Resin composition

The resin composition addresses the challenge of uniformly dispersing near-infrared emitting materials by using specific cation and anion species in silicone resin, enhancing dispersibility and fluorescence performance for medical devices.

JP2024144206APending Publication Date: 2024-10-11MITSUBISHI CHEM CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024037426
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-11
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing resin compositions for medical applications face challenges in uniformly dispersing near-infrared emitting materials, such as near-infrared fluorescent materials, due to aggregation and concentration quenching, which affects their fluorescence performance and suitability for medical devices.

Method used

A resin composition containing near-infrared emitting materials with specific cation and anion species, formulated to suppress aggregation and concentration quenching, using silicone resin and a counter ion to enhance dispersibility, allowing for uniform distribution within the resin.

Benefits of technology

The resin composition achieves high dispersibility and consistent brightness of near-infrared fluorescence, suitable for medical devices, reducing the burden of precision work and enabling accurate visualization of medical devices within the body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144206000025
    Figure 2024144206000025
  • Figure 2024144206000026
    Figure 2024144206000026
  • Figure 2024144206000027
    Figure 2024144206000027
Patent Text Reader

Abstract

To provide a resin composition which can uniformly and highly disperse a near-infrared light-emitting material such as a near-infrared fluorescent material in a resin.SOLUTION: A resin composition contains a near-infrared light-emitting material, and a silicone resin, wherein the near-infrared light-emitting material is one or more kinds of compounds composed of cationic species represented by the following chemical formula (1) and anionic species.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition. More specifically, the present invention relates to a resin composition imparted with a function of emitting light such as fluorescence or phosphorescence uniformly and evenly, and to a molded article containing the resin composition. [Background technology]

[0002] The method of remotely operating small, lightweight devices by introducing them into places that cannot be touched directly is used in a wide range of fields, including construction and medicine. In order to confirm the location of the inserted device, there is a method of giving the device itself a function to notify its location. Specific methods include spontaneous devices such as electronic devices that emit electromagnetic waves, and devices that supplement external measuring devices by adding luminescent or radiopaque substances. The latter are easy to process into small, lightweight devices due to their simplicity, and are widely used in fields that require precise operation, such as the medical field. Luminescent materials include fluorescent materials and phosphorescent materials.

[0003] Specific examples of medical devices used in the medical field include medical devices that are used while embedded in a living body, such as shunt tubes, catheters, and stents, and it is important to know how to confirm their position in the living body from outside the living body. Currently, the main method for visualizing medical devices in the living body is to make the medical device contain a radiopaque substance (see, for example, Patent Documents 1 and 2). For example, the position in the living body of a medical device made of a resin containing a radiopaque substance can be confirmed based on an X-ray image captured by irradiating it with X-rays.

[0004] Another method is to include a near-infrared fluorescent material, which is one of the luminescent substances, in the medical device. In particular, the near-infrared wavelength region is known to have the following characteristics: it is invisible to the naked human eye, it has little effect on the living body, and it has high biological permeability through the skin, etc. These characteristics can be utilized by including a near-infrared fluorescent material in the medical device itself. For example, a system has been disclosed in which a medical device such as a shunt tube is included with a near-infrared fluorescent material, and the position of the medical device embedded in the living body is confirmed by irradiating the medical device with near-infrared light from outside the living body (see, for example, Patent Document 3). Near-infrared light has a smaller effect on the living body than X-rays, and therefore the medical device can be visualized in the living body more safely.

[0005] Near-infrared fluorescent materials include inorganic and organic fluorescent materials. Inorganic materials require rare earth elements, which raises concerns about resources and costs, while organic fluorescent materials are relatively easy to synthesize and have characteristics such as easy wavelength adjustment. In recent years, organic near-infrared fluorescent materials with various structures have been developed. A representative example is indocyanine green (ICG), a cyanine dye. ICG has been approved for medical use by the U.S. Food and Drug Administration (FDA) and is widely used clinically in liver function tests and fundus angiography.

[0006] Another fluorescent material used for medical purposes similar to ICG is methylene blue (MB). MB is known as a treatment for methemoglobinemia, but it is also used to stain colorectal tumors during chromoendoscopy.

[0007] Squarium dyes (SQs), which are analogues of cyanine dyes, have a unique structure with a squaric acid moiety in the center and are zwitterionic, and are being studied as sensitizing dyes for dye-sensitized solar cells (DSSCs) (Non-Patent Document 1).

[0008] Xanthene dyes are controlled by functional groups attached to the xanthene moiety, and rhodamine modified with an amino group can be used as a near-infrared fluorescent dye. This dye is also expected to be applied to DSSCs, similar to the squarylium dyes mentioned above (Non-Patent Document 2).

[0009] Boron complexes have been attracting attention in recent years. Many dyes have been reported that are crosslinked and fixed by boron to suppress non-radiative deactivation, resulting in high quantum efficiency. Boron complexes are further differentiated by their skeletons, and azo-boron complex compounds with excellent light resistance and heat resistance (Non-Patent Document 3, Patent Document 4) and BODIPY dyes with a boron-dipyrromethene skeleton, which are boron complexes of π-conjugated compounds known for their high luminescence quantum yield, are known (Non-Patent Document 4). The latter BODIPY dyes have been disclosed as dyes with heterocycles in the BODIPY skeleton that are controlled to emit near-infrared fluorescence for medical use (Non-Patent Document 5, Patent Document 5).

[0010] BODIPY dyes have been investigated as biomarkers for labeling biological molecules such as nucleic acids and proteins, as well as tumor tissues (Non-Patent Document 6). For this purpose, boron complexes of diketopyrrolopyrrole (DPP) derivatives have also been reported (Non-Patent Document 7).

[0011] On the other hand, examples of applications to resin compositions include a case in which a dye having an ICG skeleton was prepared in an acetonitrile solution with poly(methyl methacrylate) and processed into a coating film (Patent Document 6), a case in which a siloxane-containing BODIPY dye in which an organosiloxanyl group was introduced via an alkylene group was copolymerized into a silicone resin (Patent Document 7), and a case in which it was mixed with a solvent (Patent Document 8).

[0012] As examples of mixing a BODIPY dye into a resin like Patent Document 6, Patent Document 9 discloses an optical filter, and Patent Document 10 discloses a color conversion material.

[0013] As described above, there are several cases in which a dye has been added to a resin composition. However, there are not many that can be used as a near-infrared emitting material, such as a near-infrared fluorescent material for medical applications. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] JP 2000-060975 A [Patent Document 2] Special Publication No. 2008-541987 [Patent Document 3] JP 2012-115535 A [Patent Document 4] JP 2011-162445 A [Patent Document 5] Patent No. 5177427 [Patent Document 6] Special Publication No. 2021-512748 [Patent Document 7] JP 2013-060399 A [Patent Document 8] US Patent Application Publication No. 2013 / 0249137 [Patent Document 9] US Patent Application Publication No. 2013 / 0252000 [Patent Document 10] JP 2011-241160 A [Patent Document 11] International Publication No. 2015 / 022977 [Non-patent literature]

[0015] [Non-Patent Document 1] Burke, A., et al., (2007). "A novel blue dye for near-IR 'dye-sensitized' solar cell applications.", Chemical Communications, 3, 234-236, 2007 [Non-Patent Document 2] Guillen, E., et al., "Photovoltaic performance of nanostructured zinc oxide sensitised with xanthene dyes.", Journal of Photochemistry and Photobiology A: Chemistry, 200(2-3), 364-370, 2008 [Non-Patent Document 3] Yoshino, J., et al., "Intensely fluorescent azobenzenes: synthesis, crystal structures, effects of substituents, and application to fluorescent vital stain.", Chemistry-A European Journal, 16(17), 5026-5035, 2010 [Non-Patent Document 4] Tomimori, Y., et al., "Synthesis of π-expanded O-chelated boron-dipyrromethene as an NIR dye.", Tetrahedron, 67(18), 3187-3193, 2011 [Non-Patent Document 5] Gorman, A., et al., "In vitro demonstration of the heavy-atom effect for photodynamic therapy.", Journal of the American Chemical Society, 126(34), 10619-10631, 2004 [Non-Patent Document 6] Zhu, T., et al., "A novel amphiphilic fluorescent probe BODIPY-O-CMC-cRGD as a biomarker and nanoparticle vector." RSC advances, 8(36), 20087-20094, 2018 [Non-Patent Document 7] Fischer, GM, et al., "Near-infrared dyes and fluorophores based on diketopyrrolopyrroles.", Angewandte Chemie Intrernational Edition, 46(20), 3750-3753, 2007 [Non-Patent Document 8] Funchien, P., et al., "A highly efficient near infrared organic solid fluorophore based on naphthothiadiazole derivatives with aggregation-induced emission enhancement for a non-doped electroluminescent device." Chemical Communications, 56(46), 6305-6308, 2020 Summary of the Invention [Problem to be solved by the invention]

[0016] For example, the siloxane-containing BODIPY dye described in Patent Document 7 dissolves in silicone resins used for medical applications, but the fluorescent wavelength is outside the near-infrared region suitable for medical applications. In addition, the resin composition of Patent Document 8 has safety issues because the solvent may remain in the resin. In addition, Patent Documents 7, 8, 9, and 10 do not describe near-infrared fluorescent materials, nor do they describe applications to medical applications.

[0017] The ICG in Patent Document 6 is also obtained by drying a solution for a certain period of time, and when considering its application in medical applications, active removal of the solvent by drying and processing without a solvent are required.

