Molding material

A cellulose-based molding material with specific derivatives improves strength, impact resistance, and heat resistance by optimizing hydrogen atom substitution, enabling durable and environmentally friendly molded products.

JP2024140801AInactive Publication Date: 2024-10-10SEIKO EPSON CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023052140
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Molded bodies made from cellulose-based materials suffer from inferior strength, impact resistance, and heat resistance, limiting their practical applications.

Method used

A molding material comprising cellulose fibers with specific cellulose derivatives, where some hydrogen atoms of cellulose are replaced by chemical structures of general formulas (1) or (3), and the other hydrogen atoms are substituted with structures of general formulas (2) or (4), with a cellulose fiber content of 50% to 70% by mass, enhancing compatibility and functional synergy.

Benefits of technology

The material exhibits excellent strength, impact resistance, and heat resistance, enabling the production of durable molded articles suitable for various applications while addressing environmental concerns through the use of abundant natural resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140801000017
    Figure 2024140801000017
  • Figure 2024140801000018
    Figure 2024140801000018
  • Figure 2024140801000019
    Figure 2024140801000019
Patent Text Reader

Abstract

To provide a molding material that includes cellulose fiber in a prescribed content range and can be suitably used for manufacturing a molded product excellent in strength, shock resistance and heat resistance.SOLUTION: The molding material includes cellulose fiber, and a specific cellulose derivative in which some of the hydrogen atoms constituting the hydroxy groups of cellulose are substituted with a chemical structure of a general formula (1) or (3) and others of the hydrogen atoms are substituted with a chemical structure of a formula (2) or (4), where the content of the cellulose fiber is from 50 mass% to 70 mass% inclusive.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a molding material. [Background technology]

[0002] As a measure to combat the depletion of petroleum and global warming, attempts are being considered to replace conventional plastic materials with molding materials that use cellulose, a plant-derived, abundant natural material.

[0003] For example, nonwoven webs or composite structures that can be treated in composting landfills have been proposed that contain natural cellulose fibers and cellulose esters such as cellulose acetate butyrate and cellulose acetate propionate (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Special Publication No. 2005-504184 Summary of the Invention [Problem to be solved by the invention]

[0005] However, such molded articles have problems in that they are poor in strength, impact resistance, and heat resistance. [Means for solving the problem]

[0006] The present invention has been made to solve the above-mentioned problems, and can be realized as the following application examples.

[0007] The molding material according to an application example of the present invention comprises cellulose fibers and a specific cellulose derivative in which some of the hydrogen atoms constituting the hydroxyl groups of cellulose are replaced by a chemical structure of the general formula (1) or (3) below, and other some of the hydrogen atoms are replaced by a chemical structure of the general formula (2) or (4) below, and the content of the cellulose fibers is 50% by mass or more and 70% by mass or less.

[0008] [ka] (In formula (1), R A is an alkyl group.

[0009] [ka] (In formula (2), R C1 is an alkyl group having 1 to 6 carbon atoms, and R C2 is an alkylene group having 2 to 3 carbon atoms, and R C3 is an alkylene group having 3 to 6 carbon atoms, and m is an integer of 3 to 6.

[0010] [ka] (In formula (3), R B is an alkyl group.

[0011] [ka] (In formula (4), R C1 is an alkyl group having 1 to 6 carbon atoms, and R C2 is an alkylene group having 2 to 3 carbon atoms, and R C4 is an alkylene group having 3 to 6 carbon atoms, and n is an integer of 3 to 6. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a table summarizing the conditions under which the cellulose derivatives were synthesized in each synthesis example. [Diagram 2] FIG. 2 is a table showing the compositions of the molding materials, molding methods, and evaluation results of Examples 1-17. [Diagram 3] FIG. 3 is a table showing the compositions of the molding materials, molding methods, and evaluation results of Examples 18 to 25 and Comparative Examples 1 to 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Preferred embodiments of the present invention will now be described in detail. [1] Molding material First, the molding material of the present invention will be described.

[0014] The molding material of the present invention contains cellulose fibers and a specific cellulose derivative in which some of the hydrogen atoms constituting hydroxyl groups of cellulose are substituted with a chemical structure of the general formula (1) or (3) below, and the other hydrogen atoms are substituted with a chemical structure of the general formula (2) or (4) below. The content of the cellulose fibers in the molding material is 50% by mass or more and 70% by mass or less.

[0015] [ka] (In formula (1), R A is an alkyl group.

[0016] [ka] (In formula (2), R C1 is an alkyl group having 1 to 6 carbon atoms, and R C2 is an alkylene group having 2 to 3 carbon atoms, and R C3 is an alkylene group having 3 to 6 carbon atoms, and m is an integer of 3 to 6.

[0017] [ka] (In formula (3), RB is an alkyl group.

[0018] [ka] (In formula (4), R C1 is an alkyl group having 1 to 6 carbon atoms, and R C2 is an alkylene group having 2 to 3 carbon atoms, and R C4 is an alkylene group having 3 to 6 carbon atoms, and n is an integer of 3 to 6.

[0019] With this configuration, it is possible to provide a molding material that contains cellulose fibers in a predetermined range, i.e., a sufficiently high content of 50% by mass or more and 70% by mass or less, and that can be suitably used for producing molded bodies that have excellent strength, impact resistance, and heat resistance.

[0020] Such excellent effects are believed to be obtained for the following reasons. That is, by including a specific cellulose derivative having excellent compatibility and affinity with cellulose fibers, and excellent heat resistance and toughness, together with cellulose having high theoretical strength and excellent shape stability, the functions of these components can be prevented and suppressed from being offset, and the functions of these components can be fully exerted. More specifically, during the production of a molded body using the molding material, or in a molded body produced using the molding material, the functions of the cellulose fibers and the specific cellulose derivative can be fully exerted, while the wettability of the specific cellulose derivative with respect to the cellulose fibers can be increased, and interfacial peeling between different components constituting the molded body can be suitably prevented and suppressed. As a result, it is believed that the above-mentioned excellent effects can be obtained.

[0021] Furthermore, since interfacial peeling between different components constituting the molded article can be suitably prevented or suppressed, a molded article in which problems such as dust generation are effectively prevented can be obtained.

[0022] Furthermore, by containing a high content of cellulose fiber, which is a plant-derived and abundant natural material, it is possible to appropriately address environmental issues and save buried resources, etc., and is also advantageous from the viewpoints of stable supply of molding materials and molded articles produced using the same, cost reduction, etc. Furthermore, cellulose fiber is a component that is contained in large amounts not only in virgin pulp but also in waste paper, old cloth, etc., and is also advantageous from the viewpoint of promoting effective reuse of resources.

