Method for producing anionically modified fine cellulose fiber dried solid

By pulverizing anion-modified fine cellulose fibers below 60°C and collecting them effectively, the method maintains the redispersion properties and viscosity of the fibers, addressing the loss of functionality in dried cellulose fibers.

JP2024141072APending Publication Date: 2024-10-10NIPPON PAPER IND CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023052522
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing methods for producing dried fine cellulose fibers fail to maintain the redispersibility and viscosity characteristics of anion-modified fine cellulose fibers after drying, leading to a loss of their functional properties.

Method used

A method involving pulverization of dry anion-modified fine cellulose fibers at temperatures below 60°C, followed by collection and optional classification, to preserve the redispersion properties of the fibers.

Benefits of technology

The method ensures that the redispersion liquid of anion-modified fine cellulose fibers retains viscosity characteristics and redispersibility comparable to the original state, enhancing the usability of the dried product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141072000001
    Figure 2024141072000001
Patent Text Reader

Abstract

To provide a method for producing an anionically modified fine cellulose fiber dried solid that yields a redispersed liquid with viscosity characteristics and redispersibility comparable or close to those of a redispersed liquid of the pre-ground anionically modified fine cellulose fiber dried body.SOLUTION: This method includes the steps for (A) grinding dry raw materials containing anionically modified fine cellulose fibers with a grinder and (B) recovering the ground materials, where the temperature of step (A) is set to be lower than 60°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a dry solid product of anionically modified fine cellulose fibers. [Background technology]

[0002] Cellulose nanofibers and microfibrillated cellulose (hereinafter collectively referred to as "fine cellulose fibers") obtained by micronizing cellulose are fine fibers with diameters on the nano to micro order. As new materials with properties not found in ordinary pulp, such as high strength, high elasticity, and thixotropy, they are expected to be used in a variety of fields.

[0003] Generally, cellulose nanofibers are produced in a state where they are stably dispersed in water, and are usually used in the form of a cellulose nanofiber dispersion of a specified concentration for various purposes as an industrial material or an additive material for foods and cosmetics. In order to keep the state of cellulose nanofibers stable, water is required that is several tens of times that of the cellulose nanofiber, and since this high water content leads to increased costs for packaging, storage, transportation, etc. of the cellulose nanofibers, they are dried to produce a dried body, and when used, water is added to redisperse them, and they are used as a redispersion.

[0004] Dried fine cellulose fibers are manufactured by subjecting fine cellulose fibers in a water-dispersed (wet) state to processes such as drying, grinding, classification, and recovery. However, due to the formation of hydrogen bonds between the fine cellulose fibers during these processes, even if water is added to the dried and ground product to redisperse it, the viscosity characteristics, etc. cannot be restored to the same level as before drying, and the excellent properties of the fine cellulose fibers cannot be exhibited.

[0005] As a technique for obtaining a dried product of fine cellulose fibers that is easily redispersible, a method of drying a mixture of fine cellulose fibers and a solvent using a vacuum drum dryer (Patent Document 1) has been proposed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2019 / 189318 Summary of the Invention [Problem to be solved by the invention]

[0007] In Patent Document 1, a drying method is investigated in order to obtain a dried product of fine cellulose fibers having excellent redispersibility, but no consideration has been given at all to steps subsequent to the drying step.

[0008] Therefore, the present invention aims to provide a method for producing a dry solid of anion-modified fine cellulose fibers, which can provide a dispersion having viscosity characteristics and redispersibility equivalent to or close to those obtained when a dry raw material containing anion-modified fine cellulose fibers is ground, and the resulting ground material is dispersed in a solvent such as water to obtain a redispersion having properties similar to those obtained when the dry raw material before grinding is directly used as a dispersion. [Means for solving the problem]

[0009] As a result of extensive research to achieve this object, the inventors have discovered that it is extremely effective to carry out the step of pulverizing the dried raw material under specific conditions, and have completed the present invention.

[0010] The present invention provides the following: (1) A method for producing a dry solid of anion-modified fine cellulose fibers, comprising: (A) a step of grinding a dry raw material containing anion-modified fine cellulose fibers in a grinder; and (B) a step of recovering the ground product, wherein the temperature in step (A) is less than 60°C. (2) The method for producing a dry solid product of anion-modified fine cellulose fibers according to (1), wherein the temperature in the step (B) is less than 60°C. (3) The method for producing a dry solid material according to (1), wherein the anion-modified fine cellulose fibers are oxidized fine cellulose fibers. (4) The method for producing a dry solid material according to (1), wherein the anion-modified fine cellulose fiber is a carboxymethylated fine cellulose fiber. (5) The method for producing a dry solid material according to any one of (1) to (3), further comprising the step (C) of classifying the pulverized material. Effect of the Invention

[0011] According to the present invention, a method for producing a dry solid of anion-modified fine cellulose fibers can be provided, which can obtain a redispersion liquid having the same or similar viscosity characteristics and redispersibility as the redispersion liquid of the dried anion-modified fine cellulose fibers before grinding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below. In the present invention, "to" includes the end values. In other words, "X to Y" includes the values ​​X and Y at both ends.

[0013] (Method for producing dry solid material of anion-modified fine cellulose fibers) The present invention relates to a method for producing a dry solid material of anion-modified fine cellulose fibers, which comprises the steps of (A) pulverizing a dry raw material containing anion-modified fine cellulose fibers with a pulverizer and (B) recovering the pulverized product, and further, the temperature in the step (A) is set to less than 60°C.

[0014] (Process (A)) The step (A) included in the production method of the present invention is a step of pulverizing a dry raw material containing anionically modified fine cellulose fibers with a pulverizer.

[0015] (Anion-modified fine cellulose fiber) The anionically modified fine cellulose fibers used in the present invention can be obtained by defibrating anionically modified cellulose.

[0016] (Microfine cellulose fiber) The fine cellulose fibers used in the present invention are fine fibers made from cellulose, and are a general term for cellulose nanofibers (hereinafter sometimes referred to as "CNF") having an average fiber diameter of less than 500 nm and microfibrillated cellulose (hereinafter sometimes referred to as "MFC") having an average fiber diameter of 500 nm or more. The average fiber diameter is a length-weighted average fiber diameter, and can be measured by observing the fine cellulose fibers using, for example, a fractionator manufactured by Valmet Co., Ltd. or an atomic force microscope (AFM). The average fiber diameter of the fine cellulose fibers is not particularly limited, but is about 1 nm to 60 μm. The fine cellulose fibers can be produced by defibrating cellulose (pulp).

