Polycarbonate resin composition and molding
A polycarbonate resin composition with specific structural units and acrylic resin blends addresses incompatibility issues, ensuring high transparency and scratch resistance for durable applications.
Patent Information
- Application Number
- JP2023049927
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polycarbonate resins containing ISB and organopolysiloxane structures suffer from incompatibility, leading to reduced transparency and scratch resistance due to differences in refractive index and loss of additives from the surface, especially under environmental exposure.
A polycarbonate resin composition is developed by blending specific structural units of polycarbonate resin with acrylic resin, including 30-90% of structural unit (1), 50-99% of structural unit (2), and 1-50% of structural units (3) and (4), with controlled molecular weights and glass transition temperatures, to enhance compatibility and maintain transparency and scratch resistance.
The composition achieves excellent transparency and scratch resistance, suitable for long-term use in applications like automobile parts and containers, maintaining appearance and mechanical properties.
Smart Images

Figure 2024139122000001 
Figure 2024139122000002 
Figure 2024139122000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polycarbonate resin composition having excellent transparency and scratch resistance, and a molded article thereof. [Background technology]
[0002] Due to concerns about global warming due to the depletion of petroleum resources and the increase in carbon dioxide emissions, there is a demand for the development of plastics made from plant-derived monomers. A polycarbonate resin using the plant-derived raw material isosorbide (hereinafter sometimes referred to as "ISB") has been developed and is beginning to be used in automobile interior and exterior components and as a glass replacement (see, for example, Patent Documents 1 and 2). High scratch resistance is required for such applications, and Patent Documents 3 and 4 show that compounds having an organopolysiloxane structure, such as silicone oil or silicone-containing resin, are added to the resin to reduce the friction coefficient of the molded product surface, thereby improving scratch resistance. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2004 / 111106 [Patent Document 2] International Publication No. 2007 / 148604 [Patent Document 3] JP 2015-199954 A [Patent Document 4] JP 2017-8140 A Summary of the Invention [Problem to be solved by the invention]
[0004] According to the study by the present inventors, polycarbonate resin containing an ISB structure and an organopolysiloxane structure are incompatible, and the refractive index is also significantly different, so that the silicone-containing resin used in Patent Documents 3 and 4 impairs the excellent transparency that polycarbonate resin originally has. In addition, it was found that when a relatively low molecular weight compound such as silicone oil is added, the additive is lost from the surface when the surface of the molded product is washed or exposed to wind and rain for a long period of time, and the improvement effect of scratch resistance is lost. In polycarbonate resins made from plant-derived raw materials, a material that can maintain high transparency and scratch resistance while taking advantage of the characteristics of the organopolysiloxane structure has not yet been reported.
[0005] In view of the above, an object of the present application is to provide a polycarbonate resin composition having excellent transparency and scratch resistance. [Means for solving the problem]
[0006] As a result of intensive research aimed at solving the above problems, the present inventors have found that a polycarbonate resin composition in which an acrylic resin having a specific structure is blended with a polycarbonate resin having a specific structure has excellent transparency and scratch resistance.
[0007] [1] A polycarbonate resin containing 30% by weight or more and 90% by weight or less of a structural unit represented by the following formula (1): A polycarbonate resin composition containing an acrylic resin that contains 50% by weight or more and 99% by weight or less of a structural unit represented by the following formula (2), and 1% by weight or more and 50% by weight or less of at least one selected from a structural unit represented by the following formula (3) and a structural unit represented by the following formula (4):
[0008] [ka]
[0009] [ka]
[0010] (In formula (2), R 1 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent. 2 represents an alkyl group or a cycloalkyl group that contains a cyclohexane structure and may further have a substituent.
[0011] [ka]
[0012] (In formula (3), R 3 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent. 4 is an alkyl group having 10 to 30 carbon atoms which may have a substituent.
[0013] [ka]
[0014] (In formula (4), R 5 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent. 6 is an alkyl group having 1 to 6 carbon atoms which has an organopolysiloxane as a substituent and which may have an ether bond. The number average molecular weight of the structural unit represented by formula (4) is 500 or more and 3,000 or less.
[0015] [2] The polycarbonate resin composition according to [1], wherein the polycarbonate resin has a glass transition temperature of 90°C or higher and 150°C or lower. [3] The polycarbonate resin composition according to [1] or [2], wherein the polycarbonate resin contains a structural unit derived from an aliphatic dihydroxy compound or an alicyclic dihydroxy compound.
[0016] [4] The polycarbonate resin composition according to any one of [1] to [3], wherein the acrylic resin has a weight average molecular weight (Mw) of 10,000 or more and 200,000 or less. [5] The polycarbonate resin composition according to any one of [1] to [4], comprising 70% by weight or more and 99% by weight or less of the polycarbonate resin and 1% by weight or more and 30% by weight or less of the acrylic resin.
[0017] [6] A molded article obtained by molding the polycarbonate resin composition according to any one of [1] to [5]. [7] The molded article according to [6], which is used for automobile interior or exterior materials. Effect of the Invention
[0018] The polycarbonate resin composition of the present invention has excellent transparency and scratch resistance, and can be suitably used in applications where excellent appearance must be maintained for a long period of time, such as automobile interior and exterior components and containers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention will be described in detail below, but the present invention is not limited to the following description, and can be modified in any manner without departing from the gist of the present invention.
[0020] In this specification, when an expression is used with "xxx to xxx" followed by a numerical value or a physical property value, this means "greater than xxx and less than xxx," and more preferably means "greater than xxx but less than xxx."
[0021] In this specification, the term "repeated structural unit" refers to a structural unit in which the same structure appears repeatedly in a resin, and each of the structural units is linked to form the resin. For example, in the case of a polycarbonate resin, the carbonyl group is also referred to as the repeating structural unit. In addition, the term "structural unit" refers to a partial structure that constitutes a resin, and a specific partial structure contained in the repeating structural unit. For example, it refers to a partial structure sandwiched between adjacent linking groups in a resin, or a partial structure sandwiched between a polymerizable reactive group present at the end of a polymer and a linking group adjacent to the polymerizable reactive group. More specifically, in the case of a polycarbonate resin, a carbonyl group is a linking group, and a partial structure sandwiched between adjacent carbonyl groups is referred to as a structural unit.
[0022] [Polycarbonate resin composition] The polycarbonate resin composition of the present invention contains a polycarbonate resin containing 30% by weight or more and 90% by weight or less of a structural unit represented by the following formula (1), and an acrylic resin containing 50% by weight or more and 99% by weight or less of a structural unit represented by the following formula (2), and containing 1% by weight or more and 50% by weight or less of at least one selected from a structural unit represented by the following formula (3) and a structural unit represented by the following formula (4).
[0023] Hereinafter, the structural unit represented by the formula (1) may be referred to as "structural unit (1)", the (meth)acrylate structural unit represented by the formula (2) may be referred to as "structural unit (2)", the (meth)acrylate structural unit represented by the formula (3) may be referred to as "structural unit (3)", and the (meth)acrylate structural unit represented by the formula (4) may be referred to as "structural unit (4)". The weight ratios of the various structural units may be expressed, for example, as follows: 1 By analyzing H-NMR, the area ratio of the peaks originating from each structural unit and the molecular weight of each structural unit can be calculated.
[0024] [ka]
[0025] [ka] (In formula (2), R 1 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent. 2 represents an alkyl group or a cycloalkyl group that contains a cyclohexane structure and may further have a substituent.
[0026] [ka] (In formula (3), R 3 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent. 4 is an alkyl group having 10 to 30 carbon atoms which may have a substituent.
[0027] [ka] (In formula (4), R 5 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent. 6 is an alkyl group having 1 to 6 carbon atoms which has an organopolysiloxane as a substituent and which may have an ether bond. The number average molecular weight of the structural unit represented by formula (4) is 500 or more and 3,000 or less.
