Air battery module
The air battery module addresses energy density and assembly challenges by using a laminated structure with a rigid positive electrode current collector plate and connecting pieces, ensuring even air distribution and precise cell connections, thus enhancing energy efficiency and longevity.
Patent Information
- Application Number
- JP2023058423
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing air battery modules face issues with reduced energy density due to increased housing and frame structures, uneven air flow, difficulty in assembling large modules, and misalignment of parts leading to capacity variations and electrolyte leakage.
The air battery module design includes a laminated structure with a positive electrode current collector plate having a conductive frame and connecting pieces that intersect the frame surface, enhancing rigidity and reducing part distortion during assembly, while ensuring even air distribution and precise cell connections.
This design maintains high energy density, suppresses part distortion, and ensures uniform air supply to each cell, reducing capacity and voltage differences, thereby extending battery life and improving assembly accuracy.
Smart Images

Figure 2024145873000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an air battery module, and more particularly to a battery pack in which a plurality of air batteries that utilize oxygen in the air are connected in series. [Background technology]
[0002] Air batteries use oxygen in the air as the positive electrode active material, and have the advantages of high energy density and ease of miniaturization and weight reduction. As an example of such air batteries, zinc-air primary batteries have been put to practical use in hearing aids and other devices. Furthermore, air secondary batteries, whose negative electrodes are made of metals such as Li, Zn, Al, and Mg, are expected to be developed as new secondary batteries with energy densities that exceed those of lithium-ion secondary batteries.
[0003] Furthermore, in order to put air secondary batteries into practical use, it is necessary to make battery modules by connecting battery cells in series or parallel in order to increase the battery voltage and capacity. Because air batteries require air (oxygen) for the discharge reaction, when they are made into a battery module, the battery module needs to be structured with a supply path for supplying air to each cell. Thus, as an example of an air battery module, a configuration has been proposed in which multiple air batteries are connected side by side inside a single housing (Patent Document 1).
[0004] Furthermore, a bipolar air battery module has been proposed as an example of a battery pack (Patent Document 2). In a bipolar air battery module, the negative electrode of one air battery cell and the positive electrode of the air battery cell adjacent to this cell are configured to be electrically connected through a wall material that separates the two air battery cells. This configuration has the advantages of low connection resistance between the cells, making it possible to achieve high energy density even on an actual cell basis, and allowing the battery capacity to be freely designed regardless of the case size. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-084650 A [Patent Document 2] JP 2014-194920 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, when multiple air batteries are arranged inside a single housing to create a module, the proportion of structures such as the housing and battery frame in the module increases, which tends to significantly reduce the actual energy density and cause uneven flow of air supplied to each battery cell. Thus, there are disadvantages such as the difficulty of assembling a large module due to limitations on the concentration of battery cells, and the limited freedom of design due to the fixed size of the housing.
[0007] In addition, because it is not possible to remove and replace only the battery cell in which an abnormality occurs in a bipolar battery module, high quality is required for the electrodes and other components. In particular, distortion of parts and misalignment of parts during assembly into the module can cause capacity variations in each battery cell and electrolyte leakage. Furthermore, increasing the number of stacked battery cells can cause instability in charging and discharging.
[0008] The present invention has been made in consideration of the above-mentioned problems, and its object is to provide an air battery module that has a simple structure, low connection resistance between components, and can suppress the occurrence of misalignment between components and distortion of components during assembly. [Means for solving the problem]
[0009] In order to achieve the above object, the air battery module of the present invention is an air battery module configured by connecting a plurality of air battery cells in series along one direction, and each of the plurality of air battery cells is configured by stacking a negative electrode current collector plate, a negative electrode plate, a separator, a positive electrode current collector plate supporting an air electrode, a water-repellent membrane, and a flow path plate along the one direction, and the positive electrode current collector plate has a conductive frame body that supports the air electrode and is electrically connected to the air electrode, and a conductive connection piece portion that is formed integrally with the frame body and extends in a direction intersecting a frame surface of the frame body and on the opposite side to the negative electrode current collector plate, and at least two of the connection pieces are formed so as to face each other across the air electrode supported by the frame body, and when the negative electrode side of a second air battery cell is connected to the positive electrode side of a first air battery cell among the plurality of air battery cells, the connection piece portion of the positive electrode current collector plate of the first air battery cell comes into contact with and is electrically connected to the negative electrode current collector plate of the second air battery cell. Effect of the Invention
[0010] In the air battery module of the present invention, the connection piece increases the rigidity of the positive current collector plate, which can suppress distortion of the positive current collector plate after the air electrode is attached to the frame. Also, distortion of the positive current collector plate when connecting the negative electrode side of the second air battery cell to the positive electrode side of the first air battery cell is reduced, improving assembly accuracy. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a perspective view showing an air battery module according to an embodiment. [Diagram 2] FIG. 2 is an exploded perspective view of one air secondary battery cell. [Diagram 3] FIG. 4 is a plan view showing an example of an air electrode welded to a positive electrode current collector plate. [Figure 4] FIG. 11 is a diagram illustrating the electrical connection between the positive electrode collector plate of one battery cell and the negative electrode collector plate of the other battery cell in two battery cells adjacent in the stacking direction, where (a) is an exploded view and (b) is a cross-sectional view. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an air battery module according to an embodiment will be described with reference to the drawings. 1. Battery cell configuration An air battery module is shown in Figure 1. The air battery module (hereinafter also referred to as "battery module") 1 comprises a battery set 3 in which 60 air secondary battery cells 2 (hereinafter also referred to as "battery cells") are arranged in a row along one direction A and connected in series, and a pair of clamping plates 4, 5 that sandwich both ends of the battery set 3.
