Crystalline gel and production method, polymer, and article

By crosslinking multifunctional polymers to form a three-dimensional network and stretching them, the crystalline gel achieves periodic crystal domains and enhanced fracture strength, addressing the limitations of existing methods in size and structure periodicity, enabling large-scale applications in filtration, drug release, electronics, and optics.

JP2024144370APending Publication Date: 2024-10-11HOKKAIDO UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024053626
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-28
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing methods for forming three-dimensional structures with nanometer resolution, such as nanolithography and metal-organic structures, are limited in size and struggle to construct larger structures, and crystallized gels with disordered polymer chains lack periodicity and structural defects, limiting their crystalline domains to small sizes and reduced fracture strength.

Method used

A crystalline gel is created by crosslinking multifunctional polymers with two or more functional groups to form a three-dimensional network structure, which is then stretched to achieve periodic crystal domains, using hyperbranched or linear polymers with specific molecular weights and functional groups, and a solvent to enhance crystallization.

Benefits of technology

The resulting crystalline gel exhibits a highly ordered structure with periodic crystal domains, improved fracture strength, and anisotropic properties, allowing for large-scale production and applications in filtration, drug release, electronics, and optics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144370000001_ABST
    Figure 2024144370000001_ABST
Patent Text Reader

Abstract

To provide crystalline gel which is crystallized, and has a structure having high order.SOLUTION: There is provided crystalline gel including: a cross linkage polymer where, a poly functional polymer having two or more functional groups is cross linked so as to form a three-dimensional network structure; and a solvent. A part of the cross linkage polymer is crystallized, and in a two-dimensional image where a small angle X-ray scattering is detected, when an extension direction is set as an equator direction, there is a streak extending from a beam center to a meridian direction in a range where, a size of a scattering vector is 0.001 to 0.5 Å-1, one or more scattering images having a peak at a position symmetric to the meridian, exist on the equator, and crystalline domains periodically exist.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a crystalline gel, a method for producing a crystalline gel, a polymer obtained from the crystalline gel, and an article containing the crystalline gel or the polymer. [Background technology]

[0002] Ordered three-dimensional network structures containing nanopores are important for a wide range of applications including filtration, sensing, drug release, electronics and optics. Methods for forming precise structures with nanometer resolution include nanolithography and metal-organic frameworks, but the size of the entire structure is only a few μm. 3 Even current technology is still limited in the scale at which it can be manufactured, so it is limited to a size that can be handled by hand (e.g. 1 cm 3 It is extremely difficult to construct a three-dimensional structure of this size.

[0003] Gels are made by cross-linking polymers in a solvent to form a three-dimensional mesh-like polymer that retains solvents such as water inside. Although they are materials with nanopores, they have the advantage that they can be grown through simple chemical synthesis to a size that can be handled by hand. It has been reported that when a gel is stretched, polymer chains are oriented in the gel, and stretch-induced crystallization occurs. For example, Non-Patent Document 1 describes that when a tri-branched gel in which a tri-branched polymer is crosslinked is stretched, the stretch ratio until breakage is higher than when a tetra-branched gel is stretched, and the formation of microcrystals due to stretching was confirmed by measurements using small-angle X-ray scattering (SAXS) and wide-angle X-ray scattering (WAXS). [Prior art documents] [Non-patent literature]

[0004] [Non-Patent Document 1] Takeshi Fujiyabu et al., 'Tri-branched gels: Rubbery materials with the lowest branching factor approach the ideal elastic limit', Science Advances, 8, DOI:10.1126 / sciadv.abk0010, April 6, 2022 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the small-angle X-ray scattering measurement of the crystallized gel described in Non-Patent Document 1, only streaks that are seen when the polymer gel is stretched and the polymer chains are oriented are observed, and no scattering spots showing periodicity between crystalline domains are observed. Moreover, in the wide-angle X-ray scattering measurement, only two scattering spots are observed, indicating that they are minute crystalline domains of a few nanometers in size. Gels have a random cross-linked structure of polymer chains and a considerable amount of structural defects, so the crystal domains formed by stretching are small and are thought to be arranged without periodicity. Therefore, the advantage of crystallized gels is limited to improved breaking strength. An object of the present invention is to provide a crystalline gel which has a highly ordered structure despite being a crystallized gel. [Means for solving the problem]

[0006] The present invention has the following aspects. [1] A crystalline gel comprising a crosslinked polymer in which a multifunctional polymer having two or more functional groups is crosslinked to form a three-dimensional network structure, and a solvent, in which a portion of the crosslinked polymer is crystallized and crystalline domains exist periodically. [2] The crystalline gel according to [1], wherein the crosslinked polymer comprises at least one selected from the group consisting of crosslinked polymers in which one or more types of P1 are crosslinked, crosslinked polymers in which one or more types of P1 are crosslinked with one or more types of P2, crosslinked polymers in which one or more types of P1 are crosslinked with one or more types of Q1, crosslinked polymers in which one or more types of P1 are crosslinked with one or more types of Q2, and crosslinked polymers in which one or more types of P2 are crosslinked with one or more types of Q1. P1: A hyperbranched polymer having three or more functional groups and a branching point with three or more branched chains. P2: A linear polymer that has no branching points with three or more branches and has two functional groups. Q1: A branched monomer having three or more functional groups. Q2: A bifunctional monomer having two functional groups. [3] The crystalline gel described in [1] or [2], wherein the concentration of the crosslinked polymer in the crystalline gel is equal to or higher than the concentration at which adjacent crosslinked multifunctional polymers overlap with each other. [4] The crystalline gel according to any one of [1] to [3], wherein the polyfunctional polymer is one or both of a hyperbranched polymer having a branch point with three or more branched chains, three or more functional groups, and a weight-average molecular weight per branch chain of 500 to 100,000, and a linear polymer having no branch point with three or more branched chains, two functional groups, and a weight-average molecular weight of 500 to 100,000. [5] The crystalline gel according to any one of [1] to [4], wherein the solvent is a good solvent for the multifunctional polymer. [6] A crystalline gel containing a crosslinked polymer in which a multifunctional polymer having two or more functional groups is crosslinked to form a three-dimensional network structure and a solvent, and crystallized by stretching, in which, in a two-dimensional image in which small-angle X-ray scattering is detected, the magnitude of the scattering vector is 0.001 to 0.5 Å when the stretching direction is the equator direction. -1 A crystalline gel in which, within the range, there is a streak extending from the beam center in the meridian direction and, at the equator, there is one or more pairs of scattering images having peaks at positions symmetrical with respect to the meridian. [7] A crystalline gel containing a crosslinked polymer in which a multifunctional polymer having two or more functional groups is crosslinked to form a three-dimensional network structure and a solvent, and crystallized by stretching, in which the magnitude of the scattering vector is 0.5 to 3.0 Å in a two-dimensional image obtained by detecting wide-angle X-ray scattering. -1 Crystalline gel with more than 20 scattering spots in the range. [8] A polymer obtained by reducing or removing the solvent from the crystalline gel according to any one of [1] to [7] above. [9] A method for producing a crystalline gel in which crystalline domains exist periodically, the method comprising: stretching an unstretched gel containing a crosslinked polymer in which a multifunctional polymer having two or more functional groups is crosslinked to form a three-dimensional mesh structure, and a solvent, the gel having a concentration of the crosslinked polymer equal to or higher than the concentration at which adjacent multifunctional polymers among the crosslinked multifunctional polymers overlap with each other, so that part of the crosslinked polymer crystallizes.

