Carbon nanotube composite and method for producing the same, and use thereof

A binderless CNT composite with specific properties effectively immobilizes metal nanoparticles, enhancing catalytic activity and battery performance by eliminating the negative effects of insulating binders, resulting in high-performance electrode catalysts and batteries.

JP2024144174APending Publication Date: 2024-10-11OSAKA UNIVERSITY +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024028947
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-02-28
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional carbon nanotube (CNT) composites require the use of a binder to immobilize metal nanoparticles, which leads to decreased catalytic activity and battery performance due to the insulating properties of the binder.

Method used

A binderless CNT composite is produced by immobilizing metal nanoparticles on single-walled carbon nanotubes with specific properties, including a length of 10 μm or more, carbon purity of 90% or more, and a BET specific surface area of 600 m²/g or more, without using a binder, utilizing a reduction treatment such as radiation reduction.

Benefits of technology

The binderless CNT composite exhibits improved catalytic activity and reduced internal resistance, suitable for high-performance electrode catalysts and batteries with enhanced charging and discharging capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144174000001_ABST
    Figure 2024144174000001_ABST
Patent Text Reader

Abstract

To provide a carbon nanotube composite with improved catalytic activity.SOLUTION: A carbon nanotube composite according to one embodiment includes: single-wall carbon nanotubes with a length of 10 μm or more, a carbon purity of 90% or more, and a BET specific surface area of 600 m2 / g or more; and metal nanoparticles fixed on the single-wall carbon nanotubes.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a carbon nanotube composite, a method for producing the same, and uses thereof. [Background technology]

[0002] Composites of metal nanoparticles and carbon nanotubes (CNTs) (CNT composites) are used in electrode catalysts, etc. Various CNT composites have been produced, and for example, Patent Document 1 describes a support-nanoparticle composite that includes nanoparticles and a carbon support having a polymer layer on its surface. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Special Publication No. 2018-538134 Summary of the Invention [Problem to be solved by the invention]

[0004] The CNT composites described in the above-mentioned prior art require the use of a binder to fix nanoparticles on the surface of the CNTs. However, when an insulating binder is used, the catalytic activity of the CNT composite decreases, which results in a decrease in battery performance.

[0005] One aspect of the present invention has been made in consideration of the above-mentioned problems, and has an object to provide a CNT composite with improved catalytic activity. [Means for solving the problem]

[0006] In order to solve the above problems, the present inventors conducted intensive research and found that by using a specific CNT, metal nanoparticles can be fixed to the surface of the CNT without using a binder, and a binderless CNT composite can be produced, leading to the completion of the present invention. Note that, when fixing metal nanoparticles to the surface of the CNT, it is common technical knowledge for those skilled in the art to use a binder, and it is not expected that a binderless CNT composite can be obtained by using the specific CNT according to one embodiment of the present invention.

[0007] That is, the present invention includes the following configurations. <1> Length is 10μm or more, carbon purity is 90% or more, BET specific surface area is 600m 2 / g or more, and metal nanoparticles fixed on the single-walled carbon nanotubes. <2> At least a portion of the surface of the metal nanoparticles is oxidized, and the average valence of the metal element on the oxidized surface is greater than 0 and less than 2; <1> The carbon nanotube composite according to claim 1, <3> The content of the metal nanoparticles is 1 to 20% by weight when the total weight of the carbon nanotube composite is 100% by weight. <1> or <2> The carbon nanotube composite according to claim 1, <4> <1> ~ <3> A molded article comprising the carbon nanotube composite according to any one of claims 1 to 5. <5> <1> ~ <3> 2. An electrode catalyst comprising the carbon nanotube composite according to claim 1 . <6> <1> ~ <3> 13. The carbon nanotube composite according to claim 12, <4> or <5> An electrode for a battery, comprising the electrode catalyst according to claim 1. <7> <5> or <6> A battery comprising the battery electrode according to claim 1. <8> Length is 10μm or more, carbon purity is 90% or more, BET specific surface area is 600m 2 The present invention relates to a method for producing a binderless carbon nanotube composite, the method including a fixation step of performing a reduction treatment on a solution containing single-walled carbon nanotubes having a molecular weight of 1000 nm or more and metal nanoparticles. <9> At least a portion of the surface of the metal nanoparticles contained in the carbon nanotube composite is oxidized, and the average valence of the metal element on the oxidized surface is greater than 0 and less than 2. <8> 2. A method for producing the carbon nanotube composite according to claim 1 . <10> The reduction treatment is carried out by radiation reduction; <8> or <9> 2. A method for producing the carbon nanotube composite according to claim 1 . <11> <8> ~ <10> 2. A method for producing a molded article, comprising the steps of obtaining a carbon nanotube composite by the method for producing a carbon nanotube composite according to claim 1, and molding the carbon nanotube composite. <12> In the step of forming the carbon nanotube composite, pressure is applied. <11> A method for producing the molded article according to claim 1. Effect of the Invention

