Urethane-based adhesive composition

The urethane adhesive composition with a solvent SP value below 8.0 addresses solvent-induced swelling, ensuring efficient bonding and structural integrity by eliminating waiting time, enhancing construction efficiency.

JP2024139098APending Publication Date: 2024-10-09TOYOPOLYMER CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023049892
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Urethane adhesives cause swelling in bonded objects due to their solvents, leading to warping and gaps between bonded materials, particularly in applications like artificial turf where urethane backings swell, affecting construction efficiency and aesthetics.

Method used

A urethane adhesive composition with a solvent having a solubility parameter SP value of less than 8.0, primarily composed of aliphatic and cyclic hydrocarbon solvents, is used to minimize solvent-induced swelling, eliminating the need for waiting time after application.

Benefits of technology

The composition effectively suppresses swelling in urethane-based materials, ensuring efficient bonding without waiting for solvent evaporation, maintaining structural integrity and improving construction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139098000001
    Figure 2024139098000001
Patent Text Reader

Abstract

To provide an urethane-based adhesive composition which can lower a degree of influence of a solvent of an urethane-based adhesive on an adhesive object, and can suppress swelling of the urethane resin.SOLUTION: An urethane-based adhesive composition contains an urethane prepolymer and a solvent, where the urethane prepolymer has an isocyanate group at a terminal, the isocyanate group at the terminal is derived from at least one of diphenylmethane diisocyanate and modified diphenylmethane diisocyanate, and the solvent contains 50 wt.% or more of a solvent having a solubility parameter SP value of less than 8.0 with respect to the total amount of the solvent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a urethane adhesive composition. [Background technology]

[0002] Conventionally, urethane adhesives have been used to attach floor finishing materials to buildings. Examples of floor finishing materials include polymer-based flooring materials such as vinyl flooring materials, linoleum flooring materials, and rubber flooring materials, tile carpets, wood flooring materials, and artificial turf. The urethane adhesives contain a solvent that dissolves urethane prepolymers well. For example, ethyl acetate or the like is used as the solvent (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2004-2748 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the object to be bonded to which the urethane adhesive is applied may swell due to the solvent of the urethane adhesive. For example, when the object to be bonded is a urethane resin, swelling may occur in the object to be bonded. As a result, the swollen object to be bonded may warp, or when a plurality of objects to be bonded are arranged closely together and bonded, gaps (openings) may occur between the objects to be bonded. Thus, there is a demand for a urethane adhesive composition that can suppress the swelling of the object to be bonded.

[0005] The present invention is devised to solve the above-mentioned problems, and has an object to provide a urethane-based adhesive composition that can reduce the degree of effect of the solvent of the urethane adhesive on the object to be bonded, thereby suppressing swelling of the object to be bonded. [Means for solving the problem]

[0006] The urethane adhesive composition of the present invention contains a urethane prepolymer and a solvent, The urethane prepolymer has an isocyanate group at a terminal thereof, the terminal isocyanate group is derived from at least one of diphenylmethane diisocyanate and modified diphenylmethane diisocyanate, The solvent contains 50% by weight or more of a solvent having a solubility parameter SP value of less than 8.0 based on the total amount of the solvent.

[0007] In the urethane adhesive composition of the present invention, the solvent having a solubility parameter SP value of less than 8.0 is preferably at least one selected from aliphatic hydrocarbon solvents and cyclic hydrocarbon solvents.

[0008] In the urethane adhesive composition of the present invention, it is preferred that the solvent contains a solvent having a solubility parameter SP value of less than 8.0 and a solvent having a solubility parameter SP value of 8.0 or more, and that the solvent average SP value is less than 9.7. Effect of the Invention

[0009] According to the present invention, it is possible to provide a urethane adhesive composition that can reduce the degree of effect of the solvent in the urethane adhesive on an object to be adhered, thereby suppressing swelling of the urethane resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] <Constituents of the urethane adhesive composition> The urethane adhesive composition according to an embodiment of the present invention contains a urethane prepolymer and a solvent. The urethane prepolymer has an isocyanate group at a terminal thereof, and the terminal isocyanate group is derived from at least one of diphenylmethane diisocyanate and modified diphenylmethane diisocyanate. The solvent contains a solvent having a solubility parameter SP value of less than 8.0 in an amount of 50% by weight or more based on the total amount of the solvent.

[0011] Conventionally, when a urethane adhesive is applied to some materials, the materials swell due to the solvent contained in the urethane adhesive. In order to prevent swelling in materials that swell due to the urethane adhesive, the present inventors focused on the solubility parameter SP value, which relates to the solubility (swelling) property of the solvent.