[0018] In recent years, a case has been disclosed in which the above-mentioned boron complexes are melt-kneaded into resin as near-infrared fluorescent materials (Patent Document 11), and products using these materials are beginning to appear on the market. However, their concentration is limited to 400 ppm relative to the resin. This is because as the concentration of the fluorescent material increases, the interaction between the fluorescent materials causes a phenomenon called concentration quenching, which causes attenuation of fluorescence due to aggregation.

[0019] These fluorescent materials have an extended conjugated structure and have strong intermolecular interactions such as π-π interactions, which makes them prone to aggregation. Therefore, when the concentration is increased, there is a risk of concentration quenching easily occurring.

[0020] In particular, the dye in Patent Document 11 has excellent heat resistance and fluorescence yield due to its rigid structure based on aromatic rings, and boasts high performance, but the interaction between the dye molecules is stronger, making it difficult to redisperse it in a kneader with low shear force. If the shear force is increased to knead the dye, the effects on other materials, such as a decrease in the molecular weight of the resin, cannot be ignored, and the intended physical properties are deviated from those intended, making it difficult to apply the dye to products.

[0021] In recent years, fluorescent materials that utilize aggregation-induced emission, which increases luminescence through aggregation, have been reported (Non-Patent Document 8), but these are still in the molecular design stage for organic fluorescent light-emitting diodes, and have not yet been deployed in medical applications.

[0022] The present inventors have studied and developed a new near-infrared light-emitting material such as a fluorescent material, and have succeeded in quickly spreading the material in the resin and stabilizing it in a uniform state by improving the dispersibility in the resin while following the proven structure of ICG. One aspect of the present invention provides a resin composition capable of uniformly and highly dispersing a near-infrared light-emitting material such as a near-infrared fluorescent material in the resin. [Means for solving the problem]

[0023] [1] A resin composition comprising a near-infrared light-emitting material and a silicone resin, The near-infrared emitting material is one or more compounds composed of a cation species and an anion species represented by the following chemical formula (1): [ka] In chemical formula (1), l is 1 or 2; X is selected from the group consisting of a single bond, a carbon atom, a nitrogen atom, an oxygen atom, a phosphorus atom, and a sulfur atom; m is 1 or 2; R1 is an aliphatic hydrocarbon group or an aromatic hydrocarbon group, which may form a ring together with another R1, at least one hydrogen in the aliphatic hydrocarbon group or aromatic hydrocarbon group may be substituted with a halogen, and two R1 may be the same or different; n is 1 to 4, and two n's may be the same or different. R2 is a linear, branched or cyclic aliphatic hydrocarbon group, and the two R2 may be the same or different; R3, R4, R5, and R6 each independently represent an alkyl group which may have a substituent; A is an aromatic hydrocarbon group which may have a substituent, or an aromatic heterocyclic group which may have a substituent. [2] The resin composition according to [1], wherein the chemical formula (1) is the following chemical formula (2): [ka] In chemical formula (2), l is 1 or 2; X is selected from the group consisting of a single bond, a carbon atom, a nitrogen atom, an oxygen atom, a phosphorus atom, and a sulfur atom; m is 1 or 2; R7 is an aliphatic hydrocarbon group or an aromatic hydrocarbon group, in which at least one hydrogen atom may be substituted with a halogen atom; o is 1 to 5; When o is 2 to 5, R7 may form a ring together with other R7. R1 is an aliphatic hydrocarbon group or an aromatic hydrocarbon group, which may form a ring together with other R1s, and at least one hydrogen in the aliphatic hydrocarbon group or the aromatic hydrocarbon group may be substituted with a halogen; n is 1 to 4, and two n's may be the same or different. R2 is a linear, branched or cyclic aliphatic hydrocarbon group, and the two R2's may be the same or different. [3] The resin composition according to [1] or [2], wherein in the chemical formula (1), X is selected from the group consisting of a single bond, a nitrogen atom, and an oxygen atom. [4] The resin composition according to any one of [1] to [3], wherein in the chemical formula (1), R2 is an aliphatic hydrocarbon group having 1 to 6 carbon atoms. [5] The resin composition according to any one of [1] to [4], wherein the anion species is a counter ion containing boron or phosphorus, or a halide ion. [6] The resin composition according to any one of [1] to [5], wherein the near-infrared light emitting material is a near-infrared fluorescent material. [7] The cationic species has the following chemical formula: [ka] The resin composition according to any one of [1] to [6], wherein the compound is one or more compounds selected from the following: [8] The resin composition according to any one of [1] to [7], wherein the silicone resin contains silicone oil. [9] The resin composition according to any one of [1] to [8], wherein the silicone resin comprises an addition polymerization type silicone resin.

[10] The resin composition according to any one of [1] to [9], further comprising a radiopaque substance.

[11] The resin composition according to any one of [1] to

[10] , which is used as a medical material.

[12] A molded article comprising the resin composition according to any one of [1] to

[11] .

[13] The molded article according to

[12] , at least a part of which is a medical device for use inside a patient's body. Effect of the Invention

[0024] According to one aspect of the present invention, it is possible to provide a resin composition capable of uniformly and highly dispersing a near-infrared light emitting material, such as a near-infrared fluorescent material, in the resin. [Brief description of the drawings]

[0025] [Figure 1] FIG. 1 is a diagram showing the results of measuring the luminance of the resin composition of Example 1-1. [Diagram 2] FIG. 1 is a diagram showing the results of measuring the luminance inside the molded body of Example 1-2. [Diagram 3] FIG. 13 is a diagram showing the results of measuring the brightness of the edge portion of the molded article of Example 1-2. [Figure 4] FIG. 1 is a diagram showing the results of measuring the luminance of the molded article of Example 2-1. [Diagram 5] FIG. 1 is a diagram showing the results of measuring the luminance of the molded article of Comparative Example 2-1. [Figure 6] FIG. 13 is a diagram showing the results of measuring the luminance of the molded body of Comparative Example 2-2. [Figure 7] FIG. 13 is a diagram showing the results of measuring the luminance of the molded article of Example 2-2. [Figure 8] FIG. 13 is a diagram showing the results of measuring the luminance of the molded article of Example 2-3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] One embodiment of the present invention will be described in detail below. In this specification, unless otherwise specified, "A to B" indicating a numerical range means "A or more and B or less."

[0027] A resin composition according to one embodiment of the present invention is a resin composition containing a near-infrared light-emitting material having high dispersibility in a silicone resin and a silicone resin.

[0028] The near-infrared light emitting material contained in the resin composition according to one embodiment of the present invention can be appropriately selected and used in consideration of the product quality required for a molded article obtained from the resin composition, the type of resin to be mixed, etc. The near-infrared light emitting material may be a near-infrared fluorescent material or a near-infrared phosphorescent material.

[0029] Since the resin composition containing the near-infrared light emitting material and the molded article obtained therefrom can be excited and detected by invisible light in the near-infrared region, the excitation light and the emitted light can be detected without changing the color tone of the biological tissue, etc. In addition, the transmittance to biological tissue is higher than that of visible light, making it possible to clearly visualize deep inside the living body, and it is suitable, for example, as a material for medical devices to be used in the living body.

[0030] Specifically, the near-infrared light-emitting material contained in the resin composition according to one embodiment of the present invention is one or more compounds composed of a cation species and an anion species represented by the following chemical formula (1).

[0031] [ka]

[0032] In chemical formula (1), l is 1 or 2.

[0033] In the chemical formula (1), X is selected from the group consisting of a single bond, a carbon atom, a nitrogen atom, an oxygen atom, a phosphorus atom, and a sulfur atom, and m is 1 or 2.

[0034] In terms of suppressing aggregation of the near-infrared emitting material and making it difficult for concentration quenching to occur, X is preferably selected from the group consisting of a single bond, a nitrogen atom, and an oxygen atom.

[0035] In the chemical formula (1), R1 is an aliphatic hydrocarbon group or an aromatic hydrocarbon group, and may form a ring together with another R1, and at least one hydrogen in the aliphatic hydrocarbon group or aromatic hydrocarbon group may be substituted with a halogen. The two R1 may be the same or different. Examples of the halogen include fluorine, chlorine, bromine, and iodine.

[0036] From the viewpoint of solubility, the aliphatic hydrocarbon group preferably has 1 to 20 carbon atoms, more preferably 1 to 18 carbon atoms, and even more preferably 1 to 14 carbon atoms. The aliphatic hydrocarbon group may be a linear, branched, or cyclic aliphatic hydrocarbon group. Examples of the aliphatic hydrocarbon group include alkyl groups such as methyl, ethyl, isopropyl, and t-butyl, and cycloalkyl groups such as cyclohexyl.

[0037] From the viewpoint of solubility, the aromatic hydrocarbon group preferably has a carbon number of 6 to 20, more preferably has a carbon number of 6 to 18, and further preferably has a carbon number of 6 to 14. Examples of the aromatic hydrocarbon group include aryl groups such as a phenyl group, a naphthyl group, and a phenanthryl group.

[0038] In the chemical formula (1), n ​​is 1 to 4, and may be 2 or 3. The two n's may be the same or different.

[0039] In the chemical formula (1), R2 is a linear, branched or cyclic aliphatic hydrocarbon group, and the two R2's may be the same or different.

