Laminate, image display device and adhesive sheet
The laminate with a tailored adhesive layer using an acrylic copolymer addresses the impact resistance issues of organic EL panels in mobile terminals, ensuring effective shock absorption and protection against drops.
Patent Information
- Application Number
- JP2023053921
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Mobile terminals with organic EL panels face significant impact resistance issues due to their thin and delicate construction, lacking sufficient protection against drops and shocks, which conventional adhesive technologies do not adequately address.
A laminate structure is developed with a specific adhesive layer composed of an acrylic copolymer, where the storage modulus of the first member is lower than the second member, and the adhesive layer is designed to withstand impacts by maintaining a maximum pressure of 18 MPa or less and compressive displacement of 8 mm, using impact analysis software to optimize shock absorption.
The laminate provides excellent impact resistance, effectively protecting organic EL panels by mitigating shock and preventing damage, suitable for various image display devices including organic EL displays.
Smart Images

Figure 2024141996000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate, an image display device, and a pressure-sensitive adhesive sheet. [Background technology]
[0002] In order to improve the visibility of image display devices, the gap between an image display panel such as a liquid crystal display (LCD), a plasma display panel (PDP) or an electroluminescence display (ELD) and a protective panel or a touch panel member placed on the front side (viewing side) of the image display panel is filled with a resin such as an adhesive or bonding agent to suppress reflection of incident light and outgoing light from the displayed image at the air layer interface.
[0003] For example, Patent Document 1 discloses a method for manufacturing a component laminate for an image display device having an image display device component laminated on at least one side of a transparent double-sided adhesive sheet, in which an adhesive sheet that has been primarily crosslinked by ultraviolet light is attached to the image display device component, and then the adhesive sheet is irradiated with ultraviolet light through the image display device component for secondary curing.
[0004] Furthermore, Patent Document 2 discloses a pressure-sensitive adhesive sheet containing a (meth)acrylic copolymer having an ultraviolet-crosslinkable site, as an adhesive sheet useful for displays and touch panels. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 4971529 [Patent Document 2] Patent No. 6062740 Summary of the Invention [Problem to be solved by the invention]
[0006] It is important that mobile devices such as smartphones and tablet computers have high resistance to drops and shocks. In recent years, with the need for these mobile devices to be more energy-efficient, lightweight, and slim, organic electroluminescence (EL) panels are becoming more and more popular as image display panels, replacing conventional LCD panels. In addition, it is expected that the demand for OLED panels will increase dramatically in a wide range of sizes and applications, not only for the above mobile devices, but also for a wider range of everyday uses, such as digital signage for exhibitions. Although organic EL displays require fewer components than LCD panels, they are prone to breakage when subjected to impact. In addition, the surface protection materials used for image display devices are becoming thinner, resulting in fewer screen protectors. Such problems become more pronounced as image display devices become thinner and higher definition, and pressure-sensitive adhesive layers used to bond component parts of image display devices are increasingly required to have impact resistance that absorbs impact even when it is applied to the laminate after the components are bonded together, and prevents damage to the components.
[0007] The inventions described in the cited documents 1 and 2 are directed to laminates using conventional components of image display devices, and no consideration is given to impact resistance.
[0008] In view of the above circumstances, an object of the present invention is to provide a laminate having excellent impact resistance and an image display device using the same. [Means for solving the problem]
[0009] That is, the present invention has the following aspects. [1] A laminate comprising a first member and a second member via a pressure-sensitive adhesive layer, The storage modulus (E1) of the first member is lower than the storage modulus (E2) of the second member, The pressure-sensitive adhesive layer is a pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition (I) containing an acrylic copolymer (A), and the maximum pressure acting on a first member, as determined by the following impact analysis program (1) using impact analysis software, is 18 MPa or less. <Impact Analysis Program (1)> (Analysis model) A model including a test specimen, an impactor for impacting the test specimen, and a support for placing the test specimen. (Test specimen) A laminate in which a first member, a pressure-sensitive adhesive layer, and a second member are laminated in this order. (Setting physical properties) (1) Test specimen First component Thickness: 120μm Elastic modulus: 5GPa Poisson's ratio: 0.2 Material model: Elastic body model Second component Thickness: 560μm Elastic modulus: 70GPa Poisson's ratio: 0.2 Material model: Elastic body model Adhesive layer Thickness: 50~100μm Poisson's ratio: 0.493 Material model: Hyperelastic material model (2) Support stand Thickness: 1000μm Elastic modulus: 75GPa Poisson's ratio: 0.2 Material model: Elastic body model (3) Impactor Ball material: Iron Weight: 0.5kg (4) Test conditions Impactor drop height: 30cm (natural fall; initial velocity 0) Impactor drop surface: Second component surface Test temperature: 25℃ [2] A laminate comprising a first member and a second member disposed on the first member via a pressure-sensitive adhesive layer, The storage modulus (E1) of the first member is lower than the storage modulus (E2) of the second member, The pressure-sensitive adhesive layer is a pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition (I) containing an acrylic copolymer (A), and the compressive displacement of the first member is less than 8 mm, as determined by the following impact analysis program (2) using impact analysis software. 3 The laminate is as follows: <Impact Analysis Program (2)> (Analysis model) A model including a test specimen, an impactor for impacting the test specimen, and a support for placing the test specimen. (Test specimen) A laminate in which a first member, a pressure-sensitive adhesive layer, and a second member are laminated in this order. (Setting physical properties) (1) Test specimen First component Thickness: 120μm Elastic modulus: 5GPa Poisson's ratio: 0.2 Material model: Elastic body model Second component Thickness: 560μm Elastic modulus: 70GPa Poisson's ratio: 0.2 Material model: Elastic body model Adhesive layer Thickness: 50~100μm Poisson's ratio: 0.493 Material model: Hyperelastic material model (2) Support stand Thickness: 1000μm Elastic modulus: 75GPa Poisson's ratio: 0.2 Material model: Elastic body model (3) Impactor Ball material: Iron Weight: 0.5kg (4) Test conditions Impactor drop height: 30cm (natural fall; initial velocity 0) Impactor drop surface: Second component surface Test temperature: 25℃ [3] The laminate according to [1] or [2], wherein the pressure-sensitive adhesive layer has a storage shear modulus (G'(25)) at 25°C obtained by dynamic viscoelastic measurement in a shear mode at a frequency of 1 Hz of 5 kPa or more and 100 kPa or less. [4] The laminate according to any one of [1] to [3], wherein the pressure-sensitive adhesive layer has a gel fraction of 30% or more and 95% or less. [5] The laminate described in any one of [1] to [4], wherein the pressure-sensitive adhesive layer has a glass transition temperature (Tg) of -20°C or higher, defined as the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz. [6] The laminate according to any one of [1] to [5], wherein the pressure-sensitive adhesive composition (I) contains a radically polymerizable compound (B) and a photopolymerization initiator (C). [7] The laminate according to [6], wherein the photopolymerization initiator (C) includes a photopolymerization initiator (C1) having, in its molecule, a radical-polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals. [8] The laminate according to any one of [1] to [7], wherein the thickness of the laminate is 1000 μm or less. [9] The laminate according to any one of [1] to [8], wherein the first member and the second member are components of an image display device selected from the group consisting of a surface protection panel, a touch sensor, an image display panel, a color filter, a polarizing film, and a retardation film.
[10] The laminate according to [9], wherein the first member is an image display panel and the second member is a surface protection panel.
[11] An image display device comprising the laminate according to [9] or
[10] .
[12] An adhesive sheet for bonding together a first member and a second member having a storage modulus (E') higher than that of the first member, the maximum pressure acting on the first member being 18 MPa or less as calculated by the following impact analysis program (1). <Impact Analysis Program (1)> (Analysis model) A model including a test specimen, an impactor for impacting the test specimen, and a support for placing the test specimen. (Test specimen) A laminate in which a first member, a pressure-sensitive adhesive layer, and a second member are laminated in this order. (Setting physical properties) (1) Test specimen First component Thickness: 120μm Elastic modulus: 5GPa Poisson's ratio: 0.2 Material model: Elastic body model Second component Thickness: 560μm Elastic modulus: 70GPa Poisson's ratio: 0.2 Material model: Elastic body model Adhesive layer Thickness: 50~100μm Poisson's ratio: 0.493 Material model: Hyperelastic material model (2) Support stand Thickness: 1000μm Elastic modulus: 75GPa Poisson's ratio: 0.2 Material model: Elastic body model (3) Impactor Ball material: Iron Weight: 0.5kg (4) Test conditions Impactor drop height: 30cm (natural fall; initial velocity 0) Impactor drop surface: Second component surface Test temperature: 25℃ Effect of the Invention
[0010] The laminate of the present invention has a pressure-sensitive adhesive layer that exerts a maximum pressure on a member when an impact is applied thereto of 18 MPa or less, as calculated by a predetermined impact analysis method. Also, the laminate of the present invention has a pressure-sensitive adhesive layer that exerts a maximum pressure on a member when an impact is applied thereto of 18 MPa or less, as calculated by a predetermined impact analysis method. 3 The adhesive layer is as follows: Therefore, the adhesive layer has excellent impact resistance and can be suitably used for image display devices, particularly organic EL image display devices. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 shows a diagram for explaining an impact test model used in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] An example of an embodiment of the present invention will be described in detail below. However, the present invention is not limited to the embodiment described below. In the present invention, the term "film" conceptually includes a sheet, a film, and a tape. Furthermore, when the term "panel" is used, such as an image display panel or a protective panel, it encompasses a plate, a sheet, and a film.
[0013] In the present invention, when it is described as "x to y" (x and y are any numbers), unless otherwise specified, it includes the meaning of "greater than x and less than y", as well as "preferably greater than x" or "preferably smaller than y". In addition, when it is stated that the amount is "x or more" (where x is any number), it also means that the amount is "preferably greater than x" unless otherwise specified, and when it is stated that the amount is "y or less" (where y is any number), it also means that the amount is "preferably smaller than y" unless otherwise specified. Furthermore, "x and / or y (x and y are optional configurations)" means at least one of x and y, and means three possibilities: x only, y only, and x and y. In the present invention, "(meth)acrylic" means acryl and methacryl inclusively, "(meth)acrylate" means acrylate and methacrylate inclusively, and "(meth)acryloyl" means acryloyl and methacryloyl inclusively. In the present invention, the term "main component" refers to a component that has a significant effect on the properties of the material, and the content of the component is usually 40 mass % or more of the entire material, preferably 50 mass % or more, more preferably 60 mass % or more, and particularly preferably 70 mass % or more.
[0014] A laminate according to one embodiment of the present invention (hereinafter referred to as "the laminate 1") is a laminate comprising a first member and a second member via a pressure-sensitive adhesive layer, wherein the storage modulus (E1) of the first member is lower than the storage modulus (E2) of the second member, the pressure-sensitive adhesive layer is a pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition (I) containing an acrylic copolymer (A), and the maximum pressure acting on the first member, as determined by an impact analysis program (1) described below using impact analysis software, is 18 MPa or less. Furthermore, a laminate according to another embodiment of the present invention (hereinafter referred to as "the present laminate 2") is a laminate comprising a first member and a second member via a pressure-sensitive adhesive layer, wherein the storage modulus (E1) of the first member is lower than the storage modulus (E2) of the second member, the pressure-sensitive adhesive layer is a pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition (I) containing an acrylic copolymer (A), and the compression displacement of the first member is less than 8 mm as determined by an impact analysis program (2) described later using impact analysis software. 3 The following is the result. Hereinafter, the present laminate 1 and the present laminate 2 (hereinafter sometimes simply referred to as "the present laminate") will be described.
[0015] [First member, second member] The first member used in this laminate has a storage modulus (E1) lower than the storage shear modulus (E2) of the second member.
[0016] The storage modulus (E1) of the first member is usually 0.5 to 250 GPa, preferably 1 to 200 GPa, and particularly preferably 2 to 100 GPa. The storage modulus (E2) of the second member is higher than the storage modulus (E1) of the first member, and is usually 30 to 500 GPa, preferably 40 to 300 GPa, and particularly preferably 50 to 200 GPa.