[0012] With this configuration, the urethane adhesive composition according to the embodiment can suppress swelling of materials such as polyurethane (urethane rubber) that would conventionally swell when a urethane adhesive is applied. In order to prevent swelling, it is not necessary to wait for the solvent to evaporate after application of the urethane adhesive, as in the past. This eliminates the need for an open time until lamination, improving workability. In addition, when waiting for the solvent to evaporate, the adhesive may dry faster than expected, resulting in a decrease in adhesive strength. However, the urethane adhesive composition according to the embodiment does not require a waiting time, and therefore does not have the disadvantage of a decrease in adhesive strength due to the waiting time.

[0013] The urethane adhesive composition according to the embodiment can be suitably used for bonding polyurethane (urethane rubber). For example, the SP value of polyurethane (urethane rubber) is 10. The present inventors have found that in order to dissolve the urethane prepolymer while suppressing dissolution and swelling of the urethane (molded product, urethane sole, etc.) after curing (after crosslinking), it is important that the solvent contains 50% by weight or more of a solvent with an SP value of less than 8.0 relative to the total amount of the solvent.

[0014] An example of adhering an artificial turf sheet having a urethane backing, that is, an artificial turf sheet whose back surface is made of urethane, will be described. In this case, the urethane adhesive composition is used as an artificial turf adhesive composition. Conventional urethane adhesives tend to easily cause urethane to swell because the solvent dissolves the urethane. When the urethane backing of the artificial turf swells, the artificial turf warps, and the artificial turf may lift at the joint between the artificial turfs or have gaps (gaps) in the turf. However, the urethane adhesive composition according to the embodiment suppresses the swelling of the urethane backing. Furthermore, in order to suppress the swelling of the urethane backing, it was necessary to wait for the solvent to evaporate after the adhesive was applied before attaching the sheet. However, with the adhesive of the present invention, no waiting time (open time) is required for the solvent to evaporate.

[0015] A catalyst for accelerating the curing reaction at low temperatures may be added to the urethane adhesive composition according to the embodiment, and known additives may be added according to other purposes. Each of the above components will be described in detail below.

[0016] (1) Urethane prepolymer In the present invention, the urethane prepolymer is an isocyanate compound obtained by addition reaction of an isocyanate group with a main chain component, and is usually obtained by reacting a polyol with an isocyanate. In the present invention, the urethane prepolymer has an isocyanate group at its terminal, and the terminal isocyanate group is derived from at least one of diphenylmethane diisocyanate and modified diphenylmethane diisocyanate. The urethane prepolymer hardens when the terminal isocyanate group (NCO) reacts with moisture in the air or adsorbed water on the surface of the adherend.

[0017] The polyol refers to polyethylene glycol, polypropylene glycol, neopentyl glycol, polyether glycol having active hydrogen, polyester glycol, polyether triol, etc., and other modified polyols. Specifically, as the polyether glycol, polyoxyethylene diol, polyoxypropylene diol, polyoxybutylene diol, polytetramethylene diol, etc. can be used. As the polyester glycol, there are poly(ethylene adipate) glycol, poly(propylene adipate) glycol, poly(ethylene butylene adipate) glycol, poly(neopentyl sebacate) glycol, etc. In addition, as various triols and modified polyols, there are castor oil modified polyol, epoxy modified polyol, etc. The molecular weight of these is preferably 200 to 9,000, more preferably 500 to 5,000, in terms of number average molecular weight.

[0018] Needless to say, other than the above-mentioned polyols, any other main chain component can be used as long as it can add an isocyanate group to the end and has a structure that does not inhibit the urethane-forming reaction, such as polyamines and polyamides.

[0019] As such a urethane prepolymer, a prepolymer obtained by reacting a polyether polyol or a polyester polyol (bifunctional or trifunctional) with 4,4-diphenylmethane diisocyanate (MDI), 2,4-diphenylmethane diisocyanate, or polymeric diphenylmethane diisocyanate can be suitably used.

[0020] Diphenylmethane diisocyanate is sold by Tosoh Corporation under the names Millionate MT, MT-F, MTNBP, NM, etc. Polymeric diphenylmethane diisocyanate is sold by Tosoh Corporation under the names Millionate MR-100, MR-200, MR-400, etc., and by BASF under the name "Lupranate" (registered trademark) M20S, etc.

