Zinc secondary battery

The zinc secondary battery design with a non-porous negative electrode core and composite separator enhances cycle life by balancing dendrite resistance and electrolyte retention, addressing the issues of short circuits and dry-out.

JP2024141534APending Publication Date: 2024-10-10FDK CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023053248
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Zinc secondary batteries suffer from shortened cycle life due to dendrite growth causing short circuits and separator dry-out phenomena, which current solutions like incorporating a microporous film into the separator fail to adequately address.

Method used

A zinc secondary battery design featuring a negative electrode core made of a non-porous sheet metal conductor and a separator composed of a composite of nonwoven fabric and microporous film, with a specific thickness ratio of 0.28 to 0.53, to balance dendrite resistance and electrolyte retention.

Benefits of technology

The design effectively suppresses short circuits and maintains electrolyte stability, enhancing the battery's cycle life characteristics by preventing dendrite penetration and dry-out, thereby improving durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141534000001_ABST
    Figure 2024141534000001_ABST
Patent Text Reader

Abstract

To provide a zinc secondary battery that has better cycle life characteristics than conventional batteries.SOLUTION: A battery 2 includes an outer can 10 and an electrode group 22 accommodated in the outer can 10 together with an alkaline electrolyte. The electrode group 22 is formed by stacking a positive electrode 24 and a negative electrode 26 with a separator 28 between them. The negative electrode 26 includes a negative electrode core and a negative electrode mixture held in the negative electrode core. The negative electrode mixture includes at least one of zinc, a zinc alloy, and a zinc-containing compound. The negative electrode core is made of imperforate copper foil. The separator 28 is a composite in which a nonwoven fabric 42 and a microporous film 40 are aligned in the thickness direction. When the total thickness of the microporous film 40 is A and the total thickness of the nonwoven fabric 42 is B, the value of A / B is 0.28 or more and 0.53 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a zinc secondary battery. [Background technology]

[0002] In the zinc battery using zinc, zinc alloy or zinc-containing compound as the negative electrode active material, primary battery and secondary battery have been researched and developed. Zinc batteries are classified according to the material used for the positive electrode active material. Examples of such zinc batteries include air-zinc batteries using oxygen in the air as the positive electrode active material, nickel-zinc batteries using nickel-containing compounds as the positive electrode active material, manganese-zinc batteries using manganese-containing compounds as the positive electrode active material, and silver-zinc batteries using silver-containing compounds as the positive electrode active material. In particular, air-zinc primary batteries, manganese-zinc primary batteries, and silver-zinc primary batteries have been put into practical use and are widely used.

[0003] On the other hand, zinc secondary batteries such as nickel-zinc secondary batteries are highly safe because they can use an aqueous solution as an electrolyte, and they have an extremely high theoretical volumetric energy density, making them potentially superior to the performance of existing lithium-ion secondary batteries.

[0004] However, zinc secondary batteries generate so-called dendrites, in which zinc deposits are formed in the form of branches on the negative electrode during charging and discharging. These dendrites grow after a relatively small number of charge-discharge cycles, and penetrate the separator to the positive electrode, causing a short circuit. For this reason, zinc secondary batteries have the problem of shortening their cycle life due to short circuits caused by dendrites.

[0005] In order to solve this problem, various studies have been conducted, for example, a microporous film is incorporated into the separator, as in the zinc battery disclosed in Patent Document 1. This makes it possible to reduce the occurrence of short circuits. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2019-133844 A Summary of the Invention [Problem to be solved by the invention]

[0007] In recent years, batteries have been used in various portable devices, hybrid electric vehicles, and other devices, and the applications of batteries are expanding. With such expansion of applications, the importance of developing and improving batteries is increasing in many industries, and mainly, high performance batteries are desired. In this situation, high performance is also desired for zinc secondary batteries. Here, one of the performances that should be improved for zinc secondary batteries is the ability to repeat charging and discharging for a longer period of time, that is, cycle life performance.

[0008] In addition to the short circuit caused by dendrite growth as described above, the cause of the shortened cycle life of zinc secondary batteries is the so-called separator dry-out phenomenon, in which the positive electrode swells due to deterioration and presses against the separator, pushing the electrolyte out of the separator and causing the separator to be unable to retain a sufficient amount of electrolyte. When a microporous film is incorporated into the separator as in Patent Document 1, the resistance to dendrites penetrating through (hereinafter also referred to as dendrite resistance) is improved, but the separator's ability to retain electrolyte is reduced, and the separator dry-out phenomenon causes insufficient charging and discharging, resulting in a shortened cycle life.

