Polarizer protection film, polarizing plate, and liquid crystal panel
A polarizer protective film with a ring structure in its main chain and controlled retardations addresses the yellowish tinge and uneven display issues in IPS type liquid crystal panels, ensuring uniformity and reduced yellowness.
Patent Information
- Application Number
- JP2024050656
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-11
AI Technical Summary
Polarizer protective films containing acrylic resin applied to IPS type liquid crystal panels exhibit a slight yellowish tinge when viewed from an oblique direction and cause uneven display due to variations in in-plane retardation.
A polarizer protective film composed of an acrylic resin with specific optical properties, including a ring structure in its main chain, controlled in-plane and thickness direction retardations, and a glass transition temperature of 120°C or higher, is used to achieve uniformity of in-plane retardation and reduce yellowness.
The film provides both uniform in-plane retardation and reduced yellowness when viewed from an oblique direction, improving display quality on IPS type liquid crystal panels.
Smart Images

Figure 2024144326000001 
Figure 2024144326000002 
Figure 2024144326000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizer protective film, a polarizing plate, and a liquid crystal panel. [Background technology]
[0002] Acrylic resins have excellent transparency, color tone, appearance, heat resistance, and processability, and are therefore used, for example, in polarizer protective films (see, for example, Patent Document 1). Here, the polarizer protective films are attached to both sides of a polarizer to form polarizing plates, which are then placed on both sides of a liquid crystal cell to be used in liquid crystal panels.
[0003] On the other hand, IPS type liquid crystal panels are preferably used for applications such as liquid crystal televisions because of their wide viewing angle and excellent color reproducibility. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-25333 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when a polarizer protective film containing an acrylic resin is applied to an IPS liquid crystal panel, the liquid crystal panel may have a slight yellowish tinge when the black display is viewed from an oblique direction. On the other hand, when such a color tone problem is optically compensated for by the retardation of the polarizer protective film, if there is variation in the in-plane retardation of the polarizer protective film, unevenness in the display of the liquid crystal panel may occur.
[0006] An object of the present invention is to provide a polarizer protective film that can achieve both uniformity of in-plane retardation and reduction in yellowness when viewed from an oblique direction of a liquid crystal panel. [Means for solving the problem]
[0007] [1] A polarizer protective film comprising an acrylic resin composition, the polarizer protective film having an average in-plane retardation of more than 0.0 nm and not more than 0.7 nm, and a thickness direction retardation Rth at a wavelength of 590 nm of −15.0 nm or more and less than 0.0 nm, the acrylic resin composition comprising an acrylic resin having a ring structure in its main chain, and having a glass transition temperature of 120° C. or more.
[0008] [2] The polarizer protective film described in [1], wherein the acrylic resin having a ring structure in its main chain has a structural unit including in its main chain one or more ring structures selected from the group consisting of a glutarimide ring, a lactone ring, a maleic anhydride ring, a maleimide ring, and a glutaric anhydride ring.
[0009] [3] The polarizer protective film according to [2], wherein the acrylic resin having a ring structure in its main chain has a structural unit represented by the following formula (1):
[0010] [ka] (In the formula, R 1 and R 2 are each independently a hydrogen atom or an alkyl group having 1 to 8 carbon atoms; R 3 is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, or a cycloalkyl group having 3 to 12 carbon atoms.
[0011] [4] The polarizer protective film described in any one of [1] to [3], wherein the acrylic resin composition has a content of structural units derived from aromatic vinyl of 0% by weight or more and 8% by weight or less.
[0012] [5] The polarizer protective film according to [4], wherein the acrylic resin composition has a content of structural units derived from styrene of 0% by weight or more and 8% by weight or less.
[0013] [6] The polarizer protective film described in any one of [1] to [5], wherein the acrylic resin composition further contains polymethyl methacrylate or a methyl methacrylate-styrene copolymer.
[0014] [7] The polarizer protective film according to any one of [1] to [6], wherein the acrylic resin composition has a 1% weight loss temperature of 300°C or higher.
[0015] [8] The polarizer protective film according to any one of [1] to [7], which does not contain an ultraviolet absorber.
[0016] [9] The polarizer protective film according to any one of [1] to [8], which is a biaxially stretched film.
[0017]
[10] The polarizer protective film according to any one of [1] to [9], having a yellowness index of 0.01 or more and 5.00 or less.
[0018]
[11] The polarizer protective film according to any one of [1] to
[10] , which has an absorbance at a wavelength of 380 nm of 0.01 or more and 1.00 or less.
[0019]
[12] The polarizer protective film according to any one of [1] to
[11] , wherein the absolute value of the Nz coefficient is 0.1 or more and 30.0 or less, the ratio Rth(447) / Rth(548) of the thickness direction retardation Rth(447) at a wavelength of 447 nm to the thickness direction retardation Rth(548) at a wavelength of 548 nm is 0.50 or more and 1.10 or less, and the ratio Rth(628) / Rth(548) of the thickness direction retardation Rth(628) at a wavelength of 628 nm to the thickness direction retardation Rth(548) at a wavelength of 548 nm is 0.50 or more and 2.00 or less.