[0017] (Cellulose nanofiber (CNF)) The average fiber diameter of the CNF that can be used in the present invention is preferably 100 nm or less, more preferably 50 nm or less. The average fiber length is preferably 5 μm or less, more preferably 3 μm or less. The lower limit of the average fiber length is about 0.1 μm or more. The average fiber length can be measured by analyzing 200 randomly selected fibers using an atomic force microscope (AFM) when the diameter is less than 20 nm, or a field emission scanning electron microscope (FE-SEM) when the diameter is 20 nm or more, and calculating the average. The average aspect ratio of the CNF that can be used in the present invention is preferably 50 or more. The upper limit is not particularly limited, but is usually 1000 or less. The average aspect ratio can be calculated by the following formula: Aspect ratio = average fiber length / average fiber diameter

[0018] (Microfibrillated Cellulose (MFC)) The average fiber length of the MFC that can be used in the present invention is preferably 5 μm or more, more preferably 200 μm or more. The upper limit of the average fiber length is preferably 2.0 mm or less, more preferably about 1.5 mm or less. The average fiber length (length-weighted average fiber length) can be determined by measurement using a fractionator manufactured by Valmet Co., Ltd.

[0019] The cellulose raw material is not particularly limited as long as it contains cellulose, and examples thereof include plants (e.g., wood, bamboo, hemp, jute, kenaf, agricultural waste, cloth, pulp (softwood unbleached kraft pulp (NUKP), softwood bleached kraft pulp (NBKP), hardwood unbleached kraft pulp (LUKP), hardwood bleached kraft pulp (LBKP), bleached kraft pulp (BKP), softwood unbleached sulfite pulp (NUSP), softwood bleached sulfite pulp (NBSP), thermomechanical pulp (TMP), recycled pulp, waste paper, etc.), animals (e.g., ascidians), algae, microorganisms (e.g., acetic acid bacteria (Acetobacter)), microbial products, and the like. The cellulose raw material may be any one of these or a combination of two or more types, but is preferably a cellulose raw material derived from a plant or a microorganism (e.g., cellulose fiber), and more preferably a cellulose raw material derived from a plant (e.g., cellulose fiber).

[0020] The number average fiber diameter of the cellulose raw material is not particularly limited, but in the case of softwood kraft pulp, which is a common pulp, it is about 30 to 60 μm, and in the case of hardwood kraft pulp, it is about 10 to 30 μm. In the case of other pulps, those that have undergone general refining have a diameter of about 50 μm. For example, in the case of refining chips or the like that are several centimeters in size, it is preferable to adjust the diameter to about 50 μm by mechanical processing using a disintegrator such as a refiner or beater.

[0021] Cellulose has three hydroxyl groups per glucose unit and can be chemically modified in various ways. In the present invention, from the viewpoint of promoting the progress of defibration, it is preferable to use anionically modified fine cellulose fibers produced by defibrating a cellulose raw material (anionically modified cellulose) obtained by anionically modifying it among chemical modifications.

[0022] (anion modified) In the present invention, anionic modification refers to the introduction of anionic groups into cellulose, specifically, the introduction of anionic groups into the pyranose ring of cellulose by oxidation or substitution reaction. In the present invention, the oxidation reaction refers to a reaction in which the hydroxyl group of the pyranose ring is directly oxidized to a carboxyl group. In addition, in the present invention, the substitution reaction refers to a reaction in which anionic groups are introduced into the pyranose ring by a substitution reaction other than the oxidation.

[0023] Examples of the anion modification include oxidation (carboxylation), carboxymethylation, esterification, etc. Among them, oxidation (carboxylation) and carboxymethylation are more preferable, and oxidation (carboxylation) is particularly preferable.

[0024] (Oxidation) In the present invention, when using oxidized fine cellulose fibers obtained by defibrating oxidized (carboxylated) cellulose, the oxidized cellulose (also called carboxylated cellulose) can be obtained by oxidizing (carboxylating) the above-mentioned cellulose raw material by a known method. Although not particularly limited, during oxidation, it is preferable to adjust the amount of carboxyl groups to 0.6 to 2.0 mmol / g, and more preferably to adjust to 1.0 mmol / g to 2.0 mmol / g, based on the bone dry mass of the anion-modified fine cellulose fiber.

[0025] One example of the oxidation (carboxylation) method is a method in which a cellulose raw material is oxidized in water using an oxidizing agent in the presence of an N-oxyl compound and a compound selected from the group consisting of bromides, iodides, or a mixture thereof. This oxidation reaction selectively oxidizes the primary hydroxyl group at the C6 position of the glucopyranose ring on the cellulose surface, resulting in the formation of aldehyde groups and carboxyl groups (-COOH) or carboxylate groups (-COO - The concentration of cellulose during the reaction is not particularly limited, but is preferably 5% by mass or less.

[0026] The term "N-oxyl compound" refers to a compound capable of generating a nitroxy radical. Any compound that can promote the desired oxidation reaction can be used as the N-oxyl compound. For example, 2,2,6,6-tetramethylpiperidine-1-oxy radical (TEMPO) and its derivatives (e.g., 4-hydroxyTEMPO) can be mentioned.

[0027] The amount of the N-oxyl compound used is not particularly limited as long as it is a catalytic amount capable of oxidizing the raw material cellulose. For example, the amount is preferably 0.01 to 5 mmol, more preferably 0.01 to 1 mmol, and even more preferably 0.01 to 0.5 mmol, per 1 g of bone dry cellulose. Also, the amount is preferably about 0.02 to 0.5 mmol / L relative to the reaction system.

[0028] Bromides are compounds containing bromine, examples of which include alkali metal bromides that can dissociate and ionize in water. Also, iodides are compounds containing iodine, examples of which include alkali metal iodides. The amount of bromide or iodide used can be selected within a range that can promote the oxidation reaction. The total amount of bromide and iodide is, for example, preferably 0.1 to 100 mmol, more preferably 0.1 to 10 mmol, and even more preferably 0.5 to 5 mmol, per 1 g of bone-dry cellulose.

