Positive electrode active material for lithium ion battery, positive electrode for lithium ion battery, lithium ion battery, method for producing precursor of positive electrode active material for lithium ion battery, and method for producing positive electrode active material for lithium ion battery

A controlled crystallization and firing process for a specific composition of Li a Ni (1-b-c-d) Co b Mn c Mg d O 2 active material addresses purity and cost issues, enhancing lithium ion battery performance and reducing production costs by optimizing particle size, density, and surface area.

JP2024143839AActive Publication Date: 2024-10-11JX NIPPON MINING & METALS CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023056746
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

The production of positive electrode active materials for lithium ion batteries is hindered by variations in synthetic raw material purity and refining conditions, leading to inconsistent cycle performance and storage stability, and the high cost of recovering high-purity nickel, cobalt, and lithium due to the difficulty in purifying and removing impurities like magnesium.

Method used

A positive electrode active material with a specific composition formula Li a Ni (1-b-c-d) Co b Mn c Mg d O 2, where 0.98≦a≦1.09, 0.06≦b≦0.21, 0.02≦c≦0.32, and 0.00005≦d≦0.003, is produced through a controlled crystallization reaction using an aqueous solution with pH 10.0 to 11.5 and ammonium ion concentration of 5 to 20 g/L, followed by firing to achieve optimal particle size, density, and surface area for improved battery characteristics.

Benefits of technology

The solution results in a positive electrode active material with enhanced battery characteristics, including stable crystal structure, reduced expansion and contraction of the crystal lattice, improved cycle characteristics, and lower production costs by minimizing the need for extensive impurity removal during recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143839000001
    Figure 2024143839000001
  • Figure 2024143839000002
    Figure 2024143839000002
Patent Text Reader

Abstract

To provide: a positive electrode active material for a lithium ion battery, exhibiting good battery characteristics while including Mg; a positive electrode for a lithium ion battery; a lithium ion battery; a method for producing a precursor of a positive electrode active material for a lithium ion battery; and a method for producing a positive electrode active material for a lithium ion battery.SOLUTION: There is provided a positive electrode active material for a lithium ion battery which is represented by a compositional formula: LiaNi(1-b-c-d)CobMncMgdO2 (in the formula, 0.98≤a≤1.09, 0.06≤b≤0.21, 0.02≤c≤0.32, and 0.00005≤d≤0.003 are satisfied), and has a 50% cumulative volume particle size D50 of 3.0-11.0 μm, a tap density of 2.0-2.6 g / cc, and a c-axis lattice constant of 14.184-14.240 Å.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material for a lithium ion battery, a positive electrode for a lithium ion battery, a lithium ion battery, a method for producing a precursor of a positive electrode active material for a lithium ion battery, and a method for producing a positive electrode active material for a lithium ion battery. [Background technology]

[0002] In recent years, with the rapid spread of small electronic devices such as mobile phones and laptops, the demand for non-aqueous electrolyte secondary batteries as rechargeable power sources has been growing rapidly. As the positive electrode active material for non-aqueous electrolyte secondary batteries, lithium cobalt composite oxides such as lithium cobalt oxide (LiCoO2) are widely used, as well as lithium nickel composite oxides such as lithium nickel oxide (LiNiO2) and lithium manganese composite oxides such as lithium manganese oxide (LiMnO2).

[0003] However, nickel and cobalt are relatively expensive metals, and cobalt in particular is known to be a metal with unstable supply and demand, as is produced in a limited number of countries. Therefore, in recent years, as disclosed in Patent Document 1, attempts have been made to recover high-purity metallic components such as lithium, nickel, and cobalt from discarded electrodes and discarded batteries and recycle them into positive electrode active materials. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Special Publication No. 2022-532575 [Patent Document 2] Japanese Patent Application Publication No. 11-354118 Summary of the Invention [Problem to be solved by the invention]

[0005] Although the demand for positive electrode active materials for lithium ion secondary batteries is increasing, there is a problem that excellent positive electrode active materials have fluctuations in cycle performance and storage stability depending on the purity of the synthesis raw materials and the refining conditions. For this reason, as disclosed in Patent Document 2, it is necessary to control the purity of the positive electrode active material.

[0006] Discarded electrodes and batteries contain various metals in the cans and in the flame retardant materials used to prevent fires, and it takes a huge amount of refining cost to recover high-purity nickel, cobalt, and lithium, which results in high production costs for the positive electrode active material. In particular, Mg is difficult to purify and extract, and a considerable recycling cost is required to completely remove it.

[0007] Thus, from the perspective of controlling the purity of the positive electrode active material and improving battery characteristics, it is desirable to eliminate impurities such as Mg. However, at the same time, when recovering high-purity nickel, cobalt, and lithium for recycling discarded electrodes and waste batteries, the cost of removing Mg is an issue.

[0008] The present invention has been made to solve the above-mentioned problems, and has an object to provide a positive electrode active material for a lithium ion battery that contains Mg and exhibits good battery characteristics, a positive electrode for a lithium ion battery, a lithium ion battery, a method for producing a precursor of the positive electrode active material for a lithium ion battery, and a method for producing the positive electrode active material for a lithium ion battery. [Means for solving the problem]

[0009] The present invention, which was completed based on the above findings, is defined as follows. 1.Composition formula: Li a Ni (1-b-c-d) Co b Mn c Mg d O2 (In the above formula, 0.98≦a≦1.09, 0.06≦b≦0.21, 0.02≦c≦0.32, and 0.00005≦d≦0.003.) The positive electrode active material for a lithium ion battery is represented by the formula: 2. BET specific surface area is 0.20~0.80m 2 2. The positive electrode active material for a lithium ion battery according to claim 1, wherein the molecular weight of the positive electrode active material is 1. / g. 3. A positive electrode for a lithium ion battery, comprising the positive electrode active material for a lithium ion battery according to 1 or 2 above. 4. A lithium ion battery comprising the positive electrode and the negative electrode for a lithium ion battery described in 3 above. 5. A method for producing a crystallization reaction comprising the steps of: (a) using an aqueous solution containing a nickel salt, (b) a cobalt salt, (c) a manganese salt, and (d) a magnesium salt; and (e) using an aqueous solution containing a basic solution containing ammonia and / or an aqueous solution of an alkali metal as a reaction solution, while controlling the pH of the reaction solution to 10.0 to 11.5, the ammonium ion concentration to 5 to 20 g / L, and the solution temperature to 59 to 61° C.; Composition formula: Ni (1-b-c-d) Co b Mn c Mg d (OH)2 (In the above formula, 0.06≦b≦0.21, 0.02≦c≦0.32, and 0.00005≦d≦0.003.) The 50% cumulative volumetric grain size D50 is 3.0 to 11.0 μm, the tap density is 1.8 to 2.3 g / cc, and the BET specific surface area is 4.0 to 12.0 m. 2 / g of a precursor of a positive electrode active material for a lithium ion battery. 6. The precursor produced by the method for producing a precursor of a positive electrode active material for a lithium ion battery described in 5 above and a lithium source are mixed together to produce a lithium-ion battery positive electrode active material having a total number of atoms of metals consisting of Ni, Co, Mn and Mg (Me n ) and the number of lithium atoms (Li n ) and the ratio (Li n / Me n ) is 0.98 to 1.09 to form a lithium mixture; calcining the lithium mixture in air or an oxygen atmosphere at 450 to 750° C. for 2 to 15 hours, and then calcining the lithium mixture at 700 to 900° C. for 2 to 15 hours; The method for producing a positive electrode active material for a lithium ion battery includes the steps of: Effect of the Invention

[0010] According to the present invention, it is possible to provide a positive electrode active material for a lithium ion battery that contains Mg and exhibits good battery characteristics, a positive electrode for a lithium ion battery, a lithium ion battery, a method for producing a precursor of the positive electrode active material for a lithium ion battery, and a method for producing the positive electrode active material for a lithium ion battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Next, the embodiments for carrying out the present invention will be described in detail. It should be understood that the present invention is not limited to the following embodiments, and that appropriate changes and improvements in the design may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.