[0009] In the current zinc secondary battery, dendrite resistance has been studied as in Patent Document 1. However, in the current situation, zinc secondary batteries have not yet achieved sufficient cycle life characteristics to meet the needs of users. For this reason, in order to further improve the cycle life, it is considered important to conduct a broader study without being limited to the study of dendrite resistance, to find factors that contribute to the improvement of cycle life characteristics, and to strike a balance between them. From this perspective, it is considered that the cycle life can be further extended by studying how to suppress the separator dry-out phenomenon and further suppress dendrite growth while maintaining the dendrite resistance.

[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a zinc secondary battery having better cycle life characteristics than conventional batteries. [Means for solving the problem]

[0011] According to the present invention, there is provided a zinc secondary battery comprising a container and an electrode group housed in the container together with an alkaline electrolyte, the electrode group being formed by stacking a positive electrode and a negative electrode with a separator interposed therebetween, the negative electrode including a negative electrode core and a negative electrode mixture held by the negative electrode core, the negative electrode mixture including at least one of zinc, a zinc alloy and a zinc-containing compound, the negative electrode core being made of a non-porous sheet-like metal conductor, the separator being a composite of a nonwoven fabric and a microporous film aligned in the thickness direction, and wherein, when the total thickness of the microporous film is A and the total thickness of the nonwoven fabric is B, the value of A / B is 0.28 or more and 0.53 or less. Effect of the Invention

[0012] The zinc secondary battery according to the present invention comprises a container and an electrode group housed in the container together with an alkaline electrolyte, the electrode group being formed by stacking a positive electrode and a negative electrode with a separator interposed therebetween, the negative electrode comprising a negative electrode core and a negative electrode mixture held by the negative electrode core, the negative electrode mixture comprising at least one of zinc, a zinc alloy and a zinc-containing compound, the negative electrode core being made of a non-porous sheet-like metal conductor, the separator being a composite of a nonwoven fabric and a microporous film aligned in the thickness direction, the total thickness of the microporous film being A and the total thickness of the nonwoven fabric being B, the value of A / B being 0.28 or more and 0.53 or less. With this configuration, the zinc secondary battery according to the present invention can achieve both suppression of short circuit caused by zinc dendrites and retention stability of the electrolyte between the positive and negative electrodes, and can maintain a high capacity retention rate for a long period of time. Therefore, according to the present invention, a zinc secondary battery having better cycle life characteristics than conventional ones can be provided. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a partially cutaway perspective view of a nickel-zinc battery according to one embodiment. [Diagram 2] FIG. 2 is a cross-sectional view that shows a schematic arrangement of a positive electrode and a negative electrode sandwiching a separator having a two-layer structure. [Diagram 3] FIG. 2 is a cross-sectional view that shows a schematic arrangement of a positive electrode and a negative electrode sandwiching a separator having a four-layer structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, a nickel-zinc secondary battery (hereinafter also referred to as battery) 2 according to one embodiment will be described with reference to the drawings.

[0015] The battery 2 is, for example, a cylindrical battery of 4 / 3FA size. More specifically, as shown in FIG. 1, the battery 2 includes an outer can 10 as a container having a cylindrical shape with an open top and a closed bottom. The outer can 10 is conductive, and its bottom wall 35 functions as a negative electrode terminal. A sealing body 11 is fixed to the opening of the outer can 10. The sealing body 11 includes a cover plate 14 and a positive electrode terminal 20, and seals the outer can 10 and provides the positive electrode terminal 20. The cover plate 14 is a disc-shaped member having conductivity. The cover plate 14 and a ring-shaped insulating packing 12 surrounding the cover plate 14 are disposed in the opening of the outer can 10, and the insulating packing 12 is fixed to the opening edge 37 of the outer can 10 by crimping the opening edge 37 of the outer can 10. That is, the cover plate 14 and the insulating packing 12 cooperate with each other to hermetically close the opening of the outer can 10.

[0016] Here, the cover plate 14 has a central through-hole 16 in the center, and a rubber valve body 18 that closes the central through-hole 16 is disposed on the outer surface of the cover plate 14. Furthermore, a metallic positive electrode terminal 20 having a flanged cylindrical shape is electrically connected to the outer surface of the cover plate 14 so as to cover the valve body 18. This positive electrode terminal 20 presses the valve body 18 toward the cover plate 14. The positive electrode terminal 20 is provided with a gas vent hole (not shown).

[0017] Under normal circumstances, the central through hole 16 is airtightly closed by the valve body 18. On the other hand, if gas is generated inside the outer can 10 and the internal pressure increases, the valve body 18 is compressed by the internal pressure and opens the central through hole 16, causing gas to be released from inside the outer can 10 to the outside via the central through hole 16 and a gas vent hole (not shown) in the positive terminal 20. In other words, the central through hole 16, the valve body 18, and the positive terminal 20 form a safety valve for the battery.