[0029] The oxidizing agent may be a known one, such as halogen, hypohalous acid, halous acid, perhalogen acid or their salts, halogen oxide, peroxide, etc. Among them, sodium hypochlorite is preferable because it is inexpensive and has a low environmental impact. The amount of the oxidizing agent used is preferably 0.5 to 500 mmol, more preferably 0.5 to 50 mmol, even more preferably 1 to 25 mmol, and most preferably 3 to 10 mmol, per 1 g of bone-dry cellulose. Also, for example, 2 to 500 mol is preferable per 1 mol of the N-oxyl compound.

[0030] The oxidation of cellulose can proceed efficiently even under relatively mild conditions. Therefore, the reaction temperature is preferably 4 to 40°C, or may be room temperature of about 15 to 30°C. As the reaction proceeds, carboxyl groups are generated in the cellulose, and the pH of the reaction solution decreases. In order to efficiently proceed with the oxidation reaction, it is preferable to add an alkaline solution such as an aqueous sodium hydroxide solution to maintain the pH of the reaction solution at about 8 to 12, preferably 10 to 11. The reaction medium is preferably water, because it is easy to handle and does not easily cause side reactions.

[0031] The reaction time in the oxidation reaction can be appropriately set according to the degree of progress of the oxidation, and is usually from 0.5 to 6 hours, for example, about 0.5 to 4 hours.

[0032] The oxidation reaction may also be carried out in two stages. For example, the oxidized cellulose obtained by filtration after completion of the first-stage reaction can be oxidized again under the same or different reaction conditions, allowing efficient oxidation without reaction inhibition by table salt produced as a by-product in the first-stage reaction.

[0033] Another example of the oxidation (carboxylation) method is a method in which the cellulose raw material is oxidized by contacting an ozone-containing gas with the raw material. This oxidation reaction oxidizes at least the hydroxyl groups at positions 2 and 6 of the glucopyranose ring, and decomposes the cellulose chain. The ozone concentration in the ozone-containing gas is 50 to 250 g / m 3 It is preferable that the thickness is 50 to 220 g / m 3It is more preferable that the ozone is added to the cellulose raw material in an amount of 0.1 to 30 parts by mass, and more preferably 5 to 30 parts by mass, based on 100 parts by mass of the solid content of the cellulose raw material. The ozone treatment temperature is preferably 0 to 50°C, and more preferably 20 to 50°C. The ozone treatment time is not particularly limited, but is about 1 to 360 minutes, and is preferably about 30 to 360 minutes. When the ozone treatment conditions are within these ranges, it is possible to prevent cellulose from being excessively oxidized and decomposed, and the yield of oxidized cellulose is good. After the ozone treatment, an oxidizing agent may be used to perform a post-oxidation treatment. The oxidizing agent used in the post-oxidation treatment is not particularly limited, but examples thereof include chlorine-based compounds such as chlorine dioxide and sodium chlorite, oxygen, hydrogen peroxide, persulfuric acid, and peracetic acid. For example, these oxidizing agents are dissolved in a polar organic solvent such as water or alcohol to prepare an oxidizing agent solution, and the cellulose raw material is immersed in the solution to perform the post-oxidation treatment.

[0034] The amount of carboxyl groups in oxidized cellulose can be adjusted by controlling reaction conditions such as the amount of oxidizing agent added, reaction time, etc. The amount of carboxyl groups in oxidized cellulose and the amount of carboxyl groups when the oxidized cellulose is micronized are usually the same.

[0035] (Carboxymethylation) In the present invention, when using carboxymethylated fine cellulose fibers obtained by fibrillating carboxymethylated cellulose, the carboxymethylated cellulose may be obtained by carboxymethylating the above-mentioned cellulose raw material by a known method, or a commercially available product may be used. In either case, it is preferable that the degree of carboxymethyl substitution per anhydrous glucose unit of cellulose is 0.01 to 0.50. An example of a method for producing such carboxymethylated cellulose can be mentioned as follows. Cellulose is used as a starting material, and 3 to 20 times by mass of water and / or lower alcohol, specifically water, methanol, ethanol, N-propyl alcohol, isopropyl alcohol, N-butanol, isobutanol, tertiary butanol, etc., are used as a solvent, or a mixture of two or more of them is used. In addition, when a lower alcohol is mixed, the mixing ratio of the lower alcohol is 60 to 95% by mass. As a mercerizing agent, 0.5 to 20 times mol of an alkali metal hydroxide, specifically sodium hydroxide or potassium hydroxide, is used per anhydrous glucose residue of the starting material. The starting material, solvent, and mercerizing agent are mixed, and a mercerization treatment is carried out at a reaction temperature of 0 to 70° C., preferably 10 to 60° C., for a reaction time of 15 minutes to 8 hours, preferably 30 minutes to 7 hours. Then, 0.05 to 10.0 times the moles of a carboxymethylating agent per glucose residue is added, and an etherification reaction is carried out at a reaction temperature of 30 to 90° C., preferably 40 to 80° C., for a reaction time of 30 minutes to 10 hours, preferably 1 hour to 4 hours.

[0036] The degree of carboxymethyl substitution in carboxymethylated cellulose is usually the same as the degree of carboxymethyl substitution when the carboxymethylated cellulose is finely divided.

[0037] In this specification, "carboxymethylated cellulose", which is a type of chemically modified cellulose used in the preparation of fine cellulose fibers, refers to cellulose that maintains at least a part of its fibrous shape even when dispersed in water. Therefore, it is distinguished from carboxymethyl cellulose, which is a type of water-soluble polymer. When an aqueous dispersion of "carboxymethylated cellulose" is observed with an electron microscope, a fibrous substance can be observed. On the other hand, even when an aqueous dispersion of carboxymethyl cellulose, which is a type of water-soluble polymer, is observed, no fibrous substance is observed because it is dissolved in water and in a molecular state, and fine cellulose fibers cannot be obtained even if a strong shear force is applied to the aqueous dispersion. Furthermore, when "carboxymethylated cellulose" is measured by X-ray diffraction, a peak of cellulose type I crystals can be observed, but a peak of cellulose type I crystals is not observed in the case of carboxymethyl cellulose, a water-soluble polymer.