[0028] <Polycarbonate resin> The polycarbonate resin composition of the present invention contains a polycarbonate resin containing 30% by weight or more and 90% by weight or less of the structural unit represented by the formula (1). Hereinafter, this polycarbonate resin may be referred to as the "polycarbonate resin of the present invention."
[0029] (Dihydroxy Compounds) Dihydroxy compounds forming the structural unit (1) include isosorbide (ISB), isomannide, and isoidet, which are stereoisomers. These may be used alone or in combination of two or more. Among them, isosorbide obtained by dehydration condensation of sorbitol produced from various starches, which are abundant and easily available as a plant-derived resource, is most preferred in terms of availability, ease of production, and properties of the resulting molded product (for example, heat resistance, impact resistance, surface hardness, carbon neutrality).
[0030] The lower limit of the content of the structural unit (1) in the polycarbonate resin is preferably 35% by weight or more, more preferably 40% by weight or more. The upper limit is preferably 80% by weight or less, more preferably 70% by weight or less. Since the structural unit (2) in the acrylic resin of the present invention described later has high compatibility with the structural unit (1), within the above range, a resin composition with high transparency can be obtained, and mechanical properties, heat resistance, and melt moldability are also good. In this specification, the content of the structural unit (1) in the polycarbonate resin means the content (weight %) of the structural unit (1) when the total weight of all structural units and linking groups constituting the polycarbonate resin is 100% by weight. The contents of other structural units in the polycarbonate resin are defined in the same manner.
[0031] The polycarbonate resin in the present invention may contain structural units other than the structural unit (1). Hereinafter, structural units other than the structural unit (1) may be referred to as "other structural units". Examples of compounds forming other structural units include aliphatic dihydroxy compounds, alicyclic dihydroxy compounds, ether-containing dihydroxy compounds, acetal-containing dihydroxy compounds, aromatic-containing dihydroxy compounds, and diester compounds. A polycarbonate resin partially incorporating a structural unit derived from a diester compound is referred to as a polyester carbonate resin. In this specification, the term "polycarbonate resin" includes polyester carbonate resins.
[0032] Examples of the aliphatic dihydroxy compound include the following dihydroxy compounds: straight-chain aliphatic dihydroxy compounds such as ethylene glycol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 1,5-heptanediol, 1,6-hexanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol; and branched-chain aliphatic dihydroxy compounds such as 1,3-butanediol, 1,2-butanediol, neopentyl glycol, and hexylene glycol.
[0033] Examples of the alicyclic dihydroxy compound include the following dihydroxy compounds: dihydroxy compounds which are primary alcohols of alicyclic hydrocarbons, such as 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, pentacyclopentadecane dimethanol, 2,6-decalin dimethanol, 1,5-decalin dimethanol, 2,3-decalin dimethanol, 2,3-norbornane dimethanol, 2,5-norbornane dimethanol, 1,3-adamantanedimethanol, and dihydroxy compounds derived from terpene compounds such as limonene; dihydroxy compounds which are secondary or tertiary alcohols of alicyclic hydrocarbons, such as 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,3-adamantanediol, hydrogenated bisphenol A, and 2,2,4,4-tetramethyl-1,3-cyclobutanediol.
[0034] Examples of the ether-containing dihydroxy compound include oxyalkylene glycols and dihydroxy compounds containing an acetal ring. Examples of the oxyalkylene glycol that can be used include diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol.
[0035] Examples of acetal-containing dihydroxy compounds that can be used include spiroglycol (also known as 3,9-bis(1,1-dimethyl-2-hydroxyethyl-2,4,8,10-tetraoxaspiro[5,5]undecane) and dioxane glycol (also known as 2-(1,1-dimethyl-2-hydroxyethyl)-5-ethyl-5-hydroxymethyl-1,3-dioxane).
[0036] As the aromatic dihydroxy compound, for example, the following dihydroxy compounds can be used: 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3,5-diethylphenyl)propane, 2,2-bis(4-hydroxy-(3-phenyl)phenyl)propane, 2,2-bis(4-hydroxy-(3,5-diphenyl)phenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, bis(4-hydroxyphenyl)propane, )methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)pentane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane, 1,1-bis(4-hydroxyphenyl)-2-ethylhexane, 1,1-bis(4-hydroxyphenyl)decane, bis(4-hydroxy-3-nitrophenyl)methane, 3,3-bis(4-hydroxyphenyl)pentane, 1,3-bis(4-hydroxyphenyl)pentane, Bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 1,1-bis(4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)sulfone, 2,4'-dihydroxydiphenyl sulfone, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxy-3-methylphenyl)sulfide, bis(4-hydroxyphenyl)disulfide, 4, Aromatic bisphenol compounds such as 4'-dihydroxydiphenyl ether and 4,4'-dihydroxy-3,3'-dichlorodiphenyl ether; dihydroxy compounds having an ether group bonded to an aromatic group such as 2,2-bis(4-(2-hydroxyethoxy)phenyl)propane, 2,2-bis(4-(2-hydroxypropoxy)phenyl)propane, 1,3-bis(2-hydroxyethoxy)benzene, 4,4'-bis(2-hydroxyethoxy)biphenyl, and bis(4-(2-hydroxyethoxy)phenyl)sulfone;9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxypropoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene , 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl)fluorene and other dihydroxy compounds having a fluorene ring;
[0037] Examples of diester compounds include the following dicarboxylic acids: aromatic dicarboxylic acids such as terephthalic acid, phthalic acid, isophthalic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-benzophenonedicarboxylic acid, 4,4'-diphenoxyethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, and 2,6-naphthalenedicarboxylic acid; alicyclic dicarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid; and aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid. These dicarboxylic acid components can be used as raw materials for polyester carbonate resins as dicarboxylic acids themselves, but dicarboxylic acid esters such as methyl esters and phenyl esters, and dicarboxylic acid derivatives such as dicarboxylic acid halides can also be used as raw materials depending on the production method.
[0038] Among the above other structural units, it is preferable to contain a structural unit derived from an aliphatic dihydroxy compound or an alicyclic dihydroxy compound from the viewpoint of mechanical properties and heat resistance. Among them, 1,4-cyclohexanedimethanol and tricyclodecane dimethanol are more preferable, and it is even more preferable to contain a structural unit derived from 1,4-cyclohexanedimethanol.
[0039] In the polycarbonate resin of the present invention, the lower limit of the content of the other structural units is preferably 5% by weight or more, more preferably 10% by weight or more. The upper limit is preferably 60% by weight or less, more preferably 50% by weight or less, and even more preferably 45% by weight or less. Within the above range, the excellent properties of the structural unit (1) are not significantly impaired, and the balance with other physical properties can be improved.
[0040] By using aromatic dihydroxy compounds or diester compounds such as bisphenol compounds as copolymerization components, the heat resistance of polycarbonate resins can be improved in some cases, but on the other hand, when the polycarbonate resin contains a large amount of aromatic structures, the weather resistance tends to decrease. In addition, since there is a large difference in the polymerization reactivity between bisphenol compounds or diester compounds and dihydroxy compounds forming the structural unit (1), it becomes difficult to obtain a polycarbonate resin with a high molecular weight, and mechanical properties such as impact resistance tend to decrease when the bisphenol compounds or diester compounds remain in the terminal groups. If the reaction temperature is raised to promote the reaction, the structural unit (1) is thermally decomposed, and the obtained polycarbonate resin tends to become colored. For these reasons, the content ratio of the structural unit derived from aromatic dihydroxy compounds or diester compounds is preferably 20% by weight or less, more preferably 10% by weight or less.
[0041] (linking group) The linking group contained in the polycarbonate resin in the present invention is introduced by using a carbonic acid diester or a carbonyl halide in a polycondensation reaction. The linking group introduced into the polycarbonate resin by the carbonic acid diester or the carbonyl halide is a carbonyl group.
[0042] (carbonic acid diester) As a compound for introducing a linking group, it is preferable to use a carbonate diester represented by the following formula (5) from the viewpoint of being usable in the melt polymerization method described later.
