Manufacturing method for all-solid battery
By incorporating a controlled amount of release agent during the lamination of electrodes and solid electrolytes, the method addresses resistive adhesive issues, enhancing the bonding and performance of all-solid-state batteries.
Patent Information
- Application Number
- JP2023056395
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The bonding between electrodes and solid electrolytes in all-solid-state batteries is affected by resistive adhesive layers, leading to poor battery characteristics and potential peeling at the interface, which compromises the battery's performance.
A manufacturing method that involves laminating a negative electrode, solid electrolyte membrane, and positive electrode with a controlled amount of release agent between them, ensuring minimal resistance and improved bonding.
This method suppresses peeling at the electrode-solid electrolyte boundary, resulting in a high-quality all-solid-state battery with enhanced short-circuitability and cycle characteristics.
Smart Images

Figure 2024143622000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an all-solid-state battery having a solid electrolyte membrane and a method for manufacturing the all-solid-state battery. The all-solid-state battery of the present invention includes a lithium ion secondary battery and the like. [Background technology]
[0002] In recent years, with environmental considerations in mind, the development of secondary batteries that can be repeatedly charged and discharged as energy sources for automobiles and homes has been progressing. While the development of secondary batteries that can be expected to have high capacity and high output is expected, at the same time, greater emphasis must be placed on safety.
[0003] Among lithium-ion secondary batteries, which are one of the representative secondary batteries, solid-state batteries using solid electrolytes are known. An all-solid-state battery, which is one of the solid-state batteries, includes a solid electrolyte layer, a positive electrode layer formed on one side of the solid electrolyte layer, a negative electrode layer formed on the other side, a positive electrode plate connected to the positive electrode layer, and a negative electrode plate connected to the negative electrode layer.
[0004] The positive electrode layer can be obtained by coating a positive electrode current collector with a slurry containing positive electrode active material particles, a binder, a solid electrolyte, and a solvent, and drying the slurry. The positive electrode current collector can be made of aluminum foil or the like. On the other hand, the negative electrode can be obtained by coating a negative electrode current collector with a slurry containing negative electrode active material particles, a binder, a solid electrolyte, and a solvent, and drying the slurry. The negative electrode current collector can be made of copper foil. Alternatively, a lithium metal layer formed on stainless steel foil can be used as the negative electrode. The positive electrode layer and the negative electrode layer can further contain a conductive assistant.
[0005] The solid electrolyte layer can be formed by dispersing a solid electrolyte powder in a solvent to form a slurry, which is then applied and dried. For example, the solid electrolyte layer can be formed directly on the surface of the negative electrode layer or the positive electrode layer. The solid electrolyte layer can also be obtained by forming the solid electrolyte layer on the surface of a polyester substrate such as a polyethylene terephthalate (PET) film, and then peeling off the substrate.
[0006] The resulting positive and negative electrodes are laminated with a solid electrolyte sandwiched therebetween and pressurized to obtain an electrode laminate. A positive electrode terminal and a negative electrode terminal are attached to this electrode laminate, and the electrode laminate is housed and sealed in an outer container so that one end of each terminal is extended to the outside, to obtain an all-solid-state battery.
[0007] A release agent layer such as a silicone compound is generally formed on the surface of the polyester film to facilitate peeling of the solid electrolyte layer. If this release agent layer transfers to the solid electrolyte layer, there is concern that poor bonding between the solid electrolyte layer and the electrodes and irreversible capacitance may occur due to electrolyte ions being taken into the release agent layer. Therefore, measures are being considered to prevent the silicone compound from transferring to the solid electrolyte layer, etc.
[0008] In addition, there is a problem that the positive electrode, negative electrode, and solid electrolyte layer used in the all-solid-state battery are easily peeled off at the bonding interface between them. In order to increase the strength of the bonding interface between them, a measure has been taken to laminate them via an adhesive layer.
