Piezoelectric film element and manufacturing method thereof
The aerosol deposition method for forming thick piezoelectric films with annealing and poling treatments addresses the limitations of sputtering, enhancing power generation capacity by compensating for lower constants with increased thickness, resulting in efficient and environmentally friendly piezoelectric elements.
Patent Information
- Application Number
- JP2023055808
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional piezoelectric film elements manufactured by sputtering are limited to thin films due to slow deposition rates, high vacuum requirements, and high equipment costs, restricting their power generation capacity.
Aerosol deposition method is used to form multiple piezoelectric films with a thickness of 10 μm or more on a substrate, followed by annealing and poling treatments to enhance the piezoelectric constant, utilizing potassium sodium niobate as the piezoelectric material.
The method enables the production of thick film piezoelectric elements with increased power generation capacity, overcoming the limitations of sputtering by compensating for lower piezoelectric constants with thicker films, thus achieving power generation comparable to or exceeding that of sputtered films.
Smart Images

Figure 2024143239000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a piezoelectric film element and a method for manufacturing the same. [Background technology]
[0002] Piezoelectric film elements can generate electricity according to the amount of deformation when force is applied, and are attracting attention for use in applications such as energy harvesting. Conventional piezoelectric film elements are generally manufactured by depositing a piezoelectric film on a substrate using a sputtering method, as described in Patent Document 1, for example.
[0003] The sputtering method has a slow film formation speed (said to be a maximum of 1.0 μm / h), and requires a high vacuum environment, which makes the equipment expensive, so its application to the formation of piezoelectric films of 10 μm or more is impractical in terms of manufacturing costs. Therefore, piezoelectric film elements manufactured using the sputtering method have been limited to those with so-called thin-film type piezoelectric films with a thickness of several μm. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-023483 A Summary of the Invention [Problem to be solved by the invention]
[0005] By the way, it is known that the power generation performance of a piezoelectric film element is positively related to the thickness of the piezoelectric film, and the larger the thickness of the piezoelectric film, the greater the amount of power generated by the piezoelectric film element. For this reason, there is a demand for piezoelectric film elements with thicker piezoelectric films so that they can generate more power.
[0006] The present invention has been made in view of the above problems, and an object of the present invention is to provide a piezoelectric film element having a thickened piezoelectric film and a manufacturing method thereof.
Means for Solving the Problem
[0007] A characteristic configuration of a method for manufacturing a piezoelectric film element according to an aspect of the present invention for achieving the above object includes a step of forming a plurality of piezoelectric films having a film thickness of 10 μm or more on at least one surface of a substrate by an aerosol deposition method, and a step of annealing each of the piezoelectric films formed on the substrate.
[0008] Film formation by the aerosol deposition method has a high film formation rate (about 5 - 50 μm / min) and low equipment costs. According to the manufacturing method of the present invention, a piezoelectric film element provided with a so-called thick film type piezoelectric film having a film thickness of 10 μm or more can be easily manufactured. A piezoelectric film element provided with a plurality of such thickened piezoelectric films can ensure a larger amount of generated electricity.
[0009] In addition, although crystal defects and strains are introduced into the piezoelectric film formed by the aerosol deposition method during the film formation process, the piezoelectric constant increases by removing these defects and strains by annealing treatment. That is, according to the manufacturing method of the present invention, a piezoelectric film element having a high piezoelectric constant of the piezoelectric film can be manufactured, and thereby, a piezoelectric film element capable of ensuring an even larger amount of generated electricity can be manufactured.
[0010] A further characteristic configuration of the method for manufacturing a piezoelectric film element according to the present invention is that each of the piezoelectric films is made of potassium sodium niobate.
[0011] Lead zirconate titanate (Pb(Zr,Ti)O 3 : PZT), which is widely used as a material for piezoelectric films, has a very high piezoelectric constant, which is one of the factors affecting the amount of generated electricity of the piezoelectric film. However, it is being strictly regulated because it contains a high concentration of lead, which is a substance harmful to the environment and the human body. In contrast, potassium sodium niobate (K 1-x Na x NbO 3 , 0 < x < 1: KNN) is a lead-free piezoelectric material. According to the manufacturing method of the present invention, a piezoelectric film element with a low environmental impact can be obtained.
[0012] A further characteristic feature of the method for manufacturing a piezoelectric film element according to the present invention is that it further includes a step of subjecting each of the annealed piezoelectric films to a poling treatment.
