A laminated film with a resin layer containing a chromic compound in microcapsules addresses flexibility and scratch resistance issues, enabling high hardness and repeated bending while maintaining color tone change, suitable for decorative uses.

JP2024140941APending Publication Date: 2024-10-10MITSUBISHI CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023052322
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing laminated films with chromic compounds lack flexibility and scratch resistance, and the chromic compounds are often destroyed by ultraviolet irradiation when mixed with a hard coat agent, limiting their application to decorative purposes and the ability to follow complex curved surfaces.

Method used

A laminated film structure is developed with a resin layer containing a binder resin and a chromic compound, encapsulated in microcapsules, which provides flexibility, scratch resistance, and color tone change in response to external stimuli, while using a specific resin composition and layer thickness to enhance durability.

Benefits of technology

The laminated film achieves high surface hardness (H or higher), excellent repeated bending properties (up to 200,000 bends), and effective color tone change, suitable for decorative applications without the need for increased base film tensile modulus, allowing use on general-purpose films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140941000001
    Figure 2024140941000001
  • Figure 2024140941000002
    Figure 2024140941000002
  • Figure 2024140941000003
    Figure 2024140941000003
Patent Text Reader

Abstract

To provide a laminate film which is excellent in practical repeated bending characteristics and scratch resistance while having adequate hardness and flexibility, and has such characteristics that color tone is changed by stimulation from outside.SOLUTION: A laminate film has such a structure that a resin layer is provided on at least one surface of a base material film, wherein the resin layer contains a binder resin (A) and a chromic compound (B), and a change amount of light transmittance of a wavelength at a minimum value of light transmittance of the surface of the resin layer is 5% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated film, and more particularly to a laminated film excellent in abrasion resistance, repeated folding characteristics, and the characteristic of changing color tone in response to an external stimulus. [Background technology]

[0002] Laminated films with a functional layer on at least one side of a base film are used in various fields such as industrial compounds, optical compounds, electronic component compounds, and battery packaging materials. Polyethylene terephthalate (PET) films, which are representative polyester films, and biaxially oriented PET films in particular, are widely used as the base film for laminated films because of their excellent transparency, mechanical strength, heat resistance, flexibility, and other properties.

[0003] In recent years, thermochromic compounds and photochromic compounds have been used as light-adjusting materials, mainly for optical applications such as contact lenses, window glass, and liquid crystal displays (for example, Patent Document 1). There are also examples of their use as an anti-counterfeiting measure (Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-353801 A [Patent Document 2] Japanese Patent Application Publication No. 3-231394 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the above-mentioned chromic compounds have hardly been applied to decorative purposes. Furthermore, when applied to decorative purposes, it is common to provide an active energy curing type hard coat layer, so when a hard coat agent and a chromic compound are mixed and cured, there is a concern that the chromic compound may be destroyed by ultraviolet light irradiation. Furthermore, depending on the application, it may be necessary to be able to follow complex curved shapes.

[0006] Therefore, the present invention proposes a new laminated film that has appropriate hardness and flexibility, while also having practical repeated bending properties and excellent abrasion resistance, and yet has the property of changing color tone in response to external stimuli. [Means for solving the problem]

[0007] In view of the above circumstances, the present inventors have conducted extensive research and found that the above problems can be easily solved by providing a laminated structure of resin layers having specific configurations, and have completed the present invention. That is, the present invention provides the following items [1] to

[19] .

[0008] [1] A laminate film having a resin layer on at least one surface of a base film, the resin layer containing a binder resin (A) and a chromic compound (B), and a change in light transmittance at a wavelength at a minimum value of the light transmittance of the surface of the resin layer of 5% or more. [2] The laminated film according to the above [1], wherein the binder resin (A) is an acrylic resin. [3] The laminate film according to the above [1] or [2], wherein the chromic compound (B) is a photochromic compound or a thermochromic compound. [4] The laminate film according to any one of the above [1] to [3], wherein the content of the chromic compound (B) in the resin layer is 0.1% by mass to 5.0% by mass. [5] The laminate film according to any one of the above [1] to [4], wherein the resin layer is formed by curing a resin composition containing a chromic compound (B) in microcapsules. [6] The laminated film according to any one of the above [1] to [5], wherein the acrylic resin is an active energy ray-curable type. [7] The laminate film according to any one of the above [1] to [6], wherein the base film is a polyester film. [8] The laminate film according to any one of the above [1] to [7], wherein the base film is a polyethylene terephthalate (PET) film. [9] The laminate film according to any one of the above [1] to [8], wherein the base film is a copolymer polyester film.

[10] The laminate film according to any one of the above [1] to [9], which can be folded 200,000 times or more in a repeated folding property evaluation (outward bending, under the condition of R=1.5).

[11] The laminate film according to any one of the above [1] to

[10] , further comprising a printed layer between the base film and the resin layer.

[12] The laminate film according to any one of the above [1] to

[11] , wherein the resin layer has a thickness of 20 μm or less.

[13] A laminate having a resin layer on at least one side of a base film, the resin layer containing a binder resin (A) and a chromic compound (B), and other resin films bonded to both sides of the base film via adhesive layers.

[14] The laminate according to the above

[13] , wherein the other resin layer to be bonded to the resin layer side is a PMMA resin.

[15] The laminate according to the above

[13] , wherein the other resin layer to be bonded to the surface of the base film via an adhesive layer is an ABS resin.

[16] The laminate film according to any one of the above [1] to

[12] , which is for molding or decoration.

[17] The laminate according to any one of the above

[13] to

[15] , which is for molding or decoration.

[18] The laminate film according to any one of the above [1] to

[12] , which is used for decorating automobile parts.

[19] The laminate according to any one of the above

[13] to

[15] , which is used for decorating an automobile part. Effect of the Invention

[0009] According to the present invention, it is possible to provide a laminated film that has appropriate hardness and flexibility, is excellent in practical repeated bending properties and abrasion resistance, and yet has the property of changing color tone in response to an external stimulus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Next, the present invention will be described based on an embodiment, however, the present invention is not limited to the embodiment described below.

[0011] <<Laminated film>> A laminate film according to one embodiment of the present invention (hereinafter, sometimes referred to as "the present laminate film") is a laminate film having a configuration in which a cured resin layer is laminated on at least one surface of a base film (hereinafter, sometimes referred to as "the present base film"). As long as the present laminate film has the above-mentioned structure, it may have other layers.

[0012] <Base film> The material and configuration of the base film are not limited as long as the film can provide sufficient rigidity and repeated folding properties. However, a polyester film is preferred because it has suitable hardness and flexibility while providing practical repeated folding properties and excellent abrasion resistance.

[0013] The substrate film may have a single layer structure or a multilayer structure. When the base film has a multi-layer structure, it may have not only a two-layer or three-layer structure but also a four-layer or more layer structure as long as it does not deviate from the gist of the present invention.

[0014] The base film may be a single layer or a multilayer, and the main component resin of each layer is preferably polyester. Such a film is called a "polyester film." In this case, "main component resin" means the resin that is contained in the largest proportion among the resins constituting the base film, for example, a resin that accounts for 50 mass % or more, particularly 70 mass % or more, and even more particularly 80 mass % or more (including 100 mass %) of the resins constituting the base film. Each layer constituting the base film may contain a resin other than polyester or a component other than resin, so long as the main component resin is polyester.

[0015] (polyester) The polyester as the main component resin of each layer constituting the base film (hereinafter sometimes referred to as "the polyester") may be either a homopolyester or a copolymer polyester.

[0016] When the present polyester is a homopolyester, it is preferably one obtained by polycondensation of an aromatic dicarboxylic acid and an aliphatic glycol. Examples of the aromatic dicarboxylic acid include terephthalic acid and 2,6-naphthalenedicarboxylic acid. Examples of the aliphatic glycol include ethylene glycol, diethylene glycol, and 1,4-cyclohexanedimethanol.

[0017] When the polyester is a copolymer polyester, the dicarboxylic acid component may be, for example, one or more of isophthalic acid, phthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, sebacic acid, etc. On the other hand, the glycol component may be, for example, one or more of ethylene glycol, diethylene glycol, propylene glycol, butanediol, 1,4-cyclohexanedimethanol, neopentyl glycol, etc.

