Manufacturing method of stack

The method addresses the issue of electrolyte return in stack manufacturing by controlling load application, ensuring the thickness of power storage cells increases, thus maintaining a sufficient restraining load.

JP2024142762AActive Publication Date: 2024-10-11PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023055073
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Existing stack manufacturing methods fail to consider the ease with which non-aqueous electrolyte returns to the electrode body, leading to insufficient restraining load when temperature or state of charge is low, causing the thickness of power storage cells to decrease.

Method used

A method for manufacturing a stack involving a flat wound electrode body with a separator, applying a controlled load to ensure a sufficient thickness difference, allowing non-aqueous electrolyte to return, thereby maintaining a sufficient restraining load.

Benefits of technology

The method ensures that the thickness of the power storage cells increases as the electrolyte returns, maintaining a sufficient load on the stack, even under low temperature or low state of charge conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142762000001_ABST
    Figure 2024142762000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of a stack, which is able to suitably control thicknesses of storage cells and to prevent decreases in stack restraining loads.SOLUTION: A technology disclosed herein relates to a manufacturing method of a stack that includes a plurality of storage cells. When the storage cells prepared herein undergo five cycles of a process, one cycle being a process that involves applying a load of up to 0.1 MPa to each of the storage cells at a speed of 0.1 mm / min in the thickness direction of each of the storage cells, and applying a load of up to 0.1 MPa to each of the storage cells prepared in the preparation process at a speed of 0.1 mm / min in the thickness direction of each of the storage cells, and then reducing the load to 0.01 MPa at a speed of 0.1 mm / min, a relationship between a storage cell thickness X1 determined relative to a surface pressure of 0.04 MPa by a pressurized side F-s curve in a first cycle and a storage cell thickness X5 determined relative to a surface pressure of 0.04 MPa by a pressurized side F-s curve in a fifth cycle satisfies the following expression: (X1-X5) / X1×100≥0.3.SELECTED DRAWING: Figure 8
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing a stack. [Background technology]

[0002] In recent years, stacks including a plurality of storage cells are suitably used as driving power sources mounted on vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), and electric vehicles (BEVs). Patent Document 1 is an example of a related prior art document. Patent Document 1 discloses a technology related to a non-aqueous electrolyte secondary battery (storage cell) that has an electrode body including a housing, a non-aqueous electrolyte (nonaqueous electrolyte), a positive electrode, a negative electrode, and a separator, and the electrode body further includes a low spring constant film having a spring constant (second spring constant) lower than the spring constant (first spring constant) of the negative electrode, thereby suppressing the extrusion of the non-aqueous electrolyte inside the electrode body due to the expansion and contraction of the electrode body. Conventionally, a stack is used by stacking storage cells and applying a load to restrain them. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-055806 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, when the stack is used, the thickness of the storage cell is reduced under low temperature or low SOC (State of Charge) conditions. When the stack is in such a state, the non-aqueous electrolyte extruded to the outside of the electrode assembly in the storage cell returns to the electrode assembly, thereby increasing the thickness of the storage cell again and maintaining the binding load of the stack. However, if the non-aqueous electrolyte is difficult to return to the electrode assembly in the storage cell, the storage cell thickness remains small, so the binding load of the stack decreases and the storage cell cannot be sufficiently bound. Therefore, in the manufacture of the stack, it is necessary to consider not only the extrusion of the non-aqueous electrolyte of the storage cell but also the ease of return of the non-aqueous electrolyte. In this regard, the above-mentioned Patent Document 1 does not consider the ease of return of the non-aqueous electrolyte to the inside of the electrode assembly, and the above technology has room for improvement.

[0005] The technology disclosed herein has been made in consideration of the above circumstances, and its main purpose is to relate to a method for manufacturing a stack that can appropriately control the thickness of the storage cells stacked in the stack and suppress a decrease in the restraining load of the stack. [Means for solving the problem]

[0006] The technology disclosed herein is a manufacturing method for a stack including a plurality of rectangular energy storage cells, and includes a preparation step of preparing the energy storage cell including a flat-shaped wound electrode body formed by stacking and winding a positive electrode and a negative electrode with a separator interposed therebetween, a non-aqueous electrolyte, and a case that houses the wound electrode body and the non-aqueous electrolyte, and a stacking step of stacking a plurality of the energy storage cells along a thickness direction of the energy storage cell. Here, the storage cell prepared in the preparation step is characterized in that when a process in which a load is applied to the storage cell in the thickness direction of the storage cell at a rate of 0.1 mm / min up to 0.1 MPa and, after the application, the load is reduced to 0.01 MPa at a rate of 0.1 mm / min, is defined as one cycle, and when this process is performed for five cycles, the relationship between the storage cell thickness X1 for a surface pressure of 0.04 MPa on the pressure-side Fs curve in the first cycle and the storage cell thickness X5 for a surface pressure of 0.04 MPa on the pressure-side Fs curve in the fifth cycle satisfies the following formula: (X1-X5) / X1×100≧0.3.

[0007] The storage cell prepared in the preparation step is a storage cell that satisfies the above formula. In a storage cell having such a configuration, a thickness difference is provided so that the non-aqueous electrolyte pushed out from the wound electrode body in the stacking step can return to the inside of the wound electrode body. Therefore, the thickness of the wound electrode body increases as the storage cell re-incorporates the non-aqueous electrolyte, and the thickness of the storage cell increases. This makes it possible to suppress a decrease in the load applied to the storage cell and maintain a sufficient load on the storage cell in the stack. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a perspective view illustrating a stack according to an embodiment. [Diagram 2] FIG. 2 is a perspective view of the electricity storage cell. [Diagram 3] FIG. 3 is a schematic vertical cross-sectional view taken along line III-III in FIG. [Figure 4] FIG. 4 is a perspective view that shows a schematic view of a wound electrode body attached to a sealing plate. [Diagram 5] FIG. 5 is a perspective view showing a schematic diagram of a wound electrode body. [Figure 6] FIG. 6 is a schematic diagram showing the configuration of a wound electrode body. [Figure 7] FIG. 7 is a flow diagram showing a method for manufacturing a stack according to one embodiment. [Figure 8] FIG. 8 is an example of an Fs curve obtained in the preparation process according to one embodiment. [Figure 9] 9 is a schematic diagram for explaining the thickness change of the wound electrode body according to one embodiment, in which (a) shows the wound electrode body before stack restraint, (b) shows the wound electrode body when the stack is restrained, and (c) shows the wound electrode body when the non-aqueous electrolyte returns to the wound electrode body. [Figure 10] FIG. 10 is a schematic diagram illustrating the measurement of the amount of change in cell thickness in the preparation step. [Figure 11]FIG. 11 is a flow diagram showing a method for manufacturing an electricity storage cell according to one embodiment. [Figure 12] FIG. 12 is a graph in which the change in cell thickness between the first and fifth cycles under the same load is plotted on the horizontal axis as Δcell thickness (mm) and the applied load (kN) on the vertical axis for Examples 1 and 2 and Comparative Example 2. [Figure 13] 13 is a schematic diagram for explaining the change in thickness of a wound electrode body according to a conventional example, in which (a) shows the wound electrode body before stack restraint, (b) shows the wound electrode body when the stack is restrained, and (c) shows the wound electrode body when the non-aqueous electrolyte returns to the wound electrode body. [Figure 14] FIG. 14 is an example of an Fs curve according to a conventional example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, some preferred embodiments of the stack disclosed herein will be described with reference to the drawings as appropriate. Matters other than those specifically mentioned in this specification and necessary for carrying out the present disclosure (for example, the general configuration and manufacturing process of the storage cell that do not characterize the present disclosure) can be understood as design matters of a person skilled in the art based on the prior art in the field. The stack disclosed herein can be carried out based on the contents disclosed in this specification and the technical common sense in the field.

[0010] In the following drawings, the same reference numerals are used for components and parts having the same function, and duplicated explanations may be omitted or simplified. In addition, in this specification, the expression "A to B" indicating a range includes the meaning of "A or more and B or less," as well as "preferably larger than A" and "preferably smaller than B."

