Material evaluation test method, breakage determination method of structure, and test piece
A uniaxial tensile test method with controlled strain gradients in both radial and circumferential directions addresses the challenge of evaluating material fracture in automobile parts, providing accurate rupture predictions.
Patent Information
- Application Number
- JP2023058583
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing material evaluation methods fail to accurately assess the impact of strain gradient on tensile input during actual collision deformation, particularly in automobile parts, leading to inadequate energy absorption and potential material fracture.
A uniaxial tensile test method using a plate-shaped specimen with a notch on one side and an arc-shaped edge on the other, where the notch tip radius (Ra) and arc radius (Rb) satisfy a specific relationship, allowing for controlled strain gradients in both radial and circumferential directions, enabling evaluation of elongation at break and fracture determination.
Enables accurate prediction of rupture limits under actual collision conditions, facilitating improved material evaluation and fracture determination in structures like automobile bodies, by correlating strain gradient ratios with elongation at break.
Smart Images

Figure 2024145955000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a material evaluation test method, and more particularly to an evaluation test method that takes into account the strain gradient of a metal material. [Background technology]
[0002] The development of a body structure that can reduce the impact of a collision is always one of the most important issues for automobiles. One of the methods to deal with a collision is to absorb the collision energy by the structural members of the automobile and protect the passenger space. In order to absorb the collision energy, it is important that the structural members deform in the mode aimed at at the time of design. If material fracture occurs during the deformation process, the deformation mode will not be the aimed one, and sufficient energy absorption performance may not be obtained.
[0003] Material fracture may occur due to in-plane tensile or bending deformation, but in addition, stretch flange fracture may occur at the edges of punched openings or holes, or at the edges of punched notches or corners around the periphery of the component.
[0004] The characteristics of stretch flange fracture are that it occurs from the edge of the sheet or near the edge of the sheet that was damaged when punched out by the die, and that it is accompanied by deformation that generates a strain gradient in the in-plane direction (for example, the circumferential direction and radial direction of the notch tip) at the edge of the sheet, that is, stretch flange deformation. It is said that the fracture limit when stretch flange deformation is accompanied changes depending on the punching damage and strain gradient.
[0005] In a crash test of an automobile body, the impactor penetrates the component, and the part on the outside of the bend undergoes bending deformation as a whole, which mainly undergoes tensile deformation. If a punched hole or notch is present in the part where this mainly tensile deformation occurs, strain concentration occurs at the periphery of the hole or the plate edge of the notch tip, resulting in a strain gradient in the relevant part. In other words, if a hole or notch is present in a part where tensile deformation occurs in a main structural member that absorbs energy during a car crash, stretch flange deformation often occurs at the plate edge.
[0006] The hole expansion test, which is standardized by the JIS, is generally used as a test method for evaluating the stretch flangeability of steel materials. The hole expansion test can evaluate the effect of punching damage by changing the punching clearance, but while a high strain gradient occurs in the radial direction, there is almost no strain gradient in the circumferential direction due to axisymmetric deformation, making it an evaluation test under a peculiar strain gradient condition.
[0007] For this reason, several methods have been proposed for evaluating stretch flange properties under conditions close to actual stretch flange deformation. For example, Patent Documents 1 and 2 disclose that when material (flange) flows into a corner during press forming, a strain gradient occurs due to the difference in linear length change accompanying the flow, resulting in stretch flange deformation. In order to reproduce these, a side bend test method has been proposed for evaluating the stretch flangeability in press forming by applying tensile bending deformation in the plane. In addition, Patent Document 3, for example, discloses a method for evaluating the relationship between the necking limit strain and the strain gradient in the tensile orthogonal direction (radial direction) obtained from a single-sided notch tensile test to evaluate the occurrence of necking at the edge of a sheet, which is a problem in the press forming process. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2009-145138 A [Patent Document 2] JP 2011-140046 A [Patent Document 3] Patent Publication No. 2021-164933 Summary of the Invention [Problem to be solved by the invention]
[0009] The side bend test methods proposed in Patent Documents 1 and 2 are effective in terms of reproducing stretch flange deformation in actual press forming. However, since the purpose is to reproduce the stretch flange deformation during press forming, the test method applies in-plane bending (rotation) while pulling, and the input is different from the part that is mainly subjected to tensile deformation during collision, which is the subject of the present invention. In addition, since the test method is complicated, there is a demand for improvement and simplification of operability.
