Wiring material, and production method of wiring material
A silane crosslinkable polymer mixture with controlled pressure and cooling in a pressurized environment addresses voids and mechanical strength issues in wiring materials, ensuring high-quality coating layers with simplified equipment.
Patent Information
- Application Number
- JP2023051166
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Existing silane crosslinking methods for wiring materials face issues such as void formation, mechanical strength degradation, and increased equipment complexity due to high temperatures and pressures, leading to reduced productivity and damaged coating layers.
A method involving a silane crosslinkable polymer mixture with specific proportions of organic peroxide, silane coupling agent, and inorganic filler, which is extruded into a pressurized environment and cooled under pressure to prevent void formation and enhance mechanical strength, using a simplified equipment setup.
The method enables continuous production of wiring materials with excellent appearance, mechanical strength, and heat resistance while suppressing voids and surface defects, even at increased productivity levels.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a wiring material and a method for manufacturing the wiring material. [Background technology]
[0002] Various resin or rubber molded products are used as coating layers (insulating layers, sheaths, etc.) provided on wiring materials such as insulated wires, cables, cords, optical fiber cores, and optical fiber cords (optical fiber cables) used in the fields of electric and electronic equipment and industry. Various properties are required for such molded products depending on the application and usage form, and for example, heat resistance and the like are required from the viewpoint of safety and reliability. As a technique for improving the heat resistance of wiring materials, a technique for crosslinking the resin or rubber forming the coating layer (a technique for forming a crosslinked coating layer) is commonly used. Electron beam crosslinking, chemical crosslinking, and the like are used as a method for crosslinking the resin or rubber. Among them, a technique for crosslinking the resin or rubber by graft bonding with radicals generated from a silane coupling agent and an organic peroxide, etc., followed by a silanol condensation reaction (silane crosslinking method) is generally used as a crosslinking method for the coating layer because it does not require special equipment in the crosslinking process and is advantageous in terms of production compared to other crosslinking methods. On the other hand, in the silane crosslinking method, when the silane coupling agent is graft bonded to the resin or rubber, an excessive crosslinking reaction occurs between the resins or between the rubbers, forming a crosslinked gel, which may cause protruding aggregates (surface bumps) on the surface of the crosslinked coating layer. Therefore, in the silane crosslinking method, in order to form a crosslinked coating layer with excellent appearance, it is also necessary to suppress the formation of the crosslinked gel (the occurrence of surface bumps).
[0003] When manufacturing a wiring material having a crosslinked coating layer by the silane crosslinking method, a resin composition or a rubber composition is extruded onto a conductor while being extruded (extruded) under normal pressure, cooled, and brought into contact with water to crosslink the resin or rubber and form a crosslinked coating layer. However, it is known that when a resin composition or the like is cooled and brought into contact with water under such normal pressure, voids (gaps due to air bubbles, delamination, etc.) are generated in the coating layer formed due to various factors. The presence (generation) of voids causes various problems such as a decrease in the electrical and mechanical properties of the coating layer (wiring material). Therefore, a method for suppressing the generation of voids in the coating layer in the silane crosslinking method has been studied. For example, Patent Document 1 discloses a method for suppressing the generation of voids due to gas generated during decomposition of organic peroxides, in which an organic peroxide crosslinked polyolefin and an organic silane crosslinked polyolefin are extruded onto a conductor in sequence, and in this case, the conductor is heated to 140°C or higher while a pressure of 3 kg / cm is applied from the outer layer. 2 The above method proposes heating to 150°C under saturated steam pressure. Patent Document 2 also proposes a method for suppressing the generation of voids due to thermal shrinkage of the composition (residual air, peeling, etc.) by extruding a silane crosslinkable resin composition onto a conductor to coat it, and then cooling it in pressurized water to cause a reaction and crosslinking. In this method, in order to suppress the generation of voids, the pressure must be 3 kg / cm. 2 It is described that the pressure is 6 kg / cm or more, and in the embodiment, 2 It is set to a high pressure environment. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 62-88213 [Patent Document 2] Japanese Patent Application Publication No. 59-25110 Summary of the Invention [Problem to be solved by the invention]
[0005] The present inventors have conducted studies on the formation of a crosslinked coating layer by the silane crosslinking method (production of wiring material) and have found the following problems. That is, the method described in Patent Document 1 requires crosslinking at a high temperature of 140°C or higher (an additional heating step) after extrusion molding. This not only undermines the advantage of the silane crosslinking method, which is more advantageous in terms of production than other crosslinking methods, but also worsens productivity. In addition, when producing continuously, the coated conductor is heated to a high temperature in the additional heating step and the surface is softened, and then the coated conductor is fed to the production line, so there is a risk of scratches and deformation occurring in the tubular molded body (coating layer) of organosilane crosslinked polyolefin that coats the conductor at various points in the equipment. On the other hand, the method described in Patent Document 2 requires a pressure of 3 kg / cm as a pressing condition after extrusion coating. 2 As a result, the equipment for circulating the cooling water while maintaining high pressure becomes large-scale and complicated, resulting in high equipment costs. Furthermore, in order to maintain the high-pressure environment of the pressurizing device, it is necessary to reduce the clearance between the outlet part (seal part and packing part) and the outer circumferential surface of the coated conductor to be led out (to maintain airtightness), and the tubular molding (coating layer) of the resin composition or the like that covers the conductor is easily damaged by contact with the outlet part. Moreover, the coated conductor led out of the pressurizing device in a high-pressure environment is easily shaken by air or water leaking from the outlet part, etc., and tends to become more unstable in the conveying direction. Even if the conveying speed is increased to increase the productivity of the wiring material, the shaking becomes larger, and the coated conductor is strongly rubbed against the outlet part and damaged. As described above, the methods described in Patent Documents 1 and 2 result in the formation of a damaged crosslinked coating layer, which not only impairs the appearance but also leads to a decrease in mechanical strength.
[0006] Incidentally, in the silane crosslinking method, when an inorganic filler is coexisted during the grafting reaction between a resin or rubber and a silane coupling agent, a crosslinked structure can also be constructed via the inorganic filler, and it is said that the mechanical strength, heat resistance (crosslinking density), etc. of the crosslinked coating layer can be further improved. However, when the methods described in Patent Documents 1 and 2 are applied to the silane crosslinking method using an inorganic filler, in addition to the above-mentioned problems, it has been found that the improving effect of the inorganic filler on mechanical strength and heat resistance is not fully exhibited.
[0007] In addition, in the above-mentioned study of the above-mentioned patent documents, the present inventors further investigated the cause of the generation of voids in the coating layer, and found that the main cause is not only the organic peroxides and thermal shrinkage described in the above-mentioned patent documents, but also that in the silane crosslinking method in which an inorganic filler is coexisted, the silane coupling agent that does not undergo a grafting reaction with the resin and remains is less likely to volatilize, but volatilizes due to the high temperature during extrusion molding to form fine bubbles (air bubbles). In particular, when the rotation speed of the extruder is increased, for example, in order to increase the productivity of the wiring material, strong shear is applied to the resin composition, etc., causing a temperature rise, which promotes (accelerates) the volatilization of the silane coupling agent and generates a large number of voids. However, Patent Documents 1 and 2 do not consider the viewpoint of fully utilizing the effect of improving mechanical strength and heat resistance of inorganic filler in the silane crosslinking method in which inorganic filler is coexisted, nor the viewpoint of suppressing the occurrence of voids caused by remaining silane coupling agent.
[0008] The present invention aims to provide a method for manufacturing wiring material, which can continuously produce wiring material having a cross-linked coating layer that has excellent appearance characteristics, mechanical strength, and heat resistance while suppressing the occurrence of voids even when productivity is increased, and wiring material manufactured by this manufacturing method. [Means for solving the problem]
[0009] The present inventors have found that in a specific silane crosslinking method using a silane crosslinkable polymer mixture containing a specific ratio of organic peroxide and a silane coupling agent, and further an inorganic filler, a coated conductor having a silane crosslinkable polymer mixture coated on the outer periphery of the conductor is directly introduced from an extruder into a pressurized environment at a specific pressure, and the surface temperature is cooled under pressure with a liquid medium until 100°C or less, and then the coated conductor is discharged into a normal pressure environment, thereby forming a crosslinked coating layer that is excellent in appearance characteristics, and maintains high mechanical strength and heat resistance due to the cooperation of an inorganic filler, while preventing foaming and expansion, suppressing the generation of voids, and suppressing the generation of scratches and surface bumps, even if unreacted silane coupling agent remains, and even if productivity is increased, the present inventors have further researched and have come to the present invention.
[0010] That is, the object of the present invention has been achieved by the following means. <1> A method for producing a wiring material having a crosslinked coating layer of a silane crosslinkable polymer mixture on an outer peripheral surface of a conductor, comprising the steps of: In preparing a silane crosslinkable polymer mixture using 100 parts by mass of a base polymer, 0.01 to 0.6 parts by mass of an organic peroxide, 0.5 to 15 parts by mass of a silane coupling agent, 0.5 to 400 parts by mass of an inorganic filler, and a silanol condensation catalyst, a silane master batch prepared by melt-mixing a part of the base polymer with the organic peroxide, the silane coupling agent, and the inorganic filler in the above-mentioned mixing ratio at a temperature equal to or higher than the decomposition temperature of the organic peroxide, and a catalyst master batch prepared by melt-mixing the remainder of the base polymer and the silanol condensation catalyst are mixed to prepare the silane crosslinkable polymer mixture, The silane crosslinkable polymer mixture is introduced into an extruder to coat the outer peripheral surface of a conductor; This method for producing a wiring material comprises directly introducing the obtained coated conductor from the extruder into a pressurized environment of 0.05 to 0.25 MPa higher than normal pressure, cooling the coated conductor with a liquid medium in the pressurized environment until the surface temperature of the coated conductor becomes 100°C or lower, and then removing the coated conductor from the pressurized environment into a normal pressure environment. <2> The coated conductor introduced into the atmospheric pressure environment is brought into contact with water in the atmospheric pressure environment. <1> The manufacturing method described in <3> The base polymer contains at least one of a polyolefin resin, an ethylene-vinyl acetate copolymer resin, an ethylene-alkyl (meth)acrylate copolymer resin, an ethylene rubber, a silicone rubber, a fluororubber, and a styrene-based elastomer. <1> or <2> The manufacturing method described in <4> The liquid medium is sprayed onto the coated conductor to cool it. <1> ~ <3> The method for producing a product according to any one of claims 1 to 5. <5> The pressure in the pressurized environment is 0.10 to 0.20 MPa higher than normal pressure. <1> ~ <4> The method for producing a product according to any one of claims 1 to 5. <6> The amount of the silane coupling agent mixed is 2.0 to 6.0 parts by mass based on 100 parts by mass of the base polymer. <1> ~ <5> The method for producing a product according to any one of claims 1 to 5. <7> cooling the coated conductor in the pressurized environment until the surface temperature becomes 80° C. or less; <1> ~ <6> The method for producing a product according to any one of claims 1 to 5. <8> The mixing amount of the inorganic filler is 3 to 200 parts by mass. <1> ~ <7> The method for producing a product according to any one of claims 1 to 5. <9> In preparing the silane master batch, the silane coupling agent and the inorganic filler are mixed in advance, and then a part of the base polymer is melt-mixed therewith. <1> ~ <8> The method for producing a product according to any one of claims 1 to 5. <10> the above <1> ~ <9> 13. A wiring material manufactured by the manufacturing method according to any one of claims 1 to 12. Effect of the Invention
[0011] The present invention provides a method for producing wiring material that can continuously produce wiring material having a cross-linked coating layer that has excellent appearance characteristics, mechanical strength, and heat resistance while suppressing the occurrence of voids, even if, for example, the rotation speed of the extruder is increased to increase productivity, and even if unreacted silane coupling agent remains, and provides wiring material produced by this production method. [Brief description of the drawings]
[0012] [Figure 1]FIG. 1 is an explanatory diagram showing a schematic diagram of a manufacturing apparatus preferably used in the manufacturing method of the wiring material of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] In the present invention, when the content, physical properties, etc. of a component are described by showing a numerical range, and when the upper limit and lower limit of the numerical range are described separately, any of the upper limit and lower limit can be appropriately combined to form a specific numerical range. On the other hand, when multiple numerical ranges expressed using "~" are set and described, the upper limit and lower limit forming the numerical range are not limited to the specific combination described before and after "~" as a specific numerical range, and can be a numerical range obtained by appropriately combining the upper limit and lower limit of each numerical range. In addition, in the present invention, a numerical range expressed using "~" means a range including the numerical values described before and after "~" as the upper limit and lower limit. In the present invention, "(meth)acrylic acid" refers to either or both of acrylic acid and methacrylic acid, and "(meth)acrylic acid ester" refers to either or both of acrylic acid ester and methacrylic acid ester.
