Electrolysis cell
The electrolytic cell with a Ni-based and porous YCZ fuel electrode addresses the oxidation issue in SOECs, maintaining stability and performance by enhancing reaction sites and suppressing Ni oxidation.
Patent Information
- Application Number
- JP2023056751
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
The electrode structure of solid oxide electrolytic cells (SOECs) deteriorates due to oxidation of Ni-based particles when exposed to high-temperature water vapor, leading to a decrease in electrolytic properties.
The electrolytic cell is designed with a fuel electrode composed of Ni-based particles and porous electrolyte particles made of solid oxide electrolyte B, such as YCZ, which have a high specific surface area and oxygen storage capacity, incorporating macropores and mesopores to enhance stability and reaction activity.
The fuel electrode maintains structural integrity and electrolytic performance by suppressing Ni oxidation and increasing reaction sites, resulting in a significant reduction in reaction resistance increase, even under high-temperature steam exposure.
Smart Images

Figure 2024143843000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrolysis cell, and more particularly to an electrolysis cell equipped with a fuel electrode that undergoes little change in electrode structure even when exposed to high-temperature water vapor. [Background technology]
[0002] A solid oxide fuel cell (SOFC) is a fuel cell that uses an oxide ion conductor as an electrolyte. When fuel gases such as H2, CO, and CH4 are supplied to the anode (fuel electrode) of the SOFC and O2 is supplied to the cathode (oxygen electrode), an electrode reaction proceeds and electricity can be extracted. The CO2 and H2O produced by the electrode reaction are discharged outside the SOFC. On the other hand, solid oxide electrolysis cells (SOECs) have the same structure as SOFCs, but they operate in the opposite direction to the SOFC reaction: when CO2 or H2O is supplied to the cathode (fuel electrode) of an SOEC and an electric current is passed between the electrodes, CO and H2 can be produced.
[0003] The SOEC is equipped with a single cell in which an anode (air electrode) is bonded to one side of an electrolyte, and a cathode (fuel electrode) is bonded to the other side. The following materials are generally used as materials for components constituting such an SOEC (see Non-Patent Documents 1 to 6). (a) Electrolytes: yttria-stabilized zirconia (YSZ), scandia-stabilized zirconia (SSZ), samaria-doped ceria (SDC), lanthanum strontium gallium magnesium oxide (LSGM), etc. (b) Air electrode: lanthanum strontium manganite (LSM), lanthanum strontium cobalt ferrite (LSCF), lanthanum strontium cobaltite (LSC), etc. (c) Anode: Ni / YSZ, Ni / SDC, Ni-Fe / SDC, etc.
[0004] Ni / YSZ cermet is generally used for the fuel electrode of SOEC. However, water vapor, which is the raw material for hydrogen production, is supplied to the fuel electrode at high temperatures (700°C or higher). As a result, the Ni contained in the fuel electrode is easily oxidized, causing a change in the electrode structure. As a result, the electrolytic characteristics are degraded.
[0005] To solve this problem, Patent Document 1 proposes a fuel electrode containing Ni-containing particles and ACZ particles made of a composite oxide (ACZ) of A2O3 (where A=Y, La, and / or Sc), CeO2, and ZrO2. Moreover, Patent Document 2 proposes an active layer made of a cermet containing Ni-containing particles and YScCZ particles made of ZrO2 doped with Y, Sc, and Ce. However, there is a limit to how much the durability of SOEC can be improved by simply optimizing the materials used in the anode. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2022-181976 A [Patent Document 2] JP 2022-074189 A [Non-patent literature]
[0007] [Non-Patent Document 1] Ebbesen, SD; Hansen, JB; Morgensen, MB ECS Trans. 2013, 57, 3217. [Non-Patent Document 2] Jensen, SH; Larsen, PH; Mogensen, M. Int. J. Hydrogen Energy 2007, 32, 3253. [Non-Patent Document 3] Katahira, K.; Kohchi, Y.; Shimura, T.; Iwahara, H. Solid State Ionics 2000, 138, 91. [Non-Patent Document 4] Languna-Bercero, MA; Skinner, SJ; Kilner, JAJ Power Sources 2009, 192, 126. [Non-Patent Document 5] O'Brien, JE; Stoots, CM; Herring, JS; Lessing, PA; Hartvigsen, JJ; Elangovan, SJ Fuel Cell Sci. Technol. 2005, 2, 156. [Non-Patent Document 6] Sune Dalgaard Ebbesen, Soren Hojgaard Jensen, Anne Hauch, and Morgens Bjerg Morgensen, Chem. Rev. 2014, 114, 1069 Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide an electrolysis cell having a fuel electrode that undergoes minimal change in electrode structure even when exposed to high-temperature water vapor. [Means for solving the problem]
[0009] In order to solve the above problems, the electrolytic cell according to the present invention has the following configuration. (1) The electrolysis cell comprises: an electrolyte layer including a solid oxide electrolyte A; a fuel electrode formed on one surface of the electrolyte layer; an air electrode formed on the other surface of the electrolyte layer; an intermediate layer inserted between the electrolyte layer and the air electrode; It is equipped with: (2) The fuel electrode is Ni-based particles, Porous electrolyte particles made of solid oxide electrolyte B with oxygen storage capacity It is equipped with: (3) The specific surface area of the fuel electrode is 100 m 2 / g or more. Effect of the Invention
[0010] The fuel electrode of an electrolytic cell is generally made of a cermet containing Ni-based particles and electrolyte particles. The electrolyte particles are usually dense particles (particles with few pores) manufactured by a method such as coprecipitation. A fuel electrode using dense electrolyte particles has a low specific surface area, and when the specific surface area of the fuel electrode is less than 100 m 2 / g.
[0011] In contrast, when manufacturing a fuel electrode containing Ni-based particles and electrolyte particles, if porous particles containing mesopores are used as the electrolyte particles, a fuel electrode with a larger specific surface area than conventional fuel electrodes can be obtained. Furthermore, when an electrolytic cell is produced using such a fuel electrode with a high specific surface area, an electrolytic cell with a larger specific surface area than conventional electrolytic cells can be obtained. When the manufacturing conditions are optimized, the specific surface area of the fuel electrode and the specific surface area of the entire electrolytic cell can be increased to 100 m2 or more. 2 / g or more.