[0043] [ka]
[0044] In formula (5), A 1 and A 2 each represents an aliphatic hydrocarbon group having 1 to 18 carbon atoms which may have a substituent, or an aromatic hydrocarbon group which may have a substituent, 1 and A 2 may be the same or different.
[0045] A 1 and A 2 is preferably a substituted or unsubstituted aromatic hydrocarbon group, more preferably an unsubstituted aromatic hydrocarbon group. Examples of the substituent of the aliphatic hydrocarbon group include an ester group, an ether group, an amide group, and a halogen atom, and examples of the substituent of the aromatic hydrocarbon group include an alkyl group such as a methyl group or an ethyl group.
[0046] Examples of the carbonic acid diester represented by the formula (5) include diphenyl carbonate (hereinafter sometimes abbreviated as DPC), substituted diphenyl carbonates such as ditolyl carbonate, and dialkyl carbonates such as dimethyl carbonate, diethyl carbonate, and di-tert-butyl carbonate. From the viewpoint of reactivity, preferred are diphenyl carbonate and substituted diphenyl carbonates, and particularly preferred is diphenyl carbonate.
[0047] The carbonate diester may contain impurities such as chloride ions, and these impurities may inhibit the polymerization reaction or deteriorate the hue of the resulting resin. Therefore, it is preferable to use a diester that has been purified, as necessary, by distillation or the like.
[0048] In the polycondensation reaction, the reaction rate and the molecular weight of the resin obtained can be controlled by strictly adjusting the molar ratio of all dihydroxy compounds and all diester compounds used in the reaction. The molar ratio of all diester compounds to all dihydroxy compounds is preferably adjusted to 0.90 to 1.10, more preferably adjusted to 0.96 to 1.05, and particularly preferably adjusted to 0.98 to 1.03. When the above-mentioned diester compounds are used in addition to the carbonic acid diester, the total diester compounds means the total amount of the carbonic acid diester and the other diester compounds. When the molar ratio is within the above range, a resin with a desired molecular weight can be produced at a good reaction rate, and the amount of low molecular weight compounds remaining in the resin can be reduced, so that a resin with excellent color tone, thermal stability, and moldability can be obtained.
[0049] <Production method of polycarbonate resin> The polycarbonate resin of the present invention can be produced by a commonly used polymerization method. For example, it can be produced by a solution polymerization method or an interfacial polymerization method using phosgene or a carboxylic acid halide, or a melt polymerization method in which a reaction is carried out without using a solvent. Among these production methods, it is preferable to produce the polycarbonate resin by the melt polymerization method, which is excellent in productivity and can reduce the environmental load because it does not use a solvent or a highly toxic compound.
[0050] In the melt polymerization method, the above-mentioned dihydroxy compound and the carbonic acid diester are polycondensed by transesterification to obtain a polycarbonate resin. More specifically, the polycarbonate resin can be obtained by removing the monohydroxy compound and the like that are by-produced in the transesterification reaction from the system.
[0051] The transesterification reaction proceeds in the presence of a transesterification catalyst (hereinafter, the transesterification catalyst is referred to as a "polymerization catalyst.") The type of polymerization catalyst can have a significant effect on the reaction rate of the transesterification reaction and the quality of the resulting polycarbonate resin.
[0052] The polymerization catalyst is not particularly limited as long as it satisfies the transparency, color tone, heat resistance, weather resistance, and mechanical properties of the resulting polycarbonate resin. For example, metal compounds of Group I or Group II (hereinafter simply referred to as "Group 1" and "Group 2") in the long-form periodic table, as well as basic compounds such as basic boron compounds, basic phosphorus compounds, basic ammonium compounds, and amine compounds can be used as the polymerization catalyst, and among these, Group 1 metal compounds and / or Group 2 metal compounds are preferred.
[0053] Examples of Group 1 metal compounds include the following compounds: sodium hydroxide, potassium hydroxide, lithium hydroxide, cesium hydroxide, sodium hydrogen carbonate, potassium hydrogen carbonate, lithium hydrogen carbonate, cesium hydrogen carbonate, sodium carbonate, potassium carbonate, lithium carbonate, cesium carbonate, sodium acetate, potassium acetate, lithium acetate, cesium acetate, sodium stearate, potassium stearate, lithium stearate, cesium stearate, sodium borohydride, potassium borohydride, lithium borohydride, cesium borohydride, sodium phenylborohydride, and boron phenylide. Potassium, lithium phenyl boron, cesium phenyl boron, sodium benzoate, potassium benzoate, lithium benzoate, cesium benzoate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, dilithium hydrogen phosphate, dicesium hydrogen phosphate, disodium phenylphosphate, dipotassium phenylphosphate, dilithium phenylphosphate, dicesium phenylphosphate, alcoholates, phenolates of sodium, potassium, lithium, and cesium, and disodium salts, dipotassium salts, dilithium salts, and dicesium salts of bisphenol A. As the Group 1 metal compound, lithium compounds are preferred from the viewpoints of polymerization activity and the color tone of the resulting polycarbonate resin.
[0054] Examples of Group 2 metal compounds include the following compounds: calcium hydroxide, barium hydroxide, magnesium hydroxide, strontium hydroxide, calcium hydrogen carbonate, barium hydrogen carbonate, magnesium hydrogen carbonate, strontium hydrogen carbonate, calcium carbonate, barium carbonate, magnesium carbonate, strontium carbonate, calcium acetate, barium acetate, magnesium acetate, strontium acetate, calcium stearate, barium stearate, magnesium stearate, and strontium stearate. As the Group 2 metal compound, magnesium compounds, calcium compounds, or barium compounds are preferred, and from the viewpoints of polymerization activity and color tone of the resulting polycarbonate resin, magnesium compounds and / or calcium compounds are more preferred, and calcium compounds are even more preferred.
[0055] Although it is possible to use a basic compound such as a basic boron compound, a basic phosphorus compound, a basic ammonium compound, or an amine compound in combination with the Group 1 metal compound and / or the Group 2 metal compound, it is preferable to use only the Group 1 metal compound and / or the Group 2 metal compound, and more preferably to use only the Group 2 metal compound from the viewpoint of the color tone of the resulting polycarbonate resin.
[0056] The amount of the polymerization catalyst used is preferably 0.1 μmol or more, more preferably 0.5 μmol or more, and even more preferably 1.0 μmol or more per mol of the total dihydroxy compounds used in the reaction, and is preferably 50 μmol or less, more preferably 20 μmol or less, and even more preferably 10 μmol or less per mol of the total dihydroxy compounds used in the reaction.
[0057] By adjusting the amount of the polymerization catalyst used within the above range, the polymerization rate can be increased, so that it is possible to obtain a polycarbonate resin with a desired molecular weight without necessarily increasing the polymerization temperature, and the deterioration of the color tone of the polycarbonate resin can be suppressed. In addition, it is possible to prevent the unreacted raw materials from volatilizing during the polymerization, which would cause the molar ratio of the dihydroxy compound and the carbonic acid diester to be lost, so that a resin with a desired molecular weight and copolymerization ratio can be obtained more reliably. Furthermore, it is possible to suppress the occurrence of side reactions, so that the deterioration of the color tone of the polycarbonate resin or coloring during molding can be further prevented.
[0058] Considering the adverse effects of sodium, potassium, and cesium among the group 1 metals on the color tone of the polycarbonate resin and the adverse effects of iron on the color tone of the polycarbonate resin, the total content of sodium, potassium, cesium, and iron in the polycarbonate resin is preferably 1 weight ppm or less. In this case, the deterioration of the color tone of the polycarbonate resin can be further prevented, and the color tone of the polycarbonate resin can be further improved. From the same viewpoint, the total content of sodium, potassium, cesium, and iron in the polycarbonate resin is more preferably 0.5 weight ppm or less. Note that these metals may be mixed in not only from the catalyst used, but also from the raw materials or reaction equipment. Regardless of the source, the content of these metals in the polycarbonate resin is preferably within the above-mentioned range as the total content of sodium, potassium, cesium, and iron.
