this case, the batteries (e.g., single cells or assembled batteries) included in the battery pack 300 may be connected in series, in parallel, or in a combination of series and parallel connections.
[0217] 11 illustrates an example in which the battery pack 300 is mounted in an engine room located in the front of the vehicle body 40. As described above, the battery pack 300 may be mounted, for example, in the rear of the vehicle body 40 or under a seat. This battery pack 300 can be used as a power source for the vehicle 400. In addition, this battery pack 300 can recover regenerative energy for the motive power of the vehicle 400.
[0218] The vehicle according to the fifth embodiment is equipped with the battery pack according to the fourth embodiment, and therefore the vehicle has excellent driving performance and reliability.
[0219] [Sixth embodiment] According to a sixth embodiment, there is provided a stationary power source including the battery pack according to the fourth embodiment.
[0220] The stationary power source may be equipped with the assembled battery according to the fourth embodiment or the secondary battery according to the third embodiment, instead of the battery pack according to the fifth embodiment. The stationary power source according to the embodiments can achieve a long life.
[0221] FIG. 12 is a block diagram showing an example of a system including a stationary power source according to the embodiment. FIG. 12 is a diagram showing an example of application to stationary power sources 112 and 123 as an example of use of the battery packs 300A and 300B according to the embodiment. In the example shown in FIG. 12, a system 110 in which the stationary power sources 112 and 123 are used is shown. The system 110 includes a power plant 111, a stationary power source 112, a consumer-side power system 113, and an energy management system (EMS) 115. In addition, a power grid 116 and a communication network 117 are formed in the system 110, and the power plant 111, the stationary power source 112, the consumer-side power system 113, and the EMS 115 are connected via the power grid 116 and the communication network 117. The EMS 115 uses the power grid 116 and the communication network 117 to perform control to stabilize the entire system 110.
[0222] The power plant 111 generates a large amount of power using fuel sources such as thermal power and atomic power. Power is supplied from the power plant 111 through a power grid 116 or the like. A battery pack 300A is mounted on the stationary power source 112. The battery pack 300A can store the power supplied from the power plant 111. The stationary power source 112 can supply the power stored in the battery pack 300A through the power grid 116 or the like. The system 110 is provided with a power conversion device 118. The power conversion device 118 includes a converter, an inverter, a transformer, and the like. Thus, the power conversion device 118 can perform conversion between direct current and alternating current, conversion between alternating currents having different frequencies, and voltage transformation (boosting and bucking), and the like. Thus, the power conversion device 118 can convert the power from the power plant 111 into power that can be stored in the battery pack 300A.
[0223] The consumer-side power system 113 includes a power system for a factory, a power system for a building, a power system for a home, etc. The consumer-side power system 113 includes a consumer-side EMS 121, a power conversion device 122, and a stationary power source 123. The stationary power source 123 is equipped with a battery pack 300B. The consumer-side EMS 121 performs control to stabilize the consumer-side power system 113.
[0224] The consumer-side power system 113 is supplied with power from the power plant 111 and power from the battery pack 300A through the power grid 116. The battery pack 300B can store the power supplied to the consumer-side power system 113. Similarly to the power conversion device 118, the power conversion device 122 includes a converter, an inverter, a transformer, and the like. Therefore, the power conversion device 122 can perform conversion between DC and AC, conversion between ACs with different frequencies, and voltage transformation (boost and step-down), etc. Therefore, the power conversion device 122 can convert the power supplied to the consumer-side power system 113 into power that can be stored in the battery pack 300B.
[0225] The power stored in the battery pack 300B can be used, for example, to charge a vehicle such as an electric car. The system 110 may also be provided with a natural energy source. In this case, the natural energy source generates power using natural energy such as wind power and solar power. Power is supplied from the natural energy source in addition to the power plant 111 through the power grid 116.
[0226] [Example] Example 1 <Preparation of electrode structure> In Example 1, the electrode structure used as the negative electrode was prepared according to the following method. The proportions of the conductive agent and the binder in the negative electrode active material-containing layer were 5 parts by mass and 1 part by mass, respectively, per 100 parts by mass of the negative electrode active material. Lithium titanium oxide Li4Ti5O 12 The powder (TLO), graphite powder as a conductive agent, and PVdF as a binder were mixed and dispersed in N-methyl-2-pyrrolidone (NMP) solvent to prepare a slurry for forming an active material-containing layer.
