Manufacturing method for all-solid secondary battery
A multi-step compression process with controlled pressures and intermediate layers improves the homogeneity and structural integrity of all-solid-state secondary batteries by preventing electrolyte penetration and enhancing bondability, addressing existing manufacturing challenges.
Patent Information
- Application Number
- JP2023052753
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing methods for manufacturing all-solid-state secondary batteries face challenges in achieving homogeneity due to issues such as electrolyte layer penetration into intermediate layers and poor bondability between electrode layers, leading to potential damage and reduced structural integrity.
A multi-step compression process involving specific pressure levels is employed to flatten electrolyte layers, densify electrode layers, and improve bondability through intermediate layers and surface roughening, while using protective sheets to prevent damage to electrode collectors.
The method enhances the homogeneity and structural integrity of all-solid-state secondary batteries by preventing electrolyte layer penetration, improving bondability, and reducing damage, thus ensuring durability under varying loads.
Smart Images

Figure 2024141229000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an all-solid-state secondary battery. [Background technology]
[0002] In recent years, research and development has been conducted on secondary batteries that contribute to energy efficiency in order to ensure that more people have access to affordable, reliable, sustainable, and advanced energy. Among secondary batteries, all-solid-state secondary batteries have attracted attention because of their excellent properties in terms of safety, life, output, etc. As a method for manufacturing all-solid-state secondary batteries, a method of pressing a laminate consisting of a positive electrode layer, a solid electrolyte, and a negative electrode layer is known (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 6251974 Summary of the Invention [Problem to be solved by the invention]
[0004] Incidentally, in the technology relating to secondary batteries, a challenge is to obtain uniformity in all-solid-state batteries.
[0005] The present invention has been made in view of the above circumstances, and aims to achieve a method for producing an all-solid-state secondary battery having excellent homogeneity, which will in turn contribute to improving energy efficiency. [Means for solving the problem]
[0006] In order to solve the above problems, the following means are provided.
[0007] A method for producing an all-solid-state secondary battery according to one embodiment of the present invention includes a cathode layer forming step of forming a cathode layer containing a cathode active material, an electrolyte layer lamination step of laminating an electrolyte layer containing a solid electrolyte on one surface of the cathode layer, a first compression step of compressing the cathode layer and the electrolyte layer at a first pressure to obtain a first compressed body, an intermediate layer lamination step of laminating an intermediate layer on the surface on which the electrolyte layer is exposed in the first compressed body, a second compression step of compressing the cathode layer, the electrolyte layer, and the intermediate layer at a second pressure to obtain a second compressed body, an anode layer lamination step of laminating an anode layer on the surface on which the intermediate layer is exposed in the second compressed body, and a third compression step of compressing the cathode layer, the electrolyte layer, the intermediate layer, and the anode layer at a third pressure to obtain a third compressed body. The cathode layer forming step, the electrolyte layer lamination step, the first compression step, the intermediate layer lamination step, the second compression step, the anode layer lamination step, and the third compression step are performed in this order. The second pressure is greater than each of the first pressure and the third pressure.
[0008] According to this method, the electrolyte layer is flattened by performing the first compression step. Since the electrolyte layer is flattened, even if an intermediate layer is laminated on the electrolyte layer and the second compression step is performed, the electrolyte layer can be prevented from being embedded in the intermediate layer. The second compression step densifies the positive electrode layer and the intermediate layer, which makes it possible to prevent the electrolyte layer from penetrating into the intermediate layer. By carrying out the third compression step, the strength of the all-solid-state secondary battery is improved, and even if the all-solid-state secondary battery is subjected to repeated loads such as compression and non-compression in the plane direction of the electrolyte layer in the usage environment of the all-solid-state secondary battery, the occurrence of breakage due to elongation or cracking in the electrolyte layer can be suppressed. Furthermore, since the smoothness of the interface between the electrolyte layer and the intermediate layer is improved, an all-solid-state secondary battery with excellent homogeneity can be realized.
[0009] In the method for producing an all-solid-state secondary battery according to one aspect of the present invention, in the positive electrode layer forming step, the positive electrode layer may be formed so as to be laminated on a positive electrode current collector.
[0010] According to this method, the first compressed body has a positive electrode current collector, a positive electrode layer, and an electrolyte layer, and even if the first compression step is performed, damage to the positive electrode current collector in the first compressed body can be suppressed.
[0011] In the method for producing an all-solid-state secondary battery according to one aspect of the present invention, the positive electrode current collector may have a first surface and a second surface opposite to the first surface, and in the positive electrode layer forming step, the positive electrode layer may be formed on each of the first surface and the second surface of the positive electrode current collector.
[0012] According to this method, a positive electrode layer is formed on the first surface of the positive electrode current collector. Similarly, a positive electrode layer is formed on the second surface of the positive electrode current collector. That is, a structure in which a positive electrode layer is formed on both surfaces of the positive electrode current collector is obtained. In such a structure, even after the first compression step, the second compression step, and the third compression step, the restoring force of the positive electrode layer generated on the first surface and the restoring force of the positive electrode layer generated on the second surface cancel each other out. Therefore, the occurrence of warping is suppressed in the entire all-solid-state secondary battery. Therefore, the flatness of the all-solid-state secondary battery can be improved. In particular, when the roll press method is used in the first compression step, the second compression step, and the third compression step, the difference in the friction coefficient between the surface of the roll and the surface of the laminate laminated on both surfaces of the positive electrode current collector can be reduced. This can improve the flatness of the all-solid-state secondary battery.