[0023] In addition, the specific cellulose derivative can be suitably obtained from the above-mentioned cellulose as a raw material, and is generally a component having excellent biodegradability. As a result, the entire molding material and the entire molded product produced using the molding material can suitably address environmental issues, etc.

[0024] On the other hand, if the above conditions are not met, satisfactory results will not be obtained. For example, even if a molding material contains cellulose fibers, if it does not contain a specific cellulose derivative, the molded article produced using the molding material will be significantly inferior in strength, impact resistance, and the like.

[0025] Furthermore, if another cellulose derivative is used in place of the specific cellulose derivative and the specific cellulose derivative is not included, the strength, impact resistance, and heat resistance of the molded body produced using the molding material cannot be made sufficiently excellent.

[0026] For example, if a cellulose derivative having the general chemical structure of the above formula (1) or (3) but not the general chemical structure of the above formula (2) or (4) is used instead of a specific cellulose derivative, compatibility with the cellulose fiber and other materials contained therein cannot be ensured, and the respective materials undergo phase separation, making it impossible to guarantee molding properties.

[0027] Furthermore, if a cellulose derivative having the general chemical structure of the above formula (2) or (4) but not the general chemical structure of the above formula (1) or (3) is used instead of the specific cellulose derivative, the moisture resistance and water resistance of the molded body will decrease because the side chain is highly polar.

[0028] In addition, instead of the specific cellulose derivative, R C1 When a cellulose derivative having a substituent where the substituent is a hydrogen atom is used, hydrogen bonds between hydroxyl groups in the cellulose fibers or derivatives cause strong interactions between the fibers, preventing fiber defibration.

[0029] In addition, instead of the specific cellulose derivative, R C1 When a cellulose derivative having a substituent that is an alkyl group having 7 or more carbon atoms is used, the glass transition temperature and melting point of the derivative decrease, and the heat resistance of the obtained molded article cannot be ensured.

[0030] In addition, instead of the specific cellulose derivative, R C2 When a cellulose derivative having a substituent that is an alkylene group having one carbon atom, i.e., a methylene group, is used, the constituent oxymethylene group is unstable to heat and undergoes thermal decomposition during the composite and molding processes.

[0031] In addition, instead of the specific cellulose derivative, R C2 When a cellulose derivative having a substituent that is an alkylene group having 4 or more carbon atoms is used, the proportion of oxygen atoms in the side chain decreases, resulting in low polarity and reduced compatibility with cellulose.

[0032] In addition, instead of the specific cellulose derivative, R C3 When a cellulose derivative having a substituent that is an alkylene group having 2 or less carbon atoms is used, the glass transition temperature and melting point become high, and the temperatures required for compounding and molding become high.

[0033] In addition, instead of the specific cellulose derivative, R C3 When a cellulose derivative having a substituent that is an alkylene group having 7 or more carbon atoms is used, the glass transition temperature and melting point of the derivative decrease, and the heat resistance of the obtained molded article cannot be ensured.

[0034] Furthermore, when a cellulose derivative having a substituent in which m in the above formula (2) is 2 or less is used instead of the specific cellulose derivative, the strength, particularly the bending strength and bending modulus, of the molded body produced using the molding material becomes inferior.

[0035] Furthermore, when a cellulose derivative having a substituent in which m in the above formula (2) is 7 or more is used instead of the specific cellulose derivative, the impact resistance, etc. of the molded body produced using the molding material will be significantly inferior.

[0036] In addition, instead of the specific cellulose derivative, R C1 When a cellulose derivative having a substituent where R is a hydrogen atom is used, the polarity of the side chain becomes high, the compatibility with the resin decreases, and the moisture absorption of the molding material increases, resulting in reduced moisture resistance and water resistance.

[0037] In addition, instead of the specific cellulose derivative, R C1 When a cellulose derivative having a substituent that is an alkyl group having 7 or more carbon atoms is used, the strength, impact resistance, and heat resistance of the molded body produced using the molding material are all inferior.

[0038] In addition, instead of the specific cellulose derivative, R C2 When a cellulose derivative having a substituent that is an alkylene group having one carbon atom, i.e., a methylene group, is used, the constituent oxymethylene group is unstable to heat and undergoes thermal decomposition during the composite and molding processes.

[0039] In addition, instead of the specific cellulose derivative, R C2When a cellulose derivative having a substituent that is an alkylene group having 4 or more carbon atoms is used, the proportion of oxygen atoms in the side chain decreases, resulting in low polarity and reduced compatibility with cellulose.

[0040] In addition, instead of the specific cellulose derivative, R C4 When a cellulose derivative having a substituent that is an alkylene group having 2 or less carbon atoms is used, the glass transition temperature and melting point become high, and the temperatures required for compounding and molding become high.

[0041] In addition, instead of the specific cellulose derivative, R C4 When a cellulose derivative having a substituent which is an alkylene group having 7 or more carbon atoms is used, the strength, impact resistance and heat resistance of the molded body produced from the molding material are all inferior.

[0042] Furthermore, when a cellulose derivative having a substituent in which n in the above formula (4) is 2 or less is used instead of the specific cellulose derivative, the strength, particularly the bending strength and bending modulus, of the molded body produced using the molding material becomes inferior.

[0043] Furthermore, when a cellulose derivative having a substituent in which n in the above formula (4) is 7 or more is used instead of the specific cellulose derivative, the impact resistance and heat resistance of the molded body produced using the molding material will be inferior.

[0044] Furthermore, even if the molding material contains cellulose fibers and specific cellulose derivatives, if the content of cellulose fibers in the molding material is less than the lower limit, the above-mentioned effects of containing cellulose fibers are not fully exerted.

[0045] Furthermore, even if the molding material contains cellulose fibers and specific cellulose derivatives, if the content of cellulose fibers in the molding material exceeds the upper limit value, the content of the specific cellulose derivatives will decrease relatively, and the moldability of the molded body as well as the strength, impact resistance, and heat resistance of the molded body will decrease rapidly.

[0046] [1-1] Cellulose fiber The molding material of the present invention contains cellulose fibers.

[0047] Cellulose fiber is the main component of the molding material of the present invention, and is a component that greatly contributes to maintaining the shape of the molded body produced using the molding material of the present invention, as well as having a significant effect on the properties of the molded body, such as its strength.

[0048] Cellulose is a plant-derived, abundant natural material. Therefore, the use of cellulose fibers can suitably address environmental issues and save buried resources, and is also preferable from the viewpoints of stable supply of molding materials and molded articles produced using the same, cost reduction, etc. Furthermore, among various fibers, cellulose fibers have particularly high theoretical strength, and are advantageous from the viewpoint of improving the strength of molded articles.

[0049] As the cellulose fibers, virgin pulp may be used, or recycled waste paper, old cloth, etc. may be used.