[0009] Patent Document 1 discloses a technique for preventing the transfer of a release agent to a solid electrolyte layer by forming an antistatic layer on the surface of a polyester film in advance and carrying out pretreatment such as anchor coating, corona treatment, plasma treatment, atmospheric pressure plasma treatment, etc. Patent Document 2 discloses a technique for bonding a solid electrolyte layer and an electrode via an adhesive layer. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2022-142259 A [Patent Document 2] International Publication No. 2020 / 137354 Summary of the Invention [Problem to be solved by the invention]
[0011] However, when an electrode such as a positive electrode or a negative electrode is bonded to a solid electrolyte or when solid electrolytes are bonded to each other via an adhesive layer, the components of the adhesive layer become a resistance and adversely affect the battery characteristics. On the other hand, when the adhesive layer is completely removed, the bond between the electrode such as a positive electrode or a negative electrode and the solid electrolyte or the bond between solid electrolytes is weakened, and the bonded surfaces may peel off.
[0012] As a result of extensive research, the inventors have found that by leaving an appropriate amount of release agent, which is transferred from a film to a solid electrolyte, on the surface of the solid electrolyte or electrode, it is possible to suppress the resistance of the all-solid-state battery to a tolerable minimum range and prevent insulation of the battery. [Means for solving the problem]
[0013] The present invention relates to a method for producing an all-solid-state battery, which includes a step of laminating a negative electrode, a solid electrolyte film, and a positive electrode to form an electrode laminate. The method for producing an all-solid-state battery includes a step of applying a slurry containing a solid electrolyte in a solvent onto a surface of a film on which a release agent layer containing a release agent is formed to form the solid electrolyte film, a step of removing the film from the release agent layer, and a step of laminating the solid electrolyte film containing the release agent layer exposed by removing the film on the positive electrode, in which the release agent is present in an amount of 0.01 mg / cm between the solid electrolyte film and the positive electrode. 2 More than 0.5mg / cm 2 The present invention is characterized in that the solid electrolyte membrane and the positive electrode are laminated so as to have a density as follows: Effect of the Invention
[0014] According to the manufacturing method of the present invention, in an all-solid-state battery, peeling at the boundary between the electrode and the solid electrolyte film is suppressed, and a high-quality all-solid-state battery having excellent short-circuiting potential and cycle characteristics can be obtained. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a flow diagram showing an outline of an assembly process for an all-solid-state battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The following describes an embodiment of the present invention with reference to the drawings. Note that the present invention is not limited to the embodiment described below, and can be implemented within the scope of the present invention. The following is an example, and does not limit the present invention in any way.
[0017] <All-solid-state battery> In this specification, the term "all-solid-state battery" refers to a battery in which the electrolyte is made of a solid electrolyte, which will be described later. In addition, in this specification, the term "all-solid-state battery" includes secondary batteries and primary batteries. <Negative electrode> The negative electrode may be any negative electrode used in non-aqueous secondary battery materials, and is not particularly limited. For example, the negative electrode includes a negative electrode collector such as copper foil, and a negative electrode layer containing a negative electrode active material and a solid electrolyte. The negative electrode layer preferably contains a binder. A negative electrode collector made of stainless steel may be used instead of the negative electrode collector such as copper foil, and a lithium metal layer may be formed on the surface of the negative electrode collector by rolling or the like instead of the negative electrode active material. The negative electrode layer containing the negative electrode active material, the solid electrolyte, and the binder may be formed on at least one surface of the negative electrode collector.
[0018] When a negative electrode active material is used for the negative electrode, it is preferable to use a carbon-based active material. As the carbon-based active material, natural graphite, artificial graphite, hard carbon, soft carbon, carbon black, or any mixture thereof can be selected. Natural graphite includes natural graphite with amorphous carbon coated on the particle surface, and similarly, artificial graphite includes artificial graphite with amorphous carbon coated on the particle surface. These natural graphites and artificial graphites can be used in the form of primary particles, particles in which primary particles are aggregated to form secondary particles, or mixtures thereof. In addition, the negative electrode active material may be a mixture of a carbon-based active material and a silicon-based active material. The negative electrode active material may include a metal material such as aluminum, aluminum, silver, bismuth, calcium, cerium, indium, magnesium, tin, zinc, or nickel.
