Secondary battery binder composition, electrode composition, electrode sheet, secondary battery, production method for electrode sheet, and production method for secondary battery

The use of a copolymer-based binder with water-soluble and hydrophobic vinyl compounds addresses conductivity and adhesion issues in silicon-based secondary batteries, enhancing cycle life and performance.

JP2024143601AInactive Publication Date: 2024-10-11FUJIFILM CORP

Patent Information

Application Number
JP2023056364
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Secondary batteries using silicon-based active materials in the negative electrode face challenges in maintaining conductivity and adhesion due to significant volume changes during charging and discharging, leading to impaired cycle characteristics and manufacturing issues.

Method used

A binder composition for secondary batteries comprising a copolymer with a water-soluble vinyl compound and a hydrophobic vinyl compound, along with a surfactant component, which enhances adhesion and flexibility, ensuring effective binding even with large volume changes.

Benefits of technology

The binder composition significantly improves the adhesion of electrode sheets and cycle characteristics of secondary batteries, extending their life and maintaining performance under repeated charging and discharging cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143601000009
    Figure 2024143601000009
  • Figure 2024143601000001
    Figure 2024143601000001
  • Figure 2024143601000002
    Figure 2024143601000002
Patent Text Reader

Abstract

To provide: a secondary battery binder composition and an electrode composition, which, even when an electrode active material having a large volume change during charging / discharging is used, are capable of sufficiently improving adhesion of an obtained electrode sheet and also capable of sufficiently improving cycle characteristics of an obtained secondary battery; an electrode sheet and a secondary battery in which the electrode composition is used; and a manufacturing method for each of the electrode sheet and the secondary battery.SOLUTION: There are provided: a secondary battery binder composition including a liquid medium and a copolymer X; an electrode composition; an electrode sheet and a secondary battery; and production methods for the electrode sheet and the secondary battery. The secondary battery binder composition contains, as constituents of the copolymer X, (A) a water-soluble vinyl compound component, and (B) a hydrophobic vinyl compound component. When a homopolymer (a) comprising the (A) water-soluble vinyl compound component is assumed, the homopolymer (a) has a glass transition temperature of 90°C or above, and when a homopolymer (b) comprising the (B) hydrophobic vinyl compound component is assumed, the homopolymer (b) has a glass transition temperature of 0°C or below.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a binder composition for a secondary battery, a composition for an electrode, an electrode sheet, a secondary battery, a method for producing an electrode sheet, and a method for producing a secondary battery. [Background technology]

[0002] Secondary batteries, such as lithium-ion secondary batteries, are used as power sources for portable electronic devices such as personal computers, video cameras, mobile phones, etc. Recently, against the backdrop of the global environmental challenge of reducing carbon dioxide emissions, they have become widespread as power sources for transportation equipment such as automobiles, and for storing electricity such as nighttime electricity and electricity generated by natural energy sources.

[0003] The electrodes (positive and negative electrodes) of a secondary battery generally have electrode active material layers (positive and negative active material layers), and these electrode active material layers contain electrode active material particles capable of absorbing or releasing ions during charging and discharging. The electrode active material layers also contain conductive assistants and the like as necessary. The electrode active material, conductive assistants, and the like are so-called solid particles, and the electrical continuity (adhesion) between the solid particles is easily impaired by the expansion and contraction of the electrode active material particles accompanying charging and discharging (absorbing and releasing ions) of the secondary battery. If the electrical continuity is impaired, the internal resistance of the battery increases and the battery capacity decreases. In order to improve the cycle characteristics of the secondary battery (to extend the cycle life), it is important to be able to maintain the electrical continuity between the solid particles even after repeated charging and discharging, and the electrode active material layers usually contain a binder.

[0004] In recent years, with the expansion of the use of secondary batteries, secondary batteries are required to have higher energy density (higher capacity) and further improved cycle characteristics. In order to realize a further high capacity of secondary batteries, the use of silicon-based active materials as negative electrode active materials has been studied. However, silicon-based active materials absorb a large amount of ions during charging and expand significantly, so that the contraction range of the silicon-based active material during discharging is also large. That is, secondary batteries using silicon-based active materials as negative electrode active materials have a large volume change of the negative electrode active material during charging and discharging. Therefore, the conduction state between solid particles (electrode active material, conductive assistant, etc.) is easily impaired, and peeling between the negative electrode active material layer and the current collector is also easily caused. Therefore, high-capacity secondary batteries using silicon-based active materials as negative electrode active materials are prone to deterioration of battery performance due to repeated charging and discharging, and there are limitations in improving cycle characteristics.

[0005] In high-capacity secondary batteries that contain a silicon-based active material in the negative electrode active material layer, there have been attempts to address the above-mentioned limitations in improving cycle characteristics. For example, Patent Document 1 describes an invention relating to a binder for secondary batteries, which comprises a water-soluble block polymer having, in the polymer main chain, a segment A made of a chain-polymerized polymer having a glass transition temperature of 150° C. or higher, and a segment B made of a chain-polymerized polymer having a glass transition temperature of less than 150° C. According to Patent Document 1, this binder for secondary batteries can firmly bind solid particles together, and it is said that in a secondary battery having an electrode produced using this binder for secondary batteries, the cycle life of the secondary battery can be sufficiently extended even when an electrode active material that undergoes a large volume change during charging and discharging is used.

[0006] Patent Document 2 describes an invention of a silicon electrode binder, which includes a copolymer having a first monomer unit having a homopolymer glass transition temperature of 80° C. or higher, a second monomer unit having a homopolymer glass transition temperature of 70° C. or lower, and a third monomer unit having a water solubility of less than 5% at room temperature. According to Patent Document 2, by applying the silicon electrode binder to a negative electrode active material layer containing a silicon-based active material (silicon-based active material), it is possible to increase the binding strength between active materials and also increase the adhesive strength of the negative electrode active material layer to the current collector, and as a result, it is said that the above problems associated with repeated charging and discharging can be addressed. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication No. 2022 / 210737 [Patent Document 2] Special Publication No. 2020-533771 Summary of the Invention [Problem to be solved by the invention]

[0008] In a secondary battery containing a silicon-based active material in the negative electrode active material layer, in order to improve the cycle characteristics, it is considered to use a binder with a high elastic modulus (hardness) so that even if the volume of the electrode active material particles changes, it is difficult for it to affect the volume of the negative electrode active material layer. However, if the binder is made highly elastic, the flexibility is impaired and the adhesion with the current collector tends to be impaired. Therefore, the use of a highly elastic binder tends to reduce the process suitability of battery production, for example, in the case of producing a wound type secondary battery, in which the electrode is easily damaged. In the technology described in Patent Documents 1 and 2, a component derived from a water-soluble acrylic monomer whose homopolymer has a relatively high elasticity is incorporated into a polymer together with other components, and the obtained polymer is used as a binder. By using these binders, it is possible to improve the cycle characteristics while ensuring the flexibility of the electrode to a certain extent. On the other hand, with the expansion of the applications of secondary batteries, it is becoming necessary to achieve both improved cycle characteristics (improved battery performance) and improved process suitability (improved manufacturing efficiency) at a higher level.

[0009] An object of the present invention is to provide a binder composition for secondary batteries and a composition for electrodes that can sufficiently increase the adhesion of the resulting electrode sheet (adhesion between the electrode active material layer and the current collector) and can sufficiently increase the cycle characteristics of the resulting secondary battery (sufficiently prolong the cycle life) even when an electrode active material that undergoes a large volume change during charging and discharging is used. Another object of the present invention is to provide an electrode sheet and a secondary battery using the electrode composition. Another object of the present invention is to provide methods for producing the electrode sheet and the secondary battery. [Means for solving the problem]

[0010] That is, the above-mentioned object of the present invention has been achieved by the following means. [1] A binder composition for a secondary battery comprising a liquid medium and a copolymer X, The binder composition for a secondary battery contains (A) a water-soluble vinyl compound component and (B) a hydrophobic vinyl compound component as constituent components of the copolymer X, A binder composition for a secondary battery, in which, when the (A) homopolymer a composed of the water-soluble vinyl compound component is assumed, the homopolymer a has a glass transition temperature of 90°C or higher, and when the (B) homopolymer b composed of the hydrophobic vinyl compound component is assumed, the homopolymer b has a glass transition temperature of 0°C or lower. [2] The binder composition for a secondary battery according to [1], wherein the binder composition for a secondary battery contains a surfactant component (C). [3] The binder composition for a secondary battery according to [2], comprising the surfactant component (C) as a constituent of the copolymer X. [4] The binder composition for secondary batteries according to any one of [1] to [3], wherein the (A) water-soluble vinyl compound component is a (meth)acrylamide component. [5] The binder composition for a secondary battery according to any one of [1] to [4], wherein the copolymer X has a breaking elongation of 15% or more. [6] The binder composition for a secondary battery according to any one of [1] to [5], wherein the binder composition for a secondary battery contains a water-soluble polymer. [7] The binder composition for a secondary battery according to [6], wherein the water-soluble polymer comprises at least one of carboxymethyl cellulose, cellulose nanofiber, hydroxyethyl cellulose, hydroxypropyl cellulose, and xanthan gum. [8] The binder composition for a secondary battery according to any one of [1] to [7], wherein the liquid medium is water. [9] A composition for an electrode comprising a liquid medium, a copolymer X, and an active material, The copolymer X contains, as constituent components, (A) a water-soluble vinyl compound component and (B) a hydrophobic vinyl compound component, A composition for an electrode, in which, when the above (A) homopolymer a composed of a water-soluble vinyl compound component is assumed, the glass transition temperature of the homopolymer a is 90°C or higher, and when the above (B) homopolymer b composed of a hydrophobic vinyl compound component is assumed, the glass transition temperature of the homopolymer b is 0°C or lower.

[10] The electrode composition according to [9], wherein the active material comprises a silicon-based active material.

[11] An electrode sheet having a layer formed using the electrode composition according to [9] or

[10] .

[12] A secondary battery having a positive electrode active material layer, a separator, and a negative electrode active material layer in this order, A secondary battery, wherein at least one of the positive electrode active material layer and the negative electrode active material layer is a layer formed using the electrode composition according to [9] or

[10] .

[13] A method for producing an electrode sheet, comprising forming an electrode active material layer using the electrode composition according to [9] or

[10] .

[14] A method for producing a secondary battery, comprising incorporating an electrode sheet obtained by the method for producing a secondary battery according to

[13] as an electrode of the secondary battery.