[0014] First, each component used in the present invention will be described. Each of the components may be used alone or in combination of two or more.
[0015] <Base polymer> The base polymer is a polymer that serves as the base for forming the crosslinked coating layer (silane-crosslinked polymer molded body) and the molding material (silane-crosslinkable polymer mixture), and is usually a resin, elastomer (including rubber), etc. The base polymer used in the present invention can be any of various known polymers that form a crosslinked coating layer of a wiring material, without any particular limitation. Examples of the base polymer include polyolefin resins, copolymer resins having an acid copolymerization component, copolymer resins having an acid ester copolymerization component, (meth)acrylic resins, ethylene rubber, silicone rubber, fluororubber, acrylic rubber, synthetic rubber, and styrene-based elastomers.
[0016] The base polymer preferably contains at least one polymer having a site (e.g., an unsaturated bond site in a carbon chain or a carbon atom having a hydrogen atom) capable of undergoing a grafting reaction with a silane coupling agent described later in the presence of an organic peroxide in the main chain or at its end, more preferably at least one of a polyolefin resin, a copolymer resin having an acid copolymerization component, a copolymer resin having an acid ester copolymerization component, an ethylene rubber, a silicone rubber, a fluororubber, and a styrene-based elastomer, and even more preferably at least one of a polyolefin resin, an ethylene-vinyl acetate copolymer resin, an ethylene-(meth)acrylic acid alkyl copolymer resin, an ethylene rubber, a silicone rubber, a fluororubber, and a styrene-based elastomer. As the base polymer, two or more of the above resins or rubbers can be used in combination depending on the application or required characteristics. The ethylene rubber and the styrene-based elastomer can each be used alone, but are preferably used in combination with a polyolefin resin. In addition, oil can be used as a plasticizing component, and in particular, the styrene-based elastomer is preferably used in combination with an oil. In the present invention, a base polymer containing a resin may be referred to as a base resin, and a base polymer containing a rubber may be referred to as a base rubber.
[0017] (Polyolefin resin) The polyolefin resin is not particularly limited as long as it is a resin made of a polymer obtained by polymerizing or copolymerizing a compound having an ethylenically unsaturated bond (also called an olefin compound, excluding carboxylic acid compounds and acid ester compounds described below), and known resins used in various resin compositions can be used. Examples include resins of polyethylene, polypropylene, ethylene-α-olefin copolymers, and block copolymers of polypropylene and ethylene-α-olefin resins. Other examples include rubbers or elastomers of these copolymers (excluding ethylene rubber and styrene-based elastomers).
[0018] - Polyethylene resin - The polyethylene resin (PE) is not particularly limited as long as it is a polymer resin mainly composed of ethylene. For example, high density polyethylene (HDPE), low density polyethylene (LDPE), ultra-high molecular weight polyethylene (UHMW-PE), linear low density polyethylene (LLDPE), and very low density polyethylene (VLDPE) resins can be mentioned. Among them, linear low density polyethylene and low density polyethylene resins are preferable.
[0019] - Polypropylene resin - The polypropylene resin (PP) is not particularly limited as long as it is a polymer resin mainly composed of propylene, and examples thereof include propylene homopolymers, random polypropylenes, and block polypropylenes.
[0020] - Ethylene-α-olefin copolymer resin - The ethylene-α-olefin copolymer resin (ethylene-α-olefin copolymer resin) preferably includes a copolymer of ethylene and an α-olefin having 3 to 12 carbon atoms (excluding those included in the above polyethylene and polypropylene).
[0021] (Copolymer resin having an acid copolymerization component) The compound that leads to the acid copolymerization component in the resin of the copolymer having an acid copolymerization component (copolymer resin having an acid copolymerization component) is not particularly limited, and includes carboxylic acid compounds such as (meth)acrylic acid, etc. The copolymer resin having an acid copolymerization component (excluding those contained in polyethylene resin) includes, for example, ethylene-(meth)acrylic acid copolymer resin.
[0022] (Copolymer resin having an acid ester copolymer component) The compound that leads to the acid ester copolymerization component in the resin of the copolymer having an acid ester copolymerization component (copolymer resin having an acid ester copolymerization component) is not particularly limited, and examples thereof include acid ester compounds such as vinyl acetate and (meth)acrylic acid ester. The (meth)acrylic acid ester is not particularly limited, and examples thereof include alkyl (meth)acrylate. The alkyl group of the alkyl (meth)acrylate is preferably one having 1 to 12 carbon atoms. Examples of the copolymer resin having an acid ester copolymerization component (excluding those contained in polyethylene resin) include, for example, ethylene-vinyl acetate copolymer (EVA), ethylene-alkyl (meth)acrylate copolymer, and other resins. Specific examples of the ethylene-alkyl (meth)acrylate copolymer resin include ethylene-methyl acrylate copolymer (EMA), ethylene-ethyl acrylate copolymer (EEA), and ethylene-butyl acrylate copolymer (EBA). Among these, ethylene-vinyl acetate copolymer and ethylene-methyl acrylate copolymer resins are preferred.
[0023] (Ethylene rubber) The ethylene rubber is not particularly limited as long as it is a rubber (including elastomers) made of a copolymer obtained by copolymerizing a compound having an ethylenically unsaturated bond, and known rubbers can be used. Preferred examples of the ethylene rubber include a copolymer of ethylene and an α-olefin, and a terpolymer of ethylene, an α-olefin, and a diene. Examples of the terpolymer include a terpolymer of ethylene, an α-olefin, and a conjugated diene, and a terpolymer of ethylene, an α-olefin, and a non-conjugated diene. The α-olefin is preferably an α-olefin having a carbon number of 3 to 12. The diene compound constituting the terpolymer is not particularly limited, and examples thereof include conjugated diene compounds such as butadiene, isoprene, 1,3-pentadiene, and 2,3-dimethyl-1,3-butadiene, and non-conjugated diene compounds such as dicyclopentadiene (DCPD), ethylidenenorbornene (ENB), and 1,4-hexadiene, with non-conjugated diene compounds being preferred. As the binary copolymer rubber, ethylene-propylene rubber (EPM) is preferred, and as the ternary copolymer rubber, ethylene-propylene-diene rubber (EPDM) is preferred. The amount of ethylene constituents in the copolymer of ethylene rubber (referred to as ethylene content) is preferably 45 to 75 mass%. The ethylene content is a value measured in accordance with the method described in ASTM D3900. When the content of ethylene rubber in the base polymer is 60 parts by mass or more, the amount of diene constituents in the ethylene rubber (referred to as diene content) is preferably 0 to 7 mass%. The diene content can be measured, for example, by infrared absorption spectroscopy (FT-IR), proton NMR ( 1 It can be measured by H-NMR, etc.
[0024] (Silicone rubber) The silicone rubber may be any rubber made of a polymer (organopolysiloxane) having a polysiloxane structure, and may be any rubber that is generally used in rubber compositions and the like, without any particular limitations. Examples of silicone rubber include various silicone rubbers such as methylpolysiloxane, dimethylpolysiloxane, methylvinylpolysiloxane, phenylpolysiloxane, and methylphenylpolysiloxane. The silicone rubber may be liquid silicone rubber, but is preferably millable silicone rubber in terms of grafting reaction with a silane coupling agent.
[0025] - Millable silicone rubber - Millable silicone rubber can be any silicone rubber that uses linear organopolysiloxane (uncrosslinked) as the main raw material (silicone raw rubber), and is usually used as a compound in which a reinforcing agent is mixed with linear organopolysiloxane. Millable silicone rubber exhibits high thermal stability even above the decomposition temperature of organic peroxides, and can initiate a grafting reaction with a silane coupling agent with good workability. The organopolysiloxane may be any that can undergo grafting reaction with a silane coupling agent, and includes organopolysiloxanes containing vinyl groups as grafting sites (crosslinking points), specifically methylvinylpolysiloxane, methylphenylvinylpolysiloxane, methylfluoroalkylpolysiloxane, etc. The reinforcing agent is not particularly limited, and may be, for example, various types of silica. The content of the reinforcing agent in the millable silicone rubber can be appropriately set according to the specific gravity, use, and required properties of the millable silicone rubber, and may be, for example, 10 to 40% by mass in 100% by mass of the millable silicone rubber.
[0026] (Fluorine rubber) The fluororubber is not particularly limited, and may be any ordinary fluororubber that has been used in various rubber moldings. Examples of the fluororubber include homopolymer or copolymer rubbers that contain fluorine atoms in the main chain or side chain. Fluororubbers are usually obtained by (co)polymerizing a monomer that contains fluorine atoms. Such fluororubbers are not particularly limited, but include copolymer rubbers of fluorine-containing monomers such as perfluorohydrocarbons such as tetrafluoroethylene and hexafluoropropylene, and partially fluorinated hydrocarbons such as vinylidene fluoride, and further copolymer rubbers of these fluorine-containing monomers and hydrocarbons (olefin compounds) such as ethylene and / or propylene.Specific examples include tetrafluoroethylene-propylene copolymer rubber (FEPM), tetrafluoroethylene-fluorinated (e.g., hexafluoro)propylene copolymer rubber, tetrafluoroethylene-perfluorovinyl ether copolymer rubber (FFKM), vinylidene fluoride rubber (FKM, e.g., vinylidene fluoride-hexafluoropropylene copolymer rubber), and the like.Of these fluororubbers, tetrafluoroethylene-propylene copolymer rubber and vinylidene fluoride-hexafluoropropylene copolymer rubber are preferred, and tetrafluoroethylene-propylene copolymer rubber is more preferred.
[0027] (styrene elastomer) The styrene-based elastomer refers to an elastomer made of a polymer having a component derived from an aromatic vinyl compound in the molecule. Such styrene-based elastomers include block copolymers and random copolymers of conjugated diene compounds and aromatic vinyl compounds, or hydrogenated products thereof. Examples of aromatic vinyl compounds include styrene, p-(t-butyl)styrene, α-methylstyrene, p-methylstyrene, divinylbenzene, 1,1-diphenylstyrene, N,N-diethyl-p-aminoethylstyrene, vinyltoluene, etc. Examples of conjugated diene compounds include butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, etc. Examples of styrene-based elastomers include styrene-ethylene-butylene-styrene block copolymer (SEBS), styrene-isoprene-styrene block copolymer (SIS), hydrogenated SIS, styrene-butadiene-styrene block copolymer (SBS), hydrogenated SBS, styrene-ethylene-ethylene-propylene-styrene block copolymer (SEEPS), styrene-ethylene-propylene-styrene block copolymer (SEPS), styrene-butadiene rubber (SBR), hydrogenated styrene-butadiene rubber (HSBR), and the like.
