All-solid battery

Fibrous conductive additives with controlled dimensions and electrolyte layer thickness enhance ion conduction and capacity in all-solid-state batteries, addressing alignment and defect issues.

JP2024142141APending Publication Date: 2024-10-10TAIYO YUDEN KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023054166
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing all-solid-state batteries face issues with inhibited ion conduction paths due to plate-like carbon alignment and high conductive additive ratios, leading to potential short-circuit defects and reduced capacity.

Method used

Employing fibrous conductive additives with controlled average diameters and area ratios, combined with a solid electrolyte layer thickness of 5 μm to 20 μm, to ensure effective ion conduction and prevent short-circuits.

Benefits of technology

The solution achieves both good battery operation and improved yield by ensuring sufficient conductivity, capacity, and reducing short-circuit defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide an all-solid battery that can achieve both a good battery operation and improved yield.SOLUTION: An all-solid battery includes a solid electrolyte layer, and electrode layers provided on both main surfaces of the solid electrolyte layer and containing an electrode active material and a fibrous conductive assistant, and in a cross section of the electrode layer, an average diameter of the conductive assistant is 2 nm or more and less than 150 nm, an area ratio occupied by the conductive assistant is 0.5% or more and 5.0% or less, and an area ratio occupied by the electrode active material is 28% or more and less than 80%, and a thickness of the solid electrolyte layer is 5 μm or more and 20 μm or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an all-solid-state battery. [Background technology]

[0002] All-solid-state batteries using oxide-based solid electrolytes are expected to be a technology that can provide safe secondary batteries that do not suffer from concerns about fire and toxic gas emissions, which are associated with organic electrolytes and sulfide-based solid electrolytes (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2021-034202 [Patent Document 2] International Publication No. 2014 / 042083 Summary of the Invention [Problem to be solved by the invention]

[0004] In Patent Document 1, plate-like carbon is used. Plate-like carbon is likely to be parallel to the stacking direction, and may block the ion conduction path in the stacking direction (between the positive and negative electrodes). In addition, the volume ratio of the conductive additive is high, and a large amount of the conductive additive that does not contribute to the capacity is included. Therefore, there is a risk that a high capacity will not be achieved.

[0005] Fibrous carbon is used in Patent Document 2. However, the VGCF used in Patent Document 2 has a relatively large fiber diameter of 150 nm, and may break through the solid electrolyte sheet during molding, causing a risk of short circuit failure.

[0006] The present invention has been made in consideration of the above problems, and has an object to provide an all-solid-state battery that can achieve both good battery operation and improved yield. [Means for solving the problem]

[0007] The all-solid-state battery according to the present invention comprises a solid electrolyte layer, and electrode layers provided on both main surfaces of the solid electrolyte layer and containing an electrode active material and a fibrous conductive assistant, wherein in a cross section of the electrode layer, the average diameter of the conductive assistant is 2 nm or more and less than 150 nm, the area ratio occupied by the conductive assistant is 0.5% or more and 5.0% or less, and the area ratio occupied by the electrode active material is 28% or more and less than 80%, and the thickness of the solid electrolyte layer is 5 μm or more and 20 μm or less.

[0008] In the all-solid-state battery, the conductive assistant may be a carbon material.

[0009] In the all-solid-state battery, the conductive assistant may be a carbon nanotube.

[0010] In the all-solid-state battery, the solid electrolyte layer may be an oxide.

[0011] In the all-solid-state battery, the conductive assistant may have a total length of 5 μm or more.

[0012] According to the present invention, it is possible to provide an all-solid-state battery that can achieve both good battery operation and improved yield, and a manufacturing method thereof. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a basic structure of an all-solid-state battery. [Diagram 2] FIG. [Diagram 3] FIG. 2 is a partial cross-sectional perspective view of a stacked-type all-solid-state battery in which a plurality of battery units are stacked. [Figure 4] FIG. 2 is a partial cross-sectional perspective view of a stacked-type all-solid-state battery in which a plurality of battery units are stacked. [Diagram 5] 1A and 1B are perspective views illustrating an example of a conductive additive, and FIG. 1C is a cross-sectional view illustrating a laminated positive electrode layer. [Figure 6]FIG. 1 is a diagram illustrating a flow of a method for producing an all-solid-state battery. [Figure 7] 1(a) to 1(c) are diagrams illustrating a lamination process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment will be described with reference to the drawings.