[0012] The fuel electrode and electrolysis cell obtained in this way may exhibit properties different from those of conventional fuel electrodes and electrolysis cells due to their high specific surface area. For example, when porous electrolyte particles having oxygen storage capacity are used as the electrolyte particles contained in the fuel electrode, the stability of the electrode structure in a high-temperature water vapor environment is higher than that of a fuel electrode using dense electrolyte particles having oxygen storage capacity. This is thought to be because the reactive active sites are increased while maintaining the electrode activity by making the electrolyte particles porous (increasing the specific surface area). [Brief description of the drawings]
[0013] [Figure 1]This is a schematic diagram of an electrolysis cell using Ni / YCZ as the fuel electrode (active layer). [Diagram 2] FIG. 1 is a schematic diagram of a conventional electrolysis cell that uses Ni / YSZ as the fuel electrode (active layer). [Diagram 3] FIG. 1 is a schematic diagram of an electrolytic cell used in impedance measurement. [Figure 4] FIG. 2 is a diagram showing the specific surface areas of the electrolytic cells obtained in Example 1 and Comparative Example 1. [Diagram 5] FIG. 2 is a diagram showing the pore volumes of the electrolytic cells obtained in Example 1 and Comparative Example 1. [Figure 6] FIG. 13 is a diagram showing an example of an impedance analysis result. [Figure 7] 2 shows the reaction resistance (Rct2) increase rates of the fuel electrodes obtained in Example 1 and Comparative Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] [Configuration 1] An electrolysis cell comprising: (1) The electrolysis cell comprises: an electrolyte layer including a solid oxide electrolyte A; a fuel electrode formed on one surface of the electrolyte layer; an air electrode formed on the other surface of the electrolyte layer; an intermediate layer inserted between the electrolyte layer and the air electrode; It is equipped with: (2) The fuel electrode is Ni-based particles, Porous electrolyte particles made of solid oxide electrolyte B with oxygen storage capacity It is equipped with: (3) The specific surface area of the fuel electrode is 100 m 2 / g or more.
[0015] [Configuration 2] The electrolysis cell comprises: Macropores A having a pore diameter of 0.1 μm or more and 0.5 μm or less; Mesopores A having a pore diameter of 5 nm or more and 50 nm or less; Includes The pore volume of the macropores A is 0.02 cc / g or more, The pore volume of the mesopores A is 0.2 cc / g or more. 2. The electrolytic cell according to claim 1.
[0016] [Configuration 3] The fuel electrode is Macropores B having a pore diameter of 0.1 μm or more and 0.5 μm or less; Mesopores B having a pore diameter of 5 nm or more and 50 nm or less; Including, The pore volume of the macropores B is 0.01 cc / g or more, The pore volume of the mesopores B is 0.2 cc / g or more. 3. The electrolytic cell according to claim 1 or 2.
[0017] [Configuration 4] The electrolytic cell according to any one of configurations 1 to 3, wherein the solid oxide electrolyte B is made of YCZ having a composition represented by the following formula (1): Y x Ce y Zr 1-x-y O 2-δ (1) however, 0 <x≦0.2、0<y≦0.2、 δ is the value at which electrical neutrality is maintained.
[0018] [Configuration 5] An electrolytic cell according to any one of configurations 1 to 4, wherein the reaction resistance (Rct2) increase rate represented by the following formula (2) is 200% or less. Reaction resistance (Rct2) increase rate = (R2-R1) x 100 / R1…(2) however, R1 is the electrochemical reaction resistance of the anode immediately after manufacture; R2 is the electrochemical reaction resistance of the fuel electrode after the durability test.
[0019] [Configuration 6] The electrolyte layer includes the solid oxide electrolyte A, Yttria-stabilized zirconia (YSZ), Scandia-stabilized zirconia (SSZ), Samaritan Doptheriae (SDC), or Lanthanum Strontium Gallium Magnesium Oxide (LSGM) 6. The electrolytic cell of any one of configurations 1 to 5, comprising:
[0020] [Configuration 7] The air electrode is Lanthanum strontium manganite (LSM), Lanthanum strontium cobalt ferrite (LSCF), or Lanthanum strontium cobaltite (LSC), 7. The electrolytic cell of any one of configurations 1 to 6, comprising:
[0021] [Configuration 8] 8. The electrolytic cell of any one of claims 1 to 7, wherein the intermediate layer comprises Gd-doped CeO2 (GDC).
[0022] [Configuration 9] An air electrode-side current collecting layer formed on the surface of the air electrode, and / or A fuel electrode-side current collecting layer formed on the surface of the fuel electrode 9. The electrolysis cell of any one of configurations 1 to 8, further comprising:
[0023] An embodiment of the present invention will be described in detail below. [1. Fuel electrode] The fuel electrode according to the present invention is Ni-based particles, Porous electrolyte particles made of solid oxide electrolyte B with oxygen storage capacity It is equipped with:
[0024] [1.1. Ni-based particles] The "Ni-based particles" refer to metal particles in which the mass ratio of Ni to the total mass of metal elements contained in the particles is 90 mass% or more. The mass ratio of Ni contained in the Ni-based particles is preferably 95 mass% or more. The Ni-based particles function as an electrode catalyst and an electron conductor in the fuel electrode, and the composition of the Ni-based particles is not particularly limited as long as it exhibits such functions. Examples of Ni-based particles include Ni, Ni-Fe alloys, Ni-Co alloys, etc. Among these, the Ni-based particles are preferably Ni or Ni-Fe alloys.
[0025] [1.2. Electrolyte particles] [1.2.1. Definition] In the present invention, the term "electrolyte particles" refers to porous particles made of a solid oxide electrolyte B having an oxygen storage capacity. The term "porous particles" refers to particles in which minute crystallites are bonded together, and in which pores with a diameter of 50 nm or less exist between the crystallites. In other words, "porous particles" refer to particles that have mesopores inside. The raw powder of such porous particles is obtained by firing a mixture of fine oxide particles (precursor particles) produced by a coprecipitation method and carbon derived from a resin. The carbon derived from the resin suppresses densification of the electrolyte particles and functions as a template when increasing the specific surface area of the electrolyte particles. The details of the method for producing the raw powder of the porous particles will be described later.
[0026] [1.2.2. Solid oxide electrolyte B] In the present invention, the composition of the solid oxide electrolyte B is not particularly limited as long as it has oxygen storage capacity and functions as an oxide ion conductor. Among oxide ion conductors, a composite oxide containing CeO2 and ZrO2 (CZ-based oxide) has high oxygen storage capacity and is therefore suitable as the solid oxide electrolyte B.
[0027] The solid oxide electrolyte B may be, for example, (a) A composite oxide of Y2O3, CeO2 and ZrO2 (YCZ), (b) Composite oxide of Sc2O3, CeO2 and ZrO2 (ScCZ), (c) Composite oxide of La2O3, CeO2 and ZrO2 (LaCZ), (d) Composite oxide of Y2O3, Sc2O3, CeO2, and ZrO2 (YScCZ) etc. Among these, YCZ has a high oxygen storage capacity and is therefore suitable as the solid oxide electrolyte B constituting the electrolyte particles.
[0028] [1.2.3. Oxygen storage and release capacity] The YCZ particles are made of ZrO2 doped with Y and Ce. In general, the more Ce contained in the YCZ particles, the more the oxygen storage capacity increases, the lower the oxide ion conductivity, the higher the electronic conductivity, and the lower the strength. In other words, the YCZ particles in the fuel electrode function as oxide ion conductors, as electron conductors, as a function to suppress the oxidation of Ni contained in the Ni-based particles, and as a function to maintain the strength of the fuel electrode.
[0029] The main function of Y doped in ZrO2 is to give ZrO2 high ionic conductivity. The main function of Ce doped in ZrO2 is to give ZrO2 oxygen storage and release capacity and electronic conductivity. Therefore, when YCZ particles are added to a fuel electrode containing Ni-based particles, the oxidation of Ni contained in the Ni-based particles is significantly suppressed while maintaining high electrode activity. Even if the Ni-based particles are oxidized, electrons are conducted via the YCZ particles. Even if the Ni-based particles contain a metal element other than Ni, if the oxidation of at least Ni can be suppressed, a three-phase boundary (TPB) can be ensured in the electrode.
