Medical device and method for manufacturing the same

A laminated medical device with a plastic base and adhesive/biocompatible layers using specific monomers addresses the challenge of maintaining antithrombotic properties by preventing polymer aggregation and ensuring a smooth surface, thereby enhancing the durability of antithrombotic performance.

JP2024143544AInactive Publication Date: 2024-10-11TERUMO KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023056279
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing medical devices face challenges in maintaining antithrombotic properties over a long period due to mechanical stress and inferior mobility between base materials and antithrombotic coatings, leading to potential thrombosis, especially in small-diameter implants like artificial blood vessels and stent grafts.

Method used

A medical device with a laminated structure comprising a plastic base material, a first layer derived from a monomer with an epoxy group and a monomer with a low glass transition temperature, and a second layer containing an antithrombotic monomer, where the first layer acts as an adhesive layer to firmly fix the biocompatible layer, preventing aggregation and ensuring a smooth surface.

Benefits of technology

The device maintains excellent antithrombotic properties by suppressing polymer aggregation and ensuring a smooth surface, reducing mechanical stress, and enhancing the longevity of antithrombotic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143544000016
    Figure 2024143544000016
  • Figure 2024143544000017
    Figure 2024143544000017
  • Figure 2024143544000018
    Figure 2024143544000018
Patent Text Reader

Abstract

To provide a medical device having an adhesive layer containing a polymer having an epoxy group between a substrate and a layer containing an antithrombogenic material, which has excellent antithrombotic properties.SOLUTION: There is provided a medical device comprising: a plastic substrate; a first layer supported on at least a part of the plastic substrate; and a second layer supported on at least a part of the first layer, wherein the first layer contains a first copolymer having a constituent unit (A-1) derived from a monomer (a-1) having an epoxy group and a constituent unit (A-2) derived from a monomer (a-2) whose homopolymer has a glass transition temperature less than -10°C and the second layer contains a second copolymer having a constituent unit (B-1) derived from a monomer (b-1) capable of bonding to an epoxy group contained in the constituent unit (A-1) and a constituent unit (B-2) derived from an antithrombogenic monomer (b-2).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a medical device and a method for producing the same. [Background technology]

[0002] In recent years, medical materials using various polymeric materials have been studied, and their use in artificial kidney membranes, plasma separation membranes, catheters, stents, artificial lung membranes, artificial blood vessels, adhesion prevention membranes, artificial skin, etc. is expected. In these applications, synthetic polymeric materials, which are foreign bodies to the living body, are used in contact with biological tissues and body fluids such as blood. Therefore, medical materials are required to be biocompatible. The biocompatibility required of medical materials varies depending on the purpose and method of use, but medical materials used as materials that come into contact with blood are required to have the properties of suppressing the blood coagulation system, inhibiting platelet adhesion and activation, and inhibiting the activation of the complement system (antithrombotic properties).

[0003] Usually, antithrombotic properties are imparted to a medical device by coating the base material constituting the medical device with an antithrombotic material or by fixing an antithrombotic material to the surface of the base material. For example, Patent Document 1 discloses a medical device having a synthetic polymer (antithrombotic material) on the surface of the base material, which simultaneously satisfies biocompatibility such as inhibition of platelet adhesion and activation, inhibition of activation of the complement system, and affinity with tissues in the body. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 4-152952 Summary of the Invention [Problem to be solved by the invention]

[0005] The invention disclosed in Patent Document 1 shows good results in terms of inhibiting platelet adhesion and activation.

[0006] In order to maintain excellent antithrombotic properties for a long period of time, some of these medical devices are required to be able to retain the antithrombotic material on the substrate for a long period of time (i.e., to form an antithrombotic coating with excellent durability).

[0007] For example, in implantable medical devices (especially those with small diameters) such as artificial blood vessels, stent grafts, and covered stents, there is a tendency for patency to decrease due to stenosis or occlusion, and therefore it is particularly required to maintain antithrombotic properties over a long period of time. However, some of the base materials used in medical devices have inferior mobility (flexibility) compared to antithrombotic materials, and mechanical stress is easily applied between such base materials and the antithrombotic material, resulting in difficulty in maintaining antithrombotic properties over a long period of time.

[0008] Therefore, the present inventors have conducted extensive research with the aim of forming an antithrombogenic coating with excellent durability, and have investigated a technology for retaining (firmly fixing) an antithrombogenic material on a substrate for a long period of time by forming an appropriate adhesive layer between the antithrombogenic material (also referred to as an "antithrombogenic material layer") and the substrate.

[0009] In the course of their investigations, the inventors conducted extensive research into materials for forming the adhesive layer, and concluded that by forming an adhesive layer using a polymer having an epoxy group, it might be possible to firmly support (fix) the antithrombotic material onto the substrate.

[0010] However, in the course of the above investigations, it was found that when an adhesive layer was formed using a polymer having an epoxy group, sufficient antithrombotic properties were not always obtained.

[0011] Therefore, the present invention has been made in consideration of the above circumstances, and has an object to provide a medical device having excellent antithrombogenicity, which is a medical device having an adhesive layer containing a polymer having an epoxy group between a substrate and a layer containing an antithrombogenic material. Another object of the present invention is to provide a method for producing the above medical device. [Means for solving the problem]

[0012] The present inventors have conducted extensive research to solve the above problems, and as a result, have found that in a medical device in which a substrate, a first layer, and a second layer are laminated in this order, the above problems can be solved by each copolymer contained in the first layer and the second layer having a constitutional unit derived from a specific monomer, thereby completing the present invention.

[0013] That is, the above objects can be achieved by the present invention having the following configuration, and the present invention includes the following aspects and configurations.

[0014] One aspect of the present invention is 1. A medical device comprising a plastic substrate, a first layer supported on at least a portion of the plastic substrate, and a second layer supported on at least a portion of the first layer, the first layer comprises a first copolymer having a structural unit (A-1) derived from a monomer (a-1) having an epoxy group and a structural unit (A-2) derived from a monomer (a-2) having a homopolymer glass transition temperature of less than −10° C.; The second layer is a medical device comprising a second copolymer having a structural unit (B-1) derived from a monomer (b-1) capable of bonding with an epoxy group contained in the structural unit (A-1) and a structural unit (B-2) derived from an antithrombotic monomer (b-2).

[0015] 2. In the medical device described in 1 above, the monomer (a-2) is represented by the following formula (I):

[0016] [ka]

[0017] In the above formula (I), R 1 represents a hydrogen atom or a methyl group, and X 1 -O-(R 2 O) m -R 3or a tetrahydrofurfuryloxy group, R 2 each independently represents a linear or branched alkylene group having 1 to 4 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 4 carbon atoms, and m represents an integer of 1 to 5; It is preferable that the monomer is one or more selected from the monomers represented by the following formula:

[0018] 3. In the medical device described in 2 above, the monomer (a-2) is represented by the formula (I), R 1 represents a hydrogen atom or a methyl group, and X 1 -O-(R 2 O) m -R 3 R 2 represents a linear or branched alkylene group having 1 to 4 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 4 carbon atoms, and m is 1;

[0019] 4. In the medical device described in any one of 1. to 3. above, the epoxy group-containing monomer (a-1) preferably includes at least one selected from the group consisting of glycidyl acrylate, glycidyl methacrylate (GMA), 3,4-epoxycyclohexylmethyl acrylate, 3,4-epoxycyclohexylmethyl methacrylate, β-methylglycidyl acrylate, and β-methylglycidyl methacrylate.

[0020] 5. In the medical device described in any one of 1. to 4. above, the first copolymer is preferably a random copolymer having a segment having the structural unit (A-1) and a segment having the structural unit (A-2).

[0021] 6. In the medical device described in any one of 1. to 5. above, it is preferable that the first copolymer contains the structural unit (A-1) and the structural unit (A-2) in a molar ratio ((A-1):(A-2)) of 2:8 to 6:4.

[0022] 7. In the medical device described in any one of 1. to 6. above, the monomer (b-1) preferably contains at least one functional group selected from the group consisting of a primary amino group (-NH2), a carboxyl group (-COOH), and a hydroxyl group (-OH).

[0023] 8. In the medical device according to any one of 1. to 7. above, the monomer (b-1) is preferably one or more selected from monomers represented by the following formula (II) and the following formula (III) and salts thereof:

[0024] [ka]

[0025] In the above formula (II), R 4 represents a hydrogen atom or a methyl group, p represents an integer from 1 to 4;

[0026] [ka]

[0027] In the above formula (III), R 5 represents a hydrogen atom or a methyl group, q represents an integer of 1 to 4.

[0028] 9. In the medical device according to any one of the above items 1. to 8., the antithrombotic monomer (b-2) is represented by the following formula (IV):

[0029] [ka]

[0030] In the above formula (IV), R 6 represents a hydrogen atom or a methyl group, and X 2 -O-(R 7 O) n -R 8 or a tetrahydrofurfuryloxy group, R 7 each independently represents a linear or branched alkylene group having 1 to 4 carbon atoms; R 8 represents a linear or branched alkyl group having 1 to 4 carbon atoms, and n represents an integer of 1 to 5; It is preferable that the monomer is one or more selected from the monomers represented by the following formula:

[0031] 10. In the medical device according to any one of the above 1. to 9., the antithrombotic monomer (b-2) is preferably the same as the monomer (a-2).

[0032] 11. In the medical device according to any one of the above 1. to 10., the first copolymer preferably has a total content of the structural units (A-1) and (A-2) of 95 mol % or more.

[0033] 12. In the medical device according to any one of the above 1. to 11., the second copolymer preferably has a total content of the structural units (B-1) and (B-2) of 95 mol % or more.

[0034] 13. In the medical device according to any one of 1. to 12. above, the plastic is preferably at least one selected from the group consisting of polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), and polybutylene terephthalate (PBT).

[0035] 14. In the medical device according to any one of the above items 1. to 13, the medical device is preferably an artificial blood vessel, a stent graft, a covered stent or a catheter.

[0036] Another aspect of the present invention is 15. Contacting at least a portion of the plastic substrate with the first copolymer to form the first layer; and A method for producing the medical device according to any one of 1. to 14. above, comprising contacting at least a portion of the first layer with the second copolymer to form the second layer.

[0037] 16. The method for producing a medical device as described in 15 above preferably further comprises irradiating the plastic substrate with plasma before contacting the plastic substrate with the first copolymer. Effect of the Invention

[0038] According to the present invention, it is possible to provide a medical device having an adhesive layer containing a polymer having an epoxy group between a substrate and a layer containing an antithrombogenic material, and thus having excellent antithrombogenicity. [Brief description of the drawings]

[0039] [Figure 1] FIG. 1 is a partial cross-sectional view that illustrates a schematic representation of a layered structure on the surface of a representative embodiment of a medical device according to the present invention. [Diagram 2] FIG. 2 is a partial cross-sectional view showing a schematic example of a different surface layer structure as an application example of the embodiment of FIG. [Diagram 3] FIG. 3 is an SEM image of the first layer (adhesive layer) of the sample obtained in Production Example 1, observed with a scanning electron microscope. [Figure 4] FIG. 4 is an SEM image of the first layer (adhesive layer) of the sample obtained in Production Example 2, observed with a scanning electron microscope. [Diagram 5] FIG. 5 is an SEM image of the first layer (adhesive layer) of the sample obtained in Production Example 3, observed with a scanning electron microscope. [Figure 6]FIG. 6 is an SEM image of the first layer (adhesive layer) of the sample obtained in Production Example 4, observed with a scanning electron microscope. [Figure 7] FIG. 7 is an SEM image of the first layer (adhesive layer) of the sample obtained in Comparative Production Example 1, observed with a scanning electron microscope. [Figure 8] FIG. 8 is an SEM image of the first layer (adhesive layer) of the sample obtained in Comparative Production Example 2, observed with a scanning electron microscope. [Figure 9] FIG. 9 is an SEM image of the first layer (adhesive layer) of the sample obtained in Comparative Production Example 3, observed with a scanning electron microscope. [Figure 10] FIG. 10 is an SEM image of the first layer (adhesive layer) of the sample obtained in Comparative Production Example 4, observed with a scanning electron microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0040] The present invention provides a medical device comprising a plastic substrate, a first layer supported on at least a part of the plastic substrate, and a second layer supported on at least a part of the first layer, the first layer comprising a first copolymer having a structural unit (A-1) derived from a monomer (a-1) having an epoxy group and a structural unit (A-2) derived from a monomer (a-2) having a homopolymer glass transition temperature of less than -10°C, and the second layer comprising a second copolymer having a structural unit (B-1) derived from a monomer (b-1) capable of bonding with an epoxy group contained in the structural unit (A-1) and a structural unit (B-2) derived from an antithrombotic monomer (b-2). Hereinafter, the medical device having the above structure is also referred to simply as "the medical device according to the present invention" or "medical device". The first layer may also be referred to as an "adhesive layer", and the second layer may also be referred to as a "biocompatible layer" or "antithrombotic material layer".

[0041] The medical device of the present invention is a medical device comprising a plastic substrate, a first layer, and a second layer laminated in this order, wherein (1) the first copolymer contained in the first layer has a structural unit (A-1) derived from a monomer (a-1) having an epoxy group and a structural unit (A-2) derived from a monomer (a-2) having a homopolymer glass transition temperature of less than -10°C, and (2) the second copolymer contained in the second layer has a structural unit (B-1) derived from a monomer (b-1) capable of bonding to the epoxy group contained in the structural unit (A-1), and a structural unit (B-2) derived from an antithrombotic monomer (b-2).

[0042] The present inventors have surprisingly found that a medical device having such a configuration has excellent antithrombotic properties (that is, it can effectively inhibit the adhesion of proteins, cells, etc. that can form thrombi).

[0043] The mechanism by which the present invention provides the above-mentioned effects is believed to be as follows.

[0044] The medical device according to the present invention has an adhesive layer (first layer) between the substrate and the biocompatible layer (second layer). The present inventors first considered that the adhesive layer could be formed using a polymer having an epoxy group, thereby allowing the biocompatible layer (second layer) to be maintained (strongly fixed) on the substrate for a long period of time. Specifically, they speculated that the epoxy group contained in the adhesive layer could act as a reactive group, thereby allowing the biocompatible layer (second layer) to be more firmly fixed on the substrate. However, when the adhesive layer (first layer) was formed using a polymer having an epoxy group, there were cases where sufficient antithrombotic properties were not obtained. Then, the present inventors investigated the cause of this in detail, and came to the hypothesis that such a decrease in antithrombotic properties was due to the polymer having an epoxy group agglomerating on the substrate. In this way, when the polymer constituting the adhesive layer (first layer) agglomerates, unevenness is formed on the surface of the adhesive layer (first layer) (i.e., the surface is not smooth). This will then result in unevenness on the surface of the biocompatible layer (second layer) placed on the adhesive layer (first layer), and it is presumed that these uneven areas will make it easier for blood clots to form.

[0045] Therefore, the present inventors have further studied to suppress the aggregation of the polymer constituting the adhesive layer (first layer). As a result, it has been found that the above-mentioned aggregation can be effectively suppressed by having a structural unit (A-2) derived from a monomer (a-2) having a homopolymer glass transition temperature of less than -10°C in addition to the structural unit (A-1) derived from a monomer (a-1) having an epoxy group in the polymer (first copolymer) forming the adhesive layer (first layer). Thus, by having a structural unit (A-2) derived from a monomer (a-2) having a glass transition temperature of less than -10°C in addition to the structural unit (A-1), the glass transition temperature of the polymer (first copolymer) forming the adhesive layer (first layer) is lowered. It is presumed that this decrease in glass transition temperature allows the first copolymer to maintain a state having mobility such as micro-Brownian motion even at room temperature. Therefore, it is considered that the volume in which the first copolymer can move (move) is increased, thereby suppressing aggregation. Therefore, the adhesive layer (first layer) containing the first copolymer having the above-mentioned structure is unlikely to form irregularities on its surface, so that the surface of the biocompatible layer (second layer) can also be formed smoothly, and excellent antithrombotic properties can be exhibited. In other words, the desired effect of improving the adhesiveness of the adhesive layer (first layer) (long-term maintenance of the biocompatible layer (second layer)) can be obtained without impairing the antithrombotic properties obtained by the biocompatible layer (second layer).

[0046] On the other hand, a homopolymer of a monomer having an epoxy group (i.e., a polymer having only the above-mentioned structural unit (A-1) as a structural unit) has a higher glass transition temperature than a copolymer (first copolymer) having the above-mentioned structural unit (A-1) and structural unit (A-2), and has almost no mobility around room temperature. Therefore, when such a homopolymer is used to form an adhesive layer (first layer), it will aggregate, resulting in the above-mentioned decrease in antithrombotic properties.