[0028] (oil) The oil that the base polymer may contain is not particularly limited, and may be an organic oil or a mineral oil. When the base polymer contains an oil, the occurrence of surface bumps (granular objects protruding from the surface) can be suppressed, and a crosslinked coating layer having excellent appearance can be produced. Examples of the organic oil or mineral oil include soybean oil, paraffin oil, naphthenic oil, and aromatic oil. Paraffin oil or naphthenic oil is preferred, and paraffin oil is more preferred in terms of mechanical strength.
[0029] (Base Polymer Composition) When the base polymer contains two or more components, the content of each component in the base polymer is not particularly limited and is set appropriately depending on the application and mode of use. For example, when the base polymer contains a polyolefin resin and an ethylene rubber, the content of the polyolefin resin is preferably 10 to 50 mass%, more preferably 20 to 40 mass%, when the total content of each component in the base polymer is 100 mass%, while the content of the ethylene rubber is preferably 50 to 90 mass%, more preferably 60 to 80 mass%. In addition, when the base polymer contains a polyolefin resin and a styrene-based elastomer, the content of the polyolefin resin is preferably 5 to 50 mass%, and more preferably 10 to 30 mass%, when the total content of each component in the base polymer is 100 mass%. On the other hand, the content of the styrene-based elastomer is preferably 50 to 95 mass%, and more preferably 60 to 80 mass%. It is preferable that the base polymer contains oil, and the content of the oil is preferably 10 to 40 mass%, and more preferably 20 to 30 mass%, when the total content of each component in the base polymer is 100 mass%.
[0030] The base polymer may contain other components, such as various additives and solvents, which will be described later.
[0031] <Organic peroxide> The organic peroxide generates radicals by thermal decomposition, and thereby has the function of initiating and promoting the grafting reaction between the silane coupling agent and the base polymer (a covalent bond forming reaction between the grafting reaction site of the silane coupling agent and the grafting reaction site of the base polymer, which is also called a (radical) addition reaction). There are no particular limitations on the organic peroxide, and examples thereof include compounds represented by the general formula: R 1 -O-O-R 2 , R 3 -OO-C(=O)R 4 , R 5 C(=O)-OO(C=O)R 6 Preferred are compounds represented by the formula: 1 ~R 6 Each independently represents an alkyl group, an aryl group, or an acyl group. R 1 ~R 6 Among these, it is preferable that all of them are alkyl groups, or that one of them is an alkyl group and the remaining is an acyl group.
[0032] The decomposition temperature of the organic peroxide is preferably 80 to 195°C, particularly preferably 125 to 180°C, as measured by the method described in JP-A-2016-121203. Examples of such organic peroxides include those described in paragraph
[0036] of JP 2016-121203 A, the contents of which are incorporated herein by reference as part of the present specification. Among these, dicumyl peroxide, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane (Perhexa 25B), and 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3 are preferred.
[0033] <Silane coupling agent> The silane coupling agent (before grafting reaction) used in the present invention has a grafting reaction site (functional group such as a group or an ethylenically unsaturated group) that can undergo grafting reaction with the grafting reaction site of the base polymer in the presence of radicals generated by decomposition of organic peroxide, and is preferably capable of reacting with the site of chemical bonding of the inorganic filler.In addition, it has a hydrolyzable silyl group as a reaction site capable of silanol condensation.As such a silane coupling agent, there can be mentioned a silane coupling agent used in the conventional silane crosslinking method. Suitable examples of the silane coupling agent include silane coupling agents having an ethylenically unsaturated group and a hydrolyzable silyl group. Specific examples include vinyl alkoxylanes such as vinyl trimethoxylane, vinyl triethoxylane, vinyl tributoxylane, vinyl dimethoxyethoxylane, vinyl dimethoxybutoxylane, vinyl diethoxybutoxylane, allyl trimethoxylane, allyl triethoxylane, and vinyl triacetoxylane; and (meth)acryloxyalkoxylanes such as methacryloxypropyl trimethoxylane, methacryloxypropyl triethoxylane, and methacryloxypropyl methyl dimethoxylane. The method for manufacturing wiring material of the present invention can suppress the generation of voids caused by the silane coupling agent, so it is possible to use a silane coupling agent that is easily volatile. Among the above, vinyltrimethoxysilane and vinyltriethoxysilane, which are easily grafted to the base polymer, are particularly suitable for use. The silane coupling agent may be used alone or in combination of two or more kinds. In addition, the silane coupling agent may be used as it is or after diluting with a solvent or the like.
[0034] <Inorganic filler> In the present invention, an inorganic filler is made to coexist during the grafting reaction between the base polymer and the silane coupling agent. This allows the inorganic filler to be incorporated into the crosslinked structure of the base polymer, and the mechanical strength and heat resistance of the resulting crosslinked coating layer can be further improved. In the present invention, the inorganic filler may be mixed in any form, but for example, it is preferable to use it in a form in which it is mixed (added) separately to the base polymer (compound or mixture), and it is more preferable to use it in a form in which it is premixed with the silane coupling agent before mixing with the base polymer. The inorganic filler is not particularly limited as long as it is a commonly used one, but it is preferable that the inorganic filler has a site on its surface that can be chemically bonded to the silanol condensation reactive site of the silane coupling agent by hydrogen bond, covalent bond, or intermolecular bond. The site that can be chemically bonded to the silanol condensation reactive site of the silane coupling agent is not particularly limited, but includes OH group (hydroxyl group, water molecule of water or crystal water, OH group of carboxyl group, etc.), amino group, SH group, etc. Examples of inorganic fillers include those that are commonly used in resin compositions, such as metal hydrates such as compounds having hydroxyl groups or crystal water, such as aluminum hydroxide, magnesium hydroxide, boehmite, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whiskers, hydrated aluminum silicate, hydrated magnesium silicate, basic magnesium carbonate, hydrotalcite, and talc. In addition, examples of inorganic fillers include boron nitride, silica (crystalline silica, amorphous silica, etc.), carbon black, clay (calcined clay), zinc oxide, tin oxide, titanium oxide, molybdenum oxide, antimony trioxide, silicone compounds, quartz, zinc borate, white carbon, zinc borate, zinc hydroxystannate, and zinc stannate. Examples of inorganic fillers include aluminum hydroxide, magnesium hydroxide, boehmite, talc, clay, silica, and calcium carbonate.
[0035] The inorganic filler is preferably in the form of particles, and the average particle size is preferably 0.2 to 10 μm, more preferably 0.3 to 8 μm, further preferably 0.4 to 5 μm, and particularly preferably 0.4 to 3 μm. The average particle size is determined by dispersing the inorganic filler in alcohol or water and using an optical particle size measuring device such as a laser diffraction / scattering type particle size distribution measuring device. The inorganic filler may be surface-treated with various surface treatment agents. The inorganic filler may be used alone or in combination of two or more kinds.
[0036] <Silanol condensation catalyst> The silanol condensation catalyst acts to promote the condensation reaction of the silanol condensable reactive sites of the silane coupling agent grafted to the base polymer in the presence of water (moisture). Based on the action of this silanol condensation catalyst, the base polymer is crosslinked via the silane coupling agent. Such silanol condensation catalysts are not particularly limited, and examples thereof include organotin compounds, metal soaps, platinum compounds, etc. Examples of organotin compounds include dibutyltin dilaurate, dioctyltin dilaurate, dibutyltin dioctiate, dibutyltin diacetate, and other organotin compounds.
[0037] <Carrier resin> The silanol condensation catalyst is mixed with a resin or rubber as desired and used. Such resin or rubber (also called carrier resin) is not particularly limited, but the components described in the base polymer can be used. From the viewpoint of compatibility with the base polymer, the carrier resin is preferably at least one of the components constituting the base polymer, and preferably contains the same components as the base polymer.
[0038] <Additives> In the present invention, various additives generally used in various wiring materials such as electric wires, electric cables, and electric cords, and various resin molded products such as sheets, foams, tubes, and pipes may be contained within a range that does not impair the effects of the present invention. Examples of such additives include crosslinking assistants, antioxidants, lubricants, metal deactivators, plasticizers, flame retardants, and flame retardant assistants.
[0039] The antioxidant is not particularly limited, but examples thereof include amine antioxidants, phenol antioxidants, and sulfur antioxidants. Examples of amine antioxidants include 4,4'-dioctyldiphenylamine, N,N'-diphenyl-p-phenylenediamine, and polymers of 2,2,4-trimethyl-1,2-dihydroquinoline. Examples of phenol antioxidants include pentaerythritol-tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene. Examples of sulfur antioxidants include bis(2-methyl-4-(3-n-alkylthiopropionyloxy)-5-tert-butylphenyl)sulfide, 2-mercaptobenzimidazole and its zinc salt, pentaerythritol-tetrakis(3-lauryl-thiopropionate), etc. The antioxidant can be added in an amount of preferably 0.1 to 15.0 parts by mass, more preferably 0.1 to 10 parts by mass, per 100 parts by mass of the base polymer. The flame retardant is not particularly limited, and examples thereof include bromine-based flame retardants, chlorine-based flame retardants, etc. The content of the flame retardant is appropriately set within a range that does not impair the effects of the present invention.
[0040] [Manufacturing method of wiring material] The method for producing a wiring material of the present invention (hereinafter sometimes referred to as the production method of the present invention) will be described below. The manufacturing method of the present invention is a manufacturing method of a wiring material having a crosslinked coating layer of a silane crosslinked polymer mixture on the outer peripheral surface of a conductor, comprising the steps of: In preparing a silane crosslinkable polymer mixture using 100 parts by mass of a base polymer, 0.01 to 0.6 parts by mass of an organic peroxide, 0.5 to 15 parts by mass of a silane coupling agent, 0.5 to 400 parts by mass of an inorganic filler, and a silanol condensation catalyst, a silane master batch prepared by melt-mixing a part of the base polymer with the organic peroxide, the silane coupling agent, and the inorganic filler in the above-mentioned mixing ratio at a temperature equal to or higher than the decomposition temperature of the organic peroxide, and a catalyst master batch prepared by melt-mixing the remainder of the base polymer and the silanol condensation catalyst are mixed to prepare a silane crosslinkable polymer mixture, The prepared silane crosslinkable polymer mixture is introduced into an extruder to coat the outer peripheral surface of the conductor; The obtained coated conductor is directly introduced from the extruder into a pressurized environment of 0.05 to 0.25 MPa higher than normal pressure, and cooled with a liquid medium in the pressurized environment until the surface temperature of the coated conductor becomes 100°C or lower, and then withdrawn into a normal pressure environment.