[0013] In the method for producing an all-solid-state secondary battery according to one aspect of the present invention, the intermediate layer may include a solid electrolyte, a carbide, and a binder.
[0014] Generally, the electrolyte layer is made of powder. Therefore, in a structure in which the electrolyte layer is directly bonded to the anode layer, the adhesion of the anode layer to the electrolyte layer is low. In contrast, in the method for producing an all-solid-state secondary battery according to one aspect of the present invention, an intermediate layer is interposed between the anode layer and the electrolyte layer, and the intermediate layer includes a solid electrolyte, a carbide, and a binder. Therefore, compared to a structure in which the electrolyte layer is directly bonded to the negative electrode layer, a structure including an intermediate layer can improve the bonding strength of the negative electrode layer to the electrolyte layer.
[0015] In the method for producing an all-solid-state secondary battery according to one aspect of the present invention, the negative electrode layer may have a negative electrode facing surface facing the intermediate layer, and the negative electrode layer lamination step may be performed after performing a surface roughening treatment on the negative electrode facing surface before performing the negative electrode layer lamination step.
[0016] According to this method, the negative electrode facing surface of the negative electrode layer is roughened to form a fine uneven shape on the negative electrode facing surface. In this case, at the interface where the negative electrode facing surface and the intermediate layer contact each other, the intermediate layer is easily inserted into the uneven shape of the negative electrode facing surface. Therefore, the bonding between the negative electrode layer and the intermediate layer can be improved.
[0017] In the method for producing the all-solid-state secondary battery according to the aspect of the present invention, the surface roughening treatment may be performed so that the surface roughness of the negative electrode facing surface is 20 μm or more.
[0018] According to this method, the surface roughness of the negative electrode layer on the surface facing the negative electrode can be sufficiently ensured. In addition, the surface facing the negative electrode is a surface that is prone to deformation. Therefore, when the negative electrode layer is deformed in the third compression step, the stress generated between the negative electrode layer and the intermediate layer is absorbed, and cushioning properties can be improved. Therefore, unintended deformation can be suppressed, and uniform pressure can be applied between the negative electrode layer and the intermediate layer. The bonding property between the negative electrode layer and the intermediate layer can be improved.
[0019] In the method for producing an all-solid-state secondary battery according to one embodiment of the present invention, a compression member is used to compress an object to be compressed in each of the first compression step, the second compression step, and the third compression step, and in at least one of the first compression step, the second compression step, and the third compression step, the compression member may compress the object to be compressed with a protective sheet interposed between the object to be compressed and the compression member.
[0020] According to this method, at least one of the first compression step, the second compression step, and the third compression step is performed using a protective sheet. Therefore, even if pressure is applied to the layers constituting the all-solid-state secondary battery, damage to the layers can be suppressed. Here, the layers constituting the all-solid-state secondary battery are, for example, a positive electrode current collector and a negative electrode layer. In particular, when the layers constituting the all-solid-state secondary battery are made of a thin foil-like material, the effect of suppressing damage to the layers can be obtained.
[0021] A method for producing an all-solid-state secondary battery according to one aspect of the present invention may include, after performing the third compression step, a negative electrode current collector lamination step of laminating a negative electrode current collector on a surface of the third compressed body where the negative electrode layer is exposed, and a fourth compression step of compressing the positive electrode layer, the electrolyte layer, the intermediate layer, the negative electrode layer, and the negative electrode current collector to obtain an all-solid-state secondary battery.
[0022] According to this method, a structure in which a negative electrode current collector is laminated on a negative electrode layer can be obtained.
[0023] In the method for producing an all-solid-state secondary battery according to one aspect of the present invention, a compression member that compresses the compression object is used in the fourth compression step, and in the fourth compression step, the compression member may compress the compression object with a protective sheet interposed between the compression object and the compression member.
[0024] According to this method, the fourth compression step is performed using a protective sheet. Therefore, even if pressure is applied to the negative electrode current collector constituting the all-solid-state secondary battery, damage to the negative electrode current collector can be suppressed. In particular, when the negative electrode current collector is a thin foil-like material, the effect of suppressing damage to the negative electrode current collector can be obtained. Effect of the Invention
[0025] According to the method for producing an all-solid-state secondary battery according to one aspect of the present invention, it is possible to provide a method for producing an all-solid-state secondary battery having excellent homogeneity. [Brief description of the drawings]
[0026] [Figure 1] 1 is a cross-sectional view partially showing the structure of an all-solid-state secondary battery according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view illustrating a part of a roll press device, illustrating a roll press method used in the production of the all-solid-state secondary battery according to the first embodiment of the present invention. [Diagram 3] FIG. 2 is a diagram for explaining the method for producing the all-solid-state secondary battery according to the first embodiment of the present invention, and is a cross-sectional view partially showing the structure of a first compressed body obtained in the middle of the production. [Figure 4] FIG. 2 is a diagram for explaining the method for producing the all-solid-state secondary battery according to the first embodiment of the present invention, and is a cross-sectional view partially showing the structure of a second compressed body obtained in the middle of the production. [Diagram 5] FIG. 2 is a diagram for explaining the method for producing the all-solid-state secondary battery according to the first embodiment of the present invention, and is a cross-sectional view partially showing the structure of a third compressed body obtained in the middle of the production. [Figure 6] FIG. 13 is a cross-sectional view illustrating a part of a roll press device, illustrating a roll press method used in manufacturing an all-solid-state secondary battery according to a fourth embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] A method for producing an all-solid-state secondary battery according to an embodiment of the present invention will be described with reference to the drawings. In the drawings used in the following description, the scale of each component has been appropriately changed so that each component is of a recognizable size. The meaning of the term "laminating" is not limited to molding a layer onto a target member, but includes pre-molding a layer and transferring the layer onto the target member.