[0021] The isocyanate reacted to obtain the urethane prepolymer may contain 4,4-diphenylmethane diisocyanate (MDI), 2,4-diphenylmethane diisocyanate, or polymeric diphenylmethane diisocyanate as well as isocyanates other than 4,4-diphenylmethane diisocyanate (MDI), 2,4-diphenylmethane diisocyanate, and polymeric diphenylmethane diisocyanate. For example, aliphatic isocyanates such as methylene diisocyanate, ethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, lysine diisocyanate (LDI), and 1,3,6-hexamethylene triisocyanate; alicyclic isocyanates such as hydrogenated 4,4'-diphenylmethane diisocyanate (hydrogenated MDI), hydrogenated xylylene diisocyanate (hydrogenated XDI), 1,4-cyclohexane diisocyanate, hydrogenated 2,4-tolylene diisocyanate (hydrogenated TDI), and isophorone diisocyanate (IPDI); The isocyanate may include one or more isocyanates selected from the group consisting of aromatic aliphatic isocyanates such as tetramethyl xylylene diisocyanate (TMXDI), 1,4-diphenyl diisocyanate, 2,4- or 2,6-tolylene diisocyanate (TDI), 1,5-naphthalene diisocyanate (NDI), 3,3'-dimethyl-4,4'-diphenylmethane diisocyanate, O-tolidine diisocyanate, crude TDI, polyphenylmethane polyisocyanate (crude MDI), triphenylmethane triisocyanate, and aromatic isocyanates such as tris(isocyanatephenyl)thiophosphate.

[0022] The number average molecular weight of the urethane prepolymer is preferably in the range of 1,000 to 30,000, more preferably in the range of 1,200 to 20,000. If the molecular weight is 30,000 or less, the drying property is good. Since the molecular weight is 1,000 or more, there is no problem in terms of foaming.

[0023] For example, a urethane prepolymer with a molecular weight peak of about 2,500 can be used, which is prepared by reacting 100 parts by weight of the polyol with 25 parts by weight of isocyanate at 80°C for 5 hours, with the polyol being polypropylene glycol (molecular weight about 2,000) and the isocyanate group-imparting substance being 4,4'-MDI. Note that unreacted isocyanate remains.

[0024] Alternatively, a urethane prepolymer having a molecular weight peak of about 2,500 may be used, in which the polyol is polypropylene glycol (molecular weight about 2,000), the isocyanate group-imparting substances are 2,4'-MDI and 4,4'-MDI, and 100 parts by weight of this polyol mixture and 25 parts by weight of an isocyanate mixture are reacted at 80°C for 5 hours. Note that unreacted isocyanate remains.

[0025] (2) Solvent The urethane adhesive composition of the present invention contains a solvent having a solubility parameter SP value of less than 8.0 in an amount of 50% by weight or more based on the total amount of the solvent. The solubility parameter SP value in the present invention is the Hildebrand solubility parameter (unit: (cal / cm) 1 / 2 In this specification, unless otherwise specified, the SP value is the SP value at 25° C. and 1 atm. The solubility parameters of the compounds and trade names exemplified below are only examples.

[0026] Solvents with a solubility parameter SP value of less than 8.0 include isoparaffin (light isoparaffin, Class 4, Class 2 petroleum, SP value 7.4 to 7.6), methylcyclohexane (SP value 7.8), isopropyl ether (Class 4, Class 1 petroleum, SP value 6.9), normal hexane (Class 4, Class 1 petroleum, SP value 7.3), normal paraffin (Class 4, Class 2 or Class 3 petroleum, SP value 7.8 to 7.9), isohexane (Class 4, Class 1 petroleum, SP value 7.1), naphthenes (Class 4, Class 2 petroleum, SP value 7.8 to 7.9), alkylbenzenes (Class 4, Class 3 petroleum, SP value 7.2 to 7.6), nonylbenzene (Class 4, Class 3 petroleum, SP value 7.9), and the like. Here, in the fourth category, the first petroleum has a flash point of less than 21°C, the second petroleum has a flash point of 21°C or more and less than 70°C, the third petroleum has a flash point of 70°C or more and less than 200°C, and the fourth petroleum has a flash point of 200°C or more. Generally, the lower the flash point, the better the drying property. In the present invention, the solvent having a solubility parameter SP value of less than 8.0 is preferably at least one selected from aliphatic hydrocarbon solvents and cyclic hydrocarbon solvents, since it suppresses swelling of the substrate and improves volatility, and carbonate esters, fatty acid esters, etc., having a flash point in the range of 70°C or more and less than 200°C are preferable.

[0027] For example, the isoparaffin-based hydrocarbon solvent may be IP Solvent 1620 (Idemitsu Kosan Co., Ltd., Hydrocarbon Solvent (Light Isoparaffin), SP value 7.4), Isozol 200 (ENEOS Corporation, 4th Class 1 Petroleum, SP value 7.4), Isozol 300 (ENEOS Corporation, 4th Class 2 Petroleum, SP value 7.5), or Isozol 400 (ENEOS Corporation, 4th Class 3 Petroleum, SP value 7.6). For example, the normal paraffin-based solvent may be normal paraffin series (ENEOS Corporation, 4th Class 2 or 3 Petroleum, SP value 7.8 to 7.9). For example, the naphthenic solvent may be naphthesol LL (JXTG Energy Corporation, 4th Class 2 Petroleum, SP value 7.8), or naphthesol L (JXTG Energy Corporation, 4th Class 2 Petroleum, SP value 7.9). The urethane adhesive composition according to the embodiment contains at least one solvent selected from these solvents.

