Electronic component and manufacturing method of electronic component

A laminated external electrode layer structure addresses moisture infiltration issues in electronic components by ensuring uniform thickness and preventing cracks, thereby maintaining component integrity and performance.

JP2024145496APending Publication Date: 2024-10-15FDK CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023057871
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Electronic components with external connection terminals on the end surface are prone to moisture infiltration due to thinner edges, leading to deterioration of characteristics.

Method used

A laminated structure for the external electrode layer comprising a first conductive-insulating layer and a second conductive-insulating layer is applied to cover the edge portions, ensuring a uniform thickness and preventing moisture ingress.

Benefits of technology

The laminated structure effectively prevents moisture penetration, reducing cracks and maintaining component integrity and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145496000001_ABST
    Figure 2024145496000001_ABST
Patent Text Reader

Abstract

To realize an electronic component with an excellent resistance against a moisture content.SOLUTION: A solid battery 1 as an example of an electronic component contains: a component main body 10 having an end surface 10a; and an external electrode layer 30 that covers the end surface 10a of the component main body 10 and an edge part 10c on the end surface 10a side. The external electrode layer 30 contains a first layer 31 and a second layer 32. The first layer 31 convers the end surface 10a of the component main body 10 and the edge part 10c, and includes a first conductive material and a first insulation material. A second layer 32 covers the first layer 31, and contains a second conductive material and a second insulation material. A thickness T2 of the external electrode layer 30 in the edge part 10c is increased, and a formation of an infiltration path into the component main body 10 of a plating liquid when forming a plating layer 40 or a moisture vapor contained in an external air is suppressed, so that a resistance against a moisture content of the solid battery 1 is enhanced.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electronic component and a method for manufacturing an electronic component. [Background technology]

[0002] Regarding electronic components such as solid-state batteries and multilayer ceramic capacitors, there is known a technique of providing an external connection terminal on the end face of the component body, which is connected to an internal electrode in the component body. For example, there is known an all-solid-state secondary battery in which an external electrode is formed on the end face of a laminate in which a plurality of electrode layers are laminated with a solid electrolyte layer interposed therebetween, and an all-solid-state secondary battery in which the external electrode is covered with diamond-like carbon (Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-126791 A Summary of the Invention [Problem to be solved by the invention]

[0004] In electronic components having external connection terminals on the end faces of the component body, for example, a method is used in which an external electrode layer paste is applied to the end face side of the component body and a predetermined heat treatment is performed to form an external electrode layer that becomes a part of the external connection terminal. However, in electronic components obtained by adopting such a method, the thickness of the external electrode layer at the edge portion on the end face side of the component body may be thinner than the thickness of other parts. If the thickness of the external electrode layer at the edge portion of the component body becomes thinner, the thinner portion may become a path for penetration of moisture such as water vapor contained in the plating solution or in the outside air when the surface of the external electrode layer is further plated, which may lead to a deterioration in the characteristics of the component body and the electronic component equipped with it.

[0005] In one aspect, the present invention aims to provide an electronic component having excellent resistance to moisture. [Means for solving the problem]

[0006] In one embodiment, an electronic component is provided, comprising: a component body having an end face; and an external electrode layer covering the end face and an edge portion of the component body on the end face side, the external electrode layer comprising: a first layer covering the end face and the edge portion and containing a first conductive material and a first insulating material; and a second layer covering the first layer and containing a second conductive material and a second insulating material.

[0007] In another aspect, a method for manufacturing an electronic component as described above is provided. Effect of the Invention

[0008] In one aspect, it is possible to realize electronic components with excellent resistance to moisture. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a diagram illustrating an example of a solid-state battery. [Diagram 2] 1A to 1C are diagrams illustrating a phenomenon that may occur in forming an external connection terminal of a solid-state battery. [Diagram 3] FIG. 2 is a diagram illustrating an example of a solid-state battery according to an embodiment. [Figure 4] 11A and 11B are diagrams illustrating modified examples of the solid-state battery according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Various electronic components are known that have external connection terminals on end faces of a component body, such as multilayer chip capacitors, multilayer chip inductors, solid-state batteries, etc. In the following, a solid-state battery will be mainly used as an example of an electronic component.

[0011] FIG. 1 is a diagram for explaining an example of a solid-state battery. FIG. 1(A) is a schematic perspective view of a main part of an example of a solid-state battery. FIG. 1(B) is a schematic cross-sectional view of a main part of an example of a solid-state battery. FIG. 1(B) is a schematic cross-sectional view of a main part taken along line L1 in FIG. 1(A).

[0012] The solid-state battery 1A shown in FIG. 1(A) and FIG. 1(B) includes a component body 10 and external connection terminals 20A provided at both ends of the component body 10. The component body 10 is also called the "battery element," "battery body," or "body" of the solid-state battery 1A. The external connection terminals 20A are provided so as to cover the end faces 10a and 10b (FIG. 1(B)) of the component body 10 that face each other in the direction along the line L1. The external connection terminals 20A provided on the end face 10a side and the end face 10b side function as the positive electrode terminal and the negative electrode terminal of the solid-state battery 1A, respectively. Each external connection terminal 20A includes an external electrode layer 30A and a plating layer 40A provided on the surface thereof.

[0013] As shown in FIG. 1B, the component body 10 of the solid-state battery 1A has a positive electrode layer 11, a negative electrode layer 12 facing the positive electrode layer 11, and an electrolyte layer 13 interposed therebetween. In the component body 10, the positive electrode layer 11 and the negative electrode layer 12 are laminated in multiple layers so as to be alternately arranged with the electrolyte layer 13 in between. In the component body 10, the positive electrode layer 11 and the negative electrode layer 12 are provided so as to partially overlap each other with the electrolyte layer 13 interposed therebetween. The surface of the laminate of the positive electrode layer 11, the negative electrode layer 12, and the electrolyte layer 13 is covered with a cover layer 14, except for the end surface 10a and the end surface 10b. Note that one or both of the positive electrode layer 11 and the negative electrode layer 12 are also referred to as "internal electrode layers."

