Polymer film, laminated film, tubular fixing member, fixing device, and image forming device

A polymer film with controlled filler length and density improves thermal conductivity and heat storage, addressing the limitations of existing films in ultra-thin configurations for fixing devices and image forming apparatuses.

JP2024139388APending Publication Date: 2024-10-09FUJIFILM BUSINESS INNOVATION CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023050298
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing polymer films lack superior thermal conductivity and heat storage properties in the film thickness direction, particularly in ultra-thin configurations.

Method used

The development of a polymer film with specific filler characteristics, including an average maximum filler length of 10 μm or less and densities ranging from 1.0 g/cm³ to 2.6 g/cm³, combined with resins or rubbers, enhances thermal conductivity and heat storage properties.

Benefits of technology

The polymer film exhibits improved thermal conductivity and heat storage capabilities in the thickness direction, outperforming ultra-thin counterparts, and is applicable in fixing devices and image forming apparatuses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139388000003
    Figure 2024139388000003
  • Figure 2024139388000004
    Figure 2024139388000004
  • Figure 2024139388000005
    Figure 2024139388000005
Patent Text Reader

Abstract

To provide a polymer film with superior heat conductivity and heat storage properties in a thickness direction.SOLUTION: A polymer film disclosed herein comprises at least one type of polymer selected from resins and a filler dispersed in the polymer, the filler having an average maximum length of 10 μm or less in a cross-section in a thickness direction, and has a density in a range of 1.0 g / cm3 to 2.0 g / cm3, inclusive. Another polymer film disclosed herein comprises at least one type of polymer selected from rubbers and a filler dispersed in the polymer, the filler having an average maximum length of 10 μm or less in a cross-section in a thickness direction, and has a density in a range of 1.3 g / cm3 to 2.6 g / cm3, inclusive.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a polymeric film, a laminated film, a tubular fusing member, a fusing device, and an image forming apparatus. [Background technology]

[0002] Patent Document 1 discloses a fixing belt having a tubular substrate, an elastic layer, and a surface layer, in which the elastic layer is formed by blending a filler with a heat-resistant elastomer, and the thermal conductivity, density, and specific heat capacity of the elastic layer are calculated based on the formula: (thermal conductivity x density x specific heat capacity) 0.5 The fixing belt has a thermal effusivity of 1.2 or more. Patent Document 2 discloses a fixing belt having a releasable coating layer on the outer peripheral surface of a thin endless metallic belt having a thickness of 10 μm to 35 μm, and a resin layer on the inner peripheral surface. Patent Document 3 discloses a flat-plate-shaped thermally conductive polymer material containing a polymer, spheres, and fibers, in which the fibers are oriented substantially in the planar direction. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-225986 A [Patent Document 2] Japanese Patent Application Publication No. 6-222695 [Patent Document 3] JP 2018-136427 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present disclosure is to provide a polymer membrane having excellent thermal conductivity and heat storage capacity in the membrane thickness direction. [Means for solving the problem]

[0005] Specific means for solving the above problems include the following aspects. <1> A polymer membrane comprising at least one polymer selected from a resin and a filler dispersed in the polymer, The average maximum length of the filler in a cross section in the thickness direction of the polymer film is 10 μm or less, The density of the polymer film is 1.0 g / cm 3 More than 2.0g / cm 3 Below is the Polymer membrane. <2> A polymer membrane comprising at least one polymer selected from rubber and a filler dispersed in the polymer, The average maximum length of the filler in a cross section in the thickness direction of the polymer film is 10 μm or less, The density of the polymer film is 1.3 g / cm 3 More than 2.6g / cm 3 Below is the Polymer membrane. <3> the resin comprises a polyimide resin, The density of the polymer film is 1.4 g / cm 3 More than 2.0g / cm 3 Below is the <1> The polymer membrane according to claim 1. <4> The storage modulus of the polymer film is 0.5 MPa or more and 2.5 MPa or less. <2> The polymer membrane according to claim 1. <5> The filler contains at least one type of ceramic particles selected from the group consisting of aluminum nitride, boron nitride, and silicon carbide. <1> ~ <4> 13. The polymer membrane according to claim 12 . <6> The filler comprises carbon fiber. <1> ~ <5> 13. The polymer membrane according to claim 12 . <7> The volume ratio of the filler in the polymer film is 10% by volume or more and 70% by volume or less. <1> ~ <6> 13. The polymer membrane according to claim 12 . <8> The thermal conductivity of the polymer film in the thickness direction is 1.2 W / m K or more. <1> ~ <7> 13. The polymer membrane according to claim 12 . <9> <1> The polymer membrane according to <2> The polymer membrane according to <3> The polymer membrane according to <4> The polymer membrane according to <5> The polymer membrane according to <6> The polymer membrane according to <7> The polymer membrane according to <8> A laminated film comprising at least one selected from the group consisting of the polymer films described in 1. <10> A base layer, an elastic layer, and a release layer are laminated in this order; At least one of the base material layer and the elastic layer is <1> ~ <8> The polymer membrane according to any one of the above items. Tubular fixing member. <11> A first rotating body and a second rotating body arranged in contact with an outer surface of the first rotating body, At least one of the first rotating body and the second rotating body, <10> The tubular fixing member according to claim 1, a recording medium having a toner image formed on its surface is passed through a contact portion between the first rotating body and the second rotating body to fix the toner image; Fixing device. <12> An image carrier; a charging device for charging the surface of the image carrier; an electrostatic latent image forming device for forming an electrostatic latent image on a charged surface of the image carrier; a developing device for developing the electrostatic latent image formed on the surface of the image carrier with a developer containing a toner to form a toner image; a transfer device for transferring the toner image onto a surface of a recording medium; fixing the toner image onto the recording medium; <11> and a fixing device according to the above. Image forming device. Effect of the Invention