[10] The method for producing a crystalline gel according to [9], wherein the crosslinked polymer comprises at least one selected from the group consisting of crosslinked polymers in which one or more types of P1 are crosslinked, crosslinked polymers in which one or more types of P1 are crosslinked with one or more types of P2, crosslinked polymers in which one or more types of P1 are crosslinked with one or more types of Q1, crosslinked polymers in which one or more types of P1 are crosslinked with one or more types of Q2, and crosslinked polymers in which one or more types of P2 are crosslinked with one or more types of Q1. P1: A hyperbranched polymer having three or more functional groups and a branching point with three or more branched chains. P2: A linear polymer that has no branching points with three or more branches and has two functional groups. Q1: A branched monomer having three or more functional groups. Q2: A bifunctional monomer having two functional groups.

[11] The method for producing a crystalline gel according to [9] or

[10] , wherein the polyfunctional polymer is one or both of a hyperbranched polymer having a branch point with three or more branched chains, three or more functional groups, and a weight-average molecular weight per branch chain of 500 to 100,000, and a linear polymer having no branch point with three or more branched chains, two functional groups, and a weight-average molecular weight of 500 to 100,000.

[12] The method for producing a crystalline gel according to any one of [9] to

[11] , wherein the solvent is a good solvent for the multifunctional polymer.

[13] An article comprising the crystalline gel described in any one of [1] to [7] above.

[14] An article comprising the polymeric substance described in [8]. Effect of the Invention

[0007] According to the present invention, a crystalline gel can be obtained which has a highly ordered structure in which crystal domains exist periodically, even though it is a crystallized gel. [Brief description of the drawings]

[0008] [Figure 1] 1 is a two-dimensional image showing the results of measuring small-angle X-ray scattering (SAXS) and wide-angle X-ray scattering (WAXS) in the process of producing a crystalline gel in an example. [Diagram 2] This is a 1D pattern obtained by taking a partial circular average of the area shown in FIG. 2(A) of each image in FIG. 1 and making it one-dimensional. [Diagram 3] This is a two-dimensional image showing the results of wide-angle X-ray scattering (WAXS) measurements during the process of producing the same crystalline gel as in Figure 1. [Figure 4] This is a processed image shown by performing coordinate transformation on the two-dimensional image selected from FIG. [Diagram 5] 11 is a two-dimensional image showing the results of measuring small-angle X-ray scattering (SAXS) and wide-angle X-ray scattering (WAXS) during the process of producing a crystalline gel in another example. [Figure 6] This is a 1D pattern obtained by taking the partial circular average of each image in FIG. 5 and making it one-dimensional. [Figure 7] 11 is a two-dimensional image showing the results of measuring small-angle X-ray scattering (SAXS) and wide-angle X-ray scattering (WAXS) during the process of producing a crystalline gel in another example. [Figure 8] This is a 1D pattern obtained by taking the partial circular average of each image in FIG. [Figure 9] 1 is a graph showing tensile test results for examples of unstretched gels. [Figure 10] 1 is a graph showing the results of tensile tests on examples of crystalline gels and polymeric bodies. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The following definitions of terms apply throughout the specification and claims. The term "monomer" refers to any compound that can form a chemical bond through a reaction, and is not limited to this. For example, the term refers to a compound that can undergo a condensation reaction, an addition reaction, or a polymerization reaction. A "polymer" is a compound having a polymeric chain consisting of two or more units based on a monomer. The term "unit based on a monomer" is a general term for an atomic group formed directly by polymerization of a monomer, and an atomic group obtained by chemically converting a part of the atomic group. "(Meth)acrylic" refers to acrylic, methacrylic, or both. "% by weight" can be used interchangeably with "% by mass." A numerical range expressed by "to" means that the numerical values ​​before and after the "to" are the lower and upper limits of the numerical range.

[0010] <Crystalline gel> The crystalline gel of the present embodiment is a gel containing a partially crystallized crosslinked polymer and a solvent, in which crystalline domains exist periodically. Crystallized portions and amorphous portions exist alternately in the molecular chains of the crosslinked polymer.

[0011] <Crosslinked polymer> A cross-linked polymer is a multifunctional polymer that has been cross-linked to form a three-dimensional network structure. Cross-linked polymers have a three-dimensional network structure. The polyfunctional polymer preferably contains one or both of the following P1 and P2. P1: A hyperbranched polymer having three or more functional groups and a branching point with three or more branched chains. P2: A linear polymer that has no branching points with three or more branches and has two functional groups.

[0012] The crosslinked polymer may be one obtained by crosslinking between polyfunctional polymers, or one obtained by crosslinking between a polyfunctional polymer and a polyfunctional monomer (crosslinking agent). Preferred embodiments of the crosslinked polymer having a three-dimensional network structure include, for example, the following embodiments 1 to 5. The crosslinked polymer preferably includes one or more types selected from the group consisting of the crosslinked polymers of the following embodiments 1 to 5. Aspect 1: A crosslinked polymer in which one or more types of P1 are crosslinked. Aspect 2: A crosslinked polymer in which one or more types of P1 are crosslinked with one or more types of P2. Aspect 3: A crosslinked polymer in which one or more types of P1 are crosslinked with one or more types of Q1 below. Aspect 4: A crosslinked polymer in which one or more types of P1 are crosslinked with one or more types of Q2 below. Aspect 5: A crosslinked polymer in which one or more types of P2 are crosslinked with one or more types of Q1 below. Q1: A branched monomer having three or more functional groups. Q2: A bifunctional monomer having two functional groups.

[0013] The functional groups P1, P2, Q1, and Q2 are reactive groups capable of undergoing a crosslinking reaction. Known reactive groups can be used. The crosslinking reaction may be a reaction between one type of functional group or a reaction between two types of functional groups, and any known crosslinking reaction may be used. As an example of a crosslinking reaction between two types of functional groups, a crosslinking reaction in which a nucleophilic functional group and an electrophilic functional group form a covalent bond is known as an AB-type cross-end coupling reaction (Matsunaga et al., Macromolecules, Vol. 42, No. 4, pp. 1344-1351, 2009). As the combination of the nucleophilic functional group and the electrophilic functional group, a known combination can be adopted. Examples of the nucleophilic functional group include a thiol group (-SH), an amino group, and -COOPhNO2 (Ph represents an o-, m-, or p-phenylene group). The electrophilic functional group may be an active ester group. Examples of the active ester group include a maleimidyl group, an N-hydroxy-succinimidyl (NHS) group, a sulfosuccinimidyl group, a phthalimidyl group, an imidazoyl group, an acryloyl group, and a nitrophenyl group. Other known active ester groups may be used as appropriate. Examples of crosslinking reactions of one type of functional group include a reaction between thiol groups and a reaction between maleimide groups.

[0014] [P1: Hyperbranched polymer] The hyperbranched polymer P1 is a polymer having a branch point with three or more branched chains and having three or more functional groups. The number of branched chains extending from one branch point is preferably 3 to 8, more preferably 3 to 6, and particularly preferably 4. The branched chain has a polymer chain consisting of units based on one or more monomers. The monomer constituting the polymer chain is not particularly limited as long as it is a monomer capable of constituting a multi-branched polymer. Known monomers can be used. For example, ethylene glycol and vinyl compounds can be exemplified. Examples of vinyl compounds include (meth)acrylic acid or its derivatives, and styrene or its derivatives. The functional group of the hyperbranched polymer may be present at the end of a branched chain or may be present in a pendant group of the branched chain (a group not containing a polymer chain), and is preferably present at the end of a branched chain. It is preferable that the structures of the branched chains constituting one molecule of the hyperbranched polymer are the same. The weight average molecular weight per branch chain of the hyperbranched polymer is preferably from 500 to 500,000, more preferably from 1,000 to 100,000, and even more preferably from 5,000 to 50,000. As the hyperbranched polymer constituting the crosslinked polymer, a hyperbranched polymer in which the branched chain has a polyethylene glycol skeleton, which is a polymer chain of ethylene glycol (hereinafter, also referred to as a "PEG polymer"), is preferable.