[0017] The difference between the storage modulus (E2) of the second member and the storage modulus (E1) of the first member [(E2)-(E1)] is usually 5 to 400 GPa, preferably 10 to 200 GPa, and particularly preferably 20 to 100 GPa.
[0018] The storage moduli (E1) and (E2) can be determined, for example, by measuring the storage modulus at 20°C using a viscoelasticity spectrometer "DVA-200 (manufactured by IT Measurement & Control Co., Ltd.)" in accordance with an ultrasonic pulse method (JIS R1602:1995) or JIS K 7244-4:1999 (measurement mode: tension, frequency: 10 Hz, strain: 0.1%, temperature range: -100 to 300°C, heating rate: 3°C / min).
[0019] The first member and the second member are preferably those used as components of an image display device, such as a component of a flat panel image display device, a component of an image display device having a curved portion, a component of a flexible image display device, etc. In other words, the present laminate is preferably for use in constituting an image display device. Specific examples of the first and second members include liquid crystal displays, organic electroluminescence (EL) displays, surface protection panels (surface protection films), polarizing plates, polarizers, retardation films, barrier films, viewing angle compensation films, brightness improvement films, contrast improvement films, diffusion films, semi-transparent reflective films, electrode films, transparent conductive films, metal mesh films, and touch sensor films. The first and second members may be selected from two of these so that the storage modulus (E1) of the first member is lower than the storage modulus (E2) of the second member. Among these, the first and second members are preferably image display device components selected from the group consisting of surface protection panels, touch sensors, image display panels, color filters, polarizing films, and retardation films, and it is particularly preferable that the first member is an image display panel and the second member is a surface protection panel.
[0020] The thickness of the first member and the second member is usually 10 to 250 μm, preferably 25 to 200 μm, and particularly preferably 35 to 190 μm.
[0021] [Adhesive Layer] The pressure-sensitive adhesive layer included in this laminate 1 has a maximum pressure acting on the first member of 18 MPa or less, as determined by the following impact analysis program (1) using LS-DYNA (impact analysis software) manufactured by Ansys. The pressure-sensitive adhesive layer of the laminate 2 has a compressive displacement of 8 mm on the first member, which is calculated by the following impact analysis program (2) using LS-DYNA (impact analysis software) manufactured by Ansys, Inc. 3 The following is the result.
[0022] <Impact Analysis Program (1)> (Analysis model) A model including a test specimen, an impactor for impacting the test specimen, and a support for placing the test specimen. (Test specimen) A laminate in which a first member, a pressure-sensitive adhesive layer, and a second member are laminated in this order. (Setting physical properties) (1) Test specimen First component Thickness: 120μm Elastic modulus: 5GPa Poisson's ratio: 0.2 Material model: Elastic body model Second component Thickness: 560μm Elastic modulus: 70GPa Poisson's ratio: 0.2 Material model: Elastic body model Adhesive layer Thickness: 50~100μm Poisson's ratio: 0.493 Material model: Hyperelastic material model (2) Support stand Thickness: 1000μm Elastic modulus: 75GPa Poisson's ratio: 0.2 Material model: Elastic body model (3) Impactor Ball material: Iron Weight: 0.5kg (4) Test conditions Impactor drop height: 30cm (natural fall; initial velocity 0) Impactor drop surface: Second component surface Test temperature: 25℃
[0023] <Impact Analysis Program (2)> (Analysis model) A model including a test specimen, an impactor for impacting the test specimen, and a support for placing the test specimen. (Test specimen) A laminate in which a first member, a pressure-sensitive adhesive layer, and a second member are laminated in this order. (Setting physical properties) (1) Test specimen First component Thickness: 120μm Elastic modulus: 5GPa Poisson's ratio: 0.2 Material model: Elastic body model Second component Thickness: 560μm Elastic modulus: 70GPa Poisson's ratio: 0.2 Material model: Elastic body model Adhesive layer Thickness: 50~100μm Poisson's ratio: 0.493 Material model: Hyperelastic material model (2) Support stand Thickness: 1000μm Elastic modulus: 75GPa Poisson's ratio: 0.2 Material model: Elastic body model (3) Impactor Ball material: Iron Weight: 0.5kg (4) Test conditions Impactor drop height: 30cm (natural fall; initial velocity 0) Impactor drop surface: Second component surface Test temperature: 25℃
[0024] Normally, when a laminate made of two bonded components receives an impact, the impact extends to the component behind the impacted surface (collision surface), and there is a risk that even the surface that is not directly impacted may be damaged. Therefore, the inventors conducted various analytical studies to maximize the impact energy absorbing effect of the adhesive layer in a laminate in which two components are bonded together via an adhesive layer, and found that the impact energy absorbing effect of the adhesive layer can be maximized by setting the maximum pressure acting on the components or the compressive displacement on the components to a specific range. The impact energy absorbing effect of the pressure-sensitive adhesive layer is caused by shock waves traveling in various directions which interfere with each other on the component and become a composite wave, making it difficult to quantitatively isolate the contributing factors; however, qualitatively, it is thought to be manifested by the following mechanism. When the laminate receives an impact, it bends vertically around the impact point, and the impact energy is absorbed by the vertical deformation (vertical impact absorption). In addition, by transmitting the impact energy in the in-plane direction, the stress concentration is reduced and the energy is dispersed over a wide area, which is expected to have the effect of mitigating the impact energy (impact mitigation in the in-plane direction). The lower the storage modulus of the pressure-sensitive adhesive layer, the greater the contribution to impact absorption in the perpendicular direction. On the other hand, the higher the storage modulus of the pressure-sensitive adhesive layer, the greater the contribution to impact absorption in the in-plane direction. Therefore, in order to enjoy a high impact absorption effect, the pressure-sensitive adhesive layer of the present laminate needs to have an optimal storage modulus range taking into account the above-mentioned contradictory phenomena. As a result of intensive research under these circumstances, we discovered that there is an optimal range in which the impact energy can be minimized. We also discovered that by satisfying the requirements of this analysis program, it is possible to create a laminate with excellent impact resistance based on the above-mentioned mechanism.
[0025] The pressure-sensitive adhesive layer of the present laminate 1 has a maximum pressure acting on the first member of 18 MPa or less, preferably 17 MPa or less, and particularly preferably 16 MPa or less, as determined by the above-mentioned impact analysis program (1). By setting the maximum pressure acting on the first member within the above range, the present laminate 1 has excellent impact resistance.
[0026] In addition, the pressure-sensitive adhesive layer of the present laminate 2 has a compressive displacement of 8 mm to the first member, as determined by the impact analysis program (2). 3 Less than or equal to 7 mm, preferably3 Less than 6 mm, especially preferred 3 By setting the compressive displacement of the first member within the above range, the present laminate 2 has excellent impact resistance.
[0027] Such a pressure-sensitive adhesive layer in which the maximum pressure acting on the first member is within a specific range as determined by the impact analysis program (1), or the pressure-sensitive adhesive layer in which the compressive displacement on the first member is within a specific range as determined by the impact program (2) is formed from a pressure-sensitive adhesive composition (I) containing an acrylic copolymer (A). Each component contained in the pressure-sensitive adhesive composition (I) will be described below.
[0028] [Acrylic copolymer (A)] The acrylic copolymer (A) generally contains a structural portion derived from a (meth)acrylate (a1) having an alkyl group with 3 or more alkyl carbon atoms (hereinafter, sometimes referred to as "alkyl (meth)acrylate (a1)"). In particular, the acrylic copolymer (A) used in the present invention preferably contains a structural portion derived from an alkyl (meth)acrylate (a1) and a structural portion derived from a hydroxyl group-containing (meth)acrylate (a2). Such an acrylic copolymer (A) is usually obtained by polymerizing a copolymerization component containing an alkyl (meth)acrylate (a1) and a hydroxyl group-containing (meth)acrylate (a2).
[0029] In addition to the structural portion derived from the alkyl (meth)acrylate (a1) and the structural portion derived from the hydroxyl group-containing (meth)acrylate (a2), the acrylic copolymer (A) may also have, for example, a structural portion derived from at least one copolymerizable monomer (a3) selected from the group consisting of (meth)acrylates having an alkyl group with 1 or 2 carbon atoms and vinyl ester monomers (hereinafter referred to as "copolymerizable monomer (a3)"), a structural portion derived from a functional group-containing ethylenically unsaturated monomer (a4), a structural portion derived from another copolymerizable monomer (a5), and the like. That is, the copolymerization components may contain components other than the alkyl (meth)acrylate (a1) and the hydroxyl group-containing (meth)acrylate (a2), such as a copolymerizable monomer (a3), a functional group-containing ethylenically unsaturated monomer (a4), and other copolymerizable monomers (a5). In addition, from the viewpoint of adhesive properties, the acrylic copolymer (A) preferably does not contain a structural portion derived from a carboxy group-containing (meth)acrylate.
[0030] [Alkyl (meth)acrylate (a1)] Examples of the alkyl (meth)acrylate (a1) include linear alkyl (meth)acrylates such as n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, lauryl (meth)acrylate, n-tridecyl (meth)acrylate, stearyl (meth)acrylate, icosyl (meth)acrylate, henicosyl (meth)acrylate, and behenyl (meth)acrylate; isopropyl (meth)acrylate, isobutyl (meth)acrylate, and sec-butyl (meth)acrylate. Examples of the branched alkyl (meth)acrylates include butyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, isostearyl (meth)acrylate, and isoicosyl (meth)acrylate; and alicyclic (meth)acrylates such as cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, and adamantyl (meth)acrylate. These may be used alone or in combination of two or more.
[0031] Among these, linear alkyl (meth)acrylates are preferred from the standpoint of adhesion and impact resistance. From the viewpoint of balancing adhesion and shape stability, preferred are straight-chain or branched alkyl (meth)acrylates having an alkyl group with 3 to 18 carbon atoms, more preferably an alkyl group with 3 to 16 carbon atoms, particularly preferably an alkyl group with 3 to 12 carbon atoms, and especially preferably an alkyl group with 3 to 8 carbon atoms. Specific examples include n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, decyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. Of these, n-butyl (meth)acrylate and 2-ethylhexyl (meth)acrylate are preferred. Moreover, the alkyl (meth)acrylate (a1) is particularly preferably an acrylate, from the viewpoint of suppressing an increase in the storage shear modulus (G') at low temperatures and obtaining high flexibility.
[0032] The content of the structural portion derived from the alkyl (meth)acrylate (a1) in the acrylic copolymer (A) is usually 40 to 95 mass %, preferably 45 to 90 mass %, and particularly preferably 50 to 85 mass % of the acrylic copolymer (A) in order to suppress an increase in the storage shear modulus (G') at low temperatures. When the content of the structural portion derived from the alkyl (meth)acrylate (a1) is equal to or more than the lower limit, an increase in the storage shear modulus (G') at low temperatures can be suppressed, and when it is equal to or less than the upper limit, it is preferable in terms of compatibility with other physical properties such as adhesion.
[0033] [Hydroxyl group-containing (meth)acrylate (a2)] Examples of the hydroxyl group-containing (meth)acrylate (a2) include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; caprolactone-modified hydroxy (meth)acrylates such as caprolactone-modified 2-hydroxyethyl (meth)acrylate; diethylene glycol (meth)acrylate; polyethylene glycol (meth)acrylate; and polytetrafluoroethylene (meth)acrylate. Examples of such acrylates include (meth)acrylates having an oxyalkylene glycol structure such as methylene glycol (meth)acrylate and polyoxyethylene polyoxypropylene glycol (meth)acrylate, primary hydroxyl group-containing (meth)acrylates such as 2-acryloyloxyethyl-2-hydroxyethyl phthalate, secondary hydroxyl group-containing (meth)acrylates such as 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate and 3-chloro-2-hydroxypropyl (meth)acrylate, and tertiary hydroxyl group-containing (meth)acrylates such as 2,2-dimethyl 2-hydroxyethyl (meth)acrylate. These may be used alone or in combination of two or more.
