Active energy ray-curable resin composition, cured coating film, and laminate
A urethane (meth)acrylate-based active energy ray-curable resin composition addresses adhesion and hardness issues in polycarbonate coatings by using isosorbide-derived materials, offering improved properties and environmental sustainability.
Patent Information
- Application Number
- JP2023049986
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Existing coatings for polycarbonate materials derived from petroleum resources face challenges in achieving adequate adhesion, processability, and hardness, particularly when using urethane (meth)acrylate compositions, and there is a demand for plant-based alternatives to reduce environmental impact.
A coating material comprising a urethane (meth)acrylate synthesized from an isocyanate compound and a hydroxyl group-containing monofunctional (meth)acrylate, combined with an acrylic monomer (co)polymer and a photopolymerization initiator, forms an active energy ray-curable resin composition that can be applied to isosorbide-containing substrates, ensuring excellent hardness, elongation, and adhesion.
The composition provides a cured coating film with enhanced hardness, elongation, and adhesion, suitable for isosorbide-containing substrates, while promoting the use of plant-based materials and reducing environmental impact.
Smart Images

Figure 2024139167000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating material to be applied to an isosorbide-containing substrate. [Background technology]
[0002] Display materials, electric and electronic parts, automotive parts, construction materials, lenses, containers, packaging Polycarbonate, polyester, polymethyl methacrylate, trimethyl methacrylate, etc. are used for various applications. Plastic materials such as acetyl cellulose, polystyrene, and polyvinyl chloride are used. Among them, polycarbonate, for example, is used because of its excellent impact resistance and heat resistance. It is one of the resins that can be used in a wide range of applications.
[0003] Polycarbonate and many other plastic products are generally derived from petroleum resources. However, because this would lead to the depletion of petroleum resources, it is now being used with plant-based raw materials. In addition, due to the increase in carbon dioxide emissions, Global warming caused by carbon dioxide is also an issue, and plant-based biofuels are also considered to be carbon neutral. It is required to use raw materials of
[0004] Polycarbonate using isosorbide as a plant-derived compound has been proposed (Patent Reference 1) Coating using urethane (meth)acrylate on polycarbonate However, the coating film with many (meth)acryloyl groups does not have sufficient processability. In addition, when a bifunctional (meth)urethane acrylate is used, Adequate adhesion was not obtained. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication No. 2016-079321 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention relates to a copolymer of a specific urethane (meth)acrylate and a (meth)acrylic monomer. By forming an active energy ray-curable resin composition containing a polymer, an active energy ray-curable resin composition which is excellent in hardness, elongation, and adhesion when applied to a material; A cured coating film made of the active energy ray-curable resin composition, and The present invention aims to provide a laminate having a layer made of a curable resin composition. [Means for solving the problem]
[0007] The present invention has the following aspects. That is, the above object of the present invention can be achieved by the following means [1] to [7]. [1] A coating material to be applied to an isosorbide-containing substrate, A urethane (meth)acrylate (A) synthesized from the following (a1) and (a2), (B) an active energy polymer containing an acrylic monomer (co)polymer and a photopolymerization initiator (C) A gy-ray curable resin composition. (a1) An isocyanate compound having at least two isocyanate groups (a2) Hydroxyl group-containing monofunctional (meth)acrylate [2] The amount of urethane (meth)acrylate (A) in the active energy ray curable resin composition is The active ingredient according to [1] is 5% by mass or more and 80% by mass or less based on the total amount of solids in the composition. Energy ray curable resin composition. [3] The substrate is a polycarbonate substrate having isosorbide as a structural unit. [1 ] or [2]. The active energy ray-curable resin composition according to the present invention. [4] The amount of the (co)polymer (B) of the (meth)acrylic monomer is such that the active energy [1] The content is 5% by mass or more and 60% by mass or less based on the total amount of solids in the radiation-curable resin composition. The active energy ray-curable resin composition according to [3]. [5] The compound according to any one of [1] to [4], further comprising a compound (D) having a quaternary ammonium base. An active energy ray-curable resin composition. [6] A cured coating film of the active energy ray-curable resin composition according to any one of [1] to [5]. [7] (Co)polymer of urethane (meth)acrylate (A) and (meth)acrylic monomer An active energy ray-curable resin composition comprising (B) and a photopolymerization initiator (C), The cured product obtained by curing the active energy ray-curable resin composition has an elongation property at 80° C. The active energy ray-curable resin composition has a viscosity of 20% or more. [8] A urethane (meth)acrylate (A) synthesized from the following (a1) and (a2); , (B) a (co)polymer of a (meth)acrylic monomer and (C) an active ethylene glycol containing a photopolymerization initiator A laminate obtained by coating an energy ray-curable resin composition on an isosorbide-containing substrate. (a1) An isocyanate compound having at least two isocyanate groups (a2) Hydroxyl group-containing monofunctional (meth)acrylate Effect of the Invention
[0008] According to the present invention, when applied to an isosorbide-containing substrate, the composition has excellent hardness, elongation, and adhesion. Active energy ray curable resin composition having properties of: and a laminate having a layer made of the active energy ray-curable resin composition. You can donate your body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] <Active energy ray resin composition> The active energy ray-curable resin composition of the present invention (hereinafter referred to as the present composition) is The urethane (meth)acrylate ( A) [referred to as component (A)], (co)polymer (B) of a (meth)acrylic monomer [referred to as component ( A photopolymerization initiator (C) [hereinafter referred to as component (C)] is used. It is a curable resin composition.
[0010] [Component A] The component (A) contained in the composition has a structure derived from the compound (a1) and the compound (a2). Component (A) is, for example, a compound (a 1) and compound (a2) are reacted to obtain urethane (meth)acrylates. Component (A) is a cured coating film obtained by curing the present composition (hereinafter simply referred to as the cured coating film). Contributes to the toughness of the steel.
[0011] [Compound (a1)] The compound (a1) is an isocyanate compound having at least two isocyanate groups. The compound (a1) contributes to the flexibility of the coating film. As the compound (a1), for example, a compound which has been conventionally used for producing urethane (meth)acrylates can be used. As the compound (a1), for example, 1,3-phenylene can be used. Diisocyanate, 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate 2,6-tolylene diisocyanate, 2,4-diphenylmethane diisocyanate Aromatic polyisocyanates such as ethyl ether, 4,4'-diphenylmethane diisocyanate, etc. Diisocyanate, Hexamethylene diisocyanate, 2,2,4-trimethylhexyl Hexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate aliphatic polyisocyanates such as lysine diisocyanate and lysine triisocyanate; Isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, Alicyclic polyisocyanates such as methylcyclohexylene diisocyanate; xylene diisocyanate Aromatic and aliphatic polyisocyanates such as isocyanate, tetramethylxylylene diisocyanate, etc. biuret, allophanate, isocyanurate, etc. of these. . Among these, 1,3-phenylenediisopropyl ether is preferred because it can impart excellent toughness to the coating film. Cyanate, 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate , 2,6-tolylene diisocyanate, 2,4-diphenylmethane diisocyanate, 4 ,4'-Diphenylmethane diisocyanate, Isophorone diisocyanate, Bis(4- Isocyanatocyclohexyl)methane, 1,2-hydrogenated xylylene diisocyanate, 1,4 -Hydrogenated xylylene diisocyanate, hydrogenated tetramethyl xylylene diisocyanate, Bornane diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, Aliphatic diisocyanates such as 2,2,4-trimethylhexamethylene diisocyanate is preferred. In the synthesis of component (A), one type of compound may be used alone as compound (a1), or two or more types of compound (a2) may be used in combination. The compounds may be used in combination.
