Positive electrode active material and lithium secondary battery including the same

By removing excess light element oxides and lithium impurities from the surface of high-Ni cathode active materials in lithium secondary batteries through heat treatment and water washing, the electrochemical and thermal stability of the batteries are improved, addressing structural instability and degradation issues.

JP2024144487AActive Publication Date: 2024-10-11ECOPRO BM CO LTD

Patent Information

Application Number
JP2024117384
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-06-09
Filing Date
2024-07-23
Publication Date
2024-10-11
Estimated Expiration
2041-06-11

AI Technical Summary

Technical Problem

Existing lithium secondary batteries face issues with structural instability and rapid degradation due to high-Ni cathode active materials, leading to poor electrochemical characteristics and stability, especially at high temperatures, primarily caused by lithium-containing impurities and light element-containing oxides on the surface of the positive electrode active material.

Method used

A positive electrode active material is developed by removing excess light element-containing oxides and lithium-containing impurities through heat treatment and water washing, forming a coating layer of boron-containing oxides on the surface of primary and secondary particles, thereby improving electrochemical properties and stability.

Benefits of technology

The solution enhances the electrochemical performance and thermal stability of lithium secondary batteries by reducing the amount of lithium-containing impurities and light element oxides, resulting in improved discharge capacity, output characteristics, and life characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144487000001_ABST
    Figure 2024144487000001_ABST
Patent Text Reader

Abstract

To provide a positive electrode active material which is improved in electrochemical properties and stability.SOLUTION: There is provided a positive electrode active material which includes a lithium composite oxide containing a primary particle containing at least Li, Ni, and B, and a secondary particle in which a plurality of the primary particles are aggregated. A coating layer containing a boron-containing oxide presents on at least part of a surface of the secondary particle. A content of boron (B) in the lithium composite oxide is 0.09 mol% or more and 0.49 mol% or less, and a content of lithium impurities (LiOH) in the lithium composite oxide is 11,661 ppm or less. Weight loss is measured under normal pressure in an Ar atmosphere from 25°C to 350°C at a temperature increase rate of 10°C / min. Here, the onset temperature at which a weight loss (thermal decomposition) peak appears is 231.2°C or above.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cathode active material including a lithium composite oxide having improved electrochemical properties and stability, and a lithium secondary battery including the same. More specifically, the present invention relates to a cathode active material having improved electrochemical properties and stability by removing at least a portion of a coating layer present on a surface of the lithium composite oxide and lithium-containing impurities, and a lithium secondary battery including the same. [Background technology]

[0002] Batteries store electricity by using materials capable of electrochemical reaction at the positive and negative electrodes. A representative example of such batteries is a lithium secondary battery, which stores electrical energy by the difference in chemical potential when lithium ions are intercalated / deintercalated at the positive and negative electrodes.

[0003] The lithium secondary battery is manufactured by using a material capable of reversible intercalation / deintercalation of lithium ions as a positive electrode and a negative electrode active material, and filling an organic electrolyte or a polymer electrolyte between the positive electrode and the negative electrode.

[0004] Representative materials used as positive electrode active materials for lithium secondary batteries include lithium composite oxides, such as LiCoO2, LiMn2O4, LiNiO2, LiMnO2, or oxides of Ni, Co, Mn, or Al as disclosed in Korean Patent Publication No. 10-2015-0069334 (published on June 23, 2015).

[0005] Among the positive electrode active materials, LiCoO2 is the most widely used because of its excellent life characteristics and charge / discharge efficiency. However, it has a drawback in that it is expensive due to the limited availability of cobalt as a raw material, and therefore has limited price competitiveness.

[0006] Lithium manganese oxides such as LiMnO2 and LiMn2O4 have the advantages of being thermally safe and inexpensive, but have problems with small capacity and poor high-temperature characteristics. In addition, LiNiO2-based positive electrode active materials show high discharge capacity battery characteristics, but are difficult to synthesize due to the problem of cation mixing between Li and transition metals, which causes major problems in rate characteristics.

[0007] In addition, a large amount of Li by-products is generated depending on the depth of the cation mixing. Most of the Li by-products contain LiOH and Li2CO3, which may cause gelation during the preparation of the positive electrode paste or gas generation due to repeated charging and discharging after the electrode is manufactured. In addition, the residual Li2CO3 among the Li by-products increases the swelling phenomenon of the cell, thereby reducing the life characteristics.

[0008] To overcome these shortcomings, the demand for high-Ni positive electrode active materials with Ni content of 50% or more as the positive electrode active material for secondary batteries has started to increase. However, while such high-Ni positive electrode active materials exhibit high capacity characteristics, they have a problem in that structural instability due to Li / Ni cation mixing is caused by the increase in Ni content in the positive electrode active material. Due to the structural instability of such positive electrode active materials, lithium secondary batteries can rapidly deteriorate not only at high temperatures but also at room temperature.

[0009] Therefore, it is necessary to develop a positive electrode active material that can overcome these problems of high-Ni positive electrode active materials. Summary of the Invention [Problem to be solved by the invention]

[0010] In the lithium secondary battery market, the growth of lithium secondary batteries for electric vehicles is playing a leading role in the market, while the demand for positive electrode active materials used in lithium secondary batteries is also continuously changing.

[0011] For example, lithium secondary batteries using LFP have traditionally been used primarily from the standpoint of ensuring safety, but recently there has been a trend toward expanding use of nickel-based lithium composite oxides, which have a larger energy capacity per weight than LFP.

[0012] Accordingly, an object of the present invention is to provide a high-Ni positive electrode active material capable of improving the electrochemical characteristics and stability of a lithium secondary battery.

[0013] Another object of the present invention is to provide a lithium secondary battery using a positive electrode containing the lithium composite oxide defined in the present application. [Means for solving the problem]

[0014] A technology has been proposed to reduce surface side reactions of the positive electrode active material and improve stability by making light elements, typically boron, in the positive electrode active material exist in the form of oxide (Korean Patent Registration No. 10-1651338, published on August 25, 2016).

[0015] However, although the formation of the light element-containing oxide on the surface of the positive electrode active material can reduce side reactions between the positive electrode active material and the electrolyte, there is a problem in that the content of lithium-containing impurities in the surface of the positive electrode active material increases due to the reaction between the positive electrode active material and the light element-containing raw material.

[0016] This problem occurs because at least a portion of the lithium-containing impurities present on the surface of the positive active material reacts with the light-element-containing raw material to be converted into a light-element-containing oxide, but the amount of the lithium-containing impurities converted into the light-element-containing oxide is much smaller than the content of the lithium-containing impurities generated by the reaction of the positive active material with the light-element-containing raw material.

[0017] Thus, according to one aspect of the present invention, a mixture of the precursor of the lithium composite oxide and a light element-containing raw material contained in the positive electrode active material is heat-treated to form the light element-containing oxide on at least a portion of the surface of the primary particles and / or secondary particles, and then excess light element-containing oxide and lithium-containing impurities are removed from the positive electrode active material, thereby providing a positive electrode active material with improved electrochemical properties and stability.