[0059] The method of polycondensing a dihydroxy compound and a carbonic acid diester is carried out in multiple stages using multiple reactors in the presence of the above-mentioned catalyst. The reaction may be carried out in a batchwise manner, a continuous manner, or a combination of a batchwise manner and a continuous manner, but it is preferable to adopt a continuous manner, which is excellent in productivity and can obtain a polycarbonate resin with less heat history.
[0060] From the viewpoint of controlling the polymerization rate and the quality of the resulting polycarbonate resin, it is important to appropriately select the jacket temperature, the internal temperature, and the pressure in the reaction system according to the reaction stage. Specifically, it is preferable to obtain a prepolymer at a relatively low temperature and low vacuum in the early stage of the polycondensation reaction, and to increase the molecular weight to a predetermined value at a relatively high temperature and high vacuum in the later stage of the reaction. In this case, the distillation of unreacted monomers is suppressed, and it becomes easier to adjust the molar ratio of the dihydroxy compound and the carbonate diester to a desired ratio. As a result, the decrease in the polymerization rate can be suppressed. In addition, it becomes possible to more reliably obtain a polymer having a desired molecular weight and terminal group.
[0061] By adjusting the temperature of the polycondensation reaction, it is possible to improve productivity and prevent the increase of the heat history of the product. Furthermore, it is possible to further prevent the volatilization of the monomer and the decomposition and coloration of the polycarbonate resin. Specifically, the following conditions can be adopted as the reaction conditions in the first stage reaction. That is, the maximum temperature inside the polymerization reactor is set in the range of usually 160 to 230°C, preferably 170 to 220°C, and more preferably 180 to 210°C. In addition, the pressure of the polymerization reactor (hereinafter, pressure refers to absolute pressure) is set in the range of usually 1 to 110 kPa, preferably 5 to 50 kPa, and more preferably 7 to 30 kPa. In addition, the reaction time is set in the range of usually 0.1 to 10 hours, preferably 1 to 5 hours. It is preferable that the first stage reaction is carried out while distilling off the generated monohydroxy compound outside the reaction system.
[0062] From the second stage onwards, it is preferable to gradually reduce the pressure of the reaction system from the pressure of the first stage, and ultimately reduce the pressure (absolute pressure) of the reaction system to 1 kPa or less while removing the monohydroxy compound that is subsequently generated from the reaction system. The maximum internal temperature of the polymerization reactor in the final stage is usually set in the range of 200 to 260° C., preferably 210 to 240° C., and more preferably 215 to 230° C. The reaction time is usually set in the range of 0.1 to 10 hours, preferably 0.5 to 5 hours, and more preferably 1 to 3 hours.
[0063] Using the stirring power as an indicator, once it has been confirmed that the specified reduced viscosity (molecular weight) has been reached, the polycondensation reaction is stopped by introducing nitrogen into the reactor to return the pressure to normal pressure, or by withdrawing the molten resin from the reactor. The molten resin is discharged from the die head in the form of strands, cooled and solidified, and pelletized using a rotary cutter or the like. If necessary, extrusion devolatilization, extrusion kneading, and extrusion filtration processes may be added before pelletization. In these processes, additives are mixed into the resin, low molecular weight components are devolatilized using a vacuum vent, and foreign matter is removed using a polymer filter.
[0064] <Characteristics of polycarbonate resin> (molecular weight) The molecular weight of polycarbonate resin is related to reduced viscosity and 1 It can be expressed as the number average molecular weight measured by H-NMR, etc. The higher the value obtained by these measurement methods, the higher the molecular weight. 1 The number average molecular weight measured by H-NMR is preferably 8,000 or more and 30,000 or less. The lower limit is more preferably 9,000 or more, and even more preferably 10,000 or more. The upper limit is more preferably 25,000 or less, and even more preferably 20,000 or less. The reduced viscosity of the polycarbonate resin is preferably 0.3 dL / g or more and 1.0 dL / g or less. The lower limit is more preferably 0.35 dL / g or more, and even more preferably 0.4 dL / g or more. The upper limit is more preferably 0.8 dL / g or less, and even more preferably 0.7 dL / g or less. Within the above range, sufficient mechanical strength can be obtained, and the fluidity during melt molding can also be adjusted to a preferred range. In this specification, 1 The number average molecular weight measured by H-NMR is 1 When the term "number average molecular weight (Mn)," "number average molecular weight," or "Mn" is used, it refers to the number average molecular weight measured by GPC, which will be described later.
[0065] (glass transition temperature) The glass transition temperature of the polycarbonate resin is preferably 90° C. or higher and 150° C. or lower. The lower limit is more preferably 95° C. or higher, and even more preferably 100° C. or higher. The upper limit is more preferably 145° C. or lower, and even more preferably 140° C. or lower. Within the above range, the polycarbonate resin has sufficient heat resistance and mechanical properties, and is also excellent in melt processability.
[0066] (Melt Viscosity) The melt viscosity of the polycarbonate resin at 240°C is preferably 800 Pa·s or more and 3000 Pa·s or less. The lower limit is more preferably 1000 Pa·s or more, and even more preferably 1200 Pa·s or more. The upper limit is more preferably 2500 Pa·s or less, and even more preferably 2000 Pa·s or less. Within the above range, sufficient mechanical strength can be obtained and fluidity during melt molding can be ensured. Furthermore, in this case, coloring and foaming caused by an increase in resin temperature due to shear heat can be further prevented. In this specification, the melt viscosity is the melt viscosity measured using a capillary rheometer (manufactured by Toyo Seiki Seisakusho Co., Ltd.) at a temperature of 240°C and a shear rate of 91.2 sec -1 The method for measuring the melt viscosity will be described in detail later.
[0067] <Acrylic resin> The polycarbonate resin composition of the present invention contains an acrylic resin containing 50% by weight or more and 99% by weight or less of the structural unit (2) and 1% by weight or more and 50% by weight or less of at least one selected from the structural unit (3) and the structural unit (4). Hereinafter, this acrylic resin may be referred to as the "acrylic resin of the present invention". In this specification, the content of the (meth)acrylate structural units represented by the formulas (2) to (4) in the acrylic resin means the content (weight %) of each of the (meth)acrylate structural units represented by the formulas (2) to (4) when the total weight of all the structural units constituting the acrylic resin is taken as 100% by weight. The contents of other structural units in the acrylic resin are defined in the same manner.
[0068] The acrylic resin in the present invention preferably has compatibility with the polycarbonate resin in the present invention. From this viewpoint, R 1 R is preferably a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent, and among these, a methyl group which has higher heat resistance is more preferable. 2is an alkyl group or cycloalkyl group containing a cyclohexane structure and which may further have a substituent, and this structure enhances compatibility with the polycarbonate resin in the present invention. Examples of vinyl compounds forming the structural unit (2) include cyclohexyl acrylate, cyclohexyl methacrylate, cyclohexyl methyl acrylate, cyclohexyl methyl methacrylate, 1-ethylcyclohexyl acrylate, 1-ethylcyclohexyl methacrylate, 2-cyclohexylpropyl-2-yl acrylate, 2-cyclohexylpropyl-2-yl methacrylate, hydroxycyclohexyl acrylate, hydroxycyclohexyl methacrylate, cyclohexanedimethanol monoacrylate, cyclohexanedimethanol monomethacrylate, 3,4-epoxycyclohexylmethyl acrylate, and 3,4-epoxycyclohexylmethyl methacrylate. These may be used alone or in combination of two or more. Among these, from the viewpoints of availability and physical properties such as heat resistance of the resulting acrylic resin, it is more preferable to use cyclohexyl methacrylate, hydroxycyclohexyl methacrylate, and cyclohexane monomethacrylate, and cyclohexyl methacrylate is even more preferable.
[0069] The lower limit of the content of the structural unit (2) in the acrylic resin of the present invention is preferably 70% by weight or more, more preferably 80% by weight or more, and particularly preferably 85% by weight or more. The upper limit is preferably 95% by weight or less, more preferably 92% by weight or less, and even more preferably 90% by weight or less. Within the above range, compatibility with the polycarbonate resin of the present invention and the effect of improving scratch resistance can be achieved at the same time.