[0040] In terms of solubility, R2 is preferably an aliphatic hydrocarbon group having 1 to 12 carbon atoms, more preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms, and even more preferably an aliphatic hydrocarbon group having 1 to 8 carbon atoms. Examples of the aliphatic hydrocarbon group having 1 to 6 carbon atoms include alkyl groups such as a methyl group, an ethyl group, an isopropyl group, and an ethylhexyl group, and cycloalkyl groups such as a cyclohexyl group.

[0041] In the chemical formula (1), R3, R4, R5, and R6 are each independently an alkyl group which may have a substituent. Examples of the substituent include a methyl group and an ethyl group. The number of the substituent may be one or more.

[0042] The carbon number of the alkyl group of R3, R4, R5, and R6 may be 1 to 6, and preferably 1 to 4. Examples of the alkyl group of R3, R4, R5, and R6 include a methyl group, an ethyl group, and an isopropyl group.

[0043] In the chemical formula (1), A is preferably an aromatic hydrocarbon group which may have a substituent, or an aromatic heterocyclic group which may have a substituent. Examples of the substituent include a phenyl group, a naphthyl group, a pyridyl group, a furyl group, and a thienyl group. The number of the substituent may be one or more.

[0044] Specific examples and preferred embodiments of the aromatic hydrocarbon group in A in the chemical formula (1) are the same as those of the aromatic hydrocarbon group in R1 in the chemical formula (1).

[0045] The aromatic heterocyclic group for A in chemical formula (1) preferably has 6 to 20 carbon atoms, more preferably has 6 to 18 carbon atoms, and further preferably has 6 to 16 carbon atoms. Examples of the aromatic heterocyclic group include heteroaryl groups such as a thienyl group, a furyl group, and a pyridyl group.

[0046] An example of chemical formula (1) is the following chemical formula (2).

[0047] [ka]

[0048] In the chemical formula (2), l is preferably 1 or 2.

[0049] In the chemical formula (2), X is preferably selected from the group consisting of a single bond, a carbon atom, a nitrogen atom, an oxygen atom, a phosphorus atom, and a sulfur atom, and more preferably selected from the group consisting of a single bond, a nitrogen atom, and an oxygen atom. m is preferably 1 or 2.

[0050] In chemical formula (2), R7 is preferably the aliphatic hydrocarbon group or aromatic hydrocarbon group, and may form a ring together with other R1, and at least one hydrogen in the aliphatic hydrocarbon group or aromatic hydrocarbon group may be substituted with a halogen. o may be 1 to 5, 2 to 4, or 2 to 3. When o is 2 to 5, R7 may form a ring together with other R7.

[0051] In the chemical formula (2), R1 is preferably an aliphatic hydrocarbon group or an aromatic hydrocarbon group, and may form a ring together with other R1, and at least one hydrogen in the aliphatic hydrocarbon group or aromatic hydrocarbon group may be substituted with a halogen. Examples of the halogen include fluorine, chlorine, bromine, and iodine. n may be 1 to 4, or 2 to 3. Two n's may be the same or different.

[0052] Specific examples and preferred embodiments of R1 in the chemical formula (2) are the same as those of R1 in the chemical formula (1).

[0053] In chemical formula (2), R2 is preferably a linear, branched or cyclic aliphatic hydrocarbon group, and more preferably a linear, branched or cyclic aliphatic hydrocarbon group having 1 to 6 carbon atoms. Specific examples and preferred aspects of R2 in chemical formula (2) are the same as those of R2 in chemical formula (1).

[0054] The near-infrared emitting material contained in the resin composition according to one embodiment of the present invention has an ICG-based structure, which is an aliphatic conjugated system with a small π-π interaction, as its main skeleton, compared to other emitting materials such as fluorescent materials. By designing the central and terminal substituents of the near-infrared emitting material and further selecting the type of counter ion, the near-infrared emitting material has a high dispersibility in the resin. The high dispersibility allows the material to spread quickly in the resin and settle into a uniform state, suppressing concentration quenching at high concentrations and suppressing unevenness due to local aggregation that occurs even at low concentrations.

[0055] Near-infrared emitting materials, such as high-concentration near-infrared fluorescent materials, can be used as masterbatches, which can reduce costs even for medical parts that are produced in small quantities and in a wide variety of products.

[0056] Furthermore, a molded product processed from a near-infrared emitting material such as a uniform near-infrared fluorescent material has a constant brightness throughout, so that its shape can be displayed accurately, contributing to reducing the burden when performing precision work.

[0057] In addition, since the near-infrared light-emitting material contained in the resin composition according to one embodiment of the present invention has a structure similar to that of the proven ICG, a molded article containing the resin composition can be used as is in conventional medical devices, and therefore, it is expected to lower the hurdle for introducing a molded article containing the resin composition for medical use.

[0058] The cationic species has the following chemical formula: [ka] It is preferable that the compound is one or more compounds selected from the following:

[0059] The anionic species is preferably a boron or phosphorus containing counterion, or a halide ion.

[0060] The counter ions are expected to delocalize the ionicity of the near-infrared emitting material, thereby suppressing aggregation between the emitting materials and the resulting quenching. Therefore, bulky counter ions are preferable. The counter ions are preferably inorganic or organic counter ions other than halogen. Examples of preferable counter ions include bulky organic counter ions such as tetraphenylborate, tetrakis(pentafluorophenyl)borate, tetrakis(4-fluorophenyl)borate, tetraphenylborate, tetrakis[3,5-bis-(trifluoromethyl)phenyl]borate, tetrakis[3,5-bis-(1,1,1,3,3,3-hexafluoro-2-methoxy-2-propyl)phenyl]borate, and tetrakis[perfluoro-tert-butoxy]aluminate; and inorganic counter ions such as tetrafluoroborate and hexafluorophosphate.

[0061] An example of the above halide ion is the fluoride ion (F - ), chloride ion (Cl - ), bromide ion (Br - ), iodide ion (I - ) etc.

[0062] (Silicone resin) The resin composition according to one aspect of the present invention includes a silicone resin. This composition allows a near-infrared light-emitting material such as a near-infrared fluorescent material to be uniformly and highly dispersed. The silicone resin may be one type or two or more types.

[0063] The content of the silicone resin is preferably in the following range from the viewpoint of ensuring mechanical properties. Specifically, the content of the silicone resin is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, relative to 100% by mass of the resin composition. Furthermore, the content of the silicone resin is preferably in the following range from the viewpoint of ensuring radiopacity. Specifically, the content of the silicone resin is preferably 99% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less, relative to 100% by mass of the resin composition.

[0064] The silicone resin preferably contains silicone oil from the viewpoint of improving the affinity between the near-infrared light emitting material and the silicone resin and thus improving the uniformity. Also, by dissolving the near-infrared light emitting material in the silicone oil in advance, the silicone resin becomes easier to handle than powdered silicone resin.

[0065] In addition, the silicone resin preferably includes an addition polymerization type silicone resin. In particular, an addition polymerization type silicone resin using a platinum catalyst is preferable in terms of having fewer impurities and excellent cleanliness than a polycondensation type silicone resin. For materials that come into direct contact with the body, such as medical and health care, cleanliness is important because it can reduce the impact on the body. In fact, the current situation is that the majority of medical grade silicone resins are addition polymerization type silicone resins.

[0066] (Silicone oil) Examples of silicone oils include straight silicone oils such as methylphenyl silicone oil, dimethyl silicone oil, and methylhydrogen silicone oil, and modified silicone oils. Modified silicone oils are silicone oils in which an organic group other than a methyl group and a phenyl group (hereinafter also referred to as a "modified group") is introduced into a part of the silicon atoms of straight silicone oils. Examples of the modified group include a chlorophenyl group, a methylstyrene group, a long-chain alkyl group (e.g., an alkyl group having 2 to 18 carbon atoms), a polyether group, a carbinol group, an aminoalkyl group, an epoxy group, a (meth)acryloyl group, and a higher fatty acid ester group. Among them, from the viewpoint of achieving both non-reactivity and affinity with the near-infrared light-emitting material, the modified group of the modified silicone oil is preferably a methylphenyl group, a long-chain alkyl group, a polyether group, or a higher fatty acid ester group. The resin composition according to one aspect of the present invention may contain one type of silicone oil, or may contain two or more types of silicone oils.

[0067] As the silicone oil, commercially available products can be used. Examples of commercially available silicone oils include "KF-54", "KF-96", "KF-50", "KF-56", and "KF-6016" (all manufactured by Shin-Etsu Chemical Co., Ltd.), "TSF451", "TSF4421", "TSF4440", "TSF4450", and "TSF410" (all manufactured by Momentive Performance Materials), "Fluid47" (manufactured by Rhoneplan (France)), "SH200", "SH510", "SH550", "SH710", "DC200", "ST-114PA", and "FZ209" (all manufactured by Dow Corning Toray Co., Ltd.).

[0068] (Silicone resin other than silicone oil) The silicone resin may be an addition-curing silicone resin. The main components of addition-curing silicone resins that are primarily used in medical applications are polysiloxane having an alkenyl group as the main component, hydrogen polysiloxane as a crosslinking agent, a platinum catalyst, and a reaction control agent.