[0028] In the urethane adhesive composition of the present invention, the solvent contains 50% by weight or more of a solvent having a solubility parameter SP value of less than 8.0, but the remaining solvent may contain a solvent having a solubility parameter SP value of 8.0 or more. In that case, the average solvent SP value is preferably less than 9.7, more preferably less than 9.0. Here, the average solvent SP value is a value obtained by multiplying the volume fraction of each solvent by the solubility parameter SP value of that solvent and summing them. As a solvent having a solubility parameter SP value of 8.0 or more, ethyl acetate (SP value 9.1), dimethyl carbonate (SP value 9.9), etc., which are solvents capable of diluting general urethane, can be used. When such a solvent is contained, the polyurethane, which is the adherend (object to be bonded), is slightly swollen, but if the content is 50% by weight or less while the average solvent SP value is less than 9.7, the swelling is suppressed within an acceptable range. Furthermore, if the average solvent SP value is less than 9.7, it is preferable because the curing property at low temperatures can be improved.

[0029] (3) Additives The urethane adhesive composition of the present invention may contain fillers, curing catalysts, diluents (such as solvents having a solubility parameter SP value of 8.0 or more), stabilizers, pigments, antioxidants and other additives, provided such additions do not impair the spirit and scope of the present invention.

[0030] Examples of the filler include calcium carbonate, carbon black, clay, talc, mica, titanium oxide, zeolite, diatomaceous earth, and silica, and these can be used alone or in combination. Examples of the calcium carbonate include ground calcium carbonate and surface-treated calcium carbonate. Silica and surface-treated calcium carbonate can be used as thixotropy-imparting agents.

[0031] Among diluents, examples of solvents with a solubility parameter SP value of 8.0 or more include dimethyl carbonate (Class 4, Class 1 petroleum, SP value 9.9) and propylene carbonate (Class 4, Class 3 petroleum, SP value 13.3). Addition of propylene carbonate improves workability and is preferable. Solvents with a solubility parameter SP value of 8.0 or more can be added in an amount of less than 50% by weight based on the total amount of solvent.

[0032] As the curing catalyst, metal catalysts such as dibutyltin dilaurate, cobalt naphthenate, stannous chloride, and tetra-n-butyltin can be used. As the amine catalysts, triethylamine, triethylenediamine, morpholino ether, imidazole, and the like can be used. Amine catalysts have better low-temperature curing properties than metal catalysts, so it is preferable to use amine catalysts. In the urethane adhesive composition of the present invention, the curing catalyst is preferably in the range of 0.1% by mass or more and less than 2.0% by mass based on the total amount. If the catalyst is too little, the curing is weak, and if the catalyst is too much, the storage stability is impaired. This range of catalyst addition is particularly effective when 2,2-dimorpholino diethyl ether, a tertiary amine, is used as the curing catalyst, as there are no problems in terms of both curing and storage stability.

[0033] Other additives include silane coupling agents, titanate coupling agents, ultraviolet absorbers, antioxidants, drying agents, tackifiers, etc., which may be used alone or in combination.

[0034] The adhesive of the present invention is particularly suitable for use on artificial turf with a urethane backing. In the case of artificial turf, the adhesive is applied in an amount of, for example, 1500 g / m 2 (For other uses, 350g / m 2 However, since sand is often added the day after application, it is desirable for the material to harden the next day, even in the low temperatures of winter. In structures other than artificial turf, there are cases where design requires the suppression of structural displacement caused by swelling, and the material can also be used for long polyvinyl chloride sheets, rubber tiles, linoleum sheets, composition tiles, homogenous tiles, cork tiles, wood flooring, etc.

[0035] <Method of producing urethane adhesive composition> The method for producing the urethane adhesive composition may be a known method, and is not particularly limited as long as the produced urethane adhesive composition does not impair the object of the present invention. The urethane adhesive composition according to the embodiment of the present invention can be produced, for example, by the following method.

[0036] For example, a urethane prepolymer is produced by putting a predetermined amount of polyol and a predetermined amount of isocyanate including at least one of diphenylmethane diisocyanate and modified diphenylmethane diisocyanate into a reaction vessel and then heating the vessel. In producing the urethane prepolymer, the reaction is carried out under conditions in which the isocyanate groups of the isocyanate are in excess relative to the hydroxyl groups of the polyol. The reaction is usually carried out at a temperature of 50 to 120°C, preferably 70 to 110°C. The reaction time is usually 1 to 15 hours.