[0012] [Compound (a2)] Compound (a2) has one hydroxyl group and one (meth)acryloyloxy group in the compound. Compound (a2) is a compound having a hydroxyl group similar to that of compound (a1) or compound (a1 The isocyanate group of the intermediate compound having an isocyanate group obtained from Any compound capable of forming a bond and introducing a (meth)acryloyloxy group into component (A) may be used. . Examples of the compound (a2) include 2-hydroxyethyl (meth)acrylate, 2- Hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate , 6-hydroxyhexyl (meth)acrylate, cyclohexanedimethanol mono(meth)acrylate (meth)acrylates and caprolactone adducts of these (meth)acrylates. . Among these, 2-hydroxyethyl ( (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyric acid Chile (meth)acrylate is preferred. In the synthesis of the component (A), one type of compound may be used alone or two or more types of compound (a2) may be used. Can be used together.
[0013] In the synthesis of component (A), in addition to compounds (a1) and (a2), polyol (a3) is The polyols may be used in combination, for example, neopentyl glycol, ethylene glycol, Glycol, Diethylene Glycol, Propylene Glycol, 1,6-Hexanediol 1,4-butanediol, 1,9-nonanediol, 1,10-decanediol, 3- Methylpentanediol, 2,4-diethylpentanediol, tricyclodecane dimeth 1,4-Cyclohexanedimethanol, 1,2-Cyclohexanedimethanol, 1 ,3-Cyclohexanedimethanol, Cyclohexanediol, Hydrogenated Bisphenol A, Polyols such as trimethylolpropane and pentaerythritol; these polyhydric alcohols In addition, alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide These polyhydric alcohols and ε-caproic acid-added polyether modified polyols Lactones such as γ-butyrolactone, γ-valerolactone, and δ-valerolactone polycaprolactone polyols obtained by reacting these polyhydric alcohols and Polybasic acids and ε-caprolactone, γ-butyrolactone, γ-valerolactone, δ-valerolactone Caprolactone-modified polyester poly(propylene glycol) obtained by reacting with lactones such as lactone and tetrahydrofuran. 1,6-Hexanediol, 3-Methylpentanediol, 2,4-Diethylpentanediol Tandiol, trimethylhexanediol, 1,4-butanediol, 1,5-pentane Diol, 1,4-cyclohexanediol and other diols, ethylene carbonate, Dimethyl carbonate, diethyl carbonate, di-n-propyl carbonate, diisopropyl carbonate Propyl carbonate, dibutyl carbonate, dicyclohexyl carbonate, diphenyl carbonate Polycarbonate obtained by transesterification with carbonate esters such as diphenyl carbonate Polybutadiene glycol, polyether polyol, polyester polyol diols and amide diols. Among these, neopentyl glycol and ethyl glycol are preferred because they provide good curing properties for the present composition. Ethylene glycol, diethylene glycol, propylene glycol, 1,6-hexanediol 1,4-butanediol, 1,9-nonanediol, 1,10-decanediol, 3 -Methylpentanediol, 2,4-diethylpentanediol, tricyclodecanediol Methanol, 1,4-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, 1,3-Cyclohexanedimethanol, Cyclohexanediol, Hydrogenated Bisphenol A Polyols such as trimethylolpropane and pentaerythritol are preferred. In the synthesis of component (A), one type of compound may be used alone or two or more types of compound (a3) may be used. They may also be used in combination.
[0014] The molecular weight of (a3) is preferably 500 or more and less than 3,000. When formed into a coating film, the moisture resistance becomes good, and when it is below the upper limit, the appearance of the coating film becomes good.
[0015] [Synthesis method of component (A)] The component (A) can be synthesized, for example, by a conventionally known urethane (meth)acrylate synthesis method. As a specific synthesis method, for example, 2 mo of compound (a1) is placed in a flask. 1 mole of the mixture was added, and a known catalyst such as dibutyltin dilaurate was added. The temperature in the flask was then increased to 1. While maintaining the temperature at 40 to 80°C, 1 mol of compound (a3) was added dropwise using a dropping funnel. A urethane prepolymer having an isocyanate group at its end is obtained. Compound (a2) having a hydroxyl group equivalent to the isocyanate group remaining at the terminal of the tandem polymer )2 mol is added dropwise and reacts with the isocyanate group of the urethane prepolymer at 60 to 85°C. By carrying out an addition reaction with the hydroxyl group of the compound (a2), component (A) can be synthesized. The end point of the reaction can be determined by quantifying the remaining isocyanate groups. The reaction rate at the end point is It is preferably 97% or more, and more preferably 99% or more.
[0016] [Mixing ratio of component (A)] The blending ratio of component (A) in the present composition is determined from the viewpoint of the balance between hardness and elongation. The amount is preferably 5% by mass or more and 80% by mass or less based on the total amount of solids in the gyro-curable resin composition. More preferably, the content is 7% by mass or more and 70% by mass or less, and even more preferably, the content is 10% by mass or more and 60% by mass or less. The blending ratio of component (A) is equal to or less than the lower limit, and the balance between hardness and elongation is improved. If it is below the upper limit, the adhesion is excellent.
[0017] [Component (B)] Component (B) is a (co)polymer of a (meth)acrylic monomer. For example, one or more conventionally known radical polymerization initiators may be used in the presence of the initiator. The (meth)acrylic monomer is polymerized by a method such as solution polymerization, bulk polymerization, or emulsion polymerization. Methods include:
[0018] Examples of the vinyl monomers that are the raw materials for component (B) include methyl (meth)acrylate. ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate Acrylates, t-butyl (meth)acrylate, isobutyl (meth)acrylate, 2 -Ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, cyclohexyl Sil(meth)acrylate, benzyl(meth)acrylate, dicyclopentanyl(meth)acrylate ) acrylate, dicyclopentenyl (meth)acrylate, 2-dicyclopentenoxy Ethyl (meth)acrylate, isobornyl (meth)acrylate, methoxyethyl (meth)acrylate (meth)acrylate, ethoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate acrylate, methoxyethoxyethyl (meth)acrylate, ethoxyethoxyethyl (meth)acrylate (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, etc., which do not contain hydroxyl groups (Meth)acrylate; 2-Hydroxyethyl (meth)acrylate, 2-Hydroxyprop 3-Hydroxypropyl (meth)acrylate, 4-Hydroxypropyl (meth)acrylate hydroxyalkyl (meth)acrylates such as 2-hydroxybutyl (meth)acrylate; Adduct of hydroxyethyl (meth)acrylate and ethylene oxide, 2-hydroxyethyl Adduct of ethyl (meth)acrylate and propylene oxide, 2-hydroxyethyl (meth)acrylate ) acrylate and ε-caprolactone adducts, etc. hydroxyl-containing vinyl monomers such as adducts of vinylates with alkylene oxides or organic lactones; Styrene, α-methylstyrene, pt-butylstyrene, vinyltoluene, and other styrenes or styrene derivatives; N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide p) Acrylamide and other acrylamides; (meth)acrylic acid, itaconic acid, maleic acid unsaturated carboxylic acids such as fumaric acid; unsaturated nitriles such as (meth)acrylonitrile; diethyl itaconate, dibutyl maleate, dibutyl fumarate, diethyl itaconate, unsaturated carboxylates such as dibutyl phosphate; vinyl acetate, vinyl propionate, and other vinyls Esters are included. Among these, methyl (meth)acrylate and ethyl (meth)acrylate are preferred from the viewpoint of hardness. acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (Meth)acrylate, Isobutyl (Meth)acrylate, 2-Ethylhexyl (Meth)acrylate Acrylate, isobornyl (meth)acrylate is preferred. As component (B), one type of (co)polymer may be used alone, or two or more types of (co)polymers may be used in combination. It can be used in combination.