[0019] Examples of the binder used in the negative electrode layer include fluororesins such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and polyvinyl fluoride (PVF), conductive polymers such as polyanilines, polythiophenes, polyacetylenes, and polypyrroles, synthetic rubbers such as styrene butadiene rubber (SBR), butadiene rubber (BR), chloroprene rubber (CR), isoprene rubber (IR), and acrylonitrile butadiene rubber (NBR), and polysaccharides such as carboxymethyl cellulose (CMC), xanthan gum, guar gum, and pectin. In addition, examples of the binder include polyacrylic acid, polymethacrylic acid, sodium polyacrylate, potassium polyacrylate, sodium polymethacrylate, potassium polymethacrylate; ethyl polyacrylate, ethyl polyacrylate, butyl polyacrylate, methyl polymethacrylate, ethyl polymethacrylate, butyl polymethacrylate, and any mixture thereof. The content of the binder is preferably 1% by mass or more and less than 10% by mass with respect to the total solid content of the negative electrode layer. If the content of the binder is too high, the surface of the negative electrode active material is covered with the binder in a large area, which may reduce the ionic conductivity and electronic conductivity. If the content of the binder is too low, the electrical contact between the particles of the negative electrode active material may not be properly performed.
[0020] In addition to the above compounds, the binder component may further include carboxymethylcellulose (referred to as "CMC"), which is a cellulose derivative, or a metal salt of carboxymethylcellulose (e.g., sodium carboxymethylcellulose, potassium carboxymethylcellulose). When CMC or a metal salt of CMC is further added as a binder component, the content of CMC or the CMC metal salt is preferably 0.05% by mass or more and 1.5% by mass or less with respect to the total solid content of the negative electrode layer.
[0021] The negative electrode layer may further contain a conductive assistant. The conductive assistant is a material for reducing the resistance of the electrode. Examples of the conductive assistant include carbon black such as acetylene black and ketjen black, activated carbon, graphite, mesoporous carbon, fullerenes, carbon nanotubes, carbon nanofibers, carbon brushes, and other carbon fibers.
[0022] When carbon nanotubes or carbon nanofibers are used as the conductive assistant, the content of the conductive assistant is 0.01% by mass to 3% by mass, preferably 0.03% by mass to 1% by mass, based on the total solid content of the negative electrode layer.
[0023] In addition to the above-mentioned materials, the negative electrode layer may appropriately contain electrode additives that are generally used for forming electrodes, such as thickeners, dispersants, and stabilizers.
[0024] <Solid electrolyte membrane> The negative electrode, the solid electrolyte film, and the positive electrode used in the manufacturing method of the embodiment include a solid electrolyte. The solid electrolyte used here can be exemplified by an oxide-based solid electrolyte and a sulfide-based solid electrolyte. The oxide-based solid electrolyte can be, but is not limited to, an oxide-based material such as a garnet type, a NASICON type, or a perovskite type. As the sulfide-based solid electrolyte, any known sulfide-based substance can be used, for example, LiPO4-Li2S-SiS, 75% Li2S-25% P2S5 mixture, Li2S-SiS2, Li2S-P2S5, Li3PS4, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiI-Li2S-B2S3, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5Li2S-P2S5-LiCl, Li6PS5Cl, Li 10 GeP2S 12 , Li 3.25 Ge 0.25 P 0.75 S4, etc. In the embodiment, it is preferable to use a sulfide-based solid electrolyte. The solid electrolyte membrane used in the embodiment refers to a thin flat surface having a predetermined area and made of a solid electrolyte. The solid electrolyte membrane may be a single layer (a solid electrolyte membrane made of one type of solid electrolyte) or a multi-layer (a solid electrolyte membrane made of two or more types of solid electrolyte membranes stacked together).