[0037] A thixotropic agent, filler, and curing catalyst were added to the obtained urethane prepolymer and stirred uniformly, and a solvent was added to adjust the viscosity to obtain a polyurethane adhesive. The amount of the additives was adjusted so that the viscosity of the mixture (adhesive) was 10,000 to 30,000 mPa s (25°C).

[0038] The urethane prepolymer can be produced without a solvent. However, the urethane prepolymer can be produced by reacting a polyol with an isocyanate in a solvent. The polyol and isocyanate used in producing the urethane prepolymer are blended such that the equivalent ratio (NCO group / OH group) of the isocyanate group of the isocyanate to the hydroxyl group of the polyol is preferably within a range of 1.1 to 5.0, more preferably within a range of 1.5 to 2.0. EXAMPLES

[0039] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these.

[0040] The urethane prepolymers used in the examples and comparative examples are as follows: [Urethane prepolymer] Polyol: Polypropylene glycol (molecular weight approximately 2000) Isocyanate group-adding material: 2,4'-MDI 4,4'-MDI 100 parts by weight of this polyol mixture and 25 parts by weight of the isocyanate mixture were reacted at 80° C. for 5 hours to obtain a substance with a molecular weight peak of about 2500. Naturally, unreacted isocyanate remained.

[0041] [Example 1] 1. Preparation of urethane adhesive composition A urethane adhesive composition of this example was obtained by mixing 50 parts by mass of urethane prepolymer, 22 parts by mass of heavy calcium carbonate (filler, "Super SS" manufactured by Maruo Calcium Co., Ltd.), 13 parts by mass of surface-treated calcium carbonate (thixotropy imparting agent, "Kalfine 200M" manufactured by Maruo Calcium Co., Ltd.), 0.4 parts by mass of 2,2-dimorpholinodiethyl ether (curing catalyst), and 15 parts by mass of "Isol 200" (aliphatic hydrocarbon solvent, isoparaffinic hydrocarbon solvent manufactured by ENEOS Corporation, SP value 7.4).

[0042] 2. Evaluation of the physical properties of urethane adhesive compositions (1) Evaluation of swelling (lifting, warping) 2 hours after lamination a. Preparation of test specimens In a temperature environment of 25°C, the urethane adhesive composition of Example 1 was applied to the flat surface of a flexible board at a rate of 450 g / m 2 Immediately after applying the coating amount, a urethane resin sheet measuring 25 mm in length and 175 mm in width was laminated to the flexible board. The flexible board complies with the JIS A 5430 standard. The urethane resin sheet is a 0.5 mm thick film-like urethane resin obtained by drying Pollinate 977, a one-liquid urethane resin composition manufactured by Toyo Polymer Co., Ltd. After laminating the urethane resin sheet to the flexible board, it was left for 2 hours in a temperature environment of 25°C.

[0043] b.Measurement method The test piece was placed on a horizontal plane after being left for 2 hours in a temperature environment of 25°C, and the change in shape of the urethane resin sheet in a direction perpendicular to the plane, i.e., the warping of the urethane resin sheet, was measured with a metal straightedge. In this measurement, the evaluation was made according to the following criteria. A: Less than 1.5 mm B: 1.5mm or more and less than 2mm C: 2mm or more

[0044] If a sheet becomes loose, gaps will appear at the joints (between the sheets) even if the sheets are lined up without any gaps. In the case of construction products such as artificial turf, looseness of 2mm or more is noticeable and leads to a decrease in aesthetic appearance. Furthermore, looseness of 2mm or more can be difficult to correct due to the pressure applied after adhesion. Thus, in this evaluation, looseness of less than 2mm is desirable, and less than 1.5mm is even more desirable.

[0045] The urethane adhesive composition of this example had a lift of less than 1.5 mm and was rated "A" in this evaluation.

[0046] (2) Curing property (25℃) evaluation a. Preparation of test specimens In a temperature environment of 25°C, the urethane adhesive composition of Example 1 was applied at 450 g / m 2 Immediately after applying the coating, the urethane resin sheet having a length of 25 mm and a width of 175 mm was attached to the flexible board. After the flexible board and the urethane resin sheet were attached to each other, the flexible board and the urethane resin sheet were left in a temperature environment of 25° C. for 16 hours.