[0013] Each battery cell 2 is stacked in the following order along direction A from the positive electrode side to the negative electrode side: gasket A11, flow path plate 12, water-repellent membrane 13, positive electrode current collector plate 15 supporting air electrode 14, separator 16, negative electrode plate 17, gasket B18, and negative electrode current collector plate 19.
[0014] The flow path plate 12 is made of a rectangular flat plate exhibiting electrical conductivity, and has a flow path through which air that is taken in from the outside of the battery module 1 and reacts with the air electrode 14 flows. The flow path communicates with an air supply port 20 that introduces air from the outside of the battery module 1, and communicates with an air outlet port 21 that discharges the air that has flowed through the flow path to the outside. For example, the flow path is formed in the flow path plate 12 as a corrugated plate by press molding a metal plate, as unevenness by mold pressing a resin material, or as a gas diffusion layer made of a porous material. The form of the flow path in the flow path plate 12 is an appropriate form that can supply air to the entire air electrode 14. In addition, a gasket A11 is attached so as to surround the flow path plate 12.
[0015] The water-repellent membrane 13 is located between the flow path plate 12 and the air electrode 14 to transfer air during charging and discharging, and also blocks the flow path to prevent the electrolyte in the battery cell 2 from leaking into the flow path. The water-repellent membrane 13 is a liquid-tight, breathable membrane made of a water-repellent microporous membrane such as PTFE. The water-repellent microporous membrane allows air to pass from the flow path side toward the air electrode 14, and prevents the electrolyte present on the air electrode 14 side from leaking into the flow path.
[0016] The air electrode 14 has a conductive substrate and an air electrode mixture layer made of an air electrode mixture (positive electrode mixture) held on the substrate, and is disposed in close contact with the water-repellent film 13. The air electrode mixture includes an oxidation-reduction catalyst for utilizing oxygen reduction and oxygen generation reactions, a conductive material, a binder, and a water-repellent material. The oxidation-reduction catalyst is one having a dual function of oxidation and reduction, and it is preferable to use pyrochlore-type bismuth ruthenium oxide. The air electrode 14 causes a reaction to reduce oxygen from air supplied through the water-repellent film 13 during discharge, and causes a reaction to generate oxygen from water during charge, and the generated oxygen passes through the water-repellent film 13 and is discharged to the flow path. Electrons generated in the air electrode 14 are collected on the positive electrode current collector 15. In order to reduce the resistance value of the air electrode 14, the substrate is preferably welded to the positive electrode current collector 15. The fabrication of the air electrode 14 will be described later.
[0017] The positive current collector 15 is made of a metal plate whose surface has been treated to be corrosion-resistant, and has a rectangular frame 15A. The frame 15A is formed by punching the inside of the metal plate to match the shape of the base of the air electrode 14, and each side of the frame 15A has a predetermined width. The outer edge 14A of the base of the air electrode 14 is welded to the inner edge of the frame 15A, and the frame 15A supports the air electrode 14. The thickness of the positive current collector 15 is preferably 0.1 mm to 0.3 mm, taking into consideration ease of processing, the energy density of the battery cell 2, and the internal resistance.
[0018] In addition, when the size of the battery cell 2 is large or the area of the air electrode 14 is large, the frame 15A of the positive electrode current collector plate 15 has a conductive beam 15B formed integrally with the center of the frame 15A in order to improve current collection from the air electrode 14, as shown in Fig. 2. The inside of the frame is divided into two by the beam 15B, and two openings 15D are provided, and each opening 15D accommodates an air electrode 14. The edge and inner edge of the beam 15B are each defined by a long side 15D. L The long side is 15D. L The inner edge of the frame 15A perpendicular to the short side 15D S Air electrode 14 housed in opening 15D of frame 15A is resistance-welded to frame 15A of positive current collector plate 15 and electrically connected to positive current collector plate 15.
[0019] Furthermore, the positive electrode current collector plate 15 has connection pieces 15C that are integral with the outer peripheral edge of the frame body 15A and that face each other across the beams 15B. The connection pieces 15C are formed by bending the outer peripheral edge of the frame body 15A in the same direction that intersects with the frame surface of the frame body 15A. In this embodiment, the connection pieces 15C are formed by bending the outer peripheral edge of the side of the frame body 15A to which the base of the air electrode 14 is welded at an angle of 60 degrees with respect to the in-plane direction of the frame body 15A over a width of 1 mm, as shown in FIG.
[0020] The separator 16 is disposed between the air electrode 14 and the negative electrode plate 17 to electrically insulate the air electrode 14 from the negative electrode plate 17. The separator 16 is made of, for example, a nonwoven fabric made of polyamide fiber or a nonwoven fabric made of polyolefin fiber, and contains an alkaline electrolyte such as a KOH solution inside. In this embodiment, the separator 16 has an overall rectangular shape. As shown in FIG. 2, the separator 16 may have a three-layer structure in which a hydrophilically treated PP microporous membrane 16A is sandwiched between nonwoven fabrics 16B on both sides.