[0030] The reaction of oxygen storage and release in CeO2-doped ZrO2 (CZ) is shown in the following formula (a). In formula (a), the reaction proceeding to the right side is an oxidation reaction, and the reaction proceeding to the left side is a reduction reaction. CEO 2-x -ZrO2+(x / 2)O2⇔ CeO2-ZrO2…(a)
[0031] The Ce ions dissolved in ZrO2 can reversibly take a trivalent state (reduced state) or a tetravalent state (oxidized state) depending on the oxygen partial pressure in the surrounding atmosphere. Therefore, when CZ is exposed to an oxidizing atmosphere, CZ takes in oxygen ions in the atmosphere into its crystal lattice. On the other hand, when CZ is exposed to a reducing atmosphere, CZ releases oxygen ions in its crystal lattice into the atmosphere. This is also true for YCZ and solid oxide electrolyte B other than YCZ that has oxygen storage capacity.
[0032] [1.2.4. Composition of YCZ particles] When YCZ is used as the solid oxide electrolyte B, the electrolyte particles made of YCZ (YCZ particles) preferably have a composition represented by the following formula (1). Y x Ce y Zr 1-x-y O 2-δ (1) however, 0 <x≦0.2、0<y≦0.2、 δ is the value at which electrical neutrality is maintained.
[0033] In formula (1), x represents the ratio of the number of moles of Y to the total number of moles of Y, Ce, and Zr contained in the YCZ particles. If x is too small, the oxide ion conductivity of the YCZ particles may decrease. Therefore, x must be greater than 0. x is preferably 0.04 or more, or 0.08 or more. On the other hand, if x is too large, the oxide ion conductivity may decrease. Therefore, x is preferably 0.2 or less. More preferably, x is 0.15 or less, or 0.1 or less.
[0034] In formula (1), y represents the ratio of the number of moles of Ce to the total number of moles of Y, Ce, and Zr contained in the YCZ particles. If y is too small, the amount of oxygen stored decreases, and the oxidation inhibition function of Ni contained in the Ni-based particles may decrease. Also, if y is too small, the electronic conductivity of the YCZ particles may decrease. Therefore, y must be greater than 0. y is preferably 0.04 or more, or 0.08 or more. On the other hand, if y is too large, not only the oxide ion conductivity of the fuel electrode decreases, but also the mechanical strength of the fuel electrode may decrease. Therefore, y is preferably 0.2 or less. y is more preferably 0.15 or less, or 0.1 or less.
[0035] [1.3. Composition of the fuel electrode] The "content of Ni-based particles" refers to the ratio of the mass of Ni-based particles to the total mass of the electrolyte particles and Ni-based particles contained in the fuel electrode.
[0036] If the content of the Ni-based particles is too low, the total cell resistance increases and the efficiency of the electrode reaction decreases. Therefore, the content of the Ni-based particles is preferably 30 mass% or more. The content is more preferably 40 mass% or more. On the other hand, if the content of Ni-based particles is excessive, the content of electrolyte particles will be reduced, and the efficiency of the electrode reaction may decrease. In addition, when the electrolyte particles are made of solid oxide electrolyte B having oxygen storage capacity, if the content of Ni-based particles is excessive, the oxidation of Ni contained in the Ni-based particles cannot be sufficiently suppressed. Therefore, the content of Ni-based particles is preferably 70 mass% or less.
[0037] [1.4. Porosity] The porosity of the fuel electrode affects the electrolysis characteristics. If the porosity of the fuel electrode is too small, the gas diffusion decreases, and the efficiency of the electrode reaction decreases. Therefore, the porosity of the fuel electrode is preferably 15% or more. The porosity is more preferably 20% or more, or 25% or more. On the other hand, if the porosity of the fuel electrode is too large, the number of three-phase interfaces becomes relatively small, and the efficiency of the electrode reaction decreases. Therefore, the porosity of the fuel electrode is preferably 40% or less. The porosity is more preferably 35% or less, or 30% or less.
[0038] [1.5. Characteristics” [1.5.1. Specific surface area] Strictly speaking, the "specific surface area of the fuel electrode" refers to the specific surface area calculated based on the injection pressure and amount of mercury obtained by measuring the amount of mercury injected at a mercury injection pressure P by mercury porosimetry for the fuel electrode separated from the electrolytic cell. When the specific surface area of an electrolytic cell (sample cell) equipped with a fuel electrode having a high specific surface area according to the present invention and an electrolytic cell (reference cell) having the same structure as the electrolytic cell according to the present invention except that the fuel electrode has a low specific surface area are measured by mercury intrusion porosimetry, the specific surface area of the fuel electrode having a high specific surface area can be estimated from the difference between the specific surface areas of the sample cell and the reference cell. The fuel electrode according to the present invention contains porous electrolyte particles, and therefore has a larger specific surface area than conventional fuel electrodes. When the manufacturing conditions are optimized, the specific surface area of the fuel electrode can be increased to 100 m2 or more. 2 / g or more, or 150m 2 / g or more.
[0039] [1.5.2. Macropores B, Mesopores B] The term "macropore" generally refers to a pore having a diameter of 50 nm or more. However, in the present invention, the term "macropore B" refers to a pore having a pore diameter of 0.1 μm or more and 0.5 μm or less among the pores contained in the fuel electrode. Similarly, the term "mesopore" generally refers to a pore having a diameter of 2 nm or more and 50 nm or less. However, in the present invention, the term "mesopore B" refers to a pore contained in the fuel electrode, the pore having a pore diameter of 5 nm or more and 50 nm or less.
[0040] Strictly speaking, the "pore volume of macropore B" refers to the volume of macropore B measured by mercury intrusion porosimetry for the fuel electrode separated from the electrolysis cell. Strictly speaking, the "pore volume of mesopores B" refers to the volume of mesopores B measured by mercury intrusion porosimetry for the fuel electrode separated from the electrolysis cell. As with the specific surface area, the pore volume of the sample cell and the reference cell are measured by mercury intrusion porosimetry, and the pore volume of mesopore B can be estimated from the difference between the pore volumes of the sample cell and the reference cell.
[0041] The fuel electrode according to the present invention includes porous electrolyte particles, and therefore includes not only macropores B originating from large voids between the Ni-based particles or electrolyte particles, but also mesopores B originating from fine voids within the electrolyte particles or fine voids at the Ni-based particle / electrolyte particle interfaces. When the manufacturing conditions are optimized, the pore volume of macropore B becomes 0.01 cc / g or more. When the manufacturing conditions are further optimized, the pore volume of macropore B becomes 0.02 cc / g or more, or 0.03 cc / g or more. Similarly, when the production conditions are optimized, the pore volume of mesopores B becomes 0.2 cc / g or more. When the production conditions are further optimized, the pore volume of mesopores B becomes 0.3 cc / g or more, or 0.4 cc / g or more.