[0038] (Esterification) In the present invention, esterified fine cellulose fibers obtained by defibrating esterified cellulose can be used. The esterified cellulose can be obtained by mixing a powder or an aqueous solution of phosphoric acid compound A with the above-mentioned cellulose raw material, or by adding an aqueous solution of phosphoric acid compound A to a slurry of the cellulose raw material.

[0039] Examples of the phosphoric acid compound A include phosphoric acid, polyphosphoric acid, phosphorous acid, hypophosphorous acid, phosphonic acid, polyphosphonic acid, and esters thereof. These may be in the form of a salt. Among these, compounds having a phosphoric acid group are preferred because they are low cost, easy to handle, and can be introduced into the cellulose of the pulp fiber to improve the defibration efficiency. Examples of compounds having a phosphoric acid group include phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, sodium phosphite, potassium phosphite, sodium hypophosphite, potassium hypophosphite, sodium pyrophosphate, sodium metaphosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, tripotassium phosphate, potassium pyrophosphate, potassium metaphosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, ammonium pyrophosphate, and ammonium metaphosphate. These can be used alone or in combination of two or more. Among these, phosphoric acid, sodium salts of phosphoric acid, potassium salts of phosphoric acid, and ammonium salts of phosphoric acid are more preferred from the viewpoints of high efficiency of phosphoric acid group introduction, ease of defibration in the defibration step described below, and ease of industrial application. Sodium dihydrogen phosphate and disodium hydrogen phosphate are particularly preferred. In addition, it is preferable to use the phosphoric acid compound A as an aqueous solution, since this increases the uniformity of the reaction and the efficiency of introducing the phosphoric acid group. The pH of the aqueous solution of the phosphoric acid compound A is preferably 7 or less, since this increases the efficiency of introducing the phosphoric acid group, but from the viewpoint of suppressing hydrolysis of the pulp fiber, a pH of 3 to 7 is preferable.

[0040] The following method can be given as an example of a method for producing cellulose phosphate. A phosphoric acid compound A is added to a dispersion of a cellulose raw material having a solid content concentration of 0.1 to 10% by mass while stirring to introduce a phosphoric acid group into the cellulose. When the cellulose raw material is taken as 100 parts by mass, the amount of phosphoric acid compound A added is preferably 0.2 to 500 parts by mass, more preferably 1 to 400 parts by mass, in terms of the amount of phosphorus element. If the proportion of phosphoric acid compound A is equal to or greater than the lower limit, the yield of fine cellulose fibers can be further improved. However, if the upper limit is exceeded, the effect of improving the yield reaches a plateau, which is not preferable from the viewpoint of cost.

[0041] In this case, in addition to the cellulose raw material and the phosphoric acid compound A, a powder or an aqueous solution of the other compound B may be mixed. The compound B is not particularly limited, but is preferably a nitrogen-containing compound exhibiting basicity. Here, "basicity" is defined as an aqueous solution exhibiting pink to red color in the presence of a phenolphthalein indicator, or an aqueous solution having a pH of more than 7. The nitrogen-containing compound exhibiting basicity used in the present invention is not particularly limited as long as it exhibits the effects of the present invention, but is preferably a compound having an amino group. Examples include, but are not limited to, urea, methylamine, ethylamine, trimethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, pyridine, ethylenediamine, and hexamethylenediamine. Among these, urea, which is low-cost and easy to handle, is preferred. The amount of compound B added is preferably 2 to 1000 parts by mass, more preferably 100 to 700 parts by mass, relative to 100 parts by mass of the solid content of the cellulose raw material. The reaction temperature is preferably 0 to 95°C, more preferably 30 to 90°C. The reaction time is not particularly limited, but is about 1 to 600 minutes, and more preferably 30 to 480 minutes. When the esterification reaction conditions are within these ranges, it is possible to prevent cellulose from being excessively esterified and becoming easily soluble, and the yield of phosphated cellulose is good. After the obtained phosphated cellulose suspension is dehydrated, it is preferable to heat treat it at 100 to 170°C from the viewpoint of suppressing hydrolysis of cellulose. Furthermore, it is preferable to heat it at 130°C or less, preferably 110°C or less while water is contained during the heat treatment, and after removing the water, heat treat it at 100 to 170°C.

[0042] The degree of substitution of phosphoric acid group per glucose unit of the phosphoric acid esterified cellulose is preferably 0.001 to 0.40. By introducing a phosphoric acid group substituent into cellulose, the cellulose particles are electrically repelled from each other. Therefore, the cellulose into which the phosphoric acid group has been introduced can be easily defibrated. If the degree of substitution of phosphoric acid group per glucose unit is less than 0.001, it cannot be defibrated sufficiently. On the other hand, if the degree of substitution of phosphoric acid group per glucose unit is more than 0.40, it may swell or dissolve, and may not be obtained as fine cellulose fibers. In order to perform defibration efficiently, it is preferable that the phosphoric acid esterified cellulose raw material obtained above is washed by boiling and then washing with cold water. The modification by these esterifications is a modification by substitution reaction. The degree of substitution in the esterified cellulose and the degree of substitution when the esterified cellulose is finely pulverized are usually the same.

[0043] (Defibrilization) In the present invention, the device for defibrating anion-modified cellulose is not particularly limited, but it is preferable to apply a strong shear force to the aqueous dispersion of anion-modified cellulose using a device such as a high-speed rotation type, a colloid mill type, a high-pressure type, a roll mill type, or an ultrasonic type. In particular, in order to defibrate efficiently, it is preferable to use a wet-type high-pressure or ultra-high-pressure homogenizer that can apply a pressure of 50 MPa or more to the aqueous dispersion and a strong shear force. The pressure is more preferably 100 MPa or more, and further preferably 140 MPa or more. In addition, prior to the defibration and dispersion treatment with the high-pressure homogenizer, it is also possible to subject the above-mentioned fine cellulose fibers to a preliminary treatment using a known mixing, stirring, emulsifying, and dispersing device such as a high-speed shear mixer, if necessary. The number of treatments (passes) in the defibration device may be one or two or more, and two or more are preferable.

