Manufacturing method for all-solid battery
By forming a solid electrolyte membrane on a release film with controlled moisture, the method addresses peeling issues in all-solid-state batteries, improving manufacturing yield and quality.
Patent Information
- Application Number
- JP2023056406
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The manufacturing yield of all-solid-state batteries is compromised due to peeling damage at the electrode and solid electrolyte membrane boundary, even with sufficient reduction of water content in the solid electrolyte, active material, and binder.
A method for manufacturing all-solid-state batteries involving the formation of a solid electrolyte membrane on a release film with a controlled moisture content of 70-200 ppm, allowing for easier peeling and reducing damage during the peeling process.
This method suppresses peeling damage and enhances the manufacturing yield of high-quality all-solid-state batteries.
Smart Images

Figure 2024143632000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an all-solid-state electrolyte. The all-solid-state battery of the present invention includes a lithium ion secondary battery and the like. [Background technology]
[0002] In recent years, with environmental considerations in mind, the development of secondary batteries that can be repeatedly charged and discharged as energy sources for automobiles and homes has been progressing. While the development of secondary batteries that can be expected to have high capacity and high output is expected, at the same time, greater emphasis must be placed on safety.
[0003] Among lithium-ion secondary batteries, which are one of the representative secondary batteries, solid-state batteries using solid electrolytes are known. An all-solid-state battery, which is one of the solid-state batteries, includes a solid electrolyte layer, a positive electrode layer formed on one side of the solid electrolyte layer, a negative electrode layer formed on the other side, a positive electrode plate connected to the positive electrode layer, and a negative electrode plate connected to the negative electrode layer.
[0004] The positive electrode layer can be obtained by coating a positive electrode current collector with a slurry containing positive electrode active material particles, a binder, a solid electrolyte, and a solvent, and then drying the slurry. The positive electrode current collector can be made of aluminum foil or the like. On the other hand, the negative electrode can be obtained by coating a negative electrode current collector with a slurry containing negative electrode active material particles, a binder, a solid electrolyte, and a solvent, and then drying the slurry. The negative electrode current collector can be made of copper foil. Alternatively, a lithium metal layer formed on stainless steel foil can be used as the negative electrode. The positive electrode layer or the negative electrode layer can further contain a conductive assistant.
[0005] The solid electrolyte layer can be formed by dispersing a solid electrolyte powder in a solvent to form a slurry, which is then applied and dried. For example, the solid electrolyte layer can be formed directly on the surface of the negative electrode layer or the positive electrode layer. The solid electrolyte layer can also be obtained by forming the solid electrolyte layer on the surface of a substrate such as a polyethylene terephthalate (PET) film, and peeling off the PET film. A release agent such as a silicone compound is formed on the surface of the polyester film to facilitate peeling off of the solid electrolyte layer.
[0006] The resulting positive and negative electrodes are laminated with a solid electrolyte sandwiched therebetween and pressurized to obtain an electrode laminate. A positive electrode terminal and a negative electrode terminal are attached to this electrode laminate, and the electrode laminate is housed and sealed in an outer container so that one end of each terminal is extended to the outside, to obtain an all-solid-state battery.
[0007] As a solid electrolyte, a sulfide solid electrolyte is known. It is known that a sulfide solid electrolyte is chemically unstable and that its ionic conductivity decreases due to moisture when exposed to the atmosphere. Therefore, when a sulfide solid electrolyte is used, the positive or negative electrode active material and the solid electrolyte material itself are sufficiently dried in advance, and further, the dew point is strictly controlled in the lamination process of the positive electrode, negative electrode, and solid electrolyte layer, so that the assembly can be performed quickly under a low moisture concentration.
[0008] Patent Document 1 discloses that in the manufacturing process of an all-solid-state battery, after the negative electrode active material layer is produced, only the negative electrode active material layer is heated before assembling the all-solid-state battery to remove water absorbed by the solid electrolyte in the negative electrode active material layer. Patent Document 2 discloses that the moisture content of positive electrode active material particles, the surface of which is partially coated with a lithium ion conductive oxide, is 319 ppm or less. Patent Document 3 discloses a technology for reducing the moisture content of the binder to 200 ppm. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2017-50209 A [Patent Document 2] JP 2018-125214 A [Patent Document 3] WO 2022 / 44815 Summary of the Invention [Problem to be solved by the invention]
[0010] However, even if the moisture content of the solid electrolyte, active material, and binder is sufficiently reduced, the manufacturing yield of the product may decrease when the battery is fabricated and the cycle characteristics are evaluated.
