Electrolyte enclosed structure

The electrolyte encapsulation structure with controlled oxygen and moisture levels in dual packaging bodies maintains the ionic conductivity of sulfide solid electrolytes by minimizing reactions during storage and transportation.

JP2024145441APending Publication Date: 2024-10-15MITSUI MINING & SMELTING CO LTD

Patent Information

Application Number
JP2023057791
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Sulfide solid electrolytes in powder form react with moisture and oxygen in the atmosphere, leading to a decrease in ionic conductivity during storage and transportation, and conventional packaging materials with high moisture and oxygen permeability exacerbate this issue.

Method used

An electrolyte encapsulation structure comprising a first packaging body that encapsulates the sulfide solid electrolyte and a second packaging body that accommodates the first, with both spaces maintaining an oxygen concentration of 30% or less and a dew point temperature of -20°C or less, using materials like aluminum and organic resins to minimize permeability.

Benefits of technology

The structure effectively maintains the ionic conductivity of the sulfide solid electrolyte over time by preventing reactions with moisture and oxygen, ensuring high storage efficiency and protection against external forces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145441000001_ABST
    Figure 2024145441000001_ABST
Patent Text Reader

Abstract

To provide an electrolyte enclosed structure with which an enclosed sulfide solid electrolyte is less prone to be decreased in ion conductivity over time.SOLUTION: Provided is an electrolyte enclosed structure 1 having a sulfide solid electrolyte 3, a first package 100 in which the sulfide solid electrolyte 3 is enclosed, and a second package 200 that houses the first package 100 to enclose. In the electrolyte enclosed structure 1, both inside a first space 109 of the first package 100, the space being defined by an inner surface 107 which is a front surface of the side to which the sulfide solid electrolyte 3 is enclosed, and inside a second space 209 defined by an outer surface 108 of the first package 100 and an inner surface 207 of the second package 200, a filling FG having an oxygen concentration of 30% or less and a dew point temperature of -20°C or less is enclosed.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrolyte containment structure. [Background technology]

[0002] In recent years, CO 2 Secondary batteries have been attracting attention as an effort to prevent global warming by reducing CO2 emissions. As such secondary batteries, solid-state batteries using a sulfide solid electrolyte are known. As sulfide solid electrolytes, for example, materials having an argyrodite-type crystal structure are known from the viewpoint of further improving lithium ion conductivity. Here, the argyrodite-type crystal structure is a material having the chemical formula: Ag 8 GeS 6 The sulfide solid electrolyte used as an electrolyte for a solid-state battery is usually in a powder form. After production, the powdered sulfide solid electrolyte is usually sealed in a package, and then stored and transported. Hereinafter, a structure in which a sulfide solid electrolyte is sealed in a package is also referred to as an "electrolyte-encapsulated structure."

[0003] However, the sulfide solid electrolyte is likely to react easily with moisture and oxygen in the air and to decrease in ionic conductivity, and therefore, it is preferable that the electrolyte encapsulation structure has a structure that makes it difficult for the sulfide solid electrolyte to react with moisture and oxygen in the air during storage and transportation.

[0004] Moreover, the sulfide solid electrolyte is usually in the form of a powder whose shape and particle size are controlled within a predetermined range. When a large external force is applied to the sulfide solid electrolyte powder, the particles may be damaged, and the desired characteristics may not be exhibited. For this reason, it is preferable that the shape and particle size of the sulfide solid electrolyte are unlikely to change during storage and transportation.

[0005] As a conventional example of an electrolyte encapsulation structure, Patent Document 1 discloses a water-absorbent sulfur-based gas absorbing packaging material for a sulfide-based inorganic solid electrolyte type all-solid-state lithium ion battery that absorbs gaseous water and / or liquid water and sulfur-based gas. This water-absorbent sulfur-based gas absorbing packaging material includes a base layer made of nylon film or the like, a gas barrier layer made of aluminum foil, a resin film made of oxygen barrier resin, or the like, and a heat-sealable sealant layer made of a water-absorbent sulfur-based gas absorbing sealant film, and the sealant layer is said to include a sulfur-based gas absorbent, an inorganic water absorbent, and a heat-sealable resin. Note that the examples of Patent Document 1 disclose only aluminum foil as the gas barrier layer, and do not disclose a resin film made of oxygen barrier resin. When a sulfide solid electrolyte is encapsulated in a package with the sealant layer of the water-absorbent sulfur-based gas absorbing packaging material of Patent Document 1 on the inside, an electrolyte encapsulation structure is formed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent Publication No. 2021-57232 Summary of the Invention [Problem to be solved by the invention]

[0007] However, the water-absorbent sulfur-based gas absorbing packaging material shown in the examples of Patent Document 1 has a high relative humidity of up to 45% in a relative humidity test using a gas absorbing film that is part of the layer structure, and the base layer is made of a nylon film or the like that is generally known as a material with high moisture permeability and oxygen permeability. Therefore, if an electrolyte encapsulation structure in which a sulfide solid electrolyte is encapsulated is used in this water-absorbent sulfur-based gas absorbing packaging material, there is a risk that the ionic conductivity of the sulfide solid electrolyte will decrease due to the reaction between the sulfide solid electrolyte and moisture and oxygen in the air during storage and transportation.

[0008] The present invention has been made in consideration of the above problems, and has an object to provide an electrolyte containment structure in which the ionic conductivity of the enclosed sulfide solid electrolyte is less likely to decrease over time. [Means for solving the problem]

[0009] The inventors have discovered that an electrolyte containment structure having a first packaging body that contains a sulfide solid electrolyte and a second packaging body that contains and encloses the first packaging body, and that by sealing a filling gas (FG) having an oxygen concentration of 30% or less and a dew point temperature of -20°C or less in both a first space partitioned by the inner surface of the first packaging body and a second space partitioned by the outer surface of the first packaging body and the inner surface of the second packaging body, an electrolyte containment structure can be obtained in which the ionic conductivity of the sealed sulfide solid electrolyte is less likely to decrease, and have completed the present invention.

[0010] That is, the gist of the present invention is as follows. (1) The electrolyte containment structure of the present invention is an electrolyte containment structure having a sulfide solid electrolyte, a first packaging body that contains the sulfide solid electrolyte, and a second packaging body that contains and contains the first packaging body, and a filling gas having an oxygen concentration of 30% or less and a dew point temperature of -20°C or less is contained in both a first space defined by the inner surface of the first packaging body, which is the surface that contains the sulfide solid electrolyte, and in a second space defined by the outer surface of the first packaging body and the inner surface of the second packaging body.

[0011] (2) It is preferable that the device further includes a third packaging body that contains and encloses the second packaging body, and that a filling gas having an oxygen concentration of 30% or less and a dew point temperature of -20°C or less is enclosed in a third space defined by the outer surface of the second packaging body and the inner surface of the third packaging body.

[0012] (3) The filling gas is Ar, air, N 2 or CO 2 It is preferable that:

[0013] (4) It is preferable that the packaging material constituting the first package includes a layer made of aluminum.

[0014] (5) It is preferable that the packaging material constituting the first packaging body has an inner welded portion made of a weldable organic material and an outer non-welded portion which is a layer made of aluminum and is laminated on the outer surface of the inner welded portion.

[0015] (6) The organic material is preferably one or more organic resins selected from the group consisting of polyethylene terephthalate (PET), polyethylene (PE), chlorinated polyethylene (SPE), high density polyethylene, nylon, and polyvinyl alcohol.

[0016] (7) The first package is preferably a heat-sealed bag having an opening sealed therein.

[0017] (8) The first package is preferably a lidded bottle equipped with a screw cap.

[0018] (9) The first packaging body is preferably made of a packaging material having a layer made of an organic substance. Effect of the Invention

[0019] According to the present invention, it is possible to provide an electrolyte containment structure in which the ionic conductivity of the contained sulfide solid electrolyte is unlikely to decrease over time. [Brief description of the drawings]

[0020] [Figure 1] 1 is a plan view showing an electrolyte containment structure according to a first embodiment of the present invention; [Diagram 2] FIG. 2 is a diagram showing the internal state of the electrolyte containment structure of FIG. 1 so as to be clearly understood. [Diagram 3] FIG. 6 is a perspective view of a package constituting the electrolyte containment structure of FIGS. 1 and 5, with the opening in an open state. [Figure 4] 4 is a cross-sectional view of a packaging material that constitutes the package of FIG. 3. [Diagram 5] FIG. 4 is a plan view showing an electrolyte containment structure according to a modified example of the first embodiment of the present invention. [Figure 6] FIG. 6 is a diagram showing the internal state of the electrolyte containment structure of FIG. 5 so as to be clearly understood. [Figure 7] FIG. 4 is a perspective view showing an electrolyte containment structure according to a second embodiment of the present invention. [Figure 8] FIG. 8 is a diagram showing the internal state of the electrolyte containment structure of FIG. 7 so as to be clearly understood. [Figure 9] 13 is a perspective view of a package constituting the electrolyte containment structure of FIG. 7 and FIG. 12, with the opening in a closed state. FIG. [Figure 10] FIG. 8 is an exploded perspective view of a package constituting the electrolyte containment structure of FIG. 7. [Figure 11] 10 is a cross-sectional view of a packaging material that constitutes the package of FIG. 9. [Figure 12] 1 is a perspective view showing an electrolyte containment structure according to a modified example of the second embodiment of the present invention, and FIG. 2 is a schematic view showing an electrolyte containment structure according to a modified example of the second embodiment of the present invention. [Figure 13] FIG. 13 is a diagram showing the internal state of the electrolyte containment structure of FIG. 12 so as to be clearly understood. [Figure 14] FIG. 1 is a plan view showing a conventional electrolyte containment structure. [Figure 15] FIG. 15 is a diagram showing the internal state of the electrolyte containment structure of FIG. 14 so as to be clearly understood. [Figure 16] 15 is a perspective view of a package constituting the electrolyte containment structure of FIG. 14, with the opening open. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that the shape and size of the drawings are appropriately changed for convenience of explanation. Therefore, the present invention is not limited to the shape of the drawings.

[0022] [Electrolyte Encapsulation Structure] <First embodiment> Fig. 1 is a plan view showing an electrolyte containment structure according to a first embodiment of the present invention, Fig. 2 is a diagram showing the internal state of the electrolyte containment structure of Fig. 1, Fig. 3 is a perspective view of a package constituting the electrolyte containment structure of Fig. 1 and Fig. 5, with the opening open, Fig. 4 is a cross-sectional view of a package constituting the package of Fig. 3.

