Polyester resin composition and molding

A tailored polyester resin composition addresses the limitations of PET by enhancing flexibility, slipperiness, and heat resistance, ensuring compatibility with PET for seamless recycling and handling, while maintaining transparency.

JP2024140642APending Publication Date: 2024-10-10MITSUBISHI CHEM CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023051887
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Polyester resins, such as PET, lack flexibility, slipperiness, and heat resistance, making them unsuitable for certain applications like containers with reverse tapered parts and difficult to stack and transport, and they cannot be recycled without separating from PET bottles due to incompatibility with polyolefins and polystyrene.

Method used

A polyester resin composition is developed with specific ranges for bending stress, coefficient of friction, haze difference, and heat resistance, ensuring compatibility with PET while providing flexibility, slipperiness, and heat resistance, allowing for recycling without separation.

Benefits of technology

The composition achieves excellent compatibility with PET, enabling easy mold release, secure sealing, smooth handling, and heat resistance, facilitating recycling of containers without separation, and maintaining transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140642000001
    Figure 2024140642000001
  • Figure 2024140642000002
    Figure 2024140642000002
Patent Text Reader

Abstract

To provide a polyester resin composition capable of recycling by recovering without differentiating from PET bottles and capable of satisfying physical properties as a product for various containers.SOLUTION: A polyester resin composition comprising a polyester resin composed of dicarboxylic acid units and diol units, wherein a 1 mm thick plate molded using the polyester resin composition satisfies the following requirements (1) to (3): requirement (1) bending stress at a strain of 2.0% is 10 to 50 MPa, requirement (2) coefficient of friction at a flat portion of the 1 mm thick plate with a 2 mm diameter sapphire ball at an applied load of 1 kgf is 0.02 to 0.12, and requirement (3) difference between the haze of a 3 mm thick plate obtained by injection molding a mixture of a pulverized product of the 1 mm thick plate and polyethylene terephthalate resin in a mass ratio of 1:4 and the haze of a 3 mm thick plate obtained by injection molding only the polyethylene terephthalate resin without the pulverized product being added is 5% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester resin composition. More specifically, the present invention relates to a polyester resin composition that can be collected and recycled without being separated from PET bottles, and that has excellent recyclability and can satisfy the physical properties required for products such as various containers, specifically, flexibility, slipperiness, and heat resistance, and a molded article using the polyester resin composition. [Background technology]

[0002] Polyester resins, such as polyethylene terephthalate (PET), are excellent in mechanical strength, chemical stability, gas barrier properties, aroma retention, hygiene, etc., and molded products such as containers can be collected, washed, crushed, and melt-molded again, so they are widely used as environmentally friendly recyclable packaging containers, etc. However, polyester resins are poor in flexibility, and improvements in this area have been required.

[0003] Patent Document 1 proposes a polyester that contains terephthalic acid units and a specific amount of dimer acid units as dicarboxylic acid units, and contains ethylene glycol units and a specific amount of polyalkylene glycol units as diol units, as a polyester that can obtain molded articles that are excellent in flexibility and transparency, is free from the problem of loss of transparency during storage, and can obtain transparent molded articles even when the obtained molded articles are recovered, crushed, and then melt-molded again, and has excellent reuse suitability (recyclability).

[0004] On the other hand, various containers such as food containers and beverage containers are required to have flexibility (bending properties), slipperiness, and heat resistance (resistance to deformation due to heat), depending on their uses and applications. Conventionally, polyolefins and polystyrenes have been used for containers which require such physical properties. That is, the PET currently used for PET bottles is hard and lacks flexibility, and therefore cannot be elastically deformed when released from the mold. For example, it cannot be used for products with a reverse tapered portion due to its poor release properties. On the other hand, highly flexible PET has poor sliding properties, and when such PET containers are stacked for transportation, they are difficult to separate when taken out, and in severe cases the container may break. In addition, PET has poor sliding properties (difficult to slide) when stacked on objects that are relatively difficult to deform, making it difficult to handle.

[0005] For these reasons, polyolefins and polystyrenes have conventionally been used as molding materials in applications requiring flexibility and slipperiness. However, polyolefin and polystyrene containers cannot be melt molded together with PET containers such as PET bottles. In other words, because they are not compatible with PET, the molded products obtained by melt molding with PET are opaque and cannot be reused. For this reason, polyolefin and polystyrene containers must be collected separately from PET bottles.

[0006] For these reasons, there is a need for the development of molding materials that can be collected and recycled without being separated from PET containers such as PET bottles, and that also have excellent flexibility and slipperiness. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent Publication No. 2021-24951 Summary of the Invention [Problem to be solved by the invention]

[0008] In view of the above-mentioned conventional situation, the present invention has an object to provide a polyester resin composition which can be collected and recycled without being separated from PET bottles, and which satisfies the physical properties required for products such as various containers, specifically, an appropriate flexibility which combines softness which allows the container to be released from the mold without deformation during molding, and hardness which allows the container to be securely sealed with a cap having a screw thread shape, etc.; an appropriate slipperiness which combines slipperiness which allows the container to be easily removed after being stacked for storage, and a non-slipperiness which prevents the container from easily slipping over when placed on a tray, etc.; and good compatibility with PET which results in a small difference in haze depending on whether the container is mixed with PET and does not impair transparency, when used in combination with PET, and a molded article using this polyester resin composition. [Means for solving the problem]

[0009] As a result of intensive research by the present inventors to solve the above-mentioned problems, they have found that the above-mentioned problems can be solved by a polyester resin composition comprising a polyester resin consisting of dicarboxylic acid units and diol units, wherein the bending stress of a 1 mm thick plate molded using the polyester resin composition, the friction coefficient with a sapphire sphere, and the difference in haze between a 3 mm thick plate injection-molded from a mixture of crushed plate material and polyethylene terephthalate resin and a 3 mm thick plate injection-molded from polyethylene terephthalate resin to which the crushed plate material is not added fall within specific ranges, thereby completing the present invention.

[0010] That is, the present invention relates to the following.

[0011] [1] A polyester resin composition comprising a polyester resin composed of dicarboxylic acid units and diol units, wherein a 1 mm thick plate molded from the polyester resin composition satisfies the following requirements (1) to (3): Requirement (1) Bending stress at strain of 2.0% is 10 to 50 MPa Requirement (2) The coefficient of friction between the flat part of the 1 mm thick plate and a 2 mm diameter sapphire ball under an applied load of 1 kgf is 0.02 to 0.12. Requirement (3) The difference in haze between a 3 mm thick plate obtained by injection molding a mixture of the crushed material obtained by crushing the 1 mm thick plate and polyethylene terephthalate resin in a mass ratio of 1:4 and a 3 mm thick plate obtained by injection molding only the polyethylene terephthalate resin without adding the crushed material is 5% or less.