[0011] As a result of intensive research, the inventors have found that when a solid electrolyte layer is formed on the surface of a polyester film, by appropriately removing moisture contained in a release agent formed on the surface of the polyester film, it is possible to suppress damage to the solid electrolyte layer when the solid electrolyte layer is peeled off from the release film, and to improve the manufacturing yield when the solid electrolyte layer is made into a battery. [Means for solving the problem]
[0012] The present invention relates to a method for producing an all-solid-state battery, which includes a step of forming an electrode laminate by stacking a negative electrode, a solid electrolyte film, and a positive electrode. The method for producing an all-solid-state battery includes a step of applying a slurry containing a solid electrolyte in a solvent onto a surface of a film on which a release agent layer having a water content of 70 ppm or more and 200 ppm or less has been formed, to form the solid electrolyte film. Effect of the Invention
[0013] According to the manufacturing method of the present invention, peeling at the boundary between the electrode and the solid electrolyte film in the all-solid-state battery is suppressed, and an all-solid-state battery with high quality and good manufacturing yield can be obtained. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a flow diagram showing an outline of an assembly process for an all-solid-state battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The following describes an embodiment of the present invention with reference to the drawings. Note that the present invention is not limited to the embodiment described below, and can be implemented within the scope of the present invention. The following is an example, and does not limit the present invention in any way.
[0016] <All-solid-state battery> In this specification, the term "all-solid-state battery" refers to a battery in which the electrolyte is made of a solid electrolyte, which will be described later. In addition, in this specification, the term "all-solid-state battery" includes secondary batteries and primary batteries. <Negative electrode> The negative electrode may be any negative electrode used in non-aqueous secondary battery materials, and is not particularly limited. For example, the negative electrode includes a negative electrode collector such as copper foil, and a negative electrode layer containing a negative electrode active material and a solid electrolyte. The negative electrode layer preferably contains a binder. A negative electrode collector made of stainless steel may be used instead of the negative electrode collector such as copper foil, and a lithium metal layer may be formed on the surface of the negative electrode collector by rolling or the like instead of the negative electrode active material. The negative electrode layer containing the negative electrode active material, the solid electrolyte, and the binder may be formed on at least one surface of the negative electrode collector.
[0017] When a negative electrode active material is used for the negative electrode, it is preferable to use a carbon-based active material. As the carbon-based active material, natural graphite, artificial graphite, hard carbon, soft carbon, carbon black, or any mixture thereof can be selected. Natural graphite includes natural graphite with amorphous carbon coated on the particle surface, and similarly, artificial graphite includes artificial graphite with amorphous carbon coated on the particle surface. These natural graphites and artificial graphites can be primary particles or particles in which primary particles are aggregated to form secondary particles, and mixtures thereof. In addition, the negative electrode active material may be a mixture of a carbon-based active material and a silicon-based active material. The negative electrode active material may include metal materials such as aluminum, silver, bismuth, calcium, cerium, indium, magnesium, tin, zinc, and nickel.
[0018] Examples of the binder used in the negative electrode layer include fluororesins such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and polyvinyl fluoride (PVF), conductive polymers such as polyanilines, polythiophenes, polyacetylenes, and polypyrroles, synthetic rubbers such as styrene butadiene rubber (SBR), butadiene rubber (BR), chloroprene rubber (CR), isoprene rubber (IR), and acrylonitrile butadiene rubber (NBR), and polysaccharides such as carboxymethyl cellulose (CMC), xanthan gum, guar gum, and pectin. In addition, examples of the binder include polyacrylic acid, polymethacrylic acid, sodium polyacrylate, potassium polyacrylate, sodium polymethacrylate, potassium polymethacrylate, ethyl polyacrylate, ethyl polyacrylate, butyl polyacrylate, methyl polymethacrylate, ethyl polymethacrylate, butyl polymethacrylate, and any mixture thereof. The content of the binder is preferably 1% by mass or more and less than 10% by mass with respect to the total solid content of the negative electrode layer. If the content of the binder is too high, the surface of the negative electrode active material is covered with the binder in a large area, which may reduce the ionic conductivity and electronic conductivity. If the content of the binder is too low, the electrical contact between the particles of the negative electrode active material may not be properly performed.