[0018] In one embodiment, the primary particles may be represented by the following Formula 1:

[0019] [Chemical formula 1] Li w Ni 1-(x+y+z+z′) Co x B y M1 z M2 z′ O2

[0020] (wherein M1 is at least one selected from Mn and Al, M2 is at least one selected from Mn, Ba, Ce, Hf, Ta, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr, Ge, Nd, Gd and Cu, M1 and M2 are elements different from each other, and 0.5≦w≦1.5, 0≦x≦0.50, 0 <y≦0.20、0≦z≦0.20、0≦z′≦0.20である)

[0021] On the other hand, the amount of LiOH dissolved from the positive electrode active material measured by neutralization titration using HCl satisfies the following formula 1.

[0022] [Formula 1] r<(19,153×x1)+x2

[0023] (wherein x1 is the boron content (mol %) in the lithium composite oxide before washing with water, x2 is the amount of LiOH (ppm) converted from the amount of HCl consumed corresponding to the x-axis value of the first peak appearing at the minimum x-axis value in a differential graph showing the differentiation of the pH value against the amount of HCl added by the neutralization titration method for the lithium composite oxide before washing with water, and r is the amount of LiOH eluted (ppm) from the lithium composite oxide after washing with water).

[0024] In addition, the amount of LiOH dissolved from the positive electrode active material measured by neutralization titration using HCl can satisfy the following formula 2.

[0025] [Formula 2] y1≦r≦y1+(y2×(1-y3)×18,429)

[0026] (wherein y1 is the amount of LiOH (ppm) converted from the amount of HCl consumed corresponding to the x-axis value of the first peak appearing at the minimum x-axis value in a differential graph showing the differentiation of the pH value against the amount of HCl added by the neutralization titration method for the lithium composite oxide after washing with water, y2 is the boron content (mol %) in the lithium composite oxide before washing with water, y3 is the rate of change in the boron content in the lithium composite oxide before and after washing with water, which has a value exceeding 0 and not exceeding 0.90, and r is the amount of LiOH eluted from the lithium composite oxide after washing with water (ppm).

[0027] According to another aspect of the present invention, there is provided a positive electrode comprising the positive electrode active material as described above.

[0028] According to yet another aspect of the present invention, there is provided a lithium secondary battery using the above-mentioned positive electrode. Effect of the Invention

[0029] According to the present invention, a light element-containing oxide in the positive electrode active material is formed on at least a portion of the surfaces of primary particles and / or secondary particles by heat-treating a mixture of a precursor of the positive electrode active material and a light element-containing raw material, and then excess light element-containing oxide and lithium-containing impurities in the positive electrode active material are removed, thereby improving electrochemical properties and stability.

[0030] In particular, in the cathode active material according to the present invention, the precursor of the cathode active material and the light element-containing raw material are mixed and heat-treated in the step of calcining the precursor of the cathode active material, so that the light element in the cathode active material is doped and at the same time, the light element-containing oxide in the cathode active material can be concentrated on the surface and / or interface of the primary particles.

[0031] In addition, by controlling the content of the light element-containing oxide present on the surface of the secondary particles, it is possible to prevent the electrochemical properties of the positive electrode active material from being deteriorated by the light element-containing oxide and / or the lithium-containing impurities. [Brief description of the drawings]

[0032] [Figure 1] FIG. 2 is a schematic diagram of a positive electrode active material according to an embodiment of the present invention, and is a schematic diagram showing a coating layer including a boron-containing oxide on a surface of a secondary particle and a process of removing lithium-containing impurities. [Diagram 2] 1 is a differential graph obtained through neutralization titration before washing with water of lithium composite oxides constituting positive electrode active materials according to Examples 1, 2, and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] Hereinafter, a positive electrode active material for a lithium secondary battery having improved electrochemical properties and stability and a lithium secondary battery including the same according to the present invention will be described in more detail.

[0034] positive electrode active material According to one aspect of the present invention, there is provided a positive electrode active material including secondary particles formed by agglomerating a plurality of primary particles that are a lithium composite oxide capable of intercalating and deintercalating lithium.

[0035] Here, the primary particle means one crystal grain (grain or crystallite), and the secondary particle means an aggregate formed by agglomeration of a plurality of primary particles. The primary particle may have a rod-like, elliptical and / or irregular shape. A gap and / or a grain boundary may exist between the primary particles constituting the secondary particle.

[0036] For example, the primary particles may be separated from adjacent primary particles within the secondary particle to form internal voids. Also, the primary particles may contact adjacent primary particles without forming grain boundaries and contact internal voids to form a surface present within the secondary particle. Meanwhile, the surface of the primary particles present at the outermost surface of the secondary particle that is exposed to the outside air forms the surface of the secondary particle.

[0037] Here, the average major axis diameter of the primary particles is within a range of 0.1 μm to 5 μm, preferably 0.1 μm to 2 μm, so that the optimal density of the positive electrode manufactured using the positive electrode active material according to various embodiments of the present invention can be realized. Also, the average particle size of the secondary particles may be 1 μm to 30 μm, depending on the number of aggregated primary particles.

[0038] Meanwhile, the positive electrode active material may be in a bimodal form including small particles, which are secondary particles with an average particle size of 5 μm or less, and large particles, which are secondary particles with an average particle size of 12 μm or more.

[0039] In one embodiment, the primary particles may be a lithium composite oxide including at least Li, Ni, and B. More specifically, the primary particles may be represented by the following Chemical Formula 1.

[0040] [Chemical formula 1] Li w Ni 1-(x+y+z+z′) Co x B y M1 z M2 z′ O2

[0041] (wherein M1 is at least one selected from Mn and Al, M2 is at least one selected from Mn, Ba, Ce, Hf, Ta, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr, Ge, Nd, Gd and Cu, M1 and M2 are elements different from each other, and 0.5≦w≦1.5, 0≦x≦0.50, 0 <y≦0.20、0≦z≦0.20、0≦z′≦0.20である)

[0042] If the positive electrode active material has a bimodal form including small particles and large particles, the concentration of M1 in the small particles may be greater than the concentration of M1 in the large particles.

[0043] In general, the content of a light element, typically boron, in a positive electrode active material can be predicted depending on the content of a boron-containing raw material added during preparation of the positive electrode active material, and it is difficult to specifically identify how the light element is present in the positive electrode active material compared to other elements.

[0044] However, according to the present invention, in the step of calcining the precursor (hydroxide precursor or roasted precursor) of the lithium composite oxide, the precursor is mixed with a light element-containing raw material and then heat-treated, so that the light elements in the primary particles are doped as represented by Chemical Formula 1, and at the same time, a coating layer containing a light element-containing oxide in the positive electrode active material is concentrated on the surface and / or interface of the primary particles.

[0045] In addition, when the precursor (hydroxide precursor or roasted precursor) of the lithium composite oxide is mixed with a light element-containing raw material in the calcination step and then heat-treated, a coating layer containing the light element-containing oxide may be formed on at least a portion of the surface of the secondary particles.