[0015] (Embodiment) Fig. 1 is a schematic cross-sectional view showing a basic structure of an all-solid-state battery 100 according to an embodiment. As illustrated in Fig. 1, the all-solid-state battery 100 has a structure in which a solid electrolyte layer 30 is sandwiched between a positive electrode layer 10 and a negative electrode layer 20. For example, the positive electrode layer 10 is formed on a first main surface of the solid electrolyte layer 30, and the negative electrode layer 20 is formed on a second main surface of the solid electrolyte layer 30. The positive electrode layer 10, the negative electrode layer 20, and the solid electrolyte layer 30 are sintered bodies.

[0016] The solid electrolyte layer 30 is mainly composed of a solid electrolyte having ion conductivity. The solid electrolyte of the solid electrolyte layer 30 is, for example, an oxide-based solid electrolyte having lithium ion conductivity. The solid electrolyte is, for example, a phosphate-based solid electrolyte having a NASICON structure. The phosphate-based solid electrolyte having a NASICON structure has a high electrical conductivity and is stable in the air. The phosphate-based solid electrolyte is, for example, a phosphate containing lithium. The phosphate is not particularly limited, but examples thereof include a composite lithium phosphate salt with Ti (for example, LiTi2(PO4)3). Alternatively, Ti can be partially or completely replaced with a tetravalent transition metal such as Ge, Sn, Hf, or Zr. In order to increase the Li content, it may be partially replaced with a trivalent transition metal such as Al, Ga, In, Y, or La. More specifically, for example, Li 1+x Al x Ge 2-x (PO4)3 and Li 1+x Al x Zr 2-x (PO4)3, Li 1+x Alx Ti 2-x (PO4)3. For example, Li-Al-Ge-PO4-based material to which the same transition metal as that contained in the phosphate having an olivine crystal structure contained in the positive electrode layer 10 and the negative electrode layer 20 is added in advance is preferable. For example, when the positive electrode layer 10 and the negative electrode layer 20 contain a phosphate containing Co and Li, it is preferable that the solid electrolyte layer 30 contains a Li-Al-Ge-PO4-based material to which Co is added in advance. In this case, the effect of suppressing the elution of the transition metal contained in the electrode active material into the electrolyte can be obtained. When the positive electrode layer 10 and the negative electrode layer 20 contain a phosphate containing a transition element other than Co and Li, it is preferable that the solid electrolyte layer 30 contains a Li-Al-Ge-PO4-based material to which the transition metal is added in advance.

[0017] As illustrated in FIG. 2, the positive electrode layer 10 has a structure in which an electrode active material 11, a solid electrolyte 12, a conductive assistant 13, and the like are dispersed. The negative electrode layer 20 has a structure in which an electrode active material 21, a solid electrolyte 22, a conductive assistant 23, and the like are dispersed. The positive electrode layer 10 includes the electrode active material 11, and the negative electrode layer 20 includes the electrode active material 21, so that the all-solid-state battery 100 can be used as a secondary battery. The positive electrode layer 10 includes the solid electrolyte 12, and the negative electrode layer 20 includes the solid electrolyte 22, so that the positive electrode layer 10 and the negative electrode layer 20 have ion conductivity. The positive electrode layer 10 includes the conductive assistant 13, and the negative electrode layer 20 includes the conductive assistant 23, so that the positive electrode layer 10 and the negative electrode layer 20 have conductivity.

[0018] The electrode active material 11 is, for example, an electrode active material having an olivine crystal structure. The electrode active material having an olivine crystal structure may also be contained in the negative electrode layer 20. An example of such an electrode active material is a phosphate containing a transition metal and lithium. The olivine crystal structure is a crystal that natural olivine has, and can be identified by X-ray diffraction.

[0019] A typical example of an electrode active material having an olivine crystal structure is LiCoPO4 containing Co and P. Phosphates in which the transition metal Co is substituted in this chemical formula can also be used. The ratio of Li and PO4 can vary depending on the valence. It is preferable to use Co, Mn, Fe, Ni, etc. as the transition metal. LiCo2P3O 10 , Li2CoP2O7, Li6Co5(P2O7)4, etc. can also be used.

[0020] For example, when an electrode active material having an olivine crystal structure is contained only in the positive electrode layer 10, the electrode active material acts as a positive electrode active material. When an electrode active material having an olivine crystal structure is also contained in the negative electrode layer 20, although the mechanism of action is not completely clear, the effect of increasing the discharge capacity and increasing the operating potential with discharge is exhibited, which is presumed to be based on the formation of a partial solid solution state with the negative electrode active material.