[0069] The polysiloxane having an alkenyl group preferably contains two or more alkenyl groups in one molecule. Specifically, the silicone resin preferably contains at least two alkenyl-containing polysiloxane units represented by the following formula (4) in the molecule. The polysiloxane having an alkenyl group may be linear, branched, or cyclic. One of these may be used alone, or two or more may be used in any ratio and combination. (R8) a (R9) b SiO 〔(4-a-b) / 2〕 (4)

[0070] In the above formula (4), R8 represents an alkenyl group, and R9 represents a substituted or unsubstituted monovalent aliphatic hydrocarbon group or aromatic hydrocarbon group not containing an aliphatic carbon-carbon unsaturated bond, an alkoxy group, or a hydroxyl group. a is an integer of 1 to 3, and preferably 1. b is an integer of 0 to 2. However, a+b is an integer of 1 to 3. When a is 2 or 3, multiple R8s may be the same or different. When b is 2, multiple R9s may be the same or different.

[0071] The alkenyl group R8 contained in the polysiloxane is preferably an alkenyl group having 2 to 8 carbon atoms, such as a vinyl group, an allyl group, a butenyl group, or a pentenyl group, and more preferably a vinyl group.

[0072] Examples of the aliphatic or aromatic hydrocarbon group of R9 in the above formula (4) include monovalent aliphatic or aromatic hydrocarbon groups having 1 to 20 carbon atoms, such as alkyl groups such as methyl and ethyl groups, cycloalkyl groups such as cyclohexyl groups, aryl groups such as phenyl groups, and aralkyl groups such as 2-phenylethyl groups. Methyl, ethyl, and phenyl groups are preferred. When light resistance (UV resistance) is required, R9 is more preferably a methyl group. R9 may be an alkoxy group or hydroxyl group having 1 to 8 carbon atoms, but the content of the alkoxy group and the hydroxyl group is preferably 10% by mass or less of the polysiloxane from the viewpoints of the storage stability of the resin composition according to one embodiment of the present invention and the dimensional stability of the molded product.

[0073] On the other hand, from the viewpoint of affinity with the near-infrared emitting material, polysiloxane containing a siloxane monomer containing a polar group may be used, and the polar group preferably contains an oxygen element, specifically, a hydroxyl group, a higher fatty acid ester group, a carboxyl group, a ketone group, a furanyl group, etc. The shape may be selected according to the situation, such as a chain shape or a ring shape. Specific examples include MCS-VX16, a polyethylene glycol trimer at both ends, and MCS-VF14, a tetrahydrofuranyl ring at both ends, both of which are sold by Gelest.

[0074] One of the preferred forms includes, as the polysiloxane, a linear polyalkylsiloxane containing an alkenyl group at both ends, and / or a linear polyalkylsiloxane having both ends blocked with trialkylsilyl groups and containing an alkenyl group in the side chain. Examples of the linear polyalkylsiloxane containing an alkenyl group at both ends include polydimethylsiloxane blocked with dimethylvinylsilyl groups at both ends, and a dimethylsiloxane-diphenylsiloxane copolymer blocked with dimethylvinylsilyl groups at both ends. Examples of the linear polyalkylsiloxane blocked with trialkylsilyl groups at both ends and containing an alkenyl group in the side chain include polyvinylmethylsiloxane blocked with trimethylsilyl groups at both ends, and a vinylmethylsiloxane-dimethylsiloxane copolymer blocked with trimethylsilyl groups at both ends.

[0075] The viscosity of the linear polyalkylsiloxane at 25°C is usually 500,000 mPa·s or less, preferably 50,000 mPa·s or less, and usually 5 mPa·s or more, preferably 10 mPa·s or more. If the viscosity of the linear polyalkylsiloxane is equal to or less than the upper limit, the viscosity of the resin composition according to one embodiment of the present invention can be suppressed from increasing, and the resin composition has excellent handleability. If the viscosity of the linear polyalkylsiloxane is equal to or less than the lower limit, a uniform cured product tends to be difficult to obtain.

[0076] The alkenyl group content per unit mass of the linear polyalkylsiloxane is usually 0.01 mmol / g or more, preferably 0.02 mmol / g or more, and usually 3 mmol / g or less, preferably 1 mmol / g or less. If the alkenyl group content is equal to or more than the lower limit, the resin composition according to one embodiment of the present invention exhibits a sufficient curing reaction rate, and if it is equal to or less than the upper limit, a more uniform molded product tends to be obtained.

[0077] Here, the alkenyl group content of the linear polyalkylsiloxane is 1 It can be calculated from the ratio of the signal intensity (peak area) of the alkenyl group to the signal intensity (peak area) of the internal standard reagent in the H-NMR spectrum, and the weighed values ​​of the linear polyalkylsiloxane and the internal standard reagent when preparing the NMR measurement sample.

[0078] Commercially available products of polydimethylsiloxanes blocked at both ends with dimethylvinylsilyl groups include DMS-V00, DMS-V03, DMS-V05, DMS-V21, DMS-V22, DMS-V25, DMS-V31, DMS-V33, DMS-V35, DMS-V41, DMS-V42, DMS-V46, and DMS-V51 (all manufactured by Gelest).

[0079] Commercially available products of dimethylsiloxane-diphenylsiloxane copolymers capped at both ends with dimethylvinylsilyl groups include PDV-0325, PDV-0331, PDV-0341, PDV-0346, PDV-0525, PDV-0535, PDV-0541, PDV-1625, PDV-1631, PDV-1635, PDV-1641, PDV-2331, and PDV-2335 (all manufactured by Gelest).

[0080] Commercially available trimethylsilyl-blocked vinylmethylsiloxane-dimethylsiloxane copolymers include VDT-123, VDT-127, VDT-131, VDT-153, VDT-431, VDT-731, and VDT-954 (all manufactured by Gelest Corporation).

[0081] These may be used alone or in any combination and ratio of two or more.

[0082] (Hydrogen polysiloxane) When an addition-curable silicone resin is used as the silicone resin in the resin composition according to one embodiment of the present invention, from the viewpoints of ensuring mechanical properties such as tensile strength and improving affinity with the near-infrared light-emitting material, it is preferable that the addition-curable silicone resin contains a hydrogen polysiloxane having a hydrogen atom bonded to a silicon atom.

[0083] For example, hydrogen polysiloxanes that act as crosslinkers having hydrogen atoms bonded to silicon atoms at both ends can be used to improve mechanical properties. In addition, those that contain polar groups in the molecule can be used to improve affinity with near-infrared emitting materials. These properties can be imparted to one polysiloxane, or multiple polysiloxanes that have any of these properties can be used.

[0084] The content of hydrogen atoms bonded to silicon atoms per unit mass of the hydrogen polysiloxane is usually 0.01 mmol / g or more, preferably 0.02 mmol / g or more, and usually 3 mmol / g or less, preferably 1 mmol / g or less. If the hydrogen atom content is equal to or more than the lower limit, the resin composition according to one embodiment of the present invention exhibits a sufficient curing reaction rate, and if it is equal to or less than the upper limit, a more uniform molded product tends to be obtained.

[0085] The content of hydrogen polysiloxane is preferably in the following range from the viewpoint of hardness of the addition curing silicone resin. Specifically, the content of hydrogen polysiloxane is preferably 0.01 or more per alkenyl group contained in the addition curing silicone resin, more preferably 0.05 or more, and even more preferably 0.1 or more. The content of hydrogen polysiloxane is preferably 10 or less per alkenyl group contained in the addition curing silicone resin, more preferably 5 or less, and even more preferably 3 or less.

[0086] (radiopaque material) The resin composition according to one aspect of the present invention preferably contains a radiopaque substance from the viewpoint of imparting radiopacity. The radiopaque substance may also function as a dispersant. The radiopaque substance is preferably one having a lower radiation permeability than skin, muscle, and fat, and more preferably one having a lower radiation permeability than bone and calcium. Examples of such radiopaque substances include barium sulfate, calcium carbonate, aluminum hydroxide, bromine, bromide, iodine, and iodide, which are made of nonmetallic atoms, and metal powders and oxides of metals such as titanium, zinc, zirconium, rhodium, palladium, silver, tin, tantalum, tungsten, rhenium, iridium, platinum, gold, and bismuth, which are made of metal atoms. Mica, talc, and the like can also be used as radiopaque substances. In terms of further improving the brightness of the molded article obtained by processing the resin composition, the radiopaque substance is preferably barium sulfate or a metal oxide, and more preferably barium sulfate or titanium oxide.

[0087] The resin composition according to one embodiment of the present invention can be used as a medical material. When the resin composition according to one embodiment of the present invention is used, for example, as a material for a medical device used in a living body, it is preferable that the resin composition contains a radiopaque substance having high biocompatibility. Examples of radiopaque substances having high biocompatibility include barium sulfate, bismuth oxide, bismuth subcarbonate, calcium carbonate, aluminum hydroxide, tungsten, zinc oxide, zirconium oxide, zirconium, titanium, platinum, bismuth subnitrate, and bismuth. As the radiopaque substance used in one embodiment of the present invention, barium sulfate, calcium carbonate, bismuth subcarbonate, or bismuth oxide is more preferable from the viewpoint of safety, and barium sulfate is particularly preferable from the viewpoint of sensitizing effect on luminescent substances. The resin composition according to one embodiment of the present invention may contain one type of radiopaque substance, or may contain two or more types. In the resin composition according to one embodiment of the present invention, it is preferable that the resin composition contains one or more types of the radiopaque substances listed above.

[0088] The shape of the radiopaque substance used in one embodiment of the present invention is not particularly limited as long as it can impart radiopaqueness to the resin composition to which it is blended, and may be any of particulate, filamentous, and irregular shapes. From the viewpoints of dispersibility in the resin and radiotransmittance, the radiopaque substance used in one embodiment of the present invention is preferably particulate.