[0021] The negative electrode plate 17 is composed of a conductive negative electrode core having a large number of pores, and a negative electrode mixture held in the pores and on the surface of the negative electrode core. For example, foamed nickel is used as the negative electrode core. The negative electrode mixture contains hydrogen storage alloy powder as a negative electrode active material, a conductive agent, and a binder. As the conductive agent, graphite, carbon black, etc. can be used. The preparation of the negative electrode plate 17 will be described later.
[0022] The negative electrode current collector 19 is made of a conductive metal plate with a corrosion-resistant surface and has a rectangular shape. The negative electrode current collector 19 is in contact with the negative electrode plate 17 to collect electrons. The separator 16 and the negative electrode plate 17 are housed inside a cylindrical gasket B18.
[0023] Furthermore, it is preferable to sandwich a plate 22 made of foamed nickel between the negative electrode plate 17 and the negative current collector plate 19 to improve current collection and to act as a dimensional relaxation material for the expansion and contraction of the electrode plate due to charging and discharging.
[0024] 2, in order to facilitate alignment when stacking the flow path plate 12, the positive current collector plate 15, and the negative current collector plate 19, notches C are provided at both ends in the longitudinal direction of the beam 15B of the positive current collector plate 15, and near the peripheral edges of the flow path plate 12 and the negative current collector plate 19 that correspond to both ends of the positive current collector plate 15 when stacked. In this embodiment, the flow path plate 12, the positive current collector plate 15, and the negative current collector plate 19 each have four U-shaped notches C.
[0025] Furthermore, an air supply port 20 and an air exhaust port 21 are formed penetrating the battery cell 2 in the stacking direction, the battery cell 2 being made up of gasket A11, flow path plate 12, water-repellent film 13, positive electrode current collector plate 15 supporting air electrode 14, gasket B18, and negative electrode current collector plate 19, which are stacked and positioned using cut C. The air supply port 20 communicates with air supply port 4A of one fastening plate 4 attached to one end side of the battery module 1. The air exhaust port 21 communicates with air exhaust port 5A of the other fastening plate 5 attached to the other end side of the battery module 1. The battery cell 2 has such a configuration.
[0026] 2. Manufacturing of battery cells and battery modules 1 The manufacture of the battery cell 2 and the battery module 1 in which a plurality of battery cells 2 are connected in series will be described below.
[0027] (1) Preparation of the air electrode The air electrode 14 is made of a pyrochlore-type metal oxide, Bi2Ru2O 7-Z was used.
[0028] Bi(NO3)3·5H2O and RuCl3·3H2O were added to a dilute nitric acid solution at 75°C so that the molar concentration ratio was 0.75:1.00, and the solution was stirred to prepare a mixed solution of Bi(NO3)3·5H2O and RuCl3·3H2O. A 2mol / L NaOH solution was added to the mixed solution. The bath temperature was set to 75°C, and the mixed solution with the NaOH solution was stirred while bubbling oxygen. The precipitate generated by this operation was collected by suction filtration and dried to obtain a precursor powder. The precursor obtained was heated to 540°C in an air atmosphere and held for 3 hours to obtain a fired product. The fired product obtained was suction filtered in the order of 75°C distilled water, 2mol / L nitric acid solution, and 75°C distilled water to wash and remove by-products. The fired product was collected by suction filtration, then heated to 120°C and dried to obtain an air electrode catalyst (bismuth ruthenium oxide catalyst) for hydrogen-air secondary batteries. The primary particle size of the air electrode catalyst observed by SEM was 10 to 50 nm.
[0029] This bismuth ruthenium oxide catalyst was pulverized using a wet bead mill (Ashizawa Finetech, Labstar Mini, DMS65). Ion-exchanged water was added to the pulverized bismuth ruthenium oxide catalyst so that the solid content ratio per weight of the bismuth ruthenium oxide catalyst was 20 wt%. Furthermore, a dispersant (San Nopco, SN Dispersant 5468) was added at 2 wt% relative to the catalyst weight to prepare a catalyst dispersion. This catalyst dispersion was pumped into a bead mill device at a predetermined flow rate and pulverized together with zirconia beads (bead diameter φ0.1 mm) at a peripheral speed of 8 m / s. The discharged treatment liquid was then sent back into the bead mill device, and the pulverization and discharge were repeated a total of five times (5 passes) to obtain a dispersion with a bismuth ruthenium oxide concentration of 20 wt%.