[0021] When both the positive electrode layer 10 and the negative electrode layer 20 contain an electrode active material having an olivine crystal structure, the electrode active materials preferably contain transition metals that may be the same or different from each other. "May be the same or different from each other" means that the electrode active materials contained in the positive electrode layer 10 and the negative electrode layer 20 may contain the same type of transition metal, or may contain different types of transition metals. The positive electrode layer 10 and the negative electrode layer 20 may contain only one type of transition metal, or may contain two or more types of transition metals. Preferably, the positive electrode layer 10 and the negative electrode layer 20 contain the same type of transition metal. More preferably, the electrode active materials contained in both electrodes have the same chemical composition. If the positive electrode layer 10 and the negative electrode layer 20 contain the same type of transition metal or contain an electrode active material of the same composition, the similarity of the compositions of the two internal electrode layers is increased, so that even if the terminals of the all-solid-state battery 100 are attached in the opposite direction, the battery can withstand practical use without malfunction depending on the application.

[0022] The negative electrode layer 20 functions as a negative electrode layer by including the electrode active material 21. By including the negative electrode active material in only one electrode, it becomes clear that the one electrode acts as a negative electrode and the other electrode acts as a positive electrode. However, both electrodes may include a material that is known as a negative electrode active material. For the negative electrode active material of the electrode, reference can be made to conventional techniques in secondary batteries as appropriate, and examples thereof include compounds such as titanium oxide, lithium titanium composite oxide, lithium titanium composite phosphate, carbon, and lithium vanadium phosphate.

[0023] The solid electrolyte 12 and the solid electrolyte 22 are not particularly limited as long as they are oxide-based solid electrolytes having ion conductivity. The solid electrolyte 12 and the solid electrolyte 22 are, for example, oxide-based solid electrolytes having lithium ion conductivity. The solid electrolyte is, for example, a phosphate-based solid electrolyte having a NASICON structure. The phosphate-based solid electrolyte is, for example, a phosphate containing lithium. The phosphate is not particularly limited, but examples thereof include a composite lithium phosphate salt with Ti (for example, LiTi2(PO4)3). Alternatively, Ti can be partially or completely replaced with a tetravalent transition metal such as Ge, Sn, Hf, or Zr. In addition, in order to increase the Li content, it may be partially replaced with a trivalent transition metal such as Al, Ga, In, Y, or La. More specifically, for example, Li 1+x Al x Ge 2-x (PO4)3 and Li 1+x Al x Zr 2-x (PO4)3, Li 1+x Al x Ti 2-x (PO4)3, etc. The solid electrolyte 12 and the solid electrolyte 22 may be, for example, the same as the main component solid electrolyte of the solid electrolyte layer 30. Alternatively, when the electrode active material contains Co and P, the solid electrolytes 12 and 22 preferably contain Co. Although the detailed mechanism is unclear, the inclusion of Co during co-firing tends to improve the oxidation resistance stability of the solid electrolyte, which makes it easier to ensure cycle stability.

[0024] A carbon material or the like is used as the conductive assistants 13 and 23. A metal may be used as the conductive assistants 13 and 23. Examples of the metal for the conductive assistant include Pd, Ni, Cu, Fe, and alloys containing these metals.

[0025] 3 is a schematic cross-sectional view of a stacked type all-solid-state battery 100a in which a plurality of battery units are stacked. The all-solid-state battery 100a includes a stacked chip 60 having a substantially rectangular parallelepiped shape. In the stacked chip 60, a first external electrode 40a and a second external electrode 40b are provided so as to contact two side surfaces, which are two of the four surfaces other than the upper and lower surfaces at the ends in the stacking direction. The two side surfaces may be two adjacent side surfaces, or may be two side surfaces facing each other. In this embodiment, the first external electrode 40a and the second external electrode 40b are provided so as to contact two side surfaces facing each other (hereinafter referred to as two end surfaces).

[0026] In the following description, components having the same composition range, thickness range, and particle size distribution range as those of the all-solid-state battery 100 are denoted by the same reference numerals and detailed description thereof will be omitted.

[0027] In the all-solid-state battery 100a, a plurality of positive electrode layers 10 and a plurality of negative electrode layers 20 are alternately stacked with a solid electrolyte layer 30 interposed therebetween. The edges of the plurality of positive electrode layers 10 are exposed to the first end face of the stacked chip 60, but are not exposed to the second end face. The edges of the plurality of negative electrode layers 20 are exposed to the second end face of the stacked chip 60, but are not exposed to the first end face. As a result, the positive electrode layer 10 is electrically connected to the first external electrode 40a, and the negative electrode layer 20 is electrically connected to the second external electrode 40b. The solid electrolyte layer 30 extends from the first external electrode 40a to the second external electrode 40b. In this way, the all-solid-state battery 100a has a structure in which a plurality of battery units are stacked.