[0042] [1.5.3. Reaction resistance (Rct2) increase rate] "Reaction resistance (Rct2) increase rate (%)" refers to the value expressed by the following formula (2). Reaction resistance (Rct2) increase rate = (R2-R1) x 100 / R1…(2) however, R1 is the electrochemical reaction resistance of the anode immediately after manufacture; R2 is the electrochemical reaction resistance of the fuel electrode after the durability test, "Electrochemical reaction resistance (Rct2)" is the reaction resistance of the three-phase interface in the fuel electrode obtained by performing impedance measurement on the electrolytic cell, and is the diameter of the arc (second arc) that contributes to the electrode reaction. The "durability test" refers to a test in which steam electrolysis is performed for 100 hours under the conditions shown in Table 1.
[0043] [Table 1]
[0044] Conventional fuel electrodes have low oxidation resistance, so the reaction resistance (Rct2) increase rate exceeds 900%. In contrast, when the material and structure of the fuel electrode according to the present invention are optimized, the reaction resistance (Rct2) increase rate becomes smaller than that of the conventional fuel electrode. Specifically, when the material and structure of the fuel electrode are optimized, the reaction resistance (Rct2) increase rate becomes 200% or less. When the material and structure of the fuel electrode are further optimized, the reaction resistance (Rct2) increase rate becomes 150% or less, or 120% or less.
[0045] [1.6. Usage] The fuel electrode according to the present invention is suitable as a fuel electrode for electrolysis cells for performing various electrolysis processes such as steam electrolysis and CO2 electrolysis, but can also be used as a fuel electrode for solid oxide fuel cells.
[0046] [2. Manufacturing method of porous electrolyte powder] In order to manufacture a fuel electrode with a high specific surface area, it is first necessary to manufacture a porous electrolyte powder. A method for manufacturing a porous YCZ powder is described in detail below, but the following method can also be applied to solid oxide electrolytes B other than YCZ.
[0047] When the solid oxide electrolyte B is YCZ, the porous YCZ powder, which is the raw material for producing a high specific surface area anode, is (a) preparing a precursor slurry A containing a YCZ precursor by a coprecipitation method; (b) adding a monomer capable of forming a resin by polymerization to the precursor slurry A, and polymerizing the monomer in the precursor slurry A to obtain a precursor slurry B consisting of a mixture of the resin and the YCZ precursor; (c) drying the precursor slurry B under appropriate conditions, and then primarily baking the dried powder to carbonize the resin, thereby obtaining a primarily baked product consisting of a mixture of carbon and the YCZ precursor; (d) subjecting the primary fired product to secondary firing in a reducing atmosphere to obtain a secondary fired product; (e) The second fired product is subjected to a third firing in an oxidizing atmosphere. This is obtained by:
[0048] [2.1. 1st step] First, a precursor slurry A containing a YCZ precursor is prepared by a coprecipitation method. In the present invention, the raw materials for producing the YCZ precursor are not particularly limited, and the most suitable raw materials can be selected depending on the purpose.
[0049] The Y source may be, for example, yttrium nitrate hexahydrate, yttrium sulfate, yttrium chloride, yttrium chloride hexahydrate, yttrium carbonate, or the like. Examples of Zr sources include zirconium oxynitrate dihydrate, zirconium oxychloride octahydrate, zirconium tetrachloride, zirconium oxyacetate, and zirconium sulfate tetrahydrate. Examples of the Ce source include diammonium cerium (IV) nitrate, cerium (III) nitrate hexahydrate, cerium chloride, and cerium carbonate. When a neutralizing agent (alkali) is added to a solution containing a Y source, a Zr source, and a Ce source (hereinafter also referred to as “liquid A”), poorly soluble salts are precipitated in liquid A, and precursor slurry A is obtained.
[0050] [2.2. 2nd process] Next, a monomer capable of forming a resin by polymerization is added to the precursor slurry A, and the monomer is polymerized in the precursor slurry A. This results in a precursor slurry B consisting of a mixture of the resin and the YCZ precursor. The types of monomers and resins obtained by polymerizing the monomers are not particularly limited, and an optimum material can be selected depending on the purpose.
[0051] Examples of the monomer (and the resin synthesized from the monomer) include: (a) Urea and formalin (urea resin), (b) melamine and formalin (melamine resin), (c) Phenol and formalin (resole type phenolic resin), etc. The method for polymerizing the monomers is not particularly limited, and an optimal method can be selected depending on the type of monomer.
[0052] [2.3. Third step] Next, the precursor slurry B is dried under appropriate conditions to obtain a dried powder. The dried powder is then subjected to primary firing, which carbonizes the resin and obtains a primary fired product consisting of a mixture of carbon and the YCZ precursor. The drying conditions for the precursor slurry B are not particularly limited, and the optimum conditions can be selected depending on the purpose. The conditions for the primary firing of the dried powder are not particularly limited, so long as the conditions are such that the resin can be carbonized.
[0053] [2.4. 4th step] Next, the primary fired product is subjected to secondary firing in a reducing atmosphere, thereby obtaining a secondary fired product. The secondary firing (reduction treatment) is performed to form necks between the YCZ precursor fine particles while suppressing the progress of sintering of the YCZ precursor fine particles by heating while leaving carbon between the particles, and to grow the formed necks thicker. The conditions for the secondary firing are not particularly limited as long as they provide such functions.
[0054] [2.5. 5th step] The secondary fired product is then tertiary fired in an oxidizing atmosphere to obtain a porous YCZ powder. The third firing is (a) To burn off carbon contained in the secondary burnt product, and (b) To generate YCZ particles by reacting the YCZ precursor in a solid state. will be held. The conditions for the tertiary firing are not particularly limited as long as they provide such functions. In particular, the tertiary firing is preferably performed by burning off carbon at a low temperature (about 500°C) and then firing at a high temperature (1300°C to 1400°C, preferably a temperature higher than the firing temperature of the fuel electrode) to cause a solid-phase reaction.
[0055] Using this method, a specific surface area of 10 m 2 / g or more, or 15m2 The porous electrolyte powder having a specific surface area of 100 m / g or more can be obtained. Furthermore, when such a porous electrolyte powder is used as a raw material for the fuel electrode, 2 / g or more can be obtained. This is thought to be because new mesoscale pores are formed at the interfaces between the porous YCZ particles and the Ni particles when the NiO contained in the anode is reduced.
[0056] [3. Manufacturing method of fuel electrode] The fuel electrode according to the present invention is (a) A compact is produced using a raw material mixture containing a raw material of Ni-based particles and a porous electrolyte powder (e.g., a porous YCZ powder); (b) sintering the resulting green body; (c) The obtained sintered body is subjected to a reduction treatment. It can be produced by the above method.
[0057] [3.1. Molded object forming process] First, a raw material mixture containing raw materials of Ni-based particles and porous electrolyte powder (for example, porous YCZ powder) is used to produce a compact.
[0058] "Raw material for Ni-based particles" refers to a raw material that becomes Ni-based particles after sintering and reduction. In the present invention, the type of raw material for Ni-based particles is not particularly limited, and an optimal raw material can be selected depending on the purpose. Examples of raw materials for Ni-based particles include NiO powder, Fe2O3 powder, Fe3O4 powder, a mixture of metal Fe and NiO or metal Ni, CoO powder, and Co2O3 powder. The porous electrolyte powder and the method for producing the same are as described above, and therefore description thereof will be omitted.