[0014] The electrolyte layer 13 of the component body 10 includes a solid electrolyte. For example, an oxide solid electrolyte is used as the solid electrolyte of the electrolyte layer 13. For example, LAGP, which is a type of NASICON (Na super ionic conductor) type (also called "NaSICON type") oxide solid electrolyte, is used as the oxide solid electrolyte of the electrolyte layer 13. LAGP is a type of oxide solid electrolyte having the general formula Li 1+x Al x Ge 2-xIt is an oxide solid electrolyte represented by (PO4)3(0 < x ≤ 1). In addition, a sulfide solid electrolyte such as Li2S (lithium sulfide)-P2S5 (diphosphorus pentasulfide) may be used as the solid electrolyte of the electrolyte layer 13.

[0015] The positive electrode layer 11 of the component body 10 contains a positive electrode active material, a conductive assistant, and a solid electrolyte. As the solid electrolyte of the positive electrode layer 11, an oxide solid electrolyte or a sulfide solid electrolyte, for example, the same kind of material as the solid electrolyte used for the electrolyte layer 13 is used. As the positive electrode active material of the positive electrode layer 11, for example, Li2CoP2O7 (lithium cobalt pyrophosphate, also referred to as "LCPO") etc. are used. As the conductive assistant of the positive electrode layer 11, for example, carbon materials such as carbon fiber, carbon black, graphite, graphene or carbon nanotubes, and conductive materials such as iron silicide are used.

[0016] The negative electrode layer 12 of the component body 10 contains a negative electrode active material, a conductive assistant, and a solid electrolyte. As the solid electrolyte of the negative electrode layer 12, an oxide solid electrolyte or a sulfide solid electrolyte, for example, the same kind of material as the solid electrolyte used for the electrolyte layer 13 is used. As the negative electrode active material of the negative electrode layer 12, for example, TiO2 (titanium oxide), Nb2O5 (niobium pentoxide) etc. are used. In addition, as the negative electrode active material of the negative electrode layer 12, Li3V2(PO4)3 (lithium vanadium phosphate), Li4Ti5O 12 (lithium titanate) etc. may be used. As the conductive assistant of the negative electrode layer 12, for example, carbon materials such as carbon fiber, carbon black, graphite, graphene or carbon nanotubes, and conductive materials such as iron silicide are used.

[0017] In the solid battery 1A, during charging, lithium ions are conducted and taken in from the positive electrode layer 11 through the electrolyte layer 13 to the negative electrode layer 12, and during discharging, lithium ions are conducted and taken in from the negative electrode layer 12 through the electrolyte layer 13 to the positive electrode layer 11. In the solid battery 1A, such charge and discharge operations are realized by the conduction of lithium ions in the component body 10.

[0018] For example, a solid electrolyte is used for the cover layer 14 of the component body 10. In addition, an insulating material having a higher hardness than the solid electrolyte is used for the cover layer 14. For example, an insulating material having a higher hardness than the solid electrolyte used for the electrolyte layer 13 is used for the cover layer 14. Alternatively, an insulating material having a higher hardness than the solid electrolyte used for the electrolyte layer 13 and the solid electrolyte used for the positive electrode layer 11 and the negative electrode layer 12, which are the internal electrode layers, is used for the cover layer 14. The insulating property of the cover layer 14 refers to a property that has no effect on the lithium ion conduction and the electron conduction in the component body 10 or has a sufficiently low effect. For example, glass or ceramics is used for the insulating cover layer 14 having a higher hardness than the solid electrolyte. The cover layer 14 has a function of protecting the component body 10 from external forces and the outside air. For this reason, the cover layer 14 has the above-mentioned hardness and insulating property, and is low in moisture permeability or gas permeability such as hydrogen and oxygen, and can realize good sealing. Of the materials that can be used for the cover layer 14, glass or ceramics is one type of material that can combine these properties and is therefore suitable as a material for forming the cover layer 14.

[0019] A part of the side surface of the positive electrode layer 11 is exposed at one end face 10a of the component body 10. A part of the side surface of the negative electrode layer 12 is exposed at the other end face 10b of the component body 10. The part of the side surface of the positive electrode layer 11 exposed at the end face 10a and the part of the side surface of the negative electrode layer 12 exposed at the end face 10b are used for electrical connection to the outside of the component body 10. Here, the end face 10a where the positive electrode layer 11 is exposed is also referred to as the "positive electrode extraction surface." The end face 10b where the negative electrode layer 12 is exposed is also referred to as the "negative electrode extraction surface." One or both of the positive electrode extraction surface and the negative electrode extraction surface are also referred to as the "electrode extraction surface."

[0020] An external electrode layer 30A is provided on one end face 10a (positive electrode lead-out face) of the component body 10 so as to cover the end face 10a of the component body 10 and the edge portion 10c on the end face 10a side. The edge portion 10c includes a boundary (ridge portion or corner portion) between the end face 10a and the outer surface 10e of the component body 10 that is continuous with the end face 10a. The external electrode layer 30A on the end face 10a side is provided so as to cover the end face 10a and the edge portion 10c of the component body 10 and extend onto a part of the outer surface 10e. The external electrode layer 30A on the end face 10a side is formed, for example, by applying a paste for the external electrode layer 30A containing a conductive material such as powdered Ag (silver) and subjecting it to a heat treatment. The positive electrode layer 11 exposed on the end face 10a side of the component body 10 is connected to the external electrode layer 30A provided on the end face 10a side.

[0021] On the other end face 10b (negative electrode lead surface) side of the component body 10, an external electrode layer 30A is provided so as to cover the end face 10b of the component body 10 and the edge portion 10d on the end face 10b side. The edge portion 10d includes a boundary (ridge portion or corner portion) between the end face 10b and the outer surface 10e of the component body 10 that is continuous with the end face 10b. The external electrode layer 30A on the end face 10b side is provided so as to cover the end face 10b and the edge portion 10d of the component body 10 and extend onto a part of the outer surface 10e. The external electrode layer 30A on the end face 10b side is formed, for example, by applying a paste for the external electrode layer 30A containing a conductive material such as powdered Ag and subjecting it to a heat treatment. The negative electrode layer 12 exposed on the end face 10b side of the component body 10 is connected to the external electrode layer 30A provided on the end face 10b side.

[0022] A plating layer 40A is provided so as to cover each of the external electrode layers 30A on the surfaces of the external electrode layers 30A provided on the end face 10a side and the end face 10b side of the component body 10. The plating layer 40A is formed, for example, by depositing a metal such as Ni (nickel) or Sn (tin) using an electrolytic plating method.