[0034] Among the hydroxyl group-containing (meth)acrylates (a2), from the viewpoint of reducing the storage shear modulus (G') at low temperatures, hydroxyl group-containing (meth)acrylates having a hydroxyalkyl group having 1 to 10 carbon atoms, further 1 to 6, especially 2 to 4 carbon atoms, such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, etc. are preferred, and primary hydroxyl group-containing (meth)acrylates, such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate are particularly preferred, with 4-hydroxybutyl (meth)acrylate being particularly preferred.
[0035] When 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are used as the hydroxyl group-containing (meth)acrylate (a2), the ratio [2-hydroxyethyl (meth)acrylate / 4-hydroxybutyl (meth)acrylate] is preferably 95 / 5 to 30 / 70 by mass, more preferably 90 / 10 to 40 / 60, particularly preferably 85 / 15 to 45 / 65, and especially preferably 80 / 20 to 50 / 50. If the amount of 2-hydroxyethyl (meth)acrylate is too small, the adhesive strength when used as an adhesive decreases, and if the amount is too large, the bending durability when used as an adhesive tends to decrease.
[0036] In addition, the hydroxyl group-containing monomer (a2) preferably has a smaller content of di(meth)acrylate as an impurity in the hydroxyl group-containing monomer (a2). Specifically, it is preferable to use a hydroxyl group-containing monomer (a2) having a content of 0.5 mass % or less, particularly preferably 0.2 mass % or less, and further preferably 0.1 mass % or less.
[0037] The content of the structural portion derived from the hydroxyl group-containing monomer (a2) in the acrylic copolymer (A) is usually 5 to 60 mass %, preferably 8 to 45 mass %, particularly preferably 10 to 35 mass %, further preferably 11 to 30 mass %, and particularly preferably 12 to 25 mass % of the acrylic copolymer (A). If the content is too low, the moist heat resistance when used as an adhesive tends to decrease, whereas if the content is too high, the acrylic resin (A) tends to easily undergo a self-crosslinking reaction, resulting in a decrease in heat resistance.
[0038] [Copolymerizable monomer (a3)] In the present invention, it is preferred to further contain a copolymerizable monomer (a3) as a copolymerization component from the viewpoint of improving the cohesive strength and further improving the adhesive strength when used as a pressure-sensitive adhesive.
[0039] Examples of the copolymerizable monomer (a3) include methyl (meth)acrylate, ethyl (meth)acrylate, vinyl acetate, etc. These copolymerizable monomers (a3) may be used alone or in combination of two or more. Among them, from the viewpoint of improving the cohesive strength when used as an adhesive, methyl (meth)acrylate and ethyl (meth)acrylate are preferred, and ethyl (meth)acrylate is particularly preferred.
[0040] When the acrylic copolymer (A) contains a structural portion derived from the copolymerizable monomer (a3), the content is usually preferably 1 to 70 mass %, particularly preferably 3 to 60 mass %, and further preferably 5 to 45 mass % of the acrylic copolymer (A). If the content of the copolymerizable monomer (a3) is too low, the adhesive strength tends to decrease when used as an adhesive, whereas if the content is too high, the durability tends to decrease when used as an adhesive when the molecular weight of the acrylic copolymer (A) is small.
[0041] When methyl (meth)acrylate and / or ethyl (meth)acrylate are used as the copolymerizable monomer (a3), the content of the structural portion derived from methyl (meth)acrylate and / or ethyl (meth)acrylate in the acrylic copolymer (A) is usually 5 to 40 mass %, preferably 7 to 30 mass %, and more preferably 10 to 25 mass % of the acrylic copolymer (A). If the content of the structural portion derived from methyl (meth)acrylate and / or ethyl (meth)acrylate is too high, the viscosity increases and the handling property during processing tends to decrease, while if it is too low, the adhesive strength tends to decrease when used as an adhesive.
[0042] [Functional Group-Containing Ethylenically Unsaturated Monomer (a4)] In the present invention, a functional group-containing ethylenically unsaturated monomer (a4) (excluding the above-mentioned hydroxyl group-containing monomer (a2)) can be used as a copolymerization component of the acrylic copolymer (A) if necessary.
[0043] Examples of the functional group-containing ethylenically unsaturated monomer (a4) include functional group-containing monomers having a nitrogen atom, acetoacetyl group-containing monomers, isocyanate group-containing monomers, and glycidyl group-containing monomers. Among these, from the viewpoint of imparting cohesive strength and crosslinking promoting action, functional group-containing monomers having a nitrogen atom are preferred, amino group-containing monomers and amide group-containing monomers are more preferred, and amino group-containing monomers are particularly preferred.
[0044] Examples of the amino group-containing monomer include primary amino group-containing (meth)acrylates such as aminomethyl (meth)acrylate and aminoethyl (meth)acrylate; secondary amino group-containing (meth)acrylates such as t-butylaminoethyl (meth)acrylate and t-butylaminopropyl (meth)acrylate; and tertiary amino group-containing (meth)acrylates such as ethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, diethylaminopropyl (meth)acrylate, and dimethylaminopropylacrylamide.
[0045] Examples of the amide group-containing monomer include (meth)acrylamide; N-alkyl (meth)acrylamides such as N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, N-propyl (meth)acrylamide, Nn-butyl (meth)acrylamide, diacetone (meth)acrylamide, and N,N'-methylene bis (meth)acrylamide; N,N-dialkyl (meth)acrylamides such as N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dipropyl (meth)acrylamide, N,N-ethyl methyl acrylamide, and N,N-diallyl (meth)acrylamide; hydroxyalkyl (meth)acrylamides such as N-hydroxymethyl (meth)acrylamide and N-hydroxyethyl (meth)acrylamide; and alkoxyalkyl (meth)acrylamides such as N-methoxymethyl (meth)acrylamide and N-(n-butoxymethyl) (meth)acrylamide.
[0046] Examples of the acetoacetyl group-containing monomer include 2-(acetoacetoxy)ethyl (meth)acrylate and allyl acetoacetate.
[0047] Examples of the isocyanate group-containing monomer include 2-(meth)acryloyloxyethyl isocyanate and alkylene oxide adducts thereof.
[0048] Examples of the glycidyl group-containing monomer include glycidyl (meth)acrylate and allyl glycidyl (meth)acrylate.
[0049] These functional group-containing ethylenically unsaturated monomers (a4) may be used alone or in combination of two or more kinds.
[0050] When the acrylic copolymer (A) has a structural part derived from the functional group-containing ethylenically unsaturated monomer (a4), its content is usually 30% by mass or less of the acrylic copolymer (A), preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably 5% by mass or less. If the content of the structural part derived from the functional group-containing ethylenically unsaturated monomer (a4) is too high, the heat resistance of the acrylic copolymer (A) tends to decrease. The lower limit is usually 0.1% by mass, preferably 1% by mass.
[0051] [Other copolymerizable monomers (a5)] In the present invention, other copolymerizable monomers (a5) can be used as copolymerization components of the acrylic copolymer (A) as required.
[0052] Examples of the other copolymerizable monomers (a5) include (meth)acrylates having an alkoxyalkylene glycol skeleton, such as methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, butoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, butoxypolypropylene glycol (meth)acrylate, methoxypolytetramethylene glycol (meth)acrylate, butoxypolytetramethylene glycol (meth)acrylate, methoxypolyoxyethylene polyoxypropylene glycol (meth)acrylate, and butoxypolyoxyethylene polyoxypropylene glycol (meth)acrylate; phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenyl di Examples of the monomers include aromatic (meth)acrylic acid ester monomers such as ethylene glycol (meth)acrylate, phenoxy polyethylene glycol (meth)acrylate, phenoxy polyethylene glycol-polypropylene glycol-(meth)acrylate, and nonylphenol ethylene oxide adduct (meth)acrylate, and monomers such as acrylonitrile, methacrylonitrile, styrene, α-methylstyrene, vinyl propionate, vinyl stearate, vinyl chloride, vinylidene chloride, alkyl vinyl ether, vinyl toluene, vinyl pyridine, vinyl pyrrolidone, itaconic acid dialkyl ester, fumaric acid dialkyl ester, allyl alcohol, acrylic chloride, methyl vinyl ketone, N-acrylamidomethyl trimethyl ammonium chloride, allyl trimethyl ammonium chloride, and dimethyl allyl vinyl ketone. These monomers may be used alone or in combination of two or more.
[0053] In addition, when the purpose is to increase the molecular weight of the acrylic copolymer (A), a small amount of a compound having two or more ethylenically unsaturated groups, such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, or divinylbenzene, can also be used in combination. In this case, these compounds having two or more ethylenically unsaturated groups are highly reactive, and when used as a polymerization component of the acrylic copolymer (A), they usually do not remain unreacted. However, if the amount used is too large, these compounds having two or more ethylenically unsaturated groups will remain unreacted, and the acrylic copolymer (A) tends to gel.
[0054] When the acrylic copolymer (A) contains a structural portion derived from the other copolymerization monomer (a5), the content is usually 50% by mass or less, preferably 40% by mass or less, more preferably 20% by mass or less of the acrylic copolymer (A). If the content ratio of the other copolymerization monomer (a5) is too high, the heat resistance tends to decrease and the adhesive strength tends to decrease. The lower limit is usually 0.1% by mass, preferably 1% by mass.
[0055] The acrylic copolymer (A) can be obtained by appropriately selecting and polymerizing the above copolymerization components.
[0056] Examples of the method for polymerizing the acrylic copolymer (A) include conventionally known methods such as solution polymerization, suspension polymerization, bulk polymerization, and emulsion polymerization. Among these, solution polymerization is preferred in that it can safely and stably produce the acrylic copolymer (A) with any monomer composition. An example of a preferred method for producing the acrylic copolymer (A) used in the present invention will be described below.
[0057] First, the copolymerization components and a polymerization initiator are mixed or dropped into an organic solvent, and solution polymerization is carried out to obtain an acrylic copolymer solution.
[0058] [Organic solvents] Examples of organic solvents used in the polymerization reaction include aromatic hydrocarbons such as toluene and xylene, aliphatic hydrocarbons such as hexane, esters such as ethyl acetate and butyl acetate, aliphatic alcohols such as N-propyl alcohol and isopropyl alcohol, and ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone. These can be used alone or in combination of two or more. Among these solvents, ethyl acetate is preferred.
[0059] [Polymerization initiator] As the polymerization initiator used in the polymerization reaction, azo-based polymerization initiators and peroxide-based polymerization initiators, which are ordinary radical polymerization initiators, can be used. Examples of the azo-based polymerization initiator include 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobisisobutyronitrile, (1-phenylethyl)azodiphenylmethane, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-cyclopropylpropionitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile). Examples of the peroxide-based polymerization initiator include benzoyl peroxide, di-t-butyl peroxide, cumene hydroperoxide, lauroyl peroxide, t-butyl peroxypivalate, t-hexyl peroxypivalate, t-hexyl peroxyneodecanoate, diisopropyl peroxycarbonate, and diisobutyryl peroxide. These may be used alone or in combination of two or more. Among these, 2,2'-azobis(2,4-dimethylvaleronitrile) is preferred.
[0060] The amount of the polymerization initiator used is usually 0.001 to 10 parts by mass, preferably 0.1 to 8 parts by mass, particularly preferably 0.5 to 6 parts by mass, further preferably 1 to 4 parts by mass, particularly preferably 1.5 to 3 parts by mass, and most preferably 2 to 2.5 parts by mass, based on 100 parts by mass of the copolymerization components. If the amount of the polymerization initiator used is too small, the polymerization rate of the acrylic copolymer (A) tends to decrease, the amount of residual monomers tends to increase, and the weight average molecular weight of the acrylic copolymer (A) tends to increase. If the amount used is too large, gelation of the acrylic copolymer (A) described below tends to occur.
[0061] [Polymerization conditions, etc.] The solution polymerization may be carried out under known polymerization conditions. For example, the polymerization components and a polymerization initiator may be mixed or dropped into a solvent, and polymerization may be carried out under predetermined polymerization conditions.
[0062] The polymerization temperature in the polymerization reaction is usually 40 to 120° C., but in the present invention, from the viewpoint of stable reaction, it is preferably 50 to 90° C., particularly preferably 55 to 75° C., and further preferably 60 to 70° C. If the polymerization temperature is too high, the acrylic copolymer (A) tends to gel easily, while if it is too low, the activity of the polymerization initiator decreases, so that the polymerization rate decreases and the amount of residual monomers tends to increase.