[0025] In the present invention, the solid electrolyte membrane is preferably formed to have a thickness of 15 to 150 μm. If the thickness is smaller than this, the battery is likely to short-circuit when the solid electrolyte is press-formed under high pressure. On the other hand, if the thickness is larger than this, the cell volume increases excessively, and the energy density per unit volume of the all-solid-state battery does not increase.
[0026] <Release sheet> The release sheet refers to a flexible sheet on which a release agent layer that makes it easy to peel off the solid electrolyte membrane is formed on the surface of the sheet member. As the flexible sheet, for example, a general polyester film can be used, and a film mainly containing a component selected from polyethylene terephthalate, polyethylene-2,6-naphthalate, polybutylene terephthalate, polytrimethylene terephthalate, and a mixture thereof can be used, but is not limited to this. As the release agent constituting the release agent layer, a silicone-based, alkyd-based, olefin-based, fluorine-based, or alkyl-based release agent, or a combination of these can be used. Among them, it is preferable to use a release agent containing a silicone resin having a reactive functional group that can be cured by ultraviolet light or heat, and which can easily control the amount of transfer of the release agent by controlling the temperature.
[0027] <Positive electrode> The positive electrode can be a positive electrode used in a non-aqueous secondary battery material, and is not particularly limited. For example, the positive electrode includes a positive electrode collector, a positive electrode active material, and a positive electrode layer containing a solid electrolyte. The positive electrode layer preferably contains a binder. The positive electrode layer containing the positive electrode active material, the solid electrolyte, and the binder can be formed on at least one surface of the positive electrode collector.
[0028] The positive electrode current collector can be made of stainless steel, aluminum, nickel, titanium, or a positive electrode current collector in which the surface of aluminum or stainless steel is surface-treated with carbon, nickel, titanium, or silver.
[0029] The positive electrode active material preferably contains a lithium nickel-based composite oxide as the positive electrode active material. The lithium nickel-based composite oxide is represented by the general formula Li x Ni y Me (1-y) The positive electrode active material is a transition metal composite oxide containing lithium and nickel, represented by the general formula LiMnO2 (wherein Me is at least one metal selected from the group consisting of Al, Mn, Na, Fe, Co, Cr, Cu, Zn, Ca, K, Mg, and Pb). Examples of the lithium manganese composite oxide that can contain the lithium manganese composite oxide include lithium manganese oxide (LiMnO2) with a zigzag layer structure and lithium manganese oxide (LiMn2O4). The positive electrode active material is particularly a transition metal composite oxide represented by the general formula Li x Ni y Co z Mn (1-y-z)It is preferable that the positive electrode active material contains a lithium nickel manganese cobalt composite oxide having a layered crystal structure represented by O2. Here, in the general formula, x is 1≦x≦1.2, y and z are positive numbers satisfying y+z<1, and the value of y is 0.5 or more. In order to obtain a high-capacity battery, it is particularly preferable to make y>1-yz and y>z. The lithium nickel composite oxide having this general formula is, in other words, a lithium nickel cobalt manganese composite oxide. The lithium nickel cobalt manganese composite oxide is a lithium nickel composite oxide that is preferably used to increase the capacity of a battery. In addition, the positive electrode active material may contain the general formula LiMPO4 (M is at least one selected from the group consisting of Mn, Fe, Co, and Ni). The surface of the positive electrode active material may be coated with a material such as LiNbO3 to form a buffer layer. The buffer layer can be formed of a buffer layer forming material to a thickness of 10 nm or less to suppress the interface resistance between the positive electrode layer and the solid electrolyte film. The buffer layer can be formed on the surface of the positive electrode layer by a sol-gel method or the like.