[0023] The external electrode layer 30A provided on one end face 10a of the component body 10 and the plating layer 40A on its surface function as a positive terminal, which is one of the external connection terminals 20A of the solid-state battery 1A. The external electrode layer 30A provided on the other end face 10b of the component body 10 and the plating layer 40A on its surface function as a negative terminal, which is another of the external connection terminals 20A of the solid-state battery 1A. The positive and negative terminals are used to realize the charging and discharging operations of the solid-state battery 1A.

[0024] As described above, in the solid-state battery 1A, when the external connection terminal 20A is formed, for example, a paste for the external electrode layer 30A is applied to the end face 10a side and the end face 10b side of the component body 10 by a dipping method, and a predetermined heat treatment is performed to form the external electrode layer 30A. Then, a predetermined metal is deposited on the surface of the formed external electrode layer 30A by an electrolytic plating method to form a plating layer 40A. In this case, the following situation may occur as shown in FIG. 2.

[0025] FIG. 2 is a diagram for explaining a phenomenon that may occur in the formation of an external connection terminal of a solid-state battery. FIG. 2(A) is a schematic cross-sectional view of a main part of an example of an external electrode layer forming step. FIG. 2(B) is a schematic cross-sectional view of a main part of an example of a plating layer forming step. FIG. 2(A) and FIG. 2(B) are enlarged schematic cross-sectional views of part P1 of FIG. 1(B). FIG. 2(C) is a schematic perspective view of a main part of an example of a defective solid-state battery. FIG. 2(C) shows a view in which a part of the external connection terminal (a part of the plating layer) has been removed.

[0026] During the formation of the external electrode layer 30A, for example, as shown in FIG. 2(A), the paste for the external electrode layer 30A applied by dipping to the end face 10a side of the component body 10 may become thinner at the edge portion 10c, and the thickness T1 of the external electrode layer 30A formed at the edge portion 10c may become thinner than the thickness of other portions (on the end face 10a and on the outer surface 10e). Note that, although only a portion of the edge portion 10c of one end face 10a is illustrated in FIG. 2(A) and FIG. 2(B), the external electrode layer 30A may become partially thin in other portions of the edge portion 10c of the end face 10a, and in part or all of the edge portion 10d of the other end face 10b. When the external electrode layer 30A becomes partially thin in this way, the thinned portion may be a factor in causing defects in the component body 10 and the solid-state battery 1A including the same.

[0027] For example, as shown in FIG. 2(A), if the applied paste for the external electrode layer 30A is thin at the edge portion 10c, the external electrode layer 30A formed by the paste may have a crack 101 (shrinkage crack) caused by shrinkage due to the heat treatment, as shown in FIG. 2(C). In addition, as shown in FIG. 2(B), when forming the plating layer 40A after forming the external electrode layer 30A, the plating solution may penetrate into the inside of the component body 10 through the thinned portion or crack 101 of the external electrode layer 30A. Alternatively, water vapor contained in the outside air may penetrate into the inside of the component body 10 through the thinned portion or crack 101 of the external electrode layer 30A before forming the plating layer 40A. When moisture penetrates into the inside of the component body 10, the inside of the component body 10 expands due to moisture due to heat applied during charge / discharge operations or mounting of the solid-state battery 1A including the component body 10, and a crack 102 may occur in the component body 10 as shown in FIG. 2(C).

[0028] Thus, the thinned portion of the external electrode layer 30A can become a path for moisture to penetrate. Partial thinning of the external electrode layer 30A at the edge portion 10c or the like can cause cracks 101 in the external electrode layer 30A, moisture penetration, and cracks 102 in the component body 10 due to the penetrated moisture. In addition to cracks 102 and the like, the penetration of moisture into the component body 10 may cause a deterioration in characteristics such as the charge / discharge characteristics of the component body 10 and the solid-state battery 1A including the same.

[0029] Here, solid-state battery 1A is used as an example, but the same thing as described above for solid-state battery 1A can occur in electronic components that have external connection terminals on the end faces of the component body, such as multilayer chip capacitors and multilayer chip inductors.

[0030] In view of this, the following embodiment employs a configuration to realize an electronic component with excellent resistance to moisture. For convenience, a solid-state battery is used as an example of the electronic component. Fig. 3 is a diagram for explaining an example of a solid-state battery according to an embodiment. Fig. 3(A) is a schematic cross-sectional view of a main part of an example of a solid-state battery. Fig. 3(B) is a schematic enlarged cross-sectional view of a P2 portion of Fig. 3(A).

[0031] The solid-state battery 1 shown in FIG. 3(A) and FIG. 3(B) includes a component body 10 and external connection terminals 20 provided at both ends of the component body 10. The component body 10 is the same as that described for the solid-state battery 1A (FIG. 1(A) and FIG. 1(B)). That is, the component body 10 includes a positive electrode layer 11 (internal electrode layer), a negative electrode layer 12 (internal electrode layer), an electrolyte layer 13 interposed therebetween, and a cover layer 14 that covers the surface of the laminate except for the opposing end face 10a (positive electrode lead-out surface) and end face 10b (negative electrode lead-out surface). The external connection terminals 20 are provided so as to cover the opposing end faces 10a and 10b of the component body 10. The external connection terminals 20 provided on the end face 10a side and the end face 10b side function as the positive electrode terminal and the negative electrode terminal of the solid-state battery 1, respectively. Each external connection terminal 20 includes an external electrode layer 30 and a plating layer 40 provided on the surface thereof. The external electrode layer 30 includes a first layer 31 provided on the inside and a second layer 32 provided on the outside thereof.

[0032] The first layers 31 of the external electrode layer 30 are provided on the end faces 10a and 10b of the component body 10, respectively. The first layer 31 on the end face 10a side is provided so as to cover the end face 10a of the component body 10 and the edge portion 10c on the end face 10a side. The edge portion 10c includes the boundary (ridge portion or corner portion) between the end face 10a and the outer surface 10e of the component body 10 that is continuous with the end face 10a. The first layer 31 on the end face 10a side is provided so as to cover the end face 10a and the edge portion 10c of the component body 10 and extend onto a part of the outer surface 10e. The positive electrode layer 11 exposed on the end face 10a side of the component body 10 is connected to the first layer 31 provided on the end face 10a side.