[0046] As described above, the coating layer may include at least one boron-containing oxide represented by the following Chemical Formula 2:

[0047] [Chemical formula 2] Li a B b O c

[0048] (where: 0≦a≦8, 0 <b≦8、2≦c≦13である) That is, the boron-containing oxide is a borate-based compound or an LBO (lithium borate)-based compound, and non-limiting examples of the borate-based compound or the LBO (lithium borate)-based compound are B2O3, Li2O-B2O3, Li3BO3, Li2B4O7, Li2B2O7, Li2BO 13 etc.

[0049] The coating layer is present on at least a portion of the surface of the primary particles and / or the secondary particles, and the coating layer can be defined as a region in which the boron-containing oxide represented by Chemical Formula 2 is present.

[0050] The coating layer may coat at least a portion of the surface of the primary particles and / or the secondary particles continuously or discontinuously, and when the coating layer is discontinuous, it may be present in the form of islands. The coating layer may also be, but is not necessarily, present in the form of a solid solution that does not form a boundary with the primary particles and / or the secondary particles.

[0051] The coating layer is not formed by calcining the precursor of the lithium composite oxide (hydroxide precursor or roasted precursor), mixing the calcination result with a boron-containing raw material, and heat-treating the mixture, but by mixing the precursor of the lithium composite oxide (hydroxide precursor or roasted precursor) with a boron-containing raw material, and heat-treating the mixture.

[0052] Meanwhile, after the mixture of the lithium composite oxide precursor (hydroxide precursor or roasted precursor) and the boron-containing raw material is heat-treated, at least a portion of the coating layer present on at least a portion of the surface of the primary particles and / or the secondary particles may be removed by washing with water.

[0053] In particular, by washing the lithium composite oxide having a coating layer containing a boron-containing oxide formed thereon with water, the coating layer present on the surface and / or interface of the primary particles in an area relatively closer to the surface of the secondary particles can be further removed compared to the coating layer present on the surface and / or interface of the primary particles in an area relatively closer to the center of the secondary particles.

[0054] In addition, by washing the lithium composite oxide having the coating layer containing the boron-containing oxide formed thereon with water, the coating layer present on the surface of the secondary particles can be further removed, compared with the coating layer present on the surface and / or interface of the primary particles present in a region relatively close to the center of the secondary particles.

[0055] Through the above-mentioned water washing, the light element-containing oxide is partially removed from the surface of the positive electrode active material, particularly the secondary particles, to expose the surfaces of the secondary particles, and at the same time, lithium-containing impurities present on the surfaces of the secondary particles can be removed.

[0056] Thereby, the boron content in the positive electrode active material after washing with water can be reduced compared to the boron content in the positive electrode active material before washing with water, and the rate of change (rate of reduction) of the boron content in the positive electrode active material after washing with water may be more than 0 and not more than 0.90 (more than 0% and not more than 95%), preferably 0.10 to 0.90 (10% to 95%), and more preferably 0.20 to 0.90 (20% to 90%).

[0057] As a result of washing the positive electrode active material with water, the content of residual boron in the lithium composite oxide is preferably at least 0.3 mol% or less. However, when the content of residual boron in the lithium composite oxide is 0.3 mol% or less, and when the content of boron in the lithium composite oxide before washing with water is 0.3 mol% or less, the distribution of boron-containing oxide and lithium-containing impurities present on the surfaces of primary particles and / or secondary particles constituting the lithium composite oxide and the morphology of the coating layer containing boron-containing oxide are different, and therefore they must be distinguished from each other.

[0058] When the reduction rate of the boron content in the positive active material due to washing with water exceeds 95%, the content of the boron-containing oxide in the positive active material, particularly in the surface of the secondary particles, becomes too low, so that it may be difficult to realize the effect of suppressing surface side reactions due to the boron-containing oxide.

[0059] On the other hand, if the boron-containing oxide is not washed with water after forming the boron-containing oxide on the surface of the lithium composite oxide, or if the boron content in the positive electrode active material is not substantially reduced as a result of washing the positive electrode active material with water, there is a risk that the electrochemical properties of the positive electrode active material will be deteriorated due to the presence of an excessive amount of boron-containing oxide on the surface of the secondary particles or the presence of an excessive amount of lithium-containing impurities on the surface of the secondary particles.

[0060] In one embodiment, the amount of LiOH dissolved from the positive electrode active material measured by a neutralization titration method using HCl may satisfy the following formula 1:

[0061] [Formula 1] r<(19,153×x1)+x2

[0062] (where: x1 is the boron content (mol%) in the lithium composite oxide before washing with water, x2 is the amount of LiOH (ppm) calculated from the amount of HCl consumed corresponding to the x-axis value of the first peak appearing at the minimum x-axis value in the differential graph showing the differentiation of the pH value versus the amount of HCl added by the neutralization titration method for the lithium composite oxide before washing with water; r is the amount (ppm) of LiOH dissolved from the lithium composite oxide after washing with water.

[0063] In this case, the neutralization titration may be performed using 0.1N HCl for 5 g of the positive active material, and the amount of LiOH dissolved may be measured through a differential graph of the change in pH according to the amount of HCl added obtained through the neutralization titration.

[0064] In the above formula 1, the constant "19,153" is used to calculate the increase in LiOH due to the boron content in the lithium composite oxide before washing with water.

[0065] As described above, the greater the compounding ratio of the light element-containing raw material reacting with the precursor of the lithium composite oxide, the greater the boron content in the lithium composite oxide and the boron-containing oxide content in the lithium composite oxide. The greater the content of the boron-containing oxide in the lithium composite oxide, the greater the amount of LiOH eluted according to the following reaction formula 1 during neutralization titration.

[0066] [Reaction Scheme 1] Li3BO3+H2O→LiOH+H3BO3

[0067] Meanwhile, x2 is the amount of LiOH (ppm) converted from the amount of HCl consumption corresponding to the x-axis value of the first peak appearing at the minimum x-axis value in the differential graph obtained by differentiating the pH value against the amount of HCl added by the neutralization titration method for the lithium composite oxide before washing with water, and the amount of HCl consumption corresponding to the x-axis value of the first peak appearing at the minimum x-axis value is determined by the amount of LiOH present in the lithium composite oxide before washing with water, not by LiOH converted from Li3BO3 according to Reaction Scheme 1.

[0068] For example, referring to the differential graph corresponding to Example 1 in Fig. 2, the amount of HCl consumption corresponding to the x-axis value of the first peak appearing at the minimum x-axis value can be converted to the amount of LiOH present in the lithium composite oxide, and the amount of HCl consumption corresponding to the difference between the x-axis value of the first peak appearing at the minimum x-axis value and the x-axis value of the second peak appearing next can be converted to the amount of LiOH converted from Li3BO3 according to Reaction Scheme 1. In addition, the amount of HCl consumption corresponding to the difference between the x-axis value of the second peak and the x-axis value of the third peak appearing next can be converted to the amount of Li2CO3 in the lithium-containing impurity.

[0069] Therefore, if the boron content (mol%) in the lithium composite oxide before washing is 1.0 mol%, and the amount of LiOH (ppm) calculated from the amount of HCl consumed corresponding to the x-axis value of the first peak appearing at the minimum x-axis value in the differential graph showing the differentiation of the pH value against the amount of HCl added by the neutralization titration method for the lithium composite oxide before washing is 8,638 ppm, the amount of LiOH calculated from the right side of Equation 1 may be 27,791 ppm.