[0018] As the polymerization catalyst for polyester, known catalysts such as antimony compounds, germanium compounds, titanium compounds, aluminum compounds, etc. can be used. Among these, in the present invention, polyesters polymerized using antimony compounds or titanium compounds as catalysts are preferred. Specific examples of typical polyesters include polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), polybutylene naphthalate (PBN), polyethylene furanoate (PEF), etc. Among them, PET and PEN are preferable from the viewpoint of handling, and PET is most preferable. When the main component resin of each layer constituting the base film is, for example, polyethylene terephthalate, the film is called a “polyethylene terephthalate film.” The same applies when the main component resin is another resin.

[0019] (Other resin components) Each layer constituting the base film may be made of a resin other than polyester as the main component resin, such as epoxy, polyarylate, polyethersulfone, polycarbonate, polyetherketone, polysulfone, polyphenylene sulfide, polyester-based liquid crystal polymer, triacetyl cellulose, cellulose derivatives, polypropylene, polyamides, polycycloolefins, etc.

[0020] (particle) The base film may contain particles for the main purposes of imparting lubricity to the film surface and preventing scratches during each process. The type of the particles is not particularly limited as long as they are particles that can provide easy slipping. For example, inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, and titanium oxide, and organic particles such as acrylic resin, styrene resin, urea resin, phenol resin, epoxy resin, and benzoguanamine resin can be mentioned. These can be used alone or in combination of two or more kinds. Furthermore, precipitated particles obtained by precipitating and finely dispersing a part of a metal compound such as a catalyst during the polyester production process can also be used.

[0021] The shape of the particles is not particularly limited, and may be, for example, spherical, blocky, rod-like, flat, or the like. Furthermore, there is no particular limitation on the hardness, specific gravity, color, etc. of the above particles. Two or more kinds of these particles may be used in combination as necessary.

[0022] The average particle size of the particles is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 2.5 μm or less. If it is 5 μm or less, the surface roughness of the substrate film is not too rough, and no problems occur when forming a cured resin layer made of various curing compositions in a later process. On the other hand, the average particle size of the particles is preferably 0.01 μm or more, and even more preferably 0.5 μm or more.

[0023] The content of the particles in the base film is preferably 5% by mass or less, more preferably from 0.0003% to 3% by mass, and even more preferably from 0.01% to 2% by mass. When the average particle size of the particles is within the above range, the surface roughness of the base film is not too rough, and problems that arise when forming a cured resin layer made of various curing compositions in a subsequent process can be suppressed.

[0024] The method of adding particles to the base film is not particularly limited, and any conventionally known method can be used. For example, the particles can be added at any stage of the production of raw material resin such as polyester. When the base film is polyester, it is preferable to add the particles after the completion of esterification or transesterification reaction.

[0025] (Other Ingredients) The substrate film may contain other components as required, such as conventionally known antioxidants, antistatic agents, heat stabilizers, lubricants, dyes, pigments, and ultraviolet absorbing agents. In particular, it is preferred that the laminate film contains an ultraviolet absorbing agent in order to ensure the weather resistance of the film.

[0026] (Thickness of base film) The thickness of the present base film is, for example, preferably 9 μm or more and 125 μm or less, more preferably 12 μm or more and 100 μm or less, and even more preferably 20 μm or more and 75 μm or less, in order to obtain sufficient rigidity and repeated folding properties.

[0027] (Production method) The substrate film can be formed, for example, from a resin composition by a melt casting method or a solution casting method. In the case of a multi-layer structure, co-extrusion may be used. The film may be uniaxially or biaxially stretched, with the biaxially stretched film being preferred from the standpoint of rigidity.

[0028] In general, first, undried or dried polyester chips are fed into a melt extrusion device by a known method, and heated to a temperature equal to or higher than the melting point of each polymer to melt it. The molten polymer is then extruded from a die and rapidly cooled to a temperature equal to or lower than the glass transition temperature on a rotating cooling drum to obtain a substantially amorphous unoriented sheet. In this case, in order to improve the flatness of the sheet, it is preferable to increase the adhesion between the sheet and the rotating cooling drum, and in the present invention, an electrostatic application adhesion method and / or a liquid application adhesion method are preferably adopted.

[0029] From the viewpoint of film strength, it is preferable to biaxially stretch the sheet obtained as described above to form a film. Specifically, the stretching conditions are as follows: the unstretched sheet is stretched in the longitudinal direction (machine direction) at 70 to 145°C, preferably 80 to 120°C, at a stretch ratio of 2.0 to 4.5 times, preferably 3.0 to 4.0 times, to form a uniaxially stretched film. Next, the film is stretched in the transverse direction (width direction) perpendicular to the longitudinal direction (machine direction) at a stretching ratio of 3.0 to 6.5 times or 3.5 to 6.0 times at 90 to 160° C. to obtain a biaxially stretched film. Subsequently, it is preferable to carry out a heat treatment (heat setting) for 10 to 600 seconds under tension or relaxation of 30% or less at 210 to 260° C. Then, it is preferable to relax the film by 1 to 10% in the longitudinal and / or transverse directions in the maximum temperature zone of the heat treatment and / or in the cooling zone at the exit of the heat treatment. The longitudinal direction (machine direction) of the film refers to the direction in which the film advances during the film manufacturing process, i.e., the direction in which the film roll is wound. The transverse direction (width direction) refers to the direction parallel to the film surface and perpendicular to the longitudinal direction, i.e., the direction parallel to the central axis of the roll when the film is in a roll shape.

[0030] (Characteristics of the base film) The tensile modulus of the base film (JIS K 7161) is preferably 2.0 GPa or more, and the upper limit is preferably 9.0 GPa or less, from the viewpoint of obtaining necessary and sufficient rigidity and repeated bending property, more preferably 3.0 GPa to 8.0 GPa, and even more preferably 3.0 GPa to 7.0 GPa.

[0031] <Resin layer> The laminated film has a resin layer provided on at least one surface of a substrate film. The resin layer contains a binder resin (A) and a chromic compound (B). The resin layer may be formed from a resin composition.

[0032] <Resin composition> The resin composition for forming the resin layer will be described below. (A) Binder resin The binder resin can be any resin that is generally used together with a chromic material, and examples of the binder resin include polyester resins, polycarbonate resins, acrylic resins, and polyurethane resins. Among these, acrylic resins are preferred from the viewpoint of transparency, etc.

[0033] (Acrylic resin) The acrylic resin is a polymer made of polymerizable monomers including acrylic and methacrylic monomers. These may be homopolymers or copolymers, or copolymers with polymerizable monomers other than acrylic and methacrylic monomers. Among the above, a polymer obtained by polymerizing a polymerizable monomer including an acrylic or methacrylic monomer is preferred, and it is more preferred that the polymerizable monomer includes an alkyl (meth)acrylic acid ester. In addition, in order to make it easier to dissolve or disperse the binder resin when the coating liquid is water-based, it is preferred that the polymerizable monomer has a hydrophilic group such as a hydroxyl group or a carboxyl group. Therefore, the acrylic resin is also preferably a polymer obtained by polymerizing a polymerizable monomer including an alkyl (meth)acrylic acid ester and a hydrophilic group-containing monomer such as a hydroxyl group-containing monomer or a carboxyl group-containing monomer. The acrylic resin may also be an emulsion polymer obtained by polymerizing a polymerizable monomer in the presence of a surfactant. The acrylic resin in the present invention is preferably an active energy ray curable type, and the coating film is cured by irradiation with active energy rays, thereby forming a cured coating film on the substrate.

[0034] Examples of the alkyl (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, etc. In addition, the alkyl (meth)acrylic acid esters may be hydroxyl group-containing alkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. These may be used alone or in combination of two or more. Among these, from the viewpoint of the effect of preventing oligomer precipitation by heat treatment, (meth)acrylic acid is preferable, and acrylic acid is more preferable. That is, the acrylic structure of the (meth)acrylic polymer is preferably a (meth)acrylic acid structure. The (meth)acrylic polymer may have a radically polymerizable double bond.

