Solid electrolytic capacitor element, method for manufacturing the same, and solid electrolytic capacitor
The solid electrolytic capacitor design with a porous anode body, dielectric layer, and unevenly distributed polyglycerin derivative in the first portion addresses capacitance loss and reliability issues under high temperatures, achieving stable performance.
Patent Information
- Application Number
- JP2023050114
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Solid electrolytic capacitors face a significant decrease in capacitance and reliability when exposed to high temperatures due to dielectric layer deterioration and increased leakage current, which existing additives like polyoxyalkylene polyglyceryl ether and polyglycerin fatty acid ester fail to adequately address.
The capacitor element incorporates an anode body with a porous portion, a dielectric layer, and a solid electrolyte layer with a first portion filled in the voids of the porous portion and a second portion protruding from the dielectric layer, where the polyglycerin derivative is unevenly distributed in the first portion to enhance heat resistance and maintain capacitance.
This configuration effectively suppresses capacitance decline and ensures high reliability by reducing dielectric layer defects and leakage current, even under high-temperature conditions and repeated charging/discharging cycles.
Smart Images

Figure 2024139254000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a solid electrolytic capacitor element, a method for producing the same, and a solid electrolytic capacitor. [Background technology]
[0002] The solid electrolytic capacitor includes a solid electrolytic capacitor element, a resin exterior body or case that seals the solid electrolytic capacitor element, and an external electrode that is electrically connected to the solid electrolytic capacitor element. The solid electrolytic capacitor element includes, for example, an anode body, a dielectric layer formed on the surface of the anode body, and a cathode portion that covers at least a portion of the dielectric layer. The cathode portion includes a conductive polymer that covers at least a portion of the dielectric layer. The conductive polymer is also called a solid electrolyte.
[0003] Patent Document 1 proposes a solid electrolytic capacitor containing a conductive polymer and an additive, characterized in that the solid electrolytic capacitor contains one or more additives selected from the group consisting of polyoxyalkylene polyglyceryl ethers and polyglycerin fatty acid esters. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-125410 A Summary of the Invention [Problem to be solved by the invention]
[0005] Solid electrolytic capacitors are required to have high reliability, so that they can maintain high capacitance even when exposed to high-temperature environments. [Means for solving the problem]
[0006] A first aspect of the present disclosure includes an anode body having a porous portion at least on a surface layer, a dielectric layer covering at least a portion of the anode body; a solid electrolyte layer covering at least a portion of the dielectric layer; the solid electrolyte layer includes a first portion filled in voids of the porous portion in the anode body having the dielectric layer and a second portion protruding from a main surface of the anode body having the dielectric layer, and includes a polyglycerin derivative; The present invention relates to a solid electrolytic capacitor element, in which the polyglycerin derivative is unevenly distributed in the first portion.
[0007] A second aspect of the present disclosure relates to a solid electrolytic capacitor including at least one of the solid electrolytic capacitor elements described above.
[0008] A third aspect of the present disclosure is a method for manufacturing a solid electrolytic capacitor element including an anode body having a porous portion at least in a surface layer, a dielectric layer covering at least a portion of the anode body, and a solid electrolyte layer covering at least a portion of the dielectric layer, the solid electrolyte layer includes a first portion filled in voids of the porous portion in the anode body having the dielectric layer and a second portion protruding from a main surface of the anode body having the dielectric layer, and includes a polyglycerin derivative; The manufacturing method includes: a first step of forming at least a part of the first portion using a first conjugated polymer or a precursor thereof and the polyglycerin derivative; a second step of forming the second portion using a second conjugated polymer or a precursor thereof; The present invention relates to a method for producing a solid electrolytic capacitor element, Effect of the Invention
[0009] This can suppress the decrease in capacitance when the solid electrolytic capacitor or the solid electrolytic capacitor element is exposed to high temperatures. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view of a solid electrolytic capacitor according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Depending on the application, solid electrolytic capacitors may be used in high-temperature environments or exposed to high temperatures during a reflow process. When a solid electrolytic capacitor is exposed to high temperatures, the dielectric layer formed on the surface of the anode body deteriorates, causing defects in the dielectric layer and increasing leakage current. When the leakage current increases, the conductive polymer in the vicinity of the dielectric layer becomes insulated, reducing the capacity, making it difficult to maintain a high capacity. Therefore, when a solid electrolytic capacitor is exposed to high temperatures, it is difficult to ensure high reliability.
[0012] Patent Document 1 proposes a solid electrolytic capacitor containing polyoxyalkylene polyglyceryl ether or polyglycerin fatty acid ester as an additive from the viewpoint of high heat resistance and high breakdown voltage. However, it has become clear that depending on the distribution state of these polyglycerin derivatives, the capacity of the solid electrolytic capacitor or the solid electrolytic capacitor element is significantly reduced when exposed to high temperatures.
[0013] In view of the above, (1) a solid electrolytic capacitor element according to a first aspect of the present disclosure includes an anode body having a porous portion at least on a surface layer thereof, a dielectric layer covering at least a portion of the anode body, and a solid electrolyte layer covering at least a portion of the dielectric layer. The solid electrolyte layer includes a first portion filled in the voids of the porous portion in the anode body having the dielectric layer, and a second portion protruding from a main surface of the anode body having the dielectric layer, and includes a polyglycerin derivative. The polyglycerin derivative is unevenly distributed in the first portion.
[0014] According to the first aspect, the polyglycerin derivative is unevenly distributed in the first portion filled in the voids of the porous portion, so that the capacity reduction can be suppressed when the solid electrolytic capacitor element (or the solid electrolytic capacitor) is exposed to high temperatures. This ensures high reliability of the solid electrolytic capacitor. On the other hand, even if the polyglycerin derivative is unevenly distributed in the second portion, it is difficult to maintain a high capacity when the solid electrolytic capacitor element is exposed to high temperatures, and the effect is almost the same as when no polyglycerin derivative is used at all. In other words, even if the second portion contains a large amount of polyglycerin derivative, there is almost no effect of suppressing the capacity reduction. In addition, since the polyglycerin derivative is insulating, when the second portion contains a large amount of polyglycerin derivative, the initial characteristics are reduced, such as a reduction in initial capacity and an increase in equivalent series resistance (ESR).
[0015] In the present disclosure, the details of the mechanism by which the uneven distribution of the polyglycerin derivative in the first portion suppresses the decrease in capacity are unclear, but it is assumed to be due to the following reasons. Since the polyglycerin derivative itself has high heat resistance, the uneven distribution of the polyglycerin derivative in the first portion improves the heat resistance of the first portion. The improved heat resistance suppresses deterioration of the first portion, and the application of stress associated with deterioration to the dielectric layer is suppressed, thereby reducing the occurrence of defects in the dielectric layer. The reduced defects in the dielectric layer and the increased heat resistance of the first portion reduce leakage current, and the insulating effect of the conductive polymer in the first portion due to leakage current is suppressed. As a result, it is believed that the capacitance decrease of the solid electrolytic capacitor is suppressed and high reliability is obtained.
[0016] In addition, the present disclosure can also suppress the decrease in capacity when the solid electrolytic capacitor is repeatedly charged and discharged at room temperature (for example, at a temperature of 20° C. or higher and 35° C. or lower). From this perspective, the solid electrolytic capacitor of the present disclosure can achieve high reliability. The degradation mechanism due to charging and discharging is assumed to be a mode in which the solid electrolyte expands and contracts (swells and contracts, etc.) as moisture and the like are adsorbed to and desorbed from the solid electrolyte, causing the solid electrolyte to peel off from the chemical conversion film. In the present disclosure, it is believed that the uneven distribution of the polyglycerin derivative in the first portion suppresses the expansion and contraction of the first portion, thereby suppressing the decrease in capacity.
[0017] (2) In the above (1), the first portion may include a portion IA and a portion IB present between the portion IA and the dielectric layer. In this case, the polyglycerin derivative is preferably distributed unevenly in the portion IA. By distributing the polyglycerin derivative unevenly in the portion IA, the decrease in capacity of the solid electrolytic capacitor element (or the solid electrolytic capacitor) when exposed to high temperatures can be more effectively suppressed. The decrease in capacity when the solid electrolytic capacitor is repeatedly charged and discharged can also be further suppressed. Thus, the solid electrolytic capacitor can have higher reliability. It is considered that the effect of suppressing the degradation of the conductive polymer by the polyglycerin derivative is more easily exhibited when the polyglycerin derivative is distributed unevenly in the portion IA away from the dielectric layer among the voids of the porous portion, rather than in the portion IB close to the dielectric layer.