[0011] FIG. 1 is a perspective view showing a stack 500 according to an embodiment. The stack 500 includes a plurality of storage cells 100 and a restraining mechanism 300. Although not shown here for convenience of explanation, the plurality of storage cells 100 of the stack 500 are electrically connected by a bus bar. In the following description, the symbols L, R, F, Rr, U, and D in the drawings represent left, right, front, rear, top, and bottom, and the symbols X, Y, and Z in the drawings represent the short side direction (thickness direction) of the storage cell 100, the long side direction (width direction) perpendicular to the short side direction, and the up-down direction, respectively. The short side direction X is also the arrangement direction of the storage cells 100. However, these are merely directions for convenience of explanation and do not limit the installation form of the stack 500 in any way.

[0012] The restraining mechanism 300 is configured to apply a prescribed restraining pressure to the multiple energy storage cells 100 from the thickness direction X. Here, the restraining mechanism 300 is configured with a pair of end plates 310, a pair of side plates 320, and multiple screws 330. The pair of end plates 310 are aligned in a predetermined thickness direction X. The pair of end plates 310 are arranged at both ends of the stack 500 in the thickness direction X. The multiple energy storage cells 100 are arranged between the pair of end plates 310 along the thickness direction X. An insulating sheet, an inter-cell separator, or the like may be arranged between the multiple energy storage cells 100.

[0013] The pair of side plates 320 bridge the pair of end plates 310. The pair of side plates 320 are fixed to the end plates 310 by, for example, a plurality of screws 330 while a load is applied to the plurality of energy storage cells 100. As a result, a restraining load is applied to the plurality of energy storage cells 100 and the plurality of porous elastic members 200 from the thickness direction X, and the stack 500 is held integrally. However, the restraining mechanism is not limited to this. The restraining mechanism 300 may include, for example, a plurality of restraining bands, bind bars, or the like, instead of the side plates 320.

[0014] <Electricity storage cell 100> In this specification, the term "storage cell" refers to a device that can be repeatedly charged and discharged. The storage cell includes batteries generally called lithium ion batteries and lithium secondary batteries, as well as lithium polymer batteries and lithium ion capacitors. A secondary battery generally refers to a battery that can be repeatedly charged and discharged by the movement of charge carriers between the positive and negative electrodes. Here, a lithium ion secondary battery is exemplified as one form of storage cell.

[0015] Fig. 2 is a perspective view of the storage cell 100. As shown in Figs. 1 and 2, the multiple storage cells 100 are arranged in the thickness direction X such that first side walls 12b described below face each other. Fig. 3 is a schematic vertical cross-sectional view taken along line III-III in Fig. 2. As shown in Fig. 3, the storage cell 100 includes a case 10, a wound electrode body 20, a non-aqueous electrolyte (not shown), and further includes a positive electrode terminal 30, a negative electrode terminal 40, a positive electrode current collector 50, and a negative electrode current collector 60. Here, the storage cell 100 is a lithium ion secondary battery.

[0016] The case 10 is a housing that houses the wound electrode body 20 and the non-aqueous electrolyte. As shown in FIG. 2, the case 10 has a flat, bottomed rectangular parallelepiped (rectangular) outer shape. The material of the case 10 may be the same as that used conventionally, and is not particularly limited. The case 10 is preferably made of a metal, and more preferably made of, for example, aluminum, an aluminum alloy, iron, an iron alloy, or the like. As shown in FIG. 2, the case 10 includes an exterior body 12 having an opening 12h, and a sealing plate (lid) 14 that seals the opening 12h. As in this embodiment, the case 10 preferably includes an exterior body 12 having an opening 12h, and a sealing plate 14 that seals the opening 12h.

[0017] As shown in FIG. 2, the exterior body 12 includes a bottom 12a, a pair of first side walls 12b extending from the bottom 12a and facing each other, and a pair of second side walls 12c extending from the bottom 12a and facing each other. The bottom 12a is substantially rectangular. The bottom 12a faces the opening 12h. The first side wall 12b is flat. The first side wall 12b extends from a long side of the bottom 12a. The second side wall 12c extends from a short side of the bottom 12a. In a plan view, the area of ​​the first side wall 12b is larger than the area of ​​the second side wall 12c. The size of the exterior body 12 is not particularly limited, but it is preferable that the width (long side direction Y) is 300 to 330 mm, the height (vertical direction Z) is 100 to 130 mm, and the thickness (short side direction X) is 30 to 50 mm.

[0018] The sealing plate 14 is attached to the exterior body 12 so as to close the opening 12h of the exterior body 12. The sealing plate 14 faces the bottom 12a of the exterior body 12. The sealing plate 14 has a substantially rectangular shape in a plan view. The case 10 is integrated by joining (preferably welding) the sealing plate 14 to the periphery of the opening 12h of the exterior body 12. The case 10 is hermetically sealed (sealed).

[0019] As shown in FIG. 3, the sealing plate 14 is provided with a liquid inlet 15, a drain valve 17, and two terminal outlet holes 18 and 19. The liquid inlet 15 is for injecting a non-aqueous electrolyte after the sealing plate 14 is assembled to the exterior body 12. The liquid inlet 15 is sealed by a sealing member 16. The drain valve 17 is configured to break when the pressure inside the case 10 reaches or exceeds a predetermined value, thereby discharging the gas inside the case 10 to the outside. The terminal outlet holes 18 and 19 penetrate the sealing plate 14 in the vertical direction Z. The terminal outlet holes 18 and 19 each have an inner diameter large enough to insert the positive electrode terminal 30 and the negative electrode terminal 40 before being attached to the sealing plate 14 (before being crimped).

[0020] The non-aqueous electrolyte may be the same as that of the conventional one, and is not particularly limited. The non-aqueous electrolyte contains a non-aqueous solvent and a supporting salt (electrolyte salt). The non-aqueous electrolyte may further contain additives as necessary. The non-aqueous solvent includes, for example, carbonates such as ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate. The non-aqueous solvent preferably includes carbonates. In particular, it is preferable that the non-aqueous solvent includes a cyclic carbonate and a chain carbonate. The supporting salt is, for example, lithium hexafluorophosphate (LiPF 6 ) and other fluorine-containing lithium salts. Examples of additives that can be included in the non-aqueous electrolyte include film-forming agents, gas generating agents, dispersants, and thickeners. Examples of film-forming agents include carbonate compounds such as vinylene carbonate (VC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), chloroethylene carbonate, and methyl phenyl carbonate; lithium salts with oxalato complexes as anions, such as lithium bis(oxalato)borate (LiBOB), lithium difluoro(oxalato)borate (LiFOB), and lithium difluorobis(oxalato)phosphate (LPFO); and the like.

[0021] The positive electrode terminal 30 is disposed at one end of the sealing plate 14 in the long side direction Y (the left end in FIG. 2 and FIG. 3). The negative electrode terminal 40 is disposed at the other end of the sealing plate 14 in the long side direction Y (the right end in FIG. 2 and FIG. 3). As shown in FIG. 3, the positive electrode terminal 30 and the negative electrode terminal 40 extend from the inside to the outside of the sealing plate 14 through the terminal drawing holes 18 and 19. The positive electrode terminal 30 and the negative electrode terminal 40 are fixed to the sealing plate 14. Here, the positive electrode terminal 30 and the negative electrode terminal 40 are crimped to the peripheral portion surrounding the terminal drawing holes 18 and 19 of the sealing plate 14 by crimping. The crimped portions 30c and 40c are formed at the ends of the positive electrode terminal 30 and the negative electrode terminal 40 on the exterior body 12 side (the lower end in FIG. 3).

[0022] As shown in Fig. 3, the positive electrode terminal 30 is electrically connected to the positive electrode 22 (see Fig. 6) of the wound electrode body 20 via the positive electrode current collector 50 inside the exterior body 12. The negative electrode terminal 40 is electrically connected to the negative electrode 24 (see Fig. 6) of the wound electrode body 20 via the negative electrode current collector 60 inside the exterior body 12. The positive electrode terminal 30 is insulated from the sealing plate 14 by an internal insulating member 80 and a gasket 90. The negative electrode terminal 40 is insulated from the sealing plate 14 by an internal insulating member 80 and a gasket 90.

