Spectacle lense

The spectacle lens design uses aliphatic compounds and coated film layers to transmit UVA rays and reflect UVB rays, addressing the need for beneficial sunlight exposure while adhering to UVB blocking standards, achieving high UVA transmission and low UVB transmission.

JP2024143079AInactive Publication Date: 2024-10-11JINS HLDG INC

Patent Information

Application Number
JP2023055572
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing spectacle lenses either block all ultraviolet rays, preventing the beneficial effects of sunlight, or allow harmful UVB rays to pass through, failing to meet the contradictory needs of allowing UVA transmission while blocking UVB.

Method used

A spectacle lens design comprising a base material layer made from aliphatic compounds that transmit UVA rays and a coated film layer that reflects UVB rays, using materials like aliphatic polycarbonate and organosiloxane resin with inorganic oxide fine particles, and an antireflection film to achieve high UVA transmission and low UVB transmission.

Benefits of technology

The lens allows maximum UVA transmission while minimizing UVB transmission, mimicking natural light conditions and meeting JIS standards for refractive correction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143079000001_ABST
    Figure 2024143079000001_ABST
Patent Text Reader

Abstract

To provide a spectacle lense which can properly respond to two conflicting needs of a user for a state as close as possible to the state with naked eyes and natural light and for removing wavelengths of UBV regions.SOLUTION: The spectacle lense has a base material layer and a coat film layer. The total UVA average transmission of the base material layer and the coat film layer is higher than the UVA average transmission of the base material layer. The total UVB average transmission of the base material layer and the coat film layer is lower than the UVB average transmission of the base material layer.SELECTED DRAWING: Figure 11
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lens for spectacles. [Background technology]

[0002] Existing eyeglass lenses use materials that block ultraviolet rays (see, for example, Patent Document 1), and most lenses do not transmit ultraviolet rays (see, for example, Patent Document 2). On the other hand, it has been pointed out that sunlight has a positive effect on the physical and mental development of children in particular, and that if children are not exposed to sufficient sunlight, the risk of myopia progression increases (see, for example, Non-Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2009-209120 A [Patent Document 2] International Publication No. 2019 / 188447 [Non-patent literature]

[0004] [Non-Patent Document 1] Japan Ophthalmological Society and five other societies, “Cautionary opinion regarding the use of blue light blocking glasses in children,” April 14, 2021, [Retrieved January 27, 2022], Internet<https: / / www.gankaikai.or.jp / info / 20210414_bluelight.pdf> Summary of the Invention [Problem to be solved by the invention]

[0005] Here, for a user who wears eyeglasses, in order to allow natural light, including ultraviolet rays, to reach their eyes, they must remove their eyeglasses, and therefore cannot obtain the benefits of eyeglasses, such as vision correction.

[0006] In order to solve the above problems, it is conceivable to form the substrate of the eyeglass lens using a compound that transmits ultraviolet light, but in order to satisfy the durability requirements of eyeglass lenses, a coating film is generally applied to the substrate. In eyeglass lenses of such a general configuration, there is a new demand for transmitting ultraviolet light that was previously blocked, taking into consideration the overall characteristics of the substrate and the coating film, in order to allow as much natural light as possible to reach the eye.

[0007] Furthermore, ultraviolet rays include two types of ultraviolet rays: UVA with a long wavelength and UVB with a short wavelength. Regarding UVB, the JIS standard stipulates that the maximum transmittance of refractive correction eyeglass lenses in the solar ultraviolet B region must be 5% or less of the visual transmittance (T 7333:2018 (ISO 8980-3:2013)). Therefore, in order to configure eyeglass lenses that meet or approach the JIS standard, it is also necessary to focus on the UVB region and cut the wavelengths in the UVB region.

[0008] Therefore, an object of the present invention is to provide a spectacle lens that appropriately meets the conflicting needs of wanting to achieve an environment similar to that experienced when exposed to natural light with the naked eye, while at the same time cutting out wavelengths in the UVB region. [Means for solving the problem]

[0009] In one embodiment of the present invention, the eyeglass lens comprises a substrate layer and a coating film layer, and the total average UVA transmittance of the substrate layer and the coating film layer is higher than the average UVA transmittance of the substrate layer, and the total average UVB transmittance of the substrate layer and the coating film layer is lower than the average UVB transmittance of the substrate layer. Effect of the Invention

[0010] According to the present invention, it is possible to provide a lens for glasses that transmits as much UVA ultraviolet light as possible with long wavelengths and transmits as little UVB ultraviolet light as possible with short wavelengths. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a diagram showing the light transmittance of each eyeglass lens according to the prior art. [Diagram 2] FIG. 1 is a diagram showing an example of the total transmittance of each substrate layer based on substrate resin 1 and each AR coating. [Diagram 3] FIG. 1 is a diagram showing an example of the reflectance of test pieces 11 to 16. [Figure 4] FIG. 13 is a diagram showing an example of the total transmittance of each substrate layer based on substrate resin 2 and each AR coat. [Diagram 5] FIG. 1 is a diagram showing an example of the reflectance of test pieces 21 to 29. [Figure 6] FIG. 13 is a diagram showing an example of the transmittance of each base material layer to which an ultraviolet absorber (LA-46) and / or a radical scavenger (LA-52) is added, based on the base material resin 3. [Figure 7] FIG. 7 is a diagram showing an example of transmittance when a UVA visible light AR coating is formed on each of the base layers shown in FIG. 6. [Figure 8] FIG. 13 is a diagram showing comparative examples of the transmittance of a test piece 31 on which each AR coating is formed. [Figure 9] FIG. 13 is a diagram showing comparative examples of the reflectance of a test piece 31 on which each AR coating is formed. [Figure 10] FIG. 13 is a diagram showing comparative examples of the reflectance of a test piece 32 and a test piece 35 on which each AR coating is formed. [Figure 11] FIG. 13 is a diagram showing comparative examples of the reflectance of each test piece on which a UVA visible light AR coating is formed. [Figure 12A] FIG. 2 is a table comparing the transmittance of each substrate resin in each wavelength range. [Figure 12B] FIG. 2 is a table comparing the transmittance of each substrate resin in each wavelength range. [Figure 12C] FIG. 2 is a table comparing the transmittance of each substrate resin in each wavelength range. [Figure 12D] FIG. 2 is a table comparing the transmittance of each substrate resin in each wavelength range. [Figure 13A] FIG. 2 is a table comparing the solar ultraviolet ray transmittance in each wavelength range of each base resin. [Figure 13B] FIG. 2 is a table comparing the solar ultraviolet ray transmittance in each wavelength range of each base resin. [Figure 13C] FIG. 2 is a table comparing the solar ultraviolet ray transmittance in each wavelength range of each base resin. [Figure 13D] FIG. 2 is a table comparing the solar ultraviolet ray transmittance in each wavelength range of each base resin. [Figure 14A] FIG. 1 is a table comparing the luminous transmittance of each test specimen. [Figure 14B] FIG. 1 is a table comparing the luminous transmittance of each test specimen. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. However, the embodiments described below are merely examples, and there is no intention to exclude the application of various modifications and techniques not specified below. In other words, the present invention can be implemented with various modifications within the scope of the gist of the present invention. In addition, in the following description of the drawings, the same or similar parts are represented by the same or similar reference numerals. The drawings are schematic and do not necessarily correspond to actual dimensions, ratios, etc. The drawings may also include parts with different dimensional relationships and ratios.

[0013] [Embodiment] <Existing eyeglass lenses> Fig. 1 is a diagram showing the light transmittance of each spectacle lens according to the conventional technology (special eyeglass lenses according to the conventional technology are also collectively referred to as "existing lenses"). In the example shown in Fig. 1, the light transmittance is measured using the following four lenses. Lens A: A lens (refractive index 1.50) made of CR-39 (registered trademark) (allyl diglycol carbonate) manufactured by PPG Industries, Inc. Lens B: Thiourethane lens (refractive index 1.60) Lens C: Thiourethane lens (refractive index 1.67) Lens D: Thiourethane lens (refractive index 1.74)

[0014] Lenses A to D each have a hard coat and an anti-reflective coat formed on both sides of the substrate. As shown in Fig. 1, lenses A to D each cut off wavelengths shorter than 380 nm. This shows that lenses A to D each have at least one of the following: the substrate contains an ultraviolet absorbing agent, the hard coat contains an ultraviolet absorbing agent, and the anti-reflective coat contains an ultraviolet absorbing agent.

[0015] Therefore, in many existing lenses, not just those for vision correction, the wavelengths absorbed by the lens vary slightly depending on the lens manufacturer and material, but all lenses cut out wavelengths shorter than 380 nm.