[0013] The piezoelectric film formed by the aerosol deposition method has a higher piezoelectric constant when the direction of polarization is aligned in one direction by a poling process in which an electric field is applied. In other words, the manufacturing method according to the present invention makes it possible to manufacture a piezoelectric film element having a high piezoelectric constant and thus capable of generating even more electricity.
[0014] A further characteristic feature of the manufacturing method of the piezoelectric film element according to the present invention is that each of the piezoelectric films is heated to 500°C to 850°C in the annealing treatment.
[0015] By carrying out the annealing treatment under the above conditions, a piezoelectric film exhibiting a high piezoelectric constant can be obtained.
[0016] A further characteristic feature of the manufacturing method of the piezoelectric film element according to the present invention is that in the poling treatment, a voltage of 40 kV / cm to 50 kV / cm is applied to each of the piezoelectric films at 0° C. to 150° C. for 10 to 30 minutes.
[0017] By carrying out the poling treatment under the above conditions, a piezoelectric film exhibiting a high piezoelectric constant can be obtained.
[0018] A further characteristic feature of the manufacturing method of the piezoelectric film element according to the present invention is that a plurality of the piezoelectric films are formed on each of both sides of the substrate.
[0019] According to the above-mentioned characteristic configuration of the present invention, the area of the substrate can be effectively utilized to provide more piezoelectric films, so that the amount of power generated by the entire piezoelectric film element can be increased.
[0020] In order to achieve the above-mentioned object, a characteristic configuration of a piezoelectric film element according to one embodiment of the present invention is that it comprises a substrate and a plurality of piezoelectric films formed on at least one side of the substrate, and each of the piezoelectric films is an aerosol deposition film having a thickness of 10 μm or more.
[0021] Compared with a sputtering film, an aerosol deposition film can form a film at a high speed using relatively low-cost equipment, so it is easy to increase the film thickness. By adopting an aerosol deposition film as the piezoelectric film, a piezoelectric film element having a so-called thick film type piezoelectric film with a film thickness of 10 μm or more can be easily obtained. According to the piezoelectric film element according to the present invention having a plurality of such thickened piezoelectric films, more power generation can be ensured.
[0022] A further characteristic configuration of the piezoelectric film element according to the present invention is that each of the piezoelectric films is made of potassium sodium niobate.
[0023] Potassium sodium niobate (K 1-x Na x NbO 3 , 0 < x < 1: KNN) is a lead-free piezoelectric material. According to the above characteristic configuration of the present invention, a piezoelectric film element with a low environmental load can be obtained.
[0024] A further characteristic configuration of the piezoelectric film element according to the present invention is that the piezoelectric constant d of each of the piezoelectric films 33 is less than 100 pC / N.
[0025] The aerosol deposition film tends to have a lower piezoelectric constant compared to a sputtering film made of the same piezoelectric material. When the piezoelectric material is KNN, the piezoelectric constant d of the sputtering film 33 is about 110, whereas the piezoelectric constant of the aerosol deposition film is less than 100.
[0026] When an aerosol deposition film with a low piezoelectric constant is adopted, usually the power generation of the piezoelectric film element is low. However, as described above, the aerosol deposition film is easy to thicken. Therefore, the piezoelectric film element according to the present invention can ensure a power generation equivalent to or higher than that of the sputtering film by increasing the film thickness of the aerosol deposition film.
[0027] A further characteristic feature of the piezoelectric film element according to the present invention is that a plurality of the piezoelectric films are formed on each of both sides of the substrate.
[0028] According to the above-mentioned characteristic configuration of the present invention, the area of the substrate can be effectively utilized to provide more piezoelectric films, so that the amount of power generated by the entire piezoelectric film element can be increased. [Brief description of the drawings]
[0029] [Figure 1] 1 is a plan view showing a piezoelectric film element according to the present invention. [Diagram 2] 1 is a cross-sectional view showing a piezoelectric film element according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] Hereinafter, the piezoelectric film element and the manufacturing method thereof according to the present invention will be specifically described using embodiments.
[0031] <Piezoelectric film element> As shown in FIGS. 1 and 2, a piezoelectric film element 10 according to one embodiment of the present invention includes a substrate 11 and a piezoelectric film 12 formed on the substrate 11. The piezoelectric film 12 is a piezoelectric material.