[0059] The raw material mixture may contain a pore-forming material (e.g., carbon powder). The metal oxide (e.g., NiO powder) contained in the raw material of the Ni-based particles added to the raw material mixture is reduced after the sintered body is produced. During this process, volumetric shrinkage occurs, and pores are introduced into the sintered body. Therefore, the pore-forming material is not necessarily required. However, adding a pore-forming material to the raw material mixture increases the degree of freedom in controlling the porosity. Furthermore, the raw materials are preferably mixed so as to obtain a fuel electrode having a desired composition after sintering and reduction.
[0060] The method for producing the molded body is not particularly limited, and an optimal method can be selected depending on the purpose. Examples of the method for producing the molded body include (a) A method of tape-casting a slurry containing a raw material mixture, laminating the obtained green sheet on a substrate (e.g., a green sheet to be a current collector layer on the anode side after sintering, or a green sheet to be an electrolyte layer after sintering), and isostatically pressing the laminate; (b) preparing a slurry containing the raw material mixture and screen printing the slurry on a surface of a substrate; etc.
[0061] [3.2. Sintering process] Next, the obtained molded body is sintered (sintering step). It is preferable to select the optimum sintering conditions according to the raw material composition. Sintering is usually performed in an air atmosphere at 1000°C to 1500°C (preferably 1000°C to 1300°C) for 1 hour to 5 hours. If a pore-forming material is contained in the raw material mixture, the pore-forming material disappears during sintering, and pores are formed in the sintered body.
[0062] [3.3. Reduction process] Next, the obtained sintered body is subjected to a reduction treatment (reduction step). As a result, the fuel electrode according to the present invention is obtained. The reduction treatment is carried out to reduce metal oxides such as NiO contained in the sintered body and generate Ni-based particles. The reduction conditions are not particularly limited, and it is preferable to select the optimum conditions depending on the composition of the fuel electrode.
[0063] As described below, the electrolysis cell is composed of an assembly of a fuel electrode (cathode), an electrolyte layer, a reaction prevention layer, and an air electrode (anode). An anode-side current collecting layer may be further joined to the outside of the fuel electrode, and / or an air electrode-side current collecting layer may be further joined to the outside of the air electrode. Sintering and joining of each layer is performed by stacking the compacts and then heating the stack to a predetermined temperature. When the optimal sintering temperature of each layer is different, sintering is usually performed in multiple stages. Furthermore, reduction of the fuel electrode is usually performed after all layers have been joined.
[0064] [4. Electrolysis cell] [4.1. Configuration] FIG. 1 shows a schematic diagram of an electrolysis cell using Ni / YCZ as the fuel electrode (active layer). In FIG. 1, the electrolysis cell 10 is an electrolyte layer 12 including a solid oxide electrolyte A; a fuel electrode 14 bonded to one surface of the electrolyte layer 12; a cathode 16 bonded to the other surface of the electrolyte layer 12; An intermediate layer (reaction prevention layer) 18 inserted between the electrolyte layer 12 and the air electrode 16; It is equipped with:
[0065] The high specific surface area fuel electrode according to the present invention is used for the fuel electrode 14. Details of the fuel electrode 14 are as described above, and therefore will not be described here. 1, an anode-side current collecting layer 20 is further disposed on the outer side of the anode 14. The anode-side current collecting layer 20 is for supporting the anode 14 when the thickness of the anode 14 is thin. The anode-side current collecting layer 20 can be omitted. Similarly, although not shown, an air electrode side current collecting layer may be further disposed on the outside of the air electrode 16. The air electrode side current collecting layer (not shown) is for supporting the air electrode 16 when the thickness of the air electrode 16 is thin. The air electrode side current collecting layer may be omitted.
[0066] [4.2. Materials] The materials for the electrolyte layer 12, the air electrode 16, the intermediate layer 18, the fuel electrode side current collecting layer 20, and the air electrode side current collecting layer (not shown) are not particularly limited, and an optimum material can be selected depending on the purpose.
[0067] [4.2.1. Electrolyte layer, air electrode, intermediate layer] For example, the solid oxide electrolyte A constituting the electrolyte layer 12 may include Yttria-stabilized zirconia (YSZ), Scandia-stabilized zirconia (SSZ), Samaritan Doptheria (SDC), Lanthanum Strontium Gallium Magnesium Oxide (LSGM) The electrolyte layer 12 may be made of any one of these solid oxide electrolytes A, or may be a mixture or solid solution of two or more of them.
[0068] The air electrode 16 has: Lanthanum strontium manganite (LSM), Lanthanum strontium cobalt ferrite (LSCF), Lanthanum strontium cobaltite (LSC), The air electrode 16 may be made of any one of these materials, or may be a mixture or solid solution of two or more of these materials. The intermediate layer 18 is inserted as necessary to prevent a reaction caused by direct contact between the electrolyte layer 12 and the air electrode 16. For example, when the electrolyte layer 12 is YSZ and the air electrode 16 is LSC, it is preferable to use Gd-doped CeO2 (GDC) for the intermediate layer 18.
[0069] [4.2.2. Fuel electrode side current collecting layer] The fuel electrode side current collecting layer 20 includes at least (a) a function of supporting the fuel electrode 14 formed on the surface of the electrolyte layer 12; (b) Diffusion of the raw material for electrolysis to the fuel electrode 14; (c) a function of transporting electrons required for the reduction reaction from the current collector to the fuel electrode 14; and (d) A function of discharging hydrogen generated at the fuel electrode 14 by the electrode reaction to the outside of the fuel electrode 14 It is necessary to have the following. There are no particular limitations on the composition of the fuel electrode side current collecting layer 20 as long as it exhibits the above-mentioned functions. The current collecting layer is preferably a cermet containing Ni-based particles and electrolyte particles made of a solid oxide electrolyte.
[0070] [A. Ni-based particles contained in the current collecting layer] The "Ni-based particles (hereinafter also referred to as "Ni-based particles C")" contained in the hydrogen electrode side current collecting layer 20 (hereinafter also simply referred to as the "current collecting layer") refer to metal particles in which the mass ratio of Ni to the total mass of metal elements contained in the particles is 10 mass% or more. The mass ratio of Ni contained in the Ni-based particles C is preferably 50 mass% or more, and more preferably 90 mass% or more.
[0071] The Ni-based particles C function as an electron conductor in the current collecting layer. The composition of the Ni-based particles C is not particularly limited as long as it exhibits such a function. Examples of the Ni-based particles B include Ni, Ni-Fe alloys, and Ni-Co alloys.
[0072] [B. Electrolyte particles] The composition of the electrolyte particles contained in anode current collecting layer 20 (hereinafter also referred to as "electrolyte particles C") is not particularly limited as long as it functions as a current collecting layer. The electrolyte particles C may be, for example, (a) Yttria-stabilized zirconia (YSZ) containing 3–15 mol% Y2O3; (b) a material having the same or similar composition as the electrolyte particles contained in the anode; etc. Among these, YSZ is preferable for the electrolyte particles C because it has stable mechanical strength.