[0019] In addition to the above compounds, the binder component may further include carboxymethylcellulose (referred to as "CMC"), which is a cellulose derivative, or a metal salt of carboxymethylcellulose (e.g., sodium carboxymethylcellulose, potassium carboxymethylcellulose). When CMC or a metal salt of CMC is further added as a binder component, the content of CMC or the CMC metal salt is preferably 0.05% by mass or more and 1.5% by mass or less with respect to the total solid content of the negative electrode layer.
[0020] The negative electrode layer may further contain a conductive assistant. The conductive assistant is a material for reducing the resistance of the electrode. Examples of the conductive assistant include carbon black such as acetylene black and ketjen black, activated carbon, graphite, mesoporous carbon, fullerenes, carbon nanotubes, carbon nanofibers, carbon brushes, and other carbon fibers.
[0021] When carbon nanotubes or carbon nanofibers are used as the conductive assistant, the content of the conductive assistant is 0.01% by mass to 3% by mass, preferably 0.03% by mass to 1% by mass, based on the total solid content of the negative electrode layer.
[0022] In addition to the materials described above, the negative electrode layer may contain, as appropriate, electrode additives that are generally used for forming electrodes, such as thickeners, dispersants, and stabilizers.
[0023] <Solid electrolyte membrane> The negative electrode, the solid electrolyte film, and the positive electrode used in the manufacturing method of the embodiment include a solid electrolyte. The solid electrolyte used here can be exemplified by an oxide-based solid electrolyte and a sulfide-based solid electrolyte. For example, a garnet-type, NASICON-type, or perovskite-type oxide-based material can be used as the oxide-based solid electrolyte. As the sulfide-based solid electrolyte, any known sulfide-based substance can be used, for example, LiPO4-Li2S-SiS, 75% Li2S-25% P2S5 mixture, Li2S-SiS2, Li2S-P2S5, Li3PS4, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiI-Li2S-B2S3, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5Li2S-P2S5-LiCl, Li6PS5Cl, Li 10 GeP2S 12 , Li 3.25 Ge 0.25 P 0.75 S4, etc. In the embodiment, it is preferable to use a sulfide-based solid electrolyte. The solid electrolyte membrane used in the embodiment refers to a thin flat surface having a predetermined area and made of a solid electrolyte. The solid electrolyte membrane may be a single layer (a solid electrolyte membrane made of one type of solid electrolyte) or a multi-layer (a solid electrolyte membrane made of two or more types of solid electrolyte membranes stacked together). In addition, it is also possible to fill the above-mentioned solid electrolyte into a general porous separator such as polyethylene or polypropylene.
[0024] In the present invention, the solid electrolyte membrane is preferably formed to have a thickness of 15 to 150 μm. If the thickness is smaller than this, a short circuit is likely to occur when the solid electrolyte is press-formed under high pressure. On the other hand, if the thickness is larger than this, the cell volume will be excessively increased, and the energy density per unit volume of the all-solid-state battery will not increase.
[0025] <Release sheet> The release sheet refers to a flexible sheet on which a release agent layer that makes it easy to peel off the solid electrolyte membrane is formed on the surface of the sheet member. As the flexible sheet, for example, a general polyester film can be used, and a film mainly containing a component selected from polyethylene terephthalate, polyethylene-2,6-naphthalate, polybutylene terephthalate, polytrimethylene terephthalate, and a mixture thereof can be used, but is not limited to this. As the release agent constituting the release agent layer, a silicone-based, alkyd-based, olefin-based, fluorine-based, or alkyl-based release agent, or a combination of these can be used. Among them, it is preferable to use a release agent containing a silicone resin having a reactive functional group that can be cured by ultraviolet light or heat, and which can easily control the amount of transfer of the release agent by controlling the temperature.
[0026] <Positive electrode> The positive electrode can be a positive electrode used in a non-aqueous secondary battery material, and is not particularly limited. For example, the positive electrode includes a positive electrode current collector and a positive electrode layer containing a positive electrode active material and a solid electrolyte. The positive electrode layer preferably contains a binder. The positive electrode layer containing the positive electrode active material, the solid electrolyte, and the binder can be formed on at least one surface of the positive electrode current collector.