[0070] By containing at least one selected from structural unit (3) and structural unit (4) in the acrylic resin of the present invention, the coefficient of friction of the surface of a molded article made of the composition of the present invention can be reduced, thereby improving scratch resistance. The structural units (3) and (4) may be used alone or in combination of two or more. From the viewpoint of balancing various physical properties such as compatibility with the polycarbonate resin of the present invention, scratch resistance, heat resistance, and mechanical properties, R 3 R is preferably a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent, and more preferably a methyl group. 4 is an alkyl group having 10 to 30 carbon atoms which may have a substituent, the lower limit of the number of carbon atoms is preferably 14 or more, more preferably 16 or more. The upper limit is preferably 28 or less, more preferably 26 or less. These may be used alone or in combination of two or more. Examples of compounds forming the structural unit (3) include lauryl (meth)acrylate, myristyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate. From the viewpoint of the heat resistance of the obtained acrylic resin, it is preferable to use a methacrylate type among the above compounds, and it is more preferable to use cetyl methacrylate, stearyl methacrylate, and behenyl methacrylate, and stearyl methacrylate is particularly preferable.
[0071] Similarly, in the formula (4), R 5 R is preferably a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent, and among these, a methyl group is more preferable. 6 is an alkyl group having 1 to 6 carbon atoms which has an organopolysiloxane as a substituent and which may have an ether bond, and the number of carbon atoms in the alkyl group is preferably 2 or more, more preferably 5 or less, and particularly preferably 4 or less. As the structural unit forming the organopolysiloxane, dimethylsiloxane, diphenylsiloxane, and methylphenylsiloxane are preferred. These structural units may be used in combination, but to obtain better scratch resistance, it is preferred to contain a large amount of dimethylsiloxane structural units, and it is preferred that 70% by weight or more and 100% by weight or less of the structural units forming the organopolysiloxane are dimethylsiloxane structural units. The number average molecular weight of the structural unit (4) is 500 or more and 3000 or less, with the lower limit being preferably 600 or more and more preferably 700 or more. The upper limit is preferably 2,000 or less and more preferably 1,500 or less. The number average molecular weight of the (meth)acrylate compound forming the structural unit (4) is 1 It can be determined by analysis such as H-NMR.
[0072] The lower limit of the content of the structural unit (3) and the structural unit (4) in the acrylic resin of the present invention is preferably 5% by weight or more, more preferably 8% by weight or more, and even more preferably 10% by weight or more. The upper limit is preferably 30% by weight or less, more preferably 20% by weight or less, and even more preferably 15% by weight or less. Within the above range, scratch resistance can be imparted while balancing the desired properties.
[0073] The acrylic resin of the present invention may contain structural units other than the structural units (2) to (4). When the acrylic resin contains a (meth)acrylate structural unit containing an ether group or a hydroxyl group as a structural unit other than the structural units (2) to (4), the compatibility with the polycarbonate resin of the present invention can be improved. Examples of vinyl compounds forming a (meth)acrylate structural unit containing an ether group or a hydroxyl group include 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, methoxyethyl acrylate, methoxyethyl methacrylate, 2-hydroxyethoxyethyl acrylate, 2-hydroxyethoxyethyl methacrylate, glycerin monoacrylate, glycerin monomethacrylate, polyethylene glycol monoacrylate, polyethylene glycol monomethacrylate, methoxypolyethylene glycol acrylate, methoxypolyethylene glycol acrylate, polypropylene glycol monoacrylate, polypropylene glycol monomethacrylate, polytrimethylene glycol monoacrylate, polytrimethylene glycol monomethacrylate, polycaprolactone-modified 2-hydroxyethyl acrylate, polycaprolactone-modified 2-hydroxyethyl methacrylate, etc. These may be used alone or in combination of two or more.
[0074] When an acrylate structural unit is introduced into the acrylic resin of the present invention, the thermal decomposition of the main chain of the acrylic resin can be suppressed and the thermal stability can be improved. When all of the structural units (2) to (4) are methacrylate structural units, it is preferable to further introduce an acrylate structural unit. From the viewpoint of improving the thermal stability without changing the desired resin properties, the vinyl compound forming the acrylate structural unit is preferably one having a relatively small molecular weight or a structure similar to the structural unit (2), and more preferably methyl acrylate, ethyl acrylate, or cyclohexyl acrylate is used. The lower limit of the content of the acrylate structural unit is preferably 0.5% by weight or more, more preferably 1% by weight or more. The upper limit is preferably 5% by weight or less, more preferably 3% by weight or less. Within the above range, sufficient thermal stability for use in melt molding can be imparted without impairing the desired properties.
[0075] The acrylic resin in the present invention may further contain another structural unit, and as the vinyl compound forming the other structural unit, acrylonitrile, styrene, α-methylstyrene, butadiene, polyfunctional (meth)acrylate, etc. can be used. By appropriately combining these, it is possible to improve the thermal stability of the acrylic resin, adjust the refractive index of the acrylic resin, and improve the transparency of the resin composition of the present invention. From the viewpoint of ensuring compatibility with the polycarbonate resin in the present invention, it is preferable that the content of the component is relatively small, and it is preferably 0.1% by weight or more and 10% by weight or less. The lower limit is more preferably 0.3% by weight or more, and more preferably 0.5% by weight or more. The upper limit is more preferably 7% by weight or less, and more preferably 5% by weight or less.
[0076] <Characteristics of acrylic resin> Various molecular weights of the acrylic resin in the present invention can be measured by GPC, which will be described later. The weight average molecular weight (Mw) of the acrylic resin in the present invention is preferably 10,000 or more and 200,000 or less. The lower limit of the weight average molecular weight is more preferably 15,000 or more, and even more preferably 20,000 or more. The upper limit is more preferably 150,000 or less, and even more preferably 100,000 or less. Within the above range, scratch resistance can be imparted without impairing compatibility with the polycarbonate resin in the present invention or mechanical properties.
[0077] The number average molecular weight (Mn) is preferably 10,000 or more and 200,000 or less. The molecular weight distribution (Mw / Mn) is preferably 1.0 or more and 5.0 or less. The molecular weight of the acrylic resin can be adjusted by the ratio of the amount of the monomer used in the polymerization to the amount of the radical polymerization initiator and the chain transfer agent.
[0078] The glass transition temperature of the acrylic resin in the present invention is preferably 30°C or higher and 120°C or lower. The lower limit is more preferably 40°C or higher, and even more preferably 50°C or higher. The upper limit is more preferably 110°C or lower, and even more preferably 100°C or lower. Within the above range, the acrylic resin becomes solid at room temperature and has excellent handleability. In addition, it can be melt-processed at the same temperature as the polycarbonate resin in the present invention.
[0079] <Method of manufacturing acrylic resin> Examples of the method for producing the acrylic resin of the present invention include bulk polymerization, solution polymerization, and aqueous dispersion polymerization such as suspension polymerization and emulsion polymerization. Among these, aqueous dispersion polymerization is preferred from the viewpoint of simplifying the recovery process of the resin after polymerization and controlling the heat generated by polymerization, and suspension polymerization is particularly preferred. In the suspension polymerization, the resin after polymerization is obtained as spherical particles with an average particle size of about 5 μm to 1 mm, so that the flowability is good when used in processing operations such as extrusion and molding, and also, the handling is excellent because there is little concern about dust scattering.
[0080] <Composition of polycarbonate resin composition> The polycarbonate resin composition of the present invention preferably contains 70% by weight or more and 99% by weight or less of the polycarbonate resin of the present invention, and 1% by weight or more and 30% by weight or less of the acrylic resin of the present invention. The lower limit of the content of the polycarbonate resin of the present invention is more preferably 75% by weight or more, and even more preferably 80% by weight or more. The upper limit is more preferably 97% by weight or less, and even more preferably 95% by weight or less. The lower limit of the content of the acrylic resin in the present invention is more preferably 3% by weight or more, and even more preferably 5% by weight or more. The upper limit is more preferably 25% by weight or less, and even more preferably 20% by weight or less. By keeping the content within the above range, it is possible to impart scratch resistance while balancing various required physical properties such as transparency, heat resistance, and mechanical properties at a high level.