[0020]
[13] A polarizing plate comprising the polarizer protective film according to any one of [1] to
[12] .
[0021]
[14] A liquid crystal panel comprising the polarizing plate according to
[13] . Effect of the Invention
[0022] According to the present invention, it is possible to provide a polarizer protective film that can achieve both uniformity of in-plane retardation and reduction in yellowness when viewed from an oblique direction of a liquid crystal panel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, an embodiment of the present invention will be described.
[0024] (Polarizer protection film) The polarizer protective film of the present embodiment contains an acrylic resin composition.
[0025] The average value of the in-plane retardation Re of the polarizer protective film of this embodiment is greater than 0.0 nm and is 0.7 nm or less, and is preferably 0.6 nm or less. When the average value of Re is 0.7 nm or less, the uniformity of the in-plane retardation is improved. In this case, the polarizer protective film of this embodiment preferably has a standard deviation of the in-plane retardation Re of less than 0.2.
[0026] The thickness direction retardation Rth of the polarizer protective film of this embodiment at a wavelength of 590 nm is -15.0 nm or more and less than 0.0 nm, more preferably -13.0 nm or more and less than -2.5 nm, even more preferably -10.0 nm or more and less than -2.5 nm, even more preferably -10.0 nm or more and less than -5.0 nm, and particularly preferably -10.0 nm or more and less than -7.0 nm. When Rth is -15.0 nm or more and less than 0.0 nm, the yellowness when viewed from an oblique direction of the liquid crystal panel is reduced. In this case, the polarizer protective film of this embodiment preferably has a yellowness of 50 or less when viewed from an oblique direction of the liquid crystal panel.
[0027] Note that Re and Rth are represented by the formula Re = (nx-ny) × d Rth = [(nx + ny) / 2-nz] × d Here, nx, ny, and nz are the refractive indices in the X-axis direction, Y-axis direction, and Z-axis direction, respectively, when the MD direction is the X-axis, the TD direction is the Y-axis, and the thickness direction of the film is the Z-axis. Also, d is the thickness of the film.
[0028] The yellowness index of the polarizer protective film of the present embodiment is preferably from 0.01 to 5.00, and more preferably from 0.1 to 2.0. When the yellowness index of the polarizer protective film of the present embodiment is 5.00 or less, the polarizer protective film of the present embodiment is less colored and has less effect on the color rendering properties of the liquid crystal display.
[0029] The absorbance of the polarizer protective film of this embodiment at a wavelength of 380 nm is preferably 0.01 to 1.00, and more preferably 0.10 to 0.80. When the absorbance of the polarizer protective film of this embodiment at a wavelength of 380 nm is 1.00 or less, the polarizer protective film of this embodiment is substantially free of an ultraviolet absorbing agent.
[0030] The absolute value of the Nz coefficient of the polarizer protective film of this embodiment is preferably 0.1 or more and 30.0 or less. When the absolute value of the Nz coefficient of the polarizer protective film of this embodiment is 0.1 or more and 30.0 or less, the yellowness when viewed from an oblique direction of the liquid crystal panel is reduced.
[0031] The ratio Rth(447) / Rth(548) of the thickness direction retardation Rth(447) at a wavelength of 447 nm to the thickness direction retardation Rth(548) at a wavelength of 548 nm of the polarizer protective film of this embodiment is preferably 0.50 or more and 1.10 or less, more preferably 0.80 or more and 1.08 or less. When Rth(447) / Rth(548) of the polarizer protective film of this embodiment is 0.50 or more and 1.10 or less, the yellowness when viewed from an oblique direction of the liquid crystal panel is reduced.
[0032] The ratio Rth(628) / Rth(548) of the thickness direction retardation Rth(628) at a wavelength of 628 nm to the thickness direction retardation Rth(548) at a wavelength of 548 nm of the polarizer protective film of this embodiment is preferably 0.50 or more and 2.00 or less, more preferably 0.7 or more and 1.5 or less. When Rth(628) / Rth(548) of the polarizer protective film of this embodiment is 0.50 or more and 2.00 or less, the yellowness when viewed from an oblique direction of the liquid crystal panel is reduced.
[0033] The photoelastic coefficient of the polarizer protective film of this embodiment is −10×10 -12 Pa -1 More than 10x10 -12 Pa -1 It is preferable that the value is less than or equal to -5.5×10 -12 Pa -1 More than 5.5 x 10 -12 Pa -1 It is more preferable that it is less than or equal to -4.5×10 -12 Pa -1 More than 4.5×10 -12 Pa -1 It is more preferable that the photoelastic coefficient of the polarizer protective film of the present embodiment is −10×10 or less. -12 Pa -1 More than 10x10 -12 Pa -1 When it is equal to or less than this, the polarizer protective film of the present embodiment is less likely to have color unevenness, and this tendency becomes remarkable particularly under a high-temperature and high-humidity environment.
