Method for manufacturing electrode body for non-aqueous secondary battery

By employing a solvent with higher solubility for the binder in the adhesive layer, the method strengthens the bond between the positive electrode layer and the solid electrolyte layer, addressing the weakness of existing bonds and enhancing battery performance.

JP2024140119APending Publication Date: 2024-10-10HONDA MOTOR CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023051118
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

The bond between the positive electrode layer and the solid electrolyte layer in non-aqueous secondary batteries is weak and discontinuous, necessitating improved mechanical bonding strength to enhance stability and durability.

Method used

A manufacturing method involving the use of a solvent with higher solubility for the binder in the adhesive layer, promoting binder elution and migration to form a continuous and stronger bond between the positive electrode layer and the solid electrolyte layer, utilizing a solvent with a lower boiling point to fill voids and prevent interface void generation.

Benefits of technology

The method enhances the bondability and continuity between the positive electrode layer and the solid electrolyte layer, reducing interface resistance and improving battery capacity and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140119000001_ABST
    Figure 2024140119000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing an electrode body for a non-aqueous secondary battery, which can make the bonding between a positive electrode layer and a solid electrolyte layer more continuous or stronger.SOLUTION: A method for manufacturing an electrode body for a non-aqueous secondary battery includes a positive electrode layer solution preparation step of preparing a positive electrode layer solution containing a positive electrode active material, a binder, and a first solvent, a positive electrode layer formation step of forming a positive electrode layer using the positive electrode layer solution, an electrolyte layer formation step of forming an electrolyte layer containing a solid electrolyte, an adhesive layer solution preparation step of preparing an adhesive layer solution containing a solid electrolyte and a second solvent, an adhesive layer formation step of forming an adhesive layer using the adhesive layer solution, and a lamination step of laminating the positive electrode layer, the adhesive layer, and the electrolyte layer in this order, and the second solvent has a higher solubility in the binder than the first solvent.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an electrode assembly for a non-aqueous secondary battery. [Background technology]

[0002] In recent years, research and development into secondary batteries that contribute to energy efficiency has been conducted in order to ensure that more people have access to affordable, reliable, sustainable and advanced energy.

[0003] Known examples of such secondary batteries include non-aqueous secondary batteries such as lithium ion secondary batteries in which an electrolyte layer is disposed between a positive electrode layer and a negative electrode layer. In non-aqueous secondary batteries, the interface between the electrode layer and the electrolyte layer is a solid contact, and the formation of an ion path is an important issue. However, the mechanical bonding strength of the interface is low, and since it is a dissimilar material bond, it is necessary to improve the strength against potentially occurring interface distortion. As a technique for maintaining the stability of the interface between the electrode layer and the electrolyte layer, a technique for crosslinking the binder of the electrode layer with a crosslinking agent is known (see, for example, Patent Document 1).

[0004] In addition to the above, a technology for forming a good interface between solid particles is known that relates to an all-solid-state secondary battery having an intermediate layer containing a compound such as Li2Ti2O5 between a solid electrolyte layer and a negative electrode active material layer (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2014-116164 A [Patent Document 2] JP 2016-212991 A Summary of the Invention [Problem to be solved by the invention]

[0006] In the technology disclosed in Patent Document 1, the positive electrode and the negative electrode contain a non-polar binder, and the binder is cross-linked by a cross-linking agent. The positive electrode and the negative electrode are then bound to the electrolyte layer by the non-polar binder. In the technology disclosed in Patent Document 2, an intermediate layer is disposed between the solid electrolyte layer and the negative electrode active material layer, and a good interface between the negative electrode active material layer and the solid electrolyte layer is formed. On the other hand, it is desired to make the bond between the positive electrode layer and the solid electrolyte layer more continuous or stronger.