[0044] In the dispersion treatment, anionically modified cellulose is usually dispersed in a solvent. The solvent is not particularly limited as long as it can disperse anionically modified cellulose, and examples thereof include water, organic solvents (e.g., hydrophilic organic solvents such as methanol), and mixtures thereof. Since the cellulose raw material is hydrophilic, the solvent is preferably water.

[0045] The solid content concentration of the anion-modified cellulose in the dispersion is usually 0.1% by mass or more, preferably 0.2% by mass or more, and more preferably 0.3% by mass or more. This allows the amount of liquid to be appropriate relative to the amount of the cellulose fiber raw material, which is efficient. The upper limit is usually 10% by mass or less, and preferably 6% by mass or less. This allows the fluidity to be maintained.

[0046] Prior to the defibration or dispersion treatment, a pretreatment may be carried out as necessary. The pretreatment may be carried out using a mixing, stirring, emulsifying or dispersing device such as a high-speed shear mixer.

[0047] When the anion-modified fine cellulose fibers obtained through the defibration step are in a salt form, they may be used as they are, or may be converted into an acid form by an acid treatment using a mineral acid, a method using a cation exchange resin, etc. Also, they may be used after being imparted with hydrophobicity by a method using a cationic additive.

[0048] (Dispersant) In the production method of the present invention, the dry raw material containing anion-modified fine cellulose fibers preferably contains a dispersant from the viewpoint of improving redispersibility. Examples of the dispersant include water-soluble polymers, surfactants, etc., and it is preferable to use a water-soluble polymer because the water-soluble polymer covers the low charge density part on the surface of the anion-modified fine cellulose fibers, suppresses the formation of hydrogen bonds, and prevents the fine cellulose fibers from coagulating during drying.

[0049] (Water-soluble polymer) Examples of water-soluble polymers that can be used in the production method of the present invention include cellulose derivatives (carboxymethylcellulose, methylcellulose, hydroxypropylcellulose, ethylcellulose), xanthan gum, xyloglucan, dextrin, dextran, carrageenan, locust bean gum, alginic acid, alginates, pullulan, starch, potato starch, kudzu starch, modified starch (cationized starch, phosphorylated starch, phosphate crosslinked starch, phosphate monoesterified phosphate crosslinked starch, hydroxypropyl starch, hydroxypropylated phosphate crosslinked starch, acetylated adipic acid crosslinked starch, acetylated phosphate crosslinked starch, acetylated oxidized starch, sodium octenylsuccinate starch, acetate starch, oxidized starch), corn starch, gum arabic, locust bean gum, alginic acid, alginates, pullulan, starch, potato starch, kudzu starch, modified starch (cationized starch, phosphorylated starch, phosphate crosslinked starch, phosphate monoesterified phosphate crosslinked starch, hydroxypropyl starch, hydroxypropylated phosphate crosslinked starch, acetylated adipic acid crosslinked starch, acetylated phosphate crosslinked starch, sodium octenylsuccinate starch, acetate starch, oxidized starch), corn starch, gum arabic, Examples of the suitable cellulose gum include tobean gum, gellan gum, polydextrose, pectin, chitin, water-soluble chitin, chitosan, casein, albumin, soy protein lysate, peptone, polyvinyl alcohol, polyacrylamide, sodium polyacrylate, polyvinylpyrrolidone, polyvinyl acetate, polyamino acid, polylactic acid, polymalic acid, polyglycerin, latex, rosin-based sizing agent, petroleum resin-based sizing agent, urea resin, melamine resin, epoxy resin, polyamide resin, polyamide-polyamine resin, polyethyleneimine, polyamine, vegetable gum, polyethylene oxide, hydrophilic crosslinked polymer, polyacrylate, starch polyacrylic acid copolymer, tamarind gum, guar gum, and colloidal silica, and mixtures of one or more thereof. Among these, cellulose derivatives are preferred in terms of their affinity with chemically modified fine cellulose fibers, and carboxymethylcellulose and its salts are particularly preferred. It is believed that water-soluble polymers such as carboxymethylcellulose and its salts penetrate between the fibers of fine cellulose fibers and increase the distance between the fibers, thereby improving redispersibility.

[0050] Examples of surfactants that can be used in the production method of the present invention include, but are not limited to, nonionic surfactants such as fatty acid salts, higher alkyl sulfates, alkylbenzene sulfonates, higher alcohols, alkylphenols, and alkylene oxide adducts of fatty acids, anionic surfactants, cationic surfactants, amphoteric surfactants, organic solvents, proteins, enzymes, natural polymers, synthetic polymers, etc. The surfactants may be composed of a single component of these or a mixture of two or more components.

[0051] When carboxymethylcellulose or a salt thereof is used as the water-soluble polymer, it is preferable to use carboxymethylcellulose with a degree of carboxymethyl substitution per anhydrous glucose unit of 0.55 to 1.6, more preferably 0.55 to 1.1, and even more preferably 0.65 to 1.1. In addition, carboxymethylcellulose with a longer molecule (higher viscosity) is preferable because it has a higher effect of widening the distance between nanofibers. In addition, the B-type viscosity of a 1% by mass aqueous solution of carboxymethylcellulose at 25°C and 60 rpm is preferably 3 mPa·s to 14000 mPa·s, more preferably 7 mPa·s to 14000 mPa·s, and even more preferably 1000 mPa·s to 8000 mPa·s. Note that the "carboxymethylcellulose or a salt thereof" as the water-soluble polymer referred to here is completely dissolved in water, and is therefore distinguished from the above-mentioned carboxymethylated cellulose whose fiber shape can be confirmed in water.

[0052] In the present invention, when the raw material contains a dispersant, the compounding ratio of the anion-modified fine cellulose fiber (bone dry solid content) to the dispersant is preferably 5:5 to 8:2, more preferably 6:4 to 7:3, from the viewpoint of obtaining an effect of improving redispersibility. If the compounding ratio of the dispersant is too high above the upper limit, problems such as viscosity characteristics such as thixotropy, which is a characteristic of the anion-modified fine cellulose fiber, and a decrease in dispersion stability may occur. If the compounding ratio of the dispersant is too low below the lower limit, sufficient redispersibility cannot be obtained.