[0032] The substrate 11 is preferably made of a resin such as polyimide or a metal such as titanium or stainless steel, and has a thickness of 0.1 mm or more and 2 mm or less. However, the present invention is not limited to this, and substrates made of other materials or having thicknesses outside the above ranges can also be used. In this embodiment, the substrate 11 is rectangular in plan view, and a plurality of piezoelectric films 12 each having a rectangular shape in plan view are arranged in parallel on each of both sides of the substrate 11 with their long sides facing each other. However, the substrate 11 and the piezoelectric film 12 may be of other shapes, and the piezoelectric film 12 may be provided on only one side of the substrate 11.
[0033] The piezoelectric film 12 is an aerosol deposition film with a film thickness of 10 μm or more, which is formed on the substrate 11 by the aerosol deposition (AD) method. The film thickness of the piezoelectric film 12 can be set to any value within the range (~1 mm) that can be formed by the aerosol deposition method. For example, it can be 10 μm, 30 μm, 40 μm, 100 μm, etc.
[0034] In this embodiment, the piezoelectric film 12 is formed using potassium sodium niobate (K 1-x Na x NbO 3 , 0 < x < 1: KNN). However, the present invention is not limited to this, and any material that can form a piezoelectric film with a film thickness of 10 μm or more by the aerosol deposition method can be used. For example, oxide materials having piezoelectric properties such as barium titanate (BaTiO 3 ), lithium niobate (LiNbO 3 ) can be used.
[0035] The piezoelectric film formed by the aerosol deposition method tends to have a lower piezoelectric constant than the piezoelectric film formed by the sputtering method. When the piezoelectric material is KNN, the piezoelectric constant d 33 of the piezoelectric film formed by the sputtering method is about 110 pC / N, while the piezoelectric constant d 33 of the piezoelectric film formed by the aerosol deposition method varies depending on the film formation conditions but is basically less than 100 pC / N. That is, in this embodiment, the piezoelectric film 12 has a piezoelectric constant d 33 less than 100 pC / N.
[0036] Although not shown in FIG. 2, the piezoelectric film element 10 may further include a lower electrode formed on the surface of each piezoelectric film 12 on the side of the substrate 11, and an upper electrode formed on the surface of each piezoelectric film 12 opposite to the substrate 11. As the materials of the lower electrode and the upper electrode, any conductive material can be used. For example, a metal (such as a laminate of Pt / Ti) or a metal oxide can be used. When the substrate 11 is made of metal, the piezoelectric film element 10 further includes an insulating layer provided between the substrate 11 and the lower electrode.
[0037] <Manufacturing method of piezoelectric film element> Next, a method for manufacturing the piezoelectric film element 10 described above will be described. First, a piezoelectric film 12 having a thickness of 10 μm or more is formed on a substrate 11 by an aerosol deposition method. In the film formation by the aerosol deposition method, a powder of KNN having the same composition as the desired piezoelectric film 12 is used as a raw material, and an aerosol in which the powder raw material is dispersed in a carrier gas is sprayed onto the substrate 11. As a result, a piezoelectric film 12 made of KNN is formed on the substrate 11. The film thickness of the piezoelectric film 12 can be controlled by adjusting the film formation time, for example. Note that the multiple piezoelectric films 12 may be formed one by one in order, or may be simultaneously formed by scanning the nozzle over the substrate 11 with a mask having slits in the number corresponding to the piezoelectric films 12, placed between the substrate 11 and the nozzle.
[0038] Next, an annealing process is performed on each piezoelectric film 12 formed on the substrate 11. In the annealing process, the piezoelectric film 12 is heated at a predetermined temperature for a predetermined time. This removes crystal defects and distortions introduced during the film formation process of the piezoelectric film 12, and increases the piezoelectric constant of the piezoelectric film 12. The annealing temperature is preferably 500°C to 850°C, and can be, for example, 600°C, 700°C, or 800°C. The holding time of the annealing process is preferably 10 minutes to 120 minutes, and can be, for example, 30 minutes or 60 minutes.