[0081] <Additives> The polycarbonate resin composition of the present invention may contain other components such as additives in addition to the polycarbonate resin of the present invention and the acrylic resin of the present invention described above, and within the range that does not impair the effects of the present invention, antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, fillers such as fillers, neutralizing agents, lubricants, antifogging agents, antiblocking agents, slip agents, dispersants, colorants, flame retardants, antistatic agents, conductivity imparting agents, crosslinking agents, crosslinking assistants, metal deactivators, molecular weight regulators, antibacterial agents, antifungal agents, fluorescent brighteners, organic diffusing agents, inorganic diffusing agents, etc. The content of the additives is preferably more than 0% by weight and not more than 5% by weight, more preferably 0.01% by weight or more and not more than 3% by weight, based on the entire polycarbonate resin composition of the present invention (100% by weight).
[0082] Furthermore, within a range that does not impair the effects of the present invention, the composition may further contain one or more other resins, such as synthetic resins such as aromatic polycarbonates, aromatic polyesters, aliphatic polyesters, polyamides, polystyrenes, polyolefins, amorphous polyolefins, acrylonitrile-butadiene-styrene copolymers (ABS resins), and acrylonitrile-styrene copolymers (AS resins); elastomers such as acrylic rubber, butadiene rubber, and silicone rubber; and biodegradable resins such as polylactic acid and polybutylene succinate.
[0083] <Method of producing the resin composition of the present invention> The polycarbonate resin composition of the present invention can be produced, for example, by a method of mechanically melt-kneading each of the above-mentioned components constituting the resin composition. As the melt kneader, a single screw extruder, a twin screw extruder, a Brabender, a Banbury mixer, a kneader blender, a roll mill, etc. can be used. In kneading, each component may be kneaded at once, or a multi-stage division kneading method in which an arbitrary component is kneaded and then the remaining components are added and kneaded may be used. Among them, a method in which each component is continuously charged using a twin screw extruder equipped with a vacuum vent and a resin composition is continuously obtained is preferable from the viewpoint of productivity and quality uniformity. The lower limit of the kneading temperature is usually 150°C or more, preferably 180°C or more, and more preferably 200°C or more. The upper limit of the kneading temperature is usually 280°C or less, preferably 260°C or less, more preferably 250°C or less, and even more preferably 240°C or less. Within this range, productivity (processing speed of kneading) can be increased while suppressing heat deterioration due to heating by the kneader and heat generation due to shear.
[0084] <Characteristics of polycarbonate resin composition> (transparency) The polycarbonate resin composition of the present invention has a haze value of preferably 30% or less, more preferably 20% or less, and even more preferably 10% or less, as measured by the method described below. When the haze value is within the above range, the composition can be applied to components that require high transparency, such as automotive interior and exterior components and glass replacement applications.
[0085] (Scratch resistance) It is preferable that the polycarbonate resin composition of the present invention has no visible scratches when the scratch resistance is evaluated by the method described below.
[0086] (Heat resistance) The polycarbonate resin composition of the present invention preferably has a glass transition temperature of 80° C. or more and 150° C. or less, as measured by the method described below. The lower limit is more preferably 90° C. or more, and even more preferably 100° C. or more. The upper limit is more preferably 140° C. or less, and even more preferably 130° C. or less. When the glass transition temperature is within the above range, the composition has practical heat resistance and is also excellent in mechanical properties such as impact resistance and melt processability.
[0087] [Molded products] The polycarbonate resin composition of the present invention can be processed into various molded articles by molding methods such as injection molding (insert molding, two-color molding, sandwich molding, gas injection molding, etc.), extrusion molding, inflation molding, T-die film molding, lamination molding, blow molding, hollow molding, compression molding, and calendar molding. The shape of the molded article is not particularly limited, and examples thereof include sheets, films, plates, particles, lumps, fibers, rods, porous bodies, and foams. The polycarbonate resin composition of the present invention can be molded into molded articles by, for example, injection molding, extrusion molding, or blow molding.
[0088] <Applications of molded products> The applications of the molded articles are not particularly limited, but since the polycarbonate resin composition of the present invention has excellent mechanical properties, weather resistance, and optical properties in addition to scratch resistance and transparency, it is suitably used for interior and exterior components of automobiles, building materials used outdoors (lighting covers, carports, highway soundproofing walls, etc.), display front panels, housings for electric and electronic devices, etc. EXAMPLES
[0089] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples.
[0090] <Measurement method> Various physical properties were measured according to the following methods.
[0091] (reduced viscosity) A polycarbonate resin sample was dissolved in methylene chloride to prepare a resin solution with a concentration of 0.6 g / dL. Using an Ubbelohde viscometer (manufactured by Moritomo Rika Kogyo Co., Ltd.), the solvent transit time t0 and the solution transit time t were measured at a temperature of 20.0°C ± 0.1°C. The relative viscosity η was calculated using the obtained t0 and t values according to the following formula (i). rel The relative viscosity η rel Using the concentration c [g / dL], the reduced viscosity η is calculated using the following equation (ii): sp The higher this value, the larger the molecular weight. η rel =t / t0(i) η sp / c=(η rel -1) / c (ii)
[0092] ( 1 (number average molecular weight measured by H-NMR) Approximately 15 mg of a polycarbonate resin sample was weighed out and dissolved in approximately 0.7 mL of deuterated chloroform. This was then placed in an NMR tube with an inner diameter of 5 mm. 1 H-NMR spectrum was measured. From the intensity ratio of the signals based on each repeating structural unit of the polycarbonate resin and the signals of various terminal groups, 1 The number average molecular weight was calculated using H-NMR. The equipment and conditions used are as follows: Equipment: JNM-ECZ400S (manufactured by JEOL Ltd.) ·Measurement temperature: 30℃ Relaxation time: 6 seconds Number of times accumulated: 64
[0093] For example, the copolymer polycarbonate resin of ISB (isosorbide) and CHDM (1,4-cyclohexanedimethanol) 1The H-NMR analysis is carried out as follows. The ISB double bond end and the CHDM double bond end are end group structures formed by a thermal decomposition reaction during the polymerization reaction.
[0094] [Range for calculating integral value] (a): 5.6-4.4 ppm: All derived from ISB repeating structural units (proton number: 4, molecular weight: 172.14) (b): 2.2-0.5 ppm: All derived from CHDM repeating structural units (proton number: 10, molecular weight: 170.21) (c): 4.4 ppm: from the hydroxyl end group of ISB (proton number: 1) (d): 3.6-3.5 ppm: derived from ISB hydroxy end group (proton number: 1) and CHDM hydroxy end group (proton number: 2) (e): 3.5-3.4 ppm: derived from CHDM hydroxyl end groups (proton count: 2) and ISB double bond end groups (proton count: 1) (f): 2.6 ppm: from ISB hydroxyl end group (proton number: 1) (g): 6.7-6.5 ppm: ISB double bond end group (proton number: 1) (h): 2.3 ppm: derived from CHDM double bond end group (proton number: 2) (i): 7.4 ppm: DPC (diphenyl carbonate) end group (proton number: 2, molecular weight: 93.10)
[0095] [Calculation of the value equivalent to the number of moles of each structure] Total ISB repeating units (a´): (a) integral value / 4 Total CHDM repeating unit (b´): (b) integral value / 10 ISB hydroxyl end group (c´): (c) integral value + (f) integral value CHDM hydroxy end group (d´): {(d) integral value - (f) integral value} / 2 + {(e) integral value - (g) integral value} / 2 ISB double bond end group (e´): (g) integral value ·CHDM double bond end group (f´): (h) integral value / 2 DPC end group (i´): (i) integral value / 2
[0096] [ 1 Calculation of number average molecular weight measured by H-NMR] (a´×172.14+b´×170.21+i´×93.10) / {(c´+d´+e´+f´+i´) / 2}
[0097] (Melt Viscosity) The polycarbonate resin sample was vacuum dried at 90° C. for 5 hours or more. Then, the melt viscosity of the polycarbonate resin sample was measured using a capillary rheometer (manufactured by Toyo Seiki Seisakusho Co., Ltd.). The measurement temperature was 240° C., and the shear rate was 6.08 to 1824 sec -1 The shear rate was set to 91.2 sec -1 The value at was used as the melt viscosity of the resin to be measured. The orifice used was 1 mmφ×10 mmL.
