Spectacle lens, method of fabricating spectacle lens, and insert molding film for spectacle lens
By embedding a film with an ultraviolet absorber between lens elements and using a curable composition, the method addresses compatibility issues in eyeglass lens manufacturing, enabling stable production of lenses with effective UV absorption.
Patent Information
- Application Number
- JP2023058220
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing methods for imparting ultraviolet absorption to eyeglass lenses face challenges such as compatibility issues between the base resin and ultraviolet absorbers, leading to difficulties in achieving uniform distribution and stability during polymerization.
Incorporating a film containing an ultraviolet absorber between two lens elements of the eyeglass lens, which is molded using a curable composition to form a spectacle lens with the absorber embedded within.
The method allows for the stable production of eyeglass lenses with ultraviolet absorption functionality without relying on the base material's composition, ensuring uniform distribution and improved manufacturing stability.
Smart Images

Figure 2024145738000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a spectacle lens, a method for manufacturing a spectacle lens, and a film for insert molding of a spectacle lens. [Background technology]
[0002] Optical components such as eyeglass lenses are required to cut ultraviolet rays (wavelength range of 400 nm or less) from sunlight to protect the eyes. In addition, by cutting light rays in the blue region (wavelength range of 380 to 500 nm) in optical components such as eyeglass lenses, glare is reduced and visibility and contrast are improved. In addition, light rays in the blue region (380 to 500 nm) have high energy and are considered to cause damage to the retina and other parts of the eye, which is harmful to eye health. Damage caused by blue light is called "blue light hazard," and light around 420 nm on the low wavelength side is particularly dangerous, so it is considered desirable to cut light in this region.
[0003] Patent Document 1 describes a highly light-resistant plastic lens that is impregnated or transferred with an ultraviolet absorber, and a method for producing the same, with the aim of preventing a decrease in mechanical properties, i.e., strength, and coloring of the material itself due to stabilizers. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-105772 Summary of the Invention [Problem to be solved by the invention]
[0005] For example, a method for imparting ultraviolet absorbing functionality to a spectacle lens includes a method in which an ultraviolet absorber is added to a resin before curing, and the resin is molded and polymerized in a mold to obtain a spectacle lens base material containing the ultraviolet absorber.
[0006] However, depending on the compatibility between the base resin and the UV absorbent, it can be difficult to dissolve them to obtain a uniform resin, or the UV absorbent can react and change during molding and polymerization, which can cause problems.
[0007] Therefore, one embodiment of the present disclosure relates to a spectacle lens that has an ultraviolet absorbing function and can be stably produced regardless of the material of the substrate, a method for producing a spectacle lens, and a film for insert molding of a spectacle lens. [Means for solving the problem]
[0008] The present inventors have discovered that the above-mentioned problems can be solved by introducing a film containing an ultraviolet absorbing agent into the substrate of a spectacle lens.
[0009] One embodiment of the present disclosure includes: a first lens element portion forming an object-side surface; a second lens element forming an eye-facing surface; and a film provided between the first lens element portion and the second lens element portion; Equipped with The present invention relates to a spectacle lens, wherein the film contains an ultraviolet absorbing agent.
[0010] One embodiment of the present disclosure includes: Providing a mold having a cavity with a film containing an ultraviolet absorbing agent disposed therein; injecting a hardenable composition into the cavity; and obtaining a spectacle lens having a film disposed therein by curing the curable composition; The present invention relates to a method for manufacturing a spectacle lens,
[0011] One embodiment of the present disclosure includes: The present invention relates to a film for insert molding of eyeglass lenses, which contains an ultraviolet absorbing agent. Effect of the Invention
[0012] According to one embodiment of the present disclosure, it is possible to provide a spectacle lens that has an ultraviolet absorbing function and can be stably produced independently of the material of the substrate, a method for producing a spectacle lens, and a film for insert molding of a spectacle lens. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a cross-sectional view of a spectacle lens 100 of the present embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of a spectacle lens 100a of this embodiment having a minus power. [Diagram 3] FIG. 3 is a cross-sectional view of a spectacle lens 100b of this embodiment having a plus power. [Figure 4] FIG. 4 is a flowchart showing an outline of the method for manufacturing a spectacle lens according to this embodiment. [Diagram 5] FIG. 5 is a schematic diagram of a curved surface processing table equipped with a male mold having a spherical molding surface. [Figure 6] FIG. 6 is a schematic cross-sectional view of upper mold 16, dried film 14, and lower mold 18. As shown in FIG. [Figure 7] FIG. 7 is a plan view showing a state in which a holding member 20 made of an adhesive for holding the film 14 is formed on the upper mold 16. As shown in FIG. [Figure 8] FIG. 8 is a schematic cross-sectional view taken along line AA' in a state in which holding member 20 made of adhesive for holding film 14 on upper mold 16 has been formed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present disclosure (hereinafter referred to as "the present embodiment") will be described in detail with reference to the drawings as necessary, but the present invention is not limited thereto, and various modifications are possible without departing from the gist of the present invention. In addition, in the drawings, the same elements are given the same reference numerals, and duplicated explanations are omitted. Furthermore, positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings, unless otherwise specified. Furthermore, the dimensional ratios of the drawings are not limited to those shown in the drawings.
[0015] [Eyeglass lenses] The spectacle lens according to the present embodiment includes a first lens element forming an object side surface, a second lens element forming an eyeball side surface, and a film provided between the first lens element and the second lens element, the film containing an ultraviolet absorbing agent. According to the above-mentioned embodiment, it is possible to provide a spectacle lens having an ultraviolet absorbing function and capable of being stably manufactured independently of the material of the substrate, a manufacturing method for a spectacle lens, and a film for insert molding of a spectacle lens.
[0016] In this disclosure, various terms have the following meanings: The "object-side surface" refers to a surface that is located on the object side when a wearer wears spectacles equipped with the spectacle lens, and the "eyeball-side surface" refers to the opposite, that is, a surface that is located on the eyeball side when a wearer wears spectacles equipped with the spectacle lens. Regarding the surface shape, in one embodiment, the object-side surface is a convex surface, and the eyeball-side surface is a concave surface. However, the present invention is not limited to this embodiment.
[0017] FIG. 1 is a cross-sectional view of a spectacle lens 100 of this embodiment. As shown in FIG. 1, the spectacle lens 100 of this embodiment is a plastic lens having a meniscus shape, and includes a lens substrate having a first lens element portion 110, a second lens element portion 120, and a curved film 14 between the first and second lens element portions. The first lens element portion 110 is provided on an object side surface 111 (convex side) of the spectacle lens 100 with respect to the film 14, and the second lens element portion 120 is provided on an eyeball side surface 121 (concave side) of the spectacle lens 100. Both the first lens element portion 110 and the second lens element portion 120 have a meniscus shape, and in the first lens element portion 110, the object side is the object side surface 111 of the spectacle lens 100, and the eyeball side is the surface that abuts against the film 14. Similarly, in the second lens element portion 120 , the eyeball side is the eyeball side surface 121 of the spectacle lens 100 , and the object side is the surface that abuts against the film 14 .