[0033] The first layer 31 on the end face 10b side is provided so as to cover the end face 10b of the component body 10 and the edge portion 10d on the end face 10b side. The edge portion 10d includes a boundary (ridge portion or corner portion) between the end face 10b and the outer surface 10e of the component body 10 that is continuous with the end face 10b. The first layer 31 on the end face 10b side is provided so as to cover the end face 10b and the edge portion 10d of the component body 10 and extend onto a part of the outer surface 10e. The negative electrode layer 12 exposed on the end face 10b side of the component body 10 is connected to the first layer 31 provided on the end face 10b side.

[0034] The first layer 31 on the end face 10a side and the end face 10b side of the component body 10 is formed using a paste for the first layer 31. The paste for the first layer 31 contains a first conductive material and a first insulating material. The first conductive material is a metal such as powdered Ag. The first insulating material is powdered glass. The paste for the first layer 31 contains organic components such as a resin and a solvent in addition to the first conductive material and the first insulating material.

[0035] The first layer 31 is formed by applying a paste for the first layer 31 to each of the end faces 10a and 10b of the component body 10 by a dipping method, and then baking the paste by a predetermined heat treatment. The heat treatment for baking removes organic components from the paste for the first layer 31. As a result, the first layer 31 containing a metal as the first conductive material and glass as the first insulating material is formed on each of the end faces 10a and 10b of the component body 10.

[0036] Here, when forming the first layer 31, for example, as shown in Figures 3(A) and 3(B), the paste for the first layer 31 applied by the dip method to the end face 10a side of the component body 10 may be thinner at the edge portion 10c, and the thickness of the first layer 31 formed on the edge portion 10c may be thinner than the thickness of the other portions (on the end face 10a and on the outer surface 10e). Similarly, the paste for the first layer 31 applied by the dip method to the end face 10b side of the component body 10 may be thinner at the edge portion 10d, and the thickness of the first layer 31 formed on the edge portion 10d may be thinner than the thickness of the other portions (on the end face 10b and on the outer surface 10e).

[0037] The second layers 32 of the external electrode layer 30 are provided on the end face 10a side and the end face 10b side of the component body 10, respectively, on the outer sides of the first layers 31. The second layer 32 on the end face 10a side is provided, for example, so as to cover the first layer 31 on its inner side. The second layer 32 on the end face 10b side is provided, for example, so as to cover the first layer 31 on its inner side.

[0038] The second layer 32 on the end face 10a side and the end face 10b side of the component body 10 is formed using a paste for the second layer 32. The paste for the second layer 32 contains a second conductive material and a second insulating material. The second conductive material is a metal such as powdered Ag. The second insulating material is, for example, powdered glass. Alternatively, the second insulating material is, for example, a thermosetting resin that is hardened by heat treatment. Regardless of whether the second insulating material is glass or a thermosetting resin, the paste for the second layer 32 contains organic components such as a resin, a solvent, and the like in addition to the second conductive material and the second insulating material.

[0039] For example, when glass is used as the second insulating material, the second layer 32 is formed by applying a paste for the second layer 32 to each of the end faces 10a and 10b of the component body 10 by a dipping method and baking the paste by a predetermined heat treatment. The heat treatment for baking removes organic components from the paste for the second layer 32. As a result, the second layer 32 containing a metal as the second conductive material and glass as the second insulating material is formed on each of the end faces 10a and 10b of the component body 10.

[0040] For example, when a thermosetting resin is used as the second insulating material, the second layer 32 is formed by applying a paste for the second layer 32 to each of the end faces 10a and 10b of the component body 10 by a dipping method, and hardening the thermosetting resin contained therein by a predetermined heat treatment. The heat treatment for hardening can remove a part of the organic components of the paste for the second layer 32. As a result, the second layer 32 containing a metal as the second conductive material and a resin as the second insulating material is formed on each of the end faces 10a and 10b of the component body 10.

[0041] The second layer 32 is formed, for example, after the first layer 31 is formed, that is, after the paste for the first layer 31 is applied and baked by heat treatment. When a thermosetting resin is used as the second insulating material of the paste for the second layer 32, depending on the curing temperature of the resin, it is also possible to form the second layer 32 by curing the paste for the second layer 32 under conditions lower than the heat treatment temperature when baking the paste for the first layer 31. By lowering the formation temperature of the second layer 32, it is possible to suppress thermal damage to the component body 10 accompanying the formation of the external electrode layer 30. Also, although an example of using a thermosetting resin as the second insulating material of the paste for the second layer 32 is shown here, it is also possible to use a photocurable resin as the second insulating material in addition to a thermosetting resin.

[0042] The external electrode layer 30 is formed by the first layer 31 on the inside and the second layer 32 on the outside. Here, the second layer 32 on the end face 10a side is formed so as to cover the part of the first layer 31 on the inside that is thinned at the edge portion 10c. Similarly, the second layer 32 on the end face 10b side is formed so as to cover the part of the first layer 31 on the inside that is thinned at the edge portion 10d. As a result, the external electrode layer 30 is formed at the edge portions 10c and 10d with a thickness T2 equal to or greater than a certain value, which is the sum of the thickness of the first layer 31 and the thickness of the second layer 32.

[0043] A plating layer 40 is provided on the surface of the external electrode layer 30 provided on the end face 10a side and the end face 10b side of the component body 10. The plating layer 40 is provided so as to cover the external electrode layer 30. The plating layer 40 is formed, for example, by depositing a metal such as Ni or Sn using an electrolytic plating method, for example, by depositing and stacking a Sn layer on a deposited Ni layer.

[0044] The external electrode layer 30 provided on one end face 10a of the component body 10, together with the plating layer 40 on its surface, functions as a positive terminal, which is one of the external connection terminals 20 of the solid-state battery 1. The external electrode layer 30 provided on the other end face 10b of the component body 10, together with the plating layer 40 on its surface, functions as a negative terminal, which is another of the external connection terminals 20 of the solid-state battery 1. The positive and negative terminals are used to realize the charging and discharging operations of the solid-state battery 1.

