Polarizing plate
The polarizing plate design with a polyester resin film and acrylic resin film addresses rainbow unevenness and power consumption issues, enhancing display quality and efficiency.
Patent Information
- Application Number
- JP2023055365
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing polarizing plates suffer from visible rainbow unevenness from oblique directions and increased power consumption due to high backlight luminosity, which is not adequately addressed by current technologies.
A polarizing plate design comprising a polyester resin film with specific retardation values and thickness, combined with an acrylic resin film and adhesive layers, to enhance brightness and reduce rainbow unevenness while minimizing power consumption.
The proposed polarizing plate effectively suppresses rainbow unevenness and maintains good brightness, reducing power consumption by optimizing the retardation values and layer configurations.
Smart Images

Figure 2024142943000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizing plate, and further to a polarizing plate with a pressure-sensitive adhesive layer and an image display device that include the polarizing plate. [Background technology]
[0002] In recent years, there has been a demand for improved visibility of liquid crystal display devices. In order to improve the visibility of liquid crystal display devices, there is also a demand for suppressing unevenness in polarizing plates, which are one of the components constituting liquid crystal displays, and for improving the transmittance of the polarizing plates.
[0003] In order to suppress unevenness and improve the transmittance of a polarizing plate, the types and combinations of polarizer protective films in the polarizing plate have been studied. For example, Patent Document 1 describes that when a polyethylene terephthalate film is used as one polarizer protective film, an acrylic resin film is used as the other polarizer protective film, thereby improving the optical durability of the polarizing plate in a high-temperature environment and improving the transmittance. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2016-500833 Summary of the Invention [Problem to be solved by the invention]
[0005] However, even with the polarizing plate described in Patent Document 1, rainbow unevenness visible from an oblique direction of the polarizing plate cannot be sufficiently suppressed.
[0006] In addition, in order to improve the display quality of a liquid crystal display device, such as high brightness, it is common to increase the luminous intensity of the backlight of the liquid crystal display device. Since an increase in the luminous intensity of the backlight increases power consumption, it is required to suppress this increase in consideration of carbon neutrality, etc. Therefore, polarizing plates are also being studied to suppress the increase in power consumption. However, the polarizing plate described in Patent Document 1 does not sufficiently suppress the increase in power consumption.
[0007] An object of the present invention is to provide a polarizing plate which suppresses rainbow unevenness visible from an oblique direction of the polarizing plate and has good luminance. [Means for solving the problem]
[0008] The present invention includes the following inventions. [1] A polarizing plate comprising, in this order, a polyester resin film, a first adhesive layer, a polarizer, a second adhesive layer, and an acrylic resin film, The polarizing plate has a visibility-corrected single transmittance of 43.0% or more, The polyester resin film is a polarizing plate in which the retardation value Re defined by the formula (1) satisfies the following [i] to [iv]. Re = (n x -n y )×d (1) [where n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and d represents the thickness of the film. [i] The retardation value Re1 measured in a first arrangement in which the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 90° is 6000 nm or more. [ii] The polyester-based resin film in the first arrangement is rotated 30° about its fast axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this second arrangement, the phase difference value Re2 is measured to be 5000 nm or more. [iii] The polyester-based resin film in the first arrangement is rotated by 30° around an axis that is at an angle of 45° to the fast axis in the plane of the polyester-based resin film as a central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this third arrangement, the phase difference value Re3 measured is 6000 nm or more. [iv] The polyester-based resin film in the first arrangement is rotated 30° about its slow axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this fourth arrangement, the phase difference value Re4 measured is 7000 nm or more. [2] The polarizing plate according to [1], wherein the polyester resin film has a thickness of 60 μm or more. [3] The polarizing plate according to [1] or [2], wherein the ratio of a retardation value Re1 to a retardation value Rth in the thickness direction of the polyester resin film defined by the formula (2) is 0.5 or more. Rth = (n x +n y ) / 2-n z 〕×d (2) [where n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and n z represents the refractive index in the thickness direction of the film, and d represents the thickness of the film. [4] The polarizing plate according to any one of [1] to [3], wherein the polarizing plate has a luminosity-corrected polarization degree of 99.996% or more. [5] The polarizing plate according to any one of [1] to [4], wherein the polarizing plate has a luminous efficiency-corrected single transmittance of 44.5% or less. [6] A polarizing plate with a pressure-sensitive adhesive layer, comprising the polarizing plate according to any one of [1] to [5] and a pressure-sensitive adhesive layer, A polarizing plate with a pressure-sensitive adhesive layer, in which the pressure-sensitive adhesive layer is laminated on a surface of the (meth)acrylic resin film opposite to the polarizer. [7] A liquid crystal display device comprising the polarizing plate with the pressure-sensitive adhesive layer according to [6]. Effect of the Invention
[0009] The present invention can provide a polarizing plate that suppresses rainbow unevenness visible from an oblique direction of the polarizing plate and has good luminance. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the polarizing plate of the present invention. [Diagram 2] FIG. 11 is a schematic perspective view for explaining a phase difference value Re1 and a method for measuring the same. [Diagram 3] FIG. 13 is a schematic perspective view illustrating a phase difference value Re2 and a method for measuring the phase difference value Re2. [Figure 4] FIG. 11 is a schematic perspective view illustrating a phase difference value Re3 and a method for measuring the phase difference value Re3. [Diagram 5] FIG. 13 is a schematic perspective view illustrating a phase difference value Re4 and a method for measuring the same. [Figure 6] FIG. 2 is a schematic cross-sectional view showing another example of the polarizing plate of the present invention. [Figure 7] FIG. 1 is a schematic cross-sectional view showing an example of a pressure-sensitive adhesive layer-attached polarizing plate of the present invention. [Figure 8] FIG. 1 is a schematic cross-sectional view showing an example of an optical laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The polarizing plate of the present invention comprises, in this order, a polyester resin film, a first adhesive layer, a polarizer, a second adhesive layer, and a (meth)acrylic resin film. An example of the layer structure of the polarizing plate of the present invention is shown in Figure 1. The polarizing plate 1 shown in Figure 1 includes a polyester resin film 10, a first adhesive layer 15, a polarizer 30, a second adhesive layer 25, and a (meth)acrylic resin film 20, in this order. 1, in the polarizing plate of the present invention, the polyester resin film 10 and the first adhesive layer 15 are preferably in direct contact with each other. Also, the (meth)acrylic resin film 20 and the second adhesive layer 25 are preferably in direct contact with each other. The polarizer 30 and the first adhesive layer 15 are preferably in direct contact with each other. The polarizer 30 and the second adhesive layer 25 are preferably in direct contact with each other.
[0012] The luminosity-corrected single transmittance of the polarizing plate in the present invention is 43.0% or more. When the luminosity-corrected single transmittance of the polarizing plate is 43.0% or more, the brightness of the polarizing plate tends to be good. The luminosity-corrected single transmittance of the polarizing plate is preferably 43.2% or more, more preferably 43.3% or more, and even more preferably 43.5% or more. The luminosity-corrected single transmittance of the polarizing plate may be, for example, less than 50.0%, or may be 49.0% or less, 47.0% or less, or 45.0% or less. The luminosity-corrected polarization degree of the polarizing plate in the present invention is preferably 99.995% or more. When the luminosity-corrected polarization degree of the polarizing plate is 99.995% or more, the contrast tends to be increased when the polarizing plate is incorporated into an image display device. The luminosity-corrected polarization degree of the polarizing plate is preferably 99.996% or more, more preferably 99.997% or more, and is usually 100% or less, and may be, for example, less than 100%, 99.999% or less, or 99.998% or less. In addition, if the polarizing plate has a luminosity-corrected polarization degree of 99.996% or more and a luminosity-corrected single transmittance of 44.5% or less, the polarizing plate tends to reduce the light leakage phenomenon when incorporated into an image display device in a liquid crystal display device that divides a direct-type LED backlight into multiple regions to control the brightness. From the viewpoint of reducing the light leakage phenomenon, the luminosity-corrected single transmittance of the polarizing plate is preferably 44.5% or less, more preferably 44.3% or less, even more preferably 44.0% or less, and even more preferably 43.7% or less. From the viewpoint of reducing the light leakage phenomenon, the luminosity-corrected polarization degree of the polarizing plate is preferably 99.997% or more, and usually 100% or less, and may be, for example, less than 100%, or 99.999% or less, or 99.998% or less. The luminosity-corrected single transmittance and luminosity-corrected polarization degree of the polarizing plate can be obtained, for example, by selecting the material constituting the polarizing plate, or by adjusting the luminosity-corrected single transmittance and luminosity-corrected polarization degree of the polarizer, for example, by adjusting the amount of dichroic dye or boric acid contained in the dye bath and crosslinking bath when producing the polarizer, the immersion time in each treatment bath, the temperature of each treatment bath, and the total stretch ratio based on the original film. The luminosity-corrected single transmittance and luminosity-corrected polarization degree of the polarizing plate can be measured according to the method described in the Examples section.
[0013] <Polyester resin film> The polyester resin film preferably has a retardation Re defined by the following formula (1) that satisfies the following [i] to [iv]. Re = (n x -n y )×d (1) [where n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane (the direction perpendicular to the slow axis direction in the film plane), and d represents the thickness of the film. [i] The retardation value Re1 measured in a first arrangement in which the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 90° is 6000 nm or more. [ii] The polyester-based resin film in the first arrangement is rotated 30° about its fast axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this second arrangement, the phase difference value Re2 is measured to be 5000 nm or more. [iii] The polyester-based resin film in the first arrangement is rotated by 30° around an axis that is at an angle of 45° to the fast axis in the plane of the polyester-based resin film as a central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this third arrangement, the phase difference value Re3 measured is 6000 nm or more. [iv] The polyester-based resin film in the first arrangement is rotated 30° about its slow axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this fourth arrangement, the phase difference value Re4 measured is 7000 nm or more.
[0014] The slow axis direction in the film plane is the direction in which the refractive index is maximum in the plane. In addition, in this specification, the retardation value Re is the retardation value at a wavelength of 587 nm.
[0015] 2 is a schematic perspective view illustrating the retardation value Re1 and a method for measuring the retardation value Re1. The retardation value Re1 is a retardation value measured in a first arrangement in which the polyester resin film 100 is arranged so that the angle between the surface of the polyester resin film 100 and a measurement direction 210 is 90°. The measurement direction is a direction from a light source 201 of the retardation measurement device to an observation device 202 that detects and observes light transmitted through the polyester resin film, and is the so-called optical path of the retardation measurement device.
[0016] 3 is a schematic perspective view illustrating the retardation value Re2 and a method for measuring the retardation value Re2. The retardation value Re2 is a retardation value measured for a polyester resin film tilted by rotating the polyester resin film 100 in the first arrangement by 30° about its fast axis 400 as a central axis 300, that is, a polyester resin film 110 in the second arrangement. The angle between the surface of the polyester resin film 110 in the second arrangement and the measurement direction 210 is 60°.
[0017] 4 is a schematic perspective view illustrating the retardation value Re3 and its measurement method. The retardation value Re3 is a retardation value measured for a polyester resin film tilted by rotating the polyester resin film 100 in the first arrangement by 30° around an axis 310 that forms an angle of 45° with respect to the fast axis 400 in the polyester resin film plane, that is, a polyester resin film 120 in the third arrangement. The angle between the plane of the polyester resin film 120 in the third arrangement and the measurement direction 210 is 60°.
[0018] 5 is a schematic perspective view illustrating the retardation value Re4 and its measurement method. The retardation value Re4 is a retardation value measured for a polyester resin film tilted by rotating the polyester resin film 100 in the first arrangement by 30° about its slow axis 500 as the central axis 320, that is, a polyester resin film 130 in the fourth arrangement. The angle between the surface of the polyester resin film 130 in the fourth arrangement and the measurement direction 210 is 60°.
[0019] The retardation value Re1 of the polyester resin film is preferably 7000nm or more, more preferably 7500nm or more, and even more preferably 8000nm or more. The retardation value Re1 of the polyester resin film is usually 30000nm or less, preferably 20000nm or less, more preferably 15000nm or less, even more preferably 10000nm or less, and even more preferably 9000nm or less. When the upper limit of the retardation value Re1 exceeds 30000nm, the thickness of the polyester resin film becomes considerably large in order to satisfy the retardation value, and the handleability as an optical film tends to be greatly reduced. When the retardation value Re1 of the polyester resin film is 6000nm or more, it is easy to reduce rainbow unevenness (rainbow-like color spots) when viewed from an oblique direction.
[0020] The retardation value Re2 of the polyester resin film is 5000 nm or more. The retardation value Re2 is preferably 5500 nm or more, more preferably 6000 nm or more, even more preferably 6500 nm or more, and even more preferably 7000 nm or more. The retardation value Re2 is usually 30000 nm or less, preferably 20000 nm or less, more preferably 15000 nm or less, even more preferably 10000 nm or less, and even more preferably 9000 nm or less. When the retardation value Re2 of the polyester resin film is 5000 nm or more, rainbow unevenness when viewed from an oblique direction is easily reduced.
[0021] The phase difference value Re3 of the polyester resin film is 6000 nm or more. The phase difference value Re3 is preferably 7000 nm or more, more preferably 7500 nm or more, and even more preferably 8000 nm or more. The phase difference value Re3 is usually 30000 nm or less, preferably 20000 nm or less, more preferably 15000 nm or less, even more preferably 10000 nm or less, and even more preferably 9000 nm or less. When the phase difference value Re3 of the polyester resin film is 6000 nm or more, rainbow unevenness when viewed from an oblique direction is easily reduced.
[0022] The phase difference value Re4 of the polyester resin film is 7000 nm or more. The phase difference value Re4 is preferably 8000 nm or more, more preferably 8500 nm or more, and even more preferably 9000 nm or more. The phase difference value Re4 is usually 30000 nm or less, preferably 20000 nm or less, more preferably 15000 nm or less, and even more preferably 10000 nm or less. When the phase difference value Re4 of the polyester resin film is 7000 nm or more, rainbow unevenness when viewed from an oblique direction is easily reduced.
[0023] Re1 to Re4 can be measured using a phase difference measuring device (KOBRA-HB-RESPC, manufactured by Oji Scientific Instruments Co., Ltd.).
[0024] By using a polyester resin film in which Re1 to Re4 are each within the above range, rainbow unevenness visible from an oblique direction of the polarizing plate can be suppressed.
[0025] The ratio Re1 / Rth of the retardation value Re1 to the retardation value Rth in the thickness direction of the polyester resin film is usually 0.4 or more, preferably 0.5 or more, more preferably 0.6 or more, even more preferably 0.7 or more, and even more preferably 0.9 or more. If the ratio Re1 / Rth is large, rainbow unevenness due to the observation angle tends to be less likely to occur. Since the ratio Re1 / Rth is 2.0 in a completely uniaxial (uniaxially symmetric) film, the ratio Re1 / Rth is preferably 2.0 or less, and more preferably 1.5 or less.
[0026] The thickness direction retardation value Rth is expressed by the following formula (2): The thickness direction retardation value Rth is the thickness direction retardation value at a wavelength of 587 nm. Rth = (n x +n y ) / 2-n z 〕×d (2) [where n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and n z represents the refractive index in the film thickness direction (direction perpendicular to the film surface), and d represents the film thickness.
[0027] The angle between the fast axis or slow axis of the polyester resin film and the transmission axis of the polarizer is, for example, -20° to +20°, preferably -15° to +15°, more preferably -10° to +10°, even more preferably -5° to +5°, still more preferably -3° to +3°, particularly preferably -2° to +2°, and particularly preferably -1° to +1°. In a preferred embodiment, the fast axis or slow axis of the polyester resin film and the transmission axis of the polarizer are substantially parallel. Here, being substantially parallel means that the transmission axis of the polarizer and the fast axis or slow axis of the polyester resin film are parallel to an extent that allows for a misalignment that inevitably occurs when the polarizer and the polyester resin film are bonded together. The smaller the angle between the fast axis or slow axis of the polyester-based resin film and the transmission axis of the polarizer, the smaller the change in polarization state caused by linearly polarized light passing through the polyester-based resin film, and therefore the more likely it is that rainbow unevenness will be suppressed.