[0073] [C. Composition of the current collecting layer] The "content of Ni-based particles C" refers to the ratio of the mass of Ni-based particles C to the total mass of electrolyte particles C and Ni-based particles C contained in the current collecting layer. The content of the Ni-based particles C is not particularly limited as long as the current collecting layer functions as such. The content of the Ni-based particles C contained in the current collecting layer may be the same as or different from the content of the Ni-based particles contained in the fuel electrode. The content of the Ni-based particles C contained in the current collecting layer is usually 30 to 70 mass%.
[0074] [D. Porosity] The porosity of the current collecting layer affects the gas diffusibility, strength, electronic conductivity, etc. of the fuel electrode 14. In general, if the porosity of the current collecting layer is too small, the gas diffusibility decreases. Therefore, the porosity of the current collecting layer is preferably 40% or more. The porosity is more preferably 45% or more, and even more preferably 50% or more. On the other hand, if the porosity of the current collecting layer is too high, the strength and electronic conductivity may decrease. Therefore, the porosity of the current collecting layer is preferably 60% or less. The porosity is preferably 58% or less, and more preferably 55% or less.
[0075] [4.2.3. Cathode side current collecting layer] The function of the air electrode side current collecting layer is almost the same as that of the anode side current collecting layer 20 , except that the reaction form at the air electrode 16 differs from that at the anode 14 . The material of the electrolyte particles in the air electrode side current collecting layer is LSC, LSCF, etc. Other points regarding the air electrode side current collecting layer are similar to those of the fuel electrode side current collecting layer 20, so a description thereof will be omitted.
[0076] [4.3. Characteristics] [4.3.1. Specific surface area] The "specific surface area of the electrolytic cell" refers to the specific surface area calculated based on the amount of mercury injected into the electrolytic cell at a mercury injection pressure P measured using the mercury injection method and the obtained mercury injection pressure and amount of mercury injected. The "electrolytic cell" used when measuring the specific surface area may or may not include a current collecting layer. The electrolytic cell according to the present invention has a high specific surface area, but since this high specific surface area is mainly derived from the fuel electrode, the presence or absence of a current collecting layer does not significantly change the specific surface area of the electrolytic cell. The same applies to the pore volume of mesopores A in the electrolytic cell.
[0077] The electrolytic cell according to the present invention has a fuel electrode containing porous electrolyte particles, and therefore has a larger specific surface area than conventional electrolytic cells. When the manufacturing conditions are optimized, the specific surface area of the electrolytic cell is 100 m 2 By further optimizing the manufacturing conditions, the specific surface area of the electrolytic cell can be increased to 150 m 2 / g or more, or 200m 2 / g or more.
[0078] [4.3.2. Macropores A, Mesopores A] In the present invention, the "macropores A" refer to pores contained in the electrolytic cell, the pores having a pore diameter of 0.1 μm or more and 0.5 μm or less. In the present invention, "mesopores A" refer to pores having a pore diameter of 5 nm or more and 50 nm or less among the pores contained in the electrolytic cell.
[0079] "Pore volume of macropore A" refers to the volume of macropore A measured using mercury intrusion porosimetry for an electrolytic cell. "Mesopore A pore volume" refers to the volume of mesopore A measured by mercury intrusion porosimetry for an electrolytic cell.
[0080] The electrolysis cell according to the present invention includes an anode with a high specific surface area. As described above, the anode contains macropores B and mesopores B. The voids in the cathode, intermediate layer, and current collecting layer are mainly macropores, but may contain a small amount of mesopores. That is, the electrolysis cell according to the present invention contains coarse macropores A originating from the fuel electrode, air electrode, intermediate layer and current collecting layer, and fine mesopores A originating mainly from the fuel electrode.
[0081] When the manufacturing conditions are optimized, the pore volume of macropore A becomes 0.02 cc / g or more. When the manufacturing conditions are further optimized, the pore volume of macropore A becomes 0.03 cc / g or more, or 0.04 cc / g or more. Similarly, when the production conditions are optimized, the pore volume of mesopores A becomes 0.2 cc / g or more. When the production conditions are further optimized, the pore volume of mesopores A becomes 0.3 cc / g or more, or 0.4 cc / g or more.
[0082] [5. Effect] [5.1. Oxidation of Ni] Fig. 2 shows a schematic diagram of a conventional electrolysis cell using Ni / YSZ as the fuel electrode (active layer). In Fig. 2, the conventional electrolysis cell 10' includes an electrolyte layer 12, a fuel electrode 14' bonded to one surface of the electrolyte layer 12, a cathode 16 bonded to the other surface of the electrolyte layer 12, and an intermediate layer (reaction prevention layer) 18 inserted between the electrolyte layer 12 and the cathode 16. In the conventional electrolysis cell 10', Ni / YSZ cermet is used as the fuel electrode 14'.
[0083] In an electrolysis cell 10′ in which an anode 14′ is made of Ni / YSZ cermet, when H2O is supplied to the anode 14′ and a current is passed between the anode 14′ and the air electrode 16, a reduction reaction shown in the following formula (3) proceeds in the anode 14′. H2O+2e - → H2+O 2- …(3)
[0084] However, in water electrolysis using the electrolysis cell 10', high-temperature (700°C or higher) water vapor, which serves as the raw material, is supplied to the fuel electrode 14'. As a result, Ni contained in the fuel electrode 14' is easily oxidized to form Ni(OH)2. Ni(OH)2 is easily evaporated, and the evaporation of Ni(OH)2 changes the morphology of the three-phase interface, which is the electrode reaction site. As a result, the electrolysis characteristics are degraded. The same is true for SOFCs. That is, water is generated by an electrode reaction at the anode (fuel electrode) of SOFCs. Therefore, especially under high-load operating conditions, the generated water may oxidize Ni in the fuel electrode, resulting in a decrease in power generation characteristics.
[0085] [4.2. Suppression of Ni oxidation by solid oxide electrolyte (YCZ) with oxygen storage capacity] In contrast, certain solid oxide electrolytes have oxygen storage capacity. In particular, YCZ exhibits high oxygen storage capacity. Therefore, when steam electrolysis is performed using an electrolysis cell equipped with a fuel electrode containing Ni-based particles and YCZ particles, the oxidation of Ni is significantly suppressed. The reason why the addition of YCZ particles to the fuel electrode in an electrolysis cell significantly suppresses the oxidation of Ni is believed to be as follows.
[0086] [4.2.1. Fixation of oxygen ions by YCZ] When an anode containing Ni and YCZ is exposed to high-temperature water vapor, the Ni is oxidized and the surface of the Ni particles becomes Ni(OH)2 (Step 1). At this time, if there are YCZ particles in the vicinity of the Ni particles, oxygen is extracted from the Ni(OH)2 and the extracted oxygen is fixed to the YCZ (Step 2). It is thought that the trigger for this is the oxygen storage ability of YCZ.