[0007] The present invention has been made in view of the above, and has an object to provide a method for manufacturing an electrode body for a nonaqueous secondary battery, which can make the bonding between the positive electrode layer and the solid electrolyte layer more continuous or stronger. [Means for solving the problem]

[0008] (1) A method for producing an electrode body for a non-aqueous secondary battery, the method comprising: a positive electrode layer solution preparation step of preparing a positive electrode layer solution containing a positive electrode active material, a binder, and a first solvent; a positive electrode layer formation step of forming a positive electrode layer using the positive electrode layer solution; an electrolyte layer formation step of forming an electrolyte layer containing a solid electrolyte; an adhesive layer solution preparation step of preparing an adhesive layer solution containing a solid electrolyte and a second solvent; an adhesive layer formation step of forming an adhesive layer using the adhesive layer solution; and a lamination step of laminating the positive electrode layer, the adhesive layer, and the electrolyte layer in this order, wherein the second solvent has a higher solubility for the binder than the first solvent.

[0009] According to the invention of (1), the amount of binder dissolved at the interface between the positive electrode layer and the adhesive layer can be increased, thereby providing a method for producing an electrode body for a non-aqueous secondary battery that can make the bond between the positive electrode layer and the solid electrolyte layer more continuous or stronger.

[0010] (2) The method for producing an electrode body for a non-aqueous secondary battery according to (1), wherein the second solvent has a boiling point lower than that of the first solvent.

[0011] According to the invention of (2), after the voids at the interface between the positive electrode layer and the adhesive layer are filled with the binder, the second solvent evaporates smoothly, so that the interface is easily filled with the binder and voids are unlikely to occur at the interface, thereby further improving the bonding between the positive electrode layer and the adhesive layer.

[0012] (3) The method for producing an electrode body for a non-aqueous secondary battery according to (1) or (2), wherein in the lamination step, when the positive electrode layer and the adhesive layer are laminated, the second solvent is present at least in the adhesive layer.

[0013] According to the invention of (3), the anchor effect of the binder contained in the positive electrode layer is exerted, and the bond between the positive electrode layer and the adhesive layer can be further improved.

[0014] (4) The method for producing an electrode body for a non-aqueous secondary battery according to any one of (1) to (3), wherein the adhesive layer solution does not contain a binder.

[0015] According to the invention of (4), the dissolution of the binder contained in the positive electrode layer by the second solvent and the penetration into the adhesive layer are further promoted, so that the bonding strength between the positive electrode layer and the adhesive layer can be further improved.

[0016] (5) The method for producing an electrode body for a nonaqueous secondary battery according to any one of (1) to (3), wherein the adhesive layer solution contains the same type of binder as that contained in the positive electrode layer solution.

[0017] According to the invention of (5), the compatibility between the binder contained in the positive electrode layer and the binder contained in the adhesive layer is improved, so that the positive electrode layer and the adhesive layer can be made more continuous or stronger. [Brief description of the drawings]

[0018] [Figure 1] 4A and 4B are diagrams illustrating a state in which a positive electrode layer and an adhesive layer according to the embodiment are laminated. [Diagram 2] 4A and 4B are diagrams illustrating a bonding state between a positive electrode layer and an adhesive layer according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The method for manufacturing an electrode body for a non-aqueous secondary battery according to this embodiment is a method for manufacturing an electrode body for a non-aqueous secondary battery including at least a positive electrode layer, an electrolyte layer, and an adhesive layer laminated between these layers that constitute the non-aqueous secondary battery. The non-aqueous secondary battery includes at least a negative electrode layer in addition to the above-mentioned respective layers. The negative electrode layer is laminated so as to be in contact with the electrolyte layer.

[0020] [Non-aqueous secondary battery] Examples of the non-aqueous secondary battery according to this embodiment include a semi-solid lithium-ion battery having a gel-like electrolyte, an all-solid lithium-ion battery having a solid electrolyte, and the like. As the non-aqueous secondary battery, in particular, a semi-solid lithium metal battery or an all-solid lithium metal battery using lithium metal for the negative electrode is preferable. These solid batteries have relatively large expansion and contraction due to charge and discharge, and a stronger bonding strength between the positive electrode layer and the solid electrolyte layer is desired. According to the method for manufacturing an electrode body for a non-aqueous secondary battery according to this embodiment, the bonding between the positive electrode layer and the solid electrolyte layer can be made more continuous or stronger.