[0034] (Acrylic resin composition) The acrylic resin composition contains an acrylic resin having a ring structure in the main chain. The glass transition temperature of the acrylic resin composition is 120°C or higher, preferably more than 120°C, more preferably 121°C or higher, and even more preferably 122°C or higher. If the glass transition temperature of the acrylic resin composition is lower than 120°C, orientation relaxation may proceed in a high-temperature and high-humidity environment, and the stability of the retardation may decrease. The glass transition temperature of the acrylic resin composition is, for example, 160°C or lower.
[0035] In the present specification and claims, the acrylic resin means a polymer of a monomer having an acryloyl group and / or a monomer having a methacryloyl group. In this case, the acrylic resin may be either a homopolymer or a copolymer. When the acrylic resin is a copolymer, the acrylic resin may be a copolymer of a monomer not having an acryloyl group or a methacryloyl group.
[0036] The acrylic resin composition may further contain, for example, polymethyl methacrylate or a methyl methacrylate-styrene copolymer. It is preferable that the acrylic resin contained in the acrylic resin composition does not have a structural unit derived from an aromatic vinyl.
[0037] The acrylic resin composition may further contain additives within a range that does not impair the object of the present invention. The additives are not particularly limited, but include, for example, antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, specific wavelength absorbing agents or specific wavelength absorbing dyes for cutting blue light, light resistance stabilizers such as radical scavengers, retardation adjusters, catalysts, plasticizers, lubricants, antistatic agents, colorants, shrinkage inhibitors, antibacterial and deodorant agents, fluorescent brighteners, and compatibilizers, and two or more of these may be used in combination.
[0038] The birefringence expression Δnxy of the acrylic resin composition is -1.0×10 -3 More than -0.1×10 -3 It is preferable that the value is less than or equal to -0.8×10 -3 Over - 0.25 x 10 -3 More preferably, it is less than or equal to -0.8×10 -3 More than -0.20×10 -3 More preferably, it is less than or equal to -0.8×10 -3 Over - 0.12 x 10 -3 It is even more preferable that Δnxy is −1.0×10 or less. -3 When the film is biaxially stretched, the desired thickness direction retardation is easily exhibited. -3 If it is equal to or less than this, the in-plane retardation tends to become uniform when biaxially stretched.
[0039] In this specification and the claims, the birefringence manifestation Δnxy of the acrylic resin composition means the birefringence manifested when a film of the acrylic resin composition in an unstretched state is uniaxially stretched at its free end to a stretch ratio of 2 in the longitudinal direction (machine direction) at a temperature 5°C higher than the glass transition temperature of the acrylic resin composition.
[0040] In addition, Δnxy is expressed by the formula Δnxy=nx-ny=Re / d Here, nx and ny are the refractive indices in the X-axis direction and the Y-axis direction, respectively, when the MD direction is the X-axis, the TD direction is the Y-axis, and the thickness direction of the film is the Z-axis. In addition, Re is the in-plane retardation of the film, and d is the thickness of the film.
[0041] The content of the structural unit derived from aromatic vinyl (e.g., styrene) in the acrylic resin composition is preferably 0% by weight or more and 8% by weight or less, more preferably 0.5% by weight or more and 5% by weight or less, even more preferably 0.5% by weight or more and 3% by weight or less, even more preferably 0.5% by weight or more and 2.5% by weight or less, and particularly preferably 1.0% by weight or more and 2.5% by weight or more. When the content of the structural unit derived from aromatic vinyl (e.g., styrene) in the acrylic resin composition is 8% by weight or less, the uniformity of the in-plane retardation of the polarizer protective film of this embodiment is improved.
[0042] The 1% weight loss temperature of the acrylic resin composition is preferably 300° C. or higher, more preferably 302° C. or higher, and even more preferably 305° C. or higher. When the 1% weight loss temperature of the acrylic resin composition is 300° C. or higher, contamination of the cooling roll during the production of the raw film is suppressed, and the film formability of the raw film is improved. The 1% weight loss temperature of the acrylic resin composition is, for example, 380° C. or lower.
[0043] The weight average molecular weight of the acrylic resin composition is preferably from 50,000 to 200,000, and more preferably from 90,000 to 150,000. When the weight average molecular weight of the acrylic resin composition is 50,000 or more, the mechanical properties of a molded product of the acrylic resin composition tend to be improved, and when it is 200,000 or less, the moldability of the acrylic resin composition tends to be improved.