[0028] In order to suppress deterioration of the optically functional dye such as iodine contained in the polarizer, the polyester resin film preferably has a light transmittance of 40% or less at a wavelength of 380 nm. The light transmittance of 380 nm is more preferably 35% or less, even more preferably 30% or less, and particularly preferably 20% or less. If the light transmittance is 40% or less, deterioration of the optically functional dye due to ultraviolet light can be suppressed.
[0029] At least one layer selected from the group consisting of an antireflection layer and a low antireflection layer may be provided on at least one surface of the polyester resin film. The surface reflectance of the antireflection layer is preferably 5.7% or less. If the surface reflectance of the antireflection layer exceeds 5.7%, rainbow unevenness tends to be easily visible. The surface reflectance of the antireflection layer is more preferably 5.3% or less, even more preferably 5.0% or less, and particularly preferably 4.5% or less. The lower limit of the surface reflectance of the antireflection layer is not particularly limited, but is, for example, 2.0%. The surface reflectance can be measured by any method. For example, a polyester resin film is attached to a black acrylic plate via an adhesive on the opposite side of the antireflection layer side of the polyester resin film, and the light reflectance at a wavelength of 550 nm can be measured from the surface on the antireflection layer side using a spectrophotometer (CM-2600d, manufactured by Konica Minolta Japan, Inc.).
[0030] The anti-reflection layer may be a single layer or a multi-layer. Examples of the anti-reflection layer include an anti-glare hard coat layer having a fine uneven surface to prevent reflection of external light. The anti-glare hard coat layer may be formed by dispersing a filler inside the hard coat layer to form an uneven surface, or may be formed by embossing the hard coat layer to form an uneven surface. For example, when forming an anti-glare hard coat layer using an ultraviolet curing resin, a resin composition obtained by dispersing a filler in an ultraviolet curing resin may be applied to a polyester resin film and irradiated with ultraviolet light, or an ultraviolet curing resin may be applied to a polyester resin film and the coating film may be adhered to the uneven surface of a mold and irradiated with ultraviolet light.
[0031] As a material for forming the antiglare hard coat layer, an ultraviolet curable resin, a thermosetting resin, an electron beam curable resin, etc. can be used, but from the viewpoints of productivity, hardness, etc., an ultraviolet curable resin is preferably used.
[0032] The surface reflectance of the low antireflection layer is preferably 4.0% or less. The surface reflectance of the low antireflection layer is more preferably 3.0% or less, even more preferably 2.0% or less, even more preferably 1.5% or less, and particularly preferably 1.0% or less. The lower limit of the surface reflectance of the low antireflection layer is not particularly limited, but is, for example, 0.01%.
[0033] The low-reflection anti-layer may be a single layer or a multilayer. When the low-reflection anti-layer is a single layer, the anti-reflection effect can be obtained by forming the low-refractive index layer made of a material having a lower refractive index than the polyester resin film so that the thickness of the low-refractive index layer is 1 / 4 the wavelength of the light or an odd multiple of that wavelength. When the anti-reflection anti-layer is a multilayer, the anti-reflection effect can be obtained by laminating low-refractive index layers and high-refractive index layers alternately in two or more layers, with the thickness of each layer being appropriately controlled. If necessary, a hard coat layer can be laminated between the low-reflection anti-layer and the polyester resin film.
[0034] The low-reflection anti-layer may be a known one, and is preferably a layer formed by coating an organic thin film having a lower refractive index than the polyester resin film or the hard coat layer laminated on the polyester resin film.
[0035] The thickness of at least one layer selected from the group consisting of an antireflection layer and a low antireflection layer is usually 0.01 to 20 μm, preferably 0.03 to 1 μm, and more preferably 0.05 to 0.15 μm.
[0036] The surface reflectance of the polyester resin film is preferably 5.7% or less, more preferably 5.3% or less, even more preferably 4.0% or less, even more preferably 3.0% or less, particularly preferably 2.0% or less, and most preferably 1.5% or less. The surface reflectance of the polyester resin film is usually 0.01% or more. When the surface reflectance of the polyester-based resin film is 5.7% or less, rainbow unevenness in a polarizing plate to which the polyester-based resin film is applied tends to be more effectively suppressed. In addition, when at least one layer selected from the group consisting of an antireflection layer and a low reflection layer is laminated as described above, the surface reflectance of the entire laminate of at least one layer selected from the group consisting of an antireflection layer and a low reflection layer may be 5.7% or less. By lowering the surface reflectance, the interface reflectance between the substrate film and air can be lowered, and it is presumed that rainbow unevenness is suppressed.
[0037] In the case where at least one layer selected from the group consisting of an antireflection layer and a low antireflection layer is provided on only one surface of the polyester-based resin film, it is preferable that the at least one layer selected from the group consisting of an antireflection layer and a low antireflection layer is provided on the surface of the polyester-based resin film opposite the polarizer.
[0038] When providing at least one selected from the group consisting of an antireflection layer and a low antireflection layer, it is preferable that the polyester resin film has an easy-adhesion layer on its surface. In this case, from the viewpoint of suppressing interference due to reflected light, it is preferable to adjust the refractive index of the easy-adhesion layer so that it is close to the geometric mean of the refractive index of the antireflection layer or low antireflection layer and the refractive index of the polyester resin film. The refractive index of the easy-adhesion layer can be adjusted by a known method, and can be easily adjusted, for example, by adding titanium, germanium, or other metal species to the binder resin.
[0039] In order to improve the adhesion to the polarizer, the polyester-based resin film preferably has an easy-adhesion layer on at least one side thereof, the easy-adhesion layer being composed mainly of at least one of polyester resin, polyurethane resin, and polyacrylic resin. Here, the "main component" refers to a component that is 50% by mass or more of the solid components constituting the easy-adhesion layer. The coating liquid used to form the easy-adhesion layer is preferably an aqueous coating liquid containing at least one of water-soluble or water-dispersible copolymer polyester resin, acrylic resin, and polyurethane resin. Examples of these coating liquids include water-soluble or water-dispersible copolymer polyester resin solutions, acrylic resin solutions, and polyurethane resin solutions disclosed in Japanese Patent No. 3567927, Japanese Patent No. 3589232, Japanese Patent No. 3589233, Japanese Patent No. 3900191, and Japanese Patent No. 4150982, etc.
[0040] When a polyester resin is used as the easy-adhesion layer, it is preferable to use a water-soluble or water-dispersible resin in terms of compatibility with the polyvinyl alcohol resin. In order to make the polyester resin water-soluble or water-dispersible, it is preferable to copolymerize a compound containing a hydrophilic group such as a sulfonate group or a carboxylate group. Among them, a dicarboxylic acid component having a sulfonate group is suitable from the viewpoint of imparting hydrophilicity while maintaining the acid value of the polyester resin low and controlling the reactivity with the crosslinking agent. Examples of the dicarboxylic acid component having a sulfonate group include sulfoterephthalic acid, 5-sulfoisophthalic acid, 4-sulfonaphthaleneisophthalic acid-2,7-dicarboxylic acid, and 5-(4-sulfophenoxy)isophthalic acid or an alkali metal salt thereof, and among them, 5-sulfoisophthalic acid is preferable. The dicarboxylic acid component having a sulfonate group is preferably 1 to 15 mol %, more preferably 1.5 to 12 mol %, and even more preferably 2 to 10 mol % of the dicarboxylic acid component of the polyester resin. When the amount of the dicarboxylic acid component having a sulfonate group is equal to or more than the lower limit, it is suitable for making the polyester resin water-soluble or water-dispersible, whereas when the amount of the dicarboxylic acid component having a sulfonate group is equal to or less than the upper limit, it is suitable for improving adhesion to the polyester film substrate.
[0041] The easy-adhesion layer can be obtained by applying the coating liquid to one or both sides of a polyester resin film, drying the film at 100 to 150° C., and then stretching the film in the lateral direction. The final coating amount of the easy-adhesion layer is 0.05 to 0.20 g / m 2 The coating amount is preferably 0.05 g / m 2 If the coating amount is less than 0.20 g / m, the adhesion to the polarizer may be insufficient. 2 When the easy-adhesion layer is provided on both sides of the polyester-based resin film, the coating amount of the easy-adhesion layer on both sides may be the same or different, and each can be independently set within the above range.
[0042] It is preferable to add particles to the easy-adhesion layer to give it easy slipperiness. The average particle size of the particles is preferably 2 μm or less. If the average particle size of the particles exceeds 2 μm, the particles are likely to fall off from the easy-adhesion layer. Examples of particles to be contained in the easy-adhesion layer include inorganic particles such as titanium oxide, barium sulfate, calcium carbonate, calcium sulfate, silica, alumina, talc, kaolin, clay, calcium phosphate, mica, hectorite, zirconia, tungsten oxide, lithium fluoride, and calcium fluoride, and organic polymer particles such as styrene-based, acrylic-based, melamine-based, benzoguanamine-based, and silicone-based particles. These may be added to the easy-adhesion layer alone, or two or more types may be added in combination.
[0043] The coating liquid can be applied by any known method, such as reverse roll coating, gravure coating, kiss coating, roll brushing, spray coating, air knife coating, wire bar coating, and pipe doctor coating, which can be used alone or in combination.
[0044] The thickness of the polyester resin film is optional, but is usually 15 μm to 200 μm, preferably 20 μm to 100 μm, more preferably 25 μm to 95 μm, even more preferably 60 μm to 90 μm, and even more preferably 75 μm to 85 μm. If the thickness of the polyester-based resin film is less than 15 μm, the anisotropy of the mechanical properties of the film becomes significant, making it more susceptible to tears, breaks, etc., and the practicality of the film tends to decrease. On the other hand, if the thickness of the polyester-based resin film exceeds 200 μm, the thickness as a polarizing plate becomes too thick. When at least one layer selected from the group consisting of an antireflection layer and a low antireflection layer is provided as described above, the total thickness including the layer may be within the above range.
[0045] The polyester resin film used in the present invention can be produced according to a general polyester film production method, for example, by the method described in JP-A-2021-103319, JP-A-2021-99521, etc. The retardation values of Re1 to Re4 can be controlled within a specific range by appropriately setting the stretching ratio, stretching temperature, and film thickness. For example, a high retardation value can be easily obtained by increasing the stretching ratio, decreasing the stretching temperature, and increasing the film thickness. The retardation values of Re1 to Re4 can be set by selecting the film formation conditions and thickness from the above conditions, taking into account the physical properties required for processing.
[0046] The material for forming the polyester-based resin film is not particularly limited, and polyethylene terephthalate or polyethylene naphthalate can be used, but other copolymer components may be included. From the viewpoint of controlling the retardation value of the polyester-based resin film, the material for forming the polyester-based resin film is preferably a polyethylene terephthalate resin.
[0047] <(Meth)acrylic resin film> The (meth)acrylic resin film is excellent in mechanical properties, solvent resistance, scratch resistance, light resistance, transparency, cost, etc. By using a (meth)acrylic resin film as a polarizer protective film, it is possible to improve the mechanical strength and reduce the thickness of a polarizing plate, a liquid crystal panel including the same, and a liquid crystal display device. In addition, by using the above-mentioned polyester resin film as one polarizer protective film and a (meth)acrylic resin film as the other polarizer protective film, it is possible to effectively suppress rainbow unevenness when viewed from an oblique direction. Furthermore, by using the above-mentioned polyester resin film as one polarizer protective film and a (meth)acrylic resin film as the other polarizer protective film, it is possible to effectively suppress light leakage in a high-temperature environment.
[0048] The (meth)acrylic resin constituting the (meth)acrylic resin film means a material obtained by mixing a (meth)acrylic resin and additives added as necessary, and melt-kneading the mixture. In this specification, the term "(meth)acrylic resin" means either an acrylic resin or a methacrylic resin, and the "(meth)" in (meth)acrylic acid ester, (meth)acrylate, (meth)acryloyl, etc. has the same meaning.
[0049] The (meth)acrylic resin is preferably a polymer mainly composed of a (meth)acrylic acid ester. The (meth)acrylic resin may be a homopolymer of one type of (meth)acrylic ester, or may be a copolymer of a (meth)acrylic acid ester and another (meth)acrylic acid ester. Examples of the (meth)acrylic acid ester include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate, and the number of carbon atoms in the alkyl group is usually about 1 to 8. Examples of polymerizable monomers that can be copolymerized with the (meth)acrylic acid ester include styrene-based monomers such as styrene and alkylstyrene; monofunctional monomers such as unsaturated nitriles such as acrylonitrile and methacrylonitrile; and polyfunctional monomers such as alkenyl esters of unsaturated carboxylic acids such as allyl (meth)acrylate and methallyl (meth)acrylate; dialkenyl esters of dibasic acids such as diallyl maleate; and unsaturated carboxylic acid diesters of glycols such as alkylene glycol di(meth)acrylate. The (meth)acrylic resin film may contain two or more kinds of (meth)acrylic resins.
[0050] When the (meth)acrylic resin film contains two or more kinds of (meth)acrylic resins, it is preferable that the syndiotacticity (rr) of at least one of the (meth)acrylic resins is 50% or more. From the viewpoint of increasing the toughness of the film and increasing the heat resistance and adhesion to the polarizer of the film, the syndiotacticity (rr) of the triad is preferably 55% or more, more preferably 60% or more, even more preferably 65% or more, and even more preferably 70% or more. The syndiotacticity (rr) of the triad is usually 90% or less, and may be 85% or less.
[0051] The syndiotacticity (rr) of a triad is the proportion of two diads (diads) in a triad of three consecutive units that are both racemo (denoted as rr). The syndiotacticity (rr) of a triad (%) is calculated by the following formula: 1 The H-NMR spectrum is measured, and the area (X) of the region from 0.6 to 0.95 ppm and the area (Y) of the region from 0.6 to 1.35 ppm are measured from the spectrum when the internal standard TMS is set to 0 ppm, and the area is calculated as (X / Y)×100.
[0052] A (meth)acrylic resin having a triad syndiotacticity (rr) of 50% or more can be prepared, for example, according to the method described in WO 2016 / 080124.
[0053] When a (meth)acrylic resin having a syndiotacticity (rr) of 50% or more, expressed as a triad, is contained, the content of the (meth)acrylic resin having a syndiotacticity (rr) of 50% or more, expressed as a triad, relative to the entire (meth)acrylic resin, from the viewpoints of toughness of the film and adhesion to a polarizer, is preferably 1% by mass or more and 50% by mass or less, more preferably 5% by mass or more and 40% by mass or less, even more preferably 10% by mass or more and 35% by mass or less, and still more preferably 15% by mass or more and 30% by mass or less.
[0054] As the (meth)acrylic resin, a (meth)acrylic resin having a ring structure can be used. Examples of the (meth)acrylic resin having a ring structure include a (meth)acrylic resin having a lactone ring structure, and a (meth)acrylic resin having a glutaric anhydride structure or a glutarimide structure. The (meth)acrylic resin having a ring structure is preferred because it has high heat resistance, high moist heat resistance, high transparency, and high mechanical strength when biaxially stretched. Examples of (meth)acrylic resins having a ring structure such as a lactone ring structure include those described in JP-A Nos. 2000-230016, 2001-151814, 2002-120326, 2002-254544, and 2005-146084. Examples of (meth)acrylic resins having a glutaric anhydride structure or a glutarimide structure include those described in JP-A-6-256537, JP-A-6-11615, and JP-A-2009-203348.
[0055] The (meth)acrylic resin having a lactone ring structure is preferably represented by the following general formula: <1> The ring structure is represented by the following formula:
[0056] [ka] (In the formula, R 1 , R 2 and R 3 each independently represents a hydrogen atom or an organic residue having 1 to 20 carbon atoms. The organic residue may contain an oxygen atom.