[0050] Cellulosic fibers are generally composed mainly of cellulose, but may contain components other than cellulose, such as hemicellulose and lignin.

[0051] The cellulose fibers used may be those that have been subjected to a treatment such as bleaching. Examples of cellulose fibers include cotton, hemp, rayon, and cupra.

[0052] As mentioned above, the content of cellulose fibers in the molding material of the present invention may be 50% by mass or more and 70% by mass or less, but is preferably 52% by mass or more and 68% by mass or less, more preferably 54% by mass or more and 66% by mass or less, and even more preferably 56% by mass or more and 64% by mass or less.

[0053] This allows the above-mentioned effects of the present invention to be more significantly exhibited, and also makes it possible to improve the moldability of the molded article, which is advantageous in terms of improving the productivity of the molded article.

[0054] The average length of the cellulose fibers is not particularly limited, but is preferably from 1 μm to 5000 μm, and more preferably from 1 μm to 400 μm.

[0055] This makes it possible to improve the shape stability, strength, etc. of a molded body produced using the molding material. In addition, dust generation in a molded body produced using the molding material can be more effectively prevented or suppressed. In addition, it is possible to more effectively prevent the occurrence of undesired irregularities on the surface of a molded body produced using the molding material. The fiber length of the cellulose fiber is determined by a method conforming to ISO 16065-2:2007.

[0056] The average thickness of the cellulose fibers is not particularly limited, but is preferably from 1 μm to 100 μm, and more preferably from 1 μm to 20 μm.

[0057] This makes it possible to improve the stability of shape, strength, etc. of the molded article produced using the molding material. In addition, it is possible to more effectively prevent the occurrence of undesired irregularities on the surface of the molded article produced using the molding material.

[0058] The average aspect ratio of the cellulose fibers, that is, the average length to the average thickness, is not particularly limited, but is preferably 10 or more and 1,000 or less, and more preferably 15 or more and 100 or less.

[0059] This makes it possible to improve the stability of shape, strength, etc. of the molded body produced using the molding material. In addition, dust generation in the molded body produced using the molding material can be more effectively prevented or suppressed. In addition, it is possible to more effectively prevent the occurrence of undesired irregularities on the surface of the molded body produced using the molding material.

[0060] [1-2] Specific cellulose derivatives The molding material of the present invention contains a specific cellulose derivative.

[0061] The specific cellulose derivative is a compound in which some of the hydrogen atoms constituting the hydroxyl groups of cellulose are replaced with a chemical structure having the general formula (1) or (3) above, and other hydrogen atoms are replaced with a chemical structure having the general formula (2) or (4) above.

[0062] Specifically, the specific cellulose derivatives include: Cellulose derivatives having the general chemical structures of the above formula (1) and the above formula (2) Cellulose derivatives having the general chemical structures of the above formula (1) and the above formula (4) Cellulose derivatives having the general chemical structures of the above formula (3) and the above formula (2) Cellulose derivatives having the general chemical structures of the above formula (3) and the above formula (4) Examples include:

[0063] Among these, preferred specific cellulose derivatives are etherified cellulose derivatives, which are cellulose derivatives having the general chemical structures of the above formulas (1) and (2), and esterified cellulose derivatives, which are cellulose derivatives having the general chemical structures of the above formulas (3) and (4).

[0064] In other words, the etherified cellulose derivative is one in which at least a portion of the hydrogen atoms constituting the hydroxyl groups of cellulose are replaced by the chemical structures of the above formulas (1) and (2), and the esterified cellulose derivative is one in which at least a portion of the hydrogen atoms constituting the hydroxyl groups of cellulose are replaced by the chemical structures of the above formulas (3) and (4).

[0065] R in the above formula (1) A may be an alkyl group, preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 8 carbon atoms, and even more preferably an alkyl group having 1 to 6 carbon atoms.

[0066] This makes it possible to provide a molded article produced using the molding material with improved strength, impact resistance, and heat resistance.

[0067] The specific cellulose derivative may have, in the molecule, chemical structures having different conditions as the chemical structure represented by the above formula (1).

[0068] R in the above formula (2) C1 may be an alkyl group having 1 to 6 carbon atoms, preferably an alkyl group having 1 to 4 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and even more preferably an alkyl group having 1 to 2 carbon atoms.

[0069] This makes it possible to provide a molded article produced using the molding material with improved strength, impact resistance, and heat resistance.

[0070] R in the above formula (2) C2 is an alkylene group having 2 to 3 carbon atoms, but is preferably an alkylene group having 3 carbon atoms, that is, a propylene group.

[0071] This makes it possible to provide a molded article produced using the molding material with improved strength, impact resistance, and heat resistance.

[0072] R in the above formula (2) C3 may be an alkylene group having 3 to 6 carbon atoms, is preferably an alkylene group having 3 to 5 carbon atoms, is more preferably an alkylene group having 3 to 4 carbon atoms, and is even more preferably an alkylene group having 3 carbon atoms, i.e., a propylene group.

[0073] This makes it possible to provide a molded article produced using the molding material with improved strength, impact resistance, and heat resistance.

[0074] In the above formula (2), m may be an integer of 3 or more and 6 or less, preferably an integer of 3 or more and 5 or less, more preferably an integer of 3 or more and 4 or less, and even more preferably 3.

[0075] This makes it possible to provide a molded article produced using the molding material with improved strength, impact resistance, and heat resistance.

[0076] The specific cellulose derivative may have, in the molecule, chemical structures having different conditions as the chemical structure represented by the above formula (2).

[0077] R in the above formula (3) B may be an alkyl group, preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 2 to 8 carbon atoms, and even more preferably an alkyl group having 3 to 5 carbon atoms.

[0078] This makes it possible to provide a molded article produced using the molding material with improved strength, impact resistance, and heat resistance.

[0079] The specific cellulose derivative may have, in the molecule, chemical structures having different conditions as the chemical structure represented by the above formula (3).

[0080] R in the above formula (4) C1 may be an alkyl group having 1 to 6 carbon atoms, preferably an alkyl group having 1 to 4 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and even more preferably an alkyl group having 1 to 2 carbon atoms.

[0081] This makes it possible to provide a molded article produced using the molding material with improved strength, impact resistance, and heat resistance.

[0082] R in the above formula (4) C2 is an alkylene group having 2 or more and 3 or less carbon atoms, but is preferably an alkylene group having 2 carbon atoms, that is, an ethylene group.

[0083] This makes it possible to provide a molded article produced using the molding material with improved strength, impact resistance, and heat resistance.

