Negative electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery using the same
The use of a silicon-based and carbon-based active material layer with controlled specific surface areas addresses the energy density limitations in lithium ion batteries, enhancing both energy density and cycle performance by reducing particle expansion and contraction.
Patent Information
- Application Number
- JP2023052986
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional lithium ion secondary batteries using graphite as a negative electrode active material face limitations in improving energy density, and the contact loss between active material particles due to expansion and contraction during charging and discharging is not adequately addressed.
A negative electrode for nonaqueous electrolyte secondary batteries comprising a negative electrode active material layer with specific surface area ratios between silicon-based and carbon-based materials, optimized to suppress expansion and contraction, enhancing the lifespan and charging performance.
The optimized negative electrode structure improves the energy density and cycle characteristics by minimizing peeling between the current collector and active material layer, maintaining high capacity retention rates.
Smart Images

Figure 2024141382000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a negative electrode for a non-aqueous electrolyte secondary battery, and a non-aqueous electrolyte secondary battery using the negative electrode for a non-aqueous electrolyte secondary battery. [Background technology]
[0002] Non-aqueous electrolyte secondary batteries are used as batteries for automobiles including hybrid cars and electric cars, and are also used as batteries for small electronic devices including mobile terminals. As such batteries, lithium ion secondary batteries are particularly widely used. Lithium ion secondary batteries are required to have various characteristics such as output characteristics, energy density, capacity, life, and high temperature stability. In particular, in order to miniaturize the battery, it is an urgent task to improve the volumetric energy density and increase the capacity of the battery. In particular, lithium ion secondary batteries for electric cars are required to improve their energy density in order to further extend the driving range. For this reason, various improvements have been made to the battery configuration including the electrodes and electrolyte.
[0003] It is known that graphite is used as an anode active material for lithium-ion secondary batteries. Graphite is inexpensive, does not deteriorate much due to the charge / discharge cycle of the battery, and is highly safe, so it is widely used. However, since it is difficult to expect any further improvement in energy density in conventional lithium-ion secondary batteries that use graphite materials as the anode active material, a search is being made for anode active materials with even higher capacity. Silicon-based anode active materials containing silicon or silicon oxide (hereinafter, sometimes referred to as "Si-based anode active materials" or "Si-based anode active materials") are attracting attention as high-capacity anode active materials.
[0004] For example, Patent Document 1 discloses the specific surface area of a negative electrode material containing carbonaceous particles and silicon oxide particles. Patent Document 2 discloses a negative electrode material containing SiO xThe document discloses a lithium-ion secondary battery that uses three types of negative electrode active materials, including graphite having an average particle size of more than 15 μm and not more than 25 μm, and graphite having an average particle size of 8 μm or more and 15 μm or less, the surfaces of which are coated with amorphous carbon. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2018 / 097212 [Patent Document 2] JP 2016-219275 A Summary of the Invention [Problem to be solved by the invention]
[0006] The specific surface areas of the carbonaceous particles are described in Patent Documents 1 and 2. However, the specific surface area combinations described in the examples of these documents were not sufficient to suppress loss of contact between active material particles due to repeated expansion and contraction of the negative electrode during charging and discharging of a lithium ion secondary battery.
[0007] The present invention aims to suppress expansion and contraction during charging and discharging of a non-aqueous electrolyte secondary battery, including a lithium-ion secondary battery, when a Si-based negative electrode active material is used, thereby improving the life (cycle characteristics) and rapid chargeability of the non-aqueous electrolyte secondary battery. [Means for solving the problem]
[0008] One embodiment of the present invention is a negative electrode for a non-aqueous electrolyte secondary battery, comprising a negative electrode active material layer including a negative electrode active material, a binder, and a conductive additive. The negative electrode comprises a negative electrode active material layer including a negative electrode active material, a binder, and a conductive additive, The negative electrode active material is SiO x (wherein x is a number satisfying 0.5≦x≦1.6), A carbon-based active material (B) consisting of secondary particles formed by aggregation of primary particles; A carbon-based active material (C) consisting of primary particles different from the carbon-based active material (B); Including, The specific surface area of each of the silicon-based active material (A), the carbon-based active material (B) and the carbon-based active material (C) is represented by S A [m 2 / g], S B [m 2 / g], and S C [m 2 / g], and the maximum specific surface area is S max The smallest specific surface area among these is S min Then, S max / S min The value of is 3 or less, and S max is less than or equal to 3, It is characterized by: Effect of the Invention
[0009] The negative electrode for a nonaqueous electrolyte secondary battery of the present invention suppresses expansion and contraction even when a Si-based negative electrode active material is used, and it is possible to provide a negative electrode for a nonaqueous electrolyte secondary battery that is excellent in rapid charging and discharging, and a nonaqueous electrolyte secondary battery using the negative electrode. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] An embodiment of the present invention will be described below. One embodiment is a negative electrode for a non-aqueous electrolyte secondary battery, comprising a negative electrode active material layer containing a negative electrode active material, a binder, and a conductive assistant. The negative electrode comprises a negative electrode active material layer containing a negative electrode active material, a binder, and a conductive assistant, The negative electrode active material is SiO x (wherein x is a number satisfying 0.5≦x≦1.6), A carbon-based active material (B) that forms secondary particles formed by aggregation of primary particles; A carbon-based active material (C) consisting of primary particles different from the carbon-based active material (B); Including, The specific surface area of each of the silicon-based active material (A), the carbon-based active material (B) and the carbon-based active material (C) is represented by S A [m 2 / g], S B [m 2 / g], and S C [m 2 / g], and the maximum specific surface area is S max The smallest specific surface area among these is S min Then, S max / S min The value of is 3 or less, and S max is less than or equal to 3, It is characterized by:
[0011] In the embodiment, the non-aqueous electrolyte secondary battery is a battery that mainly uses an organic solvent-based electrolyte and can be repeatedly charged and discharged. An example of the non-aqueous electrolyte secondary battery is a lithium ion secondary battery. The non-aqueous electrolyte secondary battery includes a negative electrode for a non-aqueous electrolyte secondary battery as a component thereof. In the embodiment, the negative electrode is a thin plate-like or sheet-like battery component in which a mixture containing a negative electrode active material is applied or rolled and dried to a negative electrode current collector, which is a metal foil such as copper foil, to form a negative electrode active material layer. That is, the negative electrode is composed of a negative electrode current collector and a negative electrode active material layer containing a negative electrode active material applied to both sides of the negative electrode current collector. In the embodiment, the negative electrode active material layer preferably contains a negative electrode active material, a binder, and a conductive assistant. The negative electrode active material is a material used for the negative electrode among materials involved in a reaction that generates electric energy. The binder is generally a material for binding negative electrode active material particles in order to electrically contact the particle-shaped negative electrode active materials with each other. The conductive assistant is a material for reducing the resistance of the electrode.
[0012] In an embodiment, the negative electrode active material is SiO x (wherein x is a number satisfying 0.5≦x≦1.6) and a carbon-based active material. The silicon-based active material (A) has the chemical formula SiO xThe silicon oxide in the formula is represented by the formula: x is a number satisfying 0.5≦x≦1.6. The silicon-based active material (A) may be a single compound or a mixture of multiple compounds. The silicon-based active material (A) is preferably in the form of particles having substantially uniform or irregular sizes. The negative electrode active material may further contain a lithium silicon compound. The lithium silicon compound is represented by the chemical formula Li 4.4 Si, Li 3.75 Si and Li 4 SiO 4 (lithium silicate) and other compounds containing lithium and silicon elements. Lithium silicon compounds are stable compounds and do not release lithium during charging and discharging of a non-aqueous electrolyte secondary battery. Therefore, by using them in combination with a silicon-based active material that is prone to volumetric changes during charging and discharging of a non-aqueous electrolyte secondary battery, the volumetric changes of the negative electrode active material layer can be suppressed. Furthermore, the silicon-based active material (A) may be doped with lithium in advance. In the case of a lithium silicon compound or lithium-doped silicon, the specific surface area of the silicon-based active material (A) refers to the overall specific surface area of these silicon-containing compounds, unless otherwise specified. In this specification, the specific surface area of the silicon-based active material (A) is expressed as. Specific surface area S A But 0.7m 2 A silicon-based active material having a specific surface area of 1000 nm or more can be used as the silicon-based active material (A) of the embodiment. In this specification, the specific surface area refers to the BET specific surface area. The BET specific surface area can be determined by adsorbing gas molecules (such as nitrogen) with a known adsorption area to a material and measuring the amount of the gas molecules. The BET specific surface area of the negative electrode active material can be measured according to the Japanese Industrial Standard JIS Z 8830 "Method for measuring the specific surface area of powder (solid) by gas adsorption".
[0013] The negative electrode active material further includes a carbon-based active material. The carbon-based active material is preferably natural graphite, artificial graphite, hard carbon, soft carbon, or any mixture thereof. Here, graphite is a carbon material with hexagonal plate-like crystals in a hexagonal system, and may be called graphite or the like. Natural graphite and artificial graphite include natural graphite coated with amorphous carbon, and artificial graphite coated with amorphous carbon. Here, amorphous carbon refers to a carbon material that is amorphous as a whole, having a structure in which microcrystals are randomly networked, and may have a structure similar to that of graphite in part. Examples of amorphous carbon include carbon black, coke, activated carbon, carbon fiber, hard carbon, soft carbon, and mesoporous carbon. When artificial graphite is used, the interlayer distance d value (d 002 ) is preferably 0.33 nm or more. The crystal structure of artificial graphite is generally thinner than that of natural graphite. When artificial graphite is used as a negative electrode active material for non-aqueous electrolyte secondary batteries, particularly lithium ion secondary batteries, it is necessary that the artificial graphite has an interlayer distance that allows lithium ions to be inserted. The interlayer distance that allows lithium ions to be inserted and removed is called the d value (d 002 ), and if the d value is 0.33 nm or more, lithium ions are inserted and removed without any problems. In the embodiment, it is preferable that the carbon-based active material contains at least two kinds. The two kinds of carbon-based active materials are referred to as carbon-based active material (B) and carbon-based active material (C), respectively. The carbon-based active material (B) is preferably a carbon-based active material consisting of secondary particles formed by aggregation of primary particles. The carbon-based active material (B) is preferably artificial graphite whose surface is coated with amorphous carbon. The carbon-based active material (C) is a carbon-based active material whose primary particles are different from the primary particles of the carbon-based active material (B) and whose primary particles do not aggregate to form secondary particles. The carbon-based active material (C) is preferably artificial graphite whose surface is not coated. In this specification, the specific surface area of the carbon-based active material (B) is defined as S B and the specific surface area of the carbon-based active material (C) is S C (The unit is m 2 / g). Specific surface area is 0.5 to 2.5 m 2A carbon-based active material having a specific surface area of 0.5 to 2.5 m / g can be used as the carbon-based active material (B) of this embodiment. 2 / g of carbon-based active material can be used as the carbon-based active material (C) of this embodiment.