[0045] As described above, in the solid-state battery 1 according to the embodiment, the first layer 31 is provided on the inside as the external electrode layer 30, and the second layer 32 is provided on the outside thereof. Even if a thinned portion is formed in the first layer 31 at the edge portion 10c and the edge portion 10d of the component body 10, the thinned portion is covered with the second layer 32. Therefore, at the edge portion 10c and the edge portion 10d, the external electrode layer 30 having a thickness T2 equal to or greater than a certain value, which is the sum of the thickness of the first layer 31 and the thickness of the second layer 32, is formed. This prevents cracks from remaining in the external electrode layer 30 after the first layer 31 of the external electrode layer 30 is formed and the second layer 32 is further formed. Furthermore, water vapor contained in the outside air is prevented from penetrating into the component body 10 through the thinned portion or crack of the external electrode layer 30 before the plating layer 40 is formed. Furthermore, when the plating layer 40 is formed, the plating solution is prevented from penetrating into the component body 10 through the thinned portion or crack of the external electrode layer 30. By forming the external electrode layer 30 in a laminated structure including the first layer 31 on the inside and the second layer 32 on the outside thereof, it is possible to prevent the formation of a path for moisture penetration in the external electrode layer 30. Thus, a solid-state battery 1 with excellent resistance to moisture is realized.

[0046] In the solid-state battery 1, the intrusion of moisture into the component body 10 is suppressed, which suppresses the inside of the component body 10 from expanding due to moisture caused by heat applied during charging / discharging operations or mounting, and thus suppresses the occurrence of cracks in the component body 10. By suppressing cracks in the external electrode layer 30, the intrusion of moisture, and cracks in the component body 10 due to the intruded moisture, deterioration of characteristics such as the charge / discharge characteristics of the component body 10 and the solid-state battery 1 including it is suppressed.

[0047] Fig. 4 is a diagram for explaining a modified example of the solid-state battery according to the embodiment, Fig. 4(A) and Fig. 4(B) each show a schematic cross-sectional view of a main part of an example of the solid-state battery. The solid-state battery 1a shown in FIG. 4(A) includes an external connection terminal 20 having an external electrode layer 30 including a first layer 31 and a second layer 32, and a plating layer 40 on the surface thereof. In the solid-state battery 1a, the second layer 32 is provided so as to cover a part of the first layer 31. The second layer 32 is provided as a part of the first layer 31 so as to cover the thinned portion of the first layer 31 formed at the edge portion 10c and the edge portion 10d of the component body 10. For example, the first layer 31 is provided on the outer surface 10e of the component body 10 in an area of ​​dimension W1 from the edge portion 10c and the edge portion 10d, and the second layer 32 is provided in an area of ​​dimension W2 smaller than dimension W1 from the edge portion 10c and the edge portion 10d. The solid-state battery 1a differs from the above-mentioned solid-state battery 1 (FIGS. 3(A) and 3(B)) in having such a configuration.

[0048] As in the solid-state battery 1a, the external electrode layer 30 including the first layer 31 and the second layer 32 may have a region where the first layer 31 exists as a single layer and a region where the first layer 31 and the second layer 32 exist in a laminated state. In this case, a step 34 is formed between the region where the first layer 31 exists as a single layer and the region where the first layer 31 and the second layer 32 exist in a laminated state. The second layer 32 may be provided so as to cover not only the entire first layer 31 but also a part of the first layer 31, as long as it can cover the parts of the first layer 31 that are thinned at the edge portion 10c and the edge portion 10d.

[0049] A solid-state battery 1b shown in Fig. 4(B) has a configuration in which the external connection terminal 20 has an external electrode layer 30 and a plating layer 40, and the external electrode layer 30 further includes a third layer 33 in addition to the first layer 31 and the second layer 32. The solid-state battery 1b differs from the above-described solid-state battery 1 (Figs. 3(A) and 3(B)) in having such a configuration.

[0050] The third layer 33 is provided on the end face 10a side and the end face 10b side of the component body 10, respectively, on the outside of each of the second layers 32. The third layer 33 is formed using a paste for the third layer 33 containing a third conductive material and a third insulating material. The third conductive material is a metal such as powdered Ag. The third insulating material is powdered glass or a thermosetting resin. The paste for the third layer 33 contains organic components such as resin and solvent in addition to the third conductive material and the third insulating material. The third layer 33 is formed by applying the paste for the third layer 33 to the end face 10a side and the end face 10b side of the component body 10 by a dipping method, and baking or curing the paste by a predetermined heat treatment. The organic components in the paste for the third layer 33 can be removed by the heat treatment. As a result, third layers 33 containing a metal as a third conductive material and glass or resin as a third insulating material are formed on the end faces 10a and 10b of the component body 10, respectively.

[0051] The third layer 33 is formed, for example, after the second layer 32 is formed, that is, after the paste for the second layer 32 is applied and baked or hardened by heat treatment. When a thermosetting resin is used as the third insulating material of the paste for the third layer 33, the curing temperature can be set lower than the baking temperature of the paste for the first layer 31 (or the paste for the first layer 31 and the second layer 32), thereby suppressing thermal damage to the component body 10. In addition to a thermosetting resin, a photocurable resin can also be used as the third insulating material of the paste for the third layer 33.

[0052] As in the solid-state battery 1b, by providing the third layer 33 in addition to the first layer 31 and the second layer 32, it is possible to further increase the thickness of the external electrode layer 30 at the edge portions 10c and 10d where the external electrode layer 30 is likely to become thin. For example, even if the second layer 32 is provided on the outside of the first layer 31, if the thickness of the external electrode layer 30 at the edge portions 10c and 10d is not sufficient to suppress the intrusion of moisture, etc., the third layer 33 may be further provided to further increase the thickness of the external electrode layer 30 so that the intrusion of moisture, etc. can be sufficiently suppressed.

[0053] In the solid-state battery 1b, the number of layers of the external electrode layer 30 in the external connection terminal 20 is not limited to three layers, the first layer 31, the second layer 32, and the third layer 33, and may be four or more layers. In this case, each layer included in the external electrode layer 30 is formed, for example, after application of a paste of a base layer and heat treatment.

[0054] In the solid-state battery 1b, following the example of the solid-state battery 1a (FIG. 4(A)), the second layer 32 may be provided so as to cover a part of the first layer 31, and the third layer 33 may be provided so as to cover a part of the second layer 32. The same applies when the external electrode layer 30 is four or more layers.