[0084] R in the above formula (4) C4 may be an alkylene group having 3 to 6 carbon atoms, is preferably an alkylene group having 3 to 5 carbon atoms, is more preferably an alkylene group having 3 to 4 carbon atoms, and is even more preferably an alkylene group having 3 carbon atoms, i.e., a propylene group.

[0085] This makes it possible to provide a molded article produced using the molding material with improved strength, impact resistance, and heat resistance.

[0086] In the above formula (4), n may be an integer of 3 or more and 6 or less, preferably an integer of 3 or more and 5 or less, more preferably an integer of 3 or more and 4 or less, and even more preferably 3.

[0087] This makes it possible to provide a molded article produced using the molding material with improved strength, impact resistance, and heat resistance.

[0088] The specific cellulose derivative may have, in the molecule, chemical structures having different conditions as the chemical structure represented by the above formula (4).

[0089] In the specific cellulose derivative, the total DS value of the chemical structures represented by the above formula (1) and formula (3), i.e., the degree of substitution, which is the value corresponding to the number of hydrogen atoms of all hydroxyl groups in cellulose that are substituted with the chemical structures represented by the above formula (1) and formula (3), is preferably 1.5 or more and 2.7 or less, more preferably 1.6 or more and 2.5 or less, and even more preferably 1.7 or more and 2.3 or less.

[0090] This makes it possible to provide a molded article produced using the molding material with improved strength, impact resistance, and heat resistance.

[0091] In the specific cellulose derivative, the total DS value of the chemical structures represented by the above formula (2) and formula (4), i.e., the degree of substitution, which is the value corresponding to the number of hydrogen atoms of all hydroxyl groups in cellulose that are substituted with the chemical structures represented by the above formula (2) and formula (4), is preferably 0.3 to 1.5, more preferably 0.4 to 1.3, and even more preferably 0.5 to 1.1.

[0092] This makes it possible to provide a molded article produced using the molding material with improved strength, impact resistance, and heat resistance.

[0093] In a specific cellulose derivative, the degree of substitution, which is the total DS value of all substituents, i.e., the value corresponding to the number of hydrogen atoms of all hydroxyl groups in cellulose that are substituted with substituents, is preferably 2.0 or more and 2.7 or less, more preferably 2.2 or more and 2.7 or less, and even more preferably 2.4 or more and 2.7 or less.

[0094] This makes it possible to provide a molded article produced using the molding material with improved strength, impact resistance, and heat resistance.

[0095] In particular, when the total DS values ​​of the chemical structures represented by the above formulas (1) and (3), the total DS values ​​of the chemical structures represented by the above formulas (2) and (4), and the total DS values ​​of all the substituents in a specific cellulose derivative all satisfy the above-mentioned conditions, the above-mentioned effects are more pronounced.

[0096] The number average molecular weight of the specific cellulose derivative is preferably from 10,000 to 400,000, more preferably from 20,000 to 300,000, and even more preferably from 35,000 to 200,000.

[0097] This makes it possible to improve the affinity and compatibility of the specific cellulose derivative with cellulose fibers, and to improve the strength, impact resistance, and heat resistance of the molded body produced using the molding material.

[0098] The glass transition temperature of the specific cellulose derivative is preferably 80°C or higher and 200°C or lower, more preferably 90°C or higher and 180°C or lower, and even more preferably 100°C or higher and 170°C or lower.

[0099] This makes it possible to improve the affinity and compatibility of the specific cellulose derivative with cellulose fibers, and to improve the strength, impact resistance, and heat resistance of the molded body produced using the molding material.

[0100] The content of the specific cellulose derivative in the molding material is preferably from 10% by mass to 40% by mass, more preferably from 13% by mass to 30% by mass, and even more preferably from 15% by mass to 25% by mass.

[0101] This makes it possible to provide a molded article produced using the molding material with improved strength, impact resistance, and heat resistance.

[0102] When the content of cellulose fiber in the molding material is XC [% by mass] and the content of the specific cellulose derivative is XD [% by mass], it is preferable to satisfy the relationship of 0.14≦XD / XC≦0.80, it is more preferable to satisfy the relationship of 0.19≦XD / XC≦0.60, and it is even more preferable to satisfy the relationship of 0.22≦XD / XC≦0.50.

[0103] This makes it possible to provide a molded article produced using the molding material with improved strength, impact resistance, and heat resistance.

[0104] [1-3] Second cellulose derivative The molding material of the present invention may further contain, in addition to the above-mentioned cellulose fibers and specific cellulose derivative, a second cellulose derivative which is at least one selected from the group consisting of cellulose acetate propionate, cellulose acetate butyrate, and cellulose acetate.

[0105] These second cellulose derivatives have excellent affinity and compatibility with the specific cellulose derivatives described above, and by containing such second cellulose derivatives, the strength, impact resistance, and heat resistance of the molded body produced using the molding material can be improved.

[0106] The content of the second cellulose derivative in the molding material is preferably 10% by mass or more and 40% by mass or less, more preferably 12% by mass or more and 36% by mass or less, and even more preferably 14% by mass or more and 32% by mass or less.

[0107] This makes it possible to further improve the strength, impact resistance, and heat resistance of a molded article produced using the molding material.

[0108] [1-4] Flame retardants The molding material of the present invention may further contain a flame retardant.

[0109] This makes it possible to improve the flame retardancy of a molded article produced using the molding material of the present invention.

[0110] Examples of the flame retardant include bromine-based flame retardants, chlorine-based flame retardants, phosphorus-containing flame retardants, silicon-containing flame retardants, nitrogen compound-based flame retardants, and inorganic flame retardants.

[0111] Among these, phosphorus-containing flame retardants and silicon-containing flame retardants are preferred because they do not undergo thermal decomposition during mixing / kneading with other components or during molding to generate hydrogen halides that corrode processing machines or dies or deteriorate the working environment, and because there is little risk of halogens dispersing or decomposing to generate dioxins and other harmful effects on the environment when they are incinerated.

[0112] Examples of phosphorus-containing flame retardants include organic phosphorus compounds such as phosphoric acid esters, phosphoric acid condensed esters, and polyphosphates.

[0113] Examples of the phosphoric acid ester include trimethyl phosphate, triethyl phosphate, tributyl phosphate, tri(2-ethylhexyl) phosphate, tributoxyethyl phosphate, triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, tris(isopropylphenyl) phosphate, tris(phenylphenyl) phosphate, trinaphthyl phosphate, cresyl diphenyl phosphate, xylenyl diphenyl phosphate, diphenyl(2-ethylhexyl) phosphate, di(isopropylphenyl) phosphate, Examples of the acryloyloxyethyl phosphate include 2-propylphenyl)phenyl phosphate, monoisodecyl phosphate, 2-acryloyloxyethyl acid phosphate, 2-methacryloyloxyethyl acid phosphate, diphenyl-2-acryloyloxyethyl phosphate, diphenyl-2-methacryloyloxyethyl phosphate, melamine phosphate, dimelamine phosphate, melamine pyrophosphate, triphenylphosphine oxide, tricresylphosphine oxide, diphenyl methanephosphonate, and diethyl phenylphosphonate.