[0028] First Embodiment <Structure of all-solid-state secondary battery> As shown in FIG. 1, the all-solid-state secondary battery 1 includes a positive electrode current collector 2, positive electrode layers 3U, 3L, electrolyte layers 4U, 4L, intermediate layers 5U, 5L, negative electrode layers 6U, 6L, and negative electrode current collectors 7U, 7L. The positive electrode current collector 2 has a first surface 2U and a second surface 2L opposite to the first surface 2U. In the direction from the positive electrode current collector 2 toward the negative electrode current collector 7U, a positive electrode layer 3U, an electrolyte layer 4U, an intermediate layer 5U, a negative electrode layer 6U, and a negative electrode current collector 7U are laminated in this order on the first surface 2U. The positive electrode layer 3U, the electrolyte layer 4U, the intermediate layer 5U, the negative electrode layer 6U, and the negative electrode current collector 7U are compressed with respect to the positive electrode current collector 2, and constitute a laminated compression structure 1U. In the direction from the positive electrode current collector 2 toward the negative electrode current collector 7L, a positive electrode layer 3L, an electrolyte layer 4L, an intermediate layer 5L, a negative electrode layer 6L, and a negative electrode current collector 7L are laminated in this order on the second surface 2L. The positive electrode layer 3L, the electrolyte layer 4L, the intermediate layer 5L, the negative electrode layer 6L, and the negative electrode current collector 7L are compressed with respect to the positive electrode current collector 2, and constitute a laminated compression structure 1L.
[0029] <Positive electrode current collector> The positive electrode current collector 2 is a layer that contacts the positive electrode layers 3U and 3L. The material constituting the positive electrode current collector 2 is not particularly limited, and known substances that can be used as a positive electrode current collector of a solid secondary battery can be used for the positive electrode current collector 2. Examples of the positive electrode current collector 2 include metal foils such as stainless steel (SUS) foil and aluminum (Al) foil.
[0030] <Positive electrode layer> Each of the positive electrode layers 3U and 3L is a layer that contacts the electrolyte layers 4U and 4L. Each of the positive electrode layers 3U and 3L is a layer containing a positive electrode active material. The positive electrode active material is not particularly limited, and known substances that can be used as a positive electrode active material of a solid secondary battery can be used. Examples of the positive electrode active material include, for example, LiCoO2, LiNiO2, NCM (Li(Ni x Co y Mn z )O2, (0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1)) and other ternary cathode materials, layered cathode active material particles such as LiVO2 and LiCrO2, spinel-type cathode active materials such as LiMn2O4, Li(Ni 0.25 Mn 0.75 )2O4, LiCoMnO4, Li2NiMn3O8, and olivine-type cathode active materials such as LiCoPO4, LiMnPO4, and LiFePO4 can be used.
[0031] Each of the positive electrode layers 3U and 3L may further include a solid electrolyte, a conductive additive, a binder, etc., in addition to the positive electrode active material. The solid electrolyte, the conductive additive, the binder, etc. are not particularly limited, and a material known as an electrode material for a solid secondary battery can be applied. An adhesive layer may be laminated on the outer surface of the positive electrode layers 3U and 3L.
[0032] <Electrolyte layer> Each of the electrolyte layers 4U and 4L is a layer in contact with the intermediate layer 5U or 5L. Each of the electrolyte layers 4U and 4L is a layer including a solid electrolyte. The electrolyte layers 4U and 4L may include a binder or the like in addition to the above. The type of solid electrolyte is not particularly limited, and examples of the solid electrolyte include sulfide-based solid electrolytes, oxide-based solid electrolytes, nitride-based solid electrolytes, and halide-based solid electrolytes. The binder material is not particularly limited, and examples of the binder material include polyvinylidene fluoride (PVdF), polymethyl methacrylate (PMMA), polyisobutene (PIB), styrene butadiene rubber (SBR), polyethylene-vinyl acetate copolymer (PEVA), nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), etc. These may be used alone or in combination of two or more.
[0033] <Middle Class> The intermediate layers 5U and 5L are layers in contact with the negative electrode layers 6U and 6L, respectively. Examples of materials for the intermediate layers 5U and 5L include a solid electrolyte, a carbide, and a binder. For example, SnC can be used as the carbide. The intermediate layer 5U has at least one of a function of increasing ion conductivity between the corresponding electrolyte layer 4U and the negative electrode layer 6U, and a function of protecting the surface of the negative electrode layer 6U. Similarly, the intermediate layer 5L has at least one of a function of increasing ion conductivity between the corresponding electrolyte layer 4L and the negative electrode layer 6L, and a function of protecting the surface of the negative electrode layer 6L.