[0015] [P2: Linear polymer] The linear polymer P2 is a polymer having two functional groups. A linear polymer has a polymer chain made up of units based on one or more types of monomer. A linear polymer does not have a branch point with three or more branches emanate from it, i.e., linear polymers do not include hyperbranched polymers as described above. The monomer constituting the polymer chain is not particularly limited as long as it is a monomer capable of constituting a linear polymer. Known monomers can be used. For example, ethylene glycol and vinyl compounds can be exemplified. Examples of vinyl compounds include (meth)acrylic acid or its derivatives, and styrene or its derivatives. The functional groups of the linear polymer may be attached to the ends of the polymer chains directly or via a linker, or may be present as pendant groups of the polymer chains, preferably attached to the ends of the polymer chains directly or via a linker. The weight average molecular weight of the linear polymer is preferably from 500 to 500,000, more preferably from 1,000 to 100,000, and further preferably from 5,000 to 50,000. An example of a linear polymer constituting a crosslinked polymer is a polymer having a polyethylene glycol skeleton, which is a polymer chain of ethylene glycol, and having functional groups at both ends.

[0016] [Q1: Branched monomer] The branched monomer Q1 is a monomer (crosslinking agent) having three or more functional groups. A branched monomer typically has a carbon-containing backbone and three or more functional groups attached to the backbone. A branched monomer does not contain a polymer chain. The functional group of the branching monomer may be present at the molecular terminal or as a pendant group on the backbone portion. The branching monomer may be a homomultifunctional crosslinker in which the three or more reactive groups are the same as each other, or a heteromultifunctional crosslinker in which the three or more reactive groups are different from each other. The molecular weight of the branched monomer is preferably 30 or more and less than 500, more preferably 40-400, and even more preferably 50-300. As the branching monomer, a known crosslinking agent having three or more functional groups can be used, such as methanetriol, 1,2,4-butanetriol, trimethylolpropane, erythritol, pentaerythritol, dipentaerythritol, 2,2'-diethyl-2,2'-[[2-ethyl-2-(hydroxymethyl)propane-1,3-diyl]bis(oxymethylene)]bis(propane-1,3-diol), bis-trispropane, 2-amino-2-hydroxymethyl-1,3-propanediol, ethylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, diethylenetriamine, asparagine, etc.

[0017] [Q2: Difunctional monomer] The bifunctional monomer Q2 is a monomer (crosslinking agent) having two functional groups. A bifunctional monomer generally has a backbone portion that contains carbon and two functional groups attached to the backbone portion. The backbone portion does not contain a polymer chain. That is, a bifunctional monomer does not contain the linear polymer. The functional groups of the bifunctional monomer may be present at the molecular terminals or as pendant groups on the backbone. The bifunctional monomer may be a homobifunctional crosslinker in which two or more reactive groups are the same, or a heterobifunctional crosslinker in which the reactive groups are different from one another. The molecular weight of the bifunctional monomer is preferably 30 or more and less than 500, more preferably 40-400, and even more preferably 50-300. As the bifunctional monomer, a known crosslinking agent having two functional groups can be used, such as methanediol, ethylene glycol, diethylene glycol, dipropylene glycol, ethylenediamine, oxalic acid, maleic acid, adipic acid, lactic acid, and alanine.

[0018] [Aspect 1] The crosslinked polymer of this embodiment is a crosslinked polymer in which one or more types of hyperbranched polymers P1 are crosslinked. A crosslinked polymer obtained by crosslinking one or more types of hyperbranched polymers is a polymer formed by a crosslinking reaction between reactive groups (functional groups) present in the branched chains of the hyperbranched polymers. In the case of a crosslinked polymer obtained by crosslinking two or more kinds of hyperbranched polymers, the weight average molecular weight per branch chain of each hyperbranched polymer may be the same or different. It is preferable that they are the same.

[0019] The number of hyperbranched polymers to be crosslinked may be two. The number of branched chains of the two hyperbranched polymers may be the same or different. It is preferable that the number of branched chains is the same. The covalent cross-linking reaction between a reactive group present in a branched chain of a first hyperbranched polymer and a reactive group present in a branched chain of a second hyperbranched polymer is known as the AB-type cross-end coupling reaction. For example, a four-branched polymer having a nucleophilic functional group at each end of four branches is used as the first multibranched polymer, and a four-branched polymer having an electrophilic functional group at each end of four branches is used as the second multibranched polymer, and these are crosslinked to form a polymer having a three-dimensional network structure. The multiple nucleophilic functional groups present in one molecule may be the same or different, but are preferably the same in that a periodic crystal structure is more easily obtained. The electrophilic functional groups present in one molecule may be the same or different, but are preferably the same in that a periodic crystal structure is more easily obtained. A preferred combination of the first hyperbranched polymer and the second hyperbranched polymer is also described in JP 2018-116043 A.

[0020] A preferred, non-limiting example of the first multi-branched polymer having a nucleophilic functional group is a 4-branched PEG polymer represented by the following formula (I).

[0021] [ka]

[0022] In formula (I), n 11 ~n 14 may be the same or different. 11 ~n 14 The closer the values ​​of n are, the more uniform the three-dimensional structure can be and the higher the strength will be. Therefore, in order to obtain a gel with high strength, it is preferable that they are the same. 11 ~n 14 If the value of is too large, the gel strength will be weak, and 11 ~n 14 If the value of n is too small, the gel is difficult to form due to the steric hindrance of the compound. 11 ~n 14 is an integer value of 25 to 250, preferably 35 to 180, more preferably 50 to 115, and particularly preferably 50 to 60.

[0023] In formula (I), B is a nucleophilic functional group, which is a thiol group (-SH), an amino group, or -COOPhNO2 (Ph represents an o-, m-, or p-phenylene group). In formula (I), R 11 ~R 14 is a linker moiety connecting the nucleophilic functional group and the core moiety. R 11 ~R 14 may be the same or different, but are preferably the same in order to produce a high-strength gel having a uniform three-dimensional structure. 11 ~R 14 represents a C1-C7 alkylene group, a C2-C7 alkenylene group, -NH-R15 -, -CO-R 15 -, -R 16 -OR 17 -, -R 16 -NH-R 17 -, -R 16 -COO-R 17 -, -R 16 -COO-NH-R 17 -, -R 16 -CO-R 17 -, R 16 -NH-CO-R 17 -or-R 16 -CO-NH-R 17 - where R 15 R represents a C1-C7 alkylene group. 16 R represents a C1-C3 alkylene group. 17 represents a C1-C5 alkylene group.

[0024] Here, the term "C1-C7 alkylene group" refers to an alkylene group having 1 to 7 carbon atoms which may have branches, and refers to a linear C1-C7 alkylene group or a C2-C7 alkylene group having one or more branches (having 2 to 7 carbon atoms including the branches). Examples of the C1-C7 alkylene group include a methylene group, an ethylene group, a propylene group, and a butylene group. Examples of C1-C7 alkylene groups include -CH2-, -(CH2)2-, -(CH2)3-, -CH(CH3)-, -(CH2)3-, -(CH(CH3))2-, -(CH2)2-CH(CH3)-, -(CH2)3-CH(CH3)-, -(CH2)2-CH(C2H5)-, -(CH2)6-, -(CH2)2-C(C2H5)2-, and -(CH2)3C(CH3)2CH2-.