[0008] According to one aspect of the present invention, a CNT composite with improved catalytic activity can be provided. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a diagram showing a TEM observation image of a CNT composite according to an example of the present invention. [Diagram 2] FIG. 1 is a diagram showing the results of PXRD measurement of a CNT composite according to an example of the present invention. [Diagram 3] FIG. 2 is a diagram showing the results of EXAFS analysis of a CNT composite according to an embodiment of the present invention. [Figure 4] FIG. 1 is a diagram showing the results of XANES analysis and EXAFS analysis of a CNT complex according to an embodiment of the present invention. [Diagram 5] FIG. 1 is a diagram showing the results of electrochemical measurement of a CNT composite according to an example of the present invention. [Figure 6] FIG. 1 is a diagram showing the results of XANES analysis of a CNT complex according to an example of the present invention. [Figure 7] FIG. 2 is a diagram showing the results of EXAFS analysis of a CNT composite according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [1. CNT Composite] The binderless CNT composite according to one embodiment of the present invention has a length of 10 μm or more, a carbon purity of 90% or more, and a BET specific surface area of ​​600 m. 2 / g or more, and metal nanoparticles fixed on the single-walled CNTs.

[0011] Conventionally, the method of fixing metal nanoparticles on the surface of CNTs has been to use an insulating binder. However, the binder also adheres to the surface of the CNTs, reducing the active surface area and increasing the internal resistance. As a result, conventional CNT composites have low catalytic activity, and battery characteristics are degraded, especially when applied to batteries that perform high-power charging and discharging.

[0012] The CNT composite has the above-mentioned structure, and thus can be made into a binderless CNT composite. Therefore, due to its high catalytic activity and low internal resistance, it can be used as a high-performance electrode catalyst or a high-performance battery (capacitor). In this specification, the "binderless CNT composite" is also simply referred to as a "CNT composite."

[0013] In this specification, "binderless" means that no binder is included as a component of the CNT composite. However, the CNT composite may contain a small amount of binder that is derived from the raw material of the CNT composite, that may be unavoidably mixed in the manufacturing process, or that is below the detection limit. The binder is not particularly limited and may include any binder that is normally used in batteries.

[0014] <cnt> A CNT complex according to one embodiment of the present invention includes CNTs, the CNTs having a length of 10 μm or more, a carbon purity of 90% or more, and a BET specific surface area of ​​600 m. 2 The CNTs have the above-mentioned structure, which makes it possible to fix metal nanoparticles to the CNT surface without using a binder.

[0015] The length of the CNT is 10 μm or more, preferably 150 μm or more. The upper limit of the length of the CNT is not particularly limited, but may be, for example, 10 cm or less. If the length of the CNT is 10 μm or more, the CNTs are easily entangled with each other, making it easy to produce a binderless composite. The length of the CNT can be determined, for example, by electron microscope observation or infrared absorption spectroscopy.

[0016] The diameter of the CNT is, for example, 1 to 5 nm. The diameter of the CNT can be determined, for example, by electron microscope observation or Raman spectroscopy. The CNT may have a G band / D band intensity ratio of 5 or less as measured by Raman spectroscopy.

[0017] The carbon purity of the CNT is 90% or more, preferably 95% or more, and more preferably 99% or more. The upper limit of the carbon purity of the CNT may be, for example, 100% or less. When the purity of the CNT is 99% or more, the reaction between the impurities and the electrolyte of the battery is less likely to occur, and the influence on other materials is reduced. The carbon purity of the CNT may be determined from the weight loss at 400°C or at 800°C by thermogravimetric analysis. For example, the weight loss of the CNT at 400°C or at 800°C by thermogravimetric analysis may be 10% by weight or less, 5% by weight or less, or 1% by weight or less. For example, the weight loss of the CNT at 400°C by thermogravimetric analysis may be 2% by weight or less, and the weight loss at 800°C by thermogravimetric analysis may be 1% by weight or less.

[0018] The BET specific surface area of ​​CNT is 600m 2 / g or more, preferably 800m 2 / g or more, more preferably 1000m 2 / g or more. The upper limit of the BET specific surface area of ​​CNTs is, for example, 1300 m 2 / g or less. The BET specific surface area is 600 m 2 / g or more, it can store a large amount of charge when used in a battery. The BET specific surface area can be measured by measuring the adsorption / desorption isotherm of liquid nitrogen at 77K and measuring from this adsorption / desorption isotherm using the method of Brunauer, Emmett, and Teller. The BET specific surface area can be measured, for example, using a commercially available BET specific surface area measuring device.

[0019] When the CNTs are primarily unopened, the specific surface area is preferably 600 m 2 / g or more, more preferably 800m 2 / g or more, more preferably 1000m 2 / g or more. When the CNTs are mainly unopened, the specific surface area is 1300 m 2 / g or less. Also, if the CNTs are mainly open, the specific surface area is preferably 1600 m 2 / g or more, 2500m 2 / g or more.