[0018] The outer can 10 contains an electrode group 22. The electrode group 22 includes a strip-shaped positive electrode 24, a negative electrode 26, and a separator 28. More specifically, the positive electrode 24 and the negative electrode 26 are wound in a spiral shape with the separator 28 sandwiched between them. That is, the positive electrode 24 and the negative electrode 26 are stacked on top of each other with the separator 28 interposed therebetween. The outermost periphery of the electrode group 22 is formed by a part (outermost periphery) of the negative electrode 26, and is in contact with the inner circumferential wall of the outer can 10. That is, the negative electrode 26 and the outer can 10 are electrically connected to each other.

[0019] In the exterior can 10, a positive electrode lead 30 is disposed between one end of the electrode group 22 and the cover plate 14. More specifically, one end of the positive electrode lead 30 is connected to the positive electrode 24, and the other end is connected to the cover plate 14. Thus, the positive electrode terminal 20 and the positive electrode 24 are electrically connected to each other via the positive electrode lead 30 and the cover plate 14. A circular upper insulating member 32 is disposed between the cover plate 14 and the electrode group 22, and the positive electrode lead 30 extends through a slit 39 provided in the upper insulating member 32. A circular lower insulating member 34 is also disposed between the electrode group 22 and the bottom of the exterior can 10.

[0020] Furthermore, a predetermined amount of alkaline electrolyte (not shown) is injected into the exterior can 10. The alkaline electrolyte is impregnated into the electrode group 22 and is mainly held by the separator 28. This alkaline electrolyte promotes an electrochemical reaction (charge / discharge reaction) between the positive electrode 24 and the negative electrode 26 during charging and discharging. As this alkaline electrolyte, an aqueous solution containing at least one of KOH, NaOH, and LiOH as a solute is preferably used. The concentration of the alkaline electrolyte is not particularly limited, and for example, 7N is used. Furthermore, since the battery 2 is a nickel-zinc battery, it is preferable to use the above-mentioned alkaline electrolyte in which zinc oxide is dissolved to a saturated concentration. This makes it possible to reduce the dissolution of zinc from the negative electrode into the alkaline electrolyte.

[0021] The positive electrode 24 includes a conductive positive electrode core having a porous structure and a positive electrode mixture held by the positive electrode core. The positive electrode core as described above is, for example, a metal body made of nickel having a three-dimensional mesh-like skeleton. The skeleton of the metal body spreads over the entire positive electrode core, and the gaps in the skeleton form communication holes. The communication holes are filled with the positive electrode mixture. For example, nickel foam can be used as such a metal body.

[0022] The positive electrode mixture contains a positive electrode active material, a positive electrode additive, and a thickener. Examples of the thickener include hydroxypropyl cellulose. It is also preferable to add a binder as necessary. Examples of the binder include hydrophilic or hydrophobic polymers.

[0023] Nickel hydroxide is used as the positive electrode active material. The nickel hydroxide is in the form of a powder. That is, nickel hydroxide powder, which is an aggregate of nickel hydroxide particles, is used. It is preferable to use highly ordered nickel hydroxide particles as the nickel hydroxide particles.

[0024] The nickel hydroxide particles preferably contain Co, Zn, Cd, or the like in solid solution.

[0025] In addition, the nickel hydroxide particles are preferably covered with a surface layer containing a cobalt compound. As the surface layer, a high-order cobalt compound layer containing a cobalt compound having a valence of 3 or more is preferably used.

[0026] The high cobalt compound layer has excellent electrical conductivity and forms a conductive network. As the high cobalt compound layer, it is preferable to adopt a layer containing a cobalt compound such as cobalt oxyhydroxide (CoOOH) that has been made higher in order to have a valence of three or more.

[0027] As another method for forming a conductive network, it is preferable to adopt a method of adding a powder of a cobalt compound to the positive electrode mixture instead of forming a surface layer containing a cobalt compound on the surface of nickel hydroxide particles. As the powder of this cobalt compound, cobalt hydroxide powder can be mentioned. The method of adding a powder of a cobalt compound has an advantage that the conductive network can be formed more easily than the method of forming a surface layer of a cobalt compound on the surface of nickel hydroxide particles.

[0028] Next, examples of the positive electrode additive include yttrium oxide. It is also preferable to use cobalt oxide, metallic cobalt, cobalt hydroxide, and other cobalt compounds, zinc metal, zinc oxide, zinc hydroxide, and other zinc compounds, niobium oxide, erbium oxide, and the like.