[0010] In addition, the necking limit strain determination method proposed in Patent Document 3 evaluates necking occurrence but does not directly evaluate fracture. Furthermore, the strain gradient is a factor that affects the fracture limit, and it is known that both the radial and circumferential strain gradients affect the fracture limit, but the necking limit strain determination method proposed in Patent Document 3 evaluates only the radial strain gradient, so it cannot be said that it is capable of evaluating the actual stretch flange deformation at fracture.
[0011] Therefore, the present invention aims to easily evaluate material properties taking into account the effect of strain gradient against tensile input that corresponds to actual collision deformation of automotive components, and to provide a material evaluation method and test specimen shape for such evaluation. [Means for solving the problem]
[0012] The present inventors have conducted intensive research and development to achieve the above object, and have obtained the following findings.
[0013] [a] It was discovered that in a test piece for a normal uniaxial tensile test (hereinafter simply referred to as a tensile test), by providing a notch of radius Ra on one side of the plate edge and making the plate edge on the opposite side into an inwardly concave arc shape, a straight line, or an outwardly convex arc shape with a radius larger than Ra, it is possible to change the state of strain at the tip of the notch of radius Ra. In other words, it was discovered that by changing the shape of the notch of radius Ra placed on one side of the plate edge and the plate edge on the opposite side, it is possible to control the maximum principal strain at the notch tip, as well as the radial and circumferential gradients of that maximum principal strain (hereinafter simply referred to as the radial strain gradient and circumferential strain gradient).
[0014] [stomach] When experiments were carried out by introducing the strain gradient ratio (= circumferential strain gradient / radial strain gradient), which is the ratio of the circumferential strain gradient to the radial strain gradient, as an index of the strain field at the tip of the notch, it was found that there is a strong correlation between the fracture elongation and the strain gradient ratio, and that there is a specific relationship for each steel material. In other words, if the relationship between the strain gradient ratio and fracture elongation for each steel material is understood, it was realized that in actual collision deformation, for example, if the strain gradient ratio at the tip of the notch is known, the fracture elongation of that part can be obtained.
[0015] [cormorant] By utilizing the relationship between the strain gradient ratio and fracture elongation for each steel material and converting it into the relationship between the strain gradient ratio and fracture strain, we discovered that it is possible to make fracture judgments based on the actual strain gradient in automobile crash simulations and structural fracture (destruction) simulations using FEM (finite element method) and the like.
[0016] The present invention was made based on these findings, and the gist of the present invention is given below.
[0017] [1] A material evaluation method comprising the steps of: performing a uniaxial tensile test in which a plate-shaped test piece for a uniaxial tensile test has a notch with a tip radius Ra on one side in the width direction of the test piece; and the other side of the test piece is arc-shaped with a radius Rb, with Ra and Rb satisfying the relationship in the following formula 1; and applying a tensile force to both ends in the longitudinal direction of the test piece. 2Ra≦Rb (Formula 1) [2] The material evaluation method described in [1] above, which determines the fracture elongation, which is the gage-to-point elongation of the test piece when a crack initiates from the tip of the notch, and the radial strain gradient and circumferential strain gradient, which are the gradients of the maximum principal strain in the radial direction and circumferential direction of the notch at the tip of the notch, respectively, obtains the relationship between the fracture elongation and the strain gradient ratio (circumferential strain gradient / radial strain gradient), which is the ratio of the circumferential strain gradient to the radial strain gradient, and the fracture elongation, and performs material evaluation. [3] The material evaluation method according to [2], wherein the radial strain gradient and the circumferential strain gradient are determined by FEM (finite element method) analysis. [4] The material evaluation method according to [2] or [3], wherein the relationship between the strain gradient ratio and the fracture elongation is a fracture limit line obtained in a two-dimensional graph with the fracture elongation on the vertical axis and the strain gradient ratio on the horizontal axis. [5] A method for determining whether a structure will break in a deformation simulation by FEM, the method comprising: determining whether the structure will break from the relationship between the strain gradient ratio and the breaking elongation described in any one of [2] to [4] above. Structures include the body structure of an automobile and the beam structure of a building. [6] A method for determining whether an element of a structure will break in a deformation simulation by FEM of the structure, characterized in that the vertical axis of the two-dimensional graph shown in [4] above is replaced with the maximum principal strain of the element at the notch root when the fracture elongation is applied in the FEM analysis, and a fracture limit line is obtained as the relationship between the strain gradient ratio and the maximum principal strain of the element at the notch root when the fracture elongation is applied. [7] A test piece for a uniaxial tensile test, the test piece being in the form of a plate, having a notch with a tip radius Ra on one side in the width direction, and the other side of the test piece being in the form of a circular arc with a radius Rb, wherein Ra and Rb satisfy the relationship in the following formula 1. 2Ra≦Rb (Formula 1) [8] The test piece according to [7], wherein the test piece is a steel plate having a tensile strength of 980 MPa or more. [9] The test piece according to [7] or [8], wherein the notch of radius Ra is a part of a hole punched with the same diameter and the same clearance as in the hole expansion test.