[0012] (Positive electrode active material for lithium-ion batteries) The positive electrode active material for a lithium ion battery according to an embodiment of the present invention has the composition formula: Li a Ni (1-b-c-d) Co b Mn c Mg d O2 (wherein, 0.98≦a≦1.09, 0.06≦b≦0.21, 0.02≦c≦0.32, 0.00005≦d≦0.003). In the composition formula of the positive electrode active material, a, which indicates the lithium composition, is controlled to 0.98≦a≦1.09. Since a, which indicates the lithium composition, is 0.98 or more, it is possible to suppress the reduction of nickel due to lithium deficiency. In addition, since a, which indicates the lithium composition, is 1.09 or less, it is possible to suppress residual alkaline components such as lithium carbonate and lithium hydroxide present on the surface of the positive electrode active material particles, which may become resistance components when used in a battery.

[0013] In the positive electrode active material for lithium ion batteries according to the embodiment of the present invention, the nickel composition in the composition formula is controlled to 1-bcd (0.467≦1-bcd≦0.91995), and since the nickel composition is 0.467 or more, a good battery capacity of the lithium ion battery can be obtained. In addition, since the nickel composition is 0.91995 or less, the crystal structure is stable, and the expansion and contraction behavior of the crystal lattice due to the insertion and extraction of lithium during charging and discharging is reduced, thereby improving the cycle characteristics.

[0014] In the positive electrode active material for lithium ion batteries according to the embodiment of the present invention, the sum of b indicating the cobalt composition, c indicating the manganese composition, and d indicating the magnesium composition in the composition formula is 0.08005≦b+c+d≦0.533, and therefore the cycle characteristics are improved and the expansion and contraction behavior of the crystal lattice due to the insertion and extraction of lithium during charging and discharging can be reduced. If the sum of the cobalt composition, manganese composition, and magnesium composition exceeds 0.533, the amounts of cobalt, manganese, and magnesium added may be too large, resulting in a large decrease in initial discharge capacity, or may be disadvantageous in terms of cost.

[0015] In the lithium ion battery positive electrode active material according to the embodiment of the present invention, d, which indicates the magnesium composition, is controlled to 0.00005≦d≦0.003. Since d, which indicates the magnesium composition, is 0.00005 or more, the cycle characteristics are improved, and the expansion and contraction behavior of the crystal lattice due to the insertion and elimination of lithium accompanying charge and discharge can be reduced. If d, which indicates the magnesium composition, exceeds 0.003, the amount of magnesium added is too large, and the initial discharge capacity decreases significantly. Thus, the lithium ion battery positive electrode active material according to the embodiment of the present invention contains Mg, but the battery characteristics of the lithium ion battery using it are good. Therefore, when recovering high-purity nickel, cobalt, and lithium as a recycling of waste electrodes and waste batteries, a lithium ion battery having good battery characteristics can be produced using the lithium ion battery positive electrode active material while suppressing the cost for removing Mg.

[0016] The positive electrode active material for lithium ion batteries according to the embodiment of the present invention may have a form of secondary particles in which a plurality of primary particles are aggregated, and may partially contain primary particles that are not aggregated as secondary particles. The shapes of the primary particles constituting the secondary particles and the primary particles existing alone are not particularly limited, and may be various shapes such as, for example, substantially spherical, substantially elliptical, substantially plate-like, and substantially needle-like. The form in which the plurality of primary particles are aggregated is also not particularly limited, and may be various forms such as, for example, a form in which the particles are aggregated in a random direction, or a form in which the particles are aggregated almost uniformly radially from the center to form substantially spherical or substantially elliptical secondary particles.

[0017] The positive electrode active material for lithium ion batteries according to the embodiment of the present invention has a 50% cumulative volume particle size D50 of 3.0 to 11.0 μm. Here, the 50% cumulative volume particle size D50 is the volume particle size at 50% accumulation in a volume-based cumulative particle size distribution curve. If the 50% cumulative volume particle size D50 of the positive electrode active material for lithium ion batteries is 3.0 μm or less, the tap density decreases, and the energy density per volume decreases. If the 50% cumulative volume particle size D50 of the positive electrode active material for lithium ion batteries is 11.0 μm or more, the number of coarse particles increases, and the coating property deteriorates when the slurried positive electrode active material is coated on the current collector. The 50% cumulative volume particle size D50 of the positive electrode active material for lithium ion batteries is more preferably 4.0 to 11.0 μm, and even more preferably 7.0 to 10.0 μm. The method for measuring the 50% cumulative volumetric particle size D50 is as follows: First, 100 mg of a sample (powder) of the positive electrode active material is dispersed by irradiating 40 W ultrasonic waves for 60 seconds at 50% flow rate using a Microtrac laser diffraction particle size distribution measuring device "MT3300EXII", and then the particle size distribution is measured to obtain a volume-based cumulative particle size distribution curve. Next, in the obtained cumulative particle size distribution curve, the volumetric particle size at 50% accumulation can be taken as the 50% cumulative volumetric particle size D50 of the powder of the positive electrode active material. In addition, the water-soluble solvent during the measurement is passed through a 0.02 μm filter, the solvent refractive index is 1.333, the particle permeability conditions are permeable, the particle refractive index is 1.81, the shape is non-spherical, the measurement range is 0.021 to 2000 μm, and the measurement time is 30 seconds.

[0018] The positive electrode active material for lithium ion batteries according to the embodiment of the present invention has a tap density of 2.0 to 2.6 g / cc. When the tap density of the positive electrode active material is 2.0 g / cc or more, a battery with a high energy density per volume can be formed. The tap density of the positive electrode active material is preferably 2.1 to 2.6 g / cc, more preferably 2.3 to 2.6 g / cc. The tap density of the positive electrode active material is measured, for example, by putting 5 g of the positive electrode active material (powder) into a 10 cc graduated cylinder, placing it in a powder density measuring instrument "KYT-4000K" manufactured by Seishin Enterprise Co., Ltd., tapping with a stroke length of 55 mm 1500 times, and then reading the graduations on the graduated cylinder. Next, "sample amount (5 g) / graduated cylinder graduation reading (cc)" is calculated, and this is taken as the tap density (g / cc).

