Binder for lithium ion secondary battery negative electrode, slurry composition for lithium ion secondary battery negative electrode, negative electrode for lithium ion secondary battery, and lithium ion secondary battery
A binder for lithium ion secondary battery negative electrodes, composed of a (meth)acrylic acid monomer and crosslinkable polymer, addresses the performance degradation issue by enhancing adhesion and stability, thereby improving battery performance and reducing environmental impact.
Patent Information
- Application Number
- JP2023059383
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Lithium ion secondary batteries using silicon-based materials for negative electrodes face issues with high expansion and contraction rates during lithium ion intercalation and deintercalation, leading to separation between the electrode and the composite material layer, resulting in a sudden drop in performance.
A binder for lithium ion secondary battery negative electrodes containing a structural unit derived from a (meth)acrylic acid monomer and a crosslinkable polymer with a weight average molecular weight of 50,000 to 2,500,000, crosslinked with a crosslinking group, providing superior binding strength and dispersion stability in water.
The binder composition enhances electrode adhesion and maintains high dispersion stability, improving the performance and reducing environmental impact.
Smart Images

Figure 2024146469000001 
Figure 2024146469000002 
Figure 2024146469000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a binder for a lithium ion secondary battery negative electrode, a slurry composition for a lithium ion secondary battery negative electrode, a lithium ion secondary battery negative electrode, and a lithium ion secondary battery. [Background technology]
[0002] Secondary batteries include lead-acid batteries, nickel-metal hydride secondary batteries, lithium-ion secondary batteries, etc. Among these, lithium-ion secondary batteries have a high energy density and a high capacity, and therefore are used in a wide range of applications.
[0003] Lithium-ion secondary batteries are composed of a positive electrode, a negative electrode, and an electrolyte, and charge and discharge are performed by the movement of lithium ions between the positive and negative electrodes via the electrolyte. Although lithium-ion secondary batteries have the characteristics of high energy density and high capacity, development is being carried out to further increase the energy density and capacity for application in automotive applications such as hybrid cars. For example, carbon-based materials such as graphite and hard carbon are commonly used for the negative electrode active material, which is a component of the negative electrode, but development of higher-capacity silicon-based materials is underway. Silicon-based materials have a capacity more than 10 times higher than carbon-based materials and show a relatively low operating potential. However, silicon-based materials have a high expansion and contraction rate during the process of absorbing and desorbing lithium ions, and peeling occurs between the electrode and the composite layer containing the negative electrode active material every time the battery is charged and discharged, resulting in a rapid deterioration in performance.
[0004] In response to these issues, efforts are being made to develop binder components that have stronger adhesion to electrodes. For example, Patent Document 1 proposes that the dry strength and wet strength of electrodes can be improved by using a copolymer binder that contains units derived from a vinyl monomer, units derived from a conjugated diene monomer or a conjugated diene polymer, units derived from a (meth)acrylic acid ester monomer, and units derived from a water-soluble polymer.
[0005] Furthermore, Patent Document 2 proposes a slurry for the negative electrode of a lithium ion secondary battery, which contains a negative electrode active material containing 20 mass % or more of silicon particles having a specific median size, a radical copolymer of a monomer group including a (meth)acrylamide skeleton-containing monomer and a sulfonic acid group-substituted unsaturated hydrocarbon group-containing monomer, and water. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 7034407 [Patent Document 2] JP 2018-006334 A Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a binder for a negative electrode of a lithium ion secondary battery having superior binding strength and high dispersion stability in water, and a slurry composition for a negative electrode of a lithium ion secondary battery using the binder, a negative electrode for a lithium ion secondary battery, and a lithium ion secondary battery. [Means for solving the problem]
[0008] As a result of extensive investigations to achieve the above object, the present inventors have found that a binder for a lithium ion battery negative electrode containing at least a constituent unit derived from a (meth)acrylic acid monomer and a constituent unit derived from a crosslinkable polymer having a crosslinking group and a weight average molecular weight of 50,000 to 2,500,000 has excellent adhesive strength with the electrode, and have completed the present invention.
[0009] The aspects of the present invention are as follows. Item 1: A binder for a lithium ion secondary electrode comprising at least a structural unit (A) derived from a (meth)acrylic acid monomer and a structural unit (B) derived from a crosslinkable polymer having a crosslinking group and a weight average molecular weight of 50,000 to 2,500,000, and crosslinking these; A binder for a lithium ion secondary electrode negative electrode, wherein the content of the structural unit (B) is 0.005 to 4 mass % based on 100 mass % of the binder for a lithium ion secondary electrode negative electrode. Item 2. The binder for a lithium ion secondary battery negative electrode according to Item 1, wherein the crosslinking group of the structural unit (B) is an allyl group. Item 3. A slurry composition for a lithium ion secondary battery negative electrode, comprising at least the binder for a lithium ion secondary battery negative electrode according to item 1, an aqueous solvent, and a negative electrode active material made of a carbon material and / or a silicon compound. Item 4. A negative electrode for a lithium ion secondary battery, produced using the slurry composition for a lithium ion secondary battery negative electrode according to item 3. Item 5. A lithium ion secondary battery produced by using the negative electrode for lithium ion secondary batteries according to item 4. Effect of the Invention
[0010] The binder composition for a lithium ion secondary battery negative electrode of the present invention can provide a binder for a lithium ion secondary battery negative electrode that has excellent binding properties with an electrode and has high dispersion stability in water, which enables a reduction in the environmental load. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The binder for lithium ion secondary battery negative electrodes of the present invention contains at least a constituent unit derived from a (meth)acrylic acid monomer and a constituent unit derived from a crosslinkable polymer having a crosslinking group and a weight average molecular weight of 50,000 to 2,500,000.
[0012] <Binder for negative electrodes of lithium-ion secondary batteries> The binder for a lithium ion secondary battery negative electrode of the present invention (hereinafter, may be also referred to as a binder) is a binder containing at least a structural unit (A) derived from a (meth)acrylic acid monomer, a structural unit (B) derived from a crosslinkable polymer having a crosslinking group and a weight average molecular weight of 50,000 to 2,500,000, and, if necessary, a structural unit (C) derived from a (meth)acrylic acid alkyl ester monomer, The following general formula (1) [ka] (In the formula, R 1 is hydrogen or an alkyl group having 1 to 4 carbon atoms; R 2 is an aromatic group which may have a substituent. A structural unit (D) derived from a monomer represented by A structural unit (E) derived from a reactive monomer having at least one member selected from the group consisting of an epoxy group, a (blocked) isocyanate group, and a urethane group; The following general formula (3) [ka] (In the formula, R 15 is a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, x is an integer of 2 to 8, and n is an integer of 2 to 30. The binder for the negative electrode of a lithium ion secondary battery contains a structural unit (F) derived from a monomer represented by the following formula:
[0013] Examples of the structural unit (A) derived from a (meth)acrylic acid monomer include structural units derived from a compound selected from acrylic acid, methacrylic acid, crotonic acid, itaconic acid, maleic acid, and fumaric acid. Among these, acrylic acid and methacrylic acid are preferable. The structural unit (A) contained in the polymer may be one type or two or more types. It is preferable to include the structural unit (A) derived from a (meth)acrylic acid monomer in terms of improving the affinity with the active material when used in an electrode.
[0014] In 100% by mass of the binder of the present invention, the content of the structural unit (A) derived from a (meth)acrylic acid monomer is preferably 3 to 99.99% by mass. More specifically, the lower limit is preferably 3% by mass or more, more preferably 4% by mass or more, and even more preferably 5% by mass or more. The upper limit is preferably 99.99% by mass or less, more preferably 99.95% by mass or less, and even more preferably 99.9% by mass or less.
[0015] Examples of the structural unit (B) derived from a crosslinkable polymer having a weight average molecular weight of 50,000 to 2,500,000 and having a crosslinking group include crosslinkable polymers in which unsaturated hydrocarbon groups such as vinyl groups, acryloyl groups, methacryloyl groups, and allyl groups, halogen groups such as chloro groups and bromo groups, and cyclic ether groups such as epoxide, oxetane, and tetrahydrofuran have been introduced as crosslinking groups into the side chains of copolymers containing alkylene oxides such as ethylene oxide, propylene oxide, and n-butylene oxide, and glycidyl ethers such as methyl glycidyl ether, methoxyethoxyethyl glycidyl ether, and 2-(2-methoxyethoxy)ethyl glycidyl ether as structural units.