[0012] [2] The polyester resin composition according to [1], further comprising the following requirement (4): Requirement (4) The temperature at which a needle with a tip diameter of 1 mm penetrates the flat part of the 1 mm thick plate to a depth of 0.1 mm when a load of 0.5 N is applied is 60°C or higher.

[0013] [3] A molded article using the polyester resin composition according to [1] or [2]. Effect of the Invention

[0014] The polyester resin composition of the present invention has excellent compatibility with PET resin when mixed with PET resin, and therefore the haze difference of the molded product when mixed with PET can be reduced. Therefore, the polyester resin composition can be collected and recycled without being separated from PET containers such as bottles (hereinafter, this property may be referred to as "recyclability"). The polyester resin composition of the present invention has good releasability even when it has a shape with a reverse tapered portion, and has an appropriate bending stress (flexibility) that provides good sealing performance with a cap. In addition, they have a moderate coefficient of friction (slipperiness) that allows them to be easily removed after stacking and storage, yet is also less likely to tip over during transport, etc. For this reason, the polyester resin composition of the present invention can be used as a molding material for various containers and the like for which polyolefins or polystyrenes have conventionally been used, and the waste materials can be easily recovered and recycled together with PET products without the need for separation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The best mode for carrying out the present invention will be described in detail below. However, the description of the components described below is a representative example of an embodiment of the present invention, and the present invention is not limited to these contents.

[0016] [Polyester resin composition] The polyester resin composition of the present invention is a polyester resin composition containing a polyester resin composed of dicarboxylic acid units and diol units, and is characterized in that a 1 mm thick plate molded using the polyester resin composition satisfies the following requirements (1) to (3), and preferably further satisfies the following requirement (4). Requirement (1) Bending stress at strain of 2.0% is 10 to 50 MPa Requirement (2) The coefficient of friction between the flat part of the 1 mm thick plate and a 2 mm diameter sapphire ball under an applied load of 1 kgf is 0.02 to 0.12. Requirement (3) The difference in haze between a 3 mm thick plate obtained by injection molding a mixture of the crushed material obtained by crushing the 1 mm thick plate and polyethylene terephthalate resin in a mass ratio of 1:4 and a 3 mm thick plate obtained by injection molding only the polyethylene terephthalate resin without adding the crushed material is 5% or less. Requirement (4) The temperature at which a needle with a tip diameter of 1 mm penetrates the flat part of the 1 mm thick plate to a depth of 0.1 mm when a load of 0.5 N is applied is 60°C or higher. The method for forming the 1 mm thick plate which is the subject of the measurement of the above requirements (1) to (4) and the specific method for measuring each requirement are as shown in the Examples section below.

[0017] As mentioned above, it can be collected and recycled without being separated from PET bottles, and the physical properties required for products such as various containers are as follows: (i) Appropriate flexibility that is soft enough to allow release from molds without deformation during molding of containers, etc., and hard enough to ensure tight sealing with a cap having a screw thread, etc.; (ii) Appropriate slipperiness that allows the containers to be easily removed after stacking and storing, and is also slippery enough that the containers do not easily slip and fall over when placed on a tray or the like; (iii) When mixed with PET, there is little difference in haze due to the presence or absence of mixing, and transparency is not impaired. Good compatibility with PET; is desired. In addition, depending on the application, storage or use in a high temperature environment may be expected. (iv) Heat resistance with small deformation at high temperatures; may also be required. The polyester resin composition of the present invention can satisfy the required characteristic of appropriate flexibility (i) above due to the requirement (1), can satisfy the required characteristic of appropriate slipperiness (ii) above due to the requirement (2), can satisfy the required characteristics of compatibility and transparency (iii) above due to the requirement (3), and can further satisfy the required characteristic of heat resistance (iv) above due to the requirement (4). In the present invention, the problems of the present invention can be solved by satisfying these requirements (1) to (3), and preferably further requirement (4).

[0018] In the present invention, the term "unit" refers to a repeating unit that is derived from a compound (monomer) used as a raw material for producing the polyester resin and that is introduced into the polyester resin. For example, a terephthalic acid unit refers to a unit that is derived from terephthalic acid or an ester-forming derivative thereof (hereinafter, these will be referred to as "terephthalic acid components", and similarly, a dicarboxylic acid or an ester-forming derivative thereof used to introduce a dicarboxylic acid unit will also be referred to as "dicarboxylic acid component") and that is introduced into the polyester resin. Similarly, a diol unit refers to a repeating unit that is derived from a diol used as a raw material for producing the polyester resin and that is introduced into the polyester resin. The constituent units such as each dicarboxylic acid unit and each diol unit in the polyester resin are 1 It can be quantified by measuring the H-NMR spectrum.

[0019] Hereinafter, the polyester resin contained in the polyester resin composition of the present invention may be referred to as the "polyester of the present invention." The polyester of the present invention may consist of only a single polyester, or may be a blend of two or more types of polyester.

[0020] [Requirement (1)] The requirement (1) is that a bending stress at a strain of 2.0% for a 1 mm thick plate molded using the polyester resin composition of the present invention is 10 to 50 MPa. If the bending stress is 50 MPa or less, it is possible to obtain a softness that allows the container to be released from the mold without deformation during molding. On the other hand, if the bending stress is 10 MPa or more, it is possible to obtain a hardness that allows the container to be securely sealed with a cap having a thread shape. From the viewpoint of appropriate flexibility that combines these characteristics, the bending stress of a 1 mm thick plate is preferably 11 to 50 MPa, and more preferably 12 to 48 MPa.

[0021] Examples of ways in which the polyester resin composition of the present invention can satisfy the above-mentioned requirement (1) include a method of combining rigid components such as benzene rings and naphthalene rings with flexible components such as ethylene chains and propylene chains in the dicarboxylic acid units and diol units constituting the polyester resin, with the types and ratios being changed; and a method of adding plasticizers such as phthalate esters, dibutyl adipate, and dibutyl sebacate to the polyester resin composition, with the types, combinations, and amounts being changed. These can be used alone or in combination.

