Preparation method of super-hydrophobic high-temperature-resistant fluoride-free acrylic acid-silicon resin composite coating

Through the composite of fluorine-free acrylic resin and silicone resin and filling of modified zirconium dioxide particles, the environmental problems of fluorine materials in existing high-temperature hydrophobic coatings are solved, and the superhydrophobic and high-temperature resistance is improved, which is suitable for applications in multiple fields.

CN118931297AActive Publication Date: 2024-11-12BEIHANG UNIV

Patent Information

Application Number
CN202411179842.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Existing high-temperature hydrophobic coatings often contain fluorine systems that are harmful to the environment, and their heat resistance still has room for improvement, which limits its application areas.

Method used

Fluorine-free acrylic resin is used to combine with silicone resin, form a network structure with vinyl triethoxysilane and silicone resin, and fill it with modified zirconium dioxide particles to form a micro-nano structure, enhancing the hydrophobic and heat-resistant properties of the coating.

Benefits of technology

It has achieved superhydrophobic and high temperature-resistant fluorine-free coatings, with water contact angle greater than 150° and rolling angle less than 10°, and still maintains good hydrophobic performance at high temperature of 500°, which has environmental protection and wide application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931297A_ABST
    Figure CN118931297A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-temperature-resistant, super-hydrophobic and fluorine-free acrylic resin-silicon resin composite coating, and relates to the technical field of acrylic resin-silicon resin composite coatings, the high-temperature-resistant, super-hydrophobic and fluorine-free acrylic resin-silicon resin composite coating is mainly prepared from the following raw materials by mass: 3-10 parts of an acrylic resin emulsion; 3-10 parts of a silicon resin emulsion; 0.5 to 1.5 parts of modified zirconium dioxide with different particle sizes; 0.2 to 0.5 part of dispersant; and 3 to 10 parts of water. The adopted raw materials are environment-friendly substances, the surface energy is reduced through the synergistic effect of the raw materials, the hydrophobic modified zirconium dioxide nanoparticles are adopted for filling, a stable micro-nano structure is obtained by utilizing the good dispersity of the zirconium dioxide nanoparticles, and the heat resistance of the composite coating is improved by utilizing the good heat stability and oxidation resistance. The contact angle is increased; and the hydrophobic property is still kept after high temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of acrylic resin-silicone resin composite coatings, and in particular to a method for preparing a super-hydrophobic, high-temperature-resistant, fluorine-free acrylic resin-silicone resin composite coating. Background Art

[0002] Super hydrophobic surface refers to the surface with water contact angle greater than 150° and rolling angle less than 10°.

[0003] The huge application prospects in the fields of self-cleaning, anti-icing, anti-fogging and oil-water separation have attracted wide attention in basic science and practical applications. Acrylic resin-silicone resin composite coatings have excellent hydrophobicity, high temperature resistance and solvent resistance, and are widely used in the fields of automobiles, military industry and aerospace.

[0004] At present, the preparation of high temperature resistant hydrophobic coating generally adopts a single resin, and mostly contains environmentally harmful fluorine systems. For example, the patent with publication number CN11581466A discloses a method for obtaining high temperature resistant fluorocarbon super hydrophobic coating by in-situ cross-linking polymerization on the surface of perfluorobenzene sulfonate modified nano titanium dioxide, and the patent with publication number CN117362703A discloses a method for preparing hydrophobic nylon isolation membrane using nylon resin, high density polyethylene fluorocarbon mixture, phase stabilizer and fluorocarbon resin. Due to the presence of environmentally harmful fluorinated substances, its application field is limited, and heat resistance still has room for improvement. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention discloses a method for preparing a super-hydrophobic, high-temperature-resistant, fluorine-free acrylic resin-silicone resin composite coating, which is a resin composite system and has an environmentally friendly effect.

[0006] The complete technical solution of the present invention includes:

[0007] A method for preparing a super-hydrophobic, high-temperature-resistant, fluorine-free acrylic-silicone resin composite coating, comprising at least the steps of mixing acrylic resin emulsion, silicone resin emulsion and modified zirconium dioxide particles;

[0008] The acrylic resin emulsion and silicone resin emulsion do not contain fluorine elements, and the mixed monomers used in the preparation process of the acrylic resin emulsion at least include acrylate-terminated siloxane and vinyl triethoxysilane;

[0009] In the mixing step, vinyl triethoxysilane and silicone resin form a network structure, the modified zirconium dioxide particles fill the network structure, and the composite coating obtains a micro-nano structure. The modified zirconium dioxide particles are a combination of particles of different particle sizes, and the water contact angle on the surface of the composite coating is greater than 150° and the rolling angle is less than 10°.