[0016] Among these, a crosslinkable polymer in which the above-mentioned unsaturated hydrocarbon group, halogen group, or cyclic ether group has been introduced as a crosslinking group into the side chain of a copolymer consisting of at least one type selected from ethylene oxide (sometimes written as EO), propylene oxide (sometimes written as PO), and 2-(2-methoxyethoxy)ethyl glycidyl ether (sometimes written as EM2) is preferable, a crosslinkable polymer in which an unsaturated hydrocarbon group has been inserted into the side chain of the copolymer is more preferable, and a crosslinkable polymer in which an allyl group has been introduced into the side chain of the copolymer is even more preferable.
[0017] Specific examples of crosslinkable polymers having allyl groups introduced into the side chains of copolymers consisting of at least one type selected from ethylene oxide, propylene oxide, and 2-(2-methoxyethoxy)ethyl glycidyl ether include allyl glycidyl ether (sometimes also referred to as AGE) as the allyl group in the side chain, and include EO-AGE copolymer, PO-AGE copolymer, EM2-AGE copolymer, EO-PO-AGE copolymer, EO-EM2-AGE copolymer, PO-EM2-AGE copolymer, EO-PO-EM2-AGE copolymer, etc. In the present invention, EO-PO-AGE copolymer and EO-EM2-AGE copolymer are preferred.
[0018] In 100% by mass of the EO-PO-AGE copolymer, the content of ethylene oxide is preferably 89 to 98% by mass, more preferably 90 to 97% by mass, and even more preferably 91 to 95% by mass. The content of propylene oxide is preferably 1 to 10% by mass, more preferably 2 to 8% by mass, and even more preferably 3 to 7% by mass. The content of allyl glycidyl ether is preferably 0.1 to 5% by mass, more preferably 0.3 to 4% by mass, and even more preferably 0.5 to 3% by mass.
[0019] In 100% by mass of the EO-EM2-AGE copolymer, the content of ethylene oxide is preferably 12% by mass to 95% by mass, more preferably 22% by mass to 85% by mass, and even more preferably 32% by mass to 75% by mass. The content of 2-(2-methoxyethoxy)ethyl glycidyl ether is preferably 3% by mass to 80% by mass, more preferably 13% by mass to 70% by mass, and even more preferably 23% by mass to 60% by mass. The content of allyl glycidyl ether is preferably 0.5% by mass to 31% by mass, more preferably 1% by mass to 20% by mass, and even more preferably 2% by mass to 10% by mass.
[0020] In addition, a crosslinkable resin can be used as a constituent unit derived from a crosslinkable polymer having a weight average molecular weight of 50,000 to 2,500,000 and having a crosslinking group, and examples thereof include acrylic resin, epoxy resin, epoxy-acrylate copolymer resin, urethane resin, ethylene resin, urethane-acrylic copolymer resin, melamine resin, phenol resin, urea resin, urea resin, urea-melamine copolymer resin, diallyl phthalate resin, etc. Among these, diallyl phthalate resin is preferable.
[0021] The weight-average molecular weight of the crosslinkable polymer having a crosslinking group and a weight-average molecular weight of 50,000 to 2,500,000 is preferably 50,000 to 2,500,000. More specifically, the lower limit is preferably 50,000 or more, more preferably 60,000 or more, and even more preferably 70,000 or more. The upper limit is preferably 2,500,000 or less, more preferably 2,000,000 or less, even more preferably 1,500,000 or less, and particularly preferably 1,000,000 or less. If it is within these ranges, the crosslink density becomes gentle, and flexibility can be imparted to the binder.
[0022] In 100% by mass of the binder of the present invention, the constituent unit (B) derived from a crosslinkable polymer having a weight average molecular weight of 50,000 to 2,500,000 and having a crosslinking group is preferably 0.005 to 4% by mass. More specifically, the lower limit is preferably 0.005% by mass or more, more preferably 0.01% by mass or more, even more preferably 0.05% by mass or more, and particularly preferably 0.1% by mass or more. The upper limit is preferably 4% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less. If it is lower than the lower limit, binding property tends to be not obtained, and if it is higher than the upper limit, water solubility tends to be not maintained.
[0023] The structural unit (C) derived from a (meth)acrylic acid alkyl ester monomer is preferably a structural unit derived from a (meth)acrylic acid alkyl ester monomer having an alkyl group having 1 to 22 carbon atoms, more preferably a structural unit derived from a (meth)acrylic acid alkyl ester monomer having an alkyl group having 2 to 18 carbon atoms, and particularly preferably a structural unit derived from a (meth)acrylic acid alkyl ester monomer having an alkyl group having 4 to 18 carbon atoms.
[0024] Preferred specific examples include structural units derived from alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, and stearyl (meth)acrylate. The structural unit (C) may be one type or two or more types.
[0025] In 100% by mass of the binder of the present invention, the content of the structural unit (C) derived from a (meth)acrylic acid alkyl ester monomer is preferably 0 to 65% by mass. More specifically, the lower limit is preferably 0% by mass or more, more preferably 10% by mass or more, and even more preferably 30% by mass or more. The upper limit is preferably 65% by mass or less, more preferably 60% by mass or less, and even more preferably 55% by mass or less. Within these ranges, swelling with respect to the electrolytic solution is suppressed.
[0026] In the structural unit (D) derived from the following general formula (1), R 1 R is hydrogen or an alkyl group having 1 to 4 carbon atoms, preferably hydrogen or an alkyl group having 1 to 2 carbon atoms, and particularly preferably hydrogen or a methyl group. 2 is an aromatic group which may have a substituent, and examples of the substituent include alkyl groups such as methyl, ethyl, and isopropyl groups, unsaturated hydrocarbon groups such as vinyl groups, halogeno groups such as fluoro, chloro, bromo, and iodo groups, amino groups, nitro groups, and carboxyl groups. The aromatic ring may have two or more rings. [ka] (In the formula, R 1 is hydrogen or an alkyl group having 1 to 4 carbon atoms; R 2 is an aromatic group which may have a substituent.
[0027] More specifically, the structural unit derived from the general formula (1) is represented by the following general formula (2): [ka] (wherein R1 is hydrogen or an alkyl group having 1 to 4 carbon atoms, R12 is an alkylene group having 1 to 3 carbon atoms or a carbonyl group, and R13 is -ph-(W)-ph. -ph is a phenyl group which may have a substituent, W is any of a single bond, -O-, or an alkylene group, t and u are integers of 0 to 3, and s is an integer of 0 to 1).
[0028] In the structural unit derived from general formula (2), R1 is hydrogen or an alkyl group having 1 to 4 carbon atoms, preferably hydrogen or an alkyl group having 1 to 2 carbon atoms, and particularly preferably hydrogen or a methyl group. R12 is an alkylene group having 1 to 3 carbon atoms or a carbonyl group, preferably an alkylene group having 1 to 2 carbon atoms or a carbonyl group. R13 is -ph-(W)-ph. -ph is a phenyl group which may have a substituent, and W is any one of a single bond, -O-, or an alkylene group, and the alkylene group is preferably an alkylene group having 1 to 3 carbon atoms. Examples of the substituent include alkyl groups, such as methyl, ethyl, and isopropyl alkyl groups, unsaturated hydrocarbon groups such as vinyl, halogeno groups such as fluoro, chloro, bromo, and iodo groups, amino groups, nitro groups, and carboxyl groups. s is an integer of 0 or 1. t and u are integers of 0 to 3, preferably 0 to 2, and both may be 0.
[0029] Specific examples of the structural unit derived from general formula (1) include structural units based on benzyl (meth)acrylate, phenoxymethyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, neopentyl glycol-(meth)acrylic acid-benzoic acid ester, 2-(meth)acryloyloxyethyl-phthalic acid, etc. The structural unit based on general formula (1) may be of one type or of two or more types.
[0030] In 100% by mass of the binder of the present invention, the content of the structural unit (D) derived from general formula (1) is preferably 0 to 60% by mass. More specifically, the lower limit is preferably 0% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more. The upper limit is preferably 60% by mass or less, more preferably 50% by mass or less, and particularly preferably 45% by mass or less. This range is preferable in that the affinity between the current collector and the active material is improved when used in an electrode.
[0031] The structural unit (E) derived from a reactive monomer having at least one selected from the group consisting of an epoxy group, a (blocked) isocyanate group, and a urethane group is preferably a structural unit derived from a reactive monomer having an epoxy group. This structural unit may be of one type or of two or more types.