[0016] In light of the effects of ultraviolet light on the eyes that have become evident in recent years, the inventors came up with the idea of ​​transmitting ultraviolet light through eyeglass lenses. However, as shown in Figure 1, most existing eyeglass lenses block ultraviolet light, and no lenses that meet the inventors' desire exist.

[0017] <Substrate of eyeglass lenses in the disclosed technology> First, the substrate of the eyeglass lens according to the embodiment of the present invention will be described. The eyeglass lens according to the embodiment does not use a substrate mainly made of a material that absorbs ultraviolet light. For example, aromatic compounds and aliphatic compounds having a conjugated structure are known as materials that absorb ultraviolet light, so substrates mainly made of these compounds do not need to be used as eyeglass lenses in the embodiment.

[0018] The eyeglass lens according to the embodiment includes a base layer mainly made of a first compound other than the compound that absorbs a predetermined percentage or more of ultraviolet light. The material that absorbs a predetermined percentage or more of ultraviolet light includes the aromatic compound described above, for example. The base layer may also contain the aromatic compound to the extent that it does not interfere with the purpose of the embodiment.

[0019] In this way, since the base layer is made of the first compound other than the compound that absorbs a certain percentage or more of ultraviolet light, it is possible to prevent the transmission of ultraviolet light from being significantly hindered by at least the base layer of the eyeglass lens. Therefore, ultraviolet light passes through the eyeglass lens, and light similar to natural light including ultraviolet light reaches the eye.

[0020] In the embodiment, the ultraviolet light has a wavelength in the wavelength range of, for example, 280 to 400 nm. Of these, 320 to 400 nm is called UVA (first wavelength range), and 280 to 320 nm is called UVB (second wavelength range). The boundary between UVA and UVB may be 315 nm, and the upper limit of UVA may be 380 nm. The eyeglass lens in the embodiment is configured to transmit wavelengths in the UVA range while cutting wavelengths in the UVB range.

[0021] The first compound used to form the base layer is, for example, a compound other than an aromatic compound, and may include at least one of an aliphatic polycarbonate, an aliphatic olefin polymer, an aliphatic acrylic resin, and an aliphatic nylon resin.

[0022] Substrates made of aliphatic polycarbonate include, for example, at least one of commercially available CR-39 (registered trademark) manufactured by PPG Corporation and DURABIO (registered trademark) manufactured by Mitsubishi Chemical Corporation. CR-39 (registered trademark) is a linear aliphatic polycarbonate without aromatic rings, and therefore has a low ultraviolet absorption function. DURABIO (registered trademark) is a partially biomaterial polycarbonate that uses isosorbide, which is a biomaterial. This compound is considered to have a low ultraviolet absorption function because the diol copolymerized with isosorbide is also alicyclic and does not have an aromatic ring.

[0023] The aliphatic olefin polymer includes, for example, at least one of a cycloolefin polymer (alicyclic olefin polymer) and an aliphatic olefin polymer having no cyclic structure, etc. The substrate formed using the cycloolefin polymer may include, for example, any one of commercially available APEL (registered trademark) manufactured by Mitsui Chemicals, Inc. (refractive index 1.544, Abbe number 56), ZEONEX (registered trademark) manufactured by Zeon Corporation (refractive index 1.509 to 1.535), and ARTON (registered trademark) manufactured by JSR Corporation (refractive index 1.513 to 1.516, Abbe number 56 or 57).

[0024] The substrate formed of an aliphatic olefin polymer having no cyclic structure may include, for example, TPX (registered trademark) (chemical compound name: polymethyltempene) (refractive index: 1.46) commercially available from Mitsui Chemicals.

[0025] An example of a substrate made of aliphatic acrylic resin that can be used is the "UV-transmitting PMMA lens" (refractive index: approx. 1.49, Abbe number: 55) manufactured by Nippon Tokushu Kogaku Jushi Co., Ltd. PMMA is an abbreviation for polymethyl methacrylate. UV-transmitting PMMA is an acrylic resin that transmits UV rays.

[0026] <Coating> The eyeglass lens may have a hard coat film layer (which may be written as "hard coat", "hard coat film", or "hard coat layer") formed on at least one surface of the substrate layer. The eyeglass lens in the embodiment may have a hard coat film layer formed of a material that does not contain an ultraviolet absorbent, coated on at least one surface of the substrate layer. The hard coat film layer is formed, for example, by uniformly applying a hard coat liquid to the surface of the substrate layer, and it is preferable that a resin that does not contain an aromatic compound is used.

[0027] For example, the hard coat film layer of the eyeglass lens may preferably be an organosiloxane resin containing inorganic oxide fine particles. The organosiloxane resin is preferably obtained by hydrolyzing and condensing an alkoxysilane. Specific examples of the organosiloxane resin include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, methyltrimethoxysilane, ethyl silicate, or a combination thereof. The hydrolysis condensate of the alkoxysilane is produced by hydrolyzing the alkoxysilane compound or a combination thereof with an acidic aqueous solution such as hydrochloric acid.

[0028] In addition, the material of the inorganic oxide microparticles includes, for example, sols of zinc oxide, silicon dioxide (silica microparticles), aluminum oxide, titanium oxide (titania microparticles), zirconium oxide (zirconia microparticles), tin oxide, beryllium oxide, antimony oxide, tungsten oxide, and cerium oxide, either alone or in combination of two or more of them.

[0029] From the viewpoint of ensuring the transparency of the hard coat film layer, the diameter of the inorganic oxide fine particles is preferably 1 nm to 100 nm, more preferably 1 nm to 50 nm. Also, from the viewpoint of ensuring an appropriate degree of hardness and toughness in the hard coat film layer, the blending amount (concentration) of the inorganic oxide fine particles is preferably 40 wt % to 60 wt % of the total components of the hard coat film layer.

[0030] In addition, at least one of acetylacetone metal salt and ethylenediaminetetraacetic acid metal salt is added to the hard coat liquid as a curing catalyst, and further, a surfactant, a colorant, a solvent, etc. are added as necessary for ensuring adhesion to the substrate, facilitating formation, imparting a desired (semi)transparent color, etc.

[0031] The inorganic oxide (metal oxide) in the inorganic oxide microparticles is selected to have as little absorption as possible in the visible range. This is from the viewpoint of ensuring high transmittance over the entire visible range and ensuring a state in which the difference in color seen with the naked eye and the color seen when wearing the lens is extremely small. From this viewpoint, the inorganic oxide is preferably an oxide of one or more metals other than Ti (titanium) and Ce (cerium). Since Ti (titanium) oxide and Ce (cerium) oxide have absorption in the visible range (especially on the short wavelength side), they are excluded from the preferable metal oxides.

[0032] Examples of suitable metal oxides include oxides of Sb (antimony), Sn (tin), Si (silicon), Al (aluminum), Ta (tantalum), La (lanthanum), Fe (iron), Zn (zinc), W (tungsten), Zr (zirconium), and In (indium), or combinations thereof.

[0033] The physical thickness of the hard coat film layer is preferably 0.5 μm (micrometers) or more and 4.0 μm or less. The lower limit of this film thickness range is determined because it is difficult to obtain sufficient hardness if the film thickness is thinner than this. On the other hand, the upper limit is determined because if the film thickness is made thicker than this, the possibility of problems with physical properties such as cracks and brittleness increases dramatically, and the influence of absorption (reduction in transmittance) in the visible range by inorganic oxide fine particles increases. In addition to these thermosetting coating agents, the hard coat agent used in the hard coat film layer may be a known photocuring coating agent.

[0034] The eyeglass lens in the embodiment may also include an anti-reflection coating layer (which may be written as "anti-reflection coating" or "anti-reflection layer") that is coated on at least one surface of the substrate layer and is formed to transmit wavelengths in the UVA region and reflect wavelengths in the UVB region. The anti-reflection coating layer may be formed on the substrate layer, but is preferably formed on the hard coat film layer. The anti-reflection coating layer may also be formed of an optical multilayer film.

[0035] From the viewpoint of ensuring an anti-reflection function, the optical multilayer film is preferably formed so as to have a nearly flat and high transmittance distribution over the entire range of UVA and visible light. A high transmittance is, for example, 90% or more.

[0036] The optical multilayer film is formed by alternately laminating low-refractive index layers and high-refractive index layers, and preferably has an odd number of layers overall (a total of 5 layers, 7 layers, etc.). More preferably, assuming that the layer closest to the substrate (the layer closest to the substrate) is the first layer, the odd-numbered layers are low-refractive index layers and the even-numbered layers are high-refractive index layers. The low-refractive index layers and high-refractive index layers are formed by vacuum deposition, ion-assisted deposition, ion plating, sputtering, etc.