[0011] In the present invention, a numerical range expressed using "to" means a range including the numerical values ​​before and after "to" as the lower and upper limits. In the present invention, one type of each component may be contained, or two or more types may be contained. In the present invention, (meth)acrylic means one or both of acrylic and methacrylic, and the same applies to (meth)acrylic acid, (meth)acrylamide, (meth)acrylic acid alkyl ester, etc. In the present invention, the term "secondary battery" refers to a device in general in which ions pass between positive and negative electrodes via an electrolyte by charging and discharging, and energy is stored and released at the positive and negative electrodes. That is, the term "secondary battery" in the present invention includes both batteries and capacitors (e.g., lithium ion capacitors). From the viewpoint of the amount of energy stored, it is preferable that the secondary battery of the present invention is used for battery applications (not as a capacitor). Secondary batteries can be broadly divided into aqueous secondary batteries and nonaqueous secondary batteries according to the electrolyte used, and in the present invention, nonaqueous secondary batteries are preferred. In the present invention, the term "aqueous secondary battery" refers to a secondary battery using an aqueous electrolyte as an electrolyte. In the present invention, the term "nonaqueous secondary battery" refers to a nonaqueous electrolyte secondary battery and an all-solid-state secondary battery. In the present invention, the term "nonaqueous electrolyte secondary battery" refers to a secondary battery using a nonaqueous electrolyte as an electrolyte. In the present invention, the term "nonaqueous electrolyte" refers to an electrolyte that does not substantially contain water. The term "electrolyte that does not substantially contain water" means that the "nonaqueous electrolyte" may contain a small amount of water within a range that does not impede the effects of the present invention. In the present invention, the "nonaqueous electrolyte" has a water concentration of 200 ppm (by mass) or less, preferably 100 ppm or less, and more preferably 20 ppm or less. Note that it is practically difficult to make a nonaqueous electrolyte completely anhydrous, and it usually contains 1 ppm or more of water. In the present invention, the term "all-solid-state secondary battery" refers to a secondary battery that does not use a liquid electrolyte, but uses a solid electrolyte such as an inorganic solid electrolyte or a solid polymer electrolyte. In the present invention, the terms "solid content" and "total solid content" used when describing the content or content ratio refer to components other than the liquid medium described below. Effect of the Invention

[0012] The binder composition for secondary batteries and the electrode composition of the present invention can sufficiently increase the adhesion of the obtained electrode sheet and sufficiently increase the cycle characteristics of the obtained secondary battery, even when an electrode active material that undergoes a large volume change during charging and discharging is used. The electrode sheet of the present invention has excellent adhesion. According to the method for producing an electrode sheet of the present invention, the electrode sheet of the present invention can be obtained. Also, according to the method for producing a secondary battery of the present invention, the secondary battery of the present invention can be obtained. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a vertical cross-sectional view showing a schematic diagram of a basic layered structure of an embodiment of a secondary battery according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] [Binder composition for secondary batteries] The binder composition for secondary batteries of the present invention (hereinafter also referred to as "the binder composition of the present invention") contains a liquid medium and a copolymer X, which is a copolymer having a specific constituent composition. This copolymer X contains (A) a water-soluble vinyl compound component and (B) a hydrophobic vinyl compound component as constituent components, and when a homopolymer a made of the (A) water-soluble vinyl compound component is assumed, the glass transition temperature of this homopolymer a is 90°C or higher, and when a homopolymer b made of the (B) hydrophobic vinyl compound component is assumed, the glass transition temperature of this homopolymer b is 0°C or lower. The binder composition of the present invention is preferably suitable as a material for forming a member or a constituent layer constituting a non-aqueous secondary battery, more preferably a non-aqueous electrolyte secondary battery. The binder composition of the present invention preferably contains water as a liquid medium. Typically, the binder composition of the present invention can be suitably used for forming an electrode active material layer in an electrode of a secondary battery. For example, the binder composition of the present invention can be used for forming an electrode (positive electrode or negative electrode) active material layer of a non-aqueous secondary battery by containing an electrode active material (positive electrode active material or negative electrode active material, collectively referred to simply as "active material").

[0015] The copolymer X contained in the binder composition of the present invention is considered to function, for example, as a binder that mainly binds solid particles (electrode active material, conductive assistant, etc.) to each other in a layer formed by mixing the binder composition of the present invention with solid particles. It can also function as a binder that binds a current collector to solid particles. The adsorption of the copolymer X to the solid particles and current collector includes not only physical adsorption but also chemical adsorption (adsorption by the formation of chemical bonds, adsorption by the transfer of electrons, etc.).

[0016] The binder composition of the present invention can be used, for example, to prepare an electrode sheet containing an active material and apply it to the electrode of a secondary battery, thereby increasing the adhesion of the electrode sheet and improving the cycle characteristics of the secondary battery. The reason for this is unclear, but one of the reasons is thought to be that the copolymer X has a unique physical property of both hardness and flexibility due to the presence of a component derived from a water-soluble vinyl compound and a component derived from a hydrophobic vinyl compound in its structure, and thus effectively suppresses the volume change of the electrode active material layer while fully bringing out the adhesion of the obtained electrode active material layer to the current collector.

[0017] <Copolymer X> Copolymer X contains (A) a water-soluble vinyl compound component and (B) a hydrophobic vinyl compound component as its constituent components. That is, copolymer X is a copolymer obtained by copolymerizing at least a water-soluble vinyl compound that derives (A) the water-soluble vinyl compound component (hereinafter sometimes referred to as a "water-soluble vinyl compound" or a "monomer that derives (A) the water-soluble vinyl compound component") and a hydrophobic vinyl compound that derives (B) the hydrophobic vinyl compound component (hereinafter sometimes referred to as a "hydrophobic vinyl compound" or a "monomer that derives (B) the hydrophobic vinyl compound component") as monomers. Copolymer X may further contain other components in addition to these constituent components. Examples of other components include (C) a surfactant component described later. In the present invention, the term "vinyl compound" refers to a compound having an unsaturated double bond, and includes not only compounds having a vinyl group but also compounds having the structure R2C=CR2 (R is a hydrogen atom or a substituent). A "vinyl compound" is typically CH2=CH- * It is a compound having the structure ( * is the join, and so on). In the present invention, the term "water-soluble vinyl compound component" refers to a component in which the ClogP value of the water-soluble vinyl compound from which the water-soluble vinyl compound component is derived is less than 1.00. In addition, in the present invention, the term "hydrophobic vinyl compound component" refers to a component in which the ClogP value of the hydrophobic vinyl compound from which the hydrophobic vinyl compound component is derived is 1.00 or more. In the present invention, the above ClogP value is calculated from the structural formula of the compound using ChemDraw (registered trademark, molecular structural formula editor software, manufactured by PerkinElmer Co., Ltd.), and the calculated value is rounded off to two decimal places. The smaller the ClogP value, the higher the hydrophilicity. The copolymer X may be a random copolymer or a block copolymer, and is preferably a random copolymer.

[0018] -(A) Water-soluble vinyl compound component- The (A) water-soluble vinyl compound component is a constituent component derived from a water-soluble vinyl compound, and may be a component in which the homopolymer a (homopolymer of a water-soluble vinyl compound) consisting of this component has a glass transition temperature of 90° C. or higher. By including a water-soluble vinyl compound component exhibiting the above glass transition temperature, it is possible to impart a desired high elasticity (hardness) to the copolymer X. The glass transition temperature of the homopolymer a is preferably 100°C or higher, more preferably 110°C or higher, even more preferably 120°C or higher, still more preferably 130°C or higher, even more preferably 140°C or higher, still more preferably 150°C or higher, and particularly preferably 160°C or higher. The upper limit of the glass transition temperature of the homopolymer a is not particularly limited, but is practically 250° C. Therefore, the glass transition temperature of the homopolymer a is preferably 100 to 250° C., more preferably 110 to 250° C., further preferably 120 to 250° C., still more preferably 130 to 250° C., still more preferably 140 to 250° C., still more preferably 150 to 250° C., and particularly preferably 160 to 250° C.

[0019] The homopolymer a can be obtained by polymerizing (A) a monomer leading to a water-soluble vinyl compound by the method described in the Examples. The glass transition temperature of the homopolymer a can be determined by the method described in the Examples.

[0020] The (A) water-soluble vinyl compound component may be one type or two types. When a plurality of (A) water-soluble vinyl compound components are used, the glass transition temperature (Tg) of each of the water-soluble vinyl compound components is 90° C. or higher. The vinyl group in the water-soluble vinyl compound is a methacryloyl group (CH2=C(CH3)-COO- * ), acryloyl group (CH2=CHCOO- * ), or an allyl group (CH2=CH-CH2- * ) is preferably included. The water-soluble vinyl compound is preferably a vinyl compound having a hydrophilic group, and the hydrophilic group is preferably a hydroxy group, an amino group, or the like. As the (A) water-soluble vinyl compound component, for example, an acrylonitrile component, an unsaturated carboxylic acid component (such as (meth)acrylic acid, maleic acid, itaconic acid, and fumaric acid), a (meth)acrylamide component (such as (meth)acrylamide, N-methyl(meth)acrylamide), etc. are preferable. In addition, the unsaturated carboxylic acid component may be in the form of a salt such as a sodium salt, a lithium salt, or a potassium salt (an embodiment in which a carboxy group of the unsaturated carboxylic acid component forms a salt structure). The (A) water-soluble vinyl compound component is preferably a (meth)acrylamide component, and more preferably an acrylamide component. The water-soluble vinyl compound preferably has a molecular weight (Mw) of 50-200.

[0021] Preferred specific examples of the water-soluble vinyl compound are shown below, together with their Mw, Tg and ClogP values ​​(calculated by Chemdraw and rounded off to the second decimal place).

[0022] [ka]

[0023] -(B) Hydrophobic vinyl compound component- The hydrophobic vinyl compound from which the hydrophobic vinyl compound component (B) is derived may be any component that is hydrophobic and has a Tg of the homopolymer b of 0° C. or less. The hydrophobic vinyl compound component is considered to contribute to imparting flexibility to the copolymer X. The Tg of the homopolymer b is preferably −20° C. or lower, more preferably −30° C. or lower, even more preferably −40° C. or lower, still more preferably −50° C. or lower, still more preferably −60° C. or lower, and particularly preferably −70° C. or lower. From the viewpoint of increasing the discharge capacity retention rate of the resulting battery, a lower Tg is preferable. The lower limit of Tg of the homopolymer b is not particularly limited, but is practically −80° C. Therefore, the Tg of the homopolymer b is preferably −80 to −20° C., more preferably −80 to −30° C., further preferably −80 to −40° C., further preferably −80 to −50° C., and particularly preferably −80 to −60° C. The number of types of (B) hydrophobic vinyl compound components may be one or two. When a plurality of types of (B) hydrophobic vinyl compound components are used, the glass transition temperature is measured for each of the hydrophobic vinyl compound components. The homopolymer b can be obtained by polymerizing (B) a monomer which leads to a hydrophobic vinyl compound, by the method described in the Examples. The glass transition temperature of the homopolymer b can be determined by the method described in the Examples.

[0024] The vinyl group in the hydrophobic vinyl compound is a methacryloyl group (CH2=C(CH3)-COO- * ), acryloyl group (CH2=CHCOO- * ), or an allyl group (CH2=CH-CH2- * ) and more preferably in the form of an acryloyl group (CH2=CHCOO-). The hydrophobic vinyl compound is not particularly limited as long as it leads to a component exhibiting the above-mentioned properties, and for example, (meth)acrylic acid alkyl ester is preferable. The number of carbon atoms in the alkyl group of the alkyl ester moiety is preferably 2 to 16, more preferably 4 to 14, and even more preferably 6 to 14. The alkyl group may have a substituent. The substituent is preferably an aryl group or an aryloxy group. The hydrophobic vinyl compound from which the hydrophobic vinyl compound component (B) is derived preferably has a molecular weight (Mw) of 50-300.

[0025] Preferred specific examples of hydrophobic vinyl compounds are shown below, together with their Mw, Tg and ClogP values ​​(calculated by Chemdraw and rounded off to the second decimal place).

[0026] [ka]

[0027] Copolymer X may contain a component other than the water-soluble vinyl compound component (A) and the hydrophobic vinyl compound component (B). As such a component other than the water-soluble vinyl compound component (A) and the hydrophobic vinyl compound component (B), for example, a surfactant component (C) may be contained in copolymer X. The surfactant component (C) will be described later.