[0032] Examples of structural units derived from monomers having an epoxy group include allyl glycidyl ether, glycidyl acrylate, glycidyl methacrylate, and 4-hydroxybutyl acrylate glycidyl ether.
[0033] Examples of structural units derived from a monomer having a (blocked) isocyanate group include structural units derived from 2-methacryloyloxyethyl isocyanate, 2-acryloyloxyethyl isocyanate, 2-[0-(1'-methylpropylideneamino)carboxyamino]ethyl methacrylate, 2-[(3,5-dimethylpyrazolyl)carbonylamino]ethyl methacrylate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate, and 2-(2-methacryloyloxyethyloxy)ethyl isocyanate.
[0034] Examples of structural units derived from monomers having a urethane group include pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer, phenyl glycidyl ether acrylate hexamethylene diisocyanate urethane prepolymer, pentaerythritol triacrylate toluene diisocyanate urethane prepolymer, pentaerythritol triacrylate isophorone diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate hexamethylene diisocyanate urethane prepolymer, and the like.
[0035] In 100% by mass of the binder of the present invention, the content of the structural unit (E) derived from a monomer having at least one selected from the group consisting of an epoxy group, a (blocked) isocyanate group, and a urethane group is preferably 0 to 10% by mass. More specifically, the lower limit is preferably 0% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more. The upper limit is preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 6% by mass or less.
[0036] In the structural unit (F) derived from a monomer having a hydroxyl group represented by the following general formula (3), R 15Preferred examples of R include a hydrogen atom, a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, and an isobutyl group. A hydrogen atom or a methyl group is preferable. That is, in the structural unit (F), the monomer having a hydroxyl group is (R 15 is a hydrogen atom or a methyl group. [ka] (In the formula, R 15 is a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, x is an integer of 2 to 8, and n is an integer of 2 to 30.
[0037] In the general formula (3), (C x H 2x O) is a linear or branched alkyl ether group; x is an integer of 2 to 8, preferably an integer of 2 to 7, and more preferably an integer of 2 to 6.
[0038] In formula (3), n is an integer of 2 to 30, preferably an integer of 2 to 25, and more preferably an integer of 2 to 20.
[0039] The structural unit (F) derived from a monomer having a hydroxyl group represented by general formula (3) is preferably derived from a monomer having a hydroxyl group represented by general formula (4). [ka] In the general formula (4), R 15is a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, o is an integer from 0 to 30, p is an integer from 0 to 30, and o+p is 2 to 30. Here, o and p merely represent the constituent ratio of the constituent units, and do not mean only compounds consisting of blocks of (C2H4O) repeating units and blocks of (C3H6O) repeating units, but may also be compounds in which the (C2H4O) repeating units and the (C3H6O) repeating units are arranged alternately or randomly, or compounds in which random portions and block portions are mixed.
[0040] In the general formula (4), R 15 Preferred examples of R include a hydrogen atom, a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, and an isobutyl group. A hydrogen atom or a methyl group is preferable. That is, in the structural unit (F), the monomer having a hydroxyl group is (R 15 is a hydrogen atom or a methyl group.
[0041] In general formula (4), o is an integer of 0 to 30, p is an integer of 0 to 30, and o+p is 2 to 30, it is preferable that o is an integer of 0 to 25, p is an integer of 0 to 25, and o+p is 2 to 25, and it is preferable that o is an integer of 0 to 20, p is an integer of 0 to 20, and o+p is 2 to 20.
[0042] Examples of the structural unit derived from a monomer having a hydroxyl group represented by general formula (3) include diethylene glycol mono(meth)acrylate, triethylene glycol mono(meth)acrylate, tetraethylene glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, dipropylene glycol mono(meth)acrylate, tripropylene glycol mono(meth)acrylate, tetrapropylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polyethylene glycol-propylene glycol-mono(meth)acrylate, polyethylene glycol-tetramethylene glycol-mono(meth)acrylate, etc. These can be used alone or in combination of two or more. Among these, tetraethylene glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, tetrapropylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate are preferred. These may be one type or two or more types.
[0043] In 100% by mass of the binder of the present invention, the content of the structural unit (F) based on the monomer having a hydroxyl group represented by the general formula (3) is preferably 0 to 15% by mass. More specifically, the lower limit is preferably 0% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more. The upper limit is preferably 15% by mass or less, more preferably 12% by mass or less, and even more preferably 10% by mass or less.
[0044] The weight average molecular weight of the binder of the present invention is preferably 50,000 to 5,000,000. More specifically, the lower limit is preferably 50,000 or more, more preferably 100,000 or more, and even more preferably 150,000 or more. The upper limit is preferably 5,000,000 or less, more preferably 2,500,000 or less, and even more preferably 2,000,000 or less. If the molecular weight is within these ranges, there is a tendency for improved binding property, solubility in water, and dispersion stability to be improved.
[0045] The binder of the present invention may contain, in addition to the above-mentioned structural units, structural units derived from other monomers copolymerizable therewith, to the extent that the object of the present invention is not exceeded. Examples of the other structural units include structural units derived from ethylenically unsaturated nitriles, structural units derived from (meth)acrylamide monomers, structural units derived from aromatic vinyl monomers, structural units derived from conjugated diene monomers, structural units derived from non-conjugated diene monomers, and structural units derived from other olefins.
[0046] In the present invention, when structural units derived from these other copolymerizable monomers are contained, their content in all structural units is preferably 0 to 45 mass%, more preferably 0 to 20 mass%, and even more preferably 0 to 10 mass%.
[0047] <Method for producing binder for negative electrode of lithium ion secondary battery> The binder of the present invention can be produced by polymerizing various copolymerizable monomers and crosslinkable polymers. The copolymerizable monomers and crosslinkable polymers used may be commercially available products and are not particularly limited.
[0048] As the form of the polymerization reaction, any of emulsion polymerization, suspension polymerization, bulk polymerization, and solution polymerization can be used. From the viewpoint of ease of control of the polymerization reaction, it is preferable to use emulsion polymerization under normal pressure, and in the case of using a water-insoluble crosslinkable polymer, it is preferable to use solution polymerization.
[0049] In the case of emulsion polymerization, a general emulsion polymerization method, a soap-free emulsion polymerization method, a seed polymerization method, a method of swelling a seed particle with a monomer, etc., and then polymerizing the same can be used. Specifically, a composition containing a copolymerizable monomer, a crosslinkable polymer, an emulsifier, a polymerization initiator, water, and, if necessary, a dispersant, a chain transfer agent, a pH adjuster, etc., is stirred at room temperature in a sealed container equipped with a stirrer and a heater under an inert gas atmosphere to emulsify the copolymerizable monomer, the crosslinkable polymer, etc. in water. The emulsification method can be a method using stirring, shearing, ultrasonic waves, etc., and a stirring blade, a homogenizer, etc. can be used. Next, the temperature is raised while stirring to start polymerization, thereby obtaining a latex of a spherical polymer in which the polymer is dispersed in water. In addition, the spherical polymer thus produced may be separately isolated and then dispersed in an organic solvent such as N-methylpyrrolidone using a dispersant, etc. for use. Furthermore, there is also a method of dispersing the polymer again in water using a monomer, an emulsifier, a dispersant, etc. to obtain a latex of a polymer. The method of adding the monomer during polymerization may be a lump-sum charge, a monomer dropwise addition, a pre-emulsion dropwise addition, or the like, and two or more of these methods may be used in combination.
[0050] The particle structure of the polymer in the binder of the present invention is not particularly limited. For example, a polymer latex containing composite polymer particles with a core-shell structure produced by seed polymerization can be used. The seed polymerization method can be, for example, the method described in "Chemistry of Dispersion and Emulsion Systems" (published by Kogaku Tosho Co., Ltd.). Specifically, this method is a method in which a monomer, a polymerization initiator, and an emulsifier are added to a system in which seed particles produced by the above method are dispersed, and core particles are grown, and the above method may be repeated one or more times.
[0051] The seed polymerization may employ particles using the polymer of the present invention or known polymers. Examples of known polymers include, but are not limited to, polyethylene, polypropylene, polyvinyl alcohol, polystyrene, poly(meth)acrylate, and polyether, and other known polymers may be used. Also, one type of homopolymer or two or more types of copolymers or blends may be used.
[0052] The particle shape of the polymer in the binder of the present invention may be, in addition to a spherical shape, a plate shape, a hollow structure, a composite structure, a localized structure, a daruma-shaped structure, an octopus-shaped structure, a raspberry-shaped structure, etc., and particles of two or more types of structures and compositions may be used without departing from the scope of the present invention.