[0047] It should be noted that the above mechanism is merely speculation and does not limit the technical scope of the present invention in any way.

[0048] Hereinafter, the embodiments of the present invention will be described. Note that the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the claims. In addition, the embodiments described in this specification can be arbitrarily combined to form other embodiments. The dimensional ratios in the drawings are exaggerated for the convenience of explanation, and may differ from the actual ratios. In addition, when the embodiments of the present invention are explained with reference to the drawings, the same elements are given the same reference numerals in the explanation of the drawings, and duplicate explanations are omitted.

[0049] In this specification, when a certain structural unit is defined as being "derived from" a certain monomer, it means that the structural unit is a divalent structural unit generated by cleavage of one of the polymerizable unsaturated double bonds of the corresponding monomer.

[0050] In this specification, the term "(meth)acrylic" includes both acrylic and methacrylic. Thus, for example, the term "(meth)acrylic acid" includes both acrylic acid and methacrylic acid. Similarly, the term "(meth)acryloyl" includes both acryloyl and methacryloyl. Thus, for example, the term "(meth)acryloyl group" includes both acryloyl group and methacryloyl group. Similarly, the term "(meth)acrylate" includes both acrylate and methacrylate. Thus, for example, the term "alkoxyalkyl (meth)acrylate" includes both alkoxyalkyl acrylate and alkoxyalkyl methacrylate.

[0051] In this specification, the term "X to Y" indicating a range includes X and Y and means "X or more and Y or less." Furthermore, "A and / or B" includes each of A and B and all combinations of one or more, and specifically means at least one of A and B, and means A, B, and a combination of A and B. Furthermore, unless otherwise specified, the operations and measurements of physical properties are performed under conditions of room temperature (20 to 25°C) and relative humidity of 40 to 50% RH.

[0052] [Medical equipment] A medical device according to one embodiment of the present invention comprises a plastic substrate, a first layer supported on at least a portion of the plastic substrate, and a second layer supported on at least a portion of the first layer. The first layer comprises a first copolymer having a structural unit (A-1) derived from a monomer (a-1) having an epoxy group and a structural unit (A-2) derived from a monomer (a-2) having a homopolymer glass transition temperature of less than -10°C. The second layer comprises a second copolymer having a structural unit (B-1) derived from a monomer (b-1) capable of bonding with an epoxy group contained in the structural unit (A-1), and a structural unit (B-2) derived from an antithrombotic monomer (b-2).

[0053] Hereinafter, the configuration of a medical device according to one embodiment of the present invention will be described with reference to the attached drawings.

[0054] Fig. 1 is a partial cross-sectional view showing a schematic representation of a surface layer structure of a representative embodiment of a medical device according to the present invention, and Fig. 2 is a partial cross-sectional view showing a schematic representation of a different example of the surface layer structure as an application example of this embodiment.

[0055] As shown in FIG. 1 and FIG. 2, the medical device 100 of this embodiment is formed by directly laminating a plastic substrate (also simply referred to as a "substrate") 10, a first layer (adhesive layer) 11, and a second layer (biocompatible layer) 12 in this order. That is, the substrate 10, the first layer 11, and the second layer 12 are adjacently laminated in this order. In the medical device 100, the first layer 11 is supported on at least a part of the substrate 10 (the figure shows an example in which the first layer 11 is fixed to the entire surface (whole surface) of the substrate 10 in the drawing), and the second layer 12 is supported on at least a part of the first layer 11 (the figure shows an example in which the second layer 12 is fixed to the entire surface (whole surface) of the first layer 11 in the drawing). In this specification, "supported" means that a certain layer (upper layer) is fixed in a state in which it is not easily separated (peeled off) from the surface of the lower layer. Specifically, the state in which the first layer is "supported" by the substrate may be a state in which the first copolymer is bonded (immobilized) to the substrate surface to form the first layer, a state in which the first copolymer (first layer) is deposited on the substrate surface, or a state in which the first copolymer (first layer) is impregnated into the substrate surface. Similarly, the state in which the second layer (biocompatible layer) is "supported" by the first layer may be a state in which the second copolymer is bonded (immobilized) to the substrate surface to form the second layer, a state in which the second copolymer (second layer) is deposited on the substrate surface, or a state in which the second copolymer (second layer) is impregnated into the substrate surface.

[0056] From the viewpoint of maintaining antithrombotic properties for a long period of time, a preferred form of "support" is a state in which the surface of a certain layer (upper layer) is physically and / or chemically bonded to the surface of the layer below, and a more preferred form is a state in which they are chemically bonded. Note that the "chemically bonded state" here refers to a state in which at least a part of the surface of a certain layer (upper layer) is bonded to at least a part of the surface of the layer below by covalent bonds, ionic bonds, hydrogen bonds, intermolecular forces, etc.

[0057] Moreover, as described above, the reason why "the first layer 11 is supported on at least a part of the substrate 10" and "the second layer 12 is supported on at least a part of the first layer 11" are that in artificial blood vessels, stent grafts, covered stents, catheters, etc., which are examples of uses of medical devices, it is not necessary to impart antithrombotic properties to all surfaces (whole surfaces) of these medical devices, and it is sufficient that the second layer 12 (and further the first layer 11 provided below the second layer 12) is supported only on the surface portion (sometimes a part or sometimes the whole) that is required to have antithrombotic properties. For this reason, it is preferable that the second layer 12 (and further the first layer 11 provided below the second layer 12) is supported on at least the portion of the substrate 10 that comes into contact with blood (for example, the inner wall of an artificial blood vessel). For example, when the medical device is an artificial blood vessel, a stent graft, a covered stent or the like, it is preferable that the first layer and the second layer are supported (formed) on the entire surface of the base material.

[0058] Each component of the medical device according to the present invention will be described below.

[0059] <Plastic substrate (plastic substrate layer)> The substrate 10 constituting the medical device according to one embodiment of the present invention is a plastic substrate (polymer substrate). As the plastic substrate, an optimal substrate can be appropriately selected according to the characteristics (e.g., mechanical strength, etc.) required for the medical device such as an artificial blood vessel, a stent graft, a covered stent, a catheter, etc., and as an example, a substrate having the characteristics required for a substrate such as mechanical strength, flexibility, smoothness, etc. is preferable.

[0060] The substrate 10 may have at least a surface made of plastic (polymer material). As an example, as shown in FIG. 1, the entire substrate may be made of plastic (polymer material). As shown in FIG. 2, the substrate may have a structure in which a plastic (polymer material) that is softer than the reinforcing material such as metal material is coated on the surface of the substrate core portion 10a formed of a hard reinforcing material such as metal material or ceramic material by a suitable method (conventional known method such as dipping, spraying, coating, printing, etc.) to form the substrate surface layer 10b. The reinforcing material of the substrate core portion 10a and the plastic (polymer material) of the substrate surface layer 10b may be composited (suitable reaction treatment) to form the substrate 10. Therefore, the substrate core portion 10a may be a multilayer structure formed by laminating different materials in multiple layers, or a structure (composite) in which members formed of different materials are joined for each part of the medical device. In addition, another middle layer (not shown) may be formed between the substrate core portion 10a and the substrate surface layer 10b. Furthermore, as for the substrate surface layer 10b, as long as its surface is made of plastic (polymer material), it may be a multi-layer structure made of multiple layers of different materials, or a structure (composite) in which members made of different materials are joined together for each part of the medical device.

[0061] The material (polymer material) constituting (forming) the substrate 10 and the substrate surface layer 10b is not particularly limited, and polymer materials commonly used in medical devices such as artificial blood vessels, stent grafts, covered stents, and catheters can be used. Specifically, polyamide resins such as nylon 6, nylon 11, nylon 12, and nylon 66 (all of which are registered trademarks), polyethylenes such as linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), high-density polyethylene (HDPE), and modified polyethylene, polyolefin resins such as polypropylene, polyester resins such as polyethylene terephthalate, styrene resins such as polystyrene, cyclic polyolefin resins, modified polyolefin resins, epoxy resins, urethane resins, diallyl phthalate resins (allyl resins), polycarbonate resins, fluororesins such as ePTFE (expanded polyethylene tetrafluoroethylene), amino resins (urea resins, melamine resins, benzoguanamine resins), acrylic resins, polyacetal resins, vinyl acetate resins, phenolic resins, vinyl chloride resins, silicone resins (silicon resins), polyether resins such as polyether ether ketone (PEEK), and polyimide resins can be mentioned. These may be used alone or in combination of two or more. The above polymer materials can be appropriately selected depending on the application of the medical device. Polymeric materials (plastics) constituting (forming) the base materials of artificial blood vessels, stent grafts, covered stents, catheters, etc., which are examples of applications, preferably contain polyester resins and / or fluororesins. Furthermore, from the viewpoint of mechanical strength, the polymeric materials (plastics) more preferably contain polyester resins. Examples of such polyester resins include polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), polybutylene terephthalate (PBT), etc.Therefore, the polymeric material (plastic) constituting (forming) the substrate 10 or the substrate surface layer 10b is preferably at least one selected from the group consisting of polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), and polybutylene terephthalate (PBT), and is more preferably polyethylene terephthalate (PET).

[0062] The material that can be used for the above-mentioned substrate core portion 10a is not particularly limited, and a reinforcing material that can fully exhibit the optimal function of the substrate core portion 10a may be appropriately selected depending on the application of the medical device (e.g., artificial blood vessel). For example, various stainless steels (SUS) such as SUS304, SUS316L, SUS420J2, and SUS630, various metal materials such as gold, platinum, silver, copper, nickel, cobalt, titanium, iron, aluminum, tin, and alloys thereof (for example, nickel-titanium alloy, cobalt-chromium alloy, zinc-tungsten alloy, etc.), inorganic materials such as various ceramic materials, and metal-ceramic composites can be exemplified, but are not limited to these.

[0063] Alternatively, the substrate core portion 10a may be made of a polymeric material other than the plastic (polymeric material) that forms (constitutes) the substrate surface layer 10b. Examples of such polymeric materials are not particularly limited, and include the same materials as those mentioned above. These may be used alone or in combination of two or more types.

[0064] Preferably, the substrate 10 includes or is made of a plastic (polymeric material), or the substrate surface layer 10b includes or is made of a plastic (polymeric material). More preferably, the substrate 10 includes or is made of a plastic (polymeric material), or the substrate surface layer 10b is made of a plastic (polymeric material).

[0065] The shape of the substrate 10 is not particularly limited, and may be appropriately selected depending on the mode of use, such as a sheet, a film, a tube, a shape having multiple branched tubes such as a bifurcated shape (for example, a Y-shape), a linear shape (wire), a fiber (yarn), etc. The substrate 10 may also be a fabric made of fiber (yarn), and the fabric may be in any form including woven fabric, knitted fabric, nonwoven fabric, etc.

[0066] 《1st layer (adhesive layer)》 The first layer (adhesive layer) comprises a first copolymer having a structural unit (A-1) derived from a monomer (a-1) having an epoxy group and a structural unit (A-2) derived from a monomer (a-2) having a homopolymer glass transition temperature of less than -10°C.

[0067] The first copolymer is firmly supported (fixed) on the substrate by the epoxy group contained in the monomer (a-1) (i.e., the structural unit (A-1)). Specifically, the epoxy group contained in the monomer (a-1) (structural unit (A-1)) can form a physical and / or chemical bond (preferably, a chemical bond) between the first copolymer and the plastic substrate. The epoxy group contained in the monomer (a-1) (structural unit (A-1)) forms a physical and / or chemical bond (preferably, a chemical bond) with the structural unit (B-1) (i.e., a structural unit derived from the monomer (b-1) capable of bonding with an epoxy group) constituting the second copolymer contained in the second layer (biocompatible layer). As described above, the second layer is firmly fixed on the plastic substrate via the first layer, and therefore the medical device according to the present invention can maintain antithrombotic properties for a long period of time.

[0068] The first copolymer has, in addition to the above-mentioned structural unit (A-1), a structural unit (A-2) derived from a monomer (a-2) whose homopolymer has a glass transition temperature of less than -10°C. By including the structural unit (A-2), the mobility of the first copolymer is improved, and as a result, aggregation is suppressed, and a first layer having a smooth surface can be formed. Therefore, the second layer formed on the first layer having such a smooth surface also has a smooth surface, and therefore the effect of suppressing the formation of thrombus by the second copolymer can be sufficiently obtained. That is, the second layer can be firmly fixed to the substrate by the epoxy group contained in the structural unit (A-1), while maintaining good antithrombotic properties by the second layer.

[0069] In addition, the first copolymer according to the present invention has a suitable mobility (flexibility) due to the structural unit (A-2), and therefore can reduce the difference in mobility (flexibility) between the plastic substrate and the second copolymer constituting the second layer. Therefore, the mechanical stress between the plastic substrate and the second layer can be reduced, and as a result, the second layer can be maintained on the plastic substrate for a long period of time.

[0070] The first layer may be in the form of a single layer or a laminate of two or more layers. Preferably, the first layer is in the form of a single layer.

[0071] The first copolymer has a structural unit (A-1) derived from a monomer (a-1) (also referred to as "monomer (a-1)") having an epoxy group. The monomer (a-1) is not particularly limited as long as it has an epoxy group (-C2H3O), but it is preferable that the monomer (a-1) has a glycidyl group (-CH2-C2H3O).

[0072] Furthermore, it is preferable that the monomer (a-1) further has an ethylenically unsaturated group such as an acryloyl group (CH2=CH-C(=O)-), a methacryloyl group (CH2=C(CH3)-C(=O)-) or a vinyl group (CH2=CH-), and it is more preferable that the monomer (a-1) further has an acryloyl group or a methacryloyl group.

[0073] That is, in a preferred embodiment of the present invention, the monomer (a-1) and the structural unit (A-1) derived therefrom preferably have an epoxy group and an ethylenically unsaturated group, more preferably have a glycidyl group and an ethylenically unsaturated group, and particularly preferably have a glycidyl group and a (meth)acryloyl group.

[0074] Specific examples of monomers having an epoxy group and an ethylenically unsaturated group include (meth)acrylic acid esters having a glycidyl group (epoxy group), such as glycidyl acrylate, glycidyl methacrylate (GMA), 3,4-epoxycyclohexylmethyl acrylate, 3,4-epoxycyclohexylmethyl methacrylate, β-methylglycidyl acrylate, and β-methylglycidyl methacrylate; vinyl ethers having a glycidyl group (epoxy group), such as allyl glycidyl ether, but are not limited thereto. Among these, from the viewpoints of further improving the adhesion to the substrate and easiness of controlling the polymerization during the preparation of the copolymer, it is preferable that the monomer (a-1) contains at least one selected from the group consisting of glycidyl acrylate, glycidyl methacrylate (GMA), 3,4-epoxycyclohexylmethyl acrylate, 3,4-epoxycyclohexylmethyl methacrylate, β-methylglycidyl acrylate, and β-methylglycidyl methacrylate. Furthermore, the monomer (a-1) more preferably contains at least one selected from the group consisting of glycidyl acrylate and glycidyl methacrylate. Furthermore, the monomer (a-1) more preferably contains glycidyl acrylate or glycidyl methacrylate, particularly preferably contains glycidyl methacrylate, and most preferably is glycidyl methacrylate.

[0075] The structural unit (A-1) is preferably a structural unit derived from a monomer that is preferably used as the monomer (a-1) above. This configuration has the advantage that it is easier to form stronger bonds with the substrate and the second layer, and is also easy to manufacture.

[0076] The monomer (a-1) may be used alone or in combination of two or more. That is, the structural unit (A-1) may be a homopolymer type composed of one type of structural unit, or a copolymer type composed of two or more types of structural units. When two or more types of the monomer (a-1) are used, the segment composed of the monomer (a-1) may be in the form of a block copolymer, a random copolymer, or an alternating copolymer.

[0077] The content of the structural unit (A-1) is preferably more than 5 mol% and less than 70 mol%, more preferably 10 mol% or more and 60 mol% or less, and particularly preferably more than 20 mol% and less than 50 mol%, based on 100 mol% of all structural units constituting the first copolymer. With such a composition, the first copolymer is less likely to aggregate, and a first layer having a smoother surface can be formed.