[0041] As described above, in the manufacturing method of the present invention, a coated conductor obtained by coating the outer peripheral surface of a conductor with a silane crosslinkable polymer mixture (molding material) in which the above components are mixed at a specific mixing ratio in an extruder is directly introduced (discharged, discharged) from the extruder into a pressurized environment set at a specific pressure without being exposed to a normal pressure (0.1 MPa) environment (without passing through a normal pressure environment), and after cooling to a predetermined temperature while applying pressure, it is discharged (introduced, discharged) into the normal pressure environment. That is, in the manufacturing method of the present invention, the coated conductor is not discharged from the extruder into a normal pressure environment all at once, but is temporarily held in a pressurized environment, and is discharged into the normal pressure environment after the surface temperature of the coated conductor has decreased to a predetermined temperature. By subjecting the coated conductor to the pressurized cooling in the pressurized environment before exposing it to a normal pressure environment, even if unreacted silane coupling agent remains in the silane crosslinkable polymer mixture, the generation of bubbles (foaming) due to the volatilization of the silane coupling agent and the growth (expansion) of the bubbles can be suppressed. In addition, damage to the coated conductor molded in a molten mixture state can be suppressed.
[0042] Hereinafter, each step in the production method of the present invention will be described with reference to a production apparatus suitable for carrying out the production method of the present invention, particularly step (2) and step (3) described below. <Production apparatus suitable for carrying out the production method of the present invention> A suitable production apparatus may include a preparation apparatus for a silane crosslinkable polymer mixture, an extruder, and a pressurized cooler having a pressurized environment (area), and may be, for example, a production apparatus 1 shown in Fig. 1. Note that the preparation apparatus for a silane crosslinkable polymer mixture is not shown in Fig. 1, but it is actually connected to the extruder 2, and the silane crosslinkable polymer mixture can be prepared and transferred to the extruder 2. The extruder 2 is not particularly limited as long as it can co-extrude the conductor or core 11 of the wiring material and the silane crosslinkable polymer mixture, and a typical extruder can be used.
[0043] The pressure cooling section 3 is connected to the outlet (usually a die) of the extruder 2, and the coated conductor extruded from the extruder 2 is introduced without being exposed to a normal pressure environment (without passing through a normal pressure environment). Note that the connection between the outlet of the extruder 2 and the pressure cooling section 3 is preferably insulated. The pressurized cooling unit 3 has a configuration for realizing the pressurized environment (area) and cooling of the coated conductor defined in step (3), and examples thereof include a configuration having a pressurizing mechanism and a liquid medium cooling mechanism (neither of which is shown in FIG. 1) provided in the internal space, or a configuration having a pressurizing mechanism provided in the internal space and a liquid medium cooling mechanism (neither of which is shown in FIG. 1) provided in or near the outlet portion 3A of the pressurized cooling unit 3. Examples of the pressurizing mechanism include a pressure device, a device for filling or circulating a liquid medium in a pressurized state, a device for introducing compressed gas and maintaining pressure, etc. On the other hand, examples of the liquid medium cooling device include a liquid medium injection device (spray nozzle, sprinkler, etc.) that continuously or intermittently injects (sprays) the liquid medium into the coated conductor introduced into the pressurized cooling part 3 in the pressurized cooling part 3, a device that continuously or intermittently applies (sprays) the liquid medium flowed out in a rod shape in the pressurized cooling part 3 to the coated conductor introduced into the pressurized cooling part 3, a liquid medium injection device (spray nozzle, etc.) that continuously or intermittently injects (sprays) the liquid medium from the outlet part 3A or its vicinity to the coated conductor led to the pressurized cooling part 3, a liquid medium reflux device, a liquid medium storage device, a reflux liquid medium cooling device, etc. The pressurized cooling part 3 is preferably a pressure device that has a liquid medium spray device built in or attached (to the outlet part 3A or its vicinity), a device that fills or circulates the liquid medium in a pressurized state, a device that introduces compressed gas to maintain pressure, etc. In particular, in a manufacturing apparatus suitable for carrying out the manufacturing method of the present invention, a clearance can be provided between the outlet part (seal part or packing part) 3A of the pressurized environment and the outer peripheral surface of the coated conductor to be led out, and therefore a pressure device having a built-in or attached liquid medium spray device is preferred in terms of simple device configuration and reduced equipment costs. The clearance is not particularly limited, but is appropriately determined within a range in which the pressure of the pressurized environment can be maintained within the above range, taking into consideration, for example, the size of the coated conductor (outer diameter and cross-sectional area) and the set pressure of the pressurizing mechanism. As an example of the clearance, it can be 0.1 mm or more, and the upper limit can be 2.0 mm or less. The liquid medium is not particularly limited, but examples thereof include water, various solvents (for example, refrigerants such as ethylene glycol), and mixtures of water and alcohol, etc., with water being preferred in terms of low cost and high safety. The pressurized cooling unit 3 is configured to be able to cool the surface temperature of the coated conductor to 100°C or lower, and conditions such as the residence time of the coated conductor in the pressurized environment (dimensions of the internal space, rotation speed of the extruder (conveying speed of the coated conductor)), temperature or amount of the liquid medium, etc. are appropriately set and adjusted. The outlet portion 3A of the pressurized cooling portion 3 is open to a normal pressure environment. The suitable manufacturing apparatus 1 may include a winding device (not shown) or the like.
[0044] <Process (1)> In the manufacturing method of the present invention, first, a step (1) is carried out in which a silane crosslinkable polymer mixture (molding material) is prepared using 0.01 to 0.6 parts by mass of an organic peroxide, 0.5 to 15 parts by mass of a silane coupling agent, 0.5 to 400 parts by mass of an inorganic filler, and a silanol condensation catalyst relative to 100 parts by mass of a base polymer. In this step (1), a silane master batch (Silane MB) and a catalyst master batch (Catalyst MB) are separately prepared, and the two master batches are mixed together. Specifically, the following steps (a) to (c) are carried out. Step (a): A part of a base polymer, 0.01 to 0.6 parts by mass of an organic peroxide, and a silane 0.5 to 15 parts by mass of a coupling agent and 0.5 to 400 parts by mass of an inorganic filler The above-mentioned parts are melt-mixed at a temperature equal to or higher than the decomposition temperature of the organic peroxide to prepare Silane MB. The process Step (b): The remainder of the base polymer is melt mixed with a silanol condensation catalyst to form catalyst MB. Preparation process Step (c): The silane MB and the catalyst MB are melt-mixed to prepare a silane crosslinkable polymer mixture. Manufacturing process
[0045] The base polymer is used (mixed) in step (a) and step (b), and the total amount mixed in step (a) and the amount mixed in step (b) is 100 parts by mass. The ratio of the base polymer mixed in step (a) is preferably 60 to 95% by mass of the 100% by mass of the base polymer mixed in steps (a) and (b), and more preferably 70 to 95% by mass in order to establish a sufficient crosslinked structure and achieve both high levels of heat resistance and mechanical properties. The remainder of the base polymer (type of polymer) mixed in step (b) is appropriately determined depending on the portion of the base polymer mixed in step (a).
[0046] In the production method of the present invention, when the base polymer contains two or more components, the content of each component is the same as the content described above as the composition of the base polymer.
[0047] In step (a), the amount of organic peroxide mixed is 0.01 to 0.6 parts by mass relative to 100 parts by mass of the base polymer. By mixing the organic peroxide in the above content, the silane coupling agent and the base polymer can be effectively grafted, and the amount of remaining unreacted silane coupling agent can be reduced. As a result, the degree of crosslinking can be increased to form a crosslinked coating layer that is less susceptible to scratches. In addition, the crosslinking reaction between polymers can be suppressed to suppress the generation of gel-like surface bumps (projecting aggregates caused by crosslinked gel, etc.). The amount of organic peroxide mixed is preferably 0.03 to 0.5 parts by mass, more preferably 0.05 to 0.2 parts by mass, from the viewpoints of reducing the amount of remaining unreacted silane coupling agent and suppressing the generation of surface bumps.
[0048] Since the silane coupling agent is less likely to volatilize even if it remains during extrusion molding due to the coexistence of the inorganic filler, the mixing amount in the manufacturing method of the present invention can be set to be larger, and as a result, a crosslinked coating layer that forms a sufficient crosslinked structure and exhibits excellent mechanical strength and heat resistance can be realized. Specifically, the amount of the silane coupling agent mixed is 0.5 to 15 parts by mass relative to 100 parts by mass of the base polymer. When the silane coupling agent is mixed in the above content, the amount of the remaining unreacted silane coupling agent is reduced, and the generation of bubbles (foaming) can be suppressed. In addition, a sufficiently dense crosslinked structure can be formed, and excellent mechanical strength and heat resistance can be realized. Furthermore, the generation of surface bumps caused by the condensation product of the silane coupling agent can be suppressed, and excellent appearance characteristics can be realized. The amount of the silane coupling agent mixed is preferably 1.0 to 10 parts by mass, more preferably 2.0 to 6.0 parts by mass, and even more preferably 2.0 to 4.0 parts by mass relative to 100 parts by mass of the base polymer, in order to highly suppress the generation of bubbles while building a sufficiently dense crosslinked structure, and further to realize excellent appearance characteristics, mechanical strength, and heat resistance.
[0049] The amount of inorganic filler mixed is 0.5 to 400 parts by mass relative to 100 parts by mass of the base polymer, from the viewpoints of being able to suppress the volatilization of the silane coupling agent, and being able to realize a crosslinked coating layer exhibiting excellent mechanical strength and heat resistance, and being able to realize excellent appearance characteristics by suppressing the generation of surface bumps caused by the aggregation of the inorganic filler. The amount of inorganic filler mixed is preferably 3 to 200 parts by mass, more preferably 5 to 150 parts by mass, and even more preferably 5 to 120 parts by mass relative to 100 parts by mass of the base polymer, from the viewpoints of being able to further improve the mechanical strength, heat resistance, and appearance characteristics while suppressing the volatilization of the silane coupling agent.
[0050] The amount of the silanol condensation catalyst to be mixed is not particularly limited and can be set appropriately. For example, it is preferably 0.01 to 0.5 parts by mass, more preferably 0.03 to 0.3 parts by mass, and even more preferably 0.05 to 0.15 parts by mass, relative to 100 parts by mass of the base polymer.
[0051] The antioxidant may be contained when carrying out step (c), and may be mixed in any step. It is preferable to mix the antioxidant in step (b) in order to efficiently generate and progress the grafting reaction between the silane coupling agent and the base polymer without inhibiting it. When mixing in step (a), the amount of the antioxidant mixed is preferably 0.5 parts by mass or less per 100 parts by mass of the base polymer. Each of the various additives may be mixed in either step (a) or step (b).
[0052] (Step (a)) In step (a), a part of the base polymer, an organic peroxide, a silane coupling agent, and an inorganic filler are melt-mixed at the above-mentioned mixing ratio at a temperature equal to or higher than the decomposition temperature of the organic peroxide to prepare a molten mixture, silane MB. This melt-mixing causes a grafting reaction between the silane coupling agent and the base polymer, and a silane MB containing a silane crosslinkable resin (silane graft polymer) to which the silane coupling agent is grafted can be prepared. In this step, the mixing amount is set within the above-mentioned range, so that excessive crosslinking reaction between the base polymers (generation of surface bumps) can be prevented while suppressing the volatilization and self-condensation of the unreacted silane coupling agent. A part of the inorganic filler can also be mixed in the step (b) described below.
[0053] In step (a), the temperature (also called mixing temperature) at which the above components are melt-mixed (also called melt-kneading or kneading) is equal to or higher than the decomposition temperature of the organic peroxide, preferably the decomposition temperature of the organic peroxide + (25 to 110) ° C, more preferably 150 to 230 ° C, and even more preferably 175 to 210 ° C. Here, the decomposition temperature of the organic peroxide, which is the standard for the melt-mixing temperature, is the temperature in an environment of normal pressure (about 0.1 MPa). At the above mixing temperature, the above components melt, and the organic peroxide decomposes and acts to proceed with the necessary grafting reaction. Other conditions, such as the mixing time, can be set appropriately. For example, the mixing time can be 1 to 25 minutes, and is preferably 3 to 20 minutes.