[0053] The emulsifier used in the present invention is not particularly limited, and nonionic emulsifiers and anionic emulsifiers that are generally used in emulsion polymerization methods can be used. Examples of nonionic emulsifiers include polyoxyethylene alkyl ethers, polyoxyethylene alcohol ethers, polyoxyethylene alkyl phenyl ethers, polyoxyethylene polycyclic phenyl ethers, polyoxyalkylene alkyl ethers, sorbitan fatty acid esters, polyoxyethylene fatty acid esters, and polyoxyethylene sorbitan fatty acid esters, and examples of anionic emulsifiers include alkylbenzene sulfonates, alkyl sulfates, polyoxyethylene alkyl ether sulfates, fatty acid salts, and the like, and these may be used alone or in combination. Representative examples of anionic emulsifiers include sodium dodecyl sulfate, sodium dodecyl benzene sulfonate, and triethanolamine lauryl sulfate.
[0054] The amount of the emulsifier used in the present invention may be any amount generally used in emulsion polymerization, specifically, in the range of 0.01 to 10% by weight, preferably 0.05 to 5% by weight, and more preferably 0.05 to 3% by weight, based on the amount of the charged monomer.
[0055] The polymerization initiator used in the present invention is not particularly limited, and polymerization initiators generally used in emulsion polymerization methods can be used. Specific examples thereof include water-soluble polymerization initiators such as persulfates, such as potassium persulfate, sodium persulfate, and ammonium persulfate, oil-soluble polymerization initiators such as cumene hydroperoxide and diisopropylbenzene hydroperoxide, hydroperoxides, 4-4'-azobis(4-cyanovaleric acid), 2-2'-azobis[2-(2-imidazolin-2-yl)propane, 2-2'-azobis(propane-2-carboxamidine) Examples of the polymerization initiator include azo initiators such as 2-2'-azobis[N-(2-carboxyethyl)-2-methylpropanamide, 2-2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}, 2-2'-azobis(1-imino-1-pyrrolidino-2-methylpropane) and 2-2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propanamide}, and redox initiators. These polymerization initiators may be used alone or in combination of two or more.
[0056] The amount of the polymerization initiator used in the present invention may be an amount generally used in emulsion polymerization, specifically, in the range of 0.05 to 10 mol %, preferably 0.1 to 5 mol %, and more preferably 0.2 to 3 mol %, based on 100 mol % of the charged monomer.
[0057] The water used in preparing the binder of the present invention is not particularly limited, and any commonly used water can be used. Specific examples of water include tap water, distilled water, ion-exchanged water, and ultrapure water. Among these, distilled water, ion-exchanged water, and ultrapure water are preferred.
[0058] In the present invention, a dispersant can be used as necessary, and the type and amount of the dispersant used are not particularly limited, and any amount of a commonly used dispersant can be freely used. Specific examples include sodium hexametaphosphate, sodium tripolyphosphate, sodium pyrophosphate, and sodium polyacrylate.
[0059] In the present invention, a chain transfer agent can be used as necessary. Specific examples of the chain transfer agent include alkyl mercaptans such as n-hexyl mercaptan, n-octyl mercaptan, t-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, and n-stearyl mercaptan, xanthogen compounds such as 2,4-diphenyl-4-methyl-1-pentene, 2,4-diphenyl-4-methyl-2-pentene, dimethyl xanthogen disulfide, and diisopropyl xanthogen disulfide, terpinolene, tetramethyl thiuram disulfide, tetraethyl thiuram disulfide, and tetramethyl thiuram monosulfide. Thiuram compounds, phenolic compounds such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol, allyl compounds such as allyl alcohol, halogenated hydrocarbon compounds such as dichloromethane, dibromomethane and carbon tetrabromide, vinyl ethers such as α-benzyloxystyrene, α-benzyloxyacrylonitrile and α-benzyloxyacrylamide, triphenylethane, pentaphenylethane, acrolein, methacrolein, thioglycolic acid, thiomalic acid, 2-ethylhexyl thioglycolate, etc., may be used alone or in combination. The amount of these chain transfer agents is not particularly limited, but is usually 0 to 5 parts by weight per 100 parts by weight of the charged monomer.
[0060] The polymerization time and temperature are not particularly limited and can be appropriately selected depending on the type of polymerization initiator used, but generally, the polymerization temperature is 20 to 100° C. and the polymerization time is 0.5 to 100 hours.
[0061] Furthermore, the pH of the polymer obtained by the above method can be adjusted as necessary by using a base as a pH adjuster. Specific examples of the base include alkali metal (Li, Na, K, Rb, Cs) hydroxides, ammonia, inorganic ammonium compounds, organic amine compounds, etc. The pH range is pH 1 to 11, preferably pH 2 to 11, more preferably pH 2 to 10, for example pH 3 to 10, particularly pH 5 to 9.
[0062] The particle size of the polymer in the binder of the present invention can be measured by dynamic light scattering, transmission electron microscopy, optical microscopy, etc. The average particle size calculated from the scattering intensity obtained by dynamic light scattering is 0.001 μm to 1 μm, preferably 0.001 μm to 0.500 μm. A specific example of a measuring device is Zetasizer Nano manufactured by Spectris.
[0063] After the polymerization reaction is completed, the polymerization solution can be used as it is, or the produced polymer can be isolated from the reaction solution by a known method such as reprecipitation, solvent distillation, etc. The obtained polymer can also be used after purification by removing unreacted monomers, etc., by reprecipitation, membrane separation, chromatography, extraction, etc.
[0064] When the solution polymerization method is used, the organic solvent used in the present invention is not particularly limited, and any organic solvent generally used in the solution polymerization method can be used. A polar organic solvent is preferable, and examples of the organic solvent include aliphatic alcohols, ketones, ethers, and esters.
[0065] Examples of the aliphatic alcohols include aliphatic alcohols having an alkyl group having 1 to 3 carbon atoms, and more specific examples include methanol, ethanol, n-propanol, and isopropanol.
[0066] More specific examples include ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; ethers such as diethyl ether and tetrahydrofuran; and esters such as ethyl acetate, butyl acetate, and γ-butyrolactone.
[0067] In the present invention, the solid content concentration during solution polymerization is preferably 0.5 to 80% by mass, more specifically, the lower limit is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 5% by mass or more, and the upper limit is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less.
[0068] The polymerization initiator used in the present invention is not particularly limited, and any polymerization initiator generally used in solution polymerization methods can be used. Specific examples of such initiators include known polymerization initiators such as azo compounds such as 2,2'-azobisisobutyronitrile and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), and organic peroxides such as t-butyl peroxyoctoate and benzoyl peroxide.
[0069] The amount of the polymerization initiator used in the present invention may be an amount generally used in solution polymerization, specifically, in the range of 0.05 to 10 mol %, preferably 0.1 to 5 mol %, and more preferably 0.2 to 3 mol %, based on the total amount of the charged constitutional units.
[0070] As the polymerization chain transfer agent, known polymerization chain transfer agents such as carboxyl group-containing mercaptans such as 2-mercaptopropionic acid; alkyl mercaptans such as octanethiol; and hydroxyl group-containing mercaptans such as 2-mercaptoethanol and 3-mercapto-1,2-propanediol can be used. Furthermore, there is no limitation on the chain form of the polymerized monomers, and any of the polymerization forms such as random, block, and graft may be used.
[0071] The polymerization temperature is not particularly limited and can be appropriately selected depending on the type of polymerization initiator used, but is preferably 20 to 100° C. More specifically, the lower limit is preferably 20° C. or higher, more preferably 30° C. or higher, and even more preferably 40° C. or higher. The upper limit is preferably 100° C. or lower, more preferably 90° C. or lower, and even more preferably 80° C. or lower.
[0072] The polymerization time is not particularly limited and can be appropriately selected depending on the type of polymerization initiator used, but is preferably 0.5 to 100 hours. More specifically, the lower limit is preferably 0.5 hours or more, more preferably 2 hours or more, and even more preferably 5 hours or more. The upper limit is preferably 100 hours or less, more preferably 72 hours or less, and even more preferably 48 hours or less.
[0073] In the present invention, the polymerization atmosphere is preferably an inert gas atmosphere such as a nitrogen gas atmosphere or argon atmosphere.