[0010] In the preparation process of the acrylic-silicone resin composite coating of the present invention, the mixed monomers of the acrylic resin emulsion are acrylate-terminated siloxane and vinyl triethoxysilane.

[0011] The two functional monomers, acrylate-terminated siloxane and vinyl triethoxysilane, have good compatibility with acrylic monomers and good emulsification effect, making the product uniform and the emulsion stable after emulsion polymerization. Specifically, as a long-chain siloxane, acrylate-terminated siloxane has good leveling properties, and can reduce defects such as pores and ripples during film formation without adding a leveling agent, giving the resin excellent film-forming properties; at the same time, as a long-chain siloxane, it has extremely low surface energy and excellent heat resistance, so that the resin as a whole maintains a low surface energy and has good hydrophobic properties, and can still maintain hydrophobic properties after high temperatures.

[0012] Specifically for vinyl triethoxysilane: it has good thermal stability and provides cross-linking sites without the need to add cross-linking agents. It forms a cross-linked network structure through the hydrolysis and condensation of silicon to further increase thermal stability while providing a carrier for the nanoparticles.

[0013] Preferably, the raw materials of the composite coating also include dispersant and water, and the raw material ratio is: 3-10 parts of acrylic resin emulsion, 3-10 parts of silicone resin emulsion, 0.5-1.5 parts of modified zirconium dioxide, 0.2-0.5 parts of dispersant, and 3-10 parts of water, and the above proportions are in parts by weight.

[0014] Furthermore, the preparation method of the super hydrophobic high temperature resistant fluorine-free acrylic-silicone resin composite coating specifically comprises the following steps:

[0015] S1. Weigh the acrylic resin emulsion, the silicone resin emulsion and water, stir and mix to obtain a composite resin;

[0016] S2. Weigh modified zirconium dioxide and dispersant of different particle sizes, add them to the composite resin, and mix them by ball milling to obtain a high temperature resistant, super hydrophobic, fluorine-free acrylic resin-silicone resin composite coating.

[0017] Furthermore, in S1, the stirring and mixing is: stirring at a rotation speed of 400 r / min for 1 h.

[0018] Furthermore, in S2, the ball milling speed is 400 r / min, and the ball milling is maintained for 3 h.

[0019] Preferably, the acrylic resin emulsion is prepared by mixing monomers, initiators, emulsifiers and water in the following proportions: 20-40 parts of mixed monomers, 0.2-0.3 parts of initiators, 0.3-1 parts of emulsifiers; and 30-60 parts of water.

[0020] Preferably, the mixed monomer further comprises methyl methacrylate, butyl acrylate, methacrylic acid, hydroxyethyl methacrylate; the initiator is ammonium persulfate or potassium persulfate; the emulsifier comprises: polyoxyethylene octylphenol ether-10 and nonylphenol polyoxyethylene ether ammonium sulfate.

[0021] Furthermore, the preparation method of the acrylic resin emulsion specifically comprises the following steps:

[0022] (1) weighing methyl methacrylate, butyl acrylate, methacrylic acid, hydroxyethyl methacrylate, acrylate-terminated siloxane, vinyl triethoxysilane and water, stirring and mixing to obtain a mixture A;

[0023] (2) weighing an emulsifier, slowly adding it to the stirred mixture A, and continuing to stir to obtain a prepolymer emulsion;

[0024] (3) Weigh an initiator, slowly add it dropwise to the prepolymer emulsion which is kept in a stirring state, and continue stirring to obtain an acrylic resin emulsion.

[0025] Furthermore, in step (1), the stirring and mixing method is: stirring at a rotation speed of 400 r / min for 20 min.

[0026] Furthermore, in step (2), stirring is performed at a rotation speed of 600 r / min for 1 h.

[0027] Furthermore, in step (3), the stirring mixing speed is maintained at 300 r / min and the temperature is maintained at 75°C.

[0028] Preferably, the silicone resin emulsion comprises: 8 to 15 parts of mixed monomers; 0.3 to 0.5 parts of catalysts; 0.3 to 1 parts of emulsifiers; and 15 to 20 parts of water, wherein the mixed monomers are methyltriethoxysilane, phenyltriethoxysilane, and dimethyldimethoxysilane; the catalyst is sodium hydroxide or ammonia water; and the emulsifier is fatty alcohol polyoxyethylene ether.