[0019] [Bulk Proportion of Component (B)] The blending ratio of component (B) is based on the total amount of solids in the active energy ray-curable resin composition. Preferably, the content is 5% by mass or more and 60% by mass or less, more preferably 6% by mass or more and 55% by mass or less. More preferably, the blending ratio of component (B) is 8% by mass or more and 50% by mass or less. If it is equal to or less than the upper limit, the hardness is superior.
[0020] The molecular weight of component (B) is preferably 3,000 to 150,000, more preferably 4,000 to 1 The molecular weight is more preferably 40,000, and further preferably 5,000 to 130,000. If it is above the lower limit range, the toughness of the coating film will improve and the hardness will increase. If it is below the upper limit range, The smoothness of the surface is improved. The glass transition temperature (Tg) of the component (B) is preferably 30 to 150°C, and more preferably 40 to 140°C. The glass transition temperature is more preferably 0° C., and further preferably 50 to 130° C. If it is present, the toughness of the coating film will improve, resulting in improved hardness. If it is below the upper limit of the range, the workability of the coating film will improve. do.
[0021] [Component (C)] Component (C) is a photopolymerization initiator that cures the composition by irradiation with active energy rays. Component (C) is, for example, a benzophenone type, an anthraquinone type, an arsenic type, Kilphenone type, thioxanthone type, acylphosphine oxide type, phenylglyon Examples of photopolymerization initiators include xylate-type photopolymerization initiators.
[0022] Examples of component (C) include benzophenone, 4-methylbenzophenone, 2,4, 6-Trimethylbenzophenone, methyl orthobenzoylbenzoate and 4-phenyl Benzophenone and other benzophenone types; t-butylanthraquinone and 2-ethylanthraquinone Anthraquinone type such as laquinone; 2-hydroxy-2-methyl-1-phenylpropane 1-one, oligo{2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl Benzyl]propanone}, benzyl dimethyl ketal, 1-hydroxycyclohexylphenyl Ketone, Benzoin Methyl Ether, 2-Methyl-[4-(methylthio)phenyl]- 2-Morpholino-1-propanone and 2-hydroxy-1-{4-[4-(2-hydroxy dimethyl-2-methylpropionyl)benzyl]phenyl}-2-methylpropan-1-one, Alkylphenone type such as 2,2-dimethoxy-1,2-diphenylethan-1-one;2 -Benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,di Thioxanthone types such as ethylthioxanthone and isopropylthioxanthone; 2,4, 6-Trimethylbenzoyldiphenylphosphine oxide, bis(2,6-dimethoxy Benzoyl)-2,4,4-trimethylpentylphosphine oxide and bis(2,4 ,6-trimethylbenzoyl)-phenylphosphine oxide and other acylphosphines Oxide type: Phenylglyoxylic acid methyl ester and other phenylglyoxylic acids Examples of the photopolymerization initiator include a silyl type photopolymerization initiator. Among these, benzophenone and 2-ethyl anthracene are preferred from the viewpoint of dryness to the touch of the present composition. Lakinone, 1-hydroxycyclohexyl phenyl ketone, 2,2-dimethoxy-1,2 -Diphenylethan-1-one is preferred. As component (C), one type of compound can be used alone, or two or more types can be used in combination.
[0023] [Amount of component (C)] The amount of component (C) to be blended is, based on the total amount of solids in the active energy ray-curable resin composition, The content is preferably 0.1% by mass or more and 15% by mass or less, and more preferably 1% by mass or more and 10% by mass or less. The greater the amount of component (C), the better the curing properties of the composition in an air atmosphere. The lower the concentration, the less amount of component (C) tends to remain in the cured coating film.
[0024] [Component (D)] Component (D) is a compound having a quaternary ammonium salt group (provided that the (meth)acrylic (Excluding (B) the (co)polymer of a cyclic monomer). Component (D) is, for example, a quaternary ammonium salt. Homopolymers of monomers having a group or monomers having a quaternary ammonium salt group or other monomers and polymers obtained by copolymerizing the same with the copolymer.
[0025] Examples of the quaternary ammonium base-containing monomer that can be used as component (D) include amines. (Meth)acrylic acid esters of non-alcohols, specifically, N,N-dimethylaminoethyl N,N-Diethylaminoethyl (meth)acrylate, N,N -Dimethylaminopropyl (meth)acrylate, N,N-Diethylaminopropyl (meth)acrylate (meth)acrylate, N,N-dimethylaminobutyl (meth)acrylate, N,N-diethylene N,N-Dihydroxyethylaminoethyl(meth)acrylate (meth)acrylate, and in particular N,N-dimethylaminoethyl (meth)acrylate. The two alkyl groups in the N,N-dialkylamino group may be different. good. As the quaternary ammonium salt of the N,N-dialkylamino group-containing monomer, for example, commercially available Quaternary products of N,N-dimethylaminoethyl methacrylate with methyl chloride [e.g. For example, the product name "Light Ester (registered trademark) DQ-100" manufactured by Kyoeisha Chemical Co., Ltd. The quaternary ammonium salts of N,N-dialkylamino group-containing monomers are It can also be produced by the quaternization reaction of (meth)acrylic acid esters of non-alcohols. .
[0026] The polymer contains polymerizable monomer units other than the monomer having a quaternary ammonium salt group. Examples of such polymerizable monomers include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate , 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, lauryl alkyl(meth)acrylates such as tridecyl(meth)acrylate, tridecyl(meth)acrylate, etc. (Meth)acrylic esters of the above amino alcohols; 2-Hydroxyethyl (Meth)acrylate, 2-hydroxypropyl (meth)acrylate, hydroxybutyrate hydroxyalkyl (meth)acrylates such as benzyl (meth)acrylate; ) acrylate, cyclohexyl (meth) acrylate, isobornyl (meth) acrylate acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate (meth)acrylate, ethoxyethyl (meth)acrylate, ethyl carbitol (meth) Acrylate, butoxyethyl (meth)acrylate, cyanoethyl (meth)acrylate glycidyl (meth)acrylate and other (meth)acrylates, styrene, methyl These may be used alone or in combination of two or more. Among these, the polymerizable monomer having a highly hydrophobic long-chain alkyl group is preferably used to form a polymer. This is preferred because it allows the cured material layer to segregate at the air interface, thereby enhancing the antistatic properties of the cured material layer. As a polymerizable monomer having such a long chain alkyl group, stearyl (meth)aryl is preferably used. acrylate, lauryl (meth)acrylate, and tridecyl (meth)acrylate. can be.