[0074] After the polymerization reaction is completed, the polymerization solution can be used as it is, or the produced polymer can be isolated from the reaction solution by a known method such as reprecipitation, solvent distillation, etc. The obtained polymer can also be used after purification by removing unreacted monomers, etc., by reprecipitation, membrane separation, chromatography, extraction, etc.
[0075] <Slurry composition for lithium-ion battery negative electrodes> The slurry composition for a lithium ion secondary battery negative electrode of the present invention contains at least the binder, an aqueous solvent, and a negative electrode active material.
[0076] <Water-based solvent> The aqueous solvent used in the present invention is a general term for water alone or a mixed solvent of water and a water-soluble organic solvent. The water is not particularly limited, and examples thereof include tap water, distilled water, ion-exchanged water, and ultrapure water. Among these, distilled water, ion-exchanged water, and ultrapure water are preferred. Specific examples of the water-soluble organic solvent include alcohols such as methanol and ethanol, ketones such as acetone and methyl ethyl ketone, glycol ethers such as propylene glycol monomethyl ether, methyl cellosolve, ethyl cellosolve, and butyl cellosolve, and ethers such as 1,3-dioxolane, 1,4-dioxolane, and tetrahydrofuran.
[0077] In the slurry composition for lithium ion battery negative electrode of the present invention, the binder content (solid content concentration) is preferably 0.1 to 15% by weight, more specifically, the lower limit is preferably 0.1% by weight or more, more preferably 0.2% by weight or more, and even more preferably 0.5% by weight or more, and the upper limit is preferably 15% by weight or less, more preferably 10% by weight or less, and even more preferably 5% by weight or less.
[0078] <Negative electrode active material> The negative electrode active material used in the lithium ion secondary battery negative electrode slurry composition of the present invention is a powder of a carbon material (natural graphite, artificial graphite, amorphous carbon, etc.) having a structure (porous structure) capable of absorbing and releasing lithium ions, or a powder of a silicon-based compound. The particle size is preferably 10 nm or more and 100 μm or less, more preferably 20 nm or more and 20 μm or less. A mixed active material of a metal and a carbon material may also be used. It is preferable to use a negative electrode active material having a porosity of about 70%.
[0079] Examples of carbon materials include graphite, low-crystalline carbon (soft carbon, hard carbon), carbon black (Ketjen black, acetylene black, channel black, lamp black, oil furnace black, thermal black, etc.), fullerene, carbon nanotube, carbon nanofiber, carbon nanohorn, carbon fibril, coke, mesocarbon microbeads (MCMB), mesophase pitch-based carbon fiber, phenol resin fired body, polyacrylonitrile-based carbon fiber, etc., and graphite is preferred.
[0080] Examples of silicon-based compounds include Si element, alloys with Si, oxides containing Si, carbides containing Si, etc., such as Si, SiB4, SiB6, Mg2Si, Ni2Si, TiSi2, MoSi2, CoSi2, NiSi2, CaSi2, CrSi2, Cu5Si, FeSi2, MnSi2, NbSi2, TaSi2, VSi2, WSi2, ZnSi2, SiC, Si3N4, Si2N2O, SiO x (0 < x ≤ 2), SnSiO x , LiSiO can be exemplified, and SiO x (0 < x ≤ 2) is preferred, and it is silicon monoxide (SiO), etc.
[0081] In the negative electrode active material, it may be composed only of a carbon material or a silicon-based compound, or a carbon material and a silicon-based compound may be used in combination. When a carbon material and a silicon-based compound are used in combination, it is preferably contained as follows.
[0082] The content of the carbon material with respect to the total amount (100% by mass) of the negative electrode active material is preferably 20% by mass or more, more preferably 40% by mass or more, particularly preferably 60% by mass or more, and may be 70% by mass or more at the lower limit, and preferably 99% by mass or less, more preferably 98% by mass or less, and particularly preferably 96% by mass or less at the upper limit.
[0083] The lower limit of the content of the silicon-based compound relative to the total amount (100 mass%) of the negative electrode active material is preferably 1 mass% or more, more preferably 2 mass% or more, and particularly preferably 4 mass% or more, and the upper limit is preferably 80 mass% or less, more preferably 60 mass% or less, particularly preferably 40 mass% or less, and may be 30 mass% or less.
[0084] The activation may be performed by any known activation method, such as a gas activation method or a chemical activation method. In the gas activation method, the carbonized material is activated by contacting it with a gas such as steam, carbon dioxide, or oxygen under heating. In the chemical activation method, the carbonized material is activated by heating it in contact with a known activation chemical. Examples of the activation chemical include zinc chloride, phosphoric acid, and / or an alkali compound (metal hydroxide such as sodium hydroxide). It is preferable to use activated carbon activated with steam (referred to as steam-activated carbon in this application) and / or activated carbon activated with alkali (referred to as alkali-activated activated carbon in this application).
[0085] The content of the negative electrode active material in the slurry composition for lithium ion secondary battery negative electrode of the present invention is not particularly limited, and is preferably 10 to 70 mass %, more preferably 20 to 60 mass %, and particularly preferably 20 to 50 mass %, relative to 100 mass % of the slurry composition for lithium ion secondary battery negative electrode. The negative electrode active material may be used alone or in combination of two or more kinds.
[0086] When a conductive assistant is used, a known conductive assistant can be used, and examples of the conductive assistant include conductive carbon black such as graphite, furnace black, acetylene black, and ketjen black, carbon fibers such as carbon nanotubes (CNT), and metal powders, etc. These conductive assistants may be used alone or in combination of two or more kinds.
[0087] When a conductive assistant is used, the content of the conductive assistant is not particularly limited, but is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, relative to 100 parts by mass of the active material. The lower limit of the content of the conductive assistant is usually 0.05 parts by mass or more, 0.1 parts by mass or more, 0.2 parts by mass or more, or 0.5 parts by mass or more.
[0088] The lithium ion secondary battery negative electrode slurry composition of the present invention may contain a thickener as necessary. The type of thickener is not particularly limited, but is preferably a sodium salt or ammonium salt of a cellulose compound, polyvinyl alcohol and its salt, etc.
[0089] Examples of the sodium salt or ammonium salt of a cellulose compound include sodium salt or ammonium salt of alkylcellulose in which a cellulose polymer is substituted with various derivative groups. Specific examples include methyl cellulose, methyl ethyl cellulose, ethyl cellulose, sodium salt, ammonium salt, and triethanol ammonium salt of carboxymethyl cellulose (CMC). Sodium salt or ammonium salt of carboxymethyl cellulose is particularly preferred. These thickeners may be used alone or in combination of two or more at any ratio.
[0090] When a thickener is used, the content of the thickener is not particularly limited, but is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, relative to 100 parts by mass of the active material. When a thickener is included, the lower limit of the content of the thickener is usually 0.05 parts by mass or more, 0.1 parts by mass or more, 0.2 parts by mass or more, 0.5 parts by mass or more, or 1 part by mass or more.
[0091] Method for producing slurry composition for negative electrode of lithium ion secondary battery The slurry composition for a lithium ion secondary battery negative electrode of the present invention can be produced by a conventional method for producing a slurry composition for a lithium ion secondary battery negative electrode, but in the present invention, the most effective method can be achieved in terms of the binding property with the current collector by going through the steps shown below. That is, it is preferable to include a step of dispersing the negative electrode active material in water and a step of adding and dispersing a binder.
[0092] In the step of dispersing the negative electrode active material in an aqueous solvent, when the negative electrode active material is a solid content, the solid content concentration is preferably 10% by mass to 70% by mass, more preferably 20% by mass to 60% by mass, and further preferably 20% by mass to 50% by mass.
[0093] In the step of adding and dispersing the binder, the amount of the binder added per 100 parts by mass of the negative electrode active material is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.5 parts by mass or more, and preferably 16 parts by mass or less, more preferably 12 parts by mass or less, and even more preferably 6 parts by mass or less.
[0094] As the dispersion method in each step, any commonly used dispersion method can be used without any limitation. For example, a planetary mixer, a homodisper, a rotation-revolution type mixer, an ultrasonic homogenizer, etc. can be used.
[0095] <Negative electrodes for lithium-ion secondary batteries> The negative electrode for a lithium ion secondary battery of the present invention can be obtained by providing a negative electrode active material layer in which the slurry composition for a lithium ion secondary battery negative electrode of the present invention is applied onto a current collector.
[0096] The current collector (metal electrode substrate) used in the negative electrode of the lithium ion secondary battery of the present invention may be a known current collector. Specifically, metals such as copper, nickel, stainless steel, gold, platinum, titanium, and aluminum are used.