[0023] A plate-shaped positive electrode external conductive member 32 and a plate-shaped negative electrode external conductive member 42 are attached to the outer surface of the sealing plate 14. The positive electrode external conductive member 32 is electrically connected to the positive electrode terminal 30. The negative electrode external conductive member 42 is electrically connected to the negative electrode terminal 40. The positive electrode external conductive member 32 and the negative electrode external conductive member 42 are members to which a bus bar or the like is attached to electrically connect the multiple storage cells 100 to each other. The positive electrode external conductive member 32 and the negative electrode external conductive member 42 are insulated from the sealing plate 14 by an external insulating member 92. Although not shown in FIG. 1, when the stack 500 is used, the adjacent storage cells 100 are electrically connected to each other. For example, among the adjacent storage cells 100, the positive electrode external conductive member 32 of one storage cell 100 and the negative electrode external conductive member 42 of the other storage cell 100 are electrically connected by a bus bar or the like. As a result, the stack 500 is electrically connected. The stack 500 may be connected in series, in parallel, or in a so-called multi-series / multi-parallel connection which is a combination of series and parallel.

[0024] FIG. 4 is a perspective view that shows a schematic diagram of the wound electrode body 20 attached to the sealing plate 14. The wound electrode body 20 has three wound electrode bodies 20 here. However, the number of electrode bodies arranged inside one exterior body 12 is not particularly limited, and may be one or more (two or more). The wound electrode bodies 20 are electrically connected in parallel here. The wound electrode body 20 is arranged inside the exterior body 12 with the winding axis WL (see FIG. 6) oriented substantially parallel to the long side direction Y. The wound electrode bodies 20 are arranged side by side in a direction (short side direction X) in which the thickness direction of the energy storage cell 100 (in other words, a direction substantially perpendicular to the first side wall 12b of the case 10) and the thickness direction of the wound electrode body 20 coincide with each other. The wound electrode body 20 preferably has a flattened outer shape. An end face of the wound electrode body 20 perpendicular to the winding axis WL (in other words, a layered surface where the positive electrode 22 and the negative electrode 24 are layered) faces the second side wall 12c. Although not shown, an insulating sheet is disposed between the wound electrode body 20 and the exterior body 12.

[0025] FIG. 5 is a perspective view showing a schematic diagram of the wound electrode body 20. Note that all the wound electrode bodies 20 housed in the case 10 can have the same configuration. The wound electrode body 20 has a pair of curved portions (R portions) 20r and a flat portion 20f connecting the pair of curved portions 20r. One curved portion 20r (upper side of FIG. 5) faces the sealing plate 14, and the other curved portion 20r (lower side of FIG. 5) faces the bottom portion 12a of the exterior body 12. The flat portion 20f faces the first side wall 12b of the exterior body 12. Here, the flat portions 20f of the multiple wound electrode bodies 20 adjacent to each other in the short side direction X face each other.

[0026] 6 is a schematic diagram showing the configuration of the wound electrode body 20. The wound electrode body 20 has a positive electrode 22, a negative electrode 24, and a separator 26. In this example, the wound electrode body 20 is configured by stacking a strip-shaped positive electrode 22 and a strip-shaped negative electrode 24 with a strip-shaped separator 26 interposed therebetween, and winding them in the longitudinal direction around a winding axis WL. The direction of the winding axis WL is approximately parallel to the long side direction Y.

[0027] As shown in FIG. 6, the positive electrode 22 has a positive electrode core 22c, and a positive electrode active material layer 22a and a positive electrode protective layer 22p fixed on at least one surface of the positive electrode core 22c. However, the positive electrode protective layer 22p is not essential and can be omitted in other embodiments. The positive electrode core 22c is strip-shaped. The positive electrode core 22c is preferably a metal foil, more preferably an aluminum foil or an aluminum alloy foil. The positive electrode core 22c is an aluminum foil here. The thickness of the positive electrode core 22c is not particularly limited, but is preferably 5 to 30 μm, more preferably 10 to 25 μm. The number of layers of the positive electrode 22 is preferably 30 or more.

[0028] A plurality of positive electrode tabs 22t are provided at one end (left end in FIG. 6) in the long side direction Y of the positive electrode core 22c. The plurality of positive electrode tabs 22t protrude toward one side (left end in FIG. 6) in the long side direction Y. The plurality of positive electrode tabs 22t protrude in the long side direction Y beyond the separator 26. The positive electrode tab 22t is a part of the positive electrode core 22c here, and is made of metal foil (aluminum foil). As shown in FIG. 3 to FIG. 6, the plurality of positive electrode tabs 22t are stacked at one end (left end in FIG. 3 to FIG. 6) in the long side direction Y to form a positive electrode tab group 23. The positive electrode tab group 23 is electrically connected to the positive electrode terminal 30 via the positive electrode current collector 50.

[0029] As shown in FIG. 6, the positive electrode active material layer 22a is provided in a strip shape along the longitudinal direction of the positive electrode core 22c. The positive electrode active material layer 22a contains a positive electrode active material capable of reversibly absorbing and releasing charge carriers. For example, a lithium transition metal composite oxide is preferably used as the positive electrode active material, and it is particularly preferable that the positive electrode active material contains nickel (Ni). The positive electrode active material layer 22a may contain various additive components such as an optional component other than the positive electrode active material, for example, a binder, a conductive material, etc., and it is preferable that the positive electrode active material layer 22a contains a conductive material and a binder as the additive component. For example, polyvinylidene fluoride (PVdF) is used as the binder. The conductive material used in the positive electrode active material layer 22a is not particularly limited, but a carbon material is preferably used. The density of the positive electrode active material layer 22a is preferably 3.0 g / cc or more, more preferably 3.5 g / cc or more. On the other hand, the density of the positive electrode active material layer 22a is preferably 3.7 g / cc or less.

[0030] As shown in Fig. 6, the positive electrode protective layer 22p is provided at the boundary between the positive electrode core 22c and the positive electrode active material layer 22a in the long side direction Y. The positive electrode protective layer 22p is provided in a strip shape along the positive electrode active material layer 22a. The positive electrode protective layer 22p contains an inorganic filler (e.g., alumina). The positive electrode protective layer 22p may contain any component other than the inorganic filler, such as a conductive material, a binder, various additive components, and the like.

[0031] As shown in FIG. 6, the negative electrode 24 has a negative electrode core 24c and a negative electrode active material layer 24a fixed on at least one surface of the negative electrode core 24c. The negative electrode core 24c is strip-shaped. The negative electrode core 24c is preferably a metal foil, more preferably a copper foil or a copper alloy foil. The negative electrode core 24c is a copper foil here. The thickness of the negative electrode core 24c is not particularly limited, but is preferably 5 to 30 μm, more preferably 10 to 25 μm.

[0032] A plurality of negative electrode tabs 24t are provided at one end (right end in FIG. 6) in the long side direction Y of the negative electrode core 24c. The plurality of negative electrode tabs 24t protrude toward one side (right end in FIG. 6) in the long side direction Y. The plurality of negative electrode tabs 24t protrude in the long side direction Y beyond the separator 26. The negative electrode tab 24t is a part of the negative electrode core 24c here, and is made of metal foil (copper foil). As shown in FIG. 3 to FIG. 6, the plurality of negative electrode tabs 24t are stacked at one end (right end in FIG. 3 to FIG. 6) in the long side direction Y to form a negative electrode tab group 25. The negative electrode tab group 25 is provided at a position symmetrical to the positive electrode tab group 23 in the long side direction Y. The negative electrode tab group 25 is electrically connected to the negative electrode terminal 40 via the negative electrode current collector 60.

[0033] As shown in FIG. 6, the negative electrode active material layer 24a is provided in a strip shape along the longitudinal direction of the negative electrode core 24c. The negative electrode active material layer 24a contains a negative electrode active material capable of reversibly absorbing and releasing charge carriers. For example, graphite, a silicon-based material (a silicon-containing material), and a mixed oxide thereof are preferably used as the negative electrode active material. The negative electrode active material layer 24a may contain any component other than the negative electrode active material, for example, various additive components such as a binder, a thickener, and a dispersant. For example, a binder used in the negative electrode active material layer 24a includes styrene butadiene rubber (SBR) and carboxymethyl cellulose (CMC). The conductive material used in the negative electrode active material layer 24a is not particularly limited, but a carbon material is preferably used. The density of the negative electrode active material layer 24a is preferably 1.3 g / cc or more, more preferably 1.4 g / cc or more. On the other hand, the density of the negative electrode active material layer 24a is preferably 1.7 g / cc or less.

