Manufacturing method of solar cell and solar cell
By employing pattern printing resist and a lift-off method to pattern transparent electrode layers in solar cells, the manufacturing process is simplified and performance is enhanced through improved contact properties and reduced bulk resistance.
Patent Information
- Application Number
- JP2023050771
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Existing methods for manufacturing back electrode type solar cells, such as those using photolithography and lift-off techniques, are complex and do not adequately improve the performance due to issues with etching and contact properties of transparent electrode layers.
The use of pattern printing resist and a lift-off method to pattern transparent electrode layers, where the edges of the lift-off layer are altered and utilized to improve contact properties and reduce bulk resistance, allowing for the formation of crystalline transparent electrode layers.
This approach simplifies the manufacturing process and enhances the performance of solar cells by improving contact properties and reducing bulk resistance of transparent electrode layers, leading to increased output and efficiency.
Smart Images

Figure 2024139850000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a back electrode type (back contact type) solar cell, and to a back electrode type solar cell. [Background technology]
[0002] Patent Document 1 discloses a back electrode type solar cell. Such a back electrode type solar cell includes a semiconductor substrate that functions as a photoelectric conversion layer, a first intrinsic semiconductor layer, a first conductive type semiconductor layer, and a first electrode layer that are stacked in this order on a portion of the back side of the semiconductor substrate, and a second intrinsic semiconductor layer, a second conductive type semiconductor layer, and a second electrode layer that are stacked in this order on another portion of the back side of the semiconductor substrate. The solar cell also includes a third intrinsic semiconductor layer and an optical adjustment layer that are stacked in this order on the light receiving surface side of the semiconductor substrate.
[0003] In general, an etching method using photolithography technology is used in the patterning of the first conductive type semiconductor layer (first patterning) and the patterning of the second conductive type semiconductor layer (second patterning).However, the etching method using photolithography technology requires processes such as applying photoresist by spin coating, drying the photoresist, exposing the photoresist, developing the photoresist, etching the semiconductor layer using the photoresist as a mask, and removing the photoresist, making the process complicated.
[0004] In this regard, Patent Document 1 describes a technique for simplifying the patterning process by using a lift-off method that uses a lift-off layer (sacrificial layer) in the second patterning. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2014-75526 A Summary of the Invention [Problem to be solved by the invention]
[0006] The inventors of the present application have devised the use of a pattern printing resist by a pattern printing method in the first patterning, which makes it possible to reduce the exposure and development steps compared to the case where a photoresist by a spin coating method (photolithography method) is used, and thus makes it possible to further simplify the patterning process.
[0007] The inventors of the present application have also devised a method of patterning the transparent electrode layer by using a wet etching method that uses a metal electrode layer as a mask. In this case, it is necessary to form an amorphous transparent electrode layer that is easily etched, and the transparent electrode layer has low contact properties and high bulk resistance. Therefore, there is a problem that the performance of the solar cell cannot be sufficiently improved.
[0008] An object of the present invention is to provide a method for manufacturing a solar cell that enables performance improvement, and a solar cell. [Means for solving the problem]
[0009] Here, the inventor(s) of the present application discovered that, in the first patterning, when a pattern printing resist is used by a pattern printing method, the ends of the pattern printing resist become thin due to printing sagging, and as a result, the etching solution penetrates into the ends of the lift-off layer through the thin ends of the pattern printing resist, causing the ends of the lift-off layer to become half-etched and to become porous, and as a result, the ends of the lift-off layer remain in a film-like state without being peeled off during the lift-off process.
[0010] The present inventors then discovered that in patterning the transparent electrode layer, the transparent electrode layer can be patterned by a lift-off method that utilizes the residue of this lift-off layer, i.e., the residue of the lift-off layer at the boundary between the p region and the n region.
[0011] In the lift-off method, the lift-off layer is removed to peel off the transparent electrode layer thereon, so that even if a crystalline transparent electrode layer that cannot be easily etched is formed, the transparent electrode layer can be patterned. Therefore, the contact property of the transparent electrode layer can be improved and the bulk resistance of the transparent electrode layer can be reduced. Therefore, the performance of the solar cell can be improved.
[0012] Therefore, the present invention provides a method for manufacturing a solar cell, which includes a semiconductor substrate, a first conductive type semiconductor layer disposed in a first region that is a part of the back surface side of the semiconductor substrate, a second conductive type semiconductor layer disposed in a second region that is another part of the back surface side of the semiconductor substrate, a first transparent electrode layer and a first metal electrode layer corresponding to the first conductive type semiconductor layer, and a second transparent electrode layer and a second metal electrode layer corresponding to the second conductive type semiconductor layer, wherein the first conductive type semiconductor layer is a p-type semiconductor layer and the second conductive type semiconductor layer is an n-type semiconductor layer, and the method includes the steps of: (a) a first semiconductor layer material film formation step of forming a first conductive type semiconductor layer material film and a lift-off layer material film on the back surface side of the semiconductor substrate; (b) a first semiconductor layer formation step of patterning the first conductive type semiconductor layer material film and the lift-off layer material film using a printing resist to form the first conductive type semiconductor layer and the lift-off layer in the first region; and (c) a second semiconductor layer material film forming step of forming a second conductive type semiconductor layer material film on the back surface side of the semiconductor substrate; (d) a second semiconductor layer forming step of forming a second conductive type semiconductor layer in the second region by removing the lift-off layer using a lift-off method, in which the transformed portion of the lift-off layer in the third region remains and the second conductive type semiconductor layer remains on the transformed portion of the lift-off layer in the third region; and (e) a transparent electrode layer material film forming step of forming a transparent electrode layer material film on the back surface side of the semiconductor substrate. (g) a transparent electrode layer forming step of removing a portion of the second conductive type semiconductor layer on the altered portion of the lift-off layer in the third region by using a lift-off method, thereby forming the first transparent electrode layer and the second transparent electrode layer in the first region and the second region excluding the third region; and (h) a metal electrode layer forming step of forming the first metal electrode layer and the first metal electrode layer on the first transparent electrode layer and the second transparent electrode layer.