[0006] <1> , <5> , <6> , <7> or <8> According to the method, a polymer film containing a resin has a filler having an average maximum length of more than 10 μm in a cross section in the thickness direction of the polymer film, or has a density of 1.0 g / cm 3 Less than or equal to 2.0g / cm 3 The present invention provides a polymer membrane that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to conventional polymer membranes. <2> , <5> , <6> , <7> or <8> According to the method, a polymer film containing rubber has a filler whose average maximum length exceeds 10 μm in a cross section in the thickness direction of the polymer film, or has a density of 1.3 g / cm 3 Less than or equal to 2.6g / cm 3 The present invention provides a polymer membrane that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to conventional polymer membranes. <3> According to the method, a polymer film containing a resin has a density of 1.4 g / cm 3 Less than or equal to 2.0 g / cm 3 The present invention provides a polymer membrane that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to conventional polymer membranes. <4> According to the present invention, there is provided a polymer membrane containing rubber, which has excellent thermal conductivity and heat storage capacity in the thickness direction compared to polymer membranes having a storage modulus of less than 0.5 MPa or more than 2.5 MPa. <9> According to the method, a polymer film containing a resin has a filler having an average maximum length of more than 10 μm in a cross section in the thickness direction of the polymer film, or has a density of 1.0 g / cm 3 Less than or equal to 2.0g / cm 3 The present invention provides a laminated film having a polymer film that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to polymer films that are thinner than 100%. <9> According to the method, a polymer film containing rubber has a filler whose average maximum length exceeds 10 μm in a cross section in the thickness direction of the polymer film, or has a density of 1.3 g / cm 3 Less than or equal to 2.6g / cm 3 The present invention provides a laminated film having a polymer film that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to polymer films that are thinner than 100%. <10> According to the method, a polymer film containing a resin has a filler having an average maximum length of more than 10 μm in a cross section in the thickness direction of the polymer film, or has a density of 1.0 g / cm 3 Less than or equal to 2.0g / cm 3 The present invention provides a tubular fusing member having a polymer film that has superior through-thickness thermal conductivity and heat storage properties compared to polymer films that have a larger thickness than the conventional tubular fusing member. <10> According to the method, a polymer film containing rubber has a filler whose average maximum length exceeds 10 μm in a cross section in the thickness direction of the polymer film, or has a density of 1.3 g / cm 3 Less than or equal to 2.6g / cm 3 The present invention provides a tubular fusing member having a polymer film that has superior through-thickness thermal conductivity and heat storage properties compared to polymer films that have a larger thickness than the conventional tubular fusing member. <11> According to the method, a polymer film containing a resin has a filler having an average maximum length of more than 10 μm in a cross section in the thickness direction of the polymer film, or has a density of 1.0 g / cm 3 Less than or equal to 2.0g / cm 3 The present invention provides a fixing device including a tubular fixing member having a polymer film that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to polymer films that are thinner than 100 mm. <11> According to the method, a polymer film containing rubber has a filler whose average maximum length exceeds 10 μm in a cross section in the thickness direction of the polymer film, or has a density of 1.3 g / cm 3 Less than or equal to 2.6g / cm 3 The present invention provides a fixing device including a tubular fixing member having a polymer film that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to polymer films that are thinner than 100 mm. <12> According to the method, a polymer film containing a resin has a filler having an average maximum length of more than 10 μm in a cross section in the thickness direction of the polymer film, or has a density of 1.0 g / cm 3 Less than or equal to 2.0g / cm 3 The present invention provides an image forming apparatus including a fixing device having a tubular fixing member having a polymer film that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to polymer films that are superior in thermal conductivity and heat storage capacity in the thickness direction. <12> According to the method, a polymer film containing rubber has a filler whose average maximum length exceeds 10 μm in a cross section in the thickness direction of the polymer film, or has a density of 1.3 g / cm 3 Less than or equal to 2.6g / cm 3 The present invention provides an image forming apparatus including a fixing device having a tubular fixing member having a polymer film that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to polymer films that are superior in thermal conductivity and heat storage capacity in the thickness direction. [Brief description of the drawings]

[0007] [Figure 1] FIG. 2 is a schematic cross-sectional view illustrating an example of a tubular fixing member according to the present disclosure. [Diagram 2] 1 is a schematic configuration diagram illustrating an example of a fixing device according to a first embodiment of the present disclosure. [Diagram 3] FIG. 4 is a schematic configuration diagram illustrating an example of a fixing device according to a second embodiment of the present disclosure. [Figure 4] 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, embodiments of the present disclosure will be described. These descriptions and examples are merely illustrative of the embodiments, and are not intended to limit the scope of the embodiments.

[0009] In the present disclosure, a numerical range indicated using "~" indicates a range that includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples.

[0010] In the present disclosure, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps as long as the purpose of the step is achieved.

[0011] When an embodiment of the present disclosure is described with reference to the drawings, the configuration of the embodiment is not limited to the configuration shown in the drawings. In addition, the size of the members in each drawing is conceptual, and the relative relationship between the sizes of the members is not limited to this.

[0012] In the present disclosure, each component may contain multiple types of corresponding substances. When referring to the amount of each component in a composition in the present disclosure, if multiple substances corresponding to each component are present in the composition, the total amount of the multiple substances present in the composition is meant unless otherwise specified.

[0013] In this disclosure, the "axial direction" of a tubular member means the direction in which the axis of rotation of the tubular member extends, and the "circumferential direction" of the tubular member means the direction of rotation of the tubular member.

[0014] <Polymer membrane> The present disclosure provides a first polymer membrane and a second polymer membrane. When describing matters common to the first polymer membrane and the second polymer membrane, they are collectively referred to as the "polymer membranes of the present disclosure."

[0015] The first polymer film is a polymer film containing at least one polymer selected from resins and a filler dispersed in the polymer (i.e., the resin), the average maximum length of the filler in a cross section in the thickness direction of the polymer film is 10 μm or less, and the density of the polymer film is 1.0 g / cm 3 More than 2.0g / cm 3 The following is the result.

[0016] The second polymer film is a polymer film containing at least one polymer selected from rubber and a filler dispersed in the polymer (i.e., rubber), the average maximum length of the filler in the cross section in the thickness direction of the polymer film is 10 μm or less, and the density of the polymer film is 1.3 g / cm 3 More than 2.6g / cm 3 The following is the result.

[0017] A method for determining the average maximum length of the filler in the polymer membrane of the present disclosure will be described. A cross section is made in the thickness direction of the polymer film, the cross section is observed with a SEM (scanning electron microscope), and 100 fillers are randomly selected. The maximum distance between any two points on the outline of one filler is measured, and the average of the 100 measurements is taken as the average maximum length of the filler.

[0018] The density (g / cm 3 ) is a value determined by measuring as follows. The density of the first polymer film is measured according to the underwater displacement method of JIS K7112:1999 "Method of measurement of density and specific gravity of plastics-nonfoamed plastics". The immersion liquid is new distilled water containing 0.1% by mass or less of a wetting agent to remove air bubbles. The density of the second polymer film is measured in accordance with Method A of JIS K6268:1998 "Vulcanized rubber - Density measurement".

[0019] The polymer membrane of the present disclosure has an average maximum length of the filler in the cross section in the thickness direction of the polymer membrane of 10 μm or less, i.e., by dispersing relatively small fillers, increasing the number density of the fillers (number per unit volume), and facilitating heat transfer between the fillers, and thus has excellent thermal conductivity in the thickness direction. From this viewpoint, the average maximum length of the filler in the cross section in the thickness direction of the polymer membrane is preferably 9 μm or less, more preferably 8 μm or less, and even more preferably 7 μm or less. The average maximum length of the filler in the cross section in the thickness direction of the polymer film is preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 3 μm or more, from the viewpoint of the length of the heat conduction path of one filler.

[0020] The average maximum length of the fillers described above can be controlled by selecting fillers of appropriate particle size or fiber length for use in producing the polymeric membranes of the present disclosure.

[0021] The first polymer film has a density of 1.0 g / cm 3 From this viewpoint, the density of the first polymer film is 1.1 g / cm or more.3 More than 1.2 g / cm is preferable. 3 More preferably, 1.3 g / cm 3 The above is more preferable. However, if the density of the polymer film is too high, the thermal conductivity tends to decrease. Therefore, the density of the first polymer film is set to 2.0 g / cm. 3 Less than or equal to 1.9 g / cm 3 Less than 1.8 g / cm is preferred. 3 The following is more preferred:

[0022] The second polymer membrane has a density of 1.3 g / cm 3 From this viewpoint, the density of the second polymer film is 1.4 g / cm or more. 3 More than 1.5 g / cm is preferable. 3 The above is more preferable. However, if the density of the polymer film is too high, the thermal conductivity tends to decrease. Therefore, the density of the second polymer film is set to 2.6 g / cm. 3 Less than or equal to 2.5 g / cm 3 Less than 2.4 g / cm is preferred. 3 The following is more preferred:

[0023] The density of the polymer membrane of the present disclosure can be controlled by selecting a resin or rubber with an appropriate density to be used in the manufacture of the polymer membrane, and adjusting the filler content in the polymer membrane to an appropriate range.