[10] A method for manufacturing the test piece according to [7] or [8] above, characterized in that the notch of radius Ra in the test piece is produced by punching out the notch with the same diameter and with the same clearance as in the hole expanding test. Effect of the Invention
[0018] The present invention makes it possible to easily perform material evaluation that takes into account the effect of strain gradient on tensile input that corresponds to the actual collision deformation of automobile components. Furthermore, it makes it possible to predict fracture limits that correspond to the strain gradient state in various structures, and it is possible to easily perform fracture judgment of structures using this. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a diagram illustrating a test piece according to one embodiment of the present invention. [Diagram 2] 2(A) to (F) are diagrams showing examples of a test piece according to one embodiment of the present invention. [Diagram 3] Fig. 3 is a diagram for explaining an example of a method for determining the strain gradient, where Fig. 3(a) is a diagram for explaining an example of the result of the FEM analysis, and Fig. 3(b) is a diagram for explaining an example of a method for determining the radial strain gradient and the circumferential strain gradient. [Figure 4] FIG. 4 is a diagram for explaining the strain field (circumferential strain gradient and radial strain gradient) for each test piece obtained according to one embodiment of the present invention. [Diagram 5] FIG. 5 is a diagram for explaining a breaking limit line in a graph in which the horizontal axis represents the strain gradient ratio and the vertical axis represents the breaking elongation, which is determined according to one embodiment of the present invention. [Figure 6] FIG. 6 is a diagram for explaining a fracture limit line in a graph in which the horizontal axis represents the strain gradient ratio and the vertical axis represents the maximum principal strain at the notch bottom, which is determined according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention will be described based on examples. Note that the examples used in the description are merely illustrative of the present invention and are one of the embodiments, and therefore the present invention is not limited to these examples.
[0021] [Test piece] In a crash test or the like, when strain is concentrated at a plate edge such as a punched hole or a notch at a portion that is mainly subjected to tensile deformation, a strain gradient is generated starting from the strain concentration portion. Therefore, the inventors have intensively studied specimen shapes that generate various strain gradients in tensile tests. As a result, the inventors have found that in a test specimen in which a part of a plate edge on one side of the test specimen has a concave notch (toward the inside of the test specimen) with a tip radius Ra, and the shape of the plate edge on the opposite side of the notch (the anti-notch side) is an arc shape with a radius Rb larger than Ra, by changing (a) the notch depth, (b) the test specimen width at the notch tip, and (c) the shape of the plate edge on the anti-notch side, it is possible to variously change the strain gradients of the principal strains in the circumferential and radial directions at the notch tip (also called the notch bottom).
[0022] Here, the radius Rb on the anti-notch side is an arc shape, which may be a concave arc shape with respect to the test piece (toward the inside of the test piece) at radius Rb, or a case where Rb is infinite, i.e., a straight line, or a convex arc shape with radius R2 with respect to the test piece (toward the outside of the test piece).
[0023] An example of a test specimen is shown in Figure 1. The test specimen 1 has a notch on the plate edge on one side (left side in Figure 1), and the tip (notch bottom) radius of the notch is Ra. The plate edge on the other side of the test specimen, i.e., the opposite side of the notch (anti-notch side (right side in Figure 1)), is an arc shape with a radius of Rb. Although not shown, a material evaluation test can be performed by applying a load along the longitudinal axis of the test specimen 1 (vertical direction in Figure 1) and performing a uniaxial tensile test in which a tensile force is applied to both ends of the longitudinal direction of the test specimen. The longitudinal axis of the test specimen 1 (vertical direction in Figure 1), which is the direction in which this load is applied, is called the test specimen center line, and the direction perpendicular to the test specimen center line is called the width direction.