[0013] The solar cell of the present invention is a back electrode type solar cell comprising a semiconductor substrate, a first conductivity type semiconductor layer arranged in a first region which is a part of the back surface side of the semiconductor substrate, a second conductivity type semiconductor layer arranged in a second region which is another part of the back surface side of the semiconductor substrate, a first transparent electrode layer and a first metal electrode layer corresponding to the first conductivity type semiconductor layer, and a second transparent electrode layer and a second metal electrode layer corresponding to the second conductivity type semiconductor layer, wherein the first conductivity type semiconductor layer is a p-type semiconductor layer, the second conductivity type semiconductor layer is an n-type semiconductor layer, and the entire second conductivity type semiconductor layer in the second region is covered with the second transparent electrode layer. Effect of the Invention
[0014] According to the present invention, the performance of a solar cell can be improved. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a diagram showing the solar cell according to the embodiment as viewed from the back surface side. [Diagram 2] 2 is a cross-sectional view of the solar cell shown in FIG. 1 taken along line II-II. [Figure 3A] 3A to 3C are diagrams illustrating a first semiconductor layer material film forming step and a lift-off layer forming step in the method for manufacturing a solar cell according to the present embodiment. [Figure 3B] 3A to 3C are diagrams illustrating a resist formation step in the method for manufacturing a solar cell according to the present embodiment. [Figure 3C] 5A to 5C are diagrams illustrating a first semiconductor layer forming step in the method for manufacturing a solar cell according to the embodiment. [Figure 3D] 5A to 5C are diagrams illustrating a resist removal step in the method for manufacturing a solar cell according to the present embodiment. [Figure 3E] 4A to 4C are diagrams illustrating a second semiconductor layer material film forming step in the method for manufacturing a solar cell according to the embodiment. [Figure 3F] 5A to 5C are diagrams illustrating a second semiconductor layer forming step in the method for manufacturing a solar cell according to the embodiment. [Figure 3G]3A to 3C are diagrams illustrating a transparent electrode layer material film forming step in the manufacturing method for the solar cell according to the present embodiment. [Figure 3H] 3A to 3C are diagrams illustrating a transparent electrode layer forming step in the manufacturing method for the solar cell according to the embodiment. [Figure 3I] 3A to 3C are diagrams illustrating a metal electrode layer forming step in the manufacturing method for the solar cell according to the embodiment. [Figure 4A] 10A to 10C are diagrams illustrating a first semiconductor layer material film forming step and a lift-off layer forming step in a solar cell manufacturing method of a comparative example. [Figure 4B] 1A to 1C are diagrams illustrating a resist formation step in a solar cell manufacturing method according to a comparative example. [Figure 4C] 5A to 5C are diagrams illustrating a first semiconductor layer forming step in the solar cell manufacturing method of the comparative example. [Figure 4D] 1A to 1C are diagrams illustrating a resist removal step in a solar cell manufacturing method according to a comparative example. [Figure 4E] FIG. 4 is a diagram showing a second semiconductor layer material film forming step in the solar cell manufacturing method of the comparative example. [Figure 4F] FIG. 4 is a diagram showing a second semiconductor layer forming step in the solar cell manufacturing method of the comparative example. [Figure 4G] FIG. 13 is a diagram showing a transparent electrode layer material film forming step in the solar cell manufacturing method of the comparative example. [Figure 4H] 11A and 11B are diagrams illustrating a metal electrode layer forming step in a solar cell manufacturing method according to a comparative example. [Figure 4I] FIG. 4 is a diagram showing a transparent electrode layer forming step in a solar cell manufacturing method of a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings. In each drawing, the same or corresponding parts are denoted by the same reference numerals. For convenience, hatching and reference numerals may be omitted, in which case other drawings shall be referred to.
[0017] (Solar Cell) Fig. 1 is a view of the solar cell according to this embodiment as seen from the back surface side, and Fig. 2 is a cross-sectional view of the solar cell along line II-II in Fig. 1. The solar cell 1 shown in Fig. 1 and Fig. 2 is a back electrode type (also called a back contact type or back junction type) heterojunction solar cell.
[0018] Solar cell 1 includes a semiconductor substrate 11 with two main surfaces, and the main surface of semiconductor substrate 11 has a first region 7 and a second region 8. In the following, the main surface of semiconductor substrate 11 that receives light is referred to as the light-receiving surface, and the main surface of semiconductor substrate 11 opposite the light-receiving surface is referred to as the back surface.
[0019] The first region 7 has a so-called comb shape and includes a plurality of finger portions 7f corresponding to the teeth of the comb and busbar portions 7b corresponding to supports for the teeth of the comb. The busbar portions 7b extend in a first direction (X direction) along one side of the semiconductor substrate 11, and the finger portions 7f extend from the busbar portions 7b in a second direction (Y direction) intersecting the first direction.
[0020] Similarly, the second region 8 has a so-called comb shape and has a plurality of finger portions 8f corresponding to the teeth of the comb and a busbar portion 8b corresponding to a support portion of the teeth of the comb. The busbar portion 8b extends in a first direction along one side portion of the semiconductor substrate 11 opposite the other side portion, and the finger portions 8f extend in a second direction from the busbar portion 8b.
[0021] The finger portions 7f and 8f are strip-shaped extending in the second direction and are alternately provided in the first direction. The first region 7 and the second region 8 may be formed in a stripe pattern.
[0022] 2, the solar cell 1 includes a passivation layer 13 and an optical adjustment layer 15, which are formed (deposited, stacked) in this order on the light-receiving surface side of the semiconductor substrate 11. The solar cell 1 also includes a passivation layer 23, a p-type (first conductivity type) semiconductor layer 25, and a first electrode layer 27, which are formed (deposited, stacked) in this order on a portion (mainly, the first region 7) of the back surface side of the semiconductor substrate 11. The solar cell 1 also includes a passivation layer 33, an n-type (second conductivity type) semiconductor layer 35, and a second electrode layer 37, which are formed (deposited, stacked) in this order on another portion (mainly, the second region 8) of the back surface side of the semiconductor substrate 11.