[0020] CNTs can be obtained by a conventional method, but preferably, they are produced by a production method (super-growth method) in which a trace amount of oxidizing agent is present in the system when a raw material compound and a carrier gas are supplied onto a substrate having a catalyst layer for CNT growth on the surface to synthesize carbon nanotubes by chemical vapor deposition, thereby dramatically improving the catalytic activity of the catalyst layer. The super-growth method is disclosed in International Publication No. 2006 / 011655 and Kenji Hata et. al. "Water-Assisted Highly Efficient Synthesis of Impurity-Free Single-Walled Carbon Nanotubes" SCIENCE VOL306, p.1362-1364, 19 November 2004. Carbon nanotubes produced by the super-growth method are more preferable because they easily satisfy the above-mentioned CNT parameters and can fix metal nanoparticles to the CNT surface without using a binder.

[0021] The CNT content is preferably 80 to 99% by weight, more preferably 80 to 95% by weight, and even more preferably 80 to 90% by weight, assuming the total weight of the CNT composite to be 100% by weight.

[0022] <Metal nanoparticles> A CNT composite according to one embodiment of the present invention contains metal nanoparticles. By fixing the metal nanoparticles to the carbon surface of the CNT composite, the electrical conductivity of the CNT composite is improved.

[0023] The metal nanoparticles may include, for example, platinum, gold, silver, palladium, ruthenium, rhodium, molybdenum, osmium, iridium, rhenium, vanadium, tungsten, cobalt, iron, nickel, bismuth, tin, chromium, titanium, copper, or alloys thereof. Among these, from the viewpoint of catalytic activity, platinum, gold, silver, and palladium are preferable, and platinum is more preferable. The surface of the metal nanoparticles may be at least partially oxidized. Preferably, the surface of the metal nanoparticles is not entirely but partially oxidized. The average value of the valence of the metal element in the oxidized part of the metal nanoparticle surface is preferably greater than 0 and less than 2, and more preferably greater than 0 and less than 1. The fact that the metal nanoparticle surface is partially oxidized and the average value of the valence of the metal element can be confirmed by XANES analysis described in the examples.

[0024] The content of the metal nanoparticles is preferably 1 to 20% by weight, more preferably 5 to 20% by weight, and further preferably 10 to 20% by weight, when the total weight of the CNT composite is taken as 100% by weight. If the content of the metal nanoparticles is 1% by weight or more, sufficient catalytic activity can be obtained. If the content of the metal nanoparticles is 20% by weight or less, the CNT content in the CNT composite is sufficient. The content of the metal nanoparticles can be calculated from inductively coupled plasma (ICP) measurement.

[0025] The average particle size of the metal nanoparticles is preferably 1 to 10 nm, and more preferably 1 to 5 nm. When the average particle size of the metal nanoparticles is within the above range, the metal nanoparticles are easily dispersed on the surface of the CNT. The average particle size of the metal nanoparticles means the average particle size of the primary particle diameter, and is measured by a transmission electron microscope (TEM), powder X-ray diffraction (XRD), X-ray absorption spectroscopy (XAS), or the like.

[0026] The shape of the metal nanoparticles may be, for example, spherical. In this specification, spherical does not mean only a perfect sphere, but may include an approximately spherical shape. For example, the outer surface of the sphere of the metal nanoparticles may not be flat, and the radius of curvature of each metal nanoparticle may not be constant. The shape of the metal nanoparticles may be any shape, such as a rectangular parallelepiped, rod, or tetrahedron. When the metal nanoparticles are not spherical, the size of the metal nanoparticles is preferably 1 to 10 nm in diameter.

[0027] <Other> The CNT composite can be formed into a desired shape. For example, when used in an electrode or the like described below, the CNT composite may be accumulated into a film. When the CNT composite is formed into a film, the thickness may be, for example, 0.1 μm to 1000 μm. In that case, the density may be 0.05 to 1.0 g / cm. 3 may be also possible.

[0028] [2. Molded body containing CNT composite, electrode catalyst, battery electrode, and battery] <Molded body> The molded body according to one embodiment of the present invention includes the above-mentioned CNT composite. As described above, the CNT composite is binderless, but the molded body may contain a binder from the viewpoint of moldability and strength. The molded body is binderless in the composite of CNT and metal nanoparticles. As the binder, an insulating binder or a conductive binder may be used. However, when the molded body according to one embodiment of the present invention is used for an electrode catalyst or a battery electrode, a conductive binder with lower resistance is preferable. Here, the conductive binder is not particularly limited, but examples thereof include polyethylene, polystyrene, fluororesin, etc., into which a hydrophilic functional group such as a sulfonic acid group or a carboxyl group has been introduced, and more specifically, examples of fluororesin into which a sulfonic acid group has been introduced include Nafion (registered trademark). The insulating binder is not particularly limited, but examples thereof include polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF).