[0034] <Negative electrode layer> Each of the negative electrode layers 6U and 6L is a layer in contact with the negative electrode current collectors 7U and 7L. Each of the negative electrode layers 6U and 6L is a layer including a negative electrode active material. The negative electrode active material is not particularly limited, and a material known as a negative electrode active material for solid secondary batteries can be used. As the negative electrode active material, for example, lithium titanate (Li4Ti5O 12 ), transition metal oxides such as TiO2, Nb2O3, and WO3, metal sulfides, metal nitrides, carbon materials such as graphite, soft carbon, and hard carbon, silicon-based materials such as silicon elemental, silicon alloys, and silicon compounds, as well as lithium metal, lithium alloys, and metallic indium. Each of the negative electrode layers 6U and 6L may further contain, in addition to the negative electrode active material, a solid electrolyte, a conductive additive, a binder, etc. The solid electrolyte, the conductive additive, the binder, etc. are not particularly limited, and any substance known as an electrode material for a solid secondary battery can be used.
[0035] <Negative electrode current collector> Each of the negative electrode current collectors 7U and 7L corresponds to the outermost layer of the all-solid-state secondary battery 1. In other words, the negative electrode current collector 7U corresponds to the outermost layer of the laminated compression structure 1U. The negative electrode current collector 7L corresponds to the outermost layer of the laminated compression structure 1L. The material of the negative electrode current collectors 7U and 7L is not particularly limited, and any known material can be used as a negative electrode current collector for a solid secondary battery. Examples of the negative electrode current collector include metal foils such as copper (Cu) foil, stainless steel (SUS) foil, and aluminum (Al) foil.
[0036] <Method for manufacturing the all-solid-state secondary battery according to the first embodiment> Next, a method for manufacturing the all-solid-state secondary battery 1 according to the first embodiment will be described with reference to FIGS. The method for manufacturing the all-solid-state secondary battery 1 includes the following steps. Step 1: Positive electrode layer forming process Step 2: Electrolyte layer stacking process Step 3: First compression process Step 4: Interlayer Lamination Step 5: Second compression process Step 6: Anode layer stacking process Step 7: Third compression process Step 8: Negative electrode current collector lamination process Step 9: Fourth compression process Furthermore, in the manufacturing method of the all-solid-state secondary battery 1, steps 1 to 9 are performed in this order. Furthermore, in the first compression step, the second compression step, the third compression step, and the fourth compression step, known compression steps are performed. As an example of the compression steps, in this embodiment, a roll press method is adopted.
[0037] <Roll press device> FIG. 2 is a cross-sectional view showing a part of a roll press apparatus for performing the roll press method. The roll press device has a first roll R1 and a second roll R2 facing each other, and a sending mechanism (not shown). The first roll R1 can rotate counterclockwise. The second roll R2 can rotate clockwise. The sending mechanism can send the compression object 20 to the gap between the first roll R1 and the second roll R2 in the direction from the insertion part 11 toward the discharge part 12. The distance between the first roll R1 and the second roll R2 can be adjusted as appropriate. In addition, the roll press device can appropriately adjust the compression force applied to the compression object 20. In the following description, when the first roll R1 and the second roll R2 are not distinguished from each other, the first roll R1 and the second roll R2 may be simply referred to as "roll R". Each of the first roll R1 and the second roll R2 is an example of a compression member that compresses the compression target.
[0038] <Roll press method> The compressed object 20 is a laminate having a first layer 10A and a second layer 10B. Before being compressed, the compressed object 20 has a thickness h0. First, the delivery mechanism sends the compressed object 20 to the gap between the first roll R1 and the second roll R2 through the insertion section 11. As the first roll R1 and the second roll R2 rotate, the compressed object 20 moves from the insertion section 11 toward the discharge section 12. The compressed object 20 is compressed by the first roll R1 and the second roll R2, and the thickness of the compressed object 20 gradually decreases. The thicknesses of the first layer 10A and the second layer 10B constituting the compressed object 20 also gradually decrease. After being compressed, the compressed object 20 has a thickness h that is thinner than the thickness h0.
[0039] Next, each of steps 1 to 9 will be described.
[0040] <Step 1: Positive electrode layer molding process> First, the positive electrode current collector 2 and the positive electrode layers 3U and 3L are prepared. Next, a positive electrode layer 3U is laminated on the first surface 2U of the positive electrode collector 2. A positive electrode layer 3L is laminated on the second surface 2L of the positive electrode collector 2. This results in a laminate in which the positive electrode collector 2 and the positive electrode layers 3U and 3L are laminated.
[0041] <Step 2: Electrolyte layer stacking process> Next, the electrolyte layers 4U and 4L are prepared. Next, the electrolyte layer 4U is laminated on the positive electrode layer 3U. The electrolyte layer 4L is laminated on the positive electrode layer 3L. This results in a laminate in which the positive electrode current collector 2, the positive electrode layers 3U and 3L, and the electrolyte layers 4U and 4L are laminated. In the electrolyte layer lamination process, instead of directly forming the electrolyte layers 4U, 4L on the positive electrode layers 3U, 3L, a method of transferring the electrolyte layers 4U, 4L formed separately in advance to the positive electrode layers 3U, 3L may be used.