[0023] The semiconductor substrate 11 is formed of a crystalline silicon material such as single crystal silicon or polycrystalline silicon. The semiconductor substrate 11 is, for example, an n-type semiconductor substrate in which a crystalline silicon material is doped with an n-type dopant. The semiconductor substrate 11 may be, for example, a p-type semiconductor substrate in which a crystalline silicon material is doped with a p-type dopant. An example of the n-type dopant is phosphorus (P). An example of the p-type dopant is boron (B). The semiconductor substrate 11 functions as a photoelectric conversion substrate that absorbs incident light from the light-receiving surface side and generates photocarriers (electrons and holes).
[0024] By using crystalline silicon as the material for the semiconductor substrate 11, the dark current is relatively small, and a relatively high output (stable output regardless of illuminance) can be obtained even when the intensity of incident light is low.
[0025] Semiconductor substrate 11 may have a pyramidal fine uneven structure called a texture structure on the light-receiving surface side, which reduces the reflection of incident light on the light-receiving surface and improves the light trapping effect in semiconductor substrate 11.
[0026] Furthermore, the semiconductor substrate 11 may have a pyramidal fine uneven structure, called a texture structure, on the back surface side thereof, which increases the efficiency of collection of light that is not absorbed by the semiconductor substrate 11 and passes through it.
[0027] The passivation layer 13 is formed on the light-receiving surface side of the semiconductor substrate 11. The passivation layer 23 is formed in a first region 7 on the back surface side of the semiconductor substrate 11. The passivation layer 33 is formed in a second region 8 on the back surface side of the semiconductor substrate 11. The passivation layers 13, 23, and 33 are formed of, for example, an intrinsic (i-type) amorphous silicon material. The passivation layers 13, 23, and 33 suppress recombination of carriers generated in the semiconductor substrate 11 and increase the carrier collection efficiency.
[0028] The optical adjustment layer 15 is formed on the passivation layer 13 on the light-receiving surface side of the semiconductor substrate 11. The optical adjustment layer 15 functions as an anti-reflection layer that prevents or suppresses reflection of incident light, and improves the efficiency of light incidence on the semiconductor substrate 11. The optical adjustment layer 15 also functions as a protective layer that protects the light-receiving surface side of the semiconductor substrate 11 and the passivation layer 13. The optical adjustment layer 15 is formed of an insulating material, for example, silicon oxide (SiO), silicon nitride (SiN), or a composite thereof such as silicon oxynitride (SiON).
[0029] The p-type (first conductivity type) semiconductor layer 25 is formed on the passivation layer 23, i.e., in the first region 7 on the back surface side of the semiconductor substrate 11. The p-type semiconductor layer 25 is formed of, for example, an amorphous silicon material. The p-type semiconductor layer 25 is, for example, a p-type semiconductor layer in which an amorphous silicon material is doped with a p-type dopant (for example, the above-mentioned boron (B)).
[0030] The n-type (second conductivity type) semiconductor layer 35 is formed on the passivation layer 33, i.e., in the second region 8 on the back surface side of the semiconductor substrate 11. The n-type semiconductor layer 35 is formed of, for example, an amorphous silicon material. The n-type semiconductor layer 35 is, for example, an n-type semiconductor layer in which an amorphous silicon material is doped with an n-type dopant (for example, the above-mentioned phosphorus (P)).
[0031] The p-type semiconductor layer 25 and the passivation layer 23, and the n-type semiconductor layer 35 and the passivation layer 33 form strips extending in the second direction (Y direction) and are arranged alternately in the first direction (X direction).
[0032] The first electrode layer 27 corresponds to the p-type semiconductor layer 25, specifically, is formed on the p-type semiconductor layer 25 in a first region 7 on the back surface side of the semiconductor substrate 11. The second electrode layer 37 corresponds to the n-type semiconductor layer 35, specifically, is formed on the n-type semiconductor layer 35 in a second region 8 on the back surface side of the semiconductor substrate 11. The first electrode layer 27 has a first transparent electrode layer 28 and a first metal electrode layer 29 formed in this order on the p-type semiconductor layer 25. The second electrode layer 37 has a second transparent electrode layer 38 and a second metal electrode layer 39 formed in this order on the n-type semiconductor layer 35.
[0033] The first transparent electrode layer 28 and the second transparent electrode layer 38 are formed of a transparent conductive material. Examples of the transparent conductive material include ITO (Indium Tin Oxide: a composite oxide of indium oxide and tin oxide). The first metal electrode layer 29 and the second metal electrode layer 39 are formed of a conductive paste material containing, for example, a particulate metal material such as silver, copper, or aluminum, an insulating resin material, and a solvent.
[0034] The first electrode layer 27 and the second electrode layer 37 are in the form of strips extending in the second direction (Y direction) and are arranged alternately in the first direction (X direction). The first electrode layer 27 and the second electrode layer 37 are separated from each other.
[0035] 2, the width of the first transparent electrode layer 28 in the first direction (X direction) is wider than the width of the first metal electrode layer 29 in the first direction. Moreover, the width of the second transparent electrode layer 38 in the first direction is wider than the width of the second metal electrode layer 39 in the first direction.
[0036] The first transparent electrode layer 28 covers the p-type semiconductor layer 25 except for a portion of the first region 7 on the second region 8 side (third region 9: described in detail later). Meanwhile, the second transparent electrode layer 38 covers the entire n-type semiconductor layer 35 in the second region 8. The end face of the n-type semiconductor layer 35 on the first region 7 side and the end face of the second transparent electrode layer 38 on the first region 7 side are aligned in the order of the crystal grain boundaries of the second transparent electrode layer 38, and are continuous with no steps in the stacking direction of these layers (direction intersecting the XY plane).