[0025] The term "C2-C7 alkenylene group" refers to a linear or branched alkenylene group having 2 to 7 carbon atoms and having one or more double bonds in the chain, and examples thereof include divalent groups having double bonds formed by removing 2 to 5 hydrogen atoms from adjacent carbon atoms of the alkylene group.

[0026] On the other hand, a preferred, non-limiting example of the second multi-branched polymer having an electrophilic functional group is a 4-branched PEG polymer represented by the following formula (II).

[0027] [ka]

[0028] In formula (II), n 21 ~n 24 may be the same or different. 21 ~n 24 The closer the values ​​of n are, the more uniform the gel can be in a three-dimensional structure and the stronger it will be, so this is preferable, and it is more preferable for them to be the same. 21 ~n 24 If the value of is too large, the gel strength will be weak, and 21 ~n 24 If the value of n is too small, the gel is difficult to form due to the steric hindrance of the compound. 21 ~n 24 is an integer value of 5 to 300, preferably 20 to 250, more preferably 30 to 180, further preferably 45 to 115, and even more preferably 45 to 55.

[0029] In formula (II), D is an electrophilic functional group, which is a maleimidyl group, an N-hydroxy-succinimidyl (NHS) group, a sulfosuccinimidyl group, a phthalimidyl group, an imidazoyl group, an acryloyl group, or a nitrophenyl group. In formula (II), R 21 ~R 24 R is the linker moiety that connects the electrophilic functional group to the core moiety. 21 ~R 24 may be the same or different, but are preferably the same in order to produce a high-strength gel having a uniform three-dimensional structure. 21 ~R 24 are the same or different, and each represents a C1-C7 alkylene group, a C2-C7 alkenylene group, -NH-R 25 -, -CO-R 25 -, -R 26 -OR 27-, -R 26 -NH-R 27 -, -R 26 -COO-R 27 -, -R 26 -COO-NH-R 27 -, -R 26 -CO-R 27 -, -R 26 -NH-CO-R 27 - or -R 26 -CO-NH-R 27 - where R 25 R represents a C1-C7 alkylene group. 26 R represents a C1-C3 alkylene group. 27 represents a C1-C5 alkylene group.

[0030] In this specification, the alkylene group and the alkenylene group may have one or more optional substituents. Examples of the substituents include, but are not limited to, an alkoxy group, a halogen atom (which may be a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom), an amino group, a mono- or di-substituted amino group, a substituted silyl group, an acyl group, or an aryl group. When an alkyl group has two or more substituents, they may be the same or different. The same applies to the alkyl portion of other substituents containing an alkyl portion (e.g., an alkyloxy group, an aralkyl group, etc.).

[0031] When there are two types of hyperbranched polymers undergoing a crosslinking reaction, the molar ratio of the first hyperbranched polymer to the second hyperbranched polymer constituting the crosslinked polymer (first hyperbranched polymer:second hyperbranched polymer) is preferably 0.5:1 to 1.5:1, more preferably 0.9:1 to 1.1:1.

[0032] [Aspect 2] The crosslinked polymer of this embodiment is a crosslinked polymer in which the hyperbranched polymer P1 and the linear polymer P2 are crosslinked. The number of types of hyperbranched polymers may be one or more. The number of types of linear polymers may be one or more. A crosslinked polymer formed by crosslinking a hyperbranched polymer and a linear polymer is a polymer formed by a crosslinking reaction between a reactive group (functional group) present in a branched chain of the hyperbranched polymer and a reactive group (functional group) of the linear polymer.

[0033] The combination of the reactive group of the hyperbranched polymer and the reactive group of the linear polymer may be any known combination, for example, the combination of the above-mentioned nucleophilic functional group and electrophilic functional group. When a hyperbranched polymer and a linear polymer are subjected to a crosslinking reaction, the ratio (molar ratio) of the total number of reactive groups present in the hyperbranched polymer to the total number of reactive groups present in the linear polymer is preferably 0.8:1 to 1.2:1, and more preferably 0.9:1 to 1.1:0.9.

[0034] [Aspect 3] The crosslinked polymer of this embodiment is a crosslinked polymer in which the multibranched polymer P1 is crosslinked with the branched monomer (crosslinking agent) Q1. The multi-branched polymer may be of one type or two or more types. The branched monomer may be of one type or two or more types. A crosslinked polymer formed by crosslinking a hyperbranched polymer with a branched monomer is a polymer formed by a crosslinking reaction between a reactive group (functional group) present in a branched chain of the hyperbranched polymer and a reactive group (functional group) of the branched monomer.

[0035] The combination of the reactive group of the hyperbranched polymer and the reactive group of the branched monomer may be any known combination, for example, the combination of the above-mentioned nucleophilic functional group and electrophilic functional group. When a hyperbranched polymer and a branched monomer are subjected to a crosslinking reaction, the ratio (molar ratio) of the total number of reactive groups present in the hyperbranched polymer to the total number of reactive groups present in the branched monomer is preferably 0.8:1 to 1.2:1, and more preferably 0.9:1 to 1.1:0.9. Preferred combinations of hyperbranched polymers and branched monomers include, for example, the combinations described in WO 2021 / 106662.

[0036] [Aspect 4] The crosslinked polymer of this embodiment is a crosslinked polymer in which the hyperbranched polymer P1 is crosslinked with the bifunctional monomer (crosslinking agent) Q2. The number of types of the hyperbranched polymer may be one or more. The number of types of the bifunctional monomer may be one or more. A crosslinked polymer formed by crosslinking a hyperbranched polymer with a bifunctional monomer is a polymer formed by a crosslinking reaction between a reactive group (functional group) present in the branched chain of the hyperbranched polymer and a reactive group (functional group) of the bifunctional monomer.

[0037] The combination of the reactive group of the hyperbranched polymer and the reactive group of the bifunctional monomer may be any known combination, for example, the combination of the above-mentioned nucleophilic functional group and electrophilic functional group. When a hyperbranched polymer is crosslinked with a bifunctional monomer, the ratio (molar ratio) of the total number of reactive groups present in the hyperbranched polymer to the total number of reactive groups present in the bifunctional monomer is preferably 0.8:1 to 1.2:1, and more preferably 0.9:1 to 1.1:0.9.

[0038] [Aspect 5] The crosslinked polymer of this embodiment is a crosslinked polymer in which the linear polymer P2 is crosslinked with the branched monomer (crosslinking agent) Q1. The linear polymer may be one type or two or more types. The branched monomer may be one type or two or more types. A crosslinked polymer obtained by crosslinking a linear polymer with a branched monomer is a polymer formed by a crosslinking reaction between a reactive group (functional group) present in the linear polymer and a reactive group (functional group) of the branched monomer.

[0039] The combination of the reactive group of the linear polymer and the reactive group of the branched monomer may be any known combination, for example, the combination of the above-mentioned nucleophilic functional group and electrophilic functional group. When a linear polymer and a branched monomer are subjected to a crosslinking reaction, the ratio (molar ratio) of the total number of reactive groups present in the linear polymer to the total number of reactive groups present in the branched monomer is preferably 0.8:1 to 1.2:1, and more preferably 0.9:1 to 1.1:0.9. Preferred combinations of linear polymers and branched monomers include, for example, the combinations described in WO 2021 / 106662.