[0039] Although not necessarily required, a poling process may be further performed on each of the annealed piezoelectric films 12. In the poling process, a predetermined voltage is applied to the piezoelectric film 12 at a predetermined temperature for a predetermined time. This aligns the polarization direction in one direction, and increases the piezoelectric constant of the piezoelectric film 12. The temperature of the poling process is preferably 0°C to 150°C, and can be, for example, 140°C or 150°C. The voltage of the poling process is preferably 40 kV / cm to 50 kV / cm, and can be, for example, 40 kV / cm, 45 kV / cm, or 50 kV / cm. The time of the poling process is preferably 10 minutes to 30 minutes, and can be, for example, 10 minutes or 20 minutes.
[0040] <Effects of the embodiment> The piezoelectric film element 10 according to the present invention employs a piezoelectric film 12 formed by the aerosol deposition method, which has a lower piezoelectric constant than a piezoelectric film formed by the sputtering method, and therefore generates less power. However, the piezoelectric film 12 formed by the aerosol deposition method can be formed at a high speed (approximately 5 to 50 μm / min) and can be easily thickened to a thickness of 10 μm or more. Therefore, the decrease in the amount of power generated due to the low piezoelectric constant can be compensated for by the increase in the amount of power generated by the thickening of the piezoelectric film 12. In other words, according to the piezoelectric film element 10 of the present invention, by increasing the thickness of the piezoelectric film 12, it is possible to ensure an amount of power generated that is equal to or higher than that of a piezoelectric film formed by sputtering.
[0041] For example, the amount of power generated by each piezoelectric film of the piezoelectric film element can be calculated using the following formulas 1 and 2. V∝d×t×X / A (Formula 1) In Equation 1, V is the electromotive force of the piezoelectric film, d is the piezoelectric constant of the piezoelectric film, t is the film thickness of the piezoelectric film, X is the stress applied to the piezoelectric film, and A is the cross-sectional area of the piezoelectric film. P=V 2 / 2R (Formula 2) In Equation 2, P is the amount of power generated, and R is the resistance value of the load resistor connected to the piezoelectric film element.
[0042] As shown in formula 1, both the piezoelectric constant d and film thickness t are proportional to the electromotive force V. Therefore, for example, in the case of a piezoelectric film of the same thickness produced by aerosol deposition, which has a piezoelectric constant 1 / 3 of that of a piezoelectric film produced by sputtering, the power generation amount P calculated based on formula 2 is 1 / 9 of that of a piezoelectric film produced by sputtering. Nevertheless, if the film thickness t of the piezoelectric film produced by aerosol deposition is made three times larger, the power generation amount P will be equal to or greater than that of a piezoelectric film produced by sputtering. EXAMPLES
[0043] The piezoelectric film element and the manufacturing method thereof according to the present invention will be specifically described below with reference to examples.
[0044] Example 1: Evaluation of the effect of manufacturing conditions on the piezoelectric constant (Production Example 1) The substrate was made of Ti and had a thickness of 0.5 mm, and the raw material powder had a composition of KNN and an average particle size of 1 μm. The raw material powder was sprayed onto the surface of the substrate by the aerosol deposition method to form a piezoelectric film with a thickness of 40 μm. The conditions for film formation were as follows. The piezoelectric film element thus produced was designated as Production Example 1. Deposition chamber vacuum degree: 650Pa Carrier gas: Air Gas flow rate: 90L / min Nozzle scan speed: 4mm / sec
[0045] (Production Example 2) The piezoelectric film of the piezoelectric film element of Production Example 1 was further subjected to a poling treatment in which a voltage of 40 kV / cm was applied for 20 minutes at 140° C. The piezoelectric film element thus produced was designated Production Example 2.
[0046] (Production Example 3) The piezoelectric film of the piezoelectric film element of Production Example 1 was further subjected to an annealing treatment in an air atmosphere at a heating temperature of 600° C. for a holding time of 60 minutes.
[0047] (Production Example 4) The piezoelectric film of the piezoelectric film element of Production Example 3 was further subjected to a poling treatment in which a voltage of 40 kV / cm was applied for 20 minutes at 140° C. The piezoelectric film element thus produced was designated Production Example 4.
[0048] (Production Example 5) The piezoelectric film of the piezoelectric film element of Production Example 1 was further subjected to an annealing treatment in an air atmosphere at a heating temperature of 700° C. for a holding time of 60 minutes.
[0049] (Production Example 6) The piezoelectric film of the piezoelectric film element of Production Example 5 was further subjected to a poling treatment in which a voltage of 40 kV / cm was applied for 20 minutes at 140° C. The piezoelectric film element thus produced was designated Production Example 6.