[0019] The positive electrode active material for lithium ion batteries according to the embodiment of the present invention has a c-axis lattice constant controlled to 14.184 to 14.240 Å. When the c-axis lattice constant of the positive electrode active material is 14.184 Å or more, the crystal structure of the positive electrode active material for lithium ion batteries can be stabilized and Li insertion and desorption can be ensured. When the c-axis lattice constant of the positive electrode active material exceeds 14.240 Å, the crystal lattice is distorted, and the charge and discharge capacity of the lithium ion battery may be deteriorated due to the influence of the deterioration of the load characteristics caused by the decrease in the mobility of Li. The c-axis lattice constant of the positive electrode active material is preferably 14.185 to 14.238 Å, and more preferably 14.190 to 14.235 Å. The c-axis lattice constant of the positive electrode active material can be measured, for example, using the following XRD diffractometer under the following conditions. XRD Diffraction Equipment: SmartLab (Rigaku Corporation) ·Radiation source: CuKα (λ=1.5406Å) Apply the sample (positive electrode active material) to a glass sample holder (2 cm x 1.5 cm, depth 0.3 mm). Detector: D / tex Measurement range: 2θ=10°~80° Scan axis: 2θ / θ, Scan speed: 1 degree min -1 Step width: 0.01 degree Slit width: IS(DS)1 / 4°, RS1 10mm, RS2 10mm The c-axis lattice constant can be calculated from the peaks derived from a total of nine crystal planes, namely (003), (101), (012), (104), (015), (107), (018), (110), and (113), in the XRD diffraction pattern measured under the above conditions, using the analytical software "PDXL" (Rigaku Corporation).

[0020] The positive electrode active material for a lithium ion battery according to the embodiment of the present invention has a BET specific surface area of ​​0.20 to 0.80 m 2 / g. The BET specific surface area is preferably 0.20 m 2 / g or more, the contact area of ​​the positive electrode active material is large and the Li ion conductivity is good. This makes it possible to manufacture a high-capacity lithium ion battery. In addition, 2 / g or less, the precipitation reaction of lithium ions from the residual alkali in the positive electrode active material is promoted during repeated charge and discharge. The precipitated lithium compounds become the internal resistance of the battery, reducing the charge and discharge capacity. The BET specific surface area is 0.3 to 0.70 m 2 / g is more preferable. The BET specific surface area can be measured by the following method. That is, first, 1.0 g of the positive electrode active material (powder) is weighed into a glass cell, set in a degassing device, and filled with nitrogen gas in the glass cell, and then heat-treated in a nitrogen gas atmosphere at 40°C for 20 minutes to degas it. Then, the glass cell containing the degassed sample (powder) is set in a specific surface area measuring device "Monosorb Model MS-21" manufactured by Quantachrome, and the specific surface area X is measured by the BET method (one-point method) while flowing a mixed gas of He: 70 at %-N2: 30 at % as the adsorption gas.

[0021] (Method for producing precursor of positive electrode active material for lithium ion batteries) Next, a method for producing a precursor of a positive electrode active material for a lithium ion battery according to an embodiment of the present invention will be described in detail. The precursor of the positive electrode active material for a lithium ion battery according to the embodiment of the present invention has the composition formula: Ni (1-b-c-d) Cob Mn c Mg d (OH)2 (In the above formula, 0.06≦b≦0.21, 0.02≦c≦0.32, and 0.00005≦d≦0.003.) The 50% cumulative volumetric grain size D50 is 3.0 to 11.0 μm, the tap density is 1.8 to 2.3 g / cc, and the BET specific surface area is 4.0 to 12.0 m. 2 / g of a precursor of a positive electrode active material for a lithium ion battery. In the method for producing a precursor of a positive electrode active material for a lithium ion battery according to the embodiment of the present invention, first, an aqueous solution containing (a) a nickel salt, (b) a cobalt salt, (c) a manganese salt, and (d) a magnesium salt, and (e) a basic aqueous solution containing ammonia and / or an aqueous solution containing an alkali metal are prepared. (a) The nickel salt may be nickel sulfate, nickel nitrate, or nickel hydrochloride. (b) The cobalt salt may be cobalt sulfate, cobalt nitrate, or cobalt hydrochloride. (c) The manganese salt may be manganese sulfate, manganese nitrate, or manganese hydrochloride. (d) The magnesium salt may be magnesium sulfate, magnesium nitrate, or magnesium hydrochloride. The magnesium salt may be added as a raw material or may be mixed in as an impurity. (e) The basic aqueous solution containing ammonia may be an aqueous solution of ammonia, ammonium sulfate, ammonium carbonate, ammonium hydrochloride, or the like. The basic aqueous solution of an alkali metal may be an aqueous solution of sodium hydroxide, potassium hydroxide, carbonate, or the like. Examples of the aqueous carbonate solution include aqueous solutions using salts of carbonate groups, such as an aqueous sodium carbonate solution, an aqueous potassium carbonate solution, an aqueous sodium hydrogen carbonate solution, and an aqueous potassium hydrogen carbonate solution.

[0022] The composition of the aqueous solution can be appropriately adjusted depending on the composition of the precursor to be produced, but is preferably (a) an aqueous solution containing 30 to 150 g / L of nickel ions, (b) an aqueous solution containing 3 to 25 g / L of cobalt ions, (c) an aqueous solution containing 1 to 32 g / L of manganese ions, (d) an aqueous solution containing 0.001 to 0.1 g / L of magnesium ions, or (e) a basic aqueous solution containing 7 to 28 mass% ammonia and / or a basic aqueous solution with an alkali metal concentration of 10 to 30 mass%.

[0023] Next, the above-mentioned aqueous solution containing (a) nickel salt, (b) cobalt salt, (c) manganese salt, and (d) magnesium salt, and the aqueous solution containing (e) ammonia-containing basic aqueous solution and / or alkali metal basic aqueous solution are used as reaction solutions, and a crystallization reaction is carried out while controlling the pH of the reaction solution to 10.0 to 11.5, the ammonium ion concentration to 5 to 20 g / L, and the liquid temperature to 59 to 61° C. At this time, the chemical solutions may be sent to the reaction tank from three tanks, namely, a tank containing a mixed aqueous solution of nickel salt, cobalt salt, manganese salt, and magnesium salt, a tank containing ammonia-containing basic aqueous solution, and a tank containing an alkali metal basic aqueous solution. By carrying out the crystallization reaction while controlling the pH of the reaction solution during the coprecipitation reaction to 10.0 to 11.5, the ammonium ion concentration to 5 to 20 g / L, and the solution temperature to 59 to 61° C., the metal solubility in the reaction solution can be controlled, particles in which magnesium is uniformly dispersed can be produced, and a precursor of the positive electrode active material according to the embodiment of the present invention having good discharge characteristics can be produced. In addition, by optimizing the reaction conditions of the metal hydroxide precursor as described above, the adhesion of impurities to the surface of the positive electrode active material obtained after baking is well suppressed, making cleaning unnecessary. Furthermore, a chelating agent or metal oxide coat during the coprecipitation reaction is not required. As a result, the production efficiency is improved.

[0024] (Method of manufacturing positive electrode active material for lithium ion batteries) Next, a method for producing a positive electrode active material for a lithium ion battery according to an embodiment of the present invention will be described in detail. In the method for producing a positive electrode active material for a lithium ion battery according to an embodiment of the present invention, first, a lithium source is added to the precursor of the positive electrode active material for a lithium ion battery according to the embodiment of the present invention produced as described above, and the total number of atoms of metals consisting of Ni, Co, Mn, and Mg (Me n ) and the number of lithium atoms (Li n ) and the ratio (Li n / Me n ) is 0.98 to 1.09 to form a lithium mixture. Examples of the lithium source include lithium carbonate and lithium hydroxide. As a mixing method, it is preferable to adjust the mixing ratio of each raw material and dry mix it with a Henschel mixer, an automatic mortar, a V-type mixer, or the like.

[0025] Next, the lithium mixture is calcined in an air atmosphere, preferably an oxygen atmosphere, at 450 to 750° C. for 2 to 15 hours in the air or oxygen atmosphere, and then further calcined for 2 to 15 hours at 700 to 900° C. Thereafter, if necessary, the calcined body can be crushed using, for example, a pulverizer to obtain a powder of the positive electrode active material.