[0078] The first copolymer has a structural unit (A-2) derived from a monomer (a-2) (also referred to as "monomer (a-2)") whose homopolymer has a glass transition temperature of less than -10°C. Here, "monomer (a-2) whose homopolymer has a glass transition temperature of less than -10°C" means that a homopolymer (single polymer) using the monomer has a glass transition temperature of less than -10°C. The glass transition temperature is a value measured by differential scanning calorimetry of a homopolymer (single polymer) using the monomer (a-2). The differential scanning calorimetry is performed under the following conditions. That is, the measurement procedure is to seal 3.0 mg of a sample (homopolymer) in an aluminum pan and set it in a holder. An empty aluminum pan is used as a reference. The measurement conditions are a measurement temperature of -100°C to 100°C, a heating rate of 10°C / min, a cooling rate of 10°C / min, and a temperature control of heating-cooling-heating, and analysis is performed based on the data from the second heating process. For the obtained DSC chart, an extension line of the baseline before the rise of the first endothermic peak and a tangent line showing the maximum slope between the rise part of the first endothermic peak and the peak apex are drawn, and the temperature at the intersection of these lines is regarded as the glass transition temperature [Tg (°C)].

[0079] The glass transition temperature of the homopolymer may be less than -10°C, but from the viewpoint of suppressing aggregation of the first copolymer and obtaining a medical device having good antithrombogenicity, the glass transition temperature is preferably -12°C or lower, more preferably -30°C or lower. If the glass transition temperature is -10°C or higher, the mobility of the molecular chains constituting the first copolymer decreases and they aggregate, resulting in insufficient antithrombogenicity. In addition, if the glass transition temperature of the homopolymer of monomer (a-2) is within the above range, the flexibility of the first copolymer is improved and the mechanical stress generated between the substrate and the second layer can be alleviated, so that the second layer can be prevented from peeling off from the substrate, and antithrombogenicity can be maintained for a long period of time.

[0080] On the other hand, the lower limit of the glass transition temperature of the homopolymer is not particularly limited, but from the viewpoint of forming a first layer having good strength, it is preferably -120°C or higher, more preferably -100°C or higher, and particularly preferably -70°C or higher.

[0081] Therefore, the glass transition temperature of the homopolymer of monomer (a-2) is preferably lower than -10°C and -120°C or higher, more preferably -12°C or lower and -100°C or higher, and particularly preferably -30°C or lower and -70°C or higher.

[0082] In addition, in consideration of the use of medical devices (e.g., artificial blood vessels, stent grafts, covered stents, etc.), it is preferable that the monomer (a-2) is a homopolymer that exhibits antithrombotic properties. Here, "antithrombotic properties" refers to the property of reducing blood coagulation on the surface that comes into contact with blood.

[0083] Examples of such monomers (a-2) include (meth)acrylic monomers whose homopolymers have a glass transition temperature of less than -10°C.

[0084] Among them, the monomer (a-2) is preferably one or more monomers selected from the monomers represented by the following formula (I):

[0085] [ka]

[0086] In the above formula (I), R 1 represents a hydrogen atom or a methyl group, and X 1 -O-(R 2 O) m -R 3 or a tetrahydrofurfuryloxy group, R 2 each independently represents a linear or branched alkylene group having 1 to 4 carbon atoms; R 3represents a linear or branched alkyl group having 1 to 4 carbon atoms; and m represents an integer of 1 to 5.

[0087] The first copolymer containing the structural unit (A-2) derived from the monomer represented by the above formula (I) has excellent antithrombotic biocompatibility (the effect of inhibiting and preventing platelet adhesion / adhesion and the effect of inhibiting and preventing platelet activation), particularly the effect of inhibiting and preventing platelet adhesion / adhesion. The tetrahydrofurfuryloxy group is a group having the following structure.

[0088] [ka]

[0089] In the above formula (I), R 1 is a hydrogen atom or a methyl group, and is preferably R 1 is a hydrogen atom.

[0090] In the above formula (I), X 1 R that can be included in 2 are each independently a linear or branched alkylene group having 1 to 4 carbon atoms, and specific examples thereof include a methylene group, an ethylene group, a trimethylene group, a propylene group, and a tetramethylene group. Among these, from the viewpoint of further suppressing aggregation and obtaining better antithrombotic properties, R 2 are each independently preferably a methylene group, an ethylene group, or a trimethylene group, more preferably an ethylene group or a trimethylene group, and most preferably an ethylene group. 2 When multiple O- are present (m is 2 or more), each -R 2 The O- may be the same or different.

[0091] In the above formula (I), X 1 R that can be included in 3is a linear or branched alkyl group having 1 to 4 carbon atoms, and specific examples thereof include linear or branched alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, and tert-butyl. Of these, from the viewpoint of further suppressing aggregation and obtaining better antithrombotic properties, R 3 is preferably a linear or branched alkyl group having 1 to 3 carbon atoms, more preferably an alkyl group having 1 or 2 carbon atoms (methyl group, ethyl group), and particularly preferably a methyl group.

[0092] In the above formula (I), X 1 The m that can be included in (-R 2 O—) groups and is an integer of 1 to 5. From the viewpoint of improving antithrombotic properties, m is preferably an integer of 1 to 3, more preferably 1 or 2, and particularly preferably 1.

[0093] In the above formula (I), X 1 is -O-(-R 2 O-) m -R 3 or a tetrahydrofurfuryloxy group, and from the viewpoint of further suppressing the aggregation of the first copolymer and obtaining better antithrombotic properties, X 1 is -O-(-R 2 O-) m -R 3 From the same viewpoint, it is preferable that the monomer (a-2) is R 1 represents a hydrogen atom or a methyl group, and X 1 -O-(-R 2 O-) m -R 3 R 2 represents a linear or branched alkylene group having 1 to 4 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 4 carbon atoms, and m is 1. From the same viewpoint, the monomer (a-2) is preferably an alkoxyalkyl(meth)acrylate represented by the above formula (I), in which R 1 represents a hydrogen atom or a methyl group, and X 1 -O-(-R 2 O-)m -R 3 R 2 represents a methylene group, an ethylene group, or a trimethylene group; R 3 It is more preferable that the monomer (a-2) is an alkoxyalkyl(meth)acrylate represented by the above formula (I) in which R represents a methyl group or an ethyl group, and m is 1. From the same viewpoint, furthermore, the monomer (a-2) is an alkoxyalkyl(meth)acrylate represented by the above formula (I) in which R 1 represents a hydrogen atom or a methyl group, and X 1 -O-(R 2 O) m -R 3 R 2 represents an ethylene group or a trimethylene group, and R 3 It is particularly preferable that the monomer (a-2) is an alkoxyalkyl(meth)acrylate represented by the above formula (I) in which R represents a methyl group or an ethyl group, and m is 1. From the same viewpoint, the monomer (a-2) is particularly preferably an alkoxyalkyl(meth)acrylate represented by the above formula (I) in which R 1 represents a hydrogen atom or a methyl group, and X 1 -O-(RO) m -R 3 In this case, R 2 represents an ethylene group, and R 3 It is most preferable that the alkoxyalkyl(meth)acrylate is an alkoxyalkyl(meth)acrylate represented by the above formula (I), in which represents a methyl group and m is 1.

[0094] Specific examples of the monomer represented by the above formula (I) include, but are not limited to, methoxymethyl acrylate, methoxyethyl acrylate (MEA), methoxypropyl acrylate, ethoxymethyl acrylate, ethoxyethyl acrylate (EEA), 2-(2-ethoxyethoxy)ethyl acrylate (EEEA), ethoxypropyl acrylate, ethoxybutyl acrylate, propoxymethyl acrylate, butoxyethyl acrylate, methoxybutyl acrylate, tetrahydrofurfuryl acrylate (THFA), methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, 2-(2-ethoxyethoxy)ethyl methacrylate, propoxymethyl methacrylate, butoxyethyl methacrylate, tetrahydrofurfuryl methacrylate, and the like. Of these, from the viewpoint of suppressing aggregation of the first copolymer and obtaining good antithrombotic properties, it is preferable that the monomer (a-2) contains at least one selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), methoxypropyl acrylate, ethoxymethyl acrylate, ethoxyethyl acrylate (EEA), 2-(2-ethoxyethoxy)ethyl acrylate (EEEA), ethoxypropyl acrylate, ethoxybutyl acrylate, propoxymethyl acrylate, butoxyethyl acrylate, methoxybutyl acrylate, tetrahydrofurfuryl acrylate (THFA), methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, 2-(2-ethoxyethoxy)ethyl methacrylate, propoxymethyl methacrylate, butoxyethyl methacrylate, and tetrahydrofurfuryl methacrylate.Furthermore, it is more preferable that the monomer (a-2) includes at least one selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), ethoxymethyl acrylate, ethoxyethyl acrylate (EEA), 2-(2-ethoxyethoxy)ethyl acrylate (EEEA), tetrahydrofurfuryl acrylate (THFA), methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, 2-(2-ethoxyethoxy)ethyl methacrylate, and tetrahydrofurfuryl methacrylate.

[0095] The structural unit (A-2) is preferably a structural unit derived from a monomer that is preferably used as the monomer (a-2) above. This embodiment has the advantage that aggregation of the first copolymer is further suppressed, a medical device having excellent antithrombotic properties can be obtained, and the medical device is also easy to produce.

[0096] The monomer (a-2) may be used alone or in combination of two or more. That is, the structural unit (A-2) may be a homopolymer type composed of one type of structural unit, or a copolymer type composed of two or more types of structural units. Even in this case, the glass transition temperatures of homopolymers using two or more types of monomers (a-2) are all less than -10°C. When two or more types of monomers (a-2) are used, the segment composed of the monomer (a-2) may be in the form of a block copolymer, a random copolymer, or an alternating copolymer.

[0097] The content of the structural unit (A-2) is preferably more than 30 mol% and less than 95 mol%, more preferably 40 mol% or more and 90 mol% or less, and particularly preferably more than 50 mol% and less than 80 mol%, based on 100 mol% of all structural units constituting the first copolymer. With such a composition, the first copolymer is less likely to aggregate, and a first layer having a smoother surface can be formed.

[0098] Preferred specific examples of monomers ((meth)acrylic monomers) having a homopolymer glass transition temperature of less than -10°C are shown below, but the monomer (a-2) is not limited thereto. The numbers in parentheses indicate the glass transition temperature of the homopolymer made of the monomer.

[0099] Specific examples include methoxyethyl acrylate (MEA: -50°C), tetrahydrofurfuryl acrylate (THFA: -12°C), 2-ethoxyethyl acrylate (EEA: -50°C), 2-(2-ethoxyethoxy)ethyl acrylate (EEEA: -67°C), etc. Among them, for the purpose of suppressing aggregation and obtaining excellent antithrombotic properties, the monomer (a-2) is preferably methoxyethyl acrylate and / or tetrahydrofurfuryl acrylate, and particularly preferably methoxyethyl acrylate. These monomers can be used alone or in combination of two or more kinds.

[0100] The structure of the first copolymer is not particularly limited, and may be any of a random copolymer, an alternating copolymer, a periodic copolymer, and a block copolymer. Preferably, the first copolymer is a random copolymer. That is, the first copolymer is preferably a random copolymer having a segment having a structural unit (A-1) derived from a monomer (a-1) and a segment having a structural unit (A-2) derived from a monomer (a-2). The first copolymer in such a form has further improved flexibility and is more likely to relieve mechanical stress occurring between the substrate and the second layer. As a result, it is possible to easily suppress peeling of the second layer from the substrate.

[0101] The composition of the structural unit (A-1) and the structural unit (A-2) constituting the first copolymer is appropriately selected in consideration of the cohesiveness (flexibility) of the first copolymer. Specifically, the composition of the structural unit (A-1) derived from the monomer (a-1) and the structural unit (A-2) derived from the monomer (a-2) in the first copolymer (molar ratio of structural unit (A-1): structural unit (A-2)) is preferably 1:9 to 6:4, more preferably 2:8 to 6:4, more preferably 2:8 to 5:5, even more preferably 2.5:7.5 to 5:5, particularly preferably 3:7 to 5:5, and most preferably 3:7 to 4.5:5.5. The composition of each structural unit is substantially the same as the ratio of the amount (mol) of the monomer to the total amount (mol) of each monomer when producing the first copolymer.

[0102] The first copolymer essentially contains the structural unit (A-1) derived from the monomer (a-1) and the structural unit (A-2) derived from the monomer (a-2), but may have other structural units in addition to these structural units. When the first copolymer has other structural units, examples of monomers constituting the other structural units include acrylic acid, methacrylic acid, acryloylmorpholine, N,N-dimethylaminoethyl acrylate, N-vinylpyrrolidone, 2-methacryloyloxyethyl phosphorylcholine, 2-methacryloyloxyethyl-D-glycoside, 2-methacryloyloxyethyl-D-mannoside, vinyl methyl ether, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, 1-chloro-2-hydroxypropyl Examples of the monomers constituting the other structural units include 1,6-hexanediol mono(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, neopentyl glycol mono(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolethane di(meth)acrylate, 2-hydroxy-3-phenyloxypropyl(meth)acrylate, 4-hydroxycyclohexyl(meth)acrylate, 2-hydroxy-3-phenyloxy(meth)acrylate, 4-hydroxycyclohexyl(meth)acrylate, cyclohexanedimethanol mono(meth)acrylate, adipic acid, glutaric acid, triethylene glycol, and tripropylene glycol. The monomers constituting the other structural units may be used alone or in combination of two or more. That is, the other structural units may be a homopolymer type composed of one type of structural unit, or a copolymer type composed of two or more types of structural units. In addition, when two or more types of monomers constituting the other structural units are used, the segment constituted by the monomers may be in the form of a block copolymer, a random copolymer, or an alternating copolymer.

[0103] When the first copolymer has other structural units, the content of the other structural units is preferably more than 0 mol% and not more than 5 mol% relative to the total structural units constituting the first copolymer. That is, in the first copolymer, when the total of all structural units constituting the first copolymer is taken as 100 mol%, the total content of the structural units (A-1) and (A-2) is preferably 95 mol% or more (upper limit: less than 100 mol%). More preferably, the first copolymer is substantially composed of the structural units (A-1) and (A-2) (content of other structural units = more than 0 mol% and less than 5 mol%). In this form, the first copolymer has high flexibility and aggregation is suppressed. Therefore, a medical device having a first layer containing the first copolymer can exhibit excellent antithrombotic properties without impairing the antithrombotic properties of the second layer. Preferably, the copolymer according to the present invention does not contain the above-mentioned other structural units (content of other structural units = 0 mol%).

[0104] The composition of each structural unit can be measured by a known method. For example, 1 The composition (molar ratio) of the structural units can be determined by measuring the integral ratio of the intensities of each signal in the H-NMR spectrum.

[0105] In one embodiment of the present invention, the first copolymer comprises a structural unit (A-1) derived from at least one monomer (a-1) selected from the group consisting of glycidyl acrylate, glycidyl methacrylate (GMA), 3,4-epoxycyclohexylmethyl acrylate, 3,4-epoxycyclohexylmethyl methacrylate, β-methylglycidyl acrylate, and β-methylglycidyl methacrylate, and a structural unit (A-2) derived from at least one monomer (a-2) selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), methoxypropyl acrylate, ethoxymethyl acrylate, ethoxyethyl acrylate (EEA), 2-(2-ethoxyethoxy)ethyl acrylate (EEEA), ethoxypropyl acrylate, ... and a structural unit (A-2) derived from at least one monomer (a-2) selected from the group consisting of propyl acrylate, ethoxybutyl acrylate, propoxymethyl acrylate, butoxyethyl acrylate, methoxybutyl acrylate, tetrahydrofurfuryl acrylate (THFA), methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, 2-(2-ethoxyethoxy)ethyl methacrylate, propoxymethyl methacrylate, butoxyethyl methacrylate, and tetrahydrofurfuryl methacrylate.

[0106] In one embodiment of the present invention, the first copolymer is essentially composed of, or is composed only of, a structural unit (A-1) derived from at least one monomer (a-1) selected from the group consisting of glycidyl acrylate and glycidyl methacrylate, and a structural unit (A-2) derived from at least one monomer (a-2) selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), ethoxymethyl acrylate, ethoxyethyl acrylate (EEA), 2-(2-ethoxyethoxy)ethyl acrylate (EEEA), tetrahydrofurfuryl acrylate (THFA), methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, 2-(2-ethoxyethoxy)ethyl methacrylate, and tetrahydrofurfuryl methacrylate.