[0030] This dispersion was weighed out so that the amount was 50 parts by mass per weight of bismuth ruthenium oxide. 30 parts by mass of high-purity natural graphite (SNO-1T, average particle size 1-2 μm, manufactured by SEC Carbon Co., Ltd.) as a carbon material, 30 parts by mass of FEP dispersion (perfluoroethylene propene copolymer, 120-JRB, average particle size 0.2 μm, manufactured by Mitsui-Chemours Fluoro Products Co., Ltd.) as a fluororesin in terms of solid content ratio, and 1 part by mass of hydroxypropyl cellulose (HPC) as a viscosity adjuster were added to the weighed dispersion, and then ion-exchanged water was added as a viscosity adjuster. At this time, the total amount of water in the slurry was the sum of the amount of water contained in the ion-exchanged water contained in the dispersion and the amount of water contained in the FEP dispersion in addition to the added ion-exchanged water, and the total was 385 parts by mass. These were mixed and stirred in a planetary centrifugal mixer, and the solids weight ratio of the resulting slurry, excluding the water content in the ion-exchanged water and FEP dispersion, was 21.4% of the total slurry.The weight ratios of bismuth ruthenium oxide, graphite, fluororesin, HPC, and dispersant in the solids were 44.9%, 26.9%, 26.9%, 0.9%, and 0.4%, respectively.
[0031] A roll-shaped foamed nickel (thickness 1.6 mm, average pore size 580 μm, basis weight 575 g / m2) as a substrate was adjusted in advance to a thickness of 0.45 mm by roll rolling, the width of the filled part was 80 mm, and the above-mentioned slurry was filled with uncoated parts at both ends to prepare a positive electrode mixture layer. Next, the foamed nickel filled with the slurry was dried at 60 ° C for 1 hour, and then rolled to 0.20 mm by roll rolling. The obtained air electrode was cut into a long length of 125 mm width, and then cut into a short length of 84 mm width so that the width of the uncoated part was 2 mm.
[0032] The resulting air electrode was baked in an electric furnace at 250°C for 13 minutes while flowing nitrogen gas at a flow rate of 1 L / min. The weight of the dried slurry (air electrode mixture) applied to the foamed nickel was calculated from the difference between the weight of the resulting air electrode and the weight of the foamed nickel substrate, and the amount of catalyst per unit area of bismuth ruthenium oxide was calculated from the weight ratio of the input amount. As a result, the amount of catalyst in this air electrode was 7.5 mg / cm. 2 It was.
[0033] (2) Preparation of negative electrode plate The metallic materials Nd, Mg, Ni, and Al were mixed in a predetermined molar ratio, then charged into a high-frequency induction melting furnace and melted in an argon gas atmosphere. The resulting molten metal was poured into a mold and cooled to room temperature of 25°C to produce an ingot.
[0034] Next, this ingot was subjected to a heat treatment in which it was held in an argon gas atmosphere at a temperature of 1000°C for 10 hours, and then cooled to room temperature of 25°C. The cooled ingot was mechanically pulverized in an argon gas atmosphere to obtain a rare earth-Mg-Ni based hydrogen storage alloy powder. The volume average particle size (MV) of the obtained rare earth-Mg-Ni based hydrogen storage alloy powder was measured by a laser diffraction / scattering type particle size distribution measuring device. As a result, the volume average particle size (MV) was 65 μm.
[0035] The hydrogen storage alloy powder was analyzed by inductively coupled plasma spectrometry (ICP), and the composition was found to be Nd 0.89 Mg 0.11 Ni 3.23 Al 0.17 It was.
[0036] Next, 0.25g of hydrogen storage alloy powder and 0.75g of nickel powder were mixed as the negative electrode active material, and after molding, a pellet electrode with a diameter of 10mm was prepared. 100mL of 8mol / L KOH aqueous solution was inserted into a cylindrical container, and the pellet electrode and mercury oxide reference electrode were inserted in the center. A nickel hydroxide counter electrode with a larger electric capacity than the negative electrode was placed on the edge of the container. In this battery with a negative electrode capacity regulation, the negative electrode capacity calculated assuming the alloy capacity to be 300mAh / g was set to 1It. A charge-discharge test was performed by charging for 0.5It x 200 minutes and discharging to a negative electrode potential of -0.3V against the mercury oxide reference electrode at 0.5It to determine the electrochemical alloy capacity. The obtained electrochemical capacity was 350mAh / g.
[0037] To 100 parts by weight of the obtained hydrogen storage alloy powder, 0.2 parts by weight of sodium polyacrylate, 0.04 parts by weight of carboxymethyl cellulose, 0.3 parts by weight of carbon black, and 22.4 parts by weight of water were added and kneaded to prepare a negative electrode mixture paste.
[0038] The negative electrode mixture paste was filled into a sheet-shaped nickel foam as a negative electrode core. The nickel foam had a thickness of 1.6 mm and a basis weight of 300 g / m 2 The nickel foam holding the negative electrode mixture was dried and then rolled to increase the amount of alloy per unit volume. It was then cut to obtain a negative electrode plate 17 of 80 mm x 125 mm. The amount of the negative electrode alloy was adjusted so that the capacity calculated from the alloy capacity was 15.6 Ah.
[0039] (3) Manufacturing components that make up the battery cells The flow path plate 12 was made of SUS316L steel with a thickness of 0.1 mm, and was molded into a corrugated plate shape by die pressing to form the flow paths. The depth of the flow paths formed in the flow path plate 12 was 0.4 mm, the pitch was 2 mm, and the height of the flow path plate 12 including the plate thickness was 0.5 mm. After molding, the air supply port 20, the air exhaust port 21, and the U-shaped notch C were made by laser cutting. The size of the flow path plate 12 was 180 mm x 180 mm.