[0114] Examples of the phosphoric acid condensation ester include aromatic phosphoric acid condensation esters such as resorcinol polyphenyl phosphate, resorcinol poly(di-2,6-xylyl) phosphate, bisphenol A polycresyl phosphate, hydroquinone poly(2,6-xylyl) phosphate, and condensations thereof.

[0115] Further examples include polyphosphates formed from salts of phosphoric acid or polyphosphoric acid with metals of Groups 1 to 14 of the periodic table, ammonia, aliphatic amines, and aromatic amines. Representative salts of polyphosphates include metal salts such as lithium salts, sodium salts, calcium salts, barium salts, iron (II) salts, iron (III) salts, and aluminum salts, aliphatic amine salts such as methylamine salts, ethylamine salts, diethylamine salts, triethylamine salts, ethylenediamine salts, and piperazine salts, and aromatic amine salts such as pyridine salts and triazines.

[0116] In addition to the above, examples of the phosphate ester include halogen-containing phosphate esters such as trischloroethyl phosphate, trisdichloropropyl phosphate, and tris(β-chloropropyl) phosphate, phosphazene compounds having a structure in which a phosphorus atom and a nitrogen atom are linked by a double bond, and phosphate ester amides.

[0117] Examples of silicon-containing flame retardants include organosilicon compounds having a two-dimensional or three-dimensional structure, polydimethylsiloxanes, or polydimethylsiloxanes in which the methyl groups at the side chains or ends are substituted or modified with hydrogen atoms, substituted or unsubstituted aliphatic hydrocarbon groups, or aromatic hydrocarbon groups, so-called silicone oils, or modified silicone oils.

[0118] Examples of the substituted or unsubstituted aliphatic hydrocarbon group and aromatic hydrocarbon group include an alkyl group, a cycloalkyl group, a phenyl group, a benzyl group, an amino group, an epoxy group, a polyether group, a carboxyl group, a mercapto group, a chloroalkyl group, an alkyl higher alcohol ester group, an alcohol group, an aralkyl group, a vinyl group, and a trifluoromethyl group.

[0119] In addition, as flame retardants other than the phosphorus-containing flame retardants and silicon-containing flame retardants, for example, inorganic flame retardants such as magnesium hydroxide, aluminum hydroxide, antimony trioxide, antimony pentoxide, sodium antimonate, zinc hydroxystannate, zinc stannate, metastannic acid, tin oxide, stannic oxide salts, zinc sulfate, zinc oxide, ferrous oxide, ferric oxide, stannous oxide, stannic oxide, zinc borate, ammonium borate, ammonium octamolybdate, metal salts of tungstic acid, composite oxides of tungsten and metalloid, ammonium sulfamate, ammonium bromide, zirconium-based compounds, guanidine-based compounds, fluorine-based compounds, graphite, and expandable graphite can be used.

[0120] When the molding material contains a flame retardant, the content of the flame retardant can be 1 part by mass or more and 30 parts by mass or less, based on 100 parts by mass of the total content of the cellulose fiber and the specific cellulose derivative.

[0121] This makes it possible to more effectively exert the effects of the present invention described above, while at the same time making it possible to provide a molded article produced using the molding material of the present invention with more excellent flame retardancy.

[0122] [1-5] Antioxidants The molding material of the present invention may further contain an antioxidant. This improves the resin's stability against heating during the kneading and molding processes.

[0123] Examples of the antioxidant include phosphorus-based antioxidants and hindered phenol-based antioxidants (e.g., "Irganox 1010," "Irganox 1076," and "Irganox 3114," manufactured by Ciba Specialty Chemicals; and "Sumilizer GP," manufactured by Sumitomo Chemical Co., Ltd.).

[0124] When the molding material contains an antioxidant, the content of the antioxidant can be 0.05 parts by mass or more and 2.0 parts by mass or less when the total content of the cellulose fiber and the specific cellulose derivative is 100 parts by mass.

[0125] This makes it possible to more suitably prevent deterioration in the impact resistance, moldability, rigidity, bending strength, heat resistance, etc., which are inherent to the specific cellulose derivative, while more suitably improving the scratch resistance and stain resistance.

[0126] [1-6] Other ingredients The molding material of the present invention may contain components other than those described above. Hereinafter, in this section, such components are also referred to as "other components".

[0127] Examples of other components include colorants, insect repellents, antifungal agents, antibacterial agents, antistatic agents, flame retardant assistants, ultraviolet absorbers, aggregation inhibitors, release agents, processing aids, drip prevention agents, cellulose derivatives other than those mentioned above, resin materials, and plasticizers.

[0128] However, the content of other components in the molding material of the present invention is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less.

[0129] [2] Manufacturing method of molding material Next, the method for producing the molding material of the present invention will be described.

[0130] The molding material of the present invention can be produced, for example, by mixing the above-mentioned components. In this case, the components may be mixed at the same time or at different times.

[0131] The molding material of the present invention may be produced, for example, by kneading the above-mentioned components. For kneading the components, for example, a single-screw kneader, a twin-screw kneader, a multi-screw kneader, a mixer, or a roll Banbury machine can be used.

[0132] The strand-like molding material obtained by kneading may be pelletized using a pelletizer of the strand type or water ring hot cut type to form a pellet-like molding material.

[0133] The following method may also be applied as a method for producing a molding material. That is, the kneaded material of the above-mentioned components may be formed into a sheet, and then, for example, cut into a desired shape using a shredder device to obtain a pellet-shaped molding material. The method for forming the kneaded material into a sheet is not particularly limited, but for example, the kneaded material is first deposited in air to form a sheet-shaped deposit, and the deposit is compressed using a calendar device to remove air and increase the density, and then heated in a non-contact manner using a heating furnace, and then hot-pressed using a heat press device. The shape and size of the pellets obtained by cutting are not particularly limited, but for example, they can be approximately rectangular parallelepipeds with a side length of 2 mm to 5 mm.

[0134] The cellulose fibers used in the production of the molding material of the present invention may be those that have been previously subjected to a defibration treatment. In particular, cellulose fiber sources containing cellulose fibers, such as waste paper, may be used that have been defibrated.

[0135] [3] Molded body Next, a molded article produced by using the molding material of the present invention will be described.

[0136] The molded article according to the present invention contains cellulose fibers and a specific cellulose derivative, and the content of the cellulose fibers is 50% by mass or more and 70% by mass or less.