[0037] <Eyeglass lenses> Regarding the eyeglass lens according to the embodiment, examples of various base resins that are candidates for the base layer of the eyeglass lens of the disclosed technology are listed below. Base material resin 1: ACRYPET (registered trademark) VH000 Base material resin 2: ZEONEX (registered trademark) K22R Base resin 3: ARTON(registered trademark) F3500 Base material resin 4: Acrylite (registered trademark) L000 Base material resin 5: ZEONEX (registered trademark) K26R Base material resin 6: TPX (registered trademark) RT18 Base material resin 7: APEL (registered trademark) 5014XH Base material resin 8: CR-39 (registered trademark) Base material resin 9: MR-8 (registered trademark) Base material resin 10: MR-10 (registered trademark)

[0038] All of the above-mentioned examples of substrate resins are candidates for the substrate layer, but below, substrate resins 1 to 3 will be described as examples of resins that transmit wavelengths in the UVA region while blocking wavelengths in the UVB region. The inventors also conducted experiments to investigate the total transmittance of the resin (substrate layer) and the AR coat by changing the type of anti-reflection film layer (also called "AR (Anti Reflection) coat") for each substrate resin as a spectacle lens according to the embodiment.

[0039] The AR coatings used in the experiment included a visible light AR coating that prevents reflection (or transmits) of visible light, and a UVA visible light AR coating that prevents reflection of the UVA region and the visible light region. The substrate layer used in the experiment included only a substrate resin and a substrate resin to which a radical scavenger and / or ultraviolet absorbing agent was added, and was a test piece with a thickness of 2 mm. The radical scavenger or ultraviolet absorbing agent was Adeka STAB (registered trademark) (LA-63P, LA-52, LA-57, or LA-46) from ADEKA Corporation, and 0.2 wt%, 0.003 wt%, or 0.005 wt% was added to each substrate layer. The radical scavenger prevents deterioration of the lens, making it possible to improve the durability of the lens.

[0040] Fig. 2 is a diagram showing an example of the total transmittance of each substrate layer based on substrate resin 1 and each AR coat. In the graph shown in Fig. 2, the vertical axis represents transmittance and the horizontal axis represents wavelength, and the transmittance of each combination pattern of substrate resin and AR coat is shown below. Hereinafter, "transmittance" refers to the transmittance of a predetermined wavelength or any wavelength within a predetermined region, and "average transmittance" refers to the average transmittance of the transmittance at each wavelength within a predetermined region. Test piece 11: Base material resin 1 without AR coating Test piece 12: Base material resin 1 with visible light AR coating formed on both sides Test piece 13: Base material resin 1 with UVA visible light AR coating on both sides Test piece 14: No AR coating, Base material resin 1 with LA-63P (0.2 wt%) added Test piece 15: Visible light AR coating formed on both sides, base material resin 1 to which LA-63P (0.2 wt%) was added Test piece 16: UVA visible light AR coating formed on both sides, base material resin 1 to which LA-63P (0.2 wt%) was added

[0041] For test piece 11, the transmittance is about 90% in the region of 330 nm or more, and decreases as the wavelength becomes shorter in the region of 330 nm or less, with the transmittance at 280 nm being just under 65%.

[0042] For test piece 12, the transmittance is 90% or more in the region above 380 nm because reflection of visible light is prevented, but since no consideration is given to light other than visible light, the transmittance decreases as the wavelength becomes shorter in the region of approximately 400 nm or less, and at 280 nm the transmittance is approximately 60%.

[0043] For test piece 13, since reflection of the UVA region and visible light is prevented, the transmittance is approximately 90% or more in the region above 330 nm, but since the UVB region is not specifically taken into consideration, the decrease in transmittance increases as the wavelength becomes shorter in the region below approximately 315 nm, and at 280 nm the transmittance is 40% or less.

[0044] For test piece 14, the transmittance is about 90% in the region of 380 nm or more, and decreases as the wavelength becomes shorter in the region of 315 nm or more and 380 nm or less, but the transmittance is still 80% or more, and decreases further below 315 nm, with the transmittance at 280 nm being just under 65%. According to this result, by adding a radical scavenger to the base layer, it is possible to reduce the transmittance at wavelengths below visible light.

[0045] For test piece 15, reflection of visible light is prevented, so the transmittance is basically the same as that of test piece 12. However, due to the influence of the radical scavenger, the transmittance of test piece 15 is further reduced than that of test piece 12 at wavelengths of 330 nm or less, and the transmittance at 280 nm is 50% or less.

[0046] Test piece 16 has approximately the same transmittance as test piece 13 in the region of 380 nm or more. However, due to the influence of the radical scavenger, the transmittance of test piece 16 is reduced by approximately several percent compared to the transmittance of test piece 13 in the region of 380 nm or less.

[0047] According to the example shown in Fig. 2, the transmittance of the substrate resin 1 in the UVB region is relatively lower than the transmittance in the UVA region and the visible light region, so that the substrate resin 1 is suitable for the technology of the present disclosure (see, for example, test piece 11). In addition, compared with the substrate resin 1 alone or a test piece having a visible light AR coating film layer, coating with a UVA visible light AR coating makes it possible to improve the transmittance in the UVA region and to reduce the transmittance in the UVB region (see, for example, test pieces 11, 12, and 13). Furthermore, adding a radical scavenger (LA-63P) to the substrate resin 1 makes it possible to reduce the transmittance, particularly in the UVB region (see, for example, test pieces 13 and 16).

[0048] Fig. 3 is a diagram showing an example of the reflectance of test pieces 11 to 16. In the graph shown in Fig. 3, the vertical axis represents reflectance and the horizontal axis represents wavelength, showing the reflectance of each test piece. Since both test pieces 11 and 14 have no AR coating, the reflectance is almost flat (<10%) in the range of 280 nm to 780 nm. Hereinafter, "reflectance" refers to the reflectance of a predetermined wavelength or any wavelength within a predetermined region, and "average reflectance" refers to the average reflectance of the reflectance at each wavelength within a predetermined region.

[0049] The reflectance of the test pieces 12 and 15 is 5% or less on average in the visible light region (380 to 780 nm), and 3% or less on average in the 400 to 630 nm region in particular. On the other hand, in the visible light AR coating, the region below 380 nm is not particularly taken into consideration, so the reflectance has a characteristic similar to a generally normal distribution with a maximum value of about 27% at about 300 nm in the region below 380 nm.

[0050] For test pieces 13 and 16, the UVA visible light AR coating is applied to both sides, so the reflectance is 10% or less in the region of 330 nm or more. On the other hand, in the UVB region below 330 nm, in particular, the UVA visible light AR coating does not take the reflectance into consideration, so the reflectance increases as the wavelength becomes shorter, and at about 280 nm the reflectance is about 30% or more.

[0051] As shown in FIG. 3, the UVA visible light AR coating prevents reflection of wavelengths in the UVA and visible light regions, but the UVB region is not particularly considered, so the reflectance increases as the wavelength becomes shorter. Therefore, when designing a spectacle lens that transmits as much as possible of the UVA and visible light regions and prevents as much as possible of the UVB region, it is preferable to coat at least one surface with the UVA visible light AR coating. In addition, for the UVB region, it is sufficient that the total average reflectance of the coating film layer and the substrate resin 1 is higher than the average reflectance of the substrate resin 1 only, as in the test pieces 13 and 16. For example, a coating film layer having a reflectance characteristic with a maximum value in the UVB region may be formed. This makes it possible to actively cut light in the UVB region by selecting a coating film layer whose average reflectance for wavelengths in the UVB region is higher than the average reflectance for wavelengths in other regions and forming it on the substrate layer.

[0052] Fig. 4 is a diagram showing an example of the total transmittance of each substrate layer based on substrate resin 2 and each AR coating. In the graph shown in Fig. 4, the vertical axis represents transmittance and the horizontal axis represents wavelength, and the transmittance of each combination pattern of the substrate resin and AR coating shown below is shown. Test piece 21: Base material resin 2 without AR coating Test piece 22: Base material resin 2 with visible light AR coating formed on both sides Test piece 23: Base material resin 2 with UVA visible light AR coating on both sides Test piece 24: No AR coating, base resin 2 with LA-52 (0.2 wt%) added Test piece 25: Visible light AR coating formed on both sides, base material resin 2 to which LA-52 (0.2 wt%) was added Test piece 26: UVA visible light AR coating formed on both sides, base material resin 2 to which LA-52 (0.2 wt%) was added Test piece 27: No AR coating, base resin 2 with LA-57 (0.2 wt%) added Test piece 28: Visible light AR coating formed on both sides, base material resin 2 to which LA-57 (0.2 wt%) was added Test piece 29: UVA visible light AR coating formed on both sides, base material resin 2 to which LA-57 (0.2 wt%) was added

[0053] For the test piece 21, the transmittance is constant at about 90% in the region of about 360 nm or more. The transmittance of the test piece 21 suddenly decreases to about 60% as the wavelength becomes shorter in the region of about 320 nm to about 360 nm. Moreover, the transmittance of the test piece 21 gradually decreases as the wavelength becomes shorter in the region of about 300 nm to 320 nm, and then suddenly decreases to about 0% as the wavelength becomes shorter in the region of about 280 nm to 300 nm.