[0018] (3) In the above (2), the second portion and the portion IA may contain a non-self-doping conductive polymer. The portion IB may contain a self-doping conductive polymer. The portion IB is formed by applying a treatment liquid (for example, a fourth treatment liquid described later) containing a self-doping conductive polymer to an anode body having a dielectric layer. The treatment liquid containing a self-doping conductive polymer has a relatively low viscosity, so that it is easy to penetrate into the voids of the porous portion and to form a relatively uniform coating on the surface of the inner wall of the void. Since a relatively uniform conductive coating is formed on the surface of the anode body having a dielectric layer, including the inner wall of the void, it is easy to form a coating of the self-doping conductive polymer so as to cover this surface. This reduces the resistance at the interface between the dielectric layer and the solid electrolyte layer, and high initial characteristics (initial capacity, etc.) can be ensured. In addition, the polyglycerin derivative is unevenly distributed in the vicinity of the non-self-doping conductive polymer, so that deterioration of the conductive polymer is easily suppressed and higher reliability is easily obtained.
[0019] (4) In any one of the above (1) to (3), the polyglycerin derivative may include at least one selected from the group consisting of an ether compound having a moiety corresponding to polyglycerin and an ester compound having a moiety corresponding to polyglycerin, which makes it easier to obtain a solid electrolytic capacitor with higher reliability.
[0020] (5) In the above (4), the ether compound may contain polyoxyalkylene polyglyceryl ether, which makes it easier to obtain higher reliability of the solid electrolytic capacitor.
[0021] (6) The present disclosure also includes a solid electrolytic capacitor including at least one solid electrolytic capacitor element according to any one of (1) to (5) above.
[0022] (7) The present disclosure also includes a method for manufacturing a solid electrolytic capacitor element. In the manufacturing method, the solid electrolytic capacitor element includes an anode body having a porous portion at least on its surface, a dielectric layer covering at least a portion of the anode body, and a solid electrolyte layer covering at least a portion of the dielectric layer. The solid electrolyte layer includes a first portion filled in the voids of the porous portion in the anode body having the dielectric layer, and a second portion protruding from a main surface of the anode body having the dielectric layer, and also includes a polyglycerin derivative. The manufacturing method includes a first step of forming at least a portion of the first portion using a first conjugated polymer or a precursor thereof and a polyglycerin derivative, and a second step of forming the second portion using a second conjugated polymer or a precursor thereof.
[0023] According to the above (7), the polyglycerin derivative can be unevenly distributed in the first portion of the solid electrolyte layer filled in the voids of the porous portion. This makes it possible to suppress a decrease in capacity when the solid electrolytic capacitor element (or the solid electrolytic capacitor) is exposed to high temperatures. In addition, it is possible to suppress a decrease in capacity when the solid electrolytic capacitor is repeatedly charged and discharged. This makes it possible to ensure high reliability of the solid electrolytic capacitor.
[0024] (8) Regarding the above (7), in the first step, at least a part of the first portion may be formed using a treatment liquid (first treatment liquid) containing a first conjugated polymer or its precursor, a first dopant, and a polyglycerin derivative. In this case, the part containing the polyglycerin derivative contains a non-self-doping conductive polymer. Therefore, the polyglycerin derivative effectively suppresses the deterioration of the non-self-doping conductive polymer, and further suppresses the decrease in capacity when the solid electrolytic capacitor is exposed to high temperatures or repeatedly charged and discharged.
[0025] (9) In the above (8), the concentration of the polyglycerin derivative in the first treatment liquid may be less than 10% by mass, which further suppresses the decrease in capacity when the solid electrolytic capacitor is exposed to high temperatures or when it is repeatedly charged and discharged.
[0026] (10) In the above (7), the first step may include a sub-step A of forming a non-self-doping conductive polymer using a treatment liquid (second treatment liquid) containing a first conjugated polymer or its precursor and a first dopant, and a sub-step B of forming at least a part of the first portion by applying a treatment liquid (third treatment liquid) containing a polyglycerin derivative to the non-self-doping conductive polymer. In this case, the polyglycerin derivative can be unevenly distributed in at least a part of the first portion containing the non-self-doping conductive polymer. By having the polyglycerin derivative exist in the vicinity of the non-self-doping conductive polymer, it is easy to suppress the deterioration of the non-self-doping conductive polymer. Therefore, the decrease in capacity when the solid electrolytic capacitor is exposed to high temperatures or repeatedly charged and discharged is further suppressed.
[0027] (11) In the above (10), the concentration of the polyglycerol derivative in the third treatment liquid may be 10% by mass or more, which further suppresses the decrease in capacity when the solid electrolytic capacitor is exposed to high temperatures or when it is repeatedly charged and discharged.
[0028] (12) In any one of the above (7) to (10), the method for producing a solid electrolytic capacitor element may include, prior to the first step, a step of applying a treatment liquid (fourth treatment liquid) containing a self-doping conductive polymer to the dielectric layer to form a part of the first portion. The fourth treatment liquid has a relatively low viscosity, so that it is easy to penetrate into the voids of the porous portion and to form a relatively uniform coating on the surface of the inner wall of the void. Since a relatively uniform conductive coating is formed on the surface of the anode body having the dielectric layer, including the inner wall of the void, it is easy to form a coating of the conductive polymer so as to cover this surface. In addition, since the polyglycerin derivative is unevenly distributed in the first portion, deterioration of the conductive polymer located near the polyglycerin derivative is easily suppressed, and stress is not easily applied to the dielectric layer, so that high reliability is easily obtained.
[0029] The solid electrolytic capacitor element and its manufacturing method, and the solid electrolytic capacitor of the present disclosure will be described in more detail below, including the above (1) to (12). At least one of the above (1) to (12) may be combined with at least one of the elements described below, provided that there is no technical contradiction. The solid electrolytic capacitor element may be simply referred to as a capacitor element.
[0030] [Solid electrolytic capacitor] The capacitor element included in the solid electrolytic capacitor includes an anode part and a cathode part. In the solid electrolytic capacitor and capacitor element of the present disclosure, the components other than the solid electrolyte layer constituting the cathode part are not particularly limited, and components used in known solid electrolytic capacitors may be applied.
[0031] (Capacitor element) The capacitor element includes an anode body, a dielectric layer formed on the surface of the anode body, and a cathode portion covering at least a portion of the dielectric layer. The anode body constitutes the anode portion.
[0032] (Anode) The anode section includes an anode body. The anode section may include an anode body and an anode wire.
[0033] (Anode body) The anode body may contain a valve metal, an alloy containing a valve metal, a compound containing a valve metal, etc. The anode body may contain one of these materials or a combination of two or more of them. Examples of the valve metal are preferably aluminum, tantalum, niobium, and titanium.
[0034] The anode body has a porous portion at least on the surface layer thereof. The porous portion of the anode body has a large number of minute voids. Due to such a porous portion, the anode body has a finely uneven shape.
[0035] An anode body having a porous portion on the surface layer can be obtained, for example, by roughening the surface of a substrate (such as a sheet-shaped (e.g., foil-shaped, plate-shaped) substrate) containing a valve metal. The roughening may be performed, for example, by etching (electrolytic etching, chemical etching, etc.). Such an anode body has, for example, a core and a porous portion formed on both surfaces of the core, integrally with the core.
[0036] The anode body may be a porous molded body or a porous sintered body (such as a sintered body of a porous molded body) of particles containing a valve metal. Each of the molded body and the sintered body may be in a sheet shape, a rectangular parallelepiped, a cube, or a shape similar thereto. The porous sintered body may be, for example, a porous sintered body containing tantalum.
[0037] The anode body may generally have an anode lead portion including a first end portion and a cathode forming portion including a second end portion opposite to the first end portion. A cathode portion including a solid electrolyte layer is formed on the surface of the cathode forming portion of the anode body. The anode lead portion is used, for example, for electrical connection with an external electrode on the anode side. An anode lead terminal may be connected to the anode lead portion.