[0029] Next, the positive electrode 24 can be produced, for example, as follows. First, a cathode additive, a thickener, and water are added to the cathode active material powder, which is an aggregate of the cathode active material particles obtained as described above, and the mixture is kneaded to prepare a cathode mixture slurry. The obtained cathode mixture slurry is filled, for example, in a foamed nickel, which is then dried. After the drying process, the foamed nickel filled with nickel hydroxide particles and the like is rolled and then cut. This results in a cathode 24 containing the cathode mixture.

[0030] Next, the negative electrode 26 will be described. As shown in FIGS. 2 and 3, the negative electrode 26 has a strip-shaped conductive negative electrode core 27, and the negative electrode core 27 holds a negative electrode mixture 29.

[0031] The negative electrode core 27 is a non-porous sheet-like metal conductor, so-called non-porous foil. Here, non-porous refers to a state in which the sheet does not have holes penetrating from the front surface to the back surface. Specifically, it is preferable to use copper foil having a thickness of 20 μm or more and 50 μm or less as the negative electrode core 27.

[0032] The negative electrode core 27 described above does not have any holes, and therefore has no corners or edges at the holes, and is generally flat. In such a generally flat surface, a uniform current flows generally during charging and discharging.

[0033] In zinc secondary batteries, charging and discharging are repeated by the exchange of zinc ions between the positive and negative electrodes, but if there is a part of the electrode that is uneven in shape, current will concentrate in that uneven part. Then, zinc will precipitate in the form of dendrites in the part where the current concentrates. In other words, if the shape of the negative electrode is uneven, dendrites are likely to form.

[0034] In this embodiment, as described above, the negative electrode core 27 is generally flat, and therefore has few uneven parts in shape, and therefore has few parts where current concentrates. Therefore, using a non-porous sheet-like metal conductor as the negative electrode core 27 can contribute to suppressing the formation of zinc dendrites.

[0035] The negative electrode mixture 29 is held in layers on both sides of the negative electrode core 27. The layers of the negative electrode mixture 29 have a flat and uniform shape following the shape of the flat negative electrode core 27. Therefore, the negative electrode 26 as a whole also has a flat and uniform shape, and the formation of zinc dendrites can be suppressed to a minimum.

[0036] The negative electrode mixture 29 described above contains a negative electrode active material and a binder, and may also contain a negative electrode additive and a thickener as required.

[0037] The negative electrode active material contains at least zinc, and may further contain at least one of a zinc alloy and a zinc-containing compound. Here, as the raw material constituting the zinc alloy, it is preferable to use bismuth, aluminum, indium, etc. in addition to zinc. Examples of the zinc-containing compound include zinc oxide (one type / two types / three types), zinc hydroxide, zinc sulfide, tetrahydroxyzinc ion salt, zinc halide, zinc acetate, zinc tartrate, zinc oxalate and other zinc carboxylate compounds, magnesium zincate, calcium zincate, barium zincate, zinc borate, zinc silicate, zinc aluminate, zinc fluoride, zinc carbonate, zinc hydrogen carbonate, zinc nitrate, zinc sulfate, etc.

[0038] The negative electrode active material is in the form of a powder. That is, a negative electrode active material powder that is an aggregate of negative electrode active material particles is used. The average particle size of zinc particles as the negative electrode active material is preferably 49 μm or more and 71 μm or less.

[0039] Here, the average particle size of the zinc alloy particles is preferably 10 to 1000 μm, and the average particle size of the zinc-containing compound particles is preferably 0.1 to 100 μm. In this specification, the average particle size means the average particle size at which the mass-based integration determined by a laser diffraction / scattering method using a particle size distribution measuring device corresponds to 50%, unless otherwise specified.

[0040] The binder functions to bind the negative electrode active material, the negative electrode additive, etc. to each other and at the same time bind the negative electrode active material, the negative electrode additive, etc. to the negative electrode core. Synthetic rubber is used as the binder. In particular, styrene butadiene rubber (SBR) has a high binding effect, so it is preferable to use SBR as the binder.

[0041] The negative electrode additive serves to improve the characteristics of the negative electrode, and examples of the negative electrode additive include bismuth oxide, bismuth hydroxide, indium oxide, indium hydroxide, potassium oxalate, and hydrates thereof.

[0042] The thickener is not particularly limited, and for example, hydroxypropyl cellulose is used.

[0043] Next, the negative electrode 26 can be produced, for example, as follows. First, a negative electrode mixture paste is prepared by kneading a negative electrode active material powder, which is an aggregate of particles of a negative electrode active material (e.g., zinc), a negative electrode additive, a binder, a thickener, and water. The obtained negative electrode mixture paste is applied to a negative electrode core and is dried. After drying, the negative electrode core 27 holding the negative electrode active material powder, the binder, etc. is rolled overall to increase the packing density of the negative electrode active material, thereby obtaining a negative electrode intermediate product. Then, this negative electrode intermediate product is cut into a predetermined shape. In this way, a negative electrode 26 is manufactured.

