Depolymerization method of liquid crystalline resin
The use of supercritical methanol with metal oxides in the depolymerization of liquid crystal resins addresses the inefficiencies in recovering aromatic hydroxycarboxylic acid units, enabling effective recycling of these resins.
Patent Information
- Application Number
- JP2023054172
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing methods for recycling wholly aromatic polyesters and polyesteramides do not effectively recover structural units derived from aromatic hydroxycarboxylic acids, limiting the efficient recycling of liquid crystal resins.
A depolymerization process using supercritical methanol in the presence of metal oxides, such as titanium or zinc oxide, to react with liquid crystal resins containing aromatic hydroxycarboxylic acid units, achieving a high recovery rate of methyl esters of these components.
The method enables the recovery of structural units from aromatic hydroxycarboxylic acids at a sufficient rate, facilitating the recycling of liquid crystal resins.
Smart Images

Figure 2024142143000001 
Figure 2024142143000002 
Figure 2024142143000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for depolymerizing a liquid crystalline resin. [Background technology]
[0002] Liquid crystal resins have a good balance of excellent fluidity, mechanical strength, heat resistance, chemical resistance, electrical properties, etc., and are therefore widely used as high-performance engineering plastics. On the other hand, from the viewpoint of effective use of resources for protecting the global environment, effective recycling of engineering plastics is required. Known recycling methods include, for example, chemical recycling, material recycling, and thermal recycling (see Patent Document 1).
[0003] Patent Document 1 proposes a method for recycling wholly aromatic polyesters, in which wholly aromatic polyesters are depolymerized under pressure in an aliphatic monohydric alcohol at a temperature of 150°C or higher to recover aromatic dicarboxylic acid diesters and aromatic dihydroxy compounds, comprising: (1) a first step of depolymerizing a wholly aromatic polyester resin in an aliphatic monohydric alcohol under pressure at a temperature of 150°C or higher; (2) a second step of crystallizing and separating an aromatic dicarboxylic acid diester from the reaction mixture obtained in the first step; (3) a third step of distilling off an aliphatic monohydric alcohol from the mother liquor remaining in the second step; and (4) a fourth step of crystallizing the high-boiling point mixture remaining in the third step using a solvent having a solubility parameter (δs) of 10.5 or lower to separate the aromatic dihydroxy compound. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2003-147121 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the method for recycling wholly aromatic polyesters described in Patent Document 1, the wholly aromatic polyesters to be treated are those derived from aromatic dicarboxylic acids and aromatic dihydroxy compounds as monomers, and there is no description of aromatic polyesters or aromatic polyesteramides having structural units derived from aromatic hydroxycarboxylic acids as constituent components.
[0006] The present invention has been made in consideration of the above-mentioned problems in the conventional art, and an object of the present invention is to provide a method for depolymerizing a liquid crystalline resin, which is capable of recovering the structural unit monomer of a liquid crystalline resin having a structural unit derived from an aromatic hydroxycarboxylic acid as a constituent component at a sufficient recovery rate. [Means for solving the problem]
[0007] As a result of intensive research to solve the above problems, the present inventors discovered that in the reaction of liquid crystalline resin with methanol in a supercritical state, a good recovery rate is possible in the presence of a metal oxide, and thus completed the present invention.
[0008] One aspect of the present invention that solves the above problems is as follows. (1) Step A of mixing a liquid crystal resin, methanol, and a metal oxide; and step B of bringing the methanol into a supercritical state and reacting the liquid crystalline resin with the methanol in the presence of a metal oxide to depolymerize the liquid crystalline resin, The method for depolymerizing a liquid crystalline resin, wherein the liquid crystalline resin is an aromatic polyester or an aromatic polyester amide having, as a constituent, a structural unit derived from an aromatic hydroxycarboxylic acid.
[0009] (2) The method for depolymerizing a liquid crystalline resin according to (1) above, wherein the reaction temperature in step B is 240 to 350° C.
[0010] (3) The method for depolymerizing a liquid crystalline resin according to (1) or (2) above, wherein the metal oxide comprises at least one selected from the group consisting of titanium oxide, zirconium oxide, zinc oxide and magnesium oxide. Effect of the Invention
[0011] According to the present invention, there can be provided a method for depolymerizing a liquid crystalline resin, which is capable of recovering the structural unit monomer of a liquid crystalline resin having a structural unit derived from an aromatic hydroxycarboxylic acid as a constituent component at a sufficient recovery rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The method for depolymerizing a liquid crystalline resin according to the present embodiment includes step A of mixing a liquid crystalline resin, methanol, and a metal oxide, and step B of depolymerizing the liquid crystalline resin by bringing the methanol into a supercritical state and reacting the liquid crystalline resin with methanol in the presence of the metal oxide. The liquid crystalline resin is an aromatic polyester or aromatic polyester amide having a structural unit derived from an aromatic hydroxycarboxylic acid as a constituent component.