[0018] The film 14 embedded inside the eyeglass lens 100 may be, for example, a commercially available iodine-based film that has been curved to a predetermined curvature by press molding to correspond to the lens shape and cut into a circular outer shape. Details of the curved surface processing will be described later.
[0019] The minimum value W1 of the distance between the object-side surface 111 of the eyeglass lens 100 and the film 14 is preferably 0.3 mm or more and 0.7 mm or less. The position at which the minimum value W1 occurs varies depending on the shape of the eyeglass lens based on the lens prescription, etc. In other words, in the case of a lens with minus power, the lens thickness increases in the direction from the center to the periphery, and in the case of a lens with plus power, the opposite is true.
[0020] FIG. 2 is a cross-sectional view of a spectacle lens 100a of this embodiment having a negative power. The spectacle lens 100a shown in FIG. 2 is a single-focus lens with a base curve of 2 base, a curvature of the film 14 of 3 base, and a prescription power of negative power. In the spectacle lens 100a having a negative power, the distance between the apex T at the center of the object-side surface 111 and the film 14 is the above-mentioned minimum value W1, and the distance between the apex T and the film 14 is 0.05 mm or more and 2.0 mm or less. In the case of a spherical design, the apex T is the geometric center and also the optical center.
[0021] In general, eyeglass lenses having a film tend to be thick overall. For example, the eyeglass lens 100a shown in FIG. 2 has a curved surface on the eyeball-side surface 121, and has a structure in which the thickness of the eyeglass lens is the thinnest at the optical center and the thickest at the periphery. The eyeglass lens 100a cannot be made thinner than the thickness from the object-side surface 111 to the position of the film. In other words, the thickness of the eyeglass lens 100a at its thinnest optical center is limited to the thickness from the object-side surface 111 to the position of the film 14. Furthermore, the thickness of the periphery becomes more noticeable with the thickness of the optical center, giving the eyeglass lens an overall thick impression. From this perspective, it is preferable that the film 14 is located as close as possible to the object-side surface of the eyeglass lens. Therefore, by processing the film into a curved surface, the film can be located as close as possible to the object-side surface even at the center of the eyeglass lens, making the thickness of the center thinner.
[0022] FIG. 3 is a cross-sectional view of a spectacle lens 100b of this embodiment having a positive power. The spectacle lens 100b shown in FIG. 3 is a single-focus lens with a base curve of 10 base, a curvature of the film 14 of 8 base, and a prescription power of a positive power. In the lens 100b having a positive power, the distance between the film 14 and the outer periphery is the above-mentioned minimum value W1, and the distance between the outer periphery and the film 14 is 0.05 mm or more and 2.0 mm or less. The minimum value W1 is preferably 0.1 mm or more and 1.0 mm or less, more preferably 0.3 mm or more and 0.7 mm or less, and even more preferably 0.2 mm or more and 0.6 mm or less.
[0023] In a type of eyeglass lens in which a film is sandwiched between two lens element portions as shown in Fig. 1, the refracting surface of object-side surface 111 of first lens element portion 110 is preferably a rotationally symmetric surface, and more preferably a spherical surface, because this makes it easier to manufacture the mold and create the curved surface of the film.
[0024] <Film> The film in this embodiment contains an ultraviolet absorbing agent, which preferably has a maximum absorption wavelength of 345 nm or more in a chloroform solution.
[0025] As described herein, the film is a film for insert molding of a spectacle lens. The film may have a lens spherical curved surface in accordance with the shape of the spectacle lens in order to be insert molded into the base material of the spectacle lens.
[0026] Examples of the ultraviolet absorbent include benzophenone compounds, benzotriazole compounds, dibenzoylmethane, and 4-tert-butyl-4'-methoxybenzoylmethane.
[0027] Examples of benzophenone compounds include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid, 2-hydroxy-4-n-octoxybenzophenone, 2-hydroxy-4-n-dodecyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, and 2,2'-dihydroxy-4-methoxybenzophenone.
[0028] Benzotriazole compounds include, for example, 2-ethylhexyl Benzotriazole compounds such as 2-(2-hydroxy-4-ethoxyphenyl)-2H-benzotriazole-5-carboxylate, 2-(2-hydroxy-5-methylphenyl)-2H-benzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)-5-chloro-2H-benzotriazole, 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chloro-2H-benzotriazole, 2-(2-hydroxy-3,5-di-tert-amylphenyl)-2H-benzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)-2H-benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)-2H-benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)-2H-benzotriazole and 2-(2-hydroxy-4-octyloxyphenyl)-2H-benzotriazole are included. These may be used alone or in combination of two or more.
[0029] The amount of the ultraviolet absorber added is preferably 0.01 mass % to 5 mass %, more preferably 0.05 mass % to 3 mass %, even more preferably 0.1 mass % to 2 mass %, even more preferably 0.3 mass % to 2 mass %, even more preferably 0.5 mass % to 2 mass %, and even more preferably 0.8 mass % to 2 mass % or less, relative to the total weight of the film.
[0030] The film may contain a resin such as polyvinyl alcohol (hereinafter, also simply referred to as "PVA") or polyethylene terephthalate (hereinafter, also simply referred to as "PET"). Among these resins, PVA is preferable. PVA is preferable as a material for the film because of its excellent transparency and heat resistance. For example, the film may be a film in which an ultraviolet absorbing agent is impregnated into the resin of the film, or a film in which an ultraviolet absorbing agent is kneaded into the resin.
[0031] The content of PVA is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, based on the total mass of the film. The upper limit of the content of PVA is not particularly limited, but may be, for example, 100% by mass or less, based on the total mass of the film.
[0032] The film may have a protective layer on one or both sides thereof, for example, a film containing triacetyl cellulose (hereinafter also referred to as "TAC").
[0033] The polarization degree of the film is preferably 40% or less, more preferably 20% or less, even more preferably 10% or less, and even more preferably 5% or less. The lower limit of the polarization degree of the film is not particularly limited, but is, for example, 0% or more. The polarization degree can be measured by the method described in the examples.
[0034] The thickness of the film is preferably such that the film can be curved, but is not particularly limited and is preferably 10 μm to 90 μm, more preferably 15 μm to 80 μm, even more preferably 18 μm to 60 μm, and even more preferably 20 μm to 50 μm. A thickness of 10 μm or more provides high rigidity and ease of handling, while a thickness of 90 μm or less facilitates curved processing of the film.