[0057] General formula in the structure of (meth)acrylic resin having a lactone ring structure <1> The content of the lactone ring structure represented by the general formula in the structure of the (meth)acrylic resin having a lactone ring structure is preferably 5 to 90 mass %, more preferably 10 to 70 mass %, further preferably 10 to 60 mass %, and particularly preferably 10 to 50 mass %. <1> If the content of the lactone ring structure represented by the general formula in the structure of the (meth)acrylic resin having a lactone ring structure is less than 5 mass %, the heat resistance, solvent resistance, and surface hardness may be insufficient. <1> If the content of the lactone ring structure represented by the formula (I) is more than 90% by mass, the molding processability may be poor. The content of the lactone ring structure in the (meth)acrylic resin having the lactone ring structure can be determined by gas chromatography and dynamic TG measurement, for example, as described in JP-A-2006-171464.
[0058] The (meth)acrylic resin having a lactone ring structure is represented by the general formula: <1> The lactone ring structure may have a structure other than the lactone ring structure represented by the general formula: <1> The structure other than the lactone ring structure represented by the following general formula (I) is not particularly limited, but a method for producing a (meth)acrylic resin having a lactone ring structure includes the steps of: <2> A polymer structural unit (repeating structural unit) formed by polymerizing at least one monomer selected from the monomers represented by the following formula is preferred.
[0059] [ka]
[0060] In the formula, R 4 represents a hydrogen atom or a methyl group, and X represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group, a -OAc group, a -CN group, or a -CO-R 5 represents an acetyl group; 5 represents a hydrogen atom or an organic residue having 1 to 20 carbon atoms.
[0061] General formula in (meth)acrylic resin structure having lactone ring structure <1> The content ratio of structures other than the lactone ring structure represented by the formula (I) is preferably 10 to 95% by mass, more preferably 10 to 90% by mass, even more preferably 40 to 90% by mass, and particularly preferably 50 to 90% by mass in the case of a polymer structural unit (repeating structural unit) formed by polymerizing a (meth)acrylic acid ester, and is preferably 0 to 30% by mass, more preferably 0 to 20% by mass, even more preferably 0 to 15% by mass, and particularly preferably 0 to 10% by mass in the case of a polymer structural unit (repeating structural unit) formed by polymerizing a hydroxyl group-containing monomer. In the case of a polymer structural unit (repeating structural unit) formed by polymerizing an unsaturated carboxylic acid, it is preferably 0 to 30% by mass, more preferably 0 to 20% by mass, even more preferably 0 to 15% by mass, and particularly preferably 0 to 10% by mass. <2> In the case of a polymer structural unit (repeating structural unit) formed by polymerizing a monomer represented by the following formula:
[0062] The (meth)acrylic resin having a lactone ring structure has a weight average molecular weight of preferably 1000 to 2000000, more preferably 5000 to 1000000, still more preferably 10000 to 500000, and particularly preferably 50000 to 500000. If the weight average molecular weight is outside the above range, it is not preferable from the viewpoint of molding processability.
[0063] Examples of thermoplastic resins to be mixed with the (meth)acrylic resin having a lactone ring structure include olefin polymers such as polyethylene, polypropylene, ethylene-propylene copolymer, and poly(4-methyl-1-pentene); halogen-containing polymers such as vinyl chloride and chlorinated vinyl resin; acrylic polymers such as polymethyl methacrylate; styrene polymers such as polystyrene, styrene-methyl methacrylate copolymer, styrene-acrylonitrile copolymer, and acrylonitrile-butadiene-styrene block copolymer; polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyamides such as nylon 6, nylon 66, and nylon 610; polyacetal; polycarbonate; polyphenylene oxide; polyphenylene sulfide; polyether ether ketone; polysulfone; polyethersulfone; polyoxybenzylene; polyamide imide; rubbery polymers such as ABS resins and ASA resins blended with polybutadiene rubber and acrylic rubber; and the like.
[0064] The (meth)acrylic resin having a glutaric anhydride structure or a glutarimide structure is preferably represented by the above general formula <2> and the following general formula: <3> The ring structure is represented by the following formula:
[0065] [ka] (In the formula, R 1 and R 2 are each independently a hydrogen atom or an alkyl group having 1 to 8 carbon atoms; R 3 is hydrogen, an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or a substituent containing an aromatic ring having 5 to 15 carbon atoms.
[0066] The content of the glutarimide structure is preferably 20% by mass or more, more preferably 20% by mass to 95% by mass, further preferably 40% by mass to 90% by mass, and particularly preferably 50% by mass to 80% by mass, of the (meth)acrylic resin having a glutarimide structure.
[0067] When the content of the glutarimide unit is within the above range, the heat resistance and transparency of the obtained glutarimide-containing (meth)acrylic resin are not reduced, and the moldability and mechanical strength when processed into a film are not extremely reduced.
[0068] On the other hand, if the content of glutarimide units is less than the above range, the heat resistance of the resulting glutarimide resin tends to be insufficient and the transparency tends to be impaired, whereas if the content is more than the above range, the heat resistance and melt viscosity tend to be unnecessarily high, resulting in poor moldability, extremely low mechanical strength during film processing, and impaired transparency.
[0069] The weight-average molecular weight of the (meth)acrylic resin having the glutarimide structure is not particularly limited, but is preferably 10,000 to 500,000. If it is within the above range, the molding processability will not decrease, and the mechanical strength will not be insufficient when processed into a film. On the other hand, if the weight-average molecular weight is smaller than the above range, the mechanical strength when made into a film tends to be insufficient. Also, if it is larger than the above range, the viscosity during melt extrusion will be high, the molding processability will decrease, and the productivity of the molded product will tend to decrease.
[0070] In addition, the (meth)acrylic resin may be a mixture or copolymer of a (meth)acrylic acid ester and an imide compound, which is a thermoplastic resin. Examples of the imide compound include maleimide, and N-substituted maleimides such as N-methylmaleimide, N-ethylmaleimide, Nn-propylmaleimide, Ni-propylmaleimide, Nn-butylmaleimide, Ni-butylmaleimide, Ns-butylmaleimide, Nt-butylmaleimide, Nn-pentylmaleimide, Nn-hexylmaleimide, Nn-heptylmaleimide, Nn-octylmaleimide, N-laurylmaleimide, N-stearylmaleimide, N-cyclopropylmaleimide, N-cyclobutylmaleimide, N-cyclopentylmaleimide, N-cyclohexylmaleimide, N-cycloheptylmaleimide, and N-cyclooctylmaleimide. These maleimide compounds may be used alone or in combination of two or more.
[0071] The (meth)acrylic resin preferably contains acrylic rubber particles in terms of the impact resistance and film formability of the film. The amount of acrylic rubber particles that can be contained in the (meth)acrylic resin is preferably 5% by mass or more, more preferably 10% by mass or more, based on 100% by mass of the total amount of the (meth)acrylic resin and the acrylic rubber particles. The upper limit of the amount of the acrylic rubber particles is not critical, but if the amount of the acrylic rubber particles is too large, the surface hardness of the film decreases, and when the film is subjected to a surface treatment, the solvent resistance to the organic solvent in the surface treatment agent decreases. Therefore, the amount of the acrylic rubber particles that can be contained in the (meth)acrylic resin is preferably 80% by mass or less, more preferably 60% by mass or less.
[0072] The acrylic rubber particles are particles that contain an acrylic acid ester-based elastic polymer as an essential component, and may be a single-layer structure that is substantially made of this elastic polymer alone, or may be a multi-layer structure that has this elastic polymer as one layer.Specifically, as this elastic polymer, a crosslinked elastic copolymer obtained by polymerization of monomers consisting of 50-99.9 mass% alkyl acrylate, 0-49.9 mass% of at least one other vinyl monomer that can be copolymerized therewith, and 0.1-10 mass% of a copolymerizable crosslinkable monomer is preferably used.
[0073] Examples of alkyl acrylates include methyl acrylate, ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate, and the number of carbon atoms in the alkyl group is usually about 1 to 8. Examples of other vinyl monomers copolymerizable with the alkyl acrylates include compounds having one polymerizable carbon-carbon double bond in the molecule, more specifically, methacrylic acid esters such as methyl methacrylate, aromatic vinyl compounds such as styrene, and vinyl cyanide compounds such as acrylonitrile. Examples of the copolymerizable crosslinkable monomers include crosslinkable compounds having at least two polymerizable carbon-carbon double bonds in the molecule, more specifically, (meth)acrylates of polyhydric alcohols such as ethylene glycol di(meth)acrylate and butanediol di(meth)acrylate, alkenyl esters of (meth)acrylic acid such as allyl (meth)acrylate and methallyl (meth)acrylate, and divinylbenzene.
[0074] In addition to the acrylic rubber particles, the (meth)acrylic resin may contain ordinary additives such as ultraviolet absorbers, organic dyes, pigments, inorganic dyes, antioxidants, antistatic agents, surfactants, etc. Among these, ultraviolet absorbers are preferably used to improve weather resistance. Examples of ultraviolet absorbers include 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], 2-(5-methyl-2-hydroxyphenyl)-2H-benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-2H-benzotriazole, 2-(3-tert-butyl-5-methyl-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-tert-amyl-2-hydroxyphenyl)-2H-benzotriazole, Benzotriazole-based ultraviolet absorbers such as 2-(2'-hydroxy-5'-tert-octylphenyl)-2H-benzotriazole; 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octyloxybenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxy-4'-chlorobenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone; salicylic acid phenyl ester-based ultraviolet absorbers such as p-tert-butylphenyl salicylic acid ester and p-octylphenyl salicylic acid ester, and the like can be mentioned, and two or more of them may be used as necessary. When the (meth)acrylic resin contains an ultraviolet absorber, the amount thereof is usually 0.1% by mass or more, preferably 0.3% by mass or more, and preferably 2% by mass or less, based on 100% by mass of the total amount of the (meth)acrylic resin and the ultraviolet absorber.
[0075] As a method for obtaining a (meth)acrylic resin film, various generally known methods such as a method using a feed block and a method using a multi-manifold die can be used. Among them, a method of laminating via a feed block, performing multi-layer melt extrusion from a T-die, and contacting at least one side of the obtained laminated film-like material with a roll or belt to form a film is preferable in that a film with good surface properties can be obtained. In particular, from the viewpoint of improving the surface smoothness and surface gloss of the (meth)acrylic resin film, a method of contacting both sides of the laminated film-like material obtained by the above-mentioned multi-layer melt extrusion with a roll or belt surface to form a film is preferable. In the roll or belt used in this case, the roll surface or belt surface that comes into contact with the (meth)acrylic resin is preferably a mirror surface in order to impart smoothness to the (meth)acrylic resin film surface. The obtained film can be stretched to improve the film strength.
[0076] A film formed from a (meth)acrylic resin is unlikely to have a retardation in an unstretched state, but a retardation occurs when stretched, so that a retardation-reducing agent can be added to the (meth)acrylic resin to prevent the retardation from occurring even when stretched. Examples of the retardation-reducing agent include styrene-acrylonitrile copolymers. The retardation value can be controlled by the stretching ratio and the amount of the retardation-reducing agent added.
[0077] The thickness of the (meth)acrylic resin film is usually 1 μm or more and 80 μm or less, preferably 3 μm or more and 65 μm or less, more preferably 5 μm or more and 55 μm or less, even more preferably 7 μm or more and 45 μm or less, and particularly preferably 20 μm or more and 45 μm or less.
[0078] The glass transition temperature of the (meth)acrylic resin film is 100°C or higher, preferably 110°C or higher, more preferably 115°C or higher, and even more preferably 120°C or higher. The glass transition temperature is usually 170°C or lower. When the glass transition temperature of the (meth)acrylic resin film is 110°C or higher, the change in the molecular orientation of the (meth)acrylic resin in the (meth)acrylic resin film in a high-temperature environment is suppressed, and the change in the retardation value Re and the retardation value Rth in the thickness direction is suppressed, and light leakage in a high-temperature environment tends to be more effectively suppressed. The retardation value Re and the retardation value Rth in the thickness direction of the (meth)acrylic resin film are retardation values at a wavelength of 587 nm.
[0079] When the absolute value of the thickness direction retardation value Rth of the (meth)acrylic resin film is 15 nm or less, the (meth)acrylic resin film may serve both as an optical compensation film and a polarizer protective film in an IPS liquid crystal display device. The absolute value of the retardation value Rth in the thickness direction of the (meth)acrylic resin film is preferably 11 nm or less, more preferably 8 nm or less, and even more preferably 5 nm or less.
[0080] The (meth)acrylic resin film is preferably stored for 360 hours in an environment at a temperature of 85° C. and a relative humidity of 85% RH such that the absolute value of the change in thickness direction retardation value Rth is 10 nm or less. The thickness direction retardation value Rth is defined by the above formula (2). The absolute value of the change in the retardation value Rth in the thickness direction of the (meth)acrylic resin film is more preferably 7 nm or less, further preferably 5 nm or less, and particularly preferably 3 nm or less. When the absolute value of the change in the thickness direction retardation value Rth of the (meth)acrylic resin film is 10 nm or less, the change in the retardation value in a high-temperature environment is small, so that light leakage in a high-temperature environment tends to be more easily suppressed. Although the reason is not clear, it is presumed that such a (meth)acrylic resin film suppresses changes in the molecular orientation and molecular structure in the (meth)acrylic resin film due to moisture in the polarizing plate laminate in a high-temperature environment.
[0081] The thickness H1 of the polyester resin film and the thickness H2 of the (meth)acrylic resin film are preferably expressed by the following formula (i): H1 / H2>1.0 (i) When the thickness H1 of the polyester resin film and the thickness H2 of the (meth)acrylic resin film satisfy the above relationship, warping in a high-temperature environment tends to be easily suppressed. The ratio H1 / H2 of the thickness H1 of the polyester resin film to the thickness H2 of the (meth)acrylic resin film is preferably 1.2 or more, more preferably 1.5 or more, and even more preferably 2.0 or more, and is usually 200 or less, preferably 100 or less, more preferably 80 or less, even more preferably 50 or less, even more preferably 10 or less, and particularly preferably 6 or less.
[0082] <Polarizer> A polarizer is a film that has the function of selectively transmitting linearly polarized light in one direction from natural light. Examples of polarizers include iodine-based polarizers in which iodine as a dichroic pigment is adsorbed and oriented on a polyvinyl alcohol-based resin film, dye-based polarizers in which a dichroic dye as a dichroic pigment is adsorbed and oriented on a polyvinyl alcohol-based resin film, and coated polarizers in which a dichroic dye in a lyotropic liquid crystal state is coated, oriented, and fixed. These polarizers are called absorption-type polarizers because they selectively transmit linearly polarized light in one direction from natural light and absorb linearly polarized light in the other direction.
[0083] The polarizer is not limited to an absorptive polarizer, and may be a reflective polarizer that selectively transmits linearly polarized light in one direction from natural light and reflects linearly polarized light in the other direction, or a scattering polarizer that scatters linearly polarized light in the other direction. However, an absorptive polarizer is preferred because it provides excellent visibility when the polarizing plate is applied to a liquid crystal display device or the like. Among these, the polarizer is more preferably a polyvinyl alcohol-based polarizer made of a polyvinyl alcohol-based resin, even more preferably a polyvinyl alcohol-based polarizer in which a dichroic pigment such as iodine or a dichroic dye is adsorbed and oriented in a polyvinyl alcohol-based resin film, and particularly preferably a polyvinyl alcohol-based polarizer in which iodine is adsorbed and oriented in a polyvinyl alcohol-based resin film.
[0084] A polyvinyl alcohol-based polarizer in which a dichroic dye is adsorbed and oriented in a polyvinyl alcohol-based resin film can usually be produced through a dyeing step of dyeing a polyvinyl alcohol-based resin film (hereinafter, also abbreviated as "PVA-based film" or "film") with a dichroic dye, a crosslinking step of treating the PVA-based film after the dyeing step in a crosslinking bath containing a crosslinking agent, and a stretching step of uniaxially stretching the PVA-based film.
[0085] The method for producing a polarizer may further include other steps in addition to those described above, such as a swelling step for swelling the film before the dyeing step, a water washing step for washing the film surface after the crosslinking step, a drying step for drying the PVA-based film after the crosslinking step, an electromagnetic wave irradiation step for irradiating the film with electromagnetic waves after the crosslinking step, a complementary color step for adjusting the hue of the film after the crosslinking step, and a high-temperature, high-humidity step for treating the film after the crosslinking step with high temperature and humidity.