[0038] (anode wire) When the anode body is a porous sintered body or a porous molded body, the anode part may include an anode wire. The anode wire may be a wire made of a metal. Examples of the material of the anode wire include the above valve metals, copper, or copper alloys. A part of the anode wire is embedded in the anode body, and the remaining part protrudes outward from the end face of the anode body. The end of the anode wire protruding outward corresponds to the first end, and the end of the anode body opposite to the first end corresponds to the second end.
[0039] (Dielectric layer) The dielectric layer is formed, for example, so as to cover at least a part of the surface of the anode body (more specifically, the porous portion). The dielectric layer is an insulating layer that functions as a dielectric. The dielectric layer is formed by anodizing the valve metal on the surface of the anode body by chemical conversion treatment or the like. Since the dielectric layer is formed on the porous surface of the anode body, the surface of the dielectric layer has a fine uneven shape that follows the shape of the porous portion.
[0040] The dielectric layer contains an oxide of the valve metal. For example, when tantalum is used as the valve metal, the dielectric layer contains tantalum oxide, and when aluminum is used as the valve metal, the dielectric layer contains aluminum oxide. Note that the dielectric layer is not limited to these examples, and may be any layer that functions as a dielectric.
[0041] (cathode) The cathode section includes at least a solid electrolyte layer covering at least a portion of the dielectric layer. The solid electrolyte layer is formed on the portion of the anode body on the second end side (in other words, the cathode formation portion) via a dielectric layer. The cathode section usually includes a solid electrolyte layer covering at least a portion of the dielectric layer, and a cathode extraction layer covering at least a portion of the solid electrolyte layer. The solid electrolyte layer and the cathode extraction layer will be described below.
[0042] (Solid electrolyte layer) In the capacitor element, the solid electrolyte layer is formed so as to cover at least a part of the dielectric layer. The solid electrolyte layer is divided into a first part that fills the voids of the porous part in the anode body having the dielectric layer and a second part that protrudes from the main surface of the anode body having the dielectric layer. The solid electrolyte layer contains a polyglycerin derivative. In the present disclosure, since the polyglycerin derivative is unevenly distributed in the first part in the solid electrolyte layer, it is possible to suppress a decrease in capacity when the capacitor element is exposed to high temperatures or when the solid electrolytic capacitor is repeatedly charged and discharged.
[0043] The polyglycerin derivative being unevenly distributed in the first portion means that the content C1 of the polyglycerin derivative in the first portion is higher than the content C2 of the polyglycerin derivative in the second portion. Even if the second portion contains a large amount of polyglycerin derivative, the effect of suppressing the decrease in capacity due to the polyglycerin derivative is hardly obtained, and the initial capacity tends to be low and the initial ESR also tends to be high. The ratio of the content C2 to the content C1 (=C2 / C1) is less than 1, and may be 0.5 or less, or may be 0.1 or less. It is also preferable that the second portion does not contain a polyglycerin derivative (i.e., C2 / C1=0).
[0044] The polyglycerin derivative contents C1 and C2 in each portion can be determined using a sample of the solid electrolyte of the first portion (hereinafter referred to as sample S1) and a sample of the solid electrolyte of the second portion (hereinafter referred to as sample S2) taken from the cross section of the sample. More specifically, the solid electrolyte of the first portion is scraped from the gap at multiple locations (e.g., 5 locations) on the cross section to obtain a predetermined amount of sample A1. The solid electrolyte is scraped from multiple locations (e.g., 5 locations) of the second portion protruding from the main surface of the anode body on the cross section to obtain a predetermined amount of sample A2. The masses of these samples are measured. The polyglycerin derivative is extracted from each sample with a solvent at a temperature of 20°C to 40°C. The extract is concentrated, and the polyglycerin derivative is identified by liquid chromatography mass spectrometry (LC-MS) or gas chromatography mass spectrometry (GC-MS). The concentration of the polyglycerin derivative in the extract is determined by a calibration curve method. From this concentration and the masses of the samples A1 and A2, the content (mass %) of the glycerin derivative in each of the first and second portions is calculated.
[0045] The above samples are prepared by embedding a solid electrolytic capacitor or a capacitor element in acrylic resin, cutting the capacitor element in a direction parallel to the length direction at the center of the width direction to expose the cross section, and polishing it. When the anode body is flat, the direction from the first end to the second end is sometimes referred to as the length direction of the anode body. The direction from the first end side to the second end side is a direction parallel to the straight line connecting the center of the end face of the first end and the center of the end face of the second end. This direction is sometimes referred to as the length direction of the anode body or the capacitor element. In addition, the direction perpendicular to the length direction and thickness direction of the anode body (or the capacitor element) is sometimes referred to as the width direction of the anode body (or the capacitor element).
[0046] In the solid electrolyte layer, the first portion may include a portion IA and a portion IB that is present between the portion IA and the dielectric layer. In this case, the polyglycerin derivative is preferably unevenly distributed in the portion IA. The polyglycerin derivative is contained in the first portion away from the dielectric layer, which effectively suppresses deterioration of the adjacent conductive polymer, and suppresses an increase in leakage current due to stress applied to the dielectric layer.
[0047] The solid electrolyte layer includes a conductive polymer. The conductive polymer may be a self-doping conductive polymer, a non-self-doping conductive polymer, or a combination of these as necessary. When the polyglycerin derivative is present in the vicinity of the non-self-doping conductive polymer in the first portion, deterioration of the conductive polymer tends to be suppressed. Therefore, it is preferable that the first portion includes at least a non-self-doping conductive polymer, and it is preferable that the polyglycerin derivative is included in the vicinity of the non-self-doping conductive polymer.
[0048] Since the viscosity of the treatment liquid (fourth treatment liquid) containing the self-doping conductive polymer is relatively low, the self-doping conductive polymer is easily absorbed into the voids of the porous portion to form a thin coating. Therefore, it is preferable to attach the self-doping conductive polymer so as to cover the dielectric layer. For example, when the first portion is divided into a portion IA and a portion IB, the portion IB on the dielectric layer side may contain the self-doping conductive polymer. In this case, if the polyglycerin derivative is unevenly distributed in the portion IA containing the non-self-doping conductive polymer, the capacity reduction when the capacitor element is exposed to high temperatures or when the solid electrolytic capacitor is repeatedly charged and discharged can be further suppressed.
[0049] The polyglycerol derivative being concentrated in the portion IA means that the content CIA of the polyglycerol derivative in the portion IA is higher than the content CIB of the polyglycerol derivative in the portion IB. It is preferable that the content CIB of the polyglycerol derivative is lower than the content CIA.
[0050] The solid electrolytes constituting the first and second portions, or the portion IA and the portion IB, can be distinguished, for example, by an electron probe micro analyzer (EPMA) analysis of the cross-sectional image. For example, an EPMA analysis is performed at equal intervals on the cross-sectional image of the entire solid electrolyte layer, and the boundaries between adjacent solid electrolytes constituting the first or second portion, and the boundary between the portion IA and the portion IB can be determined from the difference in wavelength of the characteristic X-rays at each measurement point.
[0051] The second part may include a self-doping conductive polymer or a non-self-doping conductive polymer. From the viewpoint of ensuring a certain degree of thickness of the second part and easily ensuring initial high capacity and voltage resistance, it is preferable that the second part includes at least a non-self-doping conductive polymer. The ratio of the non-self-doping conductive polymer in the solid electrolyte constituting the second part (the total ratio of the conjugated polymer and the dopant) may be, for example, 75 mass % or more, or 90 mass % or more. The ratio of the non-self-doping conductive polymer in the solid electrolyte constituting the second part is 100 mass % or less. The conductive polymer contained in the solid electrolyte constituting the second part may be composed of only a non-self-doping conductive polymer.
[0052] (Polyglycerin derivatives) The polyglycerin derivative includes, for example, a compound having a moiety corresponding to polyglycerin, but does not include polyglycerin.The above-mentioned compound includes, for example, an ether compound having a moiety corresponding to polyglycerin, and an ester compound having a moiety corresponding to polyglycerin.The polyglycerin derivative may be used alone or in combination of two or more kinds.
[0053] In the portion corresponding to polyglycerin, the number of glycerin units (average degree of polymerization) may be 2 or more and 20 or less, 2 or more and 14 or less (for example, 4 or more and 12 or less), or 2 or more and 10 or less.
