Manufacturing method for injection molded product

By using a mixture of alkaline earth metal carbonate powder and cycloolefin resin at a mold temperature below 30°C, an injection molded product is prepared by solving the problem of difficulty in reducing both -plane retardation and haze in the prior art, and an injection molded product with low haze and low-out-of-plane retardation is achieved.

JP2024141926AInactive Publication Date: 2024-10-10UBE CORPORATION
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023053807
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to effectively reduce the -plane retardation (Re) and haze values ​​of injection molded products while maintaining low -of-plane retardation (Rth).

Method used

Injection molded products were prepared by setting the mold temperature of the injection molding machine to 30°C below the glass transition temperature (Tg) of the cycloolefin resin using a mixture of alkaline earth metal carbonate powder and the cycloolefin resin.

Benefits of technology

A significant reduction in -of-plane retardation (Re) and haze values ​​are achieved while keeping the -of-plane retardation (Rth) low.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141926000001
    Figure 2024141926000001
Patent Text Reader

Abstract

To provide a manufacturing method for manufacturing an injection-molded product having a reduced in-plane retardation (Re) and haze while maintaining a constant range of a low out-of-plane retardation (Rth).SOLUTION: There is provided a method for manufacturing an injection molded product from a resin composition containing an alkaline earth metal carbonate and a cycloolefin resin, where a mold temperature T (°C) of an injection molding machine satisfies the following formula. The formula is T<Tg-30. Herein, Tg is a glass transition temperature (°C) of the cycloolefin resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an injection molded article. [Background technology]

[0002] Cycloolefin resins are amorphous transparent resins with an excellent balance of optical properties and excellent heat resistance, making them suitable optical resins for the manufacture of optical components (see, for example, Non-Patent Document 1). It has been disclosed that optical components are molded using optical resins containing alkaline earth metal carbonate powder in order to suppress the occurrence of birefringence distribution when the optical components are used in a bent state (see, for example, Patent Document 1).

[0003] In order to improve the viewing angle characteristics of an optical component, it is necessary to reduce the out-of-plane retardation (Rth) and the in-plane retardation (Re). Also, the lower the haze calculated from the ratio of diffuse transmitted light to the total light transmission amount, the lower the turbidity and the higher the transparency of the optical component. That is, the lower the values ​​of the out-of-plane retardation (Rth), the in-plane retardation (Re) and the haze, the better the optical component. [Prior art documents] [Patent documents]

[0004] [Non-Patent Document 1] Journal of the Imaging Society of Japan, Vol. 55, No. 2, 236-242 (2016) [Patent Document 1] Patent Publication No. 2021-47402 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a method for producing an injection-molded article having reduced in-plane retardation (Re) and haze while maintaining a low out-of-plane retardation (Rth) within a certain range. [Means for solving the problem]

[0006] The present inventors have conducted studies to solve the above problems, and have found that, when producing an injection-molded article of a cycloolefin resin, by blending an alkaline earth metal carbonate and setting the mold temperature T (°C) of the injection molding machine to a predetermined temperature lower than the glass transition temperature Tg (°C) of the cycloolefin resin, specifically a temperature lower than (Tg-30)°C, it is possible to obtain an injection-molded article with reduced in-plane retardation (Re) and haze while maintaining a low out-of-plane retardation (Rth) within a certain range.

[0007] That is, the present invention is a method for producing an injection-molded article of a resin composition containing an alkaline earth metal carbonate and a cycloolefin-based resin, characterized in that the mold temperature T (°C) of the injection molding machine satisfies the following: T <Tg-30 (Here, Tg is the glass transition temperature (°C) of the cycloolefin resin.) Effect of the Invention

[0008] According to the present invention, it is possible to produce an injection-molded article having reduced in-plane retardation (Re) and haze while maintaining a constant range of low out-of-plane retardation (Rth). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described in detail.

[0010] The method for producing an injection molded article of the present invention uses a resin composition containing an alkaline earth metal carbonate and a cycloolefin resin. The positive intrinsic birefringence of the cycloolefin resin is offset by the addition of the alkaline earth metal carbonate, so that a molded article having a birefringence close to zero can be produced.