[0098] (glass transition temperature) The glass transition temperatures of polycarbonate resin, acrylic resin, and polycarbonate resin composition were measured using a differential scanning calorimeter DSC6220 (manufactured by SII Nano Technology Co., Ltd.). Approximately 10 mg of the sample was placed in an aluminum pan manufactured by the same company and sealed, and the measurement was started at 200°C under a nitrogen gas flow of 50 mL / min, and cooled to 0°C at a rate of 20°C / min. The sample was held at 0°C for 3 minutes, and then heated again to 200°C at a rate of 20°C / min. From the DSC data during the temperature rise, the extrapolated glass transition onset temperature, which is the temperature at the intersection of a straight line extending the low-temperature baseline to the high-temperature side and a tangent drawn at the point where the gradient of the curve of the stepwise change part of the glass transition is maximum, was obtained, and this was taken as the glass transition temperature.
[0099] (GPC) The number average molecular weight (Mn), weight average molecular weight (Mw), and molecular weight distribution (Mw / Mn) of the acrylic resin were measured using gel permeation chromatography (GPC). Approximately 10 mg of the obtained sample was dissolved in 10 mL of tetrahydrofuran, and the solution filtered through a 0.45 μm filter was used as a sample for GPC measurement. A polymer measurement guard column TSK-GUARD COLUMN SUPER HH (manufactured by Tosoh Corporation) and two polymer measurement columns TSK-GEL SUPER HM-H (manufactured by Tosoh Corporation) were connected in series to a gel permeation chromatography measurement device HLC-8320 (manufactured by Tosoh Corporation). A differential refractometer (RI) was used as a detector. The measurements were performed under the following conditions: separation column temperature: 40°C, mobile phase: tetrahydrofuran, mobile phase flow rate: 0.6 mL / min, sample injection amount: 10 μL. A calibration curve was prepared using polymethyl methacrylate (manufactured by Polymer Laboratories) with a known molecular weight and a peak molecular weight of 1,560 to 19,500,000 as the standard polymer, and Mn, Mw and Mw / Mn were determined.
[0100] (Haze) About 4 g of a polycarbonate resin composition sample dried at 90°C for 5 hours or more in a vacuum dryer was placed in a mold 7 cm long, 7 cm wide, and 0.5 mm thick, with polyimide films laid on the top and bottom of the sample, preheated at a temperature of 210 to 230°C for about 3 minutes, pressurized at a pressure of 10 MPa for about 3 minutes, removed from the mold, and cooled to produce a sheet of the polycarbonate resin composition. The haze of the sheet molded product made of the polycarbonate resin composition was measured using a haze meter NDH4000 (manufactured by Nippon Denshoku Industries Co., Ltd.) with a D65 light source in accordance with JIS K7136.
[0101] (Scratch resistance) The scratch resistance was evaluated using a friction and wear tester Type 30S (manufactured by Shinto Scientific Co., Ltd.) using a sheet molded product made of the above-mentioned polycarbonate resin composition. A Bencot M-3II (manufactured by Asahi Kasei Co., Ltd.) was folded six times and attached to an indenter with a bottom surface of 1 cm x 1 cm. A test was conducted to rub the surface of the sheet molded product under the conditions of room temperature, load 1 kg, stroke 30 mm, speed 9600 mm / min, and 3000 reciprocations. The sheet after the test was visually inspected, and a score of "3" was given if no scratches were visible, a score of "2" if faint scratches were visible, and a score of "1" if obvious scratches were visible.
[0102] <Raw materials used> The abbreviations and manufacturers of the compounds used in the following Examples and Production Examples are as follows.
[0103] ISB: Isosorbide (manufactured by Rocket Fleuret) CHDM: 1,4-cyclohexanedimethanol (SK Chemical) DPC: Diphenyl carbonate (manufactured by Mitsubishi Chemical Corporation) Phosphonic acid (Tokyo Chemical Industry Co., Ltd.) Irganox 1010: Pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (BASF)
[0104] CHMA: Cyclohexyl methacrylate (manufactured by Mitsubishi Chemical Corporation, corresponds to the structural unit of formula (2)) MMA: Methyl methacrylate (manufactured by Mitsubishi Chemical Corporation) ·MA: Methyl acrylate (manufactured by Mitsubishi Chemical Corporation) StMA: stearyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd., corresponds to the structural unit of formula (3))
[0105] MCR-M11: Methacrylate containing a polydimethylsiloxane structure represented by the following structural formula, number average molecular weight 900 (manufactured by Gelest, corresponds to the structural unit of formula (4))
[0106] [ka]
[0107] MCS-M11: Methacrylate containing a polydimethylsiloxane structure represented by the following structural formula, number average molecular weight 900 (manufactured by Gelest, corresponds to the structural unit of formula (4))
[0108] [ka]
[0109] MCR-M17: Methacrylate containing a polydimethylsiloxane structure represented by the following structural formula, number average molecular weight 5,000 (manufactured by Gelest)
[0110] [ka]
[0111] AMBN: 2,2'-azobis(2-methylbutyronitrile) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), product name V59 Sodium sulfate (Tokyo Chemical Industry Co., Ltd.) 1-Octanethiol (Tokyo Chemical Industry Co., Ltd.) Dispersant solution An aqueous dispersant solution containing 8% by weight of polymer was prepared by the method described in WO 2022 / 114157 and used as a dispersant for suspension polymerization.
[0112] <Production example 1 / Reference example 1: PC-1> Polycarbonate resin was polymerized using a continuous polymerization system consisting of three vertical stirring reactors, one horizontal stirring reactor, and a twin-screw extruder. ISB, CHDM, and DPC were melted in tanks, and continuously fed to the first vertical stirring reactor at flow rates of ISB 29.8 kg / hr, CHDM 12.6 kg / hr, and DPC 62.9 kg / hr (molar ratio ISB / CHDM / DPC=0.700 / 0.300 / 1.008). At the same time, an aqueous solution of calcium acetate monohydrate, a polymerization catalyst, was fed to the first vertical stirring reactor in an amount such that 1.5 μmol of calcium acetate monohydrate was added to 1 mol of all dihydroxy compounds. The internal temperature, internal pressure, and residence time of each reactor were as follows: first vertical stirring reactor: 190°C, 25kPa, 120 minutes, second vertical stirring reactor: 195°C, 10kPa, 90 minutes, third vertical stirring reactor: 205°C, 4kPa, 45 minutes, fourth horizontal stirring reactor: 220°C, 0.1-1.0kPa, 120 minutes. The internal pressure of the fourth horizontal stirring reactor was finely adjusted during operation so that the reduced viscosity of the resulting polycarbonate resin was 0.50dL / g.
[0113] The polycarbonate resin extracted from the fourth horizontal stirred reactor was fed in a vented twin-screw extruder TEX30α (manufactured by Japan Steel Works, Ltd.) in a molten state. The extruder had three vacuum vents, where the remaining low molecular weight components in the resin were removed by volatilization, and phosphonic acid was added as a catalyst deactivator just before the first vent at 0.64 ppm by weight relative to the polycarbonate resin, and Irganox1010 was added just before the third vent at 1000 ppm by weight relative to the polycarbonate resin. The polycarbonate resin that had passed through the extruder was still in a molten state and passed through a 10 μm Ultipleats candle filter (manufactured by PALL) to filter out foreign matter. The polycarbonate resin was then extruded in a strand shape from the die, cooled with water, solidified, and cut with a rotary cutter to pelletize. The polycarbonate resin obtained in this manner is designated as "PC-1". The analysis results of this polycarbonate resin are shown in Table 1 as Reference Example 1. The weight percentage of each structural unit constituting the polycarbonate resin in Table 1 is the weight percentage of the polycarbonate resin. 1This value was measured by H-NMR analysis.