[0027] The positive electrode current collector can be made of stainless steel, aluminum, nickel, titanium, or a positive electrode current collector in which the surface of aluminum or stainless steel is surface-treated with carbon, nickel, titanium, or silver.
[0028] The positive electrode active material preferably contains a lithium nickel-based composite oxide as the positive electrode active material. The lithium nickel-based composite oxide is represented by the general formula Li x Ni y Me (1-y) The positive electrode active material is a transition metal composite oxide containing lithium and nickel, represented by the general formula LiMnO2 (wherein Me is at least one metal selected from the group consisting of Al, Mn, Na, Fe, Co, Cr, Cu, Zn, Ca, K, Mg, and Pb). Examples of the lithium manganese composite oxide that can contain the lithium manganese composite oxide include lithium manganese oxide (LiMnO2) with a zigzag layer structure and lithium manganese oxide (LiMn2O4). The positive electrode active material is particularly a transition metal composite oxide represented by the general formula Li x Ni y Co z Mn (1-y-z)It is preferable that the positive electrode active material contains a lithium nickel manganese cobalt composite oxide having a layered crystal structure represented by O2. Here, in the general formula, x is 1≦x≦1.2, y and z are positive numbers satisfying y+z<1, and the value of y is 0.5 or more. In order to obtain a high-capacity battery, it is particularly preferable to make y>1-yz and y>z. The lithium nickel composite oxide having this general formula is, in other words, a lithium nickel cobalt manganese composite oxide. The lithium nickel cobalt manganese composite oxide is a lithium nickel composite oxide that is preferably used to increase the capacity of a battery. In addition, the positive electrode active material may contain the general formula LiMPO4 (M is at least one selected from the group consisting of Mn, Fe, Co, and Ni). The surface of the positive electrode layer may be coated with a material such as LiNbO3 to form a buffer layer. The buffer layer can be formed of a buffer layer-forming material with a thickness of 10 nm or less to suppress the interface resistance between the positive electrode layer and the solid electrolyte film. The buffer layer can be formed on the surface of the positive electrode layer by a sol-gel method or the like.
[0029] Examples of the binder that forms the positive electrode layer together with the positive electrode active material include fluororesins such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and polyvinyl fluoride (PVF); conductive polymers such as polyanilines, polythiophenes, polyacetylenes, and polypyrroles; synthetic rubbers such as styrene butadiene rubber (SBR), butadiene rubber (BR), chloroprene rubber (CR), isoprene rubber (IR), and acrylonitrile butadiene rubber (NBR); and polysaccharides such as carboxymethyl cellulose (CMC), xanthan gum, guar gum, and pectin.
[0030] The positive electrode layer may also contain a conductive assistant. Examples of the conductive assistant include carbon black such as acetylene black and ketjen black, activated carbon, graphite, mesoporous carbon, fullerenes, carbon nanofibers, carbon nanotubes, carbon nanobrushes, and other carbon fibers. In addition, the positive electrode layer may appropriately contain electrode additives that are generally used for forming electrodes, such as thickeners, dispersants, and stabilizers.
[0031] <Cell Preparation> First, we will explain how to prepare the negative electrode. There are several methods for preparing the negative electrode. Regardless of the method used, it is preferable to prepare the negative electrode in a low moisture environment under dew point control in order to suppress the adsorption of moisture into the solid electrolyte.
[0032] <Preparation of negative electrode> When using a negative electrode in which a negative electrode active material is formed on a negative electrode current collector, a slurry in which a negative electrode active material, a solid electrolyte, and a binder are dispersed in a dehydrated organic solvent is applied to a part or all of the surface of a negative electrode current collector such as a copper foil, and dried to obtain a negative electrode precursor sheet. The obtained negative electrode precursor sheet is compressed by a press molding method such as a roll press, a uniaxial press, a rubber press, or an isostatic press (CIP, WIP) to obtain a negative electrode sheet. Examples of organic solvents include acetonitrile, xylene, dimethoxyethane, dimethyl carbonate, tertiary amine solvents such as triethylamine, heptane, hexane, tetrahydrofuran, toluene, and N-methylpyrrolidone, as well as ether solvents, thiol solvents, and butyl butyrate, and it is preferable that all of them are dehydrated.