[0054] The ether compound may include, for example, polyoxyalkylene polyglyceryl ether. The number of carbon atoms of the alkylene moiety in the polyoxyalkylene moiety may be 2 or more and 4 or less. Examples of the polyoxyalkylene moiety include a polyoxyethylene moiety, a polyoxypropylene moiety, and a polyoxytrimethylene moiety. The polyoxyalkylene moiety may include two or more oxyalkylene units having different numbers of carbon atoms. For example, the polyoxyalkylene moiety may include an oxyethylene unit and an oxypropylene unit. The total number of oxyalkylene units in the polyoxyalkylene moiety contained in one molecule may be 2 or more and 140 or less, 4 or more and 120 or less, 4 or more and 100 or less, or 10 or more and 100 or less (for example, 30 or more and 100 or less).
[0055] Examples of the ester compound include polyglycerin fatty acid esters. The fatty acid constituting the polyglycerin fatty acid ester may be either a saturated fatty acid or an unsaturated fatty acid. The number of carbon atoms of the fatty acid may be 2 to 24, 4 to 20, or 6 to 16. Examples of the fatty acid include caprylic acid, lauric acid, myristic acid, stearic acid, and oleic acid.
[0056] (conductive polymer) Examples of the conductive polymer include a self-doping type conductive polymer and a non-self-doping type conductive polymer.
[0057] A self-doped conductive polymer has, for example, a conjugated polymer skeleton and a functional group (such as an anionic group) that functions as a dopant and is bonded directly or indirectly to the skeleton via a covalent bond.
[0058] Examples of the anionic group include a sulfo group, a carboxy group, a phosphoric acid group, and a phosphonic acid group. The self-doping conductive polymer may contain one type of anionic group, or may contain two or more types of anionic groups. From the viewpoint of easily ensuring higher conductivity of the self-doping conductive polymer, the self-doping conductive polymer may contain at least a sulfo group.
[0059] In the solid electrolyte layer, the anionic group of the self-doped conductive polymer may be contained in any form such as anion, free, ester, salt, etc., or may be contained in a form interacting or complexing with a component contained in the solid electrolyte layer. In this specification, all of these forms are simply referred to as anionic group.
[0060] Conjugated polymers constituting the skeleton of the self-doping conductive polymer include, for example, polymers having a basic skeleton of a π-conjugated polymer (polypyrrole, polythiophene, polyaniline, polyfuran, polyacetylene, polyphenylene, polyphenylenevinylene, polyacene, and polythiophenevinylene, etc.). The above polymers may contain at least one type of monomer unit constituting the basic skeleton. The above polymers include homopolymers, copolymers of two or more monomers, and derivatives thereof (such as substituted bodies having substituents). For example, polythiophenes include poly(3,4-ethylenedioxythiophene), etc. The self-doping conductive polymer has an anionic group in the skeleton of these conjugated polymers. The anionic group may be directly introduced into the skeleton of the conjugated polymer, or may be introduced via a linking group. As the linking group, a polyvalent group (divalent group) containing an alkylene group is preferable. As the linking group, for example, an aliphatic polyvalent group (divalent group, etc.) such as an alkylene group, -R 1 -XR 2 - group (X is an oxygen element or a sulfur element, R 1 and R 2are the same or different and are alkylene groups.) The number of carbon atoms in each alkylene group contained in the linking group may be, for example, 1 or more and 10 or less, or may be 1 or more and 6 or less. The alkylene group may be linear or branched. The linking group may, for example, contain at least an alkylene group having 2 or more carbon atoms. The number of carbon atoms in such an alkylene group may be 2 or more (or 3 or more) and 10 or less, or may be 2 or more (or 3 or more) and 6 or less. For example, R 1 is an alkylene group having 1 to 6 carbon atoms, and R 2 may be an alkylene group having 2 or more (or 3 or more) and 10 or less carbon atoms. However, the linking group is not limited to these.
[0061] The conjugated polymer constituting the skeleton of the self-doping conductive polymer may be polypyrrole, polythiophene or polyaniline. From the viewpoint of easily obtaining high conductivity, etc., the self-doping conductive polymer is preferably a polymer having a skeleton of a conjugated polymer containing a monomer unit corresponding to a thiophene compound and an anionic group introduced into the skeleton.
[0062] The thiophene compound includes a compound having a thiophene ring and capable of forming a repeating structure of the corresponding monomer unit. The thiophene compound can be linked at the 2-position and the 5-position of the thiophene ring to form a repeating structure of the monomer unit.
[0063] The thiophene compound may have a substituent at least at the 3rd and 4th positions of the thiophene ring. The substituent at the 3rd position and the substituent at the 4th position may be linked to form a ring condensed with the thiophene ring. Examples of the thiophene compound include thiophenes having a substituent at least at the 3rd and 4th positions, alkylenedioxythiophene compounds (C such as ethylenedioxythiophene compounds), and the like. 2-4 Alkylenedioxythiophene compounds include compounds having a substituent on the alkylene group.
[0064] The substituents are alkyl groups (C such as methyl and ethyl groups). 1-4 Alkyl groups, alkoxy groups (methoxy groups, ethoxy groups, etc.) 1-4 Alkoxy groups, hydroxy groups, hydroxyalkyl groups (hydroxy C such as hydroxymethyl groups) 1-4 Preferred are, but not limited to, alkyl groups. When the thiophene compound has two or more substituents, the respective substituents may be the same or different. The thiophene ring (at least one of the thiophene ring and the alkylene group in the alkylenedioxythiophene ring) may have the above-mentioned anionic group or a group containing an anionic group (for example, sulfoalkyl group) as a substituent.
[0065] The self-doped conductive polymer may have a backbone of a conjugated polymer (such as PEDOT) containing a monomer unit corresponding to at least a 3,4-ethylenedioxythiophene compound (such as 3,4-ethylenedioxythiophene (EDOT)). The backbone of the conjugated polymer containing at least a monomer unit corresponding to EDOT may contain only a monomer unit corresponding to EDOT, or may contain, in addition to the monomer unit, a monomer unit corresponding to a thiophene compound other than EDOT.
[0066] The weight average molecular weight (Mw) of the self-doped conductive polymer may be 1,000 or more and 1,000,000 or less, or 1,000 or more and 50,000 or less.
[0067] In this specification, the weight average molecular weight (Mw) is a value calculated as polystyrene measured by gel permeation chromatography (GPC). GPC is usually measured using a polystyrene gel column and water / methanol (volume ratio 8 / 2) as the mobile phase.
[0068] The non-self-doping conductive polymer includes, for example, a conjugated polymer (such as a non-self-doping conjugated polymer (such as a conjugated polymer having no anionic groups)) and a dopant.
[0069] Examples of the conjugated polymer include conjugated polymers (such as π-conjugated polymers) exemplified as conjugated polymers constituting the skeleton of the self-doping conductive polymer. The conjugated polymers may be used alone or in combination of two or more. From the viewpoint of easily securing high initial capacity and voltage resistance, a non-self-doping conjugated polymer containing a monomer unit of a thiophene compound may be used. Examples of the thiophene compound corresponding to the monomer unit of the non-self-doping conjugated polymer include the thiophene compound described for the self-doping conductive polymer. The non-self-doping conjugated polymer may include a conjugated polymer (such as PEDOT) containing at least a monomer unit corresponding to a 3,4-ethylenedioxythiophene compound (such as EDOT). The conjugated polymer containing at least a monomer unit corresponding to EDOT may contain only a monomer unit corresponding to EDOT, or may contain, in addition to the monomer unit, a monomer unit corresponding to a thiophene compound other than EDOT.
[0070] The dopant may be at least one selected from the group consisting of anions and polyanions (polymer anions, etc.). Examples of the anions include sulfate ions, nitrate ions, phosphate ions, borate ions, organic sulfonate ions, and carboxylate ions. Examples of dopants that generate sulfonate ions include p-toluenesulfonic acid and naphthalenesulfonic acid. From the viewpoint of facilitating higher stability and higher voltage resistance, polymer anions may be used. Examples of polymer anions having sulfo groups include polymeric polysulfonic acids. Specific examples of polymer anions include polyvinylsulfonic acid, polystyrenesulfonic acid (PSS (including copolymers and substituted bodies having substituents)), polyallylsulfonic acid, polyacrylicsulfonic acid, polymethacrylicsulfonic acid, poly(2-acrylamido-2-methylpropanesulfonic acid), polyisoprenesulfonic acid, polyestersulfonic acid (such as aromatic polyestersulfonic acid), and phenolsulfonic acid novolac resins. However, the dopant is not limited to these specific examples. The dopants may be used alone or in combination of two or more.