[0054] The mixing method is not particularly limited as long as it is a method that is usually used for mixing rubber, plastics, etc. As the mixing device, for example, a single screw extruder, a twin screw extruder, a roll, a Banbury mixer, or various kneaders, etc. are used, and a closed type mixer such as a Banbury mixer or various kneaders is preferred. The method of mixing the base polymer is not particularly limited. For example, the base polymer may be prepared in advance and used, or each component may be used separately.
[0055] In step (a), it is preferable to melt-mix the above-mentioned components without substantially mixing a silanol condensation catalyst. This can suppress the condensation reaction of the silane coupling agent. In addition, it is easy to melt-mix and can obtain a desired shape during extrusion molding. Here, "without substantially mixing a silanol condensation catalyst" does not mean that the silanol condensation catalyst that is inevitably present is excluded, but means that it may be present to an extent that the above-mentioned problems caused by the silanol condensation of the silane coupling agent do not occur. For example, in step (a), the silanol condensation catalyst may be present in an amount of 0.01 parts by mass or less relative to 100 parts by mass of the base polymer.
[0056] In step (a), it is preferable that the crosslinking aid is not substantially mixed in. If the crosslinking aid is not substantially mixed in, a crosslinking reaction between the base polymers during melt mixing can be prevented.
[0057] In the manufacturing method of the present invention, the mixing order of each component in step (a) is not specified, and the above components may be mixed in any order. For example, the above components can be melt-mixed at once, and the inorganic filler and the silane coupling agent can be mixed in advance in the following mixing order in the following steps (a-1) and (a-2). Step (a-1): A step of mixing an inorganic filler and a silane coupling agent to prepare a mixture. Process Step (a-2): The mixture obtained in step (a-1) and all or a part of the base polymer are mixed together. In the presence of organic peroxide, it dissolves at a temperature above the decomposition temperature of the organic peroxide. Melting and mixing
[0058] (Process (a-1)) In step (a-1), by premixing the inorganic filler and the silane coupling agent, a silane coupling agent bonded or adsorbed to the inorganic filler by a weak bond and a silane coupling agent bonded or adsorbed to the inorganic filler by a strong bond can be formed in a well-balanced manner. As a result, the silane coupling agent adheres or bonds to the inorganic filler, making it difficult to volatilize even at high temperatures, and the effect of suppressing foaming can be obtained. In addition, the condensation reaction between unadsorbed silane coupling agents during melt mixing in step (a-2) can be effectively prevented. In addition, the silane coupling agent attached or bonded to the inorganic filler can be uniformly dispersed in the molten base polymer during melt mixing in step (a-2), making the crosslinking by the silane coupling agent denser. As a result, a crosslinked coating layer can be produced that exhibits better appearance characteristics while further improving mechanical properties (mechanical strength) and heat resistance due to the cooperation of the inorganic filler. Here, examples of the weak bond with the inorganic filler include interactions due to hydrogen bonds, interactions between ions, partial charges or dipoles, and actions due to adsorption. Further, examples of strong bonds with inorganic fillers include chemical bonds with sites on the surface of the inorganic filler that can form chemical bonds.
[0059] The mixing method and conditions in step (a-1) are not particularly limited, but examples of the method and conditions include a method and method of mixing by a dry or wet method using a known mixer, kneader, etc., usually at a temperature below the decomposition temperature of the organic peroxide, preferably 10 to 60°C, more preferably around room temperature (20 to 25°C), for several minutes to several hours. Among them, dry mixing (dry blending) at a temperature below the decomposition temperature of the organic peroxide is preferred. Other conditions for dry mixing are appropriately determined.
[0060] In step (a-1), a base polymer can also be mixed as long as the temperature is maintained below the decomposition temperature. The organic peroxide may be present during the melt mixing in step (a-2), and may be mixed in step (a-2), but is preferably mixed in step (a-1).
[0061] (Process (a-2)) Next, the mixture obtained in step (a-1), all or a part of the base polymer, and the remaining components not mixed in step (a-1) are melt-mixed in the presence of an organic peroxide at a temperature equal to or higher than the decomposition temperature of the organic peroxide to prepare silane MB (step (a-2)). In the melt mixing in this step, it is possible to prevent the excessive crosslinking reaction (generation of gel particles) between the base polymers while suppressing the volatilization, expansion, and further self-condensation of the above-mentioned silane coupling agent. The melt mixing method and conditions in this step (a-2) are not particularly limited, and the melt mixing method and conditions in the above step (a) can be applied.
[0062] In step (a-2), the silane coupling agent and the base polymer may undergo a grafting reaction in at least the following manner. That is, the silane coupling agent bonded to or adsorbed on the inorganic filler by a weak bond is detached from the inorganic filler and undergoes a grafting reaction on the base polymer. The crosslinked structure formed in step (4) described later from this manner does not incorporate the inorganic filler, and is usually a crosslinked structure via a silanol condensate between the silane coupling agents. In addition, the silane coupling agent bonded to or adsorbed on the inorganic filler by a strong bond undergoes a grafting reaction on the base polymer while maintaining the bond or adsorption with the inorganic filler. The crosslinked structure formed in step (4) described later from this manner incorporates the inorganic filler, and is a crosslinked structure via the silane coupling agent bonded to the inorganic filler as the starting point. By mixing the crosslinked structures in both of the above manners, a highly developed crosslinked structure including a crosslinked structure involving the inorganic filler in the silane crosslinked resin molded body forming the crosslinked coating layer can be constructed.
[0063] In this way, step (a) is carried out to prepare a silane MB. This MB contains a reaction mixture of a base polymer, a silane coupling agent, and an inorganic filler, and contains a silane graft resin in which the silane coupling agent and the base polymer are grafted to such an extent that the MB can be molded in step (2) described below. The silane coupling agent grafted to the base polymer includes those that are bonded or adsorbed to the inorganic filler at their silanol condensable reaction sites. In addition, the silane crosslinkable resin forms a crosslinked structure via a silanol condensate between the silane coupling agents by the final crosslinking caused by contact with water (step (4)) described below.
[0064] (Step (b)) In the process of the present invention, either independently of step (a) or subsequent to step (a), catalyst MB is prepared by melt mixing the remainder of the base polymer (the carrier resin) with a silanol condensation catalyst.
[0065] The mixing ratio of the carrier resin and the silanol condensation catalyst is not particularly limited, but is preferably set so as to satisfy the above-mentioned mixing amount. The melt mixing method and conditions in step (b) are not particularly limited, and the melt mixing method and conditions in step (a) can be applied. For example, the mixing temperature may be equal to or higher than the melting temperature of the carrier resin, and may be 120 to 200°C, and preferably 160 to 200°C. Other conditions, such as the mixing time, may be appropriately set. For example, the mixing time may be 1 to 25 minutes, and preferably 3 to 20 minutes.
[0066] In step (b), other resins can be used as carrier resins in place of or in addition to the remainder of the base polymer. When the carrier resin is other resins, the grafting reaction in step (a) can be accelerated and lumps are less likely to occur during molding. The amount of other resins mixed is preferably 1 to 60 parts by mass, more preferably 2 to 50 parts by mass, and even more preferably 2 to 40 parts by mass, based on 100 parts by mass of the base polymer.
[0067] (Process (c)) In the production method of the present invention, next, the silane MB and the catalyst MB are mixed to prepare a silane-crosslinkable polymer mixture (also called a master batch mixture) as a molding material. The mixing method is not particularly limited, but it is preferable to mix both masterbatches in a non-molten state, and more preferably to dry blend them. The method and conditions for mixing in a non-molten state and dry blending are not particularly limited, and for example, premixing in step (a-1), particularly dry mixing, is preferred, and the above mixing conditions can be adopted without any particular restrictions. In the manufacturing method of the present invention, both masterbatches can also be melt-mixed in step (c). The melt-mixing in this case is basically the same as that in step (a), and mixing is performed at a temperature at which at least the base polymer melts. The mixing conditions in step (c) are not particularly limited, and the mixing conditions in step (a) can be applied. The melting temperature is appropriately selected according to the melting temperature of the base polymer or the carrier resin, and is, for example, preferably 80 to 250°C, more preferably 100 to 240°C. Other conditions, such as the mixing time, can be appropriately set. However, when melt-mixing in step (c), it is preferable that the silane MB and catalyst MB are not kept in a high temperature state for a long time in a mixed state in order to avoid a silanol condensation reaction.
[0068] In this manner, steps (a) to (c) (step (1)) are carried out to prepare a silane crosslinkable polymer mixture as a mixture of silane MB and catalyst MB. The silane crosslinkable polymer mixture contains the above-mentioned silane crosslinkable resin, silanol condensation catalyst, etc. In the silane graft resin, the silane coupling agent's silanol condensation-capable reactive site may be bonded or adsorbed to an inorganic filler, but is not silanol condensed. Therefore, the silane graft resin contains a silane graft resin in which a silane coupling agent bonded or adsorbed to an inorganic filler and a base polymer are grafted, and a silane graft resin in which a silane coupling agent not bonded or adsorbed to an inorganic filler and a base polymer are grafted. In this way, the silane crosslinkable resin is an uncrosslinked body in which a silanol condensation-capable reactive site of the silane coupling agent is not silanol condensed. Although some crosslinking (partial crosslinking) may occur in step (c), the obtained silane crosslinkable polymer mixture is one that maintains at least the moldability in the molding in step (2).
[0069] <Process (2)> In the production method of the present invention, the outer peripheral surface of the conductor is then coated with the silane-crosslinkable polymer mixture obtained in step (1) to produce a coated conductor. Step (2) may be a method capable of disposing (molding) the silane crosslinkable polymer mixture in a tubular shape on the outer peripheral surface of the conductor to cover the outer peripheral surface of the conductor, and typically employs extrusion molding using an extruder capable of co-extrusion molding with the conductor.
[0070] As the conductor used in step (2), various conductors and cores can be used depending on the type and use of the wiring material. As such conductors and cores, those usually used for wiring materials can be used. Examples of conductors used for wiring materials such as insulated electric wires include single wires or twisted wires (wires in which tensile strength fibers are vertically attached or twisted) made of soft copper, copper alloy, or aluminum. In addition to bare wires, tin-plated wires or those having an enamel-coated insulating layer can also be used. Examples of cores used for wiring materials such as cables include optical fiber cores, single-core cores made of a single insulated electric wire or multi-core cores made of a bundle of multiple insulated electric wires, and further, single insulated electric wires or multiple insulated electric wire bundles coated with an insulating layer or wound with an insulating tape. The outer diameter of the conductor is not particularly limited and is appropriately determined depending on the type, use, characteristics, etc. of the wiring material. For example, for insulated electric wires, it can be 0.5 to 20 mm, and for various cables, it can be 1.0 to 25 mm. The conductor may have a layer other than the crosslinked coating layer, a reinforcing tape, etc. on its surface.