[0044] The separator 28 is disposed to prevent a short circuit between the positive electrode 24 and the negative electrode 26. Therefore, an electrically insulating material is used for the separator 28. The separator 28 is a composite in which a microporous film 40 and a nonwoven fabric 42 are laminated in the thickness direction. Preferably, as shown in FIG. 2, the separator 28 is a composite having a two-layer structure in which one microporous film 40 and one nonwoven fabric 42 are laminated. When this two-layer composite is incorporated into the electrode group 22, the nonwoven fabric 42 is positioned on the positive electrode 24 side, and the microporous film 40 is positioned on the negative electrode 26 side. More preferably, as shown in FIG. 3, two nonwoven fabrics 42 (a first nonwoven fabric 44 and a second nonwoven fabric 46) and two microporous films 40 (a first microporous film 48 and a second microporous film 50) are prepared, and when these are incorporated into the electrode group 22, a composite having a four-layer structure is formed in which the first nonwoven fabric 44, the first microporous film 48, the second nonwoven fabric 46, and the second microporous film 50 are layered in this order from the positive electrode 24 to the negative electrode 26.

[0045] The microporous film 40 is a polymer film containing many pores and is made of polyolefin. If the porosity of the microporous film 40 is too high, it is difficult to prevent the dendrites from extending. On the other hand, if the porosity of the microporous film 40 is too low, the permeability of the alkaline electrolyte is hindered, and in turn, the permeability of ions is hindered. The porosity of the microporous film 40 is preferably 34% or more and 49% or less. Here, the porosity of the microporous film 40 refers to a numerical value expressed as a percentage of the volume of the pore spaces in the total volume of the microporous film.

[0046] Here, as the separator of the microporous film, a microporous film separator made of polyolefin for lithium ion batteries is known, and in this embodiment, this microporous film separator for lithium ion batteries can be used. However, in zinc secondary batteries, since an alkaline aqueous solution is used as the electrolyte, it is preferable to perform a hydrophilization treatment on the microporous film. Examples of this hydrophilization treatment include a plasma treatment in which polar functional groups are attached to the surface by surface modification with oxygen radicals, a sulfonation treatment in which sulfonic groups are generated on the surface by treatment in sulfur trioxide gas or fuming sulfuric acid, and a treatment with a surfactant. In this embodiment, it is preferable to select a hydrophilization treatment with a surfactant as the hydrophilization treatment in order to reduce damage to the microporous film 40.

[0047] In addition, in lithium ion batteries, polyethylene microporous films with a melting point of 130 to 140°C are mainly used to improve safety. This is aimed at a shutdown function that, when the battery temperature rises abnormally due to a short circuit or the like, the polyethylene constituting the microporous film melts to block the pores and stop the permeation of ions through the separator. However, since zinc secondary batteries use an alkaline aqueous solution, a polypropylene microporous film with a lower risk of combustion and a higher melting point can be used. In this embodiment, a polyethylene microporous film can of course be used.

[0048] Also, in lithium ion batteries, it is common to use a microporous film alone as a separator. However, the microporous film has a low ability to retain moisture (hereinafter also referred to as liquid retention). In zinc secondary batteries, the ability of the separator 28 to retain an alkaline aqueous solution is important, so it is effective to use a composite as a separator, which is a combination of a microporous film 40 with low liquid retention and a nonwoven fabric 42 used as a separator in nickel-hydrogen secondary batteries. In other words, the nonwoven fabric 42 is characterized by a higher porosity and better liquid retention than the microporous film 40, and is therefore suitable for complementing the liquid retention of the microporous film 40.

[0049] For example, a polyamide fiber nonwoven fabric to which hydrophilic functional groups have been added, or a polyolefin fiber nonwoven fabric such as polyethylene or polypropylene to which hydrophilic functional groups have been added can be used as the nonwoven fabric 42. Specifically, it is preferable to use a nonwoven fabric mainly made of polyolefin fibers to which sulfonation treatment has been applied to add sulfonic groups. Here, the sulfonic groups are added by treating the nonwoven fabric with an acid containing sulfuric acid groups, such as sulfuric acid or fuming sulfuric acid.

[0050] In this embodiment, when the total thickness of the microporous film 40 is A and the total thickness of the nonwoven fabric 42 is B, the ratio of A to B, A / B, is set to 0.28 or more and 0.53 or less.