[0071] In a non-self-doping conductive polymer (e.g., portion 1A or the second portion), the amount of dopant may be 10 parts by mass or more and 1000 parts by mass or less, or 20 parts by mass or more and 500 parts by mass or less, relative to 100 parts by mass of the conjugated polymer.
[0072] When each of the first and second parts includes multiple layers, a flocculant (such as a cationic component, or a cationic component and an anionic component) may be present between adjacent layers. A flocculant may be present between the first and second parts.
[0073] The solid electrolyte layer or each part may contain an additive as necessary. Examples of the additive include known additives added to the solid electrolyte layer (e.g., coupling agents, silane compounds), and known conductive materials other than conductive polymers. The solid electrolyte layer or each part may contain one of these additives, or may contain two or more of them in combination. Examples of the conductive material as an additive include at least one selected from the group consisting of conductive inorganic materials such as manganese compounds (e.g., manganese dioxide), and TCNQ complex salts.
[0074] In each portion, the adjacent solid electrolytes may have different compositions or may be the same. "Different compositions" includes cases where the components contained in each solid electrolyte are different (e.g., at least one selected from the group consisting of conjugated polymers, dopants, and additives), cases where the contents of components contained in each layer are different, etc.
[0075] (Formation of solid electrolyte layer) The solid electrolyte layer can be formed, for example, through a first step of forming at least a part of the first portion using a first conjugated polymer or its precursor and a polyglycerin derivative, and a second step of forming the second portion using a second conjugated polymer or its precursor. In each of the first and second steps, a dopant may be further used as necessary. When a precursor of each conjugated polymer is used, the conductive polymer constituting each portion is formed by polymerizing the precursor of the conjugated polymer using in situ polymerization (chemical polymerization or electrolytic polymerization, etc.) in the presence of a dopant as necessary. When each conjugated polymer is used, the conductive polymer constituting each portion is formed using a solution or liquid dispersion containing the conjugated polymer and, as necessary, a dopant.
[0076] Prior to the first step, a step (third step) of applying a self-doping conductive polymer to the dielectric layer to form a part of the first portion may be carried out.
[0077] The solid electrolytes formed in the first and third steps may be continuous or discontinuous layers. The second portion formed in the second step is layered as a whole.
[0078] (1st step) In the first step, at least a part of the first portion is formed using a first conjugated polymer or its precursor and a polyglycerin derivative. In the first step, when the first portion is formed, the conductive polymer may protrude from the main surface of the anode body having the dielectric layer, forming a part of the second portion. In addition, the conductive polymer (or solid electrolyte) formed in the first step may constitute at least a part of the portion IA.
[0079] In the first step, for example, at least a part of the first portion may be formed using a first treatment liquid containing a first conjugated polymer or a precursor thereof, a first dopant, and a polyglycerin derivative (method a).
[0080] The first treatment liquid may contain a liquid medium. The liquid medium is, for example, a medium that is liquid at room temperature (for example, 20° C. or higher and 35° C. or lower). Examples of the liquid medium include water, an organic solvent, and a mixture thereof.
[0081] The first treatment liquid may contain one type of first conjugated polymer or a combination of two or more types. When the first treatment liquid contains a precursor, the first treatment liquid may contain one type of precursor or a combination of two or more types. The first treatment liquid may contain one type of first dopant or a combination of two or more types. The first treatment liquid may contain one type of polyglycerin derivative or a combination of two or more types.
[0082] The concentration of the polyglycerin derivative in the first treatment liquid may be 0.5% by mass or more, or may be 1% by mass or more. When the concentration of the polyglycerin derivative is in such a range, the polyglycerin derivative is easily unevenly distributed at a certain content rate in the first portion, and the decrease in capacity when the capacitor element is exposed to high temperatures or when the solid electrolytic capacitor is repeatedly charged and discharged can be further suppressed. The concentration of the glycerin derivative in the first treatment liquid may be 20% by mass or less. From the viewpoint of further suppressing the decrease in capacity of the solid electrolytic capacitor, the concentration of the glycerin derivative in the first treatment liquid is preferably less than 10% by mass, and may be 7% by mass or less or 5% by mass or less. The concentration of the glycerin derivative in the first treatment liquid may be, for example, 0.5% by mass or more and 20% by mass or less, 1% by mass or more and 20% by mass or less, or 1% by mass or more and less than 10% by mass.
[0083] In the first step, application of the first treatment liquid to the anode body and drying may be repeated as necessary. Application of the first treatment liquid to the anode body, drying, application of a flocculant, and drying may be repeated. Polymerization using the first treatment liquid may be performed once or may be repeated multiple times, and washing, drying, etc. may be performed at an appropriate timing of the polymerization (for example, after the final polymerization is completed).
[0084] Besides the method a, after forming a conductive polymer, at least a part of the first portion may be formed by applying a polyglycerin derivative to the conductive polymer (method b). In the method b, for example, the first step may include a substep A of forming a non-self-doping conductive polymer using a second treatment liquid containing a first conjugated polymer or its precursor and a first dopant, and a substep B of forming at least a part of the first portion by applying a third treatment liquid containing a polyglycerin derivative to the non-self-doping conductive polymer.
[0085] Each of the second and third processing liquids may contain a liquid medium. For the liquid medium, refer to the description of the first processing liquid. Examples of the liquid medium include water, an organic solvent, and a mixture thereof.
[0086] The second treatment liquid may contain one type of the first conjugated polymer or a combination of two or more types. When the second treatment liquid contains a precursor, the second treatment liquid may contain one type of the precursor or a combination of two or more types. The second treatment liquid may contain one type of the first dopant or a combination of two or more types. The third treatment liquid may contain one type of polyglycerin derivative or a combination of two or more types.
[0087] When the second treatment liquid contains the first conjugated polymer and the first dopant, the total concentration of the first conjugated polymer and the first dopant in the second treatment liquid may be 0.5% by mass or more and 5% by mass or less, or may be 1% by mass or more and 4% by mass or less.
[0088] The concentration of the polyglycerin derivative in the third treatment liquid may be 1% by mass or more, or 5% by mass or more. When the concentration of the polyglycerin derivative is in such a range, the polyglycerin derivative is easily unevenly distributed at a certain content in the first portion, and the decrease in capacity when the capacitor element is exposed to high temperatures or when the solid electrolytic capacitor is repeatedly charged and discharged can be further suppressed. From the viewpoint of easily retaining the polyglycerin derivative in the vicinity of the non-self-doping conductive polymer, the concentration of the polyglycerin derivative in the third treatment liquid is preferably 10% by mass or more. The concentration of the glycerin derivative in the third treatment liquid may be 30% by mass or less, 25% by mass or less, or 20% by mass or less. The concentration of the glycerin derivative in the third treatment liquid may be, for example, 1% by mass or more and 30% by mass or less, 10% by mass or more and 30% by mass or less, or 10% by mass or more and 25% by mass or less.
[0089] In the first step, the application of the second treatment liquid to the anode body and drying may be repeated as necessary. The application of the second treatment liquid to the anode body, drying, application of the flocculant, and drying may be repeated as necessary. In addition, polymerization using the second treatment liquid may be performed once or may be repeated multiple times. In this case, washing, drying, etc. may be performed at an appropriate timing of the polymerization (for example, after the final polymerization is completed). The application of the third treatment liquid is performed at an appropriate timing of these operations. The application of the third treatment liquid may be performed once or may be performed multiple times. The application of the second treatment liquid and the application of the third treatment liquid may be repeated as necessary. After the application of each treatment liquid, drying may be performed as necessary, and the application of the flocculant may be performed before the application of the second treatment liquid.
[0090] In the first step, the first conjugated polymer and the first dopant correspond to the conjugated polymer and the dopant exemplified for the non-self-doping conductive polymer, respectively. Examples of the precursor of the first conjugated polymer include a monomer, an oligomer, and a prepolymer.