[0026] (Lithium-ion battery positive electrodes and lithium-ion batteries) The positive electrode for lithium ion batteries according to the embodiment of the present invention has a structure in which a positive electrode mixture prepared by mixing the positive electrode active material for lithium ion batteries having the above-mentioned configuration, a conductive auxiliary material, and a binder is provided on one or both sides of a current collector. The lithium ion battery according to the embodiment of the present invention includes a positive electrode for lithium ion batteries having such a configuration and a known negative electrode for lithium ion batteries.

[0027] Examples of the conductive assistant include metal-based conductive assistants (aluminum, stainless steel (SUS), silver, gold, copper, titanium, etc.), carbon-based conductive assistants (graphite and carbon black (acetylene black, ketjen black, furnace black, channel black, thermal lamp black), etc.), and mixtures thereof. These conductive assistants may be used alone or in combination of two or more. They may also be used as alloys or metal oxides. Among them, from the viewpoint of electrical stability, aluminum, stainless steel, silver, gold, copper, titanium, carbon-based conductive assistants, and mixtures thereof are more preferable, silver, gold, aluminum, stainless steel, and carbon-based conductive assistants are even more preferable, and carbon-based conductive assistants are particularly preferable. In addition, these conductive assistants may be particulate ceramic materials or resin materials coated with a conductive material (preferably, one of the above-mentioned conductive assistants, which is a metal) by plating or the like. The shape (form) of the conductive assistant is not limited to a particulate form, and may be a form other than a particulate form, and may be a form that is practically used as a so-called filler-based conductive assistant, such as carbon nanofibers and carbon nanotubes.

[0028] Examples of the binder include substances commonly used in positive electrode mixtures for lithium ion batteries, but it is preferable to use copolymers having a structure derived from vinylidene fluoride (PVDF), copolymers or homopolymers having a structure derived from tetrafluoroethylene (TEF), and copolymers or homopolymers having a structure derived from hexafluoropropylene (HFP).Specific examples include PVDF-HFP, PVDF-HFP-TEF, PVDF-TEF, and TEF-HFP.

[0029] The positive electrode mixture is prepared by mixing a positive electrode active material for lithium ion batteries, a conductive additive, and a binder in a solvent to form a positive electrode mixture slurry, which is then applied to one or both sides of a current collector and then dried or otherwise provided on the current collector to form a positive electrode active material layer.

[0030] As the solvent for the positive electrode mixture slurry, known organic solvents, such as hydrocarbon organic solvents, amide compounds, lactam compounds, urea compounds, organic sulfur compounds, cyclic organic phosphorus compounds, etc., can be used as a single solvent or as a mixed solvent. As the hydrocarbon organic solvent, saturated hydrocarbons, unsaturated hydrocarbons, or aromatic hydrocarbons can be used. As the saturated hydrocarbons, hexane, pentane, 2-ethylhexane, heptane, decane, cyclohexane, etc. can be used. As the unsaturated hydrocarbons, hexene, heptene, cyclohexene, etc. can be used. As the aromatic hydrocarbons, toluene, xylene, decalin, 1,2,3,4-tetrahydronaphthalene, etc. can be used. Of these, toluene and xylene are particularly preferred.

[0031] Materials constituting the current collector include metal materials such as copper, aluminum, titanium, stainless steel, nickel and alloys thereof, as well as baked carbon, conductive polymer materials, conductive glass, and the like. Among them, aluminum is more preferable from the viewpoints of weight reduction, corrosion resistance, and high conductivity. The current collector is preferably a resin current collector made of a conductive polymer material. The shape of the current collector is not particularly limited, and may be a sheet-shaped current collector made of the above material, or a deposition layer made of fine particles made of the above material. The thickness of the current collector is not particularly limited, but is preferably 1 to 30 μm. Examples of the conductive polymer material constituting the resin current collector include conductive polymers and resins to which a conductive agent is added as necessary.

[0032] From the viewpoint of battery performance, the thickness of the positive electrode for a lithium ion battery is preferably 10 to 100 μm, and more preferably 20 to 50 μm.

[0033] A lithium-ion battery using a lithium-ion battery positive electrode can be obtained by combining a negative electrode as a counter electrode, storing it together with a separator in a cell container, injecting an electrolyte, and sealing the cell container. It can also be obtained by forming a positive electrode on one side of a current collector and a negative electrode on the other side to create a bipolar electrode, stacking the bipolar electrode with a separator, storing it in a cell container, injecting an electrolyte, and sealing the cell container.

[0034] The negative electrode may include a negative electrode active material, a conductive auxiliary material, a current collector, etc. As the negative electrode active material, a known negative electrode active material for lithium ion batteries may be used, and may include carbon-based materials (graphite, non-graphitizable carbon, amorphous carbon, resin baked bodies (e.g., phenolic resins, furan resins, etc. baked and carbonized), cokes (e.g., pitch coke, needle coke, petroleum coke, etc.), carbon fibers, etc.), silicon-based materials (silicon, silicon oxide (SiO x ), silicon-carbon composites (carbon particles whose surfaces are coated with silicon and / or silicon carbide, silicon particles or silicon oxide particles whose surfaces are coated with carbon and / or silicon carbide, silicon carbide, etc.) and silicon alloys (silicon-aluminum alloys, silicon-lithium alloys, silicon-nickel alloys, silicon-iron alloys, silicon-titanium alloys, silicon-manganese alloys, silicon-copper alloys, silicon-tin alloys, etc.), conductive polymers (e.g., polyacetylene and polypyrrole), metals (tin, aluminum, zirconium, titanium, etc.), metal oxides (titanium oxide, lithium-titanium oxide, etc.), metal alloys (e.g., lithium-tin alloys, lithium-aluminum alloys, lithium-aluminum-manganese alloys, etc.), and mixtures of these with carbon-based materials. In addition, the conductive assistant may be suitably the same conductive assistant as that of the positive electrode described above.

[0035] The collector may be the same as the collector constituting the positive electrode described above, and is preferably copper from the viewpoints of weight reduction, corrosion resistance, and high conductivity. It may also be a resin collector, and the same one as the collector constituting the positive electrode described above can be suitably used. The thickness of the collector is not particularly limited, but is preferably 10 to 60 μm.

[0036] Examples of the separator include known separators for lithium ion batteries, such as porous films made of polyethylene or polypropylene, laminated films of porous polyethylene film and porous polypropylene, nonwoven fabrics made of synthetic fibers (polyester fibers, aramid fibers, etc.) or glass fibers, and those having ceramic particles such as silica, alumina, or titania attached to their surfaces. EXAMPLES

[0037] The following examples are provided to provide a better understanding of the present invention and its advantages, but the present invention is not limited to these examples.