[0040] <Solvent> The crystalline gel contains a solvent inside. The solvent is preferably a good solvent for the multifunctional polymer constituting the crosslinked polymer, and is not particularly limited as long as it has high solubility for the multifunctional polymer. When the crosslinked polymer is composed of two or more types of multifunctional polymers, the solvent is preferably a good solvent for all of the multifunctional polymers. In the unstretched gel described below, the solvent is preferably one that helps adjacent multifunctional polymers among the multifunctional polymers (crosslinked multifunctional polymers) that make up the crosslinked polymer to overlap with each other.

[0041] The good solvent may be water or an organic solvent, such as acetonitrile, acetone, N,N-dimethylformamide, methanol, or ethanol. When the multifunctional polymer is more soluble in an organic solvent than in water, the good solvent is preferably an organic solvent. For example, when the multifunctional polymer is a 4-branched PEG polymer, the good solvent is preferably anhydrous acetonitrile or N,N-dimethylformamide. An appropriate good solvent can be appropriately selected depending on the type of the multibranched polymer. For example, when a composition containing a multifunctional polymer and a good solvent is measured at a scattering angle of 90° in dynamic light scattering measurement, if only the diffusion mode of the multifunctional polymer or the cooperative diffusion mode is observed, and no relaxation mode indicating aggregates is observed, then the solvent can be determined to be a suitable good solvent.

[0042] The crystalline gel may contain one or more additives in addition to the crosslinked polymer and the solvent. Examples of additives include active ingredients of pharmaceuticals or cosmetics, buffers, isotonicity agents, preservatives, antioxidants, excipients, carriers, diluents, solvents other than good solvents, solubilizers, stabilizers, fillers, binders, surfactants, viscosity agents, stabilizers, warming agents, fragrances, salts, antioxidants, chelating agents, neutralizing agents, pH adjusters, etc.

[0043] <Manufacturing method> The crystalline gel of the present embodiment is obtained by stretching an unstretched gel containing a crosslinked polymer and a solvent so that a portion of the crosslinked polymer is crystallized. The unstretched gel is obtained by preparing a pre-gel solution containing a polyfunctional polymer before crosslinking and a solvent, and carrying out a crosslinking reaction. For example, a pre-gel solution is filled into a mold and cured to produce an unstretched gel of a desired shape. The shape of the unstretched gel is not particularly limited. For example, it may be sheet-like, spherical, or the like. The shape of the gel sheet, which is a sheet-like gel, may be any shape depending on the intended purpose, and examples of the shape include, but are not limited to, a substantially rectangular or substantially circular shape in a plan view.

[0044] By adjusting the concentration of the crosslinked polymer in the unstretched gel so that adjacent multifunctional polymers (crosslinked multifunctional polymers) that make up the crosslinked polymer overlap with each other, a crystalline gel in which crystalline domains exist periodically after stretching can be obtained. When the multifunctional polymer contains a multibranched polymer, it is preferable to adjust the concentration of the crosslinked polymer so that the branched chain portions (arms) of the multibranched polymer overlap with adjacent multifunctional polymers.

[0045] As is well known to those skilled in the art of polymers, the critical concentration at which adjacent multifunctional polymers in a solution begin to come into contact with each other (i.e., the areas occupied by the polymer chains overlap) is called the "overlap concentration." Scientifically, at the overlap concentration, the local concentration (internal concentration) of the multifunctional polymer is equal to the average concentration of the multifunctional polymer in the entire solution. The overlapping concentration is the concentration at which the zero-extrapolated scattering intensity to small angles obtained by small-angle X-ray scattering or static light scattering has a maximum value, or the concentration dependence of the zero-shear viscosity is linear (viscosity - concentration). ∧ a, a=1) from the nonlinear relationship (viscosity-concentration ∧ a, a>1), which can be confirmed by experiment. The overlap concentration that can be confirmed by the experiment is hereinafter referred to as the overlap concentration C * " The concentration of the cross-linked polymer in the unstretched gel is defined as the overlapping concentration C * Above this, preferably the overlapping concentration C * By setting the stretching length to 1.5 times or more, and more preferably 2 times or more, a crystalline gel in which crystal domains are periodically present after stretching can be obtained.

[0046] For example, in the case of a crosslinked polymer in which one or more types of multifunctional polymers are crosslinked, the total content (total concentration) of the multifunctional polymers relative to the total mass of the pre-gel solution is the same as the content (concentration) of the crosslinked polymer relative to the total mass of the unstretched gel. * Adjust so that it is equal to or greater than this. In the case of a crosslinked polymer formed by crosslinking a multifunctional monomer and a multifunctional polymer, the total content (total concentration) of the multifunctional monomer and the multifunctional polymer relative to the total mass of the pre-gel solution is the same as the content (concentration) of the crosslinked polymer relative to the total mass of the unstretched gel. * Adjust so that it is equal to or greater than this.

[0047] In this way, by densely packing the molecular chains that make up the crosslinked polymer into the pre-gel solution, the crosslinked structure in the unstretched gel becomes extremely uniform, and when stretched, it becomes a crystalline gel in which crystal domains exist periodically.

[0048] The stretching direction of the unstretched gel is not particularly limited, and may be, for example, unidirectional (uniaxial stretching) or bidirectional (biaxial stretching). As will be shown in the Examples described later, when an unstretched gel is uniaxially stretched, the molecular chains are oriented in the stretching direction, and when the stretching ratio reaches a threshold value, some of the gel crystallizes, forming a structure in which crystalline domains exist periodically. The periodic existence of crystalline domains can be confirmed by observing that the magnitude of the scattering vector is 0.001 to 0.5 Å when the stretching direction is the equator in a two-dimensional image obtained by detecting small-angle X-ray scattering (SAXS). -1 This can be confirmed by the presence of a streak extending from the beam center in the meridian direction in the range of 1 to 4, and the presence of one or more pairs of scattered images on the equator having peaks at positions symmetrical to the meridian. In this specification, the "equator" of a two-dimensional image obtained by detecting small angle X-ray scattering (SAXS) means an imaginary line that passes through the center of the beam and is parallel to the stretching direction, and the "meridian" means an imaginary line that passes through the center of the beam and is perpendicular to the stretching direction.

[0049] Furthermore, as shown in the examples below, in the process of stretching an unstretched gel, the distance between adjacent crystalline domains (hereinafter also referred to as "inter-crystalline domain distance") does not change even if the stretching ratio changes. This can be confirmed by the fact that in a 1D pattern obtained by linearizing the scattering image of a two-dimensional image obtained by detecting small-angle X-ray scattering (SAXS), the magnitude q of the scattering vector indicating the peak intensity of the scattering image does not change even when the stretching ratio is increased.

[0050] Furthermore, as shown in the examples below, by stretching an unstretched gel, a crystalline gel having a large crystal domain size (hereinafter also referred to as "crystal size") can be obtained. The large crystal size is indicated by the scattering vector magnitude of 0.5 to 3.0 Å in two-dimensional images detected by wide-angle X-ray scattering (WAXS). -1 This can be confirmed by the presence of many scattering spots in the range. The number of the scattering spots is preferably 20 or more, and more preferably 30 or more. When the number of the scattering spots is 20 or more, it can be estimated that there are crystal domains with crystal sizes on the order of several tens of nm or more.