[0227] This slurry for negative electrode preparation was applied to both sides of 12 μm Al foil used as a negative electrode current collector and dried. At this time, the negative electrode active material-containing slurry drying temperature was 130° C., and the slurry application speed was 1 m / min. The laminate was pressed with 5 kN to obtain a negative electrode.
[0228] Next, two types of slurries for forming a composite layer were prepared by the following procedure. First, for the composite layer forming slurry 1, Al2O3 powder with a mode diameter of 0.8 μm was prepared as inorganic solid particles, and PVdF was prepared as a polymer material. The inorganic solid particles and the polymer material were mixed in a mass ratio of 9:1, and then suspended in NMP as a solvent, and mixed for 30 minutes using a mixer. Similarly, for the composite layer forming slurry 2, bimodal Al2O3 powder containing both particles with mode diameters of 0.8 μm and 5 μm in a mass ratio of 2:1 was used as inorganic solid particles, and mixed with the polymer material in the same manner as for the slurry 1, suspended in a solvent, and mixed for 30 minutes using a mixer. The obtained composite layer forming slurries 1 and 2 were each subjected to disintegration of the aggregated secondary particles using a bead mill. The particle size distribution of the obtained composite layer forming slurries 1 and 2 was measured by a laser diffraction method. As a result, the particle size distribution of the composite layer forming slurries 1 and 2 had modal and bimodal characteristics, respectively, and the mode diameter was 0.8 μm and 5 μm, respectively. The composite layer forming slurry 1 was applied to the negative electrode surface layer obtained previously by a microgravure coating method to a coating thickness of 8 μm, and dried at a temperature of 130 ° C. Next, the composite layer forming slurry 2 was overcoated to a coating thickness of 12 μm by a microgravure coating method on the surface layer of the negative electrode to which the composite layer forming slurry 1 obtained previously had been applied, and dried at a temperature of 130 ° C. The laminate was pressed at 5 kN to obtain an electrode structure.
[0229] <Preparation of counter electrode> The positive electrode active material is LiNi with a primary particle mode diameter of 2 μm. 0.5 Co 0.2 Mn 0.3 A mixture of 90 mass % O2 composite oxide, 5 mass % graphite powder as a conductive agent, and 5 mass % PVdF as a binder was dispersed in an NMP solvent to prepare a slurry for forming an active material-containing layer.
[0230] A positive electrode active material, a conductive agent, a binder, and a solvent were mixed to prepare a slurry for producing a positive electrode. The positive electrode active material was LiNi 0.5 Co 0.2 Mn 0.3O2 composite oxide was used at 90% by mass. Graphite powder was used at 5% by mass as the conductive agent. 5% by mass of PVdF was blended as the binder and dispersed in NMP solvent. The above positive electrode active material, conductive agent, and binder were dispersed in NMP solvent and used. The mass ratio of the positive electrode active material, conductive agent, and binder in the slurry was 100:5:5. This slurry for preparing the positive electrode was applied to both sides of a 12 μm Ti foil used as a positive electrode current collector and dried. At this time, the drying temperature of the positive electrode active material-containing slurry was 130° C., and the slurry application speed was 1 m / min. The laminate was pressed at 5 kN to obtain a positive electrode.
[0231] <Preparation of electrode groups> The electrode structure carrying the composite layer and the positive electrode were laminated to obtain a laminate, which was then spirally wound with the negative electrode side positioned at the outermost periphery, and pressed at 5 kN to produce a flat electrode group.
[0232] <Battery Assembly> The obtained electrode group was placed in a polypropylene resin container, and then an aqueous solution containing 12 M lithium chloride, which had been prepared as an aqueous electrolyte, was poured into the container to prepare a secondary battery.
[0233] <Constant current charge / discharge test and 2C capacity retention measurement> For each of the batteries prepared in Examples 1 to 12 and Comparative Examples 1 to 7, the following capacity evaluation was performed after preparing the test battery. After performing one cycle of charge and discharge at 0.2C rate, the battery was charged under CC-CV conditions at 0.2C, with the current end condition set to 0.1C. Next, 0.2C-CC discharge was performed to the specified voltage of 1.5V. The charge capacity and 0.2C discharge capacity of the battery were obtained. The 0.2C coulomb efficiency was calculated by dividing the obtained 0.2C discharge capacity by the charge capacity of the battery. Next, the battery was charged and discharged one cycle at 0.2C rate, after which it was charged under CC-CV conditions at 0.2C, with the current end condition set to 0.1C. Next, 2C-CC discharge was performed to the specified voltage of 1.5V, with the 2C discharge capacity obtained. The obtained 2C discharge capacity was divided by the 0.2C discharge capacity to obtain the 2C capacity retention rate.