[0035] The resin layer is preferably formed from a curable resin composition C, and the resin composition preferably contains urethane (meth)acrylate. The mass average molecular weight of the resin composition is preferably 100 or more, more preferably 200 or more, and even more preferably 400 or more. On the other hand, the upper limit is preferably 500,000 or less, more preferably 400,000 or less, and even more preferably 250,000 or less.

[0036] In the present invention, when the expression "(meth)acrylic" is used, it means either or both of "acrylic" and "methacrylic". The same applies to "(meth)acrylate" and "(meth)acryloyl". Furthermore, "(poly)propylene glycol" means either or both of "propylene glycol" and "polypropylene glycol". The same applies to "(poly)ethylene glycol".

[0037] (Urethane (meth)acrylate) The urethane (meth)acrylate is a compound obtained by reacting an isocyanate compound with a hydroxyl group-containing (meth)acrylate compound, or a compound obtained by reacting an isocyanate compound with a polyol compound with a hydroxyl group-containing (meth)acrylate compound. The urethane (meth)acrylate may be used alone or in combination of two or more kinds.

[0038] Examples of the isocyanate-based compound include polyisocyanate-based compounds such as aromatic polyisocyanates, aliphatic polyisocyanates, and alicyclic polyisocyanates, and among these, diisocyanate compounds are preferred. Examples of the isocyanate-based compound include isocyanate-based compounds having an isocyanurate skeleton obtained by isocyanating a diisocyanate compound.

[0039] Examples of the aromatic polyisocyanate include tolylene diisocyanate, diphenylmethane diisocyanate, polyphenylmethane polyisocyanate, modified diphenylmethane diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, phenylene diisocyanate, and naphthalene diisocyanate.

[0040] Examples of the aliphatic polyisocyanates include hexamethylene diisocyanate, pentamethylene diisocyanate, trimethylhexamethylene diisocyanate, lysine diisocyanate, and lysine triisocyanate.

[0041] Examples of the alicyclic polyisocyanate include hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, and 1,4-bis(isocyanatomethyl)cyclohexane.

[0042] Among these, aliphatic diisocyanates and alicyclic diisocyanates are preferred from the viewpoint of excellent yellowing resistance. Also, isocyanate-based compounds having an isocyanurate skeleton are preferred, and from the same viewpoint, isocyanate-based compounds having an isocyanurate skeleton obtained by isocyanating an aliphatic diisocyanate or an alicyclic diisocyanate are also preferred, and among these, isocyanate-based compounds having an isocyanurate skeleton are more preferred. The isocyanate compounds may be used alone or in combination of two or more kinds.

[0043] The hydroxyl group-containing (meth)acrylate is a compound having a hydroxyl group and a (meth)acryloyl group, and examples thereof include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 6-hydroxyhexyl (meth)acrylate, 2-hydroxyethyl acryloyl phosphate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, caprolactone-modified 2-hydroxyethyl (meth)acrylate, dipropylene glycol (meth)acrylate, fatty acid-modified glycidyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and 2-hydroxy-3-(meth)acrylate. Examples of the hydroxyl group-containing (meth)acrylate include monofunctional hydroxyl group-containing (meth)acrylates having one ethylenically unsaturated group such as oleyloxypropyl (meth)acrylate; bifunctional hydroxyl group-containing (meth)acrylates having two ethylenically unsaturated groups such as glycerin di(meth)acrylate and 2-hydroxy-3-acryloyl-oxypropyl methacrylate; trifunctional or higher hydroxyl group-containing (meth)acrylates having three or more ethylenically unsaturated groups such as pentaerythritol tri(meth)acrylate, caprolactone-modified pentaerythritol tri(meth)acrylate, ethylene oxide-modified pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, caprolactone-modified dipentaerythritol penta(meth)acrylate, and ethylene oxide-modified dipentaerythritol penta(meth)acrylate. These can be used alone or in combination of two or more. Among these, (meth)acrylate compounds containing three or less ethylenically unsaturated groups are preferred, and polyfunctional (meth)acrylate compounds containing two or more ethylenically unsaturated groups are more preferred, with pentaerythritol tri(meth)acrylate being particularly preferred, because they have excellent reactivity and versatility and are well balanced with the scratch resistance of the cured coating film.

[0044] The polyol compound may be any compound having two or more hydroxyl groups (excluding the above hydroxyl group-containing (meth)acrylates). Examples of the polyol-based compound include aliphatic polyols, alicyclic polyols, polyether-based polyols, polyester-based polyols, polycarbonate-based polyols, polyolefin-based polyols, polybutadiene-based polyols, polyisoprene-based polyols, (meth)acrylic-based polyols, and polysiloxane-based polyols.

[0045] Examples of the aliphatic polyol include ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, trimethylene glycol, dimethylolpropane, neopentyl glycol, 2,2-diethyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,4-tetramethylenediol, 1,3-tetramethylenediol, 2-methyl-1,3-trimethylenediol, 1,5-pentamethylenediol, 1 Examples of such fatty alcohols include aliphatic alcohols containing two hydroxyl groups, such as 1,6-hexamethylenediol, 3-methyl-1,5-pentamethylenediol, 2,4-diethyl-1,5-pentamethylenediol, pentaerythritol diacrylate, 1,9-nonanediol, and 2-methyl-1,8-octanediol; sugar alcohols such as xylitol and sorbitol; and aliphatic alcohols containing three or more hydroxyl groups, such as glycerin, trimethylolpropane, and trimethylolethane.

[0046] Examples of the alicyclic polyol include cyclohexanediols such as 1,4-cyclohexanediol and cyclohexyldimethanol, hydrogenated bisphenols such as hydrogenated bisphenol A, and tricyclodecane dimethanol.

[0047] Examples of polyether polyols include alkylene structure-containing polyether polyols such as polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polybutylene glycol, polypentamethylene glycol, and polyhexamethylene glycol, and random or block copolymers of these polyalkylene glycols.

[0048] Examples of polyester-based polyols include condensation polymers of polyhydric alcohols and polycarboxylic acids, ring-opening polymers of cyclic esters (lactones), and reaction products of three components: polyhydric alcohols, polycarboxylic acids, and cyclic esters.

[0049] Examples of the polyhydric alcohol include ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, trimethylene glycol, 1,4-tetramethylene diol, 1,3-tetramethylene diol, 2-methyl-1,3-trimethylene diol, 1,5-pentamethylene diol, neopentyl glycol, 1,6-hexamethylene diol, 3-methyl-1,5-pentamethylene diol, 2,4-diethyl-1,5-pentamethylene diol, glycerin, trimethylolpropane, trimethylolethane, cyclohexanediols (such as 1,4-cyclohexanediol), bisphenols (such as bisphenol A), and sugar alcohols (such as xylitol and sorbitol).

[0050] Examples of the polyvalent carboxylic acid include aliphatic dicarboxylic acids such as malonic acid, maleic acid, fumaric acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, and dodecanedioic acid; alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid; and aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, orthophthalic acid, 2,6-naphthalenedicarboxylic acid, paraphenylenedicarboxylic acid, and trimellitic acid.

[0051] Examples of the cyclic ester include propiolactone, β-methyl-δ-valerolactone, and ε-caprolactone.

[0052] Examples of the polycarbonate-based polyol include a reaction product of a polyhydric alcohol with phosgene, and a ring-opening polymer of a cyclic carbonate (such as an alkylene carbonate).

[0053] Examples of the polyhydric alcohol used in the polycarbonate-based polyol include the polyhydric alcohols exemplified in the description of the polyester-based polyol, and examples of the alkylene carbonate include ethylene carbonate, trimethylene carbonate, tetramethylene carbonate, and hexamethylene carbonate.

[0054] The polycarbonate-based polyol may be any compound having a carbonate bond in the molecule and a hydroxyl group at the end, and may have an ester bond in addition to the carbonate bond.

[0055] The polyolefin polyols include those having a homopolymer or copolymer of ethylene, propylene, butene, or the like as a saturated hydrocarbon skeleton and having hydroxyl groups at the molecular terminals.

[0056] The polybutadiene-based polyols include those having a butadiene copolymer as a hydrocarbon skeleton and having hydroxyl groups at the molecular terminals. The polybutadiene-based polyol may be a hydrogenated polybutadiene polyol in which all or a part of the ethylenically unsaturated groups contained in the structure thereof have been hydrogenated.