[0086] The stretching step, i.e., uniaxial stretching of the PVA-based film, may be carried out simultaneously with any of the other process steps listed above.
[0087] The various treatment steps included in the polarizer manufacturing method can be continuously carried out by continuously transporting the PVA-based film, which is the raw film, along the film transport path of the polarizer manufacturing device. The film transport path is equipped with equipment (treatment baths, furnaces, etc.) for carrying out the various treatment steps described above in the order in which they are carried out. The treatment bath refers to a bath that contains a treatment liquid for treating the PVA-based film, such as a swelling bath, dyeing bath, crosslinking bath, or washing bath.
[0088] The film transport path can be constructed by arranging guide rolls, nip rolls, etc. at appropriate positions in addition to the above-mentioned equipment. For example, guide rolls can be arranged before, after, or within each treatment bath, which allows the film to be introduced into and immersed in the treatment bath and drawn out from the treatment bath. More specifically, two or more guide rolls are provided in each treatment bath, and the film can be immersed in each treatment bath by transporting the film along these guide rolls.
[0089] Polyvinyl alcohol resins are obtained by saponifying polyvinyl acetate resins. Polyvinyl acetate resins include polyvinyl acetate, which is a homopolymer of vinyl acetate, as well as copolymers of vinyl acetate and other monomers that can be copolymerized with it. Examples of other monomers that can be copolymerized with vinyl acetate include unsaturated carboxylic acid compounds, olefin compounds, vinyl ether compounds, unsaturated sulfone compounds, and (meth)acrylamide compounds having an ammonium group.
[0090] The saponification degree of the polyvinyl alcohol resin is usually about 85 mol% or more and 100 mol% or less, preferably 99 mol% or more. The polyvinyl alcohol resin may be modified, and polyvinyl formal, polyvinyl acetal, etc. modified with aldehydes can also be used. The average polymerization degree of the polyvinyl alcohol resin is usually 1000 or more and 10000 or less, preferably 1500 or more and 5000 or less. The average polymerization degree of the PVA resin can be determined in accordance with JIS K 6726 (1994). If the average polymerization degree is less than 100, it is difficult to obtain a preferable polarizing performance, and if it exceeds 10000, the film processability may be poor.
[0091] The thickness of the PVA-based film as a raw film is, for example, about 10 μm or more and 100 μm or less, and from the viewpoint of thinning polarizers, polarizing plates, liquid crystal display devices, etc., it is preferably 60 μm or less, more preferably 50 μm or less, even more preferably 30 μm or less, and even more preferably 20 μm or less.
[0092] The PVA-based film, which is the raw film, can be prepared, for example, as a roll (wound product) of a long unstretched PVA-based film. In this case, the polarizer is also obtained as a long product. Each step of the polarizer manufacturing method will be described in detail below.
[0093] (Swelling process) The swelling treatment in the swelling step is a treatment that is carried out as necessary for the purpose of removing foreign matter from the PVA-based film, which is the raw film, removing plasticizers, imparting easy dyeing properties, plasticizing the film, etc. Specifically, it can be a treatment in which the PVA-based film is immersed in a swelling bath containing water. The PVA-based film may be immersed in one swelling bath, or may be immersed in two or more swelling baths sequentially. Before the swelling treatment, during the swelling treatment, or before and during the swelling treatment, the film may or may not be subjected to a uniaxial stretching treatment. The swelling bath may be water (for example, pure water) or an aqueous solution containing a water-soluble organic solvent such as an alcohol. The temperature of the swelling bath when the PVA-based film is immersed is usually about 10 to 70° C., preferably about 15 to 50° C., and the immersion time of the film is usually about 10 to 600 seconds, preferably about 20 to 300 seconds.
[0094] (dying process) The dyeing treatment in the dyeing step is a treatment performed for the purpose of adsorbing and orienting a dichroic dye on a PVA-based film, and specifically, it can be a treatment of immersing a PVA-based film in a dye bath containing a dichroic dye. The PVA-based film may be immersed in one dye bath, or may be immersed in two or more dye baths sequentially. In order to enhance the dyeability of the dichroic dye, the PVA-based film to be subjected to the dyeing step may be subjected to at least some degree of uniaxial stretching treatment. Instead of or in addition to the uniaxial stretching treatment before the dyeing treatment, a uniaxial stretching treatment may be performed during the dyeing treatment.
[0095] The dichroic dye can be iodine or a dichroic organic dye. Examples of the dichroic organic dye include Red BR, Red LR, Red R, Pink LB, Rubin BL, Bordeaux GS, Sky Blue LG, Lemon Yellow, Blue BR, Blue 2R, Navy RY, Green LG, Violet LB, Violet B, Black H, Black B, Black GSP, Yellow 3G, Yellow R, Orange LR, Orange 3R, Scarlet GL, Scarlet KGL, Congo Red, Brilliant Violet BK, Spra Blue G, Spra Blue GL, Spra Orange GL, Direct Sky Blue, Direct Fast Orange S, Fast Black, etc. The dichroic dye may be used alone or in combination of two or more kinds.
[0096] When iodine is used as the dichroic dye, an aqueous solution containing iodine and potassium iodide can be used in the dye bath. Instead of potassium iodide, other iodides such as zinc iodide may be used, or potassium iodide may be used in combination with other iodides. In addition, compounds other than iodides, such as boric acid, zinc chloride, cobalt chloride, etc., may be coexisted. When boric acid is added, it is distinguished from the crosslinking treatment described below in that it contains iodine. The content of iodine in the aqueous solution is usually about 0.003 to 1 part by mass per 100 parts by mass of water. In addition, the content of iodides such as potassium iodide is usually about 0.1 to 20 parts by mass per 100 parts by mass of water.
[0097] The temperature of the dye bath when the PVA-based film is immersed is usually about 10 to 45°C, preferably about 10 to 40°C, and more preferably about 20 to 35°C, and the immersion time of the film is usually about 30 to 600 seconds, and preferably about 60 to 300 seconds.
[0098] When a dichroic organic dye is used as the dichroic pigment, an aqueous solution containing the dichroic organic dye can be used in the dye bath. The content of the dichroic organic dye in the aqueous solution is usually 1×10 per 100 parts by mass of water. -4 ~10 parts by mass, preferably 1 × 10 -3 The dye bath may contain a dyeing assistant, for example, an inorganic salt such as sodium sulfate, a surfactant, etc. The dichroic organic dye may be used alone or in combination of two or more kinds. The temperature of the dye bath when the film is immersed is, for example, about 20 to 80°C, preferably about 30 to 70°C, and the immersion time of the film is usually about 20 to 600 seconds, preferably about 30 to 300 seconds.
[0099] (Crosslinking process) In the crosslinking step, the PVA-based film after the dyeing step is treated with a crosslinking agent. The crosslinking treatment is a treatment performed for the purpose of water resistance or hue adjustment by crosslinking, and specifically, it can be a treatment in which the film after the dyeing step is immersed in a crosslinking bath containing a crosslinking agent. The film may be immersed in one crosslinking bath, or may be immersed in two or more crosslinking baths in sequence. A uniaxial stretching treatment may be performed during the crosslinking treatment.
[0100] The crosslinking agent includes boric acid, and may further include other crosslinking agents such as glyoxal and glutaraldehyde. The content of boric acid in the crosslinking bath is usually about 0.1 to 15 parts by mass, preferably about 1 to 10 parts by mass, per 100 parts by mass of water. When the dichroic dye is iodine, the crosslinking bath preferably contains an iodide in addition to boric acid. The content of iodide in the crosslinking bath is usually about 0.1 to 20 parts by mass, preferably about 3 to 15 parts by mass, per 100 parts by mass of water. Examples of iodides include potassium iodide and zinc iodide. In addition, compounds other than iodides, such as zinc chloride, cobalt chloride, zirconium chloride, sodium thiosulfate, potassium sulfite, and sodium sulfate, may be present in the crosslinking bath. In the crosslinking step, when the PVA-based film is immersed in two or more crosslinking baths in sequence, the compositions and contents of the components contained in the crosslinking baths may be the same as each other, but are preferably different from each other.
[0101] From the viewpoint of obtaining a polarizer having higher optical properties, the temperature of the crosslinking bath when the PVA-based film is immersed is preferably 55.0° C. or higher, more preferably 58° C. or higher, and may be 58.5° C. or higher, and is usually 85.0° C. or lower, preferably 70.0° C. or lower, may be 65.0° C. or lower, may be 63.0° C. or lower, or may be 61.0° C. or lower. The immersion time for immersion in a crosslinking bath at this temperature is usually about 10 to 600 seconds, and preferably about 20 to 300 seconds.
[0102] When the PVA-based film is immersed in two or more crosslinking baths in sequence, the temperature and crosslinking time in at least one of the crosslinking baths may be within the above-mentioned range, and the temperature and crosslinking time in the other crosslinking baths may be within or outside the above-mentioned temperature and crosslinking time ranges. When the PVA-based film is immersed in two or more crosslinking baths in sequence, it is preferable to use a crosslinking bath with a temperature of 58.0°C or higher as the crosslinking bath to be immersed first. The temperature in the other crosslinking baths may be, for example, about 50 to 85°C, or about 50 to 70°C, and the immersion time of the film may be, for example, about 10 to 600 seconds, or about 20 to 300 seconds.
[0103] (Cleaning process) The cleaning treatment in the cleaning step is a treatment carried out as necessary for the purpose of removing excess crosslinking agent and chemicals such as dichroic dye attached to the PVA-based film, and is a treatment of cleaning the PVA-based film after the crosslinking step using a cleaning solution containing water. Specifically, it can be a treatment of immersing the PVA-based film after the crosslinking step in a cleaning bath (cleaning solution). The PVA-based film may be immersed in one cleaning bath, or may be immersed in two or more cleaning baths sequentially. Alternatively, the cleaning treatment may be a treatment of spraying the cleaning solution as a shower onto the PVA-based film after the crosslinking step, or the above-mentioned immersion and spraying may be combined.
[0104] The cleaning liquid may be water (e.g., pure water) or an aqueous solution containing a water-soluble organic solvent such as alcohols. The temperature of the cleaning liquid may be, for example, about 1 to 40° C., and the cleaning time may be, for example, about 1 to 60 seconds.
[0105] (drying process) The drying process is a drying treatment for promoting crosslinking of the PVA-based film while adjusting the moisture content of the PVA-based film. The drying treatment can be performed using a hot air dryer, an infrared heater, or a heated roll conveyor. The temperature of the drying treatment is usually about 30 to 110°C, and preferably 50 to 90°C. The time of the drying treatment is usually about 60 to 600 seconds, and preferably 120 to 600 seconds. The moisture content in the polarizer is adjusted by the drying treatment. The moisture content is usually about 5 to 20 mass% and preferably 8 to 15 mass% with respect to the total mass of the polarizer. When the moisture content is 5 mass% or more, the polarizer has sufficient flexibility, and therefore, damage after drying or breakage during conveyance can be suppressed. Furthermore, when the moisture content is 20 mass% or less, the polarizer has sufficient thermal stability. The drying treatment may be performed as necessary, and may not be performed.
[0106] (Stretching process) The stretching step is a step of stretching a PVA-based film, and the PVA-based film is preferably uniaxially stretched. As described above, the PVA-based film is uniaxially stretched in one or more stages of the processing steps provided in the polarizer manufacturing facility, such as the swelling step, dyeing step, crosslinking step, washing step, and drying step. The uniaxial stretching process may be either dry stretching in air or wet stretching in a bath, or both. The uniaxial stretching process may be inter-roll stretching, which involves longitudinal uniaxial stretching with a difference in peripheral speed between two nip rolls, hot roll stretching, tenter stretching, etc., but preferably includes inter-roll stretching. The total stretching ratio based on the raw film (when stretching is performed in two or more stages, the cumulative stretching ratio) is preferably 5.0 times or more, may be 5.5 times or more, may be 5.6 times or more, may be 5.8 times or more, may be 6.0 times or more, and is usually 8 times or less.
[0107] (Electromagnetic wave irradiation process) In order to improve the optical properties of the polarizing film, the PVA-based film may be subjected to an electromagnetic wave irradiation treatment (electromagnetic wave irradiation step) after being drawn out from the crosslinking step and passing through the nip rolls, before being immersed in a washing bath. The electromagnetic waves used in the electromagnetic wave irradiation step include infrared rays, and the proportion of the radiation energy of infrared rays having a wavelength of more than 2 μm and not more than 4 μm is preferably 25% or more, more preferably 28% or more, and even more preferably 35% or more of the total radiation energy of the electromagnetic waves. By irradiating the film with such electromagnetic waves, the optical properties of the obtained polarizing film can be improved. In addition, the upper limit of the proportion of the radiation energy of infrared rays having a wavelength of more than 2 μm and not more than 4 μm is not particularly limited, but is, for example, 80% or less. Usually, electromagnetic waves having a wavelength of 0.75 μm to 1000 μm are called infrared rays.
[0108] By carrying out a high humidity treatment step described later and carrying out an electromagnetic wave irradiation step before that, it is possible to further suppress the contraction force of the polarizer and further improve the optical properties. Although the mechanism by which the contraction force of the polarizer can be suppressed and the optical properties can be improved is not clear, it is speculated that the electromagnetic wave irradiation step excites the molecular motion in the film, which promotes the fixation of the dichroic dye such as iodine in the crosslinked film, and carrying out a high humidity treatment in this state contributes to suppressing the contraction force and improving the optical properties.
[0109] (High humidity processing process) The high humidity treatment refers to a treatment in which the film is exposed to a high humidity atmosphere. For example, the film may be exposed to a high humidity atmosphere by passing the film through a high humidity treatment section. By performing the high humidity treatment in which the film is exposed to a high humidity atmosphere, the optical properties of the film can be improved. The absolute humidity in the high humidity treatment section is set to 40 g / m from the viewpoint of suppressing the shrinkage force of the film. 3 More than 60g / m 3 More preferably, 80 g / cm 3 If the absolute humidity is too high, there is a concern that condensation may occur in the high-humidity processing section and that the film may be contaminated by condensed water. Therefore, the absolute humidity is preferably 550 g / m3 Less than 400 g / m 3 More preferably, 300 g / m or less 3 Less than 180 g / m 3 By suppressing the shrinkage force, a polarizing film with excellent durability can be obtained.
[0110] From the viewpoint of easily adjusting the absolute humidity to the above-mentioned preferred range and from the viewpoint of maintaining good transportability of the film, the atmospheric temperature in the high-humidity processing section is preferably 40° C. or higher, more preferably 55° C. or higher, and further preferably 60° C. or higher. The atmospheric temperature is preferably 100° C. or lower, and from the viewpoint of obtaining excellent optical properties, it is preferably 95° C. or lower. The film was placed in an absolute humidity of 80g / cm 3 The high humidity treatment in which the film is exposed to the high humidity atmosphere is preferably 5 seconds or more, more preferably 10 seconds or more. Although the time depends on the temperature, if the time is too long, there is a concern that the optical properties may deteriorate, so the time is preferably 60 minutes or less, more preferably 30 minutes or less, even more preferably 10 minutes or less, and particularly preferably 5 minutes or less.
[0111] The high humidity treatment step may be carried out, for example, immediately after the crosslinking step or the washing step, or after carrying out another step subsequent to the crosslinking step or the washing step. The other step may include a drying step.