[0234] <Measurement of thickness ratio between first and second regions> (Pretreatment of secondary batteries) First, the secondary battery was put into a discharged state, and then disassembled to extract the electrode group including the composite layer. This disassembly was carried out in the air. Next, the extracted electrode group was immersed in pure water for 3 minutes and then dried at 100°C for 5 minutes.
[0235] (Cutting off the electrodes) Next, the electrode group was subjected to focused ion beam (FIB) processing, and the cut cross section was observed by SEM. Here, Hitachi's SMI3300SE and FEI's Strata 400s were used as FIB devices. The electrode group was cut at a position that divided the main surface of the electrode group into six equal parts in the short side direction when viewed from above, and five cross sections were obtained.
[0236] (Observation of the cross section of the electrode structure) After obtaining a cross section of the electrode group by the above FIB processing, the cross section of the electrode structure consisting of the electrode and the composite layer was observed by SEM. The SEM device used was U8020, manufactured by Hitachi High-Technologies Corporation. The region where the electrode and the composite layer existed was selected as the SEM observation site. The measurement conditions were a measurement magnification of 5000 times, and the SEM image displayed with a pixel count of 960 x 960 x 960 was converted to monochrome 256 gradations. The layer was divided into 2:8 in the thickness direction, with the side in contact with the negative electrode being the first region and the other being the second region.
[0237] (Binarization of SEM images) The obtained SEM images were subjected to binarization processing using ImageJ, with the median value of the brightness of the inorganic particles and the brightness of the resin in the composite layer being set as the threshold value.
[0238] (Calculation of thickness ratio of first region and second region) After detecting spherical or nearly spherical particles with high brightness in the composite layer in the binarized SEM image, the average particle diameter Rp [μm] per particle, which is the arithmetic mean value of the maximum and minimum diameters of each particle, was obtained. The average particle diameter of each particle was calculated by arithmetically averaging the Rp of each of all particles contained in the first region. In the composite layer, particles with an average particle diameter Rp of 3 μm or more were detected, and a cumulative frequency distribution of inorganic particles in the composite layer with an average particle diameter Rp of 3 μm or more was drawn in the thickness direction from the interface between the electrode and the composite layer to the surface of the composite layer facing the interface. At that time, the total number of inorganic particles with an average particle diameter Rp of 3 μm or more was standardized to 100. At this time, the range in which the cumulative frequency of inorganic particles is 0 to less than 25 in the axial direction of the thickness of the composite layer was defined as the first region, and the range in which the cumulative frequency of inorganic particles is 25 to 100 in the axial direction of the thickness of the composite layer. The ratio of the thickness of the first region or the thickness of the second region to the thickness of the composite layer is defined as the thickness ratio of the first region and the thickness ratio of the second region [%], respectively, below.
[0239] The above-mentioned operations from (observation of the cross section of the electrode structure) to (calculation of the thickness ratio of the first region and the second region) were performed for each cross section, and the ratio of the thickness of the first region to the thickness of the composite layer obtained for each cross section was arithmetically averaged. In the following measurements, the range of the first region was used as the arithmetically averaged value.
[0240] <Measurement of the average particle size of inorganic particles in the composite layer> First, the thickness ratio of the first region, which is a constant ratio calculated in the above-mentioned <Measurement of the thickness ratio of the first region and the second region>, was applied to each cross section imaged by SEM.
[0241] Next, in the first region of the SEM image that had been binarized using the method described above in (Binarization of SEM images), spherical or nearly spherical particles with high brightness were detected, and the average particle size Rp [μm] of each particle, which is the arithmetic mean of the maximum and minimum diameters of each particle, was calculated. This Rp calculation was performed for all particles contained in the first region. The Rp values obtained for all particles were arithmetically averaged to obtain the average particle size R of inorganic particles in the first region of one SEM image. 1-1 The above-mentioned R calculated for each SEM image was 1-1The average particle size R1 of the inorganic particles in the first region was obtained by arithmetically averaging the above values.