[0021] (Positive electrode layer) The positive electrode layer has a positive electrode active material layer and a positive electrode current collector. In this embodiment, the positive electrode active material layers are laminated on both sides of the positive electrode current collector, and adhesive layers are further laminated on the outer surfaces of the respective positive electrode active material layers.

[0022] The positive electrode active material layer is a layer that essentially contains a positive electrode active material. The positive electrode active material is not particularly limited, and a material known as a positive electrode active material for a non-aqueous secondary battery can be used. Examples of the positive electrode active material include ternary positive electrode materials such as LiCoO2, LiNiO2, NCM (Li(NixCoyMnz)O2, (0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1)), layered positive electrode active material particles such as LiVO2, LiCrO2, spinel-type positive electrode active materials such as LiMn2O4, Li(Ni 0.25 Mn 0.75 )2O4, LiCoMnO4, Li2NiMn3O8, olivine-type positive electrode active materials such as LiCoPO4, LiMnPO4, LiFePO4, and the like can be used.

[0023] The positive electrode active material layer contains a binder in addition to the positive electrode active material. It may further contain a solid electrolyte, a conductive assistant, etc. The solid electrolyte, the conductive assistant, the binder, etc. are not particularly limited, and any substance known as an electrode material for a non-aqueous secondary battery can be used.

[0024] The binder is not particularly limited, but is preferably a particulate or fibrous binder that does not prevent bulk contact between particles. Examples of the binder include polyvinylidene fluoride (PVdF), polymethyl methacrylate (PMMA), polyisobutene (PIB), styrene butadiene rubber (SBR), polyethylene-vinyl acetate copolymer (PEVA), nitrile rubber (NBR), and hydrogenated nitrile rubber (HNBR). These may be used alone or in combination of two or more.

[0025] The positive electrode current collector is not particularly limited, and may be any material known as a positive electrode current collector for non-aqueous secondary batteries. Examples of the positive electrode current collector include metal foils such as stainless steel (SUS) foil and aluminum (Al) foil.

[0026] (Adhesive layer) The adhesive layer is a layer laminated between the positive electrode layer and the electrolyte layer. The adhesive layer can make the bond between the positive electrode layer and the electrolyte layer more continuous or stronger. The adhesive layer is a layer that essentially contains a solid electrolyte. When the adhesive layer contains a solid electrolyte, the ion conductivity between the positive electrode layer and the electrolyte layer can be improved. The solid electrolyte contained in the adhesive layer is not particularly limited, and a substance known as an electrode material for a non-aqueous secondary battery can be applied.

[0027] The adhesive layer may contain a binder. When the adhesive layer contains a binder, the type of the binder is preferably the same as that of the binder contained in the positive electrode layer. The origin of the binder contained in the adhesive layer may be that the binder contained in the adhesive layer solution described later is contained in the adhesive layer, or that the binder contained in the positive electrode layer is moved and is contained in the adhesive layer.

[0028] (Negative electrode layer) The negative electrode layer includes a negative electrode active material layer and a negative electrode current collector. In the present embodiment, the negative electrode active material layer is laminated so as to be in contact with the electrolyte layer, and the negative electrode current collector is laminated on the outermost layer of the laminate.

[0029] The negative electrode active material layer is a layer that essentially contains a negative electrode active material. The negative electrode active material is not particularly limited, and any material known as a negative electrode active material for non-aqueous secondary batteries can be used. As the negative electrode active material, for example, lithium titanate (Li4Ti5O 12 transition metal oxides such as TiO2, Nb2O3, and WO3; metal sulfides, metal nitrides, carbon materials such as graphite, soft carbon, and hard carbon; silicon-based materials such as silicon elemental, silicon alloys, and silicon compounds; and lithium metal, lithium alloys, and metallic indium.

[0030] The negative electrode active material layer may further contain, in addition to the negative electrode active material, a solid electrolyte, a conductive assistant, a binder, etc. The solid electrolyte, the conductive assistant, the binder, etc. are not particularly limited, and any substance known as an electrode material for a nonaqueous secondary battery can be used.