[0028] The copolymer X can be obtained by a conventional polymer synthesis method (polymerization method) except that (A) a water-soluble vinyl compound that leads to a water-soluble vinyl compound component and (B) a hydrophobic vinyl compound that leads to a hydrophobic vinyl compound component are combined and copolymerized. The synthesis method and conditions are not particularly limited, and conventional methods and conditions can be appropriately applied depending on the purpose. The synthesis is preferably carried out in the presence of the surfactant component (C) described below. By carrying out the synthesis in the presence of the surfactant (C), the dispersibility of the water-soluble vinyl compound and the hydrophobic vinyl compound can be increased, and the synthesis reaction (polymerization reaction) can be carried out smoothly. Therefore, the ratio of the hydrophobic vinyl compound component (B) in the structure of the copolymer X can be further increased. In this case, the surfactant component (C) may be present as a constituent component of the copolymer X (polymerizable surfactant component (C-1)). In addition, the surfactant component (C) may be present in the composition as an independent component (non-polymerizable surfactant component (C-2)) different from the copolymer X.

[0029] In the copolymer X, the proportion of the water-soluble vinyl compound component (A) in the total of the water-soluble vinyl compound component (A) and the hydrophobic vinyl compound component (B) is preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, even more preferably 15% by mass or more, even more preferably 20% by mass or more, and particularly preferably 25% by mass or more. This proportion is preferably 99% by mass or less, more preferably 95% by mass or less, even more preferably 90% by mass or less, even more preferably 80% by mass or less, even more preferably 70% by mass or less, even more preferably 60% by mass or less, even more preferably 55% by mass or less, even more preferably 50% by mass or less, even more preferably 45% by mass or less, and particularly preferably 40% by mass or less. Furthermore, this ratio is preferably 1 to 99% by mass, more preferably 5 to 95% by mass, even more preferably 10 to 90% by mass, still more preferably 15 to 80% by mass, even more preferably 15 to 70% by mass, still more preferably 20 to 60% by mass, and particularly preferably 25 to 55% by mass. This ratio is also preferably 10 to 50% by mass, also preferably 15 to 50% by mass, also preferably 15 to 45% by mass, and also preferably 20 to 45% by mass. In the copolymer X, the ratio of the hydrophobic vinyl compound component (B) to the total of the water-soluble vinyl compound component (A) and the hydrophobic vinyl compound component (B) is preferably 1% by mass or more, more preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, even more preferably 30% by mass or more, even more preferably 40% by mass or more, even more preferably 45% by mass or more, even more preferably 50% by mass or more, even more preferably 55% by mass or more, and particularly preferably 60% by mass or more. This ratio is preferably 99% by mass or less, more preferably 95% by mass or less, even more preferably 90% by mass or less, even more preferably 85% by mass or less, even more preferably 80% by mass or less, and particularly preferably 75% by mass or less. Furthermore, this ratio is preferably 1 to 99% by mass, more preferably 5 to 95% by mass, even more preferably 10 to 90% by mass, still more preferably 20 to 85% by mass, even more preferably 30 to 85% by mass, still more preferably 40 to 80% by mass, and particularly preferably 45 to 75% by mass. This ratio is also preferably 50 to 90% by mass, also preferably 50 to 85% by mass, also preferably 55 to 85% by mass, and also preferably 55 to 80% by mass. When copolymer X contains a polymerizable surfactant component (C-1), the content of the polymerizable surfactant component (C-1) in copolymer X is preferably 5 mass % or less, more preferably 0.2 to 5 mass %, even more preferably 0.4 to 3 mass %, and still more preferably 0.6 to 2 mass %, based on the total content of all components in copolymer X (the total of the water-soluble vinyl compound component (A), the hydrophobic vinyl compound component (B), the polymerizable surfactant component (C-1), and other components as needed). When copolymer X contains another component in addition to (A) the water-soluble vinyl compound component, (B) the hydrophobic vinyl compound component, and (C-1) the polymerizable surfactant component, the content of the other component is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less, based on the total content of all the components in copolymer X.

[0030] -Characteristics of Copolymer X- The copolymer X preferably has a breaking elongation of 5% or more, more preferably 15% or more. From the viewpoint of effectively suppressing the volume change of the obtained electrode active material layer and improving the adhesion to the current collector, a higher breaking elongation is preferable. The breaking elongation can be calculated by carrying out a tensile test according to the method described in the Examples.

[0031] The weight average molecular weight (Mw) of the copolymer X is not particularly limited, but is preferably from 100,000 to 900,000, and more preferably from 200,000 to 500,000.

[0032] (Measurement of weight average molecular weight) In the present invention, the molecular weight of the polymer contained in the binder composition is measured by gel permeation chromatography (GPC). The molecular weight means the weight average molecular weight in terms of sodium polyacrylate, and is a value measured under the following measurement conditions 1 or 2. Depending on the type of polymer, an appropriate eluent can be selected and used. (Measurement condition 1) Measuring instrument: HLC-8220GPC (product name, manufactured by Tosoh Corporation) Columns: TOSOH TSKgel 5000PWXL (product name, manufactured by Tosoh Corporation), TOSOH TSKgel G4000PWXL (product name, manufactured by Tosoh Corporation), and TOSOH TSKgel G2500PWXL (product name, manufactured by Tosoh Corporation) are connected together. Carrier: 200mM sodium nitrate aqueous solution Measurement temperature: 40℃ Carrier flow rate: 1.0mL / min Sample concentration: 0.2% by mass Detector: RI (refractive index) detector If the molecular weight cannot be measured under the above measurement condition 1 due to crosslinking or other reasons, the molecular weight is measured by static light scattering under the following measurement condition 2. (Measurement condition 2) Measuring instrument: DLS-8000 (product name, manufactured by Otsuka Electronics Co., Ltd.) Measured concentration: 0.25, 0.50, 0.75, 1.00mg / mL Diluent: 0.1M NaCl aqueous solution Laser wavelength: 633nm Pinhole: PH1=Open, PH2=Slit Measurement angles: 60, 70, 80, 90, 100, 110, 120, 130 degrees Analysis method: Molecular weight was measured from Zimm square root plot. dn / dc required for analysis was measured with Abbe refractometer.

[0033] The copolymer X may be used alone or in combination of two or more kinds.

[0034] The content of copolymer X in the binder composition of the present invention is not particularly limited. For example, the ratio of copolymer X in the solid content of the binder composition (the content of copolymer X relative to the total solid content of the binder composition) can be 50% by mass or more. This ratio is more preferably 60% by mass or more, and even more preferably 70% by mass or more. The ratio of copolymer X in the solid content of the binder composition is preferably 50 to 90% by mass, more preferably 60 to 80% by mass, and even more preferably 65 to 80% by mass. In the present invention, when the binder composition contains a non-polymerizable surfactant component (C-2), the content of copolymer X means the total content of copolymer X and the non-polymerizable surfactant component (C-2). The same applies to the following explanation of "content of copolymer X" unless otherwise specified.

[0035] <(C) Surfactant component> The binder composition of the present invention may contain a surfactant component (C). In the present invention, the surfactant component (C) may be present as a constituent of the copolymer X as the above-mentioned polymerizable surfactant component (C-1), or may be present as a non-polymerizable surfactant component (C-2) independent of the copolymer X. When the surfactant component (C) is present as a constituent of the copolymer X as the polymerizable surfactant component (C-1), the polymerizable surfactant component (C-1) is a constituent that does not fall under the above-mentioned water-soluble vinyl compound component (A) and does not fall under the hydrophobic vinyl compound component (B). The polymerizable surfactant component (C-1) has a ClogP value of less than 1.00 (water-soluble) for the polymerizable surfactant (hereinafter sometimes referred to as "polymerizable surfactant" or "monomer leading to the polymerizable surfactant component (C-1)") that leads to this polymerizable surfactant component, and when a homopolymer c consisting of the polymerizable surfactant component (C-1) is assumed, the glass transition temperature of this homopolymer c is less than 90°C. The glass transition temperature of the homopolymer c can be determined in the same manner as the homopolymer a.

[0036] The polymerizable surfactant component (C-1) is a constituent derived from a surfactant having a polymerizable group (preferably a vinyl group). The polymerizable surfactant is preferably selected from anionic surfactants and nonionic surfactants, more preferably selected from ether sulfate type anionic surfactants and ethylene oxide addition type nonionic surfactants. From the viewpoint of structure, a surfactant component having an alkylene oxide chain in the structure is preferred. * -C(CH2OR x )HO(CH2CH2O) n -X group, or * -C(CH2-O-Ph-R y )HO(CH2CH2O) n -X group(R x and R y A surfactant having a phenylene group, X: SO3NH2 or H, n=10 to 40 is preferred. For example, Adeka Reasoap SR, ER, SE, and NE series (trade names, manufactured by ADEKA Corporation) can be used.

[0037] As the non-polymerizable surfactant component (C-2), at least any one of nonionic, cationic, and anionic surfactants having no polymerizable group can be used without any particular limitation. Examples of the nonionic surfactant in the non-polymerizable surfactant component (C-2) include higher alcohol ethylene oxide adducts, alkylphenol ethylene oxide adducts, alkylnaphthol ethylene oxide adducts, phenol ethylene oxide adducts, naphthol ethylene oxide adducts, fatty acid ethylene oxide adducts, polyhydric alcohol fatty acid ester ethylene oxide adducts, higher alkylamine ethylene oxide adducts, fatty acid amide ethylene oxide adducts, ethylene oxide adducts of fats and oils, polypropylene glycol ethylene oxide adducts, dimethylsiloxane-ethylene oxide block copolymers, dimethylsiloxane-(propylene oxide-ethylene oxide) block copolymers, fatty acid esters of glycerol, fatty acid esters of pentaerythritol, fatty acid esters of sorbitol and sorbitan, fatty acid esters of sucrose, alkyl ethers of polyhydric alcohols, and fatty acid amides of alkanolamines. Preferred specific examples of the nonionic surfactant in the non-polymerizable surfactant component (C-2) are shown below. In the following specific examples, n is 8-20.

[0038] [ka]

[0039] [ka]

[0040] Examples of the cationic surfactant in the non-polymerizable surfactant component (C-2) include alkylamine salts, quaternary ammonium salts, alkylimidazolinium salts, polyoxyethylene alkylamine salts, and polyethylene polyamine derivatives. Preferred specific examples of the cationic surfactant in the non-polymerizable surfactant component (C-2) are shown below.