[0089] The content of the radiopaque substance depends on the detection sensitivity of the radiation inspection device, but is generally preferably 5 parts by mass or more relative to 100 parts by mass of the silicone resin, and from the viewpoint of ensuring the physical properties of the resin, is preferably 80 parts by mass or less, more preferably 10 to 50 parts by mass, and even more preferably 20 to 30 parts by mass.

[0090] The content of the radiopaque substance in the resin composition is preferably 10 parts by mass or more and 80 parts by mass or less relative to 100 parts by mass of the silicone resin, more preferably 10 to 50 parts by mass, and further preferably 20 to 30 parts by mass.

[0091] (Other resins) The resin composition according to one embodiment of the present invention may contain other resins different from the silicone resin in addition to the silicone resin. The other resins are not particularly limited, and can be appropriately selected from known resin compositions and their improvements in consideration of the product quality required when forming a molded body. For example, the other resins may be thermoplastic resins or thermosetting resins. The other resins contained in the resin composition according to one embodiment of the present invention are preferably thermoplastic resins. The other resins used in one embodiment of the present invention may be one type only, or two or more types may be mixed together. When two or more types are mixed together, it is preferable to use resins with high compatibility in combination.

[0092] Other resins that can be used in the resin composition according to one embodiment of the present invention include, for example, urethane-based resins such as polyurethane (PU) and thermoplastic polyurethane (TPU); polycarbonate (PC); vinyl chloride-based resins such as polyvinyl chloride (PVC) and vinyl chloride-vinyl acetate copolymer resin; acrylic resins such as polyacrylic acid, polymethacrylic acid, polymethyl acrylate, polymethyl methacrylate (PMMA), and polyethyl methacrylate; polyester-based resins such as polyethylene terephthalate (PET), polybutylene terephthalate, polytrimethylene terephthalate, polyethylene naphthalate, and polybutylene naphthalate; polyamide-based resins such as Nylon (registered trademark); and polystyrene. Examples of suitable resins include polystyrene-based resins such as polystyrene (PS), imide-modified polystyrene, acrylonitrile-butadiene-styrene (ABS) resin, imide-modified ABS resin, styrene-acrylonitrile copolymer (SAN) resin, and acrylonitrile-ethylene-propylene-diene-styrene (AES) resin, polyethylene (PE) resin, polypropylene (PP) resin, and cycloolefin resin; cellulose-based resins such as nitrocellulose and cellulose acetate; epoxy-based resins such as bisphenol A epoxy resin, bisphenol F epoxy resin, isocyanurate epoxy resin, and hydantoin epoxy resin; melamine-based resin; silicone-based resin; fluorine-based resin; and rubber-based resin. Among these, PU, ​​PET, PVC, PC, PMMA, and PS are preferred because of their high dispersibility of the luminescent substance, and two or more of these may be mixed and used.

[0093] In addition, the other resins used in the resin composition according to one embodiment of the present invention are preferably those having radiation resistance. Examples of resins having radiation resistance include polystyrene-based resins, polycarbonate-based resins, polyester-based resins, polysulfone-based resins, polyether-based resins, etc. Even in the case of resins other than these, the radiation resistance can be improved by using additives in combination. Examples of the additives include phenol-based antioxidants, hindered amine-based light stabilizers, organic nucleating agents, etc.

[0094] In addition, when the resin composition according to one embodiment of the present invention is a thermoplastic resin composition, the other resin may be a thermoplastic resin as a whole, and may contain a small amount of a non-thermoplastic resin. Similarly, when the resin composition according to one embodiment of the present invention is a thermosetting resin composition, the other resin may be a thermosetting resin as a whole, and may contain a small amount of a non-thermosetting resin.

[0095] <Resin composition> The method for producing a resin composition according to one aspect of the present invention may include a step of mixing a near-infrared light emitting material and a silicone resin. In addition, when the resin composition includes a dispersant, the method for producing a resin composition according to one aspect of the present invention may include a first mixing step in which the near-infrared light emitting material and the dispersant are mixed in advance to obtain a mixture, and a second mixing step in which the mixture and the silicone resin are mixed to obtain a resin composition. The resin composition according to one aspect of the present invention can be produced by mixing and dispersing the mixture in which the near-infrared light emitting material and the dispersant are mixed in advance in the first mixing step with the silicone resin in the second mixing step. The method for mixing and dispersing the mixture in the resin is not particularly limited, and any known method may be used. For example, the mixture may be added to a resin composition solution dissolved in a suitable solvent and dispersed. In addition, even when a solvent is not used, the mixture can be added to the resin composition and melt-kneaded to obtain the resin composition according to one aspect of the present invention. In this way, a resin composition in which the mixture is uniformly dispersed in the resin is obtained.

[0096] The content of the near-infrared light-emitting material in the resin composition is not particularly limited as long as the light-emitting material can be mixed in the resin. It is known that the near-infrared light-emitting material has the highest light-emitting intensity corresponding to the concentration under a dilute condition where the interaction of the light-emitting material can be ignored, except for cases such as light-emitting materials using aggregation-induced emission. However, it is preferable to ensure a practical light-emitting intensity from the viewpoint of detection sensitivity in various measuring instruments. For this purpose, the content of the near-infrared light-emitting material is preferably 0.0001 parts by mass or more per 100 parts by mass of silicone resin, and is preferably 1 part by mass or less per 100 parts by mass of silicone resin from the viewpoint of the decrease in light-emitting intensity due to concentration quenching and reabsorption of light emission. The content is more preferably in the range of 0.001 to 0.1 parts by mass, and even more preferably in the range of 0.006 to 0.02 parts by mass per 100 parts by mass of silicone resin. The content of the near-infrared light-emitting material in the molded product obtained by processing the resin composition is within this range to obtain a practical light-emitting intensity.

[0097] From the above viewpoints, the content of the near-infrared light emitting material in the resin composition is preferably 0.0001 to 1 part by mass relative to 100 parts by mass of the silicone resin. From the viewpoint of processing, it is preferably 0.0001 to 0.1 part by mass, and from the viewpoint of performance, it is preferably in the range of 0.001 to 0.1 part by mass, and more preferably in the range of 0.006 to 0.02 part by mass.

[0098] The resin composition according to one embodiment of the present invention emits near-infrared light such as near-infrared fluorescence with excellent radiation resistance. Here, the resin composition emitting light such as fluorescence "has excellent radiation resistance" means that the attenuation rate of absorbance at the maximum absorption wavelength due to radiation irradiation [([absorbance before radiation irradiation]-[absorbance after radiation irradiation]) / [absorbance before radiation irradiation]×100(%)] is small. Here, the attenuation rate of absorbance at the maximum absorption wavelength means the attenuation rate of absorbance at the maximum absorption wavelength having the maximum absorbance in the wavelength region of 600 to 1100 nm. Specifically, the resin composition according to one embodiment of the present invention has an attenuation rate of absorbance at the maximum absorption wavelength due to radiation irradiation of 25 kGy of 50% or less. If the attenuation rate is within this range, there is no practical problem. However, from the viewpoint of sensitivity, the resin composition according to one embodiment of the present invention preferably has a decay rate of absorbance at the maximum absorption wavelength due to irradiation with 25 kGy of radiation of 30% or less, more preferably 20% or less, and even more preferably 15% or less.

[0099] In addition, for a resin composition according to an embodiment of the present invention, it is preferable that the change in the maximum absorption wavelength due to radiation irradiation is small. The difference between the maximum absorption wavelength before radiation irradiation and the maximum absorption wavelength after radiation irradiation may be 30 nm or less, more preferably 20 nm or less, and particularly preferably 10 nm or less. Furthermore, for a resin composition according to an embodiment of the present invention, it is preferable that the change in the maximum fluorescence wavelength due to radiation irradiation is small. The difference between the maximum fluorescence wavelength before radiation irradiation and the maximum fluorescence wavelength after radiation irradiation may be 30 nm or less, more preferably 20 nm or less, and particularly preferably 10 nm or less.

[0100] When irradiating the resin composition with radiation, the type of radiation and the dose of radiation may be appropriately selected according to the purpose. For example, when sterilizing a medical instrument with radiation, the radiation dose is often 5 kGy or more. Although the optimum dose may be appropriately selected depending on the type of medical instrument and the sterilization process equipment, there are cases where the dose of radiation needs to be set high to maintain the sterilization level. In general, if the resin composition has radiation resistance at 50 kGy or more, sufficient sterilization is possible. From this viewpoint, the resin composition according to one aspect of the present invention is preferably one in which the attenuation rate of absorbance at the maximum absorption wavelength when irradiated with 50 kGy is 70% or less, more preferably 60% or less, and even more preferably 50% or less.

[0101] Generally, when detecting luminescence such as fluorescence emitted from a light-emitting material such as a fluorescent material, scattered light and reflected light of the excitation light also enter the detector, so a filter that cuts the wavelength range of the excitation light is usually placed in the detector. With such a detector, there is a problem that the wavelength ranges of the excitation light and the fluorescence overlap, and the fluorescence of the fluorescent material whose fluorescence is in the wavelength range cut by the filter cannot be detected. In order to distinguish between the fluorescence and the excitation light and to detect only the fluorescence with high sensitivity, it is necessary that the Stokes shift (the difference between the maximum absorption wavelength and the maximum fluorescence wavelength) of the near-infrared light-emitting material such as the near-infrared fluorescent material is sufficiently large.