[0023] As shown in Fig. 1 and Fig. 2, the electrolyte encapsulation structure 1AB(1) according to the first embodiment includes a first packaging body 100A(120) that encapsulates a sulfide solid electrolyte 3, and a second packaging body 200A(220) that accommodates and encapsulates the first packaging body 100A. The first packaging body 100A, for example, a heat-sealed bag 120, has a thickness in a direction perpendicular to the paper surface of Fig. 1 because the sulfide solid electrolyte 3 is encapsulated inside a bag body 121 constituting the first packaging body 100A. In addition, the bag body 221 of the second packaging body 200A that accommodates and encapsulates the first packaging body 100A also has a thickness in a direction perpendicular to the paper surface of Fig. 1. Note that in Fig. 2, the thicknesses of the bag bodies 121 and 221 are exaggerated more than they actually are.

[0024] The first packaging body 100A containing the sulfide solid electrolyte 3 corresponds to a structure obtained by removing the second packaging body 200A from the electrolyte containment structure 1AB, in other words, an intermediate body of the electrolyte containment structure. The structure made of the first packaging body 100A containing the sulfide solid electrolyte 3 is hereinafter also referred to as the electrolyte containment intermediate structure 7A(7).

[0025] 3, the first packaging body 100A is formed into a heat-sealed bag 120 capable of encapsulating the sulfide solid electrolyte 3 by forming a heat-sealed portion 123 by welding at least a portion of the sealing portion 122. The first packaging body 100A is formed into the heat-sealed bag 120 with an opening 127 welded.

[0026] 3, the second packaging body 200A is formed into a heat-sealed bag 220 capable of enclosing the first packaging body 100A by welding at least a part of the sealing portion 222 to form a heat-sealed portion 223. The second packaging body 200A is formed into a heat-sealed bag 220 with an opening 227 welded.

[0027] (Sulfide solid electrolyte) The sulfide solid electrolyte 3 typically contains lithium (Li), phosphorus (P) and sulfur (S). When the sulfide solid electrolyte 3 has an argyrodite-type crystal structure, it has high lithium ion conductivity and is electrochemically stable, and therefore exhibits favorable characteristics as an all-solid-state battery. Here, the argyrodite-type crystal structure is represented by the chemical formula: Ag 8 GeS 6 The specific composition formula of the sulfide solid electrolyte 3 is Li 6 P.S. 5 Cl, Li 6 P.S. 5 Br, Li 5.5 P.S. 4.5 Cl 1.5 , Li 5.4 P.S. 4.4 Cl 0.8 Br 0.8 , Li 6 P.S. 5 I etc.

[0028] The contents of lithium (Li), phosphorus (P) and sulfur (S) in the sulfide solid electrolyte 3 can be adjusted as appropriate.

[0029] The sulfide solid electrolyte 3 has a Li element content of preferably 41 mol% or more, more preferably 42 mol% or more, and even more preferably 43 mol% or more, where the total molar amount of the constituent elements of the sulfide solid electrolyte 3 is taken as 100 mol%. The Li element content is preferably 50 mol% or less, more preferably 48 mol% or less, even more preferably 47 mol% or less, and even more preferably 45% or less. When the Li element content is within the above range, the lithium ion conductivity of the sulfide solid electrolyte 3 is likely to be improved.

[0030] The sulfide solid electrolyte 3 has a P element content of preferably 7.0 mol % or more, more preferably 7.2 mol % or more, even more preferably 7.5 mol % or more, and even more preferably 7.7 mol % or more, where the total molar amount of the constituent elements of the sulfide solid electrolyte 3 is taken as 100 mol %. The above content is preferably 20 mol % or less, more preferably 18 mol % or less, even more preferably 16 mol % or less, and even more preferably 12 mol % or less. When the P element content is within the above range, the lithium ion conductivity of the sulfide solid electrolyte 3 is likely to be improved.

[0031] The sulfide solid electrolyte 3 has an S element content of preferably 31 mol% or more, more preferably 32 mol% or more, even more preferably 33 mol% or more, and even more preferably 34 mol% or more, where the total molar amount of the constituent elements of the sulfide solid electrolyte 3 is taken as 100 mol%. The above content is preferably 43 mol% or less, more preferably 42 mol% or less, even more preferably 40 mol% or less, and even more preferably 38 mol% or less. When the S element content is within the above range, the lithium ion conductivity of the sulfide solid electrolyte 3 is likely to be improved.

[0032] The sulfide solid electrolyte 3 has a molar ratio of the Li element content to the P element content (Li element content / P element content) of preferably 4.8 or more, more preferably 5.0 or more, and even more preferably 5.2 or more. The molar ratio is preferably 7.0 or less, more preferably 6.4 or less, and even more preferably 5.8 or less. When the molar ratio is within the above range, the lithium ion conductivity of the sulfide solid electrolyte 3 is likely to be improved.

[0033] The sulfide solid electrolyte 3 has a molar ratio of the S element content to the P element content (S element content / P element content) of preferably 3.6 or more, more preferably 4.0 or more, and even more preferably 4.2 or more. The molar ratio is preferably 6.0 or less, more preferably 5.0 or less, and even more preferably 4.6 or less. When the molar ratio is within the above range, the lithium ion conductivity of the sulfide solid electrolyte 3 is likely to be improved.

[0034] The sulfide solid electrolyte 3 preferably further contains at least one halogen (X) element selected from fluorine (F), chlorine (Cl), bromine (Br) and iodine (I), and more preferably further contains at least one X element selected from Cl and Br. When the sulfide solid electrolyte 3 further contains the above-mentioned elements, the lithium ion conductivity of the sulfide solid electrolyte 3 is likely to be improved.

[0035] The sulfide solid electrolyte 3 has an X element content of preferably 3.7 mol% or more, more preferably 4.0 mol% or more, even more preferably 8.0 mol% or more, and even more preferably 10 mol% or more, where the total molar amount of the constituent elements of the sulfide solid electrolyte 3 is taken as 100 mol%. The content is preferably 19 mol% or less, more preferably 17 mol% or less, even more preferably 15 mol% or less, and even more preferably 14 mol% or less. When the sulfide solid electrolyte 3 contains two or more X elements, the "content of the X element" means the total content of the two or more X elements. When the content of the X element is within the above range, the lithium ion conductivity of the sulfide solid electrolyte 3 is easily improved.

[0036] In the sulfide solid electrolyte 3, the molar ratio of the content of X element to the content of P element (content of X element / content of P element) is preferably 0.50 or more, more preferably 0.80 or more, and even more preferably 1.2 or more. Moreover, the molar ratio is preferably 2.1 or less, more preferably 2.0 or less, and even more preferably 1.8 or less. When the molar ratio is within the above range, the lithium ion conductivity of the sulfide solid electrolyte 3 is likely to be improved.

[0037] The sulfide solid electrolyte 3 may contain one or more elements (hereinafter referred to as "other elements") other than Li, P, S, and X. Examples of other elements include silicon (Si), germanium (Ge), tin (Sn), lead (Pb), boron (B), aluminum (Al), gallium (Ga), arsenic (As), antimony (Sb), and bismuth (Bi).

[0038] Sulfide solid electrolyte 3 is D 50 is preferably 0.10 μm or more, more preferably 0.50 μm or more, even more preferably 1.0 μm or more, and particularly preferably 2.0 μm or more. The molar ratio is preferably 100 μm or less, more preferably 50 μm or less, even more preferably 30 μm or less, and particularly preferably 10 μm or less. 50 When D is within the above range, the sulfide solid electrolyte 3 is uniformly distributed inside the positive and negative electrodes, and good battery characteristics are easily obtained. 50 is the particle size at which the cumulative volume is 50% in the volume-based particle size distribution of the powder measured by a laser diffraction / scattering particle size distribution measurement method.

[0039] (First package) The first packaging body 100A is a structure in which the sulfide solid electrolyte 3 is enclosed.

[0040] In the electrolyte containment structure 1AB, a specific filling gas FG is sealed within a first space 109 defined by an inner surface 107, which is the surface of the first packaging body 100A that contains the sulfide solid electrolyte 3.

[0041] The first packaging body 100A has a function (hereinafter also referred to as a "first sealing function") of sealing the sulfide solid electrolyte 3. If the first packaging body 100A further has a function of low moisture permeability (hereinafter also referred to as a "first low moisture permeability function"), this is preferable because the ionic conductivity of the sulfide solid electrolyte 3 sealed in the first packaging body 100A is less likely to decrease.

[0042] As shown in FIGS. 2 and 3, the first packaging body 100A is made by using a sheet-like packaging material 110 to form a heat-sealed bag 120 in which the sulfide solid electrolyte 3 can be sealed.

[0043] 3, the heat-sealed bag 120 constituting the first packaging body 100A includes a bag body 121 and a sealing portion 122 which is a strip-shaped member formed continuously with the bag body 121 and which forms an opening 127 at an end. At least a portion of the sealing portion 122 is welded to form a heat-sealed portion 123, which makes it possible to enclose the sulfide solid electrolyte 3 in the first packaging body 100A.

[0044] 3, in first packaging body 100A, the sulfide solid electrolyte 3 is enclosed in a first space 109 defined by inner surface 107, which is the surface of first packaging body 100A that encloses sulfide solid electrolyte 3. First packaging body 100A made of heat-sealed bag 120 has a relatively flat shape, and therefore has high storage space efficiency.

[0045] A fill gas FG is sealed in the first space 109. The fill gas FG may be, for example, Ar, air, or N 2 or CO 2 Among these, Ar is preferred because it has low reactivity with the sulfide solid electrolyte 3. The filler gas FG present in the first space 109 is hereinafter also referred to as a first space gas 119. Note that the composition of the first space gas 119 may change due to a reaction with the sulfide solid electrolyte 3, etc.

[0046] The filler gas FG sealed in the first space 109 has an oxygen concentration of 30% or less and a dew point temperature of -20° C. or less. If the oxygen concentration and dew point temperature of the filler gas FG are within the above ranges, this is preferable because the ionic conductivity of the sulfide solid electrolyte 3 sealed in the first packaging body 100A is less likely to decrease.

[0047] The oxygen concentration of the filler gas FG sealed in the first space 109 is preferably 10% or less, more preferably 5% or less, and further preferably 1% or less. The oxygen concentration of the filler gas FG is preferably within the latter range, since the ionic conductivity of the sulfide solid electrolyte 3 sealed in the first packaging body 100A is less likely to decrease.

[0048] The dew point temperature of the filler gas FG sealed in the first space 109 is preferably −30° C. or less, more preferably −40° C. or less, and even more preferably −50° C. or less. The closer the dew point temperature of the filler gas FG is to the latter range, the more the reaction between the sulfide solid electrolyte 3 sealed in the first packaging body 100A and moisture is suppressed, and the less the ion conductivity is reduced, which is preferable.