[0022] [Requirement (2)] The requirement (2) is that the coefficient of friction between a flat portion of a 1 mm thick plate molded using the polyester resin composition of the present invention and a 2 mm diameter sapphire ball is 0.02 to 0.12. If the friction coefficient is 0.12 or less, the containers can be easily removed after stacking and storing. On the other hand, if the friction coefficient is 0.02 or more, the containers can be made non-slip so that they do not easily slip and fall when placed on a tray or the like. From the viewpoint of appropriate slipperiness having both of these characteristics, the friction coefficient of a 1 mm thick plate is preferably 0.02 to 0.10, and more preferably 0.03 to 0.09.

[0023]

[0043] Examples of techniques for making the polyester resin composition of the present invention satisfy the above-mentioned requirement (2) include a method in which a lubricant such as a fatty acid amide, a saturated fatty acid, or a saturated fatty acid metal salt is added to the polyester resin composition and the lubricant is precipitated on the surface of a polyester resin composition molded body to adjust the friction coefficient of the polyester resin composition molded body; a method in which particles such as silicon dioxide or calcium carbonate are added to roughen the surface of a polyester resin composition molded body to reduce the area of ​​contact of the surface of the polyester resin composition molded body with other objects, thereby adjusting the friction coefficient; and a method in which the surface of a mold for molding a polyester resin composition molded body is roughened to reduce the area of ​​contact of the surface of the polyester resin composition molded body with other objects, thereby adjusting the friction coefficient. These methods may be used alone or in combination.

[0024] [Requirement (3)] Requirement (3) is that the difference in haze between a 3 mm thick plate obtained by injection molding a mixture obtained by crushing a 1 mm thick plate molded using the polyester resin composition of the present invention, mixing the crushed material with polyethylene terephthalate resin in a mass ratio of 1:4, and a 3 mm thick plate obtained by injection molding only the polyethylene terephthalate resin without adding the crushed material, is 5% or less. If the haze difference is 5% or less, the difference in haze between the presence and absence of mixing is small when mixed with PET, and good compatibility with PET can be obtained without impairing transparency. From this viewpoint, the haze difference is preferably 4% or less, and more preferably 3% or less.

[0025] The polyester resin composition of the present invention can satisfy the requirement (3) by, for example, selecting the type and amount of each component when selecting the dicarboxylic acid component, diol component, and additives such as lubricant that constitute the polyester resin, so that the solubility parameter of the polyester resin is close to that of PET, or by selecting a polyester resin and additives that are less likely to become crystal nuclei. This provides good compatibility with PET, prevents deterioration of transparency due to crystallization when mixed with PET, and provides good transparency even when mixed with PET. These methods can be used alone or in combination.

[0026] [Requirement (4)] Requirement (4) is that the temperature at which a needle with a tip diameter of 1 mm penetrates a 1 mm thick plate molded using the polyester resin composition of the present invention to a depth of 0.1 mm when a load of 0.5 N is applied is 60°C or higher. If the temperature at which the needle penetration depth is 0.1 mm is 60° C. or higher, excellent heat resistance with little deformation at high temperatures can be obtained. From this viewpoint, the temperature at which the needle penetration depth is 0.1 mm is more preferably 65° C. or higher, and even more preferably 70° C. or higher.

[0027] Examples of techniques for making the polyester resin composition of the present invention satisfy the requirement (4) include a method of selecting a dicarboxylic acid component and a diol component constituting the polyester resin so that the glass transition temperature of the polyester resin is 60°C or higher, a method of selecting components having a crystallization rate at which crystallization proceeds sufficiently during molding of the polyester resin composition, and a method of selecting additives so that the polyester resin composition has a crystallization rate at which crystallization proceeds sufficiently during molding of the polyester resin composition, and these may be used alone or in combination.

[0028] [Dicarboxylic acid unit] Examples of dicarboxylic acid components as raw materials for constituting the dicarboxylic acid units of the polyester of the present invention include terephthalic acid components such as terephthalic acid and its esters and halides having an alkyl group having about 1 to 4 carbon atoms, dimer acid components, and isophthalic acid components such as isophthalic acid and its esters and halides having an alkyl group having about 1 to 4 carbon atoms.

[0029] Here, dimer acid refers to a dimer of an unsaturated aliphatic carboxylic acid having 16 or more carbon atoms or a hydrogenated product thereof. This dimer acid can be obtained by dimerizing or hydrogenating a mixture of unsaturated carboxylic acids having 16 or more carbon atoms (e.g., unsaturated aliphatic carboxylic acids mainly composed of linoleic acid or oleic acid) extracted from non-petroleum raw materials such as soybean oil, rapeseed oil, beef tallow, and tall oil. When dimer acid is obtained using such a production method, it contains impurities such as an over-reacted trimer and an unreacted unsaturated aliphatic carboxylic acid. Since such impurities cause bleeding out and gelation in polyesters, it is preferable that the amount of impurities is as small as possible. In addition, since dimer acid contains an unsaturated bond, if used as is, there is a possibility that a branching reaction will proceed during polymerization or that the color tone of the obtained polyester will be deteriorated. Therefore, it is preferable that the dimer acid component used as a manufacturing raw material for introducing dimer acid units into the polyester is a hydrogenated one.

[0030] Examples of other dicarboxylic acid components that can be used in addition to the above include aromatic dicarboxylic acids such as phthalic acid, sodium sulfoisophthalate, phenylenedioxydicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-diphenylketonedicarboxylic acid, 4,4'-diphenoxyethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, and 2,6-naphthalenedicarboxylic acid, alicyclic dicarboxylic acids such as hexahydroterephthalic acid and hexahydroisophthalic acid, and aliphatic dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecadicarboxylic acid, and dodecadicarboxylic acid, as well as esters and halides of these having an alkyl group having about 1 to 4 carbon atoms.

[0031] These dicarboxylic acid components may be used alone or in combination of two or more.

[0032] [Diol unit] Examples of diol components as raw materials for forming the diol units of the polyester of the present invention include aliphatic diols such as 1,4-butanediol, polyalkylene glycol, ethylene glycol, diethylene glycol, trimethylene glycol, pentamethylene glycol, hexamethylene glycol, octamethylene glycol, decamethylene glycol, neopentyl glycol, and 2-ethyl-2-butyl-1,3-propanediol; 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, and 1,1-cyclohexanediol. Examples of the diol include alicyclic diols such as cyclohexanedimethylol and 2,5-norbornanedimethylol, aromatic diols such as xylylene glycol, 4,4'-dihydroxybiphenyl, 2,2-bis(4'-hydroxyphenyl)propane, 2,2-bis(4'-β-hydroxyethoxyphenyl)propane, bis(4-hydroxyphenyl)sulfone, and bis(4-β-hydroxyethoxyphenyl)sulfonic acid, as well as ethylene oxide or propylene oxide adducts of 2,2-bis(4'-hydroxyphenyl)propane, and dimer diol. These may be used alone or in combination of two or more.