[0087] [4.2.2. Generation of reducing atmosphere using YCZ] The oxygen extracted from Ni(OH)2 is temporarily trapped by YCZ (Step 3). The fuel electrode is in a reducing atmosphere due to H2 generated from the Ni catalyst. YCZ itself has the ability to decompose water, and hydrogen is generated from it, so YCZ also functions as a H2 source. Furthermore, in a reducing atmosphere, YCZ easily releases the trapped oxygen atoms or oxygen ions as oxygen molecules. The oxygen molecules released from YCZ are discharged outside the system before reoxidizing Ni (Step 4). Alternatively, the oxygen ions in the YCZ particles diffuse within the YCZ particles due to an electrolytic reaction, and oxygen vacancies are formed (Step 5). It is believed that Ni oxidation is suppressed by repeating steps 1 to 5. The same is true when using a solid oxide electrolyte other than YCZ that has oxygen storage capacity; by adding a solid oxide electrolyte with oxygen storage capacity to the fuel electrode, Ni oxidation is suppressed.
[0088] [4.3. Improving performance by increasing the specific surface area of electrolyte particles] A composite oxide of Y2O3, CeO2, and ZrO2 (YCZ) has the ability to store oxygen. Therefore, when steam electrolysis is performed using a steam electrolysis cell equipped with a hydrogen electrode containing YCZ particles and Ni-based particles, the oxidation of the Ni-based particles is suppressed. However, there is a limit to the effect of suppressing the oxidation of the Ni-based particles in a hydrogen electrode containing dense YCZ particles. In contrast, when porous YCZ particles are used as the solid oxide electrolyte added to the hydrogen electrode, the oxidation of the Ni-based particles is further suppressed. This is thought to be because by making the YCZ particles porous (increasing the specific surface area), the number of reaction active sites increases while maintaining the electrode activity. EXAMPLES
[0089] (Example 1, Comparative Examples 1-2) [1. Sample preparation] [1.1. Preparation of high specific surface area YCZ powder (Example 1)] The Y source was yttrium nitrate hexahydrate, the Zr source was zirconium oxynitrate dihydrate, and the Ce source was diammonium cerium(IV) nitrate. 10.34 g of yttrium nitrate hexahydrate, 40.89 g of zirconium oxynitrate dihydrate, and 10.96 g of diammonium cerium (IV) nitrate were weighed out and dissolved in ion-exchanged water to obtain 400 mL of solution A. The pH of solution A was 1.2.
[0090] 57.04 g of 2-aminoethanol as a neutralizing agent and 253.16 g of ammonium polyacrylate (Aron A30SL, manufactured by Toagosei Co., Ltd.) as a dispersing agent were added to ion-exchanged water and mixed to obtain solution B. The pH of solution B was 10.8.
[0091] Using a cassette tube pump, liquid A and liquid B were sent to the high shear rate region between the rotor and stator of a super agitation (SA) reactor at a speed of 5 mL / min. The rotor rotation speed was set to 8000 rpm. When liquid A and liquid B were supplied to the SA reactor, a neutralization reaction occurred, and a precursor slurry was obtained. The pH of the precursor slurry was 9.7.
[0092] Next, 52.7 g of urea was dissolved in ion-exchanged water to obtain 250 mL of solution C. Also, 128.3 g of a 37% aqueous reagent solution of formaldehyde was added to ion-exchanged water to obtain 250 mL of solution D. Furthermore, 28.9 g of maleic acid for promoting polymerization of the urea resin was dissolved in ion-exchanged water to obtain 200 mL of solution E.
[0093] While stirring 800 mL of precursor slurry with a magnetic stirrer, liquids C and D were simultaneously added dropwise at 10 mL / min to obtain a precursor slurry containing methylol urea (pH 6.6). Next, liquid E was added dropwise to the precursor slurry containing methylol urea at 10 mL / min to obtain a precursor slurry containing urea resin.
[0094] The precursor slurry containing urea resin was placed in a 1L glass beaker and dried in an air degreasing furnace at 150°C for 12 hours. The beaker was then placed in a stainless steel pot, covered, and further heated (steamed) in an air degreasing furnace at 300°C for 4 hours to carbonize the urea resin. The carbon derived from the urea resin suppresses the densification of YCZ and serves as a template for increasing the specific surface area.
[0095] The mixture obtained was subjected to reduction firing at 900°C for 5 hours in a furnace whose internal components and heating element were made of graphite in a reducing atmosphere of Ar + a small amount of CO. The small amount of CO was generated by the reaction of oxygen generated from the sample with the graphite components in the furnace. Next, the reduced powder was oxidized in air at 500°C for 3 hours, and then sintered in air at 1340°C for 5 hours to obtain a high-specific surface area YCZ powder. The amount of Y (x) in the obtained high specific surface area YCZ powder was 0.14, and the amount of Ce (y) was 0.04. The specific surface area of the high specific surface area YCZ powder was 17.8 m 2 / g.
[0096] [1.2. Preparation of low specific surface area YCZ powder (Comparative Example 1)] Cerium nitrate was used as the Ce source. Zirconium oxynitrate was used as the Zr source. Yttrium nitrate hexahydrate was used as the Y source. Yttrium nitrate hexahydrate and zirconium oxynitrate were added to an aqueous cerium nitrate solution and mixed. 30 mass% hydrogen peroxide was further added to this and mixed to obtain a mixed solution A. The mixing ratio of each raw material was set to a ratio that would obtain a YCZ powder having the same composition as in Example 1. Separately, a mixed solution B was obtained by mixing 25% ammonia water and ion-exchanged water. Mixture A was added to mixture B with stirring. After a predetermined time had passed, the precipitate was collected.
[0097] Next, the precipitate was heat-treated in air at 150°C for 7 h and 400°C for 5 h and then dried. The dried powder was then calcined in air at 1400°C for 5 h to obtain a low-specific surface area YCZ powder. The specific surface area of the low-specific surface area YCZ powder was 3.8 m 2 / g.
[0098] [1.2. Preparation of electrolytic cell] [1.2.1 Example 1, Comparative Example 1] A GDC sheet (intermediate layer) was placed on one side of an 8YSZ electrolyte pellet (thickness 500 μm) with a reference electrode attached to the side, and then sintered at 1380°C. Next, a fuel electrode was formed on the other surface of the 8YSZ electrolyte pellet (the surface opposite to the surface on which the intermediate layer was baked) by applying Ni / YCZ paste (NiO:YCZ=1:1, mass ratio) by screen printing and firing at 1340°C.
[0099] Next, the LSC / GDC paste was applied onto the intermediate layer by screen printing and fired at 1125°C to form the air electrode. Furthermore, the LSC paste was applied onto the LSC / GDC electrode (air electrode) by screen printing and fired at 950°C to form an air electrode-side current collecting layer.
[0100] [1.2.2. Comparative Example 2] An electrolytic cell was prepared in the same manner as in Example 1, except that a commercially available 8YSZ powder was used instead of the YCZ powder.
[0101] 2. Test Method [2.1. Specific surface area, pore volume] The specific surface area and pore volume of the electrolytic cell were measured by mercury intrusion porosimetry. Anton Paar's Poremaster 60GT was used for the measurement. The low pressure measurement time was about 40 to 60 minutes, and the measurement was performed from 20 PSI (0.1379 MPa) to 40,000 PSI (275.8 MPa).