[0051] When the value of A / B is less than 0.28, the proportion of the nonwoven fabric 42 is high and the liquid retention is excellent, so that the dry-out phenomenon is unlikely to occur. However, since the proportion of the microporous film 40 is low, the dendrite resistance is low, so that short circuits due to dendrites are likely to occur, and the cycle life is reduced due to the dendrites.

[0052] When the value of A / B exceeds 0.53, the proportion of the microporous film 40 increases, and the dendrite resistance is excellent, so that the dendrite is prevented from penetrating the separator and causing a short circuit. However, the proportion of the nonwoven fabric 42 is small, so that the electrolyte retention is low overall, the amount of alkaline electrolyte retained is small, and dryout is easily caused. This causes a decrease in cycle life due to dryout.

[0053] Therefore, in order to enhance the dendrite resistance and also suppress the dry-out phenomenon, it is important to set the value of A / B to 0.28 or more and 0.53 or less, as described above.

[0054] The positive electrode 24 and the negative electrode 26 manufactured as described above are spirally wound with the separator 28 interposed therebetween, thereby forming the electrode group 22.

[0055] The electrode group 22 thus obtained is housed in an exterior can 10. Next, a predetermined amount of alkaline electrolyte is poured into the exterior can 10.

[0056] Thereafter, the exterior can 10 containing the electrode group 22 and the alkaline electrolyte is sealed with a sealing body 11 equipped with a positive electrode terminal 20 to obtain a battery 2. The obtained battery 2 is subjected to an initial activation process and is made ready for use.

[0057] [Example] 1. Battery manufacturing Example 1 (1) Manufacturing of positive electrodes To 100 parts by weight of nickel hydroxide powder prepared as a positive electrode active material, 25 parts by weight of cobalt hydroxide powder, 0.5 parts by weight of yttrium oxide powder, 0.5 parts by weight of zinc oxide powder, 0.3 parts by weight of niobium oxide powder, and 50.0 parts by weight of water containing 0.2% by weight of hydroxypropyl cellulose powder as a thickener were added and kneaded to prepare a positive electrode mixture slurry.

[0058] Next, the slurry of the positive electrode mixture was filled into a sheet-shaped foamed nickel serving as a positive electrode core. The foamed nickel had an areal density (weight per unit area) of about 350 g / m 2 The porosity was 95% and the thickness was 1.3 mm.

[0059] Next, the foamed nickel filled with the slurry of the positive electrode mixture was subjected to a drying treatment. After that, the foamed nickel filled with the positive electrode mixture was entirely rolled and then cut into a predetermined size to obtain a positive electrode 24 for 4 / 3FA size. The positive electrode capacity of the positive electrode 24 was 2400mAh.

[0060] (2) Manufacturing of negative electrodes 100 parts by weight of zinc oxide powder, 25 parts by weight of zinc powder, 3 parts by weight of bismuth oxide powder, 2 parts by weight of potassium oxalate monohydrate, 4 parts by weight of styrene-butadiene rubber powder as a binder, 1 part by weight of hydroxypropyl cellulose powder as a thickener, and 100 parts by weight of water were prepared. Then, the zinc oxide powder, zinc powder, bismuth oxide powder, potassium oxalate monohydrate, styrene-butadiene rubber powder, hydroxypropyl cellulose powder, and water were kneaded in an environment of 25° C. to prepare a negative electrode mixture paste.

[0061] Here, the zinc oxide particles constituting the zinc oxide powder had an average particle size of 0.75 μm, and the zinc particles constituting the zinc powder had an average particle size of 71 μm.

[0062] On the other hand, a tin-plated non-porous copper foil was prepared as a negative electrode core. This non-porous copper foil had a thickness of 35 μm and was in the form of a sheet that did not contain any holes penetrating from the front to the back.

[0063] The negative electrode mixture paste obtained as described above was applied evenly and to a uniform thickness on both sides of a non-porous copper foil serving as a negative electrode core.

[0064] After the negative electrode mixture paste was dried, the non-porous copper foil holding the negative electrode mixture was rolled and then cut to a predetermined size to obtain a 4 / 3FA size negative electrode 26. The negative electrode 26 had a negative electrode capacity of 4500 mAh.

[0065] (3) Nickel-zinc battery assembly The positive electrode 24 and the negative electrode 26 obtained as described above were spirally wound with a separator 28 sandwiched between them to produce an electrode group 22.