[0044] The ratio of the weight average molecular weight to the number average molecular weight of the acrylic resin composition (polydispersity) is preferably 1.5 to 2.5, more preferably 1.5 to 2.2. When the polydispersity of the acrylic resin composition is 1.5 or more, the flowability of the acrylic resin composition tends to improve and the molding becomes easier, and when it is 2.5 or less, the mechanical properties such as impact resistance, toughness, and bending resistance of the molded product of the acrylic resin composition tend to improve.
[0045] The number average molecular weight and weight average molecular weight of the acrylic resin composition are values calculated in terms of standard polystyrene measured by gel permeation chromatography (GPC). The number average molecular weight and weight average molecular weight of the acrylic resin composition can be controlled by the type and amount of the polymerization initiator and chain transfer agent used in synthesizing the acrylic resin.
[0046] The polarizer protective film of the present embodiment can be attached to a polarizer to form a polarizing plate. The polarizer is not particularly limited, and a known polarizer can be used. The polarizing plate can be combined with a liquid crystal cell to form a liquid crystal panel. In this case, it is preferable to use an IPS liquid crystal cell with a wide viewing angle. The polarizer protective film of the present embodiment may not contain an ultraviolet absorbing agent, or may not substantially contain an ultraviolet absorbing agent, when disposed on the side opposite to the liquid crystal cell.
[0047] (Acrylic resin with a ring structure in the main chain) The acrylic resin having a ring structure in the main chain (hereinafter referred to as acrylic resin) preferably has a structural unit containing one or more ring structures selected from the group consisting of a glutarimide ring, a lactone ring, a maleic anhydride ring, a maleimide ring, and a glutaric anhydride ring in the main chain.
[0048] A structural unit containing a glutarimide ring in the main chain is represented, for example, by the following formula (1).
[0049] [ka] (In the formula, R 1 and R 2 are each independently a hydrogen atom or an alkyl group having 1 to 8 carbon atoms; R 3 is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, or a cycloalkyl group having 3 to 12 carbon atoms.
[0050] The acrylic resin having the structural unit represented by formula (1) can be produced by a known method. An example of the method for producing the acrylic resin having the structural unit represented by formula (1) will be described below.
[0051] First, a twin-screw extruder equipped with a die at the outlet is used to melt the methyl methacrylate resin, which is then imidized, and a strand is extruded from the die. Next, the strand is cooled using a water bath, and the strand is pelletized using a pelletizer to obtain an imidized methyl methacrylate resin. Next, a twin-screw extruder equipped with a die at the outlet is used to melt the imidized methyl methacrylate resin, which is then esterified, and a strand is extruded from the die. Next, the strand is cooled using a water bath, and the strand is pelletized using a pelletizer to obtain an acrylic resin having a structural unit represented by formula (1).
[0052] Examples of the imidizing agent include ammonia and primary amines represented by the following formula (2): Among these, monomethylamine is preferred.
[0053] R 3 NH2(2) (In the formula, R 3 is the same as formula (1).
[0054] Examples of the esterifying agent include dimethyl carbonate, 2,2-dimethoxypropane, dimethyl sulfoxide, triethyl orthoformate, trimethyl orthoacetate, trimethyl orthoformate, diphenyl carbonate, dimethyl sulfate, methyl toluene sulfonate, methyl trifluoromethyl sulfonate, methyl acetate, methanol, ethanol, methyl isocyanate, p-chlorophenyl isocyanate, dimethylcarbodiimide, dimethyl-t-butylsilyl chloride, isopropenyl acetate, dimethylurea, tetramethylammonium hydroxide, dimethyldiethoxysilane, tetra-n-butoxysilane, dimethyl(trimethylsilane) phosphite, trimethyl phosphite, trimethyl phosphate, tricresyl phosphate, diazomethane, ethylene oxide, propylene oxide, cyclohexene oxide, 2-ethylhexyl glycidyl ether, phenyl glycidyl ether, and benzyl glycidyl ether. Of these, dimethyl carbonate is preferred.
[0055] The content of structural units containing a ring structure in the main chain in the acrylic resin is preferably 1% by weight or more and 80% by weight or less.The glass transition temperature of the acrylic resin is preferably 120°C or more and 160°C or less.
[0056] The acrylic resin may further have a structural unit derived from a (meth)acrylic acid ester.
[0057] Examples of (meth)acrylic acid esters include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate; aryl (meth)acrylates such as phenyl (meth)acrylate; aralkyl (meth)acrylates such as benzyl (meth)acrylate; and cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate, and two or more of them may be used in combination. Among these, alkyl methacrylates are preferred, and methyl methacrylate is particularly preferred.
[0058] The content of structural units derived from alkyl methacrylate in the acrylic resin is preferably 50% by weight or more, more preferably 75% by weight or more, and particularly preferably 90% by weight or more.
[0059] The content of structural units derived from acrylic ester in the acrylic resin is preferably less than 1% by weight, more preferably less than 0.5% by weight, and particularly preferably less than 0.3% by weight.