[0037] Burrs are formed by a lift-off method in a transparent electrode layer formation process described below at the end of the first transparent electrode layer 28 on the second region 8 side, the end of the second transparent electrode layer 38 on the first region 7 side, and the ends of the n-type semiconductor layer 35 and the passivation layer 33 on the first region 7 side. That is, the end of the first transparent electrode layer 28 on the second region 8 side, the end of the second transparent electrode layer 38 on the first region 7 side, and the ends of the n-type semiconductor layer 35 and the passivation layer 33 on the first region 7 side protrude in the stacking direction of these layers (direction intersecting the XY plane).
[0038] Furthermore, as described below, since a lift-off method is used in the transparent electrode layer formation process, the end of the first transparent electrode layer 28 on the second region 8 side and the end of the second transparent electrode layer 38 on the first region 7 side have no traces of erosion by the etching solution or melting by the laser.
[0039] (Comparative Example of Solar Cell Manufacturing Method)
[0040] Hereinafter, a method for manufacturing a solar cell 1X of a comparative example based on the invention of the present inventors will be described with reference to Figs. 4A to 4I. Fig. 4A is a diagram showing a first semiconductor layer material film forming step and a lift-off layer forming step in the method for manufacturing a solar cell of the comparative example, and Fig. 4B is a diagram showing a resist forming step in the method for manufacturing a solar cell of the comparative example. Fig. 4C is a diagram showing a first semiconductor layer forming step in the method for manufacturing a solar cell of the comparative example, and Fig. 4D is a diagram showing a resist removing step in the method for manufacturing a solar cell of the comparative example. Fig. 4E is a diagram showing a second semiconductor layer material film forming step in the method for manufacturing a solar cell of the comparative example, and Fig. 4F is a diagram showing a second semiconductor layer forming step in the method for manufacturing a solar cell of the comparative example. Fig. 4G is a diagram showing a transparent electrode layer material film forming step in the method for manufacturing a solar cell of the comparative example, and Fig. 4H is a diagram showing a metal electrode layer forming step in the method for manufacturing a solar cell of the comparative example. Fig. 4I is a diagram showing a transparent electrode layer forming step in the method for manufacturing a solar cell of the comparative example.
[0041] First, as shown in FIG. 4A, a passivation layer material film 23ZX and a p-type (first conductivity type) semiconductor layer material film 25ZX are sequentially formed (deposited, stacked) on the entire back surface of the semiconductor substrate 11X, for example, using a CVD method (chemical vapor deposition method) (first semiconductor layer material film formation process).
[0042] Also, for example, using a CVD method, a passivation layer 13X is formed (deposited, laminated) on the entire light-receiving surface side of the semiconductor substrate 11X. The order of forming the passivation layer material film 23ZX, the p-type semiconductor layer material film 25ZX, and the passivation layer 13X is not limited. Also, the passivation layer 13X on the light-receiving surface side may be formed in a subsequent second semiconductor layer material film forming process.
[0043] Next, a lift-off layer (sacrificial layer) 41X is formed (deposited, laminated) on the entire back surface of the semiconductor substrate 11X, specifically, on the entire surface of the p-type semiconductor layer material film 25ZX, for example, by using a CVD method. The lift-off layer 41X is made of a material such as silicon oxide (SiO), silicon nitride (SiN), or a compound thereof such as silicon oxynitride (SiON).
[0044] Next, as shown in Figures 4B to 4D, a patterned printing resist 90X is used to remove the lift-off layer 41X, the p-type semiconductor layer material film 25ZX, and the passivation layer material film 23ZX in the second region 8 on the back surface side of the semiconductor substrate 11X, thereby forming a patterned passivation layer 23X, a p-type semiconductor layer 25X, and a lift-off layer 41X in the first region 7.
[0045] 4B, on the rear surface side of the semiconductor substrate 11X, a pattern printing resist 90X is formed on the p-type semiconductor layer material film 25ZX and the lift-off layer 41X in the first region 7 by using a pattern printing method (resist forming process). Also, on the entire surface of the light receiving surface side of the semiconductor substrate 11X, a pattern printing resist 90X is formed by using a pattern printing method (resist forming process).
[0046] Pattern printing is not a printing method in which a pre-patterned resist film (non-patterned resist film) is first formed, as in photolithography, and then processes such as exposure and development are carried out, but rather a printing method in which a patterned resist (printing material) is directly applied to a resist application surface, such as press printing, such as screen printing or gravure printing, or ejection printing, such as inkjet printing.
[0047] In this way, by using a pattern printing resist by pattern printing in the patterning of the p-type semiconductor layer (first patterning), the exposure and development steps can be reduced compared to the case where a photoresist by spin coating (photolithography method) is used, and the manufacturing process of the solar cell can be simplified.
[0048] The pattern printing resist 90X is obtained by printing and curing a printing material containing a resin material and an inorganic material. At this time, due to printing sagging, the thickness of the end of the pattern printing resist 90X in the third region 9, which is a part of the first region 7 on the second region 8 side, becomes thinner than the thickness of the other parts of the pattern printing resist 90 (Point of interest 1: details will be described later).
[0049] 4C, the lift-off layer 41X, the p-type semiconductor layer material film 25ZX, and the passivation layer material film 23ZX in the second region 8 are etched on the rear surface side of the semiconductor substrate 11X using the pattern printing resist 90X as a mask, thereby forming the patterned lift-off layer 41X, the p-type semiconductor layer 25X, and the passivation layer 23X in the first region 7 (first semiconductor layer forming step). An acidic solution such as hydrofluoric acid is used as an etching solution for the lift-off layer 41X, the p-type semiconductor layer material film 25ZX, and the passivation layer material film 23ZX.
[0050] At this time, due to side etching, and further through the thin end of the pattern printing resist 90X in the third region 9, the acid solution as the etching solution corrodes the end of the lift-off layer 41X, and the end of the lift-off layer 41X is altered. The end of the lift-off layer 41X altered in this manner is called an altered portion 43X. Specifically, the altered portion 43X of the lift-off layer 41X in the third region 9 is in a half-etched state and becomes sparse (focus point 2: details will be described later).
[0051] 4D, the pattern printing resist 90X on the back surface side and the light receiving surface side is removed (resist removing step). As an etching solution for the pattern printing resist 90X, for example, an alkaline solution such as an aqueous solution of potassium hydroxide can be used.