[0057] The polyisoprene-based polyols include those having an isoprene copolymer as a hydrocarbon backbone and having hydroxyl groups at the molecular terminals. The polyisoprene-based polyol may be a hydrogenated polyisoprene polyol in which all or a part of the ethylenically unsaturated groups contained in the structure have been hydrogenated.

[0058] The (meth)acrylic polyol may be one having at least two hydroxyl groups in the molecule of a (meth)acrylic acid ester polymer or copolymer, and examples of such (meth)acrylic acid ester include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, and octadecyl (meth)acrylate. In addition, copolymers of (meth)acrylic acid esters and hydroxyalkyl (meth)acrylates such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate may also be used. The above hydroxyl group-containing (meth)acrylates are excluded.

[0059] Examples of the polysiloxane polyol include dimethylpolysiloxane polyol and methylphenylpolysiloxane polyol.

[0060] The above polyol compounds can be used alone or in combination of two or more.

[0061] In the addition reaction between the isocyanate compound and a hydroxyl group-containing (meth)acrylate compound, or the addition reaction between an isocyanate compound, a hydroxyl group-containing (meth)acrylate compound, and a polyol, the reaction is terminated when the residual isocyanate group content in the reaction system reaches 0.5 mass% or less, thereby obtaining a urethane (meth)acrylate.

[0062] When the urethane (meth)acrylate includes one obtained by reacting an isocyanate compound, a polyol compound, and a hydroxyl group-containing (meth)acrylate compound, it is preferable to obtain the urethane (meth)acrylate by reacting a reaction product having an isocyanate group obtained by reacting an isocyanate compound with a polyol compound, or a mixture of the reaction product and an isocyanate compound, with a hydroxyl group-containing (meth)acrylate compound. The urethane (meth)acrylate obtained by such a reaction may be a mixture of one obtained by reacting an isocyanate-based compound with a hydroxyl group-containing (meth)acrylate-based compound and one obtained by reacting an isocyanate-based compound, a polyol-based compound, and a hydroxyl group-containing (meth)acrylate-based compound.

[0063] In the reaction between an isocyanate compound and a hydroxyl group-containing (meth)acrylate compound, it is also preferable to use a catalyst for the purpose of promoting the reaction. Examples of such catalysts include organometallic compounds such as dibutyltin dilaurate, dibutyltin diacetate, trimethyltin hydroxide, tetra-n-butyltin, zinc bisacetylacetonate, zirconium tris(acetylacetonate)ethylacetoacetate, and zirconium tetraacetylacetonate; metal salts such as tin octenate, zinc hexanoate, zinc octenate, zinc stearate, zirconium 2-ethylhexanoate, cobalt naphthenate, stannous chloride, stannous chloride, and potassium acetate; triethylamine, triethylenediamine, benzyldiethylamine, 1,4-diazabicyclo[2,2,2]octane, and 1,8-diazabicyclo[5,4,0]un. Decene, N,N,N',N'-tetramethyl-1,3-butanediamine, N-methylmorpholine, N-ethylmorpholine, and other amine catalysts, bismuth nitrate, bismuth bromide, bismuth iodide, bismuth sulfide, and other organic bismuth compounds such as dibutyl bismuth dilaurate and dioctyl bismuth dilaurate, and organic acid bismuth salts such as bismuth 2-ethylhexanoate, bismuth naphthenate, bismuth isodecanoate, bismuth neodecanoate, bismuth laurate, bismuth maleate, bismuth stearate, bismuth oleate, bismuth linoleate, bismuth acetate, bismuth bisneodecanoate, bismuth disalicylate, and bismuth digallate, and among these, dibutyltin dilaurate and 1,8-diazabicyclo[5,4,0]undecene are preferred. These can be used alone or in combination of two or more.

[0064] In the reaction between an isocyanate compound and a hydroxyl group-containing (meth)acrylate compound, an organic solvent having no functional group reactive with an isocyanate group, for example, an ester such as ethyl acetate or butyl acetate, a ketone such as methyl ethyl ketone or methyl isobutyl ketone, an aromatic such as toluene or xylene, etc., can be used. A polymerization inhibitor or the like may also be used as appropriate.

[0065] In addition, the urethane (meth)acrylate is a reaction product of a hydroxyl group-containing (meth)acrylate compound and an isocyanate compound, or a hydroxyl group-containing (meth)acrylate compound, an isocyanate compound, and a polyol compound, but may be produced by reacting a mixture of a hydroxyl group-containing (meth)acrylate and a hydroxyl group-free (meth)acrylate with an isocyanate compound. Alternatively, it may be produced by reacting a mixture of a hydroxyl group-containing (meth)acrylate and a hydroxyl group-free (meth)acrylate with an isocyanate compound and a polyol compound. In this case, the hydroxyl group-free (meth)acrylate remains as an unreacted product, but it is preferable to use it by containing it as it is in the curable resin composition. In the reaction between the isocyanate compound and the hydroxyl group-containing (meth)acrylate compound described above, a part or all of the isocyanate compound may be a reaction product of the isocyanate compound and a polyol compound, as described above.

[0066] The mass average molecular weight of the urethane (meth)acrylate is, for example, from 3,000 to 100,000, preferably from 5,000 to 70,000, and more preferably from 8,000 to 30,000. By forming a cured resin layer satisfying the above range in a laminate structure such as a laminate film, good film flatness can be ensured.

[0067] The (meth)acryloyl group equivalent of the urethane (meth)acrylate is, for example, 120 g / eq or more and 250 g / eq or less, preferably 135 g / eq or more and 220 g / eq or less, and more preferably 150 g / eq or more and 200 g / eq or less. When the (meth)acryloyl group equivalent of the urethane (meth)acrylate is within the above range, a cured resin layer having an appropriate crosslinking density can be formed by adjusting the crosslinking points, and high hardness can be imparted by forming the cured resin layer in a laminate structure such as a laminate film.

[0068] The ratio of the urethane (meth)acrylate in the resin composition is preferably 50% by mass or more, and more preferably 60% by mass or more, based on the total solid content.

[0069] In the present invention, it is preferable to prepare a base polymer by polymerizing the above urethane (meth)acrylate alone or in combination of two or more kinds. The base polymer is preferably formed by dissolving or dispersing in a solvent or the like described below.

[0070] (solvent) The resin composition may be diluted with a solvent to form a coating liquid. The resin composition may be dissolved in a solvent to form a liquid coating liquid, or may be dispersed in the solvent. The solvent is preferably an organic solvent.Specific examples of the organic solvent include aromatic solvents such as toluene and xylene; ketone solvents such as methyl ethyl ketone (MEK), acetone, methyl isobutyl ketone (MIBK), cyclohexanone, and diisobutyl ketone; ether solvents such as diethyl ether, isopropyl ether, tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether (PGM), anisole, and phenetole; ester solvents such as ethyl acetate, butyl acetate, isopropyl acetate, and ethylene glycol diacetate; amide solvents such as dimethylformamide, diethylformamide, dimethylacetamide, and N-methylpyrrolidone; cellosolve solvents such as methyl cellosolve, ethyl cellosolve, and butyl cellosolve; alcohol solvents such as methanol, ethanol, propanol, isopropanol, and butanol; and halogen solvents such as dichloromethane and chloroform. These organic solvents may be used alone or in combination of two or more. Among these organic solvents, ester solvents, ether solvents, alcohol solvents and ketone solvents are preferably used.

[0071] The amount of the organic solvent used is not particularly limited, and is appropriately determined in consideration of the coatability of the prepared resin composition, the viscosity and surface tension of the liquid, the compatibility of the solid content, etc. The resin composition is prepared as a coating liquid having a solid content concentration of preferably 15 to 80 mass%, more preferably 20 to 70 mass%, using the above-mentioned solvent. Note that the "solid content" in the resin composition means the components excluding the solvent, which is a volatile component, and includes not only solid components but also semi-solid and viscous liquid substances.