[0060] The acrylic resin may further have a structural unit derived from another monomer. The other monomer is not particularly limited, but examples thereof include aromatic monomers such as styrene and methylstyrene, and nitrile monomers such as acrylonitrile and methacrylonitrile.
[0061] (Method of manufacturing polarizer protective film) The polarizer protective film of the present embodiment can be produced by using a known method. An example of a method for producing the polarizer protective film of the present embodiment will be described below.
[0062] First, an extruder equipped with a die at the outlet is used to knead the acrylic resin together with a methyl methacrylate-styrene copolymer, if necessary, and then a strand is extruded from the die. Next, the strand is cooled using a water tank, and then the strand is pelletized using a pelletizer to obtain an acrylic resin composition. Next, an extruder equipped with a T-die at the outlet is used to melt the acrylic resin composition, and then a sheet is extruded from the T-die and cooled with a cooling roll to obtain a raw film. Next, the raw film is biaxially stretched to obtain the polarizer protective film of this embodiment. At this time, the biaxial stretching may be simultaneous biaxial stretching or sequential biaxial stretching.
[0063] The temperature when the raw film is biaxially stretched is preferably (Tg+5)°C or more and (Tg+20)°C or less, more preferably (Tg+6)°C or more and (Tg+18)°C or less, and even more preferably (Tg+7)°C or more and (Tg+15)°C or less, where Tg is the glass transition temperature of the acrylic resin composition. The areal ratio when the raw film is biaxially stretched is not particularly limited, but is, for example, 2 times or more and 10 times or less. The stretching speed when the raw film is biaxially stretched is not particularly limited, but is, for example, 1.1 times / min or more and 100 times / min or less. When the raw film is sequentially biaxially stretched, the first-stage stretching speed and the second-stage stretching speed may be the same or different. In the sequential biaxial stretching, the first-stage stretching is usually a stretching in the longitudinal direction (MD direction), and the second-stage stretching is a stretching in the transverse direction (TD direction).
[0064] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and the above embodiment may be modified as appropriate within the scope of the spirit of the present invention. EXAMPLES
[0065] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0066] (Content of structural units containing glutarimide rings in the main chain) Using a nuclear magnetic resonance spectrometer AvanceIII (BRUKER) with a proton resonance frequency of 400 MHz, 1 H-NMR spectrum was measured. The molar ratio of the structural unit derived from methyl methacrylate and the structural unit containing a glutarimide ring in the main chain was converted into weight, and the content of the structural unit containing a glutarimide ring in the main chain was calculated. At this time, the molar ratio was calculated from the peak area A derived from the O-CH3 proton of methyl methacrylate around 3.5 to 3.8 ppm and the peak area B derived from the N-CH3 proton of glutarimide around 3.0 to 3.3 ppm.
[0067] (glass transition temperature) Using a high-sensitivity differential scanning calorimeter DSC7000X (manufactured by Hitachi High-Tech Science), 10 mg of the acrylic resin or acrylic resin composition was heated at a heating rate of 10° C. / min in a nitrogen atmosphere, and the glass transition temperature was determined by the midpoint method.
[0068] (1% weight loss temperature) Using a thermogravimetric and differential thermal analyzer STA7200 (manufactured by Hitachi High-Tech Science), 10 mg of the acrylic resin composition was heated from room temperature in a nitrogen atmosphere at a heating rate of 10° C. / min to determine the 1% weight loss temperature.
[0069] (Birefringence appearance Δnxy) A 30×100 mm area was cut out from the original film, and the free end was uniaxially stretched at a temperature 5° C. higher than the glass transition temperature of the original film so that the stretch ratio in the longitudinal direction (longitudinal direction) was 2 times, to obtain a uniaxially stretched film. Next, the in-plane retardation of the central part of the uniaxially stretched film was measured using a retardation measuring device KOBRA-WR (manufactured by Oji Scientific Instruments), and then divided by the thickness of the uniaxially stretched film to obtain the birefringence expression Δnxy.
[0070] (Thickness direction retardation Rth) The thickness direction retardation Rth of the polarizer protective film at a wavelength of 590 nm was measured using a retardation measurement device KOBRA-WR (manufactured by Oji Scientific Instruments).
[0071] (Average value and standard deviation of in-plane retardation Re) After cutting out a central 150 x 150 mm area from the polarizer protection film, the average value and standard deviation of the in-plane retardation Re were measured using a two-dimensional birefringence evaluation system WPA-200 (Photonic Lattice Co., Ltd.). At this time, three lines were drawn in each of the MD and TD directions, and the average value and standard deviation of the in-plane retardation Re were obtained using the line analysis function.
[0072] (yellowness) The polarizer protective film was cut into a 3 cm square, and the yellowness index (YI) was measured using a color meter SC-P (manufactured by Suga Test Instruments) in accordance with JIS K7373:2006.