[0029] Furthermore, the preparation method of the silicone resin emulsion comprises the following steps:

[0030] 1) Weigh an emulsifier, a catalyst and water, and stir and mix to obtain a mixture B;

[0031] 2) Weigh methyltriethoxysilane, phenyltriethoxysilane and dimethyldimethoxysilane, add them to the stirred mixture B, and continue stirring to obtain a silicone resin emulsion.

[0032] Furthermore, in step 1), the stirring and mixing method is: stirring at a rotation speed of 400 r / min for 20 min.

[0033] Furthermore, in step 2), the stirring mixing speed is maintained at 400 r / min and the temperature is maintained at 60°C.

[0034] Preferably, the modified zirconium dioxide particles have a combination of particles of different particle sizes: the ratio of nanometer-scale zirconium dioxide to micrometer-scale zirconium dioxide is 1:1.

[0035] Preferably, the nano-scale zirconium dioxide particle size is 100 nm or less; the micro-scale zirconium dioxide particle size is 1 μm or more.

[0036] In the preparation process of the acrylic-silicone resin composite coating of the present invention, modified zirconium dioxide particles with different particle sizes are used. Firstly, zirconium dioxide has the characteristics of high melting point and low thermal expansion coefficient, and its thermal stability is better than that of conventional inorganic filler silica, which helps it to maintain its micro-nano structure and super-hydrophobic properties after high temperature.

[0037] At the same time, the study found that the rolling angle, advancing angle and receding angle of the super-hydrophobic surface are controlled by the microstructure. The present invention has studied the ratio of nanoparticles of different particle sizes, and found that when the ratio of micron or nanometer-scale zirconium dioxide particles is too large, it will cause the zirconium dioxide particles of another scale to be too far apart, which is conducive to the transition of the Cassie-Wenzel state of the droplet on the super-hydrophobic surface, greatly increasing the rolling angle, which is not conducive to the formation of the super-hydrophobic surface. After analysis and experimental verification, it is determined that when the ratio of nanoscale zirconium dioxide (particle size below 100nm) to micron-scale (particle size above 1μm) zirconium dioxide is 1:1, it is most suitable, and both a higher contact angle and a lower rolling angle can be obtained.

[0038] Preferably, the modified preparation method of the modified zirconium dioxide particles is: zirconium dioxide of different particle sizes, methyltriethoxysilane, ammonia water, and anhydrous ethanol are mixed and stirred in a mass ratio of 5:5:1:20, and modified zirconium dioxide of different particle sizes is obtained by filtering, washing, and drying.

[0039] Preferably, during the modification preparation process of the modified zirconium dioxide particles, the stirring speed is maintained at 400 r / min and the stirring time is maintained at 12 h.

[0040] The super-hydrophobic high-temperature-resistant fluorine-free acrylic-silicone resin composite coating obtained by the method has a water contact angle greater than 150°.

[0041] Preferably, the water contact angle of the composite coating is greater than 150° after being kept at a high temperature of 500° C. for 12 hours.

[0042] Preferably, the dispersant is an organosilicon dispersant.

[0043] The advantages of the present invention over the prior art are:

[0044] 1. The raw materials used in the present invention are environmentally friendly fluorine-free substances, which are superior to fluorine-containing resins or fluorocarbon resins. The present application utilizes methyl methacrylate, butyl acrylate, methacrylic acid, hydroxyethyl methacrylate, acrylate-terminated siloxane and vinyl triethoxysilane to polymerize to obtain an acrylic resin emulsion, methyl triethoxysilane, phenyl triethoxysilane and dimethyl dimethoxysilane are hydrolyzed and condensed to obtain a silicone resin emulsion, the two resin emulsions are mixed, and zirconium dioxide of different particle sizes modified by methyl triethoxysilane is filled into the composite resin emulsion, the surface energy is reduced from different angles, a micro-nano structure is obtained, the contact angle is increased, and the super-hydrophobic property of the coating is increased in synergy.

[0045] 2. The present invention introduces vinyl triethoxysilane monomer into acrylic resin, which can form a network structure with silicone resin during curing, thereby improving the heat resistance of the composite resin and providing a carrier for subsequent fillers.

[0046] 3. The present invention uses hydrophobically modified zirconium dioxide nanoparticles for filling, which can not only utilize the good dispersibility of the hydrophobically modified nanoparticles to obtain a stable micro-nano structure, but also utilize the good thermal stability and oxidation resistance of zirconium dioxide to improve the heat resistance of the composite coating, so that the composite coating still maintains hydrophobic properties after high temperature.