[0013] In the method for depolymerizing a liquid crystal resin according to the present embodiment, the liquid crystal resin to be depolymerized is an aromatic polyester or aromatic polyesteramide having a structural unit derived from an aromatic hydroxycarboxylic acid as a constituent. In step A, the liquid crystal resin is mixed with methanol and a metal oxide. In step B, the methanol is brought to a supercritical state, and the liquid crystal resin is reacted with methanol in the presence of the metal oxide to depolymerize the liquid crystal resin. By such steps A and B, the monomer components can be recovered at a sufficient recovery rate. This is presumably because the presence of the metal oxide promotes the depolymerization reaction of the liquid crystal resin. The main component recovered by the depolymerization method of the present embodiment is a methyl ester of an aromatic hydroxycarboxylic acid or a derivative thereof. Therefore, the recovered component cannot strictly be called a monomer constituting a liquid crystal resin. However, since the aromatic hydroxycarboxylic acid is not decomposed into another compound but is recovered while maintaining its structure, the recovered component is called a monomer constituting a liquid crystal resin for convenience. Each step of the method for depolymerizing a liquid crystalline resin according to this embodiment will be described in detail below.
[0014] [Step A] In step A, a liquid crystal resin, methanol, and a metal oxide are mixed. In this embodiment, the liquid crystal resin to be depolymerized is, as described above, an aromatic polyester or an aromatic polyesteramide having a structural unit derived from an aromatic hydroxycarboxylic acid as a constituent. The wholly aromatic polyester contains at least a structural unit derived from an aromatic hydroxycarboxylic acid, and examples thereof include the following (1) and (2). (1) Polyesters consisting essentially of one or more aromatic hydroxycarboxylic acids and their derivatives. (2) A polyester mainly composed of (a) one or more aromatic hydroxycarboxylic acids and their derivatives, (b) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids and their derivatives, and (c) at least one or more aromatic diols, alicyclic diols, aliphatic diols and their derivatives.
[0015] Examples of aromatic hydroxycarboxylic acids include p-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, m-hydroxybenzoic acid, 6-hydroxy-3-naphthoic acid, 6-hydroxy-4-naphthoic acid, 4-hydroxy-4'-carboxydiphenyl ether, 2,6-dichloro-p-hydroxybenzoic acid, 2-chloro-p-hydroxybenzoic acid, 2,6-dimethyl-p-hydroxybenzoic acid, 2,6-difluoro-p-hydroxybenzoic acid, 4-hydroxy-4'-biphenylcarboxylic acid, and vanillic acid. In the present embodiment, the structural unit derived from an aromatic hydroxycarboxylic acid is preferably a structural unit derived from p-hydroxybenzoic acid or 6-hydroxy-2-naphthoic acid. In particular, since 6-hydroxy-2-naphthoic acid is expensive, it would be useful if it could be recovered as methyl 6-hydroxy-2-naphthoate and recycled.
[0016] The aromatic dicarboxylic acid is not particularly limited, and examples thereof include terephthalic acid, isophthalic acid, 4,4'-diphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and compounds represented by the following general formula (I).
[0017] [ka] (Y:-(CH 2 ) n -(n=1 to 4) and -O(CH 2 ) n O-(n=1 to 4).
[0018] The alicyclic dicarboxylic acid is not particularly limited, and examples thereof include 1,4-cyclohexanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, etc. The polymerizable derivative is not particularly limited, and examples thereof include alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.
[0019] The aromatic diol is not particularly limited, and examples thereof include 2,6-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 4,4'-dihydroxybiphenyl, hydroquinone, resorcinol, a compound represented by the following general formula (II), and a compound represented by the following general formula (III).
[0020] [ka] (X: alkylene (C 1 ~C 4), alkylidene, -O-, -SO-, -SO 2 is a group selected from -, -S-, and -CO-.
[0021] [ka]
[0022] The alicyclic diol is not particularly limited, and examples thereof include 1,4-cyclohexanedimethanol, 1,4-cyclohexanediol, etc. The polymerizable derivative is not particularly limited, and examples thereof include alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.
[0023] On the other hand, the wholly aromatic polyesteramide contains at least a structural unit derived from an aromatic hydroxycarboxylic acid, and examples thereof include the following (1) and (2). (1) A polyesteramide consisting essentially of (a) one or more aromatic hydroxycarboxylic acids and their derivatives, (c1) one or more aromatic hydroxyamines, aromatic diamines, and their derivatives, and (c2) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives. (2) Polyesteramides mainly composed of (a) one or more aromatic hydroxycarboxylic acids and their derivatives, (b) one or more aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and their derivatives, (c1) one or more aromatic hydroxyamines, aromatic diamines, and their derivatives, and (c2) one or more aromatic diols, alicyclic diols, and their derivatives.