[0242] <Measurement of the number of inorganic particles N1 and N2> First, the thickness ratio of the first region, which is a constant ratio calculated in the above-mentioned <Measurement of the thickness ratio of the first region and the second region>, was applied to each cross section imaged by SEM.
[0243] Based on the <Measurement of the average particle size of inorganic particles in the composite layer>, the number of particles having an Rp of 0.2 μm or more and 3 μm or less was calculated separately in the first region and the second region from the Rp of each of all particles detected in the composite layer. The number of the above-mentioned particles in the first region was N 1-1 Let the number of the aforementioned particles in the second region be N 2-1 This N calculated for each SEM image was 1-1 and N 2-1 The desired numbers N1 and N2 were calculated by taking the arithmetic mean of each of these.
[0244] <Measurement of pore diameters P1 and P2 contained in the first and second regions> First, the thickness ratio of the first region 61, which is a constant ratio calculated in the above-mentioned <Measurement of the thickness ratio of the first region and the second region>, is applied to each cross section.
[0245] The SEM image described in (Observation of Cross Section of Electrode Structure) of <Measurement of Thickness Ratio of First Region and Second Region> was used. This SEM image was binarized using the median brightness between the brightness of the resin and the brightness of the interface between the composite layer and the active material-containing layer as a threshold value, so that the solid particles and binder were displayed in white and the voids in black. After extracting the black voids from the first region 61 of the obtained image, the pore diameter in the voids was calculated by the sphere arrangement method. That is, multiple virtual spheres were fitted to the voids under the constraint that the diameter of each sphere was maximized, and the arithmetic average of the diameters of each sphere was calculated as the pore diameter P. 1-1 The pore diameter P 1-1was calculated for each SEM image, and the arithmetic average was determined as the desired pore diameter P1. The above calculation was also applied to the second region to calculate the pore volume P2 in the second region.
[0246] <Porosity measurement> First, the thickness ratio of the first region 61, which is a constant ratio calculated in the above-mentioned <Measurement of the thickness ratio of the first region and the second region>, was applied to each cross section imaged by SEM.
[0247] The SEM image described in (Observation of the cross section of the electrode structure) in <Measurement of the thickness ratio of the first region and the second region> was used. This SEM image was binarized using a threshold value of the median brightness between the brightness of the resin and the brightness of the interface between the composite layer and the active material-containing layer, so that the solid particles and binder were displayed in white and the voids were displayed in black. The ratio of the number of black pixels corresponding to the voids to the number of all pixels in the SEM image was calculated to obtain the porosity.
[0248] Example 2 A battery was fabricated in the same manner as in Example 1, except that bimodal Al2O3 powder containing particles with modal diameters of both 0.7 μm and 5 μm in a mass ratio of 2:1 was used as the composite layer forming slurry 2.
[0249] Example 3 A battery was fabricated in the same manner as in Example 1, except that bimodal Al2O3 powder containing particles with modal diameters of both 0.7 μm and 5 μm in a mass ratio of 5:1 was used as the composite layer forming slurry 2.
[0250] Example 4 As the composite layer forming slurry 2, the Al2O3 powder described in Example 1 was prepared as the inorganic solid particles, and PVdF was prepared as the polymer material, and the inorganic solid particles and the polymer material were mixed in a mass ratio of 92:8, suspended in NMP as a solvent, and mixed for 30 minutes using a mixer. A battery was produced in the same manner as in Example 1, except as described above.
[0251] Example 5 As the composite layer forming slurry 2, the Al2O3 powder described in Example 1 was prepared as the inorganic solid particles, and PVdF was prepared as the polymer material, and the inorganic solid particles and the polymer material were mixed in a mass ratio of 94:6, suspended in NMP as a solvent, and mixed for 30 minutes using a mixer. A battery was produced in the same manner as in Example 1, except as described above.
[0252] Example 6 A battery was produced in the same manner as in Example 1, except that after the composite layer was applied to the surface layer of the negative electrode, the laminate was pressed at 2 kN.
[0253] Example 7 A battery was fabricated in the same manner as in Example 1, except that molybdenum sulfide powder (MoS) was used as the negative electrode active material.
[0254] Example 8 A battery was fabricated in the same manner as in Example 1, except that LATP was used as the inorganic particles in the composite layer forming slurries 1 and 2 instead of Al2O3 powder.