[0035] The ratio of the minimum thickness of the film to the minimum thickness of first lens element 110 (minimum thickness of film / minimum thickness of first lens element) is preferably 0.10 to 1.25, more preferably 0.15 to 1.00, and even more preferably 0.20 to 0.85. By achieving such a relationship, even when the eyeglass lens is elastically deformed, the conformability of the film is improved and whitening of the film can be prevented.
[0036] The ratio of the minimum thickness of the film to the minimum thickness of the second lens element 120 (minimum thickness of film / minimum thickness of first lens element) is preferably 0.002 to 0.060, more preferably 0.005 to 0.055, and even more preferably 0.02 to 0.05. By achieving such a relationship, even when the eyeglass lens is elastically deformed, the conformability of the film is improved and whitening of the film can be prevented.
[0037] The spectacle lenses may be either finished lenses or semi-finished lenses. The spectacle lens may be any of a single-focus lens, a multifocal lens, a progressive-power lens, etc. For example, in the case of a progressive-power lens, the near area (near area) and the progressive area (intermediate area) are usually included in the lower area, and the distance area (distance area) is included in the upper area. As the spectacle lenses, colorless ones are usually used, but colored ones can also be used as long as the transparency is not impaired.
[0038] The thickness and diameter of the substrate of the eyeglass lens are not particularly limited, but the thickness is usually about 1 to 30 mm, and the diameter is usually about 50 to 100 mm. The refractive index ne of the spectacle lens substrate is preferably 1.50 or more, more preferably 1.50 to 1.80, even more preferably 1.53 to 1.70, even more preferably 1.55 to 1.67, and even more preferably 1.55 to 1.60.
[0039] The resin contained in the first lens element portion 110 and the second lens element portion 120 in the eyeglass lens according to this embodiment preferably has a glass transition temperature. The glass transition temperature is preferably 75° C. to 85° C., more preferably 75° C. to 83° C., and even more preferably 78° C. to 83° C. If the glass transition temperature of the resin is within this range, the eyeglass lens is easily elastically deformed, but in the eyeglass lens according to this embodiment, by using a film made of a material such as polyvinyl alcohol, it is possible to follow the elastic deformation of the eyeglass lens and prevent problems such as whitening.
[0040] The glass transition temperature in this embodiment can be measured by the following thermomechanical analysis method (TMA method). (Thermomechanical analysis method) The glass transition temperature is measured by applying a load of 98 mN to a needle probe (tip diameter 0.5 to 1.0 mm) and measuring the displacement of the sample. Measurements are performed by heating a φ5 mm x 3 mm sample from room temperature at a rate of 10°C / min and measuring the displacement of the sample with a thermomechanical analyzer. Normally, samples become larger due to thermal expansion as the temperature increases. However, near the glass transition temperature, the measured value may indicate that the sample changes from expansion to contraction. This phenomenon occurs when the sample can no longer withstand the load and the needle probe sinks into the sample, and this peak top temperature is taken as the glass transition temperature Tg. If the peak top is not clear, the temperature at the point where the tangents before and after the measured value near the peak top intersect is taken as the glass transition temperature.
[0041] The resin contained in the first lens element portion 110 and the second lens element portion 120 in the eyeglass lens of this embodiment may be a reactive curable composition that hardens by polymerization or the like, or a composition containing a molten thermoplastic resin that becomes a phase transition type curable composition upon cooling.
[0042] The curable composition may be, for example, a composition containing a resin monomer. The resin may be, for example, a polyurethane-based resin such as a polythiourethane resin or a polyurethane resin; an epithio-based resin such as a polysulfide resin; or an addition polymerization resin such as diethylene glycol bisallyl carbonate. The phase-transition curable composition may be, for example, a polycarbonate-based resin.
[0043] (addition polymer resin) First lens element 110 and second lens element 120 preferably comprise an addition polymer. The addition polymer is (i) a polymer of diethylene glycol bisallyl carbonate, and (ii) Copolymer of diethylene glycol bisallyl carbonate and divinylbenzene dicarboxylate It is preferable that the composition contains at least one selected from the following: The addition polymer is, for example, a cured product of the following addition polymerizable composition.
[0044] The addition polymerizable composition may contain various monomers in addition to diethylene glycol bisallyl carbonate and divinylbenzene dicarboxylate. The monomer preferably contains a monomer having two or more polymerizable unsaturated bonds in the molecule in order to obtain a three-dimensionally crosslinked optical resin. Examples of the polymerizable unsaturated bond include a (meth)acrylate group, an allyl group, a vinyl group, etc. The (meth)acrylate group is at least one selected from the group consisting of a methacrylate group and an acrylate group. Among these, at least one selected from the group consisting of a methacrylate group and an allyl group is preferable.
[0045] The monomer having two or more polymerizable unsaturated bonds in the molecule preferably includes diethylene glycol bisallyl carbonate, and more preferably includes diethylene glycol bisallyl carbonate, benzyl methacrylate, diallyl phthalate, and alkyl methacrylate having an alkyl group with 1 to 4 carbon atoms.
[0046] The amount of diethylene glycol bisallyl carbonate, based on the total amount of monomers, is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and is preferably 100% by mass or less, more preferably 80% by mass or less, even more preferably 50% by mass or less, even more preferably 40% by mass or less.
[0047] When used in combination with benzyl methacrylate, diallyl phthalate, and an alkyl methacrylate having an alkyl group with 1 to 4 carbon atoms, the amount of diethylene glycol bisallyl carbonate blended is more preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and more preferably 40% by mass or less, more preferably 35% by mass or less, based on the total amount of monomers.
[0048] The amount of benzyl methacrylate to be blended is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, based on the total amount of monomers. % by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less.
[0049] The diallyl phthalate may be one or two selected from the group consisting of diallyl isophthalate and diallyl terephthalate.
[0050] The amount of diallyl phthalate blended is preferably 14% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, based on the total amount of monomers, and is preferably 88% by mass or less, more preferably 70% by mass or less, even more preferably 60% by mass or less.
[0051] Examples of alkyl methacrylates having an alkyl group with 1 to 4 carbon atoms include at least one selected from the group consisting of methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, iso-propyl methacrylate, n-butyl methacrylate, sec-butyl methacrylate, iso-butyl methacrylate, and tert-butyl methacrylate.
[0052] The amount of alkyl methacrylate blended is preferably 1 mass % or more, more preferably 2 mass % or more, and even more preferably 3 mass % or more, based on the total amount of monomers, and is preferably 6 mass % or less, and more preferably 5 mass % or less.