[0024] The first polymer film contains a resin. Examples of the resin include polyimide resin, polyamide resin, polyamideimide resin, thermotropic liquid crystal polymer, fluororesin, silicone resin, polystyrene resin, etc. The resin may be used alone or in combination of two or more. From the viewpoint of the heat resistance of the first polymer film, the resin is preferably a polyimide resin.

[0025] As an example of an embodiment of the first polymer film, the resin includes a polyimide resin, and the density of the polymer film is 1.4 g / cm 3 More than 2.0g / cm 3In a more preferred embodiment of the present invention, the density of the first polymer film is 1.5 g / cm or less. 3 More than 1.9g / cm 3 The following is the result.

[0026] The second polymer film contains rubber. Examples of the rubber include fluororubber, silicone rubber, and fluorosilicone rubber. The rubber may be used alone or in combination of two or more. From the viewpoint of the heat resistance of the second polymer film, the rubber is preferably silicone rubber.

[0027] From the viewpoint of conformity to the object to be contacted, the second polymer film preferably has a storage modulus of 0.5 MPa or more and 2.5 MPa or less, more preferably 0.8 MPa or more and 2.0 MPa or less, and even more preferably 1.0 MPa or more and 1.8 MPa or less.

[0028] The method for measuring the storage modulus (MPa) of the polymer membrane of the present disclosure is as follows. The polymer film is cut into a rectangle of 20 mm x 4 mm to be used as a measurement sample. The sample is placed in a dynamic viscoelasticity measuring device and dynamic viscoelasticity measurement is performed under the conditions of temperature 30°C, frequency 10 Hz, load 10 gf, and amplitude 10 μm to determine the storage modulus (MPa).

[0029] The filler may be in any shape, such as particulate, fibrous, plate-like, or flake-like. From the viewpoint of thermal conductivity, the filler material is preferably at least one selected from the group consisting of carbon materials, aluminum nitride, boron nitride, and silicon carbide. Examples of filler materials include metal oxides such as alumina, boehmite (alumina monohydrate), silica, titania, zirconia, magnesium oxide, tin oxide, zinc oxide, and barium oxide. The filler may be used alone or in combination of two or more kinds.

[0030] An example of an embodiment of the filler includes particles of at least one type of ceramic selected from the group consisting of aluminum nitride, boron nitride, and silicon carbide.

[0031] An example of an embodiment of the filler is carbon fiber such as carbon nanofiber or carbon nanotube.

[0032] In the polymer membrane of the present disclosure, the volume ratio of the filler is preferably 10% by volume or more and 70% by volume or less, from the viewpoint of the balance of the flexibility, durability, thermal conductivity, and the like of the polymer membrane. The volume fraction of the filler in the first polymer film is preferably 10% by volume or more and 70% by volume or less, more preferably 15% by volume or more and 60% by volume or less, and even more preferably 20% by volume or more and 50% by volume or less. The volume fraction of the filler in the second polymer film is preferably 10% by volume or more and 70% by volume or less, more preferably 20% by volume or more and 65% by volume or less, and even more preferably 30% by volume or more and 60% by volume or less.

[0033] The polymer film of the present disclosure preferably has a thermal conductivity in the thickness direction of 1.2 W / m·K or more, more preferably 1.4 W / m·K or more, and even more preferably 1.6 W / m·K or more. From the viewpoint of heat storage property, the polymer film of the present disclosure preferably has a thermal conductivity in the film thickness direction of 3.5 W / m·K or less, more preferably 3.2 W / m·K or less, and even more preferably 3.0 W / m·K or less.

[0034] The thermal conductivity (W / m·K) in the thickness direction of the polymer membrane of the present disclosure was measured as follows. The polymer film is cut into a 2 mm x 2 mm square sample. The thermal diffusivity is measured at room temperature (25°C ± 3°C) using a thermal diffusivity measuring device, and the thermal conductivity (W / m K) is calculated by multiplying the thermal diffusivity by the specific heat and density.

[0035] The average thickness of the polymer membrane of the present disclosure may be set depending on the application, and is, for example, 10 μm or more and 1000 μm or less, 15 μm or more and 800 μm or less, or 20 μm or more and 500 μm or less.

[0036] The polymer membrane of the present disclosure may be a flat membrane or a tubular membrane. Applications of the polymer membrane of the present disclosure include sheets installed in electronic devices for the purpose of absorbing and releasing heat, tubular fixing members of image forming devices, etc.

[0037] An example of a method for producing a polymer membrane according to the present disclosure is a production method in which the following steps (1) to (3) are carried out in sequence.

[0038] Step (1): A coating liquid is prepared by mixing a resin or rubber with a filler. If necessary, a solvent or a dispersion medium is also mixed. Step (2): The coating liquid is applied onto a substrate and dried to form a coating film. Step (3): The coating film is baked to obtain a polymer film.

[0039] By forming the substrate in step (2) into a cylindrical mold, a tubular polymer membrane can be produced.

[0040] <Laminated film> The laminate film of the present disclosure comprises the polymer film of the present disclosure. The laminated film of the present disclosure may be a laminated film in which only the polymer film of the present disclosure is laminated, or may be a laminated film in which the polymer film of the present disclosure is laminated with another film (e.g., a film having releasability). When a plurality of polymer films of the present disclosure are laminated, the components and / or compositions of the plurality of polymer films may be the same or different. An adhesive layer may be provided between each laminated film.

[0041] The laminated film of the present disclosure may have one polymer film of the present disclosure, or may have two or more polymer films. When the laminated film of the present disclosure has two or more polymer films of the present disclosure, it may be a laminated film in which only the first polymer film is laminated, a laminated film in which only the second polymer film is laminated, or a laminated film in which the first polymer film and the second polymer film are laminated. The order of lamination of the polymer films is not limited.

[0042] The laminated film of the present disclosure may be a flat film or a tubular film. Applications of the laminated film of the present disclosure include a sheet installed in an electronic device for the purpose of absorbing and releasing heat, a tubular fixing member of an image forming device, etc.

[0043] <Tubular fixing member> The tubular anchoring member of the present disclosure comprises the polymeric membrane of the present disclosure. The tubular fixing member of the present disclosure may be a member consisting of only the polymer membrane of the present disclosure, a member in which the polymer membrane of the present disclosure is laminated with another membrane, or a member in which a plurality of polymer membranes of the present disclosure are laminated. When a plurality of polymer membranes of the present disclosure are laminated, the plurality of polymer membranes may be the same or different in components and / or composition.

[0044] An example of an embodiment of the tubular fixing member of the present disclosure includes a configuration in which a base layer, an elastic layer, and a release layer are laminated in this order, and at least one of the base layer and the elastic layer is the polymer film of the present disclosure. In a preferred embodiment of the above, the base layer is a first polymer film and / or the elastic layer is a second polymer film.

[0045] FIG. 1 is a schematic cross-sectional view showing an example of a tubular fixing member of the present disclosure. The tubular fixing member 110 shown in FIG. 1 has a base layer 110A, an elastic layer 110B provided on the base layer 110A, and a release layer 110C provided on the elastic layer 110B. An adhesive layer may be present between the base layer 110A and the elastic layer 110B, and between the elastic layer 110B and the release layer 110C. At least one of the base layer 110A and the elastic layer 110B is the polymer film of the present disclosure. The base layer 110A is preferably a first polymer film. The elastic layer 110B is preferably a second polymer film.