[0042] <Step 3: First compression process> Next, the laminate obtained in the electrolyte layer lamination step is compressed using a roll press device shown in Fig. 2. Specifically, the laminate obtained in the electrolyte layer lamination step is inserted between a first roll R1 and a second roll R2 as an object to be compressed 20. As the first roll R1 and the second roll R2 rotate, the laminate is gradually compressed. This results in a first compressed body 1MA shown in Fig. 3. In the first compression step, the pressure (first pressure) applied to the laminate by the first roll R1 and the second roll R2 is, for example, 300 MPa to 500 MPa.
[0043] <Step 4: Intermediate layer lamination process> Next, the intermediate layers 5U and 5L are prepared. Next, an intermediate layer 5U is laminated on the surface of the first compressed body 1MA where the electrolyte layer 4U is exposed. An intermediate layer 5L is laminated on the surface of the first compressed body 1MA where the electrolyte layer 4L is exposed. This results in a laminate in which the positive electrode current collector 2, the positive electrode layers 3U and 3L, the electrolyte layers 4U and 4L, and the intermediate layers 5U and 5L are laminated.
[0044] <Step 5: Second compression process> Next, the laminate obtained in the intermediate layer lamination step is compressed using a roll press device shown in FIG. 2. Specifically, the laminate obtained in the intermediate layer lamination step is inserted between the first roll R1 and the second roll R2 as the compression target 20. As the first roll R1 and the second roll R2 rotate, the laminate is gradually compressed. This results in a second compressed body 1MB shown in FIG. 4. In the second compression step, the pressure (second pressure) applied to the laminate by the first roll R1 and the second roll R2 is, for example, 700 MPa or more. Therefore, in comparison between the first pressure and the second pressure, the second pressure is set higher than the first pressure.
[0045] <Step 6: Negative electrode layer lamination process> Next, the negative electrode layers 6U and 6L are prepared. Next, the negative electrode layer 6U is laminated on the surface of the second compressed body 1MB where the intermediate layer 5U is exposed. The negative electrode layer 6L is laminated on the surface of the second compressed body 1MB where the intermediate layer 5L is exposed. This results in a laminate in which the positive electrode current collector 2, the positive electrode layers 3U and 3L, the electrolyte layers 4U and 4L, the intermediate layers 5U and 5L, and the negative electrode layers 6U and 6L are laminated.
[0046] <Step 7: Third compression process> Next, the laminate obtained in the negative electrode layer lamination step is compressed using a roll press device shown in FIG. 2. Specifically, the laminate obtained in the negative electrode layer lamination step is inserted between the first roll R1 and the second roll R2 as the compression target 20. With the rotation of the first roll R1 and the second roll R2, the laminate is gradually compressed. This results in a third compressed body 1MC shown in FIG. 5. In the third compression step, the pressure (third pressure) applied to the laminate by the first roll R1 and the second roll R2 is, for example, 400 MPa or less. Therefore, in comparison between the second pressure and the third pressure, the second pressure is set higher than the third pressure. More preferably, in comparison between the first pressure, the second pressure, and the third pressure, the second pressure is set higher than the third pressure, and the first pressure is set higher than the third pressure.
[0047] <Step 8: Negative electrode current collector lamination process> Next, negative electrode current collectors 7U and 7L are prepared. Next, a negative electrode current collector 7U is laminated on the surface of the third compressed body 1MC where the negative electrode layer 6U is exposed. A negative electrode current collector 7L is laminated on the surface of the third compressed body 1MC where the negative electrode layer 6L is exposed. This results in a laminate in which the positive electrode current collector 2, the positive electrode layers 3U, 3L, the electrolyte layers 4U, 4L, the intermediate layers 5U, 5L, the negative electrode current collectors 7U, 7L, and the negative electrode current collectors 7U, 7L are laminated.
[0048] <Step 9: Fourth compression process> Next, the laminate obtained in the negative electrode current collector lamination step is compressed using a roll press device shown in FIG. 2. Specifically, the laminate obtained in the negative electrode current collector lamination step is inserted between a first roll R1 and a second roll R2 as an object to be compressed 20. As the first roll R1 and the second roll R2 rotate, the laminate is gradually compressed. As a result, the all-solid-state secondary battery 1 shown in FIG. 1 is obtained.
[0049] <Action and effect> According to the above-mentioned method, the electrolyte layers 4U, 4L are each flattened by performing the first compression step. Since the electrolyte layers 4U, 4L are each flattened, even if the intermediate layers 5U, 5L are laminated on the electrolyte layers 4U, 4L, respectively, and the second compression step is performed, it is possible to prevent the electrolyte layer 4U from penetrating into the intermediate layer 5U and prevent the electrolyte layer 4L from penetrating into the intermediate layer 5L.
[0050] By carrying out the second compression step, the positive electrode layers 3U, 3L and the intermediate layers 5U, 5L are densified, whereby it is possible to prevent the electrolyte layer 4U from penetrating into the intermediate layer 5U, and it is possible to prevent the electrolyte layer 4L from penetrating into the intermediate layer 5L.