[0054] For test piece 22, since reflection of visible light is prevented, the transmittance is 90% or more in the region above 380 nm, but since no consideration is given to light other than visible light, the transmittance drops sharply to about 45% as the wavelength becomes shorter in the region from about 400 nm to about 315 nm, and then at 280 nm, the transmittance drops sharply to about 0%.

[0055] For test piece 23, reflection of the UVA region and visible light is prevented, so the transmittance is about 90% or more in the region of about 350 nm or more. For the UVA visible light AR coating, the UVB region is not particularly taken into consideration in terms of reflection, so the transmittance of resin 23 decreases as the wavelength becomes shorter in the region of about 350 nm or less, and at 280 nm the transmittance is nearly 0%.

[0056] For the test piece 24, the transmittance is about 90% in the region of about 430 nm or more, decreases to about 80% as the wavelength becomes shorter in the region of about 350 nm to about 430 nm, and then suddenly decreases to about 20% as the wavelength becomes shorter in the region of about 320 nm to about 350 nm. The transmittance of the test piece 24 is constant at about 20% in the wavelength region of 300 nm to 320 nm, and decreases to 0% as the wavelength becomes shorter in the region of 280 nm to 300 nm. According to this result, by adding the radical scavenger (LA-52) to the base layer, it is possible to reduce the transmittance at wavelengths below visible light, especially in the region of 300 nm to about 380 nm.

[0057] Since reflection of visible light is prevented in test piece 25, the transmittance in the region of about 370 nm or more is basically the same as that of test piece 22. However, due to the influence of the radical scavenger, the transmittance of test piece 25 is further reduced compared to test piece 22 and test piece 24 in the wavelength region of about 370 nm or less.

[0058] Test piece 26 basically exhibits the same transmittance as test piece 25, but in the range of approximately 300 nm to approximately 370 nm, test piece 26, which has a UVA visible light AR coating formed thereon, has a higher transmittance than test piece 25.

[0059] Regarding the test piece 27, the transmittance of the test piece 27 is almost the same as that of the test piece 24 in the region of about 380 nm or more, but in the region of about 300 nm to about 380 nm, the transmittance of the test piece 27 is lower than that of the test piece 24, being lower by about 10% at most. This shows that the transmittance of the test piece changes depending on the type of radical scavenger added. Furthermore, by adding the radical scavenger LA-57, the transmittance is significantly lowered in the UVB region, demonstrating that the disclosed technology is suitable.

[0060] Regarding test piece 28 and test piece 29, both test pieces show similar transmittance, but in the range of approximately 300 nm to approximately 370 nm, test piece 29, which has a UVA visible light AR coating formed thereon, has a higher transmittance than test piece 28.

[0061] According to the example shown in FIG. 4, the transmittance of the UVB region of the resin 2 for the substrate is relatively lower than the transmittance of the UVA region and the visible light region, so that it is suitable for the technology of the present disclosure (see, for example, the test piece 21). In addition, the transmittance of the UVB region of the resin 2 for the substrate is lower than the transmittance of the resin 1 for the substrate, so that it is more suitable for the technology of the present disclosure (see, for example, the test piece 21 in FIG. 4 and the test piece 11 in FIG. 2). In addition, by coating the resin 2 for the substrate with a visible light AR coat, it is possible to lower the transmittance in the UVB region compared to the resin 2 for the substrate alone (see, for example, the test pieces 24 and 25). Furthermore, by coating the resin 2 for the substrate with a UVA visible light AR coat, it is possible to improve the transmittance in the UVA region and lower the transmittance in the UVB region compared to the case of the resin 2 for the substrate alone or the test piece on which the visible light AR coat film layer is formed (see, for example, the test pieces 21, 22, and 23). Also, by adding a radical scavenger (LA-57 or LA-52) to the base resin 2, it becomes possible to reduce the transmittance in the UVB region (see, for example, test pieces 21 to 23 and test pieces 24 to 29). Furthermore, with regard to the added radical scavenger, LA-57 makes it possible to reduce the transmittance more than LA-52 (see, for example, test pieces 24 to 26 and test pieces 27 to 29).

[0062] Fig. 5 is a diagram showing an example of the reflectance of test pieces 21 to 29. In the graph shown in Fig. 5, the vertical axis represents reflectance and the horizontal axis represents wavelength, and shows the reflectance of each test piece. Since test piece 21, test piece 24, and test piece 27 all have no AR coating, the reflectance is almost flat (<10%) in the range of about 350 nm to 780 nm, and the reflectance further decreases in the range of 280 nm to about 350 nm.

[0063] The reflectances of the test pieces 22, 25, and 28 have almost the same tendency in the visible light region (380 nm to 780 nm), with an average reflectance of 5% or less, and especially in the region of about 400 nm to about 630 nm, the average reflectance is 3% or less. On the other hand, the visible light AR coating does not take into consideration the region of 380 nm or less, so the reflectance is high. In addition, these reflectances have characteristics similar to a normal distribution in the region of 380 nm or less, with the test piece 22 having a maximum value of about 20% at about 310 nm, and the test pieces 25 and 28 having a maximum value of about 21 to 23% at about 290 nm, and the peak wavelengths and maximum values ​​are slightly different between the test piece 22, the test piece 25, and the test piece 28.

[0064] Test piece 23, test piece 26, and test piece 29 have almost the same reflectance in the range of 280 nm to 780 nm. In addition, because both sides are coated with UVA visible light AR coating, these reflectances are around 25% at 280 nm, and the average reflectance is 5% or less in the range of about 330 nm to 780 nm. Furthermore, in the range of about 350 nm or less, the reflectances of test piece 26 and test piece 29 are slightly lower than the reflectance of test piece 23, which is thought to be due to the influence of the radical scavenger.

[0065] In the example shown in FIG. 5, as in the example shown in FIG. 3, the UVA visible light AR coating prevents reflection of wavelengths in the UVA and visible light regions, but the UVB region is not particularly considered, so the reflectance increases as the wavelength becomes shorter. In addition, the reflectance shown in FIG. 5 tends to be lower than the reflectance shown in FIG. 3 overall. This is thought to be because the substrate resin 2 has the property of absorbing light more than the substrate resin 1. Note that, for the UVB region, it is sufficient that the total average reflectance of the coating film layer and the substrate resin 2 is higher than the average reflectance of the test piece 21 (only the substrate resin 2) as in the test pieces 23, 26, and 29. For example, a coating film layer having a reflectance characteristic with a maximum value in the UVB region may be formed. As a result, by selecting a coating film layer whose average reflectance for wavelengths in the UVB region is higher than the average reflectance for wavelengths in other regions and forming it on the substrate layer, it becomes possible to actively cut light in the UVB region.

[0066] Fig. 6 is a diagram showing an example of the transmittance of each substrate layer to which an ultraviolet absorber (LA-46) and / or a radical scavenger (LA-52) based on substrate resin 3 has been added. In the graph shown in Fig. 6, the vertical axis represents transmittance and the horizontal axis represents wavelength, and the transmittance of each substrate resin described below is shown. No AR coating was formed on any of the test pieces. Test piece 31: Base resin 3 only Test piece 32: Base resin 3 with LA-52 (0.2 wt%) added Test piece 33: Base resin 3 containing LA-52 (0.2 wt%) and LA-46 (0.001 wt%) Test piece 34: Base resin 3 with LA-46 (0.003 wt%) added Test piece 35: Base resin 3 with LA-46 (0.005 wt%) added

[0067] By adding an ultraviolet absorber (LA-46) and / or a radical scavenger (LA-52) to the base resin 3, it is possible to transmit as much of the UVA region as possible while preventing transmission of the UVB region, even without an AR coating. For example, in the UVB region, the transmittance of test piece 31 without additives exceeds 10% at wavelengths above about 295 nm, whereas the transmittance of test pieces 32 to 35 is all 5% or less, preventing transmission of light in the UVB region.