[0063] The polymerization time in the polymerization reaction (when the later-described follow-up heating is performed, the time until the start of the follow-up heating) is not particularly limited, but is preferably 0.5 hours or more from the last addition of the polymerization initiator, particularly preferably 1 hour or more, further preferably 2 hours or more, and particularly preferably 5 hours or more. The upper limit of the polymerization time is usually 72 hours. The polymerization reaction is preferably carried out while refluxing the solvent in order to facilitate heat removal.
[0064] In the production of the acrylic copolymer (A), in order to reduce the amount of the remaining polymerization initiator, it is preferable to thermally decompose the polymerization initiator by further heating.
[0065] The drive-in heating temperature is preferably higher than the 10-hour half-life temperature of the polymerization initiator, and specifically is usually 40 to 150° C., preferably 55 to 130° C. from the viewpoint of suppressing gelation, and particularly preferably 75 to 95° C. If the drive-in heating temperature is too high, the acrylic copolymer (A) tends to turn yellow, whereas if it is too low, polymerization components and polymerization initiator remain, and the temporal stability and thermal stability of the acrylic copolymer (A) tend to decrease. Thus, the acrylic copolymer (A) can be obtained.
[0066] The acrylic copolymer (A) may have a photoactive site, such as a polymerizable carbon-carbon double bond group, introduced into its side chain, which can increase the crosslinking efficiency of the pressure-sensitive adhesive composition and crosslink the pressure-sensitive adhesive composition in a shorter time, thereby improving productivity.
[0067] Examples of a method for introducing a polymerizable carbon double bond group into the side chain of the acrylic copolymer (A) include a method in which a copolymer containing the above-mentioned hydroxyl group-containing (meth)acrylate (a2) or functional group-containing ethylenically unsaturated monomer (a4) is prepared, and then a compound having a functional group reactive with these functional groups and a polymerizable carbon double bond group is subjected to a condensation or addition reaction while maintaining the activity of the polymerizable carbon double bond group.
[0068] Examples of combinations of these functional groups include epoxy groups (glycidyl groups) and carboxy groups, amino groups and carboxy groups, amino groups and isocyanate groups, epoxy groups (glycidyl groups) and amino groups, hydroxyl groups and epoxy groups, and hydroxyl groups and isocyanate groups. Among these combinations of functional groups, the combination of hydroxyl groups and isocyanate groups is preferred because of the ease of reaction control. Among these combinations of functional groups, the combination of hydroxyl groups and isocyanate groups is particularly preferred, in which the copolymer has a hydroxyl group and the compound has an isocyanate group.
[0069] Examples of the isocyanate compound having a polymerizable carbon double bond group include the above-mentioned 2-(meth)acryloyloxyethyl isocyanate and its alkylene oxide adducts.
[0070] The content of the compound having a functional group capable of reacting with the functional group and a polymerizable carbon double bond group is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 1 part by mass or less, and particularly preferably 0.1 parts by mass or less, based on 100 parts by mass of the acrylic copolymer (A) from the viewpoint of improving adhesion and stress relaxation. The lower limit is usually 0 parts by mass.
[0071] The hydroxyl value of the acrylic copolymer (A) is preferably 30 mgKOH / g or more, more preferably 50 mgKOH / g or more, and particularly preferably 70 mgKOH / g or more. The upper limit of the hydroxyl value is usually 150 mgKOH / g, preferably 120 mgKOH / g. The hydroxyl value can be determined by determining the amount of free hydroxyl groups contained in 1 g of vinyl polymer from the composition ratio of the monomers used in the polymerization, and calculating the amount of potassium hydroxide (unit: mg) required to neutralize the acetic acid required for acetylating the free hydroxyl groups.
[0072] The glass transition temperature (Tg) of the acrylic copolymer (A) is preferably −20° C. or lower in order to suppress an increase in the storage shear modulus (G') at low temperatures, more preferably −23° C. or lower, even more preferably −25° C. or lower, and particularly preferably −30° C. or lower. The lower limit of the glass transition temperature (Tg) is usually −50° C. due to concerns about glue overflow caused by a decrease in the storage shear modulus at high temperatures.
[0073] In the present invention, the glass transition temperature (Tg) is determined by reading the temperature at which the loss tangent (tan δ) becomes maximum when the dynamic viscoelasticity is measured in a shear mode at a frequency of 1 Hz using a dynamic viscoelasticity measuring device. For example, the acrylic copolymer (A) is molded into a cylinder having a diameter of 8 mm (height of 1.0 mm), and the loss tangent (tan δ) of this cylinder is measured using a viscoelasticity measuring device (manufactured by TA Instruments, "DHR 2") under the following measurement conditions. (Measurement conditions) Measurement tool: Φ8mm parallel plate Distortion: 0.1% Frequency: 1Hz ·Measurement temperature: -50~80℃ Heating rate: 5℃ / min
[0074] The weight average molecular weight (Mw) of the acrylic copolymer (A) is preferably 400,000 or more, more preferably 500,000 or more, and even more preferably 550,000 or more, from the viewpoint of obtaining a pressure-sensitive adhesive composition with high cohesive strength. In addition, the upper limit of the weight average molecular weight (Mw) of the acrylic copolymer (A) is preferably 1.5 million or less, more preferably 1.2 million or less, and even more preferably 1.1 million or less, from the viewpoints of handleability and uniform stirring.
[0075] In the present invention, the weight average molecular weight (Mw) can be determined, for example, as follows. (Method of measuring weight average molecular weight) The weight average molecular weight (Mw) can be calculated by dissolving 4 mg of the acrylic copolymer (A) in 12 mL of tetrahydrofuran (THF) to prepare a measurement sample, and measuring the molecular weight distribution curve under the following conditions using a gel permeation chromatography (GPC) analyzer (Tosoh Corporation, "HLC-8320GPC"). Guard column: TSKguardcolμmnHXL Separation column: TSKgelGMHXL (4 columns) ·Temperature: 40℃ ·Injection volume: 100μL Polystyrene equivalent Solvent: THF ·Flow rate: 1.0mL / min
[0076] The content of the acrylic copolymer (A) in the pressure-sensitive adhesive composition (I) is usually 10 to 75 mass %, preferably 12 to 73 mass %, more preferably 20 to 71 mass %, and particularly preferably 30 to 69 mass %.
[0077] The pressure-sensitive adhesive composition (I) preferably contains a radically polymerizable compound (B) and a photopolymerization initiator (C) in terms of excellent impact resistance.
[0078] [Radically polymerizable compound (B)] The radical polymerizable compound (B) may be, for example, a monofunctional (meth)acrylate or a polyfunctional (meth)acrylate. These may be used alone or in combination of two or more. Among them, it is preferable to use a monofunctional (meth)acrylate.
[0079] [Monofunctional (meth)acrylate] The monofunctional (meth)acrylate may be a monofunctional (meth)acrylic monomer or a monofunctional (meth)acrylic oligomer, which may be used alone or in combination of two or more kinds. The monofunctional (meth)acrylate preferably has an alkylene glycol skeleton because it has excellent impact resistance.
[0080] As the alkylene glycol skeleton, from the viewpoint of decreasing the storage shear modulus at low temperatures, an alkylene glycol skeleton having an alkylene chain having 2 to 10 carbon atoms, further 2 to 8, particularly 2 to 6, and especially 2 to 4 carbon atoms, is preferred, and particularly preferred are an ethylene glycol skeleton, a propylene glycol skeleton, a butylene glycol skeleton, and the like, and more preferably a propylene glycol skeleton.
[0081] Examples of the monofunctional (meth)acrylic monomer include the monofunctional (meth)acrylate monomer having an alkylene glycol skeleton, as well as monofunctional (meth)acrylate monomers other than the (meth)acrylate monomer having an alkylene glycol skeleton.
[0082] Examples of the monofunctional (meth)acrylate monomer other than the (meth)acrylate monomer having an alkylene glycol skeleton include linear or branched alkyl (meth)acrylates, and specific examples thereof include n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, and the like. (meth)acrylate, isononyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, isobornyl (meth)acrylate, 3,5,5-trimethylcyclohexane (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate.
[0083] Examples of the monofunctional (meth)acrylic oligomer include polyester (meth)acrylate, epoxy (meth)acrylate, urethane (meth)acrylate, and polyether (meth)acrylate, and from the viewpoint of impact resistance, it is preferable that the oligomer has an alkylene glycol skeleton.
[0084] Specifically, for example, a monofunctional (meth)acrylic oligomer having an alkylene glycol skeleton represented by the following general formula (1) can be mentioned. CH2=CR 1 -COO-R 2 -Y-(R 3 O) k -R 4 (1) In the formula, R1 represents hydrogen or a methyl group. R2 and R4 each independently represent an alkyl group having 1 to 10 carbon atoms or an alkenyl group having 2 to 10 carbon atoms. Y represents a bonding group selected from a urethane bond, an ester bond, an ether bond, a carbonate bond, an amide bond, and a urea bond. R 3 represents an alkylene group which is an ethylene group or a propylene group. Therefore, (R 3 O) k is [(C2H4O) r (C3H6O) s ], where r is an integer of 0 or 1 or more, s is an integer of 0 or 1 or more, and r+s=k. [(C2H4O) r (C3H6O) s In the case where an oxyethylene structure (C2H4O) and an oxypropylene structure (C3H6O) coexist in the above formula (1), they may be of a random type or a block type. k is (R 3 O), that is, (C2H4O) r and (C3H6O) s It is an integer from 1 to 500, which represents the total number of repeating units, r+s.
[0085] The positive number "k" in the general formula (1) is preferably 10 to 500, more preferably 100 to 450, and even more preferably 200 to 400, from the viewpoint of imparting restorability that allows the shape to be easily restored even when an impact is received, while reducing the storage shear modulus at low temperatures to obtain impact resistance.
[0086] Among these, the monofunctional (meth)acrylic oligomer having an alkylene glycol skeleton is preferably a monofunctional urethane (meth)acrylate having a urethane bond, in view of excellent impact resistance.
[0087] The monofunctional urethane (meth)acrylate having an alkylene glycol skeleton is particularly effective because it has high polarity and a long chain length, and therefore the polymer chains tend to be entangled to provide high recovery (impact resistance), and because it has an oxypropylene structure with high molecular rotation, it tends to provide a low storage shear modulus.
[0088] [Multifunctional (meth)acrylate] The polyfunctional (meth)acrylate may be a polyfunctional (meth)acrylic monomer or a polyfunctional (meth)acrylic oligomer. Examples of the polyfunctional (meth)acrylic monomer include 1,4-butanediol di(meth)acrylate, glycerin di(meth)acrylate, neopentyl glycol di(meth)acrylate, glycerin glycidyl ether di(meth)acrylate, tricyclodecane dimethacrylate, tricyclodecane dimethanol di(meth)acrylate, bisphenol A polyethoxy di(meth)acrylate, bisphenol A polypropoxy di(meth)acrylate, and bisphenol F polyethoxy di(meth)acrylate. (meth)acrylate, ethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane trioxyethyl (meth)acrylate, ε-caprolactone modified tris(2-hydroxyethyl) isocyanurate tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propoxylated pentaerythritol tri(meth)acrylate, ethoxylated pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate Acrylate, propoxylated pentaerythritol tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, tris(acryloxyethyl)isocyanurate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate )acrylate, tripentaerythritol hexa(meth)acrylate, tripentaerythritol penta(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, di(meth)acrylate of hydroxypivalic acid neopentyl glycol adduct ε-caprolactone, trimethylolpropane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, and the like can be mentioned.
[0089] Examples of the polyfunctional (meth)acrylic oligomer include polyfunctional (meth)acrylic oligomers such as polyfunctional polyester (meth)acrylate oligomers, polyfunctional epoxy (meth)acrylate oligomers, polyfunctional urethane (meth)acrylate oligomers, and polyfunctional polyether (meth)acrylate oligomers.
[0090] When the polyfunctional (meth)acrylate is used, it also acts as a crosslinking agent.