[0053] Examples of the radical initiator used in the polymerization include 1,1-azobiscyclohexane carbonate, diisopropyl peroxycarbonate, 1,1'-azobiscyclohexane nitrate, and di-tert-butyl peroxide.
[0054] The amount of the radical initiator is preferably 0.1 part by mass or more, more preferably 0.5 part by mass or more, and even more preferably 1.0 part by mass or more, relative to 100 parts by mass of the monomer, and is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 5 parts by mass or less.
[0055] The luminous transmittance of the entire eyeglass lens according to this embodiment is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. The upper limit of the luminous transmittance of the entire eyeglass lens is not particularly limited, but may be, for example, 100% or less, or 98% or less. The luminous transmittance of the entire eyeglass lens means the luminous transmittance of the entire lens including the functional layer, if the lens has a functional layer. The luminous transmittance is measured according to JIS T7333:2005.
[0056] The degree of polarization of the entire eyeglass lens according to this embodiment may be 40% or less. The degree of polarization of the entire eyeglass lens may be 30% or less, 20% or less, 10% or less, or 5% or less. The degree of polarization can be measured by the method described in the examples.
[0057] The transmittance of light at 400 nm in the entire eyeglass lens according to this embodiment is preferably 40% or less, more preferably 30% or less, and even more preferably 20% or less.
[0058] From the viewpoint of reducing blue light hazard, the transmittance of light having a wavelength of 410 nm through the entire spectacle lens according to this embodiment is preferably 5% or less, more preferably 3% or less, and even more preferably 1.0% or less. The transmittance of light having a wavelength of 410 nm through the entire spectacle lens is not particularly limited to a lower limit, but is, for example, 0.0% or more.
[0059] The transmittance of light of each wavelength through the entire eyeglass lens means the transmittance of the entire lens including the functional layer if the lens has a functional layer. The transmittance of light of each wavelength is measured using a spectrophotometer "U-4100" (product name, manufactured by Hitachi, Ltd.).
[0060] <Functional layer> The eyeglass lens may have a functional layer. Examples of the functional layer include a hard coat layer, a base layer, an anti-reflection layer, an infrared absorbing layer, a photochromic layer, an antistatic layer, and an anti-fogging layer. These functional layers may be used alone or in combination of two or more. For these functional layers, known techniques related to eyeglass lenses can be applied. Among these, it is preferable to have a hard coat layer, a base layer, and an anti-reflection layer.
[0061] (Hard coat layer) The hard coat layer is, for example, a cured film of a hard coat composition containing an inorganic oxide and a silicon compound. The hard coat composition preferably further contains a polyfunctional epoxy compound.
[0062] Examples of inorganic oxides include silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, tungsten oxide, zinc oxide, tin oxide, beryllium oxide, antimony oxide, and composite oxides of two or more of these inorganic oxides. These may be used alone or in combination of two or more. Among these inorganic oxides, silicon oxide is preferred. In addition, colloidal silica may be used as the inorganic oxide.
[0063] The content of the inorganic oxide in the solid content of the hard coat composition is preferably 20% by mass or more and 80% by mass or less, more preferably 25% by mass or more and 70% by mass or less, and even more preferably 25% by mass or more and 50% by mass or less.
[0064] The silicon compound is, for example, a silicon compound having a hydrolyzable group such as an alkoxy group. The silicon compound is preferably a silane coupling agent having an organic group and a hydrolyzable group bonded to a silicon atom. The organic group bonded to a silicon atom is preferably an organic group having a functional group such as an epoxy group such as a glycidoxy group, a vinyl group, a methacryloxy group, an acryloxy group, a mercapto group, an amino group, or a phenyl group, and more preferably an organic group having an epoxy group. The silicon compound may have an alkyl group bonded to silicon.
[0065] Examples of commercially available products of the above-mentioned silane coupling agents include those manufactured by Shin-Etsu Chemical Co., Ltd. under the product names KBM-303, KBM-402, KBM-403, KBE-402, KBE-403, KBM-1403, KBM-502, KBM-503, KBE-502, KBE-503, KBM-5103, KBM-602, KBM-603, KBM-903, KBE-903, KBE-9103, KBM-573, KBM-575, KBM-9659, KBE-585, KBM-802, KBM-803, KBE-846, and KBE-9007.
[0066] The content of the silicon compound is preferably 20% by mass or more and 90% by mass or less, more preferably 30% by mass or more and 75% by mass or less, and even more preferably 50% by mass or more and 75% by mass or less, of the solid content of the hard coat composition.
[0067] The polyfunctional epoxy compound is a polyfunctional epoxy compound containing two or more epoxy groups in one molecule, more preferably a polyfunctional epoxy compound containing two or three epoxy groups in one molecule. Commercially available polyfunctional epoxy compounds include EX-201, EX-211, EX-212, EX-252, EX-313, EX-314, EX-321, EX-411, EX-421, EX-512, EX-521, EX-611, EX-612, EX-614, and EX-614B of the "Denacol" series manufactured by Nagase ChemteX Corporation.
[0068] The content of the polyfunctional epoxy compound is preferably from 0 to 50% by mass, more preferably from 10 to 40% by mass, and even more preferably from 15 to 30% by mass, of the solid content of the hard coat composition.
[0069] The above-mentioned hard coat composition can be prepared by mixing optional components such as an organic solvent, a leveling agent, a curing catalyst, etc., in addition to the components described above, as necessary. The above-mentioned hard coat layer can be formed by applying a curable composition onto a substrate and subjecting it to a curing treatment (thermal curing, photocuring, etc.). As a means for applying the curable composition, a commonly used method such as a dipping method, a spin coating method, a spraying method, etc. can be applied. The curing treatment is usually performed by heating for a curable composition containing a multifunctional epoxy compound. The heat curing treatment can be performed, for example, by placing the lens coated with the above-mentioned curable composition in an environment with an atmospheric temperature of 50 to 150°C for about 30 minutes to 3 hours.
[0070] (base layer) The above-mentioned undercoat layer can be formed, for example, from a water-based resin composition containing at least one type of resin particles selected from the group consisting of polyurethane resin, acrylic resin, epoxy resin, and the like.
[0071] As the above-mentioned aqueous resin composition, commercially available aqueous polyurethane can be used as it is, or diluted with an aqueous solvent as necessary. Examples of commercially available aqueous polyurethane include the "Evaphanol" series manufactured by NICCA Chemical Co., Ltd., the "Superflex" series manufactured by Daiichi Kogyo Seiyaku Co., Ltd., the "Adeka Bonditer" series manufactured by ADEKA Corporation, the "Olestar" series manufactured by Mitsui Chemicals, Inc., the "Bondic" series and the "Hydran" series manufactured by Dainippon Ink and Chemicals, Inc., the "Impranil" series manufactured by Bayer, the "Sofranate" series manufactured by Nippon Soflan Co., Ltd., the "Poise" series manufactured by Kao Corporation, the "Sanprene" series manufactured by Sanyo Chemical Industries, Ltd., the "Iselax" series manufactured by Hodogaya Chemical Co., Ltd., and the "Neolet" series manufactured by Zeneka Co., Ltd.