[0046] From the viewpoints of durability and thermal conductivity, the average thickness of the base layer is preferably from 20 μm to 200 μm, more preferably from 30 μm to 150 μm, and even more preferably from 40 μm to 100 μm.

[0047] From the viewpoints of durability and thermal conductivity, the average thickness of the elastic layer is preferably 30 μm or more and 500 μm or less, more preferably 50 μm or more and 480 μm or less, and even more preferably 80 μm or more and 450 μm or less.

[0048] The release layer desirably contains a heat-resistant release material. Examples of heat-resistant release materials include fluororesins. Examples of fluororesins include tetrafluoroethylene / perfluoroalkylvinylether copolymers (PFA), polytetrafluoroethylene (PTFE), tetrafluoroethylene / hexafluoropropylene copolymers (FEP), polyethylene-tetrafluoroethylene (ETFE), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), and vinyl fluoride (PVF).

[0049] The release layer may contain various additives, such as fillers (calcium carbonate, etc.), functional fillers (alumina, etc.), softeners (paraffin, etc.), processing aids (stearic acid, etc.), antioxidants (amines, etc.), crosslinking agents, etc.

[0050] The average thickness of the release layer is preferably from 5 μm to 30 μm, more preferably from 10 μm to 25 μm, and even more preferably from 15 μm to 20 μm.

[0051] The average thickness of each layer of the tubular fixing member is the arithmetic average of the layer thicknesses measured with an eddy current thickness gauge at 10 locations evenly spaced along the axial direction of the tubular fixing member and at 90° intervals around the circumferential direction, a total of 40 locations.

[0052] The tubular fixing member of the present disclosure may be, for example, cylindrical or belt-shaped. The tubular fuser member of the present disclosure may be a fuser belt or a fuser roll.

[0053] <Fixing device> The fixing device of the present disclosure includes a first rotating body and a second rotating body arranged in contact with the outer surface of the first rotating body, and fixes the toner image to the recording medium by passing a recording medium on the surface thereof through a contact portion between the first rotating body and the second rotating body. At least one of the first rotating body and the second rotating body is a rotating body that applies heat to the recording medium, and is the tubular fixing member of the present disclosure.

[0054] As embodiment examples of the fixing device of the present disclosure, a first embodiment and a second embodiment will be given. The fixing device according to the first embodiment includes a heating roll and a pressure belt, and at least the heating roll is the tubular fixing member of the present disclosure. The fixing device according to the second embodiment includes a heating belt and a pressure roll, and at least the heating belt is the tubular fixing member of the present disclosure.

[0055] [First embodiment] FIG. 2 is a schematic diagram showing the fixing device 60 according to the first embodiment. The fixing device 60 includes a heating roll 61 (an example of a first rotating body) and a pressure belt 62 (an example of a second rotating body).

[0056] A halogen lamp 66 (an example of a heating means) is disposed inside the heating roll 61. A temperature sensor 69 is disposed in contact with the surface of the heating roll 61. Based on the temperature measurement value by the temperature sensor 69, the lighting of the halogen lamp 66 is controlled, and the surface temperature of the heating roll 61 is maintained at a target set temperature (for example, 150°C).

[0057] The pressure belt 62 is rotatably supported by a pressure pad 64 and a belt running guide 63 arranged inside.

[0058] The pressure pad 64 presses the pressure belt 62 against the heating roll 61. The pressure belt 62 is pressed against the heating roll 61 by the pressure pad 64, and a pinch region N (nip portion) is formed.

[0059] The pressure pad 64 includes a pinching member 64a and a pinching member 64b. The pinching member 64a is disposed on the entrance side of the pinching region N in order to ensure a wide pinching region N. The pinching member 64b is disposed on the exit side of the pinching region N in order to distort the heating roll 61 and facilitate peeling of the recording medium.

[0060] A sheet-like sliding member 68 is disposed between the pressure pad 64 and the pressure belt 62 in order to reduce the sliding resistance between the inner peripheral surface of the pressure belt 62 and the pressure pad 64. The pressure pad 64 and the sliding member 68 are held by a metallic holding member 65. A belt running guide 63 is attached to the holding member 65. A lubricant supplying device 67, which is a means for supplying a lubricant (oil) to the inner peripheral surface of the pressure belt 62, is attached to the belt running guide 63.

[0061] The peeling member 70 is an auxiliary means for peeling off the recording medium from the fixing device 60, and is disposed downstream of the pinch region N. The peeling member 70 includes a peeling claw 71 and a holding member 72. The peeling claw 71 is held by the holding member 72 at a position adjacent to the heating roll 61.

[0062] The heating roll 61 is rotated by a drive motor (not shown). The heating roll 61 is rotated in the direction of the arrow S by the drive motor, and the pressure belt 62 is rotated in the direction of the arrow R in response to this rotation. Paper K (an example of a recording medium) having an unfixed toner image thereon is guided by a guide 56 and conveyed to a pinch region N, and as the paper K passes through the pinch region N, the toner image on the paper K is fixed by pressure and heat.

[0063] [Second embodiment] FIG. 3 is a schematic diagram showing a fixing device 80 according to the second embodiment. The fixing device 80 includes a fixing belt module 86 having a heating belt 84 (an example of a first rotating body), and a pressure roll 88 (an example of a second rotating body) arranged to be pressed against the heating belt 84 (fixing belt module 86).

[0064] At the contact portion between the heating belt 84 (fixing belt module 86) and the pressure roll 88, a pinch region N (nip portion) is formed.

[0065] The fixing belt module 86 includes a heating belt 84, a heating pressure roll 89, a support roll 90, a support roll 92, a posture correction roll 94, and a support roll 98. The heating belt 84 is wound around the heating pressure roll 89 and the support roll 90. The heating pressure roll 89 is rotated by a drive motor (not shown) and presses the heating belt 84 from its inner circumferential surface toward the pressure roll 88. The support roll 92 is disposed outside the heating belt 84 and defines the rotation path of the heating belt 84. The posture correction roll 94 corrects the posture of the heating belt 84 from the support roll 90 to the heating pressure roll 89, and suppresses meandering of the heating belt 84. The support roll 98 applies tension to the heating belt 84 from its inner circumferential surface on the downstream side of the pinch region N.

[0066] A sheet-like sliding member 82 is disposed between the heating belt 84 and the heating pressure roll 89 in order to reduce the sliding resistance between the inner circumferential surface of the heating belt 84 and the heating pressure roll 89. The sliding member 82 is disposed with both ends supported by support members 96.

[0067] A halogen heater 89A (an example of a heating means) is disposed inside the heating pressure roll 89, and heats the heating belt 84 from the inner circumferential surface side. A halogen heater 90A (an example of a heating means) is disposed inside the support roll 90, and heats the heating belt 84 from the inner circumferential surface side. A halogen heater 92A (an example of a heating means) is disposed inside the support roll 92, and heats the heating belt 84 from the outer circumferential surface side.

[0068] The pressure roll 88 is supported rotatably and is provided so as to be pressed by a biasing means (not shown) against the portion of the heating belt 84 wound around the heating pressure roll 89. The heating belt 84 rotates in the direction of the arrow S due to the rotational drive of the heating pressure roll 89, and the pressure roll 88 rotates in the direction of the arrow R in response to this rotational movement.

[0069] A sheet of paper K (an example of a recording medium) having an unfixed toner image thereon is transported in the direction of arrow P and guided to a pinch region N of the fixing device 80. As the sheet of paper K passes through the pinch region N, the toner image on the sheet of paper K is fixed by pressure and heat.