[0072] (Other ingredients) The resin composition may contain a photopolymerizable compound such as a (meth)acrylate in addition to the above urethane (meth)acrylate. Furthermore, various additives may be appropriately blended into the resin composition C as necessary within the scope of the present invention. Examples of additives that may be used in combination include photoinitiators, light stabilizers, antioxidants, antistatic agents, flame retardants, leveling agents, dispersants, thixotropy-imparting agents (thickeners), and defoamers. Here, examples of the leveling agent include fluorine-based leveling agents, silicone-based leveling agents, and acrylic-based leveling agents. Among them, the surface of the resin layer can be given a function of repelling water and oil, and a function of preventing adhesion of dirt such as fingerprints. In this case, the leveling agent is preferably a fluorine-based leveling agent.

[0073] (Photoinitiator) When the resin composition is a photocurable resin composition, it is preferable to contain a photoinitiator in order to improve the curability. The photoinitiator is a photopolymerization initiator, and a known one can be used. Examples of the photopolymerization initiator include a photoradical generator and a photoacid generator.

[0074] Among the photopolymerization initiators that can be used in the resin composition, examples of the photoradical generator include benzoin and its alkyl ethers, such as benzoin, benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl ether; acetophenone, 2,2-dimethoxy-2-phenylacetophenone [e.g., trade name "Omnirad (registered trademark) 651", manufactured by IGM RESINS], 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone [e.g., trade name "Omnirad (registered trademark) 184", manufactured by IGM RESINS], 2-hydroxy-2-methyl-1-phenylpropan-1-one [e.g., trade name "Omnirad (registered trademark) 1173", manufactured by IGM RESINS], and the like. IGM RESINS], 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one [e.g., trade name "Omnirad® 127, IGM RESINS], 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one [e.g., trade name "Omnirad® 2959", IGM RESINS], 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one [e.g., trade name "Omnirad® 907", IGM alkylphenones such as 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone; phosphine oxides such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide [for example, trade name "Omnirad (registered trademark) TPO", manufactured by IGM RESINS] and bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide [for example, trade name "Omnirad (registered trademark) 819", manufactured by IGM RESINS]; anthraquinones such as 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, and 2-amylanthraquinone; benzophenone and various derivatives thereof; and formic acid derivatives such as methyl benzoylformate and ethyl benzoylformate.These may be used alone or in combination of two or more.

[0075] Among these photoradical generators, from the viewpoint of the light resistance of the cured product, preferred are alkylphenones, phosphine oxides, and formic acid derivatives, more preferred are 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, and methyl benzoylformate, and particularly preferred are 1-hydroxycyclohexyl phenyl ketone and 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one.

[0076] As the photoacid generator, known ones can be used, among which diaryliodonium salts and triarylsulfonium salts are preferred from the viewpoints of curability, acid generation efficiency, etc. Specific examples include anion salts of di(alkyl-substituted)phenyliodonium (specifically, PF6 salts, SbF5 salts, tetrakis(perfluorophenyl)borate salts, etc.). A specific example of the anion salt of (alkyl-substituted) phenyliodonium is particularly preferably a PF6 salt of dialkylphenyliodonium [trade name "Omniad (registered trademark) 250", manufactured by IGM RESINS]. These photoacid generators may be used alone or in combination of two or more.

[0077] The content of the photoinitiator is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and particularly preferably 1 part by mass or more, from the viewpoint of improving the curability, relative to a total of 100 parts by mass of the compounds having a (meth)acryloyl group in the resin composition C. On the other hand, from the viewpoint of maintaining the stability of the coating liquid when the resin composition is made into a solution and from the viewpoint of the flatness of the cured coating film, the content is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and particularly preferably 5 parts by mass or less.

[0078] (Viscosity of Resin Composition) In order to ensure good coatability, the resin composition C for forming the resin layer preferably has a viscosity at 25°C measured with an E-type viscometer of 10 to 60 mPa·s, and more preferably 30 mPa·s or less, more preferably 20 mPa·s or less, more preferably 15 mPa·s or less, and even more preferably 12 mPa·s or less.

[0079] (B) Chromic Compound A chromic compound is a compound whose optical properties (e.g., transmittance, color, hue, fluorescence intensity, refractive index, reflectance) change reversibly or irreversibly in response to an external stimulus, such as temperature, light, water, pH, pressure, or electricity.

[0080] Examples of chromic compounds that can be used include thermochromic compounds, photochromic compounds, hydrochromic compounds, pH-responsive compounds (such as halochromic compounds or acidichromic compounds), piezochromic compounds, and electrochromic compounds.

[0081] As each compound, various known compounds can be used. For example, examples of thermochromic compounds include Sakura Cray-Pas' TC color (reversible), Matsui Color Chemical Industry's Chromicolor (reversible), and Matsui Color Chemical Industry's Thermolock (quasi-irreversible). Examples of photochromic compounds include Photopia Color (reversible) from Matsui Pigment Chemical Industry Co., Ltd., Photolock (irreversible) from Matsui Pigment Chemical Industry Co., Ltd., and Thermocolor (reversible) from Recording Materials Research Institute. These are just a few examples, and various chromic compounds such as irreversible type, heat accumulation type, quasi-reversible type, and reversible type can be selected according to the purpose. For example, in thermochromic compounds, examples of irreversible types include inorganic compounds using metal salts and organic compounds using a thermal recording method. Examples of reversible types include inorganic compounds using metal complex salts, organic compounds using condensed aromatic ring-substituted ethylene derivatives, organic compounds using liquid crystals (e.g., cholesteric liquid crystals), and organic compounds using Metamocolor (registered trademark).

[0082] As an example of a thermochromic compound, a leuco dye will be described. Leuco dyes are dyes that irreversibly change their chemical structure through an oxidation-reduction reaction with a developer to develop a color, and are themselves colorless or light-colored dye precursors. Leuco dyes can be classified into two types: those that act as electron donors and those that act as electron acceptors and react with the developer. Either type is acceptable, but those that act as electron donors and react are preferred. Examples of leuco dyes include triphenylmethanephthalide-based leuco compounds, triarylmethane-based leuco compounds, fluoran-based leuco compounds, phenothidian-based leuco compounds, thiofluoran-based leuco compounds, xanthene-based leuco compounds, indophthalyl-based leuco compounds, spiropyran-based leuco compounds, azaphthalide-based leuco compounds, chromenopyrazole-based leuco compounds, methine-based leuco compounds, rhodamine anilinolactam-based leuco compounds, rhodamine lactam-based leuco compounds, quinazoline-based leuco compounds, diazaxanthene-based leuco compounds, and bislactone-based leuco compounds. Among these, triphenylmethanephthalide-based leuco compounds, fluoran-based leuco compounds, or azaphthalide-based leuco compounds are preferred from the viewpoint of color development. The leuco dye may be one type, or two or more types may be used in combination.

[0083] Fluoran-based thermochromic compounds include compounds represented by the following general formula (I): [ka]

[0084] In formula (I), X is a carbon atom or a nitrogen atom, and R1 and R2 each represent a substituted or unsubstituted aromatic group, a substituted or unsubstituted heterocyclic group, or a fluoran group. R1 and R2 may form a part of the fluoran skeleton. R3 represents a hydrogen atom, a halogen atom, a substituted or unsubstituted acyl group, an alkyl group, an alkoxy group, a nitro group, an aryl group, or an amino group. Of these, R3 is preferably a hydrogen atom. In addition, when X is nitrogen, R1 and R2 are preferably aromatic groups which may have a substituent, and when X is carbon, R1 and R2 are preferably groups having a substituted or unsubstituted heterocycle. R1 and R2 may be the same or different, but in consideration of ease of production, R1 and R2 are preferably the same. Also, when X is carbon, it is preferred that R1 and R2 form a part of the fluoran skeleton. For example, examples of fluoran-based thermochromic compounds include the following:

[0085] [Table 1]

[0086] (Temperature regulator) The temperature regulator is a substance that has a melting point and is solid below its melting point, but melts and becomes liquid when the temperature rises to its melting point. The melted temperature regulator functions as a solvent for the leuco dye, and the leuco dye migrates to the surface of the developer and develops color. For example, fatty alcohols and fatty acid alkyl esters are exemplified.