[0033] Alternatively, a granulated negative electrode active material containing at least a negative electrode active material, a solid electrolyte, and a binder can be transferred to a negative electrode current collector to obtain a negative electrode precursor sheet. In this case, a surface layer containing a polymer component such as a binder that enhances adhesion to the granulated negative electrode active material may be formed in advance on the surface of the negative electrode current collector. The negative electrode layer may also contain a conductive assistant. The obtained negative electrode precursor sheet is compressed by a press molding method such as a roll press, a uniaxial press, a rubber press, or a cold isostatic press (CIP, WIP) to obtain a negative electrode sheet.
[0034] Alternatively, a metallic lithium layer such as lithium foil is disposed on all or part of a stainless steel negative electrode current collector, and these are then bonded together by rolling or the like to obtain a negative electrode sheet.
[0035] <Preparation of solid electrolyte membrane> Next, a solid electrolyte membrane is formed on the surface of the negative electrode. Regardless of the method used to form the solid electrolyte membrane, it is preferable to form it in a low moisture environment under dew point control in order to prevent moisture from being adsorbed by the solid electrolyte.
[0036] A slurry in which a solid electrolyte is dispersed in an organic solvent is applied to the surface of the negative electrode layer formed on a copper foil or the surface of metallic lithium formed on a stainless steel foil, and then dried to form a solid electrolyte film on the surface of the negative electrode. Examples of the organic solvent include acetonitrile, xylene, dimethoxyethane, dimethyl carbonate, tertiary amine solvents such as triethylamine, heptane, hexane, tetrahydrofuran, toluene, and N-methylpyrrolidone, as well as ether solvents, thiol solvents, and butyl butyrate, and it is preferable that all of them are dehydrated.
[0037] In an embodiment, a slurry in which a solid electrolyte is dispersed in an organic solvent is applied to the surface of a release film in which a release agent layer containing a release agent is formed on a polyester film mainly composed of polyester, and then the solid electrolyte film is formed by drying the polyester film and laminating the polyester film together so that the solid electrolyte film contacts the surface of the negative electrode layer or the surface of metallic lithium, thereby forming a solid electrolyte film on the surface of the negative electrode. For example, since silicone resin, which is preferably used as a release agent, is hygroscopic, it is preferable to dry the silicone resin sufficiently so that moisture is not excessively adsorbed on the solid electrolyte. However, if the release agent is dried too much, the release property decreases, and when peeled from the release film, a part of the solid electrolyte film may remain on the release film side, resulting in a decrease in yield. Although the cause is unclear, it is thought that the moisture content of the release agent layer contained in the release film is related. In an embodiment, the conditions of the release agent layer in which the solid electrolyte film does not remain on the release film were obtained. As long as the moisture content of the release agent layer is within the desired range, the drying method is not particularly important. The release sheet itself may be stored together with a desiccant such as silica gel, and it is also preferable to heat and dehydrate the release sheet under reduced pressure. When the release agent contains a silicone resin, the release sheet is preferably heated at 100 to 150° C. The moisture content can be measured by Karl Fischer titration. The moisture content of the release agent can be determined as the difference between the moisture content of the polyester film sheet on which the release agent is formed and the moisture content of the polyester film sheet alone on which the release agent is not formed.
[0038] The laminated negative electrode and the solid electrolyte membrane formed on the release surface of the release sheet are compressed by a pressing method such as roll press, uniaxial press, rubber press, or isostatic press (CIP, WIP), to obtain a negative electrode-solid electrolyte membrane laminate. After compression, the release film is peeled off from the solid electrolyte membrane.
[0039] <Preparation of positive electrode> Next, the preparation of the positive electrode will be described. Regardless of the method used to prepare the positive electrode, it is preferable to prepare the positive electrode in a low moisture environment under dew point control in order to suppress adsorption of moisture.
[0040] A slurry in which a positive electrode active material, a solid electrolyte, and a binder are dispersed in a dehydrated organic solvent is applied to a part or the whole surface of a positive electrode current collector such as aluminum, and then dried to obtain a positive electrode sheet. Examples of organic solvents include acetonitrile, xylene, dimethoxyethane, dimethyl carbonate, tertiary amine solvents such as triethylamine, heptane, hexane, tetrahydrofuran, toluene, and N-methylpyrrolidone, as well as ether solvents, thiol solvents, and butyl butyrate, and it is preferable that all of them are dehydrated.