[0072] The undercoat layer can be formed, for example, by applying the above-mentioned aqueous resin composition to the surface of the substrate and drying it.
[0073] (Anti-reflection layer) The antireflection layer has, for example, low refractive index layers and high refractive index layers arranged alternately. The number of layers in the antireflection layer is preferably 4 to 11 layers, and more preferably 5 to 8 layers.
[0074] The refractive index of the low refractive index layer is preferably 1.35 to 1.80, more preferably 1.45 to 1.50, at a wavelength of 500 to 550 nm. The low refractive index layer is made of an inorganic oxide, and is preferably made of silicon oxide.
[0075] The refractive index of the high refractive index layer is preferably 1.90 to 2.60, more preferably 2.00 to 2.40, at a wavelength of 500 to 550 nm. The high refractive index layer is made of, for example, an inorganic oxide. The inorganic oxide used in the high refractive index layer is preferably at least one selected from the group consisting of zirconium oxide, tantalum oxide, yttrium oxide, titanium oxide, niobium oxide, and aluminum oxide, more preferably at least one selected from the group consisting of zirconium oxide and tantalum oxide.
[0076] The anti-reflection layer can be formed by alternately laminating low refractive index layers and high refractive index layers by vacuum deposition.
[0077] [Method of manufacturing eyeglass lenses] Next, the method for manufacturing a spectacle lens according to the present embodiment will be described with reference to the drawings.
[0078] FIG. 4 is a flowchart showing an outline of the method for manufacturing a spectacle lens according to this embodiment. The manufacturing method for the eyeglass lens 100 of this embodiment includes the steps of preparing a film 14 containing an ultraviolet absorber, processing the film 14 into a curved surface, preparing a mold having a cavity with the film 14 disposed therein, injecting a curable composition into the cavity, curing the curable composition to obtain the eyeglass lens 100 with the film 14 disposed therein, and annealing the eyeglass lens 100. The manufacturing method for the eyeglass lens 100 of this embodiment preferably includes the steps described above in the above order. Although not shown, when manufacturing a semi-finished lens, the eyeball side surface 121 of the annealed eyeglass lens 100 may be ground and polished according to a prescription. Thereafter, a step of forming a functional layer on the surface of the eyeglass lens 100 may be included. The eyeglass lens is edged to a desired frame shape and framed.
[0079] <Preparation of film containing ultraviolet absorber> The film containing the ultraviolet absorbing agent can be produced by impregnating the ultraviolet absorbing agent into the film or by kneading the ultraviolet absorbing agent into the film.
[0080] (Impregnation of film with UV absorbent) By impregnating the film with an ultraviolet absorbing agent, a film containing the ultraviolet absorbing agent can be obtained. The impregnation of the film may be performed by a method including a step of immersing the film in an impregnation liquid containing an ultraviolet absorbent. The impregnation liquid may contain, for example, an ultraviolet absorbent, a dispersant, and water. Examples of commercially available products used as dispersants include "Nikka Sunsalt 7000" (trade name), available from Nicca Chemical Co., Ltd.
[0081] (Incorporating UV absorbers into film) By kneading an ultraviolet absorbing agent into the film, a film containing the ultraviolet absorbing agent can be obtained. The ultraviolet absorber may be kneaded into the film by a method including a step of kneading the ultraviolet absorber with a thermoplastic resin, and a step of forming the kneaded resin into a film. Examples of the thermoplastic resin include the above-mentioned polyvinyl alcohol and polyethylene terephthalate.
[0082] <Curved film processing> The film can be curved by any method as long as it can form the film into a desired curved shape. A preferred method is press molding. For example, the film is placed on a convex mold and pressed to transfer the convex shape to the film, thereby obtaining a film 14 having a curved shape.
[0083] The film may be moistened before the film is subjected to the curved surface processing. The moistening can be performed, for example, by leaving the film in a constant temperature and humidity device for a predetermined time, spraying mist of water onto the film, or the like, but the method is not particularly limited as long as it can increase the moisture content of the film. The moistening is usually performed in a heated atmosphere of about 50 to 90°C.
[0084] It is preferable to cool the wet film so that most of the absorbed water is retained in the film when it is curved. For example, the film can be cooled by leaving it at room temperature (about 20 to 25° C.) after being removed from the thermostatic chamber.
[0085] More specifically, a method for processing a film into a curved shape is to sandwich and press a flat sheet-like film in a press molding device equipped with a temperature adjustment unit (heater, cooling medium, etc.) and a pressure unit, and having a pair of molding dies, a male die and a female die, each having a spherical molding surface, and to curve the film into the shape of the molding surface.
[0086] 5 is a schematic diagram of a curved surface processing table equipped with a male mold having a spherical molding surface. The curved surface processing table 60 is equipped with a processing base portion 60a, a first male mold portion 61a having a spherical molding surface, and a second male mold portion 61b. In the figure, two male mold portions are shown, but the number is not particularly limited. The first male mold portion 61a and the second male mold portion 61b may be configured for eyeglass lenses for the left and right eyes.
[0087] The flat sheet film 10 is placed on the processing base 60a, and a female die (not shown) is pressed against it, for example, at room temperature (about 20 to 25° C.), thereby transferring the curved shape to the film, and processing the film 14 into a curved surface is performed.
[0088] The film 14 is preferably curved to correspond to the shape of the object-side surface 111. The curvature of the curved surface of the film 14 is preferably formed to correspond to the base curve of the object-side surface 111 of the eyeglass lens 100 to be manufactured. In the case where the prescription lens has a surface shape other than a spherical surface, such as a progressive lens or an aspheric lens, the curved surface may have a surface shape that matches the shape of the object-side surface 111. The curvature of the curved surface of the film 14 may be different from the base curve of the eyeglass lens 100, but in the case of a semi-finished lens, it may be different from the base curve of the object-side surface 111 of the eyeglass lens 100 to the extent that the eyeball-side surface 121 can be ground or polished.
[0089] The film 14 has a base curve, for example, of 1.0 base or more and 10.0 base or less. The base curve may be, for example, 2.0 base or more and 8.0 base or less. The absolute value of the difference between the base curve of the film 14 and the base curve of the object-side surface 111 of the eyeglass lens 100 is preferably 2.0 base or less, more preferably 1.5 base or less, and even more preferably 1.0 base or less.