[0087] Examples of the aliphatic alcohol include methyl alcohol, ethyl alcohol, 1-propyl alcohol, 1-butyl alcohol, 1-pentyl alcohol, and 1-hexyl alcohol. Examples of fatty acid alkyl esters include methyl formate, ethyl formate, isopropyl formate, isopropyl formate, methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, isopropyl propionate, isopropyl butyrate, isopropyl valerate, isopropyl caprylate, methyl laurate, ethyl laurate, and propyl laurate.

[0088] (Developer) The color developer is preferably an inorganic compound, and specific examples of the color developer include silica, alumina, and zeolite. The amount of developer to be used should be the amount necessary to react with the leuco dye to produce color, and is preferably 10 to 100 parts by weight, more preferably 30 to 200 parts by weight, and even more preferably 50 to 150 parts by weight, per part by weight of the leuco dye.

[0089] From the viewpoint of changing the color to a desired color without impairing the performance of the resin layer, the thermochromic compound is usually added in an amount of 0.1 to 5.0 parts by mass, preferably 0.5 to 3.5 parts by mass, per 100 parts by mass of the resin.

[0090] Thermochromic compounds generally change color in the range of −5° C. to 65° C. In the present invention, one type of thermochromic compound may be used, or two or more types of thermochromic compounds having different color change temperatures and color tones may be used in combination.

[0091] (Microcapsules) In the present invention, from the viewpoint of preventing deterioration of the chromic compound due to irradiation with active energy rays, it is preferable to encapsulate the chromic compound, the temperature regulator, and the color developer and form them into microcapsules. For the microencapsulation, a conventionally known method can be used. Examples of the thermosetting resin that forms the coating of the microcapsules include melamine resin, benzoguanamine resin, cycloguanamine resin, urea resin, thermosetting acrylic resin, polyurethane resin, polyester resin, and epoxy resin.

[0092] (Thickness of resin layer) The thickness of the resin layer is preferably 20.0 μm or less, more preferably 15.0 μm or less, and even more preferably 10.0 μm or less. When the thickness of the resin layer is equal to or less than the above upper limit, curling and heat wrinkles can be prevented in a laminate structure having a resin layer such as a laminate film, and good flatness can be ensured. On the other hand, there is no particular lower limit to the thickness of the resin layer, but it is preferably 1.0 μm or more in terms of adequately protecting the base film.

[0093] The resin layer surface preferably has a light transmittance of 3.0% or less at a wavelength of 380 nm. A light transmittance of 3.0% or less is advantageous in that the mating member to be bonded can be prevented from being deteriorated by ultraviolet rays. From the above viewpoint, the light transmittance of 2.8% or less at a wavelength of 380 nm is more preferable.

[0094] In addition, the maximum reflectance difference at the surface of the resin layer at wavelengths of 500 to 600 nm is preferably 1.5% or less. If the maximum reflectance difference (fluctuation width of light transmittance) is 1.5% or less, it is advantageous in that interference fringes are less visible. From the above viewpoints, the maximum reflectance difference is more preferably 1.0% or less, further preferably 0.5% or less, and particularly preferably 0.3% or less. In the present invention, the maximum reflectance difference refers to the difference between the maximum and minimum reflectance values ​​at wavelengths of 500 to 600 nm.

[0095] <Surface condition of each layer> The surface of the resin layer may be uneven or flat, but is preferably flat from the viewpoint of appearance (surface gloss). On the other hand, it is preferable that the surface is uneven from the viewpoint of imparting antiglare properties. It can be arbitrarily selected according to the required properties.

[0096] <<Laminated film manufacturing method>> The resin layer can be formed by curing a resin composition, for example, by applying a curable resin composition having a mass average molecular weight in the range of 1,000 to 500,000 onto a substrate film and curing the composition. More specifically, the present laminate film can be produced by applying a resin composition to at least one surface of a substrate film and curing the composition to form a resin layer. However, the method for producing the laminate film is not limited to this method.

[0097] <Method of forming resin layer> As described above, the resin layer can be obtained by applying a resin composition to the surface of a substrate film, drying the composition to form a coating layer, and curing the coating layer. Examples of a method for applying the resin composition include air doctor coating, blade coating, rod coating, bar coating, knife coating, squeeze coating, impregnation coating, reverse roll coating, transfer roll coating, gravure coating, kiss roll coating, cast coating, spray coating, curtain coating, calendar coating, and extrusion coating. The drying conditions are not particularly limited, and the drying may be performed at about room temperature or by heating, for example, at about 25 to 120° C., preferably 50 to 100° C., and more preferably 60 to 90° C. The drying time is not particularly limited as long as the solvent can be sufficiently evaporated, and is, for example, about 10 seconds to 30 minutes, and preferably about 15 seconds to 10 minutes.

[0098] The method for curing the resin composition may be appropriately selected depending on the curing mechanism of the resin composition, and if the resin composition is a thermosetting resin composition, it may be cured by heating, and if it is a photocurable resin composition, it may be cured by irradiating it with energy rays. In the laminated film of the present invention, active energy rays that can be used when curing the photocurable resin composition include ultraviolet rays, electron beams, X-rays, infrared rays, and visible light. Among these active energy rays, ultraviolet rays and electron beams are preferred from the viewpoints of curability and prevention of resin deterioration.

[0099] The resin composition is preferably cured by irradiation with energy rays from the viewpoints of molding time and productivity, and of preventing thermal shrinkage and thermal deterioration of each member due to heating, etc. The energy rays may be irradiated from either side, and may be irradiated from the substrate film side or the opposite side of the substrate film. When the resin composition is cured by ultraviolet irradiation in producing the laminated film of the present invention, various ultraviolet irradiation devices can be used, and as the light source, a xenon lamp, a high-pressure mercury lamp, a metal halide lamp, an LED-UV lamp, etc. can be used. The amount of ultraviolet irradiation (unit: mJ / cm 2 ) is usually 50 to 3,000 mJ / cm 2 From the viewpoints of the curability of the curable resin composition, the flexibility of the cured product (cured film), etc., it is preferably 100 to 1,000 mJ / cm 2 From the viewpoint of the flatness of the laminated film, it is more preferably 100 to 500 mJ / cm 2 and is appropriately determined depending on the reaction rate of the (meth)acryloyl group required in each curing step. When the resin composition is used in a particularly severe environment, it is preferable to increase the amount of ultraviolet light to adjust the surface hardness of the cured product of the resin composition.

[0100] In addition, when the resin composition is cured by electron beam irradiation during the production of the laminated film of the present invention, various electron beam irradiation devices can be used. The irradiation dose (Mrad) of the electron beam is usually 0.5 to 20 Mrad, and is preferably in the range of 1 to 15 Mrad from the viewpoints of the curability of the resin composition, the flexibility of the cured product, and prevention of damage to the substrate, but is appropriately determined depending on the reaction rate of the (meth)acryloyl group required in each curing step.

[0101] <<Physical properties of laminated film>> (Pencil hardness) In accordance with JIS K5600-5-4, the pencil hardness of the resin layer is H or more, preferably 2H or more.

[0102] (Repeated bending ability) The laminated film having the above-mentioned structure has a resin layer on the surface of the base film, and the structure of the resin layer is designed within a specific range, thereby further improving the practical repeated bending property. Specifically, the laminated film has enough durability to not crack even when folded more than 200,000 times in a repeated bending property evaluation (inward bending, R=1.5).

[0103] (Discoloration) When the light transmittance in the wavelength region of 380 nm to 780 nm is measured using a spectrophotometer (U-3900H, manufactured by Hitachi High-Technologies Corporation) at room temperature and when heated to 35°C, the change in light transmittance at the maximum absorption wavelength is 5% or more, and preferably 10% or more. By satisfying this range, for example, when a configuration of a resin layer containing a chromic compound / printed layer / base film is applied to the decorative use of automobile parts, it is possible to impart design features such as making the pattern of the underlying printed layer recognizable when the color changes from colored to colorless.

[0104] <<Characteristics and uses of laminated film>> This laminated film is capable of achieving both a high level of surface hardness and repeated bending resistance (flexural durability, inward bending, the ability to bend 200,000 times under conditions of R=1.0). It is presumed that this is because adjusting the composition of the resin layer makes it possible to reduce the stress transmission into the resin layer when the laminated film is bent. Furthermore, by containing a chromic compound, a desired color change can occur within a predetermined temperature range.