[0091] (3rd step) The third step is carried out prior to the first step. More specifically, in the third step, a treatment liquid (fourth treatment liquid) containing a self-doping conductive polymer is applied to the dielectric layer to form a part of the first portion. The self-doping conductive polymer attached to the surface of the dielectric layer may constitute the portion IB. The self-doping conductive polymer used in the third step corresponds to the self-doping conductive polymer described for the solid electrolyte layer.
[0092] The fourth treatment liquid contains a self-doping conductive polymer and a liquid medium. For the liquid medium, refer to the description of the first treatment liquid. For example, the liquid medium may be water, an organic solvent, or a mixture thereof.
[0093] The fourth treatment liquid may be a liquid dispersion in which particles of a self-doping conductive polymer are dispersed in a liquid medium, or a solution in which a self-doping conductive polymer is dissolved in a liquid medium. In a self-doping conductive polymer, the polymer chain is relatively flexible, the positions of functional groups such as anionic groups are random, and the orientation of the polymer chain is low and the crystallinity is low. Therefore, compared with a non-self-doping conductive polymer, it is easier to dissolve in a liquid medium or to disperse in the form of fine particles. Therefore, the viscosity of the fourth treatment liquid is relatively low, and it is easy to impregnate the voids of the porous portion with high permeability.
[0094] The concentration of the self-doping conductive polymer in the fourth treatment liquid may be 0.5% by mass or more and 5% by mass or less, or may be 1% by mass or more and 4% by mass or less.
[0095] The fourth treatment liquid may contain a polyglycerin derivative, but from the viewpoint of ensuring a higher initial capacity, it is preferable that the fourth treatment liquid does not contain a polyglycerin derivative. When the fourth treatment liquid contains a polyglycerin derivative, the concentration of the polyglycerin derivative in the fourth treatment liquid is preferably lower than the concentration of the polyglycerin derivative in the first treatment liquid or the third treatment liquid. From the viewpoint of ensuring a higher initial capacity, the concentration of the polyglycerin derivative in the fourth treatment liquid may be 5% by mass or less, less than 1% by mass or less than 0.5% by mass, or may be 0.1% by mass or less. When the fourth treatment liquid does not contain a polyglycerin derivative, this includes a case where the polyglycerin derivative in the fourth treatment liquid has a concentration below the detection limit.
[0096] In addition, it is preferable that the third step does not include a sub-step of applying a treatment liquid (fifth treatment liquid) containing a polyglycerin derivative after forming the self-doping conductive polymer. In this case, it is also easy to ensure a higher initial capacity.
[0097] (2nd process) The second step is carried out after the first step. In the second step, the second portion is formed using a second conjugated polymer or a precursor thereof. In the second step, the conductive polymer may enter the voids of the porous portion and form a part of the first portion together with the formation of the second portion.
[0098] In the second step, for example, the second portion may be formed using a treatment liquid (sixth treatment liquid) containing a second conjugated polymer or a precursor thereof and a second dopant.
[0099] The sixth treatment liquid may contain a liquid medium. For the liquid medium, see the description of the first treatment liquid. Examples of the liquid medium include water, an organic solvent, and a mixture thereof.
[0100] The sixth treatment liquid may contain one type of the second conjugated polymer or a combination of two or more types. When the sixth treatment liquid contains a precursor, the sixth treatment liquid may contain one type of the precursor or a combination of two or more types. The sixth treatment liquid may contain one type of the second dopant or a combination of two or more types.
[0101] In the second step, the second conjugated polymer and the second dopant correspond to the conjugated polymer and the dopant exemplified for the non-self-doping conductive polymer, respectively. Precursors of the second conjugated polymer include monomers, oligomers, and prepolymers.
[0102] When the sixth treatment liquid contains the second conjugated polymer and the second dopant, the total concentration of the second conjugated polymer and the second dopant in the sixth treatment liquid may be 1 mass% or more and 10 mass% or less, or may be 3 mass% or more and 8 mass% or less.
[0103] The sixth treatment liquid may contain a polyglycerin derivative, but even if the sixth treatment liquid contains a polyglycerin derivative, the effect of suppressing the capacity decrease is hardly obtained, and the initial characteristics tend to decrease. Therefore, it is preferable that the sixth treatment liquid does not contain a polyglycerin derivative. When the sixth treatment liquid contains a polyglycerin derivative, the concentration of the polyglycerin derivative in the sixth treatment liquid is preferably lower than the concentration of the polyglycerin derivative in the first treatment liquid or the third treatment liquid. From the viewpoint of ensuring higher initial characteristics (initial capacity, etc.), the concentration of the polyglycerin derivative in the sixth treatment liquid may be 5% by mass or less, less than 1% by mass or less than 0.5% by mass, or may be 0.1% by mass or less. When the sixth treatment liquid does not contain a polyglycerin derivative, the case where the polyglycerin derivative in the sixth treatment liquid is at a concentration below the detection limit is included.
[0104] In addition, the second step preferably does not include a sub-step of applying a treatment liquid containing a polyglycerin derivative after forming the conductive polymer. In this case, it is easy to ensure higher initial characteristics. In addition, it is preferable that the second step does not include a step of applying a treatment liquid containing a polyglycerin derivative after the second step.
[0105] In the second step, if necessary, the sixth treatment liquid may be applied to the anode body having the solid electrolyte formed in the first step and then dried repeatedly. Alternatively, the sixth treatment liquid may be applied to the anode body, then dried, and then the coagulant may be applied and then dried repeatedly. Polymerization using the sixth treatment liquid may be performed once or may be repeated multiple times. In this case, washing, drying, etc. may be performed at an appropriate timing of the polymerization (for example, after the final polymerization is completed).
[0106] The solid electrolytic capacitor of the present disclosure is produced by a production method including the above-mentioned steps 1 and 2. The production method may further include a third step.
[0107] (Cathode extraction layer) The cathode extraction layer may, for example, include at least a first layer in contact with the solid electrolyte layer and covering at least a portion of the solid electrolyte layer, and the cathode extraction layer may include the first layer and a second layer covering at least a portion of the first layer.
[0108] The first layer may be, for example, a layer containing conductive particles or a metal foil. The conductive particles may be, for example, at least one selected from conductive carbon and metal powder. The cathode part (more specifically, the cathode extraction layer) may include a layer containing metal powder (such as a metal particle-containing layer). The cathode extraction layer may be, for example, composed of a layer containing conductive carbon (carbon layer) as the first layer and a layer containing metal powder (such as a metal particle-containing layer) or metal foil as the second layer.
[0109] When the cathode extraction layer includes a metal foil or a metal particle-containing layer, the entire cathode extraction layer may be composed of the metal foil or the metal particle-containing layer, or at least one of the first layer and the second layer may be composed of the metal particle-containing layer.
[0110] An example of the conductive carbon is graphite (artificial graphite, natural graphite, etc.).
[0111] The layer containing metal powder as the second layer can be formed, for example, by laminating a composition containing metal powder on the surface of the first layer. Such a second layer can be, for example, a metal particle-containing layer formed using a paste containing metal powder and a resin binder. Although a thermoplastic resin can be used as the resin binder, it is preferable to use a thermosetting resin such as an imide resin or an epoxy resin. From the viewpoint of easily obtaining high conductivity of the second layer, silver-containing particles may be used as the metal powder. Examples of the silver-containing particles include silver particles and silver alloy particles. The second layer may contain one type of silver-containing particle or a combination of two or more types. The silver particles may contain a small amount of impurities.
[0112] When a metal foil is used as the first layer, the type of metal is not particularly limited. For the metal foil, it is preferable to use a valve metal (aluminum, tantalum, niobium, etc.) or an alloy containing a valve metal. If necessary, the surface of the metal foil may be roughened. The surface of the metal foil may be provided with a chemical conversion film, or may be provided with a coating of a metal (heterogeneous metal) different from the metal constituting the metal foil or a nonmetal. Examples of the heterogeneous metal or nonmetal include metals such as titanium and nonmetals such as carbon (conductive carbon, etc.).
[0113] The coating of the dissimilar metal or non-metal (eg, conductive carbon) may be the first layer, and the metal foil may be the second layer.