[0027] [Amount of component (D)] The proportion of the quaternary ammonium base-containing monomer unit in the polymer is preferably 10 to 90% by weight. The higher the ratio, the higher the antistatic property becomes. The transparency of the cured layer tends to improve as the temperature increases. The weight average molecular weight of the polymer is preferably 800 to 120,000, more preferably 2,000 to 60, 000 is more preferred.
[0028] The polymer can be produced by a radical polymerization reaction using the above-mentioned raw material monomers. The radical polymerization reaction is preferably carried out in an organic solvent in the presence of a radical polymerization initiator. stomach. Examples of organic solvents used in radical polymerization reactions include acetone and methyl ethyl ketone. Ketone solvents such as (MEK); ethanol, methanol, isopropyl alcohol (IP A) Alcohol solvents such as isobutanol; ethylene glycol dimethyl ether, Ether solvents such as propylene glycol monomethyl ether; ethyl acetate, propylene glycol Esters such as ricin monomethyl ether acetate and 2-ethoxyethyl acetate Solvent: Aromatic hydrocarbon solvents such as toluene. Only one of these organic solvents is used. or a combination of two or more of them may be used.
[0029] The radical polymerization initiator used in the radical polymerization reaction is, for example, benzoylperoxycarbonyl. peroxides such as di-t-butyl peroxide; 2,2'-azobisbutyronite aryl, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis( 4-Methoxy-2,4-dimethylvaleronitrile and other azo compounds. The radical polymerization initiator may be used alone or in combination of two or more. The polymerization initiator is used in an amount of 0.01 to 5 parts by weight per 100 parts by weight of the total raw material monomers. It is preferable to use
[0030] In addition, during radical polymerization reactions, chain transfer is performed to control the weight average molecular weight of the polymer. Examples of the chain transfer agent include butanethiol and octanethiol. thiol, decanethiol, dodecanethiol, hexadecanethiol, octadecanethiol Cyclohexyl mercaptan, thiophenol, octyl thioglycolate, 2-methyl Octyl mercaptopropionate, Octyl 3-mercaptopropionate, Mercaptopropionate Pionic acid 2-ethylhexyl ester, thioglycolic acid 2-ethylhexyl, butyl- 3-Mercaptopropionate, Mercaptopropyltrimethoxysilane, Methyl-3- Mercaptopropionate, 2,2-(ethylenedioxy)diethanethiol, ethanethiol ol, 4-methylbenzenethiol, octanoic acid 2-mercaptoethyl ester, 1, 8-Dimercapto-3,6-dioxaoctane, Decanetrithiol, Dodecylmercapto Tan, diphenyl sulfoxide, dibenzyl sulfide, 2,3-dimethylcapto-1- Propanol, mercaptoethanol, thiosalicylic acid, thioglycerol, thioglycol mercaptopropionic acid, thiomalic acid, mercaptoacetic acid, mercaptoamic acid Examples of such compounds include thiol compounds such as mercaptoethanesulfonic acid and 2-mercaptoethanesulfonic acid. Only one type may be used, or two or more types may be used in combination.
[0031] The amount of the chain transfer agent used is 0.1 to 25 parts by weight per 100 parts by weight of the total raw material monomers. It is preferably 0.5 to 20 parts by weight, more preferably 1.0 to 15 parts by weight.
[0032] The reaction time of the radical polymerization reaction is preferably 1 to 20 hours, more preferably 3 to 12 hours. The reaction temperature is preferably from 40 to 120°C, and more preferably from 50 to 100°C.
[0033] [Amount of component (D)] The amount of component (D) to be blended is, based on the total amount of solids in the active energy ray-curable resin composition, The content is preferably 3% by mass or more and 30% by mass or less, and more preferably 5% by mass or more and 20% by mass or less. The more component (D) is added, the lower the surface resistivity and the better the antistatic performance. This tends to improve the transparency of the coating film.
[0034] [Other ingredients] As other components, various (meth)acrylate compounds can be added. For example, Examples of monomers having four or more (meth)acryloyl groups include dipentaerythritol, Dipentaerythritol penta(meth)acrylate, Dipentaerythritol hexa(meth)acrylate acrylate, caprolactone-modified dipentaerythritol penta(meth)acrylate, and , Caprolactone-modified dipentaerythritol hexa(meth)acrylate, Pentaerythritol Pentaerythritol tetra(meth)acrylate, ethoxylated pentaerythritol tetra Poly(meth)acrylates having a pentaerythritol skeleton, such as poly(meth)acrylate G. Trimethylolpropane such as ditrimethylolpropane tetra(meth)acrylate Poly(meth)acrylates with a skeleton, polyester poly(meth)acrylates, urea tan(meth)acrylate and the like.
[0035] Examples of polyester poly(meth)acrylates that can be used as other components include , phthalic acid, succinic acid, hexahydrophthalic acid, tetrahydrophthalic acid, terephthalic acid, Polybasic acids such as azelaic acid and adipic acid, ethylene glycol, hexanediol, poly Esterification reaction with polyols such as polyethylene glycol and polytetramethylene glycol The polyester polyol obtained by the reaction with (meth)acrylic acid or its derivative is reacted. The resulting compounds include:
[0036] Examples of urethane (meth)acrylates that can be used as other components include isophorone. Polyisocyanates such as 1,2-diisocyanate and pentaerythritol, which have hydroxyl groups, are used. A urethane (meth)acryloyl group is obtained by a urethane reaction with a compound having several (meth)acryloyl groups. p) Acrylates.
[0037] If necessary, a photosensitizer may be added to the composition. Examples of the photosensitizer include: Methyl 4-dimethylaminobenzoate, Ethyl 4-dimethylaminobenzoate, 4-Dimethyl Examples of known photosensitizers include amyl aminobenzoate and 4-dimethylaminoacetophenone. It is possible.
[0038] The composition may contain, as required, ultraviolet absorbers, light stabilizers, leveling agents, antioxidants, yellowing agents, etc. Anti-deformation agents, bluing agents, pigments, dyes, defoamers, thickeners, anti-settling agents, anti-fogging agents, etc. The following additives may also be used:
[0039] [Organic solvents] The composition may contain an organic solvent as necessary for adjusting the viscosity, etc. The organic solvents include water, aromatic solvents such as toluene and xylene, methyl ethyl ketone, etc. Ketone solvents such as acetone, methyl isobutyl ketone, and cyclohexanone; ether, isopropyl ether, tetrahydrofuran, dioxane, ethylene glycol Dimethyl ether, ethylene glycol diethyl ether, diethylene glycol di Methyl ether, diethylene glycol diethyl ether, propylene glycol monomer Ether solvents such as diethyl ether, anisole, and phenetole; ethyl acetate, butyl acetate , isopropyl acetate, ethylene glycol diacetate and other ester solvents; dimethyl ether Amide solvents such as formamide, diethylformamide, and N-methylpyrrolidone; Cellosolve solvents such as ethyl cellosolve, butyl cellosolve, etc.; methanol, ethanol Alcohol-based solvents such as ethanol, propanol, isopropanol, butanol, etc.; dichloromethane halogenated solvents such as chloromethane and chloroform; etc. These organic solvents may be used alone or in combination of two or more. Ester-based solvents, ether-based solvents, and alcohol-based solvents are preferred because they are easy to use and improve workability. and ketone-based solvents are preferred.