[0031] The negative electrode current collector is not particularly limited, and may be any material known as a negative electrode current collector for non-aqueous secondary batteries. Examples of the negative electrode current collector include metal foils such as copper (Cu) foil, stainless steel (SUS) foil, and aluminum (Al) foil.

[0032] (electrolyte layer) The electrolyte layer is a layer that essentially contains a solid electrolyte. The electrolyte layer may contain a binder and the like in addition to the above. In this embodiment, the electrolyte layer is laminated between the positive electrode layer and the adhesive layer and the negative electrode layer.

[0033] The solid electrolyte is not particularly limited, but examples thereof include sulfide-based solid electrolytes, oxide-based solid electrolytes, nitride-based solid electrolytes, and halide-based solid electrolytes.

[0034] <Method of manufacturing electrode body for non-aqueous secondary battery> The method for producing an electrode body for a non-aqueous secondary battery includes a positive electrode layer solution preparation step, a positive electrode layer forming step, an electrolyte layer forming step, an adhesive layer solution preparation step, an adhesive layer forming step, and a lamination step.

[0035] There is no restriction on the order in which the above steps are performed, except that the forming step for each layer is performed after the solution preparation step for each layer, and the lamination step is performed after the forming step for each layer. For example, each layer may be formed independently and then the lamination step may be performed, or one layer may be formed and then another layer may be formed on the layer.

[0036] In the positive electrode layer solution preparation step, a positive electrode layer solution is prepared in which each component contained in the positive electrode active material layer is dissolved and / or dispersed in a first solvent. The first solvent is a solvent in which the solubility of the binder contained in the positive electrode layer is lower than that of a second solvent described below.

[0037] In the adhesive layer solution preparation step, an adhesive layer solution is prepared in which each component contained in the adhesive layer is dissolved and / or dispersed in a second solvent. The second solvent is a solvent in which the solubility of the binder contained in the positive electrode layer is higher than that in the first solvent.

[0038] The first solvent and the second solvent are not particularly limited as long as they have affinity with the materials contained in the positive electrode layer solution and the adhesive layer solution, and examples thereof include aliphatic hydrocarbons, aromatic hydrocarbons, esters, ethers, ketones, nitriles, etc. The first solvent and the second solvent can be selected based on the difference in solubility with respect to a preselected binder.

[0039] The adhesive layer solution may not contain a binder. This increases the amount of the binder in the positive electrode layer that dissolves into the adhesive layer solution, thereby further improving the bonding between the positive electrode layer and the adhesive layer. On the other hand, the adhesive layer solution may contain the same type of binder as the binder contained in the positive electrode layer solution. This improves the compatibility between the binder contained in the adhesive layer and the binder contained in the positive electrode layer, so that the positive electrode layer and the adhesive layer can be bonded more continuously and firmly. In addition, the adhesive layer solution contains a binder, which improves the coatability of the adhesive layer solution.

[0040] The second solvent has a higher solubility of the binder contained in the positive electrode layer solution than the first solvent. This makes it possible to make the bond between the positive electrode layer and the adhesive layer more continuous or stronger. The above effects will be described below with reference to the drawings.

[0041] Fig. 1 is a cross-sectional view conceptually showing the state when the positive electrode layer and the adhesive layer according to this embodiment are laminated. The explanation of each symbol in Fig. 1 and Fig. 2 is as follows. 10: positive electrode layer (positive electrode layer solution), 11: positive electrode active material, 20: adhesive layer (adhesive layer solution), 21: solid electrolyte, V: binder, S: second solvent.

[0042] 1, the second solvent S, in which the solubility of the binder V is higher than that of the first solvent, is present inside the adhesive layer 20. Therefore, when the first solvent is present inside the positive electrode layer 10, the binder V is compatible with the second solvent, and the movement of the binder V from inside the positive electrode layer 10 to the adhesive layer 20 is promoted. Even when the first solvent is not present inside the positive electrode layer 10, the binder V present inside the positive electrode layer 10 is dissolved by the second solvent and moves to the adhesive layer 20.