[0029] <Electrode catalyst> An electrode catalyst according to one embodiment of the present invention includes the above-mentioned CNT composite. The electrode catalyst may be a solid CNT composite, or may be a slurry, paste, or the like in which the CNT composite is dissolved in a solvent. In one embodiment, the electrode catalyst may be made of a CNT composite or a molded body. The electrode catalyst may be used for both the positive electrode and the negative electrode.

[0030] Since the CNT composite does not contain an insulating binder, the CNT surface is not covered with a binder, and the active surface area of ​​the CNT is not reduced. This allows the electrode catalyst containing the CNT composite to exhibit high catalytic activity. The electrode catalyst can also be used, for example, in organic electrosynthesis.

[0031] <Battery electrode> An electrode according to one embodiment of the present invention includes the above-mentioned CNT composite, molded body, or electrode catalyst. Since the above-mentioned CNT composite is binderless, the obtained battery electrode is suitable for high-output charging and discharging. The electrode may be a positive electrode or a negative electrode.

[0032] The electrode may include a substrate (current collector), such as glassy carbon, a graphene-coated substrate, a transparent conductive (ITO) substrate, an aluminum substrate, or a copper substrate.

[0033] The method for producing the electrode is not particularly limited, and may be, for example, a method of applying a CNT composite to a substrate. More specifically, a slurry containing an electrode catalyst and a solvent may be applied to a substrate, and then dried to obtain an electrode. Examples of the solvent include N-methyl-2-pyrrolidone, dimethylformamide, and ethanol. In another example, the electrode is made of the above-mentioned electrode catalyst. That is, the electrode may be made of a CNT composite or a molded body. In this case, for example, the electrode catalyst may be solidified without using a binder, or may be solidified using a binder.

[0034] <Battery> A battery according to one embodiment of the present invention includes the above-mentioned electrode and / or electrode catalyst. That is, the battery may include an electrode including the above-mentioned CNT composite as either the positive electrode or the negative electrode, or as an electrode catalyst for the positive electrode or the negative electrode. The battery may include a positive electrode including the above-mentioned CNT composite and a negative electrode not including the above-mentioned CNT composite, or the battery may include a negative electrode including the above-mentioned CNT composite and a positive electrode not including the above-mentioned CNT composite. Preferably, both the positive electrode and the negative electrode of the battery are electrodes including the above-mentioned CNT composite.

[0035] The battery may include an electrolyte. The electrolyte may be an aqueous electrolyte or a non-aqueous electrolyte. Examples of the aqueous electrolyte include sodium chloride aqueous solution, potassium chloride aqueous solution, calcium chloride aqueous solution, iron chloride aqueous solution, aluminum chloride aqueous solution, zinc chloride aqueous solution, nickel chloride aqueous solution, sodium sulfate aqueous solution, potassium sulfate aqueous solution, calcium sulfate aqueous solution, iron sulfate aqueous solution, aluminum sulfate aqueous solution, zinc sulfate aqueous solution, nickel sulfate aqueous solution, sodium hydroxide aqueous solution, potassium hydroxide aqueous solution, calcium hydroxide aqueous solution, zinc hydroxide aqueous solution, and sulfuric acid aqueous solution. The aqueous electrolyte may be neutral, acidic, or alkaline. The non-aqueous electrolyte is not particularly limited as long as it is an electrolyte containing an electrolyte and an organic solvent. The electrolyte may be, for example, LiClO 4 , LiPF 6 , LiAsF 6 , LiSbF 6 , LiBF 4 , LiCF 3 SO 3 , LiN(CF 3 SO 2 ) 2 , LiC(CF 3 SO 2 ) 3 , Li 2 B 10 Cl 10 , lithium salts of lower aliphatic carboxylic acids and LiAlCl 4 Examples of the organic solvent include aprotic polar solvents such as carbonates, ethers, esters, nitriles, amides, carbamates, sulfur-containing compounds, and fluorine-containing organic solvents obtained by introducing a fluorine group into these organic solvents.

[0036] The battery may include a separator between the positive electrode and the negative electrode, such as a glass filter, a cellulose separator, or a polyolefin-based porous film.

[0037] 3. Manufacturing method of CNT composite A method for producing a CNT composite according to one embodiment of the present invention is to produce a CNT composite having a length of 10 μm or more, a carbon purity of 90% or more, and a BET specific surface area of ​​600 m. 2 The method includes a fixation step of performing a reduction treatment on a solution containing single-walled CNTs having a molecular weight of at least 1000 nm and metal nanoparticles. For the CNTs and metal nanoparticles, the matters described in [1. CNT composite] above can be appropriately applied.

[0038] The above-mentioned fixing process allows the nanoparticles to be fixed on the surface of the CNTs without using a binder, which prevents the catalytic activity of the CNT composite from decreasing and the internal resistance from increasing due to the use of an insulating binder.