[0255] Example 9 A battery was fabricated in the same manner as in Example 1, except that bimodal Al2O3 powder containing particles with modal diameters of both 0.8 μm and 3 μm in a mass ratio of 5:1 was used as the composite layer forming slurry 2.
[0256] Example 10 A battery was fabricated in the same manner as in Example 1, except that bimodal Al2O3 powder containing particles with modal diameters of 0.6 μm and 5 μm in a mass ratio of 1:1 was used as the composite layer forming slurry 2.
[0257] Example 11 As the composite layer forming slurry 2, the Al2O3 powder described in Example 1 was prepared as the inorganic solid particles, and PVdF was prepared as the polymer material, and the inorganic solid particles and the polymer material were mixed in a mass ratio of 87:13, suspended in NMP as a solvent, and mixed for 30 minutes using a mixer. A battery was produced in the same manner as in Example 1, except as described above.
[0258] Example 12 A battery was produced in the same manner as in Example 1, except that after the composite layer was applied to the surface layer of the negative electrode, the laminate was pressed at 8 kN.
[0259] Comparative Example 1 Batteries were fabricated in the same manner as in Example 1, except that the composite layer forming slurries 1 and 2 were applied to thicknesses of 15 μm and 5 μm, respectively.
[0260] Comparative Example 2 Batteries were fabricated in the same manner as in Example 1, except that the composite layer forming slurries 1 and 2 were applied to thicknesses of 4 μm and 18 μm, respectively.
[0261] Comparative Example 3 A battery was fabricated in the same manner as in Example 1, except that after the composite layer was applied to the surface layer of the negative electrode, the laminate was pressed at 0.3 kN.
[0262] Comparative Example 4 A battery was fabricated in the same manner as in Comparative Example 2, except that MoS was used as the negative electrode active material.
[0263] Comparative Example 5 A battery was fabricated in the same manner as in Comparative Example 2, except that LATP was used as the inorganic particles in the composite layer forming slurries 1 and 2 instead of Al2O3 powder. [Table 1] [Table 2]
[0264] Table 1 shows the configuration of the electrode structure according to this embodiment and the evaluation results of secondary batteries prototyped using each electrode structure.
[0265] Examples 1 to 12 have higher charge / discharge efficiency and 2C capacity retention rate than Comparative Example 1. Unlike Comparative Example 1, Examples 1 to 12 have a configuration in which the thickness ratio of the first region of the composite layer is low, that is, the first region is 40% or less of the thickness of the composite layer from the interface between the electrode and the composite layer. Since the first region in Examples 1 to 12 is within the above-mentioned range, the thickness ratio of the second region is high, so that side reactions can be suppressed. This is because the ratio of the second region, which contains more inorganic particles with an average particle size of 3 μm or more than the first region and has a long path for water in the electrolyte to move, is sufficiently large. If the path for water in the electrolyte to move in the second region is long, the path for the solvent molecules, such as water in the electrolyte, to move toward the electrode through the pores of the composite layer becomes long. At this time, the solvent molecules, such as water, whose size is close to the pore diameter, can be suppressed from the composite layer to the active material-containing layer at a slower rate than lithium, which has a small ionic radius, so that side reactions such as electrolysis of water in the electrode can be suppressed.
[0266] In Examples 1 to 12, the charge / discharge efficiency and the 2C capacity retention rate are higher than those in Comparative Example 2, and the first region in Comparative Example 2 is 4%, which is less than 5% of the thickness of the composite layer from the interface between the electrode and the composite layer. In Examples 1 to 12, the thickness ratio of the first region is 5% or more, so that the movement of solvent molecules such as water in the electrolyte at the interface between the composite layer and the active material-containing layer can be sufficiently fast. As a result, it is presumed that the resistance acting on the above-mentioned interface can be reduced, and the 2C capacity retention rate is increased. In addition to the above comparison between Examples 1 to 12 and Comparative Example 1, it is found that the charge / discharge efficiency and the 2C capacity retention rate can be increased by the first region being 5% or more and 40% or less of the thickness of the composite layer from the interface between the electrode and the composite layer.