[0053] The dry raw material containing anionically modified fine cellulose fibers used in the present invention can be obtained by dehydrating and drying an aqueous suspension containing anionically modified fine cellulose fibers and, if necessary, a dispersant such as a water-soluble polymer, etc. In addition, by adjusting the pH of the aqueous suspension to 9 to 11, a dry solid of anionically modified fine cellulose fibers with better redispersibility can be obtained.

[0054] In the present invention, the method of dehydration and drying may be any method known in the art, such as spray drying, freeze drying, squeezing, air drying, hot air drying, and vacuum drying. Specific examples of drying apparatuses to be used include the following. That is, continuous tunnel drying apparatuses, band drying apparatuses, vertical drying apparatuses, vertical turbo drying apparatuses, multi-stage disk drying apparatuses, ventilation drying apparatuses, rotary drying apparatuses, air flow drying apparatuses, spray dryer drying apparatuses, spray drying apparatuses, cylindrical drying apparatuses, drum drying apparatuses, reduced pressure belt drying apparatuses, screw conveyor drying apparatuses, rotary drying apparatuses with heating tubes, vibration transport drying apparatuses, fluidized bed drying apparatuses, etc., batch type box drying apparatuses, ventilation drying apparatuses, vacuum box drying apparatuses, stirring drying apparatuses, shelf drying apparatuses, freeze drying apparatuses, etc., may be used alone or in combination of two or more. Among these, drum drying apparatuses and belt drying apparatuses are preferably used, and from the viewpoint of energy efficiency, drum drying apparatuses that directly supply heat energy to the material to be dried uniformly are more preferably used.

[0055] In the present invention, the dried raw material is one that has been dried so that the moisture content is 15% by mass or less. The moisture content is preferably 0 to 15% by mass, and more preferably 0 to 10% by mass. It may also be one that has been dried to a moisture content of 0% (bone dry).

[0056] (Crusher) In the step (A) of the present invention, the type of pulverizer that can be used is not particularly limited, and may be any type that can set the temperature in the step (A) to less than 60° C. Examples of pulverizers that can be used in the present invention include cutting type mills: mesh mill (manufactured by HORAI Co., Ltd.), Atoms (manufactured by Yamamoto Hyakuma Seisakusho Co., Ltd.), knife mill (manufactured by Palman Co., Ltd.), cutter mill (manufactured by Tokyo Atomizer Manufacturing Co., Ltd.), CS cutter (manufactured by Mitsui Mining Co., Ltd.), rotary cutter mill (manufactured by Nara Machinery Works, Ltd.), turbo cutter (manufactured by Freund Corporation), pulp coarse crusher (manufactured by Zuikou Co., Ltd.), shredder (manufactured by Kobe Steel Pantech Co., Ltd.), hammer type mills: jaw crusher (manufactured by Kobe Steel Pantech Co., Ltd.), etc. Makino Co., Ltd.), Hammer Crusher (Makino Sangyo Co., Ltd.), Impact Mill: Pulverizer (Hosokawa Micron Co., Ltd.), Fine Impact Mill (Hosokawa Micron Co., Ltd.), Super Micron Mill (Hosokawa Micron Co., Ltd.), Innomizer (Hosokawa Micron Co., Ltd.), Fine Mill (Nippon Pneumatic Mfg. Co., Ltd.), CUM Type Centrifugal Mill (Mitsui Mining Co., Ltd.), Exceed Mill (Makino Sangyo Co., Ltd.), Ultraplex (Makino Sangyo Co., Ltd.), Contraplex (Makino Sangyo Co., Ltd.), Coroplex (Makino Sangyo Co., Ltd.), Sample Mill (Seishin Co., Ltd.), Bantam Mill (Seishin Co., Ltd.), Atomizer (Seishin Co., Ltd.), Tornado Mill (Nikkiso Co., Ltd.), Nea Mill (Dalton Co., Ltd.), HT Type Fine Grinding Mill (Horai Co., Ltd.), Free Grinding Mill (Nara Machinery Works, Ltd.), New Cosmomizer (Nara Machinery Works, Ltd.), Turbo Mill (Freund Corporation), Gather Mill (Nishimura Machinery Works, Ltd.), Spar Powder mill (manufactured by Nishimura Machinery Works, Ltd.), blade mill (manufactured by Nisshin Engineering Inc.), super rotor (manufactured by Nisshin Engineering Inc.), Npa crusher (manufactured by Sansho Industry Co., Ltd.), Wheeley crusher (manufactured by Sanki Manufacturing Co., Ltd.), pulp crusher (manufactured by Zuikou Co., Ltd.), Jacobson fine grinder (manufactured by Kobe Steel Pantech Co., Ltd.), universal mill (manufactured by Tokuju Co., Ltd.), atomizer (manufactured by Tokyo Atomizer Manufacturing Co., Ltd.), Mill Star Dam (manufactured by Tokyo Atomizer Manufacturing Co., Ltd.),Airflow type mills: Stream Mill (manufactured by Nippon Coke Engineering Co., Ltd.), CGS type jet mill (manufactured by Mitsui Mining Co., Ltd.), Micron Jet (manufactured by Hosokawa Micron Corporation), Counter Jet Mill (manufactured by Hosokawa Micron Corporation), Cross Jet Mill (manufactured by Kurimoto Iron Works, Ltd.), Supersonic Jet Mill (manufactured by Japan Pneumatic Mfg. Co., Ltd.), Current Jet (manufactured by Nisshin Engineering Inc.), Jet Mill (manufactured by Sansho Industry Co., Ltd.), Ebara Jet Micronizer (manufactured by Ebara Corporation), Ebara Triad Jet (manufactured by Ebara Corporation), Selenium Mirror (manufactured by Masuko Sangyo Co., Ltd.), New Micro Sect Examples of such mills include matte (manufactured by Masuno Seisakusho Co., Ltd.), Cryptron (manufactured by Kawasaki Heavy Industries, Ltd.), disc mills: vibrating disc mills (manufactured by Retsch), centri-cutter (manufactured by Nippon Coke & Engineering Co., Ltd.), turbo disc mills (manufactured by Freund-Turbo Corporation), mortar-type high-speed grinders (manufactured by Makino Sangyo Co., Ltd.), vertical roller mills: vertical roller mills (manufactured by Chinon Co., Ltd.), vertical roller mills (manufactured by Schaeffler Japan Co., Ltd.), roller mills (manufactured by Kotobuki Giken Kogyo Co., Ltd.), VX mills (manufactured by Kurimoto Iron Works Co., Ltd.), KVM-type vertical mills (manufactured by EarthTechnica Co., Ltd.), and IS mills (manufactured by IHI Plant Engineering Co., Ltd.). Among these, it is preferable to use an impact mill, an airflow mill, or a disk mill from the viewpoint of pulverizability.