[0137] The molded article according to the present invention can be produced by using the molding material described above. This makes it possible to provide a molded article that contains cellulose fibers at a sufficiently high content within a predetermined range, that is, from 50% by mass to 70% by mass, and that has excellent strength, impact resistance, and heat resistance.

[0138] Furthermore, by containing a high content of cellulose fiber, which is a plant-derived and abundant natural material, it is possible to appropriately address environmental issues and save buried resources, etc., and is also advantageous from the viewpoints of stable supply of molded bodies, cost reduction, etc. Furthermore, cellulose fiber is a component that is contained in large amounts not only in virgin pulp but also in waste paper, used cloth, etc., and is also advantageous from the viewpoint of promoting effective reuse of resources.

[0139] In addition, the specific cellulose derivative can be suitably obtained from the above-mentioned cellulose as a raw material, and is generally a component having excellent biodegradability, which allows the molded article as a whole to suitably address environmental issues, etc.

[0140] Each component constituting the molded article preferably satisfies the conditions described above in [1-1] to [1-6].

[0141] The shape of the molded product is not particularly limited, and may be any shape, such as a sheet, a block, a sphere, or a three-dimensional shape.

[0142] The molded article may be used for any purpose, and examples thereof include various housings such as printer housings, ink cartridges, and various containers.

[0143] In particular, the molded body of the present invention has a high affinity between the cellulose fibers and the specific cellulose derivative, and effectively prevents dust generation, making it suitable for use in ink cartridges and the like where dust generation is a particular problem.

[0144] The molded article according to the present invention may be produced by any method, but can be suitably produced, for example, by injection molding, press molding, or the like using the molding material according to the present invention as described above.

[0145] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to these. EXAMPLES

[0146] Next, specific examples of the present invention will be described. [4] Synthesis of cellulose derivatives (Synthesis Example 1) First, 29.2g (0.1mol) of 2-2-(2-propoxyethoxy)ethoxyethanol (BOC SCIENCES) was placed in a reaction flask equipped with a drying tube, and 200mL of tetrahydrofuran that had been dried with sodium hydride was added to dissolve it. Next, 72.4g (0.4mol) of methyl 4-bromobutyrate (Tokyo Chemical Industry Co., Ltd.) and 3.6g (0.15mol) of sodium hydride were added. 50% oily NaH was used as sodium hydride, which had been washed with dry toluene and filtered off in advance. The reaction mixture was stirred at room temperature for 24 hours. After distilling off the solvent, 25mL of water was added and the mixture was extracted with 100mL of ether. The ether layer was washed twice with water and dried over anhydrous magnesium sulfate. After distilling off the ether, the residue was reprecipitated with methanol to obtain 5,8,11,14-tetraoxaheptadecanoic acid methyl ester.

[0147] The ester derivative obtained above, 5,8,11,14-tetraoxaheptadecanoic acid methyl ester, was added to a 200 mL three-neck flask containing 40 mL of 25% aqueous sodium hydroxide solution, and the mixture was stirred at room temperature for 6 hours. Dilute hydrochloric acid was added dropwise to the solution to make it weakly acidic, and then the solution was extracted with saturated saline-chloroform to obtain 5,8,11,14-tetraoxaheptadecanoic acid. A mixture of 27.8 g (0.1 mol) of the obtained carboxylic acid derivative and 47.6 g (0.4 mol) of thionyl chloride was refluxed at 80°C for 3 hours. Excess thionyl chloride was removed under reduced pressure, and the intermediate acid chloride was obtained by continuing the distillation.

[0148] Cellulose (Nippon Paper Industries, Floc W50, 1.90g, 11.76mmol) was placed in a 200mL three-neck flask, and N-methyl-2-pyrrolidinone (Kanto Chemical, 25.4mL) and pyridine (Kanto Chemical, 3.3mL) were added as solvents, followed by mechanical stirring at 300 rpm for 4 hours. The internal temperature was cooled to -4°C, and the above acid chloride (1.75g, 5.88mmol) and propionyl chloride (Kanto Chemical, 3.26g, 35.27mmol) were added dropwise, and the reaction was carried out at an internal temperature of 90°C for 12 hours. The internal temperature was then cooled to 65°C, and methanol (42.9mL) was added to stop the reaction. Pure water (6.3mL) was added and the mixture was filtered under reduced pressure, after which the residue was dispersed and stirred in methanol (23.8mL), and filtered under reduced pressure. This procedure was repeated five times and the mixture was dried in vacuum for 12 hours to obtain a cellulose derivative.

[0149] (Synthesis Examples 2 to 19) A cellulose derivative was synthesized in the same manner as in Synthesis Example 1, except that the composition of the cellulose derivative was changed as shown in FIG. 1 by changing the types and amounts of the reaction components with the cellulose as a raw material.

[0150] (Synthesis Example 20) First, 60.6g (0.3mol) of 1,3-dibromopropane (Tokyo Chemical Industry Co., Ltd.) and 2.4g (0.1mol) of sodium hydride were added to 200mL of tetrahydrofuran that had been dried with sodium hydride in advance in a reaction flask equipped with a drying tube, and 14.6g (0.05mol) of 2-2-(2-propoxyethoxy)ethoxyethanol (BOC Sciences Co., Ltd.) was added dropwise. 50% oily NaH was used as sodium hydride, which had been washed with dry toluene and filtered off in advance. The reaction mixture was stirred at room temperature for 24 hours. After the solvent was distilled off, 25mL of water was added and the mixture was extracted with 100mL of ether. The ether layer was washed twice with water and dried over anhydrous magnesium sulfate. After the ether was distilled off, the residue was reprecipitated with methanol to obtain 1-bromo-5,8,11,14-tetraoxahexadecane.

[0151] Cellulose (Nippon Paper Industries, Floc W50, 1.90g, 11.8mmol) was placed in a 200mL three-neck flask, and dimethylformamide (Kanto Chemical, 25.4mL) and 1.2g (50mmol) of sodium hydride were added as solvents, and mechanically stirred at 300 rpm for 4 hours. The above terminal bromo derivative (1.53g, 5.88mmol) and 1-bromopropane (Kanto Chemical, 4.55g, 35.3mmol) were added dropwise, and the reaction was carried out at an internal temperature of 60°C for 12 hours. The mixture was then cooled to room temperature, and methanol (42.9mL) was added to stop the reaction. Pure water (6.3mL) was added and the mixture was filtered under reduced pressure, after which the residue was dispersed and stirred in methanol (23.8mL), and filtered under reduced pressure. This operation was repeated five times, and the mixture was dried in vacuum for 12 hours to obtain a cellulose derivative.