[0049] In the first packaging body 100A in which the sulfide solid electrolyte 3 is sealed, the volume V of the first space 109 is 1 (cm 3 ) the volume V of the sulfide solid electrolyte 3 itself SE (cm 3 ) ratio (V SE / V 1 ) is, for example, more than 0%, preferably 10% or more, and more preferably 20% or more. The above-mentioned filling rate is, for example, 50% or less, preferably 40% or less, and more preferably 30% or less. When the first filling rate is more than 0%, the storage space efficiency tends to be high. When the first filling rate is 50% or less, aggregation and changes in particle shape due to crushing of the particles of the sulfide solid electrolyte 3 tend to be suppressed.

[0050] The first packing ratio (%) is, for example, the true density Dt (g / cm 3 ) of the sulfide solid electrolyte 3 obtained by a pycnometer method (gas replacement method). 3 ) multiplied by the mass M (g) of the sulfide solid electrolyte 3 to obtain the internal volume V of the packaging material. 1 (cm 3 ) and then multiply this value by 100 to get (1 / Dt)M / V 1 This can be calculated by multiplying by 100.

[0051] The packaging material 110 constituting the first packaging body 100A is made of a material and has a structure capable of sealing a specific filling gas FG within a first space 109 partitioned by an inner surface 107, which is the surface on the side that seals the sulfide solid electrolyte 3.

[0052] The packaging material 110 constituting the first packaging body 100A has a multilayer structure in which the entire heat-sealed bag 120, including the sealing portion 122, has an inner welded portion 117 made of a weldable organic material and an outer non-welded portion 118, which is a layer made of, for example, aluminum, laminated on the outer surface of the inner welded portion 117, as shown in Figure 4.

[0053] When the packaging material 110 has such a multi-layer structure, the moisture permeability is, for example, 10 (g / m 2 When the outer non-welded parts 118 made of a material with a low moisture permeability as described below (hereinafter also referred to as a "low moisture permeability material") are used, the first packaging body 100A can be provided with a first sealing function of sealing in the sulfide solid electrolyte 3 by welding the inner welded parts 117, and a first low moisture permeability function by the outer non-welded parts 118.

[0054] Here, the inner welding portion 117 refers to a member that includes the inner surface 107, which is the surface of the packaging material 110 that is located on the sulfide solid electrolyte 3 side when the sulfide solid electrolyte 3 is enclosed, and contributes to welding. The inner surface 107 and the surface are shown in FIG.

[0055] The inner welded portion 117 may be a single layer structure made of one or more types of weldable organic material, or may be a multi-layer structure (not shown) in which two or more types of weldable organic material are formed into two or more layers. When the inner welded portion 117 has a multi-layer structure, the inner welded portion 117 has an innermost layer including the inner surface 107, and one or more adjacent inner layers laminated on the outer non-welded portion 118 side as viewed from the innermost layer.

[0056] For example, the inner welded portion 117 can have a two-layer structure including an innermost layer made of a weldable organic material W1 and including the inner surface 107, and a first adjacent inner layer made of a weldable organic material W2 and laminated on the outer non-welded portion 118 side as viewed from the innermost layer.

[0057] In addition, the inner welded portion 117 can have a three-layer structure including an innermost layer made of a weldable organic material W1 and including the inner surface 107, a first adjacent inner layer made of a weldable organic material W2 and laminated on the outer non-welded portion 118 side as viewed from the innermost layer, and a second adjacent inner layer made of a weldable organic material W3 and laminated on the outer non-welded portion 118 side as viewed from the first adjacent inner layer.

[0058] The outer non-welded portion 118 refers to a member that includes the outer surface 108, which is the surface opposite to the inner surface 107 when the sulfide solid electrolyte 3 is enclosed, among the surfaces of the packaging material 110 and does not contribute to welding. The outer surface 108 and the surface are shown in FIG. 2.

[0059] The outer non-welded portion 118 may have a single layer structure made of one or more materials, or may have a multi-layer structure (not shown) made of two or more materials. When the outer non-welded portion 118 has a multi-layer structure, the outer non-welded portion 118 has an outermost layer including the outer surface 108, and one or more auxiliary outer layers laminated on the inner welded portion 117 side as viewed from the outermost layer.

[0060] For example, the outer non-welded portion 118 can have a two-layer structure including an outermost layer made of material N1 and including the outer surface 108, and a first adjacent outer layer made of material N2 and laminated on the inner welded portion 117 side as viewed from the outermost layer.

[0061] In addition, the outer non-welded portion 118 can have a three-layer structure including an outermost layer made of material N1 and including the outer surface 108, a first adjacent outer layer made of material N2 and laminated on the inner welded portion 117 side as viewed from the outermost layer, and a second adjacent outer layer made of material N3 and laminated on the inner welded portion 117 side as viewed from the first adjacent outer layer.

[0062] As the weldable organic material constituting the inner weld portion 117, for example, one or more organic resins selected from polyethylene terephthalate (PET), polyethylene (PE), chlorinated polyethylene (SPE), high density polyethylene, nylon, and polyvinyl alcohol are used. Among these, polyethylene PE is preferred because of its high versatility and excellent recyclability.

[0063] Each of the one or more layers constituting the inner weld portion 117 may be made of one or more organic resins that are weldable organic materials. For example, the inner weld portion 117 may include a layer made of one organic resin and a layer made of two or more organic resins. The layer made of two or more organic resins may be, for example, a layer made of a mixture of two or more organic resins.

[0064] It is preferable that the outer unwelded portion 118 is made of a low moisture permeable material, since this can impart a first low moisture permeability function to the first packaging body 100A.

[0065] Examples of low moisture permeable materials used for the outer non-welded portion 118 include metals such as aluminum, stainless steel, and iron, and organic materials such as one or more organic resins selected from polyethylene terephthalate (PET), polyethylene (PE), chlorinated polyethylene (SPE), high density polyethylene, nylon, and polyvinyl alcohol. Among these, aluminum is preferable because it is easy to reduce the moisture permeability of the packaging material 110 constituting the first packaging body 100A.

[0066] For this reason, it is preferable that the packaging material 110 includes an aluminum layer 118 as the outer non-welded portion 118, since this makes it easier to reduce the moisture permeability of the packaging material 110.

[0067] Each of the one or more layers constituting the outer non-welded portion 118 may be made of one or more materials. For example, the outer non-welded portion 118 may include a layer made of one material and a layer made of two or more materials. The layer made of two or more materials may be, for example, a layer made of a mixture of two or more organic resins.

[0068] As the multi-layered packaging material 110, for example, a three-layered packaging material can be used in which, from the inner surface 107 side, an innermost layer of an inner welded portion 117 made of polyethylene (PE), a first adjacent inner layer of the inner welded portion 117 made of chlorinated polyethylene (SPE), and an outer non-welded portion 118 made of aluminum are laminated in this order.

[0069] In addition, as the multi-layered packaging material 110, for example, a five-layered packaging material can be used in which, from the inner surface 107 side, the innermost layer of the inner welded portion 117 made of polyethylene (PE), a first adjacent inner layer of the inner welded portion 117 made of chlorinated polyethylene (SPE), a second adjacent outer layer of the outer non-welded portion 118 made of aluminum, a first adjacent outer layer of the outer non-welded portion 118 made of chlorinated polyethylene (SPE), and the outermost layer of the outer non-welded portion 118 made of polyethylene (PE) are laminated in this order.

[0070] The thickness of the packaging material 110 constituting the first packaging body 100A is, for example, 50 μm or more, preferably 100 μm or more, at the thinnest part of the first packaging body 100A. The thickness of the thinnest part is preferably 10,000 μm or less. If the thickness of the packaging material 110 is within the above range, it is preferable because it is easy to reduce the moisture permeability. It is also preferable because it increases the mechanical strength and suppresses the occurrence of pinholes and the intrusion of air when an impact is applied from the outside.

[0071] The packaging material 110 of the first packaging body 100A has a multi-layer structure as shown in Fig. 4. However, as long as the packaging material 110 has a first enclosing function, the packaging material 110 of the first packaging body 100A may have a layer structure other than the multi-layer structure shown in Fig. 4, for example, a single-layer structure as shown in Fig. 11.

[0072] When the outer non-welded portion 118 is made of a low moisture permeable material, in the first packaging body 100A consisting of a heat-sealed bag 120, the material of the packaging material 110 mainly contributes to the first sealing function and the first low moisture permeability function, and the structure of the first packaging body 100A consisting of the heat-sealed bag 120 mainly contributes to the first sealing function.

[0073] For example, when the outer non-welded portion 118 of the packaging material 110 is made of a low moisture permeable material, the first sealing function is mainly realized by welding the inner welded portion 117 of the packaging material 110 of the first packaging body 100A, and the first low moisture permeability function is also mainly realized by the outer non-welded portion 118 of the packaging material 110. In addition, the first sealing function is mainly realized by the heat-sealed portion 123 of the first packaging body 100A made of the heat-sealed bag 120.

[0074] (Second packaging) The second packaging body 200A is a structure that contains and encloses the first packaging body 100A.

[0075] In the electrolyte containment structure 1AB, a specific fill gas FG is enclosed in a second space 209 defined by the outer surface 108 of the first package 100A and the inner surface 207 of the second package 200A.

[0076] The second packaging body 200A has a function of enclosing the electrolyte encapsulated intermediate structure 7A, which is the first packaging body 100A enclosing the sulfide solid electrolyte 3. Such a function of enclosing the first packaging body 100 is hereinafter also referred to as a "second encapsulation function." Note that it is preferable that the second packaging body 200A further has a function of low moisture permeability (hereinafter also referred to as a "second low moisture permeability function"), since this makes it difficult for the ionic conductivity of the sulfide solid electrolyte 3 enclosed in the first packaging body 100A to decrease.

[0077] As shown in FIG. 2 and FIG. 3, the second package 200A is made by using a sheet-like packaging material 210 to form a heat-sealed bag 220 capable of containing and sealing the first package 100A.

[0078] As shown in Fig. 3, the heat seal bag 220 constituting the second packaging body 200A has the same structure as the heat seal bag 120 constituting the first packaging body 100A. That is, as shown in Fig. 3, the heat seal bag 220 constituting the second packaging body 200A includes a bag body 221 and a sealing portion 222 which is a strip-shaped member formed continuously with the bag body 221 and which forms an opening 227 at an end. At least a part of the sealing portion 222 of the second packaging body 200A is welded to form a heat seal portion 223, which makes it possible to contain and enclose the first packaging body 100A in the second packaging body 200A.