[0039] A CNT composite according to one embodiment of the present invention is a binderless CNT composite, and therefore the solution containing the CNTs and metal nanoparticles used in the above fixing step preferably does not contain a binder.

[0040] The method of the reduction treatment carried out in the above-mentioned immobilization step is not particularly limited. That is, the reduction treatment may be carried out by any method such as radiation reduction or chemical reduction. From the viewpoints of (i) the high permeability allows the reduction treatment to be carried out on a large scale, (ii) the reduction occurs simultaneously in multiple places, suppressing the coalescence of metal nanoparticles on the CNT surface and producing uniform metal nanoparticles, and (iii) being applicable to bulk materials or materials that are difficult to immobilize, the reduction treatment is preferably carried out by radiation reduction.

[0041] The radiation reduction may be carried out by irradiating with one or more types of radiation selected from, for example, alpha rays, beta rays, gamma rays, X-rays, electron beams, neutron beams, proton beams, deuterium beams, and the like. Among these, gamma rays and electron beams are preferred, and gamma rays are more preferred. The radiation dose is, for example, 10 to 100 kGy, and preferably 20 to 40 kGy. The frequency of the radiation to be irradiated is, for example, 10 17 ~10 22 The radiation reduction may be carried out, for example, at room temperature (10 to 30° C.).

[0042] The chemical reduction may be carried out by adding a known reducing agent. Examples of the reducing agent include thiourea, diethylthiourea, potassium borohydride, sodium borohydride, dimethylaminoborane, sodium hypophosphite, hydrazine, formaldehyde, lithium aluminum hydride, alcohol, citric acid, and ascorbic acid. The amount of the reducing agent added may be, for example, 1 to 100 moles per mole of the metal nanoparticles.

[0043] It is preferable to degas the solution before the reduction step. By degassing the solution, oxidation due to dissolved oxygen can be suppressed. Degassing may be performed, for example, in an argon atmosphere for about 10 to 30 minutes.

[0044] A method for producing a CNT composite according to one embodiment of the present invention may further include a step of dispersing and mixing CNTs and metal nanoparticles in a solvent, and a step of filtering and drying the solution that has been subjected to the reduction treatment.

[0045] Examples of the solvent for dispersing the CNTs and metal nanoparticles include, but are not limited to, water, toluene, 2-propanol, o-dichlorobenzene, tetrahydrofuran, and ethylene glycol. From the viewpoint of enabling radiation reduction, water is preferable. Not limited to these. The step of mixing the CNTs and metal nanoparticles in the solvent may be carried out, for example, at room temperature (10 to 30°C), and stirring may be carried out for about 1 to 24 hours. Furthermore, ultrasonic waves may be applied for 30 seconds to 240 minutes before and after stirring, as necessary.

[0046] The solution can be filtered, for example, using a membrane, etc. The solution can be dried by heating at 60 to 100° C. for 5 to 15 hours in a vacuum.

[0047] The CNT composite produced by the method for producing a CNT composite according to one embodiment of the present invention can be used to produce the above-mentioned electrode catalyst and battery electrode. Therefore, one embodiment of the present invention relates to a method for producing an electrode catalyst made of the above-mentioned CNT composite, or a method for producing a battery electrode made of the above-mentioned CNT composite.

[0048] 4. Manufacturing method of molded body A method for producing a molded article according to one embodiment of the present invention includes the steps of obtaining a carbon nanotube composite by the above-mentioned method for producing a carbon nanotube composite, and molding the carbon nanotube composite. As described above, the step of obtaining the carbon nanotube composite is performed binderless, but the step of molding the carbon nanotube composite may or may not use a binder.

[0049] In addition, in the step of forming the carbon nanotube composite, pressure may be applied. The pressure in the pressurization may be 5 to 20 MPa, or 10 to 15 MPa. Drying may be performed before or after the pressurization. Drying can be performed by heating and drying in a vacuum at 60 to 100°C for 5 to 15 hours, for example.

[0050] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. EXAMPLES

[0051] An embodiment of the present invention will now be described.

[0052] Example 1 A CNT composite in which platinum nanoparticles were immobilized on the CNT surface was produced by the following method. 1. 6.6 mL of 0.1 wt% CNT dispersion (product name: ZEONANO (registered trademark) SG101, manufactured by Zeon Corporation) and K 2 PtCl 4 A solution was obtained by dissolving 1.0 μmol of Sigma-Aldrich CNT in 70 μL of 2-propanol (1% v / v). The length of the CNTs used was 10 μm or more, the carbon purity was 99% or more, and the BET specific surface area was 600 m. 2 / g or more. 2. The solution was degassed under an argon atmosphere for 20 minutes. 3. The solution was irradiated with 20 kGy of gamma rays at room temperature. 4. Filtration was carried out using a 0.20 μm pore membrane. 5. After drying in vacuum at 80°C for 12 hours, a film-like CNT composite was obtained in which 1.75 wt % of Pt nanoparticles were fixed on the CNT surface.