[0052] In this way, by using an inexpensive alkaline solution as the solution for removing the pattern printing resist in the patterning of the first conductive type semiconductor layer 25 (first patterning), it is possible to reduce the cost of the solar cell.
[0053] In the first semiconductor layer formation step, the p-type semiconductor layer 25X may be patterned so that part or all of the passivation layer material film 23ZX in the second region 8 on the back surface side of the semiconductor substrate 11 remains.
[0054] Next, both sides of the semiconductor substrate 11X are cleaned (first cleaning step). In the first cleaning step, for example, ozone treatment is performed, followed by hydrofluoric acid treatment. The hydrofluoric acid treatment includes not only treatment with hydrofluoric acid, but also treatment with a mixture of hydrofluoric acid and another type of acid (for example, hydrochloric acid in the first cleaning step).
[0055] Next, as shown in FIG. 4E, for example, using a CVD method, a passivation layer material film 33ZX and an n-type (second conductivity type) semiconductor layer material film 35ZX are formed (deposited, stacked) in sequence over the entire back surface side of the semiconductor substrate 11X, specifically on the lift-off layer 41X in the first region 7 and in the second region 8 (second semiconductor layer material film formation process).
[0056] Next, as shown in FIG. 4F, a lift-off method using a lift-off layer (sacrificial layer) is used to remove the passivation layer material film 33ZX and the n-type semiconductor layer material film 35ZX in the first region 7 on the back surface side of the semiconductor substrate 11X, thereby forming a patterned passivation layer 33X and an n-type semiconductor layer 35X in the second region 8 (second semiconductor layer formation process).
[0057] Specifically, by removing the lift-off layer 41X, the passivation layer material film 33ZX and the n-type semiconductor layer material film 35ZX on the lift-off layer 41X are removed to form the passivation layer 33X and the n-type semiconductor layer 35X in the second region 8. As a removal solution for the lift-off layer 41X, for example, an acidic solution such as hydrofluoric acid is used.
[0058] In this way, by employing a lift-off method using a lift-off layer (sacrificial layer) in the patterning (second patterning) of the n-type semiconductor layer 35X, it is possible to simplify the manufacturing process of the solar cell.
[0059] Here, the lift-off layer 41X is removed by peeling it off into a film. At this time, the altered portion 43X of the lift-off layer 41X in the third region 9 is altered (semi-etched) and is in a porous state, so it remains without being peeled off into a film. Therefore, the passivation layer 33X and the n-type semiconductor layer 35X remain on the altered portion 43X of the lift-off layer 41X in the third region (focus point 3: details will be described later).
[0060] In the first semiconductor layer forming step, if the entire passivation layer material film 23ZX remains in the second region 8 on the back surface side of the semiconductor substrate 11X, the second semiconductor layer material film forming step and the second semiconductor layer forming step do not require lamination (deposition) of the passivation layer material film, but only patterning of the n-type semiconductor layer 35X. In the first semiconductor layer forming step, if a portion of the passivation layer material film 23ZX remains in the second region 8 on the back surface side of the semiconductor substrate 11X, the second semiconductor layer material film forming step and the second semiconductor layer forming step require lamination (deposition) of the passivation layer material film by the amount removed, and patterning of the passivation layer and the n-type semiconductor layer 35X.
[0061] Next, as shown in FIG. 4G, an optical adjustment layer 15X is formed over the entire light-receiving surface side of the semiconductor substrate 11X, that is, on the passivation layer 13, by using, for example, a CVD method.
[0062] Next, as shown in FIGS. 4G and 4I, a first electrode layer 27X and a second electrode layer 37X are formed on the back surface side of the semiconductor substrate 11X (electrode layer forming step).
[0063] Specifically, as shown in FIG. 4G, a PVD method (physical vapor deposition method) such as a sputtering method is used to form (deposit, laminate) a transparent electrode layer material film 28ZX on and across the p-type semiconductor layer 25X and the n-type semiconductor layer 35X on the back surface side of the semiconductor substrate 11X (transparent electrode layer material film formation process).
[0064] Then, as shown in FIG. 4H, for example, using a pattern printing method or a coating method, a first metal electrode layer 29X is formed on the p-type semiconductor layer 25X via the transparent electrode layer material film 28ZX, and a second metal electrode layer 39X is formed on the n-type semiconductor layer 35X via the transparent electrode layer material film 28ZX (metal electrode layer formation process).
[0065] Thereafter, as shown in Fig. 4I, the transparent electrode layer material film 28ZX is patterned using the first metal electrode layer 29X and the second metal electrode layer 39X as a mask to form the first transparent electrode layer 28X and the second transparent electrode layer 38X that are separated from each other (transparent electrode layer forming step). As an etching solution for the transparent electrode layer material film 28ZX, for example, hydrochloric acid or a ferric chloride aqueous solution is used.
[0066] In this manner, in patterning the transparent electrode layers 28X, 38X, the transparent electrode layer material film 28ZX is patterned using the metal electrode layers 29X, 39X as a mask to form transparent electrode layers 28X, 38X that are separated from each other. This eliminates the need to use a resist as a mask by photolithography or the like, and allows for simplification of the solar cell manufacturing process.
[0067] Through the above steps, a back electrode type solar cell 1X of the comparative example shown in FIG. 4I is obtained.
[0068] In the manufacturing method of this comparative example, since a wet etching method is used in the transparent electrode layer formation step, it is necessary to form an amorphous transparent electrode layer that is easily etched as the transparent electrode layer. However, since the contact property of such a transparent electrode layer is low and the bulk resistance of the transparent electrode layer is high, there is a problem that the performance of the solar cell cannot be sufficiently improved.
[0069] In this regard, the inventor(s) of the present application pay attention to the above-mentioned points 1 to 3. That is, the inventor(s) of the present application found that, when a pattern printing resist by a pattern printing method is used in the first patterning, the end of the pattern printing resist becomes thin due to printing sagging, and therefore the etching solution corrodes the end of the lift-off layer through the thin end of the pattern printing resist, causing the end of the lift-off layer to become half-etched and change into a porous state, and the end of the lift-off layer remains in a film shape without being peeled off in the lift-off process.