[0038] Example 1 First, nickel sulfate, cobalt sulfate, and manganese sulfate were weighed in predetermined amounts so that the ratio of Ni:Co:Mn was 50:20:30, and a 1.5 mol / L mixed metal salt solution was prepared. The Mg concentration in this mixed metal salt solution was 0.007 g / L. Next, the mixed metal salt solution, ammonia water, and 20% by mass aqueous sodium hydroxide solution were fed to a reaction vessel equipped with an agitator so that the pH in the reaction vessel was 10.6 and the ammonium ion concentration was 10.3 g / L, and a crystallization reaction was carried out to precipitate a nickel-cobalt-manganese composite hydroxide compound. At this time, the rotation speed of the agitator in the reaction vessel was set to 1000 rpm, and the liquid temperature in the reaction vessel was kept at 60°C by a water jacket. In addition, nitrogen gas was introduced into the reaction tank to prevent oxidation of the coprecipitate produced by the crystallization reaction. The gas introduced into the reaction tank is not limited to nitrogen gas, and any gas that does not promote oxidation, such as helium, neon, argon, or carbon dioxide, can be used. Next, the obtained precipitate was filtered by suction, washed with water, and dried for 12 hours at 120° C. using a tray dryer, thereby producing a precursor of the positive electrode active material. Next, the lithium carbonate and the precursor of the positive electrode active material were mixed so that the ratio (Li / Me) of the number of lithium (Li) atoms to the sum of the number of metal atoms of Ni, Co, and Mn in the precursor of the positive electrode active material was 1.06, and the mixture was mixed in an automatic mortar for 30 minutes to obtain a mixed powder. Next, the mixed powder was filled into an alumina sagger and fired in a muffle furnace in an air atmosphere at 750°C for 2 hours, and then heated to 900°C and held at that temperature for 8 hours to obtain a positive electrode active material.

[0039] Example 2 First, nickel sulfate, cobalt sulfate, and manganese sulfate were weighed in predetermined amounts so that the ratio of Ni:Co:Mn was 50:20:30, and a 1.5 mol / L mixed metal salt solution was prepared. The Mg concentration in this mixed metal salt solution was 0.008 g / L. Next, the mixed metal salt solution, ammonia water, and 20% by mass aqueous sodium hydroxide solution were fed to a reactor equipped with an agitator so that the pH in the reactor was 10.4 and the ammonium ion concentration was 11.5 g / L, and a crystallization reaction was carried out to precipitate a nickel-cobalt-manganese composite hydroxide compound. At this time, the rotation speed of the agitator in the reactor was set to 1000 rpm, and the liquid temperature in the reactor was kept at 60°C by a water jacket. In addition, nitrogen gas was introduced into the reaction tank to prevent oxidation of the coprecipitate produced by the crystallization reaction. The gas introduced into the reaction tank is not limited to nitrogen gas, and any gas that does not promote oxidation, such as helium, neon, argon, or carbon dioxide, can be used. Next, the obtained precipitate was filtered by suction, washed with water, and dried for 12 hours at 120° C. using a tray dryer, thereby producing a precursor of the positive electrode active material. Next, the lithium carbonate and the precursor of the positive electrode active material were mixed so that the ratio (Li / Me) of the number of lithium (Li) atoms to the sum of the number of metal atoms of Ni, Co, and Mn in the precursor of the positive electrode active material was 1.09, and the mixture was mixed in an automatic mortar for 30 minutes to obtain a mixed powder. Next, the mixed powder was filled into an alumina sagger, and fired in a muffle furnace in an air atmosphere at 750°C for 2 hours, and then heated to 900°C and held at that temperature for 8 hours to obtain a positive electrode active material.

[0040] Example 3 First, nickel sulfate, cobalt sulfate, and manganese sulfate were weighed in predetermined amounts so that the ratio of Ni:Co:Mn was 50:20:30, and a 1.5 mol / L mixed metal salt solution was prepared. The Mg concentration in this mixed metal salt solution was 0.006 g / L. Next, the mixed metal salt solution, ammonia water, and 20% by mass aqueous sodium hydroxide solution were fed to a reaction vessel equipped with an agitator so that the pH in the reaction vessel was 10.3 and the ammonium ion concentration was 8.2 g / L, and a crystallization reaction was carried out to precipitate a nickel-cobalt-manganese composite hydroxide compound. At this time, the rotation speed of the agitator in the reaction vessel was set to 1000 rpm, and the liquid temperature in the reaction vessel was kept at 60°C by a water jacket. In addition, nitrogen gas was introduced into the reaction tank to prevent oxidation of the coprecipitate produced by the crystallization reaction. The gas introduced into the reaction tank is not limited to nitrogen gas, and any gas that does not promote oxidation, such as helium, neon, argon, or carbon dioxide, can be used. Next, the obtained precipitate was filtered by suction, washed with water, and dried for 12 hours at 120° C. using a tray dryer, thereby producing a precursor of the positive electrode active material. Next, the lithium carbonate and the precursor of the positive electrode active material were mixed so that the ratio (Li / Me) of the number of lithium (Li) atoms to the sum of the number of metal atoms of Ni, Co, and Mn in the precursor of the positive electrode active material was 1.06, and the mixture was mixed in an automatic mortar for 30 minutes to obtain a mixed powder. Next, the mixed powder was filled into an alumina sagger, and fired in a muffle furnace in an air atmosphere at 750°C for 2 hours, and then heated to 880°C and held at that temperature for 8 hours to obtain a positive electrode active material.

[0041] Example 4 First, nickel sulfate, cobalt sulfate, and manganese sulfate were weighed in predetermined amounts so that the ratio of Ni:Co:Mn was 50:20:30, and a 1.5 mol / L mixed metal salt solution was prepared. The Mg concentration in this mixed metal salt solution was 0.007 g / L. Next, the mixed metal salt solution, ammonia water, and 20% by mass aqueous sodium hydroxide solution were fed to a reactor equipped with an agitator so that the pH in the reactor was 10.1 and the ammonium ion concentration was 11.2 g / L, and a crystallization reaction was carried out to precipitate a nickel-cobalt-manganese composite hydroxide compound. At this time, the rotation speed of the agitator in the reactor was set to 1000 rpm, and the liquid temperature in the reactor was kept at 60°C by a water jacket. In addition, nitrogen gas was introduced into the reaction tank to prevent oxidation of the coprecipitate produced by the crystallization reaction. The gas introduced into the reaction tank is not limited to nitrogen gas, and any gas that does not promote oxidation, such as helium, neon, argon, or carbon dioxide, can be used. Next, the obtained precipitate was filtered by suction, washed with water, and dried for 12 hours at 120° C. using a tray dryer, thereby producing a precursor of the positive electrode active material. Next, the lithium carbonate and the precursor of the positive electrode active material were mixed so that the ratio (Li / Me) of the number of lithium (Li) atoms to the sum of the number of metal atoms of Ni, Co, and Mn in the precursor of the positive electrode active material was 1.06, and the mixture was mixed in an automatic mortar for 30 minutes to obtain a mixed powder. Next, the mixed powder was filled into an alumina sagger and fired in a muffle furnace in an air atmosphere at 750°C for 2 hours, and then heated to 900°C and held at that temperature for 8 hours to obtain a positive electrode active material.

[0042] Example 5 First, nickel sulfate, cobalt sulfate, and manganese sulfate were weighed in predetermined amounts so that the ratio of Ni:Co:Mn was 50:20:30, and a 1.5 mol / L mixed metal salt solution was prepared. The Mg concentration in this mixed metal salt solution was 0.007 g / L. Next, the mixed metal salt solution, ammonia water, and 20% by mass aqueous sodium hydroxide solution were fed to a reactor equipped with an agitator so that the pH in the reactor was 10.2 and the ammonium ion concentration was 11.3 g / L, and a crystallization reaction was carried out to precipitate a nickel-cobalt-manganese composite hydroxide compound. At this time, the rotation speed of the agitator in the reactor was set to 1000 rpm, and the liquid temperature in the reactor was kept at 60°C by a water jacket. In addition, nitrogen gas was introduced into the reaction tank to prevent oxidation of the coprecipitate produced by the crystallization reaction. The gas introduced into the reaction tank is not limited to nitrogen gas, and any gas that does not promote oxidation, such as helium, neon, argon, or carbon dioxide, can be used. Next, the obtained precipitate was filtered by suction, washed with water, and dried for 12 hours at 120° C. using a tray dryer, thereby producing a precursor of the positive electrode active material. Next, the lithium carbonate and the precursor of the positive electrode active material were mixed so that the ratio (Li / Me) of the number of lithium (Li) atoms to the sum of the number of metal atoms of Ni, Co, and Mn in the precursor of the positive electrode active material was 1.06, and the mixture was mixed in an automatic mortar for 30 minutes to obtain a mixed powder. Next, the mixed powder was filled into an alumina sagger, and fired in a muffle furnace in an air atmosphere at 750°C for 2 hours, and then heated to 800°C and held at that temperature for 8 hours to obtain a positive electrode active material.