[0053] Example 2 A CNT complex was obtained in the same manner as in Example 1, except that electron beams were irradiated at 20 kGy instead of gamma rays.

[0054] Example 3 Instead of gamma irradiation, sodium borohydride (NaBH 4 A CNT composite was obtained in the same manner as in Example 1, except that 10 μmol of

[0055] [Test 1. Transmission electron microscope (TEM) measurement] For the TEM measurement, the powder of the CNT composite of Examples 1, 2, and 3 dispersed in ethanol was dropped onto a Cu grid (without a support film, 200 mesh) and dried overnight under reduced pressure. The TEM used was a product name: U1003 manufactured by EM Japan. The accelerating voltage used was 200 kV.

[0056] The results of observation of each CNT composite by TEM are shown in FIG. 1. As shown in FIG. 1, Pt nanoparticles were observed on the surface of all the composites in Examples 1 to 3. The diameter of the nanoparticles in Examples 1 and 2 was approximately 1.7 nm. On the other hand, it was found that the Pt nanoparticles in Example 3 were larger than those in Examples 1 and 2. Therefore, the CNT composites produced by electron beam and gamma ray irradiation had relatively high dispersibility of Pt nanoparticles, whereas the CNT composites produced by irradiation with sodium borohydride (NaBH 4 ) It was shown that in the CNT composite prepared by reduction, the Pt nanoparticles tend to coalesce together.

[0057] [Test 2. Powder X-ray diffraction (PXRD) measurement] In order to investigate the crystal structure of the Pt nanoparticles formed on the surface of the CNT composite, PXRD measurement was performed by a reflection method. The PXRD measurement was performed using a SmartLab manufactured by Rigaku. For the measurement, powder separated by centrifuging the CNT composite of Example 1 was used. A sample was prepared by pressing the powder of the CNT composite onto a Si non-reflective sample plate, and the measurement was performed in the range of 5° to 70°.

[0058] The measurement results are shown in Figure 2. As shown in Figure 2, reflection peaks were observed in the Pt 111 and Pt 200 plane regions. This indicated that Pt nanoparticles were formed on the surface of the CNT composite. Furthermore, the crystallite size was calculated using the Scherrer equation in the following formula (1), resulting in a value of 1.7 nm, which was found to be similar to that observed with a transmission electron microscope (TEM) in Test 1.

[0059]

number

[0060] In formula (1), D is the crystallite size, K is the Scherrer constant, λ is the X-ray wavelength, β is the half-width, and θ is the Bragg angle.

[0061] [Test 3. X-ray absorption fine structure (XAFS) measurement] To investigate the local structure and electronic state of the generated Pt nanoparticles, 3 Absorption edge XAFS measurement was carried out. XAFS measurement was carried out using a Photon Factory BL-9A (trade name) manufactured by the High Energy Accelerator Research Organization. Measurement was carried out by the transmission method. Synchrotron radiation was monochromatized using a dual-spectra crystal on the Si (111) surface, and the energy was calibrated so that the energy of the midpoint of the absorption edge of the Pt foil was 11564 eV. A suitable amount of the CNT composite powder of Example 1 or Example 2 was mixed with boron nitride in an agate mortar for 30 minutes or more, and the mixture was molded into a pellet with a diameter of 10 mm to prepare a sample.

[0062] The results of the extended X-ray absorption fine structure (EXAFS) analysis of the obtained spectrum are shown in Figure 3. In Figure 3, "experiment" indicates the actual measured value of the sample, and "fitting" indicates the measured value. Analysis of the measurement results revealed that the average coordination number of Pt present at the first nearest neighbors of Pt was 5.5. This analysis result corresponds to the fact that the Pt nanoparticles have a diameter of 2 nm or less, and is data supporting the idea that the nanoparticles observed by TEM are in the same state throughout the sample.

[0063] The results of X-ray absorption near edge structure (XANES) analysis of the obtained spectrum are shown in Figure 4. The XANES analysis results in Figure 4 are a graph showing the oxidation state of Pt on the surface of the Pt nanoparticles. Figure 4 also shows a graph showing the bonding state of Pt contained in the Pt nanoparticles by EXAFS analysis. From the graph of the XANES analysis results in Figure 4, it can be seen that the peak intensities are as follows: Pt foil, the CNT composite of Example 2, the CNT composite of Example 1, PtO 2 This suggests that the Pt on the surface of the Pt nanoparticles immobilized on the CNT surface is oxidized to some extent, and that the average valence of Pt is greater than 0 and less than 2. In fact, in the EXAFS analysis results for the CNT composite shown in Figure 4, a peak was observed near 1.8 Å, which corresponds to the Pt-O bond, and this also indicates that the Pt nanoparticles were subjected to some degree of surface oxidation during sample preparation.