[0057] The temperature in step (A) can be adjusted by cooling the machine body or the airflow that carries the raw material, and in the present invention, it is adjusted to less than 60° C., preferably 55° C. or less, more preferably 50° C. or less, and even more preferably 40° C. or less. There are no particular limitations on the lower limit of the temperature in step (A), but it is preferably 20° C. or more because of concerns about condensation. The temperature in step (A) can be measured using a thermometer attached to the device or a thermometer attached to the surface of the device.

[0058] The grinding conditions in step (A) can be appropriately adjusted by previously preparing a calibration curve based on the grinding conditions (eg, processing time, input amount, etc.) and the desired physical properties of the ground product, and referring to this calibration curve.

[0059] (Process (B)) Step (B) included in the production method of the present invention is a step of recovering the pulverized material. The type of device for recovering the pulverized material that can be used in the present invention is not particularly limited. It is preferable that the temperature in step (B) can be adjusted to less than 60°C. Examples of recovery devices that can be used in the present invention include cyclones and bag filters, and it is preferable to use a cyclone from the viewpoint of the risk of exposure to heat for a long time.

[0060] The temperature in step (B) can be adjusted by selecting an appropriate apparatus, adjusting the processing amount, etc., and in the present invention, it is adjusted to be preferably less than 60° C., more preferably 55° C. or less, further preferably 50° C. or less, particularly preferably 40° C. or less. There is no particular limitation on the lower limit of the temperature in step (B).

[0061] (Process (C)) The production method of the present invention may include a step of classifying the pulverized product as step (C). Step (C) may be performed between step (A) and step (B), after step (B), or multiple times between step (A) and step (B) and after step (B). Step (C) may be performed on the pulverized product obtained in step (A) using a classifier attached to or mounted on a pulverizer.

[0062] According to the method for producing a dry solid of anion-modified fine cellulose fibers of the present invention, the temperature in step (A) is set to less than 60° C., so that the effect of heat on the anion-modified fine cellulose fibers can be reduced. As a result, by using the dry solid obtained by the production method of the present invention, a redispersion liquid having the same or similar viscosity characteristics and redispersibility as the redispersion liquid of the dried anion-modified fine cellulose fibers before pulverization can be obtained. EXAMPLES

[0063] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these. In addition, unless the method of measurement / calculation of each value in each example is specifically stated, it is measured / calculated by the method described in the specification.

[0064] (Production Example 1) (Production of TEMPO oxidized (carboxylated) CNF) 5 g (bone dry) of bleached unbeaten kraft pulp (85% brightness) derived from coniferous trees was added to 500 mL of an aqueous solution containing 39 mg of TEMPO (Sigma Aldrich) and 514 mg of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system to a concentration of 5.5 mmol / g to initiate the oxidation reaction. The pH of the system decreased during the reaction, but 3 M aqueous sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. The mixture after the reaction was acidified using hydrochloric acid, filtered through a glass filter to separate the pulp, and the pulp was thoroughly washed with water to obtain an oxidized pulp (hereinafter sometimes referred to as "carboxylated cellulose", "carboxylated pulp", or "TEMPO oxidized pulp"). The pulp yield was 90%, the time required for the oxidation reaction was 90 minutes, and the amount of carboxyl groups was 1.4 mmol / g. The oxidized pulp obtained in the above process was adjusted to 1.0% (w / v) with water and treated three times with an ultra-high pressure homogenizer (20°C, 150 MPa) to obtain an oxidized CNF dispersion. The obtained fibers had an average fiber diameter of 3 nm and an aspect ratio of 150.

[0065] (Preparation of CNF aqueous dispersion) To the 1.0 mass% aqueous dispersion of TEMPO oxidized CNF obtained in Production Example 1, 4 mass parts of carboxymethyl cellulose (product name: F350HC-4, viscosity (1 mass%, 25°C) about 3000 mPa·s, degree of carboxymethyl substitution about 0.9) was added as a dispersant per 6 mass parts of solid content of CNF, and the mixture was stirred for 60 minutes with a jet paste (7200 rpm) to prepare an aqueous dispersion of CNF. The pH of this dispersion was about 7. A 0.5% aqueous sodium hydroxide solution was added to this aqueous dispersion to adjust the pH to 8 to 9. The solid content concentration of the aqueous dispersion (including TEMPO oxidized CNF and carboxymethyl cellulose) at this time was 3.1 mass%.

[0066] (Production of dried CNF) The obtained aqueous dispersion with a solid content concentration of 3.1% by mass was applied to the drum surface of a vacuum drum dryer (Katsuragi Kogyo Co., Ltd., VD-0102 model) and dried for about 1 minute at a drum surface temperature of 80° C. The obtained dried material was scraped off, pre-pulverized, and metals were detected and removed to obtain a dried body.

[0067] (Method for measuring the amount of carboxyl groups) 60 mL of a 0.5% by mass slurry (aqueous dispersion) of oxidized cellulose was prepared, and a 0.1 M aqueous hydrochloric acid solution was added to adjust the pH to 2.5. A 0.05 N aqueous sodium hydroxide solution was then added dropwise, and the electrical conductivity was measured until the pH reached 11. The electrical conductivity was calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity was gradual: Amount of carboxyl groups [mmol / g oxidized cellulose] = a [mL] × 0.05 / mass of oxidized cellulose [g].