[0070] The present inventors then discovered that in patterning the transparent electrode layer, the transparent electrode layer can be patterned by a lift-off method that utilizes the residue of this lift-off layer, i.e., the residue of the lift-off layer at the boundary between the p region and the n region.
[0071] In the lift-off method, the lift-off layer is removed to peel off the transparent electrode layer thereon, so that even if a crystalline transparent electrode layer that cannot be easily etched is formed, the transparent electrode layer can be patterned. Therefore, the contact property of the transparent electrode layer can be improved and the bulk resistance of the transparent electrode layer can be reduced. Therefore, the performance of the solar cell can be improved.
[0072] (Method of manufacturing solar cell according to the present embodiment) Hereinafter, with reference to FIG. 3A to FIG. 3I, a method for manufacturing the solar cell 1 of the present embodiment shown in FIG. 1 and FIG. 2 will be described. FIG. 3A is a diagram showing a first semiconductor layer material film forming step and a lift-off layer forming step in the method for manufacturing a solar cell according to the present embodiment, and FIG. 3B is a diagram showing a resist forming step in the method for manufacturing a solar cell according to the present embodiment. FIG. 3C is a diagram showing a first semiconductor layer forming step in the method for manufacturing a solar cell according to the present embodiment, and FIG. 3D is a diagram showing a resist removing step in the method for manufacturing a solar cell according to the present embodiment. FIG. 3E is a diagram showing a second semiconductor layer material film forming step in the method for manufacturing a solar cell according to the present embodiment, and FIG. 3F is a diagram showing a second semiconductor layer forming step in the method for manufacturing a solar cell according to the present embodiment. FIG. 3G is a diagram showing a transparent electrode layer material film forming step in the method for manufacturing a solar cell according to the present embodiment, and FIG. 3H is a diagram showing a transparent electrode layer forming step in the method for manufacturing a solar cell according to the present embodiment. FIG. 3I is a diagram showing a metal electrode layer forming step in the method for manufacturing a solar cell according to the present embodiment.
[0073] First, as shown in FIG. 3A, a passivation layer material film 23Z and a p-type (first conductivity type) semiconductor layer material film 25Z are formed (deposited, stacked) in sequence on the entire back surface of the semiconductor substrate 11, for example, by using a CVD method (first semiconductor layer material film formation process).
[0074] Further, for example, by using a CVD method, a passivation layer 13 is formed (deposited, laminated) on the entire surface of the light-receiving surface side of the semiconductor substrate 11. The order of forming the passivation layer material film 23Z and the p-type semiconductor layer material film 25Z, and the passivation layer 13, is not limited. The passivation layer 13 on the light-receiving surface side may be formed in a subsequent second semiconductor layer material film forming process.
[0075] Next, for example, by using a CVD method, a lift-off layer (sacrificial layer) 41 is formed (deposited, laminated) on the entire back surface of the semiconductor substrate 11, specifically, on the entire surface of the p-type semiconductor layer material film 25Z. The lift-off layer 41 is made of a material such as silicon oxide (SiO), silicon nitride (SiN), or a compound thereof such as silicon oxynitride (SiON).
[0076] Next, as shown in Figures 3B to 3D, a pattern printing resist 90 is used to remove the lift-off layer 41, the p-type semiconductor layer material film 25Z, and the passivation layer material film 23Z in the second region 8 on the back surface side of the semiconductor substrate 11, thereby forming a patterned passivation layer 23, the p-type semiconductor layer 25, and the lift-off layer 41 in the first region 7.
[0077] 3B, on the back surface side of the semiconductor substrate 11, a pattern printed resist 90 is formed on the p-type semiconductor layer material film 25Z and the lift-off layer 41 in the first region 7 by using a pattern printing method (resist forming step). Also, on the entire surface of the light receiving surface side of the semiconductor substrate 11, a pattern printed resist 90 is formed by using a pattern printing method (resist forming step).
[0078] The pattern printing resist 90 is obtained by printing and curing a printing material containing a resin material and an inorganic material. At this time, due to printing sagging, the thickness of the end of the pattern printing resist 90 in the third region 9, which is a part of the first region 7 on the second region 8 side, becomes thinner than the thickness of the other parts of the pattern printing resist 90.
[0079] 3C, the lift-off layer 41, the p-type semiconductor layer material film 25Z, and the passivation layer material film 23Z in the second region 8 are etched on the back surface side of the semiconductor substrate 11 using the pattern printing resist 90 as a mask, thereby forming the patterned lift-off layer 41, the p-type semiconductor layer 25, and the passivation layer 23 in the first region 7 (first semiconductor layer formation step). As an etching solution for the lift-off layer 41, the p-type semiconductor layer 25, and the passivation layer 23, for example, an acidic solution such as hydrofluoric acid is used.
[0080] At this time, due to the side etching, the acid solution as the etching solution corrodes the edge of the lift-off layer 41 through the thin edge of the pattern printing resist 90 in the third region 9, and the edge of the lift-off layer 41 is altered. The edge of the lift-off layer 41 altered in this manner is called an altered portion 43. Specifically, the altered portion 43 of the lift-off layer 41 in the third region 9 is in a half-etched state and is in a sparse state.
[0081] 3D, the pattern printing resist 90 on the back surface side and the light receiving surface side is removed (resist removing step). As an etching solution for the pattern printing resist 90, for example, an alkaline solution such as an aqueous solution of potassium hydroxide can be used.
[0082] In the first semiconductor layer formation step, the p-type semiconductor layer 25 may be patterned so that part or all of the passivation layer material film 23Z in the second region 8 on the back surface side of the semiconductor substrate 11 remains.
[0083] Next, both sides of the semiconductor substrate 11 are cleaned (first cleaning step). In the first cleaning step, for example, ozone treatment is performed, followed by hydrofluoric acid treatment. The hydrofluoric acid treatment includes not only treatment with hydrofluoric acid, but also treatment with a mixture of hydrofluoric acid and another type of acid (for example, hydrochloric acid in the first cleaning step).