[0079] 3, in the second packaging body 200A, the first packaging body 100A is enclosed in a second space 209 defined by an inner surface 207, which is the surface of the second packaging body 200A that encloses the first packaging body 100A. The second packaging body 200A made of a heat-sealed bag 220 has a relatively flat shape, and therefore has high storage space efficiency.

[0080] A filler gas FG is sealed in the second space 209. The filler gas FG sealed in the second space 209 may be the same as the filler gas FG used in the filler gas FG sealed in the first space 109, such as Ar, air, or N 2 or CO 2 or the like is used. Among these, Ar is preferred because it has low reactivity with the sulfide solid electrolyte 3 even if the first packaging body 100A is damaged and the sulfide solid electrolyte 3 is exposed to the atmosphere in the second space 209. The filling gas FG sealed in the second space 209 and the filling gas FG sealed in the first space 109 may be the same or different in composition and concentration. The filling gas FG present in the second space 209 is hereinafter also referred to as second space gas 219. The composition of the second space gas 219 may change due to a reaction with the sulfide solid electrolyte 3, etc.

[0081] The filler gas FG sealed in the second space 209 has an oxygen concentration of 30% or less and a dew point temperature of −20° C. or less. If the oxygen concentration and dew point temperature of the filler gas FG are within the above ranges, this is preferable because the ionic conductivity of the sulfide solid electrolyte 3 sealed in the first packaging body 100A is less likely to decrease.

[0082] The preferred numerical range of the oxygen concentration of the filler gas FG filled in the second space 209 and the reasons therefor are similar to those for the filler gas FG filled in the first space 109.

[0083] The preferred numerical range of the dew point temperature of the filler gas FG sealed in the second space 209 and the reasons therefor are similar to those of the filler gas FG sealed in the first space 109.

[0084] The packaging material 210 constituting the second packaging body 200A has a multilayer structure in which the entire heat-sealed bag 220, including the sealing portion 222, has an inner welded portion 217 made of a weldable organic material and an outer non-welded portion 218, which is a layer made of, for example, aluminum, laminated on the outer surface of the inner welded portion 217, as shown in Figure 4.

[0085] When the packaging material 210 has such a multi-layer structure, the moisture permeability is, for example, 10 (g / m 2 ·24h) When the outer non-welded portion 218 made of a low moisture permeable material (hereinafter also referred to as "low moisture permeable material") is used, the second packaging body 200A can be given a second encapsulation function of enclosing the first packaging body 100A by welding the inner welded portion 217, and a second low moisture permeability function by the outer non-welded portion 218.

[0086] The inner welded portion 217 and the outer non-welded portion 218 of the second packaging body 200A are conceptually similar to the inner welded portion 117 and the outer non-welded portion 118 of the first packaging body 100A, and therefore a description thereof will be omitted.

[0087] The weldable organic material constituting the inner weld portion 217 is the same as the organic material used for the inner weld portion 117 of the first packaging body 100A for the same reasons. Note that the weldable organic material constituting the inner weld portion 217 and the weldable organic material constituting the inner weld portion 117 of the first packaging body 100A may have the same components or concentrations as or different from each other.

[0088] It is preferable that the outer unwelded portion 218 is made of a low moisture permeable material, since this can impart a second low moisture permeability function to the second package 200A.

[0089] The low moisture permeable material used for the outer unwelded portion 218 is the same as the low moisture permeable material used for the outer unwelded portion 118 of the first packaging body 100A for the same reason.

[0090] For this reason, it is preferable that the packaging material 210 includes an aluminum layer 218 as the outer non-welded portion 218, since this makes it easier to reduce the moisture permeability of the packaging material 210.

[0091] The thickness of the packaging material 210 constituting the second packaging body 200A, at its thinnest portion, is within the same numerical range as the thickness of the packaging material 110 constituting the first packaging body 100 for the same reasons.

[0092] The thickness of the inner welded portion 217 at the thinnest portion of the second package 200A is within the same numerical range as the thickness of the inner welded portion 117 constituting the first package 100 for the same reasons.

[0093] The thickness of the outer non-welded portion 218 at the thinnest portion of the second packaging body 200A is within the same numerical range as the thickness of the outer non-welded portion 118 constituting the first packaging body 100 for the same reasons.

[0094] The packaging material 210 of the second packaging body 200A has a multi-layer structure as shown in Fig. 4. However, as long as the packaging material 210 has the second encapsulation function and the low moisture permeability function, the packaging material 210 of the second packaging body 200A can have a layer structure other than the multi-layer structure shown in Fig. 4, for example, a single layer structure as shown in Fig. 11.

[0095] In the second packaging body 200A consisting of the heat-sealed bag 220, the material of the packaging material 210 mainly contributes to the second sealing function and the second low moisture permeability function, and the structure of the second packaging body 200A consisting of the heat-sealed bag 220 mainly contributes to the second sealing function.

[0096] For example, the second sealing function is mainly realized by welding the inner welded portion 217 of the packaging material 210 of the second packaging body 200A, and the second low moisture permeability function is mainly realized by the outer non-welded portion 218 of the packaging material 210 being made of a low moisture permeability material. Also, the second sealing function is mainly realized by the heat-sealed portion 223 of the second packaging body 200A made of the heat-sealed bag 220.

[0097] (effect) According to the electrolyte containment structure 1AB, it is possible to provide an electrolyte containment structure in which the ionic conductivity of the sulfide solid electrolyte 3 contained in the first packaging body 100A is unlikely to decrease over time.

[0098] Furthermore, according to the electrolyte containment structure 1AB, when the first package 100A made of the heat-sealed bag 120 has a relatively flat shape, it is possible to provide an electrolyte containment structure with higher storage space efficiency.

[0099] Furthermore, the electrolyte containment structure 1AB has a double-packing structure in which the first package 100A containing the sulfide solid electrolyte 3 is further packed in the second package 200A. Therefore, even if a pinhole or the like occurs in either the first package 100A or the second package 200A due to an external force during transportation, the electrolyte containment structure 1AB can block the inflow of air from the outside, that is, the inflow of air with a relatively high dew point temperature. Therefore, the electrolyte containment structure 1AB can provide an electrolyte containment structure in which the ionic conductivity of the sulfide solid electrolyte 3 is unlikely to decrease over time.

[0100] Comparative Example 1 described later is an example of a single-packaging structure (electrolyte-encapsulated intermediate structure 7A shown in FIG. 1) in which the sulfide solid electrolyte 3 is encapsulated only in the first packaging body 100A. In Comparative Example 1, the ion conductivity was reduced due to the occurrence of pinholes in the first packaging body 100A and insufficient sealing.

[0101] In contrast, since the electrolyte encapsulation structure 1AB has a double-packaged structure, even if external forces during transportation cause pinholes or insufficient sealing in one of the first packaging body 100A and the second packaging body 200A, it is possible to block the inflow of air.

[0102] The degree of decrease in ionic conductivity of the sulfide solid electrolyte 3 enclosed in the first packaging body 100A of the electrolyte containment structure 1AB can be measured, for example, by the following method: That is, the electrolyte containment structure 1AB is stored in the atmosphere at 25° C. for 7 to 90 days, and the ionic conductivity of the sulfide solid electrolyte 3 is measured and compared with the ionic conductivity of the sulfide solid electrolyte 3 at the time of enclosure.

[0103] <Modification of the first embodiment> FIG. 5 is a plan view showing an electrolyte containment structure according to a modified example of the first embodiment of the present invention, and FIG. 6 is a diagram showing the internal state of the electrolyte containment structure of FIG. 5.

[0104] As shown in Fig. 5 and Fig. 6, the electrolyte containment structure 1AC (1) according to the modified example of the first embodiment includes a first package 100A (120) that contains a sulfide solid electrolyte 3, a second package 200A (220) that contains and contains the first package 100A, and a third package 300A (320) that contains and contains the second package 200A. The electrolyte containment structure 1AC has a thickness in the direction perpendicular to the plane of Fig. 5 because it includes the electrolyte containment structure 1AB. In Fig. 6, the thicknesses of the bag bodies 121, 221, and 321 are exaggerated compared to their actual thickness.

[0105] An electrolyte containment structure 1AC according to a modified example of the first embodiment is an electrolyte containment structure 1AB according to the first embodiment, which further includes a third packaging body 300A that accommodates and encloses the second packaging body 200A.

[0106] The electrolyte containment structure 1AC according to the modified example of the first embodiment is the same as the electrolyte containment structure 1AB according to the first embodiment except that it further includes a third packaging body 300A. Therefore, the same components in the electrolyte containment structure 1AC according to the modified example of the first embodiment and the electrolyte containment structure 1AB according to the first embodiment are denoted by the same reference numerals, and the description of the components and functions is omitted or simplified. The following mainly describes the third packaging body 300A.

[0107] (Third packaging) The third package 300A is a structure that contains and encloses the second package 200A.

[0108] In the electrolyte containment structure 1AC, a specific filler gas FG is enclosed in a third space 309 defined by an outer surface 208 of the second package 200A and an inner surface 307 of the third package 300A.

[0109] The third packaging body 300A has a function of enclosing the second packaging body 200A constituting the outermost layer of the electrolyte enclosing structure 1AB. Such a function of enclosing the second packaging body 200A is hereinafter also referred to as a "third enclosing function." Note that it is preferable that the third packaging body 300A further has a function of low moisture permeability (hereinafter also referred to as a "third low moisture permeability function"), since this makes it difficult for the ionic conductivity of the sulfide solid electrolyte 3 enclosed in the first packaging body 100A to decrease.

[0110] As shown in FIG. 6 and FIG. 3, the third package 300A is made by using a sheet-like packaging material 310 to form a heat-sealed bag 320 capable of containing and sealing the second package 200A.

[0111] As shown in Fig. 3, the heat-sealed bag 320 constituting the third packaging body 300A has the same structure as the heat-sealed bag 120 constituting the first packaging body 100A. That is, as shown in Fig. 3, the heat-sealed bag 320 constituting the third packaging body 300A includes a bag body 321 and a sealing portion 322 which is a strip-shaped member formed continuously with the bag body 321 and which forms an opening 327 at an end. At least a part of the sealing portion 322 of the third packaging body 300A is welded to form a heat-sealed portion 323, which makes it possible to accommodate and enclose the second packaging body 200A in the third packaging body 300A.

[0112] 3, in the third packaging body 300A, the second packaging body 200A is enclosed in a third space 309 defined by an inner surface 307, which is the surface of the third packaging body 300A that encloses the second packaging body 200A. When the third packaging body 300A made of the heat seal bag 320 has a relatively flat shape, it is possible to further increase the efficiency of the storage space.