[0011] (Alkaline earth metal carbonates) The alkaline earth metal carbonate is mainly composed of alkaline earth metal carbonate in the form of fine powder. The term "main component" means that auxiliary components such as a surface treatment agent may be included in addition to the alkaline earth metal carbonate, and that the alkaline earth metal carbonate is contained in an amount of, for example, 80% by mass or more. Hereinafter, the alkaline earth metal carbonate may be referred to as alkaline earth metal carbonate fine powder. The alkaline earth metal carbonate fine particles have an average major axis within the range of 10 to 100 nm, preferably within the range of 15 to 75 nm. If the average major axis is less than 10 nm, the particles are too small and tend to aggregate, which tends to deteriorate the dispersibility. On the other hand, if the average major axis is more than 100 nm, the particles are too large and tend to deteriorate the transparency when mixed with a resin.

[0012] The alkaline earth metal carbonate fine powder preferably has an aspect ratio (ratio of average major axis / average minor axis) of 1.1 or more, more preferably in the range of 1.2 to 5.0, and particularly preferably in the range of 1.3 to 4.0.

[0013] The average major axis and the average minor axis of the alkaline earth metal carbonate fine powder can be measured by visual inspection or automatic image processing of a SEM (scanning electron microscope) photograph of the alkaline earth metal carbonate fine powder. The major axis of the alkaline earth metal carbonate fine powder can be measured as the length in the longitudinal direction (length of the long side) when the alkaline earth metal carbonate particle is regarded as a rectangle.

[0014] The minor axis of the alkaline earth metal carbonate fine powder can be measured as the length in the short direction (the length of the short side) when the alkaline earth metal carbonate is considered as a rectangle. Specifically, a rectangle that circumscribes the alkaline earth metal carbonate particle in the image and has the smallest area is calculated, and the major axis and minor axis are obtained from the lengths of the major and minor sides. The "average" refers to the average value obtained by measuring the major axis and minor axis of a statistically reliable number (N number) of alkaline earth metal carbonate particles, and the number is usually 100 or more, preferably 300 or more, and more preferably 500 or more.

[0015] The alkaline earth metal carbonate fine powder includes magnesium carbonate fine powder, calcium carbonate fine powder, strontium carbonate fine powder, and barium carbonate fine powder. These alkaline earth metal carbonate fine powders may be used alone or in combination of two or more. The alkaline earth metal carbonate fine powder is preferably strontium carbonate fine powder.

[0016] The alkaline earth metal carbonate fine powder may be further surface-treated with a surfactant. The alkaline earth metal carbonate fine powder surface-treated with a surfactant has improved dispersibility. When the alkaline earth metal carbonate fine powder itself does not require dispersibility, such as when the alkaline earth metal carbonate fine powder is mechanically dispersed during the production of the alkaline earth metal carbonate fine powder-containing resin composition, the alkaline earth metal carbonate fine powder does not need to be surface-treated with a surfactant.

[0017] As the surfactant, a compound having either a hydrophilic group or a hydrophobic group, preferably having a hydrophilic group and a hydrophobic group, and further having a group that forms an anion in water can be used. This compound is preferably a compound in which the hydrophilic group is a polyoxyalkylene group, one end of which is bonded to a hydrophobic group, and the other end of which is bonded to a group that forms an anion in water. The hydrophobic group is preferably an alkyl group or an aryl group, more preferably a phenyl group. The group that forms an anion in water is preferably a carboxylate group, a sulfate group, or a phosphate group.

[0018] The surfactant is preferably a phosphoric acid ester in which the group that forms an anion in water is a phosphoric acid group. Since phosphoric acid esters have higher heat resistance than carboxylates and sulfates, polymer compositions to which alkaline earth metal carbonate fine powders that have been surface-treated with phosphoric acid esters have been added are less likely to be discolored due to thermal decomposition of the surfactant. Examples of phosphoric acid esters include polyoxyethylene styrenated phenyl ether phosphate esters and polyoxyethylene alkyl ether phosphate esters.