[0090] <Film drying> In the manufacturing method of this embodiment, the film 100 after curved surface processing is dried. The drying temperature T1 is preferably higher than 120°C and lower than 160°C. By setting the temperature T1 to be higher than 120°C, deformation of the film can be prevented, and by setting the temperature T1 to be lower than 160°C, discoloration and cracks can be prevented from occurring in the film. The temperature T1 is preferably 125°C or higher and 155°C or lower, more preferably 130°C or higher and 150°C or lower, and even more preferably 135°C or higher and 145°C or lower.
[0091] In this embodiment, the drying temperature T1 refers to the temperature of the atmosphere in which the heat treatment for drying is performed. In this embodiment, in order to maintain the luminous transmittance of the film high, the shrinkage rate of the film is reduced, which results in significant deformation of the film, but the deformation of the film can be prevented by setting the temperature T1 to satisfy the condition of the formula (1) described below. The drying can be performed in the air.
[0092] As the drying method, various methods can be used, but a method of placing the film in a hot air circulating oven heated to the above temperature T1 and exposing it to hot air can be used. There is no particular limit to the drying time. In drying, the film may be removed from the curved mold and dried, or may be dried while still attached to the mold.
[0093] <Preparing the mold> The manufacturing method of this embodiment includes preparing a mold having a cavity in which a film is disposed. In the manufacturing method of this embodiment, a spectacle lens is manufactured using, for example, a cast polymerization method (casting method). The casting method is a method for obtaining a spectacle lens by curing a curable composition in a cavity formed by an upper mold, a lower mold, and a sealing member that adjusts the distance between the upper mold and the lower mold and determines the lens thickness.
[0094] 6 is a schematic cross-sectional view of the upper mold 16, the dried film 14, and the lower mold 18. The dried film 14 preferably has a diameter approximately 2 mm smaller than those of the upper mold 16 and the lower mold 18. This allows the curable composition to flow around both sides of the film 14 during injection of the curable composition, which will be described later, and allows the curable composition to be smoothly injected into the cavities.
[0095] Fig. 7 is a plan view showing a state in which holding member 20 made of adhesive for holding film 14 is formed on upper mold 16. Fig. 8 is a schematic cross-sectional view taken along line A-A' in a state in which holding member 20 made of adhesive for holding film 14 is formed on upper mold 16.
[0096] The upper mold 16 may have a flat flange portion 16a on its periphery. In FIG. 7, holding members 20a, 20b, 20c, and 20d for holding the film 14 are arranged at four positions at 90° intervals on the cavity side surface of the flange portion 16a of the upper mold 16. The holding members 20a, 20b, 20c, and 20d are for adhering and supporting the film, and the height and position of the adhesive columns are controlled so that the film can be held while maintaining a predetermined clearance (spacing) so that the film does not come into contact with the cavity side surface of the upper mold 16 when the film is placed on the holding members 20a, 20b, 20c, and 20d. Note that the eyeglass lens is cut to match the lens shape 300 of the eyeglass frame to be framed, so that the holding members 20 are configured not to remain in the eyeglass lens after the framing process. By using the holding members, the film 14 is held while maintaining a predetermined distance (hereinafter referred to as "clearance") without contacting the surface of the film 14 with the cavity side surface of the upper mold 16. The number of holding members is not particularly limited.
[0097] The minimum distance between the side surface of the cavity of the upper mold 16 and the film 14 is preferably 0.05 mm or more and 2.0 mm or less. The minimum distance is preferably 0.1 mm or more and 1.0 mm or less, more preferably 0.3 mm or more and 0.7 mm or less, and even more preferably 0.2 mm or more and 0.6 mm or less.
[0098] The holding member is an adhesive. The adhesive is preferably applied in the form of a column (cylinder, cube, etc.) or a block, preferably in the form of a column, on the periphery of the cavity side of the upper mold or on the periphery of the object side surface of the film.
[0099] Examples of materials for the upper and lower molds include glass, ceramic, metal, and resin. Among these, glass is preferable.
[0100] The upper mold usually has a concave surface (molding surface) that is placed on the cavity side, and the shape of this concave surface is transferred to form the convex refractive surface of the lens obtained by polymerization and hardening. When the upper mold is a glass mold, the molding surface of the upper mold is usually a mirror-finished surface that has been rough ground, sanded, polished, or the like.
[0101] On the other hand, the lower mold usually has a convex molding surface, and the shape of this convex surface is transferred to form the concave refractive surface of the lens obtained by polymerization and curing. The lower mold is usually processed in the same way as the above-mentioned upper mold.
[0102] As the sealing member, a gasket or a tape having an adhesive layer on one side (hereinafter referred to as "adhesive tape") can be used. When a gasket is used, the upper mold and the lower mold may be clamped and fixed with a clamp member made of an elastic body such as a spring. On the other hand, when an adhesive tape is used, a clamp member is usually not required.
[0103] Examples of the substrate for the adhesive tape include polyester films such as polyethylene terephthalate, polyolefin films such as polypropylene, polystyrene films such as ABS, polyimide, acetate, paper, cloth, and metal. Among these, polyethylene terephthalate and polypropylene are preferred.
[0104] The adhesive tape may have any shape as long as it can be wound around the upper and lower molds. The adhesive tape may have any thickness so long as it does not buckle when the mold is assembled, and is usually preferably less than 200 μm.
[0105] Examples of the adhesive of the adhesive tape include silicone-based adhesives, acrylic-based adhesives, and natural rubber-based adhesives. From the viewpoints of dissolving in the curable composition and heat resistance, silicone-based adhesives are preferred as the adhesive component.
[0106] For assembling the mold using the adhesive tape, various assembling methods used in the casting polymerization method for plastic lenses for glasses can be adopted. For example, it is preferable to arrange the upper mold 16, the film 14, and the lower mold 18 in this order with a space between them, and close the space between the upper mold 16 and the lower mold 18 with a seal member. For more details, see, for example, JP-A-2001-330806.
[0107] <Injection of hardenable composition> 10 is a schematic cross-sectional view of the molding die after assembly. A curable composition is injected into molding die 48. The curable composition is preferably filled into cavity 50 formed by upper mold 16, lower mold 18, and adhesive tape 46 using a syringe through an injection hole so that no air bubbles remain. The injection hole may be formed either between upper mold 16 and film 14, or between lower mold 18 and film 14.
[0108] <Curing of the curable composition> The mold 48 into which the curable composition has been poured is placed in a heating furnace and heated to cure the curable composition. The heating conditions can be determined depending on the type of the curable composition, and the temperature is raised to preferably 0° C. or higher and 150° C. or lower, more preferably 10° C. or higher and 130° C. or lower, and preferably 5 hours or higher and 50 hours or lower, more preferably 10 hours or higher and 25 hours or lower, for curing. After curing, a spectacle lens 100 is obtained in which the film 14 is disposed inside the substrate.