[0105] Furthermore, by using such a resin layer, it is not necessary to extremely increase the tensile modulus of elasticity of the substrate film used. In the past, when designing a laminate film having a surface layer with high surface hardness to achieve the desired surface hardness (pencil hardness of 2H or more), it was necessary to review the structural design of the raw materials that make up the base film used and further increase the tensile modulus, if necessary. In contrast, when the resin layer is configured as described above, it is possible to appropriately select a general-purpose base film available on the market, which has the advantage of increasing the freedom in the selection of the base film.

[0106] This laminated film has excellent abrasion resistance, practical repeated folding properties, and colorfastness, and can be used for molding, decoration, and other applications. For example, it can be suitably used for decorating automobile interiors. However, the applications of this laminated film are not limited to these applications.

[0107] [Laminate] The laminate of the present invention has a structure in which a resin layer is provided on at least one side of a substrate film, the resin layer containing a binder resin (A) and a chromic compound (B), and other resin films are laminated on both sides of the substrate film via adhesive layers. Here, the substrate film and the resin layer are as described above.

[0108] (adhesive layer) The adhesive layer in the laminate of the present invention is formed from a pressure-sensitive adhesive, a pressure-sensitive adhesive sheet, an adhesive, etc., but from the viewpoint of excellent adhesiveness, an adhesive is preferably used. As the adhesive, for example, a polyolefin-based adhesive, an acrylic-based adhesive, a polyester-based adhesive, an epoxy-based adhesive, a polyurethane-based adhesive, etc. can be used.

[0109] (Other resin films) The other resin film in the laminate of the present invention is not particularly limited and is appropriately determined depending on the application. Specific examples include acrylic resin film, polyester film, polyolefin film, etc. Among these, the other resin film attached to the resin layer side is preferably an acrylic resin film, and among them, polymethylmethacrylate resin (PMMA resin) is preferable in terms of conformity to a mold during injection molding. In addition, ABS resin (acrylonitrile-butadiene-styrene copolymer resin) is also preferable as the other resin film in terms of conformity to a mold during injection molding.

[0110] (Layer composition) In the embodiment where another resin film is attached to the resin layer side, the layer structure of the laminate of the present invention may be, for example, PMMA resin film / adhesive layer / resin layer / base film. Also preferred is a laminate in which an ABS resin, which is a molding member, is provided on the opposite side of the base film to the resin layer, and specifically, a layer structure of PMMA resin film / adhesive layer / resin layer / base film / adhesive layer / ABS resin layer is preferred.

[0111] <<Explanation of terms>> In the present invention, the term "film" includes the term "sheet", and the term "sheet" includes the term "film". In addition, in this specification, when it is written "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". In addition, when it is stated that the amount is "X or more" (X is any number), it also means that the amount is "preferably greater than X" unless otherwise specified, and when it is stated that the amount is "Y or less" (Y is any number), it also means that the amount is "preferably smaller than Y" unless otherwise specified. EXAMPLES

[0112] The present invention will be specifically described below with reference to examples, although the present invention is not limited to the following examples in any way. The measurement and evaluation methods used in the present invention are as follows.

[0113] (1) Resin layer thickness measurement method Each laminated film was attached to a glass slide using "Aron Alpha Series" manufactured by Toa Gosei Co., Ltd., to prepare a sample for SAICS. The obtained sample for SAICS was set in a SAICS (DN-01 type manufactured by Daipla Wintes Co., Ltd.), and a cut of 300 μm wide and 1 μm deep was made in advance with a diamond cutting edge. The cut was made using a single crystal diamond blade with a V-angle dimension of 80°, a rake angle of 5°, and a relief angle of 5°. The measurement was performed by setting a borazon cutting blade with a width of 300 μm on the sample with a 300 μm wide cut in advance, and measuring the film thickness of each cured resin layer at an arbitrary depth, horizontal speed of 1 μm / s, and vertical speed of 0.5 μm / s. A boron nitride blade with a blade width dimension of 0.3 mm, a rake angle of 20°, and a relief angle of 10° was used for the measurement. The compound strength was measured from the vertical displacement position and cutting force, and the thickness of each layer was confirmed.

[0114] (2) Pencil hardness The pencil hardness of the resin layer was measured in accordance with JIS K5600-5-4.

[0115] (3) Flexural durability Using a folding tester (Yuasa System Co., Ltd., DLDMLH-FS), the test was performed with a minimum radius R of 1.5 (3 mm) so that the resin layer of the laminated film was the inner surface (referred to as Out-fold in Table 2), and the presence or absence of cracks in the resin layer on the inner surface was visually confirmed. The number of repeated foldings was then measured, and the results were used to make a judgment according to the following judgment criteria. The same test was also performed with a minimum radius R of 2.0 (4 mm) so that the resin layer of the laminated film was the outer surface (referred to as In-fold in Table 2). (Judgment criteria) ◎: Can be repeatedly folded 200,000 times ○: Repeated bending times: over 100,000 to less than 200,000 △: Repeated folding times: over 1,000 to 100,000 ×: Repeated folding times less than 1000

[0116] (4) Light transmittance (before and after discoloration) Using a spectrophotometer (U-3900H, manufactured by Hitachi High-Technologies Corporation), the light transmittance in the wavelength range of 380 nm to 780 nm was measured at room temperature and when the temperature was raised to 35° C., and the amount of change in the light transmittance at the maximum absorption wavelength was determined.

[0117] The various compounds used in the examples and comparative examples were prepared as follows.

[0118] <Polyester raw materials> <Polyester (I)> 100 mol% dimethyl terephthalate, 100 mol% ethylene glycol, and 0.07 parts by mass of calcium acetate monohydrate were placed in a reactor, and the mixture was heated to a higher temperature while distilling off methanol to carry out an ester exchange reaction. After the reaction started, the temperature was raised to 230°C in about 4.5 hours, and the ester exchange reaction was essentially completed. Next, 0.04 parts by mass of phosphoric acid and 0.035 parts by mass of antimony trioxide were added, and polymerization was carried out according to a conventional method. That is, the reaction temperature was gradually increased to a final temperature of 280°C, while the pressure was gradually reduced to a final temperature of 0.05 mmHg. After 4 hours, the reaction was terminated, and the mixture was chipped according to a conventional method to obtain polyester (I). The resulting intrinsic viscosity was 0.63. <Polyester (B)> Silica particles having an average particle size of 2 μm were added to the polyester (I) to obtain polyester (II) containing 0.2% by mass of silica particles, and the intrinsic viscosity was 0.65.

[0119] <Base film> <Base film PET> The mixed raw material obtained by mixing polyesters (I) and (II) at a ratio of 90% by mass and 10% by mass, respectively, was used as the raw material for the outermost layer (surface layer), and only polyester (I) was used as the raw material for the intermediate layer. Each was fed to two extruders, melted at 285°C, and then co-extruded on a cooling roll set at 40°C in a layer configuration of two types and three layers (surface layer / intermediate layer / surface layer = 1 / 8 / 1 discharge amount (mass ratio)), cooled and solidified to obtain an unstretched sheet. Next, the film was stretched 3.4 times in the longitudinal direction at a film temperature of 85°C using the roll peripheral speed difference, then introduced into a tenter, stretched 4.3 times in the transverse direction at 110°C, heat-treated at 235°C, and then relaxed 2% in the transverse direction to obtain a polyester film (base film) with a thickness of 50 μm.

[0120] <Resin composition> <Production Example 1: Urethane (meth)acrylate Compound (A-1)> Into a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a nitrogen gas inlet, 29.3 parts by mass of an isocyanurate compound whose main component is a hexamethylene diisocyanate trimer (product name: Coronate HX, manufactured by Tosoh Corporation, isocyanate group content: 21.0%, (a1-1)) and 70.7 parts by mass of a mixture of pentaerythritol triacrylate and pentaerythritol tetraacrylate (hydroxyl value 120 mgKOH / g, (a1-2)) (a1-1 / a1-2=0. 25 / 0.75 (mol / mol)), 0.06 parts by mass of 2,6-di-tert-butylcresol as a polymerization inhibitor, and 0.02 parts by mass of dibutyltin dilaurate as a reaction catalyst were charged and reacted at 60°C. The reaction was terminated when the residual isocyanate groups reached 0.3% or less, yielding a mixture (A-1) of 70 parts by mass of a urethane (meth)acrylate compound and 30 parts by mass of pentaerythritol tetraacrylate (acryloyl group equivalent 134 g / eq, weight average molecular weight 10,000).