[0019] The amount of surfactant attached to the surface of the alkaline earth metal carbonate fine powder is generally in the range of 1 to 40 parts by mass, preferably 3 to 30 parts by mass, per 100 parts by mass of the alkaline earth metal carbonate fine powder. If the amount of surfactant is too small, it may be difficult to obtain the effect of improving dispersibility. On the other hand, if the amount of surfactant is too large, the surfactant may become a foreign matter during the production of a resin composition containing the alkaline earth metal carbonate fine powder, causing a decrease in the visible light transmittance of the resulting resin composition or an increase in haze. The content of the surfactant in the alkaline earth metal carbonate fine powder can be measured, for example, by TG-DTA (thermogravimetric differential thermal analyzer).

[0020] (Method for producing alkaline earth metal carbonate) The method for producing the alkaline earth metal carbonate fine powder is described below. The alkaline earth metal carbonate fine powder can be produced, for example, by a method including a reaction step of reacting an alkaline earth metal hydroxide with carbon dioxide in the presence of a crystal growth inhibitor to produce alkaline earth metal carbonate particles, an aging step of growing the alkaline earth metal carbonate particles into needle-like shapes, a surface treatment step of treating the alkaline earth metal carbonate particles with a surfactant, and a drying step of drying the alkaline earth metal carbonate particles.

[0021] (Reaction process) In the reaction step, it is preferable to introduce carbon dioxide gas into a raw material liquid containing a crystal growth inhibitor and an alkaline earth metal hydroxide while stirring the raw material liquid, thereby carbonating the alkaline earth metal hydroxide to generate alkaline earth metal carbonate particles. The raw material liquid may be an aqueous solution in which an alkaline earth metal hydroxide is dissolved, or an aqueous suspension in which an alkaline earth metal hydrate is dispersed. The concentration of the alkaline earth metal hydroxide in the raw material liquid is not particularly limited, but is usually in the range of 1% by mass to 20% by mass, preferably in the range of 2% by mass to 18% by mass, and more preferably in the range of 3% by mass to 15% by mass.

[0022] The crystal growth inhibitor is a carboxylic acid having a hydroxyl group that adheres to the generated alkaline earth metal carbonate particles and inhibits the crystal growth of the alkaline earth metal carbonate particles. The crystal growth inhibitor is preferably an organic acid having two carboxyl groups and a total of 3 to 6 hydroxyl groups and dicarboxylic acids. Dicarboxylic acids or anhydrides thereof containing one or more hydroxyl groups in the molecule are more preferable. The crystal growth inhibitor may be a monomer that is a raw material for the optical resin to which the alkaline earth metal carbonate fine powder is added. The content of the crystal growth inhibitor in the raw material liquid is generally in the range of 0.1 to 20 parts by mass, preferably 1 to 10 parts by mass, per 100 parts by mass of the hydroxide of the alkaline earth metal.

[0023] The temperature of the raw material liquid is preferably within a range of 5° C. to 60° C. The flow rate of carbon dioxide gas introduced into the raw material liquid is generally within a range of 0.5 mL / min to 200 mL / min, preferably 0.5 mL / min to 100 mL / min, per 1 g of alkaline earth metal hydroxide.

[0024] The particle shape of the alkaline earth metal carbonate particles produced in the reaction step is not particularly limited and may be granular or acicular. The particle shape and size of the alkaline earth metal carbonate particles can be adjusted by conditions such as the liquid temperature of the raw material liquid, the concentrations of the alkaline earth metal hydroxide and monomer in the raw material liquid, and the flow rate of carbon dioxide gas introduced into the raw material liquid. When the alkaline earth metal carbonate particles produced in the reaction step are acicular, the following aging step may be omitted.

[0025] (ripening process) In the aging step, the aqueous suspension of alkaline earth metal carbonate particles obtained in the reaction step is preferably heated and aged at a temperature in the range of 75°C to 115°C to grow the alkaline earth metal carbonate particles into needle-like particles. If the heating temperature is less than 75°C, the crystal growth of the long axis of the alkaline earth metal carbonate particles is insufficient, and the average aspect ratio tends to be low. On the other hand, if the heating temperature exceeds 115°C, the crystal growth of the short axis of the alkaline earth metal carbonate particles is promoted, and the aspect ratio tends to be low. The heating temperature is preferably in the range of 80°C to 110°C, and particularly preferably in the range of 85°C to 105°C. Heat aging is preferably performed while stirring. The heating time is not particularly limited, but is usually in the range of 1 hour to 100 hours, preferably in the range of 5 hours to 50 hours, and particularly preferably in the range of 10 hours to 30 hours.