[0113] A filler gas FG is sealed in the third space 309. The filler gas FG sealed in the third space 309 may be the same as the filler gas FG used in the filler gas FG sealed in the first space 109, such as Ar, air, or N 2 or CO 2or the like is used. Among these, Ar is preferred because it has low reactivity with the sulfide solid electrolyte 3 even if the sulfide solid electrolyte 3 is exposed to the atmosphere in the third space 309 due to damage to the first packaging body 100A and the second packaging body 200A. The filling gas FG sealed in the third space 309 and the filling gas FG sealed in the first space 109 may be the same or different in composition and concentration. The filling gas FG present in the third space 309 is hereinafter also referred to as third space gas 319. The composition of the third space gas 319 may change due to a reaction with the sulfide solid electrolyte 3, etc.

[0114] The filling gas FG sealed in the third space 309 has an oxygen concentration of 30% or less and a dew point temperature of −20° C. or less. If the oxygen concentration and dew point temperature of the filling gas FG are within the above ranges, this is preferable because the ionic conductivity of the sulfide solid electrolyte 3 sealed in the first packaging body 100A is less likely to decrease.

[0115] The preferred numerical range of the oxygen concentration of the filler gas FG filled in the third space 309 and the reasons therefor are similar to those of the filler gas FG filled in the first space 109.

[0116] The preferred numerical range of the dew point temperature of the filler gas FG filled in the third space 309 and the reasons therefor are similar to those of the filler gas FG filled in the first space 109.

[0117] The packaging material 310 constituting the third packaging body 300A has a multilayer structure in which the entire heat-sealed bag 320, including the sealing portion 322, has an inner welded portion 317 made of a weldable organic material and an outer non-welded portion 318, which is a layer made of aluminum and is laminated on the outer surface of the inner welded portion 317, as shown in Figure 4.

[0118] When the packaging material 310 has such a multi-layer structure, the moisture permeability is, for example, 10 (g / m 2·24h) When using the outer non-welded portion 318 made of a low-temperature material (low-moisture permeability material) as described below, the third packaging body 300A can be given a third sealing function of enclosing the second packaging body 200A by welding the inner welded portion 317, and a third low-moisture permeability function by the outer non-welded portion 318.

[0119] The inner welded portion 317 and the outer non-welded portion 318 of the third packaging body 300A are conceptually similar to the inner welded portion 117 and the outer non-welded portion 118 of the first packaging body 100A, and therefore a description thereof will be omitted.

[0120] The weldable organic material constituting the inner weld portion 317 is the same as the organic material used for the inner weld portion 117 of the first packaging body 100A for the same reasons. Note that the weldable organic material constituting the inner weld portion 317 and the weldable organic material constituting the inner weld portion 117 of the first packaging body 100A may have the same components or concentrations as or different from each other.

[0121] It is preferable that the outer unwelded portion 318 is made of a low moisture permeable material, since this can impart a third low moisture permeability function to the third package 300A.

[0122] The low moisture permeable material used for the outer unwelded portion 318 is the same as the low moisture permeable material used for the outer unwelded portion 118 of the first package 100A for the same reason.

[0123] For this reason, it is preferable that the packaging material 310 includes an aluminum layer 318 as the outer non-welded portion 318, since this makes it easier to reduce the moisture permeability of the packaging material 310.

[0124] It is preferable that the thickness of the packaging material 310 constituting the third packaging body 300A, at the thinnest part of the third packaging body 300A, is within the same numerical range as the thickness of the packaging material 110 constituting the first packaging body 100, for the same reasons.

[0125] It is preferable that the thickness of the inner welded portion 317 at the thinnest portion of the third package 300A be within the same numerical range as the thickness of the inner welded portion 117 constituting the first package 100 for the same reasons.

[0126] It is preferable that the thickness of the outer non-welded portion 318 at the thinnest portion of the third packaging body 300A be within the same numerical range as the thickness of the outer non-welded portion 118 constituting the first packaging body 100 for the same reasons.

[0127] The packaging material 310 of the third packaging body 300A has a multi-layer structure as shown in Fig. 4. However, as long as the packaging material 310 has the third enclosing function, the packaging material 310 of the third packaging body 300A may have a layer structure other than the multi-layer structure shown in Fig. 4, for example, a single layer structure as shown in Fig. 11.

[0128] In the third packaging body 300A consisting of the heat-sealed bag 320, the material of the packaging material 310 mainly contributes to the third sealing function and the third low moisture permeability function, and the structure of the third packaging body 300A consisting of the heat-sealed bag 320 mainly contributes to the third sealing function.

[0129] For example, the third sealing function is mainly realized by welding the inner welded part 317 of the packaging material 310 of the third packaging body 300A, and the third low moisture permeability function is mainly realized by the outer non-welded part 318 of the packaging material 310 being made of a low moisture permeability material. Also, the third sealing function is mainly realized by the heat-sealed part 323 of the third packaging body 300A made of the heat-sealed bag 320.

[0130] (effect) According to the electrolyte containment structure 1AC, it is possible to provide an electrolyte containment structure in which the ionic conductivity of the sulfide solid electrolyte 3 contained in the first packaging body 100A is unlikely to decrease over time.

[0131] Furthermore, according to the electrolyte containment structure 1AC, when the first package 100A made of the heat-sealed bag 120 has a relatively flat shape, it is possible to provide an electrolyte containment structure with higher storage space efficiency.

[0132] The degree of decrease in ionic conductivity of the sulfide solid electrolyte 3 enclosed in the first packaging body 100A of the electrolyte containment structure 1AC can be confirmed in a manner similar to that used to measure the degree of decrease in ionic conductivity of the sulfide solid electrolyte 3 in the electrolyte containment structure 1AB of the first embodiment.

[0133] <Second embodiment> Figure 7 is an oblique view showing an electrolyte containment structure according to a second embodiment of the present invention, Figure 8 is a diagram showing the internal state of the electrolyte containment structure of Figure 7, Figure 9 is an oblique view of a packaging body constituting the electrolyte containment structure of Figures 7 and 12, shown with the opening closed, Figure 10 is an exploded oblique view of the packaging body constituting the electrolyte containment structure of Figure 7, and Figure 11 is a cross-sectional view of the packaging material constituting the packaging body of Figure 9.

[0134] As shown in Fig. 7 and Fig. 8, the electrolyte containment structure 1BB (1) according to the second embodiment includes a first package 100B (130) that contains a sulfide solid electrolyte 3, and a second package 200A (220) that contains and contains the first package 100B. The first package 100B is made of a bottle 130 with a lid, and is usually contained and contained in the second package 200A of the electrolyte containment structure 1BB, with a thickness equal to the diameter of the bottle. Therefore, the bag body 221 of the second package 200A that contains and contains the first package 100B and the electrolyte containment structure 1BB have a thickness in the direction perpendicular to the plane of Fig. 7.

[0135] The first packaging body 100B containing the sulfide solid electrolyte 3 corresponds to a structure obtained by removing the second packaging body 200A from the electrolyte containment structure 1BB, in other words, it is an intermediate body of the electrolyte containment structure. The structure made of the first packaging body 100B containing the sulfide solid electrolyte 3 is hereinafter also referred to as the electrolyte containment intermediate structure 7B (7). The electrolyte containment intermediate structure 7B has the sulfide solid electrolyte 3 and the first packaging body 100B (130) containing the sulfide solid electrolyte 3.

[0136] 9 and 10, the first packaging body 100B is a lidded bottle 130 capable of sealing the sulfide solid electrolyte 3 in the first packaging body 100B by screwing together a male threaded portion, which is a first connecting portion 133 provided on the outer surface of a bottle body 131, and a female threaded portion, which is a second connecting portion 134 provided on the inner surface of a screw cap 132. The first packaging body 100B is a lidded bottle 130 equipped with a screw cap 132.

[0137] The electrolyte containment structure 1BB according to the second embodiment is the same as the electrolyte containment structure 1AB according to the first embodiment, except that the first packaging body 100A is replaced with a first packaging body 100B. For this reason, the same components in the electrolyte containment structure 1BB according to the second embodiment and the electrolyte containment structure 1AB according to the first embodiment are denoted by the same reference numerals, and the explanation of the components and functions will be omitted or simplified.

[0138] (Sulfide solid electrolyte) As the sulfide solid electrolyte 3, the same sulfide solid electrolyte 3 as that used in the electrolyte containment structure 1AB according to the first embodiment can be used.

[0139] The first package 100B consisting of the covered bottle 130 of the electrolyte containment structure 1BB according to the second embodiment is generally less susceptible to deformation due to external forces than the first package 100A consisting of the heat-sealed bag 120 of the electrolyte containment structure 1AB according to the first embodiment. Therefore, in the electrolyte containment structure 1BB according to the second embodiment, the sulfide solid electrolyte 3 is generally less susceptible to deformation due to external forces and the associated deterioration of the sulfide solid electrolyte 3 compared to the electrolyte containment structure 1AB according to the first embodiment.

[0140] Therefore, in the electrolyte containment structure 1BB of the second embodiment, the ionic conductivity of the sulfide solid electrolyte 3 is less likely to decrease over time compared to the electrolyte containment structure 1AB of the first embodiment, and the electrolyte containment structure 1BB of the second embodiment can be effectively used to contain the sulfide solid electrolyte 3, which is easily deformed by external forces.

[0141] (First package) In the electrolyte containment structure 1BB, a specific filling gas FG is sealed within a first space 109 defined by an inner surface 107, which is the surface of the first packaging body 100B that contains the sulfide solid electrolyte 3.

[0142] The first packaging body 100B has an encapsulating function (first encapsulating function) of encapsulating the sulfide solid electrolyte 3. If the first packaging body 100B further has a first low moisture permeability function, it is preferable because the ionic conductivity of the sulfide solid electrolyte 3 encapsulated in the first packaging body 100B is less likely to decrease.

[0143] As shown in FIGS. 7 to 10, the first packaging body 100B is formed by using a packaging material 110 into a bottle 130 with a lid in which the sulfide solid electrolyte 3 can be enclosed.

[0144] 9 and 10, the lidded bottle 130 constituting the first packaging body 100B includes a bottle body 131 having a first connecting portion (male thread portion) 133, and a screw cap 132 having a second connecting portion (female thread portion) 134. The lidded bottle 130 is configured to be capable of sealing the sulfide solid electrolyte 3 in the first packaging body 100B by screwing the bottle body 131 and the screw cap 132 together.

[0145] 8, in first packaging body 100B, the sulfide solid electrolyte 3 is enclosed in first space 109 defined by inner surface 107, which is the surface of first packaging body 100B that encloses sulfide solid electrolyte 3. First packaging body 100B made of lidded bottle 130 generally has high mechanical strength and is not easily deformed due to its shape, so damage to the particles of the enclosed sulfide solid electrolyte 3 is strongly suppressed.