[0068] Regarding additives, ultraviolet absorbers can reduce the transmittance more than radical scavengers (see, for example, test piece 32 and test pieces 34-35). Regarding the amount of ultraviolet absorber added, there is no difference in transmittance in the UVB region for test pieces 34-35, but in the UVA region, the transmittance is slightly lower at 0.005 wt% than at 0.003 wt%. Therefore, since increasing the amount of ultraviolet absorber added reduces the transmittance in the UVA region, it may be preferable to add an amount of about 0.003 wt% or less (see, for example, test piece 33) depending on the purpose.

[0069] Fig. 7 is a diagram showing an example of the transmittance when a UVA visible light AR coating is formed on each of the resins shown in Fig. 6. In the graph shown in Fig. 7, the vertical axis represents the transmittance and the horizontal axis represents the wavelength, and the transmittance of each of the resins described below is shown. Test piece 31U: Test piece 31 with UVA visible light AR coating formed on both sides Test piece 32U: Test piece 32 with UVA visible light AR coating on both sides Test piece 33U: Test piece 33 with UVA visible light AR coating on both sides Test piece 34U: Test piece 34 with UVA visible light AR coating on both sides Test piece 35U: Test piece 35 with UVA visible light AR coating on both sides

[0070] As shown in FIG. 7, when the UVA visible light AR coating was applied to test pieces 31 to 35, there was no fundamental change in the transmittance trend, but the transmittance increased in the visible light region, and all of the average transmittances were 95% or more.

[0071] 6 and 7, adding a radical scavenger and / or an ultraviolet absorbing agent to the base resin 3 and coating both sides with a UVA visible light AR coat makes it possible to block the UVB region, transmit as much of the UVA region as possible, and transmit almost all of the visible light region. Note that the base resin 3 itself can suppress the transmittance of the UVB region wavelengths to about 15% or less, which is suitable for the technology of the present disclosure.

[0072] Fig. 8 is a diagram showing an example of the transmittance when each AR coating is formed on the substrate resin 3. In the graph shown in Fig. 8, the vertical axis represents the transmittance and the horizontal axis represents the wavelength, and the transmittance of each resin described below is shown. Specimen 31: Specimen 31 without AR coating Test piece 31A: Test piece 31 with visible light AR coating formed on both sides Test piece 31U: Test piece 31 with UVA visible light AR coating formed on both sides

[0073] The transmittance of the test piece 31 shown in Fig. 8 is the same as that of the test piece 31 shown in Fig. 6. For the test piece 31A, since a visible light AR coating is formed on both sides, the transmittance in the visible light region of about 380 nm to 780 nm is equal to or higher than that of the test piece 31. On the other hand, since no particular consideration is given to the region below about 380 nm, the average transmittance in the region of about 330 nm to about 380 nm is smaller than that of the test piece 31.

[0074] For the test piece 31U, since the UVA visible light AR coating is formed on both sides, the transmittance in the visible light region (380 nm to 780 nm) is equal to or higher than that of the test piece 31. In addition, since reflection of wavelengths in the UVA region is prevented, the average transmittance in the UVA region of the test piece 31U is equal to or higher than that of the test piece 31A, which has visible light AR coatings formed on both sides. Note that all of the test pieces shown in FIG. 8 can suppress the transmittance of wavelengths in the UVB region to about 15% or less, and therefore are suitable for the technology of the present disclosure.

[0075] Fig. 9 is a diagram showing comparative examples of the reflectance of test pieces 31 on which each AR coating is formed. The graph shown in Fig. 9 shows the reflectance of each test piece, with the vertical axis representing the reflectance and the horizontal axis representing the wavelength. The test pieces compared in Fig. 9 are the same as the test pieces shown in Fig. 8.

[0076] Since the test piece 31 does not have an AR coating, it has a nearly flat reflectance (<10%) in the range of about 350 nm to 780 nm, and the reflectance is about 5% in the range of 280 nm to 330 nm.

[0077] For the test piece 31A, the average reflectance in the visible light region (380 nm to 780 nm) is 5% or less, and in particular in the region of about 400 nm to about 630 nm, the average reflectance is 2% or less. On the other hand, the visible light AR coating does not take into consideration the region of 380 nm or less, so the reflectance is high. For example, the maximum reflectance is over 17% at about 300 nm.

[0078] For test piece 31U, the average reflectance is about 5% in the region of about 300 nm or less. As in the examples shown in Figures 3 and 5, the UVA visible light AR coating prevents reflection of wavelengths in the UVA region and the visible light region, but does not take the UVB region into consideration, so that in the region from 280 nm to about 330 nm, as the wavelength becomes shorter, the reflectance increases, reaching about 8% at 280 nm.

[0079] According to FIG. 9, the reflectance of the substrate resin 3 is generally lower than that of the substrate resin 2 shown in FIG. 5. This is believed to be because the substrate resin 3 itself has the property of absorbing light (particularly light in the ultraviolet region) more than the substrate resin 2. It is sufficient that the total average reflectance of the coating film layer and the substrate resin 3 for the UVB region is higher than the average reflectance of the test piece 31 (only the substrate resin 3). For example, a coating film layer having a reflectance characteristic with a maximum value in the UVB region may be formed. This makes it possible to actively cut light in the UVB region by selecting and forming on the substrate layer a coating film layer whose average reflectance for wavelengths in the UVB region is higher than the average reflectance for wavelengths in other regions.

[0080] Fig. 10 is a diagram showing comparative examples of the reflectance of test piece 32 and test piece 35 on which each AR coating is formed. The graph shown in Fig. 10 shows the reflectance of each test piece, with the vertical axis representing reflectance and the horizontal axis representing wavelength. The reflectance of only test piece 32 and test piece 35, both of which have no AR coating, is almost flat (<10%) in the range of 380 nm to 780 nm, and the reflectance further decreases in the range of 280 nm to 380 nm, reaching approximately 5% at 280 nm to 330 nm.

[0081] Test piece 32A and test piece 35A, which are coated on both sides with visible light AR coating, have approximately the same reflectance in the visible light range, but test piece 32A, which does not contain an ultraviolet absorber, has a higher reflectance in the wavelength range of 280 nm to approximately 320 nm, which includes UVB.

[0082] As described above, the visible light AR coating does not take into consideration the region below 380 nm, so the reflectance is high. Furthermore, these reflectances have characteristics similar to a roughly normal distribution in the region below 380 nm, with test piece 32A having a maximum value of about 22% at about 290 nm and test piece 35A having a maximum value of about 15% at about 330 nm, with the respective peak wavelengths and maximum values ​​being slightly different.

[0083] The test pieces 32U and 35U, coated on both sides with the UVA visible light AR coating, have almost the same reflectance in the range of about 350 nm to 780 nm. In addition, these reflectances are average reflectances of 5% or less because the UVA visible light AR coating is coated on both sides. Furthermore, the reflectance of both increases as the wavelength becomes shorter in the range of about 330 nm or less for the test piece 32U and about 350 nm or less for the test piece 35U.

[0084] In the example shown in FIG. 10, similar to the examples shown in FIGS. 3 and 5, the UVA visible AR coating prevents reflection of wavelengths in the UVA and visible light ranges, but does not take the UVB range into special consideration, so the reflectance increases as the wavelength becomes shorter.

[0085] Fig. 11 is a diagram showing comparative examples of the reflectance of each test piece on which a UVA visible light AR coating is formed. The graph shown in Fig. 11 shows the reflectance of each test piece, with the vertical axis representing the reflectance and the horizontal axis representing the wavelength.

[0086] In the examples shown in FIG. 11, the UVA visible light AR coating is formed on both sides, so there is no significant difference in the tendency of the reflectance. Therefore, by coating both sides with the UVA visible light AR coating, it is possible to transmit as much of the wavelengths in the UVA and visible light regions as possible while preventing the transmission of wavelengths in the UVB region as much as possible. In addition, the UVA visible light AR coating used in the experiment shown in FIG. 11 does not take the UVB region into consideration, so the reflectance is high in the UVB region. In other words, since the reflectance increases without any special consideration of the UVB region, if a UVA visible light AR coating designed to further increase the reflectance is formed on the base layer, it is possible to further cut the wavelengths in the UVB region.

[0087] Fig. 12 is a table comparing the transmittance of each base resin in each wavelength range. The table shown in Fig. 12A compares the transmittance of test pieces 11 to 16 in the ultraviolet range of 280 to 315 nm (UVB range) and 315 to 380 nm (UVA range).