[0112] The contraction force of the polarizer in the absorption axis direction is preferably less than 4.0 N / 2 mm. The contraction force of the polarizer in the absorption axis direction is more preferably 3.7 N / 2 mm or less, even more preferably 3.5 N / 2 mm or less, even more preferably 3.0 N / 2 mm or less, and particularly preferably 2.5 N / 2 mm or less. The contraction force of the polarizer in the absorption axis direction is usually 0.5 N / 2 mm or more. When the contraction force of the polarizer in the absorption axis direction is less than 4.0 N / 2 mm, the contraction of the polarizer in the absorption axis direction can be suppressed, and it is presumed that the stress on the (meth)acrylic resin film applied to the polarizing plate end at high temperatures can be reduced, and the associated change in the phase difference of the (meth)acrylic resin film can be suppressed, thereby suppressing light leakage at the polarizing plate end. The contraction force of the polarizer in the absorption axis direction can be obtained as desired by adjusting the amount of boron contained in the crosslinking bath when manufacturing the polarizer, the immersion time in the crosslinking liquid, the temperature of the crosslinking bath, the total stretch ratio based on the original film, and the like. The contraction force in the absorption axis direction of a polarizer can be measured by the following method: A measurement sample with a width of 2 mm and a length of 10 mm, with the absorption axis direction (MD, stretching direction) as the long side, is cut out from the polarizer, and this sample is set in an EXSTAR-6000 thermomechanical analyzer (TMA) manufactured by SII NanoTechnology, Inc., and the contraction force in the long side direction (absorption axis direction) that occurs when the sample is kept at 80°C for 4 hours while keeping the dimensions constant is measured.
[0113] The thickness of the polarizer can be 30 μm or less, and is preferably 25 μm or less (for example, 20 μm or less, further 15 μm or less, further 10 μm or less, and further 8 μm or less). The thickness of the polarizer is usually 2 μm or more. Reducing the thickness of the polarizer is advantageous for reducing the thickness of the polarizing plate, and further the liquid crystal panel and liquid crystal display device to which the polarizer is applied.
[0114] <Adhesive layer> The first adhesive layer for bonding the polarizer and the polyester resin film, and the second adhesive layer for bonding the polarizer and the (meth)acrylic resin film may each be formed from a known adhesive composition. The first adhesive layer and the second adhesive layer may be formed from the same adhesive composition, or may be formed from different adhesive compositions. The first adhesive layer and the second adhesive layer may each be formed from an aqueous adhesive composition, or may be formed from a curable adhesive composition that is cured by heating or irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays.
[0115] Examples of the aqueous adhesive composition include those in which a polyvinyl alcohol resin or a urethane resin is dissolved in water as the main component, and those in which a polyvinyl alcohol resin or a urethane resin is dispersed in water as the main component. The aqueous adhesive composition may further contain a curing component or a crosslinking agent such as a polyaldehyde, a melamine compound, a zirconia compound, a zinc compound, a glyoxal compound, or a water-soluble epoxy resin. Examples of the aqueous adhesive composition include the adhesive composition described in JP 2010-191389 A, the adhesive composition described in JP 2011-107686 A, the composition described in JP 2020-172088 A, and the composition described in JP 2005-208456 A.
[0116] The curable adhesive composition is preferably an active energy ray curable adhesive composition that contains a curable (polymerizable) compound as a main component and is cured by irradiation with active energy rays. Examples of the active energy ray curable adhesive composition include a cationic polymerization type adhesive composition that contains a cationic polymerizable compound as a curable compound, a radical polymerization type adhesive composition that contains a radical polymerizable compound as a curable compound, and a hybrid type adhesive composition that contains both a cationic polymerizable compound and a radical polymerizable compound as a curable compound.
[0117] The cationically polymerizable compound is a compound or oligomer that undergoes a cationic polymerization reaction and hardens when exposed to active energy rays such as ultraviolet light, visible light, electron beams, and X-rays, or when heated. Specific examples of the cationically polymerizable compound include epoxy compounds, oxetane compounds, and vinyl compounds. Examples of epoxy compounds include alicyclic epoxy compounds such as 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate (compounds having one or more epoxy groups bonded to an alicyclic ring in the molecule); aromatic epoxy compounds such as diglycidyl ether of bisphenol A (compounds having an aromatic ring and an epoxy group in the molecule); and aliphatic epoxy compounds such as 2-ethylhexyl glycidyl ether and 1,4-butanediol diglycidyl ether (compounds having at least one oxirane ring bonded to an aliphatic carbon atom in the molecule). Examples of the oxetane compound include compounds having one or more oxetane rings in the molecule, such as 3-ethyl-3-{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane.
[0118] The cationic polymerization adhesive composition preferably contains a cationic polymerization initiator. The cationic polymerization initiator may be a thermal cationic polymerization initiator or a photo-induced cationic polymerization initiator. Examples of the cationic polymerization initiator include aromatic diazonium salts such as benzenediazonium hexafluoroantimonate; aromatic iodonium salts such as diphenyliodonium tetrakis(pentafluorophenyl)borate; aromatic sulfonium salts such as triphenylsulfonium hexafluorophosphate; and iron-arene complexes such as xylene-cyclopentadienyl iron(II) hexafluoroantimonate. The content of the cationic polymerization initiator is usually 0.1 to 10 parts by mass relative to 100 parts by mass of the cationic polymerizable compound. Two or more kinds of cationic polymerization initiators may be included.
[0119] Examples of cationic polymerization adhesive compositions include the cationic polymerizable compositions described in JP 2016-126345 A and JP 2021-113969 A.
[0120] The radical polymerizable compound is a compound or oligomer that undergoes a radical polymerization reaction and hardens when exposed to active energy rays such as ultraviolet light, visible light, electron beams, and X-rays or when heated, and specifically includes a compound having an ethylenically unsaturated bond. Examples of the compound having an ethylenically unsaturated bond include a (meth)acrylic compound having one or more (meth)acryloyl groups in the molecule, and a vinyl compound having one or more vinyl groups in the molecule.
[0121] Examples of the (meth)acrylic compound include (meth)acrylate monomers having at least one (meth)acryloyloxy group in the molecule, (meth)acrylamide monomers, and (meth)acryl group-containing compounds obtained by reacting two or more functional group-containing compounds and having at least two (meth)acryloyl groups in the molecule, such as (meth)acrylic oligomers.
[0122] The (meth)acrylic oligomer is preferably a (meth)acrylate oligomer having at least two (meth)acryloyloxy groups in the molecule. The (meth)acrylic compounds may be used alone or in combination of two or more.
[0123] Examples of the (meth)acrylate monomer include a monofunctional (meth)acrylate monomer having one (meth)acryloyloxy group in the molecule, a bifunctional (meth)acrylate monomer having two (meth)acryloyloxy groups in the molecule, and a polyfunctional (meth)acrylate monomer having three or more (meth)acryloyloxy groups in the molecule.
[0124] An example of a monofunctional (meth)acrylate monomer is an alkyl (meth)acrylate. In the alkyl (meth)acrylate, the alkyl group may be linear or branched as long as it has 3 or more carbon atoms. Specific examples of alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. In addition, aralkyl (meth)acrylates such as benzyl (meth)acrylate; (meth)acrylates of terpene alcohols such as isobornyl (meth)acrylate; (meth)acrylates having a tetrahydrofurfuryl structure such as tetrahydrofurfuryl (meth)acrylate; (meth)acrylates having a cycloalkyl group at the alkyl group moiety such as cyclohexyl (meth)acrylate, cyclohexylmethyl methacrylate, dicyclopentanyl acrylate, dicyclopentenyl (meth)acrylate, and 1,4-cyclohexanedimethanol monoacrylate; aminoalkyl (meth)acrylates such as N,N-dimethylaminoethyl (meth)acrylate; and (meth)acrylates having an ether bond at the alkyl group moiety such as 2-phenoxyethyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, and phenoxypolyethylene glycol (meth)acrylate can also be used as monofunctional (meth)acrylate monomers.
[0125] Furthermore, monofunctional (meth)acrylates having a hydroxyl group at the alkyl moiety and monofunctional (meth)acrylates having a carboxyl group at the alkyl moiety can also be used. Specific examples of monofunctional (meth)acrylates having a hydroxyl group at the alkyl moiety include 2-hydroxyethyl (meth)acrylate, 2- or 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, trimethylolpropane mono(meth)acrylate, and pentaerythritol mono(meth)acrylate. Specific examples of monofunctional (meth)acrylates having a carboxyl group in the alkyl portion include 2-carboxyethyl (meth)acrylate, ω-carboxy-polycaprolactone (n≈2) mono(meth)acrylate, 1-[2-(meth)acryloyloxyethyl]phthalic acid, 1-[2-(meth)acryloyloxyethyl]hexahydrophthalic acid, 1-[2-(meth)acryloyloxyethyl]succinic acid, 4-[2-(meth)acryloyloxyethyl]trimellitic acid, and N-(meth)acryloyloxy-N',N'-dicarboxymethyl-p-phenylenediamine.
[0126] Examples of the bifunctional (meth)acrylate monomer include alkylene glycol di(meth)acrylate, polyoxyalkylene glycol di(meth)acrylate, halogen-substituted alkylene glycol di(meth)acrylate, di(meth)acrylate of an aliphatic polyol, di(meth)acrylate of hydrogenated dicyclopentadiene or tricyclodecane dialkanol, di(meth)acrylate of dioxane glycol or dioxane dialkanol, di(meth)acrylate of an alkylene oxide adduct of bisphenol A or bisphenol F, and epoxy di(meth)acrylate of bisphenol A or bisphenol F.
[0127] More specific examples of the bifunctional (meth)acrylate monomer include ethylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol di(meth)acrylate, ditrimethylolpropane di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, silicone ... Di(meth)acrylate of hydroxypivalic acid neopentyl glycol ester, 2,2-bis[4-(meth)acryloyloxyethoxyethoxyphenyl]propane, 2,2-bis[4-(meth)acryloyloxyethoxyethoxycyclohexyl]propane, hydrogenated dicyclopentadienyl di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, 1,3-dioxane-2,5-diyl di (Meth)acrylate [also known as dioxane glycol di(meth)acrylate], di(meth)acrylate of an acetal compound of hydroxypivalaldehyde and trimethylolpropane [chemical name: 2-(2-hydroxy-1,1-dimethylethyl)-5-ethyl-5-hydroxymethyl-1,3-dioxane], tris(hydroxyethyl)isocyanurate di(meth)acrylate, 1,4-cyclohexanedimethanol diacrylate, etc.
[0128] Examples of the polyfunctional (meth)acrylate monomer having three or more functional groups include glycerin tri(meth)acrylate, alkoxylated glycerin tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta ... Representative examples include poly(meth)acrylates of trifunctional or higher aliphatic polyols such as taerythritol hexa(meth)acrylate, and other examples include poly(meth)acrylates of trifunctional or higher halogen-substituted polyols, tri(meth)acrylates of alkylene oxide adducts of glycerin, tri(meth)acrylates of alkylene oxide adducts of trimethylolpropane, 1,1,1-tris[(meth)acryloyloxyethoxyethoxy]propane, and tris(hydroxyethyl)isocyanurate tri(meth)acrylate.
[0129] The (meth)acrylamide monomer is preferably a (meth)acrylamide having a substituent at the N-position (hereinafter also referred to as N-substituted (meth)acrylamide), and a typical example of the substituent at the N-position is an alkyl group, but it may form a ring together with the nitrogen atom of the (meth)acrylamide, and this ring may have an oxygen atom as a ring member in addition to the carbon atom and the nitrogen atom of the (meth)acrylamide. Furthermore, a substituent such as an alkyl or oxo (=O) may be bonded to the carbon atom constituting the ring.
[0130] Specific examples of N-substituted (meth)acrylamides include N-alkyl (meth)acrylamides such as N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, Nn-butyl (meth)acrylamide, Nt-butyl (meth)acrylamide, and N-hexyl (meth)acrylamide; and N,N-dialkyl (meth)acrylamides such as N,N-dimethyl (meth)acrylamide and N,N-diethyl (meth)acrylamide. The N-substituent may be an alkyl group having a hydroxyl group, and examples thereof include N-hydroxymethyl (meth)acrylamide, N-(2-hydroxyethyl) (meth)acrylamide, and N-(2-hydroxypropyl) (meth)acrylamide. Furthermore, specific examples of the N-substituted (meth)acrylamides forming the above-mentioned 5- or 6-membered ring include N-acryloylpyrrolidine, 3-acryloyl-2-oxazolidinone, 4-acryloylmorpholine, N-acryloylpiperidine, and N-methacryloylpiperidine.
[0131] On the other hand, the (meth)acrylic oligomer includes urethane (meth)acrylic oligomer, polyester (meth)acrylic oligomer, epoxy (meth)acrylic oligomer, and the like.
[0132] The urethane (meth)acrylic oligomer is a compound having a urethane bond (-NHCOO-) and at least two (meth)acryloyl groups in the molecule. Specifically, it may be a urethane reaction product between a hydroxyl group-containing (meth)acrylic monomer having at least one (meth)acryloyl group and at least one hydroxyl group in the molecule and a polyisocyanate, or a urethane reaction product between a terminal isocyanato group-containing urethane compound obtained by reacting a polyol with a polyisocyanate and a (meth)acrylic monomer having at least one (meth)acryloyl group and at least one hydroxyl group in the molecule.
[0133] The hydroxyl group-containing (meth)acrylic monomer used in the urethane reaction can be, for example, a hydroxyl group-containing (meth)acrylate monomer, specific examples of which include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, glycerin di(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate. Specific examples of monomers other than the hydroxyl group-containing (meth)acrylate monomer include N-hydroxyalkyl (meth)acrylamide monomers such as N-hydroxyethyl (meth)acrylamide and N-methylol (meth)acrylamide.
[0134] Examples of polyisocyanates to be subjected to the urethanization reaction with the hydroxyl group-containing (meth)acrylic monomer include hexamethylene diisocyanate, lysine diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, tolylene diisocyanate, xylylene diisocyanate, diisocyanates obtained by hydrogenating aromatic isocyanates among these diisocyanates (e.g., hydrogenated tolylene diisocyanate, hydrogenated xylylene diisocyanate, etc.), di- or tri-isocyanates such as triphenylmethane triisocyanate and dibenzylbenzene triisocyanate, and polyisocyanates obtained by polymerizing the above diisocyanates.
[0135] In addition, examples of polyols that can be used to produce a urethane compound containing a terminal isocyanato group by reaction with a polyisocyanate include aromatic, aliphatic, and alicyclic polyols, as well as polyester polyols, polyether polyols, etc. Examples of aliphatic and alicyclic polyols include 1,4-butanediol, 1,6-hexanediol, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, neopentyl glycol, trimethylolethane, trimethylolpropane, ditrimethylolpropane, pentaerythritol, dipentaerythritol, dimethylolheptane, dimethylolpropionic acid, dimethylolbutanoic acid, glycerin, and hydrogenated bisphenol A.
[0136] The polyester polyol is obtained by a dehydration condensation reaction between the above-mentioned polyol and a polybasic carboxylic acid or an anhydride thereof. Examples of the polybasic carboxylic acid or anhydride thereof, which are expressed by adding "(anhydride)" to the anhydride, include (anhydride) succinic acid, adipic acid, (anhydride) maleic acid, (anhydride) itaconic acid, (anhydride) trimellitic acid, (anhydride) pyromellitic acid, (anhydride) phthalic acid, (anhydride) isophthalic acid, terephthalic acid, and hexahydro(anhydride)phthalic acid.
[0137] The polyether polyol may be a polyalkylene glycol, or a polyoxyalkylene-modified polyol obtained by reacting the above-mentioned polyol or dihydroxybenzenes with an alkylene oxide.
[0138] The polyester (meth)acrylic oligomer is a compound having an ester bond and at least two (meth)acryloyl groups (typically (meth)acryloyloxy groups) in the molecule. Specifically, it can be obtained by a dehydration condensation reaction using (meth)acrylic acid, a polybasic carboxylic acid or its anhydride, and a polyol. Examples of the polybasic carboxylic acid or its anhydride used in the dehydration condensation reaction, which are expressed by adding "(anhydride)" to the anhydride that may be used, include (anhydride) succinic acid, adipic acid, (anhydride) maleic acid, (anhydride) itaconic acid, (anhydride) trimellitic acid, (anhydride) pyromellitic acid, hexahydrophthalic (anhydride), (anhydride) phthalic acid, isophthalic acid, terephthalic acid, etc. Examples of polyols used in the dehydration condensation reaction include 1,4-butanediol, 1,6-hexanediol, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, neopentyl glycol, trimethylolethane, trimethylolpropane, ditrimethylolpropane, pentaerythritol, dipentaerythritol, dimethylolheptane, dimethylolpropionic acid, dimethylolbutanoic acid, glycerin, and hydrogenated bisphenol A.