[0047] 4. The preparation method of the present invention is simple and utilizes the synergistic effect between various materials. The obtained acrylic resin-silicone resin composite coating is environmentally friendly and pollution-free. At the same time, it has good heat resistance and hydrophobicity. After a heat resistance test of 500°C for 12 hours, it still maintains good hydrophobicity and has application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 Graphs of surface water contact angles of uncoated glass sheets and super-hydrophobic coatings obtained in Examples 1 to 4;

[0049] Figure 2 is the surface water contact angle of the uncoated glass sheet and the super-hydrophobic coating obtained in Example 1, Comparative Example 1, and Comparative Example 2;

[0050] Figure 3 It is the surface water contact angle of the super hydrophobic coating obtained in Example 1 after being subjected to a high temperature test at 500°C. DETAILED DESCRIPTION

[0051] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0052] Unless otherwise specified, the experimental materials and reagents used in the following examples can be obtained through commercial channels.

[0053] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0054] Example 1

[0055] The super-hydrophobic, high-temperature-resistant, fluorine-free acrylic resin-silicone resin composite coating has the following raw material proportions: 50 g acrylic resin emulsion, 50 g silicone resin emulsion, 10 g modified zirconium dioxide of different particle sizes, 1 g dispersant and 50 g water.

[0056] The preparation method is as follows:

[0057] S1. Preparation of acrylic resin emulsion: 10 g of methyl methacrylate, 10 g of butyl acrylate, 1 g of methacrylic acid, 1 g of hydroxyethyl methacrylate, 2 g of acrylate-terminated siloxane, 1 g of vinyl triethoxysilane and 40 g of water were added to a flask and stirred at 400 r / min for 20 min, then 1 g of emulsifier was added and stirred at 600 r / min for 1 h, then 0.3 g of initiator was added, the temperature was maintained at 75° C. and stirred at 300 r / min for 4 h to obtain an acrylic resin emulsion;

[0058] S2. Preparation of silicone resin emulsion: 1 g of emulsifier, 0.5 g of catalyst and 40 g of water were added to a flask and stirred at 400 r / min for 20 min, then 9 g of methyltriethoxysilane, 15 g of phenyltriethoxysilane and 6 g of dimethyldimethoxysilane were added, the temperature was maintained at 60 ° C and the reaction was carried out at a speed of 400 r / m for 3 h to obtain a silicone resin emulsion;

[0059] S3. Preparation of modified zirconium dioxide of different particle sizes: 5 g of zirconium dioxide of different particle sizes, 5 g of methyltriethoxysilane, 1 g of aqueous ammonia and 20 g of anhydrous ethanol were added to a flask and stirred at 400 r / min for 12 h, and then filtered, washed and dried to obtain modified zirconium dioxide of different particle sizes;

[0060] S4. Preparation of super-hydrophobic, high-temperature resistant, fluorine-free acrylic resin-silicone resin composite coating: Add 50g of acrylic resin emulsion and 50g of silicone resin emulsion into a beaker and stir at 400r / min for 1h to obtain a composite resin; then add the composite resin, 10g of modified zirconium dioxide of different particle sizes, 1g of dispersant and 50g of water into a ball mill and ball mill at 400r / min for 3h to obtain a super-hydrophobic, high-temperature resistant, fluorine-free acrylic resin-silicone resin composite coating.

[0061] The water contact angle of the acrylic resin-silicone resin composite coating obtained in this embodiment reached 161.1°. Figure 1 As shown in Figure 1, super hydrophobicity is achieved, and the contact angle is 156.8° after being kept at a high temperature of 500°C for 12 hours. The specific performance is shown in Table 1.

[0062] Example 2

[0063] The super-hydrophobic, high temperature resistant, fluorine-free acrylic resin-silicone resin composite coating has the following raw material proportions: 30 g acrylic resin emulsion, 70 g silicone resin emulsion, 10 g modified zirconium dioxide of different particle sizes, 1 g dispersant and 50 g water.