[0109] <Annealing of eyeglass lenses> The obtained eyeglass lens 100 may be annealed. In annealing an eyeglass lens, internal strain caused by the curing of the curable composition is usually removed. The annealing can be performed in the atmosphere.
[0110] The annealing temperature T2 is preferably 100° C. or higher and 130° C. or lower, more preferably 110° C. or higher and 125° C. or lower, and even more preferably 115° C. or higher and 125° C. or lower. When the temperature T2 is within this range, a spectacle lens with reduced astigmatism can be obtained. In this embodiment, the annealing temperature T2 refers to the temperature of the atmosphere in which a heat treatment for annealing the spectacle lens is performed.
[0111] As the annealing method, various methods can be adopted, but a method of treating in a heating furnace heated to the above temperature T2 can be used. There is no particular limit to the annealing time. The annealing may be performed after removing the eyeglass lens from the mold 48 after the curable composition is cured, or may be performed while the eyeglass lens is still set in the mold 48.
[0112] The forming mold 48 is removed from the heating furnace, the adhesive tape 46 is peeled off, and the mold is released from the upper mold 16 and the lower mold 18 to obtain a spectacle lens.
[0113] If the obtained eyeglass lens is a semi-finished lens, the eyeball side surface 121 of the eyeglass lens 100 can then be ground / polished using a curve generator and a polishing device to obtain a vision correcting eyeglass lens that matches the prescribed power.
[0114] (Formation of functional layer) The spectacle lens may be formed with the above-mentioned functional layers. Each layer may be formed by a known method such as the above-mentioned method.
[0115] According to the embodiments of the present disclosure described above, a spectacle lens having high luminous transmittance and degree of polarization, and low astigmatism can be obtained.
[0116] As described above, the present specification discloses the following embodiments. <1> a first lens element portion forming an object-side surface; a second lens element forming an eye-facing surface; and a film provided between the first lens element portion and the second lens element portion; Equipped with The spectacle lens, wherein the film contains an ultraviolet absorbing agent. <2> The film contains polyvinyl alcohol. <1> The eyeglass lens according to claim 1. <3> The thickness of the film is 10 μm to 90 μm. <1> or <2> The eyeglass lens according to claim 1. <4> The ratio of the minimum thickness of the film to the minimum thickness of the first lens element portion is 0.10 to 1.25. <1> ~ <3> 2. The eyeglass lens according to claim 1 . <5> the ratio of the minimum thickness of the film to the minimum thickness of the second lens element portion is 0.002 to 0.06; <1> ~ <4> 2. The eyeglass lens according to claim 1 . <6> The polarization degree of the film is 40% or less. <1> ~ <5> 2. The eyeglass lens according to claim 1 . <7> the first lens element portion and the second lens element portion comprise an addition polymer; <1> ~ <6> 2. The eyeglass lens according to claim 1 . <8> The addition polymer is (i) a polymer of diethylene glycol bisallyl carbonate, and (ii) Copolymer of diethylene glycol bisallyl carbonate and divinylbenzene dicarboxylate At least one selected from <1> ~ <7> 2. The eyeglass lens according to claim 1 . <9> The glass transition temperature of the resin contained in the first lens element portion and the second lens element portion is 75°C to 85°C. <1> ~ <8> 2. The eyeglass lens according to claim 1 . <10> The transmittance of the spectacle lens for light having a wavelength of 400 nm is 40% or less. <1> ~ <9> 2. The eyeglass lens according to claim 1 . <11> The luminous transmittance of the eyeglass lens is 80% or more. <1> ~ <10> 2. The eyeglass lens according to claim 1 . <12> Providing a mold having a cavity with a film containing an ultraviolet absorbing agent disposed therein; injecting a hardenable composition into the cavity; and obtaining a spectacle lens having a film disposed therein by curing the curable composition; A method for manufacturing a spectacle lens, comprising: <13> impregnating the film with an ultraviolet absorber to obtain a film containing the ultraviolet absorber; Further comprising: <12> A method for manufacturing a spectacle lens according to claim 1. <14> A film for insert molding of eyeglass lenses, containing an ultraviolet absorbing agent. <15> The film has a lens-like spherical curved surface. <14> The film according to claim 1. <16> The film contains polyvinyl alcohol. <14> or <15> The film according to claim 1. <17> The thickness of the film is 10 μm to 90 μm. <14> ~ <16> 13. The film according to any one of claims 1 to 12. <18> The polarization degree of the film is 40% or less. <14> ~ <17> 13. The film according to any one of claims 1 to 12. EXAMPLES
[0117] The present embodiment will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.
[0118] [Measurement method] <Luminous transmittance> The luminous transmittance was measured in accordance with JIS T7333:2005.
[0119] <Cutting rate at wavelengths of 400 nm and 410 nm> The sample was measured for light cut rates at wavelengths of 400 nm and 410 nm using a spectrophotometer "U-4100" (product name, manufactured by Hitachi, Ltd.).
[0120] <Polarization degree> Degree of polarization (P eff ) is measured in accordance with ISO8980-3 using a UV-Vis-NIR spectrophotometer "V-660" (manufactured by JASCO Corporation) to measure the luminous transmittance (T / / The luminous transmittance (T ⊥) when the transmission axis of the polarizing element is perpendicular to the light was calculated using the following formula. / / The optical transmittance (T⊥) and luminous transmittance (T⊥) were measured using a visible spectrophotometer and a polarizer (Glan-Thompson prism). The measurement light was incident on the object side surface of the eyeglass lens. P eff (%) = [(T / / -T⊥) / (T / / +T⊥)]×100
[0121] <Impact resistance> Impact resistance was evaluated using a drop ball test issued by the Food and Drug Administration (FDA). A 16g iron ball was dropped from a height of 127cm to impact the eyeglass lenses. If there was no damage, it was rated as A, and if there was damage, it was rated as B.
[0122] Example 1: Manufacturing of eyeglass lenses 1. Film A 40 μm thick polyvinyl alcohol film (hereinafter also referred to as "PVA film") was immersed in an impregnation solution prepared by dissolving 5.0 g of 2-ethylhexyl 2-(2-hydroxy-4-ethoxyphenyl) 2H-benzotriazole-5-carboxylate as an ultraviolet absorber and 50 mL of a dispersant ("Nikka Sunsalt 7000" product name, Nicca Chemical Co., Ltd.) in 1 L of water at 80° C. for 30 minutes. The obtained film was placed in a constant temperature and humidity device and moistened so that the moisture content at the start of curved surface processing was about 4%. The moistened film was left at room temperature (20 to 25°C) for about 2 minutes. Thereafter, curved surface processing was performed by the method described above with reference to Figure 5. Curved surface processing was also performed at room temperature. The curved film removed from the mold was then heated at 140°C for 65 minutes in a commercially available hot air circulating oven. After heating, adhesive columns were provided at four locations on the periphery of the side of the cavity of the upper mold. Then, a film was placed on the adhesive columns, and the upper mold and lower mold were closed with adhesive tape as a sealing member to assemble the mold. The surface shape of the upper mold and lower mold was spherical, with an inner diameter of 80 mm and a radius of curvature of 130.4 mm.