[0051] The solvent concentration in the crystalline gel obtained by stretching the unstretched gel is the same as the solvent concentration in the unstretched gel, and is the same as the solvent concentration in the pre-gel solution. After the stretching, the solvent concentration in the crystalline gel may be reduced to obtain a crystalline gel having a desired solvent concentration, or the solvent may be further reduced or removed to obtain a polymer substantially free of solvent. The solvent can be reduced or removed by a method commonly used in the art, such as heat drying, air drying, vacuum drying, or freeze drying. In this specification, crystalline gels or polymeric bodies are the objects of measurement, and those with a solvent concentration of 10% by weight or more obtained by the measurement method described below are referred to as "crystalline gels," and those with a solvent concentration of less than 10% by weight are referred to as "polymeric bodies." <Method for measuring solvent concentration> The crystalline gel or polymer to be measured is heated and dried under normal pressure until it reaches a constant weight, and volatile components such as water are removed. When the mass before heating and drying is Wb and the mass after heating and drying is Wa, the solvent concentration (unit: mass%) is calculated using the following formula. Solvent concentration = (Wa-Wb) / Wb x 100

[0052] The content of the solvent relative to the total mass of the crystalline gel (solvent concentration) is not particularly limited, but the lower limit is 10% by weight or more, preferably 20% by weight or more, preferably 30% by weight or more, preferably 50% by weight or more, preferably 60% by weight or more, preferably 70% by weight or more, and preferably 80% by weight or more. The upper limit is preferably 99.9% by weight or less, and preferably 99% by weight or less.

[0053] The content (concentration) of the crosslinked polymer relative to the total mass of the crystalline gel is not particularly limited, but the lower limit is preferably 0.1% by weight or more, and more preferably 1% by weight or more. The upper limit is preferably 90% by weight or less, preferably 80% by weight or less, preferably 70% by weight or less, preferably 50% by weight or less, preferably 40% by weight or less, preferably 30% by weight or less, and preferably 20% by weight or less.

[0054] According to this embodiment, a crystalline gel having a highly ordered structure in which crystal domains exist periodically can be obtained, even though it is a crystallized gel. The crosslinked polymer in the crystalline gel has a higher-order structure in which crystalline domains with a long-period crystal structure and an amorphous phase are mixed together. Another characteristic of the gel is the presence of many giant domains with the long-period crystal structure. The gel before the formation of the crystalline gel contains adjacent multifunctional polymers at a concentration higher than that at which they overlap with each other, and therefore has a highly uniform structure with few spatial structural defects. Since the crosslinked polymer in the crystalline gel is oriented in the stretching direction and crystallizes, it is possible to obtain anisotropy, for example, a crystalline gel or polymer exhibiting anisotropy in thermal conduction or electrical conduction. In the process of stretching the unstretched gel, the period of the crystal domain does not change even if the stretching ratio changes, so the gel has excellent dimensional stability and good reproducibility. In the process of stretching an unstretched gel, there is a threshold stretching ratio at which crystallization occurs, and therefore an on / off switching function can be exhibited. Since an unstretched gel can be produced simply by subjecting a pre-gel solution to a cross-linking reaction in a mold, large-area, uniform crystalline gels or polymeric objects can be easily produced. By selecting the polyfunctional polymer and polyfunctional monomer that constitute the crosslinkable polymer according to the purpose, the performance of the crystalline gel or polymer body can be easily altered, providing a high degree of freedom in design.

[0055] The crystalline gel or polymer of the present embodiment is suitable as a material for forming various articles. Examples of applications of the crystalline gel or polymer of this embodiment include, but are not limited to, filtration materials, drug delivery systems (DDS), nanopore sensors, thermal conductive materials, electrical conductive materials, optically anisotropic materials, etc., and can be used in a wide range of applications. The crystalline gel or polymer of this embodiment is expected to have a ripple effect in a wide range of fields, such as medicine, pharmacology, chemistry, engineering, and electronics. EXAMPLES

[0056] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.

[0057] <Raw materials> The four-branched PEG polymers used as raw materials (all manufactured by SINOPEG, China) are shown in Table 1. The "average molecular weight (Mw)" in Table 1 is the average molecular weight indicated on the product. In general, the weight average molecular weight or peak top molecular weight measured by a measurement method such as size exclusion chromatography or MALDI-TOF (matrix-assisted laser desorption / ionization using a time-of-flight mass spectrometer) is used. As a good solvent for polyethylene glycol, DMF (N,N-dimethylformamide, specific gravity: 0.944 g / mL) treated to a super-dehydrated state was used. The overlap concentration C in Tables 2 and 3 * " is the experimentally determined value of the overlap concentration, which is defined as the concentration at which the zero-extrapolated scattering intensity to small angles obtained by small-angle X-ray scattering has a maximum value, or the transition point at which the concentration dependence of zero-shear viscosity transitions from a linear relationship to a nonlinear relationship.

[0058] [Example 1] (1) Preparation of unstretched gel An unstretched gel containing a crosslinked polymer was prepared by crosslinking tetra-PEG-NH2-40K and tetra-PEG-NHS-40K in DMF to obtain the composition shown in Table 2. The reaction rate was adjusted by adding acetic acid to the solvent, and the gelation time was controlled to less than 30 minutes. Specifically, tetra-PEG-NH2-40K was dissolved in DMF containing acetic acid, and filtered through a syringe filter with a pore size of 0.22 μm (manufactured by Advantec Toyo Co., Ltd. (Japan), the same applies below) to obtain a first hyperbranched polymer solution. Separately, tetra-PEG-NHS-40K was dissolved in DMF containing acetic acid and filtered through a syringe filter with a pore size of 0.22 μm to obtain a second hyperbranched polymer solution. The first hyperbranched polymer solution and the second hyperbranched polymer solution were mixed to obtain a pre-gel solution. The pre-gel solution was poured into a dumbbell-shaped mold (JIS K6251 No. 8 type) and allowed to gel, producing an unstretched gel with a thickness of 2 mm. The concentration of the cross-linked polymer in the unstretched gel is the total concentration of the first and second hyperbranched polymers in the pre-gel solution. As shown in Table 2, the concentration of the cross-linked polymer in this example is the overlap concentration C * That's all.

[0059] (2) Preparation of crystalline gel and X-ray scattering measurement The unstretched gel was uniaxially stretched using a tensile testing device to produce a crystalline gel. Specifically, the sample (unstretched gel) was set in a tensile tester so that the length direction of the dumbbell shape was horizontal and the width direction was vertical, and stretched in the horizontal direction at a tensile speed of 100 mm / min. If the length before stretching is L1 and the length after stretching is L2, the stretching ratio (unit: times) is L2 / L1. X-ray scattering measurements were performed by stretching a sample placed in a tensile testing device, irradiating the sample from the front in the thickness direction, and detecting the X-rays scattered backward.

[0060] X-ray scattering measurements were carried out at room temperature (set temperature 25°C) using beamline BL-15A2 at the Photon Factory of the High Energy Accelerator Research Organization (KEK, Ibaraki, Japan). In-situ measurements of two-dimensional (2D) small-angle X-ray scattering (SAXS) and two-dimensional (2D) wide-angle X-ray scattering (WAXS) were carried out on samples during stretching. The wavelength of the incident X-rays was 0.092 nm, and the exposure time was 20 seconds. The detector was a two-dimensional hybrid pixel detector (PILATUS3-2M for SAXS, PILATUS3-300K for WAXS, both DECTRIS, Switzerland) to obtain two-dimensional images (2D patterns). The distance from the sample to the detector was 3.23 m for SAXS and 0.43 m for WAXS. In order to obtain the entire WAXS2D pattern using the PILATUS3-2M detector, the distance from the sample to the detector was set to 0.33 m, and the WAXS measurement was performed while stretching the sample in the same manner as in the SAXS measurement.

[0061] In this example, multiple samples for measurement were prepared, and X-ray scattering measurement was started simultaneously with the start of stretching of the samples, with an exposure time of 20 seconds to continuously obtain data for stretching ratios of 1x (unstretched), 2x, 4x, 6x, 8x, 10x, 12x, etc. Next, data for smaller stretching ratios such as 9.25x, 9.5x, and 9.75x were also obtained in the same manner.