[0014] In this embodiment, the specific surface area S of each of the silicon-based active material (A), the carbon-based active material (B) and the carbon-based active material (C) A [m 2 / g], S B [m 2 / g], and S C [m 2 / g], the maximum specific surface area is S max The smallest specific surface area among these is S min Then, S max / S min The value of is 3 or less, and S max is preferably 3 or less. By combining negative electrode active materials having such a specific surface area relationship, the packing density of the negative electrode active material particles is optimized, and it is possible to suppress expansion and contraction accompanying charge and discharge. In the embodiment, the reason why the specific surface area of the particles constituting the negative electrode active material is adjusted as described above suppresses peeling between the negative electrode current collector and the negative electrode active material layer and improves the cycle characteristics of the battery is not clear. However, it is considered that the specific surface area of the particles constituting the negative electrode active material affects the aggregation state of the negative electrode active material particles in the negative electrode slurry and the adhesion of the binder between the negative electrode active material particles when the negative electrode active material layer is formed, causing a difference in peelability between the negative electrode current collector and the negative electrode active material layer.
[0015] In addition, with regard to the composition of the negative electrode active material, it is particularly preferable that the content of the silicon-based active material is more than 5 mass% and less than 50 mass% with respect to the total amount of the negative electrode active material in the negative electrode active material layer. More preferably, the content of the silicon-based active material is more than 10 mass% and less than 20 mass%. If the content of the silicon-based active material is too high, the volume change of the negative electrode active material during charging and discharging of the non-aqueous electrolyte secondary battery becomes large, which is undesirable. Also, if the content of the silicon-based active material is too low, it is difficult to obtain the effect of increasing the energy density.
[0016] The above-mentioned negative electrode active material can improve electrical contact by binding the particles together with the binder. The binder preferably contains poly(meth)acrylic acid, a metal salt of poly(meth)acrylic acid, an alkyl ester of poly(meth)acrylic acid, or any mixture thereof. Compounds suitable as the binder include, for example, polyacrylic acid, polymethacrylic acid; sodium polyacrylate, potassium polyacrylate, sodium polymethacrylate, potassium polymethacrylate; ethyl polyacrylate, ethyl polyacrylate, butyl polyacrylate, methyl polymethacrylate, ethyl polymethacrylate, and butyl polymethacrylate, and may be any mixture thereof. The content of the binder is preferably 2% by mass or more and less than 10% by mass with respect to the total solid content of the negative electrode active material layer. If the content of the binder is too high, the surface of the active material is covered with the binder in a large area, which may result in a decrease in ionic conductivity and electronic conductivity. If the content of the binder is too low, the electrical contact between the negative electrode active material particles may not be properly performed.
[0017] In addition to the above compounds, it is particularly preferable to further include carboxymethylcellulose (referred to as "CMC"), which is a cellulose derivative, or a metal salt of carboxymethylcellulose (e.g., sodium carboxymethylcellulose, potassium carboxymethylcellulose) as a binder component. Carboxymethylcellulose or a metal salt of carboxymethylcellulose plays a role in stabilizing the above binder compound, and also stabilizes the electrical contact of the negative electrode active material. When CMC or a metal salt of CMC is further added as a binder component, the content of CMC or a metal salt of CMC is preferably 0.05% by mass or more and 1.5% by mass or less, particularly 0.08% by mass or more and 0.8% by mass or less, and further preferably 0.15% by mass or more and 0.30% by mass or less, based on the total solid content of the negative electrode active material layer.
[0018] In an embodiment, it is preferred that the content of the silicon-based active material (A) is 5% by mass or more and 50% by mass or less, and the content of the binder is 2% by mass or more and 8% by mass or less, relative to the total solid content of the negative electrode active material layer. It is more preferable that the content of the silicon-based active material)A) is 10% by mass or more and 20% by mass or less, and the content of the binder is 2% by mass or more and 6% by mass or less, relative to the total solid content of the negative electrode active material layer. It is even more preferable that the content of the silicon-based active material (A) is 15 mass% or more and 20 mass% or less, and the content of the binder is 2.5 mass% or more and 3.8 mass% or less, relative to the total solid content of the negative electrode active material layer. By appropriately adjusting the contents of the silicon-based active material and the binder, the energy density of the non-aqueous electrolyte secondary battery can be improved.