[0047] b.Measurement method For the test pieces that had been left for 16 hours in a 25°C environment, a portion of the sheet was peeled off from the flexible board, and the film of adhesive composition remaining on the flexible board or sheet was scratched with a needle to evaluate the condition of the film (see JIS K 5600-1-1). In this measurement, the evaluation was made according to the following criteria. Hardening: Semi-hardened state (needle marks remain on the film, but it cannot be pulled) Curing △: Dry to the touch (film can be pulled with a needle)

[0048] In the urethane adhesive composition of this example, the adhesive film was in a semi-cured state 16 hours after application, and was rated as "good" in this evaluation.

[0049] (3) Curing property (5℃) evaluation a. Preparation of test specimens In a temperature environment of 5° C., the urethane adhesive composition of Example 1 was applied at 450 g / m 2 Immediately after applying the coating, a urethane resin sheet measuring 25 mm in length and 175 mm in width was attached to the flexible board. After the flexible board and the urethane resin sheet were attached to each other, the board was left in a 5°C environment for 16 hours.

[0050] b.Measurement method For the test pieces that had been left for 16 hours in an environment at 5°C, a portion of the sheet was peeled off from the flexible board, and the film of the adhesive composition remaining on the flexible board or sheet was scratched with a needle to evaluate the condition of the film (see JIS K 5600-1-1). In this measurement, the evaluation was made according to the following criteria. Hardening: Semi-hardened state (needle marks remain on the film, but it cannot be pulled) Curing △: Dry to the touch (film can be pulled with a needle) In the urethane adhesive composition of this example, the adhesive film was in a semi-cured state 16 hours after application, and was rated as "good" in this evaluation.

[0051] (4) Overall Judgment If the swelling (lifting, warping) evaluation 2 hours after lamination was A or B and the curing evaluation at 25°C was "◯", it was rated as "G", and the rest were rated as "NG". In this example, it was rated as "G".

[0052] [Example 2] 1. Preparation of urethane adhesive composition A urethane adhesive composition was obtained in the same manner as in Example 1 by mixing 50 parts by mass of urethane prepolymer, 22 parts by mass of heavy calcium carbonate (filler, "Super SS" manufactured by Maruo Calcium Co., Ltd.), 13 parts by mass of surface-treated calcium carbonate (thixotropy imparting agent, "Kalfine 200M" manufactured by Maruo Calcium Co., Ltd.), 0.4 parts by mass of 2,2-dimorpholinodiethyl ether (curing catalyst), 10 parts by mass of "Isol 200" (aliphatic hydrocarbon solvent, isoparaffinic hydrocarbon solvent manufactured by ENEOS Corporation, SP value 7.4), and 5 parts by mass of propylene carbonate (solvent, SP value 13.3).

[0053] 2. Evaluation of the physical properties of urethane adhesive compositions The physical properties of the obtained urethane adhesive composition were evaluated in the same manner as in Example 1. Swelling (lifting, warping) 2 hours after lamination using the urethane adhesive composition of this example was less than 1.5 mm, and was rated as "A." Curability (25°C) was rated as "good," with the adhesive film in a semi-cured state 16 hours after application. Curability (5°C) was rated as "good," with the adhesive film in a semi-cured state 16 hours after application. Therefore, the overall rating was "G."

[0054] [Example 3] 1. Preparation of urethane adhesive composition A urethane adhesive composition was obtained in the same manner as in Example 1 by mixing 50 parts by mass of urethane prepolymer, 22 parts by mass of heavy calcium carbonate (filler, "Super SS" manufactured by Maruo Calcium Co., Ltd.), 13 parts by mass of surface-treated calcium carbonate (thixotropy imparting agent, "Kalfine 200M" manufactured by Maruo Calcium Co., Ltd.), 0.4 parts by mass of 2,2-dimorpholinodiethyl ether (curing catalyst), 10 parts by mass of "Isol 200" (aliphatic hydrocarbon solvent, isoparaffinic hydrocarbon solvent manufactured by ENEOS Corporation, SP value 7.4), and 5 parts by mass of dimethyl carbonate (solvent, SP value 9.9).

[0055] 2. Evaluation of the physical properties of urethane adhesive compositions The physical properties of the obtained urethane adhesive composition were evaluated in the same manner as in Example 1. Swelling (lifting, warping) 2 hours after lamination using the urethane adhesive composition of this example was 1.5 mm or more and less than 2 mm, and was rated as "B." Curability (25°C) was rated as "good," with the adhesive film being in a semi-cured state 16 hours after application. Curability (5°C) was rated as "good," with the adhesive film being in a semi-cured state 16 hours after application. Therefore, the overall rating was "G."