[0070] In this case, the amount of LiOH eluted from the water-washed positive electrode active material containing the lithium composite oxide, as measured by neutralization titration using HCl, is preferably less than 27,791 ppm.

[0071] If the boron content (mol%) in the lithium composite oxide before washing with water is 1.0 mol%, and the amount of LiOH (ppm) converted from the amount of HCl consumed corresponding to the x-axis value of the first peak appearing at the minimum x-axis value in a differential graph showing the differentiation of pH value against the amount of HCl added by the neutralization titration method for the lithium composite oxide before washing with water is 8,638 ppm, when the amount of LiOH eluted from the positive electrode active material including the washed lithium composite oxide by the neutralization titration method using HCl is 27,791 ppm or more, there is a risk that the electrochemical properties of the positive electrode active material will be deteriorated due to the excessive presence of the boron-containing oxide and / or the lithium-containing impurities on the surfaces of the secondary particles.

[0072] More specifically, the amount of LiOH dissolved from the positive electrode active material measured by neutralization titration using HCl satisfies the following formula 2.

[0073] [Formula 2] y1≦r≦y1+(y2×(1-y3)×18,429)

[0074] (where: y1 is the amount of LiOH (ppm) calculated from the amount of HCl consumed corresponding to the minimum x-axis value in a differential graph showing the differentiation of the pH value versus the amount of HCl added by the neutralization titration method for the lithium composite oxide after washing with water, y2 is the boron content (mol%) in the lithium composite oxide before washing with water, y3 is a rate of change in the boron content in the lithium composite oxide before and after washing with water, and has a value of more than 0 and not more than 0.90; r is the amount (ppm) of LiOH dissolved from the lithium composite oxide after washing with water.

[0075] In the above formula 2, the constant "18,429" is used to calculate the increase in LiOH due to the boron content in the lithium composite oxide after washing with water.

[0076] y1 corresponds to x2 in Equation 1, and is the amount of LiOH (ppm) calculated from the amount of HCl consumption corresponding to the x-axis value of the first peak appearing at the minimum x-axis value in a differential graph showing the differentiation of pH value versus the amount of HCl added by the neutralization titration method for the lithium composite oxide after washing with water. The amount of HCl consumption corresponding to the x-axis value of the first peak appearing at the minimum x-axis value is determined by the amount of LiOH present in the lithium composite oxide after washing with water, not by LiOH converted from Li3BO3 according to Reaction 1.

[0077] Therefore, if the change rate of the boron content in the lithium composite oxide after washing with water is 0.88 (88%), and the amount of LiOH (ppm) calculated from the amount of HCl consumed corresponding to the x-axis value of the first peak appearing at the minimum x-axis value in the differential graph showing the differentiation of the pH value against the amount of HCl added by the neutralization titration method for the lithium composite oxide after washing with water is 2,34 ppm, the range of the amount of LiOH calculated from Equation 2 may be 2,734 ppm or more and 4,945 ppm or less.

[0078] In this case, the amount of LiOH eluted from the water-washed positive electrode active material containing the lithium composite oxide, as measured by neutralization titration using HCl, is preferably 2,734 ppm or more and 4,945 ppm or less, and more preferably more than 2,734 ppm and 4,945 ppm or less.

[0079] If the boron content (mol%) in the lithium composite oxide before washing with water is 1.0 mol%, the rate of change in the boron content in the lithium composite oxide after washing with water is 0.88 (88%), and the amount of LiOH (ppm) converted from the amount of HCl consumed corresponding to the x-axis value of a first peak appearing at the minimum x-axis value in a differential graph obtained by differentiating the pH value against the amount of HCl added by the neutralization titration method for the lithium composite oxide after washing with water is 2.34 ppm, when the water-washing process for the positive electrode active material is excessively performed, the amount of LiOH eluted from the positive electrode active material including the washed lithium composite oxide may be less than 2.34 ppm, as measured by the neutralization titration method using HCl.

[0080] In this case, the amount of lithium-containing impurities present on the surface of the lithium composite oxide can be reduced, but the surface of the lithium composite oxide may be damaged, resulting in a decrease in electrochemical properties and stability. Also, since most of the boron-containing oxide is removed from the surface of the lithium composite oxide, it may be difficult to realize the effect of suppressing surface side reactions.

[0081] On the other hand, when the amount of LiOH dissolved from the positive active material containing the lithium composite oxide washed with water under the same conditions is measured by a neutralization titration method using HCl and exceeds 4,945 ppm, the boron-containing oxide and / or the lithium-containing impurities may remain excessively on the surface of the secondary particles, which may deteriorate the electrochemical properties of the positive active material.

[0082] In another embodiment, the coating layer may further include at least one metal oxide represented by the following Chemical Formula 3:

[0083] [Chemical formula 3] Li d M3 e O f

[0084] (where: M3 is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, P, Eu, Sm, W, Ce, V, Ba, Ta, Sn, Hf, Ce, Gd, and Nd; 0≦d≦8, 0 <e≦8、2≦f≦13である。)

[0085] The metal oxide reduces lithium-containing impurities present on the surface of the positive electrode active material and acts as a diffusion path for lithium ions, thereby improving the electrochemical properties of the positive electrode active material.

[0086] The metal oxide may be formed by further mixing the M3-containing raw material before heat-treating the mixture of the precursor of the lithium composite oxide (hydroxide precursor or roasted precursor) and the B-containing raw material, and then heat-treating the mixture. In another case, the metal oxide may be formed by heat-treating the lithium composite oxide having the boron-containing oxide formed on the surface thereof before washing the lithium composite oxide with water or after mixing the lithium composite oxide with the lithium composite oxide after washing with water.

[0087] The metal oxide may be present on at least a portion of the surface of the primary particles and / or secondary particles of the lithium composite oxide, and may be present in the same layer as or a different layer from the boron-containing oxide.

[0088] The metal oxide is an oxide of lithium and an element represented by M3 in a composite form, or an oxide of M3. The metal oxide is, for example, Li a W b O c , Li a Zr b O c , Li a Ti b O c , Li a Ni b O c , Li a Co b O c , Li a Al b O c , Co b O c , Al b O c , W b O c , Zr b O c or Ti b O c However, the above-mentioned examples are merely given for the sake of convenience to facilitate understanding, and the metal oxide defined in the present application is not limited to the above-mentioned examples.

[0089] The metal oxide may be an oxide in which lithium and at least two elements represented by M3 are combined, or may further include an oxide in which lithium and at least two elements represented by M3 are combined. The oxide in which lithium and at least two elements represented by M3 are combined may be, for example, Li a (W / Ti) b O c , Li a (W / Zr) b O c , Li a (W / Ti / Zr) b O c , Li a (W / Ti / B) b O c It may be, but is not necessarily limited to, the above.

[0090] The positive electrode active material according to the present invention is characterized in that it is composed of a lithium composite oxide including primary particles containing at least Li, Ni, and B and secondary particles formed by agglomeration of the primary particles, in which a coating layer containing a boron-containing oxide is present on at least a portion of the surface of the secondary particles, and in that at least a portion of the coating layer is removed from the surface of the secondary particles.