[0267] Examples 1 to 12 have a higher 2C capacity retention rate than Comparative Example 3. In Comparative Example 3, the ratio of R1 / R2 is greater than 1, which indicates that R1 is greater than R2. In contrast, in Examples 1 to 12, R1 is smaller than R2. In Examples 1 to 12, R2 is greater than R1, which increases the average particle size of the inorganic particles in the second region, and lengthens the path through which water in the electrolyte in the second region moves, making it possible to suppress side reactions. This is presumably why the 2C capacity retention rate is higher.
[0268] Comparing Example 1 and Example 9, Example 9 has higher charge / discharge efficiency and 2C capacity retention rate than Example 1. This is because R1 / R2 in Example 9 is in the more preferable range of 0.25 or more and 0.5 or less.
[0269] From the comparison of Example 1 with Example 2 and Example 3, it is found that Example 1 has a higher charge / discharge efficiency and 2C capacity retention rate. Example 1 has a larger N1 / N2 in the composite layer than Examples 2 and 3, and is configured to be 1.1 or more and 5.0 or less. That is, it is suggested that in Example 1, the number of particles N2 of 0.2 μm or more and 3 μm or less in the second region is smaller than that in the first region, and there are more alumina particles with an average particle size of 3 μm or more. Therefore, in Example 1, the path through which water in the electrolyte moves in the second region is longer. It is considered that the side reactions including electrolysis of water are suppressed by the longer path through which water moves in the electrolyte in the second region of the composite layer in Example 1, and as a result, the charge / discharge efficiency is high. From the above, it is inferred that the range of N1 / N2 is preferably 1.1 or more and 5.0 or less. In addition, in the comparison of Example 1 and Example 10, since the charge / discharge efficiency and 2C capacity retention rate are higher in Example 10 than in Example 1, it is inferred that N1 / N2 is more preferably in the more preferable range of 1.5 or more and 3.0 or less.
[0270] It can be seen that the charge / discharge efficiency and 2C capacity retention rate of Example 1 are higher than those of Examples 4 and 5. This is because the P1 / P2 in the composite layer of Example 1 is greater than 1 compared to Examples 4 and 5. This means that the size of the pores is smaller in the second region of Example 1, which can suppress the movement of solvent molecules such as water from the composite layer toward the electrode, and side reactions such as water electrolysis are suppressed, resulting in high charge / discharge efficiency. From the above, it is presumed that the range of P1 / P2 is preferably 1.1 or more and 2.0 or less. In addition, in a comparison between Example 1 and Example 11, the charge / discharge efficiency and 2C capacity retention rate of Example 11 are higher than those of Example 1, so it is presumed that P1 / P2 is preferably in the more preferable range of 1.1 or more and 1.2 or less.
[0271] The charge-discharge efficiency of Example 1 is higher than that of Example 6. The porosity of the composite layer of Example 1 is lower than that of Example 6. In Example 1, it is presumed that the low porosity of the composite layer results in a proton concentration distribution near the surface of the composite layer and near the interface between the electrode and the composite layer, resulting in a pH difference between the two. It is considered that the aforementioned pH difference in Example 1 compared to Example 6 results in a lower proton concentration in the active material layer, suppressing side reactions such as water electrolysis, and increasing the charge-discharge efficiency. From the above, it is presumed that the porosity of the composite layer is preferably in the more preferable range of 0.60% to 1.0%.
[0272] When comparing Comparative Examples 4 and 5 with Examples 6 and 7, it was confirmed that even when different materials were used for the active material and the inorganic particles of the composite layer compared to Example 1, the 2C capacity retention rate was increased by having the thickness ratio of the first region be 5% or more and 40% or less and R1 / R2 be 0.01 or more and 0.8 or less.
[0273] As described above, regardless of the active material and inorganic particles constituting the battery, the electrode structure according to the present embodiment has an electrode and a composite layer containing inorganic particles. The composite layer has a first region and a second region. The first region exists between the electrode and the second region. In the cumulative frequency distribution of the inorganic particles having an average particle size of 3 μm or more in the composite layer with respect to the thickness direction of the composite layer, when the total number of the inorganic particles having an average particle size of 3 μm or more is normalized to 100, and the first region is in the range where the cumulative frequency of the inorganic particles having an average particle size of 3 μm or more is 0 or more and less than 25, the first region is 5% or more and 40% or less of the thickness of the composite layer from the interface between the electrode and the composite layer. In the cross-sectional SEM image in the thickness direction of the composite layer, the average particle size R1 of the inorganic particles in the first region and the average particle size R2 of the inorganic particles in the second region satisfy the relationship R1 < R2, so that it is possible to achieve a low resistance while suppressing the electrolysis of water accompanying side reactions.