[0041] <Formation of Electrode Laminate> The positive electrode sheet is laminated on the negative electrode-solid electrolyte membrane laminate to obtain an electrode laminate precursor. When a sulfide solid electrolyte is used as the solid electrolyte, the ionic conductivity of the solid electrolyte decreases due to exposure to moisture. Therefore, after obtaining the electrode laminate precursor, it is desirable to compress the electrode laminate precursor by a method such as roll press, uniaxial press, rubber press, or isostatic press (CIP, WIP) within a predetermined time to obtain an electrode laminate. The predetermined time is, for example, within 2 days in an environment with a dew point of -40°C and a moisture concentration of 127 ppm or less. If the time passes beyond this, there is a risk of performance deterioration due to water absorption by the solid electrolyte, which is not preferable from the viewpoint of decreasing productivity of all-solid-state batteries.
[0042] <Sealing of electrode laminate> The obtained electrode laminate is desirably sealed in an exterior case immediately. One end of a rectangular metal plate serving as a negative terminal is attached to the negative current collector, and one end of a rectangular metal terminal serving as a positive terminal is attached to the positive current collector, and then the electrode laminate is housed in an aluminum exterior case. Of the inner surfaces of the exterior case, at least the surface facing the electrode laminate is preferably formed with a resin layer such as polyolefin. The resin layer is heated to melt the resin, and then solidified again to seal the electrode laminate in the aluminum exterior case. At this time, the other end of the positive terminal and the other end of the negative terminal are arranged so as to be drawn out of the exterior case. At the portion where the positive terminal and the negative terminal contact the resin layer on the inner surface of the exterior case, a layer of the same or different type of resin as the resin used in the resin layer on the inner surface of the exterior case can be provided to strengthen the adhesion of the exterior case at that portion. EXAMPLES
[0043] A battery was fabricated according to the flow shown in the embodiment of the invention. Figure 1 is a flow diagram summarizing the embodiment of the invention.
[0044] [I] Formation of negative electrode-solid electrolyte membrane laminate (1) A foil (manufactured by Honjo Metals Co., Ltd.) was prepared as a negative electrode, in which a 20 μm thick metallic lithium layer was formed on the surface of a 10 μm thick stainless steel negative electrode current collector. (2) A slurry in which the solid electrolyte Li6PS5Cl (D50: 8 μm) was dispersed in xylene as an organic solvent was applied to the surface of a polyester film (release sheet) having a release agent layer made of silicone resin as a release agent, and then heated and dried in an oven to form a solid electrolyte film on the release sheet. The obtained solid electrolyte film was laminated together with the release sheet so as to be in contact with the surface of the metallic lithium. At this time, the moisture content of the release agent layer of the release sheet was variously changed as shown in Table 1 by changing the drying temperature in the oven. (3) The negative electrode-solid electrolyte membrane laminate of (2) above was laminated and vacuum sealed in a nylon vacuum pack and held at room temperature (25°C) under a pressure of 400 MPa for 1 minute. Thereafter, while still laminated and sealed, the negative electrode-solid electrolyte membrane laminate was compressed by an isostatic pressure pressing method to obtain a negative electrode-solid electrolyte membrane laminate with a porosity of 7% in the negative electrode layer. The size of the negative electrode and solid electrolyte laminate was 50 mm x 70 mm. (4) The polyester film was peeled off from the solid electrolyte membrane to obtain a negative electrode-solid electrolyte membrane laminate.
[0045] [II] Lamination of the positive electrode sheet and the negative electrode-solid electrolyte membrane laminate (1) LiNi as the positive electrode active material 0.8 Co 0.1 Mn 0.1 A slurry of 70 mass% O2 (D50: 8 μm), 25 mass% Li6PS5Cl (average particle size 1 μm) as a solid electrolyte, 2 mass% acetylene black (manufactured by Timcal Japan Co., Ltd.), and 3 mass% styrene-butadiene rubber (SBR) as a binder dispersed in xylene, an organic solvent, was applied to an aluminum foil (manufactured by UACJ Corporation) with a thickness of 10 μm and dried to form a positive electrode layer, thereby obtaining a positive electrode. (2) The positive electrode obtained in (1) above was cut to 45 mm × 65 mm, and laminated so that the positive electrode layer was in contact with the solid electrolyte membrane of the negative electrode-solid electrolyte membrane laminate prepared in [I] to obtain an electrode laminate precursor. The number of layers of the positive electrode and negative electrode-solid electrolyte membrane laminate was one each.