[0084] Next, as shown in FIG. 3E, for example, using a CVD method, a passivation layer material film 33Z and an n-type (second conductivity type) semiconductor layer material film 35Z are formed (deposited, stacked) in sequence over the entire back surface side of the semiconductor substrate 11, specifically on the lift-off layer 41 in the first region 7 and in the second region 8 (second semiconductor layer material film formation process).
[0085] Next, as shown in FIG. 3F, a lift-off method using a lift-off layer (sacrificial layer) is used to remove the passivation layer material film 33Z and the n-type semiconductor layer material film 35Z in the first region 7 on the back surface side of the semiconductor substrate 11, thereby forming a patterned passivation layer 33 and an n-type semiconductor layer 35 in the second region 8 (second semiconductor layer formation process).
[0086] Specifically, by removing the lift-off layer 41, the passivation layer material film 33Z and the n-type semiconductor layer material film 35Z on the lift-off layer 41 are removed, and the passivation layer 33 and the n-type semiconductor layer 35 are formed in the second region 8. As a removal solution for the lift-off layer 41, an acidic solution such as hydrofluoric acid is used, for example.
[0087] Here, the lift-off layer 41 is removed by peeling it off in the form of a film. At this time, the altered portion 43 of the lift-off layer 41 in the third region 9 is altered (semi-etched) and is in a porous state, so it remains without being peeled off in the form of a film. Therefore, the passivation layer 33 and the n-type semiconductor layer 35 remain on the altered portion 43 of the lift-off layer 41 in the third region.
[0088] In addition, in the first semiconductor layer forming step, if the entire passivation layer material film 23Z remains in the second region 8 on the back surface side of the semiconductor substrate 11, in the second semiconductor layer material film forming step and the second semiconductor layer forming step, lamination (deposition) of the passivation layer material film is not performed, and patterning of the n-type semiconductor layer 35 may be performed. In addition, in the first semiconductor layer forming step, if a portion of the passivation layer material film 23Z remains in the second region 8 on the back surface side of the semiconductor substrate 11, in the second semiconductor layer material film forming step and the second semiconductor layer forming step, lamination (deposition) of the passivation layer material film is performed by the amount that has been removed, and patterning of the passivation layer and the n-type semiconductor layer 35 may be performed.
[0089] Next, as shown in FIG. 3G, optical adjustment layer 15 is formed over the entire light-receiving surface side of semiconductor substrate 11, that is, on passivation layer 13, by using, for example, a CVD method.
[0090] Next, as shown in FIGS. 3H and 3I, a first electrode layer 27 and a second electrode layer 37 are formed on the back surface side of the semiconductor substrate 11 (electrode layer forming step).
[0091] Specifically, as shown in FIG. 4G, a transparent electrode layer material film 28Z is formed (deposited, laminated) on and across the p-type semiconductor layer 25 and the n-type semiconductor layer 35 on the back surface side of the semiconductor substrate 11 using a PVD method such as a sputtering method (transparent electrode layer material film formation process).
[0092] 3H, the altered portion 43 of the lift-off layer 41 in the third region 9 is removed using a lift-off method to remove a portion of the n-type semiconductor layer 35 on the altered portion 43 of the lift-off layer 41 in the third region 9, forming the first transparent electrode layer 28 in the first region 7 excluding the third region 9, and forming the second transparent electrode layer 38 in the second region 8 (transparent electrode layer forming step). As a solution for removing the altered portion 43 of the lift-off layer 41, an acidic solution such as hydrofluoric acid is used.
[0093] The acid concentration of the etching solution used in the lift-off method in the transparent electrode layer material film forming step is higher than the acid concentration of the etching solution used in the lift-off method in the second semiconductor layer forming step. For example, the acid concentration of the etching solution used in the lift-off method in the second semiconductor layer forming step is 5% or more and 8% or less, whereas the acid concentration of the etching solution used in the lift-off method in the transparent electrode layer material film forming step is 10% or more and 16% or less. This allows the altered portion 43 of the lift-off layer 41 in the third region 9, which was not peeled off in a film form in the lift-off method in the second semiconductor layer forming step, to be dissolved and removed rather than peeled off.
[0094] Thereafter, for example, by using a pattern printing method or a coating method, the first metal electrode layer 29 is formed on the first transparent electrode layer 28, and the second metal electrode layer 39 is formed on the second transparent electrode layer 38 (metal electrode layer forming step).
[0095] Through the above steps, the back electrode type solar cell 1 of this embodiment shown in Figs. 1 and 2 is obtained.
[0096] As described above, according to the solar cell manufacturing method of the present embodiment, the transparent electrode layers 28, 38 are patterned using a lift-off method that utilizes the altered portion 43 at the end of the lift-off layer 41 that remains in the patterning of the semiconductor layer using the lift-off method. In the lift-off method, the altered portion 43 of the lift-off layer 41 is removed to peel off the transparent electrode layers 28, 38 thereon, so that even if the transparent electrode layers 28, 38 are formed as crystalline layers that cannot be easily etched, the transparent electrode layers 28, 38 can be patterned. Therefore, the contact property of the transparent electrode layers 28, 38 can be improved, and the bulk resistance of the transparent electrode layers 28, 38 can be reduced. Therefore, the performance of the solar cell 1 can be improved.
[0097] According to the manufacturing method of the solar cell of this embodiment, it is possible to obtain a solar cell 1 in which the entire n-type (second conductive type) semiconductor layer 35 in the second region 8 is covered with the second transparent electrode layer 38. In other words, it is possible to obtain a solar cell 1 in which the end face of the n-type semiconductor layer 35 on the first region 7 side and the end face of the second transparent electrode layer 38 on the first region 7 side are aligned in the order of the crystal grain boundaries of the second transparent electrode layer 38. As a result, compared to the solar cell 1X of the comparative example, it is possible to increase the coverage area of the semiconductor layers 25, 35 with the transparent electrode layers 28, 38 and increase the current extraction area (effective area) with the transparent electrode layers 28, 38. Therefore, it is possible to improve the output performance of the solar cell 1.