[0064] The preparation method is as follows:

[0065] S1. Preparation of acrylic resin emulsion: 10 g of methyl methacrylate, 10 g of butyl acrylate, 1 g of methacrylic acid, 1 g of hydroxyethyl methacrylate, 2 g of acrylate-terminated siloxane, 1 g of vinyl triethoxysilane and 40 g of water were added to a flask and stirred at 400 r / min for 20 min, then 1 g of emulsifier was added and stirred at 600 r / min for 1 h, then 0.3 g of initiator was added, the temperature was maintained at 75° C. and stirred at 300 r / min for 4 h to obtain an acrylic resin emulsion;

[0066] S2. Preparation of silicone resin emulsion: 1 g of emulsifier, 0.5 g of catalyst and 40 g of water were added to a flask and stirred at 400 r / min for 20 min, then 9 g of methyltriethoxysilane, 15 g of phenyltriethoxysilane and 6 g of dimethyldimethoxysilane were added, the temperature was maintained at 60 ° C and the reaction was carried out at a speed of 400 r / m for 3 h to obtain a silicone resin emulsion;

[0067] S3. Preparation of modified zirconium dioxide of different particle sizes: 5 g of zirconium dioxide of different particle sizes, 5 g of methyltriethoxysilane, 1 g of aqueous ammonia and 20 g of anhydrous ethanol were added to a flask and stirred at 400 r / min for 12 h, and then filtered, washed and dried to obtain modified zirconium dioxide of different particle sizes;

[0068] S4. Preparation of super-hydrophobic, high-temperature resistant, fluorine-free acrylic resin-silicone resin composite coating: Add 30g of acrylic resin emulsion and 70g of silicone resin emulsion into a beaker and stir at 400r / min for 1h to obtain a composite resin; then add the composite resin, 10g of modified zirconium dioxide of different particle sizes, 1g of dispersant and 50g of water into a ball mill and ball mill at 400r / min for 3h to obtain a super-hydrophobic, high-temperature resistant, fluorine-free acrylic resin-silicone resin composite coating.

[0069] The water contact angle of the acrylic resin-silicone resin composite coating obtained in this embodiment reached 154.1°, achieving super hydrophobicity, and the contact angle was 147.2° after being kept at a high temperature of 500° C. for 12 hours. The specific properties are shown in Table 1.

[0070] Example 3

[0071] The super-hydrophobic, high temperature resistant, fluorine-free acrylic resin-silicone resin composite coating has the following raw material proportions: 70 g acrylic resin emulsion, 30 g silicone resin emulsion, 10 g modified zirconium dioxide of different particle sizes, 1 g dispersant and 50 g water.

[0072] The preparation method is as follows:

[0073] S1. Preparation of acrylic resin emulsion: 10 g of methyl methacrylate, 10 g of butyl acrylate, 1 g of methacrylic acid, 1 g of hydroxyethyl methacrylate, 2 g of acrylate-terminated siloxane, 1 g of vinyl triethoxysilane and 40 g of water were added to a flask and stirred at 400 r / min for 20 min, then 1 g of emulsifier was added and stirred at 600 r / min for 1 h, then 0.3 g of initiator was added, the temperature was maintained at 75° C. and stirred at 300 r / min for 4 h to obtain an acrylic resin emulsion;

[0074] S2. Preparation of silicone resin emulsion: 1 g of emulsifier, 0.5 g of catalyst and 40 g of water were added to a flask and stirred at 400 r / min for 20 min, then 9 g of methyltriethoxysilane, 15 g of phenyltriethoxysilane and 6 g of dimethyldimethoxysilane were added, the temperature was maintained at 60 ° C and the reaction was carried out at a speed of 400 r / m for 3 h to obtain a silicone resin emulsion;

[0075] S3. Preparation of modified zirconium dioxide of different particle sizes: 5 g of zirconium dioxide of different particle sizes, 5 g of methyltriethoxysilane, 1 g of aqueous ammonia and 20 g of anhydrous ethanol were added to a flask and stirred at 400 r / min for 12 h, and then filtered, washed and dried to obtain modified zirconium dioxide of different particle sizes;

[0076] S4. Preparation of super-hydrophobic, high-temperature resistant, fluorine-free acrylic resin-silicone resin composite coating: Add 70g of acrylic resin emulsion and 30g of silicone resin emulsion into a beaker and stir at 400r / min for 1h to obtain a composite resin; then add the composite resin, 10g of modified zirconium dioxide of different particle sizes, 1g of dispersant and 50g of water into a ball mill and ball mill at 400r / min for 3h to obtain a super-hydrophobic, high-temperature resistant, fluorine-free acrylic resin-silicone resin composite coating.