[0139] The epoxy (meth)acrylic oligomer can be obtained, for example, by an addition reaction between a polyglycidyl ether and (meth)acrylic acid, and has at least two (meth)acryloyloxy groups in the molecule. Examples of the polyglycidyl ether used in the addition reaction include ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, and bisphenol A diglycidyl ether.
[0140] The radical polymerization adhesive composition preferably contains a nitrogen-containing (meth)acrylic compound from the viewpoints of suppressing discoloration of the polarizer in a high-temperature and high-humidity environment and improving adhesion to the PVA-based resin film. Examples of the nitrogen-containing (meth)acrylic compound include N-substituted (meth)acrylamides. Among these, N,N-dimethylacrylamide and acryloylmorpholine are preferred.
[0141] The radical polymerization adhesive composition may be active energy ray curable or heat curable, but is preferably active energy ray curable. When active energy ray curability is imparted to a radical polymerization adhesive composition containing a radical polymerizable compound, it is preferable to blend a photoradical polymerization initiator into the adhesive. The photoradical polymerization initiator initiates a polymerization reaction of a radical polymerizable compound by irradiation with active energy rays such as visible light, ultraviolet light, X-rays, or electron beams. The photoradical polymerization initiator may be used alone or in combination of two or more kinds.
[0142] Specific examples of photoradical polymerization initiators include acetophenone-based initiators such as acetophenone, 3-methylacetophenone, benzyl dimethyl ketal, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 2-methyl-1-[4-(methylthio)phenyl-2-morpholinopropan-1-one, and 2-hydroxy-2-methyl-1-phenylpropan-1-one; benzophenone-based initiators such as benzophenone, 4-chlorobenzophenone, and 4,4'-diaminobenzophenone; benzoin ether-based initiators such as benzoin propyl ether and benzoin ethyl ether; thioxanthone-based initiators such as 4-isopropylthioxanthone; and others, including xanthone, fluorenone, camphorquinone, benzaldehyde, and anthraquinone.
[0143] The amount of the photoradical polymerization initiator is usually 0.5 to 20 parts by mass, preferably 1 to 6 parts by mass, based on 100 parts by mass of the radical polymerizable compound. By adding 0.5 parts by mass or more of the photoradical polymerization initiator, the radical polymerizable compound can be sufficiently cured, and the obtained polarizing plate can be given high mechanical strength and adhesive strength. On the other hand, if the amount is too large, the durability of the polarizing plate may decrease.
[0144] Examples of radical polymerization adhesive compositions include the radical polymerizable compositions described in JP 2016-126345 A, JP 2016-153474 A, and WO 2017 / 183335 A.
[0145] The active energy ray-curable adhesive composition may contain additives such as an ion trapping agent, an antioxidant, a chain transfer agent, a tackifier, a thermoplastic resin, a filler, a flow adjuster, a plasticizer, an antifoaming agent, an antistatic agent, a leveling agent, and a solvent, as necessary.
[0146] The polarizer and the polyester-based resin film can be bonded to each other by applying an adhesive composition to at least one of the bonding surfaces selected from the bonding surface of the polarizer and the bonding surface of the polyester-based resin film, laminating the two films with the coating layer of the adhesive composition therebetween, pressing the films together from above and below using a laminating roll or the like, and then drying the adhesive layer, curing it by irradiating it with active energy rays, or curing it by heating. To form a coating layer of the adhesive composition, various coating methods can be used, such as a die coater, a comma coater, a gravure coater, a wire bar coater, or a doctor blade coater. Alternatively, the adhesive composition may be allowed to flow while continuously supplying the polarizer and the polyester resin film so that the bonding surfaces of both are on the inner side.
[0147] Before forming the coating layer of the adhesive layer, at least one of the bonding surfaces selected from the bonding surface of the polarizer and the bonding surface of the polyester-based resin film may be subjected to an adhesion-improving treatment such as a saponification treatment, a corona treatment, a plasma treatment, a primer treatment, or an anchor coating treatment.
[0148] The lamination of the polarizer and the acrylic resin film can be carried out in the same manner as the lamination of the polarizer and the polyester resin film.
[0149] The light irradiation intensity when irradiating with active energy rays is determined depending on the composition of the active energy ray-curable adhesive composition and is not particularly limited, but is preferably 10 mW / cm 2 More than 1,000mW / cm 2 The irradiation intensity is preferably an intensity in a wavelength region effective for activating a photocationic polymerization initiator or a photoradical polymerization initiator. Irradiation is performed once or multiple times with such a light irradiation intensity, and the integrated light amount is 10 mJ / cm or less. 2 More preferably, it is 100 mJ / cm or more. 2 More than 1,000mJ / cm 2 It is more preferable to set it as follows:
[0150] The light source used to polymerize and cure the active energy ray-curable adhesive composition is not particularly limited, but examples include low pressure mercury lamps, medium pressure mercury lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, xenon lamps, halogen lamps, chemical lamps, black light lamps, microwave excited mercury lamps, and metal halide lamps.
[0151] When the first adhesive layer and the second adhesive layer are formed from an aqueous adhesive composition, the thickness of the first adhesive layer and the second adhesive layer may be, for example, 5 μm or less, preferably 1 μm or less, and more preferably 0.5 μm or less, and may be 0.01 μm or more, and preferably 0.05 μm or more. When the first adhesive layer and the second adhesive layer are formed from a curable adhesive composition (preferably an active energy ray-curable adhesive composition), the thickness of the first adhesive layer and the second adhesive layer may be, for example, 15 μm or less, preferably 10 μm or less, and more preferably 5 μm or less, and may be 0.1 μm or more, preferably 0.3 μm or more, and more preferably 0.5 μm or more.
[0152] The first adhesive layer and the second adhesive layer may be adhesive layers formed from the same type of adhesive composition, or may be adhesive layers formed from different types of adhesive compositions. The first adhesive layer and the second adhesive layer are preferably formed from the same type of adhesive composition. The first adhesive layer and the second adhesive layer may have the same thickness or different thicknesses, but it is preferable that they have the same thickness. Note that "the same thickness" includes an error of about 0.3 μm.
[0153] The first adhesive layer and the second adhesive layer can each be formed from a cationic polymerization type adhesive composition.
[0154] When the first adhesive layer is a layer of a cured product of a radical polymerization type adhesive composition, discoloration of the polarizer in a high-temperature and high-humidity environment tends to be suppressed.
[0155] <Other configuration requirements> The polarizing plate of the present invention may further include an optically functional film to impart a desired optical function, such as a retardation film, a light collecting plate, a brightness enhancing film, a light diffusion layer (light diffusion film), etc. The optically functional film is attached to the polarizing plate via an adhesive layer or a pressure-sensitive adhesive layer. The adhesive layer and pressure-sensitive adhesive layer may be the same as the adhesive layer described above and the pressure-sensitive adhesive layer described below, respectively.
[0156] <Light diffusing layer> The light diffusion layer may be a layer based on a light-transmitting resin in which light-transmitting fine particles are dispersed, as disclosed, for example, in JP-A No. 2012-048223 and JP-A No. 2012-212120, etc. When the polarizing plate includes a light diffusion layer, rainbow unevenness visible from an oblique direction of the polarizing plate tends to be suppressed, and good brightness tends to be easily obtained in an oblique direction.
[0157] The light-transmitting resin is not particularly limited as long as it has light-transmitting properties, and examples thereof include ionizing radiation-curable resins such as ultraviolet-curable resins and electron beam-curable resins, cured products of heat-curable resins, thermoplastic resins, and cured products of metal alkoxides. When an ionizing radiation-curable resin, a heat-curable resin, or a metal alkoxide is used, the resin is cured by irradiation with ionizing radiation or heating to form a light-transmitting resin. Among these, ionizing radiation-curable resins are preferred because they have high hardness and can provide high scratch resistance when used as a polarizer protective film to be provided on the surface of a liquid crystal display device.
[0158] Examples of ionizing radiation curable resins include polyfunctional acrylates such as acrylic acid or methacrylic acid esters of polyhydric alcohols, polyfunctional urethane acrylates such as those synthesized from diisocyanates, polyhydric alcohols, and hydroxy esters of acrylic acid or methacrylic acid, etc. In addition to these, polyether resins, polyester resins, epoxy resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiolpolyene resins, etc. having acrylate functional groups can also be used.
[0159] Examples of the thermosetting resin include a thermosetting urethane resin made of an acrylic polyol and an isocyanate prepolymer, as well as a phenol resin, a urea melamine resin, an epoxy resin, an unsaturated polyester resin, and a silicone resin.
[0160] Examples of thermoplastic resins include cellulose derivatives such as acetyl cellulose, nitrocellulose, acetyl butyl cellulose, ethyl cellulose, and methyl cellulose; vinyl resins such as vinyl acetate and its copolymers, vinyl chloride and its copolymers, and vinylidene chloride and its copolymers; acetal resins such as polyvinyl formal and polyvinyl butyral; acrylic resins such as acrylic resins and their copolymers, and methacrylic resins and their copolymers; polystyrene resins; polyamide resins; polyester resins; and polycarbonate resins.
[0161] As the metal alkoxide, a silicon oxide matrix using a silicon alkoxide-based material as a raw material can be used, for example, tetramethoxysilane, tetraethoxysilane, etc., which can be made into an inorganic or organic-inorganic composite matrix (translucent resin) by hydrolysis or dehydration condensation.
[0162] As the light-transmitting fine particles, organic or inorganic fine particles having light-transmitting properties can be used. For example, organic fine particles made of acrylic resin, melamine resin, polyethylene, polystyrene, organic silicone resin, acrylic-styrene copolymer, etc., and inorganic fine particles made of calcium carbonate, silica, aluminum oxide, barium carbonate, barium sulfate, titanium oxide, glass, etc. can be used. In addition, balloons of organic polymers and hollow glass beads can also be used. The light-transmitting fine particles may be composed of one type of fine particles, or may contain two or more types of fine particles. The shape of the light-transmitting fine particles may be any of spherical, flat, plate-like, needle-like, and irregular shapes, but spherical or approximately spherical shapes are preferred.
[0163] The filling rate of the light-transmitting fine particles is preferably 40% or more, and more preferably 50% or more.
[0164] The weight-average particle diameter of the light-transmitting fine particles is preferably 0.5 μm or more and 15 μm or less, more preferably 3 μm or more and 9 μm or less. If the weight-average particle diameter of the light-transmitting fine particles is less than 0.5 μm, the light-transmitting fine particles may not sufficiently scatter visible light in the wavelength range of 380 nm to 800 nm. If the weight-average particle diameter exceeds 15 μm, the thickness of the entire light diffusion layer may become thick, which may hinder the thinning of polarizing plates and displays. The weight-average particle diameter of the light-transmitting fine particles is measured using a Coulter Multisizer (manufactured by Beckman Coulter, Inc.) using the Coulter principle (pore electrical resistance method).
[0165] The refractive index of the light-transmitting fine particles is preferably larger than that of the light-transmitting resin, and the difference is preferably in the range of 0.04 to 0.15. By making the difference in refractive index between the light-transmitting fine particles and the light-transmitting resin within the above range, appropriate internal scattering occurs due to the difference in refractive index between the light-transmitting fine particles and the light-transmitting resin, and a light diffusion function can be imparted.
[0166] The light diffusion layer may be a layer formed from a light-diffusing adhesive composition (hereinafter also referred to as a light-diffusing adhesive composition) in which spherical fine particles are blended with an acrylic resin. In this case, the refractive index difference between the acrylic resin and the spherical fine particles is in the range of more than 0.01 and less than 0.09. The refractive index difference is preferably more than 0.01 and 0.07 or less, more preferably more than 0.01 and 0.04 or less. If the refractive index difference between the two is 0.01 or less, the desired optical performance is not exhibited in the obtained adhesive layer, and as a result, it becomes close to a transparent adhesive. On the other hand, if the refractive index difference between the acrylic resin and the spherical fine particles becomes too large, the light diffusion property is strongly exhibited, which reduces the brightness when the liquid crystal display device is viewed from the front.
[0167] As long as the spherical particles satisfy the above conditions, they can be used alone or in combination of two or more kinds. When two or more kinds of spherical particles are mixed, they may be mixed with particles having different refractive indices, or particles having different particle diameters only.
[0168] The acrylic resin contained in the adhesive composition can be composed of an acrylic resin having a weight average molecular weight in the range of 1,000 to 2,000,000. Furthermore, the spherical fine particles are selected from those having an average particle size in the range of 0.5 to 15 μm, and are mixed in a ratio of 20 to 80 parts by mass per 100 parts by mass of the acrylic resin. By using such a specific combination, good adhesive performance and optical performance are achieved.
[0169] The light-diffusing pressure-sensitive adhesive composition may contain a crosslinking agent to form a good crosslinked structure when formed into a pressure-sensitive adhesive layer, and may also contain an ionic compound to impart antistatic properties.
[0170] The material of the spherical fine particles is not particularly limited, and known organic fine particles or inorganic fine particles can be used. Examples of organic fine particles include resin particles made of polyolefin resins such as polystyrene, polyethylene, and polypropylene, and (meth)acrylic resins such as polymethacrylate resins and polyacrylate resins, and may be crosslinked polymers. Furthermore, copolymer resins in which two or more monomers selected from ethylene, propylene, styrene, methyl methacrylate, benzoguanamine, formaldehyde, melamine, butadiene, etc. are copolymerized can also be used. Examples of inorganic fine particles include particles made of silica, silicone resin, titanium oxide, aluminum oxide, etc. Considering dispersibility in acrylic resins, coatability of the adhesive composition, and optical properties of the resulting adhesive layer, the fine particles are preferably made of silicone resin or polymethyl methacrylate resin.
[0171] The amount of spherical fine particles is 20 to 80 parts by mass per 100 parts by mass of the non-volatile content of the acrylic resin. If the amount is less than 20 parts by mass per 100 parts by mass of the acrylic resin, the desired optical properties, particularly haze, are not exhibited, whereas if the amount is more than 80 parts by mass, the adhesive properties are reduced, such as peeling due to reduced adhesive strength of the resulting adhesive layer.
[0172] The light diffusion layer may further include an anti-reflection layer on the viewing side when the polarizing plate is laminated on a liquid crystal display device. The anti-reflection layer is provided to reduce the reflectance as much as possible, and the formation of the anti-reflection layer can prevent reflection on the display screen. Examples of the anti-reflection layer include a low refractive index layer made of a material with a refractive index lower than that of the light diffusion layer.
[0173] The light diffusion layer preferably has a total haze of 20% or more and an internal haze of 20% or more. The "total haze" is calculated from the ratio of the total light transmittance (Tt), which indicates the total amount of light irradiated onto the light diffusion layer and transmitted therethrough, to the diffused light transmittance (Td), which is diffused and transmitted by the light diffusion layer, according to the following formula [1]: Total haze (%) = (Td / Tt) x 100 [1] It is calculated by:
[0174] Total light transmittance (Tt) is the sum of the parallel light transmittance (Tp) that is transmitted coaxially with the incident light, and the diffuse light transmittance (Td). Total light transmittance (Tt) and diffuse light transmittance (Td) are values measured in accordance with JIS K 7361.
[0175] Moreover, the "internal haze" of the light diffusion layer refers to the total haze other than the haze (surface haze) caused by the surface shape of the light diffusion layer.
[0176] If the total haze and / or internal haze is less than 20%, the light scattering is insufficient, and it is difficult to obtain sufficient wide viewing angle performance. If the total haze and / or internal haze is more than 90%, the light scattering becomes strong, and when a polarizing plate having a light diffusion layer is applied to a liquid crystal display device, the front contrast may decrease. If the total haze and / or internal haze is more than 90%, the transparency of the light diffusion layer tends to be impaired. The total haze and / or internal haze are each preferably 25% or more, more preferably 30% or more, and even more preferably 35% or more. Also, it is preferably 85% or less, more preferably 80% or less, and even more preferably 75% or less.