[0056] [Example 4] 1. Preparation of urethane adhesive composition A urethane adhesive composition was obtained in the same manner as in Example 1 by mixing 50 parts by mass of urethane prepolymer, 22 parts by mass of heavy calcium carbonate (filler, "Super SS" manufactured by Maruo Calcium Co., Ltd.), 13 parts by mass of surface-treated calcium carbonate (thixotropy imparting agent, "Calcine 200M" manufactured by Maruo Calcium Co., Ltd.), 0.4 parts by mass of 2,2-dimorpholinodiethyl ether (curing catalyst), and 15 parts by mass of methylcyclohexane (solvent, SP value 7.8).

[0057] 2. Evaluation of the physical properties of urethane adhesive compositions The physical properties of the obtained urethane adhesive composition were evaluated in the same manner as in Example 1. Swelling (lifting, warping) 2 hours after lamination using the urethane adhesive composition of this example was less than 1.5 mm, and was rated as "A." Curability (25°C) was rated as "good," with the adhesive film in a semi-cured state 16 hours after application. Curability (5°C) was rated as "good," with the adhesive film in a semi-cured state 16 hours after application. Therefore, the overall rating was "G."

[0058] [Example 5] 1. Preparation of urethane adhesive composition A urethane adhesive composition was obtained in the same manner as in Example 1 by mixing 50 parts by mass of urethane prepolymer, 22 parts by mass of heavy calcium carbonate (filler, "Super SS" manufactured by Maruo Calcium Co., Ltd.), 13 parts by mass of surface-treated calcium carbonate (thixotropy imparting agent, "Kalfine 200M" manufactured by Maruo Calcium Co., Ltd.), 0.4 parts by mass of 2,2-dimorpholinodiethyl ether (curing catalyst), 7.5 parts by mass of "Isol 200" (aliphatic hydrocarbon solvent, isoparaffinic hydrocarbon solvent manufactured by ENEOS Corporation, SP value 7.4), and 7.5 parts by mass of dimethyl carbonate (solvent, SP value 9.9).

[0059] 2. Evaluation of the physical properties of urethane adhesive compositions The physical properties of the obtained urethane adhesive composition were evaluated in the same manner as in Example 1. Swelling (lifting, warping) 2 hours after lamination using the urethane adhesive composition of this example was 1.5 mm or more and less than 2 mm, and was rated as "B." Curability (25°C) was rated as "good," with the adhesive film being in a semi-cured state 16 hours after application. Curability (5°C) was rated as "good," with the adhesive film being in a semi-cured state 16 hours after application. Therefore, the overall rating was "G."

[0060] [Example 6] 1. Preparation of urethane adhesive composition A urethane adhesive composition was obtained in the same manner as in Example 1 by mixing 50 parts by mass of urethane prepolymer, 22 parts by mass of heavy calcium carbonate (filler, "Super SS" manufactured by Maruo Calcium Co., Ltd.), 13 parts by mass of surface-treated calcium carbonate (thixotropy imparting agent, "Kalfine 200M" manufactured by Maruo Calcium Co., Ltd.), 0.4 parts by mass of 2,2-dimorpholinodiethyl ether (curing catalyst), 7.5 parts by mass of "Isol 200" (aliphatic hydrocarbon solvent, isoparaffinic hydrocarbon solvent manufactured by ENEOS Corporation, SP value 7.4), and 7.5 parts by mass of propylene carbonate (solvent, SP value 13.3) (average solvent SP value 9.7).

[0061] 2. Evaluation of the physical properties of urethane adhesive compositions The physical properties of the obtained urethane adhesive composition were evaluated in the same manner as in Example 1. The swelling (floating, warping) 2 hours after lamination using the urethane adhesive composition of this example was 1.5 mm or more and less than 2 mm, and was rated as "B." The curability (25°C) was rated as "good," as the adhesive film was in a semi-cured state 16 hours after application. Therefore, the overall rating was "G." Furthermore, in Example 6, the curability (5°C) was rated as "△," as the adhesive film was dry to the touch 16 hours after application, indicating that if the solvent average SP value is less than 9.7, the curability at low temperatures is better.

[0062] [Comparative Example 1] 1. Preparation of urethane adhesive composition A urethane adhesive composition was obtained in the same manner as in Example 1 by mixing 50 parts by mass of urethane prepolymer, 22 parts by mass of heavy calcium carbonate (filler, "Super SS" manufactured by Maruo Calcium Co., Ltd.), 13 parts by mass of surface-treated calcium carbonate (thixotropy imparting agent, "Kalfine 200M" manufactured by Maruo Calcium Co., Ltd.), 0.4 parts by mass of 2,2-dimorpholinodiethyl ether (curing catalyst), 5 parts by mass of "Isol 200" (aliphatic hydrocarbon solvent, isoparaffinic hydrocarbon solvent manufactured by ENEOS Corporation, SP value 7.4), and 10 parts by mass of dimethyl carbonate (solvent, SP value 9.9).