[0019] The negative electrode active material layer preferably further contains a conductive assistant. Examples of the conductive assistant include carbon fibers such as carbon nanofibers, carbon blacks such as acetylene black and ketjen black, activated carbon, graphite, mesoporous carbon, fullerenes, and carbon nanotubes. In the embodiment, it is particularly preferable to use carbon nanotubes (referred to as "CNTs") as the conductive assistant. CNTs are substances in which a six-membered ring network (graphene) of carbon atoms has a single-layer or multi-layer coaxial tube structure, and include single-wall carbon nanotubes (single-layer, referred to as "SWCNTs") and multi-wall carbon nanotubes (multi-layer, referred to as "MWCNTs"). Any CNT may be used, but it is preferable to use an aggregated SWCNT in which SWCNTs are gathered together and have a longer diameter and longer length than a single SWCNT so that the conductive network in the negative electrode does not break when the negative electrode active material layer expands and contracts. It is preferable that the SWCNTs are dispersed in a solvent beforehand and mixed with at least one of the silicon-based active material (A), the carbon-based active material (B) and the carbon-based active material (C), and that the SWCNTs are attached to the surface of the at least one active material, and that the SWCNTs that have been lengthened and enlarged are disposed between at least two of the silicon-based active material (A), the carbon-based active material (B) and the carbon-based active material (C). Furthermore, in order to support the conductivity in the negative electrode active material layer, carbon black may be used in addition to the SWCNTs.
[0020] When CNTs are used as the conductive assistant, the content of CNTs is preferably 0.01 mass % or more and 1 mass % or less, particularly preferably 0.03 mass % or more and 0.8 mass % or less, and further preferably 0.1 mass % or more and 0.5 mass % or less, relative to the total solid content of the negative electrode active material layer.
[0021] In addition, in the negative electrode active material layer, electrode additives generally used for forming electrodes, such as thickeners, dispersants, and stabilizers, can be appropriately used.
[0022] Another embodiment of the present invention is a nonaqueous electrolyte secondary battery including at least the negative electrode for a nonaqueous electrolyte secondary battery of the embodiment, a positive electrode for a nonaqueous electrolyte secondary battery, a separator, and a nonaqueous electrolyte. The nonaqueous electrolyte secondary battery of the embodiment includes, as its constituent members, at least a negative electrode for a nonaqueous electrolyte secondary battery, a positive electrode for a nonaqueous electrolyte secondary battery, a separator, and a nonaqueous electrolyte. In the embodiment, the positive electrode is a thin plate or sheet-like battery member in which a mixture containing a positive electrode active material is applied or rolled and dried to a positive electrode collector, which is a metal foil such as an aluminum foil, to form a positive electrode active material layer. That is, the positive electrode is composed of a positive electrode collector and a positive electrode active material layer containing a positive electrode active material applied to both sides or one side of the positive electrode collector. In the embodiment, the positive electrode active material layer preferably contains a positive electrode active material and a binder. The positive electrode active material is a material used for the positive electrode among materials involved in a reaction that generates electric energy. The binder is a material for binding positive electrode active material particles in order to electrically contact the positive electrode active materials, which are generally in the form of particles.
[0023] The positive electrode active material used in the embodiment preferably contains a lithium-nickel based composite oxide as the positive electrode active material. The lithium-nickel based composite oxide is represented by the general formula Li x Ni y Me (1-y) O 2 (wherein Me is at least one metal selected from the group consisting of Al, Mn, Na, Fe, Co, Cr, Cu, Zn, Ca, K, Mg, and Pb). In particular, it is preferable to contain a lithium-manganese-based composite oxide. The lithium-manganese-based composite oxide is, for example, lithium manganate (LiMnO 2 ), lithium manganese spinel oxide (LiMn 2 O 4 The positive electrode active material is particularly a material represented by the general formula Li x Ni y Co z Mn (1-y-z) O 2The lithium nickel manganese cobalt composite oxide has a layered crystal structure represented by the formula: Here, x in the general formula is 1≦x≦1.2, y and z are positive numbers satisfying y+z<1, and the value of y is 0.5 or more. It is preferable to make 1-yz≦0.4 because it becomes difficult to synthesize a single-phase composite oxide when the proportion of manganese is large. In order to obtain a high-capacity battery, it is particularly preferable to make y>1-yz and y>z. The lithium nickel composite oxide having this general formula is a lithium nickel cobalt manganese composite oxide (hereinafter sometimes referred to as "NCM"). NCM is a lithium nickel composite oxide that is preferably used to increase the capacity of a battery.
[0024] Examples of binders that form a positive electrode active material layer together with the positive electrode active material include fluororesins such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and polyvinyl fluoride (PVF); conductive polymers such as polyanilines, polythiophenes, polyacetylenes, and polypyrroles; synthetic rubbers such as styrene butadiene rubber (SBR), butadiene rubber (BR), chloroprene rubber (CR), isoprene rubber (IR), and acrylonitrile butadiene rubber (NBR); and polysaccharides such as carboxymethyl cellulose (CMC), xanthan gum, guar gum, and pectin.