[0077] The water contact angle of the acrylic resin-silicone resin composite coating obtained in this embodiment reached 159.5°, achieving super hydrophobicity, and the contact angle was 154.6° after being kept at a high temperature of 500° C. for 12 hours. The specific properties are shown in Table 1.

[0078] Example 4

[0079] The super-hydrophobic, high-temperature-resistant, fluorine-free acrylic resin-silicone resin composite coating has the following raw material proportions: 50 g acrylic resin emulsion, 50 g silicone resin emulsion, 12.5 g modified zirconium dioxide of different particle sizes, 1 g dispersant and 50 g water.

[0080] The preparation method is as follows:

[0081] S1. Preparation of acrylic resin emulsion: 10 g of methyl methacrylate, 10 g of butyl acrylate, 1 g of methacrylic acid, 1 g of hydroxyethyl methacrylate, 2 g of acrylate-terminated siloxane, 1 g of vinyl triethoxysilane and 40 g of water were added to a flask and stirred at 400 r / min for 20 min, then 1 g of emulsifier was added and stirred at 600 r / min for 1 h, then 0.3 g of initiator was added, the temperature was maintained at 75° C. and stirred at 300 r / min for 4 h to obtain an acrylic resin emulsion;

[0082] S2. Preparation of silicone resin emulsion: 1 g of emulsifier, 0.5 g of catalyst and 40 g of water were added to a flask and stirred at 400 r / min for 20 min, then 9 g of methyltriethoxysilane, 15 g of phenyltriethoxysilane and 6 g of dimethyldimethoxysilane were added, the temperature was maintained at 60 ° C and the reaction was carried out at a speed of 400 r / m for 3 h to obtain a silicone resin emulsion;

[0083] S3. Preparation of modified zirconium dioxide of different particle sizes: 5 g of zirconium dioxide of different particle sizes, 5 g of methyltriethoxysilane, 1 g of aqueous ammonia and 20 g of anhydrous ethanol were added to a flask and stirred at 400 r / min for 12 h, and then filtered, washed and dried to obtain modified zirconium dioxide of different particle sizes;

[0084] S4. Preparation of super-hydrophobic, high-temperature resistant, fluorine-free acrylic resin-silicone resin composite coating: Add 50g of acrylic resin emulsion and 50g of silicone resin emulsion into a beaker and stir at 400r / min for 1h to obtain a composite resin; then add the composite resin, 12.5g of modified zirconium dioxide of different particle sizes, 1g of dispersant and 50g of water into a ball mill and ball mill at 400r / min for 3h to obtain a super-hydrophobic, high-temperature resistant, fluorine-free acrylic resin-silicone resin composite coating.

[0085] The water contact angle of the acrylic resin-silicone resin composite coating obtained in this embodiment reached 161.7°, achieving super hydrophobicity, and the contact angle was 157.4° after being kept at a high temperature of 500° C. for 12 hours. The specific properties are shown in Table 1.

[0086] Comparative Example 1

[0087] The acrylic resin-silicone resin composite coating has the following raw material proportions: 50 g acrylic resin emulsion, 50 g silicone resin emulsion, 1 g dispersant and 50 g water.

[0088] The preparation method is as follows:

[0089] S1. Preparation of acrylic resin emulsion: 10 g of methyl methacrylate, 10 g of butyl acrylate, 1 g of methacrylic acid, 1 g of hydroxyethyl methacrylate, 2 g of acrylate-terminated siloxane, 1 g of vinyl triethoxysilane and 40 g of water were added to a flask and stirred at 400 r / min for 20 min, then 1 g of emulsifier was added and stirred at 600 r / min for 1 h, then 0.3 g of initiator was added, the temperature was maintained at 75° C. and stirred at 300 r / min for 4 h to obtain an acrylic resin emulsion;

[0090] S2. Preparation of silicone resin emulsion: 1 g of emulsifier, 0.5 g of catalyst and 40 g of water were added to a flask and stirred at 400 r / min for 20 min, then 9 g of methyltriethoxysilane, 15 g of phenyltriethoxysilane and 6 g of dimethyldimethoxysilane were added, the temperature was maintained at 60 ° C and the reaction was carried out at a speed of 400 r / m for 3 h to obtain a silicone resin emulsion;

[0091] S3. Preparation of acrylic resin-silicone resin composite coating: Add 50g acrylic resin emulsion and 50g silicone resin emulsion into a beaker and stir at 400r / min for 1h to obtain a composite resin. Then add the composite resin, 1g dispersant and 50g water into a ball mill and ball mill at 400r / min for 3h to obtain an acrylic resin-silicone resin composite coating.