[0034] The length Ln of the negative electrode active material layer 24a in the width direction Y is equal to or longer than the length La of the positive electrode active material layer 22a in the width direction Y. Here, the length Ln of the negative electrode active material layer 24a in the width direction Y is preferably 20 cm or more. As will be described in detail later, this configuration allows the return of the non-aqueous electrolyte to the wound electrode body 20 to be suitably controlled. In addition, when the length in the direction perpendicular to the winding axis WL direction of the wound electrode body 20 and perpendicular to the thickness direction X of the wound electrode body 20 (here, the Z direction) is defined as the height T of the wound electrode body 20, it is preferable that the ratio (Ln / T) of the length Ln in the width direction of the negative electrode active material layer 24a to the height T of the wound electrode body 20 (hereinafter, also referred to as the "electrode body aspect ratio") is 2.8 to 3.2. This configuration allows the return of the non-aqueous electrolyte to the wound electrode body 20 to be suitably controlled. In the specification, "height T of the wound electrode body 20" refers to the distance in the Z direction from the uppermost end of one curved portion 20r of the wound electrode body 20 (U side in Figure 5) to the lowermost end of the other curved portion 20r (D side in Figure 5).

[0035] The separator 26 is a member that insulates the positive electrode active material layer 22a of the positive electrode 22 from the negative electrode active material layer 24a of the negative electrode 24. The separator 26 constitutes the outer surface of the wound electrode body 20. The length Ls of the separator 26 in the long side direction Y is equal to or longer than the length Ln of the negative electrode active material layer 24a in the long side direction Y. The separator 26 has a base material portion. The separator 26 may be formed on at least one surface of the base material portion, and may have a heat-resistant layer containing, for example, inorganic particles and a heat-resistant layer binder. The separator 26 may also have an adhesive layer containing an adhesive layer binder formed on at least one surface of the base material portion. The adhesive layer may further contain inorganic particles in addition to the adhesive layer binder. The adhesive layer may be formed to have a shape such as a dot shape, a stripe shape, a wave shape, a band shape (stripes), a dashed line shape, or a combination thereof, in a plan view. Although not shown in the drawings, in this embodiment, a heat-resistant layer is provided on the surface of the substrate of the separator 26, and an adhesive layer is further provided on the heat-resistant layer. The separator 26 preferably has a heat-resistant layer and an adhesive layer. Alternatively, the separator 26 preferably has an adhesive layer containing inorganic particles.

[0036] The substrate of the separator 26 is a sheet-like member of a microporous film. The separator 26 is preferably made of a polyolefin resin. Examples of the polyolefin resin that can be used include polyethylene (PE), polypropylene (PP), and a mixture thereof.

[0037] There is no particular limitation on the thickness of the separator 26. When the separator 26 does not contain a non-aqueous electrolyte, the thickness of the separator 26 is preferably about 10 to 30 μm. In addition, in the present specification, the "thickness of the separator 26" refers to the thickness including the adhesive layer and the heat-resistant layer when the separator 26 has an adhesive layer and a heat-resistant layer in addition to the base material, and refers to the thickness before the press molding process unless otherwise specified.

[0038] When the separator 26 has an adhesive layer, the adhesive layer binder used in the adhesive layer can be any adhesive layer binder that has been conventionally used for this type of application, without any particular limitation, and examples of such binders include acrylic resins, fluorine resins (e.g., PVdF), rubber resins (e.g., styrene butadiene rubber (SBR)), urethane resins, silicone resins, and epoxy resins. These may be used alone or in combination of two or more. When the adhesive layer contains inorganic particles, the proportion of the inorganic particles to the total mass of the heat-resistant layer is preferably about 5 to 20 mass%, and more preferably about 10 to 15 mass%.

[0039] When the separator 26 has a heat-resistant layer, the ratio of inorganic particles to the total mass of the heat-resistant layer is preferably 85% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more. As the heat-resistant layer binder used in the heat-resistant layer, any binder that has been conventionally used for this type of application can be used without particular limitation, and examples thereof include acrylic resins, fluorine-based resins, epoxy resins, urethane resins, and ethylene vinyl acetate resins. These may be used alone or in combination of two or more types. In addition, the types of the heat-resistant layer binder and the adhesive layer binder may be the same or different.

[0040] The inorganic particles used in the heat-resistant layer and adhesive layer of the separator 26 may be any particles that have been publicly known and are used for this type of application without any particular limitation, but preferably contain insulating ceramic particles, for example. Among them, from the viewpoint of heat resistance, inorganic oxides such as alumina, zirconia, silica, titania, metal hydroxides such as aluminum hydroxide, and clay minerals such as boehmite are preferred, with alumina and boehmite being more preferred. Furthermore, from the viewpoint of suppressing thermal contraction of the separator 26, compounds containing aluminum are particularly preferred.

[0041] As shown in FIG. 3, the positive electrode current collecting part 50 constitutes a conductive path that electrically connects the positive electrode tab group 23 consisting of a plurality of positive electrode tabs 22t and the positive electrode terminal 30. The positive electrode current collecting part 50 includes a positive electrode first current collecting part 51 and a positive electrode second current collecting part 52. The positive electrode first current collecting part 51 is attached to the inner surface of the sealing plate 14. The positive electrode second current collecting part 52 extends along the second side wall 12c of the exterior body 12. As shown in FIGS. 3 to 5, the positive electrode second current collecting part 52 is attached to the wound electrode body 20.

[0042] 3, the negative electrode current collecting part 60 constitutes a conductive path that electrically connects the negative electrode tab group 25 consisting of the multiple negative electrode tabs 24t to the negative electrode terminal 40. The negative electrode current collecting part 60 includes a negative electrode first current collecting part 61 and a negative electrode second current collecting part 62. The configurations of the negative electrode first current collecting part 61 and the negative electrode second current collecting part 62 may be the same as those of the positive electrode first current collecting part 51 and the positive electrode second current collecting part 52 of the positive electrode current collecting part 50.

[0043] <Stack 500 manufacturing method> 7 is a flow diagram showing a method for manufacturing a stack 500 according to an embodiment. The stack 500 disclosed herein can be manufactured by a manufacturing method including a preparation step S10 and a stacking step S20, and is characterized by performing the preparation step S10. In addition to the above steps, the manufacturing method for the stack 500 disclosed herein may further include other steps at any stage, and the other manufacturing processes may be the same as conventional methods.

[0044] (Preparation step S10) In the preparation step S10, an energy storage cell 100 is prepared, which includes the above-described wound electrode body 20, a non-aqueous electrolyte, and a case 10. In the preparation step S10, the energy storage cell 100 may be purchased and prepared, or the energy storage cell 100 may be manufactured and prepared.

[0045] Here, the storage cell 100 prepared in the preparation step S10 is characterized in that, when a load is applied to the storage cell 100 in the thickness direction (X direction in FIG. 1) at a rate of 0.1 mm / min up to 0.1 MPa, and the load is then reduced to 0.01 MPa at a rate of 0.1 mm / min after the load application, and the process is repeated five times, the relationship between the storage cell thickness X1 at a surface pressure of 0.04 MPa in the pressure-side Fs curve in the first cycle and the storage cell thickness X5 at a surface pressure of 0.04 MPa in the pressure-side Fs curve in the fifth cycle satisfies the following formula: (X1-X5) / X1×100≧0.3. Hereinafter, (X1-X5) / X1×100 is also referred to as the "cell thickness change amount". In this specification, the "cell thickness change amount" is determined by measurement using an autograph.

[0046] FIG. 8 is an example of an Fs curve obtained in the preparation step S10 in one embodiment. Here, the Fs curve in the first cycle corresponds to the Fs curve of the storage cell at the time of shipment (i.e., before use as a stack). Meanwhile, the Fs curve in the fifth cycle corresponds to the Fs curve of the storage cell from which the non-aqueous electrolyte held inside the wound electrode body has been removed. Therefore, the difference between X1 and X5 (X1-X5) corresponds to the thickness of the non-aqueous electrolyte held inside the wound electrode body at the time of shipment. And, the "cell thickness change amount" according to this embodiment is the rate of decrease in cell thickness at a surface pressure of 0.04 MPa, and is an index showing the amount of non-aqueous electrolyte held inside the wound electrode body.