[0040] The water-repellent film 13 is a microporous PTFE film, and a supply port, a discharge port, and a U-shaped cut C are formed by Thomson machining. The size is 180 mm x 180 mm.
[0041] The positive electrode current collector 15 was made by laser cutting a Ni-plated SPCC steel material having a thickness of 0.2 mm into a frame shape to produce a frame body 15A, and an air supply port 20, an air exhaust port 21, and a U-shaped notch C were made in the frame part of the frame body 15A. The size of the positive electrode current collector 15 after laser cutting was 180 mm × 182 mm. Each of the 182 mm sides was bent in the same direction at an angle of about 60 degrees with respect to the in-plane direction with a width of 1 mm to form a connection piece portion 15C. The outer edge portion 14A of the air electrode 14 was resistance welded to the surface of the frame body 15A opposite to the surface on which the connection piece portion 15C stands.
[0042] The negative electrode current collector 19 is made of Ni-plated SPCC steel having a thickness of 0.1 mm, and is laser-cut to form an air supply port 20, an air exhaust port 21, a communication hole (not shown) for electrolyte injection, and a U-shaped notch C. The size of the negative electrode current collector 19 is 180 mm × 182 mm.
[0043] The gasket A11 was produced by coating rubber on both sides of a 0.3 mm thick SPCC steel plate and laser cutting it. The gasket A11 has a shape that can engage with a groove formed in the flow path plate 12.
[0044] The gasket B18 is made of a PTFE-based joint sheet material having a thickness of 1 mm, and is processed by Thomson machining to form an air supply port 20, an air exhaust port 21, a cavity for accommodating a negative electrode plate 17, and a U-shaped notch C. The size of the gasket B18 is 180 mm x 180 mm. In this embodiment, the gasket B18 has two cavities, each of which has a size of 82 mm x 130 mm.
[0045] The clamping plates 4 and 5 were made by processing stainless steel plates with a thickness of 12 mm. The clamping plate 4 attached to the positive electrode side of the battery module 1 has an air supply port 4A formed therethrough in the plate thickness direction. On the other hand, the clamping plate 5 attached to the negative electrode side has an air exhaust port 5A formed therethrough in the plate thickness direction.
[0046] (4) Attaching the air electrode to the positive current collector plate As described above, the air electrode 14 is housed inside the frame of the frame 15A of the positive current collector plate 15, and the outer edge 14A of the base of the air electrode 14 is welded to the inner edge of the frame 15A. The air electrode 14 is supported by the frame 15A by welding. An example of a support structure for the air electrode 14 by the positive current collector plate 15 is shown in FIG.
[0047] In this embodiment, two electrodes with a catalyst-coated area of 80 mm x 125 mm (the size of the conductive support is 84 mm x 125 mm, with uncoated areas of 2 mm each along the longitudinal direction provided as welding points) are arranged side by side, and a beam 15B with a width of 4 mm is provided in the center.
[0048] More specifically, as shown in FIG. 3, a positive current collector plate 15 having dimensions of 182 mm wide by 180 mm long is cut out between the outer edge of the positive current collector plate 15 and the beam 15B in a rectangular shape so that a beam 15B having a width of 4 mm remains in the center, forming two openings 15D, 15D inside the frame 15A. The air electrode 14 is attached to this opening 15D. The base of the air electrode 14 has dimensions of 84 mm wide by 125 mm long. The base of the air electrode 14 has an uncoated portion 14A, i.e., an outer edge portion 14A, that is free of the positive electrode mixture over a width of 2 mm in the longitudinal direction. This uncoated portion 14A is disposed between the long sides 15D of the opposing openings of the frame 15A. L Nearby and long side 15D of beam 15B L The air electrode 14 is fixed to the frame 15A by resistance welding to the adjacent parts. In this manner, the air electrode 14 is supported by the positive current collector plate 15.
[0049] Furthermore, the outer peripheral edge portions of the frames 15A facing each other across the beam 15B are bent over a width of 1 mm toward the opposite side of the surface of the frame 15A to which the air electrode 14 is fixed, to provide a connecting piece portion 15C. Generally, the physical strength of a plate-like member is increased by bending the outer peripheral edge portions in a direction intersecting the in-plane direction, rather than by having the entire surface flat. Therefore, the welded portion between the air electrode 14 and the frame 15A is located near the connecting piece portion 15C of the positive current collector 15, so that distortion or bending of the positive current collector 15 due to welding is suppressed.
[0050] (5) Battery module assembly A guide screw 30 covered with an FEP tube was set in one of the two clamping plates 4, 5 so as to be approximately perpendicular to the main surface of the clamping plate, and the negative electrode current collector plate 19 and gasket B 18 were stacked in this order so that the notch C was aligned with the screw 30. The guide screw 30 is an example of a rod-shaped mounting tool. The FEP tube is an example of an elastic tube.
[0051] A 0.3 mm thick foamed nickel plate and a negative electrode plate 17 were placed in the hollow of the gasket B18. Furthermore, a separator 16 and a positive electrode current collector plate 15 to which an air electrode 14 was welded were placed on top of each other. The positive electrode current collector plate 15 was placed on the separator 16 so that the rising direction of the connection piece portion 15C of the frame body 15A was opposite to the direction toward the negative electrode plate 17. Furthermore, the water-repellent film 13, the flow path plate 12, and the gasket A11 were placed on top of each other. The positive electrode current collector plate 15, the water-repellent film 13, the flow path plate 12, and the gasket A11 were placed on top of each other. The alignment of the positive electrode current collector plate 15, the water-repellent film 13, the flow path plate 12, and the gasket A11 was performed by utilizing the engagement between the notch C formed in each of them and the guide screw 30.