[0041] [ka]

[0042] Examples of the anionic surfactant in the (C-2) non-polymerizable surfactant component include fatty acid salts, abietic acid salts, hydroxyalkanesulfonates, alkanesulfonates, dialkylsulfosuccinates, linear alkylbenzenesulfonates, branched alkylbenzenesulfonates, alkylnaphthalenesulfonates, alkyldiphenylether (di)sulfonates, alkylphenoxypolyoxyethylenealkylsulfonates, polyoxyethylenealkylsulfophenylether salts, sodium N-alkyl-N-oleyltaurates, N-alkylsulfosuccinic acid monoamide disodium salts, petroleum sulfonates, and hisufuran sulfates. Examples of the hydroxypropyl ether include maize oil, sulfated beef tallow oil, sulfate salts of fatty acid alkyl esters, alkyl sulfate salts, polyoxyethylene alkyl ether sulfate salts, fatty acid monoglyceride sulfate salts, polyoxyethylene alkyl phenyl ether sulfate salts, polyoxyethylene styryl phenyl ether sulfate salts, alkyl phosphate salts, polyoxyethylene alkyl ether phosphate salts, polyoxyethylene alkyl phenyl ether phosphate salts, partially saponified products of styrene-maleic anhydride copolymers, partially saponified products of olefin-maleic anhydride copolymers, naphthalene sulfonate formalin condensates, etc. Among these, linear alkylbenzene sulfonates are preferred, and sodium dodecylbenzene sulfonate (DBS) is more preferred. Preferred specific examples of the anionic surfactant in the non-polymerizable surfactant component (C-2) are shown below.

[0043] [ka]

[0044] The content of the non-polymerizable surfactant component (C-2) contained in the binder composition of the present invention is not particularly limited, and is preferably 0.5 to 5 mass %, more preferably 0.6 to 3 mass %, and further preferably 0.7 to 2 mass %, based on the content of copolymer X (the total content of copolymer X and the non-polymerizable surfactant component (C-2)).

[0045] <Liquid medium> The binder composition of the present invention contains a liquid medium. The liquid medium is not particularly limited, and is preferably water or a mixture of water and an organic solvent. The organic solvent is preferably an organic solvent that does not undergo phase separation when mixed with water (hereinafter referred to as a water-soluble organic solvent). Preferred examples of the water-soluble organic solvent include N-methylpyrrolidone, methanol, ethanol, acetone, and tetrahydrofuran. The binder composition of the present invention preferably contains water as the liquid medium, and more preferably the liquid medium is water.

[0046] The content of the liquid medium in the binder composition of the present invention is not particularly limited, and can be, for example, 10% by mass or more, preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and particularly preferably 50% by mass or more. The binder composition of the present invention may contain 60% by mass or more of the liquid medium, may contain 70% by mass or more, or may contain 80% by mass or more. It is practical for the content of the liquid medium in the binder composition of the present invention to be 99.5% by mass or less. The content of the liquid medium in the binder composition of the present invention is preferably from 10 to 99.5 mass%, more preferably from 20 to 99.5 mass%, even more preferably from 30 to 99.5 mass%, still more preferably from 40 to 99.5 mass%, still more preferably from 50 to 98 mass%, still more preferably from 60 to 98 mass%, still more preferably from 70 to 98 mass%, and still more preferably from 80 to 95 mass%.

[0047] <Water-soluble polymer> The binder composition of the present invention may contain a water-soluble polymer. In the present invention, the water-soluble polymer is a water-soluble polymer having a structure different from that of the above-mentioned copolymer X and the (C) surfactant component, and any of a wide variety of polymers that function as a thickener for the slurry for forming an electrode active material layer of a secondary battery can be used. In the present invention, the term "water-soluble polymer" refers to a polymer having a solubility in water of 10 g / L-H2O or more at 20° C., that is, a polymer that dissolves in an amount of 10 g or more in 1 liter of water at 20° C. The solubility of the "water-soluble polymer" is preferably 100 g / L-H2O or more. Examples of the water-soluble polymer include polysaccharides such as cellulose compounds and natural polysaccharides. Examples of the cellulose compound include methyl cellulose, ethyl cellulose, benzyl cellulose, triethyl cellulose, cyanoethyl cellulose, nitrocellulose, hydroxymethyl cellulose, hydroxyethyl cellulose (HEC), hydroxypropyl cellulose (HPC), hydroxypropyl methyl cellulose (HPMC), hydroxybutyl methyl cellulose, carboxymethyl cellulose (CMC), aminomethyl hydroxypropyl cellulose, aminoethyl hydroxypropyl cellulose, cellulose nanofiber (CNF), cellulose nanocrystal (CNC), etc. The cellulose compound may be in the form of a salt such as an ammonium salt, a sodium salt, or a lithium salt. Examples of natural polysaccharides include carrageenan, xanthan gum, guar gum, tamarind gum (tamarind seed gum), diutan gum, welan gum, gellan gum, locust bean gum, and tara gum. Among these, the water-soluble polymer preferably includes at least one of carboxymethyl cellulose, cellulose nanofiber, hydroxyethyl cellulose, hydroxypropyl cellulose, and xanthan gum. In the present invention, the water-soluble polymer may be used alone or in combination of two or more kinds.

[0048] The total content ratio of each of the copolymer X and the water-soluble polymer in all the polymers (100% by mass) contained in the binder composition of the present invention is not particularly limited. For example, it can be 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 99% by mass or more. In addition, it is preferable that all the polymers contained in the binder composition of the present invention are composed of the copolymer X and the water-soluble polymer. In the binder composition of the present invention, the mass ratio of the contents of copolymer X and the water-soluble polymer (content of copolymer X: content of water-soluble polymer) is not particularly limited, and is preferably 60-90:10-40, more preferably 65-85:15-35, and even more preferably 65-80:20-35.

[0049] The binder composition of the present invention may contain, in addition to the copolymer X and the water-soluble polymer, a typical polymer used as a binder for batteries.

[0050] The binder composition of the present invention may contain other components in addition to the copolymer X, the liquid medium, the non-polymerizable surfactant that is preferably used, and the water-soluble polymer, depending on the purpose. Examples of the other components include lithium salts, ionic liquids, thickeners, antifoaming agents, leveling agents, dehydrating agents, antioxidants, and tackifiers. The binder composition of the present invention can also be prepared by diluting a synthesis reaction solution of the copolymer X, etc. Therefore, the binder composition of the present invention may contain raw materials used in the synthesis of the copolymer X, etc., or by-products after the reaction, etc.

[0051] [Composition for electrode] The electrode composition of the present invention includes the above-mentioned liquid medium, copolymer X, and active material. That is, the electrode composition of the present invention is an electrode composition including a liquid medium, copolymer X, and active material, in which copolymer X includes (A) a water-soluble vinyl compound component and (B) a hydrophobic vinyl compound component as constituents, and when a homopolymer a consisting of (A) the water-soluble vinyl compound component is assumed, the glass transition temperature of this homopolymer a is 90°C or higher, and when a homopolymer b consisting of (B) the hydrophobic vinyl compound component is assumed, the glass transition temperature of this homopolymer b is 0°C or lower. The electrode composition of the present invention can appropriately contain components that can be contained in the binder composition of the present invention, as necessary. That is, the electrode composition of the present invention can be obtained by mixing the binder composition of the present invention with an active material. It is also preferable that the electrode composition of the present invention contains a conductive assistant. The active material may be a positive electrode active material or a negative electrode active material. When the electrode composition contains a positive electrode active material, the electrode composition can be used as a slurry for forming a positive electrode active material layer of a secondary battery. When the electrode composition contains a negative electrode active material, the electrode composition can be used as a slurry for forming a negative electrode active material layer. The electrode composition of the present invention preferably contains a negative electrode active material, and more preferably, at least a part of the negative electrode active material is a silicon-based active material. The active material, conductive assistant, etc. are not particularly limited, and can be appropriately selected according to the purpose from those usable as active materials, conductive assistants, etc. for secondary batteries.

[0052] In the electrode composition of the present invention, the content of the copolymer X is not particularly limited, and is preferably 0.3 to 15 mass%, more preferably 0.5 to 12 mass%, more preferably 1.0 to 10 mass%, further preferably 1.5 to 8 mass%, and particularly preferably 2 to 6 mass%, based on the total solid content in the electrode composition. When the electrode composition of the present invention contains a water-soluble polymer, the total content of each of the copolymer X and the water-soluble polymer in the electrode composition of the present invention is not particularly limited. For example, the total content of each of the copolymer X and the water-soluble polymer in the electrode composition of the present invention can be 1.5 to 15 mass%, preferably 1.5 to 12 mass%, more preferably 2 to 10 mass%, further preferably 2.5 to 10 mass%, and particularly preferably 3 to 8 mass%. In the electrode composition of the present invention, the mass ratio of the contents of the copolymer X and the water-soluble polymer is the same as the mass ratio of the contents of the copolymer X and the water-soluble polymer in the binder composition of the present invention.

[0053] <Active material> (Cathode active material) The positive electrode active material may be any active material capable of inserting and releasing ions of a metal belonging to Group 1 or Group 2 of the periodic table, and is preferably one capable of inserting and releasing lithium ions reversibly. The material is not particularly limited as long as it has the above characteristics, and may be a lithium-containing transition metal oxide, an organic substance, an element capable of forming a composite with Li, such as sulfur, or a composite of sulfur and a metal. Among them, it is preferable to use a lithium-containing transition metal oxide as the positive electrode active material, and the transition metal element M a It is more preferable that the transition metal oxide contains an element M (one or more elements selected from Co, Ni, Fe, Mn, Cu and V). b (Elements of Group 1 (Ia) of the periodic table other than lithium, elements of Group 2 (IIa), Al, Ga, In, Ge, Sn, Pb, Sb, Bi, Si, P, B, etc.) may be mixed. b The amount of the transition metal element M a The amount of the transition metal element M is preferably 0 to 30 mol % relative to 100 mol %. a Molar ratio of Li toa It is more preferable that the ratio of the two components be 0.3 to 2.2. Specific examples of lithium-containing transition metal oxides include (MA) transition metal oxides having a layered rock salt structure, (MB) transition metal oxides having a spinel structure, (MC) lithium-containing transition metal phosphate compounds, (MD) lithium-containing transition metal halide phosphate compounds, and (ME) lithium-containing transition metal silicate compounds.

[0054] (MA) Specific examples of transition metal oxides with a layered rock-salt structure include LiCoO2 (lithium cobalt oxide [LCO]), LiNi2O2 (lithium nickel oxide), and LiNi 0.85 Co 0.10 Al 0.05 O2 (Lithium Nickel Cobalt Aluminum Oxide [NCA]), LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (Lithium Nickel Manganese Cobalt Oxide [NMC]) and LiNi 0.5 Mn 0.5 O2 (lithium manganese nickel oxide). (MB) Specific examples of transition metal oxides having a spinel structure include LiMn2O4 (LMO), LiCoMnO4, Li2FeMn3O8, Li2CuMn3O8, Li2CrMn3O8, and Li2NiMn3O8. (MC) Examples of lithium-containing transition metal phosphate compounds include olivine-type iron phosphates such as LiFePO4 and Li3Fe2(PO4)3, iron pyrophosphates such as LiFeP2O7, cobalt phosphates such as LiCoPO4, and monoclinic Nasicon-type vanadium phosphates such as Li3V2(PO4)3 (lithium vanadium phosphate). (MD) Examples of lithium-containing transition metal halophosphate compounds include fluorophosphate iron salts such as Li2FePO4F, fluorophosphate manganese salts such as Li2MnPO4F, and fluorophosphate cobalt salts such as Li2CoPO4F. (ME) Examples of lithium-containing transition metal silicate compounds include Li2FeSiO4, Li2MnSiO4, and Li2CoSiO4. In the present invention, transition metal oxides having a layered rock-salt structure (MA) are preferred, with LCO or NMC being more preferred.