[0043] 2 is a cross-sectional view conceptually showing a state in which the positive electrode layer 10 and the adhesive layer 20 are bonded (laminated) after passing through the state shown in FIG. 1. As shown in FIG. 2, at the interface L between the positive electrode layer 10 and the adhesive layer 20, there is a binder V that has moved from the positive electrode layer 10 to the adhesive layer 20. This binder V is drawn to the vicinity of the interface L by the second solvent, and is bonded and welded with the solid electrolyte 21 and the binder originally present in the adhesive layer 20, thereby exerting an anchor effect. As a result, the voids at the interface L are filled, and the bond between the positive electrode layer and the adhesive layer can be made more continuous or stronger.

[0044] The second solvent preferably has a boiling point lower than that of the first solvent. As a result, after the voids at the interface between the positive electrode layer and the adhesive layer are filled with the binder, the second solvent evaporates smoothly, making it easier to fill the interface with the binder and less likely to cause voids at the interface. Therefore, the bonding strength between the positive electrode layer and the adhesive layer can be further improved.

[0045] The positive electrode layer forming step is a step of forming a positive electrode layer, and includes a step of applying a positive electrode layer solution. The target to which the positive electrode layer solution is applied may be an adhesive layer. In addition to the above, the positive electrode layer forming step may be a step of applying the positive electrode layer solution to an arbitrary target such as a positive electrode current collector and drying it to form a sheet-like positive electrode layer alone. Examples of a method for applying the positive electrode layer solution include a coating method using an applicator such as a doctor blade method, spray coating, screen printing, and the like.

[0046] The adhesive layer forming step is a step of forming an adhesive layer, and includes a step of applying an adhesive layer solution. The target to which the adhesive layer solution is applied may be a positive electrode layer. In addition to the above, the positive electrode layer forming step may be a step of applying the adhesive layer solution to an arbitrary target and drying it to form a sheet-like adhesive layer alone. However, the second solvent must remain in the adhesive layer after it is formed by the adhesive layer forming step. The method of applying the adhesive layer solution may be the same as the method of applying the positive electrode layer solution.

[0047] The electrolyte layer forming step is a step of forming an electrolyte layer, and includes a step of applying an electrolyte solution containing each component contained in the electrolyte layer. The object to which the electrolyte solution is applied may be an adhesive layer. In addition to the above, the electrolyte layer forming step may be a step of applying the electrolyte solution to an arbitrary object and drying it to form a sheet-like electrolyte layer alone. The method of applying the electrolyte solution may be the same as the method of applying the positive electrode layer solution.

[0048] The molding step of each layer may include a compression step of compressing each molded layer to densify it. The compression method in the compression step is not particularly limited, but includes methods such as flat pressing and roll pressing.

[0049] The lamination process is a process of laminating the positive electrode layer, adhesive layer, and electrolyte layer formed in the above-mentioned layer forming process in this order. The lamination process may be a process of laminating each layer formed independently. Alternatively, the lamination process may be a process of forming another layer on a layer formed independently. In that case, however, the above-mentioned forming process of each layer also serves as the lamination process. The lamination process may be a combination of a process of laminating each layer formed independently and a process of forming another layer on a layer formed independently.

[0050] In the lamination step, when laminating the positive electrode layer and the adhesive layer, it is preferable that the second solvent is present at least in the adhesive layer. As a result, as described above, the binder present in the positive electrode layer is moved to the adhesive layer by the second solvent, and the bonding between the positive electrode layer and the adhesive layer is made more continuous or stronger. In addition to the above, it is more preferable that the first solvent is present at least in the positive electrode layer when laminating the positive electrode layer and the adhesive layer.

[0051] The molding step or lamination step of each layer may include a heat compression step of heat-compressing each layer or the laminate of each layer. The heat compression step can increase the density of each layer, and can also increase the bonding strength of each layer by bonding each layer together and fusing the binders together. However, as described above, when laminating the positive electrode layer and the adhesive layer, it is preferable that the second solvent is present at least in the adhesive layer. Therefore, it is preferable that the heat compression step is performed on the laminate after laminating at least the positive electrode layer and the adhesive layer.