[0062] Figure 1 shows two-dimensional images of SAXS and WAXS simultaneously acquired by PILATUS3-2M and PILATUS3-300K. Two-dimensional images of SAXS (lower) and WAXS (upper) at the same stretching ratio are shown side by side. In each image, the equator direction is the horizontal direction (stretching direction) and the meridian direction is the vertical direction. Figure 2 shows the 1D patterns obtained by averaging the area of ​​±10° from the equator (indicated as (A) in Figure 2) in each image of Figure 1. The horizontal axis shows the magnitude of the scattering vector (q, unit: Å -1 ), and the vertical axis indicates scattering intensity (relative value). The analysis software used was a custom-made data processing package Red2D (https: / / github.com / hurxl / Red2D) stored in a scientific data analysis software package (Igor Pro9, WaveMetrics). Calibration was performed using glassy carbon (National Institute of Standards and Technology (NIST), USA), CeO2, and silver behenate (Nagara Chemical Industry Co., Ltd., Japan) as standard substances.

[0063] Figure 3 shows a two-dimensional WAXS image acquired by PILATUS3-2M. Figure 4 is a coordinate-transformed two-dimensional image of the stretched sample shown in Figure 3 at a stretch ratio of 13.5. The vertical axis represents the azimuth angle (unit: °) and the horizontal axis represents the magnitude of the scattering vector (q, unit: Å). -1 ) is shown.

[0064] As shown in FIG. 1, at a stretching ratio of 9.25 times, scattering that was not observed at a stretching ratio of 9 times appeared. Specifically, in the two-dimensional images at stretching ratios of 9.25 times to 13 times, streaks extending from the beam center in the meridian direction and multiple pairs of scattering images with peaks at positions symmetrical to the meridian on the equator were observed. When observed under magnification, five pairs of scattering images were observed. The streaks in the meridian direction are scattering seen when the polymer gel is stretched and the molecular chains are oriented, and in addition, a strong scattering image is seen on the equator (stretching direction), which indicates that crystalline domains exist periodically. That is, by uniaxially stretching the unstretched gel to 9.25 times or more, preferably 9.5 times or more, more preferably 10 times or more, a part of the polymer crystallizes, and a crystalline gel in which crystalline domains exist periodically is obtained. The stretching ratio at which a scattering image having a peak at a position symmetrical with respect to the meridian appears on the equator (stretching direction) is shown as a threshold value in the table (the same applies below). As shown in Figure 2, when the stretching ratio increases, the peak intensity of the scattering pattern peaks in the stretching direction increases without changing q (the magnitude of the scattering vector). This shows that when the stretching ratio is increased, crystallization proceeds while maintaining the distance between crystalline domains. As shown in Figures 3 and 4, as the stretching ratio increased, many scattering spots appeared in the WAXS two-dimensional images. The stretching ratio at which scattering spots appeared is shown as a threshold in the table (hereinafter the same). While modulating the contrast of the two-dimensional image at a stretching ratio of 13.5 times, the magnitude of the scattering vector q was changed from 0.5 to 3.0 Å. -1 The number of scattering spots in this region was measured and found to be over 90. A large number of scattering spots is an indication of large crystal domains. The size of the crystal domains (crystal size) was estimated from the spread of the diffraction spots (Scherrer's formula) to be in the range of 20 to 60 nm.

[0065] It was confirmed that after stretching to a stretch ratio of 10 times, the crystalline gel structure was maintained for a while even when the stretching force was released. The polymer was obtained by drying while maintaining the crystalline gel structure and reducing the solvent concentration to less than 10% by weight.

[0066] [Example 2] In Example 1, the composition of the unstretched gel was changed as shown in Table 2. Otherwise, the preparation of the unstretched gel, the production of the crystalline gel, and the X-ray scattering measurement were carried out in the same manner as in Example 1. Figure 5 shows two-dimensional images of SAXS and WAXS simultaneously acquired by PILATUS3-2M and PILATUS3-300K. Figure 6 shows the 1D patterns obtained by averaging each image in Figure 5 into one dimension. As shown in Fig. 5, at a stretching ratio of 10.25, in addition to streaks in the meridian direction, a scattering pattern appeared on the equator (stretching direction). That is, by uniaxially stretching the unstretched gel by 10.25 times or more, preferably by 10.5 times or more, and more preferably by 11 times or more, a part of the polymer crystallized, and a crystalline gel in which crystalline domains exist periodically was obtained. As shown in Fig. 6, when the stretch ratio was increased, the peak intensity of the scattering pattern in the stretch direction increased without changing q. This shows that when the stretch ratio was increased, crystallization proceeded while maintaining the interphase distance of the crystalline domains. Although not shown, the two-dimensional WAXS images obtained by PILATUS3-2M also showed the same tendency as in Example 1. As in Example 1, the stretching ratios at which scattering spots were clear were selected from the two-dimensional WAXS images, and the number of scattering spots was counted. The results are shown in the table (same below).

[0067] [Example 3] In Example 1, the composition of the unstretched gel was changed as shown in Table 2. Otherwise, the preparation of the unstretched gel, the production of the crystalline gel, and the X-ray scattering measurement were carried out in the same manner as in Example 1. Figure 7 shows two-dimensional images of SAXS and WAXS simultaneously acquired by PILATUS3-2M and PILATUS3-300K. Figure 8 shows the 1D patterns obtained by averaging the images in Figure 7 into one dimension using partial circular averages. As shown in Fig. 7, at a stretching ratio of 9.5 times, in addition to streaks in the meridian direction, a scattering pattern appeared on the equator (stretching direction). That is, by uniaxially stretching the unstretched gel by 9.5 times or more, preferably by 10 times or more, and more preferably by 11 times or more, a part of the polymer crystallized, and a crystalline gel in which crystalline domains exist periodically was obtained. As shown in Fig. 8, when the stretching ratio was increased, the peak intensity of the scattering pattern in the stretching direction increased without changing the q value. This shows that when the stretching ratio was increased, crystallization proceeded while maintaining the period of the crystal domain. Although not shown, the two-dimensional WAXS images acquired with PILATUS3-2M also showed a similar tendency to Example 1.

[0068] [Examples 4 and 5] In Example 1, the composition of the unstretched gel was changed as shown in Table 3. Otherwise, the preparation of the unstretched gel, the production of the crystalline gel, and the X-ray scattering measurement were carried out in the same manner as in Example 1.

[0069] In Examples 4 and 5, the X-ray scattering measurement results showed the same tendency as in Example 1. In Examples 4 and 5, the unstretched gel was uniaxially stretched, whereby a part of the polymer crystallized, and a crystalline gel in which crystal domains existed periodically was obtained.-1 A crystalline gel was obtained with more than 90 scattering spots in the region.

[0070] [Table 1]

[0071] [Table 2]

[0072] [Table 3]

[0073] [Example 6] In this example, tetra-PEG-NH2-40K and tetra-PEG-NHS-40K were mixed in a 1:1 molar ratio in DMF and subjected to a crosslinking reaction for one week to prepare an unstretched gel containing a crosslinked polymer. Table 4 shows the molecular weight between branch points of the crosslinked polymer and the polymer concentration in the unstretched gel (concentration of the crosslinked polymer, unit: g / L).