[0107] In one embodiment of the present invention, the first copolymer is essentially composed of, or consists only of, a structural unit (A-1) derived from glycidyl acrylate or glycidyl methacrylate and a structural unit (A-2) derived from methoxyethyl acrylate and / or tetrahydrofurfuryl acrylate.

[0108] In one embodiment of the present invention, the first copolymer is essentially composed of a structural unit (A-1) derived from glycidyl methacrylate and a structural unit (A-2) derived from methoxyethyl acrylate or tetrahydrofurfuryl acrylate, or is composed of the above.

[0109] The terminal of the first copolymer is not particularly limited and is appropriately determined depending on the type of raw material used, but in one embodiment, it is a hydrogen atom. In addition, as described below, when the first copolymer is prepared by radical polymerization, the terminal of the first copolymer can be blocked with a structural unit (functional group) derived from a polymerization initiator. From the viewpoint of improving adhesion to a substrate, it is preferable that the terminal of the first copolymer is in the latter form (a form blocked with a functional group derived from a polymerization initiator).

[0110] The weight average molecular weight of the first copolymer is several thousand to several million, preferably 10,000 to 5 million. In this specification, the "weight average molecular weight" is a value measured by gel permeation chromatography (GPC) using polystyrene as a standard substance and tetrahydrofuran (THF) as a mobile phase. Specifically, a polymer (copolymer) is dissolved in tetrahydrofuran (THF) to a concentration of 10 mg / mL to prepare a sample. For the sample thus prepared, a GPC column LF-804 (Shodex) is attached to a GPC system LC-20 (Shimadzu Corporation), THF is run as a mobile phase, and a chromatogram of the polymer (copolymer) is obtained. After preparing a calibration curve with standard polystyrene, the weight average molecular weight of the polymer (copolymer) is calculated based on this curve. The molecular weight of the copolymer can also be calculated based on the type and number of constituent units.

[0111] The thickness (dry film thickness) of the first layer is, for example, 0.1 to 10 μm, preferably 0.5 to 5 μm, and more preferably about 1 to 3 μm.

[0112] The method for producing the first copolymer is not particularly limited, and conventionally known polymerization methods such as radical polymerization, polymerization using a macroinitiator, and polycondensation can be applied. For example, when each structural unit is arranged randomly (the first copolymer is a random copolymer), (i) the above-mentioned monomer (a-1), monomer (a-2), and a suitable polymerization initiator, as well as monomers constituting other structural units added as necessary, are dissolved in a polymerization solvent, and the obtained polymerization reaction liquid is heated to carry out a polymerization reaction; (ii) the above-mentioned monomer (a-1) and monomer (a-2), as well as monomers constituting other structural units added as necessary, are dissolved in a polymerization solvent, and the obtained solution is mixed with a separately prepared polymerization initiator solution to prepare a polymerization reaction liquid, and a polymerization reaction is carried out. From the viewpoint of ease of operation, the method (i) is preferred.

[0113] Here, the polymerization solvent is not particularly limited as long as it can dissolve the monomer (a-1), the monomer (a-2) and a suitable polymerization initiator, as well as the monomers constituting other structural units added as necessary. For example, water (reverse osmosis membrane water (RO water), pure water, ion-exchanged water, distilled water, etc.); alcohols such as ethanol, isopropanol, n-propanol, n-butanol, isobutanol, sec-butanol, t-butanol, ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol; organic solvents such as chloroform, tetrahydrofuran, acetone, dioxane, and benzene, etc., can be selected from these, but are not limited thereto. In addition, the concentration of the monomer (a-1) and the monomer (a-2) contained in the polymerization reaction solution, as well as the monomers constituting other structural units added as necessary, is not particularly limited, but by setting the concentration relatively high, the weight average molecular weight of the resulting copolymer (first copolymer) can be increased. For example, the concentration (total concentration) of the monomer (a-1) and monomer (a-2) in the polymerization reaction solution and the monomers constituting other structural units added as necessary is preferably 10% by mass or more, more preferably 15% by mass or more. The upper limit of the monomer concentration (total concentration) is not particularly limited, but is, for example, a saturated concentration or less, for example, 70% by mass or less, preferably 50% by mass or less.

[0114] In the polymerization reaction liquid, the mixing ratio of the monomer (a-1) and the monomer (a-2) is preferably adjusted to the above-mentioned preferred composition (molar ratio).

[0115] The polymerization reaction liquid may be degassed before the polymerization reaction, for example, by bubbling with an inert gas such as nitrogen gas or argon gas for about 5 minutes to 1 hour.

[0116] The polymerization initiator used here is not particularly limited, and known initiators can be used. Preferably, radical polymerization initiators are used because of their excellent polymerization stability. Specifically, persulfates such as potassium persulfate (KPS), sodium persulfate, and ammonium persulfate; peroxides such as hydrogen peroxide, t-butyl peroxide, methyl ethyl ketone peroxide, 3-hydroxy-1,1-dimethylbutyl peroxyneodecanoate, α-cumyl peroxyneodecanoate, 1,1,3,3-tetrabutyl peroxyneodecanoate, t-butyl peroxyneodecanoate, t-butyl peroxyneoheptanoate, t-butyl peroxypivalate, t-amyl peroxyneodecanoate, t-amyl peroxypivalate, di(2-ethylhexyl)peroxydicarbonate, and di(s-butyl)peroxydicarbonate. compounds such as azobisisobutyronitrile (AIBN), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]disulfate dihydrate, 2,2'-azobis(2-methylpropionamidine)dihydrochloride, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine)]hydrate, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine)]tetrahydrate, and azobiscyanovaleric acid; Among these, the polymerization initiator is preferably an azo compound.The polymerization initiators may be used alone or in combination of two or more.

[0117] Also, for example, the radical polymerization initiator may be used in combination with a reducing agent such as sodium sulfite, sodium hydrogen sulfite, or ascorbic acid as a redox initiator. The amount (addition amount) of the polymerization initiator is preferably 0.01 to 5 mass% and more preferably 0.05 to 3 mass% based on the total of 100 mass% of the monomer (a-1), the monomer (a-2), and the monomers constituting the other structural units. Alternatively, the amount (addition amount) of the polymerization initiator is preferably 0.01 to 5 mol% and more preferably 0.02 to 3 mol% based on the total of 100 mol% of the monomer (a-1), the monomer (a-2), and the monomers constituting the other structural units. With such an amount (addition amount) of the polymerization initiator, the copolymer (first copolymer) can be produced more efficiently.

[0118] In addition, when the method (ii) is used, the solvent in which the polymerization initiator is dissolved in advance (the solvent of the polymerization initiator solution) is not particularly limited as long as it can dissolve the polymerization initiator, and the same solvent as the polymerization solvent can be exemplified. The solvent of the polymerization initiator solution may be the same as or different from the polymerization solvent, but considering the ease of controlling the polymerization, it is preferable that the solvent is the same as the polymerization solvent.

[0119] By heating the polymerization reaction solution prepared as above, the monomer (a-1) and the monomer (a-2) as well as the monomers constituting other structural units can be copolymerized. Here, as the polymerization method, for example, in addition to the above-mentioned radical polymerization, known polymerization methods such as anionic polymerization and cationic polymerization can be adopted, but it is preferable to use radical polymerization in consideration of the ease of operation.

[0120] The polymerization conditions are not particularly limited as long as the monomer (a-1) and the monomer (a-2) and other monomers constituting the structural units can be polymerized under the conditions. For example, the polymerization temperature is preferably 30 to 60°C, more preferably 35 to 55°C. The polymerization time is preferably 0.5 to 12 hours, more preferably 1 to 8 hours. Under such conditions, the copolymer (first copolymer) can be produced more efficiently.

[0121] During the polymerization, a chain transfer agent, a polymerization rate regulator, a surfactant, and other additives may be used appropriately, if necessary.

[0122] The environment in which the polymerization reaction is carried out is not particularly limited, and the reaction can be carried out in the air or in an inert gas atmosphere such as nitrogen gas or argon gas, etc. During the polymerization reaction, the reaction liquid may be stirred.

[0123] The copolymer (first copolymer) after polymerization is preferably purified by a common purification method such as reprecipitation, dialysis, ultrafiltration, or extraction, and among these, purification by reprecipitation is preferred.

[0124] The purified copolymer (first copolymer) can be dried by any method, such as freeze-drying, reduced pressure drying (vacuum drying), spray drying, or heat drying. From the viewpoint of having little effect on the physical properties of the copolymer, freeze-drying or reduced pressure drying (vacuum drying) is preferred.

[0125] In addition, when each structural unit of the first copolymer is arranged in a block form (the first copolymer is a block copolymer), a living radical polymerization method or a polymerization method using a macroinitiator is preferably used. The living radical polymerization method is not particularly limited, but for example, the methods described in JP-A-11-263819, JP-A-2002-145971, JP-A-2006-316169, etc., as well as the atom transfer radical polymerization (ATRP) method, etc., can be applied in the same manner or with appropriate modification. In addition, in the polymerization method using a macroinitiator, for example, a monomer (a-1) having an epoxy group and a macroinitiator having a radical polymerizable group such as a peroxide group are prepared, and then the macroinitiator and monomer (a-2) are polymerized in a polymerization solvent to prepare the first copolymer.

[0126] The first layer essentially contains the first copolymer. The first layer may contain other components in addition to the first copolymer, but preferably the first layer does not substantially contain other components (i.e. the first layer is substantially composed of the first copolymer) (content of other components = less than 10% by mass (solid content equivalent) relative to the mass of the first layer, preferably less than 5% by mass (solid content equivalent)). More preferably the first layer does not contain other components (i.e. the first layer is composed of the first copolymer).

[0127] Second layer (biocompatible layer) The second layer (biocompatible layer) comprises a second copolymer having a structural unit (B-1) derived from a monomer (b-1) capable of bonding with an epoxy group contained in the structural unit (A-1) and a structural unit (B-2) derived from an antithrombotic monomer (b-2).

[0128] In this specification, "biocompatibility" varies depending on the purpose and method of use, but medical materials used as materials that come into contact with blood are required to have the following characteristics (antithrombogenicity): inhibition of the blood coagulation system, inhibition of platelet adhesion and activation, inhibition of activation of the complement system, and affinity with in vivo tissues. For this reason, in this specification, the biocompatible layer includes an antithrombogenic layer.

[0129] In the second copolymer, the monomer (b-1) (i.e., the structural unit (B-1)) is firmly supported (fixed) on the first layer (hence, on the plastic substrate) by bonding with the epoxy group contained in the monomer (a-1) (i.e., the structural unit (A-1)). Specifically, the monomer (b-1) (i.e., the structural unit (B-1)) is bonded with the epoxy group contained in the monomer (a-1) (structural unit (A-1)), thereby forming a physical and / or chemical bond (preferably a chemical bond) between the first copolymer and the second copolymer. As a result, the second layer is firmly fixed on the substrate via the first layer, and the medical device according to the present invention can maintain antithrombotic properties for a long period of time.

[0130] The second layer may be in the form of a single layer or a laminate of two or more layers. Preferably, the second layer is in the form of a single layer.

[0131] The second copolymer has a structural unit (B-1) derived from a monomer (b-1) (also referred to as "monomer (b-1)") capable of bonding with an epoxy group contained in the structural unit (A-1). The monomer (b-1) is not particularly limited as long as it has a functional group capable of bonding with an epoxy group (-C2H3O) (preferably, a glycidyl group (-CH2-C2H3O)). Examples of such functional groups include a primary amino group (-NH2), a carboxyl group (-COOH), and a hydroxyl group (-OH). Therefore, the monomer (b-1) preferably contains at least one functional group selected from the group consisting of a primary amino group (-NH2), a carboxyl group (-COOH), and a hydroxyl group (-OH), and more preferably contains a primary amino group (-NH2).

[0132] In addition to the above functional groups, the monomer (b-1) preferably further has an ethylenically unsaturated group such as an acryloyl group (CH2=CH-C(=O)-), a methacryloyl group (CH2=C(CH3)-C(=O)-) or a vinyl group (CH2=CH-), and more preferably further has an acryloyl group or a methacryloyl group.

[0133] That is, in a preferred embodiment of the present invention, the monomer (b-1) and the structural unit (B-1) derived therefrom preferably have at least one functional group selected from the group consisting of a primary amino group (-NH2), a carboxyl group (-COOH), and a hydroxyl group (-OH) and an ethylenically unsaturated group, more preferably have a primary amino group (-NH2) and an ethylenically unsaturated group, and particularly preferably have a primary amino group (-NH2) and a (meth)acryloyl group.

[0134] Examples of such monomers (b-1) include (meth)acrylic monomers having a primary amino group (-NH2) and (meth)acrylamide monomers having a primary amino group (-NH2).

[0135] Among them, the monomer (b-1) is preferably one or more monomers selected from the monomers represented by the following formula (II) and the following formula (III) and salts thereof:

[0136] [ka]

[0137] In the above formula (II), R 4 represents a hydrogen atom or a methyl group, p represents an integer from 1 to 4;

[0138] [ka]

[0139] In the above formula (III), R 5 represents a hydrogen atom or a methyl group, q represents an integer of 1 to 4.

[0140] In the above, the term "salts thereof" refers to compounds formed by neutralizing the charge of a cation and an anion, and preferably refers to compounds in which the primary amino group (-NH2) in the monomers represented by the above formula (II) and the following formula (III) is an acid (H + X - ) refers to a compound that has been salified (neutralized) by . Specific examples include hydrochloride, phosphate, ribonucleic acid salt, tartrate, lactate, etc. Among these, hydrochloride is preferred.

[0141] In the above formula (II), R 4 is a hydrogen atom or a methyl group, and preferably, R 4 is a methyl group.

[0142] In the above formula (II), p is an integer of 1 to 4. From the viewpoint of improving antithrombotic properties, p is preferably an integer of 2 to 4, more preferably 2 or 3, and particularly preferably 3.

[0143] In the above formula (III), R 5 is a hydrogen atom or a methyl group, and preferably, R 5 is a methyl group.

[0144] In the above formula (III), q is an integer of 1 to 4. From the viewpoint of improving antithrombotic properties, q is preferably an integer of 2 to 4, more preferably 2 or 3, and particularly preferably 3.

[0145] From the viewpoint of obtaining excellent antithrombotic properties, the monomer (b-1) is preferably one or more selected from the monomers represented by the above formula (II) and salts thereof.

[0146] Specific examples of the monomer represented by the above formula (II) include, but are not limited to, aminomethylacrylamide, aminomethylmethacrylamide, aminoethylacrylamide, aminoethylmethacrylamide, aminopropylacrylamide, aminopropylmethacrylamide (APMA), aminobutylacrylamide, and aminobutylmethacrylamide. Of these, from the viewpoint of suppressing the aggregation of the first copolymer and obtaining good antithrombotic properties, it is preferable that the monomer (b-1) contains at least one selected from the group consisting of aminomethylacrylamide, aminomethylmethacrylamide, aminoethylacrylamide, aminoethylmethacrylamide, aminopropylacrylamide, aminopropylmethacrylamide (APMA), aminobutylacrylamide, aminobutylmethacrylamide, and salts thereof. Furthermore, it is more preferable that the monomer (b-1) contains at least one selected from the group consisting of aminoethylacrylamide, aminoethylmethacrylamide, aminopropylacrylamide, aminopropylmethacrylamide (APMA), and salts thereof. Furthermore, it is particularly preferable that the monomer (b-1) contains at least one selected from the group consisting of aminopropylacrylamide, aminopropylmethacrylamide (APMA) and salts thereof.Moreover, it is most preferable that the monomer (b-1) is selected from aminopropylmethacrylamide (APMA) and salts thereof.

[0147] The structural unit (B-1) is preferably a structural unit derived from a monomer suitable for use as the monomer (b-1). According to such an embodiment, a strong bond is formed between the second copolymer and the first copolymer (hence the first layer), and a medical device can be obtained that not only has excellent antithrombotic properties but also can maintain the antithrombotic properties for a long period of time.

[0148] The monomer (b-1) may be used alone or in combination of two or more. That is, the structural unit (B-1) may be a homopolymer type composed of one structural unit alone, or a copolymer type composed of two or more structural units. When two or more types of the monomer (b-1) are used, the segment composed of the monomer (b-1) may be in the form of a block copolymer, a random copolymer, or an alternating copolymer.

[0149] The content of the structural unit (B-1) is preferably more than 3 mol% and less than 30 mol%, more preferably 5 mol% or more and 25 mol% or less, and particularly preferably more than 5 mol% and less than 25 mol%, based on 100 mol% of all structural units constituting the second copolymer. With such a composition, the second copolymer is more likely to form a bond with the epoxy group contained in the first layer, and the second layer is more likely to be firmly supported (fixed) on the first layer (and therefore on the plastic substrate).