[0091] The coating layer may be formed by heat treating a mixture of the precursor of the lithium composite oxide and a boron-containing raw material, and at least a portion of the lithium composite oxide may be removed from the surface of the secondary particles by washing with water.

[0092] In this case, the ratio of the porosity within the secondary particles after washing with water to the porosity within the secondary particles before washing with water may be 1.7 or more.

[0093] That is, as a result of washing the lithium composite oxide with water, a part of the boron-containing oxide on the surface of the secondary particles is removed, and at the same time, a part of the boron-containing oxide present inside the secondary particles is also removed. The boron-containing oxide present inside the secondary particles may be present as a coating layer on the surface of the primary particles.

[0094] The lithium composite oxide may be washed with water to remove a portion of the boron-containing oxide present inside the secondary particles, thereby increasing the porosity of the secondary particles.

[0095] In this case, when the ratio of the porosity in the secondary particles after washing with water to the porosity in the secondary particles before washing with water for the lithium composite oxide is less than 1.7, the boron-containing oxide and / or the lithium-containing impurities remain in an excessive amount inside the secondary particles, and thus there is a risk of the electrochemical properties of the positive electrode active material being degraded.

[0096] On the other hand, when the ratio of the porosity in the secondary particles after washing with water to the porosity in the secondary particles before washing with water for the lithium composite oxide exceeds 2.0, the surface and the inside of the lithium composite oxide may be damaged, and the electrochemical properties and stability may be deteriorated. Also, since most of the boron-containing oxide is removed from the inside of the lithium composite oxide, it may be difficult to realize the effect of suppressing side reactions at the interface of the primary particles present in the secondary particles.

[0097] Lithium secondary battery According to another aspect of the present invention, there is provided a positive electrode including a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, wherein the positive electrode active material layer may include the lithium composite oxide according to the various embodiments of the present invention described above as a positive electrode active material. Therefore, a specific description of the lithium composite oxide will be omitted, and only the remaining configurations not described above will be described below. For convenience, the lithium composite oxide described above will be referred to as the positive electrode active material.

[0098] The positive electrode current collector is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity, and may be, for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The positive electrode current collector may usually have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the adhesive strength of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0099] The positive electrode active material layer may be prepared by coating a positive electrode slurry composition containing the positive electrode active material, a conductive material, and optionally a binder, on the positive electrode current collector.

[0100] At this time, the positive electrode active material may be included in an amount of 80 to 99 wt%, more specifically, 85 to 98.5 wt%, based on the total weight of the positive electrode active material layer. When included in this content range, excellent capacity characteristics can be exhibited, but the amount is not necessarily limited thereto.

[0101] The conductive material is used to impart electrical conductivity to the electrode, and can be used without any particular limitation as long as it has electronic conductivity without causing chemical changes in the battery that is constructed. Specific examples include graphite such as natural graphite and artificial graphite, carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon-based materials such as carbon fibers, metal powders or metal fibers such as copper, nickel, aluminum, and silver, conductive whiskers such as zinc oxide and potassium titanate, conductive metal oxides such as titanium oxide, and conductive polymers such as polyphenylene derivatives, and the like, and one or more of these may be used alone or in combination. The conductive material may be contained in an amount of 0.1 to 15% by weight based on the total weight of the positive electrode active material layer.

[0102] The binder serves to improve the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof, and among these, one type alone or a mixture of two or more types may be used. The binder may be included in an amount of 0.1 to 15% by weight based on the total weight of the positive electrode active material layer.

[0103] The positive electrode may be manufactured by a typical method for manufacturing a positive electrode, except for using the positive electrode active material. Specifically, the positive electrode may be manufactured by dissolving or dispersing the positive electrode active material and, optionally, a binder and a conductive material in a solvent to prepare a positive electrode slurry composition, which is then coated on a positive electrode current collector, followed by drying and rolling.

[0104] The solvent may be a solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one or more of these may be used alone or in combination. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, and to provide a viscosity that allows excellent thickness uniformity when applied to manufacture a positive electrode, taking into consideration the coating thickness of the slurry and the production yield.

[0105] In another embodiment, the positive electrode may be manufactured by casting the positive electrode slurry composition on a separate support, peeling the positive electrode slurry composition from the support, and laminating the resulting film on a positive electrode current collector.

[0106] According to yet another aspect of the present invention, there may be provided an electrochemical device including the above-mentioned positive electrode. The electrochemical device may be, for example, a battery or a capacitor, and more specifically, a lithium secondary battery.

[0107] Specifically, the lithium secondary battery may include a positive electrode, a negative electrode facing the positive electrode, and a separator and an electrolyte interposed between the positive electrode and the negative electrode. Here, since the positive electrode is as described above, a detailed description thereof will be omitted for convenience, and only the remaining components not described above will be described in detail below.

[0108] The lithium secondary battery may optionally further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0109] The negative electrode may include a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0110] The negative electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may generally have a thickness of 3 μm to 500 μm, and like the positive electrode current collector, the surface of the current collector may be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, or nonwoven fabric.

[0111] The negative electrode active material layer may be prepared by coating a negative electrode slurry composition containing the negative electrode active material, a conductive material, and optionally a binder, on the negative electrode current collector.

[0112] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon, metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys, and SiO β (0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide, or composites containing the metallic compounds and carbonaceous materials, such as Si-C composites and Sn-C composites, may be used. A metallic lithium thin film may be used as the negative electrode active material. Low-crystalline carbon and high-crystalline carbon may both be used as the carbon material. Representative examples of low crystalline carbon include soft carbon and hard carbon, and representative examples of high crystalline carbon include amorphous, plate-like, flake-like, spherical or fibrous natural graphite or artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, carbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes.

[0113] The negative electrode active material may be included in an amount of 80 to 99 wt % based on the total weight of the negative electrode active material layer.

[0114] The binder is a component that aids in bonding between the conductive material, the active material, and the current collector, and may be added in an amount of usually 0.1 to 10 wt% based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.

[0115] The conductive material may be added as a component for further improving the conductivity of the negative electrode active material in an amount of 10% by weight or less, preferably 5% by weight or less, based on the total weight of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it has conductivity without inducing a chemical change in the battery, and may be, for example, graphite such as natural graphite or artificial graphite, carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black, conductive fibers such as carbon fibers or metal fibers, metal powders such as carbon fluoride, aluminum, or nickel powder, conductive whiskey such as zinc oxide or potassium titanate, conductive metal oxides such as titanium oxide, or conductive materials such as polyphenylene derivatives.

[0116] In one embodiment, the negative electrode active material layer may be prepared by coating a negative electrode slurry composition prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent on a negative electrode current collector and drying the coating. Alternatively, the negative electrode slurry composition may be cast on a separate support, and then peeled off from the support to obtain a film, which may be laminated on the negative electrode current collector.

[0117] In another embodiment, the negative electrode active material layer may be manufactured by coating a negative electrode slurry composition prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent on a negative electrode current collector and drying the coating, or by casting the negative electrode slurry composition on a separate support and peeling the composition from the support to obtain a film, which may be laminated on the negative electrode current collector.