[0177] The light diffusion layer is preferably disposed on the polarizing plate on the side opposite to the first adhesive layer of the polyester resin film via a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer that can be used for lamination may be a pressure-sensitive adhesive layer having light diffusion properties formed from a light-diffusing pressure-sensitive adhesive composition, or may be a pressure-sensitive adhesive layer having no light diffusion properties. When a pressure-sensitive adhesive layer having light diffusion properties is used, both the pressure-sensitive adhesive layer having light diffusion properties and the layer (film) having a translucent resin as a base material are regarded as a light diffusion layer. Furthermore, as the light diffusion layer, only a pressure-sensitive adhesive layer having light diffusing properties may be used.
[0178] The polarizing plate 2 shown in FIG. 6 includes a light diffusing layer 5, a polyester resin film 10, a first adhesive layer 15, a polarizer 30, a second adhesive layer 25, and a (meth)acrylic resin film 20 in this order. 6, in the polarizing plate of the present invention, the polyester resin film 10 and the first adhesive layer 15 are preferably in direct contact with each other. Also, the (meth)acrylic resin film 20 and the second adhesive layer 25 are preferably in direct contact with each other. The polarizer 30 and the first adhesive layer 15 are preferably in direct contact with each other. The polarizer 30 and the second adhesive layer 25 are preferably in direct contact with each other. Although not shown, an adhesive layer or pressure-sensitive adhesive layer may be disposed between the light diffusion layer 5 and the polyester resin film 10.
[0179] <Polarizing plate with adhesive layer> The present invention also relates to a polarizing plate with an adhesive layer, comprising the above polarizing plate and an adhesive layer. The polarizing plate with an adhesive layer can be applied to, for example, a liquid crystal display device. In the liquid crystal display device, the polarizing plate with an adhesive layer is disposed on the viewing side and / or the back side of a liquid crystal cell, which is an image display element.
[0180] An example of the layer structure of the polarizing plate with a pressure-sensitive adhesive layer of the present invention is shown in Fig. 7. The polarizing plate with a pressure-sensitive adhesive layer 3 shown in Fig. 7 includes a polarizing plate including a polyester resin film 10, a first adhesive layer 15, a polarizer 30, a second adhesive layer 25, and a (meth)acrylic resin film 20, in this order, and a pressure-sensitive adhesive layer 40. As in the polarizing plate 3 with a pressure-sensitive adhesive layer shown in FIG. 7, the pressure-sensitive adhesive layer 40 is preferably laminated on the surface of the (meth)acrylic resin film 20 opposite to the polarizer 30.
[0181] The polarizing plate with the pressure-sensitive adhesive layer can be attached to a liquid crystal cell via the pressure-sensitive adhesive layer 40. That is, from the viewpoint of visibility, in a liquid crystal panel and a liquid crystal display device, the polarizing plate of the present invention is preferably disposed such that the (meth)acrylic resin film 20 side faces the liquid crystal cell.
[0182] The adhesive layer 40 may be laminated on either the polyester resin film 10 (or the light diffusion layer) or the (meth)acrylic resin film 20, but is preferably laminated on the (meth)acrylic resin film 20 as described above. When the adhesive layer 40 is laminated on the (meth)acrylic resin film, the polyester resin film 10 (or the light diffusion layer) is disposed on the opposite side (e.g., the viewing side) to the image display element. When an optically functional film is laminated on the opposite side of the (meth)acrylic resin film to the side of the polarizer 30, the adhesive layer 40 may be further laminated on the optically functional film on the opposite side to the (meth)acrylic resin film 20.
[0183] Examples of the pressure-sensitive adhesive composition forming the pressure-sensitive adhesive layer include pressure-sensitive adhesive compositions containing, as a base polymer, a (meth)acrylic resin, a silicone resin, a polyester resin, a polyurethane resin, a polyether resin, etc. Among these, from the viewpoints of transparency, adhesive strength, reliability, heat resistance, reworkability, etc., a (meth)acrylic pressure-sensitive adhesive composition containing a (meth)acrylic resin is preferred.
[0184] The thickness of the pressure-sensitive adhesive layer is determined depending on the adhesive strength etc., and is, for example, from 1 μm to 50 μm, preferably from 2 μm to 40 μm, and more preferably from 3 μm to 30 μm.
[0185] In a polarizing plate with an adhesive layer, when the total film thickness of the polarizing plate with an adhesive layer is y (the length of y shown in Figure 7) and the distance from the surface of the polyester resin film opposite the polarizer to the center of the film thickness of the polarizer is z (the length of z shown in Figure 7), it is preferable that the following formula (ii) is satisfied. y / 2-z<10 (ii) When y and z satisfy the relationship of formula (ii), the polarizing plate tends to suppress deformation (warping) of the liquid crystal cell to which the polarizing plate is attached in a heat-resistant environment. The reason why warping is suppressed by formula (ii) is not clear, but it is thought that warping due to shrinkage of the polarizer in a heat-resistant environment can be suppressed by positioning the polarizer close to the liquid crystal cell surface in the overall film thickness of the polarizing plate.
[0186] The value of the left side of formula (ii) is preferably 5 or less, more preferably 0 or less, further preferably -5 or less, and particularly preferably -10 or less. Also, it is usually -50 or more, and preferably -30 or more.
[0187] <Optical laminate> Another embodiment of the present invention includes an optical laminate in which the pressure-sensitive adhesive layer of the above-mentioned pressure-sensitive adhesive layer-attached polarizing plate and a substrate are laminated. Here, the substrate may be a glass substrate of a liquid crystal cell, etc. Also, a transparent electrode may be provided on the surface of the glass substrate of the liquid crystal cell. The thickness of the substrate is usually 300 μm or more and 1000 μm or less, preferably 300 μm or more and 800 μm or less, and more preferably 300 μm or more and 700 μm or less.
[0188] It is preferable that the optical laminate of the present invention satisfies the following formula (iii), when the thickness of the entire pressure-sensitive adhesive layer-attached polarizing plate is y (the length indicated by y in Figure 8), the distance from the surface of the resin film opposite the polarizer to the center of the polarizer is z (the length indicated by z in Figure 8), and the thickness of the substrate is t (the length indicated by t in Figure 8). y / 2-(z+t)<-290 (iii) When the above relational expression is satisfied, the polarizing plate tends to suppress deformation (warping) of the liquid crystal cell to which the polarizing plate is attached in a heat-resistant environment. Although the reason why the warping is suppressed by the expression (iii) is not clear, it is considered that the warping caused by the shrinkage of the polarizer in a heat-resistant environment can be suppressed by the position of the polarizer in the entire film thickness of the polarizing plate being close to the liquid crystal cell surface and the increase in substrate rigidity due to the increase in the thickness of the substrate.
[0189] The value of the left side of formula (iii) is preferably −300 or less, usually −1050 or more, and preferably −1000 or more.
[0190] FIG. 8 shows a schematic cross-sectional view of one example of the layer structure of the optical laminate of the present invention. The optical laminate 4 shown in Figure 8 has a layer structure in which a polyester resin film 10, a first adhesive layer 15, a polarizer 30, a second adhesive layer 25, a (meth)acrylic resin film layer 20, a pressure-sensitive adhesive layer 40, and a substrate 60 are laminated in this order.
[0191] On the opposite side of the substrate of the optical laminate shown in FIG. 8, the polarizing plate with a pressure-sensitive adhesive layer of the present invention may be disposed, or another polarizing plate with a pressure-sensitive adhesive layer may be disposed.
[0192] The optical laminate of the present invention can be suitably used in liquid crystal display devices, such as various mobile devices such as tablet terminals, personal computers including notebook computers, desktop computers, and PDAs (Personal Digital Assistants), televisions, and in-vehicle displays. EXAMPLES
[0193] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.
[0194] (Production Example 1: Production of Polarizer 1) A long polyvinyl alcohol (PVA) raw film having a thickness of 60 μm [average polymerization degree 2400, saponification degree 99.9 mol% or more] was continuously conveyed while being unwound from a roll, and was immersed in a swelling bath of pure water at 30 ° C. for a residence time of 89 seconds (swelling step). After that, the film pulled out from the swelling bath was immersed in a dyeing bath at 30 ° C. containing iodine with potassium iodide / boric acid / water at a ratio of 2 / 0.3 / 100 (mass ratio) for a residence time of 156 seconds (dyeing step). Next, the film pulled out from the dyeing bath was immersed in a first crosslinking bath at 56 ° C. with potassium iodide / boric acid / water at a ratio of 12 / 4 / 100 (mass ratio) for a residence time of 67 seconds, and then in a second crosslinking bath at 40 ° C. with potassium iodide / boric acid / water at a ratio of 9 / 3 / 100 (mass ratio) for a residence time of 11 seconds (crosslinking step). In the dyeing and crosslinking steps, the film was uniaxially stretched in the longitudinal direction by stretching between rolls in a bath. The total stretching ratio based on the original film was 5.69 times.
[0195] Next, it was removed from the second crosslinking bath and heated in an electromagnetic wave irradiator (medium-wavelength infrared heater (MW heater), product name: Golden 8 Medium-wave twin tube emitter, manufactured by Heraeus, heat source temperature 900°C, maximum energy density 60kW / m 2 ) was used to irradiate the film with electromagnetic waves, with the electromagnetic wave radiating port located 5 cm away from the film surface. The amount of heat irradiated by the electromagnetic waves per unit volume of the film was 290 J / cm 3 The amount of heat radiated by electromagnetic waves per unit volume of the film was calculated by the following formula. (Amount of heat irradiated by electromagnetic waves per unit volume of film) = {(maximum energy density) x (surface area of heater heating part) / (area irradiated with electromagnetic waves)} x (time of irradiating with electromagnetic waves) ÷ (film thickness) After being pulled out of the second crosslinking bath, the time required for the film to be transported to the irradiation position of the electromagnetic wave applicator and to be irradiated with electromagnetic waves was 5 seconds.
[0196] The film irradiated with electromagnetic waves was immersed in a cleaning bath of pure water at 5°C for a residence time of 3 seconds (cleaning step). Thereafter, in a high-humidity processing section, the film was immersed in a cleaning bath of pure water at 75°C and an absolute humidity of 147g / m 3The film was exposed to a high humidity environment with a residence time of 60 seconds at a relative humidity of 61%. At the same time, the film was uniaxially stretched to a magnification of 1.14. Finally, the film was placed in a drying oven at a temperature of 30°C and an absolute humidity of 10 g / cm. 3 The film was dried for a residence time of 120 seconds in a drying step, thereby obtaining a polarizer 1. The obtained polarizer 1 had a thickness of 23 μm.
[0197] (Production Example 2: Production of Polarizer 2) Polarizer 2 was obtained in the same manner as in Production Example 1, except that the electromagnetic wave irradiation step and the high humidity treatment step were not performed in the polarizer production of Production Example 1, the high humidity treatment step was not performed, and the temperature in the drying step was set to 80° C. The thickness of the obtained polarizer 2 was 23 μm.
[0198] (Production Example 3: Production of Polarizer 3) A long polyvinyl alcohol (PVA) resin film having a thickness of 45 μm [saponification degree 99.9 mol% or more] as a raw film was continuously conveyed while being unwound from a roll, and was immersed in a swelling bath of pure water at a temperature of 30 ° C for a residence time of 81 seconds (swelling step). After that, the film pulled out from the swelling bath was immersed in a dyeing bath containing iodine at a temperature of 30 ° C and having a potassium iodide / water ratio of 2 / 100 (mass ratio) for a residence time of 143 seconds (dyeing step). Next, the film pulled out from the dyeing bath was immersed in a crosslinking bath at a temperature of 58.5 ° C and having a potassium iodide / boric acid / water ratio of 12 / 3.8 / 100 (mass ratio) for a residence time of 67 seconds, and then in a crosslinking bath at a temperature of 40 ° C and having a potassium iodide / boric acid / water ratio of 9 / 2.4 / 100 (mass ratio) for a residence time of 11 seconds (crosslinking step). In the dyeing and crosslinking steps, the film was uniaxially stretched longitudinally by roll-to-roll stretching in a bath. The cumulative stretch ratio up to the crosslinking step was 5.74 times based on the original film. Next, the film was taken out of the crosslinking bath and immersed in a washing bath of pure water at 4°C for a residence time of 3 seconds (washing step), and then introduced into a humidity-controllable heating furnace for a high-temperature, high-humidity treatment with a residence time of 161 seconds (high-temperature, high-humidity step), to obtain a polarizing film. The temperature and absolute humidity in the heating furnace were 80.0°C and 88.0 g / m, respectively. 3The absolute humidity in the heating furnace was calculated from the measured temperature and relative humidity in the furnace. As a result of further longitudinal uniaxial stretching by introduction into the heating furnace (high temperature and high humidity treatment), the total stretching ratio based on the original film of the polarizer was 5.83 times. The thickness of the obtained polarizer 3 was 19 μm.
[0199] (Production Example 4: Production of Polarizer 4) A long polyvinyl alcohol film (average polymerization degree: about 2400, saponification degree: 99.9 mol% or more, thickness: 60 μm) was continuously conveyed and immersed in a swelling bath of pure water at 20 ° C. for a residence time of 31 seconds (swelling step). Thereafter, the film pulled out of the swelling bath was immersed in a dyeing bath at 30 ° C. containing iodine with potassium iodide / water at 2 / 100 (mass ratio) for a residence time of 122 seconds (dyeing step). Next, the film pulled out of the dyeing bath was immersed in a crosslinking bath at 52 ° C. with potassium iodide / boric acid / water at 12 / 4.1 / 100 (mass ratio) for a residence time of 70 seconds, and then in a crosslinking bath at 40 ° C. with potassium iodide / boric acid / water at 9 / 2.9 / 100 (mass ratio) for a residence time of 13 seconds (crosslinking step). In the dyeing and crosslinking steps, the film was uniaxially stretched longitudinally by inter-roll stretching in the bath. The total stretch ratio based on the original film was 4.5 times. Next, the film was pulled out of the crosslinking bath and immersed in a washing bath of pure water at 5°C for a residence time of 3 seconds (washing step), and then introduced into a drying furnace at 80°C for a residence time of 190 seconds and dried (drying step) to obtain polarizer 4. The thickness of polarizer 4 obtained as described above was 23 μm.
[0200] (Production Example 5: Production of Polarizer 5) Except for not performing the electromagnetic wave irradiation step, a polarizer 5 was obtained in the same manner as in Production Example 1. The thickness of the obtained polarizer 5 was 23 μm.
[0201] (Production Example 6: Production of polyethylene terephthalate resin (1)) While the esterification reactor was heated to 200°C, 86.4 parts of terephthalic acid and 64.6 parts of ethylene glycol were charged into the esterification reactor to obtain a mixture. While stirring the mixture, 0.017 parts of antimony trioxide, 0.064 parts of magnesium acetate tetrahydrate, and 0.16 parts of triethylamine were added as catalysts to the mixture. The gauge pressure in the esterification reactor was set to 0.34 MPa, and a pressurized esterification reaction was carried out under conditions of 240°C. The esterification reactor was then returned to normal pressure, and 0.014 parts of phosphoric acid were added. The temperature was then raised to 260°C over 15 minutes, and 0.012 parts of trimethyl phosphate were added to obtain a mixture. After 15 minutes, the mixture was dispersed using a high-pressure disperser, and after another 15 minutes, the esterification reaction product was transferred to a polycondensation reactor and subjected to a polycondensation reaction under reduced pressure at 280°C. After the polycondensation reaction was completed, the mixture was filtered using a Naslon filter with a 95% cutoff diameter of 5 μm, extruded from a nozzle in the form of a strand, cooled and solidified using cooling water that had been previously filtered (pore diameter: 1 μm or less), and cut into pellets to obtain polyethylene terephthalate resin (hereinafter referred to as PET (1)).
[0202] (Production Example 7: Production of polyethylene terephthalate resin (2)) 10 parts of the dried ultraviolet absorber (2,2'-(1,4-phenylene)bis(4H-3,1-benzoxazin-4-one) and 90 parts of the PET (1) obtained in Production Example 6 were mixed and kneaded using an extruder to obtain a polyethylene terephthalate resin (2) containing an ultraviolet absorber (hereinafter referred to as PET (2)).