[0055] The shape of the positive electrode active material is not particularly limited, and particulate is preferred. The average particle size (volume-based median diameter D50) of the positive electrode active material is not particularly limited. For example, it can be 0.1 to 50 μm. In order to make the positive electrode active material have a predetermined particle size, it may be prepared by a conventional method using a pulverizer or classifier. The method of preparing the negative electrode active material to have a predetermined particle size described later can also be applied. The positive electrode active material obtained by the baking method may be used after washing with water, an acidic aqueous solution, an alkaline aqueous solution, an organic solvent, or the like. When a commercially available positive electrode active material is used, the average particle size of the positive electrode active material is the value listed in the manufacturer's catalog. When the information on the average particle size from the manufacturer is not available or when a synthesized positive electrode active material is used, the value measured and calculated by the method described below in the section on negative electrode active material is used.

[0056] The chemical formula of the compound obtained by the above calcination method can be measured by inductively coupled plasma (ICP) emission spectrometry, or, as a simple method, can be calculated from the mass difference of the powder before and after calcination.

[0057] The surface of the positive electrode active material may be coated with an oxide such as another metal oxide, a carbon-based material, etc. As the surface coating material, a surface coating material that can be used to coat the surface of a negative electrode active material described later can be used.

[0058] The surface of the positive electrode active material may be treated with sulfur or phosphorus. Furthermore, the particle surfaces of the positive electrode active material may be subjected to a surface treatment with active rays or active gas (plasma, etc.) before or after the above-mentioned surface coating.

[0059] The positive electrode active materials may be used alone or in combination of two or more. When forming a positive electrode active material layer, the unit area (cm 2The mass (mg) (weight per unit area) of the positive electrode active material is not particularly limited and can be appropriately determined depending on the designed battery capacity.

[0060] The content of the positive electrode active material in the electrode composition of the present invention is not particularly limited, and is preferably 10 to 99 mass%, more preferably 30 to 98 mass%, further preferably 50 to 97 mass%, and particularly preferably 55 to 95 mass%, based on the total solid content.

[0061] (Negative electrode active material) The negative electrode active material may be any active material capable of inserting and releasing ions (preferably lithium ions) of a metal belonging to Group 1 or Group 2 of the periodic table, and is preferably one capable of reversibly absorbing and releasing lithium ions. The material is not particularly limited as long as it has the above characteristics, and examples of the material include carbonaceous materials, silicon-based materials (meaning materials containing silicon element), tin-based materials (meaning materials containing tin element), metal oxides, metal composite oxides, lithium alone, and lithium alloys. Among these, carbonaceous materials and silicon-based materials are preferably used from the viewpoint of reliability.

[0062] The carbonaceous material used as the negative electrode active material is a material that is substantially made of carbon. For example, carbon black such as petroleum pitch and acetylene black, graphite (natural graphite such as flake graphite and lump graphite, artificial graphite such as vapor-grown graphite and fibrous graphite, expanded graphite obtained by specially processing flake graphite, etc.), activated carbon, carbon fiber, coke, soft carbon, hard carbon, and carbonaceous materials obtained by firing various synthetic resins such as PAN (polyacrylonitrile)-based resins or furfuryl alcohol resins can be mentioned. In addition, various carbon fibers such as PAN-based carbon fibers, cellulose-based carbon fibers, pitch-based carbon fibers, vapor-grown carbon fibers, dehydrated PVA (polyvinyl alcohol)-based carbon fibers, lignin carbon fibers, glassy carbon fibers, and activated carbon fibers, mesophase microspheres, graphite whiskers, and plate-like graphite can also be mentioned.

[0063] Examples of tin-based materials (tin-based active materials) used as negative electrode active materials include Sn, SnO, SnO2, SnS, and SnS2.

[0064] The metal oxides and metal composite oxides used as the negative electrode active material are not particularly limited as long as they are oxides capable of inserting and releasing ions of a metal belonging to Group 1 or Group 2 of the periodic table. Examples of metal oxides include oxides of metal elements (metal oxides) and oxides of metalloid elements (metalloid oxides). Examples of metal composite oxides include composite oxides of metal elements, composite oxides of metal elements and metalloid elements, and composite oxides of metalloid elements. As these metal oxides and metal composite oxides, amorphous oxides are preferred, and further preferred examples include chalcogenides which are reaction products between metal elements and elements of group 16 of the periodic table. The term "amorphous" as used herein means that the oxide has a broad scattering band with a peak in the 2θ value range of 20° to 40° in an X-ray diffraction method using CuKα radiation, and may have crystalline diffraction lines. Among the compound group consisting of the above amorphous oxides and chalcogenides, the amorphous oxides of metalloid elements or the above chalcogenides are more preferred, and the oxides or composite oxides or chalcogenides consisting of one or more of the elements (e.g., Al, Ga, Si, Sn, Ge, Pb, Sb and Bi) of the periodic table, are particularly preferred.Specific examples of the amorphous oxides and chalcogenides include Ga2O3, GeO, PbO, PbO2, Pb2O3, Pb2O4, Pb3O4, Sb2O3, Sb2O4, Sb2O8Bi2O3, Sb2O8Si2O3, Sb2O5, Bi2O3, Bi2O4, GeS, PbS, PbS2, Sb2S3 and Sb2S5.

[0065] It is preferable from the viewpoint of high current density charge-discharge characteristics that the metal (composite) oxide and the above-mentioned chalcogenide contain at least one of titanium and lithium as constituent components. Examples of the metal composite oxide containing lithium (lithium composite metal oxide) include composite oxides of lithium oxide and the above-mentioned metal (composite) oxide or the above-mentioned chalcogenide, and more specifically, Li2SnO2.

[0066] It is also preferable that the negative electrode active material contains titanium element. More specifically, TiNb2O7 (niobium titanate oxide [NTO]), Li4Ti5O 12 (lithium titanate [LTO]) is preferable in that it has excellent rapid charge-discharge characteristics because of its small volume change during lithium ion insertion and extraction, suppresses electrode deterioration, and enables improvement of the cycle characteristics of the lithium ion secondary battery.

[0067] The lithium alloy as the negative electrode active material is not particularly limited as long as it is an alloy commonly used as the negative electrode active material of the secondary battery, and examples thereof include lithium aluminum alloy.

[0068] The silicon-based material (silicon-based active material) is a negative electrode active material containing silicon element, and examples thereof include silicon materials such as Si, SiO x (0 < x ≤ 1.5), and further, silicon-containing alloys containing titanium, vanadium, chromium, manganese, nickel, copper or lanthanum (for example, LaSi2, VSi2), or organized active materials (for example, LaSi2 / Si). In addition, oxides or composite oxides containing silicon element in the description of the above-mentioned metal oxides and metal composite oxides, active materials containing silicon element and tin element such as SnSiO3, SnSiS3, etc. are also included. SiO x can be used as a negative electrode active material (semi-metal oxide) by itself, and can also be used as an active material (its precursor material) capable of forming an alloy with lithium because Si is generated during the operation of the battery.

[0069] Although the negative electrode active material has been described above with a focus on its components, from the viewpoint of characteristics, it is preferable that the negative electrode active material is capable of forming an alloy with lithium. The negative electrode active material capable of forming an alloy with lithium is not particularly limited as long as it is a material that is normally used as a negative electrode active material for secondary batteries. Examples of such active materials include the above-mentioned negative electrode active materials containing silicon element and / or tin element, and metals such as Al and In. Silicon-based active materials are preferred in that they enable higher battery capacity, and silicon-based active materials in which the content of silicon element is 40 mol% or more of the total constituent elements are more preferred. In general, negative electrodes containing these negative electrode active materials capable of forming an alloy with lithium (for example, Si negative electrodes containing silicon-based active materials, Sn negative electrodes containing tin-based active materials) can absorb more Li ions than negative electrodes made of only carbonaceous materials (graphite, carbon black, etc.). In other words, the amount of Li ions absorbed per unit mass increases. This makes it possible to increase the battery capacity (energy density). As a result, there is an advantage in that the battery operating time can be extended. Thus, negative electrode active materials containing silicon and / or tin are also referred to as high-capacity active materials.

[0070] The surface of the negative electrode active material may be surface-coated with an oxide such as another metal oxide, a carbon-based material, or the like (hereinafter, surface-coated with a carbon-based material may be referred to as "carbon-coated"). Examples of surface-coating materials include metal oxides containing Ti, Nb, Ta, W, Zr, Al, Si, or Li. Specific examples include titanate spinel, tantalum-based oxides, niobium-based oxides, and lithium niobate-based compounds, and more specifically, Li4Ti5O 12 , Li2Ti2O5, LiTaO3, LiNbO3, LiAlO2, Li2ZrO3, Li2WO4, Li2TiO3, Li2B4O7, Li3PO4, Li2MoO4, Li3BO3, LiBO2, Li2CO3, Li2SiO3, SiO2, TiO2, ZrO2, Al2O3, B2O3, etc. Carbon-based materials such as C, SiC, and carbon-added silicon oxide can also be used as surface coating materials.

[0071] Further, the surface of the negative electrode active material may be surface-treated with sulfur or phosphorus. Furthermore, the surface of the particles of the negative electrode active material may be surface-treated with actinic rays or active gas (such as plasma) before and after the above surface coating.

[0072] The negative electrode active material may be doped with a metal element. In the negative electrode active material doped with a metal element, the metal element to be doped is preferably at least one of Li, Ni, and Ti, and more preferably Li.

[0073] In the present invention, it is preferable to use a silicon-based active material as the negative electrode active material, and more preferably silicon oxide (SiO x (0 < x ≤ 1.5)) or carbon-coated silicon oxide (carbon-coated SiO x (0 < x ≤ 1.5)), and even more preferably to use silicon oxide. Silicon oxide or carbon-coated silicon oxide may be further doped with a metal element. Commercially available products may be used for silicon oxide or carbon-coated silicon oxide. In addition, carbon-coated silicon oxide can also be prepared by carbon-coating silicon oxide, for example, referring to Japanese Patent Application Laid-Open No. 2019-204686. In the present invention, it is also preferable to use a silicon-based material doped with a metal element as the negative electrode active material, more preferably a silicon-based material doped with at least one of Li, Ni, and Ti, and even more preferably a silicon-based material doped with Li. The silicon-based material to be doped with a metal element is preferably silicon oxide or carbon-coated silicon oxide, and more preferably silicon oxide. As silicon oxide doped with a metal element, and silicon oxide doped with a metal element and carbon coated, commercially available products may be used. In addition, for example, referring to JP 2022-121582 A, WO 14 / 188851 A, and JP 2021-150077 A, silicon oxide or carbon-coated silicon oxide can be doped with a metal element, or silicon oxide can be doped with a metal element and further carbon coated as necessary.

[0074] The shape of the negative electrode active material is not particularly limited, and is preferably particulate. The average particle size (volume-based median size D50) of the negative electrode active material is preferably 0.1 to 60 μm. Furthermore, when the negative electrode active material is silicon oxide or carbon-coated silicon oxide, the average particle size is more preferably 5 to 20 μm. To obtain a desired particle size, a grinder or a classifier can be used in a conventional manner. For example, a mortar, a ball mill, a sand mill, a vibration ball mill, a satellite ball mill, a planetary ball mill, a swirling airflow type jet mill, or a sieve is preferably used. During grinding, wet grinding in the presence of water or an organic solvent such as methanol can also be performed. In order to obtain a desired particle size, it is preferable to perform classification. The classification method is not particularly limited, and a sieve, a wind classifier, or the like can be used as desired. Classification can be performed both in a dry and wet manner. When a commercially available negative electrode active material is used, the average particle size of the negative electrode active material is the value listed in the manufacturer's catalog. When information on the average particle size from the manufacturer is unavailable or when a synthesized negative electrode active material is used, the negative electrode active material is dispersed in water, and the average particle size (volume-based median diameter D50 in water) obtained by measuring with a laser diffraction / scattering type particle size distribution measurement device (for example, Particle LA-960V2 (product name) manufactured by HORIBA) is used.