[0030] Examples of binders that form the positive electrode layer together with the positive electrode active material include fluororesins such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and polyvinyl fluoride (PVF); conductive polymers such as polyanilines, polythiophenes, polyacetylenes, and polypyrroles; styrene butadiene rubber (SBR), butadiene rubber (BR), chloroprene rubber (CR), isoprene rubber (IR), and acrylonitrile butadiene rubber (ACRB). Examples of the rubber include synthetic rubber such as NBR (Nylon Brass) and polysaccharides such as carboxymethyl cellulose (CMC), xanthan gum, guar gum, and pectin.
[0031] The positive electrode layer may also contain a conductive assistant. Examples of the conductive assistant include carbon black such as acetylene black and ketjen black, activated carbon, graphite, mesoporous carbon, fullerenes, carbon nanofibers, carbon nanotubes, carbon nanobrushes, and other carbon fibers. In addition, the positive electrode layer may appropriately contain electrode additives that are generally used for forming electrodes, such as thickeners, dispersants, and stabilizers.
[0032] <Cell Preparation> First, the preparation of the negative electrode will be described. There are several methods for preparing the negative electrode, but whichever method is used, it is preferable to prepare the negative electrode in a low moisture environment under dew point control in order to suppress adsorption of moisture into the solid electrolyte.
[0033] <Preparation of negative electrode> When using a negative electrode in which a negative electrode layer is formed on a negative electrode current collector, a slurry in which a negative electrode active material, a solid electrolyte, and a binder are dispersed in a dehydrated organic solvent is applied to a part or all of the surface of a negative electrode current collector such as a copper foil, and dried to obtain a negative electrode precursor sheet. The obtained negative electrode precursor sheet is compressed by a press molding method such as a roll press, a uniaxial press, a rubber press, or an isostatic press (CIP, WIP) to obtain a negative electrode sheet. Examples of organic solvents include acetonitrile, xylene, dimethoxyethane, dimethyl carbonate, tertiary amine solvents such as triethylamine, heptane, hexane, tetrahydrofuran, toluene, and N-methylpyrrolidone, as well as ether solvents, thiol solvents, and butyl butyrate, and it is preferable that all of them are dehydrated.
[0034] Alternatively, a granulated negative electrode active material containing at least a negative electrode active material, a solid electrolyte, and a binder can be transferred to a negative electrode current collector to obtain a negative electrode precursor sheet. In this case, a surface layer containing a polymer component such as a binder that enhances adhesion to the granulated negative electrode active material may be formed in advance on the surface of the negative electrode current collector. The negative electrode layer may also contain a conductive assistant. The obtained negative electrode precursor sheet is compressed by a press molding method such as a roll press, a uniaxial press, a rubber press, or a cold isostatic press (CIP, WIP) to obtain a negative electrode sheet.
[0035] Alternatively, a metallic lithium layer such as lithium foil is disposed on all or part of a stainless steel negative electrode current collector, and these are then bonded together by rolling or other treatment to obtain a negative electrode sheet.
[0036] <Preparation of solid electrolyte membrane> Next, a solid electrolyte membrane is formed on the surface of the negative electrode. Regardless of the method used to form the solid electrolyte membrane, it is preferable to form the membrane in a low moisture environment under dew point control in order to prevent moisture from being adsorbed by the solid electrolyte.
[0037] A slurry in which a solid electrolyte is dispersed in an organic solvent is applied to the surface of the negative electrode layer formed on a copper foil or the surface of metallic lithium formed on a stainless steel foil, and then dried to form a solid electrolyte film on the surface of the negative electrode. Examples of the organic solvent include acetonitrile, xylene, dimethoxyethane, dimethyl carbonate, tertiary amine solvents such as triethylamine, heptane, hexane, tetrahydrofuran, toluene, and N-methylpyrrolidone, as well as ether solvents, thiol solvents, and butyl butyrate, and it is preferable that all of them are dehydrated.