[0033] Examples of polyalkylene glycols include polyethylene glycol, polypropylene glycol, polyethylene glycol-polypropylene glycol block copolymers, polytetramethylene glycol, and polyhexamethylene glycol. Of these, polyethylene glycol and polytetramethylene glycol are preferred from the viewpoints of transparency and flexibility of the resin.

[0034] As the polyalkylene glycol, polyethylene glycol having a weight average molecular weight of 4000 or less is preferred from the viewpoint of good compatibility with PET. If the molecular weight of the polyalkylene glycol is equal to or less than the upper limit, it is possible to obtain a transparent polyester without causing cloudiness. However, if the molecular weight of the polyalkylene glycol is too small, the melting point of the polyester becomes too low, so that in the case of polyethylene glycol, its weight average molecular weight is preferably 500 or more, more preferably 1000 or more and 2000 or less. When the weight-average molecular weight of the polyethylene glycol is within the above range, a polyester that is transparent in the molten state is obtained, and when blended with PET for PET bottles, the transparency of the recycled molded product is less likely to be affected. Here, the weight average molecular weight of the polyalkylene glycol is a value measured by size exclusion chromatography (SEC).

[0035] These polyalkylene glycols may be used alone or in combination of two or more.

[0036] [Other building blocks] The polyester of the present invention may contain other structural units than the dicarboxylic acid units and the diol units, as long as the effects of the present invention are not impaired. Other constituent components as manufacturing raw materials for introducing other constituent units into polyester are not particularly limited, and examples thereof include hydroxycarboxylic acids and alkoxycarboxylic acids such as glycolic acid, p-hydroxybenzoic acid, and p-β-hydroxyethoxybenzoic acid, monofunctional components such as stearyl alcohol, heneicosanol, octacosanol, benzyl alcohol, stearic acid, behenic acid, benzoic acid, t-butylbenzoic acid, and benzoylbenzoic acid, and polyfunctional components having three or more functional groups such as tricarballylic acid, trimellitic acid, trimesic acid, pyromellitic acid, naphthalenetetracarboxylic acid, gallic acid, trimethylolethane, trimethylolpropane, glycerol, pentaerythritol, and sugar esters. These may be used alone or in combination of two or more.

[0037] [Other ingredients] In addition to the polyester of the present invention, the polyester resin composition of the present invention may contain lubricants, crystal nucleating agents, antioxidants, coloring inhibitors, pigments, dyes, ultraviolet absorbers, release agents, flame retardants, antistatic agents, inorganic and / or organic particles, etc., depending on the application.

[0038] Among these, examples of lubricants related to the slipperiness, i.e., ease of handling, of the resulting molded article include fatty acid amides, saturated fatty acids, and saturated fatty acid metal salts. The fatty acid amides may be saturated or unsaturated fatty acid amides, but from the viewpoint of hygiene, unsaturated fatty acid amides are preferred, and specific examples include known unsaturated fatty acid amides such as erucic acid amide, oleic acid amide, brassidic acid amide, and elaidic acid amide. Examples of saturated fatty acids and saturated fatty acid metal salts include palmitic acid, stearic acid, magnesium stearate, calcium stearate, sodium stearate, and zinc stearate. From the viewpoint of maintaining the transparency of the polyester, stearic acid or magnesium stearate is preferred. Among these unsaturated fatty acid amides, erucic acid amide and oleic acid amide are preferred, and erucic acid amide is more preferred, since they have high melting points and excellent heat resistance. These unsaturated fatty acid amides, saturated fatty acids, saturated fatty acid metal salts, etc. may be used alone or in combination of two or more. When a lubricant such as erucic acid amide is blended in the polyester resin composition of the present invention, the content thereof is preferably 0.1 to 2 parts by mass, particularly 0.2 to 1.5 parts by mass, per 100 parts by mass of the polyester of the present invention.

[0039] [Intrinsic viscosity] The intrinsic viscosity (IV) of the polyester of the present invention is preferably 0.40 dL / g to 1.20 dL / g, more preferably 0.45 dL / g to 1.15 dL / g, and even more preferably 0.48 dL / g to 1.10 dL / g. When the intrinsic viscosity is within the above range, it is possible to obtain a polyester having excellent moldability without deteriorating productivity.

[0040] The intrinsic viscosity of the polyester is measured by the method described below. Approximately 0.25 g of a sample is dissolved in approximately 25 mL of a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (weight ratio 1 / 1) to a concentration of 1.00 g / dL, and then cooled to 30°C. The time it takes for the sample solution and the solvent alone to fall is measured at 30°C using a fully automatic solution viscometer (DT553, manufactured by Sentec Co., Ltd.), and the intrinsic viscosity (IV) is calculated using the following formula. IV=((1+4K H η sp ) 0.5 -1) / (2K H C) Here, η sp = η / η0-1, where η is the time it takes for the sample solution to fall, η0 is the time it takes for the solvent alone to fall, C is the concentration of the sample solution (g / dL), and K H is Huggins' constant. K H The sample dissolution conditions are 110°C for 30 minutes. When the material is properly dried and molded, the IV retention rate after molding is approximately 90 to 95%.

[0041] The intrinsic viscosity of the polyester can be adjusted to fall within the above-mentioned preferred range in the polyester production method described below, for example, by optimizing the amounts of the catalyst and the above-mentioned additives added, or by adjusting the temperature, pressure and reaction time during polycondensation to their optimum ranges.

[0042] [Method of producing polyester] The polyester of the present invention can be produced by using a dicarboxylic acid component as a production raw material for introducing a dicarboxylic acid unit and a diol component as a production raw material for introducing a diol unit, and directly producing a polyester containing dicarboxylic acid units and diol units by esterification or transesterification reaction between the dicarboxylic acid component and the diol component. However, when taking into consideration reactivity and ease of control of the content of each structural unit, it is preferable to use multiple polyesters containing some of the structural units of the polyester of the present invention and melt-knead them to obtain the polyester of the present invention, as described below. Specific examples of a method for producing a polyester containing, as main constituent units, dicarboxylic acid units including terephthalic acid units and dimer acid units, and diol units including polyalkylene glycol units and 1,4-butanediol units and / or ethylene glycol units, by melt-kneading a plurality of types of polyester will be given below, but the method for producing the polyester of the present invention is not limited to the methods described below.