[0075] The negative electrode active material may be used alone or in combination of two or more. Among them, a combination of a silicon-based active material and a carbonaceous material is preferred, a combination of a silicon-based active material and graphite is more preferred, and a combination of silicon oxide or carbon-coated silicon oxide and graphite is even more preferred. The silicon oxide and the carbon-coated silicon oxide may be silicon oxide doped with the above-mentioned metal element and silicon oxide doped with the metal element and carbon-coated, respectively. The doped metal element is preferably at least one of Li, Ni, and Ti, and more preferably Li. When a silicon-based active material is combined with graphite, the mass ratio of the silicon-based active material to the graphite (silicon-based active material / graphite) is preferably 2 or less, more preferably 1 or less, and even more preferably 0.5 or less. There is no particular lower limit to the mass ratio of the silicon-based active material to the graphite, but a mass ratio of 0.05 or more is practical. When forming a negative electrode active material layer, the unit area (cm 2 The mass (mg) (weight per unit area) of the negative electrode active material is not particularly limited and can be appropriately determined depending on the designed battery capacity.

[0076] The content of the negative electrode active material in the electrode composition of the present invention is not particularly limited, and is preferably 10 to 99 mass %, more preferably 30 to 98 mass %, further preferably 45 to 97 mass %, and particularly preferably 55 to 95 mass %, based on the total solid content.

[0077] (Conductive assistant) The electrode composition of the present invention may contain a conductive assistant, and in particular, it is preferable that the silicon-based active material as the negative electrode active material is used in combination with a conductive assistant. The conductive assistant is not particularly limited, and may be any known conductive assistant. For example, it may be an electron conductive material such as carbon blacks, such as acetylene black, ketjen black, furnace black, amorphous carbon, such as needle coke, carbon fibers, such as vapor-grown carbon fibers or carbon nanotubes, carbonaceous materials, such as graphene or fullerene, metal powders, metal fibers, such as copper or nickel, or conductive polymers, such as polyaniline, polypyrrole, polythiophene, polyacetylene, or polyphenylene derivatives. In the present invention, when an active material and a conductive assistant are used in combination, among the above-mentioned conductive assistants, those that do not insert or release Li when the battery is charged and discharged and do not function as an active material are considered to be conductive assistants. Therefore, among the conductive assistants, those that can function as an active material in the active material layer when the battery is charged and discharged are classified as active materials rather than conductive assistants. Whether or not a conductive assistant functions as an active material when the battery is charged and discharged is not unique, but is determined by the combination with the active material.

[0078] The conductive assistant may be used alone or in combination of two or more kinds. In the present invention, it is preferable to use carbon blacks and carbon nanotubes in combination. The content of the conductive assistant in the electrode composition of the present invention is preferably 0.5 to 60 mass%, more preferably 0.5 to 50 mass%, more preferably 0.5 to 40 mass%, more preferably 0.5 to 35 mass%, more preferably 0.5 to 20 mass%, more preferably 0.5 to 10 mass%, even more preferably 0.8 to 5.0 mass%, and particularly preferably 1.0 to 2.0 mass%, based on the total solid content.

[0079] The shape of the conductive assistant is not particularly limited, but is preferably particulate. The average particle size (volume-based median diameter D50) of the conductive assistant is not particularly limited, but is preferably, for example, 0.01 to 50 μm, and more preferably 0.02 to 10.0 μm. When using a commercially available conductive additive, the average particle size of the conductive additive is the value listed in the manufacturer's catalog. When information on the average particle size from the manufacturer is not available or when a synthetic conductive additive is used, the average particle size of the conductive additive may be a value obtained by applying the above-mentioned method for measuring the average particle size (volume-based median diameter D50 in water) of the negative electrode active material.

[0080] (Other additives) The electrode composition of the present invention may contain, as desired, a lithium salt, an ionic liquid, a thickener, a defoamer, a leveling agent, a dehydrating agent, an antioxidant, and the like, as components other than the above-mentioned components. For the above active materials, conductive assistants, and other additives, reference can be made to, for example, International Publication No. 2019 / 203334 and JP-A-2015-46389.

[0081] [Method of preparing binder composition for secondary battery and composition for electrode] The binder composition of the present invention can be prepared as a mixture, preferably as a slurry, by mixing a liquid medium, a copolymer X, preferably a water-soluble polymer, a non-polymerizable surfactant (C-2), and optionally any other components, for example, with various commonly used mixers. In the case of the electrode composition of the present invention, in addition to the above, an active material, preferably a conductive assistant, and optionally other additives are mixed. The mixing method is not particularly limited, and the components may be mixed all at once or sequentially. In addition, a mixture obtained by mixing a plurality of components may be mixed with other components. For example, after mixing an active material, a conductive assistant, a water-soluble polymer, and a liquid medium, copolymer X and a liquid medium are added and further mixed to obtain a composition for an electrode.

[0082] [Electrode sheet] The electrode sheet of the present invention has a layer (electrode active material layer, i.e., anode active material layer or cathode active material layer) formed using the electrode composition of the present invention. The electrode sheet of the present invention may be an electrode sheet having an electrode active material layer formed using the electrode composition of the present invention, and may be a sheet in which the electrode active material layer is formed on a substrate such as a current collector, or a sheet without a substrate and formed only with an electrode active material layer (anode active material layer or cathode active material layer). This electrode sheet is usually a sheet having a configuration in which an electrode active material layer is laminated on a current collector. The electrode sheet of the present invention may have, for example, a protective layer such as a release sheet or a coating layer as another layer. The electrode sheet of the present invention can be suitably used as a material constituting a negative electrode active material layer or a positive electrode active material layer of a secondary battery, or as a laminate of a negative electrode current collector and a negative electrode active material layer (negative electrode layer) or a laminate of a positive electrode current collector and a positive electrode active material layer (positive electrode layer).

[0083] When the electrode sheet of the present invention has a current collector, the current collector constituting the electrode sheet of the present invention is an electron carrier and is usually in the form of a film sheet. The current collector can be appropriately selected depending on the active material. Examples of the material for the positive electrode current collector include aluminum, aluminum alloy, stainless steel, nickel, titanium, etc., and aluminum or an aluminum alloy is preferable. The positive electrode current collector may also be one in which the surface of aluminum or stainless steel is treated with carbon, nickel, titanium, or silver to form a coating layer (thin film). Examples of the material for the negative electrode current collector include aluminum, copper, a copper alloy, stainless steel, nickel, titanium, etc., and aluminum, copper, a copper alloy, or stainless steel is preferable. Examples of the negative electrode current collector include those in which the surface of aluminum, copper, a copper alloy, or stainless steel is treated with carbon, nickel, titanium, or silver to form a coating layer (thin film).

[0084] There are no particular limitations on the thickness of the positive electrode active material layer constituting the electrode sheet of the present invention, and it can be, for example, 5 to 500 μm, and preferably 20 to 200 μm. Furthermore, the thickness of the positive electrode current collector constituting the electrode sheet of the present invention is not particularly limited and can be, for example, 10 to 100 μm, and preferably 10 to 50 μm.

[0085] There are no particular limitations on the thickness of the negative electrode active material layer constituting the electrode sheet of the present invention, and it can be, for example, 5 to 500 μm, and preferably 20 to 200 μm. Furthermore, the thickness of the negative electrode current collector constituting the electrode sheet of the present invention is not particularly limited and can be, for example, 10 to 100 μm, and preferably 10 to 50 μm.

[0086] [Manufacturing method of electrode sheet] The electrode sheet of the present invention can be obtained by forming an electrode active material layer using the electrode composition of the present invention. For example, the electrode sheet of the present invention can be manufactured by forming a film using the electrode composition of the present invention. Specifically, a current collector or the like is used as a substrate, and the electrode composition of the present invention is applied thereon (may be via another layer) to form a coating film, which is then dried to obtain an electrode sheet having an active material layer (coated and dried layer) on the substrate.

[0087] [Secondary battery and method of manufacturing the secondary battery] The secondary battery of the present invention is a secondary battery having a positive electrode active material layer, a separator, and a negative electrode active material layer in this order, and at least one of the positive electrode active material layer and the negative electrode active material layer is a layer formed using the electrode composition of the present invention. Preferably, the secondary battery of the present invention has a positive electrode active material layer, a separator, and a negative electrode active material layer in this order, and the negative electrode active material layer is a layer formed using the electrode composition of the present invention. The secondary battery of the present invention will be described taking a non-aqueous electrolyte secondary battery as an example, however, the secondary battery of the present invention is not limited to a non-aqueous electrolyte secondary battery and broadly includes secondary batteries in general.

[0088] A nonaqueous electrolyte secondary battery according to a preferred embodiment of the present invention includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode. The positive electrode has a positive electrode current collector and a positive electrode active material layer in contact with the positive electrode current collector, and the negative electrode has a negative electrode current collector and a negative electrode active material layer in contact with the negative electrode current collector. In the nonaqueous electrolyte secondary battery of the present invention, at least one of the positive electrode active material layer and the negative electrode active material layer is formed using the electrode composition of the present invention. The nonaqueous electrolyte secondary battery of the present invention also includes a nonaqueous electrolyte secondary battery having only one of a positive electrode active material layer and a negative electrode active material layer, the electrode active material layer being formed using the electrode composition of the present invention. The nonaqueous electrolyte secondary battery of the present invention functions as a secondary battery by charging and discharging by filling a nonaqueous electrolyte between the positive electrode and the negative electrode.

[0089] FIG. 1 is a cross-sectional view showing a schematic of the laminated structure of a general non-aqueous electrolyte secondary battery 10, including the working electrode when the battery is operated. The non-aqueous electrolyte secondary battery 10 has a laminated structure having, in this order, a negative electrode current collector 1, a negative electrode active material layer 2, a separator 3, a positive electrode active material layer 4, and a positive electrode current collector 5, as viewed from the negative electrode side. The space between the negative electrode active material layer 2 and the positive electrode active material layer 4 is filled with a non-aqueous electrolyte (not shown), and is separated by the separator 3. The separator 3 has pores, and functions as a positive / negative electrode separator that insulates between the positive and negative electrodes while allowing the electrolyte and ions to pass through the pores during normal battery use. With this structure, for example, in the case of a lithium-ion secondary battery, electrons (e - ) is supplied, and at the same time, lithium ions (Li + ) moves and accumulates in the negative electrode. On the other hand, during discharge, the lithium ions (Li + ) is returned to the positive electrode side through the electrolyte, and electrons are supplied to the operating part 6. In the illustrated example, a light bulb is used as the operating part 6, and it is lit by the discharge. In the present invention, the negative electrode current collector 1 and the negative electrode active material layer 2 are collectively referred to as the negative electrode, and the positive electrode active material layer 4 and the positive electrode current collector 5 are collectively referred to as the positive electrode.