[0038] Alternatively, a solid electrolyte film can be formed on the surface of the negative electrode by applying a slurry in which a solid electrolyte is dispersed in an organic solvent to the surface of a polyester film mainly composed of polyester, drying the film to form a solid electrolyte film, and then laminating the polyester film together so that the solid electrolyte film comes into contact with the surface of the negative electrode layer or the surface of metallic lithium. In this case, it is preferable to form a solid electrolyte film on the surface of the release sheet on which the release agent layer is applied, and then laminating the release sheet together so that the solid electrolyte film comes into contact with the surface of the negative electrode layer or the surface of metallic lithium. When the release film is peeled off from the obtained laminate, a negative electrode-solid electrolyte film laminate is obtained, and it is very preferable that some of the release agent layer of the release sheet is transferred onto the surface of this solid electrolyte film, and the release agent remains on the surface of the solid electrolyte film. By laminating such a negative electrode-solid electrolyte film laminate on the positive electrode described later, a release agent can be present between the solid electrolyte film and the positive electrode. Between the solid electrolyte film and the positive electrode, a release agent of 0.01 mg / cm is preferably used. 2 More than 0.5mg / cm 2 It is highly preferred that it is present at a density of:
[0039] The laminated negative electrode and solid electrolyte membrane are compressed by a press molding method such as roll press, uniaxial press, rubber press, or isostatic press (CIP, WIP), to obtain a negative electrode-solid electrolyte membrane laminate. When the solid electrolyte is laminated together with a polyester sheet and pressurized, the polyester film is peeled off from the solid electrolyte membrane. In this case, it is also preferable to use a polyester film whose surface is coated with a release agent such as silicone so that the polyester film can be easily peeled off from the solid electrolyte membrane.
[0040] <Preparation of positive electrode> Next, the preparation of the positive electrode will be described. Regardless of the method used to prepare the positive electrode, it is preferable to prepare the positive electrode in a low moisture environment under dew point control in order to suppress adsorption of moisture.
[0041] A slurry in which a positive electrode active material, a solid electrolyte, and a binder are dispersed in a dehydrated organic solvent is applied to a part or the whole surface of a positive electrode current collector such as aluminum, and then dried to obtain a positive electrode sheet. Examples of organic solvents include acetonitrile, xylene, dimethoxyethane, dimethyl carbonate, tertiary amine solvents such as triethylamine, heptane, hexane, tetrahydrofuran, toluene, and N-methylpyrrolidone, as well as ether solvents, thiol solvents, and butyl butyrate, and it is preferable that all of them are dehydrated.
[0042] <Formation of Electrode Laminate> A positive electrode sheet is laminated on the negative electrode-solid electrolyte membrane laminate to obtain an electrode laminate precursor. When a sulfide-based solid electrolyte is used as the solid electrolyte, the ionic conductivity of the solid electrolyte decreases due to exposure to moisture. Therefore, after obtaining the electrode laminate precursor, it is desirable to compress the electrode laminate precursor by a press molding method such as roll press, uniaxial press, rubber press, or isostatic press (CIP, WIP) within a predetermined time to obtain an electrode laminate. The predetermined time is, for example, within 2 days in an environment with a dew point of -40°C and a moisture concentration of 127 ppm or less. If the time passes beyond this, there is a risk of performance deterioration due to water absorption by the solid electrolyte, which is not preferable from the viewpoint of reducing the productivity of all Dongfeng batteries.
[0043] The positive electrode can be first roll-pressed in the form of a thin sheet consisting of only a positive electrode layer formed on a positive electrode current collector, and then laminated onto the negative electrode-solid electrolyte membrane laminate, or, from the viewpoint of production efficiency, can be placed on the negative electrode-solid electrolyte membrane laminate without applying pressure to the positive electrode sheet alone, or with only enough pressure to hold down the positive electrode sheet with the conveying arm of the lamination machine. This step is the step immediately before the isostatic pressing to form the electrode laminate.