[0073] (Absorbance at wavelength 380 nm) The absorbance of the polarizer protective film at a wavelength of 380 nm was measured using an ultraviolet-visible-near infrared spectrophotometer UV-560 (manufactured by JASCO Corporation).
[0074] (Photoelastic Coefficient) The photoelastic coefficient of the polarizer protective film was measured using a phase difference measuring device KOBRA (manufactured by Oji Scientific Instruments). Specifically, the polarizer protective film was cut into a size of 15 mm x 60 mm, and the change in phase difference was measured when a tensile load was applied to the film, which was changed in increments of 100 g from 0 g to 1100 g. The stress calculated from the tensile load value was plotted on the X-axis, and the birefringence calculated from the measured phase difference and the film thickness was plotted on the Y-axis. The slope of the straight line on the plotted graph was calculated to obtain the photoelastic coefficient.
[0075] (Yellowness when viewing the LCD panel from an oblique angle) A liquid crystal panel simulation was performed using a liquid crystal simulator LCD Master (manufactured by Shintech). At this time, a polarizing plate arranged on the light source side, an IPS type liquid crystal cell with an in-plane retardation Re of 295 nm, and a polarizing plate arranged on the viewing side were arranged in this order, and the measurement results of the thickness direction retardation Rth were input as the optical characteristics of the polarizer protective film on the side facing the liquid crystal cell of the polarizing plate arranged on the light source side and the viewing side. Next, the XYZ color values when viewed from a polar angle of 70° and an azimuth angle of 40° with the liquid crystal cell set in a dark state were obtained by simulation, and the yellowness index (YI) was calculated from the following formula in accordance with JIS K7373:2006. YI=100(1.2985X-1.1335Z) / Y
[0076] (Rth(447) / Rth(548), Rth(628) / Rth(548 and Nz coefficient) The retardation of the polarizer protective film at wavelengths λ (λ = 446.7 nm, 547.9 nm, 628.2 nm) was measured using a retardation measuring device KOBRA-WR (manufactured by Oji Scientific Instruments). Specifically, the in-plane retardation Re(λ) at each wavelength and the retardation R40(λ) measured by tilting the absorption axis by 40° were measured, and then the three-dimensional refractive index calculation software N-Calc (manufactured by Oji Scientific Instruments) was used to calculate the three-dimensional refractive indexes nx(λ), ny(λ), and nz(λ) at each wavelength. Next, the three-dimensional refractive indexes nx(λ), ny(λ), and nz(λ) were used to calculate the formula Rth(λ)=[{nx(λ)+ny(λ)} / 2-nz(λ)]×d The thickness direction retardation Rth(λ) at each wavelength was calculated using the formula: Rth(447) / Rth(548) and Rth(628) / Rth(548). In addition, the in-plane retardation Re(548) and thickness direction retardation Rth(548) at a wavelength of 548 nm were used to obtain the following wavelength dispersion characteristics: Nz coefficient = [Rth(548) / Re(548)] + 0.5 The Nz coefficient was calculated by:
[0077] (Weight average molecular weight, number average molecular weight and polydispersity index) The weight average molecular weight (Mw), number average molecular weight (Mn) and polydispersity (Mw / Mn) of the acrylic resin composition were calculated by gel permeation chromatography (GPC) under the following conditions using a sample solution prepared by dissolving 20 mg of the acrylic resin composition in 10 mL of tetrahydrofuran. Measuring equipment: HLC-8420GPC (Tosoh) Detector: RI detector Eluent: Tetrahydrofuran Guard column: TSKgel guard column SuperH-L (manufactured by Tosoh) Analytical columns: TSKgel SuperH5000, SuperH4000, SuperH3000, SuperH2000 (Tosoh) (in series) Eluent flow rate: 0.6mL / min Measurement temperature: 40℃ Standard material: Standard polystyrene (manufactured by Tosoh)
[0078] (Production of acrylic resin 1) The temperature of each temperature control zone of a 40 mm diameter co-rotating intermeshing twin screw extruder (L / D=90) equipped with a die at the outlet was set to 250-280°C, the screw speed was 85 rpm, and methyl methacrylate resin Parapet HM (Kuraray) was melted and filled by a kneading block. Next, 1.8% by weight of monomethylamine (Mitsubishi Gas Chemical) was added to the methyl methacrylate resin from the nozzle to imidize the methyl methacrylate resin. Next, the strand extruded from the die was cooled using a water tank, and the strand was pelletized using a pelletizer to obtain resin (I).
[0079] The temperature of each temperature control zone of a 40 mm diameter co-rotating intermeshing twin screw extruder (L / D=90) equipped with a die at the outlet was set to 240-260°C, the screw speed was set to 85 rpm, and the resin (I) was melted and filled by a kneading block. Next, 0.56% by weight of dimethyl carbonate was added to the resin (I) from the nozzle to esterify the carboxyl groups in the resin (I). At this time, the by-products after the reaction and excess dimethyl carbonate were removed. Next, the strands extruded from the die were cooled using a water tank, and then the strands were pelletized using a pelletizer to obtain acrylic resin 1. The acrylic resin 1 had a glass transition temperature of 123°C and a content of a structural unit containing a glutarimide ring in the main chain of 6% by weight.