[0088] In the results shown in FIG. 12A, the test piece 11 (only the base resin 1) has an average transmittance of 90.4% in the UVA region and 78.9% in the UVB region. The test piece 12 (the base resin 1 with the visible light AR coating) has an average transmittance of 79.3% in the UVA region and 63.1% in the UVB region. The test piece 13 (the base resin 1 with the UVA visible light AR coating) has an average transmittance of 91.2% in the UVA region and 64.2% in the UVB region.

[0089] In addition, for test piece 14 (base resin 1 with LA-63P (0.2 wt%) added), the average transmittance in the UVA region is 86.5%, and the average transmittance in the UVB region is 74.6%. For test piece 15 (base resin 1 with visible light AR coating formed on both sides and with LA-63P (0.2 wt%) added), the average transmittance in the UVA region is 77.4%, and the average transmittance in the UVB region is 55.4%. For test piece 16 (base resin 1 with UVA visible light AR coating formed on both sides and with LA-63P (0.2 wt%) added), the average transmittance in the UVA region is 87.0%, and the average transmittance in the UVB region is 57.6%.

[0090] In the results shown in FIG. 12B, the test piece 21 (only the base resin 2) has an average transmittance of 81.4% in the UVA region and an average transmittance of 36.2% in the UVB region. The test piece 22 (base resin 2 with a visible light AR coating) has an average transmittance of 74.3% in the UVA region and an average transmittance of 28.9% in the UVB region. The test piece 23 (base resin 2 with a UVA visible light AR coating) has an average transmittance of 82.4% in the UVA region and an average transmittance of 32.2% in the UVB region.

[0091] In addition, for test piece 24 (base resin 2 with LA-52 (0.2 wt%) added), the average transmittance in the UVA region is 63.9%, and the average transmittance in the UVB region is 13.1%. For test piece 25 (base resin 2 with visible light AR coating formed on both sides and with LA-52 (0.2 wt%) added), the average transmittance in the UVA region is 61.0%, and the average transmittance in the UVB region is 10.1%. For test piece 26 (base resin 2 with UVA visible light AR coating formed on both sides and with LA-52 (0.2 wt%) added), the average transmittance in the UVA region is 65.7%, and the average transmittance in the UVB region is 13.0%.

[0092] In addition, for test piece 27 (base resin 2 with LA-57 (0.2 wt%) added), the average transmittance in the UVA region is 57.7%, and the average transmittance in the UVB region is 6.7%. For test piece 28 (base resin 2 with visible light AR coating formed on both sides and with LA-57 (0.2 wt%) added), the average transmittance in the UVA region is 55.4%, and the average transmittance in the UVB region is 5.5%. For test piece 29 (base resin 2 with UVA visible light AR coating formed on both sides and with LA-57 (0.2 wt%) added), the average transmittance in the UVA region is 59.1%, and the average transmittance in the UVB region is 6.7%.

[0093] According to the results shown in Fig. 12B, for example, by adding a radical scavenger to the base resin 2 and forming a UVA visible light AR coating on both sides, it becomes possible to make the transmittance in the UVA region about 60% or more and the transmittance in the UVB region about 13% or less. In particular, if LA-57 is added as a radical scavenger, the transmittance in the UVB region can be made lower than that of LA-52, making it possible to make it 7% or less.

[0094] In the results shown in FIG. 12C, the test piece 31 (only the base resin 3) has an average transmittance of 57.4% in the UVA region and 7.6% in the UVB region. The test piece 31A (base resin 3 with visible light AR coating) has an average transmittance of 53.0% in the UVA region and 6.9% in the UVB region. The test piece 31U (base resin 3 with UVA visible light AR coating) has an average transmittance of 58.4% in the UVA region and 7.2% in the UVB region.

[0095] In addition, the test piece 32 (base resin 3 with LA-52 (0.2 wt%) added) has an average transmittance of 47.4% in the UVA region and 2.9% in the UVB region. The test piece 32A (base resin 3 with visible light AR coating formed on both sides and with LA-52 (0.2 wt%) added) has an average transmittance of 44.8% in the UVA region and 2.0% in the UVB region. The test piece 32U (base resin 3 with UVA visible light AR coating formed on both sides and with LA-52 (0.2 wt%) added) has an average transmittance of 48.6% in the UVA region and 2.9% in the UVB region.

[0096] In addition, the test piece 33 (resin 3 for substrate to which LA-52 (0.2 wt%) and LA-46 (0.001 wt%) were added) had an average transmittance of 42.0% in the UVA region and 2.1% in the UVB region. The test piece 33A (resin 3 for substrate to which visible light AR coating was formed on both sides and LA-52 (0.2 wt%) and LA-46 (0.001 wt%) were added) had an average transmittance of 40.5% in the UVA region and 1.6% in the UVB region. The test piece 33U (resin 3 for substrate to which UVA visible light AR coating was formed on both sides and LA-52 (0.2 wt%) and LA-46 (0.001 wt%) were added) had an average transmittance of 43.4% in the UVA region and 2.2% in the UVB region.

[0097] In the results shown in FIG. 12D, the test piece 34 (base resin 3 with LA-46 (0.003 wt%) added) has an average transmittance of 31.8% in the UVA region and 0.7% in the UVB region. The test piece 34A (base resin 3 with visible light AR coating formed on both sides and with LA-46 (0.003 wt%) added) has an average transmittance of 29.3% in the UVA region and 0.7% in the UVB region. The test piece 34U (base resin 3 with UVA visible light AR coating formed on both sides and with LA-46 (0.003 wt%) added) has an average transmittance of 32.5% in the UVA region and 0.7% in the UVB region.

[0098] In addition, the test piece 35 (base resin 3 with LA-46 (0.005 wt%) added) has an average transmittance of 26.5% in the UVA region and 0.6% in the UVB region. The test piece 35A (base resin 3 with visible light AR coating formed on both sides and with LA-46 (0.005 wt%) added) has an average transmittance of 24.2% in the UVA region and 0.5% in the UVB region. The test piece 35U (base resin 3 with UVA visible light AR coating formed on both sides and with LA-46 (0.005 wt%) added) has an average transmittance of 26.8% in the UVA region and 0.5% in the UVB region.

[0099] According to the results shown in Figures 12C and 12D, by adding a radical scavenger and / or an ultraviolet absorber to the resin 3 for the substrate, the transmittance of the UVA region can be 25% or more, and the transmittance of the UVB region can be 3% or less. When focusing on lowering the transmittance of the UVB region, adding an ultraviolet absorber to the resin 3 for the substrate can lower the transmittance of the UVB region to 1% or less (see, for example, test pieces 34 and 35 in Figure 12D). In addition, when it is desired to lower the transmittance of the UVB region as much as possible while increasing the transmittance of the UVA region, by using test pieces 32 and 33, it is possible to increase the transmittance of the UVA region to 40% or more and the transmittance of the UVB region to 3% or less. Furthermore, when a UVA visible light AR coat is formed on both sides, the transmittance of the UVA region can be improved while suppressing the transmittance of the UVB region to about 3% or less, compared to the case where only a radical scavenger and / or an ultraviolet absorber is added to the resin 3 for the substrate.

[0100] According to the example shown in Fig. 12, a spectacle lens can be formed in which the total average UVA transmittance of each substrate resin constituting the substrate layer of the spectacle lens and the coating film layer is higher than the average UVA transmittance of the substrate layer, and the total average UVB transmittance of the substrate layer and the coating film layer is lower than the average UVB transmittance of the substrate layer (see Figs. 12A to 12D, for example). This makes it possible to form a spectacle lens that transmits as much of the UVA region as possible while minimizing the transmission of the UVB region. The average UVA transmittance indicates the average transmittance of the UVA region, and the average UVB transmittance indicates the average transmittance of the UVB region.

[0101] The coating film layer of the eyeglass lens may also include an anti-reflection coating layer that prevents reflection of wavelengths in the UVA and visible light regions. This anti-reflection coating layer is referred to as a UVA visible light AR coating above. The UVA visible light AR coating reflects as much of the UVB wavelength as possible, so that the UVB wavelength is prevented from passing through the eyeglass lens (see, for example, FIG. 11).

[0102] The coating film layer may have a characteristic that the reflectance increases as the wavelength becomes shorter in the wavelength region of 280 nm or more and less than 315 nm. As shown in Figures 3, 5, 9 to 11, the UVA visible light AR coating can cut more wavelengths in the UVB region by increasing the reflectance as the wavelength becomes shorter in the region of 280 nm to 315 nm.

[0103] The substrate layer may contain a radical scavenger and / or an ultraviolet absorbing agent. For example, the addition of a radical scavenger or an ultraviolet absorbing agent to the resin 2 significantly reduces the transmission of wavelengths in the UVB region and transmits wavelengths in the UVA region as much as possible. Furthermore, the substrate layer may contain a radical scavenger and / or an ultraviolet absorbing agent, and the coating film layer may include an anti-reflection film layer that prevents reflection of wavelengths in the UVA region and visible light region.