[0203] (Production Example 8: Preparation of Coating Solution for Forming Adhesive Layer) A water-dispersible sulfonate metal salt group-containing copolymer polyester resin was prepared by carrying out an ester exchange reaction and a polycondensation reaction in a conventional manner between a dicarboxylic acid component consisting of 46 mol % terephthalic acid, 46 mol % isophthalic acid, and 8 mol % sodium 5-sulfonatoisophthalate, and a glycol component consisting of 50 mol % ethylene glycol and 50 mol % neopentyl glycol. Next, 51.4 parts of water, 38 parts of isopropyl alcohol, 5 parts of n-butyl cellosolve, and 0.06 parts of nonionic surfactant were mixed to obtain a mixture. The mixture obtained was heated to 77°C and stirred, while adding 5 parts of the above-mentioned water-dispersible sulfonate metal salt group-containing copolymer polyester resin, and continued to stir until no resin lumps remained, to obtain a resin water dispersion. The obtained resin water dispersion was cooled to 25°C to obtain a uniform water-dispersible copolymer polyester resin solution with a solid content concentration of 5.0% by mass. 3 parts of aggregated silica particles were dispersed in 50 parts of water to obtain an aqueous dispersion of aggregated silica particles. 0.54 parts of the aqueous dispersion of aggregated silica particles was added to 99.46 parts of the water-dispersible copolymerized polyester resin liquid, and 20 parts of water was further added while stirring to obtain a coating liquid for forming an easy-adhesion layer.
[0204] (Production Example 9: Production of Protective Film 1) PET (3) was prepared by mixing 90 parts of PET (1) produced in Production Example 6 and 10 parts of PET (2) produced in Production Example 7, and was dried under reduced pressure at 135 ° C for 6 hours, and then fed to extruder 2 (for intermediate layer B). PET (1) was also dried and fed to extruder 1 (for outer layer A and outer layer C). PET (1) fed to extruder 1 and PET (3) fed to extruder 2 were each melted at 285 ° C. These two types of polymers were each filtered with a stainless steel sintered filter medium (nominal filtration accuracy 10 μm particles 95% cut) and laminated in a two-type three-layer merging block, extruded from a die in the form of a sheet, and then wrapped around a casting drum with a surface temperature of 30 ° C. using an electrostatic casting method, cooled and solidified, and an unstretched PET film was produced. At this time, the discharge amount of each extruder was adjusted so that the thickness ratio of A layer, B layer, and C layer was 10:80:10. Next, both sides of the obtained unstretched PET film were coated with 0.08 g / m2 of PET using the reverse roll method. 2 After the coating liquid for forming the easy-adhesion layer was applied so as to become The unstretched PET film on which this coating layer was formed was stretched 4.0 times in the width direction in a hot air zone at a temperature of 125°C in a tenter stretching machine while holding the ends of the film with clips. Next, while maintaining the width stretched in the width direction, it was treated at a temperature of 225°C for 10 seconds, and further subjected to a relaxation treatment of 3.0% in the width direction to obtain a uniaxially stretched PET film on which an easy-adhesion layer with a film thickness of about 80 μm was formed. This was named protective film 1.
[0205] (Production Example 10: Production of Protective Film 2) A mixture of 90 parts of a (meth)acrylic resin having a lactone ring structure and 10 parts of an acrylonitrile-styrene (AS) resin (lactone ring content: 28.5%) was extruded and stretched 2.0 times in length and 2.4 times in width to obtain a 40 μm thick acrylic resin film, which was designated as protective film 2.
[0206] <Example 1> One side of each of the protective films 1 and 2 was subjected to a corona treatment, and an epoxy adhesive composition was applied to the corona-treated surface using an adhesive applicator. The polarizer 1 obtained in the above-mentioned Production Example 1 was then superimposed on the coated layer surface, and then pressed and laminated using a lamination roll to obtain a polarizing plate precursor. At this time, the protective film 1 (polyester resin film) was laminated so that the stretching direction (width direction) and the absorption axis direction (stretching direction of the polarizer) were perpendicular to each other. A belt conveyor-equipped ultraviolet irradiation device (the lamp was a metal halide lamp manufactured by Eye Graphics Co., Ltd.) was used to irradiate the polarizing plate precursor with an integrated light amount of 200 mJ / cm from the protective film 2 ((meth)acrylic resin film) side. 2 The adhesive was cured by irradiating it with ultraviolet light so that the wavelength was (UVB) to obtain a polarizing plate having a layer structure of protective film 1 (polyester resin film) / adhesive layer / polarizer 1 / adhesive layer / protective film 2 ((meth)acrylic resin film).
[0207] Next, a release film-attached adhesive layer having a (meth)acrylic adhesive layer (thickness 20 μm) on the release-treated surface of a release film was prepared. The release film-attached adhesive layer was laminated on the protective film 2 ((meth)acrylic resin film) side of the polarizing plate after corona treatment of the surface of the protective film 2 ((meth)acrylic resin film), to obtain a polarizing plate with an adhesive layer. The polarizing plate with an adhesive layer has a structure of protective film 1 (polyester resin film) / adhesive layer / polarizer 1 / adhesive layer / protective film 2 ((meth)acrylic resin film) / adhesive layer / release film.
[0208] <Example 2> A polarizing plate and a polarizing plate with a pressure-sensitive adhesive layer were obtained in the same manner as in Example 1, except that Polarizer 2 was used instead of Polarizer 1.
[0209] <Example 3> A polarizing plate and a polarizing plate with a pressure-sensitive adhesive layer were obtained in the same manner as in Example 1, except that Polarizer 3 was used instead of Polarizer 1.
[0210] <Comparative Example 1> A polarizing plate and a polarizing plate with a pressure-sensitive adhesive layer were obtained in the same manner as in Example 1, except that Polarizer 4 was used instead of Polarizer 1.
[0211] <Comparative Example 2> A polarizing plate and a polarizing plate with a pressure-sensitive adhesive layer were obtained in the same manner as in Example 1, except that Polarizer 5 was used instead of Polarizer 1.
[0212] <Comparative Example 3> A polarizing plate and a polarizing plate with an adhesive layer were obtained in the same manner as in Example 1, except that a biaxially stretched polyethylene terephthalate (PET) protective film (manufactured by Mitsubishi Chemical Corporation) made of a polyester-based resin with a thickness of 38 μm was used instead of protective film 1. Note that, like in Example 1, this polarizing plate was bonded so that the stretching direction (width direction) of the biaxially stretched polyethylene terephthalate protective film and the absorption axis direction (stretching direction of the polarizer) were perpendicular to each other. The stretching direction (width direction) of the biaxially stretched polyethylene terephthalate protective film refers to the width direction when the film is unwound from the film roll. The retardation values Re1 to Re4 of the 38 μm-thick polyester-based resin film are as shown in Table 1.
[0213] (Measurement of Retardation Value of Polyester Resin Film) The retardation values Re1 to Re4 of the polyester resin films used in the examples and comparative examples were measured at a wavelength of 587 nm using a retardation measuring device (KOBRA-HB-RESPC, manufactured by Oji Scientific Instruments Co., Ltd.). The results are shown in Table 1. Re1: Retardation value measured in the first arrangement in which the polyester resin film is arranged so that the angle between the surface of the polyester resin film and the measurement direction is 90° Re2: Retardation value measured in a second arrangement in which the polyester-based resin film in the first arrangement is rotated 30° around its fast axis as the central axis, so that the angle between the surface of the polyester-based resin film and the measurement direction is 60°. Re3: A retardation value measured in a third arrangement in which the polyester resin film is rotated 30° around an axis that is at an angle of 45° to the fast axis in the plane of the polyester resin film, so that the angle between the plane of the polyester resin film and the measurement direction is 60°. Re4: Retardation value measured in a fourth arrangement in which the polyester-based resin film in the first arrangement is rotated 30° around its slow axis as the central axis, so that the angle between the surface of the polyester-based resin film and the measurement direction is 60°.
[0214] (Measurement of Retardation Value in Thickness Direction of Polyester Resin Film) The thickness direction retardation value Rth of the polyester resin film used in the examples and comparative examples was measured using a retardation measuring device (KOBRA-HB-RESPC, manufactured by Oji Scientific Instruments Co., Ltd.) at a wavelength of 587 nm, with the angle between the surface of the polyester resin film and the measurement direction being 60°. In addition, Re / Rth was calculated from the thickness direction retardation value Rth and the retardation value Re. The results are shown in Table 1.
[0215] (Measurement of the luminous efficiency corrected single transmittance Ty and luminous efficiency corrected polarization degree Py of the polarizing plate) After peeling off the release film from the polarizing plates with adhesive layer prepared in the Examples and Comparative Examples, the adhesive layer side was attached to a non-alkali glass substrate (thickness 0.7 mm, Corning "Eagle XG") to obtain a glass-attached polarizing plate laminate. The MD transmittance and TD transmittance of the glass-attached polarizing plate laminate were measured using a spectrophotometer with an integrating sphere (JASCO "V7100"). The wavelength of the incident light was measured from the glass side in the range of 380 to 780 nm. The formula: Single layer transmittance (%) = (MD + TD) / 2 Degree of polarization (%)={(MD-TD) / (MD+TD)}×100 Based on this, the single transmittance and the degree of polarization at each wavelength were calculated. "MD transmittance" is the transmittance when the direction of polarized light exiting the Glan-Thompson prism is parallel to the transmission axis of the polarizing film sample, and is represented as "MD" in the above formula. "TD transmittance" is the transmittance when the direction of polarized light exiting the Glan-Thompson prism is perpendicular to the transmission axis of the polarizing film sample, and is represented as "TD" in the above formula. The obtained single transmittance and degree of polarization were subjected to luminosity correction using a 2-degree visual field (C light source) according to JIS Z 8701:1999 "Method of displaying color - XYZ color system and X10Y10Z10 color system" to determine the luminosity-corrected single transmittance Ty and the luminosity-corrected degree of polarization Py.
[0216] (Measurement of rainbow unevenness) After peeling off the release film from the polarizing plate with the adhesive layer obtained in Example 1, the adhesive layer side was attached to a non-alkali glass substrate (thickness 0.7 mm, Corning "Eagle XG") to obtain a glass-attached polarizing plate laminate. The above-mentioned glass-bonded polarizing plate laminate was placed in a backlight light source so that the glass substrate side was the light source, and the polarizing plate was visually observed in a dark place in an oblique direction from the polyester resin film side of the polarizing plate to check the visibility of rainbow unevenness and evaluate it according to the following criteria. Moreover, rainbow unevenness was similarly evaluated for the polarizing plates with the pressure-sensitive adhesive layer obtained in Examples 2 and 3 and the polarizing plates with the pressure-sensitive adhesive layer obtained in Comparative Examples 1 to 3. The results are shown in Table 1. ○: Weak rainbow unevenness ×: Strong rainbow unevenness
[0217] (Brightness measurement) After peeling off the release film from the polarizing plate with the adhesive layer obtained in Example 1, the adhesive layer side was attached to one side of an alkali-free glass substrate (thickness 0.7 mm, Corning "Eagle XG"). Furthermore, in order to reproduce the display state of an actual liquid crystal display device, the polarizing plate with the adhesive layer 2 obtained in Example 1 was attached to a side of the glass substrate other than the polarizing plate attachment side so that the transmission axes of the two polarizing plates were parallel to each other across the glass substrate, thereby obtaining a glass-attached polarizing plate laminate. For Examples 2 to 3 and Comparative Examples 1 to 3, glass-attached optical laminates were obtained in the same manner.
[0218] The glass-attached polarizing plate laminate was placed in a backlight source, and visual observation was performed from the protective film side of the polarizing plate in a dark place to confirm the luminance, and evaluation was performed according to the following criteria. Moreover, the luminance was similarly evaluated for the polarizing plates with the pressure-sensitive adhesive layer obtained in Examples 2 and 3 and the polarizing plates with the pressure-sensitive adhesive layer obtained in Comparative Examples 1 to 3. The results are shown in Table 1. 〇: High brightness ×: Low brightness
[0219] (Light leakage measurement) A Toshiba REGZA 43-inch Z730X was prepared as a liquid crystal display device using a method of dividing a direct-type LED backlight into multiple regions to control the brightness. The polarizing plates on the panel viewing side and the backlight side of the prepared liquid crystal display device were peeled off. After peeling the release film from the polarizing plate with the adhesive layer prepared in Example 1, the polarizing plate was attached to a panel via the adhesive so that the absorption axis of the polarizer 1 was perpendicular to the panel viewing side and the backlight side, thereby preparing a liquid crystal display device. The produced liquid crystal display device was caused to display a white display against a black display background, and light leakage from the periphery of the white display was observed and evaluated in a dark place according to the following criteria. Moreover, the polarizing plates with the pressure-sensitive adhesive layer obtained in Examples 2 and 3 and the polarizing plates with the pressure-sensitive adhesive layer obtained in Comparative Examples 1 to 3 were similarly evaluated for light leakage. 〇: Weak light leakage ×: Strong light leakage
[0220] [Table 1] [Explanation of symbols]
[0221] 1, 2 polarizing plate, 3 polarizing plate with adhesive layer, 4 optical laminate, 5 light diffusion layer, 10 polyester resin film, 15 first adhesive layer, 20 (meth)acrylic resin film, 25 second adhesive layer, 30 polarizer, 40 adhesive layer, 60 substrate, 100 polyester resin film (first arrangement), 110 polyester resin film (second arrangement), 120 polyester resin film (third arrangement), 130 polyester resin film (fourth arrangement), 201 light source, 202 observation device, 210 measurement direction, 300, 310, 320 central axis, 400 fast axis of polyester resin film in first arrangement, 500 slow axis of polyester resin film in first arrangement.
Claims
1. A polarizing plate including, in this order, a polyester resin film, a first adhesive layer, a polarizer, a second adhesive layer, and an acrylic resin film, The polarizing plate has a visibility-corrected single transmittance of 43.0% or more, The polyester resin film is a polarizing plate in which the retardation value Re defined by the formula (1) satisfies the following [i] to [iv]. Re = (n x -n y ) × d (1) [In the formula, n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and d represents the thickness of the film. [i] The retardation value Re1 measured in a first arrangement in which the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 90° is 6000 nm or more. [ii] The polyester-based resin film in the first arrangement is rotated 30° about its fast axis as a central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this second arrangement, the phase difference value Re2 is 5000 nm or more. [iii] The polyester-based resin film in the first arrangement is rotated by 30° around an axis that is at an angle of 45° to the fast axis in the plane of the polyester-based resin film as a central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this third arrangement, the phase difference value Re3 measured is 6000 nm or more. [iv] The polyester-based resin film in the first arrangement is rotated by 30° about its slow axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this fourth arrangement, the retardation value Re4 is 7000 nm or more.
2. 2. The polarizing plate according to claim 1, wherein the polyester resin film has a thickness of 60 [mu]m or more.
3. 2. The polarizing plate according to claim 1, wherein the ratio of a retardation value Re1 to a retardation value Rth in the thickness direction of the polyester resin film defined by the formula (2) is 0.5 or more. Rth = [(n x +n y ) / 2-n z 〕×d (2) [In the formula, n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and n z represents the refractive index in the thickness direction of the film, and d represents the thickness of the film.
4. 2. The polarizing plate according to claim 1, wherein the polarizing plate has a luminosity-corrected polarization degree of 99.996% or more.
5. 2. The polarizing plate according to claim 1, wherein the polarizing plate has a luminosity-corrected single transmittance of 44.5% or less.
6. A polarizing plate with a pressure-sensitive adhesive layer, comprising the polarizing plate according to any one of claims 1 to 5 and a pressure-sensitive adhesive layer, A polarizing plate with a pressure-sensitive adhesive layer, wherein the pressure-sensitive adhesive layer is laminated on a surface of the (meth)acrylic resin film opposite to the polarizer.
7. A liquid crystal display comprising the pressure-sensitive adhesive layer-attached polarizing plate according to claim 6 .
Citation Information