[0092] The difference between this comparative example and Example 1 is that modified zirconium dioxide with different particle sizes is not added.

[0093] The water contact angle of the acrylic resin-silicone resin composite coating obtained in this comparative example reached 101.0°. Figure 2 As shown in Figure 1, the contact angle is 105.2° after being kept at a high temperature of 500°C for 12 hours. The specific properties are shown in Table 1.

[0094] Comparative Example 2

[0095] The acrylic resin-silicone resin composite coating has the following raw material proportions: 50 g acrylic resin emulsion, 50 g silicone resin emulsion, 10 g modified zirconium dioxide with a single particle size, 1 g dispersant and 50 g water.

[0096] The preparation method is as follows:

[0097] S1. Preparation of acrylic resin emulsion: 10 g of methyl methacrylate, 10 g of butyl acrylate, 1 g of methacrylic acid, 1 g of hydroxyethyl methacrylate, 2 g of acrylate-terminated siloxane, 1 g of vinyl triethoxysilane and 40 g of water were added to a flask and stirred at 400 r / min for 20 min, then 1 g of emulsifier was added and stirred at 600 r / min for 1 h, then 0.3 g of initiator was added, the temperature was maintained at 75° C. and stirred at 300 r / min for 4 h to obtain an acrylic resin emulsion;

[0098] S2. Preparation of silicone resin emulsion: 1 g of emulsifier, 0.5 g of catalyst and 40 g of water were added to a flask and stirred at 400 r / min for 20 min, then 9 g of methyltriethoxysilane, 15 g of phenyltriethoxysilane and 6 g of dimethyldimethoxysilane were added, the temperature was maintained at 60 ° C and the reaction was carried out at a speed of 400 r / m for 3 h to obtain a silicone resin emulsion;

[0099] S3. Preparation of modified zirconium dioxide of a single particle size: 5 g of zirconium dioxide of a single particle size, 5 g of methyltriethoxysilane, 1 g of aqueous ammonia and 20 g of anhydrous ethanol were added to a flask and stirred at 400 r / min for 12 h, and then filtered, washed and dried to obtain a single particle size of modified zirconium dioxide;

[0100] S4. Preparation of acrylic resin-silicone resin composite coating: Add 50g acrylic resin emulsion and 50g silicone resin emulsion into a beaker and stir at 400r / min for 1h to obtain a composite resin; then add the composite resin, 10g modified zirconium dioxide of a single particle size, 1g dispersant and 50g water into a ball mill and ball mill at 400r / min for 3h to obtain an acrylic resin-silicone resin composite coating.

[0101] The difference between this comparative example and Example 1 is that modified zirconium dioxide with a single particle size is added.

[0102] The water contact angle of the acrylic resin-silicone resin composite coating obtained in this comparative example reached 122.2°. Figure 2 As shown in Figure 1, the contact angle is 111.2° after being kept at a high temperature of 500°C for 12 hours. The specific properties are shown in Table 1.

[0103] Table 1 Performance changes of various embodiments and comparative examples under different treatment conditions

[0104] Sample Water contact angle / ° Water contact angle / °(500℃-12h) Example 1 161.1 156.8 Example 2 154.1 147.2 Example 3 159.5 154.6 Example 4 161.7 157.4 Comparative Example 1 101.0 105.2 Comparative Example 2 122.2 111.2

[0105] The test standard for water contact angle is GB / T 30693-2014. The acrylic resin-silicone resin composite coating obtained by the present invention has good hydrophobicity and heat resistance. After spraying the coating to make a sample, it was found that after being placed in a high temperature environment of 500°C for 12 hours, it still maintained good hydrophobicity. Figure 3 As shown, it has broad application prospects.

[0106] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for preparing a super-hydrophobic, high-temperature-resistant, fluorine-free acrylic-silicone resin composite coating, characterized in that: The preparation method at least comprises the steps of mixing acrylic resin emulsion, silicone resin emulsion and modified zirconium dioxide particles; The acrylic resin emulsion and silicone resin emulsion do not contain fluorine elements, and the mixed monomers used in the preparation process of the acrylic resin emulsion at least include acrylate-terminated siloxane and vinyl triethoxysilane; In the mixing step, vinyl triethoxysilane and silicone resin form a network structure, the modified zirconium dioxide particles fill the network structure, and the composite coating obtains a micro-nano structure. The modified zirconium dioxide particles are a combination of particles of different particle sizes, and the water contact angle on the surface of the composite coating is greater than 150° and the rolling angle is less than 10°.