[0024] (A) The shallower the notch depth (the shortest distance from the notch bottom to the notch bottom imaginary line (extrapolated line) of the plate edge on the side having the notch), the greater the degree of strain concentration at the notch bottom and the greater the strain gradient. There is no particular limit on the lower limit of the notch depth, but it may be 0.5 mm for processing reasons. There is no particular limit on the upper limit of the notch depth, either, but it may be the same value as the radius Ra of the notch tip.
[0025] (a) The smaller the specimen width 2 from the notch bottom (the shortest distance in the width direction from the notch bottom to the edge of the plate opposite the notch), the greater the degree of strain concentration at the notch bottom and the larger the strain gradient can be. On the other hand, if the specimen width 2 is too narrow, the strain will not concentrate at the notch bottom, but will concentrate in the center of the specimen, and the strain gradient with a peak at the notch bottom will not occur. Therefore, the lower limit of the specimen width 2 should be set to the same value as the notch depth. There is no particular limit on the upper limit of the specimen width, but it is desirable for the specimen width 2 to be 50 mm or less in order to be used in a tensile test.
[0026] (c) By changing the shape of the sheet edge on the opposite side of the notch (anti-notch side), the strain field (circumferential strain gradient and radial strain gradient) at the notch root can be changed, and the strain gradient ratio (=circumferential strain gradient / radial strain gradient) can be changed. Here, the gradients of the maximum principal strain in the notch radial direction and notch circumferential direction at the tip of the notch are called the radial strain gradient and the circumferential strain gradient, respectively. The sheet edge on the anti-notch side is an arc shape with a radius Rb. By making Rb larger than the radius Ra of the notch tip, a strain gradient is generated starting from the notch root, and by changing the radius Rb of the arc on the anti-notch side, the circumferential strain gradient and the radial strain gradient can be changed. In addition, if the radius Rb of the anti-notch side arc is made infinite, that is, by making it a straight line, it is possible to reduce the ratio of the circumferential strain gradient to the radial strain gradient at the notch root. Furthermore, by making the anti-notch side arc have an outwardly convex shape with arc radius Rb, the ratio of the circumferential strain gradient to the radial strain gradient at the notch bottom can be further reduced.
[0027] The arc radius Rb of the plate edge on the opposite side to the notch is at least twice the notch bottom radius Ra (that is, satisfies formula 1), and more preferably at least five times the notch bottom radius Ra. 2Ra≦Rb (Formula 1)
[0028] On the other hand, in the case of a test piece with straight edges on both sides (normal tensile test piece shape) or a test piece with the same shape of notch on both sides, although this will vary depending on the notch root radius Ra and the test piece width, generally the strain is concentrated in the center of the test piece width and fracture occurs there, so fracture does not originate from the edge of the plate.
[0029] An example of a test piece is shown in Figure 2. The specifications of each test piece in Figures 2(A) to (F) are shown in Table 1. [Table 1]
[0030] [Relationship between strain gradient ratio and breaking elongation] Through numerous experiments, the inventors have found that the fracture limit at the notch root can be expressed by the strain gradient ratio (circumferential strain gradient / radial strain gradient), which is the ratio of the circumferential strain gradient to the radial strain gradient at the notch root. Further investigations have revealed that there is a strong correlation between the fracture elongation, which is the gauge length elongation of the test piece when a crack occurs from the tip of the notch, and the strain gradient ratio, and that there is a unique relationship for each steel material. In other words, if the relationship between the strain gradient and fracture elongation for each steel material is understood and the strain gradient at the tip of the notch in the actual stretch flange deformation mode is known, the fracture elongation at that time can be obtained.