[0118] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode to provide a passage for lithium ions to move. Any separator generally used in lithium secondary batteries may be used without any particular limitation. In particular, it is preferable that the separator has low resistance to ion movement of the electrolyte and has excellent electrolyte humidification ability. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, in order to ensure heat resistance or mechanical strength, a separator coated with a ceramic component or a polymer material may be used, and may be selectively used as a single-layer or multi-layer structure.

[0119] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.

[0120] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0121] The organic solvent may be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone, an ether solvent such as dibutyl ether or tetrahydrofuran, a ketone solvent such as cyclohexanone, an aromatic hydrocarbon solvent such as benzene or fluorobenzene, dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvents that may be used include carbonate-based solvents such as ethylene carbonate (PC), alcohol-based solvents such as ethyl alcohol and isopropyl alcohol, nitriles such as R-CN (R is a straight-chain, branched or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is more preferred. In this case, the performance of the electrolyte may be excellent if the cyclic carbonate and the chain carbonate are mixed at a volume ratio of about 1:1 to about 1:9.

[0122] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3), LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably used within a range of 0.1 to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that excellent electrolyte performance can be exhibited and lithium ions can be effectively transferred.

[0123] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing the decrease in battery capacity, improving the discharge capacity of the battery, etc. In this case, the additives may be contained in an amount of 0.1 to 5% by weight based on the total weight of the electrolyte.

[0124] As described above, the lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics and life characteristics, and is therefore useful in the fields of portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0125] The external shape of the lithium secondary battery according to the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, etc. Furthermore, the lithium secondary battery can be used not only as a battery cell used as a power source for a small device, but also preferably as a unit battery for a medium- to large-sized battery module including a plurality of battery cells.

[0126] According to yet another aspect of the present invention, there may be provided a battery module including the lithium secondary battery as a unit cell and / or a battery pack including the same.

[0127] The battery module or the battery pack can be used as a power source for one or more medium- to large-sized devices, such as a power tool, an electric vehicle (Electric Vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV), or a power storage system.

[0128] Production Example 1. Production of positive electrode active material Example 1 Spherical Ni was prepared by the co-precipitation method. 0.80 Co 0.12 Mn 0.08 (OH)2 hydroxide precursor was synthesized. Specifically, 25 wt% NaOH and 30 wt% NH4OH were added to a 1.5M composite transition metal sulfate aqueous solution, which was a mixture of nickel sulfate, cobalt sulfate, and manganese sulfate in a molar ratio of 80:12:8, in a 90L reactor. The pH in the reactor was maintained at 11.5, the temperature of the reactor was maintained at 60°C, and inert gas N2 was added to the reactor to prevent the precursor from being oxidized. After the synthesis and stirring were completed, the mixture was filtered through a filter press (F / P) equipment to remove the Ni 0.80 Co 0.12 Mn 0.08 (OH)2 hydroxide precursor (nickel composite precursor) was obtained.

[0129] Next, the nickel composite precursor was mixed with LiOH (Li / (Ni+Co+Mn) molar ratio=1.01) as a lithium compound and 1.0 mol% of H3BO3 relative to the nickel composite precursor, and then the mixture was heat-treated for 12 hours in a sintering furnace while maintaining an O2 atmosphere by increasing the temperature by 2°C per minute up to 700°C, and then crushed to obtain a lithium composite oxide.

[0130] Next, the lithium composite oxide was washed with distilled water, and the washed lithium composite oxide was filtered and then dried.

[0131] Specifically, the lithium composite oxide was washed with water as follows. ·Primary water washing First, the lithium composite oxide and distilled water were mixed in a weight ratio of 1:1, and then stirred for 30 minutes at 25° C. to prepare a mixture. Next, the mixture was added to the composite transition metal sulfate aqueous solution used in the synthesis of the precursor, and simultaneously NaOH and NH4OH were added and stirred for 30 minutes.

[0132] Secondary washing and filtration After the primary washing was completed, the lithium composite oxide was washed with distilled water in an amount equal to the total weight of the lithium composite oxide, filtered through an F / P device, and then dried to finally obtain a positive electrode active material.

[0133] Example 2 A positive electrode active material was produced in the same manner as in Example 1, except that H3BO3 was mixed in an amount of 0.5 mol % relative to the nickel composite precursor.

[0134] Example 3 A positive electrode active material was produced in the same manner as in Example 1, except that H3BO3 was mixed in an amount of 2.0 mol % relative to the nickel composite precursor.

[0135] Example 4 A positive electrode active material was prepared in the same manner as in Example 1, except that in the second washing, the lithium composite oxide was washed with distilled water in an amount twice the total weight of the lithium composite oxide.

[0136] Example 5 A positive electrode active material was prepared in the same manner as in Example 1, except that in the second washing, the lithium composite oxide was washed with distilled water in an amount 0.5 times the total weight of the lithium composite oxide.

[0137] Example 6 The lithium composite oxide was washed with water and dried, and then mixed with 0.15 mol % of Al2O3 and 0.3 mol % of TiO2, based on the lithium composite oxide, and then further heat-treated in a sintering furnace for 8 hours by increasing the temperature by 2°C per minute to 680°C while maintaining an O2 atmosphere. A positive electrode active material was produced in the same manner as in Example 1.

[0138] Comparative Example 1 A positive electrode active material was produced in the same manner as in Example 1, except that the lithium composite oxide obtained as a result of the heat treatment of the mixture of the nickel composite precursor and the lithium compound without H3BO3 was not washed with water.

[0139] Comparative Example 2 A positive electrode active material was prepared in the same manner as in Example 1, except that H3BO3 was not mixed before the heat treatment of the nickel composite precursor.

[0140] Comparative Example 3 A positive electrode active material was prepared in the same manner as in Example 1, except that the lithium composite oxide obtained by heat-treating the mixture of the nickel composite precursor, the lithium compound, and H3BO3 was not washed with water.

[0141] Comparative Example 4 A positive electrode active material was prepared in the same manner as in Example 1, except that the lithium composite oxide was washed with distilled water in an amount three times the total weight of the lithium composite oxide during the second washing.

[0142] Comparative Example 5 A positive electrode active material was prepared in the same manner as in Example 1, except that in the second washing, the lithium composite oxide was washed with distilled water in an amount of 0.2 times the total weight of the lithium composite oxide.

[0143] Manufacturing Example 2. Manufacturing of lithium secondary batteries A positive electrode slurry was prepared by dispersing 92 wt% of the positive electrode active material prepared in Preparation Example 1, 4 wt% of artificial graphite, and 4 wt% of PVDF binder in 30 g of N-methyl-2-pyrrolidone (NMP). The positive electrode slurry was uniformly applied to a thin aluminum film having a thickness of 15 μm and dried in a vacuum at 135° C. to prepare a positive electrode for a lithium secondary battery.

[0144] A coin battery was fabricated using a lithium foil as a counter electrode for the positive electrode, a porous polyethylene film (Celgard 2300, thickness: 25 μm) as a separator, and an electrolyte of LiPF6 at a concentration of 1.15 M in a solvent of ethylene carbonate and ethyl methyl carbonate mixed in a volume ratio of 3:7.