[0043] <1> Polyethylene terephthalate containing dimer acid units (a polyester containing dimer acid units, terephthalic acid units, and ethylene glycol units; hereinafter sometimes referred to as "polyester I") and polybutylene terephthalate containing polyalkylene glycol units (a polyester containing polyalkylene glycol units, terephthalic acid units, and 1,4-butanediol units; hereinafter sometimes referred to as "polyester II") are melt-kneaded. <2> Polyethylene terephthalate containing dimer acid units (polyester I), polybutylene terephthalate containing polyalkylene glycol units (polyester II), and polyethylene terephthalate not containing dimer acid units or polyalkylene glycol units (polyester containing terephthalic acid units and ethylene glycol units; hereinafter, sometimes referred to as "polyester III") are melt-kneaded. <3> Polybutylene terephthalate containing dimer acid units (a polyester containing dimer acid units, terephthalic acid units, and 1,4-butanediol units; hereinafter, sometimes referred to as "polyester IV") and polyethylene terephthalate containing polyalkylene glycol units (a polyester containing terephthalic acid units, polyalkylene glycol units, and ethylene glycol units; hereinafter, sometimes referred to as "polyester V") are melt-kneaded. <4> Polybutylene terephthalate containing dimer acid units (polyester IV), polyethylene terephthalate containing polyalkylene glycol units (polyester V), and polyethylene terephthalate containing neither dimer acid units nor polyalkylene glycol units (polyester III) are melt-kneaded. <5> Polyethylene terephthalate containing neither dimer acid units nor polyalkylene glycol units (polyester III) and a polyester containing dimer acid units and polyalkylene glycol units (hereinafter sometimes referred to as "polyester VI") are melt-kneaded. <6> Polyethylene terephthalate containing dimer acid units (polyester I), polyethylene terephthalate containing polyalkylene glycol units (polyester V), and polybutylene terephthalate containing neither dimer acid units nor polyalkylene glycol units (polyester VII) are melt-kneaded.

[0044] the above <1> ~ <6> In any case, by melt-kneading two or more of the polyesters I to VII so as to have the predetermined terephthalic acid unit content, dimer acid unit content, polyalkylene glycol unit content, and 1,4-butanediol unit content, it is possible to easily produce a polyester containing, as main constituent units, dicarboxylic acid units containing terephthalic acid units and dimer acid units, and diol units containing polyalkylene glycol units and 1,4-butanediol units and / or ethylene glycol units.

[0045] The physical properties and production method of the polyesters I to VII are not particularly limited as long as they can be melt-kneaded to obtain polyesters.

[0046] The method for producing the polyester is not particularly limited, and a normal method can be applied. For example, the polyester can be produced through a process of mixing a dicarboxylic acid component containing terephthalic acid or its ester-forming derivative, and optionally isophthalic acid or its ester-forming derivative, and a diol component containing 1,4-butanediol or ethylene glycol in a predetermined ratio under stirring to obtain a raw material slurry, then heating the raw material slurry under normal pressure or pressure to cause an esterification reaction to obtain a polyester low polymer (hereinafter sometimes referred to as "oligomer"). Next, dimer acid or its ester-forming derivative and polyalkylene glycol are added to the obtained oligomer, and the mixture is gradually reduced in pressure and heated in the presence of an ester exchange catalyst or the like to cause a melt polycondensation reaction to obtain a polyester, and if necessary, the obtained polyester can be further subjected to a solid-phase polycondensation reaction.

[0047] The dimer acid or its ester-forming derivative and the polyalkylene glycol may be added to the raw material slurry or to the oligomer.

[0048] Examples of the transesterification catalyst include antimony compounds such as diantimony trioxide; germanium compounds such as germanium dioxide and germanium tetroxide; titanium compounds such as titanium alcoholates such as tetramethyl titanate, tetraisopropyl titanate, and tetrabutyl titanate, and titanium phenolates such as tetraphenyl titanate; dibutyltin oxide, methylphenyltin oxide, tetraethyltin, hexaethylditin oxide, cyclohexahexylditin oxide, didodecyltin oxide, triethyltin hydroxide, triphenyltin hydroxide, and triisobutyl Examples of the catalyst include tin compounds such as tin acetate, dibutyltin diacetate, diphenyltin dilaurate, monobutyltin trichloride, tributyltin chloride, dibutyltin sulfide, butylhydroxytin oxide, methylstannoic acid, ethylstannoic acid, and butylstannoic acid; magnesium compounds such as magnesium acetate, magnesium hydroxide, magnesium carbonate, magnesium oxide, magnesium alkoxide, and magnesium hydrogen phosphate; and calcium compounds such as calcium acetate, calcium hydroxide, calcium carbonate, calcium oxide, calcium alkoxide, and calcium hydrogen phosphate. These catalysts can be used alone or in combination of two or more.

[0049] In addition, when producing polyester, it is preferable to use a stabilizer together with the transesterification catalyst. Examples of the stabilizer include orthophosphoric acid, polyphosphoric acid, pentavalent phosphorus compounds such as trimethyl phosphate, triethyl phosphate, tri-n-butyl phosphate, trioctyl phosphate, triphenyl phosphate, tricresyl phosphate, tris(triethylene glycol) phosphate, ethyl diethyl phosphonoacetate, methyl acid phosphate, ethyl acid phosphate, isopropyl acid phosphate, butyl acid phosphate, monobutyl phosphate, dibutyl phosphate, dioctyl phosphate, and triethylene glycol acid phosphate, phosphorous acid, hypophosphorous acid, and trivalent phosphorus compounds such as diethyl phosphite, trisdodecyl phosphite, trisnonyl decyl phosphite, and triphenyl phosphite. Among these, trivalent phosphorus compounds are generally more reducing than pentavalent phosphorus compounds, and may cause the metal compound added as a polycondensation catalyst to be reduced and precipitated, resulting in the generation of foreign matter. Therefore, pentavalent phosphorus compounds are preferred.