[0102] Therefore, the resin composition according to one embodiment of the present invention preferably has a large Stokes shift (the difference between the maximum absorption wavelength and the maximum emission wavelength), and more preferably has a Stokes shift of 50 nm or more. The larger the Stokes shift, the more sensitively the luminescence such as fluorescence emitted from the molded product can be detected, even when a general detector equipped with a filter for cutting noise due to excitation light is used.

[0103] The resin composition according to one embodiment of the present invention does not change color when visually observed even when excited by excitation light in the near-infrared region, and emits invisible light such as fluorescence in the near-infrared region, which can be detected by a detector. Therefore, the maximum absorption wavelength for excitation light in the near-infrared region may be 650 nm or more, but from the viewpoint of absorption efficiency, it is preferable that the maximum absorption wavelength is close to the wavelength of the excitation light, more preferably 665 nm or more, and particularly preferably 680 nm or more.

[0104] The resin composition according to one embodiment of the present invention and the molded article obtained from the composition are practically problem-free if the color of the irradiated object does not change and the maximum fluorescence wavelength is 700 nm or more, taking into consideration the detection sensitivity. Specifically, it is preferably 720 nm or more, more preferably 740 nm or more, and particularly preferably 760 nm or more. In addition, when the maximum absorption wavelength is short, it is preferable that the Stokes shift is larger from the viewpoint of detection sensitivity in the near infrared region.

[0105] (Other Ingredients) The resin composition according to one aspect of the present invention may contain other additives in addition to the radiopaque substance, as long as the effects of the present invention are not impaired. Examples of other additives include dispersants, catalysts, ultraviolet absorbers, heat stabilizers, light stabilizers, antioxidants, flame retardants, flame retardant assistants, crystallization accelerators, plasticizers, antistatic agents, colorants, and mold release agents. In addition, the resin composition according to one aspect of the present invention may contain an organic solvent such as xylene from the viewpoint of dissolving or dispersing each component.

[0106] <Molded body> The molded article according to one aspect of the present invention is a molded article obtained by processing the resin composition according to one aspect of the present invention, and contains the resin composition. The molding method of the molded article is not particularly limited, but examples thereof include casting (casting method), injection molding using a mold, compression molding, extrusion molding using a T-die or the like, blow molding, and the like.

[0107] Detection of luminescence such as fluorescence can be performed by a conventional method using a commercially available fluorescence detection device, etc. As the excitation light used for detecting luminescence such as fluorescence, any light source can be used, and in addition to a near-infrared lamp with a long wavelength range, a laser, an LED, etc. with a narrow wavelength range can be used.

[0108] The molded article obtained from the resin composition according to one embodiment of the present invention does not change color even when irradiated with light in the near-infrared region, and emits near-infrared light such as near-infrared fluorescence that can be detected with higher sensitivity than conventional methods. Therefore, at least a part of the molded article according to one embodiment of the present invention is preferably a medical device used inside a patient's body. Specifically, the molded article is particularly suitable for a medical device that is inserted or left in a patient's body.

[0109] When detecting the emission of fluorescence or the like of a molded article obtained from a resin composition according to one embodiment of the present invention, it is preferable to irradiate it with excitation light in the near-infrared region, but if it is acceptable for the color of the irradiated object to be somewhat reddish, it is not necessary to use excitation light in the near-infrared region. For example, when detecting the emission of fluorescence or the like of a medical device inside the body by irradiating it with excitation light, it is necessary to use excitation light in a wavelength region that is highly permeable to the skin or other living body, and in this case, excitation light of 650 nm or more that is highly permeable to the living body may be used.

[0110] Examples of such medical devices include stents, coil obturators, catheter tubes, injection needles, shunt tubes, drain tubes, and implants.

[0111] <Sterilization method> When a molded article obtained from a resin composition according to an embodiment of the present invention is sterilized, various methods used for sterilizing medical devices, etc. can be used as the sterilization method. For example, methods for sterilizing medical devices, etc. include high-pressure steam sterilization, EOG sterilization, gamma-ray sterilization, electron beam sterilization, ultraviolet sterilization, etc. Among them, radiation sterilization, such as gamma-ray and electron beam sterilization, is a preferred treatment method because it is efficient and the treatment method is simple.

[0112] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. EXAMPLES

[0113] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0114] <Brightness measurement> The luminescence data was observed in a darkroom using a near-infrared fluorescence observation camera (FL VIEW, manufactured by Nirec Co., Ltd.) equipped with a 780 nm LED light source and an 840 nm bandpass filter, and the luminescence intensity was measured using an image processing application (FL VISION, manufactured by Nirec Co., Ltd.).

[0115] <Dispersibility evaluation> The dispersibility of the near-infrared fluorescent material was evaluated by visually checking the appearance of the sheet-like molded product after compression molding.

[0116] The number of agglomerates of near-infrared fluorescent material with a size of 0.1 mm or more present on a 15 cm square sheet was used as the judgment criterion, and was defined as follows: 〇:0 pieces △:1~2 pieces ×: 3 or more or spotty

[0117] [Synthesis Example 1] Method for synthesizing near-infrared fluorescent material 1

[0118] [ka]

[0119] In a 60 mL Schlenk tube, 2,3,3-trimethylindolenine (Tokyo Chemical Industry Co., Ltd., 15.92 g, 0.100 mol) and 1-iodohexane (42.41 g, 2.0 eq.) were charged under a nitrogen atmosphere, and the mixture was heated and stirred for 18 hours with a heat block set at 110°C. After cooling to room temperature, the solid was crushed and washed by decantation with diethyl ether (20 mL x 3 times), and the residue was dried under vacuum at 50°C for 5 hours to obtain compound 1-1 (38.31 g, 100% yield).

[0120] [ka]

[0121] In a 2L four-necked reactor under nitrogen atmosphere, N,N-dimethylformamide (DMF) (super dehydrated, 120mL) was charged, and after cooling to an internal temperature of 0°C, phosphoryl chloride (101mL, 4.6eq.) was added dropwise at an internal temperature of 6°C or less, and the mixture was stirred at an internal temperature of 0-6°C for 20 minutes. Next, a solution of cyclohexanone (23.5g, 0.239mol) in dichloromethane (super dehydrated, 50mL) was added dropwise at an internal temperature of 10°C or less, and the mixture was stirred while slowly heating to the reflux temperature, and stirred at 100°C for 2 hours. After cooling again to 0°C, a solution of aniline (87.5mL, 4.0eq.) in ethanol (87.5mL) was added dropwise at an internal temperature of 10°C or less. The obtained solution was stirred at an internal temperature of 0-6°C for 1 hour, then poured into hydrochloric acid water (=6M hydrochloric acid, 72mL, 1.8eq.+purified water, 2.4L) stirred at 0°C and stirred for 30 minutes. The precipitate was collected by suction filtration, and the obtained filter cake was dissolved in methanol (720mL), poured into a mixed solvent (=hexane, 2.4L+tert-butyl methyl ether, 2.4L) stirred at 0°C, and stirred at 0°C for 30 minutes. After collecting the precipitate by suction filtration, diethyl ether (200mL) was added under a nitrogen atmosphere, and the mixture was suspended and stirred at room temperature for 20 minutes. The precipitate was collected by suction filtration, and the obtained filter cake was dried under vacuum reduced pressure at 40°C for 4 hours to obtain compound 1-2 (55.6g, crude yield 64.6%).

[0122] [ka]

[0123] Compound 1-2 (13.56 g, 37.74 mmol), ethanol (800 mL), and compound 1-1 (30.83 g, 2.2 eq.) were charged into a 2 L four-neck reactor under a nitrogen stream, and after stirring at room temperature for 10 minutes, sodium acetate (7.21 g, 2.3 eq.) was added. The mixture was stirred for 10 hours in an oil bath set at 80°C, and then allowed to cool to room temperature.

[0124] The solvent was distilled off under reduced pressure, and the residual blue-purple viscous crude body (44.4 g) was separated and purified by silica gel column chromatography (Kanto Chemical silica gel 60N spherical neutral, 63-210 μm, 750 g packed with dichloromethane, eluted with dichloromethane / methanol = 9 / 1). Hexane (40 mL) was added to the concentrated residue (12.0 g), and the mixture was suspended and stirred at room temperature for a while, then filtered with suction and rinsed with hexane (40 mL). The obtained crystals were dried under vacuum at 40 ° C for 4 hours to obtain compound 1-3 (8.820 g, yield 35.4%).

[0125] [ka]

[0126] Compound 1-3 (3.000 g, 4.547 mmol), 4-tert-octylphenol (Tokyo Chemical Industry Co., Ltd., 1.689 g, 1.8 eq.), and DMF (152 mL) were charged in a 500 mL four-necked reactor under a nitrogen atmosphere, triethylamine (1.150 g, 2.5 eq.) was added dropwise, and the mixture was heated and stirred at 85 ° C. for 8 hours. After cooling to room temperature, the mixture was quenched with purified water (150 mL) and extracted with dichloromethane (150 mL x 2 times). The organic layer was washed successively with purified water (80 mL x 2 times) and brine (30 mL), dried over anhydrous sodium sulfate, filtered, and the filtrate was concentrated to obtain a dark brown paste-like crude product (9.4 g).

[0127] This crude product was separated and purified by silica gel column chromatography (Kanto Chemical silica gel 60N spherical neutral, 63-210 μm, 380 g packed with dichloromethane, eluted with methanol / dichloromethane=1 / 19) to obtain the target compound 1-4 (1.04 g, yield 27.5%).