[0091] From the viewpoint of reducing the storage shear modulus at low temperatures while maintaining the recovery property upon impact, the radically polymerizable compound (B) preferably has a glass transition temperature of -40°C or lower, more preferably -45°C or lower, and even more preferably -50°C or lower, when homopolymerized. The radically polymerizable compound (B) preferably has a glass transition temperature of -80°C or higher, more preferably -75°C or higher, and even more preferably -70°C or higher, when homopolymerized, due to concerns about overflow of the paste due to a decrease in storage shear modulus at high temperatures.
[0092] The weight average molecular weight (Mw) of the radical polymerizable compound (B) is preferably 30,000 or less, more preferably 28,000 or less, and even more preferably 25,000 or less, from the viewpoint of reducing the storage shear modulus at low temperatures while maintaining the recovery property when impacted. The lower limit of the weight average molecular weight (Mw) of the radical polymerizable compound (B) is preferably 3,000 or more, more preferably 4,000 or more, and even more preferably 5,000 or more, from the viewpoint of preventing a decrease in adhesion due to bleed-out while maintaining the recovery property when impacted. The weight average molecular weight (Mw) of the radically polymerizable compound (B) having an alkylene glycol skeleton can be determined in accordance with the "Method of measuring weight average molecular weight" described for the acrylic copolymer (A).
[0093] When the radical polymerizable compound (B) is used, its content is usually 10 to 100 parts by mass, preferably 20 to 90 parts by mass, and particularly preferably 40 to 80 parts by mass, based on 100 parts by mass of the acrylic copolymer (A). By setting the content of the radical polymerizable compound (B) within the above range, it tends to be possible to obtain a pressure-sensitive adhesive layer having excellent impact resistance.
[0094] When the polyfunctional (meth)acrylate is used as a crosslinking agent, the content is usually 10 to 100 parts by mass, preferably 20 to 90 parts by mass, and particularly preferably 40 to 80 parts by mass, relative to 100 parts by mass of the acrylic copolymer (A). By setting the content of the polyfunctional (meth)acrylate within the above range, a pressure-sensitive adhesive sheet with excellent flexibility tends to be obtained.
[0095] [Photopolymerization initiator (C)] The photopolymerization initiator (C) is not particularly limited as long as it is a compound that generates radicals when exposed to active energy rays. Photopolymerization initiators are roughly classified into two types according to the radical generation mechanism. More specifically, they are roughly classified into cleavage-type photopolymerization initiators that can generate radicals by cleaving and decomposing the single bond of the initiator itself, and hydrogen abstraction-type photopolymerization initiators that can generate radicals by an excited initiator abstracting hydrogen from a hydrogen donor in the system. These may be used alone or in combination of two or more types. The cleavage type photopolymerization initiator is preferred in that it has high photosensitivity. On the other hand, hydrogen abstraction type photopolymerization initiators are preferred because they do not produce photodecomposition products and can incorporate the acrylic polymer (A) into a crosslinked structure by a hydrogen abstraction reaction.
[0096] Examples of the hydrogen abstraction type photopolymerization initiator include benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-phenylbenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, 2-methylbenzoylbenzoate, 4-[(4-methylphenyl)thio]benzophenone, 4-acryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, 4-acryloyloxy-4'-bromobenzophenone, 4-acryloyloxyethoxy-4'-bromobenzophenone, 4-meth ... Examples of the photopolymerization initiator include intermolecular hydrogen abstraction type photopolymerization initiators such as 4-methacryloyloxybenzophenone, 4-methacryloyloxyethoxybenzophenone, 4-methacryloyloxy-4'-methoxybenzophenone, 4-methacryloyloxyethoxy-4'-methoxybenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, and 4-methacryloyloxyethoxy-4'-bromobenzophenone; and intramolecular hydrogen abstraction type photopolymerization initiators such as methylbenzoylformate, methyl benzoylformate, oxyphenylacetic acid-2-(2-oxo-2-phenyl-acetoxy-ethoxy)ethyl ester, and oxyphenylacetic acid-2-(2-hydroxy-ethoxy)ethyl ester. These may be used alone or in combination of two or more kinds.
[0097] Among the intermolecular hydrogen abstraction type photopolymerization initiators, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, and photopolymerization initiators (C1) having a radically polymerizable functional group having a carbon-carbon double bond in the molecule, such as 4-acryloyloxybenzophenone, 4-methacryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, and 4-methacryloyloxybenzophenone are preferred, and 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-methacryloyloxybenzophenone, and 4-methacryloyloxybenzophenone are more preferred. The photopolymerization initiator (C1) having within its molecule a radically polymerizable functional group having a carbon-carbon double bond tends to be incorporated into the polymer structure after photoreaction, thereby suppressing bleed-out of the photopolymerization initiator (C) and improving the cohesive strength of the adhesive sheet. Furthermore, intramolecular hydrogen abstraction type photopolymerization initiators are preferred because they can act not only as hydrogen donors in the system but also as the starting point for radical generation themselves, and methylbenzoyl formate is more preferred.
[0098] In the present invention, it is preferable that the photopolymerization initiator (C) contains an intermolecular hydrogen abstraction type photopolymerization initiator and an intramolecular hydrogen abstraction type photopolymerization initiator, from the viewpoint of increasing the cohesive strength of the pressure-sensitive adhesive sheet.
[0099] Examples of the cleavage-type photopolymerization initiator include 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)benzyl]phenyl}-2-methyl-propan-1-one, oligo(2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone), 2-benzyl-2-dimethylamino-1-(4-morpholino-1-methylphenyl)propanone, and 2-benzyl-2-dimethylamino-1-(4-morpholino-1-methylphenyl)propanone. Examples of suitable phosphine oxides include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)2,4,4-trimethylpentylphosphine oxide, and derivatives thereof.
[0100] The content of the photopolymerization initiator (C) is usually 0.1 to 10 parts by mass, preferably 0.5 to 6 parts by mass, more preferably 1 to 4 parts by mass, based on 100 parts by mass of the acrylic copolymer (A). When the content is equal to or more than the lower limit, curing failure tends to be prevented, whereas when the content is equal to or less than the upper limit, a decrease in solution stability such as precipitation from the pressure-sensitive adhesive composition tends to be easily suppressed, and problems such as embrittlement and coloration tend to be easily suppressed.
[0101] [Thermal crosslinking agent] The pressure-sensitive adhesive composition (I) may contain a thermal crosslinking agent in order to further increase the crosslink density and improve long-term reliability. Examples of such thermal crosslinking agents include isocyanate-based crosslinking agents, aziridine-based crosslinking agents, melamine-based crosslinking agents, aldehyde-based crosslinking agents, amine-based crosslinking agents, and metal chelate-based crosslinking agents. Among these, it is preferable to use an isocyanate-based crosslinking agent because of its excellent reactivity with the acrylic copolymer.
[0102] The content of the thermal crosslinking agent is usually 5 to 40 parts by mass, and preferably 10 to 30 parts by mass, based on 100 parts by mass of the acrylic copolymer (A).
[0103] [Other ingredients] The pressure-sensitive adhesive composition (I) may contain, as "other components", various additives such as a silane coupling agent, an ultraviolet absorber, an anti-rust agent, a tackifier resin, an antioxidant, a light stabilizer, a metal deactivator, an anti-aging agent, a moisture absorbent, an anti-rust agent, and inorganic particles, as necessary, to the extent that the effects of the present invention are not impaired. If necessary, a reaction catalyst such as a tertiary amine compound, a quaternary ammonium compound, or a tin laurate compound may be appropriately contained. These can be used alone or in combination of two or more.
[0104] [Silane coupling agents] The pressure-sensitive adhesive composition (I) preferably contains a silane coupling agent in terms of durability. The silane coupling agent is an organosilicon compound that contains, in its structure, one or more reactive functional groups and one or more alkoxy groups bonded to silicon atoms.
[0105] Examples of the reactive functional group include an epoxy group, a (meth)acryloyl group, a mercapto group, a hydroxyl group, a carboxy group, an amino group, an amide group, and an isocyanate group. Among these, an epoxy group and a mercapto group are preferred from the viewpoint of balance of durability.
[0106] The alkoxy group bonded to the silicon atom preferably contains an alkoxy group having 1 to 8 carbon atoms from the standpoint of durability and storage stability, and is particularly preferably a methoxy group or an ethoxy group. The silane coupling agent may have an organic substituent other than the reactive functional group and the alkoxy group bonded to the silicon atom, such as an alkyl group or a phenyl group.
[0107] Examples of the silane coupling agent include monomeric epoxy group-containing silane coupling agents which are silane compounds such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; and oligomeric epoxy group-containing silane coupling agents which are silane compounds obtained by hydrolysis and condensation polymerization of a part of the silane compounds or by co-condensation of the silane compounds with alkyl group-containing silane compounds such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, and ethyltrimethoxysilane; Monomeric mercapto group-containing silane coupling agents which are silane compounds such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, γ-mercaptopropyldimethoxymethylsilane, and 3-mercaptopropylmethyldimethoxysilane; and oligomeric mercapto group-containing silane coupling agents which are silane compounds obtained by hydrolysis and condensation polymerization of a part of the silane compounds, or by co-condensation of the silane compounds with alkyl group-containing silane compounds such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, and ethyltrimethoxysilane; (meth)acryloyl group-containing silane coupling agents, such as 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane; Amino group-containing silane coupling agents such as N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, and N-phenyl-3-aminopropyltrimethoxysilane; Isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane; Examples of the silane coupling agent include vinyl group-containing silane coupling agents such as vinyltrimethoxysilane and vinyltriethoxysilane. These may be used alone or in combination of two or more.
[0108] Among these, from the viewpoint of excellent durability, epoxy group-containing silane coupling agents and mercapto group-containing silane coupling agents are preferably used, among which epoxy group-containing silane coupling agents are preferred, with 3-glycidoxypropyltrimethoxysilane being particularly preferred.
[0109] The content of the silane coupling agent is preferably 0.005 to 10 parts by mass, particularly preferably 0.01 to 5 parts by mass, and further preferably 0.05 to 1 part by mass, relative to 100 parts by mass of the (meth)acrylic copolymer (A). If the content is within this range, durability tends to be improved.
[0110] (UV absorber) Examples of the ultraviolet absorbent include benzophenone-based ultraviolet absorbents, benzotriazole-based ultraviolet absorbents, triazine-based ultraviolet absorbents, salicylic acid-based ultraviolet absorbents, cyanoacrylate-based ultraviolet absorbents, benzoxazine-based ultraviolet absorbents, etc. These ultraviolet absorbents can be used alone or in combination of two or more.
[0111] When an ultraviolet absorbing agent is used, its content is preferably 0.01 to 20 parts by mass, particularly preferably 0.1 to 15 parts by mass, and further preferably 0.5 to 10 parts by mass, relative to 100 parts by mass of the acrylic copolymer (A). When the content is equal to or more than the lower limit, the light resistance reliability tends to improve, and when the content is equal to or less than the upper limit, the yellowing resistance tends to improve.
[0112] (rust inhibitor) As the rust inhibitor, for example, triazoles, benzotriazoles, etc. are preferable, which can prevent corrosion of optical members. These may be used alone or in combination of two or more kinds. When a rust inhibitor is used, its content is preferably 0.01 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the acrylic copolymer (A).
[0113] The content of the other components is preferably 5 parts by mass or less, particularly preferably 1 part by mass or less, and further preferably 0.5 parts by mass or less, based on 100 parts by mass of the acrylic copolymer (A). If the content is too high, the compatibility with the acrylic copolymer decreases, and the durability tends to decrease.
[0114] The pressure-sensitive adhesive composition (I) is prepared by mixing a predetermined amount of each of the acrylic copolymer (A), preferably a radically polymerizable compound (B), a photopolymerization initiator (C), and, if necessary, a thermal crosslinking agent and other components.
[0115] <Method of manufacturing pressure-sensitive adhesive layer> Next, a method for producing the pressure-sensitive adhesive layer will be described. However, the following description is merely an example of a method for producing a pressure-sensitive adhesive layer, and the pressure-sensitive adhesive layer is not limited to that produced by this production method.