[0025] The positive electrode active material layer may contain a conductive assistant in some cases. Examples of the conductive assistant that may be used in some cases include carbon fibers such as carbon nanofibers, carbon black such as acetylene black and ketjen black, activated carbon, graphite, mesoporous carbon, fullerenes, and carbon materials such as carbon nanotubes. In the embodiment, it is particularly preferable to use carbon nanotubes (CNTs) as the conductive assistant. CNTs are substances in which a six-membered ring network (graphene) of carbon atoms has a single-layer or multi-layer coaxial tube structure, and include single-wall carbon nanotubes (single-layer, SWCNTs) and multi-wall carbon nanotubes (multi-layer, MWCNTs). Any CNT may be used, but it is preferable to use an aggregated SWCNT in which SWCNTs are gathered together and have a longer diameter and longer length than a single SWCNT so that the conductive network in the positive electrode does not break when the positive electrode active material layer expands and contracts. Furthermore, carbon black may be used in addition to SWCNTs to support the conductivity in the positive electrode active material layer. In addition, in the positive electrode active material layer, electrode additives generally used for forming electrodes, such as a thickener, a dispersant, and a stabilizer, can be appropriately used.
[0026] The non-aqueous electrolyte secondary battery of the embodiment includes a separator as a constituent member. For example, a polyolefin film can be used as the separator. Polyolefin is a compound obtained by polymerizing or copolymerizing α-olefins such as ethylene, propylene, butene, pentene, and hexene, and examples thereof include polyethylene, polypropylene, polybutene, polypentene, polyhexene, and copolymers thereof. When a polyolefin film is used as the separator, it is advantageous to use a structure having pores that are blocked when the battery temperature rises, that is, a porous or microporous polyolefin film. By having such a structure, even if the battery temperature rises, the separator can be blocked (shutdown) to cut off the ion flow. That is, the uniaxially oriented polyolefin film shrinks when the battery is heated and the pores are blocked, making it possible to prevent a short circuit between the positive and negative electrodes. In order to exert the shutdown effect, it is very preferable to use a porous polyethylene film.
[0027] Also, crosslinked films can be used as separators. Porous or microporous polyolefin films have the property of shrinking when heated, so when the battery is overheated, the film shrinks and shuts down. However, if the thermal shrinkage rate of the film is too large, the area of the film changes significantly, which may result in a large current flow. Crosslinked polyolefin films have an appropriate thermal shrinkage rate, so that even when overheated, they can shrink to the extent that they close the pores without changing the area significantly.
[0028] The separator used in the embodiment may have a heat-resistant fine particle layer on one or both sides of the separator. In this case, the heat-resistant fine particle layer provided to prevent overheating of the battery is composed of inorganic fine particles having a heat resistance of 150° C. or more and stable to electrochemical reactions. Examples of such inorganic fine particles include inorganic oxides such as silica, alumina (α-alumina, β-alumina, θ-alumina), iron oxide, titanium oxide, barium titanate, and zirconium oxide; and minerals such as boehmite, zeolite, apatite, kaolin, spinel, mica, and mullite.
[0029] The nonaqueous electrolyte secondary battery of the embodiment includes a nonaqueous electrolyte. The nonaqueous electrolyte is an electrically conductive material obtained by dissolving an ionic material in an organic solvent. The above-mentioned negative electrode for nonaqueous electrolyte secondary batteries and the positive electrode for nonaqueous electrolyte secondary batteries are stacked together, a separator is disposed between them, and a nonaqueous electrolyte secondary battery element including this and the nonaqueous electrolyte is one unit of the main components of the nonaqueous electrolyte secondary battery. Usually, a laminate formed by stacking a plurality of negative electrodes for nonaqueous electrolyte secondary batteries and a plurality of positive electrodes for nonaqueous electrolyte secondary batteries with a plurality of separators interposed therebetween is immersed in the nonaqueous electrolyte. The non-aqueous electrolyte that can be used in the embodiment is mainly a non-aqueous electrolyte solution, and is preferably a mixture containing a chain carbonate such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), di-n-propyl carbonate, di-t-propyl carbonate, di-n-butyl carbonate, di-isobutyl carbonate, or di-t-butyl carbonate, and a cyclic carbonate such as propylene carbonate (PC) or ethylene carbonate (EC). The non-aqueous electrolyte solution is preferably a mixture of such a carbonate mixture and lithium hexafluorophosphate (LiPF 6 ), lithium borofluoride (LiBF 4 ), LiFSI, Lithium perchlorate (LiClO 4 ) or other lithium salts dissolved in it.
[0030] The non-aqueous electrolyte may further contain a cyclic carbonate compound different from the above cyclic carbonate as an additive. An example of the cyclic carbonate used as an additive is vinylene carbonate (VC). A cyclic carbonate compound having a halogen may also be used as an additive. These cyclic carbonates are also compounds that form a protective coating on the negative electrode for a non-aqueous electrolyte secondary battery and the positive electrode for a non-aqueous electrolyte secondary battery during the charge / discharge process of the non-aqueous electrolyte secondary battery. In particular, they are compounds that can prevent the attack of a sulfur-containing compound such as the above disulfonic acid compound or disulfonic acid ester compound on a positive electrode active material containing a lithium-nickel composite oxide. Examples of the cyclic carbonate compound having a halogen include fluoroethylene carbonate (FEC), difluoroethylene carbonate, trifluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, and trichloroethylene carbonate. Fluoroethylene carbonate, which is a cyclic carbonate compound having a halogen and an unsaturated bond, is particularly preferably used.