[0055] Here, the solid-state batteries 1, 1a, and 1b are taken as examples, but it is possible to adopt a configuration similar to the external connection terminals 20 of the solid-state batteries 1, 1a, and 1b for various electronic components that have external connection terminals on the end faces of the component body, such as multilayer chip capacitors and multilayer chip inductors. By adopting this configuration, it is possible to obtain the same effects as those described for the external connection terminals 20 for various electronic components.

[0056] Examples and comparative examples of solid-state batteries and their characteristics will be described below. Example 1 A component body 10 of a solid-state battery 1a (FIG. 4(A)) was prepared, which had a positive electrode layer 11, a negative electrode layer 12, an electrolyte layer 13 interposed therebetween, and a cover layer 14 covering the surface of this laminate except for the opposing end faces 10a and 10b.

[0057] A paste for the first layer 31 containing Ag and glass was applied by dipping to one of the end faces 10a and 10b of the prepared component body 10 in a region from the end face to a predetermined position on the outer surface 10e of the component body 10 where the dimension W1 is in the range of 400 μm to 900 μm (this can also be said to be a predetermined value in the doctor blade gap range of 400 μm to 900 μm), and the applied surface was dried under predetermined conditions with the applied surface facing vertically upward, and then baked by heat treatment at a predetermined temperature in the range of 300° C. to 400° C. for a predetermined time in the range of 10 to 40 minutes. This was performed for each of the end faces 10a and 10b of the component body 10. This formed a first layer 31 covering the end face 10a of the component body 10 and the edge portion 10c on the side of the end face 10a, and a first layer 31 covering the end face 10b of the component body 10 and the edge portion 10d on the side of the end face 10b.

[0058] Next, a paste for the second layer 32 containing Ag and glass was applied by dip coating to one of the end faces 10a and 10b of the component body 10 on which the first layer 31 was formed, in a region from the end face to a predetermined position on the outer surface 10e of the component body 10 in a range of 100 μm to 600 μm in dimension W2 (which can also be said to be a predetermined value in a range of 100 μm to 600 μm for the doctor blade gap), and the paste was dried under predetermined conditions with the applied surface facing vertically upward, and then baked by heat treatment at a predetermined temperature in a range of 300° C. to 400° C. for a predetermined time in a range of 10 to 40 minutes. This was performed for each of the end faces 10a and 10b of the component body 10. As a result, the second layer 32 provided on the outside of the first layer 31 on the end face 10a side and the second layer 32 provided on the outside of the first layer 31 on the end face 10b side were formed.

[0059] In this manner, an external electrode layer 30 including a first layer 31 and a second layer 32 was formed. A plating layer 40 was formed on the surface of the formed external electrode layer 30 by electrolytic plating. In this manner, a solid-state battery 1a having the configuration shown in FIG. 4(A) was obtained as the solid-state battery of Example 1. Hereinafter, this solid-state battery of Example 1 is also referred to as a "twice baked" solid-state battery.

[0060] Comparative Example 1 The formation of the second layer 32 described in Example 1 above (application, drying and baking of the paste for the second layer 32) was omitted, and an external electrode layer 30 consisting of a single first layer 31 was formed. All other points were the same as in Example 1 above. In this way, a solid-state battery of Comparative Example 1 was obtained. Hereinafter, this solid-state battery of Comparative Example 1 is also referred to as a "reference" solid-state battery.

[0061] Comparative Example 2 After the paste for the first layer 31 was applied and dried by the dipping method described in Example 1 above, the paste for the second layer 32 was applied and dried by the dipping method without baking (heat treatment). Then, the paste for the first layer 31 and the paste for the second layer 32 were simultaneously baked by heat treatment at a predetermined temperature in the range of 300°C to 400°C for a predetermined time in the range of 10 minutes to 40 minutes to form an external electrode layer 30 having a laminated structure of the first layer 31 and the second layer 32. The other points were the same as those in Example 1 above. In this way, a solid battery of Comparative Example 2 was obtained. Hereinafter, this solid battery of Comparative Example 2 is also referred to as a "two-dip" solid battery.

[0062] Comparative Example 3 After the paste for the first layer 31 described in Example 1 was applied by the dipping method, the applied surface was dried facing vertically downward, and then baked by heat treatment. The formation of the second layer 32 described in Example 1 (application of the paste for the second layer 32, drying and baking) was omitted, and an external electrode layer 30 consisting of a single layer of the first layer 31 was formed. All other points were the same as in Example 1. In this way, a solid-state battery of Comparative Example 3 was obtained. Hereinafter, this solid-state battery of Comparative Example 3 is also referred to as an "upside-down dried" solid-state battery.

[0063] (Characteristics evaluation of solid-state batteries) A plurality of solid-state batteries of Example 1 and Comparative Examples 1-3 were fabricated, and cross-sectional observation and appearance observation were performed. Furthermore, the crack occurrence rate of the component body 10 was evaluated for the plurality of solid-state batteries of Example 1 and Comparative Examples 1-3. The evaluation results are shown in Table 1.

[0064] [Table 1]

[0065] From the appearance observation, in the reference solid-state battery of Comparative Example 1, no cracks (cracks 101 as described in FIG. 2(C) above, the same below) were observed after baking of the external electrode layer 30 (first layer 31 single layer), but cracks (cracks 102 as described in FIG. 2(C) above, the same below) were observed in the component body 10 after the formation of the plating layer 40. From Table 1, in the reference solid-state battery of Comparative Example 1, the crack occurrence rate of the component body 10 after the formation of the plating layer 40 was 77.1%.

[0066] From the cross-sectional observation, it was confirmed that in the double-dip solid battery of Comparative Example 2, the external electrode layer 30 (laminated structure of the first layer 31 and the second layer 32) was formed thicker at the edge portion 10c and the edge portion 10d than the external electrode layer 30 (single layer of the first layer 31) in the reference solid battery of Comparative Example 1. From the external observation, in the double-dip solid battery of Comparative Example 2, the occurrence of cracks was observed after baking of the external electrode layer 30 (laminated structure of the first layer 31 and the second layer 32), and the occurrence of cracks was also observed in the component body 10 after the formation of the plating layer 40. From Table 1, in the double-dip solid battery of Comparative Example 2, the crack occurrence rate of the component body 10 after the formation of the plating layer 40 was 90.6%.