[0152] (Synthesis Examples 21 to 23) A cellulose derivative was synthesized in the same manner as in Synthesis Example 20, except that the composition of the cellulose derivative was changed as shown in Figure 1 by changing the types and amounts of the reaction components with the cellulose as a raw material.

[0153] (Synthesis Example 24) First, cellulose (Nippon Paper Industries, Floc W50, 1.90 g, 11.8 mmol) was placed in a 200 mL three-neck flask, and dimethylformamide (Kanto Chemical, 25.4 mL) and 1.2 g (50 mmol) of sodium hydride were added as a solvent, followed by mechanical stirring at 300 rpm for 4 hours. The terminal bromo intermediate (1.53 g, 5.88 mmol) of Synthesis Example 20 was added dropwise, and the reaction was carried out at an internal temperature of 60°C for 12 hours. The mixture was then cooled to room temperature, and methanol (42.9 mL) was added to stop the reaction. Pure water (6.3 mL) was added and the mixture was filtered under reduced pressure, after which the residue was dispersed and stirred in methanol (23.8 mL), and filtered under reduced pressure. This operation was repeated five times, and the mixture was dried in vacuum for 12 hours.

[0154] The dried product was placed in a 200 mL three-neck flask, and N-methyl-2-pyrrolidinone (Kanto Chemical, 25.4 mL) and pyridine (Kanto Chemical, 3.3 mL) were added as solvents and mechanically stirred at 300 rpm for 4 hours. The internal temperature was cooled to -4°C, propionic acid chloride (Kanto Chemical, 3.26 g, 35.3 mmol) was added dropwise, and the reaction was carried out at an internal temperature of 90°C for 12 hours. The internal temperature was then cooled to 65°C, and methanol (42.9 mL) was added to stop the reaction. Pure water (6.3 mL) was added and the mixture was filtered under reduced pressure, after which the residue was dispersed and stirred in methanol (23.8 mL), and filtered under reduced pressure. This operation was repeated five times, and the mixture was dried in a vacuum for 12 hours to obtain a cellulose derivative.

[0155] (Synthesis Example 25) First, cellulose (Nippon Paper Industries, Floc W50, 1.90 g, 11.8 mmol) was placed in a 200 mL three-neck flask, and dimethylformamide (Kanto Chemical, 25.4 mL) and 1.2 g (50 mmol) of sodium hydride were added as solvents, and mechanically stirred at 300 rpm for 4 hours. 1-Bromopropane (Kanto Chemical, 4.55 g, 35.3 mmol) was added dropwise, and the reaction was carried out at an internal temperature of 60°C for 12 hours. After that, it was cooled to room temperature, and methanol (42.9 mL) was added to stop the reaction. Pure water (6.3 mL) was added and filtered under reduced pressure, and the residue was dispersed and stirred in methanol (23.8 mL), and then filtered under reduced pressure. This operation was repeated five times, and the mixture was dried in vacuum for 12 hours.

[0156] The dried product was placed in a 200 mL three-neck flask, and N-methyl-2-pyrrolidinone (Kanto Chemical, 25.4 mL) and pyridine (Kanto Chemical, 3.3 mL) were added as solvents, followed by mechanical stirring at 300 rpm for 4 hours. The internal temperature was cooled to -4°C, and the acid chloride intermediate (1.75 g, 5.88 mmol) of Synthesis Example 1 was added dropwise, and the reaction was carried out at an internal temperature of 90°C for 12 hours. The internal temperature was then cooled to 65°C, and methanol (43.9 mL) was added to terminate the reaction. Pure water (6.3 mL) was added and the mixture was filtered under reduced pressure, after which the residue was dispersed and stirred in methanol (23.8 mL), and filtered under reduced pressure. This operation was repeated five times, and the mixture was dried in a vacuum for 12 hours to obtain a cellulose derivative. The conditions for synthesizing the cellulose derivatives in each synthesis example are summarized in FIG.

[0157] [5] Preparation of molding material Example 1 Cellulose fiber (manufactured by CMPC, Guaiba BEKP): 60 parts by mass, the cellulose derivative synthesized in Synthesis Example 1: 20 parts by mass, and cellulose acetate butyrate (manufactured by Eastman Chemical Co., CAB-381-20): 20 parts by mass were weighed. These were then put into a twin-screw kneader (manufactured by Technovel, KZW15TW-45MG) and kneaded. The kneading conditions were a maximum heating temperature of 180°C and an extrusion discharge rate of 1 kg / hr. Next, the mixture was processed into a strand shape and then pelletized into a molding material in the form of pellets using a pelletizer.

[0158] (Examples 2 to 25) A pellet-shaped molding material was prepared in the same manner as in Example 1, except that the types of components to be kneaded and the compounding ratio of each component were changed as shown in FIG. 2 and FIG.

[0159] (Comparative Examples 1 to 9) A pellet-shaped molding material was prepared in the same manner as in Example 1, except that the types of components to be kneaded and the compounding ratio of each component were changed as shown in FIG.

[0160] [5] Manufacturing of molded bodies For each of the molding materials of Examples 1 to 25 and Comparative Examples 1 and 3 to 9, injection molding was performed using an injection molding machine (manufactured by Nissei Plastic Industrial Co., Ltd., THX40-5V) to produce molded bodies for Charpy impact strength evaluation, bending strength evaluation, bending modulus evaluation, and deflection temperature under load evaluation, which will be described later. The heating temperature of the molding material during injection molding was 200°C. The molded body for Charpy impact strength evaluation was a rectangular plate-shaped molded body with a long side of 80 mm ± 2 mm, a short side of 4.0 mm ± 0.2 mm, and a thickness of 10.0 mm ± 0.2 mm, and the molded bodies for bending strength evaluation, bending modulus evaluation, and deflection temperature under load evaluation were rectangular plate-shaped molded bodies with a long side of 80 mm ± 2 mm, a short side of 10.0 mm ± 0.2 mm, and a thickness of 4.0 mm ± 0.2 mm.

[0161] In addition, the molding material of Comparative Example 2 was press molded using a press processing device (Towa Seiki Co., Ltd., hydraulic press PHKS-40ABS) to produce molded bodies for Charpy impact strength evaluation, bending strength evaluation, bending modulus evaluation, and deflection temperature under load evaluation, which will be described later. The heating temperature of the molding material during press molding was 200°C. The molded body for Charpy impact strength evaluation was a rectangular plate-shaped molded body with a long side of 80 mm ± 2 mm, a short side of 4.0 mm ± 0.2 mm, and a thickness of 10.0 mm ± 0.2 mm, and the molded bodies for bending strength evaluation, bending modulus evaluation, and deflection temperature under load evaluation were rectangular plate-shaped molded bodies with a long side of 80 mm ± 2 mm, a short side of 10.0 mm ± 0.2 mm, and a thickness of 4.0 mm ± 0.2 mm.