[0074] The mechanical properties of the unstretched gel thus prepared were evaluated by the following method. Specifically, in order to determine the breaking stress, breaking elongation ratio, Young's modulus, fracture energy, and tear energy, a tensile testing machine (product name "AUTOGRAPH AG-X plus", load cell capacity 50N, manufactured by Shimadzu Corporation) was used to carry out tensile stress-strain measurements on samples molded into a specified shape at room temperature (23°C) and a deformation rate of 100 mm / min. In the extension test of the unstretched gel, a sample was used in which the unstretched gel was molded into a strip shape of 14 mm (length) × 2 mm (width) × 1 mm (thickness). In the crack propagation test of the unstretched gel, the unstretched gel was molded into a strip of 14 mm (length) x 4 mm (width) x 1 mm (thickness), and a notch with a depth of 1 mm in the width direction was made in the center of the length direction from the side toward the center (width direction). In order to evaluate the mechanical properties of the crystallized portion, the strip-shaped sample used in the extension test of the unstretched gel was uniaxially stretched to produce a crystalline gel in which a part of the polymer was crystallized. In addition, a polymer body in which the solvent of the crystalline gel was reduced was produced. Specifically, the strip-shaped sample was stretched 9 times at room temperature (23°C) at a deformation speed of 100 mm / min using the tensile tester, and processed into a rod shape of 28 mm (length) x 0.5 mm (width) x 0.25 mm (thickness) to produce a crystalline gel sample (wet fiber). In addition, a sample (wet fiber) processed into a rod shape in the same manner was dried at room temperature to produce a polymer sample (dried fiber) with a size of 28 mm (length) x 0.3 mm (width) x 0.1 mm (thickness). A tensile test was performed using the obtained wet fiber and dried fiber as samples.

[0075] <Test Results> (Mechanical properties of gel) The behavior of the unstretched gel prepared in this example in a tensile test is shown in Figure 9. In the graph in Figure 9, the horizontal axis indicates the elongation ratio, and the vertical axis indicates the nominal stress. The elongation test was performed twice (n=2), and the crack growth test was performed three times (n=3). Table 4 shows the measurement results of the breaking stress, breaking elongation ratio, Young's modulus, fracture energy, and tear energy of the gel. These results demonstrate that the gel is strong, has high extensibility and breaking stress, and also has excellent tearing energy.

[0076] [Table 4]

[0077] (Mechanical properties of crystallized part) The behavior of the wet fiber (crystalline gel) and dried fiber (polymer) produced in this example in a tensile test is shown in Figure 10. In the graph of Figure 10, the horizontal axis indicates the elongation ratio, and the vertical axis indicates the nominal stress. Table 5 shows the measurement results of breaking stress, breaking elongation ratio, and Young's modulus. From the results of Figures 9 and 10 and Tables 4 and 5, the mechanical properties of the wet fiber (crystalline gel) and dried fiber (polymer) are improved compared to the mechanical properties of the unstretched gel, with Young's modulus being 240 to 32,000 times higher and the breaking stress being 100 to 560 times higher. In particular, the improvement in mechanical properties of the dried polymer (dried fiber) is remarkable.

[0078] [Table 5]

Claims

1. The present invention includes a crosslinked polymer in which a multifunctional polymer having two or more functional groups is crosslinked so as to form a three-dimensional network structure, and a solvent, A crystalline gel in which a portion of the crosslinked polymer is crystallized and crystalline domains exist periodically.

2. The crystalline gel according to claim 1, wherein the crosslinked polymer comprises at least one selected from the group consisting of crosslinked polymers in which one or more types of P1 are crosslinked, crosslinked polymers in which one or more types of P1 are crosslinked with one or more types of P2, crosslinked polymers in which one or more types of P1 are crosslinked with one or more types of Q1, crosslinked polymers in which one or more types of P1 are crosslinked with one or more types of Q2, and crosslinked polymers in which one or more types of P2 are crosslinked with one or more types of Q1. P1: A hyperbranched polymer having a branching point with three or more branched chains and having three or more functional groups. P2: A linear polymer having no branching points with three or more branched chains and having two functional groups. Q1: A branched monomer having three or more functional groups. Q2: A bifunctional monomer having two functional groups.

3. The crystalline gel according to claim 1 , wherein the concentration of the crosslinked polymer in the crystalline gel is equal to or higher than the concentration at which adjacent crosslinked multifunctional polymers overlap each other.

4. 2. The crystalline gel according to claim 1, wherein the polyfunctional polymer is one or both of a hyperbranched polymer having a branch point with three or more branched chains, three or more functional groups, and a weight-average molecular weight per branch chain of 500 to 100,000, and a linear polymer having no branch point with three or more branched chains, two functional groups, and a weight-average molecular weight of 500 to 100,000.

5. The crystalline gel according to claim 1 , wherein the solvent is a good solvent for the multifunctional polymer.

6. A crystalline gel containing a crosslinked polymer in which a multifunctional polymer having two or more functional groups is crosslinked so as to form a three-dimensional network structure, and a solvent, and crystallized by stretching, In a two-dimensional image in which small-angle X-ray scattering is detected, the magnitude of the scattering vector is 0.001 to 0.5 Å when the stretching direction is the equator direction. -1 A crystalline gel in which, in the range, there is a streak extending from the beam center in the meridian direction and, at the equator, there is one or more pairs of scattering images having peaks at positions symmetrical with respect to the meridian.

7. A crystalline gel containing a crosslinked polymer in which a multifunctional polymer having two or more functional groups is crosslinked so as to form a three-dimensional network structure, and a solvent, and crystallized by stretching, In the two-dimensional image that detects wide-angle X-ray scattering, the magnitude of the scattering vector is 0.5 to 3.0 Å. -1 A crystalline gel in which 20 or more scattering spots exist within the range.

8. A polymeric substance, in which the solvent is reduced or removed from the crystalline gel according to any one of claims 1 to 7.

9. A method for producing a crystalline gel in which crystalline domains exist periodically, the method comprising: stretching an unstretched gel containing a crosslinked polymer in which a multifunctional polymer having two or more functional groups is crosslinked so as to form a three-dimensional network structure, and a solvent, the gel having a concentration of the crosslinked polymer equal to or higher than the concentration at which adjacent multifunctional polymers among the crosslinked multifunctional polymers overlap with each other, so that a portion of the crosslinked polymer crystallizes.

10. 10. The method for producing a crystalline gel according to claim 9, wherein the crosslinked polymer comprises at least one selected from the group consisting of crosslinked polymers in which one or more types of P1 are crosslinked, crosslinked polymers in which one or more types of P1 are crosslinked with one or more types of P2, crosslinked polymers in which one or more types of P1 are crosslinked with one or more types of Q1, crosslinked polymers in which one or more types of P1 are crosslinked with one or more types of Q2, and crosslinked polymers in which one or more types of P2 are crosslinked with one or more types of Q1. P1: A hyperbranched polymer having a branching point with three or more branched chains and having three or more functional groups. P2: A linear polymer having no branching points with three or more branched chains and having two functional groups. Q1: A branched monomer having three or more functional groups. Q2: A bifunctional monomer having two functional groups.

11. 10. The method for producing a crystalline gel according to claim 9, wherein the polyfunctional polymer is one or both of a hyperbranched polymer having a branch point with three or more branched chains, three or more functional groups, and a weight-average molecular weight per branch chain of 500 to 100,000, and a linear polymer having no branch point with three or more branched chains, two functional groups, and a weight-average molecular weight of 500 to 100,000.

12. The method for producing a crystalline gel according to claim 9 , wherein the solvent is a good solvent for the multifunctional polymer.

13. An article comprising the crystalline gel according to any one of claims 1 to 7.

14. An article comprising the polymeric body of claim 8.