[0067] From the cross-sectional observation, it was confirmed that in the upside-down dried solid battery of Comparative Example 3, the external electrode layer 30 (first layer 31 single layer) was formed at the edge portion 10c and the edge portion 10d to be equal to or slightly thicker than the external electrode layer 30 (first layer 31 single layer) in the reference solid battery of Comparative Example 1, but was formed thinner than the external electrode layer 30 (laminated structure of the first layer 31 and the second layer 32) in the double-dip solid battery of Comparative Example 2. The effect of making the thickness of the external electrode layer 30 at the edge portion 10c and the edge portion 10d sufficiently thick by the upside-down drying was not observed. From the appearance observation, although the occurrence of cracks was not observed after baking of the external electrode layer 30 (first layer 31 single layer) in the upside-down dried solid battery of Comparative Example 3, the occurrence of cracks was observed in the component body 10 after the formation of the plating layer 40. In addition, the plating layer 40 also had an appearance defect such as a burn caused by an overcurrent during its formation. As can be seen from Table 1, in the solid-state battery dried upside down in Comparative Example 3, the rate of cracking in the component body 10 after the plating layer 40 was formed was 94.1%.

[0068] From the cross-sectional observation, it was confirmed that in the twice-baked solid-state battery of Example 1, the external electrode layer 30 (laminated structure of the first layer 31 and the second layer 32) was formed at the edge portion 10c and the edge portion 10d with a thickness equivalent to that of the external electrode layer 30 (laminated structure of the first layer 31 and the second layer 32) of the twice-dipped solid-state battery of Comparative Example 2. From the external observation, in the twice-baked solid-state battery of Example 1, no cracks were observed after baking of the external electrode layer 30 (laminated structure of the first layer 31 and the second layer 32), and no cracks were observed in the component body 10 after the formation of the plating layer 40. From Table 1, in the twice-baked solid-state battery of Example 1, the crack occurrence rate of the component body 10 after the formation of the plating layer 40 was 0.0%.

[0069] In the solid-state batteries of Comparative Examples 1-3 other than the solid-state battery of Example 1, cracks occurred in the majority of the component bodies 10 out of all the batteries, and the appearance was at a level where non-defective products could not be ensured. In the reference solid-state battery of Comparative Example 1 and the upside-down dried solid-state battery of Comparative Example 3, the thickness of the external electrode layer 30 at edge portions 10c and 10d is relatively thin, and it is not possible to sufficiently prevent moisture from penetrating into the component body 10, so that it can be said that the component body 10 is prone to cracking.

[0070] In the double-dip solid-state battery of Comparative Example 2, although the thickness of the external electrode layer 30 at the edge portions 10c and 10d is relatively large, cracks due to shrinkage (shrinkage cracks) occur during baking, and the penetration of moisture into the component body 10 cannot be sufficiently suppressed, so that it can be said that the component body 10 is prone to cracking.

[0071] In the solid-state battery of Example 1, the thickness of the external electrode layer 30 at the edge portion 10c and the edge portion 10d is relatively thick, and the occurrence of cracks during baking is also suppressed. When the external electrode layer 30 has a laminated structure of the first layer 31 and the second layer 32, the occurrence of cracks is suppressed by baking the paste for the first layer 31 and the paste for the second layer 32 sequentially and separately as in the solid-state battery baked twice in Example 1, rather than baking them simultaneously as in the solid-state battery baked twice in Comparative Example 2. Therefore, it can be said that the solid-state battery of Example 1 can sufficiently suppress the intrusion of moisture into the inside of the component body 10.

[0072] Furthermore, the impedance characteristics were evaluated for the solid state batteries of Example 1 and Comparative Examples 1 to 3. The evaluation results are shown in Table 2.

[0073] [Table 2]

[0074] Table 2 shows the results of AC impedance measurement in a predetermined frequency range including 100 Hz and 0.1 Hz for the solid-state batteries of Example 1 and Comparative Examples 1-3 after baking and plating of the external electrode layer. Table 2 shows the average impedance [Ω] at 100 Hz for a plurality of solid-state batteries after baking of the external electrode layer, the average impedance [Ω] at 100 Hz after plating, and the rate of change [%] between these average values. Table 2 further shows the average impedance [Ω] at 0.1 Hz for a plurality of solid-state batteries after baking of the external electrode layer, the average impedance [Ω] at 0.1 Hz after plating, and the rate of change [%] between these average values. Table 2 also shows the degradation time [days] for the plurality of solid-state batteries of Example 1 and Comparative Example 1, which is the time until a solid-state battery whose capacity becomes 60% or less of its initial value in a high-temperature and high-humidity environment at a temperature of 85° C. and a humidity of 85% is generated.

[0075] In the Nyquist plot obtained for the reference solid-state battery of Comparative Example 1, in some parts, the impedance was found to be smaller after the formation of the plating layer 40 than after the baking of the external electrode layer 30. From Table 2, the average value of the impedance at 100 Hz after baking of the external electrode layer was 123.5Ω, and the average value of the impedance at 100 Hz after plating was 124.9Ω, and the rate of change between these average values ​​was 1.1%. From Table 2, the average value of the impedance at 0.1 Hz after baking of the external electrode layer was 1475.9Ω, and the average value of the impedance at 0.1 Hz after plating was 1393.0Ω, and the rate of change between these average values ​​was -5.6%. In addition, the degradation time until the generation of a solid-state battery in a predetermined high-temperature and high-humidity environment in which the capacity became 60% or less of the initial value was 12.8 days.

[0076] In the Nyquist plot obtained for the two-dip solid battery of Comparative Example 2, the impedance after baking of the external electrode layer 30 was equivalent to that after baking of the external electrode layer 30 in the reference solid battery of Comparative Example 1. In the Nyquist plot obtained for the two-dip solid battery of Comparative Example 2, the impedance was found to be small after the plating layer 40 was formed. From Table 2, the average value of the impedance at 100 Hz after baking of the external electrode layer was 124.9Ω, and the average value of the impedance at 100 Hz after plating was 85.9Ω, and the rate of change between these average values ​​was -31.2%. From Table 2, the average value of the impedance at 0.1 Hz after baking of the external electrode layer was 1363.3Ω, and the average value of the impedance at 0.1 Hz after plating was 226.3Ω, and the rate of change between these average values ​​was -83.4%.