[0052] The method of heat compression in the heat compression step is not particularly limited, but examples thereof include hot flat pressing and hot roll pressing.

[0053] An application example of the method for manufacturing an electrode body for a non-aqueous secondary battery is described below. First, in the positive electrode layer solution preparation step, a positive electrode layer solution is prepared containing a positive electrode active material, SBR as a binder, and butyl butyrate (boiling point 165 degrees) as a first solvent. Next, in the positive electrode layer molding step, a thin film is formed on an arbitrary target by a doctor blade method, and compressed to a high density by a roll press under a Hertzian surface pressure of 200 to 1,000 MPa.

[0054] Next, in the electrolyte layer forming step, an electrolyte solution containing a solid electrolyte and a binder is used to form a film with an applicator, and the film is compressed and densified with a roll press under conditions of a Hertzian surface pressure of 200 to 1,000 MPa.

[0055] Next, in an adhesive layer solution preparation step, an adhesive layer solution is prepared containing a solid electrolyte, toluene (boiling point 110 degrees) as a second solvent, a solid electrolyte, and a binder such as SBR as necessary. Next, in an adhesive layer forming step which also serves as a lamination step, the prepared adhesive layer solution is applied to a thickness of 1 to 5 μm on the formed positive electrode layer. Next, in a lamination step, the electrolyte layer is transferred onto the formed adhesive layer, and roll-bonding is performed using a roll press or the like.

[0056] In the above application example, butyl butyrate is used as the first solvent and toluene is used as the second solvent. However, for example, toluene can be used as the first solvent and xylene can be used as the second solvent.

[0057] According to the manufacturing method of the electrode body for a nonaqueous secondary battery of the present embodiment, the bond between the positive electrode layer and the solid electrolyte layer can be made more continuous or stronger, and therefore the resistance of the interface between the positive electrode layer and the solid electrolyte layer is reduced, leading to an increase in battery capacity and an improvement in durability.

[0058] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above-mentioned embodiments, and the present invention includes modifications and improvements within the scope of the present invention that can achieve the object of the present invention. [Explanation of symbols]

[0059] 10 Positive electrode layer 11 Cathode active material 20 Adhesive layer 21 Solid electrolyte V Binder S 2nd Solvent

Claims

1. A method for producing an electrode body for a non-aqueous secondary battery, comprising the steps of: a positive electrode layer solution preparation step of preparing a positive electrode layer solution including a positive electrode active material, a binder, and a first solvent; a positive electrode layer forming step of forming a positive electrode layer using the positive electrode layer solution; an electrolyte layer forming step of forming an electrolyte layer including a solid electrolyte; An adhesive layer solution preparation step of preparing an adhesive layer solution containing a solid electrolyte and a second solvent; An adhesive layer forming step of forming an adhesive layer using the adhesive layer solution; a lamination step of laminating the positive electrode layer, the adhesive layer, and the electrolyte layer in this order, The second solvent has a higher solubility for the binder than the first solvent.

2. The method for producing an electrode body for a non-aqueous secondary battery according to claim 1 , wherein the second solvent has a boiling point lower than that of the first solvent.

3. 3 . The method for producing an electrode body for a non-aqueous secondary battery according to claim 1 , wherein, in the lamination step, when the positive electrode layer and the adhesive layer are laminated, the second solvent is present at least in the adhesive layer.

4. The method for producing an electrode body for a non-aqueous secondary battery according to claim 3 , wherein the adhesive layer solution does not contain a binder.

5. The method for producing an electrode body for a non-aqueous secondary battery according to claim 1 , wherein the adhesive layer solution contains the same type of binder as that contained in the positive electrode layer solution.

Citation Information

Patent Citations

  • Solid-state battery electrode, solid-state battery, adhesive film for solid-state battery, and method for manufacturing solid-state battery electrode

    JP2013125707A

  • All-solid type secondary battery and method for manufacturing all-solid type secondary battery

    JP2015103451A

  • Slurry

    JP2021099950A

  • Paint control system with automated paint stirrer device and control method thereof

    KR102493272B1

  • Solid-state battery

    JP2014116164A