[0028] A cover layer 50 is laminated on the upper surface of the laminated structure of the positive electrode layer 10, the solid electrolyte layer 30, and the negative electrode layer 20 (in the example of FIG. 3, the upper surface of the uppermost positive electrode layer 10). In addition, a cover layer 50 is laminated on the lower surface of the laminated structure (in the example of FIG. 3, the lower surface of the lowermost positive electrode layer 10). The cover layer 50 is mainly composed of an inorganic material (e.g., Al2O3, ZrO2, TiO2, etc.) containing, for example, Al, Zr, Ti, etc. The cover layer 50 may contain the main component of the solid electrolyte layer 30 as a main component. The cover layer 50 is a sintered body.

[0029] The positive electrode layer 10 and the negative electrode layer 20 may each include a current collector layer. For example, as illustrated in FIG. 4, a first current collector layer 15 may be provided in the positive electrode layer 10. A second current collector layer 25 may be provided in the negative electrode layer 20. The first current collector layer 15 and the second current collector layer 25 are mainly composed of a conductive material. For example, metal, carbon, etc. may be used as the conductive material of the first current collector layer 15 and the second current collector layer 25. The current collection efficiency is improved by connecting the first current collector layer 15 to the first external electrode 40a and connecting the second current collector layer 25 to the second external electrode 40b.

[0030] As described above, the positive electrode layer 10 and the negative electrode layer 20 contain a conductive assistant from the viewpoint of electrical conductivity. For example, it is possible to use a plate-shaped conductive assistant as the conductive assistant. However, the plate-shaped conductive assistant is likely to be parallel to the stacking direction, and may obstruct the ion conduction path between the positive electrode layer 10 and the negative electrode layer 20. In addition, the volume ratio of the conductive assistant may be high, and a high capacity may not be achieved. Therefore, it is possible to use a fibrous conductive assistant. However, a conductive assistant with a large fiber diameter is thick, and may break through the solid electrolyte sheet during molding, causing a short circuit.

[0031] Therefore, the all-solid-state batteries 100, 100a according to this embodiment have a configuration that can achieve both good battery operation and improved yield.

[0032] Specifically, a fibrous conductive material is used as the conductive assistant 13, 23. By using the fibrous conductive material, the width of the conductive assistant 13, 23 is reduced, so that an ion conduction path between the positive electrode layer 10 and the negative electrode layer 20 can be secured more securely than in the case where plate-like carbon is used.

[0033] Next, in the cross section of the positive electrode layer 10, the average diameter of the conductive assistant 13 is 2 nm or more and less than 150 nm, the area ratio occupied by the conductive assistant 13 is 0.5% or more and 5.0% or less, and the area ratio occupied by the electrode active material 11 is 28% or more and less than 80%. In addition, in the cross section of the negative electrode layer 20, the average diameter of the conductive assistant 23 is 2 nm or more and less than 150 nm, the area ratio occupied by the conductive assistant 23 is 0.5% or more and 5.0% or less, and the area ratio occupied by the electrode active material 21 is 28% or more and less than 80%. In addition, the thickness of the solid electrolyte layer 30 is 5 μm or more and 20 μm or less. Note that the cross section of the stacked layers here is a cross section including the stacking direction, and is a cross section formed by the stacking direction and the direction in which the first external electrode 40a and the second external electrode 40b face each other.

[0034] According to this configuration, the conductive assistants 13, 23 have a small average diameter of less than 150 nm, so that the conductive assistants 13, 23 are thin and flexible. This prevents the conductive assistants 13, 23 from breaking through the solid electrolyte green sheet before firing, and thus prevents short circuit defects. Meanwhile, the conductive assistants 13, 23 have an average diameter of 2 nm or more, so that sufficient conductivity can be achieved.

[0035] Next, sufficient conductivity is obtained by setting the area ratio of the conductive assistant 13 in the positive electrode layer 10 and the area ratio of the conductive assistant 23 in the negative electrode layer 20 to 0.5% or more. As a result, sufficient rate characteristics and sufficient battery capacity are obtained. On the other hand, the content of the electrode active material and solid electrolyte can be ensured by setting the area ratio of the conductive assistants 13 and 23 to 5.0% or less.

[0036] Next, the electrode active material content can be ensured by setting the area ratio of the electrode active material 11 in the positive electrode layer 10 and the area ratio of the electrode active material 21 in the negative electrode layer 20 to 28% or more, thereby ensuring the battery capacity. On the other hand, the solid electrolyte content can be ensured by setting the area ratio of the electrode active material 11 in the positive electrode layer 10 and the area ratio of the electrode active material 21 in the negative electrode layer 20 to less than 80%.