[0031] The non-aqueous electrolyte may further contain a disulfonic acid compound as an additive. The disulfonic acid compound is a compound having two sulfo groups in one molecule, and includes a disulfonate compound in which the sulfo group forms a salt with a metal ion, or a disulfonic acid ester compound in which the sulfo group forms an ester. One or two of the sulfo groups of the disulfonic acid compound may form a salt with a metal ion, or may be in an anion state. Examples of the disulfonic acid compound include methane disulfonic acid, 1,2-ethane disulfonic acid, 1,3-propane disulfonic acid, 1,4-butane disulfonic acid, benzene disulfonic acid, naphthalenedisulfonic acid, biphenyl disulfonic acid, and salts thereof (lithium methane disulfonate, lithium 1,2-ethane disulfonate, etc.), and anions thereof (methane disulfonate anion, 1,2-ethane disulfonate anion, etc.). Examples of the disulfonic acid compound include disulfonic acid ester compounds, and examples of such compounds include linear disulfonic acid esters such as alkyl diesters or aryl diesters of methane disulfonic acid, 1,2-ethane disulfonic acid, 1,3-propane disulfonic acid, 1,4-butane disulfonic acid, benzene disulfonic acid, naphthalenedisulfonic acid, and biphenyl disulfonic acid; and cyclic disulfonic acid esters such as methylene methane disulfonic acid ester, ethylene methane disulfonic acid ester, and propylene methane disulfonic acid ester.
[0032] The nonaqueous electrolyte secondary battery of the embodiment is usually sealed with an exterior body. Sealing means that at least a part of the nonaqueous electrolyte secondary battery element is wrapped with an exterior body material so as not to be exposed to the outside air. The exterior body of the nonaqueous electrolyte secondary battery is a case having gas barrier properties and capable of sealing the nonaqueous electrolyte secondary battery element, or a bag-shaped body made of a flexible material. The exterior body can be suitably made of an aluminum can or an aluminum laminate sheet in which aluminum foil and polypropylene are laminated. In other words, the exterior body may be made of any material that does not allow the nonaqueous electrolyte to leach out to the outside. The outermost layer of the exterior body has a heat-resistant protective layer such as polyester, polyamide, liquid crystal polymer, etc., and the innermost layer has a sealant layer made of a thermoplastic resin such as polyethylene, polypropylene, ionomer, acid-modified polyethylene such as maleic acid-modified polyethylene, acid-modified polypropylene such as maleic acid-modified polypropylene, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyethylene isophthalate (PEI), a blend of PET and PEN, a blend of PET and PEI, a polyamide resin, a blend of polyamide resin and PET, a blend of xylylene group-containing polyamide and PET, etc., and the like. The exterior body may be formed by combining one or more of these laminate films, bonding or welding them, and further multi-layering them. Aluminum, tin, copper, nickel, and stainless steel can be used as the gas barrier metal layer. The thickness of the metal layer is preferably 30 to 50 μm. Particularly preferably, an aluminum laminate, which is a laminate of an aluminum foil and a polymer such as polyethylene or polypropylene, can be used. The nonaqueous electrolyte secondary battery of the embodiment may be in various forms, such as a coin type battery, a laminate type battery, or a wound type battery. EXAMPLES
[0033] The above describes the embodiment of the present invention. Below, examples of the present invention will be described. The above embodiment and the examples described below are merely illustrative of the present invention, and are not intended to limit the technical scope of the present invention to a specific embodiment or specific example configuration.
[0034] (Preparation of Positive Electrode, All Examples and Comparative Examples) Li(Ni) as a positive electrode active material 0.9 Co 0.05 Mn 0.05 )O 2 (97.5% by mass), polyvinylidene fluoride (PVDF, 1.5% by mass) as a positive electrode binder, and carbon nanotubes (multi-walled carbon nanotubes (MWCNT, 1% by mass) as a conductive assistant were mixed to prepare a positive electrode active material mixture. The positive electrode active material mixture was dispersed in N-methyl-2-pyrrolidone to prepare a positive electrode slurry. This positive electrode slurry was uniformly applied to one side of an aluminum current collector having a thickness of 12 μm. The initial charge capacity per unit area was 4.0 mAh / cm. 2 After drying, the coating was compressed and molded by a roll press to give a positive electrode active material layer with a density of 3.5 g / cm. 3 A positive electrode was prepared by adjusting the composition so as to satisfy the following conditions.