[0071] The extrusion conditions (melt mixing conditions) are not particularly limited as long as the silane crosslinkable polymer mixture can be melt mixed and then placed on the outer peripheral surface of the conductor, and the silanol condensation reaction does not proceed rapidly, and for example, the melt mixing conditions of step (a) can be applied. More specifically, the temperature of the extruder is preferably about 140 to 200°C in the cylinder and about 160 to 200°C in the die, although it depends on the type of base polymer, the take-up speed of the conductor, etc. The extrusion conditions (molding conditions) can also be appropriately determined. For example, the rotation speed and molding speed (linear speed) in extrusion molding are not particularly limited, and can be appropriately set according to the characteristics or performance of the extruder, the extrusion amount (coating amount), and further the productivity. More specifically, the rotation speed of the extruder can usually be set to 20 to 60 rpm, but in the present invention, the rotation speed can be set to 60 rpm or more to achieve high productivity. On the other hand, the linear speed can usually be set to 1 to 20 m / min, but like the rotation speed, it can also be set to 20 m / min or more to achieve high productivity. The internal pressure of the extruder is not particularly limited, but is usually set higher than the pressure of the pressurized environment in step (3) described below, and is preferably, for example, 1.0 MPa or more higher than normal pressure (0.1 MPa) (normal pressure + 1.0 MPa or more). The amount of the silane crosslinkable polymer mixture coated on the outer periphery of the conductor (extrusion thickness) is not particularly limited and is appropriately determined depending on the type, application, and characteristics of the wiring material, and is, for example, about 0.15 to 5 mm.
[0072] This step (2) can be carried out simultaneously with or consecutively to the above step (c). For example, a series of steps can be adopted in which silane MB and catalyst MB are premixed just before the extruder (step (c)) and then melt-mixed in a coating device, or silane MB and catalyst MB are separately charged into a coating device and then melt-mixed (step (c)), and then co-extruded (step (2)) onto the outer periphery of a conductor or the like. In step (2), the conductor may be preheated before being introduced into the extruder. However, in the production method of the present invention that employs the silane crosslinking method, it is preferable in terms of productivity, etc. to introduce the conductor into the extruder in an unheated state.
[0073] In this way, a coated conductor is obtained in which the outer peripheral surface of the conductor is coated with the silane crosslinkable polymer mixture (molten mixture). The silane crosslinkable polymer mixture (molten mixture) coating the outer peripheral surface of the conductor has the same composition as the silane crosslinkable polymer mixture (master batch mixture) except that it is a molten mixture. Incidentally, the silane crosslinkable resin of the silane crosslinkable polymer mixture may be partially crosslinked, but even in that case, it is in an uncrosslinked state or a partially crosslinked state that retains moldability that can be molded in step (2). Therefore, the uncrosslinked molded body or the partially crosslinked state of the silane crosslinkable polymer mixture (molten mixture) coating the outer peripheral surface of the conductor becomes a crosslinked molded body by final crosslinking, forming a crosslinked coating layer.
[0074] <Process (3)> In the production method of the present invention, the coated conductor obtained in step (2) is then directly introduced from the extruder into a pressurized environment of 0.05 to 0.25 MPa higher than normal pressure, and cooled with a liquid medium in the pressurized environment until the surface temperature of the coated conductor becomes 100°C or lower, and then withdrawn into a normal pressure environment. In the manufacturing method of the present invention, the coated conductor obtained in step (2) is introduced directly into a pressurized environment from the extruder without being exposed to a normal pressure environment (via a normal pressure environment). The method of introducing the coated conductor is not particularly limited as long as it can directly introduce the coated conductor into a pressurized environment, and for example, when a manufacturing apparatus 1 shown in Fig. 1 is used, a method of introducing the coated conductor into a pressurized cooling section 3 connected to the outlet (die) of an extruder 2 can be mentioned.
[0075] The pressurized environment (area), the internal space of the pressurized cooling section 3 in the manufacturing apparatus 1, is set to a pressure 0.05 to 0.25 MPa higher than normal pressure, that is, a pressure of 0.15 MPa (normal pressure + 0.05 MPa) or more and 0.35 MPa (normal pressure + 0.25 MPa) or less. In this pressure range, a clearance can be provided between the pressurized environment, for example, the outlet section (seal section or packing section) 3A of the pressurized cooling section 3 and the outer peripheral surface of the coated conductor to be led out, and excessive contact with the discharged coated conductor can be suppressed. Even if a clearance is provided, a high-pressure state can be maintained with a small-scale and simple device configuration, and the volatilization of the silane coupling agent and the expansion of bubbles can be suppressed. As a result, a crosslinked coating layer that exhibits excellent appearance characteristics while maintaining high mechanical strength and high heat resistance due to the cooperation of the inorganic filler can be formed using a small-scale and simple device (reducing equipment costs) while suppressing the generation and expansion of voids. In order to achieve a higher level of balance between mechanical strength and heat resistance, suppression of void generation, and appearance properties, the pressure of the pressurized environment (area) is preferably a high pressure of 0.10 to 0.20 MPa (0.2 MPa to 0.30 MPa) higher than normal pressure, and more preferably a high pressure of 0.10 to 0.15 MPa (0.2 MPa to 0.25 MPa) higher than normal pressure.
[0076] In step (3), the coated conductor is cooled with a liquid medium in the pressurized environment (pressurized cooling section 3) until the surface temperature of the introduced coated conductor becomes 100°C or less. This allows efficient cooling to a predetermined temperature in a shorter time than air cooling, and allows for continuous production and high productivity production. In addition, the surface of the coated conductor melted in the extruder (surface of the silane crosslinkable polymer mixture) can be cooled and solidified to increase the surface strength. Therefore, even if the coated conductor led out from the pressurized environment (pressurized cooling section 3) comes into contact with the lead-out section 3A of the pressurized environment (pressurized cooling section 3), or even if the coated conductor led out from the pressurized environment is transported, for example, on a line, toward the next process, the surface of the coated conductor can be prevented from being scratched or damaged. As a result, a crosslinked coating layer that also exhibits excellent appearance characteristics can be formed. The cooling method can be performed by contacting the coated conductor introduced into the pressurized environment with a liquid medium. The contact method may be any method capable of lowering the surface temperature of the coated conductor, such as a method of continuously or intermittently applying (spraying) the liquid medium onto the coated conductor, a method of continuously or intermittently spraying (spraying) the liquid medium onto the coated conductor, or a method of immersing the coated conductor in the liquid medium. As an apparatus for carrying out the cooling method in step (3), the above-mentioned cooling mechanisms can be applied, but in terms of simplicity of equipment, it is preferable to cool the coated conductor introduced into the pressurized environment (pressurized cooling section 3) by continuously or intermittently spraying the liquid medium within the pressurized cooling section 3 or at or near the outlet section 3A. In terms of appearance characteristics in particular, it is preferable to cool the surface temperature of the coated conductor to 80° C. or lower, and more preferably to cool to 60° C. or lower. The surface temperature of the coated conductor can be measured within the pressurized environment (pressurized cooling section 3). However, it is preferable to measure the surface temperature of the coated conductor (wiring material precursor 12) led out from the lead-out section 3A of the pressurized environment (pressurized cooling section 3) using a non-contact infrared radiation thermometer, as this can be measured with a simple configuration.
[0077] In this step, after the surface temperature is cooled to 100°C or less as described above, the coated conductor is then led out (discharged, transported) from the pressurized environment (pressurized cooling section 3) to a normal pressure environment. The temperature of the normal pressure environment is not particularly limited, but is preferably 50°C or less, and more preferably about room temperature (25°C). The humidity of the normal pressure environment is not particularly limited, but if it is set high, the step (4) described below can be performed continuously. Even if water or a water mixture is used as the liquid medium in step (3), the silane crosslinkable polymer mixture arranged on the outer peripheral surface of the conductor usually does not cause or progress a silanol condensation reaction under conditions in which the surface temperature of the coated conductor is cooled to 100°C or less. Even if a silanol condensation reaction occurs due to the conditions adopted in step (3), the silanol condensation reaction does not reach completion and the coated conductor is in a partially crosslinked state. In this way, a coated conductor (wiring material precursor 12 in a partially crosslinked state) whose surface temperature is cooled to 100°C or less can be obtained. In the present invention, the cooling conditions in the pressurized environment (pressurized cooling section 3) can be adjusted to complete the silanol condensation reaction in the silane crosslinkable polymer mixture for final crosslinking (to produce a wiring material).
[0078] <Process (4)> In the manufacturing method of the present invention, the wiring material precursor 12 obtained in step (3) (wherein the silane-crosslinkable polymer mixture is in an uncrosslinked or partially crosslinked state) is contacted with water to finally crosslink the silane-crosslinkable polymer mixture. In this process, the silane crosslinkable polymer mixture (molten mixture) undergoes and advances (promotes) a silanol condensation reaction (dehydration condensation reaction) at the silanol condensable reactive sites of the silane coupling agent grafted to the base polymer, and finally undergoes a silane crosslinking reaction. In this way, a crosslinked coating layer (made of a silanol condensate) of the silane crosslinkable polymer mixture can be formed as a silane crosslinked polymer molded product in which the silane coupling agent is crosslinked by silanol condensation. The wiring material precursor 12 can be brought into contact with water by a normal method. The silanol condensation reaction proceeds even in a non-saturated steam atmosphere, in the presence of moisture, by simply leaving the wiring material precursor 12 in a room temperature environment, for example, at a temperature of about 20 to 25° C., and therefore, in the manufacturing method of the present invention, it is not necessary to actively bring the wiring material precursor 12 into contact with water in a saturated steam atmosphere or the like as in Patent Document 1. From the viewpoint of promoting the silanol condensation reaction (crosslinking reaction), it is preferable to actively bring the wiring material precursor 12 into contact with water. Examples of the contact method include methods (conditions) that are normally applied to the silane crosslinking method, such as a method of contacting the wiring material precursor 12 in a normal pressure environment, and specifically, examples of the contact method include exposure to a saturated steam atmosphere, exposure to a high humidity environment, immersion in room temperature water or hot water (for example, 50 to 90° C.), immersion in a moist heat bath, exposure to high temperature steam, and the like. Pressure may also be applied during the contact to allow moisture to penetrate the inside.
[0079] <Other processes> In the manufacturing method of the present invention, steps other than the above steps (1) to (4) can also be performed, such as a step of forming an adhesive layer around the conductor, an intermediate layer such as an insulating layer not corresponding to the above cross-linked coating layer, and a step of forming a sheath around the cross-linked coating layer not corresponding to the above cross-linked coating layer.
[0080] In the manner described above, a wiring material having a crosslinked coating layer of a silane crosslinkable polymer mixture on the outer peripheral surface of the conductor 11 is manufactured. The crosslinked coating layer is formed of a silane crosslinked polymer molded body made of a silanol condensate of the silane crosslinked polymer mixture prepared in step (1) by melt mixing in an extruder, coating, and then silanol condensation reaction. This silane crosslinked polymer molded body contains a crosslinked resin in which a base polymer (silane crosslinkable resin) is condensed through a siloxane bond. The silane crosslinked resin molded body contains an inorganic filler, and this inorganic filler may be bonded to the silane coupling agent of the crosslinked base polymer. Therefore, the silane crosslinked polymer molded body (crosslinked coating layer) contains at least a crosslinked resin in which a plurality of base polymers are bonded or adsorbed to the inorganic filler by the silane coupling agent, and bonded (crosslinked) through the inorganic filler and the silane coupling agent, and a crosslinked resin in which the silanol condensable reactive sites of the silane coupling agent grafted to the base polymer are hydrolyzed and undergo a silanol condensation reaction with each other (without the inorganic filler being involved) through the silane coupling agent (siloxane bond). In the silane crosslinking method in which the components are mixed in the above-mentioned amounts, a crosslinked structure between the base polymers (not involving inorganic filler) and a crosslinked structure involving the inorganic filler can be constructed in a well-balanced manner with high density, and a silane-crosslinked resin molded body with excellent appearance can be formed, which exhibits high mechanical strength and excellent heat resistance.