[0037] Next, by making the thickness of the solid electrolyte layer 30 5 μm or more, the thickness of the solid electrolyte layer is ensured sufficiently, and breakthrough by the conductive assistants 13, 23, etc. can be suppressed. This makes it possible to suppress short circuit defects. On the other hand, by making the thickness of the solid electrolyte layer 30 20 μm or less, rate characteristics can be ensured.

[0038] From the above, the all-solid-state batteries 100, 100a according to this embodiment can achieve both good battery operation and improved yield.

[0039] From the viewpoint of making the conductive assistants 13 and 23 sufficiently thin, the average diameter of the conductive assistants 13 and 23 in the laminate cross section is preferably 130 nm or less, and more preferably 80 nm or less.

[0040] On the other hand, from the viewpoint of realizing sufficient electrical conductivity or sufficient thermal stability, the average diameter of the electrical conductivity assistants 13, 23 in the laminate cross section is preferably 5 nm or more, and more preferably 8 nm or more.

[0041] In addition, from the viewpoint of achieving sufficient conductivity, the area ratio of the conductive assistant 13 in the positive electrode layer 10 and the area ratio of the conductive assistant 23 in the negative electrode layer 20 in the laminate cross section are preferably 0.6% or more, and more preferably 0.7% or more.

[0042] On the other hand, from the viewpoint of ensuring the content of the electrode active material and the solid electrolyte, the area ratio of the conductive assistant 13 in the positive electrode layer 10 and the area ratio of the conductive assistant 23 in the negative electrode layer 20 in the laminate cross section are preferably 4.5% or less, and more preferably 4% or less.

[0043] In addition, from the viewpoint of ensuring the content of the electrode active material, the area ratio of the electrode active material 11 in the positive electrode layer 10 and the area ratio of the electrode active material 21 in the negative electrode layer 20 in the laminate cross section are preferably 30% or more, and more preferably 40% or more.

[0044] On the other hand, from the viewpoint of ensuring the solid electrolyte content, the area ratio of the electrode active material 11 in the positive electrode layer 10 and the area ratio of the electrode active material 21 in the negative electrode layer 20 are preferably 75% or less, and more preferably 70% or less.

[0045] From the viewpoint of preventing breakthrough by the conductive assistants 13, 23, etc., the thickness of the solid electrolyte layer 30 is preferably 6 μm or more, and more preferably 7 μm or more.

[0046] On the other hand, from the viewpoint of ensuring rate characteristics, the thickness of the solid electrolyte layer 30 is preferably 19 μm or less, and more preferably 18 μm or less.

[0047] The material of the conductive assistants 13 and 23 is not particularly limited as long as it is a material having conductivity, but is preferably a carbon material. Since the carbon material is soft, it is possible to suppress the breakthrough of the solid electrolyte layer 30. For example, it is preferable to use carbon nanotubes as the conductive assistants 13 and 23. Since the carbon nanotubes have a hollow fiber shape and are soft, it is possible to suppress the breakthrough of the solid electrolyte layer 30.

[0048] Fig. 5(a) is a perspective view illustrating the conductive assistant 13, 23. As illustrated in Fig. 5(a), the conductive assistant 13, 23 has a fibrous shape and has a long diameter and a short diameter. The aspect ratio (long diameter:short diameter), which is the ratio of the long diameter to the short diameter, is preferably 100:1 to 3000:1, more preferably 125:1 to 1000:1, and further preferably 150:1 to 500:1.

[0049] In order to ensure a sufficient conductive distance, the overall length of the conductive assistants 13, 23 is preferably 1.5 μm or more, more preferably 2.5 μm or more, and even more preferably 5 μm or more.

[0050] The conductive assistants 13, 23 do not need to extend linearly in the positive electrode layer 10 and the negative electrode layer 20, and may be curved as shown in Fig. 5(b) . When carbon nanotubes are used, the hollow portions may be voids or may be filled with other materials.

[0051] FIG. 5(c) is a diagram illustrating a cross section of the stacked layers of the positive electrode layer 10. The cross section of the stacked layers can be exposed by polishing or otherwise removing the all-solid-state battery 100, 100a. The cross section of the stacked layers can be observed with a scanning electron microscope (SEM) or the like. The average diameter of the conductive assistant 13 can be calculated by randomly observing 300 conductive assistants 13, measuring the shortest part, and averaging the measured values. The average diameter of the conductive assistant 23 in the negative electrode layer 20 can also be measured by the same procedure.