[0031] The strain gradient at the notch root can be identified by determining the strain distribution starting from the notch root. For example, as shown in Figure 3, it can be obtained from a Finite Element Method (FEM) analysis that reproduces a material evaluation test. For example, tensile deformation is applied in the FEM analysis until the elongation between the set gauge points reaches the fracture elongation confirmed in the experiment, and the distribution of maximum principal strain between elements in the circumferential and radial directions is obtained starting from the element at the notch root at that time, and the gradient of maximum principal strain near the notch root is obtained. If the range for obtaining the strain gradient is too wide, it will pick up strain gradients that are not directly related to the notch root where fracture occurs, so it is recommended that the range for analyzing the strain gradient be a square range with one side being the length of the notch tip radius Ra. For example, if the notch root radius Ra is 5 mm, it is advisable to obtain the strain gradient within a range of 5 mm or less in the radial direction (width direction of the test piece) from the notch root and within ±2.5 mm or less in the circumferential direction (center line direction of the test piece). Therefore, the smaller the element size (mesh size) in FEM analysis, the higher the accuracy, but the longer the calculation time. Therefore, it is advisable to select the optimal mesh size. For example, it is advisable to set the mesh size to 1 / 10 (0.1 times) to 1 / 2 (0.5 times) of the notch root radius Ra (the length of one side in the case of a square or triangular mesh). Figure 3 shows an example of FEM analysis. Figure 3(a) shows the mesh and a contour diagram color-coded according to the magnitude of the principal strain. Figure 3(b) shows the circumferential strain distribution and radial strain distribution at the notch root 3 (notch tip) obtained from this analysis. From this strain distribution diagram, the radial strain gradient and circumferential strain gradient at the notch bottom (corresponding to the peak of the strain distribution) can be obtained. Once the radial strain gradient and circumferential strain gradient are obtained, the strain gradient ratio (circumferential strain gradient / radial strain gradient) can be calculated by taking their ratio.
[0032] Figure 4 shows an example of a plot of the radial strain gradient and circumferential strain gradient at the notch root for the test specimen shown in Figure 2 and Table 1. As is clear from Figure 4, it is possible to change the strain field at the notch root (circumferential strain gradient and radial strain gradient) by changing the notch root radius Ra and the arc radius Rb of the anti-notch side plate edge shape, as well as the notch depth and test specimen width. For reference, points corresponding to a conventional hole expansion test are also plotted. It can be seen that in the case of a hole expansion test, the circumferential strain gradient is typically close to zero.
[0033] The method for measuring the breaking elongation is not particularly limited. For example, it may be determined according to an image correlation method or a tensile test method specified in JIS. The gauge length for evaluating the breaking elongation may be 10 times or less, preferably 5 times or less, or 2 times or less, of the radius Ra of the notch bottom.
[0034] [Break limit line] The relationship between the strain gradient ratio and the fracture elongation obtained in this way is specific to the material, and it is possible to evaluate the characteristics of the material in accordance with the strain gradient (material evaluation).
[0035] Figure 5 shows the relationship between the strain gradient ratio and the fracture elongation. This is a two-dimensional graph with the strain gradient ratio on the horizontal axis and the fracture elongation on the vertical axis. It can be seen that there is a clear correlation, and that the higher the strain gradient ratio, the lower the fracture elongation tends to be. It can be seen that the strain gradient ratio corresponding to the conventional hole expansion test is near zero (strain gradient ratio is about 0 to 0.3), which is the region showing the highest fracture elongation. On the other hand, in the case of the actual vehicle crash test, it was found from FEM analysis that the strain gradient ratio is in the range of about 0.7 to 2.2. In other words, in the conventional hole expansion test, it is possible that the correct fracture elongation in the strain gradient ratio region corresponding to the actual vehicle crash test cannot be evaluated, and it is considered that an excessive fracture elongation was evaluated.
[0036] Here, the relationship obtained from the relationship between the fracture elongation and the strain gradient ratio, that is, the line obtained by plotting the fracture elongation on the vertical axis and the strain gradient ratio on the horizontal axis as shown in Figure 5, is called the "fracture limit line". The fracture limit line may be approximated by a straight line, for example. In addition, since the fracture limit line is considered to be specific to a material, by obtaining the fracture limit property, it is possible to obtain the limit fracture elongation for each strain field (circumferential strain gradient and radial strain gradient) of the material.
[0037] By using the breaking elongation limit line, it is possible to obtain the breaking elongation for any strain gradient ratio. In addition, it is possible to obtain the breaking elongation limit line under fewer test specimen shape conditions, as long as the correlation between the breaking elongation and the strain gradient ratio can be obtained, without having to perform tensile tests with eight different test specimen shapes as was performed this time. In addition, if the strain gradient ratio in the actual vehicle crash test is clear, it is not necessary to perform tests under multiple test specimen shape conditions as was performed this time, and it is possible to obtain the breaking elongation by performing a tensile test with one type of test specimen shape that can reproduce the strain gradient ratio.
[0038] From the above, by performing the material evaluation test according to the present invention, it is possible to correctly evaluate and obtain the breaking limit of the material under deformation conditions that are closer to those during actual use and that are more in line with the actual conditions of a collision, which could not be obtained by conventional hole expansion tests.