[0070] <Image forming device> The image forming apparatus of the present disclosure includes an image carrier, a charging device for charging the surface of the image carrier, an electrostatic latent image forming device for forming an electrostatic latent image on the surface of the charged image carrier, a developing device for developing the electrostatic latent image formed on the surface of the image carrier with a developer containing toner to form a toner image, a transfer device for transferring the toner image to the surface of a recording medium, and a fixing device of the present disclosure for fixing the toner image to the recording medium. The fixing device may be a cartridge detachable from the image forming apparatus.

[0071] 4 is a schematic diagram showing the configuration of an image forming apparatus 100 according to this embodiment. The image forming apparatus 100 includes the fixing device 60 according to the first embodiment described above. The image forming apparatus 100 may include the fixing device 80 according to the second embodiment described above instead of the fixing device 60.

[0072] The image forming apparatus 100 is an intermediate transfer type image forming apparatus generally called a tandem type. The image forming apparatus 100 includes image forming units 1Y, 1M, 1C, and 1K that form toner images of each color by electrophotography, a primary transfer section 10 that sequentially transfers (primary transfer) the toner images of each color onto an intermediate transfer belt 15, a secondary transfer section 20 that collectively transfers (secondary transfer) the superimposed toner images transferred onto the intermediate transfer belt 15 onto a recording medium, paper K, a fixing device 60 that fixes the secondary transferred images onto the paper K, and a control section 40 that controls the operation of each device (each section).

[0073] The image forming units 1Y, 1M, 1C, and 1K are arranged in a substantially linear manner from the upstream side of the intermediate transfer belt 15 in the following order: 1Y (yellow unit), 1M (magenta unit), 1C (cyan unit), and 1K (black unit). Each of the image forming units 1Y, 1M, 1C, and 1K includes a photoconductor 11 (an example of an image carrier). The photoconductor 11 rotates in the direction of arrow A.

[0074] Around the photoconductor 11, a charger 12 (an example of a charging device), a laser exposure device 13 (an example of an electrostatic latent image forming device), a developer 14 (an example of a developing device), a primary transfer roll 16, and a photoconductor cleaner 17 are arranged in sequence along the rotational direction of the photoconductor 11.

[0075] The charger 12 charges the surface of the photoconductor 11 . The laser exposure device 13 emits an exposure beam Bm to form an electrostatic latent image on the photoconductor 11 . The developing unit 14 contains toner of each color, and develops the electrostatic latent image on the photoconductor 11 into a visible image using the toner. The primary transfer roll 16 transfers the toner image formed on the photoconductor 11 onto the intermediate transfer belt 15 in the primary transfer section 10 . The photoreceptor cleaner 17 removes residual toner from the photoreceptor 11 .

[0076] The intermediate transfer belt 15 is a belt made of a material in which an antistatic agent such as carbon black is added to a resin such as polyimide or polyamide. The intermediate transfer belt 15 has a volume resistivity of, for example, 1×10 6 Ω cm or more 1×10 14 It has a resistance of Ω·cm or less and a thickness of, for example, 0.1 mm.

[0077] The intermediate transfer belt 15 is supported by a drive roll 31 , a support roll 32 , a tensioning roll 33 , a back roll 25 , and a cleaning back roll 34 , and is driven (rotated) in a circular manner in the direction of arrow B as the drive roll 31 rotates. The driving roll 31 is driven by a motor (not shown) having excellent constant speed performance to rotate the intermediate transfer belt 15 . The support roll 32 , together with the drive roll 31 , supports the intermediate transfer belt 15 , which extends in a substantially straight line along the arrangement direction of the four photoconductors 11 . The tension applying roll 33 applies a constant tension to the intermediate transfer belt 15 and also functions as a correction roll for suppressing meandering of the intermediate transfer belt 15 . The back roll 25 is provided in the secondary transfer section 20 , and the cleaning back roll 34 is provided in a cleaning section that scrapes off residual toner on the intermediate transfer belt 15 .

[0078] The primary transfer roll 16 is disposed in pressure contact with the photoconductor 11 with the intermediate transfer belt 15 sandwiched therebetween, forming the primary transfer section 10 . A voltage (primary transfer bias) of the opposite polarity to the charge polarity of the toner (negative polarity; the same applies below) is applied to the primary transfer roll 16. As a result, the toner images on the photoconductors 11 are electrostatically attracted to the intermediate transfer belt 15 in sequence, and superimposed toner images are formed on the intermediate transfer belt 15. The primary transfer roll 16 is a cylindrical roll that is composed of a shaft (e.g., a cylindrical rod of metal such as iron or SUS) and an elastic layer (e.g., a sponge layer of blended rubber containing a conductive agent such as carbon black) fixed to the periphery of the shaft. The primary transfer roll 16 has a volume resistivity of, for example, 1×10 7.5 Ω cm or more 1×10 8.5 Ω·cm or less.

[0079] The secondary transfer roll 22 is disposed in pressure contact with the back roll 25 with the intermediate transfer belt 15 sandwiched therebetween, forming a secondary transfer section 20 . The secondary transfer roll 22 forms a secondary transfer bias between itself and the back roll 25, and performs second transfer of the toner image onto the paper K (recording medium) conveyed to the secondary transfer unit 20. The secondary transfer roll 22 is a cylindrical roll that is composed of a shaft (e.g., a cylindrical rod of metal such as iron or SUS) and an elastic layer (e.g., a sponge layer of blended rubber containing a conductive agent such as carbon black) that is fixed to the periphery of the shaft. The secondary transfer roll 22 has a volume resistivity of, for example, 1×10 7.5 Ω cm or more 1×10 8.5 Ω·cm or less.

[0080] The back roll 25 is disposed on the back side of the intermediate transfer belt 15 and constitutes a counter electrode for the secondary transfer roll 22 , forming a transfer electric field between itself and the secondary transfer roll 22 . The back roll 25 is formed by, for example, covering a rubber base material with a tube of blended rubber in which carbon is dispersed. The back roll 25 has a surface resistivity of, for example, 1×10 7 Ω / □ or more 1×10 10 It has a hardness of, for example, 70° (Asker C: manufactured by Kobunshi Keiki Co., Ltd.; the same applies below). A metallic power supply roll 26 is arranged in contact with the back roll 25. The power supply roll 26 applies a voltage (secondary transfer bias) of the same polarity as the charge polarity (negative polarity) of the toner, and forms a transfer electric field between the secondary transfer roll 22 and the back roll 25.

[0081] An intermediate transfer belt cleaner 35 is provided on the intermediate transfer belt 15 downstream of the secondary transfer unit 20 so as to be movable toward and away from the intermediate transfer belt 15. The intermediate transfer belt cleaner 35 removes residual toner and paper dust from the intermediate transfer belt 15 after the secondary transfer.

[0082] A reference sensor (home position sensor) 42 is disposed upstream of the image forming unit 1Y. The reference sensor 42 generates a reference signal that serves as a reference for timing image formation in each image forming unit. The reference sensor 42 recognizes a mark provided on the back side of the intermediate transfer belt 15 and generates a reference signal. Upon recognition of this reference signal, the control unit 40 issues an instruction to the image forming units 1Y, 1M, 1C, and 1K to start image formation. An image density sensor 43 for adjusting image quality is disposed downstream of the image forming unit 1K.