[0052] The thickness of the solid electrolyte layer 30 can be measured by observing a cross section of the stack of the all-solid-state batteries 100, 100a with an SEM, measuring the thickness at ten different points in one layer, and deriving the average value.

[0053] Next, a description will be given of a method for manufacturing the all-solid-state battery 100a illustrated in Fig. 3. Fig. 6 is a diagram illustrating a flow of the method for manufacturing the all-solid-state battery 100a.

[0054] (Process for producing raw powder for solid electrolyte layer) First, a raw material powder for the solid electrolyte layer constituting the above-mentioned solid electrolyte layer 30 is prepared. For example, raw materials, additives, etc. are mixed, and a solid-phase synthesis method or the like is used to prepare raw material powder for an oxide-based solid electrolyte. The obtained raw material powder can be dry-milled to adjust to a desired average particle size. For example, a planetary ball mill using 5 mmφ ZrO2 balls is used to adjust to a desired average particle size.

[0055] (Cover layer raw powder preparation process) First, the raw material powder of the ceramics constituting the above-mentioned cover layer 50 is prepared. For example, the raw material powder for the cover layer can be prepared by mixing the raw materials, additives, etc., and using a solid-phase synthesis method, etc. The obtained raw material powder can be adjusted to a desired average particle size by dry pulverizing. For example, the desired average particle size is adjusted using a planetary ball mill using 5 mmφ ZrO2 balls.

[0056] (Electrode layer paste preparation process) Next, the internal electrode pastes for producing the above-mentioned positive electrode layer 10 and negative electrode layer 20 are separately prepared. For example, the electrode active material and the solid electrolyte material are highly dispersed using a bead mill or the like to produce a ceramic paste consisting only of ceramic particles. The conductive assistants 13 and 23 are mixed into this ceramic paste. Since the fibrous carbon is entangled, a dispersion process is performed using a solvent for the paste and an appropriate dispersant using an ultrasonic homogenizer or a wet jet mill. The ceramic paste, the dispersion of the conductive assistants 13 and 23, and the binder are mixed to produce the electrode layer paste.

[0057] The sintering aid of the internal electrode paste contains one or more glass components such as Li-BO based compounds, Li-Si-O based compounds, Li-CO based compounds, Li-SO based compounds, and Li-PO based compounds.

[0058] (External electrode paste manufacturing process) Next, an external electrode paste for producing the above-mentioned first external electrode 40a and second external electrode 40b is prepared. For example, the external electrode paste can be obtained by uniformly dispersing a conductive material, a glass frit, a binder, a plasticizer, etc. in water or an organic solvent.

[0059] (Solid electrolyte green sheet manufacturing process) The raw material powder for the solid electrolyte layer is uniformly dispersed in an aqueous or organic solvent together with a binder, a dispersant, a plasticizer, etc., and wet-pulverized to obtain a solid electrolyte slurry having a desired average particle size. At this time, a bead mill, a wet jet mill, various kneaders, a high-pressure homogenizer, etc. can be used, and it is preferable to use a bead mill from the viewpoint of simultaneously adjusting the particle size distribution and dispersing. A binder is added to the obtained solid electrolyte slurry to obtain a solid electrolyte paste. The obtained solid electrolyte paste is coated to produce a solid electrolyte green sheet 51. The coating method is not particularly limited, and a slot die method, a reverse coat method, a gravure coat method, a bar coat method, a doctor blade method, etc. can be used. The particle size distribution after wet-pulverization can be measured, for example, using a laser diffraction measurement device using a laser diffraction scattering method.

[0060] (Lamination process) As illustrated in FIG. 7(a), the internal electrode paste 52 is printed on one side of the solid electrolyte green sheet 51. In the area on the solid electrolyte green sheet 51 where the internal electrode paste 52 is not printed, the reverse pattern 53 is printed. The reverse pattern 53 can be the same as the solid electrolyte green sheet 51. A plurality of printed solid electrolyte green sheets 51 are alternately shifted and stacked. As illustrated in FIG. 7(b), a laminate is obtained by pressing the cover sheets 54 from above and below in the stacking direction. In this case, a laminate having a substantially rectangular parallelepiped shape is obtained so that the internal electrode paste 52 for the positive electrode layer 10 is exposed on one end surface of the laminate and the internal electrode paste 52 for the negative electrode layer 20 is exposed on the other end surface of the laminate. The cover sheet 54 can be formed by applying the raw material powder for the cover layer in the same manner as in the solid electrolyte green sheet preparation process. The cover sheet 54 is formed to be thicker than the solid electrolyte green sheet 51. It may be made thicker during coating, or it may be made thicker by stacking multiple coated sheets.