[0040] <Cured coating> The cured coating film of the active energy ray curable resin composition is The coating is applied to the surface of a substrate or an article to form a coating film, and then dried as necessary. After that, an active ene is added to the coating film. The cured coating film can be formed by irradiating it with high-energy radiation. In addition to coating, other methods such as transfer printing can be used, but these have fewer steps. Moreover, the coating method is preferred from the viewpoint of ease of application. The coating methods used are gravure coating, reverse roll coating, die coating, and air coating. Doctor coat, blade coat, rod coat, bar coat, curtain coat, knife Coat, transfer roll coat, squeeze coat, impregnation coat, kiss coat, spray The coating may be performed by known coating methods such as sintering, calendar coating, extrusion coating, dip coating, spin coating, etc. A filtering method can be used.
[0041] The drying and curing conditions for forming the cured coating film are not particularly limited. Regarding drying of the medium such as the organic solvent used in the coating solution, the drying temperature is usually 30 to 200° C., preferably The drying temperature is preferably in the range of 50 to 150° C., and more preferably in the range of 70 to 120° C. 0.01 to 30 minutes is preferred, and 0.1 to 10 minutes is more preferred.
[0042] In the case of curing with active energy rays, the active energy rays used are ultraviolet rays. Among these, the most important are curing properties and resin deterioration prevention properties. From the viewpoint of inhibition, ultraviolet rays and electron beams are preferred, and ultraviolet rays are more preferred. The amount of radiation exposure can be appropriately selected depending on the active energy radiation to be irradiated.
[0043] For example, when using ultraviolet light, the cumulative light dose is 20 to 5,000 mJ / cm 2 I like 50~3,000mJ / cm 2 More preferably, 100 to 2,000 mJ / cm 2 The illuminance is preferably 50 to 600 mW / cm, and more preferably 75 to 400 mW / cm. The light source is more preferably 50 mW / cm, and even more preferably 100 to 300 mW / cm. These include medium pressure mercury lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, electrodeless lamps, metal halide lamps, Or scanning type, curtain type electron beam acceleration path, high pressure mercury lamp, ultra high pressure mercury lamp, low pressure A mercury lamp or the like can be used.
[0044] In addition, when curing is performed by electron beam irradiation, various electron beam irradiation devices can be used. The irradiation dose (Mrad) of the electron beam is preferably 0.5 to 20 Mrad. From the viewpoints of curability of the energy ray-curable composition, flexibility of the cured product, prevention of damage to the substrate, etc. More preferably, it is 1 to 15 Mrad.
[0045] The thickness of the cured coating film is preferably 0.01 to 20 μm, more preferably 0.05 to 10 μm. The thickness of the cured coating film is preferably in the range of 0.1 to 7 μm. In this way, it is easy to achieve the desired hardness.
[0046] <Laminate> The laminate of the present invention has a substrate and a cured coating film of an active energy ray-curable resin composition. The laminate may further include a functional layer on the cured coating film of the present invention. Examples of the layer include a conventionally known layer, such as an anti-reflection layer, a low reflection layer, a high reflection layer, an anti Examples of the layer include a glare layer, an anti-blocking layer, an antifouling layer, an anti-fogging layer, and an adhesive layer. It is also possible to provide various functional layers on the side opposite to the side on which the cured coating film is provided. It is also possible to provide a cured coating film on both the substrate and the base material.
[0047] [Base material] Any base material may be used as long as it contains a compound having an isosorbide structure. In particular, isosorbide can be used as a dihydroxy component in polycarbonate resins and polycarbonates. One example is the incorporation of isosorbide into an ester resin, which allows many isosorbide structures to be included. This is a preferred form because it allows the amount of plant-derived ingredients to be increased.
[0048] When using polycarbonate resin with isosorbide as the dihydroxy component as the base material, In this case, the carbonic acid diester used as the raw material for the polycarbonate resin is a conventionally known material. For example, phenyl carbonates such as diphenyl carbonate and ditolyl carbonate can be used. Carbonates, dimethyl carbonate, diethyl carbonate, di-t-butyl carbonate Among these, phenyl carbonates, etc. is preferred, and diphenyl carbonate is particularly preferred. These carbonate diesters can be used alone. They may be used alone or in combination of two or more.
[0049] It is also preferable to use compounds other than isosorbide as the dihydroxy component. In other words, the copolymerized polycarbonate used as a copolymerization component of isosorbide is The dihydroxy component is preferably an aliphatic dihydroxyl group. Compounds, alicyclic dihydroxy compounds, aromatic bisphenol compounds, or compounds other than isosorbide Other ether group-containing dihydroxy compounds are preferred, including isosorbide. This allows the introduction of a molecular structure that is more flexible than the conventional structure, improving the toughness of polycarbonate resin. In addition, from the viewpoint of further improving the impact resistance, it is possible to use an aliphatic dihydroxy compounds, alicyclic dihydroxy compounds, or aromatic bisphenol compounds. Furthermore, from the viewpoint of improving weather resistance, it is preferable to have an aromatic ring structure in the molecular structure. Compounds that do not have aliphatic or alicyclic dihydroxy compounds. It is more preferable that the above-mentioned compound is an alicyclic dihydroxy compound, and further, in consideration of improving heat resistance, These dihydroxy components may be used alone or in combination of two or more. In addition, it is possible to use the aryl group in combination with the dihydroxy structure. Compounds with three or more hydroxyl groups, such as trihydroxy, can also be used. do.
[0050] Alicyclic dihydroxy compounds include 1,4-cyclohexanedimethanol, tricyclohexane Rhodecane dimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol , 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, penta Cyclopentadecane dimethanol, 2,6-decalin dimethanol, 1,5-decalin dimethanol Methanol, 2,3-decalin dimethanol, 2,3-norbornane dimethanol, 2, Examples include 5-norbornane dimethanol, 1,3-adamantanedimethanol, and limonene. Among these, the balance between impact resistance and flexibility, as well as ease of manufacturing, are considered. and 1,4-cyclohexanedimethanol or tricyclodecanedimethanol are more preferred. In applications where flexibility is important, 1,4-cyclohexanedimethanol is more suitable. Preferred.
[0051] The aliphatic dihydroxy compound may be a straight chain aliphatic or a branched chain aliphatic. Specific examples of the aliphatic dihydroxy compound include ethylene glycol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 1,3-butanediol 1,2-butanediol, 1,5-heptanediol, 1,6-hexanediol , 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1 ,10-Decanediol, 1,11-Undecanediol, 1,12-Dodecanediol etc.
[0052] Aromatic bisphenol compounds include 2,2-bis(4-hydroxyphenyl)propane. Pan(bisphenol A), 2,2-bis(4-hydroxy-3,5-dimethylphenyl )propane, 2,2-bis(4-hydroxy-3,5-diethylphenyl)propane, 2 ,2-Bis(4-hydroxy-(3,5-diphenyl)phenyl)propane, 2,2-Bi Bis(4-hydroxy-3,5-dibromophenyl)propane, 2,2-bis(4-hydroxy 2,4'-dihydroxy-diphenylmethane, bis(4-hydroxyphenyl)pentane Bis(4-hydroxy-5-nitrophenyl)methane, 1,1 -Bis(4-hydroxyphenyl)ethane, 3,3-bis(4-hydroxyphenyl)ethane 1,1-bis(4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)cyclohexane 2,4'-Dihydroxydiphenyl sulfone, Bis(4-hydroxydiphenyl)sulfone Dihydroxyphenyl)sulfide, 4,4'-dihydroxydiphenyl ether, 4,4'-di Hydroxy-3,3'-dichlorodiphenyl ether, 9,9-bis(4-(2-hydroxy (2-methyl)oxyethoxyphenyl)fluorene, 9,9-bis(4-hydroxyphenyl)fluorene 9,9-bis(4-hydroxy-2-methylphenyl)fluorene Among these, bisphenol A is more preferable in terms of the balance of properties. stomach.