[0097] The method for producing the lithium ion secondary battery negative electrode is not particularly limited and may be a general method, for example, by uniformly applying the slurry composition for the lithium ion secondary battery negative electrode to a suitable thickness on the surface of a current collector by a doctor blade method, an applicator method, a silk screen method, or the like.
[0098] For example, in the doctor blade method, a slurry composition for a lithium ion secondary battery negative electrode is applied to a metal electrode substrate, and then the coating is uniformed to an appropriate thickness using a blade having a specified slit width. After the active material is applied to the electrode, the electrode is dried, for example, with hot air at 100°C or in a vacuum at 80°C to remove excess water. The dried electrode is press molded using a press device to produce an electrode material. After pressing, the electrode may be heat-treated again to remove water, solvent, emulsifier, etc.
[0099] <Lithium-ion secondary battery> The lithium ion secondary battery of the present invention is characterized by comprising the negative electrode described above in the section "Negative electrode for lithium ion secondary battery", a positive electrode serving as a counter electrode, and an electrolyte. That is, the negative electrode used in the lithium ion secondary battery of the present invention contains the slurry composition for the negative electrode of the lithium ion secondary battery of the present invention, i.e., the binder composition for the negative electrode of the lithium ion secondary battery of the present invention. Details of the negative electrode for the lithium ion secondary battery of the present invention are as described above.
[0100] <Positive electrode> The current collector used in the positive electrode of the lithium ion secondary battery of the present invention may be a known current collector. Specifically, metals such as aluminum, nickel, stainless steel, gold, platinum, and titanium are used for the positive electrode.
[0101] The positive electrode active material used in the lithium ion secondary battery of the present invention is an alkali metal-containing composite oxide having any one of the compositions AMO2, AM2O4, A2MO3, and AMBO4. A is an alkali metal, and M is a single or two or more transition metals, which may contain a non-transition metal in part. B is P, Si, or a mixture thereof. The positive electrode active material is preferably a powder, and the particle size is preferably 50 microns or less, more preferably 20 microns or less. These positive electrode active materials have an electromotive force of 3V (vs. Li / Li+) or more.
[0102] Preferred specific examples of the positive electrode active material used in lithium ion secondary batteries include LixCoO2, LixNiO2, LixMnO2, LixCrO2, LixFeO2, LixCoaMn 1-a O2, LixCoaNi 1-a O2, LixCoaCr 1-a O2, LixCoaFE -a O2, LixCoaTi 1-a O2, LixMnaNi 1-a O2, LixMnaCr 1-a O2, LixMnaFE -a O2, LixMnaTi 1-a O2, LixNiaCr 1-a O2, LixNiaFE -a O2, LixNiaTi 1-a O2, LixCraFE -a O2, LixCraTi 1-a O2, LixFeaTi 1-a O2, LixCobMncNi 1-b-C O2, LixNiaCobAlcO2, LixCrbMncNi 1-b-C O2, LixFebMncNi 1-b-C O2, LixTibMncNi 1-b-C O2, LixMn2O4, LixMndCo 2-d O4, LixMndNi 2-d O4, LixMndCr 2-d O4, LixMndFe 2-d O4, LixMndTi 2-dO4, LiyMnO3, LiyMneCo 1-e O3, LiyMneNi 1-e O3, LiyMneFE -e O3, LiyMneTi 1-e O3, LixCoPO4, LixMnPO4, LixNiPO4, LixFePO4, LixCofMn 1-f PO4, LixCofNi 1-f PO4, LixCofFE -f PO4, LixMnfNi 1-f PO4, LixMnfFE -f PO4, LixNifFE -f PO4,LiyCoSiO4, LiyMnSiO4, LiyNiSiO4, LiyFeSiO4, LiyCogMn 1-g SiO4, LiCoNi 1-g SiO4, LiCoFe -g SiO4, LiMnNi 1-g SiO4, LiMnFe -g SiO4, LiyNigFE -g SiO4, LiyCoPhSi 1-h O4, LiyMnPhSi 1-h O4, LiNiPhSi 1-h O4, LiFePhSi 1-h O4, LiCoMn 1-g PhSi 1-h O4, LiyCogNi 1-g PhSi 1-h O4, LiyCogFE -g PhSi 1-h O4, LiyMngNi 1-g PhSi 1-h O4, LiyMngFE -g PhSi 1-h O4, LiyNigFE -g PhSi 1-hO4, etc. (wherein x=0.01-1.2, y=0.01-2.2, a=0.01-0.99, b=0.01-0.98, c=0.01-0.98, b+c=0.02-0.99, d=1.49-1.99, e=0.01-0.99, f=0.01-0.99, g=0.01-0.99, h=0.01-0.99.)
[0103] Among the above-mentioned preferable positive electrode active materials for use in lithium ion secondary batteries, more preferable positive electrode active materials are specifically LixCoO2, LixNiO2, LixMnO2, LixCrO2, LixCoaNi 1-a O2, LixMnaNi 1-a O2, LixCobMncNi 1-b-C O2, LixNiaCobAlcO2, LixMn2O4, LiyMnO3, LiyMneFE -e O3, LiyMneTi 1-e O3, LixCoPO4, LixMnPO4, LixNiPO4, LixFePO4, LixMnfFE -f PO4 can be exemplified. (Here, x=0.01-1.2, y=0.01-2.2, a=0.01-0.99, b=0.01-0.98, c=0.01-0.98, but b+c=0.02-0.99, d=1.49-1.99, e=0.01-0.99, f=0.01-0.99. The above x and y values increase or decrease depending on charging and discharging.)
[0104] In order to improve the binding between the collector and the positive electrode active material, the current collector may contain a binder, and any known binder that is used for a positive electrode may be used.Specifically, fluorine-based resins such as polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, perfluoromethylvinylether-tetrafluoroethylene copolymer, polytetrafluoroethylene, and fluorine rubber, hydrocarbon elastomers such as styrene-butadiene copolymer and ethylene-propylene copolymer, polysaccharides such as carboxymethylcellulose, alginic acid, and sodium alginate, and polyimide may be used.
[0105] These materials constituting the positive electrode (hereinafter referred to as positive electrode materials) may contain water to make them into a slurry. The water is not particularly limited, and commonly used water can be used. Specific examples thereof include tap water, distilled water, ion-exchanged water, and ultrapure water. Among these, distilled water, ion-exchanged water, and ultrapure water are preferable.
[0106] When the positive electrode material is used in the form of a slurry, the solid content of the slurry is preferably 10 to 90 mass %, more preferably 20 to 85 mass %, and particularly preferably 20 to 80 mass %.
[0107] The method for preparing the positive electrode material is not particularly limited, and the binder, conductive assistant, water, etc. may be dispersed using a normal stirrer, disperser, kneader, planetary ball mill, homogenizer, etc. In order to increase the efficiency of dispersion, the material may be heated within a range that does not affect the material.
[0108] The method for producing the positive electrode is not particularly limited, and a general method can be used, which is to uniformly apply the positive electrode material to an appropriate thickness on the surface of a current collector by a doctor blade method, an applicator method, a silk screen method, or the like.
[0109] For example, in the doctor blade method, a slurry of the positive electrode material is applied to a metal electrode substrate, and then the slurry is uniformly applied to an appropriate thickness using a blade with a specified slit width. After the active material is applied to the electrode, the electrode is dried, for example, with hot air at 100°C or in a vacuum at 80°C to remove excess organic solvent and water. After drying, the electrode is press-molded using a press device to produce the electrode material. After pressing, the electrode may be heat-treated again to remove water, solvent, emulsifier, etc.
[0110] <Electrolyte> The electrolyte is not particularly limited, and a known electrolyte can be used. Specific examples of the electrolyte include a solution containing an electrolyte and a solvent, or a room temperature molten salt. The electrolyte and the solvent may each be used alone or in combination of two or more.
[0111] Examples of the electrolyte include lithium salt compounds, such as LiBF4, LiPF6, LiClO4, LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, and LiN[CF3SC(C2F5SO2)3]2, but are not limited to these.
[0112] Examples of electrolytes other than lithium salt compounds include tetraethylammonium tetrafluoroborate, triethylmonomethylammonium tetrafluoroborate, and tetraethylammonium hexafluorophosphate.