[0145] Experimental Example 1: Analysis of the Positive Electrode Active Material (1) Measurement of boron content in lithium composite oxide before and after washing with water In order to measure the content of boron (B) in the lithium composite oxide before and after washing with water, the positive electrode active material was subjected to ICP analysis.

[0146] Specifically, 0.05 g of each of the positive electrode active materials before and after washing prepared according to Preparation Example 1 was weighed out and then added to a mixed solvent of 2 mL of nitric acid, 6 mL of hydrochloric acid, and 20 mL of ultrapure water to prepare a mixture, and the positive electrode active material in the mixture was completely dissolved. Next, ultrapure water was added to the mixture to dilute it to a total of 100 mL, and the boron (B) content in the lithium composite oxide contained in the positive electrode active material was measured using ICP-OES (Perkin Elmer, Avio 500).

[0147] The measurement results of the boron (B) content in the lithium composite oxide before and after washing with water are shown in the following Table 1. In Table 1, the rate of change before and after washing with water indicates the rate of decrease in the boron (B) content in the lithium composite oxide after washing with water relative to the boron (B) content in the lithium composite oxide before washing with water, and the values ​​in parentheses are expressed in %.

[0148] [Table 1] *nd:not detected

[0149] (2) Measurement of the content of lithium-containing impurities (LiOH) in the lithium composite oxide before and after washing with water In order to measure the content of lithium-containing impurities (LiOH) in the lithium composite oxide before and after washing with water, a pH titration analysis was carried out.

[0150] Specifically, 5 g of each of the lithium composite oxides prepared in Preparation Example 1 before and after washing was added to 100 ml of DIW, stirred (300 rpm) for 10 minutes, and then filtered. Next, 0.1 N HCl was added to 50 ml of the filtered solution, and the amount of HCl consumed due to the change in pH of the solution was measured (using a pH meter and an Ag / AgCl metal wire), and the pH value was differentiated against the amount of HCl added to obtain a differential graph.

[0151] The measurement results of the lithium impurity content (LiOH) in the lithium composite oxide before and after washing with water are shown in the following Table 2. For reference, in the cases of Comparative Example 1 and Comparative Example 3, the lithium composite oxide was not washed with water, so only the lithium impurity content (LiOH) in the lithium composite oxide before washing with water is shown.

[0152] [Table 2] *nc:not changed

[0153] Further, from the results of Tables 1 and 2, it was confirmed whether the lithium composite oxide before and after washing with water satisfied the following formulas 1 and 2, and the results are shown in Table 3 below.

[0154] [Formula 1] r<(19,153×x1)+x2

[0155] (where x1 is the boron content (mol %) in the lithium composite oxide before washing with water, x2 is the amount of LiOH (ppm) converted from the amount of HCl consumed corresponding to the x-axis value of the first peak appearing at the minimum x-axis value in a differential graph showing the differentiation of the pH value against the amount of HCl added by the neutralization titration method for the lithium composite oxide before washing with water, and r is the amount of LiOH eluted (ppm) from the lithium composite oxide after washing with water.)

[0156] [Formula 2] y1≦r≦y1+(y2×(1-y3)×18,429)

[0157] (wherein, y1 is the amount of LiOH (ppm) converted from the amount of HCl consumed corresponding to the x-axis value of the first peak appearing at the minimum x-axis value in a differential graph showing the differentiation of the pH value against the amount of HCl added by the neutralization titration method for the lithium composite oxide after washing with water, y2 is the boron content (mol %) in the lithium composite oxide before washing with water, y3 is the rate of change in the boron content in the lithium composite oxide before and after washing with water, which has a value exceeding 0 and not exceeding 0.90, and r is the amount of LiOH eluted from the lithium composite oxide after washing with water (ppm).)

[0158] [Table 3] *In the case of Comparative Example 1 and Comparative Example 3, the water-washing step was not performed, so the LiOH content after water-washing was recorded as the LiOH content in the final product, the positive electrode active material.

[0159] Experimental Example 2: Evaluation of the electrochemical properties of lithium secondary batteries A charge-discharge experiment was carried out on the lithium secondary battery (coin cell) manufactured in Manufacturing Example 2 using an electrochemical analyzer (Toyo, Toscat-3100) at 25° C., voltage range of 3.0 V to 4.3 V, and discharge rate of 0.1 C, to measure the charge and discharge capacities.

[0160] In addition, the same lithium secondary battery was charged and discharged 50 times at 25°C and within a driving voltage range of 3.0 V to 4.4 V at 1 C / 1 C, and then the ratio of the discharge capacity at the 50th cycle to the initial capacity (cycle capacity retention) was measured.

[0161] The measurement results are shown in Table 4 below.

[0162] [Table 4]

[0163] Experimental Example 3. Evaluation of the stability of positive electrode active materials and lithium secondary batteries (1) Evaluation of thermal stability of positive electrode active material In order to evaluate the thermal stability of the positive electrode active material prepared in Preparation Example 1, the weight loss was measured at a heating rate of 10°C / min from 25°C to 350°C under Ar atmosphere at normal pressure using a thermogravimetric analyzer (TA Instruments, Q20). The on-set temperature at which the weight loss (thermal decomposition) peak appeared for each positive electrode active material is shown in Table 5 below.

[0164] [Table 5]

[0165] Referring to the results in Table 5, it can be seen that the thermal decomposition starting temperatures of the positive electrode active materials according to Examples 1 to 6 are higher than those of the positive electrode active materials according to Comparative Examples 1 to 5.

[0166] In particular, as shown in Table 4, the lithium secondary batteries using the positive electrode active materials according to Comparative Examples 3 and 5 appear to have similar levels in some indicators of electrochemical characteristics to the lithium secondary batteries using the positive electrode active materials according to Examples 1 to 6. However, as shown in Table 5, it can be seen that the thermal stability of the positive electrode active material is insufficient (in the case of Comparative Example 3, the level is similar to that of Example 4, which was subjected to the most severe water washing conditions among the Examples).

[0167] (2) Measurement of gas generation rate of lithium secondary batteries The lithium secondary battery prepared according to Preparation Example 2 was charged to 4.25 V at a constant current of 0.2 C and then stored at 60° C. for 14 days to measure the volume change of the lithium secondary battery caused by gas generation in the lithium secondary battery. The measurement results of the volume change are shown in Table 6 below.

[0168] [Table 6]

[0169] Referring to the results in Table 6, it can be seen that the volume change rate during high-temperature storage of the lithium secondary batteries prepared according to Preparation Example 2 using the positive electrode active materials according to Examples 1 to 6 is smaller than that of the lithium secondary batteries using the positive electrode active materials according to Comparative Examples 1 to 5.

[0170] In particular, as shown in Table 4, the lithium secondary batteries using the positive electrode active materials according to Comparative Examples 3 and 5 were found to have similar levels of some indicators of electrochemical characteristics to the lithium secondary batteries using the positive electrode active materials according to Examples 1 to 6. However, as shown in Table 6, it was confirmed that the high-temperature storage stability was insufficient.

[0171] Although the embodiments of the present invention have been described above, a person having ordinary knowledge in the art may modify and change the present invention in various ways by adding, changing, deleting or adding elements within the scope of the concept of the present invention described in the claims, and this may also be considered to be within the scope of the present invention.