[0050] (Production Example 7) A piezoelectric film element was manufactured under the same conditions as in Manufacturing Example 5, except that a substrate made of SUS445 was used and the film formation time was adjusted so that the thickness of the piezoelectric film was 20 μm. This was Manufacturing Example 7.
[0051] For the piezoelectric film elements of Manufacturing Examples 1 to 7, the piezoelectric constant d 33 was measured and listed in Table 1. For comparison, Table 1 also lists the piezoelectric constant of a KNN piezoelectric film (conventional example 1) formed to a thickness of 3 μm by sputtering, and the piezoelectric constant of a PZT piezoelectric film (conventional example 2) formed to a thickness of 3 μm by sputtering. The piezoelectric constants of these comparative examples are generally known values. [Table 1]
[0052] For the piezoelectric film elements of Production Examples 5 and 7, the elements contained in the piezoelectric film were further analyzed by a known method, and the results are shown in Table 2. [Table 2]
[0053] From Table 1, it was found that the piezoelectric constants of the piezoelectric films of the piezoelectric film elements of Production Examples 3 and 5, which were annealed, were increased compared to the piezoelectric film element of Production Example 1, which was not annealed, and the increase in the piezoelectric constant was greater with annealing at 700° C. than with annealing at 600° C. It was also found that the piezoelectric film elements of Production Examples 4 and 6, which were subjected to poling in addition to annealing, further increased the piezoelectric constant of the piezoelectric film.
[0054] Also, from Table 1, it was found that the aerosol deposition method can form a piezoelectric film that has a lower piezoelectric constant but can be made thicker for practical use, compared to the sputtering method. Therefore, according to the piezoelectric film element of the present invention manufactured by the aerosol deposition method, the decrease in the amount of power generated due to the low piezoelectric constant can be compensated for by the increase in the amount of power generated due to the thickening of the piezoelectric film. For example, in the case of the piezoelectric film element of Manufacturing Example 6, based on the above formulas 1 and 2, the contribution of the piezoelectric constant of the piezoelectric film to the amount of power generated is about 1 / 11 of that of Conventional Example 1, but the contribution of the thickness of the piezoelectric film to the amount of power generated is about 177 times or more than that of Conventional Example 1. Therefore, it is considered that the piezoelectric film element of Manufacturing Example 6 has an amount of power generated that is greater than that of Conventional Example 1. It is noted that the piezoelectric film element of Manufacturing Example 6 has a greater amount of power generated than that of Conventional Example 2. It is considered that the other manufacturing examples with a lower piezoelectric constant than Manufacturing Example 6 can also have an amount of power generated that is greater than that of the conventional example by making the piezoelectric film thicker.
[0055] Furthermore, from Tables 1 and 2, it was found that in both the piezoelectric film elements of Production Example 5 and Production Example 7, which were annealed at 700°C, elements derived from the substrate were diffused into the piezoelectric film, but the piezoelectric constant of the piezoelectric film element of Production Example 7, which used a substrate made of SUS445, could not be evaluated. This is because when Fe and Cr, which are components of stainless steel, diffuse into the film side, a short circuit occurs due to the electronic conductivity derived from the transition metal. In contrast, even if Ti diffuses into the film side, it does not develop electronic conductivity, so it does not short circuit. In addition, in the case of Production Example 7, no electromotive force is generated, so the amount of power generation is zero. Therefore, it is preferable to use a substrate made of Ti.
[0056] <Example 2: Evaluation of power generation amount of piezoelectric film element> In this example, we assumed that a piezoelectric film element was attached to the inner circumference of a vehicle tire as a power generation device, generating electricity through the rotation of the tire and supplying it to other devices (such as a tire pressure sensor), and evaluated the amount of power generated by the piezoelectric film element.
[0057] (Sample 1) A polyimide substrate with a short side length of 40 mm, a long side length of 60 mm, and a thickness of 3 mm was prepared. Ten KNN piezoelectric films with a short side length of 3.1 mm, a long side length of 30 mm, and a thickness of 100 μm were formed on each of both sides of the substrate by an aerosol deposition method. The conditions during film formation, and the conditions for the annealing and poling treatments after film formation were the same as those in Manufacturing Example 6. The ten piezoelectric films on each side of the substrate were arranged in parallel along the short side direction of the substrate so that the long side direction of each piezoelectric film was aligned with the long side direction of the substrate, and the center of the long side direction of each piezoelectric film was located at the center of the long side direction of the substrate (see FIG. 1). An electrode made of a Pt / Ti laminate was formed on the entire surface of each piezoelectric film facing the substrate and the surface of each piezoelectric film opposite the substrate by an aerosol deposition method, and the thickness of the electrode was 0.1 μm. The piezoelectric film element manufactured in this manner was designated Sample 1.