[0113] Examples of the solvent used in the electrolytic solution include organic solvents, such as aprotic organic solvents. Specifically, linear ethers such as propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, 1,2-dimethoxyethane, 1,2-diethoxyethane, γ-butyrolactone, tetrahydrofuran, 1,3-dioxolane, dipropyl carbonate, diethyl ether, sulfolane, methyl sulfolane, acetonitrile, propyl nitrile, anisole, acetate, propionate, and diethyl ether can be used, and two or more of them may be mixed and used.
[0114] Room temperature molten salts are also called ionic liquids, and are "salts" composed only of ions (anions, cations), and liquid compounds in particular are called ionic liquids.
[0115] In the present invention, the room temperature molten salt refers to a salt that is at least partially liquid at room temperature, and room temperature refers to the temperature range in which a battery is generally assumed to operate, with the upper limit being about 120°C, or in some cases about 80°C, and the lower limit being about -40°C, or in some cases about -20°C.
[0116] Known cationic species of room temperature molten salts include quaternary ammonium organic cations of pyridine, aliphatic amine, and alicyclic amine. Examples of quaternary ammonium organic cations include imidazolium ions such as dialkylimidazolium and trialkylimidazolium, tetraalkylammonium ions, alkylpyridinium ions, pyrazolium ions, pyrrolidinium ions, and piperidinium ions. In particular, imidazolium ions are preferred.
[0117] Examples of the tetraalkylammonium ion include, but are not limited to, a trimethylethylammonium ion, a trimethylethylammonium ion, a trimethylpropylammonium ion, a trimethylhexylammonium ion, a tetrapentylammonium ion, and a triethylmethylammonium ion.
[0118] Examples of alkylpyridinium ions include, but are not limited to, an N-methylpyridinium ion, an N-ethylpyridinium ion, an N-propylpyridinium ion, an N-butylpyridinium ion, a 1-ethyl-2-methylpyridinium ion, a 1-butyl-4-methylpyridinium ion, and a 1-butyl-2,4-dimethylpyridinium ion.
[0119] Examples of imidazolium ions include, but are not limited to, a 1,3-dimethylimidazolium ion, a 1-ethyl-3-methylimidazolium ion, a 1-methyl-3-ethylimidazolium ion, a 1-methyl-3-butylimidazolium ion, a 1-butyl-3-methylimidazolium ion, a 1,2,3-trimethylimidazolium ion, a 1,2-dimethyl-3-ethylimidazolium ion, a 1,2-dimethyl-3-propylimidazolium ion, and a 1-butyl-2,3-dimethylimidazolium ion.
[0120] The anion species of room temperature molten salts include halide ions such as chloride ions, bromide ions, and iodide ions, perchlorate ions, thiocyanate ions, tetrafluoroborate ions, nitrate ions, and AsF6 - , PF6 - and organic acid ions such as a stearylsulfonate ion, an octylsulfonate ion, a dodecylbenzenesulfonate ion, a naphthalenesulfonate ion, a dodecylnaphthalenesulfonate ion, and a 7,7,8,8-tetracyano-p-quinodimethane ion.
[0121] The room temperature molten salt may be used alone or in combination of two or more kinds.
[0122] Various additives can be used in the electrolyte as necessary. Examples of additives include flame retardants, flame retardants, positive electrode surface treatment agents, negative electrode surface treatment agents, and overcharge inhibitors. Examples of flame retardants and flame retardants include brominated epoxy compounds, phosphazene compounds, tetrabromobisphenol A, chlorinated paraffin and other halides, antimony trioxide, antimony pentoxide, aluminum hydroxide, magnesium hydroxide, phosphate esters, polyphosphates, and zinc borate. Examples of positive electrode surface treatment agents include inorganic compounds such as carbon and metal oxides (MgO, ZrO2, etc.), and organic compounds such as ortho-terphenyl. Examples of negative electrode surface treatment agents include vinylene carbonate, fluoroethylene carbonate, and polyethylene glycol dimethyl ether. Examples of overcharge inhibitors include biphenyl and 1-(p-tolyl)adamantane.
[0123] The method for producing the lithium ion secondary battery of the present invention is not particularly limited, and the battery is produced by a known method using a positive electrode, a negative electrode, an electrolyte, and, if necessary, a separator. For example, in the case of a coin type, the positive electrode, the separator if necessary, and the negative electrode are inserted into an outer can. The electrolyte is poured into the outer can and impregnated. Thereafter, the battery is joined to a sealing body by tab welding or the like, and the sealing body is sealed and crimped to obtain a lithium ion secondary battery. The shape of the lithium ion secondary battery is not limited, and examples thereof include a coin type, a cylindrical type, and a sheet type.
[0124] The separator prevents the positive electrode and the negative electrode from directly contacting each other and causing a short circuit in the battery, and may be made of any known material. Specific examples of the separator include porous polymer films such as polyolefin, paper, etc. As the porous polymer film, films such as polyethylene and polypropylene are preferred because they are less affected by the electrolyte. EXAMPLES
[0125] Specific embodiments for carrying out the present invention will be described below with reference to examples. However, the present invention is not limited to the following examples as long as it does not deviate from the gist of the present invention.
[0126] <Example 1> (Synthesis of negative electrode binder for lithium ion secondary batteries) 99 parts by mass of acrylic acid as the structural unit (A) and 1 part by mass of Alkox CP-A1H (manufactured by Meisei Chemical Industry Co., Ltd., EO-PO-AGE ternary copolymer, composition ratio EO:PO:AGE = 93:6:1, weight average molecular weight 110,000) as the structural unit (B) were weighed out and stirred at room temperature for 24 hours to completely dissolve Alkox CP-A1H in acrylic acid. 300 parts by mass of tetrahydrofuran and 0.03 parts by mass of 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to 100 parts by mass of the above solution, and nitrogen gas bubbling was performed to remove dissolved oxygen. Thereafter, a polymerization reaction was performed at 25 ° C. for 24 hours under a nitrogen atmosphere to obtain a binder solution for the negative electrode of a lithium ion secondary battery (solid concentration 30 wt%).
[0127] (Water dispersion stability test) The obtained binder for lithium ion secondary battery negative electrode was added to ion-exchanged water so as to be diluted 10 times, and the mixture was shaken to visually check the aqueous dispersion stability. The visual state was evaluated according to the following criteria. ◎: The binder is completely dissolved in ion-exchanged water, and no precipitate is formed after standing for one week or more. ◯: Part of the binder does not dissolve and becomes cloudy, but the dispersion remains stable for more than one week when left to stand. ×: A part of the binder does not dissolve, the solution becomes cloudy, and a precipitate accumulates within one week when left to stand.
[0128] (Preparation of slurry composition for negative electrodes of lithium ion secondary batteries) A master batch was prepared by adding 85.4 parts by mass of graphite and 10 parts by mass of SiO as negative electrode active materials, 1 part by mass of acetylene black, 0.1 parts by mass of single-walled carbon nanotubes, and 2 parts by mass of sodium carboxymethyl cellulose as conductive assistants, and further adding 183 parts by mass of water so that the solid content concentration of the slurry is 35% by mass, and stirring and mixing using a planetary mixer and homodispers. A binder solution for lithium ion secondary battery negative electrode was added to this so that the solid content of the binder for lithium ion secondary battery negative electrode was 1.5 parts by mass, and the mixture was stirred and mixed in the same manner using a rotation-revolution mixer to prepare a slurry composition for lithium ion secondary battery negative electrode.
[0129] (Preparation of negative electrodes for lithium-ion secondary batteries) The above-mentioned lithium ion secondary battery negative electrode slurry composition was applied to an electrolytic copper foil (thickness 10 μm) using a Baker-type applicator with a gap of 100 μm. After that, it was pre-dried for 15 minutes in an oven heated to 80° C., and then pressed with a roll press machine (8 kN, clearance: lower limit of the device, Tester Sangyo Co., Ltd.). Then, it was dried in a vacuum oven at 110° C. for 10 hours to prepare a lithium ion secondary battery negative electrode.