[0026] (Surface treatment process) In the surface treatment step, it is preferable to add a surfactant to the slurry of acicular alkaline earth metal carbonate particles obtained in the aging step, and treat the surfaces of the alkaline earth metal carbonate particles with the surfactant to obtain an aqueous slurry of highly dispersible acicular alkaline earth metal carbonate particles. After adding the surfactant to the slurry, it is preferable to stir the slurry to make the concentration of the surfactant uniform, and then apply shear force to the slurry. By applying shear force to break up the aggregated particles of the alkaline earth metal carbonate particles, it is possible to uniformly treat the surfaces of the alkaline earth metal carbonate particles (primary particles) with the surfactant. The amount of surfactant added to the slurry is generally in the range of 1 part by mass to 40 parts by mass, preferably 3 parts by mass to 30 parts by mass, relative to 100 parts by mass of the alkaline earth metal carbonate particles in the slurry.

[0027] (drying process) In the drying step, the aqueous slurry of highly dispersible acicular alkaline earth metal carbonate particles obtained in the surface treatment step is dried to obtain an alkaline earth metal carbonate. The drying step can be carried out by a known drying method using a dryer such as a spray dryer or a drum dryer.

[0028] (Cycloolefin resin) Cycloolefin resins are polymers having an alicyclic structure in their structural units. Cycloolefin resins are polymers having an alicyclic structure in the main chain, polymers having an alicyclic structure in the side chain, polymers having alicyclic structures in the main chain and the side chain, and mixtures of two or more of these in any ratio. Among these, polymers having an alicyclic structure in the main chain are preferred from the viewpoint of mechanical strength and heat resistance.

[0029] Examples of the alicyclic structure include saturated alicyclic hydrocarbon (cycloalkane) structure and unsaturated alicyclic hydrocarbon (cycloalkene, cycloalkyne) structure. Among these, from the viewpoint of mechanical strength and heat resistance, cycloalkane structure and cycloalkene structure are preferred, and cycloalkane structure is particularly preferred. In addition, cycloolefin copolymers having alicyclic structure and aliphatic structure can also be used suitably.

[0030] The number of carbon atoms constituting the alicyclic structure is preferably 4 or more and 30 or less per alicyclic structure. When the number of carbon atoms constituting the alicyclic structure is within this range, the molded product has a good balance of mechanical strength, heat resistance, and moldability. The number of carbon atoms constituting the alicyclic structure is more preferably 5 or more, particularly preferably 6 or more, more preferably 20 or less, particularly preferably 15 or less per alicyclic structure.

[0031] In the cycloolefin resin, the ratio of the structural unit having an alicyclic structure is preferably 50% by weight or more. When the ratio of the structural unit having an alicyclic structure in the cycloolefin resin is within this range, the transparency and heat resistance of the molded product are good. The ratio of the structural unit having an alicyclic structure is more preferably 70% by weight or more, and particularly preferably 90% by weight or more.

[0032] Specific examples of the cycloolefin resin include norbornene polymers, monocyclic olefin polymers, cyclic conjugated diene polymers, vinyl alicyclic hydrocarbon polymers, and hydrogenated products thereof. Among these, norbornene polymers and hydrogenated products thereof are more preferred from the viewpoints of transparency and moldability.

[0033] Examples of norbornene-based polymers include ring-opening polymers of monomers having a norbornene structure and their hydrogenated products; addition polymers of monomers having a norbornene structure and their hydrogenated products. Examples of ring-opening polymers of monomers having a norbornene structure include ring-opening homopolymers of one type of monomer having a norbornene structure, ring-opening copolymers of two or more types of monomers having a norbornene structure, and ring-opening copolymers of a monomer having a norbornene structure and any monomer that can be copolymerized therewith.