[0116] The pressure-sensitive adhesive layer is formed from the pressure-sensitive adhesive composition (I), and is usually produced by preparing the pressure-sensitive adhesive composition (I), forming it into a sheet, curing it by crosslinking, i.e., polymerization reaction, and then appropriately processing it as necessary. That is, the pressure-sensitive adhesive layer is preferably a pressure-sensitive adhesive sheet.
[0117] When preparing the pressure-sensitive adhesive composition (I), the components may be kneaded using a temperature-controllable kneader (such as a single-screw extruder, a twin-screw extruder, a planetary mixer, a twin-screw mixer, or a pressure kneader). When kneading the components, various additives such as antioxidants may be blended together with the resin in advance and then fed to the kneader, or all of the materials may be melt-mixed in advance and then fed, or a master batch in which only the additives are concentrated in the resin may be prepared and then fed.
[0118] The method for forming the pressure-sensitive adhesive composition (I) into a sheet can be a known method, such as a wet lamination method, a dry lamination method, an extrusion casting method using a T-die, an extrusion lamination method, a calendar method, an inflation method, an injection molding method, a liquid injection curing method, etc. Among them, when producing a sheet, the wet lamination method, the extrusion casting method, and the extrusion lamination method are preferable.
[0119] The pressure-sensitive adhesive composition (I) can be cured by irradiating it with active energy rays, and a pressure-sensitive adhesive sheet can be produced by irradiating a molded product of the pressure-sensitive adhesive composition (I), for example, a sheet, with active energy rays. In addition to the irradiation with active energy rays, the composition can also be heated to further cure.
[0120] Furthermore, there are no particular limitations on the irradiation energy, irradiation time, irradiation method, etc. of the active energy rays as long as they can activate the photopolymerization initiator (C) and polymerize the monomer components. When a hydrogen abstraction type photopolymerization initiator (c1) is used as the photopolymerization initiator (C), a hydrogen abstraction reaction also occurs from the acrylic polymer (A), and the acrylic polymer (A) is incorporated into the crosslinked structure, thereby forming a crosslinked structure having many crosslinking points. Therefore, the pressure-sensitive adhesive sheet is preferably one cured using a hydrogen abstraction type photopolymerization initiator (c1).
[0121] Examples of the active energy rays in the active energy ray irradiation include light rays such as far ultraviolet rays, ultraviolet rays, near ultraviolet rays, infrared rays, and visible light rays, and ionizing radiation such as X-rays, α rays, β rays, γ rays, electron beams, proton beams, and neutron beams. Among them, ultraviolet rays are preferable from the viewpoint of suppressing damage to optical device components and controlling reactions. In addition, curing by ultraviolet irradiation is advantageous from the viewpoints of curing speed, ease of availability of an irradiation device, price, and the like.
[0122] Examples of light sources for ultraviolet irradiation include high-pressure mercury lamps, ultra-high-pressure mercury lamps, low-pressure mercury lamps, carbon arc lamps, metal halide lamps, xenon lamps, chemical lamps, electrodeless discharge lamps, LEDs, etc. that emit light in the 150 to 450 nm wavelength range. Among these, it is preferable to use a high-pressure mercury lamp.
[0123] The amount of active energy ray irradiation (accumulated light amount) is 0.03 to 3 J / cm from the viewpoint of curing. 2 is preferable, and more preferably 0.1 to 2 J / cm 2 , and more preferably 0.3 to 1.5 J / cm 2 This is carried out under the following conditions.
[0124] A release film may be provided on at least one surface of the pressure-sensitive adhesive sheet in order to prevent blocking and adhesion of foreign matter. That is, the adhesive sheet can also be provided as an adhesive sheet with a release film (adhesive sheet laminate) having a configuration in which a release film is laminated on one or both sides of an adhesive layer (the adhesive sheet) made of an adhesive composition.
[0125] When release films are provided on both sides of the pressure-sensitive adhesive sheet, it is preferable to use a laminate structure in which a light release film having a relatively low release strength and a heavy release film having a relatively high release strength are laminated together. When using an adhesive sheet with release films provided on both sides, first, one release film (light release film) is peeled off to expose one side of the adhesive sheet, and then the adhesive sheet is bonded to a component sheet or a flexible image display device component (referred to as the first component), and the other release film (heavy release film) is peeled off to expose the other side of the adhesive sheet, and then the component sheet or a flexible image display device component (referred to as the second component) is bonded to the other side of the adhesive sheet.
[0126] As such a release film, any known release film can be appropriately used. As the material for the release film, for example, a film such as a polyester film, a polyolefin film, a polycarbonate film, a polystyrene film, an acrylic film, a triacetyl cellulose film, a fluororesin film, etc., which has been subjected to a release treatment by coating with a release agent such as a silicone resin, or release paper, etc. can be appropriately selected and used. Among them, polyester films, and more particularly polyethylene terephthalate (PET) films, particularly biaxially stretched PET films, are preferred because of their excellent transparency, mechanical strength, heat resistance, flexibility, etc. A release film can be used in which a release layer formed by curing a curable silicone-based release agent containing silicone resin as a main component is provided on the substrate.
[0127] Generally, when an adhesive sheet with excellent flexibility is made into an adhesive sheet with a release film, if the release film has a high peeling strength, the adhesive sheet is flexible and tends to deform when the release film is peeled off, leaving peeling marks. For this reason, the release film, particularly the light release film, used in the highly flexible adhesive sheet is preferably a release film that can be peeled off with even less force than the light release type release films that have been commonly used in the past.
[0128] However, when the thickness of the release agent layer is increased in order to make the release film easier to release, depending on the type of release agent used, components derived from the release agent layer may transfer to the surface of the adhesive sheet, impairing the reliability of the adhesive sheet. For this reason, it is preferable that the release film has good releasability from the adhesive sheet and has little migration of the release agent to the adhesive sheet.
[0129] The peel strength between the adhesive sheet and the release film is preferably 1.5 to 0.05 N / cm, more preferably 1.2 to 0.06 N / cm, and even more preferably 1.0 to 0.07 N / cm. The peel strength between the release film and the adhesive sheet is a value measured in a 180° peel test at a test speed of 300 m / min. If it is within the above range, it is possible to prevent peeling marks when the release film is peeled from the adhesive sheet.
[0130] In addition, the peak intensity of silicon atoms measured by a fluorescent X-ray analyzer on the adhesive surface exposed by peeling off the release film from the adhesive sheet is preferably 100 cps or less. If the peak intensity is 100 cps or less, it is preferable that the release agent transferred to the adhesive sheet surface does not impair the reliability when the adhesive sheet is used as a laminate for constituting an image display device. From this viewpoint, the peak intensity is more preferably 90 cps or less, even more preferably 80 cps or less, and particularly preferably 70 cps or less. The lower limit is usually 0 cps.
[0131] The thickness of the release film is not particularly limited, but from the viewpoint of processability and handleability, the thickness is preferably 10 to 250 μm, more preferably 25 to 200 μm, and even more preferably 35 to 190 μm.
[0132] If necessary, embossing or various unevenness (cone, pyramid, hemisphere, etc.) may be performed. In order to improve adhesion to various component sheets, the surface may be subjected to various surface treatments such as corona treatment, plasma treatment, and primer treatment.
[0133] Furthermore, as another embodiment of the method for producing the pressure-sensitive adhesive sheet, the pressure-sensitive adhesive composition (I) can be dissolved in an appropriate solvent and various coating methods can be used. When a coating method is used, a pressure-sensitive adhesive sheet can be obtained by heat curing in addition to the above-mentioned curing by irradiation with active energy rays. In the case of coating, the thickness of the pressure-sensitive adhesive sheet can be adjusted by the coating thickness and the solids concentration of the coating liquid.
[0134] For example, the adhesive composition (I) can be dissolved in a solvent, coated on a release film, dried, and cured by irradiating with active energy rays to form an adhesive sheet. Furthermore, a release film may be laminated as necessary. In this case, the adhesive composition (I) can be coated on a release film, dried, cured by irradiating with active energy rays, and a release film can be laminated thereon, or the adhesive composition (I) can be coated on a release film, dried, and cured by irradiating with active energy rays to form an adhesive sheet.
[0135] The solvent is not particularly limited as long as it dissolves the pressure-sensitive adhesive composition, and examples thereof include ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, methyl acetoacetate, and ethyl acetoacetate, ketone-based solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, aromatic solvents such as toluene and xylene, and alcohol-based solvents such as methanol, ethanol, and propyl alcohol. These can be used alone or in combination of two or more. Among them, ethyl acetate, acetone, methyl ethyl ketone, and toluene are preferred from the viewpoints of solubility, drying property, and price, and ethyl acetate is particularly preferred.
[0136] From the viewpoint of drying property, the content of the solvent is preferably 600 parts by mass or less, more preferably 500 parts by mass or less, even more preferably 400 parts by mass or less, and particularly preferably 300 parts by mass or less, relative to 100 parts by mass of the acrylic polymer (A), while being preferably 1 part by mass or more, more preferably 50 parts by mass or more, even more preferably 100 parts by mass or more, and particularly preferably 150 parts by mass or more.
[0137] Coating can be performed by a conventional method such as roll coating, die coating, gravure coating, comma coating, screen printing, bar coating, etc.
[0138] The solvent content in the pressure-sensitive adhesive composition (I) after drying is preferably 1% by mass or less, more preferably 0.5% by mass or less, particularly preferably 0.1% by mass or less, and most preferably 0% by mass.
[0139] The drying temperature is usually 40 to 150° C., more preferably 45 to 140° C., further preferably 50 to 130° C., and particularly preferably 55 to 120° C. When the temperature is within the above range, the solvent can be removed efficiently and relatively safely while suppressing thermal deformation of the release film.
[0140] The drying time is usually 1 to 30 minutes, more preferably 3 to 25 minutes, and further preferably 5 to 20 minutes. When the drying time is within the above range, the solvent can be removed efficiently and sufficiently.
[0141] Examples of drying methods include drying with a dryer, drying with a heated roll, drying by blowing hot air onto the film, etc. Among these, the use of a dryer is preferred because it allows for uniform and easy drying. These methods can be used alone or in combination of two or more.
[0142] (Thickness) The thickness of the adhesive sheet (adhesive layer) is not particularly limited, and if the thickness is 10 μm or more, the handleability is good, and if the thickness is 1000 μm or less, it can contribute to making the adhesive sheet thinner. Therefore, the thickness of the pressure-sensitive adhesive sheet is preferably 10 μm or more, more preferably 15 μm or more, particularly preferably 20 μm or more, and even more preferably 25 μm or more. On the other hand, the upper limit is preferably 1000 μm or less, more preferably 500 μm or less, particularly preferably 250 μm or less, further preferably 100 μm or less, and particularly preferably 75 μm or less.
[0143] The pressure-sensitive adhesive sheet may be a single-layer sheet consisting of only a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition (I), or a multilayer sheet in which a plurality of other pressure-sensitive adhesive layers are laminated.
[0144] <Physical properties of adhesive sheet (adhesive layer)> The pressure-sensitive adhesive sheet (pressure-sensitive adhesive layer) may have the following physical properties.
[0145] (Storage shear modulus) The pressure-sensitive adhesive sheet preferably has a storage shear modulus at 25° C. (G'(25° C.)) of 5 kPa to 100 kPa, as determined by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz. By having a storage shear modulus at 25° C. (G'(25° C.)) of 100 kPa or less, the interlaminar stress during bending of the laminate can be reduced, and delamination and cracking of the first and second members can be suppressed. From this viewpoint, the storage shear modulus at 25° C. (G′(25° C.)) is preferably 90 kPa or less, more preferably 80 kPa or less, and particularly preferably 70 kPa or less. The lower limit of the storage shear modulus (G'(25°C)) of the pressure-sensitive adhesive sheet is preferably 5 kPa or more from the viewpoints of preventing adhesive extrusion and maintaining the shape of the pressure-sensitive adhesive sheet.
[0146] The storage shear modulus (G'(-20°C)) of the pressure-sensitive adhesive sheet at -20°C, obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, is typically 1000 kPa or less, preferably 400 kPa or less, particularly preferably 300 kPa or less, and even more preferably 250 kPa or less. The lower limit of the storage shear modulus (G'(-20°C)) of the pressure-sensitive adhesive sheet is preferably 50 kPa or more in view of the balance with the storage shear modulus at high temperatures.