[0047] FIG. 9 is a schematic diagram for explaining thickness change of the wound electrode body 20 according to one embodiment. FIG. 13 is a schematic diagram for explaining thickness change of the wound electrode body 20 according to a conventional example. In FIG. 9 and FIG. 13, (a) shows the wound electrode body 20 before stack restraint, (b) shows the wound electrode body 20 when stack restraint is performed, and (c) shows the wound electrode body 20 when the non-aqueous electrolyte returns to the wound electrode body 20. FIG. 14 is an example of an Fs curve according to a conventional example. FIG. 14 is a diagram corresponding to FIG. 8. In FIG. 9 and FIG. 13, a part of the wound electrode body 20 is partially enlarged.

[0048] When a non-aqueous electrolyte is present inside the wound electrode body 20, for example, the non-aqueous electrolyte is present inside the gap 26s of the separator 26 of the wound electrode body 20. In the state shown in FIG. 13(a), the non-aqueous electrolyte is held in the gap 26s of the wound electrode body 20 in the storage cell 100 before restraint. During stack manufacturing, when the storage cell 100 is restrained, a load is applied to the storage cell 100 in the thickness direction X. As a result, as shown in FIG. 13(b), the gap 26s of the wound electrode body 20 is crushed, and the non-aqueous electrolyte held inside the gap 26s is pushed out to the outside of the wound electrode body 20. On the other hand, when the stack 500 is used, for example, during initial charging, under low temperature conditions, or under low SOC conditions, the thickness of the wound electrode body 20 is reduced. In particular, when the conditions of a low temperature environment, low SOC conditions, and initial charging are met, the reduction in the thickness of the wound electrode body 20 is remarkable. As a result, the restraining load applied to the storage cell 100 by the restraining mechanism 300 is reduced. Then, as shown in FIG. 13(c), the nonaqueous electrolyte that was outside the wound electrode body 20 attempts to return to the inside of the wound electrode body 20 again by the amount of the reduced restraining load. Here, the amount of nonaqueous electrolyte that returns to the inside of the wound electrode body 20 again is affected by the amount of the voids 26s of the wound electrode body 20. In other words, when the amount of the voids 26s of the wound electrode body 20 of the storage cell 100 is small, the amount of nonaqueous electrolyte that returns to the inside of the wound electrode body 20 again is small. As shown in FIG. 14, in the conventional storage cell 100, the difference between X1 and X5 is small. In other words, there is a state in which there are few voids 26s for the nonaqueous electrolyte that is present outside the wound electrode body 20 to return to the inside of the wound electrode body 20 again. In this way, when the amount of gaps 26s in the wound electrode body 20 of the energy storage cell 100 is small, the amount of non-aqueous electrolyte returning to the wound electrode body 20 is small, so the thickness of the wound electrode body 20 does not increase well and the thickness of the energy storage cell 100 remains thin. For this reason, the load applied to the energy storage cell 100 decreases, and it is no longer possible to restrain it with a sufficient load.

[0049] Here, the stack 500 according to this embodiment is characterized in that the storage cell having a cell thickness change (%) of 0.3% or more (≧0.3) is prepared in the preparation step S10. The difference between X1 and X5 is sufficiently provided for the storage cell 100. In other words, as shown in FIG. 9(a), the wound electrode body 20 is provided with a sufficient thickness for the non-aqueous electrolyte held inside the wound electrode body at the time of shipment. As shown in FIG. 9(c), the wound electrode body 20 has a sufficient gap 26s for the non-aqueous electrolyte present outside the wound electrode body 20 to return to the inside of the wound electrode body 20 again. Therefore, the thickness of the wound electrode body 20 increases by re-incorporating the non-aqueous electrolyte, and the thickness of the storage cell 100 increases. Therefore, the reduction in the load applied to the storage cell 100 is suppressed, and a sufficient load is maintained on the storage cell 100 in the stack 500.

[0050] FIG. 10 is a schematic diagram for explaining the measurement of the cell thickness change amount in the preparation step S10. In FIG. 10, the direction in which the autograph 600 applies a load in the thickness direction of the storage cell 100 is illustrated by a hollow arrow. As shown in FIG. 8, the storage cell 100 is first set in the autograph 600 so that a load is applied in the thickness direction (the direction of the hollow arrow). As shown in FIG. 10, the storage cell 100 is set so that a pair of first side walls 12b and the autograph 600 abut against each other. When the storage cell 100 is viewed in the horizontal direction, the autograph 600 is set so that a load is applied to the flat portion 20f of the wound electrode body 20 by the autograph 600. Here, the storage cell 100 is set in the autograph 600 so that a load is applied to the portion shown by the imaginary line in FIG. 3. The means for measuring the thickness displacement of the storage cell 100 is not particularly limited, and for example, a laser displacement meter (for example, manufactured by Keyence Corporation, product name: LK-G157, etc.) can be used. Furthermore, the thickness of the energy storage cell 100 may be measured at one location or multiple locations (two or more locations). A load is applied to the energy storage cell 100 in the thickness direction of the energy storage cell 100 (indicated by the white arrow) at a speed of 0.1 mm / min. When the load reaches 0.1 MPa, the load is reduced to 0.01 MPa at a speed of 0.1 mm / min. The above cycle counts as one cycle, and this process is repeated for five cycles. At this time, Fs curves (load-displacement curves) on the pressurized side for the first and fifth cycles are obtained (see FIG. 8). Based on the obtained Fs curve, the storage cell thickness at 0.04 MPa in the first cycle is plotted and designated as X1. On the other hand, based on the obtained Fs curve, the storage cell thickness at 0.04 MPa in the fifth cycle is plotted and designated as X5. Then, the cell thickness change amount (%) is calculated by the following formula (i). (X1-X5) / X1×100...Formula (i)

[0051] There are no particular limitations on the method for controlling the numerical range of the cell thickness change amount of the energy storage cell 100, and it can be controlled by various methods. For example, the cell thickness change amount of the energy storage cell 100 can be controlled by adjusting the gap 26s of the separator 26, the size of the wound electrode body 20, etc.

[0052] The method for controlling the numerical range of the cell thickness change of the energy storage cell 100 is not limited thereto, but for example, the cell thickness change can be controlled by adjusting the length Ln of the width direction Y of the negative electrode active material layer 24a of the wound electrode body 20. At this time, the length Ln of the width direction Y of the negative electrode active material layer 24a is preferably 20 cm or more. With this configuration, the inflow and outflow of the non-aqueous electrolyte into and from the inside of the wound electrode body 20 can be suitably controlled. That is, the numerical range of the cell thickness change of the energy storage cell 100 can be controlled. Similarly, the numerical range of the cell thickness change of the energy storage cell 100 can be controlled by adjusting the ratio (Ln / T) of the width direction length Ln of the negative electrode active material layer 24a to the height T of the wound electrode body 20 (electrode body aspect ratio). In this case, the electrode body aspect ratio is preferably 2.8 to 3.2. With this configuration, the inflow and outflow of the non-aqueous electrolyte into and from the inside of the wound electrode body 20 can also be suitably controlled.

[0053] The method for controlling the numerical range of the cell thickness change of the energy storage cell 100 is not limited thereto. For example, when an adhesive layer is present on the surface of the separator 26, the thickness change can be controlled by adjusting the ratio of the area where the adhesive layer is formed (area of ​​the adhesive layer formation region / area of ​​the separator×100). In this case, the ratio of the area where the adhesive layer is formed is preferably about 3 to 30%, and more preferably about 5 to 15%. In addition, it is preferable to apply the adhesive layer on the surface of the separator 26 in a dot pattern. This can suitably increase the voids 26s of the separator 26 and increase the amount of non-aqueous electrolyte retained. In addition, the ratio of the volume of the adhesive layer to the volume between the electrode (positive electrode or negative electrode) and the substrate of the separator (Vol%) (volume of the adhesive layer of the separator / volume between the electrode and the substrate of the separator×100) is preferably 50 to 97 vol%, and more preferably 85 to 95 vol%. By employing a wound electrode body having such a numerical range, the numerical range of the cell thickness change amount of the energy storage cell 100 can be controlled to a suitable numerical range.