[0104] In addition, the difference between the total average UVA transmittance and the average UVB transmittance of the substrate layer and the coating film layer may be larger than the difference between the total average UVA transmittance and the average UVB transmittance of the substrate layer alone, or the difference between the total average UVA transmittance and the average UVB transmittance of the substrate layer and the anti-reflection film layer that prevents reflection of a specific wavelength in the visible light region (see, for example, Figures 12A to 12D). This makes it possible to transmit as much of the UVA region wavelength as possible while not transmitting as much of the UVB region wavelength as possible, for example, compared to lenses formed with existing visible light AR coatings.

[0105] Also, the spectacle lens may have a substrate layer and a coating film layer, and the total UVA average transmittance of the substrate layer and the coating film layer may be approximately equal to or greater than the UVA average transmittance of the substrate layer, and the total UVB average transmittance of the substrate layer and the coating film layer may be approximately equal to or less than the UVB average transmittance of the substrate layer. Furthermore, the spectacle lens may have a difference between the total UVA average transmittance and the UVB average transmittance of the substrate layer and the coating film layer greater than the difference between the UVA average transmittance and the UVB average transmittance of the substrate layer alone, or the difference between the total UVA average transmittance and the UVB average transmittance of the substrate layer and the anti-reflection film layer that prevents reflection of a specific wavelength in the visible light region. This makes it possible to configure a spectacle lens that cuts as much of the UVB region wavelength as possible and transmits as much of the UVA region wavelength as possible, even if the average transmittance of the UVB region is the same as or slightly higher than the average transmittance of the substrate resin alone, depending on the type of substrate resin, the presence or absence of a radical scavenger / ultraviolet ray absorber, and the combination of the UVA visible light AR coating.

[0106] FIG. 13 is a table comparing the solar ultraviolet transmittance in each wavelength range (corresponding wavelength) of each base resin. The solar ultraviolet transmittance is the transmittance τ SUVA (Equation 1), the transmittance of the solar ultraviolet B region τ SUVB and (Equation 2).

number

number

[0107] In the table shown in FIG. 13A, the transmittance τ SUVA and (Equation 1), the transmittance in the solar ultraviolet B region τ SUVB Compare with.

[0108] In the results shown in FIG. 13A, the transmittance τ SUVB is 85.7%, and transmittance τ SUVA The transmittance τ of the test piece 12 (the resin for substrate 1 on which the visible light AR coating is formed) is 89.8%. SUVB is 65.0%, and transmittance τ SUVA The transmittance τ of the test piece 13 (resin 1 for substrate on which UVA visible light AR coating is formed) is 76.4%. SUVB is 78.7%, and transmittance τ SUVA is 89.7%.

[0109] In addition, for test piece 14 (resin 1 for base material with LA-63P (0.2 wt%) added), the transmittance τ SUVB is 80.9%, and transmittance τ SUVA The transmittance τ of the test piece 15 (a resin for substrate 1 with visible light AR coating on both sides and containing LA-63P (0.2 wt%)) is 85.7%. SUVB is 59.5%, and transmittance τ SUVA The transmittance τ of test piece 16 (resin 1 for substrate with UVA visible light AR coating on both sides and LA-63P (0.2 wt%) added) was 74.0%. SUVB is 72.3%, and transmittance τ SUVA is 85.2%.

[0110] In the results shown in FIG. 13B, the transmittance τ SUVB is 58.9%, and transmittance τ SUVAThe transmittance τ of the test piece 22 (the resin 2 for the substrate on which the visible light AR coating is formed) is 77.2%. SUVB is 46.6%, and transmittance τ SUVA The transmittance τ of the test piece 23 (the resin 2 for the substrate on which the UVA visible light AR coating is formed) is 68.7%. SUVB is 55.0%, and transmittance τ SUVA is 77.9%.

[0111] In addition, for test piece 24 (resin 2 for base material with LA-52 (0.2 wt%) added), the transmittance τ SUVB is 20.7%, and transmittance τ SUVA The transmittance τ of the test piece 25 (a resin for base material 2 with visible light AR coating formed on both sides and containing LA-52 (0.2 wt%)) is 55.2%. SUVB is 16.4%, and transmittance τ SUVA The transmittance τ of the test piece 26 (resin 2 for substrate with UVA visible light AR coating on both sides and LA-52 (0.2 wt%) added) was 51.7%. SUVB is 21.7%, and transmittance τ SUVA is 56.9%.

[0112] In addition, for test piece 27 (resin 2 for base material with LA-57 (0.2 wt%) added), the transmittance τ SUVB is 10.1%, and transmittance τ SUVA The transmittance τ of the test piece 28 (the resin 2 for the substrate with visible light AR coating on both sides and LA-57 (0.2 wt%) added) was 47.7%. SUVB is 8.4%, and transmittance τ SUVA The transmittance τ of test piece 29 (resin 2 for substrate with UVA visible light AR coating on both sides and LA-57 (0.2 wt%) added) was 45.2%. SUVB is 10.8%, and transmittance τ SUVA is 48.9%.

[0113] In the results shown in FIG. 13C, the transmittance τ SUVB is 11.8%, and transmittance τ SUVAThe transmittance τ of the test piece 31A (the resin 3 for the substrate on which the visible light AR coating is formed) is 47.3%. SUVB is 10.6%, and transmittance τ SUVA The transmittance τ SUVB is 11.2%, and transmittance τ SUVA is 47.9%.

[0114] In addition, for the test piece 32 (resin 3 for base material with LA-52 (0.2 wt%) added), the transmittance τ SUVB is 4.3%, and transmittance τ SUVA The transmittance τ of the test piece 32A (a resin for base material 3 with visible light AR coating formed on both sides and containing LA-52 (0.2 wt%)) is 37.5%. SUVB is 3.1%, and transmittance τ SUVA The transmittance τ of test piece 32U (resin 3 for substrate with UVA visible light AR coating on both sides and LA-52 (0.2 wt%) added) was 34.9%. SUVB is 4.5%, and transmittance τ SUVA is 38.4%.

[0115] In addition, for the test piece 33 (resin 3 for base material to which LA-52 (0.2 wt%) and LA-46 (0.001 wt%) were added), the transmittance τ SUVB is 3.2%, and transmittance τ SUVA The transmittance τ of the test piece 33A (a resin for base material 3 with visible light AR coating formed on both sides and containing LA-52 (0.2 wt%) and LA-46 (0.001 wt%)) was 32.8%. SUVB is 2.5%, and transmittance τ SUVA The transmittance τ of test piece 33U (a UVA visible light AR coating formed on both sides and base resin 3 containing LA-52 (0.2 wt%) and LA-46 (0.001 wt%)) was 31.3%. SUVB is 3.5%, and transmittance τ SUVA is 33.9%.

[0116] In the results shown in FIG. 13D, the transmittance τSUVB is 1.1%, and transmittance τ SUVA The transmittance τ of the test piece 34A (a resin for base material 3 with visible light AR coating formed on both sides and containing LA-46 (0.003 wt%)) is 23.9%. SUVB is 1.0%, and transmittance τ SUVA The transmittance τ of test piece 34U (a UVA visible light AR coating formed on both sides and base resin 3 to which LA-46 (0.003 wt%) was added) was 21.9%. SUVB is 1.1%, and transmittance τ SUVA is 24.5%.

[0117] In addition, for test piece 35 (resin 3 for base material to which LA-46 (0.005 wt%) was added), the transmittance τ SUVB is 1.0%, and transmittance τ SUVA The transmittance τ of test piece 35A (a resin for base material 3 with visible light AR coating on both sides and LA-46 (0.005 wt%) added) is 19.7%. SUVB is 0.9%, and transmittance τ SUVA The transmittance τ of test piece 35U (a UVA visible light AR coating formed on both sides and base resin 3 to which LA-46 (0.005 wt%) was added) was 17.9%. SUVB is 0.9%, and transmittance τ SUVA is 19.9%.

[0118] Fig. 14 is a table comparing the luminous transmittance of each test piece. The luminous transmittance is calculated by Equation 3 defined in JIS T7333:2018 (ISO8980-3:2013).

number

[0119] In the results shown in FIG. 14A, the luminous transmittance of test piece 11 (only base resin 1) was 92.5%, the luminous transmittance of test piece 12 (base resin 1 with visible light AR coating formed thereon) was 98.9%, and the luminous transmittance of test piece 13 (base resin 1 with UVA visible light AR coating formed thereon) was 99.7%. is 97.4%.