[0024] The same explanation as given above regarding the wholly aromatic polyester applies to the aromatic dicarboxylic acid, the alicyclic dicarboxylic acid, the aromatic diol, and the alicyclic diol.
[0025] The aromatic hydroxyamine is not particularly limited, and examples thereof include p-aminophenol, m-aminophenol, etc. The alicyclic hydroxyamine is not particularly limited, and examples thereof include 4-hydroxycyclohexanecarboxylic acid, 3-hydroxycyclopentanecarboxylic acid, etc. The polymerizable derivative is not particularly limited, and examples thereof include alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.
[0026] Examples of aromatic diamines include p-phenylenediamine, etc. Examples of alicyclic diamines include, but are not limited to, 1,4-cyclohexanediamine, 1,3-cyclopentanediamine, etc. Examples of polymerizable derivatives include, but are not limited to, alkyl esters (having about 1 to 4 carbon atoms) and halides of the above compounds.
[0027] In the method for depolymerizing a liquid crystalline resin according to the present embodiment, the liquid crystalline resin as described above is depolymerized mainly into a methyl ester of an aromatic hydroxycarboxylic acid.
[0028] The liquid crystal resin may also contain various known additives, such as various stabilizers, lubricants, nucleating agents, surfactants, colorants, polymer modifiers, different polymers, and inorganic or organic fibrous, powdery, or plate-like fillers, of which one or more may be blended.
[0029] In step A, examples of the liquid crystalline resin to be depolymerized and mixed with methanol include used liquid crystalline resin products, unused liquid crystalline resin pellets, resin waste generated in the manufacturing process of liquid crystalline resin pellets and liquid crystalline resin products, etc. Such liquid crystalline resin is preferably cut or crushed as necessary when mixed with methanol.
[0030] In step A, when mixing the liquid crystal resin and methanol, it is preferable to mix them so that the mass ratio of methanol to liquid crystal resin is 0.1 to 50. If the mass ratio is less than 0.1, the recovery rate of the monomer may not be increased, and even if it exceeds 50, no further effect is expected and the amount becomes excessive. The mass ratio is more preferably 0.5 to 10, and further preferably 1 to 5.
[0031] On the other hand, examples of metal oxides include oxides of alkaline earth metals (including magnesium), aluminum, zinc, tin, or transition metals, such as magnesium oxide, calcium oxide, barium oxide, aluminum oxide, zinc oxide, tin oxide, titanium oxide, vanadium oxide, manganese oxide, iron oxide, nickel oxide, copper oxide, zirconium oxide, molybdenum oxide, and silver oxide. Among these, one or more selected from the group consisting of titanium oxide, zirconium oxide, zinc oxide, and magnesium oxide are preferred. Titanium oxide and zinc oxide are particularly preferred.
[0032] From the viewpoint of increasing the recovery rate, the amount of the metal oxide used is preferably 0.1 to 100 parts by mass, and more preferably 1 to 50 parts by mass, per 100 parts by mass of the liquid crystal resin.
[0033] In step A, the liquid crystal resin, methanol, and metal oxide are mixed by any method. For example, the method includes a method of filling a mixing vessel with the liquid crystal resin, then adding methanol and the metal oxide, and mixing the liquid crystal resin and the metal oxide, a method of filling a mixing vessel with methanol, then adding the liquid crystal resin and the metal oxide, and mixing the liquid crystal resin and the methanol, a method of introducing the metal oxide into a mixing vessel, then adding the liquid crystal resin and the methanol, and a method of continuously joining the components in a pipe and then mixing them in a vessel. In addition, the mixing temperature and the mixing time in mixing the above components are not particularly limited.
[0034] After the above step A is completed, that is, after the liquid crystalline resin, methanol, and metal oxide are mixed, the process proceeds to step B. Step A and step B may be performed continuously, or there may be any time between the completion of step A and the start of step B. The mixing vessel used in step A and the reaction vessel used in step B may be the same or different. However, from the viewpoint of being able to proceed to step B in the same state after the completion of step A, it is preferable that the vessels used in steps A and B are the same.
[0035] [Step B] In step B, methanol is brought to a supercritical state, and the liquid crystalline resin is reacted with methanol in the presence of a metal oxide to depolymerize the liquid crystalline resin.
[0036] Here, methanol is put into a supercritical state by setting the temperature to 239°C or higher and the pressure to 8.1 MPa or higher. Therefore, in step B, the reaction temperature is set to 239°C or higher and the pressure to 8.1 MPa or higher to put methanol into a supercritical state. The reaction temperature in step B is preferably 240 to 350°C, more preferably 260 to 350°C, and more preferably 280 to 350°C. In addition, since the reaction rate increases as the temperature increases, it is preferable to increase the temperature in order to recover the monomer in a short time. Note that, as long as methanol is put into a supercritical state, the pressure is not particularly limited and can be appropriately set to 8.1 MPa or higher, but it is preferably 8.5 to 20 MPa.