[0162] [6] Evaluation The molded articles according to the respective Examples and Comparative Examples were evaluated as follows. [6-1] Charpy impact strength The Charpy impact strength of each of the molded articles for Charpy impact strength evaluation according to each of the Examples and Comparative Examples, which were manufactured as described in [5] above, was measured in accordance with ISO 179 (JIS K7111) using an Impact Tester IT manufactured by Toyo Seiki Seisakusho Co., Ltd., and evaluated according to the following criteria. In measuring the Charpy impact strength, the hammer weight was 4J (WR2.14N / m), the lifting angle was 150°, the notch remaining width was 8.0mm±0.2mm, and the notch angle was 45°.

[0163] A: Charpy impact strength is 10kJ / m 2 That's all. B: Charpy impact strength is 8kJ / m 2 More than 10kJ / m 2 is less than. C: Charpy impact strength is 6kJ / m 2 More than 8kJ / m 2 is less than. D: Charpy impact strength is 6 kJ / m 2 is less than.

[0164] [6-2] Bending strength The molded articles for evaluating bending strength according to each of the Examples and Comparative Examples, which were produced as described in [5] above, were measured for bending strength in accordance with ISO 178 (JIS K7171) using an Instron 68TM-30 and evaluated according to the following criteria. In measuring bending strength, the distance between supports was 64 mm.

[0165] A: The bending strength is 60 MPa or more. B: The bending strength is 40 MPa or more and less than 60 MPa. C: The bending strength is 20 MPa or more and less than 40 MPa. D: The bending strength is less than 20 MPa.

[0166] [6-3] Flexural modulus The flexural modulus of each of the molded articles for evaluating the flexural modulus of each of the Examples and Comparative Examples, which were produced as described in [5] above, was measured in accordance with ISO 178 (JIS K7171) using an Instron 68TM-30 and evaluated according to the following criteria. In measuring the flexural modulus of each of the molded articles, the distance between supporting points was set to 64 mm.

[0167] A: The flexural modulus is 2.0 GPa or more. B: The flexural modulus is 1.5 GPa or more and less than 2.0 GPa. C: The flexural modulus is 1.0 GPa or more and less than 1.5 GPa. D: The flexural modulus is less than 1.0 GPa.

[0168] [6-4] Deflection temperature under load The molded articles for evaluating the deflection temperature under load according to each of the Examples and Comparative Examples, which were manufactured as described in [5] above, were measured for deflection temperature under load in accordance with ISO 75 (JIS K7191) using a HDT tester 3M-2: Flatwise type manufactured by Toyo Seiki Seisakusho Co., Ltd., and were evaluated according to the following criteria: Three-point bending was performed in a thermostatic chamber at a bending stress of 1.8 MPa under the conditions of a support distance of 64 mm, a heating start temperature of 30°C, a heating rate of 120°C / hr, and a heating end temperature of 220°C, and the temperature at which the displacement reached 0.34 mm was taken as the deflection temperature under load.

[0169] A: The deflection temperature under load is 120°C or higher. B: The deflection temperature under load is 100°C or higher and less than 120°C. C: The deflection temperature under load is 80°C or higher and less than 100°C. D: The deflection temperature under load is less than 80°C.

[0170] These results are shown together in Figs. 2 and 3, together with the compositions of the molding materials obtained in the respective Examples and Comparative Examples, and the methods for molding moldings using the molding materials.

[0171] In Figures 2 and 3, cellulose fiber (Guaiba BEKP, manufactured by CMPC) is indicated as "cellulose fiber", cellulose acetate propionate (CAP-482-20, manufactured by Eastman Chemical Co.) as "CAP", cellulose acetate butyrate (CAB-381-20, manufactured by Eastman Chemical Co.) as "CAB", cellulose acetate (DAC:L-70, manufactured by Daicel Miraizu Co.) as "DAC", triphenyl phosphate as "flame retardant", and Irganox (registered trademark) 1010 as "antioxidant". The numerical values ​​for each component in Figures 2 and 3 indicate the content in mass%.

[0172] As is clear from Figures 2 and 3, excellent results were obtained in the Examples, whereas satisfactory results were not obtained in the Comparative Examples.

Claims

1. The present invention comprises cellulose fibers and a specific cellulose derivative in which some of the hydrogen atoms constituting hydroxyl groups of cellulose are substituted with a chemical structure of the general formula (1) or (3) below, and other hydrogen atoms are substituted with a chemical structure of the general formula (2) or (4) below, The molding material has a cellulose fiber content of 50% by mass or more and 70% by mass or less. 【Chemistry 1】 (In formula (1), R A is an alkyl group.) 【Chemistry 2】 (In formula (2), R C1 is an alkyl group having 1 to 6 carbon atoms; R C2 is an alkylene group having 2 to 3 carbon atoms; R C3 is an alkylene group having 3 to 6 carbon atoms, and m is an integer of 3 to 6. 【Chemistry 3】 (In formula (3), R B is an alkyl group.) 【Chemistry 4】 (In formula (4), R C1 is an alkyl group having 1 to 6 carbon atoms; R C2 is an alkylene group having 2 to 3 carbon atoms; R C4 is an alkylene group having 3 to 6 carbon atoms, and n is an integer of 3 to 6.

2. The molding material according to claim 1 , wherein the content of the specific cellulose derivative is 10% by mass or more and 40% by mass or less.

3. The molding material according to claim 1 or 2, wherein the content of the cellulose fiber in the molding material is XC [mass%] and the content of the specific cellulose derivative is XD [mass%], and the relationship of 0.14≦XD / XC≦0.80 is satisfied.

4. The molding material is A The molding material according to claim 1 or 2, which contains the specific cellulose derivative having an alkyl group having 1 to 10 carbon atoms.

5. The molding material according to claim 1 or 2, further comprising a second cellulose derivative which is at least one selected from the group consisting of cellulose acetate propionate, cellulose acetate butyrate, and cellulose acetate.

6. The molding material according to claim 5 , wherein the content of the second cellulose derivative is 10% by mass or more and 40% by mass or less.

7. In the specific cellulose derivative, the total DS value of the chemical structures represented by the formula (1) and the formula (3) is 1.5 or more and 2.7 or less; The total DS value of the chemical structures represented by the formula (2) and the formula (4) is 0.3 or more and 1.5 or less, The molding material according to claim 1 or 2, wherein the total DS value of all the substituents is 2.0 or more and 2.7 or less.

8. The molding material according to claim 1 or 2, further comprising a flame retardant.

9. The molding material according to claim 1 or 2, further comprising an antioxidant.

Citation Information

Patent Citations

  • Composite structure

    JP2005504184A