[0068] (Measurement of average fiber diameter, average fiber length, and aspect ratio of CNF) The average fiber diameter and average fiber length of CNF were analyzed using an atomic force microscope (AFM) for 200 randomly selected fibers. The aspect ratio was calculated using the following formula: Aspect ratio = average fiber length / average fiber diameter

[0069] (Viscosity measurement) Ion-exchanged water was added to the dried and pulverized CNF collected in the Examples and Comparative Examples, and to the dried CNF produced in Production Example 1 (before pulverization) as a Reference Example, so that the solid content concentration was 1% by mass, and the mixture was stirred for 30 minutes at 3000 rpm using a homodisper to obtain an aqueous dispersion in which the CNF was redispersed. The aqueous dispersion obtained was left to stand for one day, and before measurement, it was stirred for one minute at 3000 rpm using a homodisper, and immediately thereafter, the viscosity was measured using a B-type viscometer (manufactured by Eiko Seiki Co., Ltd.) at 25°C and 60 rpm. The results are shown in Table 1.

[0070] (Redispersibility) Ion-exchanged water was added to the dried and pulverized CNF collected in the Examples and Comparative Examples, and the dried CNF produced in Production Example 1 (before pulverization) as a reference example, so that the solid content concentration was 1% by mass, and the mixture was stirred for 30 minutes at 3000 rpm using a homodisper to obtain an aqueous dispersion in which the CNF was redispersed. Two drops of ink (Kuretake Corporation, solid content 10%) were added to 1 g of the obtained CNF redispersion, and the rotation speed of a vortex mixer (IUCHI Corporation, device name: Automatic Lab-mixer HM-10H) was set to the maximum and the mixture was stirred for 30 seconds. The liquid after stirring was sandwiched between two glass plates so that the film thickness was 0.15 mm, and observed at a magnification of 100 times using an optical microscope (KEYENCE Corporation digital microscope VHX-6000). Evaluation was performed according to the following criteria, and the results are shown in Table 1. S: No white areas indicating gel particles were observed. A: A few white areas indicating gel particles were observed. B: There were more white areas indicating gel particles than in A, but fewer than in C. C: Many white areas indicating gel particles were observed.

[0071] Example 1 The dried CNF obtained in Production Example 1 was pulverized at 40°C using an impact mill (Tokyo Atomizer Mfg. Co., Ltd., Atomizer TAP-3) to produce a pulverized product (step (A)). The pulverizer was equipped with a screen (φ0.5 mm) to adjust the particle size of the pulverized product. The pulverized product was then collected at 40°C using a cyclone (step (B)). The viscosity of the collected dried and pulverized CNF product was measured and its redispersibility was evaluated.

[0072] Example 2 The same procedure as in Example 1 was used except that an airflow mill (Stream Mill ST300, manufactured by Nippon Coke Engineering Co., Ltd.) was used as the grinding machine, and the ground material with adjusted particle size was obtained and recovered, and the viscosity was measured and the redispersibility was evaluated.

[0073] Example 3 A pulverized material was obtained in the same manner as in Example 1, except that a disk mill (Centri-cutter, manufactured by Nippon Coke & Engineering Co., Ltd.) was used as the pulverizer. The pulverized material with adjusted particle size was recovered, and the viscosity was measured and the redispersibility was evaluated.

[0074] Example 4 A pulverized material was obtained in the same manner as in Example 1, except that the temperature conditions in both steps (A) and (B) were changed to 50°C. The pulverized material with adjusted particle size was recovered, and the viscosity was measured and the redispersibility was evaluated.

[0075] Example 5 A pulverized material was obtained in the same manner as in Example 2, except that the temperature conditions in both steps (A) and (B) were changed to 50°C. The pulverized material with adjusted particle size was recovered, and the viscosity was measured and the redispersibility was evaluated.

[0076] Example 6 The same procedure as in Example 3 was followed, except that the temperature conditions in both steps (A) and (B) were changed to 50°C, to obtain a pulverized material, and the pulverized material with adjusted particle size was recovered. The viscosity was measured and the redispersibility was evaluated.

[0077] Comparative Example 1 A pulverized material was obtained in the same manner as in Example 1, except that the temperature conditions in both steps (A) and (B) were changed to 60°C. The pulverized material with adjusted particle size was recovered, and the viscosity was measured and the redispersibility was evaluated.

[0078] Comparative Example 2 A pulverized material was obtained in the same manner as in Example 2, except that the temperature conditions in both steps (A) and (B) were changed to 60°C. The pulverized material with adjusted particle size was recovered, and the viscosity was measured and the redispersibility was evaluated.

[0079] Comparative Example 3 A pulverized material was obtained in the same manner as in Example 3, except that the temperature conditions in both steps (A) and (B) were changed to 60°C. The pulverized material with adjusted particle size was recovered, and the viscosity was measured and the redispersibility was evaluated.

[0080] (Reference example) The dried CNF body obtained in Production Example 1 was not pulverized, but the viscosity was measured and the redispersibility was evaluated.

[0081] [Table 1]

[0082] As can be seen from Table 1, the dried and ground CNF products obtained in Examples 1 to 6, which employ a manufacturing method comprising (A) a step of grinding a dried raw material containing anionically modified fine cellulose in a grinder and (B) a step of recovering the ground product, in which the temperature of step (A) is less than 60°C, showed reduced viscosity decrease before and after grinding when made into a redispersion liquid and had excellent redispersibility, compared to the dried and ground CNF products obtained in Comparative Examples 1 to 3, in which the temperature condition of step (A) was higher than the above temperature.

Claims

1. (A) grinding a dry raw material containing anion-modified fine cellulose fibers in a grinder; (B) recovering the pulverized material; The method for producing a dry solid of anion-modified fine cellulose fibers comprises the steps of:

2. The method for producing a dry solid product of anion-modified fine cellulose fibers according to claim 1, wherein the temperature in the step (B) is less than 60°C.

3. The method for producing a dry solid material according to claim 1 , wherein the anion-modified fine cellulose fibers are oxidized fine cellulose fibers.

4. The method for producing a dry solid material according to claim 1 , wherein the anionically modified fine cellulose fiber is a carboxymethylated fine cellulose fiber.

5. The method for producing a dry solid material according to any one of claims 1 to 3, further comprising the step of (C) classifying the pulverized material.

Citation Information

Patent Citations

  • Method for producing cellulose nanofiber dry solid

    WO2019189318A1