[0034] Further, examples of the addition polymer of a monomer having a norbornene structure include an addition homopolymer of one type of monomer having a norbornene structure, an addition copolymer of two or more types of monomers having a norbornene structure, and an addition copolymer of a monomer having a norbornene structure and any monomer copolymerizable therewith. Examples of these polymers include the polymers disclosed in JP-A-2002-321302 and the like. Among these, the hydrogenated product of a ring-opening polymer of a monomer having a norbornene structure is particularly suitable from the viewpoints of transparency, moldability, heat resistance, low moisture absorption, dimensional stability, and light weight. Specific examples of cycloolefin resins include "ARTON" (registered trademark) manufactured by JSR Corporation; "APEL" (registered trademark) manufactured by Mitsui Chemicals, Inc.; and "TOPAS" manufactured by TOPAS ADVANCED POLYMERS.

[0035] The number average molecular weight of the cycloolefin resin, in terms of polystyrene, measured by GPC (gel permeation chromatography) using a toluene solvent, is 10,000 to 200,000, preferably 15,000 to 100,000, and more preferably 20,000 to 50,000. The glass transition temperature of the cycloolefin resin is preferably 80° C. or higher, and more preferably 100 to 250° C.

[0036] A molded article is manufactured by injection molding using a resin composition obtained by mixing the above-mentioned cycloolefin resin and alkaline earth metal carbonate powder. The content of the alkaline earth metal carbonate powder in the entire resin composition can be within a range of 0.5 to 2 parts by mass, preferably 0.5 to 1 part by mass, per 100 parts by mass of the cycloolefin resin. This makes it possible to manufacture an injection molded article with reduced in-plane retardation (Re) and haze while maintaining a constant low out-of-plane retardation (Rth).

[0037] In the manufacture of injection molded products, first, the alkaline earth metal carbonate powder and the cycloolefin resin are mixed in a predetermined ratio and premixed, and strands are produced using a twin-screw extruder. The kneading temperature can be, for example, 180 to 210°C, and the diameter of the strands can be 1 to 2 mm. Then, pellets having a length of 2 to 4 mm are produced from the strands using a pelletizer.

[0038] The obtained pellets are put into an injection molding machine and injection molded at a predetermined mold temperature to obtain a molded product. In the present invention, the temperature of the mold surface into which the resin flows in the injection molding machine is referred to as the mold temperature T. The mold temperature can generally be controlled to a predetermined temperature by setting the temperature of the injection molding machine itself.

[0039] In the present invention, the mold temperature T is lower than the glass transition temperature (Tg) of the cycloolefin resin and is specified to be less than (Tg-30)°C. This makes it possible to obtain a molded product with low in-plane retardation (Re) and low haze. The glass transition temperature Tg is measured by differential scanning calorimetry (DSC). Differential scanning calorimetry is a method in which the temperature of a reference material and a sample are measured while the sample temperature is changed according to a program, and the amount of heat is measured from the temperature difference. The glass transition temperature is obtained from the DSC curve obtained by the measurement. The mold temperature T is preferably 80°C or less, more preferably 50°C or less. The lower limit of the mold temperature is determined by the glass transition temperature Tg, and is generally (Tg-15 to Tg-3)°C.

[0040] For example, when using a cycloolefin resin having a glass transition temperature Tg of 135° C., the mold temperature T of the injection molding machine is set to less than 105° C. In this case, the mold temperature T is preferably 40 to 100° C., more preferably 50 to 100° C., further preferably 50 to 80° C., and particularly preferably 50 to 60° C.

[0041] The temperature of the resin before being introduced into the mold for injection molding is not particularly limited, and can be, for example, 260 to 300° C. Furthermore, the molded product can be, for example, a resin plate having a length of 20 to 30 mm, a width of 20 to 30 mm, and a thickness of 1 to 2 mm.

[0042] In the present invention, when an injection-molded article is produced from a resin composition containing an alkaline earth metal carbonate powder and a cycloolefin-based resin, the mold temperature T of the injection molding machine is set to a temperature lower than the glass transition temperature Tg of the cycloolefin-based resin, and the temperature difference is set to be greater than 30°C. This makes it possible to produce an injection-molded article with reduced in-plane retardation (Re) and haze while maintaining a low out-of-plane retardation (Rth) within a certain range.

[0043] The injection molded article produced by the method of the present invention can be effectively used as an optical component such as an optical resin lens, a camera module for a smartphone, or a cover sheet for an in-vehicle display.