[0054] The method for controlling the numerical range of the cell thickness change of the energy storage cell 100 is not limited to the above, and can be controlled, for example, by adjusting the particle size (D50) of the inorganic particles contained in the adhesive layer and the heat-resistant layer. In this case, the particle size (D50) of the inorganic particles contained in the adhesive layer and the heat-resistant layer is preferably about 0.1 to 0.6 μm. In this specification, the particle size (D50) of the inorganic particles refers to the average particle diameter of 50 wt% cumulative weight calculated from the smallest particle size in the particle size distribution measured by a laser diffraction method.

[0055] In the preparation process S10, a storage cell 100 having a numerical range of the cell thickness change of 0.3% or more (≧0.3) may be prepared, or the cell thickness change may be measured in the preparation process S10 by the method described above to confirm that the numerical range of the cell thickness change of the storage cell 100 is 0.3% or more (≧0.3).

[0056] Although the upper limit of the cell thickness change amount is not particularly limited, the thickness of the energy storage cells 100 in the pre-constraint state (before stack assembly) increases accordingly as the cell thickness change amount increases. Therefore, from the viewpoints of downsizing the assembly device in the stacking step S20 and saving labor in the stacking step S20, it is preferable that the cell thickness change amount is 2.0% or less.

[0057] (Lamination process S20) In the stacking step S20, the multiple energy storage cells 100 are stacked along the thickness direction X of the energy storage cells 100. The stacking step S20 may be the same as a conventionally known stack manufacturing method. Here, the multiple energy storage cells 100 are sandwiched between a pair of end plates 310 in the arrangement direction X, and are constrained by side plates 320 and multiple screws 330. At this time, a restraining load is applied in the stacking direction of the energy storage cells 100 by the restraining mechanism 300. In this manner, the stack 500 according to this embodiment is manufactured. The restraining load during cell stacking in the stacking step S20 may be, for example, 2 to 30 kN, and is preferably 3 to 20 kN.

[0058] <Method of manufacturing the energy storage cell 100> Although not particularly limited, the storage cell 100 in the preparation step S10 can be prepared, for example, by the manufacturing method shown below. The manufacturing method of the storage cell 100 shown below is an example of the preparation step S10 in this specification. FIG. 11 is a flow diagram showing a manufacturing method of the storage cell 100 according to one embodiment. As shown in FIG. 11, although not particularly limited, the storage cell 100 can be manufactured by a manufacturing method that typically includes, for example, an assembly step S101, a drying step S102, a liquid injection step S103, a degassing and charging step S104, a pressure reduction step S105, a liquid injection hole sealing step S106, an activation step S107, and an aging step S108 in this order. In addition, in the manufacturing method of the storage cell 100 disclosed herein, in addition to the above steps, other steps may be further included at any stage, and the other manufacturing processes may be the same as those of the conventional method.

[0059] (Assembly process S101) In the assembly process S101, the wound electrode body 20 is placed in the case 10 (exterior body 12) to prepare an assembly. In this specification, the term "assembly" refers to an electricity storage cell that has been assembled to a state prior to the liquid injection hole sealing process described later.

[0060] In the assembly process S101, the positive electrode second current collecting portion 52 is attached to the positive electrode tab group 23 of the wound electrode body 20, and further the negative electrode current collecting portion 60 and the negative electrode second current collecting portion 62 are attached to the negative electrode tab group 25. Next, the positive electrode terminal 30 and the negative electrode terminal 40 are attached to the sealing plate 14. Next, the positive electrode terminal 30 and the positive electrode first current collecting portion 51, and the negative electrode terminal 40 and the negative electrode first current collecting portion 61 are respectively joined by a conventionally known method (for example, ultrasonic joining, resistance welding, laser welding, etc.). Next, the wound electrode body 20 is accommodated in an insulating sheet. The insulating sheet can be prepared by folding an insulating resin sheet made of a resin material such as polyethylene (PE) into a bag shape or a box shape. Then, it is preferable to accommodate (insert) the wound electrode body 20 covered with the insulating sheet into the internal space of the exterior body 12. Then, the exterior body 12 of the case 10 and the sealing plate 14 are joined to prepare an assembly. Such joining can be performed by welding, for example, laser welding, etc. In the assembly step S101, the liquid injection hole 15 is not sealed.

[0061] In the assembly process S101, the wound electrode body 20 is preferably arranged side by side in a direction (short side direction X) in which the thickness direction of the energy storage cell 100 (in other words, a direction substantially perpendicular to the first side wall 12b of the case 10) coincides with the thickness direction of the wound electrode body 20. In other words, the wound electrode body 20 is preferably arranged inside the exterior body 12 with the winding axis WL parallel to the bottom 12a of the exterior body 12.

[0062] (Drying process S102) In the drying step S102, the assembly is dried to remove moisture contained in the assembly (e.g., the inside of the wound electrode body 20, etc.). Such a drying method can be performed by a known method. For example, the drying step S102 can be performed by transporting the assembly (the case 10 containing the wound electrode body 20) to a drying furnace (not shown) and heating it.

[0063] The drying temperature and drying time in the drying step S102 can be appropriately adjusted according to the amount of moisture contained in the wound electrode body 20. The drying temperature is not particularly limited as long as it is within a range in which moisture can be removed, but it is desirable to dry at a temperature at which the separator 26 of the wound electrode body 20 is not damaged. In addition, the drying step S102 is preferably performed in a reduced pressure atmosphere. This allows the drying time in the drying step S102 to be shortened. However, this is not limited to this, and the drying step S102 may be performed in an atmospheric pressure atmosphere. Note that the drying step S102 is not an essential step in the technology disclosed herein. In some preferred embodiments, the drying step S102 can be omitted.

[0064] (Liquid injection process S103) In the liquid injection step S103, a non-aqueous electrolyte is injected into the case 10 housing the wound electrode body 20 through an injection hole 15 provided in the sealing plate 14. The liquid injection step S103 may be performed in an atmospheric pressure atmosphere or a reduced pressure atmosphere, but is preferably performed in a reduced pressure atmosphere. This improves the impregnation of the non-aqueous electrolyte into the wound electrode body 20, and the liquid injection step S103 can be performed in a shorter time. In the liquid injection step S103, the non-aqueous electrolyte is injected in an amount that spreads throughout the entire wound electrode body 20. A conventionally known non-aqueous electrolyte injection device can be appropriately used for the liquid injection step S103. At this time, the pressurized gas that can be used to pressurize the non-aqueous electrolyte can be nitrogen (N 2 ) or dry air. After the liquid injection step S103 is completed, it is preferable to appropriately pressurize or depressurize the inside of the case 10.

[0065] (Gas removal and charging process S104) In the degassing charging step S104, the assembly is charged. This allows a coating to be formed on the surface of the negative electrode active material layer 24a. Furthermore, by discharging the gas generated during charging and discharging to the outside of the case 10, the amount of gas generated inside the case 10 after the liquid injection hole 15 is sealed can be reduced, and gas can be prevented from accumulating inside the wound electrode body 20 after the liquid injection hole 15 is sealed. The charging conditions in this step are not particularly limited, and may be the same as those in conventional manufacturing methods. Although not particularly limited, for example, the degassing charging step S104 can be performed by charging at a current of about 0.05C to 10C in a room temperature environment (for example, 25°C) until the SOC (State of Charge) reaches about 20% to 90%.

[0066] In the degassing and charging step S104, it is preferable to perform the degassing and charging step S104 with the case 10 restrained and a load applied to the case 10. This makes it easier to push out the gas in the case 10, so that gas trapping in the electrode body can be suppressed. When restraining the case 10 in the degassing and charging step S104, it is preferable to apply a load to the first side wall 12b of the case 10. In addition, in such restraint, it is preferable to restrain the case 10 so that the center CP (see FIG. 3) of the wound electrode body 20 and the center of the restrained area substantially coincide with each other when viewed from the front from the first side wall 12b of the case 10. In addition, the restrained area is not particularly limited, but it is preferable to restrain an area of ​​280 to 295 mm in the long side direction Y and 85 to 95 mm in the vertical direction Z from the center CP of the wound electrode body 20 on the first side wall 12b of the case 10. The load applied to the case 10 is not particularly limited, but it is preferable that it is 0.25 to 0.80 MPa. In this specification, the "center CP of the wound electrode body 20" refers to the point where the center MY in the long side direction Y and the center MZ in the vertical direction Z intersect perpendicularly on the surface of the wound electrode body 20 having the flat portion 20f (the surface facing the first side wall 12b of the case 10), as shown in Figure 3.