[0146] A fill gas FG is sealed in the first space 109. The fill gas FG may be Ar, air, N 2 or CO 2 Among these, Ar is preferable because it has low reactivity with the sulfide solid electrolyte 3.

[0147] The filler gas FG sealed in the first space 109 has an oxygen concentration of 30% or less and a dew point temperature of -20° C. or less. If the oxygen concentration and dew point temperature of the filler gas FG are within the above ranges, this is preferable because the ionic conductivity of the sulfide solid electrolyte 3 sealed in the first packaging body 100B is less likely to decrease.

[0148] The oxygen concentration of the filler gas FG sealed in the first space 109 is preferably 10% or less, more preferably 5% or less, and further preferably 1% or less. The oxygen concentration of the filler gas FG within the latter range is preferable because the ionic conductivity of the sulfide solid electrolyte 3 sealed in the first packaging body 100B is less likely to decrease.

[0149] The dew point temperature of the filling gas FG sealed in the first space 109 is preferably −30° C. or less, more preferably −40° C. or less, and even more preferably −50° C. or less. The closer the dew point temperature of the filling gas FG is to the latter range, the more the reaction between the sulfide solid electrolyte 3 sealed in the first packaging body 100B and moisture is suppressed, and the less the ion conductivity is reduced, which is preferable.

[0150] In the first packaging body 100B in which the sulfide solid electrolyte 3 is sealed, the volume V of the first space 109 is 1 (cm 3 ) the volume V of the sulfide solid electrolyte 3 itself SE (cm 3 ) ratio (V SE / V 1 The first filling rate (10%) is, for example, more than 0%, preferably 10% or more, and more preferably 20% or more. The filling rate is, for example, 50% or less, preferably 40% or less, and more preferably 30% or less. When the first filling rate is more than 0%, the storage space efficiency is effectively improved. When the first filling rate is 50% or less, aggregation and changes in particle shape caused by the particles of the sulfide solid electrolyte 3 being crushed can be effectively suppressed.

[0151] The packaging material 110 constituting the first packaging body 100B is made of a material and has a structure capable of sealing a specific filling gas FG within a first space 109 partitioned by an inner surface 107, which is the surface on the side that seals the sulfide solid electrolyte 3.

[0152] As shown in Fig. 11, the packaging material 110 constituting the first package 100B is a single-layer structure in which the entire capped bottle 130, including the bottle body 131 and the screw cap 132, is made of a single layer 116. Note that the bottle body 131 and the screw cap 132 constituting the capped bottle 130 have different shapes depending on the location, but have one thing in common in that the packaging material 110 is made of a single layer 116.

[0153] The packaging material 110 consisting of a single layer 116 constituting the first packaging body 100B is preferably made of a material having low moisture permeability.

[0154] When the single layer 116 is made of a low moisture permeable material, it is possible to impart a low moisture permeability function to the first packaging body 100B.

[0155] The low moisture permeable material used in the single layer 116 is the same as the low moisture permeable material used in the outer non-welded portion 118 of the first packaging body 100A of the electrolyte encapsulation structure 1AB according to the first embodiment. Specifically, the low moisture permeable material used in the single layer 116 is, for example, metals such as aluminum, stainless steel, and iron; and organic substances such as one or more organic resins selected from polyethylene terephthalate (PET), polyethylene (PE), chlorinated polyethylene (SPE), high density polyethylene, nylon, and polyvinyl alcohol. Among these, it is preferable that the first packaging body 100B is made of aluminum, since this makes it easier to reduce the moisture permeability of the packaging material 110 constituting the first packaging body 100B.

[0156] When the low moisture permeable material used in the single layer 116 of the first package 100B is aluminum, the first package 100B becomes a lidded bottle 130 made of aluminum. When the low moisture permeable material used in the single layer 116 of the first package 100B is high density polyethylene, the first package 100B becomes a lidded bottle 130 made of high density polyethylene.

[0157] The thickness of the packaging material 110 constituting the first packaging body 100B is, for example, 50 μm or more, preferably 100 μm or more, at the thinnest part of the first packaging body 100B. The thickness of the thinnest part is preferably 10,000 μm or less. If the thickness of the packaging material 110 is within the above range, it is preferable because the moisture permeability is easily reduced.

[0158] When the first packaging body 100B is a lidded bottle 130 made of aluminum, the thickness of the packaging material 110 constituting the first packaging body 100B is, for example, 50 μm or more, preferably 100 μm or more, at the thinnest part of the first packaging body 100B. The thickness of the thinnest part is preferably 10,000 μm or less. If the thickness of the packaging material 110 is within the above range, it is preferable because the moisture permeability is easily reduced.

[0159] When the first package 100B is a lidded bottle 130 made of high density polyethylene, the thickness of the packaging material 110 constituting the first package 100B is, for example, 50 μm or more, preferably 100 μm or more, at the thinnest part of the first package 100B. The thickness of the thinnest part is preferably 10,000 μm or less. If the thickness of the packaging material 110 is within the above range, it is preferable because it is easy to reduce the moisture permeability.

[0160] When the single layer 116 is made of a low moisture permeable material, in the first packaging body 100B consisting of a capped bottle 130, the material of the packaging material 110 mainly contributes to the low moisture permeability function, and the structure of the first packaging body 100B consisting of the capped bottle 130 mainly contributes to the sealing function.

[0161] For example, when the single layer 116 of the packaging material 110 of the first packaging body 100B is made of a low moisture permeable material, the low moisture permeability function is also mainly exhibited. Also, the sealing function is mainly exhibited by the screwing of the bottle body 131 and the screw cap 132 of the first packaging body 100B made of the lidded bottle 130.

[0162] (Second packaging) The second packaging body 200A is a structure that contains and encloses the first packaging body 100B.

[0163] The second packaging body 200A of the electrolyte containment structure 1BB has the same structure and material as the second packaging body 200A of the electrolyte containment structure 1AB according to the first embodiment, except for the size.

[0164] A filler gas FG is sealed in the second space 209. The filler gas FG sealed in the second space 209 may be the same as the filler gas FG used in the filler gas FG sealed in the first space 109, such as Ar, air, or N 2 or CO 2 Among these, Ar is preferred because it has low reactivity with the sulfide solid electrolyte 3 even if the first packaging body 100B is broken and opened, exposing the sulfide solid electrolyte 3 to the atmosphere in the second space 209. The filling gas FG sealed in the second space 209 and the filling gas FG sealed in the first space 109 may be the same or different in composition and concentration.

[0165] The filler gas FG sealed in the second space 209 has an oxygen concentration of 30% or less and a dew point temperature of −20° C. or less. If the oxygen concentration and dew point temperature of the filler gas FG are within the above ranges, this is preferable because the ionic conductivity of the sulfide solid electrolyte 3 sealed in the first packaging body 100B is less likely to decrease.

[0166] The preferred numerical range of the oxygen concentration of the filler gas FG filled in the second space 209 and the reasons therefor are similar to those for the filler gas FG filled in the first space 109.

[0167] The preferred numerical range of the dew point temperature of the filler gas FG sealed in the second space 209 and the reasons therefor are similar to those of the filler gas FG sealed in the first space 109.

[0168] The second packaging body 200A of the electrolyte containment structure 1BB is similar to the second packaging body 200A of the electrolyte containment structure 1AB according to the first embodiment except for the above-mentioned structure and characteristics, and therefore a description thereof will be omitted.

[0169] (effect) According to the electrolyte containment structure 1BB, it is possible to provide an electrolyte containment structure in which the ionic conductivity of the sulfide solid electrolyte 3 contained in the first packaging body 100B is unlikely to decrease.

[0170] Furthermore, according to the electrolyte containment structure 1BB, the first packaging body 100B consisting of the lidded bottle 130 generally has high mechanical strength and is not easily deformed due to its shape, so that damage to the particles of the enclosed sulfide solid electrolyte 3 is strongly suppressed.

[0171] The degree of decrease in ionic conductivity of the sulfide solid electrolyte 3 enclosed in the first packaging body 100B of the electrolyte containment structure 1BB can be measured, for example, by the following method: That is, the electrolyte containment structure 1BB is stored in the atmosphere at 25° C. for 7 to 90 days, and the ionic conductivity of the sulfide solid electrolyte 3 is measured and compared with the ionic conductivity of the sulfide solid electrolyte 3 at the time of enclosure.

[0172] <Modification of the second embodiment> FIG. 12 is a plan view showing an electrolyte containment structure according to a modified example of the second embodiment of the present invention, and FIG. 13 is a diagram showing the internal state of the electrolyte containment structure of FIG. 12 so as to be clearly understood.

[0173] 12 and 13, an electrolyte containment structure 1BC(1) according to a modification of the second embodiment includes a first package 100B(130) that contains a sulfide solid electrolyte 3, a second package 200A(220) that contains and contains the first package 100B, and a third package 300A(320) that contains and contains the second package 200A. The electrolyte containment structure 1BC includes an electrolyte containment structure 1BB, and therefore has a thickness in the direction perpendicular to the plane of FIG.

[0174] An electrolyte containment structure 1BC according to a modified example of the second embodiment is an electrolyte containment structure 1BB according to the second embodiment further including a third package 300A that accommodates and encloses the second package 200A.

[0175] The electrolyte containment structure 1BC according to the modified example of the second embodiment is the same as the electrolyte containment structure 1BB according to the second embodiment except that it further includes a third packaging body 300 A. For this reason, the same components in the electrolyte containment structure 1BC according to the modified example of the second embodiment and the electrolyte containment structure 1BB according to the second embodiment are denoted by the same reference numerals, and the description of the components and functions will be omitted or simplified.

[0176] (Third packaging) The third packaging body 300A is a structure that contains and encloses the second packaging body 200A. The third packaging body 300A constituting the electrolyte containment structure 1BC according to the modified example of the second embodiment is similar to the third packaging body 300A constituting the electrolyte containment structure 1AC according to the modified example of the first embodiment. Therefore, the description of the configuration and function of the third packaging body 300A will be omitted.

[0177] (effect) According to the electrolyte containment structure 1BC, it is possible to provide an electrolyte containment structure in which the ionic conductivity of the sulfide solid electrolyte 3 contained in the first packaging body 100B is unlikely to decrease.

[0178] In addition, according to the electrolyte containment structure 1BC, the first packaging body 100B consisting of the lidded bottle 130 generally has high mechanical strength and is not easily deformed due to its shape, so damage to the particles of the enclosed sulfide solid electrolyte 3 is strongly suppressed.

[0179] The degree of decrease in ionic conductivity of the sulfide solid electrolyte 3 enclosed in the first packaging body 100B of the electrolyte containment structure 1BC can be confirmed in a manner similar to that used to measure the degree of decrease in ionic conductivity of the sulfide solid electrolyte 3 in the electrolyte containment structure 1BB of the second embodiment.