[0039] [Method of determining fracture of structure] The fracture limit line obtained from the relationship between the strain gradient ratio and fracture elongation thus obtained can be applied to the fracture judgment of structures. For example, by applying it to a deformation simulation by FEM of a structure such as a car crash simulation using FEM (finite element method) or a fracture (destruction) simulation of a structure, it is possible to judge fracture according to the actual strain gradient.
[0040] For example, in a simulation using FEM analysis, it is possible to focus on a notch portion where fracture is a concern, determine the strain gradient ratio starting from the notch root and the elongation between the reference points of the notch root, and compare them with the fracture limit line obtained from the calculated fracture elongation to determine whether the element in question will fracture.
[0041] This makes it possible to perform simulations based on actual strain gradients in mechanical simulations of structures, such as automobile collision simulations and simulations of buildings during earthquakes.
[0042] [Other examples of the relationship between strain gradient ratio and breaking elongation] Relationships other than the fracture limit line can also be applied to the relationship between the strain gradient ratio and fracture elongation. For example, materials can also be evaluated from the relationship between the strain gradient starting from the element at the notch root and the maximum principal strain of the element at the notch root at fracture. In other words, the vertical axis of a two-dimensional graph with the strain gradient ratio on the horizontal axis and the fracture elongation on the vertical axis is replaced with the maximum principal strain of the element at the notch root.
[0043] Specifically, in an FEM analysis that reproduced the single-side notched tensile test described above, a graph is shown in Fig. 6, where the horizontal axis represents the strain gradient ratio between elements starting from the notch root when a tensile forced displacement (fracture elongation) is applied until the gauge length elongation at which fracture occurs in the experiment, and the vertical axis represents the maximum principal strain of the element at the notch root. As in Fig. 5, a correlation is observed between the strain gradient ratio and the maximum principal strain of the notch root element, making it possible to obtain a "fracture limit line" from the perspective of maximum principal strain. Therefore, for example, in an FEM analysis model that reproduces a crash test of an automobile body, the maximum principal strain of the element at the part where strain concentration occurs in the target component and the strain gradient ratio starting from the element are obtained, and using the material used in the component, the relationship in Figure 6 (fracture limit line shown in Figure 6) obtained in advance is used to determine whether the maximum principal strain of the element where strain concentration occurs exceeds the limit line, making it possible to determine whether the element will break or not, enabling a more accurate crash FEM analysis that also takes into account the occurrence of fracture. If the results of a hole expansion test were plotted on the same graph, they would be plotted near the intercept of the fracture limit line.
[0044] [Test piece thickness] In addition, the material evaluation method and the test piece according to the present invention are plate-shaped because they are used for uniaxial tensile testing. The thickness of the test piece is not particularly limited. If the thickness is too thick, the load applied in the tensile test becomes large and the equipment becomes large, so the thickness is preferably 4.2 mm or less, 4 mm or less, 3.8 mm or less, or 3.6 mm or less. The lower limit of the thickness is not particularly limited, but it is preferably thicker than 0.5 mm from the viewpoint of processing.
[0045] [material] There are no particular limitations on the material to be evaluated. From the viewpoint of applicability to structures, metallic materials are preferable, and ferrous materials (steel, iron alloys, ferrous special steel, stainless steel, etc.) are particularly preferable. Since this material evaluation method is particularly applicable to a variety of deformation forms such as collisions, it is practically suitable for application to steel materials, particularly high tensile steel. For example, it is suitable for material evaluation of high tensile steel with a tensile strength of 980 MPa or more, and for fracture judgment of structures made of that steel.
[0046] [Application to automobile crash simulation in combination with hole expansion tests] The parts that make up the automobile body are generally formed by press molding, and the holes and periphery of the parts are also formed by punching with a die during press molding. Therefore, damage due to punching is introduced to the plate edge of the notch formed in the punched hole and periphery, and it is said that the fracture limit starting from the plate edge changes depending on the degree of this punching damage. As a test method for evaluating the fracture limit from the plate edge that can take into account the influence of such punching damage, a hole expansion test is widely performed. Normally, a Φ10mm punch is used for punching, and the damage during punching can be changed by changing the clearance with the die. The hole expansion test is a test in which the punched hole is expanded with a conical punch, and the hole diameter at the time of fracture is expanded from the initial hole diameter to evaluate the hole expandability. Therefore, in order to make the state of punching damage the same as in this hole expanding test and to enable side-by-side evaluation, it is advisable to use the same Φ10mm punch as in the hole expanding test to punch a round hole with the same clearance to the die, then cut out a tensile test specimen so that part of the punched round hole becomes a notch with a small diameter Ra, and then perform a tensile test. The punched hole used in the hole expanding test is basically Φ10mm, but similar hole expanding tests can be performed up to about Φ30mm, so it is desirable that the radius Ra of the notch part of the tensile test specimen be 5mm or more and 15mm or less.