[0150] The second copolymer has a structural unit (B-2) derived from an antithrombotic monomer (b-2) (also referred to as "monomer (b-2)" or "antithrombotic monomer (b-2)"). Here, the term "antithrombotic monomer" refers to a compound whose homopolymer exhibits antithrombotic properties, i.e., the property of reducing blood coagulation on the surface that comes into contact with blood.

[0151] Examples of such monomer (b-2) include the (meth)acrylic monomers described below.

[0152] In one embodiment, the monomer (b-2) is preferably one or more monomers selected from the monomers represented by the following formula (IV):

[0153] [ka]

[0154] In the above formula (IV), R6 represents a hydrogen atom or a methyl group, and X 2 -O-(R 7 O) n -R 8 or a tetrahydrofurfuryloxy group, R 7 each independently represents a linear or branched alkylene group having 1 to 4 carbon atoms; R 8 represents a linear or branched alkyl group having 1 to 4 carbon atoms; and n represents an integer of 1 to 5.

[0155] In the above formula (IV), R 6 is a hydrogen atom or a methyl group, and from the viewpoint of obtaining excellent antithrombotic properties, R 6 is a hydrogen atom.

[0156] In the above formula (IV), X 2 R that can be included in 7 are each independently a linear or branched alkylene group having 1 to 4 carbon atoms, and specific examples thereof include a methylene group, an ethylene group, a trimethylene group, a propylene group, and a tetramethylene group. Among these, from the viewpoint of obtaining excellent antithrombotic properties, R 7 are each independently preferably a methylene group, an ethylene group, or a trimethylene group, more preferably an ethylene group or a trimethylene group, and most preferably an ethylene group. 7 When there are multiple O- (n is 2 or more), each -R 7 The O- may be the same or different.

[0157] In the above formula (IV), X 2 R that can be included in 8 is a linear or branched alkyl group having 1 to 4 carbon atoms, and specific examples thereof include linear or branched alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, and tert-butyl groups. Of these, from the viewpoint of obtaining excellent antithrombotic properties, R 8is preferably a linear or branched alkyl group having 1 to 3 carbon atoms, more preferably an alkyl group having 1 or 2 carbon atoms (methyl group, ethyl group), and particularly preferably a methyl group.

[0158] In the above formula (IV), X 2 The n that can be included in is (-R 7 From the viewpoint of improving antithrombotic properties, n is preferably an integer of 1 to 3, more preferably 1 or 2, and particularly preferably 1.

[0159] In the above formula (IV), X 2 is -O-(-R 7 O-) n -R 8 or a tetrahydrofurfuryloxy group. From the viewpoint of obtaining excellent antithrombotic properties, X 2 is -O-(-R 7 O-) n -R 8 From the same viewpoint, it is preferable that the monomer (b-2) is R 6 represents a hydrogen atom or a methyl group, and X 2 -O-(-R 7 O-) n -R 8 R 7 represents a linear or branched alkylene group having 1 to 4 carbon atoms; R 8 represents a linear or branched alkyl group having 1 to 4 carbon atoms, and n is 1. From the same viewpoint, the monomer (b-2) is preferably an alkoxyalkyl(meth)acrylate represented by the above formula (IV), in which R 6 represents a hydrogen atom or a methyl group, and X 2 -O-(-R 7 O-) n -R 8 R 7 represents a methylene group, an ethylene group, or a trimethylene group; R 8 It is more preferable that the monomer (b-2) is an alkoxyalkyl(meth)acrylate represented by the above formula (IV) in which R represents a methyl group or an ethyl group, and n is 1. From the same viewpoint, the monomer (b-2) is more preferably an alkoxyalkyl(meth)acrylate represented by the above formula (IV) in which R6 represents a hydrogen atom or a methyl group, and X 2 -O-(R 7 O) n -R 8 R 7 represents an ethylene group or a trimethylene group, and R 8 It is particularly preferable that the monomer (b-2) is an alkoxyalkyl(meth)acrylate represented by the above formula (IV) in which R represents a methyl group or an ethyl group, and n is 1. From the same viewpoint, the monomer (b-2) is particularly preferably an alkoxyalkyl(meth)acrylate represented by the above formula (IV) in which R 6 represents a hydrogen atom or a methyl group, and X 2 -O-(R 7 O)nR 8 In this case, R 7 represents an ethylene group, and R 8 It is most preferable that the alkoxyalkyl(meth)acrylate is an alkoxyalkyl(meth)acrylate represented by the above formula (IV), in which represents a methyl group and n is 1.

[0160] Specific examples of the monomer represented by the above formula (IV) include, but are not limited to, methoxymethyl acrylate, methoxyethyl acrylate (MEA), methoxypropyl acrylate, ethoxymethyl acrylate, ethoxyethyl acrylate (EEA), 2-(2-ethoxyethoxy)ethyl acrylate (EEEA), ethoxypropyl acrylate, ethoxybutyl acrylate, propoxymethyl acrylate, butoxyethyl acrylate, methoxybutyl acrylate, tetrahydrofurfuryl acrylate (THFA), methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, 2-(2-ethoxyethoxy)ethyl methacrylate, propoxymethyl methacrylate, butoxyethyl methacrylate, tetrahydrofurfuryl methacrylate, and the like. Among these, from the viewpoints of not only obtaining a second copolymer having excellent antithrombotic properties but also increasing affinity with the first copolymer (hence, the first layer) and maintaining antithrombotic properties for a longer period of time, it is preferable that the monomer (b-2) contains at least one selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), methoxypropyl acrylate, ethoxymethyl acrylate, ethoxyethyl acrylate (EEA), 2-(2-ethoxyethoxy)ethyl acrylate (EEEA), ethoxypropyl acrylate, ethoxybutyl acrylate, propoxymethyl acrylate, butoxyethyl acrylate, methoxybutyl acrylate, tetrahydrofurfuryl acrylate (THFA), methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, 2-(2-ethoxyethoxy)ethyl methacrylate, propoxymethyl methacrylate, butoxyethyl methacrylate, and tetrahydrofurfuryl methacrylate.Furthermore, it is more preferable that the monomer (b-2) contains at least one selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), ethoxymethyl acrylate, ethoxyethyl acrylate (EEA), 2-(2-ethoxyethoxy)ethyl acrylate (EEEA), tetrahydrofurfuryl acrylate (THFA), methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, 2-(2-ethoxyethoxy)ethyl methacrylate, and tetrahydrofurfuryl methacrylate. Furthermore, it is particularly preferable that the monomer (b-2) is methoxyethyl acrylate and / or tetrahydrofurfuryl acrylate. Furthermore, it is most preferable that the monomer (b-2) is methoxyethyl acrylate. These monomers can be used alone or in combination of two or more.

[0161] Furthermore, the monomer (b-2) preferably contains the same monomer as the monomer (a-2) constituting the first copolymer, and more preferably is the same as the monomer (a-2). In such an embodiment, the first copolymer and the second copolymer have a common structure (structural unit). Therefore, the affinity between the first layer and the second layer is improved, and the adhesion of the second layer to the first layer is further improved, so that antithrombotic properties can be maintained for a long period of time.

[0162] In another embodiment, the monomer (b-2) may be one or more monomers selected from the monomers represented by the following formula (V):

[0163] [ka]

[0164] In the above formula (V), R 9 represents a hydrogen atom or a methyl group, Y represents an oxygen atom or -NH-; R 10represents a linear or branched alkylene group having 1 to 6 carbon atoms, R 11 and R 12 each independently represents a linear or branched alkyl group having 1 to 4 carbon atoms, R 13 represents a linear or branched alkylene group having 1 to 4 carbon atoms, Z is -COO - or -SO3 - Represents.

[0165] In the above formula (V), R 9 is a hydrogen atom or a methyl group, and from the viewpoint of obtaining excellent antithrombotic properties, is preferably a methyl group.

[0166] In the above formula (V), Y is an oxygen atom or -NH-, and from the viewpoint of obtaining excellent antithrombotic properties, it is preferably an oxygen atom.

[0167] In the above formula (V), R 10 is a linear or branched alkylene group having 1 to 6 carbon atoms, and specific examples thereof include a methylene group, an ethylene group, a trimethylene group, a propylene group, a tetramethylene group, a pentamethylene group, and a hexamethylene group. Among these, from the viewpoint of obtaining excellent antithrombotic properties, R 10 is preferably a linear or branched alkylene group having 1 to 4 carbon atoms, more preferably a methylene group, ethylene group, or trimethylene group, and particularly preferably an ethylene group or trimethylene group.

[0168] In the above formula (V), R 11 and R 12 are each independently a straight-chain or branched alkyl group having 1 to 4 carbon atoms, and specific examples thereof include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group. Of these, from the viewpoint of obtaining excellent antithrombotic properties, R 11 and R 12are each preferably independently a linear or branched alkyl group having 1 to 3 carbon atoms, more preferably an alkyl group having 1 or 2 carbon atoms (methyl group, ethyl group), and particularly preferably a methyl group.

[0169] In the above formula (V), R 13 is a linear or branched alkylene group having 1 to 4 carbon atoms, and specific examples thereof include a methylene group, an ethylene group, a trimethylene group, a propylene group, and a tetramethylene group. Among these, from the viewpoint of obtaining excellent antithrombotic properties, R 13 is preferably a methylene group, an ethylene group, or a trimethylene group, and more preferably a methylene group.

[0170] In the above formula (V), Z is -COO - (Zwitterionic monomers of the carboxybetaine type), or -SO3 - (sulfobetaine type zwitterionic monomer).

[0171] Specifically, among the above zwitterionic monomers, zwitterionic monomers having a carboxybetaine skeleton (carboxybetaine type zwitterionic monomers; Z=-COO - Examples of the acryloyloxymethyl-N,N-dimethylammonium-α-N-methylcarboxybetaine include N-(meth)acryloyloxyethyl-N,N-dimethylammonium-α-N-methylcarboxybetaine, N-(meth)acryloyloxypropyl-N,N-dimethylammonium-α-N-methylcarboxybetaine, N-(meth)acryloyloxymethyl-N,N-diethylammonium-α-N-methylcarboxybetaine, N-(meth)acryloyloxyethyl-N,N-diethylammonium-α-N-methylcarboxybetaine, and N-(meth)acryloyloxypropyl-N,N-diethylammonium-α-N-methylcarboxybetaine, and preferably N-(meth)acryloyloxyethyl-N,N-dimethylammonium-α-N-methylcarboxybetaine (CBA).

[0172] Among the above zwitterionic monomers, the zwitterionic monomers having a sulfobetaine skeleton (sulfobetaine type zwitterionic monomers; Z = -SO3 - Examples of the ammonium hydroxide include [2-((meth)acryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide, [2-((meth)acryloyloxy)ethyl]dimethyl-(3-sulfobutyl)ammonium hydroxide, [2-((meth)acryloyloxy)ethyl]diethyl-(3-sulfopropyl)ammonium hydroxide, and [2-((meth)acryloyloxy)ethyl]diethyl-(3-sulfobutyl)ammonium hydroxide. Of these, [2-((meth)acryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide is preferred.

[0173] The structural unit (B-2) is preferably a structural unit derived from a monomer that is preferably used as the monomer (b-2) above. According to such an embodiment, the second layer can be formed from the second copolymer having excellent antithrombotic properties. In addition, there is an advantage that the adhesion between the first layer and the second layer is improved, so that a medical device capable of maintaining antithrombotic properties for a long period of time can be obtained.

[0174] The monomer (b-2) may be used alone or in combination of two or more. That is, the structural unit (B-2) may be a homopolymer type composed of one type of structural unit, or a copolymer type composed of two or more types of structural units. When two or more types of the monomer (b-2) are used, the segment composed of the monomer (b-2) may be in the form of a block copolymer, a random copolymer, or an alternating copolymer.

[0175] The structure of the second copolymer is not particularly limited, and may be any of a random copolymer, an alternating copolymer, a periodic copolymer, and a block copolymer. Preferably, the second copolymer is a random copolymer. That is, the second copolymer is preferably a random copolymer having a segment having a structural unit (B-1) derived from a monomer (b-1) and a segment having a structural unit (B-2) derived from a monomer (b-2).

[0176] The content of the structural unit (B-2) is preferably more than 70 mol% and less than 97 mol%, more preferably 75 mol% or more and 95 mol% or less, and particularly preferably more than 75 mol% and less than 95 mol%, based on 100 mol% of all structural units constituting the second copolymer. With such a composition, not only is it easy for the second layer to be firmly supported (fixed) on the first layer (hence, on the plastic substrate), but also excellent antithrombotic properties can be obtained.

[0177] The composition of the structural unit (B-1) and the structural unit (B-2) constituting the second copolymer is appropriately selected in consideration of the antithrombotic property of the second copolymer and the adhesion (affinity) to the first layer. Specifically, the composition of the structural unit (B-1) derived from the monomer (b-1) and the structural unit (B-2) derived from the monomer (b-2) in the second copolymer (molar ratio of structural unit (B-1):structural unit (B-2)) is preferably more than 1:1 and less than 1:20, more preferably more than 1:3 and less than 1:20, and particularly preferably 1:4 or more and 1:15 or less. The composition of each structural unit is substantially the same as the ratio of the amount (mol) of the monomer charged to the total amount (mol) of each monomer charged when producing the second copolymer.

[0178] The second copolymer essentially contains the structural unit (B-1) derived from the monomer (b-1) and the structural unit (B-2) derived from the monomer (b-2), but may have other structural units in addition to these structural units. When the second copolymer has other structural units, examples of the monomers constituting the other structural units include the same as the specific examples of the monomers constituting the other structural units in the first copolymer. The monomers constituting the other structural units may be used alone or in combination of two or more. That is, the other structural units may be a homopolymer type composed of one type of structural unit alone, or a copolymer type composed of two or more structural units. When two or more types of monomers constituting the other structural units are used, the segment composed of the monomers may be in the form of a block copolymer, a random copolymer, or an alternating copolymer.

[0179] When the second copolymer has other structural units, the content of the other structural units is preferably more than 0 mol% and not more than 5 mol% relative to the total structural units constituting the second copolymer. That is, in the second copolymer, when the total of all structural units constituting the second copolymer is taken as 100 mol%, the total content of the structural units (B-1) and (B-2) is preferably 95 mol% or more (upper limit: less than 100 mol%). More preferably, the second copolymer is substantially composed of the structural units (B-1) and (B-2) (content of other structural units = more than 0 mol% and less than 5 mol%). In this form, the second copolymer not only has high antithrombotic properties, but also has excellent adhesion to the first layer. Therefore, the antithrombotic properties of the second layer can be maintained for a long period of time.

[0180] In one embodiment of the present invention, the second copolymer is a structural unit (B-1) derived from at least one monomer (b-1) selected from the group consisting of aminomethylacrylamide, aminomethylmethacrylamide, aminoethylacrylamide, aminoethylmethacrylamide, aminopropylacrylamide, aminopropylmethacrylamide (APMA), aminobutylacrylamide, aminobutylmethacrylamide, and salts thereof, and a structural unit (B-2) derived from at least one monomer (b-3) selected from the group consisting of methoxymethylacrylate, methoxyethylacrylate (MEA), methoxypropylacrylate, ethoxymethylacrylate, ethoxyethylacrylate (EEA), 2-(2-ethoxyethoxy)ethylacrylate (EEEA). and a structural unit (B-2) derived from at least one monomer (b-2) selected from the group consisting of ethoxypropyl acrylate, ethoxybutyl acrylate, propoxymethyl acrylate, butoxyethyl acrylate, methoxybutyl acrylate, tetrahydrofurfuryl acrylate (THFA), methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, 2-(2-ethoxyethoxy)ethyl methacrylate, propoxymethyl methacrylate, butoxyethyl methacrylate, and tetrahydrofurfuryl methacrylate.

[0181] In one embodiment of the present invention, the second copolymer is substantially composed of a structural unit (B-1) derived from at least one monomer (b-1) selected from the group consisting of aminoethyl acrylamide, aminoethyl methacrylamide, aminopropyl acrylamide, aminopropyl methacrylamide (APMA) and salts thereof, and a structural unit (B-2) derived from at least one monomer (b-2) selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), ethoxymethyl acrylate, ethoxyethyl acrylate (EEA), 2-(2-ethoxyethoxy)ethyl acrylate (EEEA), tetrahydrofurfuryl acrylate (THFA), methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, 2-(2-ethoxyethoxy)ethyl methacrylate, and tetrahydrofurfuryl methacrylate, or is composed only of the above.