[0052] In this way, the laminated structure formed by stacking the negative electrode current collector plate 19 through the gasket A11 in order constitutes one set, and 60 sets were stacked in one direction. In one set, the positive electrode (air electrode) and the negative electrode plate 17 face each other with the separator 16 sandwiched therebetween, so that one set constitutes a single battery cell 2.
[0053] The 60 battery cells 2 were stacked in one direction using the guide screws 30 to connect the 60 battery cells 2 in series, and then one negative current collector plate 19 was placed on top of the other fastening plate 5. The last negative current collector plate 19 does not constitute a battery cell 2.
[0054] Next, a load of 8 t was applied using a vertical press, and then the fastening plates 4, 5 were fastened together using the screws 30 to assemble the battery module 1. The assembled battery module 1 is capable of having an electrolyte sealed therein.
[0055] The negative electrode current collector 19 of the first stacked battery cell 2 was used as the negative electrode terminal of the battery module 1, and the positive electrode current collector 15 of the last stacked battery cell 2 and the negative electrode current collector 19 in contact with this positive electrode current collector 15 were connected together to form an integrated member, which served as the negative electrode terminal of the battery module 1. After a leak check of the battery module 1 was performed, 1.2 kg of a 5 mol / L KOH aqueous solution was injected into the battery module 1 as the electrolyte.
[0056] In addition, in the battery module 1, the air supply port 20 and air exhaust port 21 of each battery cell 2 are connected to each other, so air is introduced into the battery module 1 from the air supply port 4A of the clamping plate 4 on the positive electrode side, passes through the 60 battery cells 2, and is then exhausted from the air exhaust port 5A of the clamping plate 5 on the negative electrode side. In other words, air is supplied to all 60 battery cells 2.
[0057] The battery module 1 was subjected to aging treatment at 60°C for 12 hours to activate the negative electrode, and then cooled to room temperature. After that, the battery module 1 was charged and discharged while supplying air from which CO2 had been removed at 6.2 L / min to the battery module 1. The charge and discharge conditions were 25 Ah, equivalent to 80% of the design capacity of the negative electrode, as 1 It, and charging was performed for 0.1 It x 10 hours, and discharging was performed at 0.05 It (discharge end voltage EV was 42 V).
[0058] (6) Series connection of battery cells Next, the electrical connection of two battery cells 2 adjacent to each other in the stacking direction in the assembly of the above-mentioned battery module 1 will be described. In the battery module 1, in order to connect stacked battery cells 2 in series, it is necessary to electrically connect the positive electrode current collector 15 of the i-th battery cell 2 (i is a natural number in which 1≦i≦59) that has already been stacked with the guide screw 30 to the negative electrode current collector 19 of the adjacent (i+1)-th battery cell 2 stacked on top of that battery cell 2. As shown in FIG. 4(a), the water-repellent film 13 and flow path plate 12 of the i-th battery cell 2 are present between the positive electrode current collector 15 of the i-th battery cell 2 and the negative electrode current collector 19 of the (i+1)-th battery cell 2.
[0059] However, since the connection piece portion 15C of the positive current collector plate 15 of the i-th battery cell 2 extends toward the negative current collector plate 19 of the (i+1)-th battery cell 2, as shown in Fig. 4(b) , by fastening with the fastening plates 4, 5, it goes beyond the water-repellent film 13 and flow path plate 12 of the i-th battery cell 2 and comes into contact with and electrically connected to the negative current collector plate 19 of the (i+1)-th battery cell 2. The i-th battery cell 2 is an example of a first battery cell, and the (i+1)-th battery cell 2 is an example of a second battery cell.
[0060] The positive current collector plate 15 has a frame shape with the inside cut out to the shape of the air electrode 14 in order to support the air electrode 14 on the inside. The frame-shaped frame body 15A has a lower rigidity than the shape before processing. However, since the frame body 15A has a connection piece portion 15C that stands up integrally from the frame body 15A in a direction perpendicular to the frame surface of the frame body 15A near the welded portion, the rigidity of the frame body 15A is reinforced. Therefore, the occurrence of distortion or bending of the positive current collector plate 15 due to welding of the air electrode 14 can be suppressed.
[0061] 3. Effect of the shape of the positive electrode current collector The suppression of distortion or bending of the positive current collector plate 15 by the connecting piece portion 15C will be described.
[0062] As described above, the connection piece portion 15C is formed by bending the side of the frame body 15A of the positive current collector plate 15 located outside the portion where the air electrode 14 is welded, by a width of 1 mm. A positive current collector plate 15 is prepared in which the side opposite to the connection piece portion 15C across the frame body 15A to be welded is not bent. After arranging the frame body 15A of the positive current collector plate 15 so that the frame surface is parallel to the horizontal direction, the vertical deflection of the positive current collector plate 15 due to its own weight is measured when the side without the connection piece portion 15C is the fixed end and the side with the connection piece is the free end. The deflection is measured as the length of vertical movement of the free end after the free end is held at the same height as the fixed end and released from the holding and allowed to move freely.