[0067] (Decompression step S105) In the depressurization step S105, the pressure inside the case 10 is reduced, thereby further discharging gas present inside the case 10 (for example, air or gas generated in the degassing / charging step S104) to the outside of the case 10. The depressurization step S105 may be the same as the means used in the depressurization step in this type of conventional manufacturing method, and is not a particular feature of the technology disclosed herein, so further detailed description will be omitted. Note that the depressurization step S105 is not an essential step in the technology disclosed herein. In some preferred embodiments, the depressurization step S105 can be omitted.

[0068] (Injection hole sealing process S106) In the liquid injection hole sealing step S106, the liquid injection hole 15 of the assembly is sealed. The liquid injection hole sealing step S106 may be the same as a conventionally known method for manufacturing the energy storage cell 100, and is not particularly limited. Here, the liquid injection hole 15 is sealed with a metallic sealing member 16, and is sealed by welding a metal portion of the sealing member 16 to the sealing plate 14 (the peripheral portion of the liquid injection hole 15). However, the method for sealing the liquid injection hole 15 is not limited to this. Although not shown in the drawings, the liquid injection hole 15 may be sealed with a rivet such as a blind rivet.

[0069] (Activation step S107) In the activation step S107, the energy storage cell 100 in which the liquid injection hole 15 has been sealed through the liquid injection hole sealing step S106 is charged while a load is applied in the thickness direction of the energy storage cell 100. This causes a coating to be formed on the surface of the negative electrode active material layer 24a. The activation step S107 is included as an example of the "preparation step S10" in this specification.

[0070] The charging conditions in the activation step S107 are not particularly limited and may be the same as those in the conventional manufacturing method. For example, the activation step S107 can be performed by charging at a current of about 0.05C to 10C in a normal temperature environment (e.g., 25°C) until the SOC (State of Charge) reaches about 20% to 90%.

[0071] In the activation step S107, the load applied to the energy storage cell 100 is preferably 0.5 to 0.7 MPa. With this configuration, the amount of change in cell thickness can be set within a more preferable range. The method of applying the load to the energy storage cell 100 is not particularly limited, and any general means that can be adopted in conventional energy storage cell manufacturing methods can be adopted. For example, the load can be applied to the energy storage cell 100 by sandwiching a pair of first side walls 12b of the energy storage cell 100 between restraining plates and connecting the restraining plates with a bridging member.

[0072] (Aging process S108) In the aging step S108, the storage cell 100 that has been through the activation step S107 is stored for a predetermined time in a predetermined temperature environment while maintaining the charged state. This makes it possible to more suitably form a coating on the surface of the negative electrode active material layer 24a. Note that in the technology disclosed herein, the aging step S108 is not an essential step. In some preferred embodiments, the aging step S108 can be omitted.

[0073] The conditions of the aging step S108 can be appropriately adjusted according to the required mode of film formation, and are not particularly limited. For example, the cell temperature (aging temperature) in the aging step S108 can be 30°C or higher, preferably 40°C or higher, for example 50°C or higher, and further 60°C or higher. The upper limit of the aging temperature is not particularly limited, but can be set to about 70°C or lower, for example. For temperature control in the aging step S108, a thermostatic bath or the like can be used. The implementation time of the aging step S108 (aging time) can be appropriately changed according to, for example, the aging temperature, and is not particularly limited. For example, when the aging temperature is about 45 to 65°C, the aging time is preferably about 3 to 30 hours.

[0074] In the aging step S108, aging is preferably performed while applying a load in the thickness direction X of the energy storage cell 100. The amount of load applied to the energy storage cell in the aging step S108 is not particularly limited, but is preferably 0.5 to 0.7 MPa. In addition, the aging step S108 can be performed while maintaining the load applied in the activation step S107.

[0075] The stack 500 can be used for various purposes, but can be suitably used, for example, as a power source (driving power source) for a motor mounted on a vehicle such as a passenger car, a truck, etc. The type of vehicle is not particularly limited, but examples thereof include a plug-in hybrid electric vehicle (PHEV), a hybrid electric vehicle (HEV), and a battery electric vehicle (BEV).

[0076] Hereinafter, examples of the technology disclosed herein will be described, but the technology disclosed herein is not intended to be limited to these examples.

[0077] <Preparing the storage cells> First, three storage cells for constructing a stack according to the embodiment were prepared. The wound electrode body housed in the storage cell according to the embodiment had a pair of curved parts as shown in FIG. 5, and a strip-shaped positive electrode and a strip-shaped negative electrode were laminated via a strip-shaped separator and wound in the longitudinal direction. As the separator of Example 1, a separator was used in which the adhesive layer and the heat-resistant layer had a ratio of the formation area of ​​30% and the particle size of the inorganic particles contained in the heat-resistant layer was 0.5 μm. The width of the negative electrode active material layer formation region of the storage cell according to the embodiment was 29 cm, and the electrode body aspect ratio (the ratio (Ln / T) of the width direction length Ln of the negative electrode active material layer to the height T of the wound electrode body) was 3.0. The number of stacked positive electrodes for the wound electrode body was 33 layers.

[0078] Next, as Example 2, three storage cells of Example 2 were prepared, which were the same as the storage cell of Example 1 except that a separator was used in which the adhesive layer formation area ratio was 7% and the inorganic particles in the adhesive layer had a particle size of 0.3 μm.

[0079] As Comparative Example 1, three storage cells according to Comparative Example 1 were prepared, which were the same as the storage cell according to Example 1 except that a separator was used in which the proportion of the area in which the adhesive layer was formed was 100% and the particle size of the inorganic particles in the adhesive layer was 1.0 μm. Similarly, as Comparative Example 2, three storage cells according to Comparative Example 2 were prepared, which were the same as the storage cell according to Example 1 except that a separator similar to that of Comparative Example 1 was used and that charging and discharging were performed while applying a load of 0.4 MPa in the thickness direction of the storage cell in the activation step. In addition, as Comparative Example 3, three storage cells according to Comparative Example 3 were prepared, which were the same as the storage cell according to Example 1 except that an electrode body having a so-called laminated structure in which a substantially rectangular positive electrode and a substantially rectangular negative electrode were laminated in the thickness direction X of the storage cell via a substantially rectangular separator was used (i.e., an electrode body that was not a wound electrode body), the aspect ratio of the electrode body was 1.6, the shape of the case was changed in conjunction with the change in the electrode body (however, the plate thickness and material were not changed), and charging and discharging were performed while applying a load of 0.18 MPa in the thickness direction of the storage cell in the activation process.