[0064] [Test 4. Electrochemical measurements] K 2 PtCl 4 A 3 wt% PtCNT composite was obtained in the same manner as in Example 1, except that the amount of Pt added was set to an amount such that Pt was 3 wt% in the CNT composite. Electrochemical measurements were performed using the 3 wt% PtCNT composite prepared on the positive electrode side, Pt on the negative electrode side, and Ag / AgCl as the reference electrode. A 0.5 mol / L aqueous sulfuric acid solution was used as the electrolyte, and the voltage was measured at 10 mVs in an air atmosphere. -1 For comparison, a 40 wt% Pt / C catalyst (trade name: 0.3 mg / cm) was used as the positive electrode. 2 Electrochemical measurements were performed using a 40% Platinum on Vulcan - Carbon Paper Electrode (purchased from Fuelcellstore).

[0065] The results of the electrochemical measurements are shown in Figure 5. As shown in Figure 5, a peak was observed at around 1.2 V (vs. Ag / AgCl) on the oxidation side, which indicates that the oxidation reaction of water (2H 2 O → O 2 +4H + +4e - ) was found to proceed. When a similar experiment was performed using Pt / C as a comparison, no activity was observed. Therefore, this difference in reactivity is considered to be specific to the CNT composite. Also, from FIG. 5, a peak rise was observed near 0.4 V (vs. Ag / AgCl) on the reduction side, indicating oxygen reduction activity. From the above, it was found that the CNT composite according to one embodiment of the present invention exhibits high catalytic activity, since a signal was observed on the higher potential side than the comparison 40 wt % Pt / C.

[0066] Example 4 A CNT composite in which gold nanoparticles were immobilized on the CNT surface was produced by the following method. HAuCl was added to 13.2 mL of 0.1 wt % CNT aqueous dispersion (product name: ZEONANO (registered trademark) SG101, manufactured by Zeon Corporation). 4 (trade name: chloroauric acid, manufactured by Tanaka Kikinzoku Co., Ltd.) was added in an amount of 1.0 μmol, and the mixture was cooled to 0° C. to obtain a dispersion. NaBH 4 Aqueous solution (NaBH 4 (10 μmol) was added and stirred at 0° C. for 1 hour. The obtained dispersion was filtered using a hydrophilic PTFE membrane filter (pore size 0.2 μm), washed with water and ethanol, and then air-dried for about 30 minutes. 168 μL of 2-propanol solution containing 0.5 wt % Nafion (registered trademark) was uniformly dropped onto the obtained CNT composite with a micropipette, and dried for about 15 minutes. Thereafter, the mixture was vacuum-dried at 80° C. for 12 hours to obtain a molded product containing a film-like CNT composite in which 3 wt % of Au nanoparticles were fixed on the CNT surface. The content of Au nanoparticles was a value calculated from ICP measurement.

[0067] Example 5 After vacuum drying, the mixture was sandwiched between stainless steel plates and pressurized with a hydraulic press at 10 MPa for about 10 to 30 seconds, and the same procedure as in Example 4 was carried out to obtain a molded body.

[0068] Example 6 A molded body was obtained in the same manner as in Example 4, except that the 2-propanol solution containing Nafion (registered trademark) was not added dropwise, and the molded body was sandwiched between stainless steel plates and pressurized with a hydraulic press at 10 MPa for approximately 10 to 30 seconds before vacuum drying.

[0069] Example 7 A molded body was obtained in the same manner as in Example 4, except that the 2-propanol solution containing Nafion (registered trademark) was not added dropwise, and after vacuum drying, the molded body was sandwiched between stainless steel plates and pressurized with a hydraulic press at 10 MPa for approximately 10 to 30 seconds.

[0070] Comparative Example 1 HAuCl 4 A molded body was obtained in the same manner as in Example 4, except that no addition was made and no dropwise addition of the 2-propanol solution containing Nafion (registered trademark) was made.

[0071] [Test 5. X-ray absorption fine structure (XAFS) measurement] To investigate the local structure and electronic state of the generated Au nanoparticles, Au L3 absorption edge XAFS measurements were performed. XAFS measurements were performed at the large-scale radiation facility SPring-8 BL14B2. Measurements were performed using the fluorescence method. Synchrotron radiation was monochromated using a dual-spectra crystal on the Si(111) surface, and the energy was calibrated so that the energy of the midpoint of the absorption edge of the Au foil was 11919 eV.

[0072] FIG. 6 shows the X-ray absorption near edge structure (XANES) spectrum obtained from the XAFS experiment. XANES is a graph showing information on the electronic state and structure of a substance. Measurements were performed on four samples (Examples 4 to 7) of CNT composites, which were formed by pressure molding and had or had not a binder. As a result, all the molded samples showed a spectrum similar to that of the reference Au foil, and therefore NaBH 4 It was found that gold ions were reduced to zero-valent gold nanoparticles by the method.