[0043] Example 6 First, nickel sulfate, cobalt sulfate, and manganese sulfate were weighed in predetermined amounts so that the ratio of Ni:Co:Mn was 50:20:30, and a 1.5 mol / L mixed metal salt solution was prepared. The Mg concentration in this mixed metal salt solution was 0.048 g / L. Next, the mixed metal salt solution, ammonia water, and 20% by mass aqueous sodium hydroxide solution were fed to a reaction vessel equipped with an agitator so that the pH in the reaction vessel was 10.1 and the ammonium ion concentration was 9.3 g / L, and a crystallization reaction was carried out to precipitate a nickel-cobalt-manganese composite hydroxide compound. At this time, the rotation speed of the agitator in the reaction vessel was set to 1000 rpm, and the liquid temperature in the reaction vessel was kept at 60°C by a water jacket. In addition, nitrogen gas was introduced into the reaction tank to prevent oxidation of the coprecipitate produced by the crystallization reaction. The gas introduced into the reaction tank is not limited to nitrogen gas, and any gas that does not promote oxidation, such as helium, neon, argon, or carbon dioxide, can be used. Next, the obtained precipitate was filtered by suction, washed with water, and dried for 12 hours at 120° C. using a tray dryer, thereby producing a precursor of the positive electrode active material. Next, the lithium carbonate and the precursor of the positive electrode active material were mixed so that the ratio (Li / Me) of the number of lithium (Li) atoms to the sum of the number of metal atoms of Ni, Co, and Mn in the precursor of the positive electrode active material was 1.06, and the mixture was mixed in an automatic mortar for 30 minutes to obtain a mixed powder. Next, the mixed powder was filled into an alumina sagger, and fired in a muffle furnace in an air atmosphere at 750°C for 2 hours, and then heated to 880°C and held at that temperature for 8 hours to obtain a positive electrode active material.

[0044] Example 7 First, nickel sulfate, cobalt sulfate, and manganese sulfate were weighed in predetermined amounts so that the ratio of Ni:Co:Mn was 50:20:30, and a 1.5 mol / L mixed metal salt solution was prepared. The Mg concentration in this mixed metal salt solution was 0.008 g / L. Next, the mixed metal salt solution, ammonia water, and 20% by mass aqueous sodium hydroxide solution were fed to a reactor equipped with an agitator so that the pH in the reactor was 10.6 and the ammonium ion concentration was 14.8 g / L, and a crystallization reaction was carried out to precipitate a nickel-cobalt-manganese composite hydroxide compound. At this time, the rotation speed of the agitator in the reactor was set to 1000 rpm, and the liquid temperature in the reactor was kept at 60°C by a water jacket. In addition, nitrogen gas was introduced into the reaction tank to prevent oxidation of the coprecipitate produced by the crystallization reaction. The gas introduced into the reaction tank is not limited to nitrogen gas, and any gas that does not promote oxidation, such as helium, neon, argon, or carbon dioxide, can be used. Next, the obtained precipitate was filtered by suction, washed with water, and dried for 12 hours at 120° C. using a tray dryer, thereby producing a precursor of the positive electrode active material. Next, the lithium carbonate and the precursor of the positive electrode active material were mixed so that the ratio (Li / Me) of the number of lithium (Li) atoms to the sum of the number of metal atoms of Ni, Co, and Mn in the precursor of the positive electrode active material was 1.06, and the mixture was mixed in an automatic mortar for 30 minutes to obtain a mixed powder. Next, the mixed powder was filled into an alumina sagger, and fired in a muffle furnace in an air atmosphere at 750°C for 2 hours, and then heated to 880°C and held at that temperature for 8 hours to obtain a positive electrode active material.

[0045] Example 8 First, a 1.5 mol / L mixed metal salt solution was prepared by weighing out predetermined amounts of nickel sulfate, cobalt sulfate, and manganese sulfate so that the ratio of Ni:Co:Mn was 82:15:3. The Mg concentration in this mixed metal salt solution was 0.001 g / L. Next, the mixed metal salt solution, ammonia water, and 20% by mass aqueous sodium hydroxide solution were fed to a reactor equipped with an agitator so that the pH in the reactor was 11.2 and the ammonium ion concentration was 13.5 g / L, and a crystallization reaction was carried out to precipitate a nickel-cobalt-manganese composite hydroxide compound. At this time, the rotation speed of the agitator in the reactor was set to 1000 rpm, and the liquid temperature in the reactor was kept at 60°C by a water jacket. In addition, nitrogen gas was introduced into the reaction tank to prevent oxidation of the coprecipitate produced by the crystallization reaction. The gas introduced into the reaction tank is not limited to nitrogen gas, and any gas that does not promote oxidation, such as helium, neon, argon, or carbon dioxide, can be used. Next, the obtained precipitate was filtered by suction, washed with water, and dried for 12 hours at 120° C. using a tray dryer, thereby producing a precursor of the positive electrode active material. Next, lithium hydroxide and the precursor of the positive electrode active material were mixed so that the ratio (Li / Me) of the number of lithium (Li) atoms to the sum of the number of metal atoms of Ni, Co, and Mn in the precursor of the positive electrode active material was 1.01, and the mixture was mixed in an automatic mortar for 30 minutes to obtain a mixed powder. Next, the mixed powder was filled into an alumina sagger and fired in an oxygen atmosphere in a muffle furnace at 500°C for 8 hours, and then heated to 740°C and held at that temperature for 4 hours to obtain a positive electrode active material.

[0046] Example 9 First, a 1.5 mol / L mixed metal salt solution was prepared by weighing out predetermined amounts of nickel sulfate, cobalt sulfate, and manganese sulfate so that the ratio of Ni:Co:Mn was 90:7:3. The Mg concentration in this mixed metal salt solution was 0.002 g / L. Next, the mixed metal salt solution, ammonia water, and 20% by mass aqueous sodium hydroxide solution were fed to a reactor equipped with an agitator so that the pH in the reactor was 11.0 and the ammonium ion concentration was 7.2 g / L, and a crystallization reaction was carried out to precipitate a nickel-cobalt-manganese composite hydroxide compound. At this time, the rotation speed of the agitator in the reactor was set to 820 rpm, and the liquid temperature in the reactor was kept at 60°C by a water jacket. In addition, nitrogen gas was introduced into the reaction tank to prevent oxidation of the coprecipitate produced by the crystallization reaction. The gas introduced into the reaction tank is not limited to nitrogen gas, and any gas that does not promote oxidation, such as helium, neon, argon, or carbon dioxide, can be used. Next, the obtained precipitate was filtered by suction, washed with water, and dried for 12 hours at 120° C. using a tray dryer, thereby producing a precursor of the positive electrode active material. Next, lithium hydroxide and the precursor of the positive electrode active material were mixed so that the ratio (Li / Me) of the number of lithium (Li) atoms to the sum of the number of metal atoms of Ni, Co, and Mn in the precursor of the positive electrode active material was 1.01, and the mixture was mixed in an automatic mortar for 30 minutes to obtain a mixed powder. Next, the mixed powder was filled into an alumina sagger and calcined in an oxygen atmosphere at 500°C for 8 hours in a muffle furnace, and then heated to 720°C and kept at that temperature for 4 hours to obtain a positive electrode active material.