[0063] Three types of rectangular positive electrode current collector plates having a side length of 180 mm and having a connecting piece portion 15C and different thicknesses of 0.1 mm, 0.2 mm, and 0.3 mm were designated, respectively, as Example 1, Example 2, and Example 3. For comparison, rectangular positive electrode current collector plates having a side length of 180 mm and no connecting piece and different thicknesses of 0.1 mm, 0.2 mm, and 0.3 mm were designated, respectively, as Comparative Example 1, Comparative Example 2, and Comparative Example 3.
[0064] Short side 15D of opening 15D of positive electrode current collector plate 15 by welding of air electrode 14 S The length change in the direction before and after welding, i.e., the amount of distortion of the opening 15D of the positive electrode current collector plate 15, was examined as follows. For example, as shown in FIG. 3, the inner edge 15D of the frame 15A was L From the outer edge 14A side of the base of the air electrode 14 welded to the edge of the beam 15B, i.e., the long side 15D of the opening 15D L Up to the short side 15D of the opening 15D S A line segment L extending parallel to the long side 15D to which the air electrode 14 is welded is L For each line segment L, three are assumed, one at the end and the other at the center. The length displacement (strain of opening 15D) was investigated before and after welding at three points, including the midpoint of line segment L, using a cantilever spring with one end in the length direction fixed and the other end free. The results are shown in standard deviation as shown in Table 1.
[0065] [Table 1]
[0066] As can be seen from Table 1, in the examples having the connecting piece portion 15C, the "deflection before welding" was 1.8 mm in Example 1, 1.1 mm in Example 2, and 0.2 mm in Example 3, with the deflection decreasing as the film thickness increases. In the comparative examples without the connecting piece portion 15C, the deflection decreased as the film thickness increases, similarly to 7.3 mm in Comparative Example 1, 3.0 mm in Comparative Example 2, and 1.5 mm in Comparative Example. Comparing the examples and comparative examples, the deflection before welding in Examples 1-3 having the connecting piece portion 15C was less than half that of the comparative examples with the same film thickness, and the degree of deflection was small for all film thicknesses.
[0067] Next, the "standard deviation of the length displacement of the fixed end, center, and free end of the inner edge of the frame" before and after welding was 0.11 mm in Example 1, 0.04 mm in Example 2, and 0.01 mm in Example 3, and the amount of displacement of the inner edge of the frame decreased as the film thickness increased. In the comparative examples without connecting piece portion 15C, the amount of displacement of the inner edge of the frame decreased as the film thickness increased, similar to 0.15 mm in Comparative Example 1, 0.13 mm in Comparative Example 2, and 0.03 mm in Comparative Example.
[0068] Thus, looking at the standard deviation of the deflection before welding and the displacement of the inner edge of frame body 15A after welding, the positive current collector plate 15 having connecting piece portion 15C can suppress the occurrence of deflection due to its own weight or welding and distortion during welding. Also, as the plate thickness of positive current collector plate 15 becomes thicker, the amount of deflection or distortion becomes smaller.
[0069] Increasing the thickness of the positive current collector plate 15 increases the rigidity and suppresses bending, but increases the weight and volume of components other than the air electrode 14 and the negative electrode, decreasing the energy density of the battery cell 2. Furthermore, if the thickness is 0.4 mm or more, bending the outer edge of the frame 15A becomes difficult, making it impossible to manufacture the connection piece 15C with high accuracy. Therefore, the optimal thickness of the positive current collector plate 15 is 0.1 to 0.3 mm, and 0.2 to 0.3 mm is more preferable.
[0070] By forming connection piece 15C by bending the outer edge of frame 15A of positive current collector plate 15 by a width of 1 mm, deformation due to welding of the air electrode to frame 15A can be suppressed.
[0071] In this embodiment, the outer edge of the frame 15A is bent at an angle of 60 degrees with respect to the in-plane direction with a width of 1 mm to form the connection piece 15C. For example, the height of the connection piece 15C of the positive electrode current collector 15 of the i-th battery cell 2 is less than 1 mm. However, the length of the connection piece in the stacking direction is longer than the total thickness of the flow path plate 12 and the water-repellent film 13 of the i-th battery cell 2 sandwiched between the positive electrode current collector 15 of the i-th battery cell 2 and the negative electrode current collector 19 of the adjacent (i+1)-th battery cell 2, so that the connection piece is in reliable contact with the negative electrode current collector 19 of the (i+1)-th battery cell 2 to connect the i-th battery cell 2 to the (i+1)-th battery cell 2 in series. The configuration of the positive electrode current collector having the connection piece 15C of this embodiment allows adjacent battery cells 2 to be connected in series.
[0072] In this way, the rigidity is improved by the connection piece portion 15C of the positive current collector plate 15, making it unnecessary to increase the thickness of the positive current collector plate 15 or the size of the beam 15B. Therefore, the energy density of the battery module 1 can be maintained.
[0073] Furthermore, because distortion of the positive current collector plate 15 is suppressed, misalignment when the battery cells 2 are stacked and clamped with the clamping plates 4, 5 is suppressed.