[0035] (Preparation of Negative Electrode, Example 1) The negative electrode active material is silicon-based active material (A), SiO x (x=1.0, S A =0.7m 2 / g) and artificial graphite (S B =1.4m 2 / g) and artificial graphite (S C =1.7m 2 / g) and the negative electrode active material mass ratio (SiO xA negative electrode active material mixture was obtained in which the mass ratio of the carbon-based active material (B) and the artificial graphite (C) of the negative electrode, ((A) / [(B)+(C)]) was 15 / 85, and the mass ratio of the carbon-based active material (B) to the carbon-based active material (C) was 1 / 1. This active material mixture (96.6% by mass), a polyacrylic acid-based binder (product name: 10CLPAH, Fujifilm Wako Pure Chemical Industries, Ltd., 3.0% by mass) as a negative electrode binder, single-wall carbon nanotube SWCNT as a conductive assistant, 0.3% by mass, and carboxymethyl cellulose (CMC, 0.1% by mass) were dissolved and dispersed in an aqueous solvent to prepare a negative electrode slurry. This negative electrode slurry was uniformly applied on a Cu current collector with a thickness of 8 μm. The initial charge capacity per unit area was 4.3 mAh / cm 2 The thickness of the coating film was then adjusted so that the density of the negative electrode active material layer was 1.65 g / cm. 3 Thus, a negative electrode was prepared. In addition, the SiO x Suitable graphite can be obtained from, for example, Sigma-Aldrich, Kojundo Chemical Laboratory, Kanto Chemical, Fujifilm Wako Pure Chemical Industries, Ltd., etc., and the surface coating components, surface condition such as roughness, particle size, etc. can be adjusted by using these alone or in a mixture and using known methods such as heat treatment such as calcination, chemical treatment such as CVD method, mechanical treatment such as crushing and classification, and sputtering. Suitable graphite can be obtained from Nippon Graphite Industry Co., Ltd., Resonac Inc., etc., and the surface coating components, surface condition such as roughness, particle size, etc. can be adjusted by using these alone or in a mixture and using known methods such as heat treatment such as calcination, chemical treatment such as CVD method, mechanical treatment such as crushing and classification, and sputtering.
[0036] The conductive additive used here is an aggregate of SWCNTs, with a length of about 1 μm and a diameter of about 10 nm, which is longer than a single SWCNT. A plurality of SWCNTs are arranged on the surface of the negative electrode active material so as to contact two or more of the silicon-based active material (A), the carbon-based active material (B), and the carbon-based active material (C). Such SWCNTs can be obtained, for example, from Meijo Nano Carbon Co., Ltd., Honjo Chemical Co., Ltd., and Kusumoto Chemical Co., Ltd.
[0037] In other examples and comparative examples, the type of negative electrode active material used and the amount of the negative electrode active material mixed were changed as shown in Table 1. Silicon-based active material (A) SiO x The carbon-based active materials (B) and (C) were obtained from the same sources as in Example 1. The mass ratio of the carbon-based active material (B) to the carbon-based active material (C) was 7:3 in Example 6 and Comparative Example 2, and 1:1 in the other Examples and Comparative Examples, as in Example 1. The types and amounts of the binder and conductive assistant, and the method of producing the negative electrode active material layer were also the same as in Example 1 in all Examples and Comparative Examples.
[0038] (Fabrication of Lithium-Ion Secondary Battery, All Examples and Comparative Examples) The positive and negative electrodes cut into 3 cm x 3 cm pieces were placed facing each other with a separator in between, which was a 10 μm-thick microporous polyethylene film with ceramic coating on both sides.
[0039] The non-aqueous electrolyte was prepared by mixing an organic solvent and a supporting salt. The volume ratio of cyclic carbonate (EC) and chain carbonate (DEC, EMC) was adjusted to 1 / 6, and lithium hexafluorophosphate (LiPF 6 ) and fluoroethylene carbonate (FEC) were added.
[0040] The positive electrode, negative electrode, separator, and non-aqueous electrolyte were placed in a laminate exterior body, and the laminate was sealed to prepare a lithium ion secondary battery, which is a non-aqueous electrolyte secondary battery. The positive electrode and negative electrode were electrically connected from the outside of the laminate by connecting tabs.
[0041] (Evaluation of lithium-ion secondary batteries) The lithium ion secondary batteries produced in each of the Examples and Comparative Examples were evaluated by measuring the capacity retention rate and the average voltage drop during 1 C discharge by the following method.
[0042] (energy density) The prepared battery was charged at 7.2mA, and after the upper limit voltage reached 4.2V, it was charged at a constant voltage until the total charging time reached 12 hours. It was then discharged at a constant current of 7.2mA until the lower limit voltage reached 2.5V. It was charged again under the same conditions, left in a thermostatic chamber at 45°C for 3 days, discharged again under the same conditions, and then charged and discharged once more. The capacity and average voltage at the final discharge were evaluated. After this evaluation, the thickness of the laminated battery (hereinafter sometimes simply referred to as "cell") was evaluated.
[0043] The sum of the thickness of the positive electrode active material layer, half the thickness of the positive electrode current collector, the thickness of the separator, the thickness of the negative electrode active material layer, and half the thickness of the negative electrode current collector, which are unit components of the laminated battery, was calculated from the thickness of the cell. Specifically, the thickness of the laminate, half the thickness of the positive electrode current collector, and half the thickness of the negative electrode current collector were subtracted from the thickness of the cell.
[0044] The formula is: [Number 1] (Capacity when cell is discharged) x (Average voltage when cell is discharged) / (Area of electrode) / (Thickness of positive electrode active material layer + Half the thickness of positive electrode current collector + Thickness of separator + Thickness of negative electrode active material layer + Half the thickness of negative electrode current collector) From this, the energy density of the unit component of the laminated battery was calculated.