[0050] The reaction pressure in the melt polycondensation reaction is preferably 0.001 kPa to 1.33 kPa in absolute pressure, and the reaction temperature is preferably 220°C to 280°C, and more preferably 230°C to 260°C. The solid-phase polycondensation reaction is carried out under reduced pressure or in an inert gas atmosphere, and the reaction temperature is preferably 180° C. to 220° C. The reaction time of the solid-phase polycondensation reaction is preferably 5 hours to 100 hours. By adopting the above melt polycondensation reaction conditions and solid phase polycondensation reaction conditions, it is possible to obtain a polyester having a desired intrinsic viscosity.

[0051] When the polyester of the present invention is produced using two or more of the above-mentioned polyesters I to VII, each polyester may be kneaded in a molten state and pelletized, or each polyester may be pelletized, and then two or more polyester pellets may be dry-mixed and further melt-kneaded. Each polyester pellet may be melt-kneaded in advance and then molded, or may be melt-kneaded in a molding machine and molded. The temperature during melt-kneading is usually about 240 to 300°C.

[0052] [Uses of polyester resin composition] The polyester resin composition of the present invention is excellent in recyclability, flexibility, slipperiness and heat resistance. For this reason, it is useful for food containers of complex shapes, which require flexibility, slipperiness, heat resistance, and further recyclability so that they can be collected and recycled together with PET bottles, as well as for protective sheets and films for such containers.

[0053] For example, as a food container, the polyester resin composition of the present invention can be injection molded to form a container having an opening and its lid. Also, a preform can be obtained by injection molding the polyester resin composition of the present invention, the preform can be made into a parison by stretch blow molding or extrusion molding, and the parison can be blow molded to form a container such as a bottle or a tube. Such a container is useful as a container for solids, beverages, and liquid seasonings such as soy sauce, sauce, mirin, dressing, and mayonnaise. The polyester of the present invention can be extruded into a sheet, and the sheet can be formed into a desired shape by vacuum forming or the like to form a container, which is useful as a beverage cup or its lid, or as a tray or container for foods such as fried foods or prepared foods. The sheet can also be stretched into a film or the like to be used as a food packaging material or a protective film for the inner and outer surfaces of a tray or container. EXAMPLES

[0054] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention.

[0055] [Quantitative analysis of dicarboxylic acid units and diol units in polyester] The amounts of the dicarboxylic acid units and diol units in the polyesters used in the following Examples and Comparative Examples were determined by the following method. Approximately 20 mg of polyester (pellets or mixture thereof) was dissolved in 0.75 mL of a mixed solvent of deuterated chloroform / deuterated hexafluoroisopropanol (mass ratio 7 / 3), and 25 μL of deuterated pyridine was added to prepare a sample solution. The sample solution was placed in an NMR sample tube with an outer diameter of 5 mm, and measured at room temperature using a nuclear magnetic resonance apparatus (Bruker's "AVANCE400"). 1 The 1 H-NMR spectrum was measured to determine the proportions of each dicarboxylic acid unit and diol unit in the polyester.

[0056] [Production Example 1: Production of Polyester 1 (Polybutylene Terephthalate)] In an ester exchange reaction tank equipped with a stirrer, a nitrogen inlet, a heater, a thermometer, and a distillation tube, 64.1 parts by mass of dimethyl terephthalate and 1,4-butanediol (hereinafter 1.4BG) were used in an amount of 1.2 times the molar ratio of dimethyl terephthalate, and tetrabutyl titanate was added as a catalyst as a 1,4BG solution so that the amount was 33 ppm relative to the polymer produced in terms of metallic titanium. Next, the liquid temperature in the tank was held at 150°C for 60 minutes, and then heated to 210°C over 90 minutes and held at 210°C for 30 minutes. During this time, the ester exchange reaction was carried out for a total of 180 minutes while distilling off the produced methanol. Fifteen minutes before the end of the ester exchange reaction, magnesium acetate tetrahydrate was dissolved in 1,4BG and added, followed by the addition of a hindered phenol-based antioxidant (Ciba-Geigy's "Irganox 1010") as a 1,4BG slurry and then the addition of tetrabutyl titanate as a 1,4BG solution. The mixture was then transferred to a polycondensation reaction vessel equipped with a stirrer, nitrogen inlet, heater, thermometer, distillation tube, and exhaust port for reducing pressure, and the polycondensation reaction was carried out under reduced pressure. The polycondensation reaction was carried out by gradually reducing the pressure in the tank from normal pressure to 0.4 kPa over 85 minutes, and then continued at 0.4 kPa or less. The reaction temperature was kept at 210°C for 15 minutes from the start of pressure reduction, and then increased to the maximum temperature of this reaction, 240°C, over 45 minutes, and maintained at this temperature for 1 hour, after which the temperature was controlled to a final temperature of 235°C. The final temperature was 235°C. The reaction was terminated when a predetermined stirring torque (corresponding to IV = 1.20 dL / g) was reached. The time required for the polycondensation reaction was 150 minutes (the polycondensation reaction time was defined as the time from the start of pressure reduction to the time when pressure was restored with nitrogen). Next, the inside of the tank was restored from the reduced pressure state with nitrogen, and then pressurized to withdraw the polymer. The temperature of the heat medium in the die during withdrawal was set to 230°C, and the polymer was withdrawn in the form of strands from the die. The strands were then cooled in a cooling water tank, and cut with a cutter to obtain pellets of polyester 1. The contents of each component in polyester 1 were as follows, and the intrinsic viscosity was 1.20 dL / g. Terephthalic acid units: 67.3% by mass 1,4-butanediol units: 32.7% by mass

[0057] [Production Example 2: Production of Polyester 2 (Polyester Containing Polyethylene Glycol Units)] The transesterification reaction and polycondensation reaction were carried out in the same manner as in Production Example 1, except that 64.1 parts by mass of dimethyl terephthalate, 36.8 parts by mass of 1,4-butanediol (1.4BG), 30 parts by mass of polyethylene glycol (weight average molecular weight 2000), and tetrabutyl titanate as a catalyst were added as a 1,4BG solution so that the amount was 33 ppm, calculated as metallic titanium, relative to the polymer produced, to the transesterification reaction tank, to obtain pellets of polyester 2. The contents of each component of polyester 2 are as follows, and the intrinsic viscosity was 1.20 dL / g. Terephthalic acid unit: 47.1% by mass Polyethylene glycol units: 30.0% by mass 1,4-butanediol units: 22.9% by mass