[0081] The silane crosslinked polymer molded body is formed by contacting the silane crosslinkable polymer mixture with water to cause a silanol condensation reaction, so the content of each of the above components in this molded body is usually the same as the content in the silane crosslinkable polymer mixture. However, in the silane crosslinked polymer molded body, the organic peroxide and the silanol condensation catalyst are usually decomposed. The content of the silane coupling agent is the same as the content before the silanol condensation reaction, and the content of the base polymer is the same as the content before crosslinking.
[0082] As described above, in the manufacturing method of the present invention, the coated conductor is pressurized and cooled in step (3), so that even if unreacted silane coupling agent remains in the silane crosslinkable polymer mixture (molten mixture) arranged on the outer peripheral surface of the conductor, the pressure and temperature in the pressurized environment can suppress the generation of bubbles (foaming) due to the volatilization of the silane coupling agent, and further the growth (expansion) of the bubbles. As a result, it is possible to suppress the generation of voids large enough to deteriorate the properties of the coating layer of the wiring material (for example, voids with a diameter of 40 μm or more) or a large number of voids, and the high mechanical strength and heat resistance exhibited by the crosslinked coating layer formed by the silane crosslinking method can be maintained without deterioration. Moreover, since the pressure in the pressurized environment in step (3) is set to be slightly higher than normal pressure as described above, the pressure in the pressurized environment is easily maintained. For example, there is no need to make the lead-out part for leading out the coated conductor from the pressurized environment highly airtight, and a clearance can be provided between the lead-out part (seal part or packing part) and the outer peripheral surface of the lead-out coated conductor. Therefore, contact between the covered conductor led out of the pressurized environment and the lead-out part (seal part or packing part) can be suppressed, and scratching and damage to the surface of the covered conductor (silane cross-linkable polymer mixture) can be prevented. Moreover, since the outer peripheral surface of the covered conductor led out in the pressurized environment is cooled to 100°C or less and cooled and solidified, scratching and damage to the surface can be prevented even if the covered conductor comes into contact with the lead-out part or during transportation of the covered conductor. Furthermore, in the manufacturing method of the present invention, since the silane coupling agent, the organic peroxide and the inorganic filler are mixed in a specific mixing ratio in step (1), it is possible to suppress excessive crosslinking reactions between base polymers (the occurrence of surface bumps), condensation reactions between silane coupling agents and aggregation of the inorganic filler. As a result, a crosslinked coating layer can be formed which has few voids, maintains high mechanical strength and excellent heat resistance, and also exhibits excellent appearance characteristics. Furthermore, the production method of the present invention can maintain the above-mentioned suppression of void generation and excellent appearance properties even when productivity is increased by increasing the rotation speed of the extruder, the conveying speed of the coated conductor, etc.
[0083] [Wiring material of the present invention] The wiring material produced by the production method of the present invention (also referred to as the wiring material of the present invention) has at least one crosslinked coating layer made of a crosslinked molded product of a silane crosslinkable polymer mixture on the outer peripheral surface of the conductor. The thickness of the crosslinked coating layer is not particularly limited and is appropriately determined depending on the type, use, characteristics, etc. of the wiring material, and is, for example, about 0.15 to 5 mm. As described above, this crosslinked coating layer has few large voids, has excellent appearance characteristics, and exhibits high mechanical strength and heat resistance. Since the crosslinked coating layer of this wiring material has a sufficient degree of crosslinking and exhibits high heat resistance, the wiring material of the present invention can be suitably used as a heat-resistant wiring material. The wiring material of the present invention may have any of various known configurations as long as it has the above-mentioned conductor and cross-linked coating layer. For example, it may have other layers such as an adhesive layer, a reinforcing layer, etc., as appropriate depending on the application, etc. EXAMPLES
[0084] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.
[0085] The compounds used in the examples and comparative examples are shown below. <Base polymer> Polyethylene: Evolu SP3010 (product name, manufactured by Prime Polymer, LLDPE) EVA resin: Evaflex V5274R (product name, manufactured by Dow Mitsui Polychemicals) EEA resin: NUC6510 (product name, manufactured by ENEOS NUC) EPDM: EPT3092PM (product name, manufactured by Mitsui Chemicals, diene component is ethylidene norbornene component) Styrene-based elastomer: Tuftec N504 (product name, manufactured by Asahi Kasei Corporation, SEBS) Oil: Diana Process Oil PW-90 (product name, manufactured by Idemitsu Kosan Co., Ltd., organic oil: paraffin oil) Fluororubber: AFLAS400E (product name, manufactured by AGC, tetrafluoroethylene-propylene copolymer rubber) Silicone rubber: ERASTOSIL R401-40S (product name, millable type silicone rubber, manufactured by Wacker Asahi Kasei Silicone Co., Ltd.) <Silane coupling agent> Silane coupling agent: KBM-1003 (product name, manufactured by Shin-Etsu Chemical Co., Ltd., vinyltrimethoxysilane) <Inorganic filler> Calcium carbonate: Softon 1200 (product name, manufactured by Bihoku Powder Industry Co., Ltd.) Fumed silica: AEROSIL 200 (product name, manufactured by Nippon Aerosil Co., Ltd.) <Organic peroxide> Organic peroxide: Perhexa 25B (trade name, NOF Corp., 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, decomposition temperature 154°C) <Silanol condensation catalyst> Silanol condensation catalyst: Adeka STAB OT-1 (trade name, manufactured by ADEKA Corporation, dioctyltin dilaurate) <Antioxidants> Antioxidant: Irganox 1010 (product name, manufactured by BASF, hindered phenol-based antioxidant)
[0086] (Examples 1 to 13 and Comparative Examples 1 to 9) Examples 1 to 13 and Comparative Examples 1 to 9 were carried out using the components shown in Tables 1 and 2 and the production apparatus 1 shown in FIG. The manufacturing equipment 1 has an extruder 2 with an L / D (ratio of effective screw length L to diameter D) of 24 and a screw diameter of 40 mm, and a pressurized cooling section 3 (length approximately 400 mm) directly connected to the die of this extruder 2. A circulating cooling device that injects water onto the coated conductor from the top of the pressurized cooling section 3 is installed in the pressurized cooling section 3 as a water injection device serving as a liquid medium cooling mechanism, and a non-contact infrared radiation thermometer (model number IT-545S, manufactured by HORIBA, Ltd.) is installed near the outlet 3A of the pressurized cooling section 3. In Tables 1 and 2, the numerical values for the mixed amount (content) of each example are in parts by mass unless otherwise specified. Furthermore, a blank for each component means that the mixed amount of the corresponding component is 0 parts by mass. In each of the Examples and Comparative Examples, a part of the base polymer (specifically, the component shown in the "Catalyst MB" column in Tables 1 and 2) was used as a carrier resin for catalyst MB in the mass ratio shown in the same column.
[0087] First, the inorganic filler and the silane coupling agent were charged in a 10 L Henschel mixer manufactured by Toyo Seiki Seisakusho Co., Ltd. in the mass ratios shown in Tables 1 and 2, and mixed at room temperature (25°C) for 1 hour (step (a-1)). Thus, the above components were dry-mixed to obtain a powder mixture. Next, the prepared powder mixture, the base polymer and the organic peroxide shown in the "Silane MB" column of Tables 1 and 2 were added to a kneader (volume 75 L) preheated to 100°C in the mass ratios shown in the same column, and mixed at 40 rpm for 5 minutes, and then finish kneaded (melt mixed) at 30 rpm for an additional 3 minutes. After confirming that the temperature of the mixture reached 180-200°C, which is higher than the decomposition temperature of the organic peroxide, the mixture was pelletized using a feeder-ruder and pelletizer to obtain Silane MB (step (a)).
[0088] On the other hand, the base polymer, antioxidant, and silanol condensation catalyst shown in the "Catalyst MB" column of Tables 1 and 2 were sequentially charged in the mass ratios shown in the same column into a kneader (volume 75 L) preheated to 80°C, mixed at 30 rpm for 5 minutes, and then finish kneaded (melt mixed) at 25 rpm for 3 minutes. After confirming that the temperature of the mixture reached about 160°C and the carrier resin was sufficiently melted, the mixture was pelletized using a feeder-ruder and pelletizer to obtain catalyst MB (step (b)).
[0089] Next, Silane MB and Catalyst MB were dry-blended in the mass ratios shown in the "Silane MB" and "Catalyst MB" columns of Tables 1 and 2 for 2 minutes at room temperature (25°C) using a stainless steel mixer (model PM-100P, manufactured by Mazera) just before extrusion molding to obtain a silane-crosslinkable polymer mixture as a master batch mixture (step (c), up to this point step (1)).
[0090] The obtained silane crosslinkable polymer mixture was introduced into an extruder 2 (screw temperature of the compression section: 150° C., die temperature shown in Table 1 or Table 2). While being melt-mixed in the extruder 2, the silane crosslinkable polymer mixture was coated on the outside of a 1 / 0.8A conductor 11 at a rotation speed shown in Table 1 or Table 2 to a thickness of 2 mm, thereby obtaining a coated conductor having an outer diameter of 4.8 mm (step (2)).
[0091] This coated conductor was directly introduced into the pressurized cooling section 3 (the clearance between the outlet section 3A and the coated conductor was 0.5 mm) directly connected to the die of the extruder 2, and water was sprayed from a water spraying device (not shown in FIG. 1 ) installed in the pressurized cooling section 3 onto the coated conductor in the pressurized cooling section 3 to cool the surface, and the coated conductor was discharged from the pressurized cooling section 3 to an atmospheric pressure environment. In this way, the coated conductor discharged from the extruder 2 was directly introduced into the pressurized cooling section 3 without being exposed to an atmospheric pressure environment, and after pressurized cooling, was discharged into an atmospheric pressure environment (temperature 23°C, relative humidity 50RH%) (step (3)). In Examples 1 to 13 and Comparative Examples 1 to 7 and 9, the velocity was 4 m per minute. 3 In Comparative Example 8, cooling water was not used and cooling was performed by air cooling. In step (3), the pressure in the pressurized cooling section 3 (the pressure at the outlet of the extruder 2) was measured with a general-purpose pressure gauge (model number G49D, manufactured by CDK) and recorded as the pressure in the pressurized cooling section 3. The surface temperature of the coated conductor immediately after being discharged from the outlet 3A of the pressurized cooling section 3 was measured with the above-mentioned infrared radiation thermometer and recorded as the surface temperature of the coated conductor. The measurement results are shown in the "Pressure of pressurized environment" and "Cooling temperature of surface" columns of Tables 1 and 2, respectively. The "Pressure of pressurized environment" column in each table shows the amount of increase in pressure from normal pressure (the difference (MPa) between the measured pressure and normal pressure). In the steps (2) and (3), the take-up speed was adjusted as needed so that the outer diameter was 4.8 mm. In Example 7, the rotation speed of the extruder 2 was increased, and the discharge amount of the silane crosslinkable polymer mixture was increased, so the take-up speed was increased accordingly.
[0092] This coated conductor was left in an atmosphere having a temperature of 60° C. and a humidity of 95% for 24 hours to come into contact with water (step (4)). In this manner, insulated wires having a crosslinked coating layer formed of the silane crosslinkable polymer mixture (crosslinked coating layer of the silane crosslinkable polymer mixture) on the outer circumferential surface of the conductor were produced.
[0093] The following tests were carried out on each of the produced insulated wires, and the results are shown in Tables 1 and 2.