[0053] Examples of the ether group-containing dihydroxy compound include diethylene glycol, triethylene glycol, Recall, polyethylene glycol, poly-1,3-propylene glycol, polytetra Examples of polyethylene glycol include those having a molecular weight of, e.g. For example, one with 150 to 2,000 can be used.
[0054] When using copolymer polycarbonate resin as the base material, all dihydroxy compounds are The proportion of structural units derived from isosorbide in 100 mol % of structural units is preferably 1 mol % or more. , more preferably 10 mol % or more, further preferably 30 mol % or more, particularly preferably 4 The range is 5 mol % or more, and most preferably 55 mol % or more. There is no particular upper limit. Although there is no particular limitation, all of the structural units may be derived from isosorbide, it is preferable that the structural units are 99 mol % or less, and more preferably 99 mol % or less. More preferably, it is 95 mol % or less, further preferably, it is 90 mol % or less, and particularly preferably, it is 85 mol % or less. By using it in the above range, heat resistance and rigidity are improved, and molding processability is improved. This makes it easier to adjust the properties to achieve a good balance between performance and mechanical strength.
[0055] The copolymer polycarbonate resin contains a structural unit other than the above-mentioned dihydroxy compound. For example, dihydroxy compounds of aromatic hydrocarbons can be mentioned. When compounds containing rings are exposed to sunlight or ultraviolet light, they absorb the ultraviolet light and undergo structural deterioration. Therefore, aromatic hydrocarbon dihydroxy compounds are often used. When using materials such as acrylic, it is necessary to ensure that the required product characteristics, such as moldability, weather resistance, and surface properties, are not impaired. It is desirable to use it within this range.
[0056] The glass transition temperature of the polycarbonate resin is preferably 100 to 200° C. in consideration of heat resistance and toughness. The temperature is preferably 40 to 180°C, more preferably 60 to 160°C, and further preferably 80 to 150°C. The temperature range is particularly preferably 90 to 140°C.
[0057] Polycarbonate resin is an ester of the above dihydroxy compound and the above carbonic acid diester. It can be synthesized by polycondensation through transesterification. The polycondensation reaction is advanced by distilling off the monohydroxy compounds and other by-products produced in the reaction. The transesterification reaction can be promoted in the presence of a transesterification catalyst. Catalysts include metal compounds of Groups 1 and 2 of the long-form periodic table, as well as basic Boron compounds, basic phosphorus compounds, basic ammonium compounds, amine compounds, etc. Among them, a Group 1 metal compound or a Group 2 metal compound can be used. It is preferable to use at least one of the following. The amount of catalyst used is determined based on the total amount of dihydrides used in the reaction. Preferably, the amount of the compound is 0.1 to 300 μmol, more preferably 0.5 to 100 μmol, per mole of the alkoxy compound. It is 100 μmol, particularly 1 to 50 μmol.
[0058] The molar ratio of the carbonic acid diester to the dihydroxy compound is preferably 0.90 to 1. In this case, the amount of hydroxyl groups in the polycarbonate resin is preferably in the range of 1.20. This suppresses the increase in the thermal stability of the resin, which makes it possible to improve the molding It is possible to reduce coloring during the polymerization. In addition, it is possible to suppress the decrease in the rate of the ester exchange reaction. This makes it possible to more reliably produce a copolymer having a desired molecular weight. From the viewpoint of being able to suppress the increase in thermal history during the reaction, polycarbonate resin In this case, the coloring of the polycarbonate resin can be reduced. The amount of the acid diester can be reduced, and from this viewpoint, the coloring of the resin can be reduced. Furthermore, the generation of odor can be prevented or reduced. From this viewpoint, the molar ratio of the carbonic acid diester to the dihydroxy compound is particularly preferably The range is preferably 0.95 to 1.10.
[0059] The polymerization reaction may be carried out by a batch method, a continuous method, or a combination thereof. Among them, a continuous process in which the reaction is carried out in multiple stages using multiple reactors in the presence of the catalyst is preferred. This is preferable from the viewpoint of productivity and ease of thermal history management.
[0060] In addition, various additives can be added to the polycarbonate resin used as the base material. Examples of additives include ultraviolet absorbers, antioxidants, light stabilizers, catalyst deactivators, These include dyes and pigments, flame retardants, flame retardant auxiliaries, fillers, impact modifiers, hydrolysis inhibitors, nucleating agents, and plasticizers. Can be obtained.
[0061] When a polyester resin containing isosorbide as a dihydroxy component is used as a base material, Examples of the acid component to be polymerized include terephthalic acid, isophthalic acid, and 2-chloroterephthalic acid. Terephthalic acid, 2,5-dichloroterephthalic acid, 2-methylterephthalic acid, 4,4-stilbene di Carboxylic acid, 4,4-biphenyldicarboxylic acid, orthophthalic acid, 2,6-naphthalenedicarboxylic acid Carboxylic acid, 2,7-naphthalenedicarboxylic acid, bisbenzoic acid, bis(p-carboxyl (phenyl)methane, anthracene dicarboxylic acid, 4,4-diphenyl ether dicarboxylic acid , 4,4-diphenoxyethanedicarboxylic acid, 5-sodium sulfoisophthalic acid, ethyl Aromatic dicarboxylic acids such as olefin-bis-p-benzoic acid, succinic acid, adipic acid, and sebacic acid , Azelaic acid, Dodecanedioic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclo Derived from aliphatic dicarboxylic acids such as hexanedicarboxylic acid or their ester derivatives The acid components may be one kind alone or two kinds. It may contain more than one type.
[0062] A homopolymer formed solely of isosorbide as a dihydroxy component may be used, but it is flexible. Considering the properties, copolymer polyester resins using other polyhydroxy components are more preferable. Examples of polyhydroxy components that can be used include ethylene glycol, diethylene glycol, and the like. Polyethylene glycol, 1,4-butanediol, neopentyl glycol, polytetramethyl 1,4-cyclohexanedimethanol, spiroglycol, 2,2,4, 4-tetramethylcyclobutane-1,3-diol and other compounds. However, in terms of balancing various performances, ethylene glycol and 1,4 It is preferred to use -cyclohexanedimethanol.
[0063] The resin containing the compound having an isosorbide structure obtained by the above-mentioned method or the like is a conventionally known It can be processed in various ways, including but not limited to the following methods: For example, the resin is introduced into an extruder, and additives are continuously added while kneading. Then, the resin is passed through a pressure reducing device. By-product gases and low molecular weight volatile matter are removed by devolatilization, and the molten material is extruded in the form of strands from the tip of the extruder. One method is to cut the mixture into pellets while cooling and solidifying it. In order to obtain a uniform dispersion of the additives and to obtain a uniform force, a twin screw extruder with a pressure reducing device at the vent is preferable. .