[0074] As described above, in this embodiment, 60 battery cells 2 are stacked, so that two types of gaskets A and B are provided for each battery cell 2, and a total of 120 gaskets are lined up in a row to seal them. Since there is little distortion or bending of the positive current collector plate 15, the gaskets are compressed evenly, making it difficult for pressure loss to occur in the flow paths of the flow path plate 12. Therefore, air can be distributed and supplied evenly to each battery cell 2, suppressing the occurrence of voltage differences and capacity differences between the battery cells 2. This can reduce causes of impaired battery life.
[0075] Furthermore, U-shaped notches C were provided in the flow path plate 12, the negative electrode current collector plate 19, and the positive electrode current collector plate 15, and the battery cells 2 were stacked using screws 30 covered with elastic tubes as guides. By making the notches C U-shaped, the members constituting the battery cells 2 can be stacked smoothly. In addition, because there is little distortion or bending of the positive electrode current collector plate 15 to which the air electrode 14 is welded, the battery cells 2 can be stacked with precision when assembling the battery module 1.
[0076] 4. Evaluation of battery characteristics The DC resistance after activation of the battery module 1 was small, at 3 mΩ per battery cell 2. The small internal resistance of the battery cell 2 is believed to be due to the following.
[0077] (a) The base of the air electrode 14 is welded to the frame 15A of the positive current collector plate 15 to ensure accurate electrical continuity. (b) The positive electrode collector 15 of the i-th battery cell 2 is in precise contact with and electrically connected to the negative electrode collector 19 of the (i+1)-th battery cell 2 located adjacent to the positive electrode collector 15 via the connection piece portion 15C. (c) By inserting a plate made of foamed nickel between the negative electrode collector plate 19 and the negative electrode plate 17, dimensional changes in the stacking direction of the battery cells 2 are absorbed, thereby maintaining good contact between the negative electrode collector plate 19 and the negative electrode plate 17.
[0078] In addition, in the battery module 1, the battery voltage of every five cells out of the 60 battery cells 2 connected in series was monitored during charging and discharging. The variation in electrical capacity was suppressed compared to a battery module 1 having battery cells 2 consisting of a positive electrode collector plate 15 without a connection piece portion 15C, and extremely stable charging and discharging characteristics with an Ah efficiency of 99.4% were achieved. [Explanation of symbols]
[0079] 1. Air battery module 2 Air battery cell 12 Flow path plate 13 Water-repellent film 14 Air electrode 15 Positive current collector 15A frame 15C Connection piece 16 Separator 17 Negative electrode plate 19 Negative current collector
Claims
1. An air battery module configured by connecting a plurality of air battery cells in series along one direction, Each of the plurality of air battery cells is configured by stacking a negative electrode current collector, a negative electrode plate, a separator, a positive electrode current collector supporting an air electrode, a water-repellent film, and a flow path plate along the one direction, The positive electrode current collector plate is a conductive frame that supports the air electrode and is electrically connected to the air electrode; a conductive connection piece portion that is formed integrally with the frame body and extends in a direction intersecting a frame surface of the frame body and toward an opposite side to the negative electrode current collector plate, At least two of the connection pieces are formed to face each other across the air electrode supported by the frame, An air battery module in which, when the negative electrode side of a second air battery cell is connected to the positive electrode side of a first air battery cell among the plurality of air battery cells, the connection piece portion of the positive electrode collector plate of the first air battery cell comes into contact with and is electrically connected to the negative electrode collector plate of the second air battery cell.
2. The air battery module in accordance with claim 1 , wherein the air electrode is resistance-welded to a frame of the positive electrode current collector plate.
3. The air battery module in accordance with claim 2 , wherein the welded portion of the air electrode to the frame is located inside the connecting pieces that face each other.
4. The air battery module in accordance with claim 1 , further comprising a member made of foamed metal sandwiched between the negative electrode current collector plate and the negative electrode plate.
5. 2. The air battery module of claim 1, wherein each of the negative current collector plate, the frame of the positive current collector plate, and the flow path plate has at least one of a notch and a protrusion on its peripheral portion, and the frame of the positive current collector plate and the flow path plate are aligned relative to the negative current collector plate using at least one of the notch and the protrusion.
6. The battery further includes two clamping plates attached to the positive and negative sides of the plurality of air battery cells connected in series, each of the negative electrode current collector plate, the frame of the positive electrode current collector plate, and the flow path plate has the notch portion; 6. The air battery module of claim 5, wherein the negative electrode collector plate, the negative electrode plate, the separator, the positive electrode collector plate, the water-repellent membrane, and the flow path plate are stacked for each air battery cell using a rod-shaped mounting fixture fixed to one of the fastening plates and covered with an elastic tube as a guide.
7. 2. The air battery module in accordance with claim 1, wherein the frame of the positive electrode current collector plate has a thickness of 0.1 to 0.3 mm.
Citation Information
Patent Citations
Metal-air secondary battery
JP2012094385A
Battery pack
JP2013175446A
Air battery and battery pack including the same
JP2014022316A
Air cell and method for manufacturing the same
JP2015035271A
Electrode Assembly and Method for Preparation thereof
JP2015537336A