[0066] The separator 28 used in the manufacture of the electrode group 22 here is a composite of a sulfonated polypropylene fiber nonwoven fabric 42 and a surfactant-treated polypropylene microporous film 40 aligned in the thickness direction. In detail, as shown in Fig. 3, a total of two sheets of the nonwoven fabric 42, a first nonwoven fabric 44 and a second nonwoven fabric 46, and a total of two sheets of the microporous film 40, a first microporous film 48 and a second microporous film 50, were prepared, and the first nonwoven fabric 44, the first microporous film 48, the second nonwoven fabric 46, and the second microporous film 50 were combined in this order to produce the separator 28 made of a four-layer composite. When the total thickness of the first microporous film 48 and the second microporous film 50 is A and the total thickness of the first nonwoven fabric 44 and the second nonwoven fabric 46 is B, A=35 μm, B=124 μm, and the value of A / B was 0.28. The first microporous film 48 and the second microporous film 50 contained pores with a pore size of 0.2 μm and a porosity of 41%. The first nonwoven fabric 44 and the second nonwoven fabric 46 each had a basis weight of 100 g / m 2 It was.

[0067] When the positive electrode 24, the negative electrode 26 and the separator 28 were combined and wound, the first nonwoven fabric 44 of the separator 28 was in contact with the positive electrode 24, and the second microporous film 50 was in contact with the negative electrode 26, as shown in FIG. 3.

[0068] On the other hand, an alkaline electrolyte was prepared, which was an aqueous solution containing an alkali metal hydroxide as a solute and saturated with zinc oxide. This alkaline electrolyte contained 30% by weight of potassium hydroxide as the alkali metal hydroxide.

[0069] Next, the above-mentioned electrode group 22 was placed in a bottomed cylindrical steel exterior can 10 that was entirely tin-plated, and 3.41 mL of the prepared alkaline electrolyte was poured in. Thereafter, the opening of the exterior can 10 was sealed with a sealing body 11, and a 4 / 3FA size battery 2 with a nominal capacity of 2000 mAh was assembled.

[0070] (4) Initial activation process The obtained battery 2 was subjected to one charge-discharge cycle in which a constant current charge of 0.2 A was performed in an environment at a temperature of 25° C. until the charge capacity reached 2400 mAh, followed by a 15-minute pause, and then a constant current discharge of 0.4 A until the battery voltage reached 1.3 V. In this manner, the initial activation process was performed, and the battery 2 was ready for use.

[0071] Example 2 A nickel-zinc secondary battery was manufactured in the same manner as in Example 1, except that the total thickness A of the first microporous film 48 and the second microporous film 50 was 41 μm, the total thickness B of the first nonwoven fabric 44 and the second nonwoven fabric 46 was 124 μm, and the value of A / B was 0.33.

[0072] Example 3 A nickel-zinc secondary battery was produced in the same manner as in Example 1, except that the total thickness A of the first microporous film 48 and the second microporous film 50 was 66 μm, the total thickness B of the first nonwoven fabric 44 and the second nonwoven fabric 46 was 124 μm, and the value of A / B was 0.53.

[0073] Comparative Example 1 A nickel-zinc secondary battery was manufactured in the same manner as in Example 1, except that the total thickness A of the first microporous film 48 and the second microporous film 50 was 70 μm, the total thickness B of the first nonwoven fabric 44 and the second nonwoven fabric 46 was 90 μm, and the value of A / B was 0.78.

[0074] Comparative Example 2 A nickel-zinc secondary battery was produced in the same manner as in Example 1, except that the total thickness A of the first microporous film 48 and the second microporous film 50 was 95 μm, the total thickness B of the first nonwoven fabric 44 and the second nonwoven fabric 46 was 90 μm, and the value of A / B was 1.06.

[0075] Comparative Example 3 A nickel-zinc secondary battery was produced in the same manner as in Example 1, except that a tin-plated copper punched metal (thickness: 60 μm, through-hole diameter: 1.0 mm) was used as the negative electrode core 27 instead of a tin-plated copper non-perforated foil, and the total thickness A of the first microporous film 48 and the second microporous film 50 was 36 μm, the total thickness B of the first nonwoven fabric 44 and the second nonwoven fabric 46 was 124 μm, and the value of A / B was 0.29.

[0076] Comparative Example 4 A nickel-zinc secondary battery was produced in the same manner as in Example 1, except that the total thickness A of the first microporous film 48 and the second microporous film 50 was 34 μm, the total thickness B of the first nonwoven fabric 48 and the second nonwoven fabric 50 was 124 μm, and the value of A / B was 0.27.

[0077] 2. Evaluation of nickel-zinc secondary batteries (1) Cycle life test For each of the batteries of Examples 1 to 3 and Comparative Examples 1 to 4 that had been subjected to the initial activation treatment, constant-current constant-voltage charging was performed in an environment of 35° C. under conditions of a current value of 3.6 A and a sustained voltage value of 1.90 V until the charge capacity reached 960 mAh, and then the charging was paused for 15 minutes. Thereafter, constant-current discharging was performed in the same environment under conditions of a current value of 3.6 A until the battery voltage reached 1.3 V, and then the charging was paused for 15 minutes.