[0064] As for the operating conditions of the extruder, in order to increase the efficiency of devolatilization, it is preferable that the melt viscosity of the resin is low. It is preferable that the melt-kneading temperature in the extruder is high. However, if the temperature is too high, discoloration and It is necessary to process at the highest possible but appropriate temperature, as thermal decomposition may occur. The appropriate melting temperature depends on the type of resin, the glass transition temperature of the resin, the molecular weight, the melt viscosity, etc. However, taking into consideration the temperature at which thermal decomposition begins to occur rapidly, 200°C to 320°C is preferable. In this case, the plasticizing load on the extruder is reduced, and productivity can be improved. Both can suppress the thermal decomposition of resin, and reduce coloration, loss of mechanical strength due to molecular weight reduction, and heat decomposition. It is possible to prevent the generation of degassing gas and the like. The melting temperature is more preferably from 210°C to 300°C, particularly preferably from 220°C to 290°C.
[0065] The mixture is melted in an extruder, preferably via a gear pump, and filtered if necessary. The resin is extruded in strand form from a die head, cooled and solidified, and then spun into a rotary mold. The strands are cut into pellets using a cutter, etc. The strands are usually cooled by air or water. In the case of air cooling, the air used is cleaned by filtering out foreign matter using a HEPA filter, etc. It is preferable to use clean air to prevent the inclusion of foreign matter in the air. The water is treated with ion exchange resin to remove metal components, and then filtered to remove foreign matter. It is preferable to use clean water from which the above-mentioned substances have been removed.
[0066] The resulting pelletized resin can be further processed by a conventional method. For example, Examples include processing into film and molding using a mold. Limited to the following methods However, for example, when making a film, the general manufacturing method is to melt the resin. The method includes melting the resin, forming the resin into a sheet, and stretching the sheet as necessary to increase its strength. .
[0067] For example, the above-mentioned resin is melt-extruded from a die using an extruder, and the molten film is cooled. The film is cooled and solidified by rolls to obtain an unstretched film. In this case, the flatness of the film is improved. Therefore, it is preferable to increase the adhesion between the molten sheet and the cooling roll. If the film is to be used as an unstretched film, the roll temperature is By adjusting the extrusion speed and extrusion temperature, thickness fluctuation can be reduced. It is also possible to stretch the resulting unstretched film in order to reduce vibration and roughness. For example, stretching in the longitudinal direction of the film can be achieved by utilizing the difference in peripheral speed of the rolls. The stretching in the transverse direction can be achieved by using a tenter type stretching machine. It is also possible to combine these two methods to produce a biaxially stretched film. The stretching temperature and stretching ratio vary depending on the type of resin, but are preferably 7 The temperature is in the range of 0 to 200°C, more preferably 80 to 160°C, and the stretching ratio is in one direction. The range is 7 times or less, and more preferably 5 times or less. There is no particular lower limit, but it is 1 time. Depending on the type of resin, a suitable heat treatment or the like can be applied to obtain a stretched film.
[0068] Various additives may be used at any stage in the processing of the above resins. It is known that it can be added before or during melt extrusion in the production of plastics or films. The additives are, for example, catalyst deactivators and heat stabilizers used in the production of resins. , neutralizer, UV absorber, light stabilizer, particle, release agent, dye, pigment, lubricant, plasticizer, lubricant , compatibilizers, flame retardants, etc.
[0069] The substrate may be in any form, for example, a film, a sheet, or the like. The thickness is also arbitrary, but for example, a film can be handled From the viewpoints of durability, productivity and processability, the thickness is 1 to 500 μm, preferably 10 to 300 μm, and more preferably The range is preferably 20 to 250 μm. In addition, in the case of a molded product, from the viewpoint of light weight, 0 In the range of 0.05 to 10 mm, preferably 0.1 to 6 mm, and more preferably 0.2 to 4 mm. be.
[0070] In addition, the substrate is a material that can be used as a substrate for improving the coating property of the active energy ray-curable resin composition. In order to improve adhesion between the cured coating layer of the radiation curable resin composition and the coating layer, corona treatment and plastic treatment are performed. It is also possible to apply Zuma processing.
[0071] The laminate of the present invention is particularly excellent in hardness among various applications, and is therefore suitable for use as a display member or an electrical component. - It can be used for electronic components and is more scratch-resistant than general polycarbonate resins. Due to its excellent adhesion, it can be suitably used for automobile parts and various lenses, and similarly, it can be used for general Compared to typical polycarbonate resins, it has excellent processability and is therefore suitable for a variety of film applications, e.g. For example, it can be suitably used for display members and decorative purposes. EXAMPLES
[0072] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples. The measurement and evaluation methods used in the present invention are as follows.
[0073] (1) Measurement of weight average molecular weight (Mw) and number average molecular weight Equipment: Tosoh Corporation "HLC-8120GPC" Column: TSKgel SuperHZM-M*HZM-M*HZ manufactured by Tosoh Corporation 2000", Detector: Differential refractive index detector (RI detector / built-in), Solvent: tetrahydrofuran, Temperature: 40℃, Flow rate: 0.5mL / min, Injection volume: 10μL, Concentration: 0.2% by mass, Calibration sample: monodisperse polystyrene, Calibration method: polystyrene equivalent.
[0074] (2) Pencil hardness measurement The coated laminate was tested according to JIS K-5600 to measure the pencil hardness. The evaluation criteria are as follows: ◎…Pencil hardness F or higher 〇…Pencil hardness is B~HB ×…Pencil hardness is 2B or less
[0075] (3) Measurement of elongation The coated laminate was cut together with the substrate into a piece 10 mm wide and 60 mm long. The sample was placed on an Imada MX2-500N-FA with a chuck distance of 40 mm and tension A tensile test was carried out at a speed of 50 mm / min and an ambient temperature of 80°C, and the yield point value was recorded as the elongation. The evaluation was based on the following criteria. ◎…Elongation is 35% or more 〇…Elongation is 20% to 34% ×…Elongation is less than 20%
[0076] (4) Adhesion measurement The coated laminate was cut with a cutter knife into a grid pattern at 1 mm intervals down to the substrate. 1mm 2 Make 100 grids of the above and stick Nichiban Cellophane Tape (registered trademark) on them. The coating layer was then peeled off rapidly to observe the state of the cross-cuts that had peeled off between the substrate and coating layer. The initial adhesion was evaluated according to the following criteria. ◎…95 or more squares remaining in a grid cut 〇…70 to 94 remaining squares in a grid cut ×…69 or less squares remaining in grid cut
[0077] (5) Antistatic property measurement The coated laminate was subjected to a Nitto Seiko Analytic Hi-Resta UP test. The surface resistivity was measured at a voltage of 500 V. The antistatic properties were evaluated according to the following criteria. ◎…Surface resistivity is 1.99E+10 or less ○…Surface resistivity is 2.00E+10~9.99E+10 ×…Surface resistivity is 1.00E+11 or more
[0078] (Production Example 1) The following urethane acrylate A was prepared. A four-neck flask equipped with a thermometer, stirrer, water-cooled condenser, and nitrogen gas inlet was Isophorone diisocyanate 37.5g (0.17 mol), polytetramethylene glycol Ludziol 25.5g (hydroxyl value 167mgKOH / g; molecular weight calculated from hydroxyl value 672; 0.04 mol), polyester triol 13.4 g (hydroxyl value 262 mg KO H / g; molecular weight calculated from hydroxyl value 642; 0.02 mol), Djibouti as a reaction catalyst 0.02 g of tin dilaurate was added and reacted at 80°C. When the concentration dropped below 11%, 23.6 g (0.2 mol) of 2-hydroxyethyl acrylate was added. ), 0.04 g of methoxyphenol was further charged as a polymerization inhibitor, and the reaction was carried out at 60°C. When the residual isocyanate group is 0.3% or less, the reaction is terminated and the urethane acrylate is As a result, copolymer A (number of functional groups: 2 to 3, weight average molecular weight: approximately 3,500) was obtained.