[0114] The cathode extraction layer is formed by a known method depending on its layer structure. For example, when the cathode extraction layer includes a metal foil as the first layer or the second layer, the first layer or the second layer is formed by laminating the metal foil so as to cover at least a part of the solid electrolyte layer or the first layer. The first layer including conductive particles is formed, for example, by applying a conductive paste or liquid dispersion including conductive particles and, if necessary, a resin binder (such as a water-soluble resin or a curable resin) to the surface of the solid electrolyte layer. The second layer including metal powder is formed, for example, by applying a paste including metal powder and a resin binder to the surface of the first layer. In the process of forming the cathode extraction layer, a drying process, a heating process, or the like may be performed as necessary.
[0115] (Separator) When a metal foil is used for the cathode extraction layer, a separator may be disposed between the metal foil and the anode foil as the anode body. The separator is not particularly limited, and may be, for example, a nonwoven fabric containing fibers of cellulose, polyethylene terephthalate, vinylon, or polyamide (e.g., aliphatic polyamide, aromatic polyamide such as aramid).
[0116] (others) The solid electrolytic capacitor includes at least one capacitor element. The solid electrolytic capacitor may be of a wound type, and may be either a chip type or a stacked type. For example, the solid electrolytic capacitor may include a plurality of stacked capacitor elements. The solid electrolytic capacitor may also include two or more wound capacitor elements. The configuration of the capacitor element may be selected according to the type of the solid electrolytic capacitor.
[0117] In the capacitor element, one end of a cathode lead terminal may be electrically connected to the cathode lead layer. The cathode lead terminal is bonded to the cathode lead layer via the conductive adhesive, for example, by applying a conductive adhesive to the cathode lead layer. One end of an anode lead terminal may be electrically connected to the anode lead portion of the anode body. The other end of the anode lead terminal and the other end of the cathode lead terminal are each drawn out from the resin exterior body or the case. The other end of each terminal exposed from the resin exterior body or the case is used for solder connection with a substrate on which the solid electrolytic capacitor is to be mounted, or the like. In addition to the case of drawing out the lead terminal, at least one end face of the anode portion and the cathode portion may be exposed from the outer surface of the sealing body and electrically connected to an external electrode.
[0118] The capacitor element is sealed using a resin exterior body or case. For example, the capacitor element and the resin material of the exterior body (e.g., uncured thermosetting resin and filler) may be housed in a mold, and the capacitor element may be sealed with the resin exterior body by transfer molding, compression molding, or the like. At this time, the other end side portions of the anode lead terminal and the cathode lead terminal connected to the anode lead drawn out from the capacitor element are exposed from the mold. Also, the capacitor element may be housed in a bottomed case such that the other end side portions of the anode lead terminal and the cathode lead terminal are positioned on the opening side of the bottomed case, and the opening of the bottomed case may be sealed with a sealant to form a solid electrolytic capacitor. The lead may be wire-shaped or frame-shaped (e.g., lead frame).
[0119] FIG. 1 is a schematic cross-sectional view of a solid electrolytic capacitor according to an embodiment of the present disclosure. Solid electrolytic capacitor 20 includes a capacitor element 10 including an anode portion 6 and a cathode portion 7, an exterior body 11 that seals capacitor element 10, an anode lead frame 13 electrically connected to the anode portion 6, and a cathode lead frame 14 electrically connected to the cathode portion 7.
[0120] The anode part 6 has an anode body 1 and an anode wire 2. A part of the anode wire 2 is embedded in the anode body 1, and the remainder protrudes outward from the outer surface of the anode body 1. A part of a first part of an anode lead frame 13 is joined to the protruding part of the anode wire 2 by welding or the like, and is electrically connected thereto.
[0121] A dielectric layer 3 is formed on the surface of the anode body 1. The cathode portion 7 has a solid electrolyte layer 4 covering at least a portion of the dielectric layer 3, and a cathode extraction layer 5 covering at least a portion of the surface of the solid electrolyte layer 4. The cathode extraction layer 5 has a carbon layer formed so as to cover at least a portion of the surface of the solid electrolyte layer 4, and a metal particle-containing layer formed so as to cover at least a portion of the carbon layer. A part of the first portion of the cathode lead frame 14 is adhered and electrically connected to the cathode extraction layer 5 via the conductive adhesive layer 8.
[0122] [Example] The present disclosure will be specifically described below based on examples and comparative examples, but the present disclosure is not limited to the following examples.
[0123] Examples 1 and 2 and Comparative Example 1 A capacitor element was produced in the following manner, and its characteristics were evaluated.
[0124] (1) Preparation of an anode body having a dielectric layer A tantalum sintered body (porous body) with a part of an anode wire embedded therein was prepared as an anode body. The surface of this tantalum sintered body was anodized to form a dielectric layer containing tantalum oxide on the surface of the anode body.
[0125] (2) Formation of solid electrolyte layer (2-1) Third step First, an aqueous dispersion (fourth treatment liquid) containing a self-doping type polythiophene-based polymer was prepared. The concentration of the polythiophene-based polymer in the fourth treatment liquid was 1 to 4 mass%. As the self-doping type polythiophene-based polymer, PEDOT (Mw: about 10,000) having a sulfo group bonded to the PEDOT skeleton via a linking group containing a butylene group was used.
[0126] The tantalum sintered compact prepared in (1) above was immersed in the fourth treatment liquid for about 30 to 60 seconds, and then pulled out of the dispersion liquid. Next, the tantalum sintered compact pulled out of the dispersion liquid was heated (dried) at 140 to 180°C for 10 to 20 minutes to form a solid electrolyte constituting a part of the first portion.
[0127] (2-2) First step A solid electrolyte constituting the remainder of the first portion was formed using the liquid dispersion. Specifically, first, the tantalum sintered body forming the solid electrolyte in (2-1) was immersed in the liquid dispersion for about 30 to 60 seconds, and then the tantalum sintered body was pulled out of the liquid dispersion. Next, the tantalum sintered body pulled out of the liquid dispersion was heated (dried) at 140 to 180°C for 10 to 20 minutes to form a solid electrolyte. In Examples 1 and 2, an aqueous dispersion was used as the liquid dispersion (first treatment liquid) containing a non-self-doping conductive polymer (PSS-doped PEDOT) at a concentration of 1 to 4 mass% and a polyglycerin derivative (polyoxyalkylene polyglyceryl ether (the polyoxyalkylene moiety contains an oxyethylene unit and an oxypropylene unit. The total number of oxyalkylene units is 40 to 80. The number of glycerin units is 6 to 10.)) at the concentration shown in Table 1. In Comparative Example 1, an aqueous dispersion containing a non-self-doping conductive polymer (PEDOT doped with PSS) at a concentration of 2 mass % was used as the liquid dispersion (first treatment liquid).
[0128] (2-3) Second process A solid electrolyte that mainly constitutes the second portion was formed using a liquid dispersion (sixth treatment liquid). Specifically, the tantalum sintered compact that formed the solid electrolyte in (2-2) was first immersed in the liquid dispersion for about 30 to 60 seconds, and then the tantalum sintered compact was pulled out of the liquid dispersion. Next, the tantalum sintered compact pulled out of the liquid dispersion was heated (dried) at 140 to 180°C for 10 to 20 minutes to form a solid electrolyte. As the liquid dispersion (sixth treatment liquid), an aqueous dispersion containing a conductive polymer (PEDOT doped with PSS) at a concentration of 1 to 4 mass% was used. In this manner, an anode body having a solid electrolyte layer was formed.
[0129] (3) Formation of cathode extraction layer The tantalum sintered compact on which the solid electrolyte layer was formed obtained in (2) above was immersed in a dispersion liquid in which graphite particles were dispersed in water, and after being taken out of the dispersion liquid, it was dried to form a carbon layer (first layer) on the surface of the solid electrolyte layer. The drying was performed at 180°C for 10 to 30 minutes.
[0130] Next, a silver paste containing silver particles and a binder resin (epoxy resin) was applied to the surface of the carbon layer, dried at 60 to 80°C for 20 to 40 minutes, and then heated at 180°C for 30 to 60 minutes to harden the binder resin, forming a metal particle-containing layer (second layer). In this way, a cathode extraction layer composed of the carbon layer and the metal particle-containing layer was formed. In this manner, a total of 20 capacitor elements including a cathode portion constituted by a solid electrolyte layer and a cathode extraction layer were fabricated.