[0114] [Table 1]
[0115] <Production Example 2 Reference Example 2: Acryl-1> In a polymerization apparatus equipped with a stirrer, a cooling tube, and a thermometer, 450 parts of deionized water, 0.1 parts of sodium sulfate, and 1 part of a dispersant aqueous solution were added and stirred to obtain a uniform aqueous solution. Next, 178 parts of CHMA, 20 parts of StMA, 2 parts of MA, 0.4 parts of 1-octanethiol, and 0.2 parts of AMBN as a polymerization initiator were added and stirred to obtain an aqueous dispersion. Next, the inside of the polymerization apparatus was fully replaced with nitrogen, and the aqueous dispersion was heated to 75°C and held for 3 hours, and then heated to 90°C and held for 1 hour. Thereafter, the reaction solution was cooled to 40°C to obtain an aqueous suspension of an acrylic resin. This aqueous suspension was filtered with a filter cloth, and the filtrate was washed with deionized water and dried in a hot air dryer at 60°C for 10 hours to obtain an acrylic resin (Acryl-1). The analysis results of this acrylic resin are shown in Table 2 as Reference Example 2. The weight percentage of each of the structural units constituting the acrylic resin in Table 2 is a value calculated from the blending amount of each of the monomers described above.
[0116] <Production Example 3 Reference Example 3: Acryl-2> An acrylic resin (Acryl-2) was obtained in the same manner as in Production Example 2, except that 178 parts of CHMA, 20 parts of MCR-M11, 2 parts of MA, 0.8 parts of 1-octanethiol, and 0.4 parts of AMBN were used. The analysis results of this acrylic resin are shown in Table 2 as Reference Example 3.
[0117] <Production Example 4, Reference Example 4: Acryl-3> An acrylic resin (Acryl-3) was obtained in the same manner as in Production Example 2, except that 178 parts of CHMA, 20 parts of MCR-M11, 2 parts of MA, 0.4 parts of 1-octanethiol, and 0.2 parts of AMBN were used. The analysis results of this acrylic resin are shown in Table 2 as Reference Example 4.
[0118] <Production Example 5, Reference Example 5: Acryl-4> An acrylic resin (Acryl-4) was obtained in the same manner as in Production Example 2, except that 158 parts of CHMA, 40 parts of MCR-M11, 2 parts of MA, 0.4 parts of 1-octanethiol, and 0.2 parts of AMBN were used. The analysis results of this acrylic resin are shown in Table 2 as Reference Example 5.
[0119] <Production Example 6, Reference Example 6: Acryl-5> An acrylic resin (Acryl-5) was obtained in the same manner as in Production Example 2, except that 178 parts of CHMA, 20 parts of MCS-M11, 2 parts of MA, 0.4 parts of 1-octanethiol, and 0.2 parts of AMBN were used. The analysis results of this acrylic resin are shown in Table 2 as Reference Example 6.
[0120] <Production Example 7, Reference Example 7: Acryl-6> An acrylic resin (Acryl-6) was obtained in the same manner as in Production Example 2, except that 178 parts of CHMA, 20 parts of MCR-M17, 2 parts of MA, 0.4 parts of 1-octanethiol, and 0.2 parts of AMBN were used. The analysis results of this acrylic resin are shown in Table 2 as Reference Example 7.
[0121] <Production Example 8, Reference Example 8: Acrylic-7> An acrylic resin (Acryl-8) was obtained in the same manner as in Production Example 2, except that 178 parts of MMA, 20 parts of MCR-M11, 2 parts of MA, 0.4 parts of 1-octanethiol, and 0.2 parts of AMBN were used. The analysis results of this acrylic resin are shown in Table 2 as Reference Example 8.
[0122] [Table 2]
[0123] <Example 1> 90 parts by weight of PC-1 and 10 parts by weight of Acryl-1 were blended and dried in a vacuum dryer at 90°C for 5 hours or more, and then melt-kneaded for 3 minutes using a kneading device, Labo Plastomill (manufactured by Toyo Seiki Seisakusho Co., Ltd.), at a temperature of 220°C and a screw rotation speed of 100 rpm, to obtain a polycarbonate resin composition. The obtained polycarbonate resin composition was subjected to the above-mentioned various evaluations. The results are shown in Table 3.
[0124] <Examples 2 to 5 and Comparative Examples 1 to 3> A polycarbonate resin composition was obtained in the same manner as in Example 1, except that the formulation was as shown in Table 3. The obtained polycarbonate resin composition was subjected to the various evaluations described above. The results are shown in Table 3.
[0125] [Table 3]
[0126] From the above results, it was found that the polycarbonate resin compositions of the present invention have a glass transition temperature in a suitable range and are excellent in transparency and scratch resistance (Examples 1 to 5). In contrast, it was found that the polycarbonate resin compositions of the comparative examples have at least one of haze and scratch resistance outside the suitable range and do not achieve both transparency and scratch resistance (Comparative Examples 1 to 3). [Industrial Applicability]
[0127] The polycarbonate resin composition of the present invention is excellent in mechanical properties, weather resistance, and optical properties in addition to transparency and scratch resistance, and is therefore suitable for use in interior and exterior components of automobiles, building materials used outdoors (lighting covers, carports, highway soundproofing walls, etc.), display front panels, housings for electric and electronic devices, etc.
Claims
1. A polycarbonate resin containing 30% by weight or more and 90% by weight or less of a structural unit represented by the following formula (1); A polycarbonate resin composition comprising an acrylic resin containing 50% by weight or more and 99% by weight or less of a structural unit represented by the following formula (2), and containing 1% by weight or more and 50% by weight or less of at least one selected from a structural unit represented by the following formula (3) and a structural unit represented by the following formula (4): 【Chemistry 1】 【Chemistry 2】 (In formula (2), R 1 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent. 2 represents an alkyl group or cycloalkyl group containing a cyclohexane structure and which may further have a substituent.) 【Chemistry 3】 (In formula (3), R 3 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent. 4 is an alkyl group having 10 to 30 carbon atoms which may have a substituent. 【Chemistry 4】 (In formula (4), R 5 R is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may have a substituent. 6 is an alkyl group having 1 to 6 carbon atoms which has an organopolysiloxane as a substituent and which may have an ether bond. The number average molecular weight of the structural unit represented by formula (4) is 500 or more and 3,000 or less.
2. The polycarbonate resin composition according to claim 1, wherein the polycarbonate resin has a glass transition temperature of 90°C or higher and 150°C or lower.
3. 3. The polycarbonate resin composition according to claim 1, wherein the polycarbonate resin contains a structural unit derived from an aliphatic dihydroxy compound or an alicyclic dihydroxy compound.
4. 3. The polycarbonate resin composition according to claim 1, wherein the acrylic resin has a weight average molecular weight (Mw) of 10,000 or more and 200,000 or less.
5. 3. The polycarbonate resin composition according to claim 1, comprising 70% by weight or more and 99% by weight or less of the polycarbonate resin and 1% by weight or more and 30% by weight or less of the acrylic resin.
6. A molded article obtained by molding the polycarbonate resin composition according to claim 1 or 2.
7. The molded article according to claim 6, which is used as an automobile interior material or an automobile exterior material.
Citation Information
Patent Citations
Polycarbonate resin composition and molded part thereof
JP2015199954A
Polycarbonate resin composition and molded article composed of the same
JP2017008140A
Polycarbonate and process for producing the same
WO2004111106A1
Polycarbonate copolymer and process for production thereof
WO2007148604A1