[0147] When the storage shear modulus (G'(-20°C)) of the adhesive sheet is within the above range, for example, when the adhesive sheet is attached to a component sheet to form a laminate or a laminate for an image display device, the interlayer stress when the laminate or the laminate for an image display device is folded can be reduced, particularly at low to high temperatures, and delamination or cracking of the component sheet or the components of a flexible image display device can be suppressed.
[0148] The storage shear modulus (G'(-30°C)) of the pressure-sensitive adhesive sheet at -30°C, obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, is preferably 1200 kPa or less, more preferably 1000 kPa or less, even more preferably 800 kPa or less, particularly preferably 700 kPa or less, and even more preferably 500 kPa or less. The lower limit of the storage shear modulus (G'(-30°C)) of the pressure-sensitive adhesive sheet is preferably 100 kPa or more in view of the balance with the storage shear modulus at high temperatures.
[0149] When the storage shear modulus (G'(-30°C)) of the pressure-sensitive adhesive sheet is within the above range, when the pressure-sensitive adhesive sheet is adhered to a first member and a second member to form a laminate, the interlayer stress when the laminate is folded can be reduced, particularly at low to high temperatures, and delamination and cracking of the first and second members can be suppressed.
[0150] In order to obtain high adhesiveness, the pressure-sensitive adhesive sheet preferably has a storage shear modulus at 60°C (G'(60°C)) of 50 kPa or less, more preferably 40 kPa or less, particularly preferably 35 kPa or less, and even more preferably 30 kPa or less, as determined by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz. The lower limit of the storage shear modulus (G'(60°C)) is preferably 1 kPa or more from the viewpoints of preventing adhesive extrusion and maintaining the shape of the pressure-sensitive adhesive sheet.
[0151] In order to obtain high adhesiveness, the pressure-sensitive adhesive sheet preferably has a storage shear modulus at 80°C (G'(80°C)) of 30 kPa or less, more preferably 25 kPa or less, particularly preferably 20 kPa or less, and even more preferably 15 kPa or less, as determined by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz. The lower limit of the storage shear modulus (G'(80°C)) is preferably 1 kPa or more from the viewpoints of preventing adhesive overflow and maintaining the shape of the pressure-sensitive adhesive sheet.
[0152] (Maximum point of loss tangent (tan δ) and glass transition temperature (Tg)) The pressure-sensitive adhesive sheet preferably has a maximum point of loss tangent (tan δ) obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz at -20°C or higher, more preferably at -15°C or higher, particularly preferably at -10°C or higher, and even more preferably at -5°C or higher. The upper limit is usually 40°C. The maximum point of the loss tangent (tan δ) can be interpreted as the glass transition temperature (Tg), and when the glass transition temperature (Tg) is in the above range, it tends to be easier to adjust the storage shear modulus (G'(25°C)) of the pressure-sensitive adhesive sheet to 5 kPa or more and 100 kPa or less.
[0153] When only one inflection point is observed in the loss tangent (tan δ) obtained by dynamic viscoelastic measurement in the shear mode at a frequency of 1 Hz, in other words, when the tan δ curve exhibits a unimodal shape, the glass transition temperature (Tg) can be considered to be single.
[0154] The "maximum point" of the loss tangent (tan δ) means the peak value in the tan δ curve, that is, the point having the maximum value in a specified range or the entire range among the inflection points where the value changes from positive (+) to negative (-) when differentiated.
[0155] (loss tangent (tanδ)) The pressure-sensitive adhesive sheet preferably has a loss tangent (tan δ) at 25 to 60° C., as determined by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, of 0.18 or more, more preferably 0.20 or more, and particularly preferably 0.25 or more. The upper limit is usually 1. When the loss tangent (tan δ) at 25 to 60° C. is equal to or more than the above value, the pressure-sensitive adhesive sheet has excellent impact resistance.
[0156] The storage shear modulus G' and loss tangent (tan δ) at various temperatures can be measured using a rheometer.
[0157] The storage shear modulus (G') and loss tangent (tan δ) can be adjusted to the above ranges by adjusting the types and weight average molecular weights of the components (e.g., the acrylic copolymer (A) and the radically polymerizable compound (B)) contained in the pressure-sensitive adhesive composition (I) and further adjusting the gel fraction of the pressure-sensitive adhesive sheet, etc. However, the method is not limited to this.
[0158] (Gel fraction) The gel fraction of the pressure-sensitive adhesive sheet is preferably 95% or less, more preferably 90% or less, and even more preferably 85% or less. By having the gel fraction of the pressure-sensitive adhesive sheet be equal to or less than the above numerical value, the adhesive strength to a flexible member can be increased. The lower limit is preferably 30% or more, more preferably 40% or more, and particularly preferably 50% or more. By having the gel fraction be equal to or more than the above lower limit, the shape tends to be sufficiently maintained.
[0159] The gel fraction is measured, for example, as follows. The adhesive sheet, the mass of which has been measured in advance, and a 150-mesh SUS wire mesh are prepared. Next, the adhesive sheet is wrapped in the SUS wire mesh and immersed in ethyl acetate at 23°C for 24 hours. After that, the sheet is dried at 70°C for 4.5 hours, and the mass of the sheet and the SUS wire mesh are measured. The mass of the insoluble adhesive sheet remaining in the wire mesh (mass after immersion) is calculated by subtracting the mass of the SUS wire mesh from the mass of the sheet. The gel fraction (%) is calculated as the percentage of the mass of the insoluble adhesive sheet remaining in the wire mesh (mass after immersion) relative to the mass of the adhesive sheet before immersion in ethyl acetate (mass before immersion).
[0160] (Adhesive strength) The pressure-sensitive adhesive sheet has an adhesive strength to polyimide at 23° C. (P(23° C.)) of usually 3.5 N / cm or more, preferably 3.6 N / cm or more, more preferably 3.8 N / cm or more, and even more preferably 4.0 N / cm or more. Also, the adhesive strength to polyimide at 60°C (P(60°C)) is usually 1.4 N / cm or more, more preferably 1.5 N / cm or more, even more preferably 1.6 N / cm or more, and particularly preferably 1.7 N / cm or more. A pressure-sensitive adhesive sheet whose adhesive strength to polyimide satisfies the above range has excellent adhesiveness over a wide temperature range, and is less likely to cause delamination even when the laminate is folded, so it tends to have excellent durability. Specifically, the adhesive strength can be measured by the method described in the Examples below.
[0161] (Transparency, Haze) The pressure-sensitive adhesive sheet has transparency when visually observed, and transparency indicates that each component is uniformly dissolved in the sheet.
[0162] Moreover, the pressure-sensitive adhesive sheet preferably has a total light transmittance of 80% or more, more preferably 85% or more, and particularly preferably 90% or more. When the pressure-sensitive adhesive sheet has a total light transmittance of the above value or more, it tends to be suitable for use in image display devices.
[0163] Furthermore, the pressure-sensitive adhesive sheet preferably has a haze of 5% or less, more preferably 4% or less, and particularly preferably 1% or less. When the haze of the pressure-sensitive adhesive sheet is equal to or less than the above-mentioned value, the sheet tends to be suitable for use in image display devices.
[0164] In order to set the total light transmittance and haze of the pressure-sensitive adhesive sheet within the above ranges, it is preferable that the pressure-sensitive adhesive sheet does not contain particles such as organic particles.
[0165] <Method of manufacturing the present laminate> The present laminate is obtained by laminating the first member and the second member via the pressure-sensitive adhesive sheet.
[0166] Alternatively, the present laminate can be obtained by preparing the pressure-sensitive adhesive composition (I), coating the pressure-sensitive adhesive composition (I) onto a first member and / or a second member, curing the pressure-sensitive adhesive composition (I), and laminating the first member and / or the second member having a pressure-sensitive adhesive layer.
[0167] The thickness of the present laminate is preferably 1000 μm or less, more preferably 900 μm or less, and particularly preferably 800 μm or less.
[0168] <<Image display devices>> An image display device according to an embodiment of the present invention (hereinafter, sometimes referred to as "the image display device") includes the present laminate. For example, the present image display device including the present laminate can be formed by laminating the present laminate on other components of the image display device.
[0169] (Image display device components) Examples of the other image display device constituent members include flexible displays such as organic electroluminescence (EL) displays, cover lenses (cover films), polarizing plates, polarizers, retardation films, barrier films, viewing angle compensation films, brightness improvement films, contrast improvement films, diffusion films, semi-transmissive reflective films, electrode films, transparent conductive films, metal mesh films, touch sensor films, etc. These may be used alone or in combination of two or more.
[0170] The image display device of the present invention has excellent impact resistance because it includes the present laminate. EXAMPLES
[0171] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited to these examples. In the examples, "parts" refers to parts by mass.
[0172] [Example 1] A pressure-sensitive adhesive composition solution was obtained by uniformly mixing 100 parts of an acrylic copolymer (weight average molecular weight: 770,000) obtained by copolymerizing 60 parts of 2-ethylhexyl acrylate, 15 parts of butyl acrylate, 5 parts of methyl acrylate, and 20 parts of 2-hydroxyethyl acrylate with 75 parts of a monofunctional urethane acrylate (manufactured by AGC Corporation) containing an oxypropylene structure as a radical polymerizable compound, 2 parts of a mixture of 4-methylbenzophenone and 2,4,6-trimethylbenzophenone ("Esacure TZT", manufactured by IGM Corporation) as a photopolymerization initiator, 0.5 parts of 3-glycidoxypropyltrimethoxysilane ("KBM403", manufactured by Shin-Etsu Silicones Co., Ltd.) as a silane coupling agent, and ethyl acetate as a solvent.
[0173] The pressure-sensitive adhesive composition solution was coated onto a heavy release film (a silicone release-treated polyester film, manufactured by Mitsubishi Chemical Corporation, thickness 100 μm) so that the thickness after drying would be 70 μm. After coating, the film was placed in a dryer heated to a temperature of 90° C. and held for 7 minutes to volatilize and dry the solvent contained in the pressure-sensitive adhesive composition. Furthermore, a light release film (polyester film with silicone release treatment, manufactured by Mitsubishi Chemical Corporation, thickness 50 μm) was laminated on the surface of the pressure-sensitive adhesive composition from which the solvent had been dried to form a laminate, and a high-pressure mercury lamp was used to irradiate the pressure-sensitive adhesive composition through the release film with an integrated light dose of 1000 mJ / cm at a wavelength of 365 nm. 2 The adhesive composition was cured by irradiating with ultraviolet light so as to obtain an adhesive sheet with a release film. In addition, a polyimide film (thickness 25 μm, elastic modulus (E') 2 GPa) was prepared as the first member, and UTG (thickness 50 μm, elastic modulus (E') 70 GPa) was prepared as the second member. The light release film was removed from the pressure-sensitive adhesive sheet with release film, and the exposed adhesive surface was bonded to the first member. Thereafter, the heavy release film was removed, and the exposed adhesive surface was bonded to the second member to obtain a laminate.
[0174] [Comparative Example 1] 100 parts of an acrylic copolymer (weight average molecular weight: 250,000) copolymerized with 27 parts of 2-ethylhexyl acrylate, 20 parts of methyl acrylate, 9 parts of methyl methacrylate, 38 parts of isobutyl acrylate, and 6 parts of N-vinylpyrrolidone, were mixed uniformly with 1.5 parts of polypropylene glycol #400 diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Ester APG-400") as a radical polymerizable compound, 1.75 parts of methylbenzoyl formate (manufactured by IGM Co., Ltd., "Omnirad MBF") as a photopolymerization initiator, 0.75 parts of 4-methallyloyloxybenzophenone, 0.2 parts of 3-glycidoxypropyltrimethoxysilane ("KBM403", manufactured by Shin-Etsu Silicones Co., Ltd.) as a silane coupling agent, and ethyl acetate as a solvent to obtain a pressure-sensitive adhesive composition solution.