[0128] [ka]

[0129] In a 60 mL Schlenk tube under nitrogen atmosphere, a solution of compound 1-4 (980 mg, 1.185 mmol) in dichloromethane (39 mL) was stirred at room temperature, and compound lithium tetrakis(pentafluorophenyl)borate-ethyl ether complex (1.17 g, 1.3 eq.) was added in portions. After stirring at room temperature for 3 hours, purified water (5 mL) was added to separate the oil and water, the organic layer was dried over anhydrous sodium sulfate, filtered, and the filtrate was concentrated to obtain a crude product (3.2 g).

[0130] This crude product was separated and purified by silica gel column chromatography (Kanto Chemical Silica Gel 60N Spherical Neutral, 40-50μm, 80g packed with hexane / dichloromethane=9 / 1, eluted with 1 / 1-1 / 2) to obtain a crude product. To remove impurities, it was purified again by column chromatography (Kanto Chemical Silica Gel 60N Spherical Neutral, 40-50μm, 80g packed with hexane / dichloromethane=9 / 1, eluted with 1 / 1) to obtain near-infrared fluorescent material 1 (914mg, yield 52.5%).

[0131] [Synthesis Example 2] Method for synthesizing near-infrared fluorescent material 2

[0132] [ka]

[0133] Near-infrared fluorescent material 2 was synthesized with reference to the method described in Fischer et al., Chemistry A European Journal, Vol. 15, No. 19, pp. 4857-4864, 2009.

[0134] Boron complexes such as near-infrared fluorescent material 2 are known to have many materials with high luminous efficiency because they suppress non-radiative deactivation by fixing the structure of the aromatic compound part, which is an anion species, with boron, which is a cationic species. The chemical formula shown below shows the intramolecular polarization of near-infrared fluorescent material 2.

[0135] [ka]

[0136] [Synthesis Example 3] Method for synthesizing near-infrared fluorescent material 3

[0137] [ka]

[0138] Compound 3-1: 4-bromophenol (94.54g, 0.5464mol), 1-bromobutane (97.34g, 0.7104mol, 1.3eq.), potassium carbonate (anhydrous) (377.6g, 2.732mol, 5.0eq.), and acetone (1L) were charged into a 3L four-necked reactor under a nitrogen stream and refluxed for 16 hours. After cooling to room temperature, insoluble matter was removed by filtration and rinsed with acetone (800mL). The filtrate was concentrated, and the residue was separated and purified by silica gel column chromatography (Kanto Chemical silica gel 60N spherical neutral 63-210μm, 2.5kg filled with hexane, eluted with hexane / dichloromethane = 19 / 1) to obtain compound 3-2 (colorless oil, 106.0g, yield 84.7%, LC purity 99.74%).

[0139] [ka]

[0140] Compound 3-3: 2,3-dicyanohydroquinone (Tokyo Chemical Industry Co., Ltd., 35.65 g, 0.2226 mol) was dissolved in dichloromethane (ultra-dehydrated, 430 mL) in a 2 L four-necked reactor under nitrogen flow, and 2,6-lutidine (70.13 g, 2.94 eq.) was added at an internal temperature of 8°C and cooled to an internal temperature of -33°C. Trifluoromethanesulfonic anhydride (147.6 g, 2.35 eq.) was added dropwise at an internal temperature of -33 to -25°C over 24 minutes, and then the mixture was stirred overnight while the internal temperature was returned to 12°C.

[0141] The mixture was quenched with purified water (300 mL) to separate the oil and water, and the aqueous layer was extracted with dichloromethane (300 mL). The two organic layers were combined, washed with purified water (300 mL) and brine (100 mL) in sequence, dried over anhydrous sodium sulfate, filtered, and the filtrate was concentrated to obtain a concentrated residue (129.8 g). This crude material was dissolved in ethyl acetate (390 mL), then dropped into hexane (1.95 L) stirred at room temperature to cause reprecipitation, and the resulting suspension was stirred at room temperature for 30 minutes. The crystals were collected by suction filtration and rinsed with a mixture of ethyl acetate and hexane (= ethyl acetate 40 mL + hexane 200 mL). The mixture was dried at 50 ° C under vacuum and reduced pressure to obtain compound 3-4 (light brown powder, 56.56 g, yield 59.9%, LC purity 92.46%).

[0142] [ka]

[0143] In a 3L four-necked reactor under argon, magnesium (turnings, 11.32g, 3.86eq.) was charged, THF (super dehydrated, 40mL) was added, and about 2mL of compound 3-2 (105.1g, 0.4586mol, 3.8eq.) was added. Iodide (granular, 3 grains) was added, and it was confirmed that the reaction had started due to heat generation. Next, the remaining compound 3-2 diluted with THF (super dehydrated, 200mL) was added dropwise over 1 hour and 30 minutes so that the internal temperature of the reaction system was within 41 to 58°C. Magnesium was still dissolved, so it was almost completely disappeared after further stirring under reflux for 2 hours. After dilution with THF (super dehydrated, 240mL), the internal temperature was cooled to -65°C, and then a solution of sulfur (powder, 11.61g, 3.0eq.) in THF (super dehydrated, 240mL) was added dropwise over 30 minutes so that the internal temperature was within -50°C. The internal temperature was raised to 30° C. over 47 minutes, and then stirred for 30 minutes at an internal temperature of 28 to 30° C. After cooling again to an internal temperature of −35° C., a solution of compound 3-4 (51.20 g, 0.1207 mol) in THF (ultra-dehydrated, 154 mL) was added dropwise over 20 minutes so that the internal temperature was within −4° C. The internal temperature was raised to 30° C. over 30 minutes, and then stirred for another hour.

[0144] After cooling to -4°C again, quenching was performed by adding 2M hydrochloric acid (460mL) dropwise, stirring for a while while returning to room temperature, and then extraction with ethyl acetate (600mL x 2 times). The two organic layers were combined and washed successively with purified water (500mL) and brine (300mL), dried over sodium sulfate, filtered, and the filtrate was concentrated to obtain a concentrated residue (175.9g).

[0145] This crude product was separated and purified by silica gel column chromatography (Kanto Chemical silica gel 60N spherical neutral 63-210μm, 1.8kg packed with hexane, eluted with hexane / ethyl acetate = 5 / 1-3 / 1). The obtained concentrated residue (34.6g) was dissolved in THF (52mL), then dropped into ethanol (312mL) stirred at room temperature to reprecipitate, and stirred at room temperature for 1 hour. The obtained crystals were collected by suction filtration and rinsed with ethanol (100mL). The mixture was dried under vacuum at 50℃ to obtain compound 3-5 (light brown powder, 22.49g, yield 38.1%, LC purity 97.69%).

[0146] [ka]

[0147] 1-butanol (dehydrated, 220mL) was charged into a 1L four-necked reactor under argon flow at room temperature, and after argon bubbling for 20 minutes, lithium (granular, 2.12g, 6.8eq.) was added, the oil bath was set to 120°C and the mixture was heated and stirred for 35 minutes until the lithium was dissolved. Compound 3-5 (22.00g, 45.02mmol) was added in portions, the water bath was set to 127°C and the mixture was heated, and the mixture was stirred at an internal temperature of 116-117°C for 2 hours.

[0148] After cooling to room temperature, the mixture was quenched with 1v / v% sulfuric acid-methanol solution (1.63L) and stirred at room temperature for 10 minutes. The precipitate obtained was collected by suction filtration and rinsed with methanol (500mL), and a black purple solid (23.8g) was obtained as a filter cake. This crude material was separated and purified by silica gel column chromatography (Kanto Chemical silica gel 60N spherical neutral 40-50μm, 440g was filled with hexane / chloroform = 1 / 1, and eluted with hexane / chloroform = 1 / 2-0 / 1). The concentrated residue obtained (16.9g) was suspended and stirred in methanol (340mL) at room temperature, and the precipitate was collected by suction filtration and rinsed with methanol (340mL). The mixture was dried at 60℃ under vacuum and reduced pressure to obtain near-infrared fluorescent material 3 (black purple powder, 14.44g, yield 65.6%).

[0149] [Synthesis Example 4] Method for synthesizing near-infrared fluorescent material 4

[0150] [ka]

[0151] Near infrared fluorescent material 3 (11.0 g, 5.62 mmol), DMSO (550 mL), chlorobenzene (2.2 L), and magnesium acetate tetrahydrate (6.03 g, 5.0 eq.) were added to a 5 L four-neck reactor at room temperature under an argon stream, and the mixture was stirred at 130° C. for 3 hours.

[0152] After cooling to room temperature, purified water (1 L) was poured in and extracted with chloroform (1 L x 3 times). The three organic layers were combined and washed with purified water (1 L) and brine (1 L). The mixture was dried over sodium sulfate, filtered, and the filtrate was concentrated to obtain a crude product (11.5 g, deep purple solid). This crude product was purified by column chromatography (Wako Pure Chemicals activated alumina 45 μm, 575 g, packed with chloroform, eluted with chloroform), and dried at 50 °C under vacuum and reduced pressure for 8 hours to obtain near-infrared fluorescent material 4 (black purple powder, 9.40 g, yield 84.5%).

[0153] It is known that the near-infrared fluorescent material 4 exhibits high durability by fixing the structure of the aromatic compound portion, which is an anion species, with magnesium, which is a cationic species. The chemical formula shown below shows the intramolecular polarization of the near-infrared fluorescent material 4.