[0051] The third compression step improves the strength of the all-solid-state secondary battery 1. For example, even if the all-solid-state secondary battery 1 is subjected to repeated loads such as compression and non-compression in the planar direction of the electrolyte layers 4U and 4L in the usage environment of the all-solid-state secondary battery 1, the occurrence of breakage due to elongation or cracking in the electrolyte layers 4U and 4L can be suppressed. Furthermore, the smoothness of the interface between the electrolyte layer 4U and the intermediate layer 5U is improved, and the smoothness of the interface between the electrolyte layer 4L and the intermediate layer 5L is improved, so that an all-solid-state secondary battery 1 with excellent homogeneity can be realized.
[0052] Furthermore, the first compressed body 1MA has the positive electrode current collector 2, the positive electrode layers 3U and 3L, and the electrolyte layers 4U and 4L. Even if the first compression step is performed, damage to the positive electrode current collector 2 in the first compressed body 1MA can be suppressed.
[0053] Furthermore, a positive electrode layer 3U is formed on the first surface 2U of the positive electrode collector 2. Similarly, a positive electrode layer 3L is formed on the second surface 2L of the positive electrode collector 2. That is, a structure in which the positive electrode layers 3U and 3L are formed on both surfaces of the positive electrode collector 2 is obtained. In such a structure, even after the first compression step, the second compression step, and the third compression step, the restoring force of the positive electrode layer 3U generated on the first surface 2U and the restoring force of the positive electrode layer 3L generated on the second surface 2L cancel each other out. Therefore, the occurrence of warping is suppressed in the entire all-solid-state secondary battery 1. Therefore, the flatness of the all-solid-state secondary battery 1 can be improved. In particular, when the roll press method is used in the first compression step, the second compression step, and the third compression step, the friction coefficient difference between the surface of the roll R and the surface of the laminate laminated on both surfaces of the positive electrode collector 2 can be reduced. This can improve the flatness of the all-solid-state secondary battery 1.
[0054] Generally, the electrolyte layer is made of powder. Therefore, in a structure in which the electrolyte layer is directly bonded to the negative electrode layer, the bonding strength of the negative electrode layer to the electrolyte layer is low. In contrast, according to this embodiment, the intermediate layer 5U is interposed between the negative electrode layer 6U and the electrolyte layer 4U. Furthermore, the intermediate layer 5L is interposed between the negative electrode layer 6L and the electrolyte layer 4L. Each of the intermediate layers 5U and 5L has a solid electrolyte, a carbide, and a binder. Therefore, compared to a structure in which the electrolyte layer is directly bonded to the negative electrode layer, a structure including intermediate layers 5U, 5L can improve the bonding strength of the negative electrode layer 6U to the electrolyte layer 4U, and can improve the bonding strength of the negative electrode layer 6L to the electrolyte layer 4L.
[0055] Furthermore, since the negative electrode current collector lamination step and the fourth compression step are performed, a structure in which the negative electrode current collectors 7U and 7L are laminated on the negative electrode layers 6U and 6L, respectively, can be obtained.
[0056] <Second embodiment> Next, the all-solid-state secondary battery 1 according to the second embodiment will be described. The second embodiment differs from the first embodiment in the configuration of the negative electrode layers 6U and 6L. In the second embodiment, the same members as those in the first embodiment are denoted by the same reference numerals, and the description thereof will be omitted or simplified.
[0057] <Negative electrode layer> In the second embodiment, the negative electrode layer 6U has a negative electrode facing surface facing the intermediate layer 5U. The negative electrode layer 6L has a negative electrode facing surface facing the intermediate layer 5L.
[0058] <Method for manufacturing all-solid-state secondary battery according to the second embodiment> First, similarly to the first embodiment, the above-mentioned steps 1 to 5 are carried out. Next, a surface roughening treatment is performed on the negative electrode-facing surface of each of the negative electrode layers 6U and 6L before performing the negative electrode layer lamination step in step 6. In the surface roughening treatment, the surface roughness of the negative electrode-facing surface is set to 20 μm or more.
[0059] After the surface roughening treatment, steps 6 to 9 described above are carried out in the same manner as in the first embodiment.
[0060] <Action and effect> According to this method, the negative electrode facing surface of the negative electrode layers 6U, 6L is roughened to form a fine uneven shape on the negative electrode facing surface. In this case, at the interface where the negative electrode facing surface contacts the intermediate layer 5U, 5L, the intermediate layer 5U, 5L is easily inserted into the uneven shape of the negative electrode facing surface. Therefore, the bonding between the negative electrode layer 6U and the intermediate layer 5U can be improved, and the bonding between the negative electrode layer 6L and the intermediate layer 5L can be improved.
[0061] Furthermore, by setting the surface roughness of the negative electrode facing surface to 20 μm or more, the surface roughness of the negative electrode facing surface of the negative electrode layers 6U and 6L can be sufficiently ensured. In addition, the negative electrode facing surface becomes a surface that is easily deformed. Therefore, when the negative electrode layers 6U and 6L are deformed in the third compression step, the stress generated between the negative electrode layer 6U and the intermediate layer 5U is absorbed, and the stress generated between the negative electrode layer 6L and the intermediate layer 5L is absorbed. Therefore, the cushioning property can be improved. Therefore, unintended deformation can be suppressed, and uniform pressure can be applied between the negative electrode layer 6U and the intermediate layer 5U, and uniform pressure can be applied between the negative electrode layer 6L and the intermediate layer 5L. The bonding property between the negative electrode layer 6U and the intermediate layer 5U can be improved, and the bonding property between the negative electrode layer 6L and the intermediate layer 5L can be improved.