[0090] The secondary battery of the present invention is not particularly limited in terms of the materials or members such as electrolytes such as electrolytes (aqueous electrolytes, nonaqueous electrolytes) or solid electrolyte materials, separators, etc., except that the secondary battery of the present invention is provided with at least one of a positive electrode active material layer and a negative electrode active material layer formed using the electrode composition of the present invention. These materials and members can be appropriately applied to those used in ordinary secondary batteries. In addition, for the method of producing the secondary battery of the present invention, ordinary methods can be appropriately adopted, except that at least one of the positive electrode active material layer and the negative electrode active material layer is formed using the electrode composition of the present invention. For the members and production methods normally used in these secondary batteries, for example, JP 2016-201308 A, JP 2005-108835 A, JP 2012-185938 A, and WO 2020 / 067106 A can be appropriately referred to.

[0091] The secondary battery of the present invention can be mounted in electronic devices such as notebook computers, pen-input computers, mobile computers, electronic book players, mobile phones, cordless phone sub-units, pagers, handheld terminals, mobile fax machines, mobile copiers, mobile printers, headphone stereos, video movie machines, liquid crystal televisions, handheld cleaners, portable CDs, mini-discs, electric shavers, transceivers, electronic organizers, calculators, portable tape recorders, radios, backup power sources, and memory cards. It can also be mounted in consumer devices such as automobiles, electric vehicles, motors, lighting equipment, toys, game devices, road conditioners, watches, strobes, cameras, and medical devices (pacemakers, hearing aids, shoulder massagers, etc.). It can also be used for various military applications and space applications. It can also be combined with solar cells. EXAMPLES

[0092] The present invention will be described in more detail with reference to the following examples. The present invention is not limited to these examples except as specified in the present invention. Room temperature means 27°C unless otherwise specified. The composition ratio, blend ratio, and content are based on mass unless otherwise specified.

[0093] [Synthesis of copolymer X] (1) Synthesis of copolymer X1 (A) 15.8 g (polymerization ratio 20 mass%) of acrylamide (AAm) (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) as a monomer that derives a water-soluble vinyl compound component, (B) 63.4 g (polymerization ratio 80 mass%) of 2-ethylhexyl acrylate (2EHA) (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) as a monomer that derives a hydrophobic vinyl compound component, (C-1) 0.40 g of Adeka Reasoap SE-10N (manufactured by ADEKA Corporation) (polymerizable surfactant) as a monomer that derives a polymerizable surfactant component, and 40.0 g of distilled water were mixed with stirring to obtain solution I. 282.2 g of distilled water was added to a 1 L three-neck flask equipped with a reflux condenser and a gas inlet cock. The temperature was raised to 80°C while introducing nitrogen gas at a flow rate of 200 mL / min. After the temperature was raised, nitrogen gas was introduced for 30 minutes, and then 0.52 g of potassium peroxodisulfate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 0.40 g of Adeka Reasoap SE-10N (manufactured by ADEKA Corporation) were added. Next, solution I was added dropwise over 2 hours. After completion of the dropwise addition, stirring was continued at 80°C for 1 hour. Next, the temperature was raised to 90°C, and stirring was continued at 90°C for 1 hour. The mixture was cooled to room temperature to obtain an aqueous dispersion of copolymer X1. The solid content was 20% by mass. In the synthesis of copolymer X1, the content of monomers leading to a polymerizable surfactant component (C-1) was 0.80 g in total, which was 1 mass % based on the total content of all components in copolymer X1 (the total content of monomers leading to a water-soluble vinyl compound component (A), monomers leading to a hydrophobic vinyl compound component (B), and monomers leading to a polymerizable surfactant component (C-1)). In this manner, an aqueous dispersion of copolymer X1, which is a copolymer of AAm, 2EHA and SE-10N, was obtained.

[0094] (2) Synthesis of copolymers X2 to X12 and CX1 to CX3 In the synthesis of the copolymer X1, the (A) monomer leading to a water-soluble vinyl compound component, the (B) monomer leading to a hydrophobic vinyl compound component, and the (C-1) monomer leading to a polymerizable surfactant component or the (C-2) non-polymerizable surfactant component were each prepared in the same manner as the copolymer X1, except that the polymerization ratio or content was set as shown in Table 1. At that time, the (C-1) polymerizable surfactant component and the (C-2) non-polymerizable surfactant component (DBS: sodium decylbenzenesulfonate) were added to solution I in half the amounts shown in Table 1, and the remaining half was added to a three-neck flask.

[0095] [Measurement of glass transition temperature] Homopolymers of (A) monomers leading to water-soluble vinyl compound components and (B) monomers leading to hydrophobic vinyl compound components shown in Table 1 were prepared as described below, and the glass transition temperatures of the obtained homopolymers were measured under the following conditions. The results are shown in the "Tg" column of Table 1. <Method of preparing homopolymer> -(A) In the case of monomers that lead to water-soluble vinyl compound components- Into a 1L three-neck flask equipped with a reflux condenser and a gas inlet cock, 0.40 g of VA-057 (trade name: Fujifilm Wako Pure Chemical Industries, Ltd.) (water-soluble azo polymerization initiator), 50.0 g of (A) monomer that derives a water-soluble vinyl compound component, and 350.0 g of distilled water were added. Nitrogen gas was introduced at a flow rate of 200 mL / min for 30 minutes, and then the temperature was raised to 80°C. After the temperature was raised, stirring was continued at 80°C for 5 hours to prepare a homopolymer of (A) monomer that derives a water-soluble vinyl compound component. -(B) In the case of monomers that lead to hydrophobic vinyl compound components- Into a 1L three-neck flask equipped with a reflux condenser and a gas inlet cock, 0.40 g of V-601 (trade name: Fujifilm Wako Pure Chemical Industries, Ltd.) (oil-soluble azo polymerization initiator), 50.0 g of (B) a monomer that derives a hydrophobic vinyl compound component, and 200.0 g of propylene glycol monomethyl ether acetate were added. Nitrogen gas was introduced at a flow rate of 200 mL / min for 30 minutes, and then the temperature was raised to 80°C. After the temperature was raised, stirring was continued at 80°C for 5 hours to prepare a homopolymer of (B) a monomer that derives a hydrophobic vinyl compound component. <Measurement of glass transition temperature> The glass transition temperature (Tg) was calculated by measuring each of the homopolymers obtained above using a differential scanning calorimeter: X-DSC7000 (trade name, manufactured by SII Nano Technology Co., Ltd.) under the following measurement conditions. The measurement was performed twice on the same sample, and the second measurement result was used. -Measurement conditions- Atmosphere in the measurement chamber: Nitrogen gas (50mL / min) Heating rate: 5℃ / min Measurement start temperature: -80℃ End of measurement temperature: 250℃ Sample pan: Aluminum pan Mass of measurement sample: 5mg Calculation of Tg: Tg was calculated by rounding off the midpoint temperature between the start and end points of the decline in a DSC (differential scanning calorimetry) chart (temperature at the end point of the decline + [(temperature at the start point of the decline - temperature at the end point of the decline) / 2]) to the nearest integer.

[0096] For each of the copolymers X obtained above, a tensile test was carried out as follows, and the breaking elongation was calculated. The results are shown in Table 1.

[0097] [Tensile test: Calculation of breaking elongation of copolymer X] A polymer sheet of copolymer X was formed on a peelable polyethylene terephthalate (PET) film (length 5 cm, width 0.5 cm, film thickness 0.1 mm) by applying the aqueous dispersion of each copolymer X obtained above and drying it. The polymer sheet was peeled off from the PET film to obtain a test piece (length 5 cm, width 0.5 cm, film thickness 0.030 to 0.150 mm). In the longitudinal (length) direction of the test piece, a position 1 cm from one end and a position 1 cm from the other end were fixed to a jig, and a tensile test was performed using a tensile tester (product name: FGS-TV, manufactured by Nidec-Shimpo Corporation). This test was performed at 23°C and a tensile speed of 5 mm / min. The breaking elongation was calculated based on the following formula. The obtained breaking elongation was evaluated according to the following evaluation rank. Breaking elongation (%) = 100 × (L-Lo) / Lo In the above formula, Lo is the length of the test piece before the tensile test (the jig distance), and L is the length of the test piece at break (the jig distance measured by butting the broken test piece together). -Evaluation rank of breaking elongation- 4: 15% or more 3: 5% or more, but less than 15% 2: 2% or more, less than 5% 1: Less than 2%

[0098] Using each copolymer X obtained above, a binder composition, an electrode composition, and an electrode sheet were prepared, and the adhesion of the obtained electrode active material layer to the current collector was evaluated. Furthermore, a secondary battery was prepared using the electrode sheet, and the discharge capacity retention rate was evaluated.

[0099] [Preparation of binder composition] (1) Preparation of Binder Composition 101 Binder composition 101, described in Table 1 below, was prepared. Specifically, 2.80g of the aqueous dispersion of the copolymer X1 (solid content 0.56g) and 11.4g of an aqueous solution of a water-soluble polymer (carboxymethylcellulose (CMC)) (solid content 0.24g) were added to a 60mL ointment container (Umano Chemical Co., Ltd.), and dispersed at 2000 rpm for 4 minutes using a THINKY THINKY Mixer (trade name). In the binder composition 101, the mass ratio of the contents of the copolymer X1 and the water-soluble polymer is the content of the copolymer X1 (solid content in the aqueous dispersion): the content of the water-soluble polymer (solid content in the aqueous solution) = 70:30. In this way, a binder composition 101 containing the liquid medium (water), the copolymer X, and the water-soluble polymer was obtained.

[0100] (2) Preparation of binder compositions 102-112, C101-103) Binder compositions 102 to 112 and C101 to 103 were obtained in the same manner as in the preparation of binder composition 101, except that binder composition 101 was changed to the composition shown in Table 1. In addition, when the binder composition contained the non-polymerizable surfactant component (C-2), the binder composition was prepared so that the mass ratio of the total content of the copolymer X and the non-polymerizable surfactant component (C-2) to the content of the water-soluble polymer was 70:30.

[0101] [Table 1]

[0102] <Notes for Table 1> AAm: Acrylamide 2EHA: 2-ethylhexyl acrylate BA: n-butyl acrylate PO-A: Phenoxyethyl acrylate (Light Acrylate PO-A (product name), manufactured by Kyoeisha Chemical Co., Ltd.) AA: Acrylic acid St: styrene SE-10N: Adeka Rear Soap SE-10N (product name) (manufactured by ADEKA) (polymerizable surfactant) DBS: Sodium dodecylbenzenesulfonate (non-polymerizable surfactant) CMC: Carboxymethylcellulose (CMC Daicel (product name), product number: 1140, manufactured by Daicel Miraize Co., Ltd.) Although AA and St are not monomers that lead to the hydrophobic vinyl compound component (B), for the sake of convenience, they are listed in the column for monomers that lead to the hydrophobic vinyl compound component (B). "-" indicates that the corresponding ingredient is not included. The "polymerization ratio" is expressed with the total content of (A) the monomer which leads to a water-soluble vinyl compound component and (B) the monomer which leads to a hydrophobic vinyl compound component being taken as 100 mass %. The "content" of the monomer from which the polymerizable surfactant component (C-1) is derived is expressed as the total content of all constituent components in copolymer X, i.e., the total content of (A) the monomer from which the water-soluble vinyl compound component is derived, (B) the monomer from which the hydrophobic vinyl compound component is derived, and (C-1) the monomer from which the polymerizable surfactant component is derived, taken as 100 mass%. The "content" of the non-polymerizable surfactant (C-2) is shown relative to the total content of the copolymer X and the non-polymerizable surfactant component (C-2) being 100 mass %. The "resin composition ratio" indicates the content (mass%) of each of the copolymer X and the water-soluble polymer when the total content of each of the copolymer X and the water-soluble polymer in the binder composition is 100 mass%. When the binder composition contains the (C-2) non-polymerizable surfactant component, the "resin composition ratio" of the copolymer X is a value including the content of the (C-2) non-polymerizable surfactant component.