[0098] Furthermore, according to the solar cell manufacturing method of this embodiment, since the lift-off method is used in the transparent electrode layer formation step, it is possible to obtain a solar cell 1 that has no erosion marks caused by the etching solution or melting marks caused by the laser on the end of the first transparent electrode layer 28 on the second region 8 side and the end of the second transparent electrode layer 38 on the first region 7 side. This makes it possible to prevent deterioration in the quality of the end of the transparent electrode layer due to erosion caused by etching and reduction in the lifetime of the irradiated region due to laser irradiation, and enables the solar cell 1 to have a high output.
[0099] Although the embodiment of the present invention has been described above, the present invention is not limited to the above-described embodiment, and various changes and modifications are possible. [Explanation of symbols]
[0100] 1,1X solar cell 7 First area 7b, 8b Busbar section 7f,8f Finger section 8 Second area 9 Third area 11,11X Semiconductor substrate 13,13X Passivation Layer 15,15X optical adjustment layer 23,23X Passivation Layer 23Z, 23ZX Passivation layer material film 25, 25X p-type semiconductor layer (first conductive type semiconductor layer) 25Z, 25ZX p-type semiconductor layer material film (first conductive type semiconductor layer material film) 27,27X 1st electrode layer 28,28X 1st transparent electrode layer 29,29X 1st metal electrode layer 33,33X Passivation layer 33Z, 33ZX Passivation layer material film 35, 35X n-type semiconductor layer (second conductive type semiconductor layer) 35Z, 35ZX n-type semiconductor layer material film (second conductive type semiconductor layer material film) 37,37X 2nd electrode layer 38,38X 2nd transparent electrode layer 39,39X 2nd metal electrode layer 41,41X Lift-off layer 43,43X Deformed part 90,90X Pattern Printing Resist
Claims
1. A method for manufacturing a back electrode type solar cell comprising: a semiconductor substrate; a first conductivity type semiconductor layer disposed in a first region which is a part of a back surface side of the semiconductor substrate; a second conductivity type semiconductor layer disposed in a second region which is another part of the back surface side of the semiconductor substrate; a first transparent electrode layer and a first metal electrode layer corresponding to the first conductivity type semiconductor layer; and a second transparent electrode layer and a second metal electrode layer corresponding to the second conductivity type semiconductor layer, The first conductive type semiconductor layer is a p-type semiconductor layer, and the second conductive type semiconductor layer is an n-type semiconductor layer, a first semiconductor layer material film forming step of forming a first conductive type semiconductor layer material film and a lift-off layer material film on the back surface side of the semiconductor substrate; a first semiconductor layer forming step of patterning the first conductive type semiconductor layer material film and the lift-off layer material film using a printing resist to form the first conductive type semiconductor layer and the lift-off layer in the first region, wherein an end of the lift-off layer in a third region, which is a part of the first region on the second region side, is altered by an acidic etching solution to become an altered portion; a second semiconductor layer material film forming step of forming a second conductive type semiconductor layer material film on the back surface side of the semiconductor substrate; a second semiconductor layer forming step of forming a second conductive type semiconductor layer in the second region by removing the lift-off layer using a lift-off method, wherein an altered portion of the lift-off layer remains in the third region, and the second conductive type semiconductor layer remains on the altered portion of the lift-off layer in the third region; a transparent electrode layer material film forming step of forming a transparent electrode layer material film on the back surface side of the semiconductor substrate; a transparent electrode layer forming step of removing a part of the second conductive type semiconductor layer on the altered part of the lift-off layer in the third region by using a lift-off method, thereby forming the first transparent electrode layer and the second transparent electrode layer in the first region and the second region excluding the third region; a metal electrode layer forming step of forming the first metal electrode layer and the second metal electrode layer on the first transparent electrode layer and the second transparent electrode layer; A method for manufacturing a solar cell, comprising:
2. In the printed resist used in the first semiconductor layer formation step, a thickness of an end portion of the printed resist in the third region is thinner than a thickness of another portion of the printed resist; In the first semiconductor layer forming step, the etching solution corrodes the edge of the lift-off layer in the third region through the thin edge of the printing resist. The method for producing the solar cell according to claim 1 .
3. 3. The method for producing a solar cell according to claim 1, wherein an acid concentration of an etching solution used in the lift-off method in the transparent electrode layer material film forming step is higher than an acid concentration of an etching solution used in the lift-off method in the second semiconductor layer forming step.
4. A back electrode type solar cell comprising: a semiconductor substrate; a first conductive type semiconductor layer disposed in a first region which is a part of a back surface side of the semiconductor substrate; a second conductive type semiconductor layer disposed in a second region which is another part of the back surface side of the semiconductor substrate; a first transparent electrode layer and a first metal electrode layer corresponding to the first conductive type semiconductor layer; and a second transparent electrode layer and a second metal electrode layer corresponding to the second conductive type semiconductor layer, The first conductive type semiconductor layer is a p-type semiconductor layer, and the second conductive type semiconductor layer is an n-type semiconductor layer, the entire second conductive type semiconductor layer in the second region is covered with the second transparent electrode layer; Solar cell.
5. 5. The solar cell according to claim 4, wherein an end face of the second conductive type semiconductor layer facing the first region and an end face of the second transparent electrode layer facing the first region are aligned in the order of the crystal grain boundaries of the second transparent electrode layer.
6. The solar cell according to claim 4 or 5, wherein the end of the first transparent electrode layer on the second region side and the end of the second transparent electrode layer on the first region side have no traces of erosion by an etching solution and no traces of melting by a laser.
Citation Information
Patent Citations
Photosensor and its manufacturing method
JP2005101240A
Photoelectric conversion element and method for manufacturing the same
JP2014022544A
Photoelectric conversion element and method of manufacturing photoelectric conversion element
JP2014067888A
Solar battery cell, and method for manufacturing solar battery cell
JP2018050006A
Manufacturing method of solar cell
JP2022097253A