[0062] <Third embodiment> Next, the all-solid-state secondary battery 1 according to a third embodiment will be described. The third embodiment differs from the first embodiment in the configurations of the negative electrode layers 6U, 6L and the negative electrode current collectors 7U, 7L. In the third embodiment, the same members as those in the first embodiment are denoted by the same reference numerals, and the description thereof will be omitted or simplified.
[0063] <Negative electrode layer> In the third embodiment, each of the negative electrode layers 6U and 6L has both a function of a negative electrode layer and a function of a negative electrode current collector. Each of the negative electrode layers 6U and 6L corresponds to the outermost layer of the all-solid-state secondary battery 1. In other words, the negative electrode layer 6U corresponds to the outermost layer of the laminated compression structure 1U. The negative electrode layer 6L corresponds to the outermost layer of the laminated compression structure 1L. Each of the negative electrode layers 6U and 6L has a structure in which a negative electrode active material layer and a negative electrode current collector layer are laminated. The negative electrode active material layer contains the negative electrode active material described in the first embodiment. The negative electrode current collector layer is a metal foil such as copper (Cu) foil, stainless steel (SUS) foil, or aluminum (Al) foil.
[0064] <Method for manufacturing all-solid-state secondary battery according to the third embodiment> First, similarly to the first embodiment, the above-mentioned steps 1 to 6 are carried out. In the negative electrode layer lamination step of step 6, a negative electrode layer 6U, which is a laminate of a negative electrode active material layer and a negative electrode current collector layer, is laminated on the surface of the second compressed body 1MB where the intermediate layer 5U is exposed. Similarly, a negative electrode layer 6L, which is a laminate of a negative electrode active material layer and a negative electrode current collector layer, is laminated on the surface of the second compressed body 1MB where the intermediate layer 5L is exposed.
[0065] Next, the above-mentioned step 7 is performed. The third compressed body obtained in step 7 is the all-solid-state secondary battery 1 shown in FIG.
[0066] <Action and effect> According to this method, each of the negative electrode layers 6U and 6L is a laminate of a negative electrode active material layer and a negative electrode current collector layer. Therefore, there is no need to prepare the negative electrode current collectors 7U and 7L described in step 8, and there is no need to compress the laminate including the negative electrode current collectors 7U and 7L described in step 9. Therefore, the number of steps for manufacturing the all-solid-state secondary battery 1 can be reduced.
[0067] <Fourth embodiment> Next, a method for manufacturing the all-solid-state secondary battery according to the fourth embodiment will be described. The fourth embodiment differs from each of the first to third embodiments described above in that a protective sheet is interposed between the compression object 20 and the roll R. In the fourth embodiment, the same members as those in the first to third embodiments are denoted by the same reference numerals, and the description thereof will be omitted or simplified.
[0068] <Protective sheet> In at least one of the above-mentioned first compression step, second compression step, third compression step, and fourth compression step, a protective sheet 30 is interposed between the compression target 20 and the first roll R1, as shown in Fig. 6. In other words, the protective sheet 30 is interposed between the first compression surface RF1 of the first roll R1 and the first compression target surface 20F of the compression target 20. Similarly, the protective sheet 30 is interposed between the compression object 20 and the second roll R2. In other words, the protective sheet 30 is interposed between the second compression surface RF2 of the second roll R2 and the second compression surface 20S of the compression object 20. In this state, the first roll R1 and the second roll R2 compress the compression target 20 while rotating.
[0069] In the method for producing the all-solid-state secondary battery according to the embodiment described above, the protective sheet 30 can be interposed between the positive electrode current collector 2 and the roll R. The protective sheet 30 can be interposed between each of the negative electrode layers 6U, 6L and the roll R. In addition, the protective sheet 30 can be interposed between each of the negative electrode current collectors 7U, 7L and the roll R.
[0070] The protective sheet 30 is separate from each of the positive electrode collector 2, the negative electrode layers 6U, 6L, and the negative electrode collectors 7U, 7L. In other words, the protective sheet 30 is a member that does not constitute an all-solid-state secondary battery. For this reason, the protective sheet 30 is removed from the compression target 20 after each of the above-mentioned multiple compression steps is completed. Note that the protective sheet 30 may remain covering the compression target 20 from the end of one compression step until the next compression step is performed. In the example shown in FIG. 6, the protective sheets 30 are placed on both sides of the compression target 20, but it is sufficient that the protective sheet 30 is placed on at least one side of the compression target 20.
[0071] Examples of the material for the protective sheet 30 include metal foil and resin film. Examples of the metal foil include copper (Cu) foil, stainless steel (SUS) foil, and aluminum (Al) foil. Examples of the resin film include polyimide, polyetherimide, and fluororesin. The thickness of the protective sheet 30 is within a range of 5 to 150 μm, for example.
[0072] <Action and effect> This method can provide the same or similar effects as those provided by the above-described embodiment. Even if pressure is applied to the positive electrode collector 2, the negative electrode layers 6U, 6L, and the negative electrode collectors 7U, 7L in at least one of the first compression step, the second compression step, the third compression step, and the fourth compression step, damage to the positive electrode collector 2, the negative electrode layers 6U, 6L, and the negative electrode collectors 7U, 7L can be suppressed because the protective sheet 30 is used. In particular, when the positive electrode collector 2, the negative electrode layers 6U, 6L, and the negative electrode collectors 7U, 7L are made of thin foil-like materials, the effect of suppressing damage to the positive electrode collector 2, the negative electrode layers 6U, 6L, and the negative electrode collectors 7U, 7L can be obtained.