[0080] (Production of acrylic resin 2) Except for changing the amount of monomethylamine added to 4.3% by weight based on the methyl methacrylate resin, acrylic resin 2 was obtained in the same manner as acrylic resin 1. Acrylic resin 2 had a glass transition temperature of 125°C and a content of structural units containing a glutarimide ring in the main chain of 15% by weight.
[0081] (Production of acrylic resin 3) Acrylic resin 3 was obtained in the same manner as acrylic resin 1, except that methyl methacrylate-styrene copolymer TX-100 (manufactured by Denka) containing 40% by weight of structural units derived from styrene was used instead of methyl methacrylate resin, and the amount of monomethylamine added was 8.2% by weight relative to the methyl methacrylate-styrene copolymer. Acrylic resin 5 had a glass transition temperature of 125°C and a content of structural units containing glutarimide rings in the main chain of 45% by weight.
[0082] Table 1 shows the properties of the acrylic resin.
[0083] [Table 1]
[0084] Example 1 Using a 15mm diameter co-rotating intermeshing twin screw extruder (L / D=45) equipped with a die at the outlet, 95% by weight of acrylic resin 1 and 5% by weight of methyl methacrylate-styrene copolymer KT-89 (manufactured by Denka) with a styrene-derived structural unit content of 11% by weight were kneaded. Next, a water tank was used to cool the strand extruded from the die at the outlet of the extruder, and the strand was pelletized using a pelletizer to obtain an acrylic resin composition. The acrylic resin composition had a glass transition temperature of 123°C, a 1% weight loss temperature of 308°C, an Mw of 81,000, and an Mw / Mn of 1.62.
[0085] The acrylic resin composition was dried at 100°C for 5 hours, and then melted using a 15mm diameter co-rotating intermeshing twin screw extruder (L / D=45) equipped with a T-die at the outlet. Next, the sheet extruded from the T-die was cooled using a cooling roll to obtain a raw film having a width of 160 mm and a thickness of 160 μm.
[0086] Using a film biaxial stretching device IMC-1905 (manufactured by Imoto Manufacturing Co., Ltd.), the raw film was simultaneously biaxially stretched at a temperature 15°C higher than the glass transition temperature of the acrylic resin composition so that the stretch ratio in the longitudinal and transverse directions was 2 times, thereby obtaining a polarizer protection film of 280 mm x 280 mm.
[0087] Example 2 A polarizer protective film was obtained in the same manner as in Example 1, except that the mixing ratios of acrylic resin 1 and KT-89 (manufactured by Denka) were changed to 90% by weight and 10% by weight, respectively. At this time, the acrylic resin composition had a glass transition temperature of 123°C, a 1% weight loss temperature of 308°C, an Mw of 81,000, and an Mw / Mn of 1.62.
[0088] Example 3 A polarizer protective film was obtained in the same manner as in Example 2, except that the raw film was simultaneously biaxially stretched at a temperature 7° C. higher than the glass transition temperature of the acrylic resin composition.
[0089] Example 4 A polarizer protective film was obtained in the same manner as in Example 2, except that a methyl methacrylate-styrene copolymer MS-750 (manufactured by Toyo Styrene) having a styrene-derived structural unit content of 25% by weight was used instead of KT-89 (manufactured by Denka), and the raw film was simultaneously biaxially stretched at a temperature 10° C. higher than the glass transition temperature of the acrylic resin composition. At this time, the acrylic resin composition had a glass transition temperature of 122° C., a 1% weight loss temperature of 306° C., an Mw of 76,000, and an Mw / Mn of 1.59.
[0090] Example 5 A polarizer protective film was obtained in the same manner as in Example 4, except that 10% by weight of methyl methacrylate resin Parapet HM (Kuraray) was added instead of KT-89 (Denka). At this time, the acrylic resin composition had a glass transition temperature of 120°C, a 1% weight loss temperature of 302°C, Mw of 81,000, and Mw / Mn of 1.59.
[0091] Comparative Example 1 Except for not using KT-89 (manufactured by Denka), a polarizer protective film was obtained in the same manner as in Example 1. At this time, the acrylic resin composition had a glass transition temperature of 123°C and a 1% weight loss temperature of 310°C.
[0092] Comparative Example 2 A polarizer protective film was obtained in the same manner as in Comparative Example 1, except that acrylic resin 2 was used instead of acrylic resin 1. At this time, the acrylic resin composition had a glass transition temperature of 125°C and a 1% weight loss temperature of 315°C.