[0063] 2. Evaluation of the physical properties of urethane adhesive compositions The physical properties of the obtained urethane adhesive composition were evaluated in the same manner as in Example 1. The swelling (floating, warping) of the urethane adhesive composition according to this example 2 hours after bonding was 2 mm or more (specifically, 3 mm), and was rated as "C." The curability (25°C) was rated as "good," as the adhesive film was in a semi-cured state 16 hours after application. The curability (5°C) was rated as "good," as the adhesive film was in a semi-cured state 16 hours after application. Therefore, the overall rating was "NG."

[0064] [Comparative Example 2] 1. Preparation of urethane adhesive composition A urethane adhesive composition was obtained in the same manner as in Example 1 by mixing 50 parts by mass of urethane prepolymer, 22 parts by mass of heavy calcium carbonate (filler, "Super SS" manufactured by Maruo Calcium Co., Ltd.), 13 parts by mass of surface-treated calcium carbonate (thixotropy imparting agent, "Kalfine 200M" manufactured by Maruo Calcium Co., Ltd.), 0.4 parts by mass of 2,2-dimorpholinodiethyl ether (curing catalyst), 5 parts by mass of "Isol 200" (aliphatic hydrocarbon solvent, isoparaffinic hydrocarbon solvent manufactured by ENEOS Corporation, SP value 7.4), and 10 parts by mass of propylene carbonate (solvent, SP value 13.3).

[0065] 2. Evaluation of the physical properties of urethane adhesive compositions The physical properties of the obtained urethane adhesive composition were evaluated in the same manner as in Example 1. The swelling (floating, warping) of the urethane adhesive composition according to this example 2 hours after lamination was 2 mm or more (specifically, 4 mm), and it was rated as "C". The curability (25°C) was rated as "good", as the adhesive film was in a semi-cured state 16 hours after application. The curability (5°C) was rated as "good", as the adhesive film was dry to the touch 16 hours after application. Therefore, the overall verdict was "NG".

[0066] [Comparative Example 3] 1. Preparation of urethane adhesive composition A urethane adhesive composition was obtained in the same manner as in Example 1 by mixing 50 parts by mass of urethane prepolymer, 22 parts by mass of heavy calcium carbonate (filler, "Super SS" manufactured by Maruo Calcium Co., Ltd.), 13 parts by mass of surface-treated calcium carbonate (thixotropy imparting agent, "Calcine 200M" manufactured by Maruo Calcium Co., Ltd.), 0.4 parts by mass of 2,2-dimorpholinodiethyl ether (curing catalyst), 7.5 parts by mass of dimethyl carbonate (solvent, SP value 9.9), and 7.5 parts by mass of propylene carbonate (solvent, SP value 13.3).

[0067] 2. Evaluation of the physical properties of urethane adhesive compositions The physical properties of the obtained urethane adhesive composition were evaluated in the same manner as in Example 1. The swelling (floating, warping) of the urethane adhesive composition according to this example 2 hours after lamination was 2 mm or more (specifically, 4 mm), and it was rated as "C". The curability (25°C) was rated as "good", as the adhesive film was in a semi-cured state 16 hours after application. The curability (5°C) was rated as "good", as the adhesive film was dry to the touch 16 hours after application. Therefore, the overall verdict was "NG".

[0068] Table 1 shows the compositions and evaluation results of the examples and comparative examples.

[0069] [Table 1]

[0070] As described above, the present invention makes it possible to obtain a urethane-based adhesive composition that can reduce the degree of effect of the solvent on the urethane resin, which is the object to be adhered, and suppress swelling of the urethane resin, without increasing the waiting time due to open time.

Claims

1. The composition includes a urethane prepolymer and a solvent, The urethane prepolymer has an isocyanate group at a terminal thereof, the terminal isocyanate group is derived from at least one of diphenylmethane diisocyanate and modified diphenylmethane diisocyanate, A urethane adhesive composition, characterized in that the solvent contains 50% by weight or more of a solvent having a solubility parameter SP value of less than 8.0, based on the total amount of the solvent.

2. 2. The urethane adhesive composition according to claim 1, wherein the solvent having a solubility parameter SP value of less than 8.0 is at least one selected from aliphatic hydrocarbon solvents and cyclic hydrocarbon solvents.

3. 3. The urethane adhesive composition according to claim 1, wherein the solvent comprises a solvent having a solubility parameter SP value of less than 8.0 and a solvent having a solubility parameter SP value of 8.0 or more, and the solvent average SP value is less than 9.7.

Citation Information

Patent Citations

  • One-pack type moisture-curable polyurethane resin liquid adhesive composition

    JP2004002748A