[0154] [ka]

[0155] [Example 1-1] Near-infrared fluorescent material 1 (1.3 mg), methylphenyl polysiloxane (methylphenyl silicone oil, Shin-Etsu Chemical Co., Ltd., KF-54, 10 g), and 0.21 mL of xylene were mixed in a vial and then stirred at room temperature. As a result, a uniform green solution with a concentration of near-infrared fluorescent material 1 of 120 ppm was obtained as a resin composition. 0.5 g of the resin composition was placed in a tray and the brightness was measured, and the result is shown in Figure 1. As shown in Figure 1, the brightness was 198, and the near-infrared fluorescent material 1 was uniformly dispersed. As a result of the above-mentioned dispersibility evaluation, no agglomerates of near-infrared fluorescent material of 0.1 mm or more were confirmed, so it was judged to be good.

[0156] [Example 1-2] Near-infrared fluorescent material 1 (1.3 mg), vinyl-terminated polydimethylsiloxane (GELEST, DMS-V05, 2.65 g), alkylhydridosiloxane (NuSil, XL1-116, 7.35 g, trimethyl-terminated hydridosiloxane, addition curing type), and 0.21 mL of xylene were mixed in a vial. Then, Pt catalyst (Karstedt catalyst) was added at a concentration of 5 ppm to obtain a resin composition. The brightness at this point was uniform at 107.

[0157] The resin composition was cured in an oven at 80°C for 2.5 hours, and the light green transparent silicone resin obtained by curing was formed into a PS sheet to obtain a molded body. Figure 2 shows the results of measuring the brightness inside the molded body. As shown in Figure 2, the brightness inside the molded body was uniform at 52. Figure 3 shows the results of measuring the brightness at the edge parts. As shown in Figure 3, the brightness at the edge parts was 117 due to total reflection within the film, and the near-infrared fluorescent material 1 was uniformly dispersed. As a result of the above-mentioned dispersibility evaluation, no agglomerates of near-infrared fluorescent material larger than 0.1 mm were confirmed, so it was judged to be good (〇).

[0158] From Examples 1-1 and 1-2, it was confirmed that the near-infrared fluorescent material 1 was dissolved in silicone oil and silicone resin raw materials at practical concentrations and was not deactivated.

[0159] In Examples 2-1 to 2-3 and Comparative Examples 2-1 and 2-2, silicone oil in which a near-infrared fluorescent material was dissolved was used to prepare a silicone sheet in which the fluorescent material was uniformly dispersed, and the luminance was confirmed.

[0160] [Example 2-1] Near-infrared fluorescent material 1 (7.2 mg) and methylphenyl silicone oil (Momentive Performance Materials, TSF437, 1.8 g) were mixed in advance and added to millable silicone rubber (Momentive Performance Materials, TSE2571-5U, 59.4 g, addition curing type).The mixture was then kneaded twice in a Toyo Seiki Seisakusho Lab Plastomill "4C150" at 20°C, 50 rpm, and air for 3 minutes.

[0161] The above-mentioned silicone elastomer resin was supplied between the biaxially oriented PET film (Mitsubishi Chemical's "Diafoil T-100", thickness: 100 μm) that was supplied along a metal roll as the raw material kneaded above, and a bank was formed on the roll at room temperature to create a silicone sheet. Note that cover films were attached to both sides of the silicone layer. The thickness of the silicone layer was 250 μm.

[0162] [Comparative Example 2-1] A silicone sheet was produced in the same manner as in Example 2-1, except that the near-infrared fluorescent material 1 in Example 2-1 was changed to the near-infrared fluorescent material 2. The thickness of the silicone layer was 250 μm.

[0163] [Comparative Example 2-2] A silicone sheet was produced in the same manner as in Example 2-1, except that the near-infrared fluorescent material 1 in Example 2-1 was changed to the near-infrared fluorescent material 4. The thickness of the silicone layer was 250 μm.

[0164] [Example 2-2] A silicone sheet was prepared in the same manner as in Example 2-1, except that the amount of millable silicone rubber (TSE2571-5U, manufactured by Momentive Performance Materials, Inc.) in Example 2-1 was reduced from 59.4 g to 53.4 g and the reduced amount was replaced with barium sulfate (Wako Pure Chemical Industries, Fujifilm, Wako Grade 1, 6.0 g). The thickness of the silicone layer was 250 μm.

[0165] [Example 2-3] A silicone sheet was prepared in the same manner as in Example 2-1, except that the amount of millable silicone rubber (TSE2571-5U, manufactured by Momentive Performance Materials, Inc.) in Example 2-1 was reduced from 59.4 g to 53.4 g and the reduced amount was replaced with rutile-type titanium dioxide (manufactured by Ishihara Sangyo Kaisha, Ltd., average particle size 0.25 μm, 6.0 g). The thickness of the silicone layer was 250 μm.

[0166] The dispersibility and luminance of Examples 2-1 to 2-3 and Comparative Examples 2-1 and 2-2 were evaluated. The results are shown in Table 1.

[0167] [Table 1]

[0168] From Example 2-1, near-infrared fluorescent material 1 was confirmed to have high dispersibility and brightness even in the silicone sheet, while from Comparative Examples 2-1 and 2-2, near-infrared fluorescent materials 2 and 3 were confirmed to have aggregates that were likely derived from the fluorescent material, and brightness could not be confirmed. From these results, it was confirmed that near-infrared fluorescent material 1 exhibits high dispersibility even in non-polar resins, and concentration quenching is suppressed. The high dispersibility was also confirmed in Figure 4, which is a photograph of brightness measurement.

[0169] From Examples 2-2 and 2-3, it was confirmed that even if barium sulfate or titanium oxide was added as a dispersant, high dispersibility was maintained, and in addition, the brightness could be increased due to the light diffusion effect of the dispersant. The high dispersibility was also confirmed in Figures 7 and 8. [Industrial Applicability]

[0170] The resin composition according to one aspect of the present invention can be used as a material for medical devices and the like.

Claims

1. A resin composition comprising a near-infrared light-emitting material and a silicone resin, The near-infrared emitting material is one or more compounds composed of a cation species and an anion species represented by the following chemical formula (1): 【Chemistry 1】 In chemical formula (1), l is 1 or 2; X is selected from the group consisting of a single bond, a carbon atom, a nitrogen atom, an oxygen atom, a phosphorus atom, and a sulfur atom; m is 1 or 2; R 1 is an aliphatic hydrocarbon group or an aromatic hydrocarbon group, and other R 1 may form a ring together with R, at least one hydrogen atom in the aliphatic hydrocarbon group or aromatic hydrocarbon group may be substituted with a halogen atom, and two R 1 may be the same or different, n is 1 to 4, and two n's may be the same or different; R 2 is a linear, branched or cyclic aliphatic hydrocarbon group, and two R 2 may be the same or different, R 3 , R 4 , R 5 , and R 6 each independently represents an alkyl group which may have a substituent, A is an aromatic hydrocarbon group which may have a substituent, or an aromatic heterocyclic group which may have a substituent.

2. The resin composition according to claim 1, wherein the chemical formula (1) is the following chemical formula (2): 【Chemistry 2】 In chemical formula (2), l is 1 or 2; X is selected from the group consisting of a single bond, a carbon atom, a nitrogen atom, an oxygen atom, a phosphorus atom, and a sulfur atom; m is 1 or 2; R 7 represents an aliphatic hydrocarbon group or an aromatic hydrocarbon group, in which at least one hydrogen atom may be substituted by a halogen atom; o is 1 to 5; When o is 2 to 5, R 7 is another R 7 may form a ring together with R 1 is an aliphatic hydrocarbon group or an aromatic hydrocarbon group, and other R 1 and at least one hydrogen atom in the aliphatic hydrocarbon group or aromatic hydrocarbon group may be substituted with a halogen atom. n is 1 to 4, and two n's may be the same or different; R 2 is a linear, branched or cyclic aliphatic hydrocarbon group, and two R 2 may be the same or different.

3. The resin composition according to claim 1, wherein in said chemical formula (1), X is selected from the group consisting of a single bond, a nitrogen atom, and an oxygen atom.

4. In the above chemical formula (1), R 2 The resin composition according to claim 3, wherein is an aliphatic hydrocarbon group having 1 to 6 carbon atoms.

5. The resin composition according to claim 4 , wherein the anion species is a counter ion containing boron or phosphorus, or a halide ion.

6. The resin composition according to claim 1 , wherein the near-infrared light emitting material is a near-infrared fluorescent material.

7. The cationic species has the following chemical formula: 【Chemistry 3】 The resin composition according to claim 5, wherein the compound is one or more compounds selected from the following:

8. The resin composition according to claim 1 , wherein the silicone resin comprises a silicone oil.

9. The resin composition according to claim 1 , wherein the silicone resin comprises an addition polymerization type silicone resin.

10. The resin composition of claim 1 further comprising a radiopaque material.

11. The resin composition according to claim 1 , which is used as a medical material.

12. A molded article comprising the resin composition according to any one of claims 1 to 11.

13. The molded article according to claim 12, at least a portion of which is a medical device for use inside a patient's body.

Citation Information

Patent Citations

  • Itotsuzurikikaino haishiannaisochi

    JP1976077427A

  • Radiation non-transmissible label and using method of the same

    JP2000060975A

  • Polymer markers with high radiopacity for use in medical devices

    JP2008541987A

  • Azo-boron complex compound and method for producing the same

    JP2011162445A

  • Color conversion material, composition including the material, color conversion optical part using the composition, and light-emitting element using the color conversion optical part