Claims

1. A positive electrode active material composed of a lithium composite oxide including primary particles containing at least Li, Ni, and B, and secondary particles formed by agglomeration of the primary particles, a coating layer containing a boron-containing oxide is present on at least a portion of the surface of the secondary particles; The content of boron (B) in the lithium composite oxide is 0.09 mol % or more and 0.49 mol % or less, The content of lithium impurities (LiOH) in the lithium composite oxide is 11,661 ppm or less, A positive electrode active material, in which the weight loss is measured at a temperature increase rate of 10°C / min from 25°C to 350°C in an Ar atmosphere at normal pressure, and the onset temperature at which a weight loss (thermal decomposition) peak appears is 231.2°C or higher.

2. The positive electrode active material according to claim 1 , wherein the primary particles are represented by the following chemical formula 1: [Chemical formula 1] Li w Ni 1-(x+y+z+z′) Co x B y M1 z M2 z′ O 2 (where: M1 is at least one selected from Mn and Al; M2 is at least one selected from Mn, Ba, Ce, Hf, Ta, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr, Ge, Nd, Gd and Cu; M1 and M2 are different elements, 0.5≦w≦1.5, 0≦x≦0.50, 0<y≦0.20, 0≦z≦0.20, 0≦z′≦0.20)

3. The positive electrode active material of claim 1 , wherein the coating layer further comprises at least one metal oxide represented by the following Chemical Formula 3: [Chemical formula 3] Li d M3 e O f (where: M3 is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, P, Eu, Sm, W, Ce, V, Ba, Ta, Sn, Hf, Gd, and Nd; 0≦d≦8, 0<e≦8, 2≦f≦13)

4. The positive electrode active material according to claim 1 , wherein the coating layer is formed by heat-treating a mixture of the lithium composite oxide precursor and a boron-containing raw material.

5. The positive electrode active material according to claim 1 , wherein the coating layer is at least partially removed from the surfaces of the secondary particles by washing the lithium composite oxide with water.

6. 6. The positive electrode active material according to claim 5, wherein the lithium composite oxide has a residual boron content of 0.3 mol % or less after washing with water.

7. The positive electrode active material according to claim 1 , wherein an amount of LiOH dissolved from the positive electrode active material measured by a neutralization titration method using HCl satisfies the following formula 1: [Formula 1] r<(19,153×x1)+x2 (where: x1 is the boron content (mol%) in the lithium composite oxide before washing with water, x2 is the amount of LiOH (ppm) calculated from the amount of HCl consumed corresponding to the x-axis value of the first peak appearing at the minimum x-axis value in the differential graph showing the differentiation of pH value versus the amount of HCl added by the neutralization titration method for the lithium composite oxide before washing with water; r is the amount (ppm) of LiOH dissolved from the lithium composite oxide after washing with water.

8. The positive electrode active material according to claim 1 , wherein an amount of LiOH dissolved from the positive electrode active material measured by a neutralization titration method using HCl satisfies the following formula 2: [Formula 2] y1≦r≦y1+(y2×(1-y3)×18,429) (where: y1 is the amount of LiOH (ppm) calculated from the amount of HCl consumed corresponding to the x-axis value of the first peak appearing at the minimum x-axis value in the differential graph showing the differentiation of the pH value versus the amount of HCl added by the neutralization titration method for the lithium composite oxide after washing with water; y2 is the content (mol%) of boron in the lithium composite oxide before washing with water, y3 is a rate of change in the boron content in the lithium composite oxide before and after washing with water, and has a value exceeding 0 and not exceeding 0.90; r is the amount (ppm) of LiOH dissolved from the lithium composite oxide after washing with water.

9. 6. The positive electrode active material according to claim 5, wherein a ratio of the porosity within the secondary particles after washing with water to the porosity within the secondary particles before washing with water for the lithium composite oxide is 1.7 or more.

10. A positive electrode active material composed of a lithium composite oxide including primary particles containing at least Li, Ni, and B, and secondary particles formed by agglomeration of the primary particles, a coating layer containing a boron-containing oxide is present on at least a portion of the surface of the secondary particles; The coating layer includes at least one boron-containing oxide represented by the following Chemical Formula 2: [Chemical formula 2] Li a B b O c (where: 0≦a≦8, 0<b≦8, 2≦c≦13) A positive electrode active material, wherein an amount of LiOH dissolved from the positive electrode active material, as measured by a neutralization titration method using HCl, satisfies the following formula 1: [Formula 1] r<(19,153×x1)+x2 (where: x1 is the boron content (mol%) in the lithium composite oxide before washing with water, x2 is the amount of LiOH (ppm) calculated from the amount of HCl consumed corresponding to the x-axis value of the first peak appearing at the minimum x-axis value in the differential graph showing the differentiation of pH value versus the amount of HCl added by the neutralization titration method for the lithium composite oxide before washing with water; r is the amount (ppm) of LiOH dissolved from the lithium composite oxide after washing with water.

11. A positive electrode active material composed of a lithium composite oxide including primary particles containing at least Li, Ni, and B, and secondary particles formed by agglomeration of the primary particles, a coating layer containing a boron-containing oxide is present on at least a portion of the surface of the secondary particles; The coating layer includes at least one boron-containing oxide represented by the following Chemical Formula 2: [Chemical formula 2] Li a B b O c (where: 0≦a≦8, 0<b≦8, 2≦c≦13) A positive electrode active material, wherein an amount of LiOH dissolved from the positive electrode active material, as measured by a neutralization titration method using HCl, satisfies the following formula 2: [Formula 2] y1≦r≦y1+(y2×(1-y3)×18,429) (where: y1 is the amount of LiOH (ppm) calculated from the amount of HCl consumed corresponding to the x-axis value of the first peak appearing at the minimum x-axis value in the differential graph showing the differentiation of the pH value versus the amount of HCl added by the neutralization titration method for the lithium composite oxide after washing with water; y2 is the content (mol%) of boron in the lithium composite oxide before washing with water, y3 is a rate of change in the boron content in the lithium composite oxide before and after washing with water, and has a value exceeding 0 and not exceeding 0.90; r is the amount (ppm) of LiOH dissolved from the lithium composite oxide after washing with water.

Citation Information

Patent Citations

  • Lithium ion battery, surface-modified ternary material and preparation method

    CN108767212A

  • Method for manufacturing positive electrode active material for secondary battery and positive electrode active material for secondary battery, manufactured according to same

    EP3388394A1

  • Cathode active material for secondary battery, method for manufacturing same, and lithium secondary battery comprising same

    EP3473600A1

  • Lithium manganese composite oxide granule secondary particle and method for producing the same and application thereof

    JP2004083388A

  • Lithium ion secondary battery and method of manufacturing cathode active material for lithium ion secondary battery

    JP2013137947A

Cited By

  • Positive electrode active material for lithium ion secondary battery, positive electrode for lithium ion secondary battery, and lithium ion secondary battery

    WO2026205576A1

  • Positive electrode active material for lithium-ion secondary battery, positive electrode for lithium-ion secondary battery, and lithium-ion secondary battery

    WO2026205579A1