[0080] <Evaluation of cell thickness change> The cell thickness change amount was evaluated for the energy storage cells according to Examples 1 and 2 and Comparative Examples 1 to 3 by the above-mentioned method. The autograph used was a precision universal testing machine (Autograph AGX-V) manufactured by Shimadzu Corporation. The cell thickness was measured using a laser displacement meter LK-G157 manufactured by Keyence Corporation. First, as shown in FIG. 10, the energy storage cell was set in the autograph. Then, a load was applied to the energy storage cell in the thickness direction (indicated by the white arrow) at a speed of 0.1 mm / min. After the load applied to the energy storage cell reached 0.1 MPa, the load was reduced to 0.01 MPa at a speed of 0.1 mm / min. These processes constitute one cycle, and the processes were performed for 5 cycles. In this manner, Fs curves (load displacement curves) for the first and fifth cycles were obtained, respectively. From the obtained Fs curve, the cell thickness X1 at the first cycle with a surface pressure of 0.04 MPa and the cell thickness X5 at the fifth cycle with a surface pressure of 0.04 MPa were obtained, and the cell thickness change (%) was calculated using X1 and X5 according to formula (i). The results are shown in Table 1. Cell thickness change (%) = (X1-X5) / X1×100 Formula (i)

[0081] [Table 1]

[0082] <0.3~3kN spring constant> A "0.3-3 kN spring constant" was calculated for the energy storage cells according to Examples 1-2 and Comparative Examples 1-3. In this specification, the "0.3-3 kN spring constant" is an index showing the degree of stack restraint load loss when the cell thickness is reduced. Specifically, based on the Fs curve obtained above, a graph was created in which the cell thickness change during the same load between the 1st and 5th cycles is plotted on the horizontal axis as Δcell thickness (mm) and the applied load (kN) on the vertical axis. Then, the spring constant when the load range was 0.3-3 kN was calculated as the "0.3-3 kN spring constant (kN / mm)". The "0.3-3 kN spring constant" was calculated according to the following formula (ii). The results are shown in Table 1. 0.3~3kN spring constant (kN / mm) = -((3-0.3)(kN) / (Δ cell thickness at 3kN - Δ cell thickness at 0.3kN))(mm) ··· Equation (ii) 12 is a graph plotting the change in cell thickness between the first and fifth cycles under the same load as Δcell thickness (mm) on the horizontal axis and the applied load (kN) on the vertical axis for Examples 1 and 2 and Comparative Example 2. In the graph of FIG. 12, the region where the load is between 0.3 and 3 kN is indicated by a thick line.

[0083] <Result> As can be seen from Table 1, Examples 1 and 2 in which the cell thickness change was 0.3% or more (≧0.3) had a lower "0.3-3 kN spring constant" compared to Comparative Examples 1-3. This indicates that even when the cell thickness is reduced due to a low temperature environment, low SOC conditions, or the like, the thickness of the power storage cell is suitably controlled (the power storage cell thickness increases again), and the degree of loss of the stack restraining load is small. Therefore, in a stack manufactured using a power storage cell in which the cell thickness change was 0.3% or more (≧0.3), even when the thickness of the power storage cell is reduced, the power storage cell thickness is suitably controlled, and therefore a decrease in the stack restraining load can be suppressed (loss of the restraining load is small).

[0084] Although the preferred embodiment of the present disclosure has been described above, the above embodiment is merely an example. The present disclosure can be implemented in various other forms. The present disclosure can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The technology described in the claims includes various modifications and changes to the above-exemplified embodiments. For example, it is possible to replace a part of the above-mentioned embodiment with another modification, and it is also possible to add another modification to the above-mentioned embodiment. In addition, if the technical feature is not described as essential, it is also possible to delete it as appropriate.

[0085] As described above, specific aspects of the technology disclosed herein include those described in the following sections. Item 1: A method for manufacturing a stack including a plurality of rectangular storage cells, the method comprising: a preparation step of preparing the storage cells including a flat-shaped wound electrode body formed by stacking and winding a positive electrode and a negative electrode with a separator interposed therebetween, a non-aqueous electrolyte, and a case that accommodates the wound electrode body and the non-aqueous electrolyte; and a stacking step of stacking a plurality of the storage cells along a thickness direction of the storage cells, the stacking step applying a load of 0.1 mm to the storage cells prepared in the preparation step in the thickness direction of the storage cells. a storage cell thickness X1 at a surface pressure of 0.04 MPa on the pressure-side Fs curve in the first cycle and a storage cell thickness X5 at a surface pressure of 0.04 MPa on the pressure-side Fs curve in the fifth cycle satisfy the following formula: (X1-X5) / X1×100≧0.3. Item 2: The method for manufacturing a stack according to item 1, wherein the negative electrode comprises a negative electrode core and a negative electrode active material layer formed on the negative electrode core, and a length Ln of the negative electrode active material layer in a width direction perpendicular to the longitudinal direction of the wound electrode body is 20 cm or more. Item 3: The method for producing a stack according to item 2, wherein, when a length in a direction perpendicular to a winding axis direction of the wound electrode body and perpendicular to a thickness direction of the wound electrode body is defined as a height T of the wound electrode body, a ratio (Ln / T) of a length Ln in a width direction of the negative electrode active material layer to the height T of the wound electrode body is 2.8 to 3.2. Item 4: The method for manufacturing a stack according to any one of items 1 to 3, wherein the preparation step includes an activation step of charging the storage cell while applying a load in a thickness direction of the storage cell, and the load applied to the storage cell in the activation step is 0.5 to 0.7 MPa. Item 5: The method for producing a stack according to any one of Items 1 to 4, wherein the number of laminations of the positive electrode is 30 or more. Item 6: The method for manufacturing a stack according to any one of Items 1 to 5, wherein a relationship between a storage cell thickness X1 at a surface pressure of 0.04 MPa in a pressure-side Fs curve in a first cycle and a storage cell thickness X5 at a surface pressure of 0.04 MPa in a pressure-side Fs curve in a fifth cycle further satisfies the following formula: (X1-X5) / X1×100≦2.0. [Explanation of symbols]

[0086] 10 Cases 12 Exterior body 14 Sealing plate 20 Wound electrode body 22 Positive electrode 24 Negative electrode 26 Separator 26s void 100 Energy Storage Cells 300 Restraint mechanism 500 stack 600 Autograph S10 Preparation process S20 Lamination process S101 Assembly process S102 Drying process S103 Liquid injection process S104 Gas removal and charging process S105 Decompression process S106 Liquid injection hole sealing process S107 Activation process S108 Aging process

Claims

1. A method for manufacturing a stack including a plurality of rectangular energy storage cells, a preparation step of preparing the storage cell including a flat wound electrode body formed by stacking and winding a positive electrode and a negative electrode with a separator interposed therebetween, a non-aqueous electrolyte, and a case that accommodates the wound electrode body and the non-aqueous electrolyte; a stacking step of stacking a plurality of the energy storage cells along a thickness direction of the energy storage cells, When a process of applying a load to the storage cell prepared in the preparing step in a thickness direction of the storage cell at a rate of 0.1 mm / min up to 0.1 MPa and then reducing the load to 0.01 MPa at a rate of 0.1 mm / min was defined as one cycle and the process was performed for five cycles, The relationship between the storage cell thickness X1 at a surface pressure of 0.04 MPa on the pressure-side F-s curve in the first cycle and the storage cell thickness X5 at a surface pressure of 0.04 MPa on the pressure-side F-s curve in the fifth cycle is The following formula: (X1-X5) / X1×100≧0.3 fulfill, Stack manufacturing method.

2. the negative electrode includes a negative electrode core and a negative electrode active material layer formed on the negative electrode core, The length Ln in the width direction of the negative electrode active material layer, which is perpendicular to the longitudinal direction of the wound electrode body, is 20 cm or more. A method for manufacturing the stack of claim 1 .

3. When the length in a direction perpendicular to the winding axis direction of the wound electrode body and perpendicular to the thickness direction of the wound electrode body is defined as the height T of the wound electrode body, a ratio (Ln / T) of a length Ln in the width direction of the negative electrode active material layer to a height T of the wound electrode body is 2.8 to 3.2; A method for manufacturing the stack according to claim 2 .

4. the preparation step includes an activation step of charging the storage cell while applying a load to the storage cell in a thickness direction of the storage cell, In the activation step, a load applied to the storage cell is 0.5 to 0.7 MPa. A method for manufacturing a stack according to claim 1 or 2.

5. The number of stacked layers of the positive electrode is 30 or more. A method for manufacturing a stack according to claim 1 or 2.

6. The relationship between the storage cell thickness X1 at a surface pressure of 0.04 MPa on the pressure-side F-s curve in the first cycle and the storage cell thickness X5 at a surface pressure of 0.04 MPa on the pressure-side F-s curve in the fifth cycle is The following formula: (X1-X5) / X1×100≦2.0 Further satisfying A method for manufacturing a stack according to claim 1 or 2.

Citation Information

Patent Citations

  • Partially coated separator

    JP2001118558A

  • Lithium secondary cell and manufacturing method thereof

    JP2011054502A

  • Laminate and secondary battery member

    JP2019117800A

  • Separator for lithium secondary battery, and lithium secondary battery comprising same

    US20220102810A1

  • Nonaqueous electrolyte secondary battery

    JP2018055806A