[0047] On the other hand, in the case of parts constituting an automobile body, instead of punching holes or peripheral parts of the parts with a die, there are cases where, for example, machining such as cutting is performed, finishing is performed after punching, or even laser trimming is performed, and in such cases, it is known that almost no damage is caused to the plate edge portion. Therefore, when evaluating a part in which a plate edge is formed by such a method, when forming the plate edge of the notch with radius Ra in the test piece shape for the tensile test, the same processing method as the processing method for the plate edge of the part to be evaluated may be used. [Industrial Applicability]
[0048] The present invention can be used in all industrial fields, such as material evaluation and fracture determination of structures using the materials, etc. In particular, the present invention can be applied to fracture determination in the event of a car collision or a structure fracture determination due to an earthquake or the like. [Explanation of symbols]
[0049] 1 Test piece 2. Test piece width 3 Notched bottom
Claims
1. A material evaluation method comprising the steps of: performing a uniaxial tensile test in which a plate-shaped test piece for a uniaxial tensile test has a notch with a tip radius Ra on one side in the width direction of the test piece; and the other side of the test piece is an arc with a radius Rb, and Ra and Rb satisfy the relationship in the following formula 1; and applying a tensile force to both ends in the longitudinal direction of the test piece. 2Ra≦Rb...(Formula 1)
2. 2. The material evaluation method according to claim 1, further comprising the steps of: determining a fracture elongation, which is the gage-to-point elongation of the test piece when a crack initiates from the tip of the notch; and determining a radial strain gradient and a circumferential strain gradient, which are gradients of the maximum principal strain in the radial direction and the circumferential direction of the notch at the tip of the notch, respectively; obtaining a relationship between the fracture elongation and a strain gradient ratio (circumferential strain gradient / radial strain gradient), which is the ratio of the circumferential strain gradient to the radial strain gradient.
3. 3. The material evaluation method according to claim 2, wherein the radial strain gradient and the circumferential strain gradient are determined by FEM (finite element method) analysis.
4. 4. The material evaluation method according to claim 2 or 3, wherein the relationship between the strain gradient ratio and the fracture elongation is a fracture limit line obtained in a two-dimensional graph with the fracture elongation on the vertical axis and the strain gradient ratio on the horizontal axis.
5. A method for determining whether a structure will break in a deformation simulation by FEM, the method comprising: determining whether the structure will break from the relationship between the strain gradient ratio and the breaking elongation as described in claim 2 or 3.
6. A method for determining whether a structure will break in a deformation simulation by FEM, the method comprising: determining whether the structure will break from the relationship between the strain gradient ratio and the breaking elongation as described in claim 4.
7. 5. A method for determining whether an element of a structure will break in a deformation simulation by FEM of the structure, using a fracture limit line obtained as a relationship between the strain gradient ratio and the maximum principal strain of the element at the notch bottom when the fracture elongation is applied in an FEM analysis, in which the vertical axis of the two-dimensional graph described in claim 4 is replaced with the maximum principal strain of the element at the notch bottom when the fracture elongation is applied in an FEM analysis.
8. A test piece for a uniaxial tensile test, the test piece being in the form of a plate, having a notch with a tip radius Ra on one side in the width direction, and the other side of the test piece being in the form of a circular arc with a radius Rb, wherein Ra and Rb satisfy the relationship of the following formula 1. 2Ra≦Rb...(Formula 1)
9. The test piece according to claim 8, which is a steel plate having a tensile strength of 980 MPa or more.
Citation Information
Patent Citations
Impact test tool and method suitable for aircraft component
CN114778057A
Fatigue test piece for nonlinear ultrasonic detection and detection method thereof
CN115628953A
Uniaxial tensile sample of spindle head notch for material tensile experiment
CN216594400U
High tensile strength hot rolled steel plate excellent in elongation flanging property and fatigue characteristic and its production
JP2000297349A
Estimation method for stretch-flange crack in consideration of strain gradient and judging system of stretch-flange crack in press forming simulation
JP2010069533A