[0077] In the Nyquist plot obtained for the upside-down dried solid battery of Comparative Example 3, after baking of the external electrode layer 30, the impedance was equivalent to that of the reference solid battery of Comparative Example 1 after baking of the external electrode layer 30. However, some short circuits were observed. In the Nyquist plot obtained for the upside-down dried solid battery of Comparative Example 3, after the formation of the plating layer 40, the impedance was dwarfed. From Table 2, the average value of the impedance at 100 Hz after baking of the external electrode layer was 123.4Ω, the average value of the impedance at 100 Hz after plating was 106.8Ω, and the rate of change between these average values ​​was -13.5%. From Table 2, the average value of the impedance at 0.1 Hz after baking of the external electrode layer was 1417.8Ω, the average value of the impedance at 0.1 Hz after plating was 299.4Ω, and the rate of change between these average values ​​was -78.9%.

[0078] In the Nyquist plot obtained for the solid-state battery baked twice in Example 1, the impedance after baking of the external electrode layer 30 was equivalent to that after baking of the external electrode layer 30 in the reference solid-state battery in Comparative Example 1. In the Nyquist plot obtained for the solid-state battery baked twice in Example 1, no change in impedance was observed even after the formation of the plating layer 40. From Table 2, the average value of the impedance at 100 Hz after baking of the external electrode layer was 126.9Ω, the average value of the impedance at 100 Hz after plating was 127.2Ω, and the rate of change between these average values ​​was 0.2%. From Table 2, the average value of the impedance at 0.1 Hz after baking of the external electrode layer was 1366.4Ω, the average value of the impedance at 0.1 Hz after plating was 1375.7Ω, and the rate of change between these average values ​​was 0.7%. In addition, the degradation time until the generation of a solid-state battery in which the capacity became 60% or less of the initial value in a specified high-temperature and high-humidity environment was 39.4 days.

[0079] In addition, in the Nyquist plot obtained for the solid-state battery baked twice in Example 1, no significant deviation was observed from the impedance obtained after the formation of the plating layer 40, either when the battery was mounted using a conductive adhesive (conductive adhesive mounting) or when the battery was mounted using solder (solder mounting).

[0080] In the twice-baked solid-state battery of Example 1, the impedance fluctuation is effectively suppressed after baking the external electrode layer 30 and after forming the plating layer 40. Furthermore, in the twice-baked solid-state battery of Example 1, the impedance fluctuation is suppressed in both mounting forms, that is, conductive adhesive mounting and solder mounting. Furthermore, in the twice-baked solid-state battery of Example 1, the deterioration time until the solid-state battery whose capacity becomes 60% or less of the initial value is generated is significantly extended compared to the reference solid-state battery of Comparative Example 1. It can be said that in the twice-baked solid-state battery of Example 1, the external electrode layer 30 at the edge portion 10c and the edge portion 10d is thickened while suppressing the occurrence of cracks, and the intrusion of moisture into the component body 10 is sufficiently suppressed, thereby suppressing the occurrence of cracks in the component body 10, while suppressing the increase in impedance.

[0081] By configuring the external electrode layer 30 to include the first layer 31 and the second layer 32, a solid-state battery with excellent resistance to moisture is realized. This reduces the occurrence of defective appearance. Furthermore, a solid-state battery with such excellent characteristics is realized while suppressing an increase in impedance.

[0082] In the solid-state battery baked twice in Example 1, it can be said that it is possible to thicken the external electrode layer 30 at the edge portion 10c and the edge portion 10d while suppressing the occurrence of cracks, while suppressing the increase in impedance, sufficiently suppress the intrusion of moisture into the component body 10, suppress the occurrence of cracks in the component body 10, and ensure sufficient charge / discharge characteristics. By configuring the external electrode layer 30 to include the first layer 31 and the second layer 32, a solid-state battery with excellent resistance to moisture is realized. This suppresses the occurrence of appearance defects and realizes a solid-state battery with excellent charge / discharge characteristics. And a solid-state battery with such excellent characteristics is realized while suppressing the increase in impedance. [Explanation of symbols]

[0083] 1, 1a, 1b, 1A solid state battery 10 Part body 10a, 10b end face 10c, 10d Edge 10e Exterior 11 Positive electrode layer 12 Negative electrode layer 13 Electrolyte layer 14 Cover Layer 20, 20A external connection terminal 30, 30A external electrode layer 31 1st layer 32 2nd layer 33 3rd layer 34 Steps 40, 40A plating layer 101 Crack 102 Crack W1, W2 dimensions

Claims

1. a component body having an end surface; an external electrode layer covering the end face and an edge portion on the end face side of the component body; Including, The external electrode layer is a first layer covering the end surface and the edge portion and containing a first conductive material and a first insulating material; a second layer overlying the first layer and including a second conductive material and a second insulating material; Including, electronic components.

2. The electronic component of claim 1 , wherein the first insulating material and the second insulating material are glass.

3. The electronic component according to claim 1 , wherein the first insulating material is glass and the second insulating material is a resin.

4. The electronic component according to claim 1 , further comprising a plating layer covering the external electrode layer.

5. providing a component body having an end surface; forming an external electrode layer that covers the end face of the component body and an edge portion on the end face side; Including, The step of forming the external electrode layer includes: forming a first layer covering the end surface and the edge portion, the first layer including a first conductive material and a first insulating material; forming a second layer overlying the first layer, the second layer including a second conductive material and a second insulating material; A method for manufacturing an electronic component, comprising:

6. forming the first layer includes a heat treatment; The method for manufacturing an electronic component according to claim 5 , wherein the step of forming the second layer includes the step of forming the second layer so as to cover the first layer after the heat treatment.

Citation Information

Patent Citations

  • Outer electrode of electronic part

    JP1997190950A

  • External electrode of chip electronic component

    JP1998163067A

  • Electronic component equipped having external terminal electrode and mounting electronic article thereof

    JP2001155955A

  • Power storage device

    JP2019004099A

  • Multilayer ceramic capacitor

    JP2019083291A