[0103] [Preparation of electrode composition] In a 60 mL ointment container (Umano Chemical Co., Ltd.), 1.43 g of lithium-doped silicon oxide (LiSiO) (particle size: 7 μm, product name: KSC-7134, Shin-Etsu Chemical Co., Ltd.), 8.08 g of graphite (product name: G49, Zichen Co., Ltd.), 0.09 g of acetylene black (AB) (product name: Denka Black, Denka Co., Ltd.), 2.50 g (solid content: 0.01 g) of carbon nanotubes (CNT) (product name: Lamiful WPB-030, Kusumoto Chemical Co., Ltd.), and 5.69 g (solid content: 0.12 g) of CMC (product name: CMC Daicel, product number: 1140, Daicel Miraize Co., Ltd.) as a water-soluble polymer were added and dispersed at 2000 rpm for 6 minutes using a foaming mixer (THINKY Co., Ltd.). 0.22 g of distilled water was added to the dispersion, and the mixture was dispersed at 2000 rpm for 12 minutes using a WAWATORI MIXER (manufactured by THINKY Co., Ltd.) Further, 1.40 g (solid content: 0.28 g) of each aqueous dispersion of copolymer X (aqueous dispersion of copolymer X corresponding to the binder composition described in the "Binder" column in Table 2) was added to the dispersion, and the mixture was dispersed at 2000 rpm for 3 minutes using a WAWATORI MIXER (manufactured by THINKY Co., Ltd.). In this way, electrode compositions (negative electrode compositions) C-1 to C-12 and BC-1 to BC-3 shown in Table 2 were obtained. These electrode compositions each contain the same components as the binder compositions shown in Table 1 in the corresponding ratios. The "Binder, Type" column in Table 2 shows the corresponding binder composition No.

[0104] [Preparation of negative electrode sheet] Each of the obtained electrode compositions was applied onto a copper foil having a thickness of 20 μm using an applicator having an arbitrary clearance, and dried for 1 hour at 80° C. Thereafter, the composition was pressed using a press machine and then dried in a vacuum at 100° C. for 10 hours to obtain an electrode sheet (negative electrode sheet) having a negative electrode active material layer having a thickness of 25 μm.

[0105] [Collector adhesion: Evaluation of adhesion of negative electrode active material layer] Three test pieces measuring 10 mm wide and 50 mm long were cut out from the prepared negative electrode sheet. Adhesive tape (10 mm wide, 50 mm long, product name: Nicetack Business Pack, double-sided tape, manufactured by Nichiban Co., Ltd.) was attached to the negative electrode active material layer of each of the three cut out test pieces, and each test piece was attached to a glass plate via the adhesive tape. The glass plate was placed on the bottom side, and the average stress when the copper foil (current collector) was peeled off from the negative electrode active material layer at an angle of 90° and a speed of 100 mm / min was measured for each of the three test pieces. The value (unit: N) obtained by dividing the sum of the obtained average stresses by 3 was assigned to the following evaluation rank and evaluated. The results are shown in the "Collector Adhesion" column in Table 2 below. -Adhesion evaluation rank- 4: 0.20N or more 3: 0.12N or more, less than 0.20N 2: 0.05N or more, less than 0.12N 1: Less than 0.05N

[0106] [Evaluation of cycle characteristics] <Preparation of non-aqueous electrolyte secondary battery (2032 type coin battery)> Using each of the negative electrode sheets, a nonaqueous electrolyte secondary battery was fabricated. Specifically, a disk with a diameter of 13.0 mm was cut out from each of the negative electrode sheets and used to form the negative electrode. Lithium foil (thickness 50 μm, diameter 14.5 mm) and a polypropylene separator (thickness 25 μm, diameter 16.0 mm) were stacked in this order, and 200 μL of electrolyte II (electrolyte (concentration 1M) in which LiPF6 was dissolved in ethylene carbonate / ethyl methyl carbonate (volume ratio 1:2)) was soaked into the separator. 200 μL of the electrolyte II was further soaked on top of the separator, and the negative electrode sheet was stacked so that the negative electrode active material layer surface was in contact with the separator. Then, a 2032-type coin case was crimped to prepare a nonaqueous electrolyte secondary battery (a battery having a laminate consisting of Li foil-separator-negative electrode active material layer-copper foil).

[0107] <Cycle characteristics> For each coin battery, the discharge capacity retention rate after charge / discharge cycles was determined using a charge / discharge evaluation device: TOSCAT-3000 (product name, manufactured by Toyo Systems Co., Ltd.). First, the batteries were charged at a C rate (capacity rate) of 0.2 C (a rate at which the batteries are fully charged in 5 hours) until the battery voltage reached 0.02 V. Next, the batteries were discharged at a C rate of 0.2 C until the battery voltage reached 1.5 V. Each coin battery was initialized by repeating three cycles of charge and discharge, with one charge and one discharge constituting one charge and discharge cycle. After the initialization, the battery was charged at 0.5 C until it reached 0.02 V. Then, the battery was discharged at 0.5 C until it reached 1.5 V. This one charge and one discharge constituted one charge-discharge cycle, and the battery was repeatedly charged and discharged 80 times. The discharge capacity retention rate at the 80th cycle (100 x "discharge capacity at the 80th cycle" / "initial discharge capacity") was calculated assuming that the discharge capacity at the first cycle after initialization (initial discharge capacity) was 100%, and the cycle characteristics were evaluated according to the following evaluation rank. The results are shown in the "Cycle characteristics" column in Table 2 below. - Evaluation rank of cycle characteristics (discharge capacity retention rate) - 6: 90% or more 5: 85% or more, but less than 90% 4: 80% or more, but less than 85% 3: 70% or more, but less than 80% 2: 50% or more, but less than 70% 1: Less than 50%

[0108] [Table 2]

[0109] <Notes for Table 2> Content (%): The percentage of each component (solid content) in the total of each component (solid content) contained in the electrode composition, expressed by mass. However, the "content" in the "Binder" column is the percentage of the component (solid content) corresponding to the binder composition in the total of each component (solid content) of the electrode composition. The components corresponding to the binder composition include copolymer X and the water-soluble polymer, and (C) surfactant component, if present. LiSiO: Lithium-doped silicon oxide (KSC-7134 (product name), manufactured by Shin-Etsu Chemical Co., Ltd.) Graphite: Graphite (G49 (product name), manufactured by Zichen) AB: Acetylene black (Denka Black (product name), manufactured by Denka Co., Ltd.) CNT: Carbon nanotube (Lamiful WPB-030 (product name), manufactured by Kusumoto Chemical Industries, Ltd.)

[0110] The following can be seen from Tables 1 and 2: Binder compositions C101 to C103 are binder compositions containing copolymers CX1 to CX3 that do not contain as a constituent a component corresponding to the (B) hydrophobic vinyl compound component. Electrode compositions BC-1 to BC-3, which contain the same components as binder compositions C101 to C103 in the same ratios and further contain a silicon-based active material, gave electrode sheets with low adhesion of less than 0.12 N, and the discharge capacity retention rate of the resulting secondary batteries was less than 70%. Binder compositions 101-112 are binder compositions containing copolymers X1-X12 containing (A) a water-soluble vinyl compound component and (B) a hydrophobic vinyl compound component as constituents. Electrode compositions C-1-C-12, which contain the same components as binder compositions 101-112 in the same ratios and further contain a silicon-based active material, all had an electrode sheet with an adhesion of 0.12 N or more and a secondary battery with a discharge capacity retention rate of 80% or more. It can be seen that the binder composition and electrode composition of the present invention can improve the adhesion of the electrode sheet and the cycle characteristics of the secondary battery. In particular, when a binder composition containing a surfactant component was used, the adhesion of the resulting electrode sheet and the cycle characteristics of the resulting secondary battery tended to be excellent. [Explanation of symbols]

[0111] 10 Nonaqueous electrolyte secondary battery 1 Negative electrode current collector 2 Negative electrode active material layer 3. Separator 4 Cathode active material layer 5 Positive electrode current collector 6. Working part (light bulb)

Claims

1. A binder composition for a secondary battery comprising a liquid medium and a copolymer X, The binder composition for a secondary battery contains (A) a water-soluble vinyl compound component and (B) a hydrophobic vinyl compound component as constituent components of the copolymer X, a glass transition temperature of the homopolymer a composed of the water-soluble vinyl compound component (A) being 90° C. or higher, and a glass transition temperature of the homopolymer b composed of the hydrophobic vinyl compound component (B) being 0° C. or lower.

2. The binder composition for a secondary battery according to claim 1 , further comprising a surfactant component (C).

3. The binder composition for a secondary battery according to claim 2 , comprising the surfactant component (C) as a constituent component of the copolymer X.

4. 2. The binder composition for a secondary battery according to claim 1, wherein the water-soluble vinyl compound component (A) is a (meth)acrylamide component.

5. 2. The binder composition for a secondary battery according to claim 1, wherein the copolymer X has a breaking elongation of 15% or more.

6. The binder composition for a secondary battery according to claim 1 , wherein the binder composition for a secondary battery contains a water-soluble polymer.

7. The binder composition for a secondary battery according to claim 6 , wherein the water-soluble polymer comprises at least one of carboxymethyl cellulose, cellulose nanofiber, hydroxyethyl cellulose, hydroxypropyl cellulose, and xanthan gum.

8. The binder composition for a secondary battery according to claim 1 , wherein the liquid medium is water.

9. A composition for an electrode comprising a liquid medium, a copolymer X, and an active material, The copolymer X contains, as constituent components, (A) a water-soluble vinyl compound component and (B) a hydrophobic vinyl compound component, a glass transition temperature of the homopolymer a composed of the water-soluble vinyl compound component (A) being 90° C. or higher, and a glass transition temperature of the homopolymer b composed of the hydrophobic vinyl compound component (B) being 0° C. or lower.

10. The electrode composition according to claim 9 , wherein the active material comprises a silicon-based active material.

11. An electrode sheet having a layer formed using the electrode composition according to claim 9.

12. A secondary battery having a positive electrode active material layer, a separator, and a negative electrode active material layer in this order, A secondary battery, wherein at least one of the positive electrode active material layer and the negative electrode active material layer is a layer formed using the electrode composition according to claim 9.

13. A method for producing an electrode sheet, comprising forming an electrode active material layer using the electrode composition according to claim 9.

14. A method for producing a secondary battery, comprising incorporating an electrode sheet obtained by the method according to claim 13 as an electrode of the secondary battery.

Citation Information

Patent Citations

  • Silicon electrode binder

    JP2020533771A

  • Binder for secondary batteries, binder composition for secondary batteries, composition for electrodes, electrode sheet, secondary battery, method for producing electrode sheet, and method for producing secondary battery

    WO2022210737A1

Cited By

  • Negative electrode slurry, negative electrode plate and battery

    CN119725537A

  • A negative electrode slurry, a negative electrode sheet, and a battery

    CN119725537B