[0180] In the above-mentioned electrolyte containment structures 1AB, 1AC, 1BB, and 1BC, examples have been shown in which the heat-sealed bag 120 (220, 320) and the lidded bottle 130 are used as the first package 130, the second package 220, and the third package 320. However, the shape and structure of each package of the electrolyte containment structure 1 according to the present invention are not particularly limited as long as they can contain the contents. As each package of the electrolyte containment structure 1 according to the present invention, in addition to the heat-sealed bag and the lidded bottle, for example, a container or the like can be used.

[0181] Moreover, the above-mentioned electrolyte containment structures 1AB, 1AC, 1BB, and 1BC have been shown as examples including the first package 130, the second package 220, and the third package 320. However, the electrolyte containment structure 1 according to the present invention may include further packages, such as a fourth package that encloses the third package (not shown).

[0182] <Conventional example> FIG. 14 is a plan view showing a conventional electrolyte containment structure, FIG. 15 is a diagram showing the internal state of the electrolyte containment structure of FIG. 14, and FIG. 16 is an oblique view of the packaging body that constitutes the electrolyte containment structure of FIG. 14, with the opening open.

[0183] 14 and 15, an electrolyte containment structure 5C (5) according to a conventional example includes a sulfide solid electrolyte 3 and a package 100C (140) that encloses the sulfide solid electrolyte 3. The package 100C is made of a chuck-sealed bag 140. Note that in FIG. 15, the thickness of the bag body 141 is exaggerated compared to the actual thickness.

[0184] 16, the package 100C is a chuck seal bag 140 that has a removable chuck portion 143 and an opening 147 that can be opened and closed to seal the sulfide solid electrolyte 3 inside the package 100C. Here, the chuck seal bag 140 refers to a bag that has a mechanism that allows the opening 147 of the chuck seal bag 140 to be opened and closed by the removable chuck portion 143.

[0185] The electrolyte containment structure 5C according to the conventional example is the same as the electrolyte containment structure 1AB according to the first embodiment, except that the first packaging body 100A is replaced with the packaging body 100C and the enclosed gas is changed. For this reason, the same components in the electrolyte containment structure 5C according to the conventional example and the electrolyte containment structure 1AB according to the first embodiment are denoted by the same reference numerals, and the explanation of the components and functions will be omitted or simplified.

[0186] (Sulfide solid electrolyte) As the sulfide solid electrolyte 3, the same sulfide solid electrolyte 3 as that used in the electrolyte containment structure 1AB according to the first embodiment can be used.

[0187] (Packaging) The package 100C made of the chuck seal bag 140 is a structure that encloses the sulfide solid electrolyte 3. However, the package 100C made of the chuck seal bag 140 is likely to have insufficient sealing function for enclosing the sulfide solid electrolyte 3 due to the structure of the chuck portion 143.

[0188] For example, the packaging material 110 constituting the package 100C made of the zipper seal bag 140 generally does not have sufficient airtightness at the zipper portion 143, and the sealing function is likely to be insufficient. EXAMPLES

[0189] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0190] [Example 1] The electrolyte containment structure 1BC shown in Fig. 12 was produced as follows. The conditions for producing the electrolyte containment structure 1BC are shown in Table 1.

[0191] (Sulfide solid electrolyte) As the sulfide solid electrolyte 3, a sulfide solid electrolyte having an argyrodite-type crystal structure containing Li, P, S, Cl, and Br (D 50 The sulfide solid electrolyte had an ionic conductivity of 3.8 (mS / cm).

[0192] (First package) As the raw material for the first package 100B, a capped bottle 130 shown in Figures 9 and 10 was prepared. The packaging material 110 for the capped bottle 130 was a single layer 116 made of high density polyethylene.

[0193] (Second packaging) As the raw material of the second package 200A, a heat-sealed bag 220 shown in Fig. 3 was prepared. The packaging material 210 of the heat-sealed bag 220 has a multi-layer structure in which an inner welded portion 217 made of chlorinated polyethylene (SPE) and polyethylene (PE) and an outer non-welded portion 218 made of aluminum (Al), chlorinated polyethylene (SPE), and polyethylene (PE) are laminated, and the minimum thickness of the entire packaging material 210 of the second package 200A was 110 μm. The inner welded portion 217 had an innermost layer made of polyethylene (PE) including the inner surface 207, and a first adjacent inner layer made of chlorinated polyethylene (SPE) laminated on the outer non-welded portion 218 side as viewed from the innermost layer. The outer non-welded portion 218 comprised an outermost layer made of polyethylene (PE) including the outer surface 208, a first adjacent outer layer made of chlorinated polyethylene (SPE) laminated on the inner welded portion 217 side as viewed from the outermost layer, and a second adjacent outer layer made of aluminum laminated on the inner welded portion 217 side as viewed from the first adjacent outer layer. Packaging material 210 had a PE layer, an SPE layer, an Al layer, an SPE layer, and a PE layer laminated in this order from inner surface 207 to outer surface 208.

[0194] (Third packaging) As the raw material of the third packaging body 300A, a heat-sealed bag 320 shown in Fig. 3 was prepared. The packaging material 310 of the heat-sealed bag 320 has a multi-layer structure in which an inner welded part 317 made of chlorinated polyethylene (SPE) and polyethylene (PE) and an outer non-welded part 318 made of aluminum (Al), chlorinated polyethylene (SPE), and polyethylene (PE) are laminated, and the minimum thickness of the entire packaging material 310 of the third packaging body 300A was 110 μm. The inner welded portion 317 had an innermost layer made of polyethylene (PE) including the inner surface 307, and a first adjacent inner layer made of chlorinated polyethylene (SPE) laminated on the outer non-welded portion 318 side as viewed from the innermost layer. The outer non-welded portion 318 had an outermost layer made of polyethylene (PE) and including the outer surface 308, a first adjacent outer layer made of chlorinated polyethylene (SPE) and laminated on the inner welded portion 317 side as viewed from the outermost layer, and a second adjacent outer layer made of aluminum (Al) and laminated on the inner welded portion 317 side as viewed from the first adjacent outer layer. Packaging material 310 had a PE layer, an SPE layer, an Al layer, an SPE layer, and a PE layer laminated in this order from inner surface 307 to outer surface 308.

[0195] (packing) 9 and 10 were heated and dried at 80° C. for 10 hours, and then allowed to cool to 25° C. Thereafter, at room temperature in an Ar gas atmosphere, the sulfide solid electrolyte 3 was charged into the bottle body 131 through the opening 137, and the screw cap 132 was screwed onto the bottle body 131, thereby sealing the sulfide solid electrolyte 3 in the first package 100B.

[0196] 3 was heated at 80° C. for 10 hours to dry, and then allowed to cool to 25° C. Thereafter, at room temperature and in an Ar gas atmosphere, the first packaging body 100B containing the sulfide solid electrolyte 3 was inserted into the heat-sealed bag 220 through the opening 227, and a part of the sealing portion 222 was welded to form a heat-sealed portion 223, thereby sealing the first packaging body 100B in the second packaging body 200A.

[0197] 3 was heated at 80° C. for 10 hours, dried, and then cooled to 25° C. Thereafter, at room temperature and in an Ar gas atmosphere, the second packaging body 200A enclosing the first packaging body 100B was inserted into the heat-sealed bag 320 through the opening 327, and a part of the sealing portion 322 was welded to form a heat-sealed portion 323, thereby enclosing the second packaging body 200A in the third packaging body 300A. In this way, the electrolyte encapsulation structure 1BC shown in FIG. 12 was produced.

[0198] (evaluation) <Storage test in air> The electrolyte encapsulation structure 1BC was stored in the atmosphere at 25° C. for 90 days. After storage for 90 days, the electrolyte enclosure structure 1BC was opened to remove the sulfide solid electrolyte 3, and the ionic conductivity of the removed sulfide solid electrolyte 3 was measured. The results are shown in Table 1.

[0199] [Table 1]

[0200] [Example 2] The electrolyte containment structure 1AB shown in FIG.

[0201] (Sulfide solid electrolyte) As the sulfide solid electrolyte 3, a sulfide solid electrolyte having the same argyrodite-type crystal structure as in Example 1 was prepared.

[0202] (First package) As the raw material of the first packaging body 100A, a heat-sealed bag 120 shown in Fig. 3 was prepared. The packaging material 110 of the heat-sealed bag 120 had a multi-layer structure in which an inner welded portion 117 made of chlorinated polyethylene (SPE) and polyethylene (PE) and an outer non-welded portion 118 made of aluminum (Al), chlorinated polyethylene (SPE), and polyethylene (PE) were laminated, and the minimum thickness of the entire packaging material 110 of the first packaging body 100A was 110 μm. The inner welded portion 117 had an innermost layer made of polyethylene (PE) including the inner surface 107, and a first adjacent inner layer made of chlorinated polyethylene (SPE) laminated on the outer non-welded portion 118 side when viewed from the innermost layer. The outer non-welded portion 118 had an outermost layer made of polyethylene (PE) and including the outer surface 108, a first adjacent outer layer made of chlorinated polyethylene (SPE) and laminated on the inner welded portion 117 side when viewed from the outermost layer, and a second adjacent outer layer made of aluminum (Al) and laminated on the inner welded portion 117 side when viewed from the first adjacent outer layer. Packaging material 110 had a PE layer, an SPE layer, an Al layer, an SPE layer, and a PE layer laminated in this order from inner surface 107 to outer surface .

[0203] (Second packaging) As the raw material of the second package 200A, the same heat seal bag 220 as in Example 1 was prepared. The minimum thickness of the entire package material 210 of the second package 200A was 110 μm.

[0204] (packing) 3 was heated and dried at 80° C. for 10 hours, and then allowed to cool to 25° C. Thereafter, at room temperature and in an Ar gas atmosphere, the sulfide solid electrolyte 3 was placed in the heat-sealed bag 120 through the opening 127, and a part of the sealed portion 122 was welded to form the heat-sealed portion 123, thereby sealing the sulfide solid electrolyte 3 in the first package 100A.

[0205] Next, the heat-sealed bag 220 shown in Fig. 3 was heated at 80°C for 10 hours, dried, and then allowed to cool to 25°C. Thereafter, at room temperature and in an Ar gas atmosphere, the first package 100B was inserted into the heat-sealed bag 220 through the opening 227, and a part of the sealing portion 222 was welded to form a heat-sealed portion 223, thereby sealing the first package 100B in the second package 200A. In this way, the electrolyte encapsulation structure 1AB shown in Fig. 1 was produced.