[0094] <Test 1: Test to confirm the presence or absence of foaming> The conductor was removed from each manufactured electric wire, and the cross-linked coating layer was cut into rings. The annular cross sections were then observed under a microscope (VHX-8000, manufactured by Keyence Corporation) to confirm the presence or absence of bubbles. The size of the bubbles was determined as the major axis of the hole corresponding to the air bubble. The annular cross sections of the cross-linked coating layer were taken at five locations at 100 mm intervals along the longitudinal direction of the cross-linked coating layer, and the total number of bubbles observed at the five locations was determined as the number of bubbles. This test was conducted to evaluate the inhibition of the generation or growth of voids in the crosslinked coating layer, and was evaluated according to the following criteria. AAA: No bubbles greater than 20 μm in size were observed (excellent) AA: Only one bubble measuring 20 μm or more and less than 40 μm in size was observed (very good) A: Two or three bubbles measuring 20 μm or more and less than 40 μm in size were observed (excellent). B: Four or five bubbles measuring 20 μm or more and less than 40 μm in size were observed (good). C: Six or more bubbles measuring 20 μm or more but less than 40 μm in size, or one or more bubbles measuring 40 μm or more in size were observed (failed)
[0095] <Test 2: Surface scratch check test> A 200 mm section was taken from each of the manufactured insulated electric wires, and its surface was observed under a microscope (VHX-8000, manufactured by Keyence Corporation). Linear depressions on the surface with a length of 10 mm or more were evaluated as scratches, and the depth of any scratches observed was measured using the microscope's three-dimensional measurement function. The depth of the deepest part among the measured depths was regarded as the depth of the scratch. This test is one of the tests for evaluating the appearance characteristics (scratch resistance) of the crosslinked coating layer, and was evaluated according to the following criteria. AAA: No scratches greater than 10 μm deep were observed (excellent) AA: The deepest scratch is between 10 μm and 20 μm deep (very good). A: The deepest scratch is between 20μm and 30μm deep (excellent) B: The deepest scratch is between 30 μm and 40 μm deep (good). C: The deepest scratch is 40 μm or more (failed)
[0096] <Test 3: Surface irregularity check test> A 200 mm section was taken from each of the manufactured insulated wires, and its surface was observed under a microscope (VHX-8000, manufactured by Keyence Corporation). The height of the protrusions present on the surface was measured using the three-dimensional dimension measuring function of the microscope, and the total number of protrusions protruding from the smooth surface of the cross-linked coating layer to a height of 50 μm or more and less than 100 μm was counted as surface bumps. Here, the number of "surface bumps" was defined as the total number of "surface bumps" caused by excessive crosslinking between polymers, "surface bumps" caused by condensation products of the silane coupling agent, and "surface bumps" caused by aggregates of inorganic filler. This test is one of the tests to evaluate the appearance characteristics of the crosslinked coating layer (the ability to suppress the occurrence of surface bumps), and was evaluated according to the following criteria. AAA: No surface irregularities greater than 50 μm in height were observed (excellent) AA: Only one surface bump measuring 50 μm or more and less than 100 μm in height was observed (very good) A: Two or three surface irregularities measuring 50 μm or more and less than 100 μm in height were observed (excellent). B: Four or five surface irregularities measuring 50 μm or more and less than 100 μm in height were observed (good). C: Six or more surface irregularities measuring 50 μm or more but less than 100 μm in size, or one or more surface irregularities measuring 100 μm or more in height were observed (failed)
[0097] <Test 4: Tensile strength test> The conductor was removed from each of the manufactured insulated wires to obtain a tubular test piece (inner diameter 0.8 mm, outer diameter 4.8 mm), and the tensile strength (MPa) was measured in accordance with JIS C 3005 under conditions of a gauge length of 20 mm and a tensile speed of 200 mm / min. In this test, a tensile strength (mechanical strength) of 10.0 MPa or more is considered to be a pass.
[0098] <Test 5: Heat deformation test> For each of the manufactured insulated wires, a heat deformation test was performed based on the test method of JIS C 3005, in which the insulated wire was preheated at 120°C for 30 minutes and then the measurement temperature was 120°C, the heating time was 30 minutes, and a load was 500gf (4.9N). In this test, the heat deformation test is a test for evaluating the degree of crosslinking (heat resistance) of the crosslinked coating layer, and was evaluated according to the following criteria: In the test, a heat deformation rate of 30% or less was considered to be pass (a sufficiently dense crosslinked structure was constructed as the crosslinked coating layer), and a deformation rate of more than 30% was considered to be fail (a sufficiently dense crosslinked structure was not constructed as the crosslinked coating layer). AAA: Deformation rate is 15% or less (very good) AA: Deformation rate is over 15% and up to 23% (excellent) A: Deformation rate is more than 23% and less than 30% (good) B: Deformation rate is more than 30% and less than 40% (failed) C: Deformation rate exceeds 40% (failure)
[0099] [Table 1]
[0100] [Table 2]
[0101] The results in Tables 1 and 2 reveal the following: In Comparative Examples 1 to 9, which do not satisfy the conditions in the manufacturing method of the present invention, the appearance characteristics cannot be improved, and the occurrence of voids or expansion cannot be suppressed, and furthermore, a crosslinked coating layer exhibiting sufficient mechanical strength and heat resistance cannot be realized. For example, Comparative Examples 1 and 2, which do not satisfy the mixed amount of organic peroxide, have sufficient mechanical strength, but cannot form a crosslinked coating layer having a sufficient degree of crosslinking (heat resistance) or a crosslinked coating layer suppressing the occurrence of surface bumps. In addition, Comparative Examples 3 and 4, which do not satisfy the mixed amount of silane coupling agent, cannot form a crosslinked coating layer having a sufficient degree of crosslinking or a crosslinked coating layer suppressing the occurrence of voids, and Comparative Example 4 does not have sufficient mechanical strength. Furthermore, Comparative Examples 5 and 9, which do not satisfy the mixed amount of inorganic filler, have sufficient mechanical strength, but cannot form a crosslinked coating layer suppressing the occurrence of surface bumps or a crosslinked coating layer having a sufficient degree of crosslinking. In addition, Comparative Example 6, in which the pressure of the pressurized environment (pressurized cooling section 3) is too low, cannot sufficiently suppress the occurrence of voids and expansion, and also does not have sufficient mechanical strength. On the other hand, in Comparative Example 7, in which the pressure of the pressurized environment (pressurized cooling section 3) was too high, the cross-linked coating layer had deep scratches due to violent contact with the outlet 3A of the pressurized environment (pressurized cooling section 3), and also did not exhibit sufficient mechanical strength. In addition, in Comparative Example 7, in order to increase the pressure of the pressurized environment, it was necessary to narrow the clearance between the outlet 3A of the pressurized environment (pressurized cooling section 3) and the coated conductor, which led to the complexity and size of the manufacturing equipment 1. In Comparative Example 8, in which the cooling of the pressurized environment (pressurized cooling section 3) was insufficient, the cross-linked coating layer had deep scratches due to contact with the manufacturing equipment such as the outlet 3A of the pressurized environment (pressurized cooling section 3), and also did not exhibit sufficient mechanical strength.
[0102] In contrast, in a specific silane crosslinking method using a silane crosslinkable polymer mixture containing a specific ratio of organic peroxide, a silane coupling agent, and an inorganic filler, a coated conductor in which the silane crosslinkable polymer mixture is coated on the outer peripheral surface of the conductor is directly introduced from an extruder into a pressurized environment at a specific pressure, and the surface temperature is pressurized and cooled with a liquid medium to 100 ° C or less, and then introduced into a normal pressure environment. In all of Examples 1 to 13, foaming of unreacted silane coupling agent and further expansion are prevented, and the occurrence of large voids is suppressed, while the occurrence of scratches and surface bumps is also suppressed, and a crosslinked coating layer exhibiting excellent appearance characteristics, heat resistance, and even high mechanical strength can be realized. A crosslinked coating layer exhibiting such excellent characteristics can also be realized by increasing the rotation speed of the extruder to increase the productivity of the wiring material, as in Example 7. Furthermore, in the manufacturing method of the present invention, the pressure is set to a low level that allows the pressure of the pressurized environment to be maintained even if there is sufficient clearance between the outlet 3A of the pressurized environment (pressurized cooling section 3) and the coated conductor, so that a simple structure can be achieved without increasing the complexity and size of the manufacturing equipment, thereby reducing equipment costs (manufacturing costs of the wiring material). [Explanation of symbols]
[0103] 1 Manufacturing equipment 2. Extruder 3. Pressurized cooling section 3A Derivation part 11 Conductor or core 12 Wiring material precursor
Claims
1. A method for producing a wiring material having a crosslinked coating layer of a silane crosslinkable polymer mixture on an outer peripheral surface of a conductor, comprising the steps of: In preparing a silane crosslinkable polymer mixture using 100 parts by mass of a base polymer, 0.01 to 0.6 parts by mass of an organic peroxide, 0.5 to 15 parts by mass of a silane coupling agent, 0.5 to 400 parts by mass of an inorganic filler, and a silanol condensation catalyst, a silane master batch prepared by melt-mixing a part of the base polymer with the organic peroxide, the silane coupling agent, and the inorganic filler in the above-mentioned mixing ratio at a temperature equal to or higher than the decomposition temperature of the organic peroxide, and a catalyst master batch prepared by melt-mixing the remainder of the base polymer and the silanol condensation catalyst are mixed to prepare the silane crosslinkable polymer mixture, The silane crosslinkable polymer mixture is introduced into an extruder to coat the outer peripheral surface of a conductor; The method for producing a wiring material includes directly introducing the obtained coated conductor from the extruder into a pressurized environment at 0.05 to 0.25 MPa higher than normal pressure, cooling the coated conductor with a liquid medium in the pressurized environment until the surface temperature of the coated conductor becomes 100°C or lower, and then extracting the coated conductor into a normal pressure environment.
2. The method according to claim 1 , wherein the coated conductor is brought into contact with water in the atmospheric pressure environment.
3. The method according to claim 1, wherein the base polymer comprises at least one of a polyolefin resin, an ethylene-vinyl acetate copolymer resin, an ethylene-alkyl (meth)acrylate copolymer resin, an ethylene rubber, a silicone rubber, a fluororubber, and a styrene-based elastomer.
4. The method according to claim 1 , wherein the liquid medium is sprayed onto the coated conductor to cool it.
5. The method according to claim 1, wherein the pressure in the pressurized environment is 0.10 to 0.20 MPa higher than normal pressure.
6. The method according to claim 1, wherein the amount of the silane coupling agent mixed is 2.0 to 6.0 parts by mass per 100 parts by mass of the base polymer.
7. The method according to claim 1 , further comprising cooling the surface of the coated conductor to a temperature of 80° C. or lower in the pressurized environment.
8. The method according to claim 1, wherein the inorganic filler is mixed in an amount of 3 to 200 parts by mass.
9. The method according to claim 1 , wherein, in preparing the silane master batch, the silane coupling agent and the inorganic filler are premixed, and then a portion of the base polymer is melt-mixed therewith.
10. A wiring material manufactured by the manufacturing method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Manufacture of molded product made of silane cross linked polyolefine
JP1985024916A
Method for selectively controlling operational characteristic of valve
JP1991057848A
Manufacturing method of heat resistant silane crosslinked polyolefin resin molded body, silane crosslinking polyolefin resin composition, heat resistant silane crosslinked polyolefin resin molded body, heat resistant product, wire, and optical fiber cable
JP2019178247A
Method of producing crosslinked polyolefin wire
JP1984025110A
Electric cable and manufacture of the same
JP1987088213A