[0073] <Modification> In the above-described embodiment, the laminated compressed structures 1U and 1L are formed on the first surface 2U and the second surface 2L of the positive electrode current collector 2, respectively. The laminated compressed structure may be formed on only one surface of the positive electrode current collector 2. In the above-described embodiment, the roll press method is used as an example of the compression step. However, a compression method other than the roll press method may be used as long as the compression target 20 can be compressed using a compression member.
[0074] Although the embodiments of the present invention have been described above, it should be understood that these are illustrative of the present invention and should not be considered as limiting. Additions, omissions, substitutions, and other modifications can be made without departing from the scope of the present invention. Therefore, the present invention should not be considered as being limited by the above description, but is limited by the scope of the claims. [Explanation of symbols]
[0075] 1 All-solid-state secondary battery 1U, 1L stacked compression structure 1MA First Compression Body 1MB 2nd compressed body 1MC 3rd compression body 2 Positive electrode current collector 2U 1st side 2L 2nd side 3U, 3L positive electrode layer 4U, 4L electrolyte layer 5U, 5L middle tier 6U, 6L negative electrode layer 7U, 7L negative electrode current collector 10A 1st layer 10B 2nd layer 11 Insertion section 12 Discharge section 20 Compression target 30 Protective Sheet 3U positive electrode layer R1 First roll R2 Second Roll R Roll
Claims
1. a positive electrode layer forming step of forming a positive electrode layer including a positive electrode active material; an electrolyte layer lamination step of laminating an electrolyte layer containing a solid electrolyte on one surface of the positive electrode layer; a first compression step of compressing the positive electrode layer and the electrolyte layer at a first pressure to obtain a first compressed body; an intermediate layer lamination step of laminating an intermediate layer on a surface of the first compressed body on which the electrolyte layer is exposed; a second compression step of compressing the positive electrode layer, the electrolyte layer, and the intermediate layer at a second pressure to obtain a second compressed body; a negative electrode layer lamination step of laminating a negative electrode layer on a surface of the second compressed body on which the intermediate layer is exposed; a third compression step of compressing the positive electrode layer, the electrolyte layer, the intermediate layer, and the negative electrode layer at a third pressure to obtain a third compressed body; having the positive electrode layer forming step, the electrolyte layer lamination step, the first compression step, the intermediate layer lamination step, the second compression step, the negative electrode layer lamination step, and the third compression step are performed in this order; The second pressure is higher than each of the first pressure and the third pressure. A method for manufacturing an all-solid-state secondary battery.
2. In the positive electrode layer forming step, the positive electrode layer is formed so as to be laminated on a positive electrode current collector. The method for producing the all-solid-state secondary battery according to claim 1 .
3. the positive electrode current collector has a first surface and a second surface opposite to the first surface, In the positive electrode layer forming step, the positive electrode layer is formed on each of the first surface and the second surface of the positive electrode current collector. The method for producing the all-solid-state secondary battery according to claim 2 .
4. The intermediate layer includes a solid electrolyte, a carbide, and a binder. The method for producing the all-solid-state secondary battery according to any one of claims 1 to 3.
5. the negative electrode layer has a negative electrode facing surface facing the intermediate layer, Before the negative electrode layer lamination step, a surface roughening treatment is performed on the negative electrode facing surface, After the surface roughening treatment, the negative electrode layer lamination step is performed. The method for producing the all-solid-state secondary battery according to any one of claims 1 to 3.
6. In the surface roughening treatment, the surface roughness of the negative electrode facing surface is set to 20 μm or more. The method for producing the all-solid-state secondary battery according to claim 5 .
7. In each of the first compression step, the second compression step, and the third compression step, a compression member is used to compress a compression target, In at least one of the first compression step, the second compression step, and the third compression step, the compression member compresses the compression object with a protective sheet interposed between the compression object and the compression member. The method for producing the all-solid-state secondary battery according to any one of claims 1 to 3.
8. a negative electrode current collector lamination step of laminating a negative electrode current collector on a surface of the third compressed body on which the negative electrode layer is exposed after the third compression step; a fourth compression step of compressing the positive electrode layer, the electrolyte layer, the intermediate layer, the negative electrode layer, and the negative electrode current collector to obtain an all-solid-state secondary battery; having The method for producing the all-solid-state secondary battery according to claim 1 .
9. In the fourth compression step, a compression member is used to compress the compression object, In the fourth compression step, the compression member compresses the compression object with a protective sheet interposed between the compression object and the compression member. The method for producing the all-solid-state secondary battery according to claim 8 .
Citation Information
Patent Citations
Method of manufacturing electrode body
JP2015026530A
Laminated electrode body having dense electrolyte layer on negative electrode layer side before lamination press
JP2015032535A
Method of manufacturing all-solid battery
JP2017010816A
Solid-state secondary battery and manufacturing method of all-solid secondary battery
JP2018206469A
All solid state battery and manufacturing method thereof
JP2020126800A
Cited By
Method for manufacturing solid-state secondary battery
JP2024146636A