[0206] (evaluation) <Storage test in air> The electrolyte encapsulation structure 1AB was stored in air at 25° C. for 90 days. After storage for 90 days, the electrolyte encapsulation structure 1AB was opened to remove the sulfide solid electrolyte 3, and the ionic conductivity of the removed sulfide solid electrolyte 3 was measured. The results are shown in Table 1.

[0207] [Example 3] 12 was produced in the same manner as in Example 1. Table 1 shows the conditions for producing the electrolyte containment structure 1BC.

[0208] (evaluation) <Storage test in air> The ionic conductivity of the sulfide solid electrolyte 3 was measured in the same manner as in Example 1, except that the storage period of the electrolyte containment structure 1BC was changed from 90 days to 7 days. The results are shown in Table 1.

[0209] [Example 4] An electrolyte containment structure 1BC shown in Fig. 12 was produced in the same manner as in Example 3, except that the atmosphere during packaging was changed from Ar gas to air. The conditions for the electrolyte containment structure 1BC are shown in Table 1. The specific packaging procedure is as follows.

[0210] (packing) 9 and 10 were heated and dried at 80° C. for 10 hours, and then allowed to cool to 25° C. Thereafter, the sulfide solid electrolyte 3 was charged into the bottle body 131 through the opening 137 at room temperature in the atmosphere, and the screw cap 132 was screwed onto the bottle body 131 to enclose the sulfide solid electrolyte 3 in the first package 100B.

[0211] Next, the heat-sealed bag 220 shown in Fig. 3 was heated at 80°C for 10 hours and dried, and then allowed to cool to 25°C. Thereafter, the first package 100B was inserted into the heat-sealed bag 220 through the opening 227 at room temperature in the air, and a part of the sealing portion 222 was welded to form a heat-sealed portion 223, thereby sealing the first package 100B in the second package 200A. In this way, the electrolyte encapsulation structure 1BC shown in Fig. 12 was produced.

[0212] (evaluation) <Storage test in air> The ionic conductivity of the sulfide solid electrolyte 3 was measured in the same manner as in Example 1, except that the storage period of the electrolyte containment structure 1BC was changed from 90 days to 7 days. The results are shown in Table 1.

[0213] [Example 5] 1 was produced in the same manner as in Example 2. The conditions for producing the electrolyte inclusion structure 1AB are shown in Table 1.

[0214] (evaluation) <Storage test in air> The electrolyte encapsulation structure 1AB was stored in air at 25° C. for 7 days. After storage for 7 days, the electrolyte encapsulation structure 1AB was opened to take out the sulfide solid electrolyte 3, and the ionic conductivity of the taken out sulfide solid electrolyte 3 was measured. The results are shown in Table 1.

[0215] [Comparative Example 1] The electrolyte encapsulated intermediate structure 7A shown in Fig. 1 was produced as follows. The conditions of the electrolyte encapsulated intermediate structure 7A are shown in Table 1. The electrolyte encapsulated intermediate structure 7A corresponds to a structure obtained by removing the second packaging body 200A from the electrolyte encapsulated structure 1AB of Example 2 and changing the filled gas.

[0216] (Sulfide solid electrolyte) As the sulfide solid electrolyte 3, the same sulfide solid electrolyte as in Example 1 was prepared.

[0217] (First package) As the raw material of the first package 100A, the same heat seal bag 120 as in Example 2 was prepared. The minimum thickness of the entire package material 110 of the first package 100A was 110 μm.

[0218] (packing) The heat-sealed bag 120 shown in Fig. 3 was heated and dried at 80°C for 10 hours, and then allowed to cool to 25°C. Thereafter, at room temperature in the air, the sulfide solid electrolyte 3 was placed in the heat-sealed bag 120 through the opening 127, and a part of the sealed portion 122 was welded to form a heat-sealed portion 123, thereby sealing the sulfide solid electrolyte 3 in the first package 100A. In this way, the electrolyte-encapsulated intermediate structure 7A shown in Fig. 1 was produced.

[0219] (evaluation) <Storage test in air> The electrolyte-encapsulated intermediate structure 7A was stored in the atmosphere at 25° C. for 7 days. After storage for 7 days, the electrolyte-encapsulated intermediate structure 7A was opened to take out the sulfide solid electrolyte 3, and the ionic conductivity of the taken-out sulfide solid electrolyte 3 was measured. The results are shown in Table 1.

[0220] [Comparative Example 2] 14 was produced as follows. The conditions for producing the electrolyte containment structure 5C are shown in Table 1.

[0221] (Sulfide solid electrolyte) As the sulfide solid electrolyte 3, the same sulfide solid electrolyte as in Example 1 was prepared.

[0222] (First package) As the raw material of the first package 100C, a zip-seal bag 140 shown in Fig. 16 was prepared. The packaging material 110 of the zip-seal bag 140 was a single layer 116 made of polypropylene (PE). The minimum thickness of the packaging material 110 of the package 100C was 40 µm.

[0223] (packing) At room temperature in an Ar gas atmosphere, the sulfide solid electrolyte 3 was charged into the chuck seal bag 140 from the opening 147, and the chuck portion 143 was closed to seal the sulfide solid electrolyte 3 in the package 100C. In this way, the electrolyte containment structure 5C shown in FIG. 14 was produced.

[0224] (evaluation) <Storage test in air> The electrolyte encapsulation structure 5C was stored in the atmosphere at 25° C. for 7 days. After storage for 7 days, electrolyte containment structure 5C was opened to remove sulfide solid electrolyte 3, and the ionic conductivity of the removed sulfide solid electrolyte 3 was measured. The results are shown in Table 1.

[0225] From the examples and comparative examples, it was found that when a filling gas (FG) having an oxygen concentration of 30% or less and a dew point temperature of -20°C or less is filled in both the first space 109 and the second space 209 of the electrolyte containment structure 1, the ionic conductivity of the filled sulfide solid electrolyte 3 is less likely to decrease.

[0226] The lithium ion conductivity of the solid electrolytes obtained in the examples and comparative examples was measured by the following method. Each solid electrolyte was uniaxially press molded under a load of approximately 6 t / cm2 in a glove box substituted with thoroughly dried argon gas (dew point below -60°C) to produce a sample for measuring lithium ion conductivity consisting of a pellet with a diameter of 10 mm and a thickness of approximately 1 mm to 8 mm. The lithium ion conductivity was measured using a Solartron 1255B manufactured by Toyo Corporation. The measurement conditions were an AC impedance method with a temperature of 25°C, a frequency of 100 Hz to 1 MHz, and an amplitude of 100 mV. [Explanation of symbols]

[0227] 1, 1AB, 1AB, 1AC, 1BB, 1BC Electrolyte Encapsulation Structure 3 Sulfide solid electrolyte 5. 5C Electrolyte Encapsulation Structure 7, 7A, 7B, Electrolyte-encapsulating intermediate structure 100, 100A, 100B, 100C First package 107 Inside 108 Exterior 109 1st space 110 Packaging materials 116 Single Layer 117 Inner weld 118 Outside non-welded part 119 First Space Gas 120 Heat seal bag 121 Bag body 122 Sealing part 123 Heat seal section 127 Opening 130 Bottle with lid 131 Bottle body 132 Screw Cap 133 1st connection part 134 2nd connection part 137 Opening 140 Ziplock bag 141 Bag body 142 Sealing part 143 Chuck part 147 Opening 200, 200A 2nd package 207 Inside 208 Exterior 209 Second space 210 Packaging materials 216 Single Layer 217 Inner weld 218 Outside non-welded part 219 Second Space Gas 220 Heat seal bag 221 Bag body 222 Sealing part 223 Heat seal section 227 Opening 300, 300A 3rd package 307 Inside 308 Exterior 309 Third space 310 Packaging materials 316 Single Layer 317 Inner weld 318 Outside non-welded part 319 Third Space Gas 320 Heat seal bag 321 Bag body 322 Sealing part 323 Heat seal section 327 Opening FG Filling gas

Claims

1. A sulfide solid electrolyte; A first packaging body that encapsulates the sulfide solid electrolyte; A second package that contains and encloses the first package; An electrolyte containment structure having An electrolyte containment structure in which a filling gas having an oxygen concentration of 30% or less and a dew point temperature of -20°C or less is sealed in a first space partitioned by an inner surface of the first packaging body, which is the surface that seals the sulfide solid electrolyte, and in a second space partitioned by the outer surface of the first packaging body and the inner surface of the second packaging body.

2. Further comprising a third package that receives and encloses the second package, The electrolyte containment structure described in claim 1, wherein a filling gas having an oxygen concentration of 30% or less and a dew point temperature of -20°C or less is sealed in a third space partitioned by the outer surface of the second packaging body and the inner surface of the third packaging body.

3. The filling gas is Ar, air, N 2 Or CO 2 3. The electrolyte encapsulation structure according to claim 1 or 2,

4. 3. The electrolyte containment structure according to claim 1, wherein the packaging material constituting the first packaging body includes a layer made of aluminum.

5. The electrolyte containment structure described in claim 4, wherein the packaging material constituting the first packaging body comprises an inner welded portion made of a weldable organic material, and an outer non-welded portion which is a layer made of aluminum and is laminated on the outer surface of the inner welded portion.

6. 6. The electrolyte containment structure according to claim 5, wherein the organic material is one or more organic resins selected from the group consisting of polyethylene terephthalate, polyethylene, chlorinated polyethylene, high density polyethylene, nylon, and polyvinyl alcohol.

7. 7. The electrolyte containment structure according to claim 6, wherein the first package is a heat-sealed bag having an opening welded therein.

8. 3. The electrolyte containment structure according to claim 1, wherein the first package is a lidded bottle equipped with a screw cap.

9. 9. The electrolyte containment structure according to claim 8, wherein the first packaging body is made of a packaging material having a layer made of an organic substance.

Citation Information

Patent Citations

  • Sulfide-based fully solid battery laminated sheet and laminated pack using same

    CN113784835A

  • The invention relates to a container for examining solid electrolytes

    DE102019102589A1

  • Material storage and dispensing package and method

    JP2008539145A

  • Production method of sulfide compound storage container

    JP2014234212A

  • Solid electrolyte composition, method for producing same, storage method and kit, solid electrolyte-containing sheet, storage method and kit therefor, and all-solid secondary battery

    WO2019054191A1

Cited By

  • Substance packaging container, method for storing substances, and method for transporting substances

    JP2026146380A

  • Method for manufacturing a packaging and packaging

    JP2026151267A

  • Packaging and method for manufacturing packaging

    JP2026151268A

  • Packaging and production method for packaging

    WO2026191730A1

  • Packaging production method and packaging

    WO2026191731A1