[0274] Although some embodiments of the present invention have been described, these embodiments are presented by way of example and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, replacements, and changes can be made without departing from the gist of the invention. These embodiments and their modifications are included in the scope and gist of the invention, and are included in the invention described in the claims and the equivalent scope thereof.
[0275] The following is an appendix according to the embodiment.
[0276] [1] An electrode and a composite layer containing inorganic particles, and the composite layer has a first region and a second region, the first region exists between the electrode and the second region, In the cumulative frequency distribution of the inorganic particles having an average particle size of 3 μm or more in the composite layer with respect to the thickness direction of the composite layer, when the total number of the inorganic particles having an average particle size of 3 μm or more is normalized to 100, and the first region is in the range where the cumulative frequency of the inorganic particles having an average particle size of 3 μm or more is 0 or more and less than 25, The first region is 5% or more and 40% or less of the thickness of the composite layer from the interface between the electrode and the composite layer, In the cross-sectional SEM image of the composite layer, an electrode structure for a secondary battery in which the average particle diameter R1 of the inorganic particles in the first region and the average particle diameter R2 of the inorganic particles in the second region satisfy the relationship R1 < R2.
[0277] [2] The electrode structure according to [1], wherein the number N1 of the inorganic particles having an average particle diameter of 0.2 μm or more and 3 μm or less in the first region and the number N2 of the inorganic particles having an average particle diameter of 0.2 μm or more and 3 μm or less in the second region satisfy the relationship N1 > N2.
[0278] [3] The electrode structure according to [2], wherein the ratio N1 / N2 of the number N1 of the inorganic particles having an average particle diameter of 0.2 μm or more and 3 μm or less to the number N2 of the inorganic particles having an average particle diameter of 0.2 μm or more and 3 μm or less is 1.1 or more and 5.0 or less.
[0279] [4] The electrode structure according to any one of [1] to [3], wherein the average pore diameter P1 in the first region and the average pore diameter P2 in the second region satisfy the relationship P1 < P2.
[0280] [5] The electrode structure according to [4], wherein the ratio P1 / P2 of the average pore diameter P1 to the average pore diameter P2 is 1.01 or more and 2.0 or less.
[0281] [6] The electrode structure according to any one of [1] to [5], wherein the ratio R1 / R2 of the average particle diameter R1 to the average particle diameter R2 is 0.01 or more and 0.8 or less.
[0282] [7] The electrode structure according to any one of [1] to [6], wherein the porosity of the composite layer is 0.10% or more and 4.0% or less.
[0283] [8] The electrode structure according to any one of [1] to [7], wherein the electrolyte is an aqueous electrolyte.
[0284] [9] [1] to [8], and and a counter electrode.
[0285]
[10] The secondary battery according to [9], wherein the counter electrode is a positive electrode.
[0286]
[11] A battery pack comprising the secondary battery according to [9] or
[10] .
[0287]
[12] An external terminal for supplying electricity; A protection circuit; The battery pack according to
[11] ,
[0288]
[13] The battery pack according to
[11] or
[12] , comprising a plurality of the secondary batteries, the plurality of secondary batteries being electrically connected in series, in parallel, or in a combination of series and parallel.
[0289]
[14] A vehicle equipped with a battery pack according to any one of claims
[11] to
[13] .
[0290]
[15] The vehicle described in
[14] , further comprising a mechanism for converting kinetic energy of the vehicle into regenerative energy.