[0083] The image forming apparatus 100 includes, as transport means for transporting the paper K, a paper storage unit 50, a paper feed roll 51, a transport roll 52, a transport guide 53, a transport belt 55, and a fixing entrance guide 56. The paper storage section 50 stores paper K before image formation. The paper feed roll 51 takes out the paper K stored in the paper storage unit 50. The transport roll 52 transports the paper K picked up by the paper feed roll 51. The transport guide 53 sends the paper K transported by the transport roll 52 to the secondary transfer unit 20 . The conveyor belt 55 conveys the paper K onto which the image has been transferred by the secondary transfer unit 20 to the fixing device 60 . The fixing entrance guide 56 guides the paper K to the fixing device 60 .

[0084] An image forming method using the image forming apparatus 100 will be described. In the image forming apparatus 100, image data output from an image reading device (not shown) or a computer (not shown) is processed by an image processing device (not shown), and an image forming operation is carried out by image forming units 1Y, 1M, 1C, and 1K.

[0085] The image processing device performs image processing such as shading correction, positional deviation correction, brightness / color space conversion, gamma correction, frame erasure, color editing, movement editing, etc. The image data that has undergone image processing is converted into color material gradation data of four colors, Y, M, C, and K, and is output to the laser exposure device 13.

[0086] The laser exposure device 13 irradiates the exposure beam Bm onto each of the photoconductors 11 of the image forming units 1Y, 1M, 1C, and 1K in accordance with the input color material gradation data. The surface of each photoconductor 11 in the image forming units 1Y, 1M, 1C, and 1K is charged by a charger 12, and then the surface is scanned and exposed by a laser exposure device 13 to form an electrostatic latent image. The electrostatic latent image formed on each photoconductor 11 is developed into a toner image of each color by each image forming unit.

[0087] The toner images formed on the photoconductors 11 of the image forming units 1Y, 1M, 1C, and 1K are transferred onto the intermediate transfer belt 15 in the primary transfer section 10 where the photoconductors 11 and the intermediate transfer belt 15 come into contact with each other. In the primary transfer section 10, a voltage (primary transfer bias) of the opposite polarity to the charge polarity (negative polarity) of the toner is applied to the intermediate transfer belt 15 by the primary transfer roll 16, and the toner images are transferred onto the intermediate transfer belt 15 in succession, overlapping each other.

[0088] The toner image that has been primarily transferred onto the intermediate transfer belt 15 is transported to a secondary transfer unit 20 as the intermediate transfer belt 15 moves. In synchronization with the timing at which the toner image reaches the secondary transfer section 20, the paper K stored in the paper storage section 50 is transported by the paper feed roll 51, the transport roll 52 and the transport guide 53, supplied to the secondary transfer section 20, and sandwiched between the intermediate transfer belt 15 and the secondary transfer roll 22. Then, in the secondary transfer section 20 where a transfer electric field is formed, the toner image on the intermediate transfer belt 15 is electrostatically transferred (secondarily transferred) onto the paper K.

[0089] The paper K onto which the toner image has been electrostatically transferred is peeled off from the intermediate transfer belt 15 by the secondary transfer roll 22 and is transported to the fixing device 60 by the transport belt 55 . The paper K conveyed to the fixing device 60 is heated and pressed by the fixing device 60, so that the unfixed toner image is fixed thereon. Through the above steps, an image is formed on the recording medium by the image forming apparatus 100. EXAMPLES

[0090] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples, but the embodiments of the present invention are in no way limited to these examples. In the following description, unless otherwise specified, "parts" and "%" are by mass. In the following description, syntheses, treatments, manufactures, etc. were carried out at room temperature (25° C.±3° C.) unless otherwise specified.

[0091] <Manufacturing of Fixing Belts> [Example 1] - Formation of base layer - A polyamic acid solution (TX-HMM, Unitika Ltd.) and carbon nanotubes were mixed to prepare coating solution (1). Coating solution (1) was prepared so that the volume ratio of carbon nanotubes in the base layer was the amount shown in Table 1. The coating liquid (1) was applied onto the outer peripheral surface of an aluminum cylindrical mold (diameter 30 mm, width 420 mm), dried at a temperature of 100°C for 80 minutes, and baked by heating at a temperature of 380°C for 40 minutes. The baked layer was removed from the mold to obtain a substrate layer (first polymer film). The amount of coating liquid (1) applied was adjusted so that the thickness of the substrate layer (first polymer film) was 80 μm.

[0092] - Formation of elastic layer - Liquid silicone rubber (two-component type, X-34-2826-A / B, Shin-Etsu Chemical Co., Ltd.) and silicon carbide were mixed to prepare coating solution (2). Coating solution (2) was prepared so that the volume ratio of silicon carbide in the elastic layer was 40 volume %. The base layer was placed on the cylindrical inner mold. The coating liquid (2) was applied onto the outer peripheral surface of the base layer, dried at a temperature of 115°C for 15 minutes, and baked at a temperature of 200°C for 2 hours to form an elastic layer. The amount of coating liquid (2) was adjusted so that the thickness of the elastic layer was 450 μm.

[0093] - Formation of release layer - A PFA tube having an inner diameter of 29.3 mm and an average thickness of 20 μm, the inner surface of which was modified by liquid ammonia treatment, was prepared. The PFA tube was coated onto a laminate having a base layer and an elastic layer. After coating, the laminate was baked at a temperature of 200° C. for 2 hours to bond the laminate. The laminate was removed from the inner mold and cut to a width of 380 mm. Thus, a fixing belt (a tubular fixing member of the present disclosure) was obtained.

[0094] [Examples 2 to 5, Comparative Examples 1 to 3] A fixing belt (a tubular fixing member of the present disclosure) was manufactured in the same manner as in Example 1, except that the resin and / or filler used to form the base layer (first polymer film) was changed to the specifications shown in Table 1. When polystyrene or polyethylene was used as the resin for the base layer, the base layer was formed by injection molding.

[0095] [Example 11] - Formation of base layer - A polyamic acid solution (TX-HMM, Unitika Ltd.) and carbon nanotubes were mixed to prepare a coating solution (11). The coating solution (11) was prepared so that the volume ratio of the carbon nanotubes in the base layer was 20 volume %. The coating liquid (11) was applied onto the outer peripheral surface of an aluminum cylindrical mold (diameter 30 mm, width 420 mm), dried at a temperature of 100°C for 80 minutes, and baked by heating at a temperature of 380°C for 40 minutes. The baked layer was removed from the mold to obtain a substrate layer. The amount of coating liquid (11) applied was adjusted so that the thickness of the substrate layer was 80 μm.

[0096] - Formation of elastic layer - Liquid silicone rubber (two-component type, X-34-2826-A / B, Shin-Etsu Chemical Co., Ltd.) and silicon carbide were mixed to prepare coating solution (12). Coating solution (12) was prepared so that the volume ratio of silicon carbide in the elastic layer was the amount shown in Table 2. The base layer was placed on the cylindrical inner mold. The coating liquid (12) was applied onto the outer peripheral surface of the base layer, dried at a temperature of 115°C for 15 minutes, and baked at a temperature of 200°C for 2 hours to form an elastic layer (second polymer film). The amount of the coating liquid (12) applied was adjusted so that the thickness of the elastic layer was 450 μm.