[0073] The results of extended X-ray absorption fine structure (EXAFS) analysis are shown in Figure 7. As with the results of XANES analysis, peaks indicating the presence of Au-Au bonds were observed at 2.7 to 3.2 Å in all samples.

[0074] [Test 6.1-Oxidation of Indanol] The oxidation reaction of 1-indanol was investigated. A reaction vessel (divided cell) separated by a diaphragm was used for the electrolysis reaction, and a Selemion (registered trademark) membrane was used as the diaphragm. The prepared CNT composite electrode was used as the anode, and a platinum electrode was used as the cathode. Ag / AgCl was used as the reference electrode, and constant potential electrolysis was performed at 0.4 V. A water / acetonitrile = 4:1 mixed solvent was used as the solvent, lithium perchlorate (0.2 mol / L) was used as the electrolyte, and potassium hydroxide (0.05 mol / L) was used as the base. The reaction vessel was filled with the solvent containing the electrolyte, and the anode and reference electrode were immersed in one side separated by a diaphragm, and the cathode was immersed in the other side. 1-indanol and base were added to the anode side to a specified concentration. The reaction was performed in air at room temperature for 6 hours, and the catalytic activity was evaluated by the catalyst turnover number (TON) relative to the total amount of gold on the electrode catalyst.

[0075] The results of the experiment are shown in Table 1. The results of a reference example in which the molded body of Example 4 was used but no voltage was applied are also shown. In Table 1, y indicates yes (present) and n indicates no (absent). a indicates that pressure was applied before vacuum drying, and y b indicates that pressing was performed after vacuum drying.

[0076] [Table 1]

[0077] When a reaction was carried out using a molded body made using Nafion (registered trademark) as a binder as an electrode catalyst, an air oxidation reaction proceeded, and 1-indanone, the oxidation reaction product of 1-indanol, was obtained with a TON of 450 (Example 4). The oxidation reaction did not proceed when an electrode not modified with gold nanoparticles was used (Comparative Example 1) or under conditions where no voltage was applied (Reference Example). This shows that both the presence of gold nanoparticles and the application of voltage are necessary for the reaction to proceed.

[0078] We also investigated the change in reactivity due to the addition of a pressurizing process. In Example 5, a molded body that was pressurized after vacuum drying was used as an electrode catalyst. As a result, the TON improved to 614. In Examples 6 and 7, a molded body produced without using Nafion (registered trademark) as a binder was used as an electrode catalyst to investigate the reaction. As a result, as shown in Example 6, when a molded body that was pressurized before vacuum drying was used as an electrode catalyst, it showed particularly high activity, and the TON improved to 1272. [Industrial Applicability]

[0079] One embodiment of the present invention can be suitably used as an electrode, an electrode catalyst, or a battery material.< / cnt>

Claims

1. Length is 10 μm or more, carbon purity is 90% or more, and BET specific surface area is 600 m 2 1. A binderless carbon nanotube composite comprising: single-walled carbon nanotubes having a molecular weight of 1000 nm or more; and metal nanoparticles fixed onto the single-walled carbon nanotubes.

2. 2. The carbon nanotube composite according to claim 1, wherein at least a portion of the surface of the metal nanoparticles is oxidized, and the average valence of the metal element on the oxidized surface is greater than 0 and less than 2.

3. 2. The carbon nanotube composite according to claim 1, wherein the content of the metal nanoparticles is 1 to 20% by weight, where the total weight of the carbon nanotube composite is taken as 100% by weight.

4. A molded article comprising the carbon nanotube composite according to claim 1 .

5. An electrode catalyst comprising the carbon nanotube composite of claim 1 .

6. A battery electrode comprising the carbon nanotube composite according to claim 1.

7. A battery comprising the electrode catalyst according to claim 5 or the battery electrode according to claim 6.

8. Length is 10 μm or more, carbon purity is 90% or more, and BET specific surface area is 600 m 2 13. A method for producing a binderless carbon nanotube composite, comprising: a fixation step of performing a reduction treatment on a solution containing single-walled carbon nanotubes having a molecular weight of 1000 to 10000 nanometers (µm) and metal nanoparticles.

9. The method for producing a carbon nanotube composite according to claim 8 , wherein at least a portion of the surface of the metal nanoparticles contained in the carbon nanotube composite is oxidized, and the average valence of the oxidized surface is greater than 0 and less than 2.

10. The method for producing a carbon nanotube composite according to claim 8 , wherein the reduction treatment is carried out by radiation reduction.

11. A step of obtaining a carbon nanotube composite by the method for producing a carbon nanotube composite according to any one of claims 8 to 10; and molding the carbon nanotube composite.

12. The method for producing a molded product according to claim 11 , wherein pressure is applied in the step of molding the carbon nanotube composite.

Citation Information

Patent Citations

  • Support-nanoparticle composite, catalyst containing the same, and method for producing the same

    JP2018538134A