[0120] Furthermore, test piece 14 (base resin 1 with added LA-63P (0.2 wt%)) had a visual transmittance of 92.0%, test piece 15 (base resin 1 with visible light AR coating formed on both sides and added LA-63P (0.2 wt%)) had a visual transmittance of 98.4%, and test piece 16 (base resin 1 with added LA-63P (0.2 wt%) and UVA visible light AR coating formed on both sides) had a visual transmittance of 97.0%.

[0121] Furthermore, the visual transmittance of test piece 21 (only substrate resin 2) was 91.4%, the visual transmittance of test piece 22 (substrate resin 2 with visible light AR coating formed thereon) was 98.9%, and the visual transmittance of test piece 23 (substrate resin 2 with UVA visible light AR coating formed thereon) was 97.0%.

[0122] Furthermore, the luminous transmittance of test piece 24 (base resin 2 to which LA-52 (0.2 wt%) has been added) is 91.0%, the luminous transmittance of test piece 25 (base resin 2 to which visible light AR coating has been formed on both sides and LA-52 (0.2 wt%) has been added) is 98.5%, and the luminous transmittance of test piece 26 (base resin 2 to which UVA visible light AR coating has been formed on both sides and LA-52 (0.2 wt%) has been added) is 96.7%.

[0123] Furthermore, test piece 27 (resin 2 for base material with added LA-57 (0.2 wt%)) had a visual transmittance of 90.9%, test piece 28 (resin 2 for base material with visible light AR coating formed on both sides and added LA-57 (0.2 wt%)) had a visual transmittance of 98.4%, and test piece 29 (resin 2 for base material with added LA-57 (0.2 wt%) and UVA visible light AR coating formed on both sides) had a visual transmittance of 96.6%.

[0124] In the results shown in Figure 14B, the luminous transmittance of test piece 31 (only substrate resin 3) is 91.9%, the luminous transmittance of test piece 31A (substrate resin 3 with visible light AR coating formed thereon) is 98.4%, and the luminous transmittance of test piece 31U (substrate resin 3 with UVA visible light AR coating formed thereon) is 97.4%.

[0125] Furthermore, the visual transmittance of test piece 32 (base resin 3 with added LA-52 (0.2 wt%)) was 91.3%, the visual transmittance of test piece 32A (base resin 3 with visible light AR coating formed on both sides and added LA-52 (0.2 wt%)) was 98.1%, and the visual transmittance of test piece 32U (base resin 3 with UVA visible light AR coating formed on both sides and added LA-52 (0.2 wt%)) was 96.6%.

[0126] Furthermore, the luminous transmittance of test piece 33 (base resin 3 to which LA-52 (0.2 wt%) and LA-46 (0.001 wt%) were added) was 91.3%, the luminous transmittance of test piece 33A (base resin 3 to which visible light AR coating was formed on both sides and LA-52 (0.2 wt%) and LA-46 (0.001 wt%) were added) was 98.3%, and the luminous transmittance of test piece 33U (base resin 3 to which UVA visible light AR coating was formed on both sides and LA-52 (0.2 wt%) and LA-46 (0.001 wt%) were added) was 96.9%.

[0127] Furthermore, the visual transmittance of test piece 34 (base resin 3 with added LA-46 (0.003 wt%)) was 91.3%, the visual transmittance of test piece 34A (base resin 3 with visible light AR coating formed on both sides and added LA-46 (0.003 wt%)) was 97.6%, and the visual transmittance of test piece 34U (base resin 3 with UVA visible light AR coating formed on both sides and added LA-46 (0.003 wt%)) was 96.5%.

[0128] Furthermore, the visual transmittance of test piece 35 (base resin 3 with added LA-46 (0.005 wt%)) was 91.6%, the visual transmittance of test piece 35A (base resin 3 with visible light AR coating formed on both sides and added LA-46 (0.005 wt%)) was 98.0%, and the visual transmittance of test piece 35U (base resin 3 with UVA visible light AR coating formed on both sides and added LA-46 (0.005 wt%)) was 96.7%.

[0129] As described above, according to FIG. 13 and FIG. 14, the transmittance τ of the solar ultraviolet B region with respect to the luminous transmittance SUVB It is possible to configure a spectacle lens in which the difference in the refractive index between the two lenses is 5% or less. This condition is defined as a condition for a spectacle lens for refractive correction in JIS T7333:2018 (ISO8980-3:2013). For example, the test pieces 32 to 35, which have a UVA visible light AR coating formed on both sides, can satisfy the JIS conditions, and by manufacturing spectacle lenses processed in the same manner as these test pieces, it is possible to configure a spectacle lens for refractive correction that meets the JIS standard while being as close as possible to the state of the naked eye.

[0130] In addition, in the substrate layer or the coating film layer in the embodiment, the above-mentioned materials and other materials that are applicable to the technology disclosed herein may be appropriately used. In addition, for example, a fluorine compound resin with high transmittance, specifically HMX10 manufactured by Daikin Industries, Ltd., may also be used as the substrate.

[0131] In addition, the eyeglass lenses in the disclosed technology can be used as non-vision corrective lenses, for example. For example, they can be used as eyewear lenses with a pollen-cutting function for emmetropic users who suffer from hay fever and do not need vision correction, or as eyewear lenses with a moisture function for emmetropic users who suffer from dry eyes.

[0132] Although the present invention has been described above using various embodiments, the technical scope of the present invention is not limited to the scope described in the above embodiments. It is clear to those skilled in the art that various modifications and improvements can be made to the above embodiments. It is clear from the description of the claims that such modifications and improvements can also be included in the technical scope of the present invention.

Claims

1. The substrate layer and the coating film layer are provided. a total average UVA transmittance of the substrate layer and the coating film layer is higher than an average UVA transmittance of the substrate layer; A spectacle lens, wherein the total average UVB transmittance of the substrate layer and the coating film layer is lower than the average UVB transmittance of the substrate layer.

2. The eyeglass lens according to claim 1 , wherein the coating film layer includes an anti-reflection film layer that prevents reflection of wavelengths in the UVA region and visible light region.

3. The eyeglass lens according to claim 1 , wherein the substrate layer contains a radical scavenger and / or an ultraviolet absorbing agent.

4. The substrate layer contains a radical scavenger and / or an ultraviolet absorbing agent, The eyeglass lens according to claim 1 , wherein the coating film layer includes an anti-reflection film layer that prevents reflection of wavelengths in the UVA region and visible light region.

5. The transmittance τ of the solar ultraviolet B region relative to the luminous transmittance of the eyeglass lens SUVB 5. The spectacle lens according to claim 1, wherein the refractive index is 5% or less.

6. 5. The eyeglass lens according to claim 1, wherein a total average UVB reflectance of the base layer and the coating film layer is higher than an average UVB reflectance of the base layer.

7. The eyeglass lens according to claim 1 , wherein the coating film layer has a characteristic that the reflectance increases as the wavelength becomes shorter in a wavelength region of 280 nm or more and less than 315 nm.

8. 5. The eyeglass lens according to claim 1, wherein a difference between a total average UVA transmittance and a total average UVB transmittance of the substrate layer and the coating film layer is greater than a difference between a total average UVA transmittance and a total average UVB transmittance of the substrate layer alone, or a difference between a total average UVA transmittance and a total average UVB transmittance of the substrate layer and an anti-reflection film layer that prevents reflection of a specific wavelength in the visible light region.

9. The substrate layer and the coating film layer are provided. the total average UVA transmittance of the substrate layer and the coating film layer is approximately equal to or greater than the average UVA transmittance of the substrate layer; a total average UVB transmittance of the base layer and the coating film layer is approximately equal to or less than an average UVB transmittance of the base layer; A lens for glasses, wherein a difference between a total average UVA transmittance and a total average UVB transmittance of the substrate layer and the coating film layer is greater than a difference between a total average UVA transmittance and a total average UVB transmittance of the substrate layer alone, or a difference between a total average UVA transmittance and a total average UVB transmittance of the substrate layer and an anti-reflection film layer that prevents reflection of a specific wavelength in the visible light region.

Citation Information

Patent Citations

  • Optical component

    JP2016224192A

  • Spectacle lens material

    JP2019015922A

  • Spectacle lens for car drivers

    US20170219848A1

  • Spectacle lens and method for calculating and producing a spectacle lens

    US20190072786A1

  • Optical member

    WO2017090128A1

Cited By

  • Eyeglasses kit with corrective daytime lenses to optimize exposure to natural light and nighttime lenses with or without correction to protect against the effects of artificial light.

    FR3168991A1