2. The method for preparing a super-hydrophobic high temperature resistant fluorine-free acrylic-silicone resin composite coating according to claim 1, characterized in that: The raw materials of the composite coating also include dispersant and water, and the raw material ratio is: 3-10 parts of acrylic resin emulsion, 3-10 parts of silicone resin emulsion, 0.5-1.5 parts of modified zirconium dioxide, 0.2-0.5 parts of dispersant, and 3-10 parts of water, and the above proportions are by weight.

3. The method for preparing a super-hydrophobic high temperature resistant fluorine-free acrylic-silicone resin composite coating according to claim 2, characterized in that: The acrylic resin emulsion is prepared by using mixed monomers, initiators, emulsifiers and water in the following proportions: 20-40 parts of mixed monomers, 0.2-0.3 parts of initiators, 0.3-1 parts of emulsifiers, and 30-60 parts of water.

4. The method for preparing a super-hydrophobic high temperature resistant fluorine-free acrylic-silicone resin composite coating according to claim 3, characterized in that: The mixed monomers also include methyl methacrylate, butyl acrylate, methacrylic acid, and hydroxyethyl methacrylate; the initiator is ammonium persulfate or potassium persulfate, and the emulsifier includes polyoxyethylene octylphenol ether-10 and nonylphenol polyoxyethylene ether ammonium sulfate.

5. The method for preparing a super-hydrophobic high temperature resistant fluorine-free acrylic-silicone resin composite coating according to claim 2, characterized in that, The silicone resin emulsion comprises: 8-15 parts of mixed monomers; 0.3-0.5 parts of catalysts; 0.3-1 parts of emulsifiers; and 15-20 parts of water. The mixed monomers are methyltriethoxysilane, phenyltriethoxysilane, and dimethyldimethoxysilane; the catalyst is sodium hydroxide or ammonia water; and the emulsifier is fatty alcohol polyoxyethylene ether.

6. The method for preparing a super-hydrophobic high temperature resistant fluorine-free acrylic-silicone resin composite coating according to claim 1, characterized in that: The modified zirconium dioxide particles have a combination of particles of different particle sizes: the ratio of nanometer-scale zirconium dioxide to micrometer-scale zirconium dioxide is 1:

1.

7. The method for preparing a super-hydrophobic high temperature resistant fluorine-free acrylic-silicone resin composite coating according to claim 6, characterized in that: The nanometer-scale zirconium dioxide particle size is 100 nm or less; the micrometer-scale zirconium dioxide particle size is 1 μm or more.

8. The method for preparing a super-hydrophobic high temperature resistant fluorine-free acrylic-silicone resin composite coating according to claim 7, characterized in that: The modified preparation method of the modified zirconium dioxide particles is: zirconium dioxide with different particle sizes, methyltriethoxysilane, ammonia water, and anhydrous ethanol are mixed and stirred in a mass ratio of 5:5:1:20, and the modified zirconium dioxide with different particle sizes is obtained by filtering, washing, and drying.

9. A super-hydrophobic, high temperature resistant, fluorine-free acrylic-silicone resin composite coating obtained by the method according to any one of claims 1 to 8, characterized in that: The water contact angle of the composite coating is greater than 150°.

10. The super-hydrophobic high temperature resistant fluorine-free acrylic-silicone resin composite coating according to claim 9, characterized in that: After the composite coating is kept at a high temperature of 500° C. for 12 hours, the water contact angle is greater than 150°.

Citation Information

Patent Citations

  • Fluorine-silicon acrylic resin nano composite anti-icing coating and preparation method thereof

    CN102321415A

  • Super-hydrophobic anticorrosive coating used for power transmission and transformation devices, and preparation method thereof

    CN106519955A

  • Nano high-temperature-resistant heat-insulating coating

    CN108715731A

  • Composite thermal-insulating heat-preservation environmental-friendly coating

    CN108727978A

  • Water-based silicone modified high-hardness hydrophobic UV insulating paint

    CN109294417A

Cited By

  • Fluorine-free wear-resistant super-hydrophobic coating capable of being applied to heat exchanger and preparation method thereof

    CN119752268A

  • Low-water-vapor-transmittance coating for packaging material and preparation method of low-water-vapor-transmittance coating

    CN121471801A

  • A low water vapor transmission rate coating for packaging material and a method for preparing the same

    CN121471801B