[0097] - Formation of release layer - A PFA tube having an inner diameter of 29.3 mm and an average thickness of 20 μm, the inner surface of which was modified by liquid ammonia treatment, was prepared. The PFA tube was coated onto a laminate having a base layer and an elastic layer. After coating, the laminate was baked at a temperature of 200° C. for 2 hours to bond the laminate. The laminate was removed from the inner mold and cut to a width of 380 mm. Thus, a fixing belt (a tubular fixing member of the present disclosure) was obtained.

[0098] [Examples 12 to 14, Comparative Examples 11 to 12] A fixing belt (a tubular fixing member of the present disclosure) was produced in the same manner as in Example 11, except that the filler used in forming the elastic layer (second polymer film) was changed to the specifications shown in Table 2.

[0099] <Physical properties of polymer membranes> Regarding the physical properties of the polymer film, the base layer (first polymer film) is measured in Example 1 etc., and the elastic layer (second polymer film) is measured in Example 11 etc. The measurement results are shown in Tables 1 and 2.

[0100] [Average maximum length of filler] A cross section of the fixing belt in the thickness direction was made, and the cross section of the base layer or elastic layer was observed with a SEM (scanning electron microscope). 100 fillers were randomly selected, and the maximum distance between any two points on the outline of one filler was measured, and the average value of the 100 fillers was calculated.

[0101] [Polymer film density] The base layer or the elastic layer was peeled off from the fixing belt. Density of the substrate layer (g / cm 3 ) was measured according to the underwater displacement method of JIS K7112:1999 "Method of measurement of density and specific gravity of plastics - non-foamed plastics". The immersion liquid used was new distilled water containing 0.1% by mass or less of a wetting agent to remove air bubbles. Density of the elastic layer (g / cm 3 ) was measured according to JIS K6268:1998 "Vulcanized rubber - Density measurement" Method A.

[0102] [Thermal Conductivity] The base material layer or elastic layer was peeled off from the fixing belt. The base material layer or elastic layer was cut into a square of 2 mm in the axial direction and 2 mm in the circumferential direction, which was used as the measurement sample. The thermal diffusivity was measured at room temperature (25°C ± 3°C) using a thermal diffusivity measuring device ai-phase (Ai-Phase Co., Ltd.), and the thermal conductivity (W / m K) was calculated by multiplying the thermal diffusivity by the specific heat and density.

[0103] [Heat capacity] The base layer or elastic layer was peeled off from the fixing belt. The heat capacity of the base layer or elastic layer was measured according to JIS K7123:2012 "Method of measuring specific heat capacity of plastics" and the heat capacity was calculated based on the unit area of ​​1 m. 2 The heat capacity was converted to J / K. In this embodiment, the heat capacity is preferably 1000 J / K or greater.

[0104] [Storage modulus] The elastic layer was peeled off from the fixing belt. The elastic layer was cut into a rectangle of 20 mm x 4 mm to be used as a measurement sample. The sample was placed in a dynamic viscoelasticity measuring device and dynamic viscoelasticity measurement was performed under the conditions of temperature 30°C, frequency 10 Hz, load 10 gf, and amplitude 10 μm to determine the storage modulus (MPa).

[0105] <Performance evaluation of fixing belt> [Adhesion to thick paper] The fixing belt was attached to an image forming apparatus (Versant3100i Press, Fujifilm Business Innovation Co., Ltd.). 100 black solid images were printed on A4-sized thick paper (COLOR COPY (A4, 350g), Mondi). Fixation of the image was visually confirmed, and then the image was rubbed with a hand to check for image defects such as crushing and blurring, and classified as follows. The evaluation results are shown in Tables 1 and 2. A: No image defects were found on 100 sheets. B: Image defects were found on 1 to 19 sheets. C: Image defects were observed on 20 or more sheets. D: There is one or more pieces of paper on which the image has not been fixed.

[0106] [Table 1]

[0107] [Table 2]

[0108] The polymer film, laminated film, tubular fixing member, fixing device, and image forming apparatus of the present disclosure include the following aspects. (((1))) A polymer membrane comprising at least one polymer selected from a resin and a filler dispersed in the polymer, The average maximum length of the filler in a cross section in the thickness direction of the polymer film is 10 μm or less, The density of the polymer film is 1.0 g / cm 3 More than 2.0g / cm 3 Below is the Polymer membrane. (((2))) A polymer membrane comprising at least one polymer selected from rubber and a filler dispersed in the polymer, The average maximum length of the filler in a cross section in the thickness direction of the polymer film is 10 μm or less, The density of the polymer film is 1.3 g / cm 3 More than 2.6g / cm 3 Below is the Polymer membrane. (((3))) the resin comprises a polyimide resin, The density of the polymer film is 1.4 g / cm 3 More than 2.0g / cm 3 Below is the The polymer membrane according to (((1))). (((4))) The storage modulus of the polymer film is 0.5 MPa or more and 2.5 MPa or less. The polymer membrane according to (((2))). (((5))) The polymer film according to any one of (((1))) to (((4))), wherein the filler contains at least one type of ceramic particle selected from the group consisting of aluminum nitride, boron nitride, and silicon carbide. (((6))) The polymer membrane according to any one of (((1))) to (((5))), wherein the filler comprises carbon fiber. (((7))) The polymer membrane according to any one of (((1))) to (((6))), wherein the volume ratio of the filler in the polymer membrane is 10 volume % or more and 70 volume % or less. (((8))) The polymer film according to any one of (((1))) to (((7))), wherein the polymer film has a thermal conductivity in a thickness direction of 1.2 W / m·K or more. (((9))) A laminated film comprising at least one selected from the group consisting of a polymer film according to (((1))), a polymer film according to (((2))), a polymer film according to (((3))), a polymer film according to (((4))), a polymer film according to (((5))), a polymer film according to (((6))), a polymer film according to (((7))), and a polymer film according to (((8))). (((10))) A base layer, an elastic layer, and a release layer are laminated in this order; At least one of the base material layer and the elastic layer is a polymer film according to any one of (((1))) to (((8))). Tubular fixing member. (((11))) A first rotating body and a second rotating body arranged in contact with an outer surface of the first rotating body, At least one of the first rotating body and the second rotating body is a tubular fixing member described in (((10))), a recording medium having a toner image formed on its surface is passed through a contact portion between the first rotating body and the second rotating body to fix the toner image; Fixing device. (((12))) An image carrier; a charging device for charging the surface of the image carrier; an electrostatic latent image forming device for forming an electrostatic latent image on a charged surface of the image carrier; a developing device for developing the electrostatic latent image formed on the surface of the image carrier with a developer containing a toner to form a toner image; a transfer device for transferring the toner image onto a surface of a recording medium; and a fixing device according to (((11))) that fixes the toner image onto the recording medium. Image forming device.