[0079] (Production Example 2) As polymer D having a quaternary ammonium salt group, the following was prepared. A reactor equipped with a stirrer, a reflux condenser, and a thermometer was charged with 18 parts by mass of DQ100, S LMA: 7.5 parts by weight, DMMA: 4.5 parts by weight, methyl ethyl ketone (MEK): 20 parts by weight, isopropyl alcohol (IPA): 50 parts by weight, and the system was stirred. The mixture was replaced with nitrogen and heated to 55°C. After adding 0.6 parts by mass of nitrile ("V-65" manufactured by Wako Pure Chemical Industries, Ltd.), the system was heated to 65° C. The temperature was raised to 100°C, and the mixture was stirred for 3 hours. After that, 2,2'-azobis(2,4-dimethylvaleronyl) Tolyl (0.6 parts by mass) was added and stirred at 65°C for 3 hours. The temperature inside the system was raised to 80°C. After stirring for 2 hours, the mixture was cooled to room temperature to obtain a solution of a polymer having a quaternary ammonium salt group. The composition of this solution was polymer / MEK / IPA=30 / 20 / 50 (weight ratio). The weight average molecular weight (Mw) of the copolymer was 45,200.
[0080] Component (A) is 40 parts by mass of the above-mentioned urethane acrylate A, and component (B) is BR -80 (manufactured by Mitsubishi Chemical, product name Dianarl BR-80) 20 parts by mass, component (C) and 5 parts by weight of Omn.184 (manufactured by IGM Resin, product name Omnirad 184 ), 26.7 parts by mass of the polymer D having a quaternary ammonium salt group as component (D), Other ingredients include 20 parts by weight of V#300, 12 parts by weight of DPHA, and PG as an organic solvent. 150 parts by mass of M and 150 parts by mass of MEK were mixed and dissolved to obtain an active energy ray curable composition. was manufactured.
[0081] On a film of D7340A (Mitsubishi Chemical product name: Durabio D7340A), The above-described active energy ray-curable resin composition was applied using a bar coater #16. After drying at 0°C for 1 minute, the specimen was irradiated with a high-pressure mercury lamp at an intensity of 120 mW / cm and an accumulated light quantity of 30 0mJ / cm 2 The laminate was irradiated with ultraviolet light at 400 rpm to obtain a laminate having a hard coat layer with a thickness of 5 μm.
[0082] [Examples 2 to 9, Comparative Examples 1 to 4] The same procedure as in Example 1 was repeated except that the blending and composition were as shown in the composition column of Table 1. A linear curable composition was prepared and evaluated, and the results are shown in Table 1.
[0083] [Table 1]
[0084] The units of values other than the compounding ratio in the table are parts by mass. The abbreviations in Table 1 are as follows: Shows. Urethane acrylate A: described in Manufacturing Example 1 Urethane acrylate B: Mitsubishi Chemical DiaBeam UK-6091 (product name, Bifunctional urethane acrylate) Urethane acrylate C: MIWON MIRAMER PU2100 (product name, 2 Functional urethane acrylate) BR-80: Mitsubishi Chemical's Dianale BR-80 (product name, acrylic copolymer) , Mw: 100,000, Tg: 104℃) MB-7940: Mitsubishi Chemical Dianale MB-7940 (product name, acrylic) Copolymer, Mw: 6000, Tg: 82℃) ·Omn.184: Omnirad 184 (product name, 1-hi) made by IGM Resins Hydroxycyclohexyl phenyl ketone Polymer D having a quaternary ammonium salt group: described in Production Example 2 V#300: Viscoat #300 (trade name, pentaerythritol) manufactured by Osaka Organic Chemical Industry Co., Ltd. Re-Acrylate) DPHA: KAYARAD DPHA (product name, dipentaerythritol) manufactured by Nippon Kayaku Hexaacrylate) ·UV-7600B: Made by Mitsubishi Chemical Purple Light UV-7600B (Product name, 6-functional urethane Acrylate) ·PGM: Propylene glycol monomethyl ether MEK: Methyl ethyl ketone
[0085] From the above examples, it can be seen that the cured coating film formed from the active energy ray-curable resin composition of the present invention The pencil hardness, elongation and adhesion were excellent. On the other hand, the comparative example 1, which did not contain the component (B), The cured coating film formed from the active energy ray-curable resin composition has insufficient adhesion and The active energy ray-curable resin composition of Comparative Example 2, which did not contain components (A) and (B), The cured coating film formed from the above composition had insufficient elongation. The cured coating film formed from the active energy ray curable resin composition has a good balance between hardness and elongation. It was insufficient.
Claims
1. A coating material to be applied to an isosorbide-containing substrate, A urethane (meth)acrylate (A) having a structure derived from the following (a1) and (a2), An active ethylene glycol polymer (B) containing a (meth)acrylic monomer and a photopolymerization initiator (C) Energy ray curable resin composition. (a1) An isocyanate compound having at least two isocyanate groups (a2) Hydroxyl group-containing monofunctional (meth)acrylate
2. The amount of the urethane (meth)acrylate (A) blended is The active energy storage medium according to claim 1, wherein the active energy storage medium is 5% by mass or more and 80% by mass or less based on the total amount of solids. Lugie wire curable resin composition.
3. 2. The method according to claim 1, wherein the substrate is a polycarbonate substrate having an isosorbide as a structural unit. The active energy ray-curable resin composition according to claim 1,
4. The amount of the (co)polymer (B) of the (meth)acrylic monomer blended is 2. The composition according to claim 1, wherein the content of the solid content of the cured resin composition is 5% by mass or more and 60% by mass or less based on the total amount of the solid content of the cured resin composition. The active energy ray-curable resin composition according to claim 1,
5. Further, a compound (D) having a quaternary ammonium salt group (provided that the (meth)acrylic monomer The active energy ray-curable resin according to claim 1, further comprising a (co)polymer (B) of the active energy ray-curable resin. composition.
6. A cured coating film of the active energy ray-curable resin composition according to any one of claims 1 to 5.
7. A urethane (meth)acrylate (A) and a (co)polymer of a (meth)acrylic monomer (B and a photopolymerization initiator (C), The cured product obtained by curing the active energy ray-curable resin composition has a temperature of 80° C. An active energy ray-curable resin composition having an elongation of 20% or more.
8. A urethane (meth)acrylate (A) having a structure derived from the following (a1) and (a2); 、 An active ingredient comprising a (co)polymer (B) of a (meth)acrylic monomer and a photopolymerization initiator (C). A laminate having a layer made of an energy ray-curable resin composition on an isosorbide-containing substrate. (a1) An isocyanate compound having at least two isocyanate groups (a2) Hydroxyl group-containing monofunctional (meth)acrylate
Citation Information
Patent Citations
Ultraviolet-curable resin composition
JP2012077272A
Film and polarizing plate
JP2016079321A
Hard coat resin composition
JP2023007298A
Photocurable resin composition, hard coat film and plastic molding including the same
JP2023040446A