[0058] (Samples 2-4) On the same substrate as Sample 1, a PZT piezoelectric film and an electrode made of a Pt / Ti laminate were formed by sputtering in the same arrangement as Sample 1. The thicknesses of the piezoelectric films were 1 μm, 3 μm, and 5 μm, and the thickness of the electrodes was 0.1 μm. The piezoelectric film elements manufactured in this way were designated Samples 2 to 4.
[0059] (Samples 5-7) On the same substrate as Sample 1, a KNN piezoelectric film and an electrode made of a Pt / Ti laminate were formed by sputtering in the same arrangement as Sample 1. The thicknesses of the piezoelectric films were 1 μm, 3 μm, and 5 μm, and the thickness of the electrodes was 0.1 μm. The piezoelectric film elements manufactured in this way were Samples 5 to 7.
[0060] The amount of electricity generated by each piezoelectric film for each sample was calculated based on the above formulas 1 and 2. The stress X was determined as the maximum stress (stress below the destruction limit of the piezoelectric film) when the center of the long side of the substrate was displaced by 1.42 mm, assuming that the deformation of the tire due to contact with the ground was 1.42 mm. The total amount of electricity generated by the 20 piezoelectric films was calculated as the amount of electricity generated by the piezoelectric film element. [Table 3]
[0061] A power generating device for energy harvesting is generally required to generate approximately 1 mW of power. From Table 3, it can be seen that the power generating capacity of the piezoelectric film elements of Samples 2 to 7, which have a thin-film type piezoelectric film of 5 μm or less formed by a sputtering method, is significantly less than 1 mW, whereas the piezoelectric film element of Sample 1, which has a thick-film type piezoelectric film of 100 μm formed by an aerosol deposition method, can realize a power generating capacity close to 1 mW. Since it is believed that the power generating capacity will increase further if the number of piezoelectric films is increased, it was found that the manufacturing method according to the present invention can manufacture a power generating film element that can be used as a power generating device for energy harvesting. [Explanation of symbols]
[0062] 10 Piezoelectric film element 11 Substrate 12 Piezoelectric film
Claims
1. forming a plurality of piezoelectric films having a thickness of 10 μm or more on at least one surface of a substrate by an aerosol deposition method; and a step of annealing each of the piezoelectric films formed on the substrate.
2. The method for manufacturing a piezoelectric film element according to claim 1 , wherein each of said piezoelectric films is made of potassium sodium niobate.
3. The method for manufacturing a piezoelectric film element according to claim 2 , further comprising a step of poling each of the annealed piezoelectric films.
4. 2. The method for manufacturing a piezoelectric film element according to claim 1, wherein the piezoelectric films are heated to 500° C. to 850° C. in the annealing process.
5. 4. The method for manufacturing a piezoelectric film element according to claim 3, wherein the poling treatment involves applying a voltage of 40 kV / cm to 50 kV / cm to each of the piezoelectric films at 0° C. to 150° C. for 10 minutes to 30 minutes.
6. The method for manufacturing a piezoelectric film element according to claim 1 , wherein the piezoelectric film is formed in a plurality of films on each of both sides of the substrate.
7. A substrate; a plurality of piezoelectric films formed on at least one surface of the substrate; Each of the piezoelectric films is an aerosol deposition film having a thickness of 10 μm or more.
8. 8. The piezoelectric film element according to claim 7, wherein each of said piezoelectric films is made of potassium sodium niobate.
9. The piezoelectric constant d of each of the piezoelectric films 33 The piezoelectric film element according to claim 8, wherein the resistivity is less than 100 pC / N.
10. The piezoelectric film element according to claim 7 , wherein a plurality of the piezoelectric films are formed on each of both sides of the substrate.
Citation Information
Patent Citations
Piezoelectric film manufacturing method, vibration piece, vibrator, oscillator, electronic equipment, and movable body
JP2015023483A