[0131] Example 3 In the above (2-2) first step, a solid electrolyte was formed using a liquid dispersion having the same composition as in Comparative Example 1 as the second treatment liquid (substep A). Next, the tantalum sintered compact with the solid electrolyte formed thereon was immersed in an aqueous solution (third treatment liquid) containing a polyglycerin derivative (polyoxyalkylene polyglyceryl ether, the total of oxyalkylene units is 40 to 80. The number of glycerin units is 6 to 10.) at the concentration shown in Table 1 under reduced pressure for about 10 to 20 minutes, and after returning to atmospheric pressure, the tantalum sintered compact was immersed for another 5 to 10 minutes, and then pulled out of the third treatment liquid. Next, the tantalum sintered compact pulled out of the third treatment liquid was dried by heating at 100 to 150°C for 10 to 30 minutes. A capacitor element was produced in the same manner as in Example 1 except for the above.
[0132] Examples 4 and 5 A capacitor element was produced in the same manner as in Example 1, except that the concentration of the polyglycerin derivative in the first treatment liquid was changed as shown in Table 2.
[0133] Examples 6 to 8 Aside from changing the concentration of the polyglycerin derivative in the third treatment liquid as shown in Table 2, a capacitor element was produced in the same manner as in Example 3.
[0134] Examples 9 to 12 After the third step and before the first step, the tantalum sintered compact on which the solid electrolyte was formed obtained in the third step was immersed in an aqueous solution (fifth treatment liquid) containing a polyglycerin derivative at a concentration shown in Table 2 under reduced pressure for about 10 to 20 minutes, and after returning to atmospheric pressure, it was further immersed for about 5 to 10 minutes, and the tantalum sintered compact was pulled out of the fifth treatment liquid. Next, the tantalum sintered compact pulled out of the fifth treatment liquid was dried by heating at 100 to 150°C for 10 to 30 minutes. A capacitor element was produced in the same manner as in Comparative Example 1 except for this.
[0135] "evaluation" The following evaluations were carried out using the capacitor elements obtained in Examples 1 to 3 and Comparative Example 1. The initial capacitance of the capacitor elements obtained in Examples 4 to 12 was measured.
[0136] (1) Initial capacitance and ESR In an environment of 20°C, the initial capacitance C0 (μF) at a frequency of 120 Hz and the initial ESR (mΩ) at a frequency of 100 kHz of the capacitor elements were measured using a four-terminal LCR meter. The average value for 20 capacitor elements was then calculated.
[0137] (2) Initial withstand voltage A voltage was applied to the capacitor element while increasing it at a rate of 1.0 V / sec, and the breakdown voltage (V) at which an overcurrent of 0.5 A flows was measured. The average value for 20 capacitor elements was then calculated.
[0138] (3) Capacity reduction rate under high temperature load Of the capacitor elements for which the initial characteristics (1) were measured, the capacitance (Cx) of 10 pieces was measured after applying a voltage of 50 V at 125°C for 24 hours in the same manner as for the initial capacitance C0. The rate of capacitance reduction due to high temperature load was calculated using the following formula. Capacity reduction rate (%)=(C0-Cx) / C0×100
[0139] (4) Capacity loss rate during charging and discharging Of the capacitor elements for which the initial characteristics (1) were measured, the remaining 10 were charged to 50 V at 25° C. and discharged to 0 V. This cycle of charging and discharging was repeated 800 cycles. The capacitance Cy (discharge capacity) after 800 cycles was measured in the same manner as for the initial capacitance. The capacity reduction rate due to charging and discharging was calculated using the following formula. Capacity reduction rate (%)=(C0-Cy) / C0×100
[0140] The evaluation results are shown in Tables 1 and 2. In Tables 1 and 2, E1 to E12 are Examples 1 to 12, and R1 is Comparative Example 1. In Tables 1 and 2, the initial characteristics are shown as standard values (relative values) when the value of Comparative Example 1 is set to 1.00.
[0141] [Table 1]
[0142] As shown in Table 1, in the examples in which the polyglycerin derivative was unevenly distributed in the first portion of the solid electrolyte layer, the capacity loss rate due to high temperature load and the capacity loss rate due to charge and discharge were both lower than those in the comparative examples. Furthermore, the examples were able to ensure relatively high initial characteristics.
[0143] [Table 2]
[0144] As shown in Table 2, from the viewpoint of facilitating obtaining a relatively high initial capacity, it is preferable that in the first portion, the polyglycerin derivative is concentrated in portion IA that is farther from the dielectric layer than in portion IB on the dielectric layer side. [Industrial Applicability]
[0145] The solid electrolytic capacitor and capacitor element of the present disclosure can suppress the decrease in capacity when exposed to high temperatures. In addition, the solid electrolytic capacitor can suppress the decrease in capacity when repeatedly charged and discharged. Therefore, it is suitable for applications requiring high reliability. However, the applications of the solid electrolytic capacitor are not limited thereto. [Explanation of symbols]
[0146] 20: Solid electrolytic capacitor 10: Capacitor element 1: Anode body 2: Anode wire 3: Dielectric layer 4: Solid electrolyte layer 5: Cathode extraction layer 6: Anode part 7: Cathode 8: Conductive adhesive layer 11: Exterior body 13: Anode lead frame 14: Cathode lead frame
Claims
1. an anode body having a porous portion at least on a surface layer; a dielectric layer covering at least a portion of the anode body; a solid electrolyte layer covering at least a portion of the dielectric layer; the solid electrolyte layer includes a first portion filled in voids of the porous portion in the anode body having the dielectric layer and a second portion protruding from a main surface of the anode body having the dielectric layer, and includes a polyglycerin derivative, The polyglycerin derivative is unevenly distributed in the first portion.
2. the first portion includes a portion IA and a portion IB that is present between the portion IA and the dielectric layer; The solid electrolytic capacitor element according to claim 1 , wherein the polyglycerin derivative is unevenly distributed in the portion IA.
3. the second portion and the portion IA include a non-self-doped conductive polymer; The solid electrolytic capacitor element of claim 2 , wherein the portion IB comprises a self-doped conductive polymer.
4. 3. The solid electrolytic capacitor element according to claim 1, wherein the polyglycerin derivative comprises at least one selected from the group consisting of an ether compound having a moiety corresponding to polyglycerin and an ester compound having a moiety corresponding to polyglycerin.
5. The solid electrolytic capacitor element according to claim 4 , wherein the ether compound comprises a polyoxyalkylene polyglyceryl ether.
6. A solid electrolytic capacitor comprising at least one solid electrolytic capacitor element according to claim 1 or 2.
7. A method for manufacturing a solid electrolytic capacitor element including an anode body having a porous portion at least on a surface layer thereof, a dielectric layer covering at least a portion of the anode body, and a solid electrolyte layer covering at least a portion of the dielectric layer, the method comprising the steps of: the solid electrolyte layer includes a first portion filled in voids of the porous portion in the anode body having the dielectric layer and a second portion protruding from a main surface of the anode body having the dielectric layer, and includes a polyglycerin derivative, The manufacturing method includes: a first step of forming at least a part of the first portion using a first conjugated polymer or a precursor thereof and the polyglycerin derivative; a second step of forming the second portion using a second conjugated polymer or a precursor thereof; A method for producing a solid electrolytic capacitor element, comprising:
8. 8. The method for manufacturing a solid electrolytic capacitor element according to claim 7, wherein in the first step, at least a part of the first portion is formed using a first treatment liquid containing the first conjugated polymer or a precursor thereof, a first dopant, and the polyglycerin derivative.
9. 9. The method for producing a solid electrolytic capacitor element according to claim 8, wherein the concentration of the polyglycerin derivative in the first treatment liquid is less than 10% by mass.
10. The first step comprises: a sub-step A of forming a non-self-doping conductive polymer using a second treatment liquid containing the first conjugated polymer or a precursor thereof and a first dopant; a sub-step B of forming at least a part of the first portion by applying a third treatment liquid containing the polyglycerin derivative to the non-self-doping conductive polymer; The method for producing the solid electrolytic capacitor element according to claim 7, comprising:
11. The method for producing a solid electrolytic capacitor element according to claim 10 , wherein the concentration of the polyglycerin derivative in the third treatment liquid is 10% by mass or more.
12. The method for manufacturing a solid electrolytic capacitor element according to any one of claims 7 to 11, further comprising, prior to the first step, applying a fourth treatment liquid containing a self-doping conductive polymer to the dielectric layer to form a part of the first portion.