[0130] <Peel strength test> A test piece was prepared by cutting the negative electrode for lithium ion secondary batteries to a long side of 60 mm and a short side of 10 mm. Cellophane tape (Cellotape (registered trademark), Nichiban Co., Ltd.) was cut to 200 mm, and one end of the test piece was sandwiched by about 10 mm, and the remaining part was attached with a handle of about 90 mm by bonding the cellophane tape together. A double-sided tape (Nistack 02, Nichiban Co., Ltd.) was attached to the side of the negative electrode for lithium ion secondary batteries on which the slurry composition for lithium ion secondary batteries was applied (hereinafter referred to as the mixture layer) and fixed to a SUS plate. A 180-degree peel test was performed by pulling the handle to peel off the copper foil using a universal testing machine (E0-L Toyo Seiki Seisakusho Co., Ltd.) (movement distance 100 mm, 50 mm / min). The peel strength was calculated as the average of the section from 10 mm to 90 mm, excluding about 10 mm immediately after the start of the measurement and at the end, and was calculated as the average of three trials. (Calculation of the increase rate of peel strength from Comparative Example 1) The peel strength relative to Comparative Example 1 can be calculated by dividing the peel strength obtained in each Example by the peel strength obtained in Comparative Example 1, that is, according to the following formula. Peel strength increase rate (%)=(peel strength of lithium ion secondary battery negative electrode obtained in each example / peel strength of lithium ion secondary battery negative electrode obtained in Comparative Example 1)×100
[0131] <Example 2> In the polymerization of the binder for the negative electrode of a lithium ion secondary battery, the structural unit (A) was changed to 99.9 parts by mass of acrylic acid, and the structural unit (B) was changed to 0.1 parts by mass of CP-A13H (manufactured by Meisei Chemical Industry Co., Ltd., EO-PO-AGE ternary copolymer, composition ratio EO:PO:AGE=93:5:2, weight average molecular weight 500,000 or more). Except for this, a binder for the negative electrode of a lithium ion secondary battery, a slurry composition for the negative electrode of a lithium ion secondary battery, and a negative electrode for a lithium ion secondary battery were produced in the same manner as in Example 1. Each was evaluated as described above, and the results are shown in Table 1.
[0132] <Example 3> In the polymerization of the binder for the negative electrode of the lithium ion secondary battery, the constituent unit (A) was changed to 98 parts by mass of acrylic acid, and the constituent unit (B) was changed to 2 parts by mass of Daisodap A (manufactured by Osaka Soda, diallyl phthalate resin, Mw 70,000 to 100,000), but other than that, the binder for the negative electrode of the lithium ion secondary battery, the slurry composition for the negative electrode of the lithium ion secondary battery, and the negative electrode for the lithium ion secondary battery were produced in the same manner as in Example 1. Each was evaluated as described above, and the results are shown in Table 1.
[0133] <Comparative Example 1> In the polymerization of the binder for the lithium ion secondary battery negative electrode, except that the structural unit (A) was 100 parts by mass of acrylic acid and the structural unit (B) was not mixed, a binder for the lithium ion secondary battery negative electrode, a slurry composition for the lithium ion secondary battery negative electrode, and a negative electrode for the lithium ion secondary battery were produced in the same manner as in Example 1. Each was evaluated as described above, and the results are shown in Table 1.
[0134] <Comparative Example 2> In the preparation of the lithium ion secondary battery negative electrode binder, a polymerization reaction was carried out only with acrylic acid, which is the structural unit (A), and then 1 part by mass of ALKOX CP-A1H, which is the structural unit (B), was added and stirred to prepare an uncrosslinked lithium ion secondary battery negative electrode binder, but other than this, a slurry composition for lithium ion secondary battery negative electrode and a negative electrode for lithium ion secondary battery were prepared in the same manner as in Example 1. Each was evaluated as described above, and the results are shown in Table 1.
[0135] <Comparative Example 3> In the polymerization of the lithium ion secondary battery negative electrode binder, except that the structural unit (A) was changed to 95 parts by mass of acrylic acid and the structural unit (B) was changed to 5 parts by mass of CP-A1H, a lithium ion secondary battery negative electrode binder was produced in the same manner as in Example 1. Note that the water solubility evaluation of the obtained lithium ion secondary battery negative electrode binder was inappropriate, so no further evaluation was performed.
[0136] <Comparative Example 4> In the polymerization of the lithium ion secondary battery negative electrode binder, except that the structural unit (A) was changed to 99.9 parts by mass of acrylic acid and the structural unit (B) was changed to 0.1 parts by mass of pentaerythritol triallyl ether (manufactured by Osaka Soda Co., Ltd., molecular weight 256), a binder for a lithium ion secondary battery negative electrode, a slurry composition for a lithium ion secondary battery negative electrode, and a negative electrode for a lithium ion secondary battery were produced in the same manner as in Example 1. Each was evaluated as described above, and the results are shown in Table 1.
[0137] <Comparative Example 5> In the polymerization of the lithium ion secondary battery negative electrode binder, except that the structural unit (A) was changed to 99 parts by mass of acrylic acid and the structural unit (B) was changed to 1 part by mass of pentaerythritol triallyl ether, a slurry composition for lithium ion secondary battery negative electrode and a negative electrode for lithium ion secondary battery were prepared in the same manner as in Comparative Example 4. Each was evaluated as described above, and the results are shown in Table 1.
[0138] <Comparative Example 6> In the polymerization of the lithium ion secondary battery negative electrode binder, except that the constituent unit (A) was changed to 99.9 parts by mass of acrylic acid and the constituent unit (B) was changed to 0.1 parts by mass of trimethylolpropane trimethacrylate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., molecular weight 338), a slurry composition for lithium ion secondary battery negative electrode and a negative electrode for lithium ion secondary battery were prepared in the same manner as in Comparative Example 1. Each was evaluated as described above, and the results are shown in Table 1.
[0139] <Comparative Example 7> In the polymerization of the lithium ion secondary battery negative electrode binder, except that the structural unit (A) was changed to 99 parts by mass of acrylic acid and the structural unit (B) was changed to 1 part by mass of trimethylolpropane trimethacrylate, a slurry composition for lithium ion secondary battery negative electrode and a negative electrode for lithium ion secondary battery were prepared in the same manner as in Comparative Example 6. Each was evaluated as described above, and the results are shown in Table 1.
[0140] [Table 1]
[0141] The binder for lithium ion secondary batteries of the present invention has high dispersion stability in water, and in addition, the electrode peel strength of the negative electrode of a lithium ion secondary battery prepared using the binder of the present invention was improved by 119% to 133% compared to Comparative Example 1 (a binder polymerized only with the structural unit (A)). In addition, it was found that the electrode peel strength was not improved unless the structural unit (A) and the structural unit (B) were in a crosslinked state, compared to Comparative Example 2. Furthermore, it was also found that the electrode peel strength was significantly reduced with the crosslinkable monomers (Comparative Examples 4 to 7) commonly used in the field. It is presumed that the use of the crosslinkable monomer increases the number of crosslinking points and shortens the distance between the crosslinking points, improving the elasticity of the polymer, but reduces the conformability and flexibility to the substrate, etc. On the other hand, the crosslinkable polymer used in the present invention can increase the distance between the crosslinking points, which is thought to increase the binding strength with the electrode. [Industrial Applicability]
[0142] The binder for the negative electrode of a lithium ion secondary battery of the present invention has excellent binding properties and high dispersion stability in water, which makes it possible to reduce the environmental load. It is useful for use in lithium ion secondary batteries for in-vehicle applications such as electric vehicles and hybrid electric vehicles, and for home power storage.
Claims
1. A binder for a lithium ion secondary electrode negative electrode, comprising at least a structural unit (A) derived from a (meth)acrylic acid monomer and a structural unit (B) derived from a crosslinkable polymer having a crosslinking group and a weight average molecular weight of 50,000 to 2,500,000, and crosslinking these structural units, A binder for a lithium ion secondary electrode negative electrode, wherein the content of the structural unit (B) is 0.005 to 4 mass % based on 100 mass % of the binder for a lithium ion secondary electrode negative electrode.
2. 2. The binder for a lithium ion secondary battery negative electrode according to claim 1, wherein the crosslinking group of the structural unit (B) is an allyl group.
3. A slurry composition for a lithium ion secondary battery negative electrode, comprising at least the binder for a lithium ion secondary battery negative electrode according to claim 1, an aqueous solvent, and a negative electrode active material comprising a carbon material and / or a silicon compound.
4. A negative electrode for a lithium ion secondary battery, produced by using the slurry composition for a negative electrode for a lithium ion secondary battery according to claim 3.
5. A lithium ion secondary battery produced by using the negative electrode for lithium ion secondary batteries according to claim 4.
Citation Information
Patent Citations
Slurry for lithium ion battery negative electrode, method for manufacturing the same, negative electrode for lithium ion battery, and lithium ion battery
JP2018006334A
Binder composition for secondary battery, electrode for secondary battery containing same, and lithium secondary battery
JP7034407B2