[0044] Up to this point, an embodiment has been described in which a negative electrode-solid electrolyte membrane laminate is produced and then a positive electrode sheet is laminated thereon. However, it is also possible to laminate a positive electrode and a solid electrolyte membrane formed on the surface of a polyester sheet, press them, peel off the polyester sheet, produce a positive electrode-solid electrolyte membrane laminate, and then laminate a negative electrode sheet on the surface on which the release agent remains.
[0045] <Sealing of electrode laminate> The obtained electrode laminate is desirably sealed in an exterior case immediately. One end of a rectangular metal plate serving as a negative terminal is attached to the negative current collector, and one end of a rectangular metal terminal serving as a positive terminal is attached to the positive current collector, and then the electrode laminate is housed in an aluminum exterior case. It is preferable that a resin layer such as polyolefin is formed on at least the inner surface of the exterior case that faces the electrode laminate. The resin layer is heated to melt the resin and then solidified again to seal the electrode laminate in the aluminum exterior case. At this time, the other end of the positive terminal and the other end of the negative terminal are arranged so as to be drawn out of the exterior case. A layer of the same or different type of resin as the resin used in the resin layer on the inner surface of the exterior case can also be provided in the portion where the positive terminal and the negative terminal contact the resin layer on the inner surface of the exterior case. By the above method, an all-solid-state battery including an electrode laminate formed by laminating an anode, a solid electrolyte film, and a cathode can be obtained. Another embodiment of the present invention is an all-solid-state battery in which the anode includes at least an anode layer, the cathode includes at least a cathode layer, the anode layer is in contact with the solid electrolyte film, and the cathode layer is in contact with the solid electrolyte film, and a release agent layer including a silicone resin and a conductive powder is present at at least one of the boundary between the anode layer and the solid electrolyte film and the boundary between the cathode layer and the solid electrolyte film. EXAMPLES
[0046] A battery was fabricated according to the flow shown in the embodiment of the invention. Figure 1 is a flow diagram summarizing the embodiment of the invention.
[0047] [I] Formation of negative electrode-solid electrolyte membrane laminate (1) A foil (manufactured by Honjo Metals Co., Ltd.) having a 20 μm thick metallic lithium layer formed on the surface of a 10 μm thick stainless steel negative electrode current collector was prepared as a negative electrode. (2) A slurry in which the solid electrolyte Li6PS5Cl (D50: 8μm) was dispersed in xylene as an organic solvent was applied to the surface of a release film (release sheet) in which a release agent layer was formed on a polyester film whose main component was polyester, and then dried to obtain a solid electrolyte film. The obtained solid electrolyte film was laminated with a polyester film so that it was in contact with the surface of metallic lithium. (3) The negative electrode-solid electrolyte membrane laminate of (2) above was laminated and vacuum sealed in a nylon vacuum pack and held at room temperature (25°C) under a pressure of 400 MPa for 1 minute. Thereafter, while still laminated and sealed, the negative electrode-solid electrolyte membrane laminate was compressed by an isostatic pressure pressing method to obtain a negative electrode-solid electrolyte membrane laminate with a porosity of the negative electrode layer of 7%. The size of the negative electrode-solid electrolyte membrane laminate was 50 mm x 70 mm. (4) The polyester film was peeled off from the solid electrolyte membrane to obtain a negative electrode-solid electrolyte membrane laminate.
[0048] [II] Peeling off the release sheet (1) By adjusting the temperature during the isostatic pressing method in the above [I](3), the amount of the release agent transferred to the negative electrode-solid electrolyte membrane laminate obtained in the above [I](4) was changed as shown in Table 1.