[0102] Using the following equation (4), the relationship between the pressure P of mercury injection into the pores and the pore diameter D was calculated, and based on this relationship, the relationship between the pore diameter and the pore volume was calculated. D = {-4γ(cosθ)} / P (4) however, γ is the surface tension of mercury (480 erg / cm 2 ), θ is the contact angle between mercury and the pore wall (135°).
[0103] The amount of mercury intrusion at a certain pressure P (pore diameter D) was converted into a cylindrical pore with a diameter D. Furthermore, the specific surface area S was calculated by converting the cylindrical pore with a diameter D into the area of the pore wall. It should be noted that a pressure of 20 to 40,000 PSI (0.1379 to 275.8 MPa) corresponds to a pore diameter of 0.005 μm to 9.8 μm.
[0104] [2.2. Reaction resistance (Rct2) increase rate] Figure 3 shows a schematic diagram of the electrolysis cell used for impedance measurement. A reference electrode was attached to the side of the electrolyte layer. The reference electrode is used to measure the voltage V1 between the electrolyte layer and the air electrode, and the voltage V2 between the electrolyte layer and the fuel electrode. By attaching the reference electrode to the electrolyte layer, the fuel electrode and the air electrode can be evaluated separately. Using the electrolysis cell shown in Figure 3, a 100-hour steam electrolysis test (durability test) was conducted under the conditions shown in Table 1. During the durability test, impedance measurements were conducted to measure the reaction resistance (Rct2). Furthermore, the reaction resistance (Rct2) increase rate was calculated using the reaction resistance (Rct2) before and after the durability test.
[0105] [3. Results] [3.1. Specific surface area, pore volume] FIG. 4 shows the specific surface areas of the electrolytic cells obtained in Example 1 and Comparative Example 1. The specific surface area of the electrolytic cell in Example 1 is 265 m 2 On the other hand, the specific surface area of the electrolytic cell of Comparative Example 1 was 72 m 2 / g. Fig. 5 shows the pore volumes of the electrolytic cells obtained in Example 1 and Comparative Example 1. The pore volume of macropores A in the electrolytic cell of Example 1 was 0.04 cc / g, and the pore volume of mesopores A was 0.51 cc / g. On the other hand, the pore volume of macropores A in the electrolytic cell of Comparative Example 1 was 0.04 cc / g, and the pore volume of mesopores A was 0.14 cc / g.
[0106] The difference in the specific surface area and pore volume between Example 1 and Comparative Example 1 is believed to be due to the difference in the structure of the fuel electrode. From FIG. 4, it can be seen that the specific surface area of the fuel electrode obtained in Example 1 is at least 265 m 2 / g-72m 2 / g ≒ 190m 2 5, the pore volume of mesopores B in the fuel electrode obtained in Example 1 is estimated to be at least 0.51 cc / g-0.14 cc / g=0.37 cc / g.
[0107] [3.2. Reaction resistance (Rct2) increase rate] Figure 6 shows an example of the impedance analysis results. In Figure 6, the second arc (Rct2) represents the magnitude of the electrochemical reaction resistance of the fuel electrode. The larger the diameter of the second arc, the greater the electrochemical reaction resistance. The arc to the left of the second arc is the first arc (Rct1), which represents the magnitude of the resistance of the electrolyte ion path in the hydrogen electrode.
[0108] 7 shows the reaction resistance (Rct2) increase rate of the fuel electrodes obtained in Example 1 and Comparative Examples 1 and 2. The reaction resistance (Rct2) increase rates of Comparative Example 2, Comparative Example 1, and Example 1 were 982%, 234%, and 112%, respectively. The reaction resistance (Rct2) of Comparative Example 1 was reduced to about 1 / 4 of that of Comparative Example 2. Furthermore, the reaction resistance (Rct2) increase rate of Example 1 was reduced to about 1 / 2 of that of Comparative Example 2.
[0109] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the gist of the present invention. [Industrial Applicability]
[0110] The electrolytic cell according to the present invention can be used for various electrolysis processes such as steam electrolysis and CO2 electrolysis.
Claims
1. An electrolysis cell comprising: (1) The electrolytic cell comprises: an electrolyte layer including a solid oxide electrolyte A; a fuel electrode formed on one surface of the electrolyte layer; an air electrode formed on the other surface of the electrolyte layer; an intermediate layer interposed between the electrolyte layer and the air electrode; It is equipped with: (2) The fuel electrode is Ni-based particles; Porous electrolyte particles made of a solid oxide electrolyte B having an oxygen storage capacity; It is equipped with: (3) The specific surface area of the fuel electrode is 100 m 2 / g or more.
2. The electrolysis cell comprises: Macropores A having a pore diameter of 0.1 μm or more and 0.5 μm or less; Mesopores A having a pore diameter of 5 nm or more and 50 nm or less; Includes The pore volume of the macropores A is 0.02 cc / g or more, The pore volume of the mesopores A is 0.2 cc / g or more.
2. The electrolysis cell of claim 1.
3. The fuel electrode is Macropores B having a pore diameter of 0.1 μm or more and 0.5 μm or less; Mesopores B having a pore diameter of 5 nm or more and 50 nm or less; Including, The pore volume of the macropores B is 0.01 cc / g or more, The pore volume of the mesopores B is 0.2 cc / g or more.
2. The electrolysis cell of claim 1.
4. 2. The electrolytic cell according to claim 1, wherein the solid oxide electrolyte B is made of YCZ having a composition represented by the following formula (1): Y x Ce y Zr 1-x-y O 2-δ (1) however, 0<x≦0.2, 0<y≦0.2, δ is the value at which electrical neutrality is maintained.
5. 2. The electrolytic cell according to claim 1, wherein the increase rate of the reaction resistance (Rct2) represented by the following formula (2) is 200% or less. Reaction resistance (Rct2) increase rate = (R 2 -R 1 ) × 100 / R 1 …(2) however, R 1 is the electrochemical reaction resistance of the anode immediately after manufacture, R 2 is the electrochemical reaction resistance of the fuel electrode after durability testing.
6. The electrolyte layer includes the solid oxide electrolyte A, Yttria stabilized zirconia (YSZ), Scandia-stabilized zirconia (SSZ), Samaria dopout ceria (SDC), or Lanthanum Strontium Gallium Magnesium Oxide (LSGM) 2. The electrolysis cell of claim 1 comprising:
7. The air electrode is Lanthanum strontium manganite (LSM), Lanthanum strontium cobalt ferrite (LSCF), or Lanthanum strontium cobaltite (LSC), 2. The electrolysis cell of claim 1 comprising:
8. The intermediate layer is Gd-doped CeO 2 2. The electrolytic cell of claim 1 comprising (GDC).
9. An air electrode-side current collecting layer formed on the surface of the air electrode, and / or A fuel electrode-side current collecting layer formed on the surface of the fuel electrode 10. The electrolysis cell of claim 1 further comprising:
Citation Information
Patent Citations
Solid oxide fuel cell or electrolytic cell electrode material and preparation method and application thereof
CN114665109A
Method for making electrochemical apparatus for recovery of oxygen
JP2006321706A
Solid oxide fuel cell
JP2013152915A
Anode for solid oxide fuel cell
JP2020155349A
Hydrogen electrode for water vapor electrolysis
JP2022181976A