[0058] [Production Example 3: Production of Polyester 3 (polyester containing polyethylene glycol units)] The ester exchange reaction and polycondensation reaction were carried out in the same manner as in Production Example 1, except that 37.7 parts by mass of dimethyl terephthalate, 17.7 parts by mass of 1,4-butanediol (1.4BG), 60 parts by mass of polyethylene glycol (weight average molecular weight 2000), and tetrabutyl titanate as a catalyst were added as a 1,4BG solution so that the amount was 33 ppm, calculated as metallic titanium, relative to the polymer produced, to the ester exchange reaction tank, to obtain pellets of polyester 3. The contents of each component of polyester 3 are as follows, and the intrinsic viscosity was 1.20 dL / g. Terephthalic acid unit: 26.9% by mass Polyethylene glycol units: 60.0% by mass 1,4-butanediol units: 13.1% by mass

[0059] [Production Example 4: Production of Polyester 4 (polyester containing dimer acid units)] Terephthalic acid and isophthalic acid were charged in amounts that would account for 58.5% by mass and 3.3% by mass, respectively, in the polyester after polymerization, and ethylene glycol was charged in an amount that was 1.2 times the molar ratio of the total amount of terephthalic acid and isophthalic acid to an esterification reaction tank equipped with a stirrer, a temperature raising device, and a distillate separation column, and the temperature and pressure were controlled at 250°C and 0.90 kg / cm. 2 The esterification reaction was carried out for 4 hours at 250° C. and atmospheric pressure for 4 hours to obtain a polyester oligomer. The oligomer was then transferred to a polycondensation reaction tank equipped with a distillation tube and a stirrer, and a hydrogenated dimer acid having 36 carbon atoms ("Pripol 1009" manufactured by Croda Japan) was added in an amount equivalent to 17.4 mass% of the polyester after polymerization, and further an ethylene glycol solution of germanium dioxide was added as a catalyst, and an ethylene glycol solution of orthophosphoric acid was added as a stabilizer. While maintaining the temperature inside the polycondensation reaction tank at 280° C., the pressure was reduced to 0.13 kPa over 2 hours, and the reaction was then carried out at the same pressure for 3 hours. After that, the reaction system was returned to normal pressure to terminate the reaction. The obtained polyester was extracted as a strand from the bottom of the polycondensation reaction tank, submerged in water, and then the strand was cut with a cutter to obtain pellets of polyester 4. The contents of each component in polyester 4 are as follows, and the intrinsic viscosity was 0.67 dL / g. Terephthalic acid unit: 58.5% by mass Isophthalic acid unit: 3.3% by mass Dimer acid unit: 17.4% by mass Ethylene glycol units: 18.8% by mass Diethylene glycol unit: 2.0% by mass

[0060] [Polyethylene terephthalate for PET bottles] As polyethylene terephthalate for PET bottles for compatibility evaluation, a polyethylene terephthalate resin "BK2180" manufactured by PT Mitsubishi Chemical Indonesia (hereinafter referred to as "PET for compatibility evaluation") was prepared. The content of each component in this PET for compatibility evaluation was as follows, and the intrinsic viscosity was 0.83 dL / g. Terephthalic acid unit: 98.4mol% Isophthalic acid unit: 1.6mol% Ethylene glycol unit: 97.3mol% Diethylene glycol unit: 2.7mol%

[0061] [How to form a 1mm thick plate] The resin pellets were dried in a vacuum dryer for 72 hours at 60° C. When a lubricant was added, the dried pellets were placed in a stainless steel can with a seal packing, a predetermined amount of lubricant was added, and the can was sealed and thoroughly stirred. The obtained polyester resin composition was injection molded into a molded plate (1 mm thick plate) under the following conditions using an injection molding machine ("FE80S12ASE" manufactured by Nissei Plastic Industrial Co., Ltd.). Molding temperature: 260℃ (cylinder setting) Mold temperature: 20℃ (chiller water setting temperature) Weight of molded plate: 40g (total weight including plate, runner, and sprue) Mold filling time: 1 second Pressure retention time: 14 seconds Cooling time: 20 seconds Forming plate dimensions: Thickness 1mm, 110mm x 110mm (excluding runners and sprues)

[0062] [Evaluation method] <Recyclability (difference in haze depending on whether or not it is mixed with PET for PET bottles)> The 1 mm thick plate obtained by the above method was pulverized using a pulverizer (V-shaped pulverizer "V-360" manufactured by Horai Co., Ltd., screen hole diameter 8 mm), and 400 g of the pulverized product was mixed with 1600 g of PET for compatibility evaluation ("BK2180" manufactured by PT Mitsubishi Chemical Indonesia) in a stainless steel can, and the mixture was dried in a vacuum dryer at 60°C for 72 hours. Using the dried mixture, a molded plate (hereinafter referred to as "recycled molded plate") was injection molded using an injection molding machine ("FE80S12ASE" manufactured by Nissei Plastic Industrial Co., Ltd.) under the following conditions. Molding temperature: 290℃ (cylinder setting) Mold temperature: 20℃ (chiller water setting temperature) Weight of molded plate: 80g (total weight including plate, runner, and sprue) Mold filling time: 1.5 seconds Pressure retention time: 13.5 seconds Cooling time: 90 seconds Forming plate dimensions: 110mm wide with steps of 3 to 7mm thickness, 7mm thickness 20mm, then 6mm thickness 20mm, then 5mm thickness 20mm, then 4mm thickness 20mm, and finally 3mm thickness 30mm, 110mm x 110mm (excluding runner and sprue) from the runner side. The haze of a 3 mm thick portion of this recycled molded plate was measured using a haze meter (NDH-300A, manufactured by Nippon Denshoku Industries Co., Ltd.), and the difference in haze between this and a 3 mm thick portion of a molded plate molded in the same manner using only the compatibility evaluation PET BK2180 was calculated to obtain the haze difference.