[0046] [III] Pressurizing the electrode stack (1) The electrode laminate precursor obtained in each Example was laminated and vacuum sealed in a nylon vacuum pack and held at room temperature (25° C.) under a pressure of 400 MPa for 1 minute. Next, while still laminated and sealed, the electrode laminate precursor was compressed by an isostatic pressing method to obtain an electrode laminate with a positive electrode layer porosity of 5%.
[0047] [IV] Encapsulation in outer case (1) The electrode laminate obtained in [III] above was enclosed in an outer case by the method described in the embodiment of the invention, and a battery was obtained in which the positive and negative terminals were extended to the outside of the aluminum outer case.
[0048] The drying conditions were changed and 40 batteries were fabricated using the release sheets with the residual moisture contents shown in Table 1. The films peeled off in step [I] (4) were visually observed to confirm whether any solid electrolyte remained on the film within an area of 50 mm x 70 mm. If no solid electrolyte remained on any of the films peeled off during the fabrication of the 40 batteries, the releasability was judged to be "good," and if any of the films was found to have solid electrolyte remaining on it, the releasability was judged to be "poor." When a release sheet having a residual moisture content of 10 ppm in the release agent layer of the release sheet was used (Comparative Example 1), two films were found to have a trace amount of solid electrolyte remaining. When the completed batteries were charged and discharged, insulation was observed in four of the batteries of Comparative Example 1 (yield: 90%). Although the film peeled off during the production of the batteries of Comparative Example 1 was only found in two batteries in which the remaining solid electrolyte was visually confirmed, insulation was observed in all four batteries. It is believed that some damage was caused to the solid electrolyte in two of the batteries of Comparative Example 1 when the film was peeled off during the production of the batteries. Note that no insulation was observed in any of the batteries produced under the conditions of Examples 1 to 3, and the yield was 100%. The obtained battery was charged at a constant current of 0.05C up to 4.25V, then switched to a constant voltage charge, and cut off at 0.005C. The average discharge operating voltage was then obtained when the battery was discharged at a constant current of 0.05C up to 2.5V. Table 1 shows the average discharge operating voltages of other examples and comparative examples when the average discharge operating voltage of Example 1 is taken as 1. It is believed that in the battery with a residual moisture content of 1000ppm in the release agent layer, the moisture content contained in the silicone resin affected the solid electrolyte, and no discharge capacity was obtained. The moisture content was measured by Karl Fischer titration at 150°C. [Table 1]
[0049] In this way, by controlling the residual moisture content in the release agent layer of the release sheet within a specific range, it is possible to suppress deterioration of the solid electrolyte membrane and obtain a high-quality all-solid-state battery.
[0050] The examples in the present invention are merely examples and are not limited thereto. For example, an aluminum laminate film is used for the exterior case, but a strong aluminum can case or a cylindrical case may be used. Li6PS5Cl is used as the solid electrolyte, but the present invention can be applied to any sulfide-based solid electrolyte that has low chemical stability with water. The positive and negative electrodes are adjusted to a predetermined size in advance, but they may be cut into a predetermined shape immediately after stacking. Needless to say, other design changes are possible within the scope of the invention.
Claims
1. A method for producing an all-solid-state battery, comprising a step of laminating a negative electrode, a solid electrolyte membrane, and a positive electrode to form an electrode laminate, The method includes a step of applying a slurry containing a solid electrolyte in a solvent onto a surface of a film on which a release agent layer having a water content of 70 ppm or more and 200 ppm or less has been formed, to form the solid electrolyte membrane. How solid-state batteries are manufactured.
2. The method for producing an all-solid-state battery according to claim 1 , wherein the release agent layer contains a silicone resin.
Citation Information
Patent Citations
Method for manufacturing all-solid battery
JP2017050209A
Composite active material particle, positive electrode, all solid lithium ion battery, and manufacturing method thereof
JP2018125214A
Method for manufacturing binder composition for all-solid-state secondary cell, method for manufacturing slurry composition for all-solid-state secondary cell, method for manufacturing solid-electrolyte-containing layer, and method for manufacturing all-solid-state secondary cell