[0044] The following supplementary notes are further disclosed regarding the above-described embodiment of the present invention.

[0045] <1> A method for producing an injection-molded article of a resin composition containing an alkaline earth metal carbonate and a cycloolefin resin, comprising the steps of: A method for producing an injection-molded product, in which the mold temperature T of the injection molding machine is lower than the glass transition temperature (Tg) of the cycloolefin resin by 30°C, and is 50 to 100°C. <2> The mold temperature T is 50 to 80° C. <1> A method for producing the injection molded article described above. <3> The content of the alkaline earth metal carbonate is 0.5 to 2 parts by mass per 100 parts by mass of the cycloolefin resin. <1> or <2> A method for producing the injection molded article described above. <4> The alkaline earth metal carbonate includes strontium carbonate. <1> ~ <3> 13. The method for producing an injection molded article according to any one of claims 1 to 12. <5> The cycloolefin resin is a cycloolefin copolymer. <1> ~ <4> 13. The method for producing an injection molded article according to any one of claims 1 to 12. <6> The injection molded product is an optical member. <1> ~ <5> 13. A method for manufacturing an injection-processed product according to any one of the preceding claims. <7> A resin composition used for producing an injection-molded article obtained by injection molding at a mold temperature of an injection molding machine lower than the glass transition temperature (Tg) of a cycloolefin resin −30° C., The resin composition contains an alkaline earth metal carbonate and a cycloolefin resin, and the content of the alkaline earth metal carbonate is 0.5 to 2 parts by mass per 100 parts by mass of the cycloolefin resin. EXAMPLES

[0046] Next, the present invention will be specifically described with reference to examples, but the present invention is not limited to the following examples.

[0047] As the alkaline earth metal carbonate powder, fine powder of strontium carbonate was prepared. (Manufacturing strontium carbonate fine powder) (a) Reaction process 2440g of strontium hydroxide octahydrate (special grade reagent, purity: 96% or more) was added to 20L of pure water at a water temperature of 10°C, and mixed to prepare an aqueous suspension of strontium hydroxide with a concentration of 5.6% by mass. DL-tartaric acid (special grade reagent, purity: 99% or more) was added to this aqueous suspension of strontium hydroxide, and stirred to dissolve in the aqueous suspension. Next, while maintaining the liquid temperature of the aqueous suspension of strontium hydroxide at 10°C and continuing stirring, carbon dioxide gas was blown into the aqueous suspension at a flow rate of 3.3L / min (flow rate of 3mL / min per 1g of strontium hydroxide) until the pH of the aqueous suspension reached 7, generating strontium carbonate particles. Then, stirring was continued for another 30 minutes to obtain an aqueous suspension of strontium carbonate particles.

[0048] (b) Aging process The obtained aqueous suspension of strontium carbonate particles was placed in a stainless steel tank and heated at 80° C. for 24 hours to grow the strontium carbonate particles into needle-like shapes, and then allowed to cool to room temperature to produce an aqueous slurry of strontium carbonate particles.

[0049] (c) Surface treatment and drying process 3,500 g of an aqueous strontium carbonate particle slurry (concentration: 5.8% by mass) was charged into a homomixer (T.K. Homomixer Mark II, manufactured by Primix Corporation), and while rotating the stirring blades of the homomixer at a peripheral speed of 7.85 m / s and stirring, 56.8 g (28 parts by mass with respect to 100 parts by mass of strontium carbonate particles) of polyoxyethylene styrenated phenyl ether phosphate ester was added to the aqueous slurry and dissolved. Thereafter, stirring and mixing were continued for 1 hour. The aqueous slurry after stirring and mixing was dried to obtain surface-treated strontium carbonate fine powder (A-1). As a result of observing the obtained strontium carbonate fine powder with an electron microscope, it was confirmed that it was a fine powder of needle-like particles (average major axis: 60 nm).

[0050] As the cycloolefin-based resin, a cycloolefin copolymer resin (Cycloolefin Copolymer APL5014CL, manufactured by Mitsui Chemicals) was prepared. The glass transition temperature Tg of the cycloolefin-based resin used here was 135°C.