[0049] [III] Lamination of the positive electrode sheet and the negative electrode-solid electrolyte membrane laminate (1) LiNi particles coated with 10 nm thick LiNbO3 as the positive electrode active material 0.8 Co 0.1 Mn 0.1 A slurry of 70 mass% O2 (D50: 8 μm), 25 mass% Li6PS5Cl (average particle size 1 μm) as a solid electrolyte, 2 mass% acetylene black (manufactured by Timcal Japan Co., Ltd.), and 3 mass% styrene-butadiene rubber (SBR) as a binder dispersed in xylene, an organic solvent, was applied to an aluminum foil (manufactured by UACJ Corporation) with a thickness of 10 μm and dried to form a positive electrode layer, thereby obtaining a positive electrode. (2) The positive electrode obtained in (1) above was cut to 45 mm × 65 mm, and laminated so that the surface of the negative electrode-solid electrolyte membrane laminate on which the release agent was transferred and the release agent layer were provided in [I] came into contact with the positive electrode layer, to obtain an electrode laminate precursor. The number of layers of the positive electrode and negative electrode-solid electrolyte membrane laminate was one each.
[0050] [IV] Pressurizing the electrode stack (1) The electrode laminate precursor obtained in each Example was laminated and vacuum sealed in a nylon vacuum pack and held at room temperature (25° C.) under a pressure of 400 MPa for 1 minute. Next, while still laminated and sealed, the electrode laminate precursor was compressed by an isostatic pressing method to obtain an electrode laminate with a positive electrode layer porosity of 5%.
[0051] [V] Encapsulation in outer case (1) The electrode laminate obtained in [IV] above was enclosed in an outer case by the method described in the embodiment, and a battery was obtained in which the positive and negative terminals were extended outside the aluminum outer case (manufactured by Dai Nippon Printing Co., Ltd.).
[0052] The resistance value of the obtained battery at 25° C. and 1 kHz and the presence or absence of a short circuit after 20 charge / discharge cycles are shown in Table 1. The 1 kHz resistance is the resistance value measured by the AC (1 kHz ±0.2 Hz) four-terminal method (using a HIOKI 3560 AC milliohm hitester). It was found that the 1 kHz resistance changes depending on the amount of release agent transferred onto the solid electrolyte film. In addition, the presence or absence of a short circuit in the battery after 20 cycles of charge and discharge was evaluated under the following charge and discharge conditions: constant current charging at 0.05C up to an upper voltage of 4.2V in a constant temperature bath at 45°C, followed by constant voltage charging with a total charging time of 20 hours for one cycle, and constant current discharging at 0.05C down to 3.0V, repeated 20 times, and then electricity was passed through the battery. If a short circuit occurred, it was evaluated as "present", and if no short circuit occurred, it was evaluated as "absent". [Table 1]
[0053] The examples in the present invention are merely examples and are not limited thereto. For example, an aluminum laminate film is used for the exterior case, but a strong aluminum can case or a cylindrical case may be used. Li6PS5Cl is used as the solid electrolyte, but the present invention can be applied to any sulfide-based solid electrolyte that has low chemical stability with water. The positive and negative electrodes are adjusted to a predetermined size in advance, but they may be cut into a predetermined shape immediately after stacking. Needless to say, other design changes are possible within the scope of the invention.
Claims
1. A method for producing an all-solid-state battery, comprising: laminating a negative electrode, a solid electrolyte membrane, and a positive electrode to form an electrode laminate, A step of applying a slurry containing a solid electrolyte in a solvent onto a film surface on which a release agent layer containing a release agent is formed to form the solid electrolyte membrane; removing the film from the release agent layer; laminating the solid electrolyte membrane, including the release agent layer exposed by removing the film, on the positive electrode; The release agent is present between the solid electrolyte membrane and the positive electrode in an amount of 0.01 mg / cm 2 0.5mg / cm or more 2 The solid electrolyte membrane and the positive electrode are laminated so as to have a density of: A method for producing an all-solid-state battery.
2. The method for producing an all-solid-state battery according to claim 1 , wherein the release agent layer contains a silicone resin.
Citation Information
Patent Citations
Mold releasing film for all-solid battery material production
JP2022142259A
Battery and method for manufacturing battery
WO2020137354A1
Cited By
Apparatus for manufacturing all-solid-state battery and method for manufacturing all-solid-state battery