[0175] The pressure-sensitive adhesive composition solution was coated onto a heavy release film (polyester film with silicone release treatment, thickness 100 μm, manufactured by Mitsubishi Chemical Corporation) so that the thickness after drying would be 75 μm. After coating, the film was placed in a dryer heated to a temperature of 90° C. and held for 7 minutes to volatilize and dry the solvent contained in the pressure-sensitive adhesive composition. Furthermore, a light release film (polyester film with silicone release treatment, manufactured by Mitsubishi Chemical Corporation, thickness 50 μm) was laminated on the surface of the pressure-sensitive adhesive composition from which the solvent had been dried to form a laminate, and a high-pressure mercury lamp was used to irradiate the pressure-sensitive adhesive composition through the release film with an integrated light amount of 2250 mJ / cm at a wavelength of 365 nm. 2 The adhesive composition was cured by irradiating with ultraviolet light so as to obtain an adhesive sheet with a release film. In addition, a polyimide film (thickness 25 μm, elastic modulus (E') 2 GPa) was prepared as the first member, and UTG (thickness 50 μm, elastic modulus (E') 70 GPa) was prepared as the second member. The light release film was removed from the pressure-sensitive adhesive sheet with release film, and the exposed adhesive surface was bonded to the first member. Thereafter, the heavy release film was removed, and the exposed adhesive surface was bonded to the second member to obtain a laminate.
[0176] The results of measurement and evaluation of the above-obtained Examples, Comparative Examples, and Reference Examples according to the measurement and evaluation methods described above are shown in Table 1 below.
[0177] <Elastic modulus (E')> The release films were removed from the pressure-sensitive adhesive sheets with release films produced in the Examples and Comparative Examples, and a plurality of pressure-sensitive adhesive sheets were laminated to form a laminate having a thickness of 1.0 mm. A cylindrical body with a diameter of 8 mm (height of 1.0 mm) was punched out from the obtained laminate of pressure-sensitive adhesive sheets, and this was used as a sample. The temperature dispersion of dynamic viscoelasticity of the sample was measured under the following measurement conditions using a viscoelasticity measuring device (manufactured by TA Instruments, product name "DHR 2"). From the obtained temperature dispersion data of dynamic viscoelasticity, the storage shear modulus (G') at 25°C was read and substituted into the following equation to obtain the elastic modulus (E'). Elastic modulus (E') = 2G' x (1 + ν) where ν is Poisson's ratio (0.493). (Measurement conditions) Measurement tool: Φ8mm parallel plate Distortion: 0.1% Frequency: 1Hz ·Measurement temperature: -60~100℃ Heating rate: 5℃ / min
[0178] <Maximum pressure, compression displacement (analysis)> An impact analysis model was created using LS-DYNA (impact analysis software) manufactured by Ansys, Inc., and the elastic modulus (E') of the adhesive layer prepared in the examples and comparative examples was used as the set value for the following impact analysis program. Impact analysis was then performed on this model to determine the maximum pressure acting on the first member and the compressive displacement of the first member.
[0179] (Analysis model) Ansys LS-DYNA was used as modeling software to create an impact test model (including a test specimen, an impactor for impacting the test specimen, and a floor surface on which the test specimen was placed) shown in Fig. 1. The test specimen was an analysis model of a laminate in which the first member, the pressure-sensitive adhesive layers prepared in the Examples and Comparative Examples, and the second member were laminated in this order.
[0180] (Setting physical properties) The test specimen, support stand, impactor, and test conditions were set as described below. (1) Test specimen First component Thickness: 120um Elastic modulus: 5GPa Poisson's ratio: 0.2 Material model: Elastic body model Second component Thickness: 560um Elastic modulus: 70GPa Poisson's ratio: 0.2 Material model: Elastic body model Adhesive layer The thickness and elastic modulus values of the pressure-sensitive adhesive layer prepared in the Examples were used as set values. Poisson's ratio: 0.493 (2) Support stand Thickness: 1000um Elastic modulus: 75GPa Poisson's ratio: 0.2 Material model: Elastic body model (3) Floor surface Material: Rigid floor Friction coefficient: 0.5 (4) Impactor Ball material: Iron Weight: 0.5kg (5) Test conditions Impactor drop height: 30cm (natural fall; initial velocity 0) Impactor drop surface: Second component surface Test temperature: 25℃
[0181] <Shock absorption (actual measurement)> The release film was removed from the pressure-sensitive adhesive sheet prepared in the examples, and a 25 μm-thick polyimide film was roll-pressed onto the exposed adhesive surface using a hand roller. The remaining release film was removed, and pressure-sensitive paper (MS type manufactured by Fujifilm Corporation) was attached to the exposed adhesive surface to prepare a sample for measuring the impact absorption rate. The sample was placed on a stone surface plate with the polyimide film side facing up, and a stainless steel ball weighing 2 g was allowed to fall freely from a height of 50 mm above the center of the sample. The maximum pressure (P1) received by the pressure-sensitive paper that received the impact of the falling ball through the polyimide film and the adhesive layer was read using a Fujifilm Corporation Prescale pressure image analysis system "FPD-8010J."
[0182] As a reference example, a stainless steel ball weighing 2g was dropped freely from a height of 50mm onto the surface of pressure-sensitive paper (MS type manufactured by Fujifilm Corporation). The maximum stress (P0) received by the pressure-sensitive paper that received the impact of the ball directly, without passing through the adhesive layer, was read using Fujifilm Corporation's Prescale pressure image analysis system "FPD-8010J." The impact absorption rate (%) was calculated by substituting the maximum pressure (P0) when the impact was received directly from a falling ball and the maximum pressure (P1) when the impact was received through the adhesive layer into the following formula. Impact absorption rate (%) = 100 x (P0-P1) / P0 Regarding the impact absorption, those having an impact absorption rate of 5% or more were judged as ◯ (Good), and those having an impact absorption rate of less than 5% were judged as × (Poor).
[0183] [Table 1]
[0184] The laminate using the pressure-sensitive adhesive sheet (adhesive layer) of the embodiment has a maximum pressure of 18 MPa or less and a compression displacement of 8 mm as determined by an impact analysis program. 3 The results showed excellent shock absorption in an actual ball drop test. On the other hand, the laminate using the comparative pressure-sensitive adhesive sheet (adhesive layer) had maximum pressure and compression displacement values that were not within the specified ranges as calculated by the impact analysis program, and also had poor impact absorption properties in an actual ball drop test. Therefore, it is clear from these results that the above-mentioned indexes obtained by the impact analysis program have a high degree of consistency with actual impact resistance. Therefore, the laminate of Example 1 has excellent impact resistance. [Industrial Applicability]
[0185] The laminate of the present invention has excellent impact resistance and can therefore be suitably used in image displays, particularly organic EL image displays. [Explanation of symbols]
[0186] 1. Adhesive layer 2. First Component 3 Second component 4 Support stand 5. Impactor
Claims
1. A laminate comprising a first member and a second member disposed on the first member via a pressure-sensitive adhesive layer, The storage modulus (E1) of the first member is lower than the storage modulus (E2) of the second member; The pressure-sensitive adhesive layer is a pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition (I) containing an acrylic copolymer (A), and the maximum pressure acting on a first member, as determined by the following impact analysis program (1) using impact analysis software, is 18 MPa or less. <Impact Analysis Program (1)> (Analysis model) A model including a test specimen, an impactor for impacting the test specimen, and a support for placing the test specimen. (Test specimen) A laminate in which a first member, a pressure-sensitive adhesive layer, and a second member are laminated in this order. (Setting physical properties) (1) Test specimen First member Thickness: 120 μm Elastic modulus: 5 GPa Poisson's ratio: 0.2 Material model: Elastic body model Second member Thickness: 560 μm Elastic modulus: 70 GPa Poisson's ratio: 0.2 Material model: Elastic body model ・Adhesive layer Thickness: 50 to 100 μm Poisson's ratio: 0.493 Material model: Hyperelastic material model (2) Support stand Thickness: 1000μm Elastic modulus: 75 GPa Poisson's ratio: 0.2 Material model: Elastic body model (3) Impactor Ball material: iron Weight: 0.5kg (4) Test conditions Impactor drop height: 30cm (natural drop; initial velocity 0) Impactor drop surface: Second component surface Test temperature: 25°C
2. A laminate comprising a first member and a second member disposed on the first member via a pressure-sensitive adhesive layer, The storage modulus (E1) of the first member is lower than the storage modulus (E2) of the second member; The pressure-sensitive adhesive layer is a pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition (I) containing an acrylic copolymer (A), and the compressive displacement of the first member is less than 8 mm as determined by the following impact analysis program (2) using impact analysis software. 3 The laminate is as follows: <Impact Analysis Program (2)> (Analysis model) A model including a test specimen, an impactor for impacting the test specimen, and a support for placing the test specimen. (Test specimen) A laminate in which a first member, a pressure-sensitive adhesive layer, and a second member are laminated in this order. (Setting physical properties) (1) Test specimen First member Thickness: 120 μm Elastic modulus: 5 GPa Poisson's ratio: 0.2 Material model: Elastic body model ・Second member Thickness: 560 μm Elastic modulus: 70 GPa Poisson's ratio: 0.2 Material model: Elastic body model ・Adhesive layer Thickness: 50 to 100 μm Poisson's ratio: 0.493 Material model: Hyperelastic material model (2) Support stand Thickness: 1000μm Elastic modulus: 75 GPa Poisson's ratio: 0.2 Material model: Elastic body model (3) Impactor Ball material: iron Weight: 0.5kg (4) Test conditions Impactor drop height: 30cm (natural drop; initial velocity 0) Impactor drop surface: Second component surface Test temperature: 25°C
3. 3. The laminate according to claim 1, wherein the pressure-sensitive adhesive layer has a storage shear modulus (G'(25)) at 25°C obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz of 5 kPa or more and 100 kPa or less.
4. The laminate according to claim 1 or 2, wherein the pressure-sensitive adhesive layer has a gel fraction of 30% or more and 95% or less.
5. The laminate according to claim 1 or 2, wherein the pressure-sensitive adhesive layer has a glass transition temperature (Tg) of -20°C or higher, defined as the maximum value of Tan δ, obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz.
6. The laminate according to claim 1 or 2, wherein the pressure-sensitive adhesive composition (I) comprises a radically polymerizable compound (B) and a photopolymerization initiator (C).
7. The laminate according to claim 6, wherein the photopolymerization initiator (C) comprises a photopolymerization initiator (C1) having, in its molecule, a radically polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals.
8. The laminate according to claim 1 or 2, wherein the thickness of the laminate is 1000 μm or less.
9. The laminate according to claim 1 or 2, wherein the first member and the second member are components of an image display device selected from the group consisting of a surface protection panel, a touch sensor, an image display panel, a color filter, a polarizing film, and a retardation film.
10. The laminate according to claim 9 , wherein the first member is an image display panel, and the second member is a surface protection panel.
11. An image display device comprising the laminate according to claim 9 .
12. An adhesive sheet for bonding and integrating a first member and a second member having a storage modulus (E') higher than that of the first member, the adhesive sheet being such that the maximum pressure exerted on the first member is 18 MPa or less, as determined by the following impact analysis program (1). <Impact Analysis Program (1)> (Analysis model) A model including a test specimen, an impactor for impacting the test specimen, and a support for placing the test specimen. (Test specimen) A laminate in which a first member, a pressure-sensitive adhesive layer, and a second member are laminated in this order. (Setting physical properties) (1) Test specimen First member Thickness: 120 μm Elastic modulus: 5 GPa Poisson's ratio: 0.2 Material model: Elastic body model ・Second member Thickness: 560 μm Elastic modulus: 70 GPa Poisson's ratio: 0.2 Material model: Elastic body model ・Adhesive layer Thickness: 50 to 100 μm Poisson's ratio: 0.493 Material model: Hyperelastic material model (2) Support stand Thickness: 1000μm Elastic modulus: 75 GPa Poisson's ratio: 0.2 Material model: Elastic body model (3) Impactor Ball material: iron Weight: 0.5kg (4) Test conditions Impactor drop height: 30cm (natural drop; initial velocity 0) Impactor drop surface: Second component side surface Test temperature: 25°C
Citation Information
Patent Citations
JP1974071529A
Split broadcast system
JP1985062740A
Cited By
Magnetic memory device
CN121645897A