[0182] In one embodiment of the present invention, the second copolymer is essentially composed of, or consists only of, a structural unit (B-1) derived from at least one monomer (b-1) selected from the group consisting of aminopropylacrylamide, aminopropylmethacrylamide (APMA), and salts thereof, and a structural unit (B-2) derived from methoxyethyl acrylate and / or tetrahydrofurfuryl acrylate.

[0183] In one embodiment of the present invention, the second copolymer is essentially composed of, or consists only of, a structural unit (B-1) derived from aminopropyl methacrylamide (APMA) and / or a salt thereof, and a structural unit (B-2) derived from methoxyethyl acrylate and / or tetrahydrofurfuryl acrylate.

[0184] In one embodiment of the present invention, the second copolymer is essentially composed of a structural unit (B-1) derived from aminopropyl methacrylamide (APMA) and / or a salt thereof, and a structural unit (B-2) derived from methoxyethyl acrylate, or is composed of the above.

[0185] The terminal of the second copolymer is not particularly limited and is appropriately determined depending on the type of raw material used, but in one embodiment, it is a hydrogen atom. When the second copolymer is prepared by radical polymerization, the terminal of the second copolymer can be blocked with a structural unit (functional group) derived from a polymerization initiator. From the viewpoint of improving the adhesion to the substrate, the terminal of the second copolymer is preferably in the latter form (blocked with a functional group derived from a polymerization initiator).

[0186] The weight average molecular weight of the second copolymer is several thousand to several million, preferably 10,000 to 5 million.

[0187] The thickness (dry film thickness) of the second layer is, for example, from 0.1 to 10 μm, preferably from 0.5 to 5 μm, and more preferably from about 1 to 3 μm.

[0188] The method for producing the second copolymer is not particularly limited, and for example, conventionally known polymerization methods such as radical polymerization, polymerization using a macroinitiator, polycondensation, etc. can be applied. Specifically, the method described above as the method for producing the first copolymer can be adopted in the same manner or with appropriate modifications, and when each structural unit is arranged randomly, it is preferable to use the above method (i). In this case, the polymerization initiator used is preferably a compound having a carboxyl group, and more preferably an azo compound having a carboxyl group, from the viewpoint of facilitating the formation of a uniform second layer. Examples of such compounds include 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine)] hydrate, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine)] tetrahydrate, and azobiscyanovaleric acid.

[0189] The concentration (total concentration) of the monomers constituting the monomer (b-1) and monomer (b-2) and other constituent units added as necessary in the polymerization reaction solution is preferably 10% by mass or more, more preferably 15% by mass or more. The upper limit of the monomer concentration (total concentration) is not particularly limited, but is, for example, a saturated concentration or less, for example, 70% by mass or less, preferably 50% by mass or less.

[0190] In the polymerization reaction liquid, the mixing ratio of the monomer (b-1) and the monomer (b-2) is preferably adjusted to the above-mentioned preferred composition (molar ratio).

[0191] In addition, the polymerization conditions are not particularly limited, but as an example, the polymerization temperature is preferably 30 to 100° C., more preferably 60 to 90° C. In addition, the polymerization time is preferably 0.5 to 12 hours, preferably 1 to 8 hours. Under such conditions, the copolymer (second copolymer) can be produced more efficiently.

[0192] Furthermore, when each structural unit of the second copolymer is arranged in a block form, the method described above as the method for producing the first copolymer can be adopted in the same manner or with appropriate modifications.

[0193] The second layer essentially contains the second copolymer. The second layer may contain other components in addition to the second copolymer. Examples of other components include unreacted monomers that did not react in the polymerization, various additives such as crosslinkers, thickeners, preservatives, and pH adjusters, as well as drugs that suppress vascular stenosis and blockage that may occur when a stent is placed in a lesion. Specific examples of other components include drugs (biologically active substances) such as anticancer drugs, immunosuppressants, antibiotics, antirheumatic drugs, antithrombotic drugs, HMG-CoA reductase inhibitors, ACE inhibitors, calcium antagonists, antihyperlipidemic drugs, integrin inhibitors, antiallergic drugs, antioxidants, GPIIbIIIa antagonists, retinoids, flavonoids, carotenoids, lipid-improving drugs, DNA synthesis inhibitors, tyrosine kinase inhibitors, antiplatelet drugs, vascular smooth muscle proliferation inhibitors, anti-inflammatory drugs, biomaterials, interferons, and NO production promoters. Here, the amount of the other ingredients to be added is not particularly limited, and the amount usually used is applied in the same manner. Ultimately, the amount of the other ingredients to be added is appropriately selected by the attending physician in consideration of the severity of the disease to be treated, the weight of the patient, etc.

[0194] Preferably, the second layer is substantially free of other components (i.e., the second layer is substantially composed of the second copolymer) (content of other components=less than 10% by mass (solid content equivalent) relative to the mass of the second layer, preferably less than 5% by mass (solid content equivalent)). More preferably, the second layer is substantially free of other components (i.e., the first layer is composed of the second copolymer).

[0195] [Manufacturing method of medical devices] Another aspect of the present invention also provides a method for producing the medical device. That is, one embodiment of the present invention is a method for producing the medical device (also referred to simply as "the method for producing the medical device according to the present invention" in this specification) that includes contacting at least a part of the plastic substrate with the first copolymer to form the first layer, and contacting at least a part of the first layer with the second copolymer to form the second layer. In one embodiment, the production method preferably further includes irradiating the plastic substrate with plasma before contacting the first copolymer with the plastic substrate.

[0196] Here, "contacting at least a portion of the plastic substrate with the first copolymer" refers to bringing at least a portion of the plastic substrate and the first copolymer (which may be in the form of a solution containing the first copolymer or a composition containing the first copolymer) close enough to react with each other, interact with each other, or physically contact each other. Similarly, "contacting at least a portion of the first layer with the second copolymer" refers to bringing at least a portion of the first layer and the second copolymer (which may be in the form of a solution containing the second copolymer or a composition containing the second copolymer) close enough to react with each other, interact with each other, or physically contact each other. The above-mentioned "interaction" may be, for example, a chemical bond such as a covalent bond, a coordinate bond, an ionic bond, a hydrogen bond, or a van der Waals bond, but is not limited thereto.

[0197] A preferred form of "contact" is contact by coating. That is, the method for producing a medical device according to the present invention preferably includes coating at least a part of a plastic substrate with a solution (first coating liquid) containing a first copolymer and a solvent to form a first layer (first solution coating step); and coating the first layer with a solution (second coating liquid) containing a second copolymer and a solvent to form a second layer (second solution coating step). It is also preferable to further irradiate the plastic substrate with plasma (plasma irradiation step) before the first solution coating step. Furthermore, after the first solution coating step and / or the second solution coating step, washing may be performed if necessary.

[0198] That is, the present invention also provides a method for producing a medical device, comprising: irradiating a plastic substrate with plasma; applying a first coating liquid containing a first copolymer having a structural unit (A-1) derived from a monomer (a-1) having an epoxy group and a structural unit (A-2) derived from a monomer (a-2) having a homopolymer glass transition temperature of less than -10°C, and a solvent, to at least a portion of the plastic substrate to support a first layer on at least a portion of the plastic substrate; and applying a second coating liquid containing a second copolymer having a structural unit (B-1) derived from a monomer (b-1) capable of bonding with an epoxy group contained in the structural unit (A-1), and a structural unit (B-2) derived from an antithrombotic monomer (b-2), and a solvent, to at least a portion of the first layer to support a second layer on at least a portion of the first layer.

[0199] Hereinafter, each step performed in the method for producing a medical device according to the present invention will be described in a preferred embodiment. However, the method for producing a medical device according to the present invention is not limited to the following embodiment.

[0200] <Plasma irradiation process (plasma treatment process)> In this step, prior to the first solution application step described below, the plastic substrate is irradiated with plasma (plasma treatment is performed). This oxidizes the surface of the plastic substrate, and hydroxyl groups (-OH) and / or carboxyl groups (-COOH) can be generated. When the first copolymer is brought into contact with the surface of such a plastic substrate (preferably by applying the first coating liquid), the epoxy groups contained in the first copolymer react with the hydroxyl groups (-OH) and / or carboxyl groups (-COOH) to form chemical bonds. As a result, the first copolymer is firmly fixed on the plastic substrate, and a medical device capable of maintaining antithrombotic properties for a long period of time can be manufactured. Therefore, in a preferred embodiment, the medical device according to the present invention has a first layer formed by chemically bonding the hydroxyl groups (-OH) and / or carboxyl groups (-COOH) formed on the surface of the plastic substrate with the epoxy groups contained in the first copolymer (structural unit (A-1)).

[0201] Since it is possible to perform the desired plasma treatment even on a thin and narrow inner surface of a small-diameter artificial blood vessel or the like, the plasma irradiation step is preferably performed by an ionized gas plasma treatment.

[0202] Before irradiating the surface of the plastic substrate with ionized gas plasma, it is preferable to clean the surface of the plastic substrate by a suitable method. That is, it is preferable to remove oils and dirt adhering to the surface of the plastic substrate before generating hydroxyl groups (-OH) and / or carboxyl groups (-COOH) on the surface of the plastic substrate by irradiating the surface with ionized gas plasma. Even if the first solution application step is performed without performing plasma treatment before the first solution application step, it is preferable to perform the cleaning treatment before applying the first solution. The method of the cleaning treatment is not particularly limited, and can be performed by cleaning with a suitable solvent (for example, ultrasonic cleaning, a method of immersing in a cleaning solvent, a method of pouring a cleaning solvent, etc.).

[0203] The pressure conditions in the plasma treatment are not particularly limited, and can be either reduced pressure or atmospheric pressure. It is preferable to perform the treatment under atmospheric pressure, because the plasma gas can be irradiated from any angle, the device can be made smaller because a vacuum device is not required, a space-saving and low-cost system configuration can be realized, and it is also economically superior. In addition, by irradiating the plasma gas while rotating the plasma irradiation nozzle around the object to be treated such as an artificial blood vessel, the entire circumference of the object to be treated can be uniformly plasma-treated without unevenness.

[0204] The ionized gas that can be used in the plasma treatment is one or more gases selected from the group consisting of helium, neon, argon, krypton, air, oxygen, carbon dioxide, carbon monoxide, water vapor, nitrogen, hydrogen, etc. The plasma treatment conditions (irradiation time, LF output, applied current, gas flow rate, electrode gap, plasma irradiation distance) are not particularly limited and can be appropriately selected depending on the binding property (ease of immobilization) between the first copolymer and the plastic substrate, the type and area of ​​the plastic substrate used, etc.

[0205] For example, the irradiation time in the plasma treatment is preferably more than 10 seconds, more preferably from 30 seconds to 10 minutes, and particularly preferably from 1 to 5 minutes. Under such conditions, the first copolymer (first layer) can be more firmly supported (fixed) on the surface of the plastic substrate layer.

[0206] As an example, the LF output in the plasma treatment is preferably 100 to 300 W, and more preferably 200 W.

[0207] For example, the gas flow rate in plasma processing is 5 to 20 cm 3 / min (sccm) is preferred, and 15 cm 3 More preferably, the flow rate is 100 sccm.

[0208] The temperature of the object to be treated (plastic substrate) in the plasma treatment is not particularly limited as long as it is lower than the melting point of the plastic (polymer) on the substrate surface and is within a temperature range in which the plastic substrate does not deform, and may be heated or cooled in addition to room temperature. From an economical point of view, it is preferable to perform the treatment at a temperature (e.g., 5 to 35°C) at which a heating device or a cooling device is not required.

[0209] The plasma irradiation device (system) that can be used for plasma processing is not particularly limited, and for example, a plasma irradiation device (system) having a plasma generating tube that introduces gas molecules and excites them to generate plasma, and an electrode that excites the gas molecules in the plasma generating tube, and a configuration in which plasma is emitted from one end of the plasma generating tube, etc. can be exemplified, but the configuration (system) is not limited in any way. For example, there can be mentioned devices that adopt a high-frequency induction type, a capacitively coupled electrode type, a corona discharge electrode-plasma jet type, a parallel plate type, a remote plasma type, an atmospheric pressure plasma type, a low pressure plasma type, an ICP type high density plasma type, etc. In addition, from those already on the market, an ionized gas plasma irradiation device (system) suitable for irradiation to artificial blood vessels, stent grafts, covered stents, etc., especially a plasma irradiation device (system) at atmospheric pressure can be used. Specifically, a plasma irradiation device: DURADYNE (product name or trademark name) manufactured by TRI-STAR TECHNOLOGIES, a plasma irradiation device: PLASMABEAM manufactured by DIENER ELECTRONIC, etc. can be used, but the configuration (system) is not limited in any way.

[0210] <<First solution application process>> In this step, a solution containing the first copolymer and a solvent, and other components as necessary (also referred to simply as "first coating liquid" in this specification) is prepared, and the first coating liquid is applied onto a plastic substrate to form (support) a first layer on the substrate layer. The method for preparing and applying the first coating liquid is not particularly limited except for using a solution containing the first copolymer and a solvent, and can be applied in the same manner as a known method or by appropriately modifying it.

[0211] The solvent used for preparing the first coating liquid is not particularly limited, and is appropriately selected according to the type of the first copolymer (and other components, if used). From the viewpoint of high solubility, water (reverse osmosis membrane water (RO water), pure water, ion-exchanged water, distilled water, etc.); alcohol-based solvents such as methanol, ethanol, isopropyl alcohol, butanol, etc.; organic solvents such as dichloromethane, chloroform, carbon tetrachloride, tetrahydrofuran (THF), dimethyl sulfoxide, N,N-dimethylformamide (DMF), acetone, dioxane, benzene, etc. are preferably used. These may be used alone or in combination of two or more (in the form of a mixed solvent).

[0212] The concentration of the first copolymer in the first coating liquid is not particularly limited. For example, the concentration of the first copolymer in the first coating liquid is preferably 0.01 to 20% by mass, more preferably 0.05 to 15% by mass, and particularly preferably 0.1 to 10% by mass. If the concentration of the first copolymer is within the above range, the resulting first layer can fully exhibit the effects of the present invention. In addition, a uniform first layer of a desired thickness can be easily obtained by one coating, and the viscosity of the solution is within an appropriate range, which is preferable in terms of operability (e.g., ease of coating) and production efficiency. However, even if the concentration is outside the above range, it can be fully used as long as it is within a range that does not affect the effects of the present invention.

[0213] Next, the first coating liquid prepared as described above is applied onto a plastic substrate. Here, the plastic substrate is the same as that described in the above section "Plastic substrate (plastic substrate layer)", so the description is omitted here.

[0214] The method of applying (coating) the first coating liquid onto the surface of the plastic substrate is not particularly limited, and conventionally known methods can be applied, such as coating / printing method, immersion method (dipping method, dip coating method), spraying method (spray method), spin coating method, mixed solution impregnated sponge coating method, bar coating method (e.g., wire bar method), die coating method, reverse coating method, comma coating method, gravure coating method, doctor knife method, etc. Among these, the immersion method (dipping method, dip coating method) and bar coating method are preferably used, and the immersion method is more preferably used.

[0215] When forming the first layer on a thin and narrow inner surface of an artificial blood vessel, a stent graft, a covered stent, etc., the plastic substrate may be immersed in the first coating liquid and the system may be depressurized to degas it. By depressurizing and degassing, the solution can be quickly permeated into the thin and narrow inner surface, accelerating the formation of the first layer.

[0216] Alternatively, the application (coating) may be performed while stirring the first coating liquid. This can further promote contact between the coating liquid and the workpiece such as an artificial blood vessel. The stirring can be performed using a known device such as an orbital shaker, a rotary shaker, or a paint shaker. The stirring conditions are not particularly limited. From the viewpoint of more efficient contact between the workpiece such as an artificial blood vessel and the first coating liquid, the stirring speed is, for example, 200 to 700 rpm. From the same viewpoint, the stirring time is, for example, 1 to 20 hours. The stirring temperature may be around room temperature (for example, 20 to 40° C.), but heating may be used as long as it is lower than the boiling point of the solvent used.

[0217] Furthermore, when forming the first layer only on a portion of the plastic substrate, the first layer can be formed on a desired surface portion of the substrate by immersing only a portion of the plastic substrate in the first coating liquid and coating the portion of the plastic substrate with the first coating liquid.