[0051] (Example 1) A resin composition containing 1 part by mass of strontium carbonate powder and 100 parts by mass of cycloolefin copolymer resin was prepared, and a molded article was manufactured by injection molding using this. Specifically, first, 100 g of strontium carbonate powder and 10,000 g of cycloolefin copolymer resin (APL5014CL) were preliminarily mixed, and using a twin-screw extruder (manufactured by Berstorff), strands with a diameter of 2 mm were produced at a kneading temperature of 195°C. Thereafter, using a pelletizer, pellets with a length of 3 mm were produced from this strand.

[0052] The obtained pellets were charged into an injection molding machine manufactured by Mayho Co., Ltd., and injection molding was performed under the conditions of a resin temperature of 260°C and a mold temperature of 50°C to manufacture the injection molded article of Example 1 (a resin plate with a length of 30 mm × a width of 30 mm × a thickness of 1 mm). The mold temperature is the temperature of the mold surface into which the resin flows in the injection molding machine, and was controlled to a predetermined temperature by setting the temperature of the injection molding machine main body. In this example, the mold temperature T (°C) satisfies (T < Tg - 30).

[0053] (Example 2) An injection-molded product of Example 2 was obtained in the same manner as in Example 1, except that the compounding amount of strontium carbonate powder was changed to 2 parts by mass without changing the compounding amount of the cycloolefin resin. In this example, the mold temperature T (°C) satisfies (T < Tg - 30).

[0054] (Example 3) An injection-molded product of Example 3 was obtained in the same manner as in Example 1, except that the mold temperature of the injection molding machine was changed to 80°C.

[0055] (Example 4) An injection-molded product of Example 4 was obtained in the same manner as in Example 2, except that the mold temperature of the injection molding machine was changed to 80°C.

[0056] (Comparative Example 1) A injection-molded product of Comparative Example 1 was obtained in the same manner as in Example 1, except that the mold temperature of the injection molding machine was changed to 120°C. The mold temperature T (°C) is (T ≥ Tg - 30).

[0057] The physical properties of the injection-molded products of the examples and comparative examples were examined as follows. Haze: Measured using a spectrophotometer (NDH4000, manufactured by Nippon Denshoku Industries Co., Ltd.). Birefringence (ΔNxy, ΔP): Using a phase measuring device (KOBRA-WR, manufactured by Oji Scientific Instruments Co., Ltd.), the in-plane retardation Re and the out-of-plane retardation (retardation in the thickness direction / retardation in the thickness direction) Rth were measured.

[0058] The above phase measuring device measures the in-plane retardation R 0 with light perpendicularly incident on the measurement object (plate), and the retardation R θThe out-of-plane retardation Rth is calculated from the thickness d (input value) of the object to be measured and the average refractive index Navr (input value) of the object to be measured. Here, in the examples and comparative examples described in this specification, the out-of-plane retardation Rth is defined by a value for light having a wavelength of 587.3 nm. The smaller the value, the lower the birefringence.

[0059] The results obtained are summarized in the table below, together with the resin composition and injection conditions.

[0060] [Table 1]

[0061] As shown in the table above, if the mold temperature T (℃) of the injection molding machine is (T <tg-30)を満たす場合には、一定範囲の低い面外位相差(rth)を維持しつつ、面内位相差(re)およびヘイズも低い成形品が得られている。In contrast, when the mold temperature T (℃) of the injection molding machine is (T≧Tg-30), although the out-of-plane retardation (Rth) is −2.69, it is not possible to obtain a molded product with low in-plane retardation (Re) and haze.< / tg-30)を満たす場合には、一定範囲の低い面外位相差(rth)を維持しつつ、面内位相差(re)およびヘイズも低い成形品が得られている。

Claims

[Claim 1] A method for producing an injection-molded article of a resin composition containing an alkaline earth metal carbonate and a cycloolefin resin, comprising the steps of: A method for producing an injection molded product, characterized in that the mold temperature T (°C) of an injection molding machine satisfies the following: T<Tg-30 (Here, Tg is the glass transition temperature (°C) of the cycloolefin resin.)

Citation Information

Patent Citations

  • Optical member and image display device

    JP2021047402A

  • JP2236-242