[0063] <Bending stress> Test pieces measuring 10 mm in width × 60 mm in length × 1 mm in thickness were cut out from the 1 mm thick plate obtained by the above-mentioned method, and a constant speed bending test was carried out under the following conditions using the following bending tester, and the bending stress at a strain of 2.0% was measured. Toyo Seiki Co., Ltd. Bending tester: Bendgraph II Model: B Distance between fulcrums: 16mm Test speed: 1mm / min

[0064] <Coefficient of friction> Using the flat portion of the 1 mm thick plate obtained by the method described above, the horizontal resistance in a constant load horizontal friction test was measured under the following conditions using Shinto Scientific's "Tribogear TYPE14DR." The kinetic friction coefficient was determined by dividing the average horizontal resistance between the friction element's travel distance of 0.3 cm and 0.7 cm by the applied load. Friction element: 2mm diameter sapphire ball needle Applied load: 1kgf Movement speed: 1cm / sec Drag measurement: 0.01 seconds / times

[0065] <Deformation temperature> Using the flat portion of the 1 mm thick plate obtained by the above-mentioned method, a constant load temperature rise test was performed under the following conditions using a Seiko Instruments Inc. "TMA / SS6100", and the temperature at which the needle penetration depth became 0.1 mm was measured. Evaluation temperature: Room temperature to 120℃ Heating rate: 5℃ / min Probe: needle probe (tip diameter 1 mm) Measurement load: 0.5N

[0066] <Container Forming and Evaluation> A bottomed flowerpot-shaped container with a top outer diameter of 38 mm, a thread on the inside for 10 mm from the top, a wall thickness of 2 mm including the thread, and a wall thickness of 2 mm below the thread was molded by injection molding, and the following evaluations (1) to (5) were carried out. In addition, a crushed product of this container was mixed with the above-mentioned PET for compatibility evaluation at 20% by mass, and a container was molded again in the same manner. The transparency of the container appearance was visually observed, and the compatibility with PET in the following (6) was confirmed. (1) Demolding property: The presence or absence of deformation when demolded was examined. (2) Tightness: The tightness (whether the contents leak or not) of the container when plugged with a polypropylene cap was evaluated. The containers that did not leak were rated as "good" and the containers that leaked were rated as "no good." (3) Removability: The same containers were stacked and stored at room temperature (about 20°C) for three days, after which it was checked whether they could be easily removed or whether they were difficult to remove. (4) Portability: When a container was placed on a stainless steel tray, it was checked whether it easily slipped or fell over, and whether it had good portability or not. (5) Deformation after high-temperature storage: The container was stored at 55°C for 3 days and then checked for deformation. (6) Compatibility with PET: The crushed containers were mixed with PET for compatibility evaluation and remolded to obtain containers. The resulting containers were then examined to see whether they were transparent and had excellent compatibility (good) or not (bad).

[0067] [Example 1] Polyester 1 (65% by mass) and polyester 2 (35% by mass) were used and blended in the form of pellets. The dried pellets were placed in a stainless steel can with a seal gasket, to which a powder lubricant (erucic acid amide "Diamid (registered trademark) L-200" manufactured by Mitsubishi Chemical Corporation) was added in an amount equivalent to 0.5% by mass based on the dried pellets. The mixture was then sealed and thoroughly stirred. The polyester resin composition thus obtained was used for the above-mentioned evaluations. The evaluation results are shown in Table 1.

[0068] [Examples 2 to 7, Comparative Examples 1 to 5] Polyester resin compositions were obtained in the same manner as in Example 1, except that the blend amounts of Polyesters 1 to 4 and the types and amounts of additives were changed as shown in Tables 1 and 2, and the above-mentioned evaluations were similarly carried out. The evaluation results are shown in Tables 1 and 2.

[0069] In Tables 1 and 2, the abbreviations for each structural unit and additive are as follows. TPA: Terephthalic acid IPA: Isophthalic acid DA: Dimer acid BG: 1,4-butanediol EG: Ethylene glycol DEG: Diethylene glycol PEG: Polyethylene glycol EA: Erucic acid amide WAX: Polyethylene wax

[0070] [Table 1]

[0071] [Table 2]

[0072] From Tables 1 and 2, it can be seen that if the bending stress of a 1 mm thick plate and the coefficient of friction with a sapphire ball, as well as the difference between the haze of a 3 mm thick plate of an injection-molded mixture of crushed material and polyethylene terephthalate resin and the haze of a 3 mm thick plate of injection-molded polyethylene terephthalate resin to which no crushed material has been added, are within the ranges specified by the present invention, the polyester resin composition will have excellent recyclability, flexibility, and slip properties. In contrast, Comparative Examples 1 to 5, which are outside the ranges specified by the present invention, are inferior in any of these physical properties. That is, in Comparative Example 1, the haze difference is large and the compatibility with PET is poor, so that the recyclability is poor and there is an adverse effect on recycling. In Comparative Example 2, the bending stress was too low, resulting in insufficient hardness, and when the cap was tightened, the opening expanded, making it impossible to seal the container. In Comparative Example 3, the bending stress was too high, so the product became too hard, and the threads were deformed when the product was released from the mold, making it impossible to form a cap. Comparative Example 4 has a low friction coefficient, so it is too slippery and easily falls over with even a slight vibration, making it difficult to transport. Furthermore, it has a large haze difference and poor compatibility with PET, which makes it poor in recyclability and has a negative impact on recycling. Comparative Example 5 had an excessively high coefficient of friction, which made it difficult to slide the containers, and made it difficult to remove the containers after stacking them, making handling difficult.

Claims

1. A polyester resin composition comprising a polyester resin composed of a dicarboxylic acid unit and a diol unit, A polyester resin composition, characterized in that a 1 mm thick plate molded from the polyester resin composition satisfies the following requirements (1) to (3): Requirement (1) Bending stress at strain of 2.0% is 10 to 50 MPa Requirement (2) The coefficient of friction between the flat part of the 1 mm thick plate and a 2 mm diameter sapphire ball under an applied load of 1 kgf is 0.02 to 0.

12. Requirement (3) The difference in haze between a 3 mm thick plate obtained by injection molding a mixture of the pulverized material obtained by pulverizing the 1 mm thick plate and polyethylene terephthalate resin in a mass ratio of 1:4 and a 3 mm thick plate obtained by injection molding only the polyethylene terephthalate resin without adding the pulverized material is 5% or less.

2. The polyester resin composition according to claim 1, further satisfying the following requirement (4): Requirement (4) The temperature at which a needle with a tip diameter of 1 mm penetrates a flat portion of the 1 mm thick plate to a depth of 0.1 mm when a load of 0.5 N is applied is 60° C. or higher.

3. A molded article using the polyester resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Polyester composition

    JP1984207963A

  • Oriented polyester film

    JP1984221354A

  • Polyester block copolymer composition

    JP2002194189A

  • Film made of biodegradable resin

    JP2003292641A

  • Aliphatic polyester resin composition, its master batch and their films

    JP2005105081A