[0218] When it is difficult to immerse only a part of the plastic substrate in the first coating liquid, the surface portion of the substrate on which the first layer is not required to be formed is protected (coated, etc.) with a suitable member or material that can be attached or detached in advance, and then the substrate is immersed in the first coating liquid to coat the substrate with the first coating liquid, and the protective member (material) on the surface portion of the substrate on which the first layer is not required to be formed is removed, and then the substrate is reacted by heat treatment or the like to form the first layer on the desired surface portion of the substrate. However, the present invention is not limited to these formation methods, and the first layer can be formed by appropriately using a conventionally known method. For example, when it is difficult to immerse only a part of the plastic substrate in the first coating liquid, other coating methods (for example, a method of applying the first coating liquid to a predetermined surface portion of a medical device using an application device such as a spray device, a bar coater, a die coater, a reverse coater, a comma coater, a gravure coater, a spray coater, or a doctor knife) may be applied instead of the immersion method. When the structure of the medical device requires that both the outer and inner surfaces of a cylindrical device have the first layer, the immersion method (dipping method) is preferably used since it allows both the outer and inner surfaces to be coated at once.

[0219] The amount of the first coating liquid applied is preferably selected so that the thickness (dry film thickness) of the resulting first layer falls within the above range.

[0220] Furthermore, the first layer formed as described above is dried if necessary, and the first layer is formed on the plastic substrate. This allows the epoxy groups contained in the first copolymer to react with the surface of the plastic substrate (preferably with the hydroxyl groups and / or carboxyl groups formed by the plasma irradiation step) to support (fix) the first layer on the substrate layer. In addition, the epoxy groups of the first copolymer react with each other to increase the film strength of the first layer.

[0221] The drying treatment includes natural drying, air drying, or heat treatment. In particular, when a plastic substrate having low heat resistance is used, the drying treatment is preferably natural drying or air drying. In addition, when the heat treatment is performed, the conditions during the heat treatment are not particularly limited as long as the solvent can be removed (the first layer can be formed on the substrate), and can be appropriately selected according to the type of solvent. For example, the heat treatment temperature is preferably 40 to 150°C. In addition, the heat treatment time is preferably 30 minutes to 30 hours. Under the above conditions, the epoxy groups of the first copolymer in the coating layer react more effectively with the surface of the plastic substrate (preferably the hydroxyl groups and / or carboxyl groups formed by the plasma irradiation step), and the first copolymer can be fixed more sufficiently and firmly to the substrate. In addition, the epoxy groups of the first copolymer in the coating layer react more efficiently with each other, and the film strength of the first layer can be further increased. Therefore, a first layer with high strength that does not easily peel off from the plastic substrate can be formed.

[0222] The pressure conditions in the drying process are not limited, and the process may be carried out under normal pressure (atmospheric pressure), or may be carried out under increased or reduced pressure. As the drying (or heating) means (apparatus), for example, an oven or a reduced pressure dryer may be used, but in the case of natural drying, no particular drying means (apparatus) is required.

[0223] In this step, the first layer may be washed if necessary. Here, the washing method is not particularly limited, but may be a method of immersing the first layer in a washing solvent, a method of pouring the washing solvent over the first layer, or a combination of these. The washing solvent used at this time is not particularly limited as long as it does not dissolve the first layer, but water (e.g., ion-exchanged water, distilled water, RO water, filtered water, sterilized water, purified water, etc.) or warm water is preferably used. The temperature of the washing water is not particularly limited, but is preferably 20°C to 80°C. In addition, the washing time (the time for contacting the washing solvent with the first layer) is not particularly limited, but is preferably 1 to 60 minutes. After the above washing step, a drying step may be further performed. The drying method and drying conditions (temperature, time, etc.) are not particularly limited, and a conventionally known method can be used.

[0224] <<Second solution application process>> In this step, a solution containing the second copolymer and a solvent, and other components as necessary (also referred to simply as "second coating liquid" in this specification) is prepared, and the second coating liquid is applied onto the first layer to form the second layer on the first layer. This results in a medical device in which the first layer and the second layer are laminated in this order on the plastic substrate.

[0225] This step can be applied by replacing the first coating liquid with the second coating liquid in the first solution application step. The solvent used to prepare the second coating liquid is not particularly limited, and is appropriately selected depending on the type of the second copolymer (and other components, if used).

[0226] Moreover, the application (coating) of the second coating liquid is preferably carried out while stirring the second coating liquid, which can further strengthen the bond between the first layer and the second layer and improve adhesion.

[0227] The amount of the second coating liquid applied is preferably selected so that the thickness (dry film thickness) of the resulting second layer falls within the above range.

[0228] By the above method, a medical device having excellent antithrombotic properties can be produced.

[0229] [Medical device uses] The medical device according to the present invention has excellent antithrombotic properties. Examples of the medical device according to the present invention include implantable artificial organs and treatment devices, extracorporeal circulation artificial organs, catheters, guide wires, and the like. Among them, the medical device is preferably an intravascular device, and specific examples thereof include an artificial blood vessel, a stent, a stent graft, a covered stent, an artificial valve, a valve clip, and a pump catheter for auxiliary circulation. The medical device according to one embodiment of the present invention is an artificial blood vessel, a stent graft, a covered stent, or a catheter. Other examples of the medical device include the following: Specific examples include implantable medical devices such as artificial trachea, artificial skin, and artificial pericardium; artificial organ systems such as artificial heart systems, artificial lung systems, artificial heart-lung systems, artificial kidney systems, artificial liver systems, and immunoregulatory systems; catheters that are inserted or placed in blood vessels, such as indwelling needles, IVH catheters, catheters for administering medicinal solutions, thermodilution catheters, catheters for angiography, catheters for dilating blood vessels, dilators, or introducers; guide wires and stylets for these catheters; and catheters that are inserted or placed in biological tissues other than blood vessels, such as gastric catheters, nutrition catheters, tube feeding (ED) tubes, urethral catheters, urinary catheters, balloon catheters, and various suction catheters and drainage catheters, including endotracheal suction catheters. EXAMPLES

[0230] The effects of the present invention will be described using the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. In the following examples, the indications "parts" or "%" may be used, but unless otherwise specified, they represent "parts by mass" or "% by mass". Furthermore, unless otherwise specified, each operation was performed at room temperature (25°C).

[0231] [Synthesis Example 1-1: Synthesis of GMA-r-MEA copolymer (5 / 5)] A water bath was filled with tap water and covered with a polypropylene (PP) ball, then the water bath was placed on a magnetic stirrer and the temperature was set to 37°C.

[0232] In a 50 mL beaker, 1.48 g (10 mmol) of glycidyl methacrylate (GMA) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 1.36 g (10 mmol) of 2-methoxyethyl acrylate (MEA) (manufactured by Osaka Organic Chemical Industry Co., Ltd., 2-MTA), 0.0028 g (0.0091 mmol) of 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., V-70) as a polymerization initiator, and about 11 mL of 1,4-dioxane were added and stirred to prepare a reaction solution (the total concentration of GMA and MEA was adjusted to 20 mass%, and the polymerization initiator was 0.1 mass% relative to the total of GMA and MEA). The reaction solution prepared as above was transferred to a glass tube with a capacity of 11 mL, and the glass tube was subjected to nitrogen bubbling for 10 minutes, and then the tube was capped with a rubber stopper. The glass tube was heated in a water bath and reacted (polymerized) for about 3 hours at 37° C. in a nitrogen atmosphere, after which the glass tube was removed from the water bath and cooled to room temperature.

[0233] The reaction product obtained after the polymerization was reprecipitated using hexane, and then reprecipitation was repeated several times using acetone and hexane to purify the polymer. The recovered polymer was then vacuum dried for 16 hours to obtain a copolymer (1-1) having glycidyl methacrylate and methoxyethyl acrylate as structural units. The content ratio (molar ratio) of the structural unit (A-1) derived from glycidyl methacrylate and the structural unit (A-2) derived from methoxyethyl acrylate in the copolymer (1-1) was calculated as follows: 1 When measured by H-NMR, the ratio (GMA:MEA=5:5 (molar ratio)) was the same as the value calculated from the above-mentioned amounts. In addition, the glass transition temperature of the homopolymer (PMEA) of methoxyethyl acrylate (MEA) is -50°C (same below).

[0234] [Synthesis Example 1-2: Synthesis of GMA-r-MEA copolymer (3 / 7)] A copolymer (1-2) having glycidyl methacrylate and methoxyethyl acrylate as structural units was obtained in the same manner as in Synthesis Example 1-1, except that the amount of GMA was changed to 0.91 g (6.4 mmol) and the amount of MEA was changed to 1.94 g (15 mmol). The content ratio (molar ratio) of the structural unit (A-1) derived from glycidyl methacrylate and the structural unit (A-2) derived from methoxyethyl acrylate in the copolymer (1-2) was 1 When measured by 1 H-NMR, the ratio (GMA:MEA=3:7 (molar ratio)) was the same as the value calculated from the above-mentioned charged amounts.

[0235] [Synthesis Example 1-3: Synthesis of GMA-r-THFA copolymer (5 / 5)] In the above Synthesis Example 1-1, the amount of GMA was changed to 1.35 g (9.5 mmol), and tetrahydrofurfuryl acrylate (THFA) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of MEA, and its amount was changed to 1.49 g (9.5 mmol), but the same procedure was followed as in Synthesis Example 1-1 to obtain a copolymer (1-3) having glycidyl methacrylate and tetrahydrofurfuryl acrylate as structural units. The content ratio (molar ratio) of the structural unit (A-1) derived from glycidyl methacrylate and the structural unit (A-2) derived from tetrahydrofurfuryl acrylate in the copolymer (1-3) was 1 When measured by H-NMR, the ratio (GMA:THFA=5 / 5 (molar ratio)) was the same as the value calculated from the above-mentioned amounts. In addition, the glass transition temperature of the homopolymer (PTHFA) of tetrahydrofurfuryl acrylate (THFA) was -12°C (same below).

[0236] [Synthesis Example 1-4: Synthesis of GMA-r-THFA copolymer (3 / 7)] A copolymer (1-4) having glycidyl methacrylate and tetrahydrofurfuryl acrylate as structural units was obtained in the same manner as in Synthesis Example 1-3, except that the amount of GMA was changed to 0.80 g (5.6 mmol) and the amount of THFA was changed to 2.04 g (13 mmol). The content ratio (molar ratio) of the structural unit (A-1) derived from glycidyl methacrylate and the structural unit (A-2) derived from tetrahydrofurfuryl acrylate in the copolymer (1-4) was 1 When measured by 1 H-NMR, the ratio (GMA:THFA=3:7 (molar ratio)) was the same as the value calculated from the above-mentioned charged amounts.

[0237] [Synthesis Example 2-1: Synthesis of AMPA-r-MEA copolymer (1 / 14)] A water bath was filled with tap water and covered with a polypropylene (PP) ball.The water bath was then placed on a magnetic stirrer and the temperature was set to 80°C.

[0238] In a 250 mL three-neck flask equipped with a cooling tube, 2.00 g (11 mmol) of N-(3-aminopropyl methacrylamide) hydrochloride (APMA hydrochloride) (manufactured by Combi-Blocks), 20.24 g (156 mmol) of 2-methoxyethyl acrylate (MEA), 0.44 g (1.6 mmol) of 4,4'-azobis(4-cyanovaleric acid) (ACVA) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a polymerization initiator, and about 30 mL of 1,4-dioxane and about 20 mL of RO water were added and stirred to dissolve all the reagents (the total concentration of APMA and MEA was adjusted to 30 mass%, and the polymerization initiator was 2 mass% relative to the total concentration of APMA and MEA). Next, the mixture was heated using a water bath and reacted (polymerized) at 80°C for about 3 hours under a nitrogen atmosphere. After that, the flask was removed from the water bath and cooled to room temperature.

[0239] The reaction product obtained after the polymerization was reprecipitated using a mixed solution of hexane and isopropyl alcohol (IPA) (volume ratio of hexane:IPA = 5:5), then reprecipitated using a mixed solution of THF and ethanol (volume ratio of THF:ethanol = 4:1) and a mixed solution of hexane and isopropyl alcohol (IPA) (volume ratio of hexane:IPA = 7:3), and further reprecipitated using a mixed solution of THF and ethanol (volume ratio of THF:ethanol = 4:1) and hexane, thereby purifying the polymer. The recovered polymer was then vacuum dried for 20 hours to obtain a copolymer (2-1) having aminopropyl methacrylamide and methoxyethyl acrylate as structural units. The content ratio (molar ratio) of the structural unit (B-1) derived from aminopropyl methacrylamide and the structural unit (B-2) derived from methoxyethyl acrylate in the copolymer (2-1) was calculated as follows: 1 When measured by 1 H-NMR, the ratio (APMA:MEA=1:14 (molar ratio)) was the same as the value calculated from the above-mentioned charged amounts.

[0240] [Comparative Synthesis Example 1-1: Synthesis of GMA homopolymer (PGMA)] In a 250mL three-neck flask equipped with a cooling tube, 23.7g (167mmol) of GMA and about 92mL of 1,4-dioxane were added and stirred to dissolve all the reagents (the concentration of GMA was adjusted to 20% by mass). To this solution, a solution in which 0.024g (0.1% by mass relative to GMA) of azoisobutyronitrile (AIBN) as a polymerization initiator was dissolved in a small amount of 1,4-dioxane in advance was added, and the reaction (polymerization) was carried out under a nitrogen atmosphere at 80°C for about 3 hours. After that, the flask was removed from the water bath and cooled to room temperature.

[0241] The reaction product obtained after the polymerization was reprecipitated with methanol, and then reprecipitated with acetone and methanol to purify the polymer. The recovered polymer was vacuum dried for 10 hours to obtain a comparative polymer (1-1) (PGMA) having glycidyl methacrylate as a structural unit.

[0242] [Comparative Synthesis Example 1-2: Synthesis of GMA-r-BMA copolymer (7 / 3)] In the above Synthesis Example 1-1, the amount of GMA was changed to 1.99 g (14 mmol), and n-butyl methacrylate (BMA) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of MEA, and its amount was changed to 0.85 g (6 mmol), but the same procedure was followed as in Synthesis Example 1-1 to obtain a comparative copolymer (1-2) having glycidyl methacrylate and n-butyl methacrylate as structural units. The content ratio (molar ratio) of the structural unit (A-1) derived from glycidyl methacrylate and the structural unit (A'-2) derived from n-butyl methacrylate in the comparative copolymer (1-2) was 1 When measured by H-NMR, the ratio (GMA:BMA=7 / 3 (molar ratio)) was the same as the value calculated from the above-mentioned amounts. In addition, the glass transition temperature of the homopolymer (PBMA) of n-butyl methacrylate (BMA) is 20°C (same below).

[0243] [Comparative Synthesis Example 1-3: Synthesis of GMA-r-BMA copolymer (5 / 5)] A comparative copolymer (1-3) having glycidyl methacrylate and n-butyl methacrylate as structural units was obtained in the same manner as in Comparative Synthesis Example 1-2, except that the amount of GMA was changed to 1.42 g (10 mmol) and the amount of BMA was changed to 1.42 g (10 mmol). The content ratio (molar ratio) of the structural unit (A-1) derived from glycidyl methacrylate and the structural unit (A'-2) derived from n-butyl methacrylate in the comparative copolymer (1-3) was 1 When measured by 1 H-NMR, the ratio (GMA:BMA=5 / 5 (molar ratio)) was the same as the value calculated from the above-mentioned charged amounts.

[0244] [Comparative Synthesis Example 1-4: Synthesis of GMA-r-BMA copolymer (3 / 7)] A comparative copolymer (1-4) having glycidyl methacrylate and n-butyl methacrylate as structural units was obtained in the same manner as in Comparative Synthesis Example 1-2, except that the amount of GMA was changed to 0.85 g (6 mmol) and the amount of BMA was changed to 1.99 g (14 mmol). The content ratio (molar ratio) of the structural unit (A-1) derived from glycidyl methacrylate and the structural unit (A'-2) derived from n-butyl methacrylate in the comparative copolymer (1-4) was 1 When measured by 1 H-NMR, the ratio (GMA:BMA=3 / 7 (molar ratio)) was the same as the value calculated from the above-mentioned charged amounts.