[0037] In step B, a reaction vessel having resistance to high temperatures and pressures is used in order to set the reaction temperature and pressure so that methanol is in a supercritical state, and the shape and volume of the reaction vessel are arbitrary. In addition, the heat source for keeping the temperature within the above range is preferably one capable of controlling the temperature, and examples of the heat medium used in liquid form, a salt bath, a fluidized bed sand bath, a metal bath, a heater, an oven, microwave heating, etc.
[0038] In the method for depolymerizing a liquid crystalline resin according to the present embodiment, the reaction time between the liquid crystalline resin and methanol in a supercritical state is preferably 1 to 300 minutes, more preferably 2 to 120 minutes, and even more preferably 5 to 60 minutes. Then, the methyl ester of aromatic hydroxycarboxylic acid, which is a liquid crystalline monomer component to be depolymerized, is recovered at a high recovery rate.
[0039] The reaction in step B may be carried out with or without stirring.
[0040] In the method for depolymerizing a liquid crystalline resin according to the present embodiment, the depolymerization of the liquid crystalline resin may be carried out in a batch manner or a continuous manner.
[0041] Furthermore, in the method for depolymerizing a liquid crystal resin according to the present embodiment, in order to promote depolymerization, it is also possible to carry out the depolymerization by using an alkaline additive other than a metal oxide in combination. Examples of the alkaline additive include compounds such as hydroxides, carbonates, hydrogencarbonates, and carboxylates of alkali metals and alkaline earth metals, and amines, and one or more of these may be used. EXAMPLES
[0042] The present embodiment will be described in more detail below with reference to examples, but the present embodiment is not limited to the following examples.
[0043] [Examples 1 to 4, Comparative Example 1] As the liquid crystalline resin to be depolymerized, 0.2 g of a liquid crystalline resin (aromatic polyester) containing 73 mol % of structural units derived from p-hydroxybenzoic acid and 27 mol % of structural units derived from 6-hydroxy-2-naphthoic acid was prepared, and the following operation was carried out. In each of the Examples and Comparative Examples, a liquid crystalline resin and methanol were mixed in the ratio shown in Table 1, and the mixture was placed in a tubular reaction vessel made of SUS316 (volume: 8.8 cm 30.06 g of the metal oxide shown in Table 1 was also added. The tube-type reaction vessel was then placed in a salt bath (KNO 3 , NaNO 2 ) and heated to the temperature shown in Table 1. After the reaction time shown in Table 1 had elapsed, the reaction was stopped by quenching. After the reaction was stopped, the decomposition product was recovered with methanol and subjected to suction filtration to separate into a filtrate and a residue. The filtrate of the decomposition product was then analyzed by liquid chromatography to measure the amounts of methyl p-hydroxybenzoate and methyl 6-hydroxy-2-naphthoate, and the recovery rate of each monomer was calculated. In addition, the filtration residue of the decomposition product was dried and then mass measured to calculate the decomposition rate of the liquid crystalline resin. The calculation of each monomer recovery rate and the decomposition rate of the liquid crystalline resin is based on the following formula.
[0044]
number
[0045]
number
[0046]
number
[0047] [Table 1]
[0048] From Table 1, it can be seen that in all of Examples 1 to 4, the yield of methyl p-hydroxybenzoate and the recovery rate of methyl 6-hydroxy-2-naphthoate are higher than those in Comparative Example 1. In particular, Example 1, which used titanium oxide, and Example 3, which used zinc oxide, have high recovery rates. From the above, it is understood that the method for depolymerizing a liquid crystalline resin according to the present embodiment makes it possible to recover aromatic hydroxycarboxylic acid in the form of methyl ester with a sufficient recovery rate.
Claims
1. Step A of mixing a liquid crystal resin, methanol, and a metal oxide; and step B of bringing the methanol into a supercritical state and reacting the liquid crystalline resin with the methanol in the presence of the metal oxide to depolymerize the liquid crystalline resin, The method for depolymerizing a liquid crystalline resin, wherein the liquid crystalline resin is an aromatic polyester or an aromatic polyester amide having, as a constituent, a structural unit derived from an aromatic hydroxycarboxylic acid.
2. 2. The method for depolymerizing a liquid crystalline resin according to claim 1, wherein the reaction temperature in step B is 240 to 350° C.
3. 3. The method for depolymerizing a liquid crystalline resin according to claim 1, wherein the metal oxide comprises at least one selected from the group consisting of titanium oxide, zirconium oxide, zinc oxide and magnesium oxide.
Citation Information
Patent Citations
Method for chemically recycling all aromatic polyester
JP2003147121A