[0061] Next, the external electrode paste 55 is applied to each of the two end faces by a dipping method or the like, and then dried, thereby obtaining a molded body for forming the all-solid-state battery 100a.

[0062] (Firing process) Next, the obtained laminate is fired. The firing conditions are not particularly limited, and may be in an oxidizing or non-oxidizing atmosphere, and the maximum temperature is preferably 400°C to 1000°C, more preferably 500°C to 900°C, etc. In order to sufficiently remove the binder before the maximum temperature is reached, a step of maintaining the temperature in an oxidizing atmosphere at a temperature lower than the maximum temperature may be provided. In order to reduce process costs, it is desirable to fire at as low a temperature as possible. After firing, a reoxidation treatment may be performed. Through the above steps, an all-solid-state battery 100a is produced.

[0063] In addition, a collector layer can be formed in the positive electrode layer 10 and the negative electrode layer 20 by sequentially laminating an internal electrode paste, a collector paste containing a conductive material, and an internal electrode paste. EXAMPLES

[0064] (Examples 1 to 5) The electrode active material and solid electrolyte were highly dispersed in a bead mill to prepare a ceramic paste consisting only of ceramic particles. Carbon nanotubes were used as a conductive assistant. Since the carbon nanotubes are entangled, they were dispersed using an ultrasonic homogenizer or a wet jet mill with a solvent for the paste and an appropriate dispersant. The dispersion conditions were adjusted so that the aspect ratio of the fiber diameter of the carbon nanotubes was 100:1 to 1000:1. The ceramic paste, the carbon nanotube dispersion, and the binder were mixed to prepare an electrode paste. The electrode paste was then printed and laminated on the solid electrolyte layer, sintered, and an external electrode was formed to prepare an all-solid-state battery.

[0065] The cross section of the sintered battery was polished by ion milling and observed with a SEM to determine the thickness of the solid electrolyte layer, the average diameter and area ratio of the conductive additive contained in the electrode layer, and the area ratio of the electrode active material. The average diameter of the conductive additive was calculated by randomly measuring 300 short pieces and averaging them.

[0066] The average diameter of the conductive assistant in the electrode layer was 5 nm in Example 1, 15 nm in Example 2, 70 nm in Example 3, 130 nm in Example 4, and 2 nm in Example 5. The area ratio of the conductive assistant in the electrode layer was 0.7% in Example 1, 2.0% in Example 2, 5.0% in Example 3, 5.0% in Example 4, and 0.5% in Example 5. The thickness of the solid electrolyte layer was 20 μm in all of Examples 1 to 4, and 5 μm in Example 5. The area ratio of the electrode active material in the electrode layer was 28% in Example 1, 55% in Example 2, 79% in Example 3, 75% in Example 4, and 28% in Example 5.

[0067] Comparative Example 1 In Comparative Example 1, the cross-sectional average diameter of the conductive assistant in the electrode layer was 130 nm, the area ratio of the conductive assistant in the electrode layer was 0.4%, the thickness of the solid electrolyte layer was 20 μm, and the area ratio of the electrode active material in the electrode layer was 28%.

[0068] Comparative Example 2 In Comparative Example 2, the cross-sectional average diameter of the conductive assistant in the electrode layer was 130 nm, the area ratio of the conductive assistant in the electrode layer was 5.0%, the thickness of the solid electrolyte layer was 4 μm, and the area ratio of the electrode active material in the electrode layer was 28%.

[0069] Comparative Example 3 In Comparative Example 3, the cross-sectional average diameter of the conductive assistant in the electrode layer was 150 nm, the area ratio of the conductive assistant in the electrode layer was 5.0%, the thickness of the solid electrolyte layer was 20 μm, and the area ratio of the electrode active material in the electrode layer was 28%.

[0070] Comparative Example 4 In Comparative Example 4, the cross-sectional average diameter of the conductive assistant in the electrode layer was 130 nm, the area ratio of the conductive assistant in the electrode layer was 5.0%, the thickness of the solid electrolyte layer was 25 μm, and the area ratio of the electrode active material in the electrode layer was 28%.