[0245] [Production Example 1: Preparation of Adhesive Layer Sample (1)] (1) Preparation of the substrate A polyethylene terephthalate (PET) film (manufactured by Toray Industries, Inc., product name: Lumirror (registered trademark), thickness: 125 μm) was cut into a size of 1 cm × 1 cm. The film thus cut out was then immersed in ethanol for 1 minute, after which the ethanol was replaced. This operation was repeated three times for cleaning.

[0246] The above-mentioned cleaned PET film was placed in a plasma irradiation device (low-pressure plasma type) and plasma was irradiated on both sides for 3 minutes under the conditions described below. After plasma irradiation, the PET film was taken out into the atmosphere and left to stand for 30 minutes to generate hydroxyl groups (-OH) and carboxyl groups (-COOH) on the surface of the above-mentioned cleaned PET film.

[0247] (Plasma irradiation conditions) Device: Diener Electronic, Product name: Pico LF output: 200W Power: 50% Introduced gas: argon gas (100% by volume) Introduced gas flow rate: 15sccm Pressure: 0.3mbar (0.3hPa) Processing time: 3 minutes.

[0248] (2) Formation of the first layer (adhesive layer) The copolymer (1-1) obtained in the above Synthesis Example 1-1 was dissolved in acetone at a concentration of 0.1% by mass to prepare a copolymer solution (1-1). The PET film prepared above after plasma irradiation was immersed in this copolymer solution (1-1) and then immediately removed. The PET film was then removed and air-dried for 12 hours or more. As a result, a first layer (adhesive layer) was formed on the surface of the PET film, and an adhesive layer sample (1) was obtained. That is, a sample having a layer (first layer) containing a GMA-r-MEA copolymer (5 / 5 (molar ratio)) was produced.

[0249] [Production Example 2: Preparation of Adhesive Layer Sample (2)] Except for changing the copolymer (1-1) used in the above Production Example 1(2) to the copolymer (1-2) obtained in Synthesis Example 1-2, an adhesive layer sample (2) was obtained in the same manner as in Production Example 1. That is, a sample having a layer (first layer) containing a GMA-r-MEA copolymer (3 / 7 (molar ratio)) was produced.

[0250] [Production Example 3: Preparation of Adhesive Layer Sample (3)] Except for changing the copolymer (1-1) used in the above Production Example 1(2) to the copolymer (1-3) obtained in Synthesis Example 1-3, an adhesive layer sample (3) was obtained in the same manner as in Production Example 1. That is, a sample having a layer (first layer) containing a GMA-r-THFA copolymer (5 / 5 (molar ratio)) was produced.

[0251] [Production Example 4: Preparation of Adhesive Layer Sample (4)] Except for changing the copolymer (1-1) used in the above Production Example 1(2) to the copolymer (1-4) obtained in Synthesis Example 1-4, an adhesive layer sample (4) was obtained in the same manner as in Production Example 1. That is, a sample having a layer (first layer) containing a GMA-r-THFA copolymer (3 / 7 (molar ratio)) was produced.

[0252] [Comparative Manufacturing Example 1: Preparation of Comparative Adhesive Layer Sample (1)] Except for changing the copolymer (1-1) used in the above Production Example 1(2) to the comparative polymer (1-1) obtained in Comparative Synthesis Example 1-1, a comparative adhesive layer sample (1) was obtained in the same manner as in Production Example 1. That is, a sample having a layer (first layer) containing GMA homopolymer (PGMA) was produced.

[0253] [Comparative Manufacturing Example 2: Preparation of Comparative Adhesive Layer Sample (2)] A comparative adhesive layer sample (2) was obtained in the same manner as in Production Example 1, except that the copolymer (1-1) used in Production Example 1(2) was changed to the comparative copolymer (1-2) obtained in Comparative Synthesis Example 1-2. That is, a sample having a layer (first layer) containing GMA-r-BMA copolymer (7 / 3) was produced.

[0254] [Comparative Manufacturing Example 3: Preparation of Comparative Adhesive Layer Sample (3)] Except for changing the copolymer (1-1) used in the above Production Example 1(2) to the comparative copolymer (1-3) obtained in Comparative Synthesis Example 1-3, a comparative adhesive layer sample (3) was obtained in the same manner as in Production Example 1. That is, a sample having a layer (first layer) containing GMA-r-BMA copolymer (5 / 5) was produced.

[0255] [Comparative Manufacturing Example 4: Preparation of Comparative Adhesive Layer Sample (4)] A comparative adhesive layer sample (4) was obtained in the same manner as in Production Example 1, except that the copolymer (1-1) used in Production Example 1 (2) was changed to the comparative copolymer (1-4) obtained in Comparative Synthesis Example 1-4. That is, a sample having a layer (first layer) containing GMA-r-BMA copolymer (3 / 7) was produced.

[0256] <Evaluation 1: Surface observation by SEM> The surface of the adhesive layer (first layer) of each sample obtained in the above-mentioned manufacturing example and comparative manufacturing example was observed by a scanning electron microscope (instrument name: S-3400N, manufactured by Hitachi Science Systems Co., Ltd.) at a magnification of 100 times. The obtained images are shown in Figs. 3 to 10. Fig. 3 is an SEM image of the first layer (adhesive layer) of the sample obtained in manufacturing example 1 observed by a scanning electron microscope. Fig. 4 is an SEM image of the first layer (adhesive layer) of the sample obtained in manufacturing example 2 (corresponding to Example 1 below) observed by a scanning electron microscope. Fig. 5 is an SEM image of the first layer (adhesive layer) of the sample obtained in manufacturing example 3 observed by a scanning electron microscope. Fig. 6 is an SEM image of the first layer (adhesive layer) of the sample obtained in manufacturing example 4 (corresponding to Example 2 below) observed by a scanning electron microscope. Fig. 7 is an SEM image of the first layer (adhesive layer) of the sample obtained in comparative manufacturing example 1 (corresponding to Comparative Example 1 below) observed by a scanning electron microscope. Fig. 8 is an SEM image of the first layer (adhesive layer) of the sample obtained in Comparative Production Example 2, observed by a scanning electron microscope. Fig. 9 is an SEM image of the first layer (adhesive layer) of the sample obtained in Comparative Production Example 3, observed by a scanning electron microscope. Fig. 10 is an SEM image of the first layer (adhesive layer) of the sample obtained in Comparative Production Example 4, observed by a scanning electron microscope.

[0257] In Fig. 7 (adhesive layer containing PGMA) and Figs. 8 to 10 (adhesive layer containing GMA-r-BMA copolymer), aggregation was observed. Thus, it became clear that when an adhesive layer (first layer) is formed using a copolymer that does not have the structural unit (A-2) according to the present invention in addition to the structural unit (A-1) derived from a monomer having an epoxy group, aggregation occurs, making it difficult to form a smooth adhesive layer (first layer).

[0258] In contrast, as shown in Figures 3 to 6, in an adhesive layer (first layer) formed using a copolymer having the structural unit (A-2) according to the present invention in addition to the structural unit (A-1) derived from a monomer having an epoxy group, it was observed that the aggregation of the copolymer was extremely reduced. Therefore, it is presumed that the use of the first copolymer according to the present invention effectively suppresses the decrease in antithrombotic properties caused by the aggregation of the adhesive layer, and a medical device with excellent antithrombotic properties can be obtained.

[0259] In particular, in Figure 4 (adhesive layer containing GMA-r-MEA copolymer (3 / 7)) and Figure 6 (adhesive layer containing GMA-r-THFA copolymer (3 / 7)), almost no aggregation was observed, indicating that an extremely smooth adhesive layer (first layer) was formed. Therefore, by comparing Figures 3 and 4, and Figures 5 and 6, it is believed that the effect of inhibiting aggregation (and also antithrombotic properties) can be further improved by increasing the content ratio (molar ratio) of the structural unit (A-2) according to the present invention relative to the structural unit (A-1) derived from a monomer having an epoxy group.

[0260] [Example 1: Preparation of biocompatible layer sample (1)] The copolymer (2-1) obtained in the above Synthesis Example 2-1 was dissolved in RO water at a concentration of 1% by mass to prepare a copolymer solution (2-1). 10 mL of this copolymer solution (2-1) was transferred to a Falcon (registered trademark) tube, and the adhesive layer sample (2) prepared in the above Production Example 2 was added to the tube. Then, the mixture was stirred at a speed of 400 rpm at room temperature for 16 hours with an orbital shaker (manufactured by Nisshin Rika Co., Ltd., product name: ROTARY SHAKER NX-20), and the sample was taken out of the tube. Next, the sample was left to stand (immersed) in RO water for 5 minutes, and the RO water was replaced with new water for cleaning. After that, this cleaning operation was repeated three times, and the sample was taken out of the RO water, left to stand at room temperature and dried to obtain a biocompatible layer sample (1). That is, a sample (1) was prepared in which a biocompatible layer was formed on a PET film via a layer containing GMA-r-MEA copolymer (3 / 7) as an adhesive layer (first layer).

[0261] [Example 2: Preparation of biocompatible layer sample (2)] A biocompatible layer sample (2) was obtained in the same manner as in Example 1, except that the adhesive layer sample (2) in Example 1 was changed to the adhesive layer sample (4) obtained in Production Example 4. A biocompatible layer sample (2) was produced on a PET film via a layer containing GMA-r-THFA copolymer (3 / 7) as an adhesive layer (first layer).

[0262] [Reference Example 1: Preparation of Comparative Biocompatible Layer Sample (1)] An untreated PET film (not subjected to the plasma treatment as in Production Example 1(1) above) was used as it was as an evaluation sample (Reference Example 1).

[0263] [Comparative Example 1: Preparation of Comparative Biocompatible Layer Sample (2)] A comparative biocompatible layer sample (1) was obtained in the same manner as in Example 1, except that the comparative adhesive layer sample (1) prepared in the above Comparative Production Example 1 was used instead of the adhesive layer sample (2) in Example 1. That is, a comparative sample (1) was produced in which a biocompatible layer was formed on a PET film via a layer containing PGMA as an adhesive layer (first layer).

[0264] <Evaluation 2: Platelet adhesion test (antithrombogenic test)> For each sample obtained in the above examples and comparative examples, a platelet adhesion test was performed according to the following procedure to evaluate the antithrombotic properties. An aqueous solution of 3.2 (w / v)% sodium citrate (anticoagulant) was added to fresh porcine blood to obtain anticoagulated fresh porcine blood (1). At this time, the fresh porcine blood and the aqueous sodium citrate solution were mixed at a mixing ratio (volume ratio) of 9:1. A 1M calcium chloride solution and a 1000U / mL heparin solution were dispensed into a 15mL Falcon tube to prepare a mixed solution. This mixed solution was added to the anticoagulated fresh porcine blood (1) and stirred slowly without foaming to obtain anticoagulated fresh porcine blood (2). At this time, the anticoagulated fresh porcine blood (2) was mixed so that 820μL of the 1M calcium chloride solution and 100μL (100U) of the 1000U / mL heparin solution were contained in 50mL of the anticoagulated fresh porcine blood (2). The final concentration of heparin in the anticoagulated fresh porcine blood (2) was 2.0 U / mL. 100 μL of anticoagulated fresh porcine blood (2) was centrifuged (1500 × g) at 22 ° C for 10 minutes to separate platelet-rich plasma (PRP). This PRP was filled into each cylindrical container with the above samples attached to the bottom, and left at room temperature for 5 hours. Then, each sample was washed with 3.2 wt% sodium citrate / phosphate buffer solution (PBS) (= 1 / 9) solution and fixed with 1 (w / v) % glutaraldehyde PBS solution. After leaving it to stand overnight in a refrigerator (4 ° C), the glutaraldehyde PBS solution was removed with a pipette tube, and then washed 7 times with RO water. Each sample was left to stand at room temperature and dried. The dried sample was fixed to a stainless steel plate, platinum was evaporated by platinum sputtering, and then observed and photographed (1000 times) with a scanning electron microscope (SEM). The number of adherent platelets was counted for each photograph and calculated in total for the five fields of view. The results are shown in Table 1 below.

[0265] [Table 1]

[0266] As a result, it was confirmed that both samples (Examples 1 and 2) having GMA-r-MEA copolymer or GMA-r-THFA copolymer as the adhesive layer (first layer) had excellent platelet adhesion inhibitory effect (antithrombotic effect). [Explanation of symbols]

[0267] 10...Base material, 10a...substrate core portion, 10b...base material surface layer, 11...1st layer (adhesive layer), 12...Second layer (biocompatible layer), 100...Medical equipment.

Claims

1. A medical device comprising a plastic substrate, a first layer supported on at least a portion of the plastic substrate, and a second layer supported on at least a portion of the first layer, the first layer comprises a first copolymer having a structural unit (A-1) derived from a monomer (a-1) having an epoxy group and a structural unit (A-2) derived from a monomer (a-2) having a homopolymer glass transition temperature of less than −10° C.; The second layer comprises a second copolymer having a structural unit (B-1) derived from a monomer (b-1) capable of bonding to an epoxy group contained in the structural unit (A-1), and a structural unit (B-2) derived from an antithrombotic monomer (b-2).

2. The monomer (a-2) is represented by the following formula (I): 【Chemistry 1】 In the above formula (I), R 1 represents a hydrogen atom or a methyl group, X 1 Is -O-(R 2 O) m -R 3 or a tetrahydrofurfuryloxy group, R 2 each independently represents a linear or branched alkylene group having 1 to 4 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 4 carbon atoms, and m represents an integer of 1 to 5; The medical device according to claim 1 , wherein the monomer is one or more monomers represented by the following formula:

3. The monomer (a-2) is represented by the formula (I), R 1 represents a hydrogen atom or a methyl group, X 1 Is -O-(R 2 O) m -R 3 represents R 2 represents a linear or branched alkylene group having 1 to 4 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 4 carbon atoms, and m is 1;

4. The medical device according to claim 1, wherein the epoxy group-containing monomer (a-1) includes at least one selected from the group consisting of glycidyl acrylate, glycidyl methacrylate (GMA), 3,4-epoxycyclohexylmethyl acrylate, 3,4-epoxycyclohexylmethyl methacrylate, β-methylglycidyl acrylate, and β-methylglycidyl methacrylate.

5. The medical device according to claim 1, wherein the first copolymer is a random copolymer having a segment having the structural unit (A-1) and a segment having the structural unit (A-2).

6. The medical device according to claim 1, wherein the first copolymer contains the structural unit (A-1) and the structural unit (A-2) in a molar ratio ((A-1):(A-2)) of 2:8 to 6:

4.

7. The monomer (b-1) has a primary amino group (-NH 2 2. The medical device according to claim 1, comprising at least one functional group selected from the group consisting of a carboxyl group (--COOH), a carboxyl group (--COOH), and a hydroxyl group (--OH).

8. The medical device according to claim 1, wherein the monomer (b-1) is one or more selected from monomers represented by the following formulas (II) and (III) and salts thereof: 【Chemistry 2】 In the above formula (II), R 4 represents a hydrogen atom or a methyl group, p represents an integer of 1 to 4; 【Chemistry 3】 In the above formula (III), R 5 represents a hydrogen atom or a methyl group, q represents an integer of 1 to 4.

9. The antithrombotic monomer (b-2) is represented by the following formula (IV): 【Chemistry 4】 In the above formula (IV), R 6 represents a hydrogen atom or a methyl group, X 2 Is -O-(R 7 O) n -R 8 or a tetrahydrofurfuryloxy group, R 7 each independently represents a linear or branched alkylene group having 1 to 4 carbon atoms; R 8 represents a linear or branched alkyl group having 1 to 4 carbon atoms, and n represents an integer of 1 to 5; The medical device according to claim 1 , wherein the monomer is one or more monomers represented by the following formula:

10. The medical device according to claim 1 , wherein the antithrombotic monomer (b-2) is the same as the monomer (a-2).

11. 2. The medical device according to claim 1, wherein the first copolymer has a total content of the structural units (A-1) and (A-2) of 95 mol % or more.

12. 2. The medical device according to claim 1, wherein the second copolymer has a total content of the structural units (B-1) and (B-2) of 95 mol % or more.

13. The medical device according to claim 1 , wherein the plastic is at least one selected from the group consisting of polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), and polybutylene terephthalate (PBT).

14. The medical device according to claim 1 , which is an artificial blood vessel, a stent graft, a covered stent or a catheter.

15. contacting at least a portion of the plastic substrate with the first copolymer to form the first layer; and The method for producing the medical device according to any one of claims 1 to 14, comprising contacting at least a portion of the first layer with the second copolymer to form the second layer.

16. 16. The method of claim 15, further comprising exposing the plastic substrate to a plasma prior to contacting the plastic substrate with the first copolymer.