[0121] <Production Example 2: Urethane (meth)acrylate Compound (A-2)> A four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a nitrogen gas inlet was charged with 37.7 parts by mass of isophorone diisocyanate, 24.5 parts by mass of polytetramethylene glycol diol (hydroxyl value 175 mg KOH / g; molecular weight calculated from the hydroxyl value 641), 14.1 parts by mass of polyester triol (hydroxyl value 250 mg KOH / g; molecular weight calculated from the hydroxyl value 673), and 0.02 parts by mass of dibutyltin dilaurate as a reaction catalyst, and the mixture was reacted at 80°C. When the residual isocyanate groups reached 11% or less, 23.7 parts by mass of 2-hydroxyethyl acrylate and 0.04 parts by mass of methoxyphenol as a polymerization inhibitor were further charged and reacted at 60°C. When the residual isocyanate groups reached 0.3% or less, the reaction was terminated to obtain a urethane (meth)acrylate compound (A-2) (acryloyl group equivalent: 493 g / eq, weight average molecular weight: 3,400).

[0122] <Acrylate (a)> Into a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a nitrogen gas inlet, 90 parts by mass of the urethane (meth)acrylate compound (A-1) and 10 parts by mass of the urethane (meth)acrylate compound (A-2) were charged and stirred at 60°C until the mixture became uniform.

[0123] <Acrylate (b)> Into a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a nitrogen gas inlet, 6.6 parts by mass of isophorone diisocyanate (b1-1), 94 parts by mass of a mixture of dipentaerythritol pentaerythritol and dipentaerythritol hexaacrylate (b1-2) having a hydroxyl value of 50 mgKOH / g (b1-1 / b1-2=0.28 / 0.72 (mol / mol)), 0.6 parts by mass of 2,6-di-tert-butylcresol as a polymerization inhibitor, and 0.05 parts by mass of dibutyltin dilaurate as a reaction catalyst were charged and reacted at 60°C. The reaction was terminated when the remaining isocyanate group reached 0.3%, and a urethane acrylate composition (b) (acryloyl group equivalent 107 g / eq; weight average molecular weight was 1,500) was obtained.

[0124] A resin composition was prepared by adding 10 parts by mass of thermochromic (thermal color 35° C., blue), 5 parts by mass of a photopolymerization initiator (Omnirad127 manufactured by IGM Resins BV), and 233 parts by mass of methyl ethyl ketone to 90 parts by mass of the acrylate (a).

[0125] [Example 1] The resin composition was applied to the PET substrate film using a bar coater (#20) so that the coating thickness (after drying) was 12 μm. The resin layer was dried by heating at 90° C. for 1 minute to obtain a resin layer (before curing). The integrated light amount was 400 mJ / cm 2 The resin layer was cured by irradiation with ultraviolet light in a nitrogen atmosphere to obtain a laminated film having a laminated structure of a substrate film PET / resin layer. The results of evaluation by the above-mentioned methods are shown in Table 1.

[0126] [Example 2] A laminated film was obtained by producing in the same manner as in Example 1, except that the resin composition in Example 1 was changed to Shikoh "UV1700B" manufactured by Mitsubishi Chemical Corporation. The results of evaluation in the same manner as in Example 1 are shown in Table 1.

[0127] [Comparative Example 1] A laminated film was obtained by producing in the same manner as in Example 1, except that no thermochromic was added. The results of evaluation in the same manner as in Example 1 are shown in Table 1.

[0128] <Evaluation Results> The properties of each of the laminated films obtained in the above Examples and Comparative Examples are shown in Table 1 below.

[0129] [Table 2]

[0130] <Consideration> From the results of the above examples and comparative examples, it was found that a resin layer is laminated on the surface of a base film, and the resin layer contains a binder resin (A) and a chromic compound (B), so that while having flexibility, it is possible to achieve a high level of surface hardness (H or more) and repeated bending resistance (the ability to bend 200,000 times under the condition of outward bending, R = 1.5). In contrast, it was found that it is difficult to achieve the desired hard coat properties, repeated bending properties, and chromic properties (discoloration properties) simultaneously by simply providing a resin layer as shown in Comparative Example 1. In addition, as an additional effect, it was found that the surface hardness is higher and yet bending is possible under harsher conditions compared to the case where the chromic compound is not contained, probably because the chromic compound used is in a microencapsulated form.

[0131] It was also found that by setting the constituent compounds and thickness ratio of the resin layer within a specific range, it is not necessary to extremely increase the tensile modulus of the base film used, and it is not necessary to use a customized base film. Conventionally, when designing a laminate film having a surface layer with high surface hardness, it has been necessary to review the structural design of the raw materials that make up the base film used and further increase the tensile modulus, if necessary. In contrast, if the cured resin layer has a specific structure, it is possible to appropriately select a general-purpose base film available on the market, which provides the advantage of increased freedom in the selection of the base film. [Industrial Applicability]

[0132] The laminated film of the present invention has a high level of excellent surface hardness (H or more) and repeated bending resistance (can be bent 200,000 times under the condition of outward bending, R=1.5), and also has good chromic properties (discoloration), so it can be used for various substrate films. It can be used for various purposes such as decorative purposes, optical purposes, and packaging purposes. It is particularly suitable for use in decorating automobile parts.

Claims

1. A laminate film having a resin layer on at least one surface of a base film, the resin layer containing a binder resin (A) and a chromic compound (B), and a change in light transmittance at a wavelength at a minimum value of the light transmittance of the surface of the resin layer of 5% or more.

2. The laminated film according to claim 1 , wherein the binder resin (A) is an acrylic resin.

3. The laminate film according to claim 1 , wherein the chromic compound (B) is a photochromic compound or a thermochromic compound.

4. The laminate film according to claim 1, wherein the content of the chromic compound (B) in the resin layer is 0.1% by mass to 5.0% by mass.

5. The laminate film according to claim 1 , wherein the resin layer is formed by curing a resin composition containing a chromic compound (B) in microcapsules.

6. The laminated film according to claim 2 , wherein the acrylic resin is an active energy ray curable type.

7. The laminate film according to claim 1 , wherein the base film is a polyester film.

8. The laminate film according to claim 1 , wherein the base film is a polyethylene terephthalate (PET) film.

9. The laminate film according to claim 1 , wherein the base film is a copolymer polyester film.

10. The laminated film according to claim 1, which can be folded 200,000 times or more in a repeated folding property evaluation (outward bending, R=1.5).

11. The laminate film according to claim 1 , further comprising a printed layer between the base film and the resin layer.

12. The laminated film according to claim 1 , wherein the resin layer has a thickness of 20 μm or less.

13. A laminate having a resin layer on at least one side of a base film, the resin layer containing a binder resin (A) and a chromic compound (B), and other resin films bonded to both sides of the base film via adhesive layers.

14. The laminate according to claim 13, wherein the other resin layer laminated to the resin layer side is made of a PMMA resin.

15. The laminate according to claim 13, wherein the other resin layer attached to the surface of the base film via the adhesive layer is an ABS resin.

16. The laminate film according to any one of claims 1 to 12, which is for molding or decoration.

17. The laminate according to any one of claims 13 to 15, which is for molding or decoration.

18. The laminate film according to claim 16, which is used for decorating automobile parts.

19. The laminate according to claim 17, which is used for decorating automobile parts.

Citation Information

Patent Citations

  • Metallic like thermally color-changeable laminate

    JP1993111975A

  • Method for producing decorative sheet

    JP2017052264A

  • Decorative sheet and method for producing the same

    JP2018024188A

  • Forgery preventive printed matter and forgery preventive information detecting method

    JP1991231394A

  • Method for manufacturing thermochromic dimming element