[0047] Example 10 First, a 1.5 mol / L mixed metal salt solution was prepared by weighing out predetermined amounts of nickel sulfate, cobalt sulfate, and manganese sulfate so that the ratio of Ni:Co:Mn was 90:7:3. The Mg concentration in this mixed metal salt solution was 0.001 g / L. Next, the mixed metal salt solution, ammonia water, and 20% by mass aqueous sodium hydroxide solution were fed to a reactor equipped with an agitator so that the pH in the reactor was 11.0 and the ammonium ion concentration was 10.0 g / L, and a crystallization reaction was carried out to precipitate a nickel-cobalt-manganese composite hydroxide compound. At this time, the rotation speed of the agitator in the reactor was set to 1000 rpm, and the liquid temperature in the reactor was kept at 60°C by a water jacket. In addition, nitrogen gas was introduced into the reaction tank to prevent oxidation of the coprecipitate produced by the crystallization reaction. The gas introduced into the reaction tank is not limited to nitrogen gas, and any gas that does not promote oxidation, such as helium, neon, argon, or carbon dioxide, can be used. Next, the obtained precipitate was filtered by suction, washed with water, and dried for 12 hours at 120° C. using a tray dryer, thereby producing a precursor of the positive electrode active material. Next, lithium hydroxide and the precursor of the positive electrode active material were mixed so that the ratio (Li / Me) of the number of lithium (Li) atoms to the sum of the number of metal atoms of Ni, Co, and Mn in the precursor of the positive electrode active material was 0.98, and the mixture was mixed in an automatic mortar for 30 minutes to obtain a mixed powder. Next, the mixed powder was filled into an alumina sagger and fired in an oxygen atmosphere in a muffle furnace at 500°C for 8 hours, and then heated to 720°C and held at that temperature for 4 hours to obtain a positive electrode active material.

[0048] Example 11 First, nickel sulfate, cobalt sulfate, and manganese sulfate were weighed in predetermined amounts so that the ratio of Ni:Co:Mn was 50:20:30, and a 1.5 mol / L mixed metal salt solution was prepared. The Mg concentration in this mixed metal salt solution was 0.094 g / L. Next, the mixed metal salt solution, ammonia water, and 20% by mass aqueous sodium hydroxide solution were fed to a reaction vessel equipped with an agitator so that the pH in the reaction vessel was 10.2 and the ammonium ion concentration was 10.5 g / L, and a crystallization reaction was carried out to precipitate a nickel-cobalt-manganese composite hydroxide compound. At this time, the rotation speed of the agitator in the reaction vessel was set to 1000 rpm, and the liquid temperature in the reaction vessel was kept at 60°C by a water jacket. In addition, nitrogen gas was introduced into the reaction tank to prevent oxidation of the coprecipitate produced by the crystallization reaction. The gas introduced into the reaction tank is not limited to nitrogen gas, and any gas that does not promote oxidation, such as helium, neon, argon, or carbon dioxide, can be used. Next, the obtained precipitate was filtered by suction, washed with water, and dried for 12 hours at 120° C. using a tray dryer, thereby producing a precursor of the positive electrode active material. Next, the lithium carbonate and the precursor of the positive electrode active material were mixed so that the ratio (Li / Me) of the number of lithium (Li) atoms to the sum of the number of metal atoms of Ni, Co, and Mn in the precursor of the positive electrode active material was 1.06, and the mixture was mixed in an automatic mortar for 30 minutes to obtain a mixed powder. Next, the mixed powder was filled into an alumina sagger, and fired in a muffle furnace in an air atmosphere at 750°C for 2 hours, and then heated to 880°C and held at that temperature for 8 hours to obtain a positive electrode active material.

[0049] Comparative Example 1 First, nickel sulfate, cobalt sulfate, and manganese sulfate were weighed in predetermined amounts so that the ratio of Ni:Co:Mn was 50:20:30, and a 1.5 mol / L mixed metal salt solution was prepared. The Mg concentration in this mixed metal salt solution was 0.13 g / L. Next, the mixed metal salt solution, ammonia water, and 20% by mass aqueous sodium hydroxide solution were fed to a reactor equipped with an agitator so that the pH in the reactor was 10.2 and the ammonium ion concentration was 11.1 g / L, and a crystallization reaction was carried out to precipitate a nickel-cobalt-manganese composite hydroxide compound. At this time, the rotation speed of the agitator in the reactor was set to 1000 rpm, and the liquid temperature in the reactor was kept at 60°C by a water jacket. In addition, nitrogen gas was introduced into the reaction tank to prevent oxidation of the coprecipitate produced by the crystallization reaction. The gas introduced into the reaction tank is not limited to nitrogen gas, and any gas that does not promote oxidation, such as helium, neon, argon, or carbon dioxide, can be used. Next, the obtained precipitate was filtered by suction, washed with water, and dried for 12 hours at 120° C. using a tray dryer, thereby producing a precursor of the positive electrode active material. Next, the lithium carbonate and the precursor of the positive electrode active material were mixed so that the ratio (Li / Me) of the number of lithium (Li) atoms to the sum of the number of metal atoms of Ni, Co, and Mn in the precursor of the positive electrode active material was 1.06, and the mixture was mixed in an automatic mortar for 30 minutes to obtain a mixed powder. Next, the mixed powder was filled into an alumina sagger, and fired in a muffle furnace in an air atmosphere at 750°C for 2 hours, and then heated to 880°C and held at that temperature for 8 hours to obtain a positive electrode active material.

[0050] (composition) The compositions of the precursors and positive electrode active material powders of Examples 1 to 11 and Comparative Example 1 were measured as follows. Regarding the nickel, cobalt, and manganese compositions, a specified amount of each of the obtained precursors and each positive electrode active material sample (powder) was weighed out, decomposed by an alkali fusion method, and then a composition analysis was performed using a Hitachi High-Tech inductively coupled plasma optical emission spectrometer (ICP-OES) "PS7800". In addition, regarding the magnesium composition of the precursors and the positive electrode active material, a specified amount of each obtained precursor and each positive electrode active material sample (powder) was weighed out and dissolved by acid decomposition, and then a composition analysis was performed using an inductively coupled plasma mass spectrometer (ICP-MS) "SPQ9700" manufactured by SII Nanotechnology.

[0051] (Average particle size D50) The average particle size D50 of each of the precursors and positive electrode active material powders of Examples 1 to 11 and Comparative Example 1 was measured as follows. 100 mg of each of the obtained precursors and each positive electrode active material sample (powder) was dispersed by irradiating 40 W ultrasonic waves for 60 seconds at 50% flow rate using a Microtrac laser diffraction particle size distribution measuring device "MT3300EXII", and then the particle size distribution was measured to obtain a volume-based cumulative particle size distribution curve. In the obtained cumulative particle size distribution curve, the volume particle size at 50% accumulation was taken as the 50% cumulative volume particle size D50 (average particle size D50) of the positive electrode active material powder. In addition, the water-soluble solvent used in the measurement was passed through a 0.02 μm filter, the solvent refractive index was 1.333, the particle permeability conditions were permeable, the particle refractive index was 1.81, the shape was non-spherical, the measurement range was 0.021 to 2000 μm, and the measurement time was 30 seconds.