[0071] (Evaluation of battery characteristics) Battery characteristics were evaluated for each of Examples 1 to 5 and Comparative Examples 1 to 4. The battery characteristics were evaluated by CC charge / discharge measurement at 25°C (charge current 0.2C-discharge current 0.2C or charge current 1C-discharge current 1C, upper cut voltage 3.6V, lower cut voltage 1.5V). The rate characteristics were calculated based on the ratio of the 1C discharge capacity when the 0.2C discharge capacity was 100%, and the ratio was judged as very good "◯" when the ratio was 70% or more, good "△" when the ratio was 60% or more, and poor "×" when the ratio was less than 60%. The capacity values ​​were compared based on the 0.2C discharge capacity. The ratio of the discharge capacity value of each battery when the discharge capacity of Example 2 was 100% was calculated, and the ratio was judged as very good "◯" when the ratio was 90% or more, good "△" when the ratio was 80% or more, and poor "×" when the ratio was less than 80%.

[0072] (Short rate) In addition, the short-circuit rate (the ratio of the number of pieces that short-circuited) of 200 samples was measured for each of Examples 1 to 5 and Comparative Examples 1 to 4. A short-circuit rate of 5% or less was judged as good (◯), and a short-circuit rate of more than 5% was judged as poor (×).

[0073] (Overall Judgment) If both the rate characteristic and the capacity value were judged to be very good (O) or good (△), and at least one of them was judged to be good (O), and the short circuit rate was judged to be good (O), the overall judgment was judged to be good (O). If the conditions for good (O) were not met in the overall judgment, the overall judgment was judged to be poor (X). The results are shown in Table 1. [Table 1]

[0074] In Examples 1 to 5, the overall evaluation was good, i.e., "◯." This is believed to be because, in the cross section of the electrode layer, the average diameter of the conductive assistant was 2 nm or more and less than 150 nm, the proportion of the electrode active material was 28% or more and less than 80%, the area proportion occupied by the conductive assistant was 0.5% or more and 5% or less, and the thickness of the solid electrolyte layer was 5 μm or more and 20 μm or less.

[0075] In Comparative Example 1, the rate characteristic was judged to be poor "x". This is believed to be because the area ratio of the conductive assistant in the electrode layer was low, resulting in low conductivity in the electrode layer. In Comparative Example 2, the short circuit rate was judged to be poor "x". This is believed to be because the solid electrolyte layer was thin, making it easier for short circuits to occur. In Comparative Example 3, the short circuit rate was also judged to be "poor". This is believed to be because the conductive assistant was thick and hard, causing the solid electrolyte layer to break through. In Comparative Example 4, the short circuit rate was judged to be good "o", but the rate characteristic and capacity value were not judged to be very good "o". This is believed to be because the solid electrolyte layer was thick, resulting in a low short circuit rate, but was unfavorable to the capacity value and rate characteristic.

[0076] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]

[0077] 10 Positive electrode layer 11 Electrode active material 12 Solid electrolyte 13 Conductive additives 15 First current collector layer 20 Negative electrode layer 21 Electrode active material 22 Solid electrolyte 23 Conductive additives 25 Second collector layer 30 Solid electrolyte layer 40a First external electrode 40b 2nd external electrode 50 Cover Layer 51 Solid electrolyte green sheet 52 Internal electrode paste 53 Reverse pattern 54 Cover Sheet 55 External electrode paste 60 Stacked Chips 70 side margin 100,100a all solid state battery

Claims

1. A solid electrolyte layer; and an electrode layer provided on each of the main surfaces of the solid electrolyte layer, the electrode layer including an electrode active material and a fibrous conductive assistant. In a cross section of the electrode layer, an average diameter of the conductive assistant is 2 nm or more and less than 150 nm, an area ratio occupied by the conductive assistant is 0.5% or more and 5.0% or less, and an area ratio occupied by the electrode active material is 28% or more and less than 80%, The solid electrolyte layer has a thickness of 5 μm or more and 20 μm or less.

2. The all-solid-state battery according to claim 1 , wherein the conductive assistant is a carbon material.

3. The all-solid-state battery according to claim 1 , wherein the conductive assistant is a carbon nanotube.

4. The all-solid-state battery according to claim 1 , wherein the solid electrolyte layer is an oxide.

5. The all-solid-state battery according to claim 1 , wherein the entire length of the conductive assistant is 5 μm or more.

Citation Information

Patent Citations

  • Lithium secondary battery

    JP2003331838A

  • Positive electrode for lithium ion secondary battery and lithium ion secondary battery

    JP2014203804A

  • All-solid type secondary battery

    JP2018170189A

  • Oxide solid electrolyte, electrode mixture material, and all-solid lithium ion battery

    JP2022107399A

  • All-solid-state battery, green laminate for all-solid-state battery, and method for producing all-solid-state battery

    WO2014042083A1