[0123] 2. Lens molding using the cast polymerization method and demolding As a raw material for the eyeglass lens substrate, 100 parts by mass of diethylene glycol bisallyl carbonate and 0.010 parts by mass of polyether modified silicone oil "DOWSIL L-7604" (product name, manufactured by Dow Toray Industries, Inc.) as an internal release agent were mixed and thoroughly stirred to completely disperse or dissolve the raw material for the eyeglass lens substrate. 5 parts by mass of diisopropyl peroxydicarbonate as a catalyst was then added to the raw material for the eyeglass lens substrate and thoroughly stirred at room temperature to obtain a homogeneous liquid. The composition was then degassed for 30 minutes while stirring under a reduced pressure of 5 mmHg, to prepare a curable composition. The prepared curable composition was poured into a mold 48 (base curve 2.50 base) in which the above-mentioned curved film was placed. Thereafter, the mold was placed in a heating furnace and held at 30°C for 7 hours, after which the temperature was raised from 30°C to 120°C over 10 hours for heat curing. After heat curing, the mold was removed from the heating furnace, the adhesive tape was peeled off, and the eyeglass lens was released from the upper mold and the lower mold to obtain an eyeglass lens. The obtained eyeglass lens was placed in a heating furnace and annealed at 120°C for 2 hours. The obtained spectacle lens was subjected to various physical properties measurement by the above-mentioned measurement method. The object side surface of the spectacle lens was designed to be spherical, and the geometric center of the object side surface was the intersection point between the perpendicular line passing through the center of the circle when the spectacle lens was viewed in a plan view and the eyeball side surface. Furthermore, the obtained spectacle lens was subjected to a ball drop test. The results are shown in Table 1. The cut rate for light with a wavelength of 410 nm was measured and found to be 0.1%.
[0124] Example 2: Manufacturing of eyeglass lenses As an ultraviolet absorbing agent, 0.5 g of 2-ethylhexyl 2-(2-hydroxy-4-ethoxyphenyl) 2H-benzotriazole-5-carboxylate and 30 g of polyvinyl alcohol were kneaded together to form a film having a thickness of 40 μm. The obtained film was placed in a constant temperature and humidity device and subjected to a moistening treatment, and was moistened so that the water content at the start of curved surface processing was about 4%. Except for this film, a spectacle lens was obtained in the same manner as in Example 1. The various physical properties of the obtained spectacle lens were measured by the above-mentioned measuring method. Furthermore, a drop ball test was performed on the obtained spectacle lens. The results are shown in Table 1. The cut rate for light with a wavelength of 410 nm was measured and found to be 0.1%.
[0125] <Production of Comparative Example 1> A spectacle lens was obtained in the same manner as in Example 1, except that 0.50 parts by mass of 2-ethylhexyl 2-(2-hydroxy-4-ethoxyphenyl) 2H-benzotriazole-5-carboxylate was added as an ultraviolet absorbing agent to the raw material of the spectacle lens substrate. The cut rate of light with a wavelength of 410 nm was measured and found to be 30%. Various physical properties of the obtained spectacle lens were measured using the above-mentioned measuring method. Furthermore, a drop ball test was performed on the obtained spectacle lens. The results are shown in Table 1.
[0126] [Table 1] [Explanation of symbols]
[0127] 14...film, 16...upper mold, 16a...flange portion, 18...lower mold, 20a, 20b, 20c, 20d...holding member, 46...adhesive tape, 48...molding die, 50...cavity, 100...spectacles lens, 110...first lens element portion, 111...object side surface, 120...second lens element portion, 121...eyeball side surface, 300: Target shape, W1: Minimum value
Claims
1. a first lens element portion forming an object-side surface; a second lens element forming an eye-side surface; and a film disposed between the first lens element portion and the second lens element portion; Equipped with The spectacle lens, wherein the film contains an ultraviolet absorbing agent.
2. The eyeglass lens of claim 1 , wherein the film comprises polyvinyl alcohol.
3. 2. The eyeglass lens according to claim 1, wherein the thickness of the film is from 10 μm to 90 μm.
4. 2. The spectacle lens according to claim 1, wherein a ratio of a minimum thickness of the film to a minimum thickness of the first lens element portion is 0.10 to 1.
25.
5. 2. The eyeglass lens according to claim 1, wherein a ratio of a minimum thickness of the film to a minimum thickness of the second lens element portion is 0.002 to 0.
06.
6. The eyeglass lens according to claim 1 , wherein the film has a polarization degree of 40% or less.
7. The spectacle lens of claim 1 , wherein the first lens element and the second lens element comprise an addition polymer.
8. The addition polymer is (i) a polymer of diethylene glycol bisallyl carbonate, and (ii) Copolymer of diethylene glycol bisallyl carbonate and divinylbenzene dicarboxylate The eyeglass lens according to claim 1 , comprising at least one selected from the following:
9. The eyeglass lens according to claim 1 , wherein the glass transition temperature of the resin contained in the first lens element portion and the second lens element portion is 75° C. to 85° C.
10. The eyeglass lens according to claim 1 , wherein the transmittance of the eyeglass lens for light with a wavelength of 400 nm is 40% or less.
11. The eyeglass lens according to claim 1 , wherein the luminous transmittance of the eyeglass lens is 80% or more.
12. Providing a mold having a cavity with a film containing an ultraviolet absorbing agent disposed therein; injecting a hardenable composition into the cavity; and obtaining a spectacle lens having a film disposed therein by curing the curable composition; A method for manufacturing a spectacle lens, comprising:
13. impregnating the film with an ultraviolet absorber to obtain a film containing the ultraviolet absorber; The method of claim 12 further comprising:
14. A film for insert molding of eyeglass lenses, containing an ultraviolet absorbing agent.
15. 15. The film of claim 14, wherein the film has a lenticular spherical curved surface.
16. 15. The film of claim 14, wherein the film comprises polyvinyl alcohol.
17. The film of claim 14, wherein the thickness of the film is from 10 μm to 90 μm.
18. 15. The film of claim 14, wherein the film has a polarization degree of 40% or less.
Citation Information
Patent Citations
Highly light-resistant plastic lens and its production
JP1993105772A