[0291]
[16] A stationary power source comprising a battery pack according to any one of
[11] to
[13] . [Explanation of symbols]
[0292] 1...electrode group, 2...exterior member, 3...negative electrode, 3a...negative electrode current collecting layer, 3b...negative electrode active material-containing layer, 4...composite film, 4a...base material layer, 4b...composite layer, 5...positive electrode, 5a...positive electrode current collector, 5b...positive electrode active material-containing layer, 6...negative electrode terminal, 7...positive electrode terminal, 8...negative electrode gasket, 9...positive electrode gasket, 10...sealing plate, 11...control valve, 12...filling port, 13...sealing plug, 16...negative electrode lead 17 ... positive electrode lead, 21 ... bus bar, 22 ... positive electrode lead, 23 ... negative electrode lead, 24 ... adhesive tape, 31 ... container, 32 ... lid, 33 ... protective sheet, 34 ... printed wiring board, 35 ... wiring, 40 ... vehicle body, 50 ... electrode, 60 ... composite layer, 60a ... inorganic particles, 70 ... electrode structure, 100 ... secondary battery, 110 ... system, 111 ... power plant, 1 12...stationary power source, 113...demand side power system, 115...energy management system, 116...power grid, 117...communication network, 118...power conversion device, 121...demand side EMS, 122...power conversion device, 123...stationary power source, 200...battery pack, 300A...battery pack, 300B...battery pack, 310...casing, 320...opening, 332...output positive terminal, 333...output negative terminal, 342...positive connector, 343...negative connector, 345...thermistor, 346...protection circuit, 342a...wiring, 343a...wiring, 350...external terminal for current supply, 352...positive terminal, 353...negative terminal, 348a...positive wiring, 348b...negative wiring, 400...vehicle, 500...electrode structure.
Claims
1. An electrode; A composite layer containing inorganic particles, the composite layer having a first region and a second region; the first region is between the electrode and the second region, In a cumulative frequency distribution of the inorganic particles having an average particle size of 3 μm or more contained in the composite layer in the thickness direction of the composite layer, the total number of the inorganic particles having an average particle size of 3 μm or more is normalized to 100, and the first region is defined as a range in which the cumulative frequency of the inorganic particles having an average particle size of 3 μm or more is 0 or more and less than 25, the first region is 5% to 40% of the thickness of the composite layer from the interface between the electrode and the composite layer, An electrode structure for a secondary battery, in which, in a cross-sectional SEM image in the thickness direction of the composite layer, an average particle size R1 of the inorganic particles in the first region and an average particle size R2 of the inorganic particles in the second region satisfy the relationship R1 < R2.
2. 2. The electrode structure according to claim 1, wherein the number N1 of the inorganic particles having an average particle size of 0.2 μm or more and 3 μm or less in the first region and the number N2 of the inorganic particles having an average particle size of 0.2 μm or more and 3 μm or less in the second region satisfy the relationship N1 > N2.
3. 3. The electrode structure according to claim 2, wherein a ratio N1 / N2 of the number N1 of the inorganic particles having an average particle size of 0.2 μm or more and 3 μm or less to the number N2 of the inorganic particles having an average particle size of 0.2 μm or more and 3 μm or less is 1.1 or more and 5.0 or less.
4. The electrode structure according to claim 1 , wherein an average pore diameter P1 in the first region and an average pore diameter P2 in the second region satisfy a relationship of P1<P2.
5. 5. The electrode structure according to claim 4, wherein a ratio P1 / P2 of the average pore diameter P1 to the average pore diameter P2 is 1.01 or more and 2.0 or less.
6. 2. The electrode structure according to claim 1, wherein a ratio R1 / R2 of the average grain size R1 to the average grain size R2 is 0.01 or more and 0.8 or less.
7. The electrode structure according to claim 1 , wherein the porosity of the composite layer is 0.10% or more and 4.0% or less.
8. The electrode structure of claim 1 , wherein the electrolyte is a water-based electrolyte.
9. The electrode structure according to claim 1 ; and a counter electrode.
10. The secondary battery according to claim 9 , wherein the counter electrode is a positive electrode.
11. A battery pack comprising the secondary battery according to claim 9.
12. An external terminal for supplying electricity; A protection circuit; The battery pack of claim 11 , comprising:
13. The battery pack according to claim 11 , comprising a plurality of the secondary batteries, the plurality of secondary batteries being electrically connected in series, in parallel, or in a combination of series and parallel.
14. A vehicle comprising the battery pack according to claim 11.
15. The vehicle of claim 14 including a mechanism for converting kinetic energy of the vehicle into regenerative energy.
16. A stationary power source comprising the battery pack according to claim 11.
Citation Information
Patent Citations
Electrode group, secondary battery, battery pack, and vehicle
JP2018163870A
Separator, electrode group, secondary cell, battery pack, vehicle and stationary power supply
JP2021044205A
Non-aqueous electrolyte secondary battery
JP2022120400A
Method for manufacturing a separation membrane integrated electrode including a multi-layered inorganic layer and a separation membrane integrated electrode made by the same
JP2023506824A
Lithium secondary battery and its manufacturing method
JP2003077463A