[0052] (Tap density) The tap density of each of the precursor and positive electrode active material powders of Examples 1 to 11 and Comparative Example 1 was measured as follows. 5 g of the obtained samples (powder) of each precursor and each positive electrode active material was placed in a 10 cc graduated cylinder and placed in a powder density measuring instrument "KYT-4000K" manufactured by Seishin Enterprise Co., Ltd. After tapping 1500 times with a stroke length of 55 mm, the graduations on the graduated cylinder were read. Next, "sample amount (5 g) / graduation reading on the graduated cylinder (cc)" was calculated, and this was taken as the tap density (g / cc).

[0053] (BET specific surface area) The BET specific surface area of ​​each of the precursors and positive electrode active material powders of Examples 1 to 11 and Comparative Example 1 was measured as follows. 1.0 g of each of the obtained precursors and samples (powder) of each of the positive electrode active materials was weighed into a glass cell, set in a degassing device, and filled with nitrogen gas in the glass cell, and then heat-treated in a nitrogen gas atmosphere at 40°C for 20 minutes to degas the sample. The glass cell containing the degassed sample (powder) was then set in a specific surface area measuring device "Monosorb Model MS-21" manufactured by Quantachrome, and the specific surface area X was measured by the BET method (one-point method) while flowing a He:70at%-N2:30at% mixed gas as the adsorption gas.

[0054] (c-axis lattice constant) The c-axis lattice constant of each of the positive electrode active material powders of Examples 1 to 11 and Comparative Example 1 was measured as follows. The following XRD diffractometer and conditions were used: XRD Diffraction Equipment: SmartLab (Rigaku Corporation) ·Radiation source: CuKα (λ=1.5406Å) Apply the sample (positive electrode active material) to a glass sample holder (2 cm x 1.5 cm, depth 0.3 mm). Detector: D / tex Measurement range: 2θ=10°~80° Scan axis: 2θ / θ, Scan speed: 1 degree min -1 Step width: 0.01 degree Slit width: IS(DS)1 / 4°, RS1 10mm, RS2 10mm The c-axis lattice constant was calculated from the peaks derived from a total of nine crystal planes, namely (003), (101), (012), (104), (015), (107), (018), (110), and (113), in the XRD diffraction pattern measured under the above conditions, using the analytical software “PDXL (Rigaku Corporation).”

[0055] (discharge capacity) The discharge capacity of each of the positive electrode active material powders of Examples 1 to 11 and Comparative Example 1 was measured as follows. The production conditions and evaluation results of the above-mentioned Examples 1 to 11 and Comparative Example 1 are shown in Tables 1 and 2.

[0056] [Table 1]

[0057] [Table 2]

[0058] (Evaluation Results) The positive electrode active materials of Examples 1 to 11 all had the following composition formula: In addition, the "Li / Me ratio" in Tables 1 and 2 indicates the composition ratio of Li to the total of Ni, Co, Mn, and Mg in the positive electrode active material. Composition formula: Li a Ni (1-b-c-d) Co b Mn c Mg d O2 (In the above formula, 0.98≦a≦1.09, 0.06≦b≦0.21, 0.02≦c≦0.32, and 0.00005≦d≦0.003.) Moreover, the positive electrode active materials of Examples 1 to 11 all had a 50% cumulative volume particle size D50 of 3.0 to 11.0 μm, a tap density of 2.0 to 2.6 g / cc, and a c-axis lattice constant of 14.184 to 14.240 Å, and had good battery characteristics (discharge capacity). The positive electrode active material of Comparative Example 1 had a Mg composition d exceeding 0.003, and the battery characteristics (discharge capacity) were inferior to those of Examples 1-11.

Claims

1. Composition formula: Li a Ni (1-b-c-d) Coco b Mn c Mg d O 2 (In the above formula, 0.98≦a≦1.09, 0.06≦b≦0.21, 0.02≦c≦0.32, and 0.00005≦d≦0.003.) The positive electrode active material for a lithium ion battery is represented by the formula (1), having a 50% cumulative volume particle size D50 of 3.0 to 11.0 μm, a tap density of 2.0 to 2.6 g / cc, and a c-axis lattice constant of 14.184 to 14.240 Å.

2. BET specific surface area: 0.20 to 0.80 m 2 The positive electrode active material for a lithium ion battery according to claim 1, wherein the Li-ion battery positive electrode active material has a molecular weight of 1.001 or more.

3. A positive electrode for a lithium ion battery comprising the positive electrode active material for a lithium ion battery according to claim 1 or 2.

4. A lithium ion battery comprising the positive electrode and the negative electrode for a lithium ion battery according to claim 3.

5. The method includes a step of performing a crystallization reaction using an aqueous solution containing (a) a nickel salt, (b) a cobalt salt, (c) a manganese salt, and (d) a magnesium salt, and (e) a basic aqueous solution containing ammonia and / or an alkaline aqueous solution of an alkali metal as a reaction solution, while controlling the pH of the reaction solution to 10.0 to 11.5, the ammonium ion concentration to 5 to 20 g / L, and the solution temperature to 59 to 61° C., Composition formula: Ni (1-b-c-d) Coco b Mn c Mg d (OH) 2 (In the above formula, 0.06≦b≦0.21, 0.02≦c≦0.32, and 0.00005≦d≦0.003.) The 50% cumulative volume particle size D50 is 3.0 to 11.0 μm, the tap density is 1.8 to 2.3 g / cc, and the BET specific surface area is 4.0 to 12.0 m. 2 / g of a precursor of a positive electrode active material for a lithium ion battery.

6. The precursor produced by the method for producing a precursor of a positive electrode active material for a lithium ion battery according to claim 5 and a lithium source are mixed together to obtain a lithium-ion battery positive electrode active material having a total number of atoms of metals consisting of Ni, Co, Mn and Mg (Me n ) and the number of lithium atoms (Li n ) and the ratio (Li n / Me n ) is 0.98 to 1.09 to form a lithium mixture; calcining the lithium mixture in air or an oxygen atmosphere at 450 to 750° C. for 2 to 15 hours, and then calcining the lithium mixture at 700 to 900° C. for 2 to 15 hours; The method for producing a positive electrode active material for a lithium ion battery includes the steps of:

Citation Information

Patent Citations

  • Positive electrode active material for lithium secondary battery, positive electrode for lithium secondary battery, and lithium secondary battery

    JP2019003955A

  • Precursor of oxide-based positive electrode active material for all-solid lithium ion battery, oxide-based positive electrode active material for all-solid lithium ion battery, positive electrode for all-solid lithium ion battery, all-solid lithium ion battery, production method of precursor of oxide-based positive electrode active material for all-solid lithium ion battery, and production method of oxide-based positive electrode active material for all-solid lithium ion battery

    JP2021158007A

  • Positive electrode active material including lithium nickel-based oxide doped with doping element, and secondary battery including the same

    JP2022518480A

  • Positive electrode active material for lithium secondary batteries

    JP6626151B2

  • Positive electrode active material particles for non-aqueous electrolyte secondary battery, method for producing the same, and non-aqueous electrolyte secondary battery

    JP6968844B2