[0045] (Capacity maintenance rate) The battery thus fabricated was placed in a thermostatic chamber at 45°C and charged at 30 mA. After the upper limit voltage reached 4.2 V, it was charged at a constant voltage until the total charging time reached 2.5 hours. It was then discharged at a constant current of 30 mA until the lower limit voltage reached 2.5 V. This charge / discharge cycle was repeated 100 times, and the ratio of the 100th discharge capacity to the first discharge capacity was taken as the capacity retention rate after 300 cycles.
[0046] (Peeling of the negative electrode current collector and the negative electrode active material layer after 300 charge / discharge cycles) After measuring the capacity retention rate, the laminated battery was disassembled, and the negative electrode was taken out and visually observed. The battery was rated as "present" when peeling was observed between the negative electrode current collector and the negative electrode active material layer, and was rated as "absent" when no peeling was observed between the negative electrode current collector and the negative electrode active material layer. [Table 1]
[0047] The nonaqueous electrolyte secondary battery using the negative electrode for nonaqueous electrolyte secondary battery of the embodiment of the present invention has a high energy density and a high capacity retention rate after charging and discharging. On the other hand, the nonaqueous electrolyte secondary battery using the negative electrode for nonaqueous electrolyte secondary battery of the comparative example showed a decrease in either the energy density or the capacity retention rate, and it was not possible to improve both the energy density and the lifespan. x By optimizing the specific surface areas of the two types of graphite, an appropriate particle packing density can be obtained in the negative electrode active material layer, and the expansion of the electrode can be suppressed, thereby improving the energy density and cycle capacity retention rate of the non-aqueous electrolyte secondary battery.
[0048] The reason why the specific surface area of the particles constituting the negative electrode active material is adjusted to the range of the present invention to suppress the peeling of the negative electrode current collector and the negative electrode active material layer and improve the cycle characteristics of the battery is unclear. However, it is considered that the specific surface area of the particles constituting the negative electrode active material affects the aggregation state of the negative electrode active material particles in the negative electrode slurry and the adhesion of the binder between the negative electrode active material particles when the negative electrode active material layer is formed, resulting in a difference in the peelability between the negative electrode current collector and the negative electrode active material layer.
[0049] Although the negative electrode for a nonaqueous electrolyte secondary battery of the present invention has been described in detail above, the present invention is not limited to the above-mentioned embodiment and examples, and various improvements and modifications may be made without departing from the spirit and scope of the present invention.
Claims
1. A negative electrode for a non-aqueous electrolyte secondary battery, comprising: the negative electrode includes a negative electrode active material layer including a negative electrode active material, a binder, and a conductive assistant; The negative electrode active material is SiO x (wherein x is a number satisfying 0.5≦x≦1.6), A carbon-based active material (B) consisting of secondary particles formed by aggregation of primary particles; A carbon-based active material (C) consisting of primary particles different from the carbon-based active material (B); Including, The specific surface areas of the silicon-based active material (A), the carbon-based active material (B) and the carbon-based active material (C) are defined as S A [m 2 / g], S B [m 2 / g], and S C [m 2 / g], and the maximum specific surface area among these specific surface areas is S max The smallest specific surface area among these specific surface areas is S min Then, S max / S min The value of is 3 or less, and S max is less than or equal to 3; A negative electrode for a non-aqueous electrolyte secondary battery.
2. The specific surface area S of the silicon-based active material (A) A But 0.7m 2 2. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the negative electrode has a molecular weight of 1 / g or more.
3. 3. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the carbon-based active material (B) and the carbon-based active material (C) comprise artificial graphite, hard carbon, soft carbon, or any mixture thereof.
4. 3. The negative electrode for a nonaqueous electrolyte secondary battery according to claim 1, wherein the carbon-based active material (B) is artificial graphite the surface of which is coated with amorphous carbon, and the carbon-based active material (C) is artificial graphite the surface of which is not coated.
5. 3. The negative electrode for a nonaqueous electrolyte secondary battery according to claim 1, wherein a content of the silicon-based active material (A) is 10 mass% or more and 20 mass% or less relative to a total amount of the silicon-based active material (A), the carbon-based active material (B), and the carbon-based active material (C) in the negative electrode.
6. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1 , wherein the conductive assistant comprises carbon nanotubes.
7. 3. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the conductive assistant is an aggregate of single-walled carbon nanotubes.
8. 3. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein a portion of the conductive assistant is present in a state of being previously attached to a surface of at least one of the silicon-based active material (A), the carbon-based active material (B) and the carbon-based active material (C).
9. 3. The negative electrode for a non-aqueous electrolyte secondary battery in accordance with claim 1, wherein the binder comprises polyacrylic acid.
10. A non-aqueous electrolyte secondary battery comprising at least the negative electrode for a non-aqueous electrolyte secondary battery according to claim 1 or 2, a positive electrode for a non-aqueous electrolyte secondary battery, a separator, and an electrolyte.
Citation Information
Patent Citations
Electrode and secondary battery including same
JP2022529987A
Negative electrode sheet and method for producing the same, secondary battery, battery module, battery pack and device
JP2023503706A
Non-aqueous electrolyte secondary battery
WO2015045314A1
Secondary battery negative electrode and secondary battery
WO2021085255A1
Lithium ion secondary battery
JP2016219275A