[0093] Comparative Example 3 A polarizer protective film was obtained in the same manner as in Example 1, except that the acrylic resin 1 was not used and the original film was simultaneously biaxially stretched at a temperature 20°C higher than the glass transition temperature of the acrylic resin composition. At this time, the acrylic resin composition had a glass transition temperature of 117°C and a 1% weight loss temperature of 297°C.
[0094] Comparative Example 4 A polarizer protective film was obtained in the same manner as in Comparative Example 3, except that a methyl methacrylate-styrene copolymer MS800 (Nippon Steel Chemical Co., Ltd.), having a styrene-derived structural unit content of 20% by weight, was used instead of KT-89 (Denka Co., Ltd.), and the raw film was simultaneously biaxially stretched at a temperature 30°C higher than the glass transition temperature of the acrylic resin composition. At this time, the acrylic resin composition had a glass transition temperature of 115°C and a 1% weight loss temperature of 296°C.
[0095] Comparative Example 5 A polarizer protective film was obtained in the same manner as in Comparative Example 1, except that acrylic resin 3 was used instead of acrylic resin 1, and the raw film was simultaneously biaxially stretched at a temperature 35°C higher than the glass transition temperature of the acrylic resin composition. At this time, the acrylic resin composition had a glass transition temperature of 125°C and a 1% weight loss temperature of 320°C.
[0096] Table 2 shows the properties and evaluation results of the acrylic resin composition and the polarizer protective film.
[0097] [Table 2]
[0098] From Table 2, it can be seen that the polarizer protective films of Examples 1 to 5 achieve both a reduced standard deviation of Re and a reduced YI when viewed from an oblique direction of the liquid crystal panel. In contrast, the polarizer protective films of Comparative Examples 1 and 2 have Rth of 0.0 nm and 10.2 nm, respectively, and therefore have a large YI when viewed from an oblique direction of the liquid crystal panel. The polarizer protective films of Comparative Examples 3 to 5 have average Re values of 0.8, 0.9, and 1.0, respectively, and therefore have a large standard deviation of Re.
Claims
1. An acrylic resin composition is included, The average value of the in-plane retardation Re is greater than 0.0 nm and is 0.7 nm or less; The thickness direction retardation Rth at a wavelength of 590 nm is −15.0 nm or more and less than 0.0 nm, The acrylic resin composition of the polarizer protective film contains an acrylic resin having a ring structure in its main chain and has a glass transition temperature of 120° C. or higher.
2. 2. The polarizer protective film according to claim 1, wherein the acrylic resin having a ring structure in its main chain has a structural unit having one or more ring structures selected from the group consisting of a glutarimide ring, a lactone ring, a maleic anhydride ring, a maleimide ring, and a glutaric anhydride ring in its main chain.
3. The polarizer protective film according to claim 2 , wherein the acrylic resin having a ring structure in its main chain has a structural unit represented by the following formula (1): 【Chemistry 1】 (In the formula, R 1 and R 2 are each independently a hydrogen atom or an alkyl group having 1 to 8 carbon atoms; R 3 is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, or a cycloalkyl group having 3 to 12 carbon atoms.
4. The polarizer protective film according to claim 1 , wherein the acrylic resin composition has a content of structural units derived from aromatic vinyl of 0% by weight or more and 8% by weight or less.
5. The polarizer protective film according to claim 4 , wherein the acrylic resin composition has a content of structural units derived from styrene of 0% by weight or more and 8% by weight or less.
6. The polarizer protective film according to claim 1 , wherein the acrylic resin composition further contains polymethyl methacrylate or a methyl methacrylate-styrene copolymer.
7. The polarizer protective film according to claim 1 , wherein the acrylic resin composition has a 1% weight loss temperature of 300° C. or higher.
8. The polarizer protective film according to claim 1 , which does not contain an ultraviolet absorbing agent.
9. The polarizer protective film according to claim 1 , which is a biaxially stretched film.
10. The polarizer protective film according to claim 1 , having a yellowness index of 0.01 or more and 5.00 or less.
11. The polarizer protective film according to claim 1 , having an absorbance at a wavelength of 380 nm of 0.01 or more and 1.00 or less.
12. The absolute value of the Nz coefficient is 0.1 or more and 30.0 or less, a ratio Rth(447) / Rth(548) of a thickness direction retardation Rth(447) at a wavelength of 447 nm to a thickness direction retardation Rth(548) at a wavelength of 548 nm is 0.50 or more and 1.10 or less; 2. The polarizer protective film according to claim 1, wherein a ratio Rth(628) / Rth(548) of a thickness direction retardation Rth(628) at a wavelength of 628 nm to a thickness direction retardation Rth(548) at a wavelength of 548 nm is 0.50 or more and 2.00 or less.
13. A polarizing plate comprising the polarizer protective film according to claim 1 .
14. A liquid crystal panel comprising the polarizing plate according to claim 13.
Citation Information
Patent Citations
Acrylic film and method of manufacturing the same
JP2017025333A