[0078] The above-mentioned charge / discharge cycle was counted as one cycle, and the charge / discharge cycle was repeated 300 times to determine the discharge capacity in each cycle. Here, the discharge capacity in the first charge / discharge cycle was taken as the initial capacity, and the capacity retention rate in each cycle was calculated by the following formula (I). Capacity retention rate [%] = (discharge capacity at each cycle / initial capacity) × 100 (I)

[0079] The number of cycles until the capacity retention rate of each battery reached 90% was counted. The number was taken as the cycle life. The results of the cycle life are shown in Table 1.

[0080] [Table 1]

[0081] (2) Consideration From the results in Table 1, in Examples 1 to 3, the capacity retention rate was maintained at 90% or more at 300 cycles, whereas in Comparative Examples 1 to 4, the capacity retention rate reached 90% at less than 300 cycles. In other words, according to this embodiment, the cycle life characteristics of the nickel-zinc secondary battery are improved. The reason for this improvement in cycle life characteristics can be assumed as follows.

[0082] The causes of the end of the cycle life of nickel-zinc secondary batteries include short circuit caused by zinc dendrite precipitation, and the nickel positive electrode swelling due to deterioration, which causes the separator to dry out, making it impossible to charge and discharge sufficiently. In the above-mentioned embodiment, when the total thickness of the microporous film is A and the total thickness of the nonwoven fabric is B, a separator is used that combines a microporous film and a nonwoven fabric so that the value of A / B is 0.28 to 0.53, which makes it possible to achieve both resistance to short circuit caused by dendrites and suppression of separator dry out. Moreover, by making the negative electrode core into a non-porous foil, the reactivity of the zinc negative electrode is made uniform compared to conventional punching metals, which makes it possible to suppress the growth of zinc dendrites. It is presumed that the cycle life characteristics are improved by the synergistic effect of these factors.

[0083] Even in an embodiment in which the total thickness of the separator is relatively small as in Example 1 described above, the cycle life of the zinc secondary battery can be extended as long as the ratio A / B of the total thickness of the microporous film and nonwoven fabric constituting the separator is within a specific range. Therefore, the present invention is considered to be particularly effective in improving the cycle life characteristics of cylindrical zinc secondary batteries using a wound electrode group in which the thickness of the separator layer is limited to a certain extent due to design.

[0084] The present invention is not limited to the above-mentioned embodiment and examples, and various modifications are possible. For example, the present invention is not limited to nickel-zinc secondary batteries, as long as the negative electrode mixture contains zinc, and can be applied to other zinc secondary batteries that do not use nickel in the positive electrode, such as air-zinc secondary batteries. In addition, the present invention is not limited to cylindrical secondary batteries in which an electrode group is wound, and the same effect of improving cycle life characteristics can be obtained even when used in a rectangular zinc secondary battery including a flat electrode group formed by stacking flat positive and negative electrodes with a separator interposed therebetween. [Explanation of symbols]

[0085] 2. Nickel-zinc secondary battery 22 electrode groups 24 Positive electrode 26 negative electrode 27 Negative electrode core 28 Separator 29 Negative electrode mixture 40 Microporous film 42 Nonwoven fabrics 44 First Nonwoven Fabric 46 Second Nonwoven Fabric 48 First microporous film 50 Second microporous film

Claims

1. A container and an electrode group accommodated in the container together with an alkaline electrolyte, The electrode group is formed by stacking a positive electrode and a negative electrode with a separator interposed therebetween, The negative electrode includes a negative electrode core and a negative electrode mixture held by the negative electrode core, The negative electrode mixture contains at least one of zinc, a zinc alloy, and a zinc-containing compound, The negative electrode core is made of a non-porous sheet-like metal conductor, The separator is a composite in which a nonwoven fabric and a microporous film are laminated in a thickness direction, A zinc secondary battery, wherein the value of A / B is 0.28 or more and 0.53 or less, where A is the total thickness of the microporous film and B is the total thickness of the nonwoven fabric.

2. The zinc secondary battery according to claim 1 , wherein the separator is a composite including a plurality of sheets of the nonwoven fabric and a plurality of sheets of the microporous film.

3. The zinc secondary battery according to claim 2, wherein the composite has a four-layer structure in which the nonwoven fabric and the microporous film are combined in the order of a first nonwoven fabric, a first microporous film, a second nonwoven fabric, and a second microporous film from the positive electrode to the negative electrode.

4. The zinc secondary battery according to claim 1, wherein the total thickness A of the microporous film is 35 μm or more and 66 μm or less.

5. 2. The zinc secondary battery according to claim 1, wherein the metallic conductor is a non-perforated copper foil.