[0109] According to (((1))), (((5))), (((6))), (((7))) or (((8))), there is provided a polymer film containing a resin, the polymer film having an average maximum length of a filler exceeding 10 μm in a cross section in the thickness direction of the polymer film, or a polymer film having a density of 1.0 g / cm 3 Less than or equal to 2.0g / cm 3 The present invention provides a polymer membrane that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to conventional polymer membranes. According to (((2)), (((5)), (((6)), (((7))) or (((8)), there is provided a polymer film containing rubber, the polymer film having an average maximum length of a filler exceeding 10 μm in a cross section in the thickness direction of the polymer film, or a polymer film having a density of 1.3 g / cm 3 Less than or equal to 2.6g / cm 3 The present invention provides a polymer membrane that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to conventional polymer membranes. According to (((3))), a polymer membrane containing a resin is provided, the density of which is 1.4 g / cm 3 Less than or equal to 2.0 g / cm 3 The present invention provides a polymer membrane that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to conventional polymer membranes. According to (((4))), there is provided a polymer membrane containing rubber, which has excellent thermal conductivity and heat storage capacity in the thickness direction compared to polymer membranes having a storage modulus of less than 0.5 MPa or more than 2.5 MPa. According to (((9))), there is provided a polymer film containing a resin, the polymer film having an average maximum length of a filler exceeding 10 μm in a cross section in the thickness direction of the polymer film, or a polymer film having a density of 1.0 g / cm 3 Less than or equal to 2.0g / cm 3 The present invention provides a laminated film having a polymer film that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to polymer films that are thinner than 100%. According to (((9))), there is provided a polymer membrane containing rubber, in which the average maximum length of the filler in a cross section in the thickness direction of the polymer membrane exceeds 10 μm, or the density of the polymer membrane is 1.3 g / cm 3 Less than or equal to 2.6g / cm 3 The present invention provides a laminated film having a polymer film that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to polymer films that are thinner than 100%. According to (((10))), there is provided a polymer film containing a resin, the polymer film having an average maximum length of a filler exceeding 10 μm in a cross section in the thickness direction of the polymer film, or a polymer film having a density of 1.0 g / cm 3 Less than or equal to 2.0g / cm 3 The present invention provides a tubular fusing member having a polymer film that has superior through-thickness thermal conductivity and heat storage properties compared to polymer films that have a larger thickness than the conventional tubular fusing member. According to (((10))), there is provided a polymer membrane containing rubber, in which the average maximum length of the filler in a cross section in the thickness direction of the polymer membrane exceeds 10 μm, or the density of the polymer membrane is 1.3 g / cm 3 Less than or equal to 2.6g / cm 3 The present invention provides a tubular fusing member having a polymer film that has superior through-thickness thermal conductivity and heat storage properties compared to polymer films that have a larger thickness than the conventional tubular fusing member. According to (((11))), there is provided a polymer film containing a resin, the polymer film having an average maximum length of a filler exceeding 10 μm in a cross section in the thickness direction of the polymer film, or a polymer film having a density of 1.0 g / cm 3 Less than or equal to 2.0g / cm 3 The present invention provides a fixing device including a tubular fixing member having a polymer film that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to polymer films that are thinner than 100 mm. According to (((11))), there is provided a polymer membrane containing rubber, in which the average maximum length of the filler in a cross section in the thickness direction of the polymer membrane exceeds 10 μm, or the density of the polymer membrane is 1.3 g / cm 3 Less than or equal to 2.6g / cm 3 The present invention provides a fixing device including a tubular fixing member having a polymer film that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to polymer films that are thinner than 100 mm. According to (((12))), there is provided a polymer film containing a resin, the polymer film having an average maximum length of a filler exceeding 10 μm in a cross section in the thickness direction of the polymer film, or a polymer film having a density of 1.0 g / cm 3 Less than or equal to 2.0g / cm 3 The present invention provides an image forming apparatus including a fixing device having a tubular fixing member having a polymer film that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to polymer films that are superior in thermal conductivity and heat storage capacity in the thickness direction. According to (((12))), there is provided a polymer membrane containing rubber, in which the average maximum length of the filler in a cross section in the thickness direction of the polymer membrane exceeds 10 μm, or the density of the polymer membrane is 1.3 g / cm 3 Less than or equal to 2.6g / cm 3 The present invention provides an image forming apparatus including a fixing device having a tubular fixing member having a polymer film that is superior in thermal conductivity and heat storage capacity in the thickness direction compared to polymer films that are superior in thermal conductivity and heat storage capacity in the thickness direction. [Explanation of symbols]

[0110] 110 Tubular fixing member 110A base material layer 110B Elastic layer 110C Release layer

[0111] 60 Fixing device 61 Heating Roll 62 Pressure Belt 63 Belt guide 64 Pressure Pad 64a Clamping member 64b Clamping member 65 Retaining member 66 Halogen lamp 67 Lubricant supply device 68 Sliding members 69 Thermosensor 70 Peeling member 71 Peeling Claw 72 Retaining member

[0112] 80 Fixing device 82 Sliding member 84 Heating Belt 86 Fuser Belt Module 88 Pressure Roll 89 Heated pressure roll 89A halogen heater 90 Support Roll 90A halogen heater 92 Support Roll 92A halogen heater 94 Posture Correction Roll 96 Support member 98 Support Roll

[0113] 100 Image forming device 1Y, 1M, 1C, 1K Image forming unit 11 Photoconductor (an example of an image carrier) 12 Charger (an example of a charging device) 13 Laser exposure device (an example of an electrostatic latent image forming device) 14 Developing unit (an example of a developing device) 15 Intermediate transfer belt 16 Primary transfer roll (an example of a transfer device) 22 Secondary transfer roll (an example of a transfer device) K Paper (an example of a recording medium)

Claims

1. A polymer membrane comprising at least one polymer selected from a resin and a filler dispersed in the polymer, the average maximum length of the filler in a cross section in the thickness direction of the polymer film is 10 μm or less; The density of the polymer film is 1.0 g / cm 3 2.0g / cm or more 3 Below is the Polymer membrane.

2. A polymer membrane comprising at least one polymer selected from rubber and a filler dispersed in the polymer, the average maximum length of the filler in a cross section in the thickness direction of the polymer film is 10 μm or less; The density of the polymer film is 1.3 g / cm 3 2.6g / cm or more 3 Below is the Polymer membrane.

3. the resin comprises a polyimide resin, The density of the polymer film is 1.4 g / cm 3 2.0g / cm or more 3 Below is the The polymer membrane according to claim 1.

4. The storage modulus of the polymer film is 0.5 MPa or more and 2.5 MPa or less. The polymer membrane according to claim 2.

5. 3. The polymer membrane according to claim 1, wherein the filler comprises at least one type of ceramic particle selected from the group consisting of aluminum nitride, boron nitride, and silicon carbide.

6. The polymer membrane of claim 1 or claim 2, wherein the filler comprises carbon fiber.

7. 3. The polymer membrane according to claim 1, wherein a volume ratio of the filler to the polymer membrane is 10 volume % or more and 70 volume % or less.

8. 3. The polymer film according to claim 1, wherein the polymer film has a thermal conductivity in a thickness direction of 1.2 W / m·K or more.

9. A laminated film comprising at least one of the polymer film according to claim 1 and the polymer film according to claim 2.

10. A base layer, an elastic layer, and a release layer are laminated in this order; At least one of the base layer and the elastic layer is the polymer membrane according to claim 1 or 2. Tubular fixing member.

11. A first rotating body and a second rotating body arranged in contact with an outer surface of the first rotating body, At least one of the first rotating body and the second rotating body is the tubular fixing member according to claim 10 , a recording medium having a toner image formed on its surface is passed through a contact portion between the first rotating body and the second rotating body to fix the toner image; Fixing device.

12. An image carrier; a charging device for charging the surface of the image carrier; an electrostatic latent image forming device for forming an electrostatic latent image on a charged surface of the image carrier; a developing device for developing the electrostatic latent image formed on the surface of the image carrier with a developer containing a toner to form a toner image; a transfer device for transferring the toner image onto a surface of a recording medium; and a fixing device according to claim 11 that fixes the toner image onto the recording medium. Image forming device.

Citation Information

Patent Citations

  • Fixing belt

    JP1994222695A

  • Fixing belt

    JP2012225986A